A rigid polyurethane foam material and its preparation process

A specialized rigid polyurethane foam composition and processing method enhance mechanical strength and thermal insulation, addressing the limitations of existing materials in cryogenic environments, achieving effective cryogenic insulation.

FR3148028A1Pending Publication Date: 2024-10-25JIANGSU YOKE TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2023007760
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2023-07-19
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing rigid polyurethane foam materials suffer from mechanical strength loss and insulation failure in cryogenic environments, limiting their use in ultra-low temperature applications.

Method used

A rigid polyurethane foam composition comprising specific ratios of poly-functional polyether and polyester polyols, polymethylene polyphenyl polyisocyanate, foaming auxiliary additives, and continuous glass fiber felt, processed under controlled conditions to enhance mechanical strength and thermal insulation.

Benefits of technology

The solution results in a foam material with improved compressive strength, thermal insulation, and controlled surface flatness, suitable for cryogenic insulation applications with a density of 70-210 kg/m3 and a base material utilization rate over 85%, maintaining mechanical resistance and thermal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention provides a rigid polyurethane foam material composed of 30-50 parts polyether polyol, 30-50 parts polyether polyol, 50-80 parts toluene diisocyanate, 50-80 parts polymethylene polyphenyl polyisocyanate, 15-30 parts a foaming auxiliary additive compound, and 5-20 parts continuous fiberglass felt (F). The present invention also provides a method for preparing a rigid polyurethane foam material: (1) weighing the various raw materials; (2) mixing all the raw materials except the continuous fiberglass felt (F); (3) pouring the mixture onto the properly laid continuous fiberglass felt (F) for foaming and shaping; (4) curing, cutting (T), and further curing; thus, the preparation is complete. The material according to the present invention has a density of 70-210 kg / m³. (Shorthand figure: Fig. 1)
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: A rigid polyurethane foam material and method of preparing the same Technical field

[0001] The present invention relates to the technical field of polymer materials, and more precisely to a rigid polyurethane foam material and its preparation method. Prior art

[0002] Rigid polyurethane plastic foam, called rigid polyurethane foam, is the second most used material just after flexible polyurethane foam among polyurethane products.Rigid polyurethane foam materials are mostly closed-cell, and have excellent properties such as good thermal insulation effect, light weight, high specific strength and easy processing, they are soundproof, anti-vibration, insulating, heat-resistant, cold-resistant and solvent-resistant, and are widely used for thermal insulation lining of refrigerators and freezers and as thermal insulation materials of cold stores and refrigerated vans, as heat-insulating materials of buildings, storage tanks and pipelines, and are rarely used in scenes other than thermal insulation such as imitation wood materials and packaging materials.Generally, low density rigid polyurethane foam is mainly used as heat insulation (thermal insulation) material, while high density rigid polyurethane foam can be used as structural material (wood imitation material).

[0003] An ordinary rigid polyurethane foam material has excellent thermal insulation performance, however, it will undergo severe shrinkage and cracking in a cryogenic environment, so that it is impossible to maintain its mechanical strength and thermal insulation performance. In order to solve this problem, the mechanical properties and low-temperature dimensional stability of the rigid polyurethane foam material can generally be enhanced by means of a combination with a continuous glass fiber felt, and the fire resistance class can be improved by adding a certain amount of flame retardant.For example, patent 2007101441393 (publication number CN101235128A) proposed a polyurethane foam material with a density of 400-800kg / m3 reinforced by continuous fibers, this material is suitable for use as a "load-bearing structural material", and cannot be used for thermal insulation in an ultra-low temperature environment. Patent 200610058849X (publication number CN1834130A) proposed . a thermal insulation material with a density of 115-135kg / m3 and a compressive strength of l.4-l.7MPa, however, this patent did not give the detailed thermal conductivity coefficient for thermal insulation performance, and the mechanical properties of this material at low temperatures are unknown.

[0004] In addition, considering the addition of a continuous glass fiber felt, the reinforced type rigid polyurethane foam material is generally prepared by a free foaming method, so the confined space foaming method is mainly adopted to prepare low-density polyurethane sandwich panels. For example, Patent 201810493822.6 (Publication No. CN109096459B) proposed an eco-friendly type low-density polyurethane sandwich panel which is a polyurethane core pre-painted sheet manufactured by a continuous polyurethane sandwich panel production method. Patent 202011587634.3 (Publication No. CN112694592A) proposed a polyurethane sandwich panel and its preparation method. However, these polyurethane materials all have a density of less than 50kg / m3 and do not contain any reinforcing material, and thus they are not suitable for the field of cryogenic insulation.

[0005] Therefore, a pressing problem to be solved by those skilled in the art is to develop a reinforced type rigid polyurethane foam material for cryogenic insulation that is continuously produced in a confined space. Content of the invention

[0006] To this end, the present invention aims to provide a rigid polyurethane foam material and its preparation method, in order to fill the gaps in the prior art.

[0007] In order to achieve the above-mentioned objective, the present invention adopts the following technical program:

[0008] A rigid polyurethane foam material, which consists of raw materials whose portions by weight are as follows: 30-50 portions of polyfunctional polyether polyol, 30-50 portions of polyfunctional polyester polyol, 50-80 portions of toluene dii-isocyanate, 50-80 portions of polymethylene polyphenyl polyisocyanate, 15-30 portions of foaming auxiliary additive compound and 5-20 portions of continuous glass fiber felt.

[0009] Preferably, it comprises 35 portions of polyfunctional polyether polyol, 50 portions of polyfunctional polyester polyol, 60 portions of toluene diisocyanate, 80 portions of polymethylene polyphenyl polyisocyanate, 15 portions of foaming auxiliary additive compound and 15 portions of continuous glass fiber felt.

[0010] More specifically, said polyfunctional polyether polyol has a molecular weight of 300-500, preferably 350-450, and even more preferably 400; a hydroxyl number of 500-800mgKOH / g, preferably 550-650mgKOH / g, and even more preferably 600mgKOH / g; a viscosity of 2000-4000mPa-S, preferably 2500-3500mPa-S and even more preferably 3000mPa-S; a moisture content of less than 0.15%. More specifically, said polyfunctional polyether polyol is composed of at least one of the following components: sucrose polyether polyol, sorbitol polyether polyol, pentaerythritol polyether polyol and polytetrahydrofuran diol.

[0011] The beneficial effect of the technical solution mentioned above more precisely is that the polyfunctional polyether polyol chosen within the scope of the present invention makes it possible to further increase the crosslinking density of the rigid polyurethane foam material, thereby improving its compressive strength.

[0012] More specifically, said polyfunctional polyester polyol has a molecular weight of 500-800, preferably 550-650, and even more preferably 600; a hydroxyl number of 200-400mgKOH / g, preferably 350-400mgKOH / g, and even more preferably 380mgKOH / g; a viscosity of 1000-3000mPa-S, preferably 1500-2000mPa-S and even more preferably 1800mPa-S; a moisture content of less than 0.15%. More specifically, said polyfunctional polyester polyol is composed of at least one of the following components: phthalic anhydride polyester polyol, metaphthalic anhydride polyester polyol and aromatic-aliphatic copolyester.

[0013] The beneficial effect of the technical solution mentioned above more precisely is that the compatibility between the polyfunctional polyester polyol and the polymethylene polyphenyl polyisocyanate chosen within the scope of the present invention is better, making it possible to increase the fineness of the foam of the rigid polyurethane foam material, thereby improving its thermal insulation performance.

[0014] More specifically, said polymethylene polyphenyl polyisocyanate has an isocyanate content of 30-40% by weight, preferably 35-37% by weight, and even more preferably 36% by weight; a viscosity of 200-400mPa-S, preferably 250-350mPa-S, and more preferably 300mPa-S; a functionality of 2.0-3.0, preferably 2.5-3.0, and more preferably 2.8.

[0015] The beneficial effect of the technical solution mentioned above more precisely is that the viscosity of the polymethylene polyphenyl polyisocyanate chosen within the scope of the present invention is moderate, which is favorable to the homogeneous mixing of the different components; and its functionality is greater, which makes it possible to further increase the crosslinking density of the rigid polyurethane foam material, thus improving its compressive strength.

[0016] More specifically, said foaming auxiliary additive compound consists of raw materials whose weight portions are as follows: 10-20 portions of copolymer of polyether-polydimethylsiloxane, 30-40 portions of pentafluoropropane, 30-40 portions of trans-l-chloro-3,3,3-trifluoropropene, 1-3 portions of small molecule amine catalyst and 1-3 portions of organotin catalyst; Preferably, it consists of 13 portions of polyether-polydimethylsiloxane copolymer, 32 portions of pentafluoropropane, 38 portions of trans-l-chloro-3,3,3-trifluoropropene, 1.4 portions of small molecule amine catalyst and 2.2 portions of organotin catalyst.

[0017] More specifically, the small molecule amine catalyst is dimethylcyclohexylamine, and the organotin catalyst is dibutyltin dilaurate.

[0018] The beneficial effect of the technical solution mentioned above more precisely is that the foaming auxiliary additive compound chosen within the scope of the present invention comprises foaming agent, stabilizer and catalyst, thus ensuring the mechanical strength and dimensional stability of the rigid polyurethane foam material.

[0019] More specifically, said continuous glass fiber felt has an apparent density of 500-700kg / m2, preferably 550kg / m2; an organic substance content of 2-3% by weight, preferably 2.2% by weight; each roll has a width of 1-3m, preferably 2.1m and a length of 100-150m, preferably 120m.

[0020] The beneficial effect of the technical solution mentioned above more precisely is that the continuous glass fiber felt selected within the scope of the present invention has a high apparent density and a strong strength, and on the surface is applied the coupling agent allowing to be effectively combined with the rigid polyurethane foam essence, to thus improve its tensile strength.

[0021] A process for preparing a rigid polyurethane foam material, comprising the following steps:

[0022] (1) Measure by weighing the different raw materials by their portions by weight composing the rigid polyurethane foam material;

[0023] (2) Mixing polyfunctional polyether polyol, polyfunctional polyester polyol functional, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and the foaming auxiliary additive compound to obtain a mixture;

[0024] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0025] (4) After natural hardening, cut the semi-finished product, with a new curing, thus obtaining the rigid polyurethane foam material.

[0026] More specifically, the equipment for mixing in step (2) above is a high pressure mixer M; The mixing pressure is 50-300bar, preferably 100-150bar; The mixing temperature is 15-35°C, preferably 20-30°C; The output flow rate of high pressure mixer M is 20-120kg / min, preferably 50-80kg / min.

[0027] The beneficial effect of the above-mentioned technical solution more precisely is that the high-pressure mixer M selected within the scope of the present invention has a large mixing pressure, making it possible to improve the mixing effect of the hydroxyl component and the isocyanate component, making the cells of the rigid polyurethane foam material finer with better thermal insulation performance.

[0028] More specifically, the upper, lower, left and right sides of the confined space in step (3) above are composed of high-strength mesh belts; the mesh belts have a width of 5-25mm, preferably 10-20mm; the flatness of the mesh belts is ±0.5-1mm, preferably ±0.5-0.7mm; the temperature of the mesh belts is 15-45°C, preferably 30-40°C; the feed rate of the mesh belts is 0.5-2.5m / min, preferably 1.0-1.5m / min.

[0029] The beneficial effect of the above-mentioned technical solution more specifically is that the polyurethane foaming process within the scope of the present invention is carried out in a confined space, the contour dimensions of the foam are regular and controllable, thereby improving the utilization rate of the polyurethane foam base material.

[0030] More specifically, in step (3) mentioned above, it is also a matter of separating the continuous glass fiber felt and the mesh strips by a kraft paper; said kraft paper has an apparent density of 90-250g / m2, preferably 150-200g / m2.

[0031] The beneficial effect of the technical solution mentioned above more precisely is that the kraft paper chosen within the scope of the present invention makes it possible to separate the glass fiber felt from the M mesh belt, thus avoiding the impact of the M mesh belt on the foaming process.

[0032] More specifically, in step (4) above, the duration of natural hardening is 15-35 min; The duration of new hardening is 48 h.

[0033] More specifically, steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 15-35°C, preferably 20-30°C; the ambient humidity is less than 80%, preferably between 30%-70%.

[0034] It is clear from the above technical solutions that the present invention has the following beneficial effects compared to the prior art:

[0035] The reinforced type rigid polyurethane foam material for cryogenic insulation which is continuously produced in a confined space according to the present invention has a density of 70-210kg / m3, making it possible to control the surface flatness to less than 5mm and to increase the utilization rate of the base material to more than 85% under the condition of ensuring the low temperature mechanical strength and the per thermal insulation performance of the material. It can be widely applied in the field of cryogenic insulation. Brief description of the drawings

[0036] [Fig. 1] represents the flowchart of the process for preparing the rigid polyurethane foam material according to the present invention;

[0037] [Fig.2] shows a physical cross-sectional view of the rigid polyurethane foam material from embodiment 5 according to the present invention;

[0038] [Fig. 3] represents a physical cross-sectional view of the rigid polyurethane foam material from comparative mode 1 according to the present invention. Specific embodiments

[0039] The technical program in the example of the present invention will be described clearly and completely by combining the accompanying figures in this example. Obviously, the described example only shows a part of examples instead of all examples. Based on the example in the present invention, provided that the creative work is not provided, the other example gained by ordinary technical personnel in the present field belongs to the scope of protection of the present invention. Example 1

[0040] A rigid MP polyurethane foam material, composed of the raw materials with the following weights: 30kg of sucrose polyether polyol, 50kg of phthalic anhydride polyester polyol, 80kg of toluene diisocyanate, 50kg of poly-methylene polyphenyl polyisocyanate, 15kg of foaming auxiliary additive compound and 15kg of continuous glass fiber felt;

[0041] Among them, sucrose polyether polyol has a molecular weight of 300, a hydroxyl number of 500mgKOH / g, a viscosity of 2000mPa-S and a moisture content of 0.15%;

[0042] The phthalic anhydride polyester polyol has a molecular weight of 500, a hydroxyl number of 200mgKOH / g, a viscosity of 1000mPa-S and a moisture content of 0.15%;

[0043] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 30% by weight, a viscosity of 200mPa-S and a functionality of 2.0;

[0044] The foaming auxiliary additive compound consists of the raw materials with the following weights: 10kg of polyether-polydimethylsiloxane copolymer, 30kg of pentafluoropropane, 30kg of trans-l-chloro-3,3,3-trifluoropropene, 1kg of di-methylcyclohexylamine and 1kg of dibutyltin dilaurate;

[0045] The continuous glass fiber felt has an apparent density of 500kg / m2, an organic substance content of 2% by weight, with a width of 1m and a length of 100m per roll;

[0046] A method of preparing the above rigid MP polyurethane foam material, as shown in [Fig.l], it involves the following steps:

[0047] (1) Measure by weighing the different raw materials by their weights composing the rigid MP polyurethane foam material above;

[0048] (2) Feed the high pressure mixer M with sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and foaming auxiliary additives compound to be mixed under a pressure of 50bar at 20°C, with an output flow rate of 30kg / min, in order to obtain a mixture;

[0049] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0050] The upper, lower, left and right sides of the confined space are composed of high-strength mesh strips; the mesh strips have a width of 5mm, a flatness of ±0.5mm and operate at a temperature of 20°C and a forward speed of 0.5m / min;

[0051] It is also a question of separating the continuous glass fiber felt and the mesh strips by a kraft paper K; the kraft paper K has an apparent density of 90g / m2;

[0052] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0053] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 15°C and the ambient humidity is equal to 40%.

[0054] Example 2

[0055] A rigid polyurethane foam material, composed of the raw materials having the following weights: 50kg of sucrose polyether polyol, 30kg of phthalic anhydride polyester polyol, 50kg of toluene diisocyanate, 80kg of polymethylene polyphenyl polyisocyanate, 30kg of foaming auxiliary additive compound and 20kg of continuous glass fiber felt;

[0056] Among them, sucrose polyether polyol has a molecular weight of 300, a hydroxyl number of 500mgKOH / g, a viscosity of 2000mPa-S and a moisture content of 0.15%;

[0057] The phthalic anhydride polyester polyol has a molecular weight of 500, a hydroxyl number of 200mgKOH / g, a viscosity of 1000mPa-S and a moisture content of 0.15%;

[0058] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 30% by weight, a viscosity of 200mPa-S and a functionality of 2.0;

[0059] The foaming auxiliary additive compound consists of the raw materials with the following weights: 10kg of polyether-polydimethylsiloxane copolymer, 30kg of pentafluoropropane, 30kg of trans-l-chloro-3,3,3-trifluoropropene, 1kg of di-methylcyclohexylamine and 1kg of dibutyltin dilaurate;

[0060] The continuous glass fiber felt has an apparent density of 500kg / m2, an organic substance content of 2% by weight, with a width of 1m and a length of 100m per roll;

[0061] A method of preparing the above rigid polyurethane foam material, as shown in [Fig.l], comprises the following steps:

[0062] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0063] (2) Feed the high pressure mixer M with sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and foaming auxiliary additives compound to be mixed under a pressure of 100 bar at 25°C, with an output flow rate of 80 kg / min, in order to obtain a mixture;

[0064] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0065] The upper, lower, left and right sides of the confined space are composed of high-strength mesh strips; the mesh strips have a width of 15mm, a flatness of ±0.5mm and operate at a temperature of 25°C and a feed rate of Im / min;

[0066] It is also a question of separating the continuous glass fiber felt and the mesh strips by kraft paper; the kraft paper has an apparent density of 150g / m2;

[0067] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0068] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 20°C and the ambient humidity is equal to 50%.

[0069] Example 3

[0070] A rigid polyurethane foam material, composed of the raw materials having the following weights: 40kg of sorbitol polyether polyol, 40kg of metaphthalic anhydride polyester polyol, 60kg of toluene diisocyanate, 70kg of polymethylene polyphenyl polyisocyanate, 20kg of foaming auxiliary additive compound and 15kg of continuous glass fiber felt;

[0071] Among them, sorbitol polyether polyol has a molecular weight of 350, an index hydroxyl of 550mgKOH / g, a viscosity of 2500mPa-S and a moisture content equal to 0.10%;

[0072] The metaphthalic anhydride polyester polyol has a molecular weight of 550, a hydroxyl number of 350mgKOH / g, a viscosity of 1500mPa-S and a moisture content of 0.10%;

[0073] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 35% by weight, a viscosity of 250mPa-S and a functionality of 2.5;

[0074] The foaming auxiliary additive compound consists of the raw materials with the following weights: 10kg of polyether-polydimethylsiloxane copolymer, 30kg of pentafluoropropane, 30kg of trans-l-chloro-3,3,3-trifluoropropene, 1kg of di-methylcyclohexylamine and 1kg of dibutyltin dilaurate;

[0075] The continuous glass fiber felt has an apparent density of 500kg / m2, an organic substance content of 2% by weight, with a width of 1m and a length of 100m per roll;

[0076] A method of preparing the above rigid polyurethane foam material, as shown in [Fig.l], comprises the following steps:

[0077] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0078] (2) Feed the high pressure mixer M with sorbitol polyether polyol, polyester polyol of metaphthalic anhydride, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and compound of foaming auxiliary additives to be mixed under a pressure of 150bar at 30°C, with an output flow rate of 100kg / min, in order to obtain a mixture;

[0079] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0080] The upper, lower, left and right sides of the confined space are composed of high-strength BM mesh strips; the mesh strips have a width of 10mm, a flatness of ±0.5mm and operate at a temperature of 30°C and a forward speed of 1.5m / min;

[0081] It is also a question of separating the continuous glass fiber felt and the mesh strips by kraft paper; the kraft paper has an apparent density of 180g / m2;

[0082] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0083] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 25°C and the ambient humidity is equal to 60%. Example 4

[0084] A rigid polyurethane foam material, composed of the raw materials having the following weights: 45kg of sorbitol polyether polyol, 35kg of metaphthalic anhydride polyester polyol, 55kg of toluene diisocyanate, 70kg of poly-methylene polyphenyl polyisocyanate, 25g of foaming auxiliary additive compound and 5g of continuous glass fiber felt;

[0085] Among them, sorbitol polyether polyol has a molecular weight of 350, a hydroxyl number of 550mgKOH / g, a viscosity of 2500mPa-S and a moisture content of 0.10%;

[0086] The metaphthalic anhydride polyester polyol has a molecular weight of 550, a hydroxyl number of 350mgKOH / g, a viscosity of 1500mPa-S and a moisture content of 0.10%;

[0087] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 35% by weight, a viscosity of 250mPa-S and a functionality of 2.5;

[0088] The foaming auxiliary additive compound consists of the raw materials with the following weights: 10kg of polyether-polydimethylsiloxane copolymer, 30kg of pentafluoropropane, 30kg of trans-l-chloro-3,3,3-trifluoropropene, 1kg of di-methylcyclohexylamine and 1kg of dibutyltin dilaurate;

[0089] The continuous glass fiber felt has an apparent density of 500kg / m2, an organic substance content of 2% by weight, with a width of 1m and a length of 100m per roll;

[0090] A method of preparing the above rigid polyurethane foam material, as shown in [Fig.l], comprises the following steps:

[0091] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0092] (2) Feed the high pressure mixer M with sorbitol polyether polyol, polyester polyol of metaphthalic anhydride, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and compound of foaming auxiliary additives to be mixed under a pressure of 300bar at 35°C, with an output flow rate of 100kg / min, in order to obtain a mixture;

[0093] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0094] The upper, lower, left and right sides of the confined space are composed of high-strength mesh strips; the mesh strips have a width of 15mm, a flatness of ±0.8mm and operate at a temperature of 35°C and a forward speed of 2.0m / min;

[0095] It is also a matter of separating the continuous glass fiber felt and the strips to meshed with kraft paper; kraft paper has an apparent density of 250g / m2;

[0096] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0097] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 30°C and the ambient humidity is equal to 60%. Example 5

[0098] A rigid polyurethane foam material, composed of the raw materials having the following weights: 35kg of sucrose polyether polyol, 50kg of phthalic anhydride polyester polyol, 60kg of toluene diisocyanate, 80kg of polymethylene polyphenyl polyisocyanate, 15kg of foaming auxiliary additive compound and 15kg of continuous glass fiber felt;

[0099] Among them, sucrose polyether polyol has a molecular weight of 400, a hydroxyl number of 600mgKOH / g, a viscosity of 3000mPa-S and a moisture content of 0.05%;

[0100] The phthalic anhydride polyester polyol has a molecular weight of 600, a hydroxyl number of 380mgKOH / g, a viscosity of 1800mPa-S and a moisture content of 0.05%;

[0101] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 36% by weight, a viscosity of 300mPa-S and a functionality of 2.8;

[0102] The foaming auxiliary additive compound consists of the raw materials with the following weights: 13kg of polyether-polydimethylsiloxane copolymer, 32kg of pentafluoropropane, 38kg of trans-l-chloro-3,3,3-trifluoropropene, 1.4kg of dimethylcyclohexylamine and 2.2kg of dibutyltin dilaurate;

[0103] The continuous glass fiber felt has an apparent density of 550kg / m2, an organic substance content of 2.2% by weight, with a width of 2.1m and a length of 120m per roll;

[0104] A method of preparing the above rigid polyurethane foam material, as shown in [Fig.l], comprises the following steps:

[0105] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0106] (2) Feed the high pressure mixer M with sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and foaming auxiliary additives compound to be mixed under a pressure of 150bar at 25°C, with an output flow rate of 120kg / min, in order to obtain a mixture;

[0107] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0108] The upper, lower, left and right sides of the confined space are composed of high-strength mesh strips; the mesh strips have a width of 20mm, a flatness of ±0.5mm and operate at a temperature of 40°C and a forward speed of 2.5m / min;

[0109] It is also a question of separating the continuous glass fiber felt and the mesh strips by kraft paper; the kraft paper has an apparent density of 160g / m2;

[0110] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0111] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 20°C and the ambient humidity is equal to 70%. Example 6

[0112] A rigid polyurethane foam material, composed of the raw materials with the following weights: 50kg of polytetrahydrofuran diol, 45kg of aromatic-aliphatic copolyester, 60kg of toluene diisocyanate, 55kg of poly-methylene polyphenyl polyisocyanate, 20kg of foaming auxiliary additive compound and 10kg of continuous glass fiber felt;

[0113] Among them, polytetrahydrofuran diol has a molecular weight of 450, a hydroxyl number of 650mgKOH / g, a viscosity of 3500mPa-S and a moisture content of 0.10%;

[0114] The aromatic-aliphatic copolyester has a molecular weight of 650, a hydroxyl number of 400mgKOH / g, a viscosity of 2000mPa-S and a moisture content of 0.10%;

[0115] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 37% by weight, a viscosity of 350mPa-S and a functionality of 3.0;

[0116] The foaming auxiliary additive compound consists of the raw materials with the following weights: 20kg of polyether-polydimethylsiloxane copolymer, 40kg of pentafluoropropane, 40kg of trans-l-chloro-3,3,3-trifluoropropene, 3kg of di-methylcyclohexylamine and 3kg of dibutyltin dilaurate;

[0117] The continuous glass fiber felt has an apparent density of 700kg / m2, an organic substance content of 3% by weight, with a width of 3m and a length of 150m per roll;

[0118] A method of preparing the above rigid polyurethane foam material, as shown in [Fig.l], comprises the following steps:

[0119] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0120] (2) Feed the high pressure mixer M with polytetrahydrofuran diol, co aromatic-aliphatic polyester, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and compound of foaming auxiliary additives to be mixed under a pressure of 150bar at 20°C, with an output flow rate of 75kg / min, in order to obtain a mixture;

[0121] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0122] The upper, lower, left and right sides of the confined space are composed of high-strength mesh strips; the mesh strips have a width of 12mm, a flatness of ±0.7mm and operate at a temperature of 30°C and a forward speed of 1.5m / min;

[0123] It is also a question of separating the continuous glass fiber felt and the mesh strips by a kraft paper K; the kraft paper K has an apparent density of 100g / m2;

[0124] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0125] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 20°C and the ambient humidity is equal to 50%. Example 7

[0126] A rigid polyurethane foam material, composed of the raw materials having the following weights: 48kg of polytetrahydrofuran diol, 48kg of aromatic-aliphatic copolyester, 66kg of toluene diisocyanate, 51kg of polymethylene polyphenyl polyisocyanate, 18kg of foaming auxiliary additive compound and 8kg of continuous glass fiber felt;

[0127] Among them, polytetrahydrofuran diol has a molecular weight of 500, a hydroxyl number of 800mgKOH / g, a viscosity of 4000mPa-S and a moisture content of 0.10%;

[0128] The aromatic-aliphatic copolyester has a molecular weight of 800, a hydroxyl number of 400mgKOH / g, a viscosity of 3000mPa-S and a moisture content of 0.10%;

[0129] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 40% by weight, a viscosity of 400mPa-S and a functionality of 3.0;

[0130] The foaming auxiliary additive compound consists of the raw materials with the following weights: 20kg of polyether-polydimethylsiloxane copolymer, 40kg of pentafluoropropane, 40kg of trans-l-chloro-3,3,3-trifluoropropene, 3kg of di- methylcyclohexylamine and 3kg of dibutyltin dilaurate;

[0131] The continuous glass fiber felt has an apparent density of 700kg / m2, an organic substance content of 3% by weight, with a width of 3m and a length of 150m per roll;

[0132] A method of preparing the above rigid polyurethane foam material, as shown in [Fig.l], comprises the following steps:

[0133] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0134] (2) Feed the high pressure mixer M with polytetrahydrofuran diol, co aromatic-aliphatic polyester, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and compound of foaming auxiliary additives to be mixed under a pressure of 80bar at 25°C, with an output flow rate of 105kg / min, in order to obtain a mixture;

[0135] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming in a confined space, to obtain a semi-finished product;

[0136] The upper, lower, left and right sides of the confined space are composed of high-strength mesh strips; the mesh strips have a width of 9mm, a flatness of ±1mm and operate at a temperature of 30°C and a forward speed of 1.3m / min;

[0137] It is also a question of separating the continuous glass fiber felt and the mesh strips by a kraft paper K; the kraft paper K has an apparent density of 130g / m2;

[0138] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0139] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 25°C and the ambient humidity is equal to 80%. Comparative mode 1

[0140] A rigid polyurethane foam material, composed of the raw materials having the following weights: 45kg of sucrose polyether polyol, 45kg of phthalic anhydride polyester polyol, 55kg of toluene diisocyanate, 65kg of polymethylene polyphenyl polyisocyanate, 20kg of foaming auxiliary additive compound and 11kg of continuous glass fiber felt;

[0141] Among them, sucrose polyether polyol has a molecular weight of 400, a hydroxyl number of 600mgKOH / g, a viscosity of 3000mPa-S and a moisture content of 0.05%;

[0142] Phthalic anhydride polyester polyol has a molecular weight of 600, an index hydroxyl of 380mgKOH / g, a viscosity of 1800mPa-S and a moisture content of 0.05%;

[0143] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 36% by weight, a viscosity of 300mPa-S and a functionality of 2.8;

[0144] The foaming auxiliary additive compound consists of the raw materials with the following weights: 13kg of polyether-polydimethylsiloxane copolymer, 32kg of pentafluoropropane, 38kg of trans-l-chloro-3,3,3-trifluoropropene, 1.4kg of dimethylcyclohexylamine and 2.2kg of dibutyltin dilaurate;

[0145] The continuous glass fiber felt has an apparent density of 550kg / m2, an organic substance content of 2.2% by weight, with a width of 2.1m and a length of 120m per roll;

[0146] A process for preparing said rigid polyurethane foam material, comprising the following steps:

[0147] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0148] (2) Feed the high pressure mixer M with sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and foaming auxiliary additives compound to be mixed under a pressure of 95bar at 25°C, with an output flow rate of 95kg / min, in order to obtain a mixture;

[0149] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming to obtain a semi-finished product;

[0150] It is also a matter of separating the continuous glass fiber felt and the foaming medium; the K kraft paper has an apparent density of 110g / m2;

[0151] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0152] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 35°C and the ambient humidity is equal to 40%. Comparative mode 2

[0153] A rigid polyurethane foam material, composed of the raw materials having the following weights: 55kg of sucrose polyether polyol, 45kg of phthalic anhydride polyester polyol, 65kg of toluene diisocyanate, 55kg of polymethylene polyphenyl polyisocyanate, 10kg of foaming auxiliary additive compound and 10kg of continuous glass fiber felt;

[0154] Among them, sucrose polyether polyol has a molecular weight of 400, a hydroxyl number of 600mgKOH / g, a viscosity of 3000mPa-S and a content of humidity equal to 0.05%;

[0155] The phthalic anhydride polyester polyol has a molecular weight of 600, a hydroxyl number of 380mgKOH / g, a viscosity of 1800mPa-S and a moisture content of 0.05%;

[0156] Polymethylene polyphenyl polyisocyanate has an isocyanate content of 36% by weight, a viscosity of 300mPa-S and a functionality of 2.8;

[0157] The foaming auxiliary additive compound consists of the raw materials with the following weights: 13kg of polyether-polydimethylsiloxane copolymer, 32kg of pentafluoropropane, 38kg of trans-l-chloro-3,3,3-trifluoropropene, 1.4kg of dimethylcyclohexylamine and 2.2kg of dibutyltin dilaurate;

[0158] The continuous glass fiber felt has an apparent density of 550kg / m2, an organic substance content of 2.2% by weight, with a width of 2.1m and a length of 120m per roll;

[0159] A process for preparing said rigid polyurethane foam material, comprising the following steps:

[0160] (1) Measure by weighing the different raw materials by their weights composing the rigid polyurethane foam material above;

[0161] (2) Feed the high pressure mixer M with sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate, and foaming auxiliary additives compound to be mixed under a pressure of 120bar at 20°C, with an output flow rate of 135kg / min, in order to obtain a mixture;

[0162] (3) Pour the mixture onto the well-laid continuous fiberglass felt, which will then subjected to foaming and forming to obtain a semi-finished product;

[0163] It is also a matter of separating the continuous glass fiber felt and the foaming medium; the K kraft paper has an apparent density of 110g / m2;

[0164] (4) The semi-finished product will be subjected to natural hardening for 20 minutes followed by of a T-cut before a new hardening for 48 hours, to obtain the rigid polyurethane foam material;

[0165] Steps (2) - (4) are carried out in an environment at constant temperature and humidity, where the ambient temperature is 30°C and the ambient humidity is equal to 60%. Performance test

[0166] 1. Take respectively polyurethane foam materials obtained according to the embodiments 1 to 7 and comparative embodiments 1 and 2, the raw material doses and process parameters of which are shown in Table 1.

[0167] Test respectively their density, their compressive strength, their tensile strength, their thermal conductivity, their percentage of closed cells, their surface flatness and their base material utilization rate, the test results are shown in Table 2.

[0168] For which the different performances are evaluated as follows:

[0169] Product density: The test is carried out in accordance with GB / T 6343-2009 after removing the skin from rigid polyurethane foam materials and cutting them into cubes.

[0170] Compressive strength: Rigid polyurethane foam materials are cut into 50mmx50rnmx50mm samples to be tested at -160°C according to GB / T 8813-2008.

[0171] Tensile strength: Rigid polyurethane foam materials are cut into dumbbell-shaped samples for testing at -160°C in accordance with BS ISO 1926-2005.

[0172] Thermal conductivity: Rigid polyurethane foam materials are cut into 300mmx300mmx30mm samples for testing at -160°C in accordance with ISO 8302.

[0173] Percentage of closed cells: Rigid polyurethane foam materials are cut into 30mmx30mmx50mm samples for testing at 20°C in accordance with GB / T 10799-1989.

[0174] Surface flatness: it is calculated from the difference in level measured between the lowest point and the highest point of the surface of rigid polyurethane foam materials.

[0175] Base material utilization rate: It is calculated from the ratio of the volume of a rigid polyurethane foam material after removing the skin from the top, bottom and side sides to the volume of the rigid polyurethane foam material blank.

[0176] Table 1 Raw material doses and process parameters for rigid polyurethane foam materials according to embodiments 1 to 7 and comparative embodiments 1 and 2 Dose or process parameter Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative mode 1 Comparative mode 2 Polyfunctional polyether polyol (kg) 30 50 40 45 35 50 48 45 55 Polyester 50 30 40 35 50 45 48 45 45 Polyfunctional polyol (kg) Toluene diisocyanate (kg) 80 50 60 55 60 60 66 55 65 Polymethylene polyphenyl polyisocyanate (kg) 50 80 70 70 80 55 51 65 55 Foaming auxiliary additives compound (kg) 15 30 20 25 15 20 18 20 10 Continuous glass fibre felt (kg) 15 20 15 5 15 10 8 11 10 Mixing pressure (bar) 50 100 150 300 150 150 80 95 120 Mixing temperature (°C) 20 25 30 35 25 20 25 25 20 Output flow rate (kg / min) 30 80 100 100 120 75 105 95 135 Mesh belt thickness 5 15 10 15 20 12 9 NA NA (mm) Mesh belt flatness (mm) ±0.5 ±0.5 ±0.5 ±0.8 ±0.5 ±0.7 ±1 NA NA Mesh belt temperature (°C) 20 25 30 35 40 30 30 NA NA Mesh belt speed (m / min) 0.5 1 1.5 2 2.5 1.5 1.3 NA NA Bulk density of kraft paper (g / m 2) 90 150 180 250 160 100 130 110 110 Ambient temperature (°C) 15 20 25 30 20 20 25 35 30 Ambient humidity (%) 40 50 60 60 70 50 80 40 60

[0177] Table 2 Results of performance tests of rigid polyurethane foam materials according to embodiments 1 to 7 and comparative modes 1 and 2 Item Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative mode 1 Comparative mode 2 Density (kg / m3) 70 130 150 150 210 120 140 130 70 Strength 0.92 2.99 3.70 3.62 5.85 3.03 3.35 2.95 0.95 Compressive strength (MPa) Tensile strength (Mpa) 1.38 3.21 3.90 4.01 6.79 3.09 3.52 3.18 1.29 Thermal conductivity (mw / m«k) 13 16 18 18 22 16 17 16 13 Percentage of closed cells (%) 95 97 98 97 98 96 96 96 95 Surface flatness (mm) 5 4 4 3 2 3 3 25 37 Base material utilization rate (%) 85 88 87 86 88 86 85 72 65

[0178] It is apparent from Table 2 that, compared to Comparative Modes 1 and 2, the rigid polyurethane foam materials obtained according to Embodiments 1 to 7 of the present invention are considerably more efficient in terms of density, compressive strength, tensile strength, thermal conductivity, percentage of closed cells, surface flatness and base material utilization rate.

[0179] 2. Taking respectively polyurethane foam materials obtained according to the Embodiment 5 and Comparative Mode 1, to be cut. Their physical cross-sectional views are respectively shown in [Fig.2] and [Fig.3].

[0180] It is clear from Figures 2 and 3 that, compared to comparative mode 1, the material in rigid polyurethane foam obtained according to embodiment 5 of the present invention has improved surface flatness.

[0181] The above tests 1 and 2 show that the reinforced type rigid polyurethane foam material for cryogenic insulation which is continuously produced in a confined space according to the present invention has a density of 70-210kg / m3, making it possible to control the surface flatness within 5mm and increase the utilization rate of the base material to more than 85% under the condition of ensuring the low temperature mechanical strength and thermal insulation performance of the material. It can be widely applied in the field of cryogenic insulation.

[0182] The above description of the disclosed embodiments enables those skilled in the art to practice or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. The present invention will therefore not be limited to the embodiments indicated in this disclosure, and should cover the broadest scope corresponding to the principles and novel features disclosed in this disclosure.

Claims

Claims

1. A rigid polyurethane (MP) foam material, characterized in that it consists of raw materials whose weight portions are as follows: 30-50 portions of polyfunctional polyether polyol, 30-50 portions of polyfunctional polyester polyol, 50-80 portions of toluene dii-isocyanate, 50-80 portions of polymethylene polyphenyl polyisocyanate, 15-30 portions of foaming auxiliary additive compound and 5-20 portions of continuous glass fiber felt (F).

2. A rigid polyurethane (MP) foam material according to claim 1, characterized in that it consists of raw materials whose portions by weight are as follows: 35 portions of polyfunctional polyether polyol, 50 portions of polyfunctional polyester polyol, 60 portions of toluene diisocyanate, 80 portions of polymethylene polyphenyl polyisocyanate, 15 portions of foaming auxiliary additive compound and 15 portions of continuous glass fiber felt (F).

3. A rigid polyurethane foam material according to claim 1 or claim 2, characterized in that said polyfunctional polyether polyol has a molecular weight of 300-500, a hydroxyl number of 500-800mgKOH / g, a viscosity of 2000-4000mPa-S and a moisture content of less than 0.15%; said polyfunctional polyester polyol has a molecular weight of 500-800, a hydroxyl number of 200-400mgKOH / g, a viscosity of 1000-3000mPa-S and a moisture content of less than 0.15%.

4. A rigid polyurethane (MP) foam material according to claim 1 or claim 2, characterized in that said polymethylene polyphenyl polyisocyanate has an isocyanate content of 30-40% by weight, a viscosity of 200-400mPa-S and a functionality of 2.0-3.

0.

5. A rigid polyurethane (MP) foam material according to claim 1 or claim 2, characterized in that said foaming auxiliary additive compound consists of raw materials whose portions by weight are as follows: 10-20 portions of polyether-polydimethylsiloxane copolymer, 30-40 portions of pentafluoropropane, 30-40 portions of trans-l-chloro-3,3,3-trifluoropropene, 1-3 portions of small molecule amine catalyst and 1-3 portions of organotin catalyst.

6. A rigid polyurethane foam (MP) material according to claim 1 or claim 2, characterized in that said continuous felt in Glass fibers (F) have an apparent density of 500-700kg / m2, an organic content of 2-3% by weight, with a width of l-3m and a length of 100-150m per roll.

7. A method for preparing a rigid polyurethane foam material (MP), characterized in that it comprises the following steps: (1) Dosing by weighing the various raw materials by their weight portions composing the rigid polyurethane foam material according to any one of claims 1 to 6; (2) Mixing polyfunctional polyether polyol, polyfunctional polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and the foaming auxiliary additive compound to obtain a mixture; (3) Pouring the mixture onto the well-laid continuous glass fiber felt (F), which will then be foamed and formed in a confined space, to obtain a semi-finished product; (4) The semi-finished product will be subjected to natural curing followed by cutting (T) before further curing, to thereby obtain said rigid polyurethane foam material (MP).

8. A process for preparing a rigid polyurethane foam (MP) material according to claim 7, characterized in that an equipment for said mixing in step (2) is a high pressure mixer (M) which operates under a pressure of 50-300bar and at a temperature of 15-35°C with an output flow rate of 20-120kg / min.

9. A method for preparing a rigid polyurethane foam (MP) material according to claim 7, characterized in that the upper, lower, left and right sides of said confined space in step (3) are composed of high-strength mesh strips; said mesh strips have a width of 5-25mm, a flatness of ±0.5-1mm and operate at a temperature of 15-45°C and a feed rate of 0.5-2.5m / min; and characterized in that the continuous glass fiber felt and the mesh strips are separated by a kraft paper; said kraft paper having an apparent density of 90-250g / m2.

10. A process for preparing a rigid polyurethane foam (MP) material according to claim 7, characterized in that the duration of said natural curing in step (4) is 15-35min and the duration of said new curing is 48h; Steps (2) - (4) are carried out in a medium at temperature and constant humidity, where the ambient temperature is 15-35°C and the ambient humidity is less than 80%.