Revolution part made of composite material with improved delamination resistance

The integration of a fibrous interface texture with polyamide or glass fibers between structural layers in composite material parts enhances impact tolerance and retention capacity, addressing delamination issues while maintaining a lightweight design.

FR3147730A1Active Publication Date: 2024-10-18SAFRAN SA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
FR2023003641
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-18
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

Existing composite material parts in propulsion assemblies, such as gas turbine fan casings and nacelle cowls, suffer from weakness at the interfaces between adjacent turns of the fibrous reinforcement, leading to potential delamination and reduced impact tolerance.

Method used

A method involving the use of a fibrous preform with a structural layer and a fibrous interface texture comprising polyamide or glass fibers, where the interface texture has a thickness less than 1 mm and a surface content of fibers between 50% and 70%, interposed between adjacent turns of the structural layer, enhancing bonding and energy dissipation during impacts.

Benefits of technology

The composite material parts exhibit improved toughness and retention capacity, with increased resistance to delamination and impact, maintaining a lower overall mass compared to prior art designs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A process for manufacturing a part of revolution made of composite material with improved delamination resistance comprises: - the production of a fibrous preform on a mandrel (200) having a profile corresponding to that of the part to be manufactured, and - the densification of the fibrous preform by a matrix. The production of the fibrous preform includes the formation of a fibrous blank (140) in the form of a strip comprising a structural layer (50) having a three-dimensional weave and an interface fibrous texture (60) comprising polyamide or glass fibers, the interface fibrous layer having a thickness of less than 1 mm and a surface proportion of polyamide or glass fibers of less than 90%, the fibrous blank being shaped on the mandrel, said interface fibrous layer extending at least one full revolution around the mandrel (200). Figure for the abbreviation: Fig. 7.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Revolutionary part made of composite material with improved delamination resistance Technical field

[0001] The present invention relates to the general field of the manufacture of revolution parts made of composite material for propulsion systems such as gas turbine fan casings, air inlets or nacelle cowls for aeronautical engines. Prior art

[0002] In a gas turbine aircraft engine, the fan casing serves several functions. It defines the air inlet stream into the engine, supports an abradable material opposite the fan blade tips, supports a possible sound wave absorption structure for acoustic treatment at the engine inlet, and incorporates or supports a retention shield. The retention shield provides a debris trap that retains debris, such as ingested objects or fragments of damaged blades, projected by centrifugation, to prevent them from passing through the casing and reaching other parts of the aircraft.

[0003] Previously made of metallic material, the casings, like the fan casing, are now made of composite material, that is to say from a fibrous preform densified by an organic matrix, which makes it possible to produce parts having a lower overall mass than these same parts when they are made of metallic material while having a mechanical resistance at least equivalent if not superior.

[0004] The manufacture of a fan casing made of organic matrix composite material is described in particular in document US 8,322,971. In the casing disclosed in document US 8,322,971, the retention shield is constituted by a portion of excess thickness obtained at the level of the fibrous reinforcement of the casing which has a progressive thickness. The fibrous reinforcement is obtained by winding a 3D woven fibrous texture which has a portion of excess thickness capable of forming a retention shield.

[0005] However, if a 3D woven texture intrinsically has better impact resistance, the interfaces present between the adjacent turns of the 3D woven texture can constitute areas of weakness in the face of an impact. The same is true for an air intake or a nacelle cover of a propulsion unit. Statement of the invention

[0006] It is therefore desirable to be able to have a composite material revolution part for a propulsion unit having increased toughness at the level of the in interfaces between adjacent turns of the fiber reinforcement of the revolution part in order to increase its impact tolerance.

[0007] To this end, according to the invention, a method is proposed for manufacturing a revolution part made of composite material for a propulsion unit comprising: - the production of a fiber preform on a mandrel having a profile corresponding to that of the part to be manufactured, and - densification of the fiber preform by a matrix, characterized in that the production of the fiber preform comprises the formation of a fiber blank in the form of a strip comprising a structural layer having a three-dimensional weave and a fiber interface texture comprising polyamide or glass fibers, the fiber interface texture having a thickness of less than 1 mm and a surface rate of polyamide or glass fibers of less than 90%, the fiber blank being shaped on the mandrel, said fiber interface texture extending at least over one complete turn around the mandrel.

[0008] The method of the invention thus makes it possible to obtain a composite material part having improved toughness at the bonding interfaces between the adjacent turns of the structural layer. The composite material part thus obtained has an increased retention capacity. The addition of a fibrous interface texture made of polyamide or glass fibers makes it possible to reinforce the bonding interface and dissipate more energy during an impact. A more flexible material (glass or polyamide fiber) than the carbon present in the three-dimensional fibrous texture has the effect of causing existing cracks to bifurcate and stop them. Stopping a crack requires re-initiation and therefore more energy. The local bifurcations of cracks increase the crack path and therefore the dissipated energy. This fibrous interface texture makes it possible to multiply the cracks and therefore dissipate more energy in the thickness for a given surface area.The structural layer ensures the cohesion and mechanical resistance of the part.

[0009] It is thus possible to manufacture revolution parts made of composite material having a very good retention capacity without requiring too great an increase in thickness, the parts having an overall mass lower than that of the composite material parts of the prior art.

[0010] According to one aspect of the method of the invention, the interface fibrous texture is chosen from at least one of the following textures: two-dimensional woven, knit, felt, veil, braid and mat.

[0011] According to another aspect of the method of the invention, the interface fibrous texture has a surface rate of polyamide fibers of between 50% and 70%.

[0012] According to another aspect of the method of the invention, the fibrous blank is wound over n turns on the mandrel, the interface fibrous texture extending over n-1 turns around the mandrel. This allows a fibrous interface texture to be interposed between all adjacent turns of the preform and, consequently, of the fibrous reinforcement.

[0013] The invention also relates to a composite material revolution part for a propulsion unit comprising a fibrous reinforcement, said fibrous reinforcement being densified by a matrix, characterized in that the fibrous reinforcement comprises in the thickness direction at least two superimposed layers having a three-dimensional weave and a fibrous interface texture present at the interface between said at least two superimposed layers, the fibrous interface texture comprising polyamide or glass fibers, said fibrous interface texture furthermore having a thickness of less than 1 mm and a surface rate of polyamide or glass fibers of less than 90%.

[0014] As explained above, the composite material part of the invention has increased impact resistance compared to the composite material parts of the prior art.

[0015] According to one aspect of the part of the invention, the interface fibrous texture is chosen from at least one of the following textures: two-dimensional woven, knit, felt, veil, braid and mat.

[0016] According to another aspect of the part of the invention, the interface fibrous texture has a surface rate of polyamide or glass fibers of between 50% and 70%.

[0017] According to another aspect of the part of the invention, the latter corresponds to a casing comprising a ferrule comprising a portion of excess thickness forming a retention zone, the ferrule further comprising at its axial ends a flange. Brief description of the drawings

[0018] [Fig-1] [Fig. 1] is a perspective and partial sectional view of an aeronautical engine equipped with a fan casing made of composite material in accordance with one embodiment of the invention,

[0019] [Fig.2] [Fig.2] is a sectional view along plane II-II of the casing of [Fig.l],

[0020] [Fig.3] [Fig.3] is a schematic perspective view of a loom showing the weaving of a three-dimensional fibrous structure used for the formation of the fibrous reinforcement of the casing of figures 1 and 2,

[0021] [Fig.4] [Fig.4] is a schematic perspective view of a fibrous structure 3D woven,

[0022] [Fig.5] [Fig.5] is a schematic perspective view of a fibrous texture interface,

[0023] [Fig.6] [Fig.6] is a schematic perspective view of a fiber blank formed with the 3D woven fiber structure and the interface fiber texture of the figures 4 and 5 in accordance with one embodiment of the invention,

[0024] [Fig.7] [Fig.7] is a schematic perspective view showing the shaping of the fiber blank of [Fig.6],

[0025] [Fig.8] [Fig.8] is a sectional view of a fiber preform obtained from the fiber blank of [Fig.6],

[0026] [Fig.9] [Fig.9] is a schematic view showing a tool for densifying the preform of [Fig.8]. Description of the embodiments

[0027] The invention applies generally to any rotating part made of composite material for a propulsion unit, the rotating part being likely to be exposed to impacts. Such parts for a propulsion unit relate in particular, but not exclusively, to gas turbine fan casings, nacelle air inlets and nacelle cowls present in aeronautical engines.

[0028] The invention will be described below in the context of its application to a fan casing of an aeronautical gas turbine engine.

[0029] Such an engine, as shown very schematically by [Fig.l] comprises, from upstream to downstream in the direction of the gas flow, a fan 1 arranged at the inlet of the engine, a compressor 2, a combustion chamber 3, a high-pressure turbine 4 and a low-pressure turbine 5.

[0030] The engine is housed inside a casing comprising several parts corresponding to different elements of the engine. Thus, the fan 1 is surrounded by a fan casing 100.

[0031] [Fig. 2] shows a fan casing profile 100 made of composite material as it can be obtained by a method according to the invention. The internal surface 101 of the casing defines the air inlet stream. It can be provided with a layer of abradable coating 102 in line with the path of the fan blade tips, a blade 13 being partially shown very schematically. The abradable coating is therefore arranged over only part of the length (in the axial direction) of the casing. An acoustic treatment coating (not shown) can also be arranged on the internal surface 101, in particular upstream of the abradable coating 102.

[0032] The casing 100 may be provided with external flanges 104, 105 at its upstream and downstream ends in order to allow its mounting and connection with other elements.

[0033] The casing 100 is made of a composite material with fiber reinforcement densified by a matrix. The reinforcement is made of fibers, for example carbon, glass, aramid or ceramic, and the matrix is ​​made of a polymer, for example epoxy, bismaleimide or polyimide, carbon or ceramic.

[0034] The fibrous reinforcement is formed by winding a fibrous blank onto a mandrel, the mandrel having a profile corresponding to that of the casing to be produced. Advantageously, the fibrous reinforcement constitutes a complete tubular fibrous preform of the casing 100 forming a single piece with reinforcing parts corresponding to the flanges 104, 105.

[0035] According to the invention, the fiber blank consists of a structural layer and an interface fiber texture comprising polyamide or glass fibers.

[0036] The structural layer is constituted by a strip-shaped fibrous structure having a three-dimensional weave. More precisely and as illustrated in [Fig. 3], a fibrous structure 50 is produced in a known manner by three-dimensional weaving using a jacquard-type loom 10 on which a bundle of warp threads or strands 20 has been arranged in a plurality of layers, the warp threads being linked by weft threads or strands 30. The threads used for weaving the fibrous structure 50 are, for example, carbon fiber threads, for example HexTow® IM7, HexTow® AS4 or HexTow® AS7 fibers, or ceramic such as silicon carbide, glass, or aramid. The count of the threads is typically 12k, 24k or 48k. Different types of threads can be used within the same preform. The fibrous structure is produced by three-dimensional weaving.By "three-dimensional weaving" or "3D weaving" is meant here a weaving method by which at least some of the weft threads bind warp threads over several layers of warp threads or vice versa. An example of three-dimensional weaving is the so-called "interlock" weave. By "interlock" we mean here a weaving weave in which each layer of warp threads binds several layers of weft threads with all the threads of the same warp column having the same movement in the plane of the weave.

[0037] As illustrated in Figures 3 and 4, the fibrous structure 50 has a strip shape which extends lengthwise in a direction X corresponding to the direction of travel of the warp threads or strands 20 and widthwise or transversely in a direction Y corresponding to the direction of the weft threads or strands 30.

[0038] As illustrated in [Fig. 4], the fibrous structure 50 has a strip shape having a thickness E50, for example 5 mm, corresponding to a 3D weave with between three and five layers of warp woven together in the plane and in the thickness of the strip using weft threads. The fibrous structure 50 extending over a width l50 defined as a function of the width of the casing to be manufactured, the width l50 being able to be for example 2 m, and over a length L50 defined as a function of the diameter of the casing to be manufactured and the desired number of turns in the fibrous reinforcement. For example, to manufacture a similarly cylindrical casing with a diameter of 4 m by making 2 rough turns, the length of the fibrous structure to be woven is approximately 25 m. The length can be extended in order to avoid the beginning and the end of the fibrous structure are not at the same angular position, which could create a weakness in the part.

[0039] In the example described here, the interface fibrous texture is a thin layer of polyamide fibers. Its thickness, which defines the thickness of the interface between the layers or turns of the structural layer, is between 0.02 mm and 1 mm.

[0040] Concerning the rate of polyamide fibers, or glass fibers, present in the interface fibrous layer, we will speak here of "fiber surface rate" rather than "fiber volume rate" given the small thickness of the interface layer. In the case of a two-dimensional interface fibrous texture, we no longer speak of fiber volume rate but of fiber surface rate. This surface rate corresponds to the proportion of surface occupied by the fibers in the plane of the interface texture, the rest of the surface being empty before injection and occupied by resin after injection.

[0041] According to the invention, the fibrous interface layer has a surface rate of polyamide or glass fibers of less than 90%. Indeed, the fibrous interface layer must remain sufficiently aerated in particular so as not to hinder the passage of the resin during the densification of the preform and not to form a privileged weak point in a given cracking plane which could reduce the dissipated energy and therefore the impact resistance.

[0042] The surface rate of polyamide or glass fibers of the interface fiber texture is preferably between 50% and 70% because it makes it possible to further optimize the mechanical performance of the bonding interfaces between two woven layers.

[0043] The fibrous interface layer may have various types of texture such as a two-dimensional woven fabric, a knit fabric, a felt fabric, a veil fabric, a braid fabric or a mat fabric.

[0044] In the example described here, the interface fibrous texture is a two-dimensional or 2D woven textile. [Fig. 5] illustrates an interface fibrous texture 60 consisting of a 2D woven fabric in the form of a strip comprising polyamide or glass fibers 61 randomly distributed over a thickness E60 of less than 1 mm. In the example described here, the interface fibrous texture 60 has a width l60 equivalent to the width l50 of the fibrous structure 50 and a length L60 less than the length L50 of the fibrous structure 50 so that only the fibrous structure 50 is present in the last winding turn of the fibrous blank.

[0045] A fiber blank 140 is then produced by arranging the interface fiber texture 60 on the 3D woven fiber structure 50 as illustrated in [Fig. 6]. A step of sewing the assembly edges between the interface fiber texture 60 and the fiber structure 50 may also be carried out in order to hold them in position in the fiber blank 140. The fiber blank 140 may be compacted in order to reduce the swelling before rolling.

[0046] As illustrated in [Fig.7], a fiber preform is then formed by winding in a direction SR on a mandrel 200 of the fiber blank 140 with the fiber structure 50 arranged against the mandrel 200, the mandrel having a profile corresponding to that of the casing to be produced. The mandrel 200 has an external surface 201 whose profile corresponds to the internal surface of the casing to be produced. By being wound on the mandrel 200, the fiber blank 140 matches the profile thereof. The mandrel 200 also comprises two flanges 220 and 230 to form fiber preform parts corresponding to the flanges 104 and 105 of the casing 100.

[0047] [Fig.8] shows a sectional view of the fiber preform 300 obtained after winding the fiber blank 140 in several layers on the mandrel 200. The number of turns or coils depends on the desired thickness and the thickness of the fiber texture. It is preferably at least equal to 2. In the example described here, the preform 300 comprises, along the direction of its thickness, two layers or turns 51 and 52 of fibrous structure 50 and two layers or turns 62 and 63 of interface fibrous texture 60, the layer or turn 62 being interposed between the adjacent layers or turns 51 and 52 while the layer or turn 63 is present on the external periphery of the preform 300. The fibrous preform 300 also comprises end portions 320, 330 corresponding to the flanges 104, 105 of the casing.

[0048] The fiber preform 300 is then densified using a matrix.

[0049] The densification of the fiber preform consists of filling the porosity of the preform, in all or part of its volume, by the material constituting the matrix.

[0050] The matrix can be obtained in a manner known per se using the liquid method.

[0051] The liquid method consists of impregnating the preform with a liquid composition containing an organic precursor of the matrix material. The organic precursor is usually in the form of a polymer, such as a resin, possibly diluted in a solvent. The fibrous preform is placed in a mold that can be closed in a sealed manner with a housing having the shape of the final molded part. As illustrated in [Fig. 9], the fibrous preform 300 is here placed between a plurality of sectors 240 forming a counter-mold and the mandrel 200 forming a support, these elements having respectively the external shape and the internal shape of the casing to be produced. Then, the liquid matrix precursor, for example a resin, is injected into the entire housing to impregnate the entire fibrous part of the preform.

[0052] The transformation of the precursor into an organic matrix, namely its polymerization, is carried out by heat treatment, generally by heating the mold, after elimination mination of the possible solvent and crosslinking of the polymer, the preform being always maintained in the mold having a shape corresponding to that of the part to be produced. The organic matrix can be obtained in particular from epoxy resins, such as, for example, the high-performance epoxy resin sold, or from liquid precursors of carbon or ceramic matrices.

[0053] In the case of the formation of a carbon or ceramic matrix, the heat treatment consists of pyrolyzing the organic precursor to transform the organic matrix into a carbon or ceramic matrix depending on the precursor used and the pyrolysis conditions. For example, liquid carbon precursors may be resins with a relatively high coke content, such as phenolic resins, while liquid ceramic precursors, in particular SiC, may be resins of the polycarbosilane (PCS) or polytitanocarbosilane (PTCS) or poly-silazane (PSZ) type. Several consecutive cycles, from impregnation to heat treatment, may be carried out to achieve the desired degree of densification.

[0054] According to one aspect of the invention, the densification of the fiber preform can be carried out by the well-known transfer molding process known as RTM ("Resin Transfer Molding"). According to the RTM process, the fiber preform is placed in a mold having the shape of the casing to be produced. A thermosetting resin is injected into the internal space delimited between the mandrel 200 and the counter-molds 240.

[0055] The resin used may be, for example, an epoxy resin. Resins suitable for RTM processes are well known. They preferably have a low viscosity to facilitate their injection into the fibers. The choice of temperature class and / or the chemical nature of the resin is determined according to the thermomechanical stresses to which the part must be subjected. Once the resin has been injected throughout the reinforcement, it is polymerized by heat treatment in accordance with the RTM process.

[0056] After injection and polymerization, the part is demolded. Finally, the part is trimmed to remove excess resin and the chamfers are machined to obtain the casing 100 illustrated in Figures 1 and 2. The casing 100 made of composite material thus comprises a fiber reinforcement consisting in the direction of its thickness of two layers or turns 51 and 52 of fiber structure 50 and two layers or turns 62 and 63 of interface fiber texture 60, the layer 62 being interposed between the adjacent layers 51 and 52 while the layer 63 is present on the external periphery of the casing 100. The number of turns or coils of fiber structure 50 is a function of the desired thickness and the thickness of the layer. It is preferably at least equal to 2. The number of turns or coils of interface fibrous texture 60 is a function of the number of interfaces in the preform whose toughness is to be reinforced.The casing 100 thus has greater resistance to delamination due to the presence of a fibrous interface texture. between the turns of the 3D woven fiber structure and, therefore, a greater capacity to retain debris, particles or objects ingested at the engine inlet, or coming from damaged fan blades, and projected radially by rotation of the fan.

[0057] The manufacturing method described above in relation to a fan casing of an aeronautical gas turbine engine also applies to the manufacturing of other revolution parts made of composite material for propulsion units such as nacelle air inlets or nacelle cowls.

Claims

Claims

1. Method for manufacturing a composite material revolution part (100) for a propulsion assembly comprising: - producing a fiber preform (300) on a mandrel (200) having a profile corresponding to that of the part to be manufactured, and - densifying the fiber preform (300) by a matrix, characterized in that producing the fiber preform comprises forming a fiber blank (140) in the form of a strip comprising a structural layer (50) having a three-dimensional weave and an interface fiber texture (60) comprising polyamide or glass fibers, the interface fiber texture having a thickness of less than 1 mm and a surface rate of polyamide or glass fibers of less than 90%, the fiber blank being shaped on the mandrel (200), said interface fiber layer extending at least over one complete turn around the mandrel.

2. The method of claim 1, wherein the interface fibrous texture (60) is selected from at least one of the following textures: two-dimensional woven, knit, felt, veil, braid and mat.

3. Method according to claim 1 or 2, in which the interface fibrous texture (60) has a surface rate of polyamide or glass fibers of between 50% and 70%.

4. A method according to any one of claims 1 to 3, wherein the fibrous blank is wound over n turns on the mandrel, the interface fibrous texture (60) extending over n-1 turns around the mandrel.

5. Revolutionary part made of composite material (100) for a propulsion unit comprising a fibrous reinforcement, said fibrous reinforcement being densified by a matrix, characterized in that the fibrous reinforcement comprises in the thickness direction at least two superimposed layers having a three-dimensional weave and a fibrous interface texture present at the interface between said at least two superimposed layers, the fibrous interface texture comprising polyamide or glass fibers, said fibrous interface texture further having a thickness of less than 1 mm and a surface rate of polyamide or glass fibers of less than 90%.

6. A part according to claim 5, wherein the interface fibrous texture corresponds to at least one of the following textures: two-dimensional woven, knit, felt, veil, braid and mat.

7. Part according to claim 5 or 6, in which the interface fibrous texture has a surface rate of polyamide or glass fibers of between 50% and 70%.

8. Part according to any one of claims 5 to 7, the part corresponding to a casing (100) comprising a ferrule comprising a portion of excess thickness forming a retention zone, the ferrule further comprising at its axial ends a flange (104, 105).

Citation Information

Patent Citations

  • Method of manufacturing a gas turbine casing out of composite material, and a casing as obtained thereby

    US8322971B2

  • Revolution part made of composite material with improved delamination resistance

    FR3097799A1

  • FIBER PREFORM FOR THE MANUFACTURE OF AN ANNULAR HOUSING IN COMPOSITE MATERIAL FOR A TURBOMACHINE

    FR3123586A1