Low density natural fiber reinforcements for composites, fabrics and reinforced plastic composites composed thereof
A hybrid roving of combed natural plant fibers with controlled density and uniform distribution addresses the limitations of natural fiber composites, enhancing mechanical performance and ecological efficiency.
Patent Information
- Application Number
- FR2023004110
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing composites reinforced with natural fibers face challenges in achieving high strength-to-weight ratios, are limited by fiber variability, and lack effective hybridization solutions, leading to reduced mechanical performance and increased ecological impact.
A roving composed of combed natural plant fibers with an apparent density of 1.35 g/cm3 or less, combined with another natural fiber type, is created through processes like combing and stretching to form a continuous ribbon with uniform distribution, resulting in a hybrid reinforcement with improved mechanical properties.
The hybrid roving achieves enhanced strength-to-weight and stiffness-to-weight ratios, reduces microfractures, and adapts to specific application needs, offering improved mechanical performance and reduced environmental footprint.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Low density natural fiber reinforcements for composites, fabrics and reinforced plastic composites composed thereof Technical field
[0001] The present disclosure relates generally to the field of fiber-reinforced or fabric-reinforced composites, and in particular to rovings, tows, continuous tapes or fabrics for use in fiber-reinforced composites, and to the resulting compositions. Context
[0002] Each year, millions of kilograms of carbon fibers, glass fibers, flax fibers, basalt fibers, and other fibers with advantageous tensile, compressive, and / or flexural strengths are produced for use as reinforcing materials in fiber-reinforced composites, or FRCs (Fiber-Reinforced Composites, which may also be referred to as FRPs). These reinforcing fibers are combined with thermosetting or thermoplastic plastic resins (collectively referred to as the matrix) to create structural materials with properties superior to those of the individual components.
[0003] The importance of natural fibers, or more precisely, plant-based composite reinforcing fibers, in a business context largely defined by the pressures of climate change and the need to reduce CO2 emissions, is significant. The ecological impact of producing one kilogram of carbon fiber includes the production of nearly 30 kg of greenhouse gases; and the manufacture of one kilogram of “E” glass fiber generates approximately 2.8 kg of greenhouse gases. Conversely, if carbon sequestration during cultivation is taken into account, most plant-based reinforcing fibers are carbon neutral until they leave the factory.
[0004] There is a need in the art for improved reinforcing fiber construction, as well as improved reinforcing fabric composition, based on natural fibers, and particularly for applications in which a relatively high strength-to-weight ratio is desired. Summary of the invention
[0005] The current state of the art in the field of composites shows that the only industrialized natural fiber for high-performance composites - that is, applications that require aligned fiber orientation to achieve the desired characteristics - is strength and stiffness characteristics relative to weight - is flax fiber. Flax fiber has a density of about 1.5 g / cm3, which is about 85% of the density of carbon fiber, whereas flax typically offers about 10% of the tensile strength of carbon fiber and 30% of the strength and bending stiffness of carbon fiber.
[0006] The closest additional fiber to industrialization for aligned natural fiber composites is hemp. This fiber has properties very similar to flax in terms of density, as well as tensile and flexural strength.
[0007] According to the "Law of Mixtures", the properties of a material are present in a composite in the proportion that the material is present. Thus, if a composite is composed of 70% carbon fibers and 30% epoxy resin, the resulting composite will have characteristics approximately equal to 70% of the characteristics of the carbon fibers plus 30% of the characteristics of the epoxy. This is a theoretical value that will be reduced depending on the effectiveness of the bond between the reinforcing fiber and the matrix, as well as the congruity of their individual mechanical properties. The Law of Mixtures also applies to composites in which more than one reinforcing fiber is present in the structure.
[0008] When materials having different mechanical properties are hybridized in a composite structure - either at the tows of a fabric or at the layers of a composite - the resulting performance is generally further reduced due to a stress concentration where the different mechanical properties of the reinforcing materials meet in the matrix that encompasses the abutting regions. Although it may be desirable, in the manufacture of structures requiring specific mechanical properties, to use hybrid reinforcements in the fabric layups, this can reduce the mechanical efficiency of the composite by up to 10% and, in some cases, beyond 10%.
[0009] Examples of negative effects include impacts on the overall performance of the composite structure due to hybridization, which may be accentuated depending on the magnitude of the difference between the mechanical characteristics of one hybridization fiber and another. For example, if flax tows are alternated with carbon tows in a fabric, the flax fiber may have a positive effect on the overall vibration characteristics of the resulting part, but the fact that the flax fibers have both a greater elongation at break and lower tensile and flexural strength means that they are likely to contribute minimally to the resistance to deformation before the carbon fibers have reached their yield strength in the composite material. Companies such as Salomon (the name "Salomon" may be covered by one or more registered trademarks) in the Sporting goods companies have produced such hybrids and have described the performance achieved as similar to that of fiberglass. However, this combination comes at a higher cost and has a greater environmental impact.
[0010] Industries that rely heavily on the use of composites for manufacturing range from the automotive and aerospace sectors to sports equipment and household goods. These different industries accordingly require different performance characteristics as well as large volumes of their chosen composite reinforcement fibers. In this context, other considerations for hybridization come to the fore. One of these is scale: of the many promising natural fibers for reinforcement, only a small percentage are grown on a scale large enough to be viable for industrial purposes.
[0011] A second factor associated with scale is fiber variability, as natural fibers—and especially plant fibers—can have very different mechanical characteristics depending on where they are grown and how they are processed. To achieve consistent roving quality (i.e., the mechanical strength of the resulting roving and / or composite), the variability inherent in the cultivation of plant-derived fibers must be sufficiently well controlled so that predictable performance can be achieved with natural fibers. This is an increasingly difficult task in the era of climate change.
[0012] Third, there is a common demand to create reinforcing materials that can be tailored to the requirements of specific applications, as is possible by using different grades of glass, carbon, aramid, and other synthetic fibers. By adjusting the recipe of the fiber precursors, or the manufacturing processes and temperatures, it is possible to modify the performance of the reinforcing material. Although the variation during cultivation mentioned above ( ), as well as the additional variation due to different processing of natural fibers, occurs, these variations are not directly controllable in the same way as with synthetic fibers.
[0013] In composites, the roving is considered the "smallest divisible unit" within which the composition of the reinforcement is uniform. Common synthetic reinforcing fibers, such as glass and carbon fibers, are drawn as continuous filaments ([Fig.l]) and combined into rovings (100) when the fibers are positioned parallel, close to each other, and lightly bonded together with a sizing agent (102). In contrast, natural reinforcing fibers ([Fig.2]) have finite lengths (201) and the rovings (200) are produced in a manner similar to the preparation of a yarn based on natural fibers. turelles, but without 'twist' - the difference being that the rovings instead rely on the surface structure of the fibers holding them in place (202) with other adjacent fibers as the continuous fiber ribbon is thinned and lightened by a series of combs and drawing units during the processing process. The finite length fibers in the roving are then attached to each other using chemical or physical binding agents.
[0014] Although the general concept of creating natural fiber reinforcements using more than one type of fiber has been mentioned in a limited number of patent filings, to date the inventor has found no evidence that industrially applicable solutions exist or even solutions where a uniform distribution of fibers in a reinforcement has been sought (i.e., at a level where the fibers are functionally distributed more uniformly than the equivalent of alternating tows in a fabric).
[0015] Furthermore, many plant fibers are not suitable for processing into hybrid rovings because they are too stiff and / or too large in diameter. In order to be doubled and blended with other fibers, a fiber must be treated by combing. Fibers such as sisal are too large in diameter and too stiff to undergo this process. These fibers can only be used in natural fiber composites in the "pre-carded" or "carded" state, where the fiber orientation is generally less than 10 to 15° relative to the longitudinal axis of the carded fiber web. These fiber webs contain both long and short fibers, as well as certain other impurities, which decrease the mechanical performance of the fiber web.Conversely, combing removes all short fibers from the composition as well as other impurities, leaving only the longest and strongest fibers in the continuous fiber ribbon.
[0016] Beyond the technical complexity of creating a hybrid roving with well-distributed fibers, the concept of creating a successful hybrid roving is complicated by the aforementioned Law of Mixtures ( ). A review of the available literature on the performance of different natural fibers in composites shows that the expected result of hybridizing virtually any other fiber with flax fiber would result in inferior performance or a gain of no consequence, which would likely not be worth the complications inherent in such an endeavor.
[0017] There is therefore a need in the art for an improved construction of reinforcing fibers and an improved composition of reinforcing fabric allowing efficient hybridization, particularly with regard to natural fiber reinforcements.
[0018] The embodiments of the present disclosure are intended to at least partially meet some or all of the needs of the prior art.
[0019] One aspect of the present disclosure ([Fig.3]) consists of a roving (300) composed of at least one combed natural plant fiber having an apparent density of 1.35 g / cm3 or less (301) of a first type and at least one natural fiber of a second type (311). The fibers of each type are, for example, oriented lengthwise and, for example, without twisting into a continuous fiber ribbon (340 and 341). The at least two fiber ribbons are then, for example, laid next to each other and blended into a single continuous fiber ribbon with a substantially equal distribution of fibers, for example through the use of at least one doubling or combing and drawing process and, preferably, multiple doublings. The resulting fiber ribbon, composed of both types of fibers, for example, has a linear weight of at least 5 grams per meter and at most 100 grams per meter, and preferably between 20 grams per meter and 50 grams per meter.This fiber ribbon is then, for example, stretched until a roving is obtained, which has, for example, a weight of at least 60 grams per linear kilometer and, for example, at most 8000 grams per linear kilometer. This hybrid roving of natural fibers is, for example, used in whole or in part to form the reinforcing element of a fiber-reinforced composite. The resulting roving has an apparent density of 1.40 g / cm3 or less, and preferably 1.35 or less, and more preferably 1.30 g / cm3 or less.
[0020] The embodiments are claimed in the claims.
[0021] One embodiment provides a continuous fiber roving, tow, or ribbon (also referred to herein as "Low Density Natural Fiber Reinforcement") for a fiber-reinforced composite comprising: - at least one natural fiber of plant origin of a first type having an apparent density of 1.35 g / cm3 or less and; - at least one additional natural fiber of a second type; wherein the fibers are blended and combed together into a single continuous roving or fiber ribbon which has an apparent density of 1.40 g / cm 3 or less, and preferably 1.35 g / cm 3 or less, and more preferably 1.30 g / cm 3 or less.
[0022] According to one embodiment, the combed natural plant fiber of a first type having an apparent density of 1.35 g / cm3 or less and the additional natural fiber of a second type are oriented in the length direction, for example without twisting, or with minimal possible twisting of the fibers to form a continuous fiber ribbon having an apparent density of 1.40 g / cm3 or less.
[0023] According to one embodiment, the combed natural plant fiber of a first type having an apparent density of 1.35 g / cm3 or less and the additional natural fiber of a second type are distributed in the continuous roving, tow or fiber ribbon, said continuous roving, tow or fiber ribbon having for example a weight of at least 60 grams per linear kilometer and at most 8000 grams per kilometer linear.
[0024] According to one embodiment, the combed natural plant fiber of a first type having an apparent density equal to or less than 1.35 g / cm3 is a combed plant fiber such as jute, kenaf, banana fiber; or other bast, leaf, grass, husk, seed or fruit fibers, and wherein the apparent density is, for example, calculated by determining the exterior volume of the fiber - including internal voids that a resin forming the matrix of a composite could not fill - and dividing the mass of the fiber by this volume.
[0025] There are various types of plant fibers whose density varies considerably depending on the growing climate, the age of the plant, and the specific variety (i.e., species or subspecies) of the plant. Bamboo fiber, for example, has been measured to have a density that can range from 0.8 g / cm3 to 1.6 g / cm3. Such a fiber can be considered a plant fiber having a density of less than 1.35 g / cm3 provided that the selection of the fibers is carried out in such a way as to maintain overall, and with a reasonable level of consistency, an apparent density of the resulting continuous fiber ribbon equal to or less than 1.35 g / cm3.
[0026] According to one embodiment, the natural fiber of a second type is a plant fiber such as hemp, flax, ramie, abaca, alfa, pineapple leaf or other bast fibers, leaves, grasses, pods, seeds or fruits.
[0027] According to one embodiment, the roving, tow or continuous fiber ribbon is composed solely of fibers of the first and second type as well as unavoidable impurities.
[0028] According to one embodiment, the continuous fiber roving, tow or ribbon is composed solely of fibers of the first and second type, and fibers made of a thermoplastic material which are then melted during the curing cycle of the composite to form the composite matrix.
[0029] According to one embodiment, the roving, tow or continuous fiber ribbon is composed of more than two types of fibers, for a resulting density less than or equal to 1.40 g / cm3.
[0030] Another embodiment provides a reinforcing strip composed of at least one tow as indicated above.
[0031] Another embodiment provides a braided reinforcement composed of at least one tow as indicated above.
[0032] Another embodiment provides a reinforcement in fabric sewn, woven or glued in a form, composed of at least one tow as indicated above.
[0033] Another embodiment provides a bonded reinforcing fabric in sheet or roll form, composed of at least one continuous natural fiber ribbon, or sliver, of a density of 1.40 g / cm3 or less, having a linear weight of at least 5 grams per meter and not more than 100 grams per meter, and preferably between 20 grams per meter and 50 grams per meter. Said at least one continuous natural fiber ribbon is, for example, spread flat and the fibers are lightly bonded in position relative to each other using a natural or synthetic adhesive which may comprise, for example, a two-step epoxy prepreg system.
[0034] Another embodiment provides a fiber-reinforced composite comprising a reinforcing element comprising at least one continuous fiber roving, tow, or ribbon as indicated above, placed or embedded in a thermosetting or thermoplastic matrix, i.e., a matrix formed, for example, from a thermosetting or thermoplastic plastic resin.
[0035] Another embodiment provides a fiber-reinforced composite comprising a reinforcing element comprising a plurality of laminates or layers as indicated above and / or one of the reinforcements as indicated above placed or incorporated in a thermosetting or thermoplastic matrix, i.e., a matrix formed, for example, from a thermosetting or thermoplastic plastic resin.
[0036] Another embodiment provides a shaft for propulsion or athletic support, such as a trekking pole or a golf club shaft, made from the aforementioned fiber-reinforced composite.
[0037] Another embodiment provides a racket or paddle comprising a handle or body made from the aforementioned fiber-reinforced composite.
[0038] Another embodiment provides a sailboat mast or other component comprising the aforementioned fiber-reinforced composite.
[0039] Another embodiment provides a wind turbine blade comprising the aforementioned fiber-reinforced composite.
[0040] Another embodiment provides an automotive panel or structural component comprising the aforementioned fiber-reinforced composite.
[0041] Another embodiment provides a method of forming a continuous fiber roving, tow, or ribbon for a fiber-reinforced composite, comprising: combing or doubling at least one combed natural plant fiber of a first type having a bulk density of 1.35 g / cm3 or less; and at least one additional natural fiber of a second type and drawing these fibers to form a single continuous fiber roving, tow, or ribbon. Brief description of the drawings
[0042] The above-mentioned and other features and advantages will be described in detail in the following description of specific embodiments given by way of example. illustrative and non-limiting with reference to the attached drawings, in which:
[0043] [Fig.l] represents a continuous filament and a roving formed from continuous filaments;
[0044] [Fig.2] represents a filament of finite length and a roving formed from filaments of finite length;
[0045] [Fig. 3] represents a natural plant filament of finite length formed of fibers of a first type; an additional natural filament of finite length formed from fibers of a second type; ribbons formed from these filaments of finite length; and a continuous roving, tow or fiber ribbon, formed from these filaments according to an embodiment of the present disclosure;
[0046] [Fig.4] represents a filament of finite length having a first length, formed from natural plant fibers of a first type; an additional natural filament of finite length having a second length and formed from natural fibers of a second type; ribbons formed from these filaments of finite length; and a continuous roving, tow or fiber ribbon formed from these filaments according to an embodiment of the present disclosure;
[0047] [Fig.5] represents a unidirectional reinforcing fabric composed of tows of reinforcing fibers as described above;
[0048] [Fig.6] represents a unidirectional stitched fabric composed of fiber tows of reinforcement using at least one tow as described above;
[0049] [Fig.7] represents a multiaxial stitched fabric composed of fiber tows of reinforcement using at least one tow as described above;
[0050] [Fig.8] represents a woven multiaxial fabric composed of tows of ren fibers necessarily using at least one tow as described above;
[0051] [Fig.9] represents a tubular braid composed of tows of ren fibers necessarily using at least one tow as described above;
[0052] [Fig. 10] represents a unidirectional fabric comprising alternating tows of reinforcing fibers located astride tows as described above;
[0053] [Fig. 11] represents a biaxial fabric comprising alternating tows of fibers of reinforcement located astride tows as described above;
[0054] [Fig. 12] shows a 2x1 twill fabric comprising alternating tows of fibers reinforcement located astride tows as described above; and
[0055] [Fig. 13] shows a plain weave fabric comprising alternating tows of reinforcing fibers located astride tows as described above. Description of the embodiments
[0056] Similar features have been designated by similar references in the various figures. In particular, structural and / or functional features common to the various embodiments may have the same references and have identical structural, dimensional and material properties.
[0057] In the present disclosure, unless otherwise indicated, when reference is made to absolute position qualifiers, such as the terms "front", "back", "top", "bottom", "left", "right", etc., or relative position qualifiers, such as the terms "above", "below", "higher", "lower", etc. or orientation qualifiers, such as "horizontal", "vertical", etc., reference is made to the orientation indicated in the figures.
[0058] Unless otherwise indicated, the expressions "about", "approximately", "substantially" and "in the order of" mean to within 10%, and preferably to within 5%.
[0059] [Fig. 3] represents a natural plant filament of finite length 301 and formed of fibers of a first type; an additional natural filament of finite length 311 and formed of fibers of a second type; ribbons 340, 341 formed of these filaments of finite length; and a roving, tow or continuous fiber ribbon 300 formed of filaments according to an embodiment of the present disclosure.
[0060] [Fig.4] shows a finite length filament 401 having a first length and formed from natural plant fibers of a first type; an additional finite length natural filament 411 having a second length and formed from natural fibers of a second type; ribbons 440, 441 formed from these finite length filaments; and a continuous roving, tow or fiber ribbon 400 formed from these filaments according to an embodiment of the present disclosure.
[0061] A "natural fiber" is a mineral, plant, or animal fiber whose prepared length is, for example, greater than 50 mm and which has desirable mechanical properties for reinforcing FRCs. Examples include basalt fibers and boron fibers (both mineral-based); flax, hemp, ramie, bamboo, pineapple leaf, sisal, kenaf, banana leaf, and coconut fibers (all plant-based); and silk, animal hair, and serosa fibers (all animal-based). For the purposes of this patent, mineral, plant, and animal fibers are considered "classes" of natural fibers; basalt, boron, flax, ramie, bamboo, silk, etc. are considered "types" of fibers.
[0062] A "continuous fiber sliver" (also known as "top" or "sliver") is a loose, flexible, untwisted yarn of coincident fibers having a substantially uniform thickness and consistent fiber orientation along the length of the sliver. It is, for example, made by the carding process, which aligns and separates raw fibers to prepare them for the production of rovings.
[0063] “Apparent density” is defined as the density of a fiber calculated by dividing the mass of the fiber by the volume defined by its outer surface, including voids internal spaces that a resin forming the matrix of a composite could not fill. Bulk density differs from "absolute density" in that absolute density is calculated by dividing the mass of the fiber by the volume of gas it displaces in a controlled environment, which excludes from the volume any voids within the fiber structure.
[0064] Apparent density (g / cm3) of selected plant fibers: Extracted cellulose - 1.58; Linen - 1.50; Ramie - 1.47; Hemp - 1.46; Pineapple leaf - 1.38; European nettle - 1.29; Jute - 1.09; Kenaf - 1.10; Banana - 0.83.
[0065] The resulting rovings may then be used in a process such as filament winding or incorporated as a unidirectional reinforcing strip in a matrix, or may be incorporated as tows in a braided, woven or sewn fabric in a multiaxial or unidirectional construction.
[0066] The fibers that are combined to produce the roving each have, for example, a finished length of at least 50 mm and at most 1500 mm ([Fig.4]). In order to further tailor the performance of the roving, the different types of fibers (401 and 411) may have different average lengths, so that the fibers of a first type may have a length of, for example, between 300 and 400 mm, while the fibers of the second type may have a length of, for example, between 120 and 180 mm, for example.
[0067] The rovings and / or fabrics may be combined with any thermosetting or thermoplastic resin system to form an FRC.
[0068] Rovings can be created with more than two types of fibers.
[0069] The tows may be incorporated into a fabric such that at least one tow in at least one axis utilizes the "Low-Density Natural-Fiber Reinforcement" construction.
[0070] The Low Density Natural Fiber Reinforcements may be incorporated into a sewn, woven, or braided fabric without other fiber tows, or a tow may be created using the Low Density Natural Fiber Reinforcements and incorporated into a fabric with tows other than the Low Density Natural Fiber Reinforcements.
[0071] The fabrics may comprise at least one Natural Fiber Reinforcement of Low Density and at least one additional roving or tow in the same axis or in an alternate axis, and these rovings or tows may be spaced from each other so as to form an open mesh or grid-like structure which is held, mechanically or chemically, coherent.
[0072] Rovings, tows and fabrics created from Low Density Natural Fiber Reinforcements may contain additional resins, resin-based filaments (such as polylactic acid, polyolefin or polyamide) or other chemicals to tailor the performance of the resulting FRC.
[0073] The advantages of the disclosed solution are multiple:
[0074] 1) Although there is a limit to the strength of a cellulose-based fiber, which is not not chemically modified or carbonized, and this limit is generally considered to be between 1200 and 1500 MPa, it is possible to improve the strength-to-weight ratio and stiffness-to-weight ratio of natural fiber composites by using lower density fibers. If, for example, two fibers have similar mechanical properties, with the first fiber having a strength that is 10% lower than the second, but also a density that is 20% lower, according to the Law of Mixtures, the fiber mixture will have both a higher strength-to-weight ratio than either of the individual fibers, and a higher ultimate strength than the lighter fiber.
[0075] 2) Research carried out by the inventor on resistance and rigidity to bending, as well as on the tensile strength and stiffness of some combinations of natural fibers, such as flax and jute for example, show an improvement of 10% to more than 100% over the specific mechanical performance expected based on the predictions of the Law of Mixtures when the fibers are blended into a roving. The same research shows that other combinations, such as flax and pineapple leaf fiber for example, can have specific mechanical characteristics that are 10 to 30% lower than those predicted by the Law of Mixtures.
[0076] 3) Hybridization of the composite reinforcement at the roving level to increase the homogeneity of the fibers in the matrix allows for more effective resistance to loads between the different fibers and a reduction in microfractures in the matrix where the mechanical characteristics of the alternating rovings have caused stress increases.
[0077] 4) The extreme rigidity of high modulus carbon fibers has made it possible to obtain a exceptionally thin wall thickness for composite parts. The typical density of carbon fiber is about 1.8 g / cm3. Although much less stiff than high modulus carbon fiber and requiring a thicker wall to achieve the same stiffness, fiberglass has a density of 2.7-3.0 g / cm3, making it much less effective at producing stiffness. Fiber Reinforcements Low Density fibers described in the present disclosure have been measured to have an apparent density between 0.9 and 1.4 g / cm3 and a specific stiffness similar to that of standard modulus carbon fiber and can be used in composites with a wall thickness greater than that of carbon fiber for a corresponding fiber mass to improve durability.
[0078] 5) By hybridizing rovings composed of fibers of different types and / or different different classes, and possibly of different lengths, it is possible to adapt the performance of the roving to an application. For example, a combination of fibers having a density of 1.40 g / cm3 or less, composed of a first combed natural fiber having a density less than 1.35 g / cm3 and a flax fiber in a 50 / 50 ratio, is capable of improving the specific tensile performance by 15% compared to the flax fiber and increasing the specific flexural performance by 25%; while a combination having a density of 1.40 g / cm3 or less, composed of a third fiber with these same two fibers in a 50 / 25 / 25 ratio, is capable of producing an increase in the specific flexural performance of 80% compared to the flax fiber with only a 10% reduction in tensile strength properties.
[0079] Examples of fabrics comprising rovings or tows as described herein are illustrated in Figures 5 to 13, these fabrics being for example similar to those described in PCT publication WO2020 / 222045, but in which the tow or roving of this publication has been replaced by the tow or roving described herein.
[0080] [Fig.5] represents a unidirectional reinforcing fabric composed of tows of reinforcing fibers as described above.
[0081] [Fig.6] shows a unidirectional stitched fabric composed of reinforcing fiber tows using at least one tow as described above.
[0082] [Fig.7] shows a multiaxial stitched fabric composed of reinforcing fiber tows using at least one tow as described above.
[0083] [Fig.8] shows a multiaxial woven fabric composed of reinforcing fiber tows using at least one tow as described above.
[0084] [Fig.9] shows a tubular braid composed of reinforcing fiber tows using at least one tow as described above.
[0085] [Fig. 10] shows a unidirectional fabric comprising alternating tows of reinforcing fibers located astride tows as described above.
[0086] [Fig. 11] shows a biaxial fabric comprising alternating tows of reinforcing fibers located astride tows as described above.
[0087] [Fig. 12] shows a 2x1 twill fabric comprising alternating tows of reinforcing fibers located astride tows as described above.
[0088] [Fig. 13] shows a plain weave fabric comprising alternating tows of reinforcing fibers located astride tows as described above.
[0089] In Figures 5 to 13, the references designate the following: - unidirectional reinforcing fabric 500; - unidirectional (UD) fabric sewn 600; - the tows described above, arranged in strips 602; - the additional thread 604; - 700 multiaxial stitched fabric; - 702 tows; - sewing 704; - 800 woven multiaxial fabric; - tows in the vertical direction 802; - 804 tows in the horizontal direction; - 900 tubular braid; - 902 tows; - unidirectional fabric 1000; - roving 1002 as described herein; - other 1004 rovings formed from other materials; - biaxial fabric 1100; - two layers 1102, 1104 of unidirectional fabric; - 2x1 1200 twill fabric; - tow 1002 as described herein; - other tow 1004; - 1300 plain weave fabric.
[0090] Various embodiments and variations have been described. Those skilled in the art will understand that certain features of these embodiments may be combined and that other variations will readily occur to those skilled in the art.
[0091] Finally, the practical implementation of the embodiments and variants described in the present disclosure is within the reach of persons skilled in the art, based on the functional description provided above.
Claims
Claims
1. A tow for a fiber-reinforced composite comprising: - at least one combed natural plant fiber of a first type having an apparent density of 1.35 g / cm3 or less; and - at least one additional natural fiber of a second type, wherein the fibers are blended and combed together to form a single continuous fiber ribbon having an apparent density of 1.40 g / cm3 or less.
2. The tow of claim 1, wherein the natural plant fiber of a first type and a natural fiber of a second type are oriented lengthwise, for example without twist, or with minimal twist achievable for the fibers, to form a continuous fiber ribbon having a linear weight of at least 5 grams per meter and at most 100 grams per meter, and more preferably between 20 grams per meter and 50 grams per meter.
3. The tow of claim 1 or 2, wherein the natural plant fiber of a first type and the natural fiber of a second type are distributed in the tow, the tow having a weight of at least 60 g per linear kilometer and at most 8,000 g per linear kilometer.
4. The tow of any one of claims 1 to 3, wherein the first natural fiber is a combed plant fiber such as jute, kenaf, banana, or other bast, leaf, grass, husk, seed, or fruit fibers having a bulk density of 1.35 g / cm3 or less, the bulk density being, for example, calculated by determining the exterior volume of the fiber—including internal voids that a resin forming the matrix of a composite could not fill—and dividing the mass of the fiber by that volume.
5. The tow of one of claims 1 to 4, composed solely of fibers of the first and second type, and unavoidable impurities.
6. The tow of any one of claims 1 to 4, composed solely of fibers of the first and second types, which combine to have an apparent density of 1.40 g / cm3 or less, and fibers formed of a thermoplastic material capable of being melted during a curing cycle of the composite to form a matrix of the composite.
7. The tow of one of claims 1 to 4 and 6, composed of more than two types of natural fibers.
8. A reinforcing strip composed of at least one tow according to one of of claims 1 to 7.
9. A braided reinforcement composed of at least one tow according to one of claims 1 to 7.
10. A fabric reinforcement sewn, woven or glued in a form, composed of at least one tow according to one of claims 1 to 7.
11. A bonded reinforcing fabric in sheet or roll form, composed of at least one of the continuous natural fiber ribbons according to one of claims 1 to 7, having a density of 1.40 g / cm3 or less, having a linear weight of at least 5 grams per meter and at most 100 grams per meter, and more preferably between 20 grams per meter and 50 grams per meter.
12. A fiber-reinforced composite comprising a reinforcing element comprising a plurality of tows according to one of claims 1 to 7, located or embedded in a matrix formed of a thermosetting or thermoplastic plastic resin.
13. A fiber-reinforced composite comprising a reinforcing element comprising a plurality of tows of any one of claims 1 to 7 and / or one of the reinforcements of claims 8 to 11 located or embedded in a matrix formed of a thermosetting or thermoplastic plastic resin.
14. An athletic propulsion or support shaft, such as a trekking pole or a golf club shaft, comprising a structural layer formed from the fiber-reinforced composite of claim 12 or 13.
15. A racket or paddle comprising a handle or body having a structural layer formed from the fiber-reinforced composite of claim 12 or 13.
16. A sailboat mast formed from the fiber-reinforced composite of claim 12 or 13.
17. A wind turbine blade formed from the fiber-reinforced composite of claim 12 or 13.
18. An automotive panel formed from the fiber-reinforced composite of claim 12 or 13.
19. A method of forming a tow for a fiber-reinforced composite, comprising: - mixing, combing or doubling at least one combed natural plant fiber of a first type having an apparent density of 1.35 g / cm3 or less and at least one other fiber of a second type for forming a single tow, in which the fibers are blended, combed, or doubled to form a single continuous tow or fiber sliver that has an apparent density equal to or less than 1.40 g / cm3.
Citation Information
Patent Citations
Rovings and fabrics for fiber-reinforced composites
WO2020222045A1
Hybridization of reinforcement using natural fibers for composite materials and fabrics made from them
FR3125542A1
Method for producing a composite material
WO2018202918A1