A tire comprising a sidewall with at least one high-contrast sidewall element
A tire sidewall composition with isoprene elastomer, anti-ozone wax, and rubber crumb microparticles maintains high contrast and durability by resisting ozone attacks, addressing the issue of sidewall degradation in tire designs.
Patent Information
- Application Number
- FR2023004443
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-03
AI Technical Summary
Existing tire sidewall designs with high-contrast elements suffer from reduced durability over time due to chemical degradation, leading to altered color and shine, which affects the visual and aesthetic appearance and contrast, especially in sports or prestige vehicles.
A tire sidewall composition comprising an elastomeric matrix with isoprene elastomer, reinforcing filler, anti-ozone wax, and rubber crumb microparticles, specifically formulated to maintain high contrast by controlling brightness and resisting ozone attacks, with a rubber composition that includes a weight ratio of anti-ozone wax to microparticles and a brightness range of 1 to 15 for the high-contrast element and 5 to 28 for adjacent surfaces.
The solution maintains significant contrast over the tire's lifespan by reducing color alteration and ozone-induced cracks, ensuring a durable and visually appealing sidewall appearance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Tire comprising a sidewall with at least one high-contrast sidewall element
[0001] The present invention relates to a tire for a vehicle, comprising a sidewall with at least one high contrast sidewall element.
[0002] A tire comprises two sidewalls, a sidewall being the portion of the tire connecting one end of the tread, intended to come into contact with a ground, to a bead, intended to be mounted on a rim.
[0003] In the following, the external surface of a sidewall, in contact with atmospheric air, is designated, more simply, by the term "sidewall surface". A sidewall surface generally comprises at least one graphic element and / or, possibly, an aesthetic element. A graphic element, usually called marking and comprising letters, numbers or symbols, is generally intended to communicate technical, commercial or legal information.
[0004] By definition, a high-contrast sidewall element refers to a sidewall surface element, consisting of a specific texture different from that of the sidewall surface, which is most often smooth. This texture gives said high-contrast sidewall element a darker appearance than that of any portion of sidewall surface adjacent to said high-contrast sidewall element, such that this high-contrast sidewall element can be visually distinguished from any portion of adjacent sidewall surface. A high-contrast sidewall element may have as its object either a graphic element or an aesthetic element, or a portion of sidewall surface surrounding said graphic or aesthetic element, which makes said graphic or aesthetic element particularly visible on the sidewall surface.
[0005] Thus, whether for the enhancement of graphic elements or aesthetic elements of the sidewall surface, there is a constant concern among tire designers to produce sidewall elements with high contrast.
[0006] The contrast between a high-contrast sidewall element and a portion of sidewall surface adjacent to said high-contrast sidewall element is due to a difference in brightness between the two areas. An adjacent surface portion, which may be smooth or have a different texture, has a brightness greater than that of the texture of said high-contrast sidewall element, i.e. it appears visually lighter. This texture is made of a rubbery material, also called a rubber composition or elastomeric composition, identical to that of the portion of sidewall in contact with atmospheric air, since this texture is integral with the sidewall.
[0007] Brightness can be quantified by luminous luminance, expressed in candela / m2, which measures the luminous flux coming from an illuminated surface that is reflected in the eye of the observer. But the relationship between luminous luminance and the visual perception of brightness is not linear and is complex. This is the reason why, on a practical level, the International Commission on Illumination (CIE) has defined the brightness L*, a parameter that characterizes the capacity of a surface to reflect light, from the luminous luminance of the light produced by a primary or secondary source, expressed in candelas per square meter (cd / m2), relative to the luminous luminance of white taken as a reference. Thus, in what follows, the brightness L* is expressed according to a scale ranging from 0 to 100 in accordance with the L*a*b* colorimetric model adopted in 1976 by the International Commission on Illumination.The value 100 represents white or total reflection and the value 0 represents black or total absorption.
[0008] To calculate the difference between a first brightness L*1 of the texture of the high-contrast flank element and a second brightness L*2 of an adjacent flank surface portion, the first brightness L*1 and the second brightness L*2 must be measured respectively using a spectro-colorimeter, for example a KONICA-MINOLTA CM 700D spectro-colorimeter. To measure the first brightness L*1 of the texture, the spectro-colorimeter is positioned on the texture and this measurement is carried out with the SCI mode (Specular Reflection Included Mode) set at an angle of 8° and with a light setting of type D65 (setting defined according to the CIE). Similarly, to measure the second brightness L*2 of an adjacent flank surface portion, the spectro-colorimeter is positioned on said flank surface portion.In order to improve the determination of this second luminosity L*2, it is possible to carry out a plurality of luminosity measurements on several adjacent portions of flank surface, then to deduce an associated average luminosity.
[0009] High contrast sidewall elements, having a brightness difference substantially lower than that of an adjacent sidewall surface portion, have been described in WO 2016005572 A1 and WO 2011036061 A1 and WO 20174919 A1
[0010] It has been observed on tire sidewall surfaces, including high contrast sidewall elements, that the contrast between the high contrast sidewall elements and any adjacent sidewall surface portion changes over time.
[0011] The evolution of the contrast, over time, results from both the evolution of the texture and that of the visual appearance of the flank surface.
[0012] The evolution of the texture can result from its fouling, its at least partial abrasion or the aging of its constituent material.
[0013] The evolution of the visual appearance of the flank surface typically results in a evolution, at least locally, of its coloring (blueing, evolution towards a dark brown color, appearance of whitish spots), an evolution of its brightness (duller appearance) or the appearance of scratches or surface cracks.
[0014] More generally, the aging of the sidewall surface is linked to the elastomeric nature of its material. As is known, the usual rubber compositions comprise diene elastomers, natural or synthetic, whose molecular chains have carbon-carbon double bonds. These double bonds are chemically more reactive than a single carbon-carbon bond and are therefore likely to deteriorate more or less rapidly after prolonged exposure to the atmosphere, due to known oxidation and ozonolysis mechanisms. The action of ozone promotes the appearance of cracks on the surface of the sidewall. These degradation mechanisms are further accelerated by the action of heat (thermo-oxidation) or by that of light (photo-oxidation).
[0015] To overcome the chemical degradation of the rubber composition by ozone, it is known to use anti-ozone agents, such as, for example, anti-ozone waxes. These anti-ozone waxes provide static protection by forming a protective coating on the surface. However, these anti-ozone waxes are characterized by their ability to migrate to the sidewall surface and to crystallize, which modifies the visual appearance of the sidewall surface, causing the appearance of stains or giving the sidewall a dull and gray appearance, or even causing a lighter coloring of the sidewall. This phenomenon is called "blooming". This phenomenon thus causes a non-uniform coloring and makes the sidewall surface, initially black and shiny, gray and dull.
[0016] Thus, a non-uniform coloring of the sidewall surface reduces the contrast effect of the high-contrast element and alters the visual and aesthetic appearance of the sidewall.
[0017] It therefore proves necessary, in order to obtain a sidewall element with high contrast that lasts throughout the life of the tire, to be able to reduce, or even eliminate, the alteration of the color and / or the brightness of the sidewall surface of the tire, while giving it a good capacity to resist ozone attacks that initiate cracks on the sidewall surface.
[0018] Increasing the durability of contrast is indeed an important commercial issue for a tire manufacturer. Thus, for example, when a user replaces only the tires fitted to the front of his vehicle, he may possibly notice a significant difference between the contrast observed on the new tires fitted to the front of the vehicle and that observed on the used tires fitted to the rear of the vehicle. This difference in contrast, between the front and rear tires, may be deemed unacceptable by the user, especially when his vehicle is a sports or prestige vehicle.
[0019] The inventors therefore set themselves the objective, for a tire comprising a sidewall with at least one high-contrast sidewall element, of increasing the durability over time of the contrast between said high-contrast sidewall element and the adjacent surface portion of the sidewall, using a suitable rubber composition of the sidewall, in particular close to the sidewall surface.
[0020] This objective has been achieved by a tire for a vehicle, comprising a sidewall with at least one high-contrast sidewall element: - the high contrast flank element being constituted by a texture having a first brightness L*1 at least equal to 1 and at most equal to 15, - any portion of flank surface adjacent to the high-contrast flank element, having a second brightness L*2 at least equal to L*l+5, -the sidewall comprising a rubber composition based on an elastomer matrix comprising an isoprene elastomer, at least one reinforcing filler, at least one crosslinking system, at least one anti-ozone wax and at least one rubber crumb comprising microparticles having a size of less than 74 pm, - the rate of isoprene elastomer being at least equal to 27.00% by weight, relative to the total weight of the rubber composition, - the anti-ozone wax rate being at least equal to 0.60% by weight and at most equal to 1.70% by weight, relative to the total weight of the rubber composition, -and a weight ratio between the rate of microparticles of rubber crumb having a size less than 74 pm and the rate of anti-ozone wax, these rates being expressed as a percentage by weight, relative to the total weight of the rubber composition, being at least equal to 0.50.
[0021] According to the invention, the high-contrast flank element is constituted by a texture having a first brightness L*1 at least equal to 1 and at most equal to 15.
[0022] The lower the brightness of the high-contrast sidewall element in the new condition of the tire, the greater the contrast for a given brightness of an adjacent sidewall surface portion, and the more significant this contrast will remain over time on the aged tire. Indeed, over time, this first brightness L*1 of the texture of the high-contrast sidewall element tends to increase due, for example, to dust, dirt, or aging of the material. Furthermore, in this brightness range, there is good contrast with any adjacent sidewall surface portion, which, in conventional tire designs, has a brightness most often between 24 and 28. It should be noted that a texture with a first brightness L*1, typically at least equal to 9, is easier to produce, but the contrast is low.
[0023] According to the invention, any portion of flank surface adjacent to the high-contrast flank element has a second brightness L*2 at least equal to L*l+5.
[0024] The greater the difference in brightness between the high-contrast sidewall element and any adjacent portion of sidewall surface, the greater the contrast. The greater this difference in brightness on the new tire, the more significant it will remain, over time, on the aged tire.
[0025] Also according to the invention, the sidewall comprises a rubber composition based on an elastomer matrix comprising an isoprene elastomer, at least one reinforcing filler, at least one crosslinking system, at least one antiozonating wax and at least one rubber crumb comprising microparticles having a size of less than 74 μm.
[0026] The expression "rubber composition based on" means a rubber composition comprising the mixture and / or the in situ reaction product of the different constituents used, some of these constituents being able to react and / or being intended to react with each other, at least partially, during the different phases of manufacture of the rubber composition, the rubber composition thus being able to be in the totally or partially crosslinked state or in the non-crosslinked state.
[0027] A rubber composition comprises at least one and often several elastomers, in particular several diene elastomers. This mixture of elastomers, in particular diene elastomers, is called an elastomer matrix. Most often the elastomer matrix comprises at least two different diene elastomers.
[0028] The term "elastomer" means a polymer, i.e. a homopolymer or a copolymer, having elastic properties obtained after crosslinking. The term rubber is a common synonym for elastomer.
[0029] By "diene elastomer" or indistinctly "diene rubber", whether natural or synthetic, is meant an elastomer consisting at least in part of diene monomer units (monomers carrying two carbon-carbon double bonds, conjugated or not). Diene elastomers are non-thermoplastic.
[0030] Diene elastomers can be classified into two categories: “essentially unsaturated” diene elastomers and “essentially saturated” diene elastomers. An “essentially unsaturated” diene elastomer is a diene elastomer derived at least in part from conjugated diene monomers, having a content of units or patterns of diene origin (conjugated dienes) which is greater than 15% (mol %). Thus, diene elastomers such as butyl rubbers or copolymers of dienes and alpha-olefins such as EPDM do not fall within the preceding definition and can be described in particular as “essentially saturated” diene elastomers (low or very low content of patterns of diene origin, always less than 15%).
[0031] The term diene elastomer capable of being used in the rubber compositions in accordance with the invention is particularly understood to mean: a. Any homopolymer of a diene monomer, conjugated or not, having from 4 to 18 carbon atoms; b. Any copolymer of a diene, conjugated or not, having from 4 to 18 carbon atoms and at least one other monomer; the other being ethylene, an olefin or a diene, conjugated or not.
[0032] Suitable conjugated dienes are conjugated dienes having from 4 to 12 carbon atoms, in particular 1,3-dienes, such as in particular 1,3-butadiene and isoprene.
[0033] Suitable non-conjugated dienes are non-conjugated dienes having from 6 to 12 carbon atoms, such as 1,4-hexadiene, ethylidene norbornene, dicyclopentadiene. Suitable olefins are vinylaromatic compounds having from 8 to 20 carbon atoms and aliphatic α-monoolefins having from 3 to 12 carbon atoms.
[0035] Suitable vinylaromatic compounds include, for example, styrene, ortho-, meta-, para-methylstyrene, the commercial mixture "vinyl-toluene", para-tert-butylstyrene.
[0036] Suitable aliphatic α-monoolefins include, in particular, acyclic aliphatic α-monoolefins having from 3 to 18 carbon atoms.
[0037] More particularly, Diene Telastomer is: a. Any homopolymer of a conjugated diene monomer, in particular any homopolymer obtained by polymerization of a conjugated diene monomer having from 4 to 12 carbon atoms; b. Any copolymer obtained by copolymerization of one or more conjugated dienes with each other or with one or more vinylaromatic compounds having from 8 to 20 carbon atoms; c. Any copolymer obtained by copolymerization of one or more dienes, conjugated or not, with ethylene, an α-monoolefin or their mixture, such as, for example, elastomers obtained from ethylene, propylene with a non-conjugated diene monomer of the aforementioned type.
[0038] By "isoprenic elastomer" is meant, in a known manner, a homopolymer or a copolymer of isoprene. In other words, an isoprene elastomer can be chosen from the group consisting of natural rubber (NR), synthetic polyisoprenes (IR), the various isoprene copolymers and the mixtures of these elastomers. Among the isoprene copolymers, mention will be made in particular of isobutene-isoprene (butyl rubber - IIR), isoprene-styrene (SIR), isoprene-butadiene (BIR) or isoprene-butadiene-styrene (SBIR) copolymers. Preferably, the isoprene elastomer can be chosen from the group consisting of natural rubber, synthetic cis-1,4 polyisoprenes, and their combinations. More more preferably still, the isoprene elastomer is chosen from the group consisting of natural rubber, synthetic polyisoprenes having a rate (mol%) of cis-1,4 bonds greater than 90% (more preferably still greater than 98%), and their combinations.
[0039] A reinforcing filler, intended to reinforce a rubber composition, may be an organic filler such as carbon black, or an inorganic filler such as silica or alumina in combination with a coupling agent between the inorganic filler and the diene elastomer, or a mixture of these types of fillers.
[0040] The crosslinking system may be any type of system known to those skilled in the art in the field of tire rubber compositions. It may in particular be based on sulfur, and / or peroxide and / or bismaleimides. Preferably, the crosslinking system is based on sulfur: this is then referred to as a vulcanization system. The sulfur may be provided in any form, in particular in the form of molecular sulfur, or a sulfur-donating agent. At least one vulcanization accelerator is also preferably present, and, optionally, also preferably, various known vulcanization activators may be used such as zinc oxide, stearic acid or an equivalent compound such as stearic acid salts and transition metal salts, guanidine derivatives (in particular diphenylguanidine), or even known vulcanization retarders.Any compound capable of acting as an accelerator for the vulcanization of diene elastomers in the presence of sulfur may be used as an accelerator, in particular accelerators of the thiazole type and their derivatives, accelerators of the sulfenamide, thiuram, dithiocarbamate, dithiophosphate, thiourea and xanthate types.
[0041] A plasticizing agent is a common processing agent, known to those skilled in the art and usually used in rubber compositions. A plasticizing agent may be chosen from the group consisting of plasticizing oils, plasticizing resins with a high glass transition temperature Tg, and combinations thereof.
[0042] Any extender oil, whether aromatic or non-aromatic in nature and known for its plasticizing properties with respect to elastomers, can be used. At room temperature (23°C), these oils, more or less viscous, are liquids (that is to say, as a reminder, substances having the capacity to eventually take the shape of their container), in contrast in particular with high Tg hydrocarbon resins which are by nature solid at room temperature. The plasticizing oil generally has a glass transition temperature Tg, less than -20°C, preferably less than -40°C. The glass transition temperature Tg of the plasticizing oil is measured according to the ASTM D3418 (2008) standard.
[0043] By definition, a high Tg hydrocarbon resin, typically at least equal to 30°C, is solid at room temperature and pressure (23°C, 1 atm), while a plasticizing oil is liquid at room temperature and a low Tg hydrocarbon resin is viscous at room temperature. Hydrocarbon resins, also called hydrocarbon plasticizing resins, are polymers well known to those skilled in the art, essentially based on carbon and hydrogen but which may contain other types of atoms, for example oxygen, which can be used in particular as plasticizing agents or tackifying agents in polymer matrices. They are by nature at least partially miscible (i.e., compatible) at the rates used with the polymer compositions for which they are intended, so as to act as true diluting agents. In a known manner, these hydrocarbon resins can also be described as thermoplastic resins in the sense that they soften upon heating and can thus be molded.The glass transition temperature Tg of the plasticizing resin is measured according to ASTM D3418 (2008).
[0044] As regards the anti-ozone waxes, they can be, for example, paraffin waxes, microcrystalline waxes or mixtures of paraffin and microcrystalline waxes. They consist of a mixture of linear alkanes and non-linear alkanes (iso-alkanes, cycloalkanes, branched alkanes) resulting from the refining of petroleum or from the catalytic hydrogenation of carbon monoxide (Fisher Tropsch process) mainly comprising chains of at least 20 carbon atoms.
[0045] The determination of the distribution of alkanes is carried out by gas chromatography coupled with a flame ionization detector ("GC-FID"). The exploitation of the chromatogram is carried out according to the EWF ("European Wax Federation") method.
[0046] All known anti-ozonating waxes can be used, including natural waxes such as, for example, candelilla wax or carnauba wax. These waxes can also be used in cutting.
[0047] Anti-ozone waxes are commercially available such as, for example, "Varazon 4959", "Varazon 6500" and "Varazon 6810" from Sasol, "Ozoace 0355" from Nippon Seiro, "Negozone 9343" from H&R and "H3841" from Yanggu Huatai.
[0048] A rubber powder (also called “crumb rubber” in English) comes in the form of granules, possibly put in the form of a rubber plate.
[0049] Most often these rubber powders come from grinding or micronizing vulcanized rubber compositions already used for a first application, for example, in a tire, shoe soles, seals. They are therefore a product of recycling these materials.
[0050] In a known manner, rubber crumb can be more particularly obtained by reducing used tires into granules from which the reinforcing materials such as steel or textile fibers have been removed.
[0051] The rubber crumbs can be prepared by cryogenic grinding of used tires, for example according to the method described in document US 7,445,170, comprising successive and independent steps of granulation, separation of the metal and textile reinforcements, cooling and micronization in order to obtain a rough distribution of micron particles of vulcanized mixture (also called microparticles). This micronization can be carried out using a conical impact crusher as described in document US 7,861,958. The cryogenized input enters the crusher (for example, CUM150 crushers from the company Netzsch or CW250 crushers from the company Alpine can be used), then is transferred by gravity to a rotor rotating at high speed. The cryogenized input is thus projected onto the walls of the rotor chamber multiple times leading to its micronization.The particles can then pass through a series of two vibrating screens of the same size in order to separate the last elements not consisting of vulcanized mixture. A rough distribution of micron particles of vulcanized mixture is obtained. By "microparticles" is meant particles which have a size, namely their diameter, in the case of spherical particles, or their largest dimension, in the case of anisometric particles, of a few tens or hundreds of microns. The size of the microparticles can be determined by techniques known to those skilled in the art such as, for example, microscopy. The rubber crumb usable in the present invention comprises in particular microparticles which have a size less than 74 μm and microparticles having a size greater than 74 μm. The distribution of the microparticles of rubber crumb is determined according to the standard ASTM D5644-01 (2013).Rubber crumb is commercially available from suppliers such as Lehigh Technology.
[0052] Rubber crumbs can be simple ground or micronised rubber, without any other treatment. However, it is also known that rubber crumbs can undergo treatment in order to modify them. This treatment can consist of a chemical modification of functionalization or devulcanization. It can also be a thermomechanical, thermochemical or biological treatment.
[0053] It should be noted that rubber crumb is not considered a reinforcing filler.
[0054] According to the invention, the level of isoprene elastomer is at least equal to 27.00% by weight, relative to the total weight of the rubber composition.
[0055] Also according to the invention the level of anti-ozone wax is at least equal to 0.60% by weight and at most equal to 1.70% by weight, relative to the total weight of the rubber composition.
[0056] Still according to the invention, a weight ratio between the rate of microparticles of rubber crumb having a size less than 74 pm and the antiozonant wax content, these contents being expressed as a percentage by weight, relative to the total weight of the rubber composition, is at least equal to 0.50.
[0057] The inventors were able to verify that the combination of the anti-ozone wax content and the weight ratio between the content of rubber crumb microparticles having a size less than 74 μm and the previous anti-ozone wax content, in particular for an elastomer matrix with the content of isoprene elastomer previously described, make it possible to obtain a satisfactory compromise between the reduction of efflorescence and the resistance to attack of the sidewall by ozone.
[0058] Advantageously, the level of isoprene elastomer is at least equal to 28.00% by weight and at most equal to 34.00% by weight, preferably at least equal to 28.50% by weight and at most equal to 34.00% by weight, relative to the total weight of the rubber composition.
[0059] Also advantageously the level of anti-ozone wax is at least equal to 0.70% by weight and at most equal to 1.68% by weight, preferably at least equal to 0.90% by weight and at most equal to 1.65% by weight, relative to the total weight of the rubber composition.
[0060] Also advantageously the weight ratio between the rate of microparticles of rubber crumb having a size less than 74 μm and the rate of antiozonating wax, these rates being expressed as a percentage by weight, relative to the total weight of the rubber composition, is at least equal to 0.65 and at most equal to 4.00, preferably at least equal to 0.70 and at most equal to 2.50.
[0061] According to an advantageous mode of distribution of the sizes of microparticles of rubber crumb, the rate of microparticles having a size less than 74 μm is at least equal to 0.90% by weight, preferably at least equal to 0.95% by weight, more preferably at least equal to 1.00% by weight, relative to the total weight of the rubber composition.
[0062] According to a first embodiment of the elastomer matrix, the isoprene elastomer is chosen from the group consisting of natural rubber, synthetic polyisoprenes, isoprene copolymers, and mixtures of these elastomers, preferably from the group consisting of natural rubber, synthetic polyisoprenes and mixtures of these elastomers.
[0063] According to a preferred variant of the first embodiment of the elastomer matrix, the isoprene elastomer is chosen from the group consisting of natural rubber, synthetic cis-1,4 polyisoprenes, preferably those having a molar rate of cis-1,4 bonds greater than 90%, preferably greater than 98%.
[0064] According to a second embodiment of the elastomer matrix, the rubber composition comprises a butadiene elastomer.
[0065] By "butadiene elastomer" is meant, in a known manner, a homopolymer or a copolymer of butadiene. In other words, a butadiene elastomer may be chosen from the group consisting of polybutadienes (BR), the various copolymers of butadiene and the mixtures of these elastomers. Among the copolymers of butadiene, mention will be made in particular of butadiene-styrene (SBR) or ethylene-butadiene (EBR) copolymers. Preferably, the butadiene elastomer may be a cis-1,4 polybutadiene; in particular a polybutadiene having a rate (mol%) of cis-1,4 bonds greater than 90%, more preferably still greater than 96%.
[0066] Advantageously, the content of butadiene elastomer is at least equal to 23.00% by weight and at most equal to 31.00% by weight, preferably at least equal to 24.00% by weight and at most equal to 30.00% by weight, more preferably at least equal to 25.00% by weight and at most equal to 29.00% by weight, relative to the total weight of the rubber composition.
[0067] According to a preferred variant of the second embodiment of the elastomer matrix, the butadiene elastomer is chosen from the group consisting of polybutadienes, butadiene copolymers, and combinations of these elastomers, more preferably is a polybutadiene, preferably a polybutadiene having a molar rate of cis-1,4 bonds greater than 90%, preferably greater than 96%.
[0068] According to an advantageous embodiment of the rubber crumb, the rubber crumb is a rubber crumb which has not undergone any modification by a treatment chosen from the group consisting of thermal, mechanical, biological and chemical treatments and their combinations.
[0069] The rubber composition previously described, with all its embodiments, is, in particular, the constituent material of the high-contrast sidewall element, integral with the sidewall and consisting of a texture comprising protuberances, in relief relative to a sidewall surface, in contact with atmospheric air, and / or cavities, hollow relative to the sidewall surface.
[0070] Advantageously, the high-contrast flank element is constituted by a texture having a first brightness L*1 at least equal to 4 and at most equal to 13.
[0071] Also advantageously any portion of flank surface adjacent to the high contrast flank element has a second brightness L*2 at least equal to L*l+10, preferably at least equal to L*l+12.
[0072] Also advantageously, any portion of flank surface adjacent to the high-contrast flank element has a second brightness L*2 at least equal to 18, preferably at least equal to 22.
[0073] According to a first and a second preferred embodiment, the high-contrast sidewall element is constituted by a texture comprising protuberances, in relief relative to a sidewall surface, in contact with atmospheric air, and / or cavities, hollow relative to the flank surface.
[0074] According to a first variant of the first preferred embodiment, the high-contrast flank element is constituted by a texture comprising strand-shaped protuberances.
[0075] According to a second variant of the first preferred embodiment, the high-contrast flank element is constituted by a texture comprising blade-shaped protuberances.
[0076] The texture of a high-contrast sidewall element, according to the first and second preferred embodiments, is most often produced by molding during the curing of the tire. The corresponding mold element, intended to produce the texture of the high-contrast sidewall element, is produced, by way of non-exhaustive examples, by machining or by laser engraving. The texture of a high-contrast sidewall element can also be produced directly on the sidewall surface of the tire after curing, for example by laser engraving. The texture is therefore made of the same material as that of the rest of the sidewall.
[0077] The texture of the high-contrast sidewall elements, comprising protrusions in the form of strands or blades, makes it possible to absorb a large portion of the incident light rays, after one or more successive reflections on the walls of the protrusions. This makes it possible to give the texture a blacker appearance and, consequently, to improve its contrast and therefore its visibility compared to any adjacent portion of the sidewall surface. Furthermore, this particular texture makes it possible to obtain a pleasant feel on the sidewall surface, of the "velvet" type. Finally, the texture used has a water-repellent and slightly hydrophobic effect. In a particular embodiment, the texture can be positioned on a surface set back from the sidewall surface, such that it is embedded in the sidewall, which has the advantage of protecting it, for example, against wear caused by the sidewall surface scraping against a pavement.
[0078] Similarly, the texture of the high-contrast sidewall elements, comprising cavities recessed relative to the sidewall surface, makes it possible to absorb a large portion of the incident light rays, after one or more successive reflections on the walls of the cavities. This specific texture has the advantage of being set back relative to the sidewall surface, which ensures the durability of said texture by protecting it against wear caused by scraping of the sidewall surface against a pavement. It also has the advantage of not disturbing the aerodynamic flow of air, in the vicinity of the sidewall surface, when the tire is rolling.
[0079] The rubber composition described within the scope of the present invention is illustrated by the following non-limiting examples.
[0080] In order to confirm the properties of the rubber composition of the present invention, twelve rubber compositions (C1, C2, C3, C4 and C5: examples according to the invention, T1: reference, and T2, T3, T4, T5, T6 and T7: comparative examples) were produced.
[0081] Each rubber composition was produced as follows: the reinforcing filler, the elastomer matrix, the anti-ozone wax, the rubber crumb when present, and the various other ingredients, for example the plasticizing agent, with the exception of the vulcanization system, were successively introduced into an internal mixer having an initial tank temperature equal to 60°C, the internal “Banbury” type mixer being filled to approximately 70% of its volume. The thermomechanical work (non-productive phase) was then carried out in a single step lasting from 3 minutes to 4 minutes, until a maximum “drop” temperature of 165°C was reached.The mixture thus obtained was recovered and cooled, then the vulcanizing agent (sulfur) and the vulcanization accelerator (N-cyclohexyl-2-benzothiazolesulfenamide) of the crosslinking system were incorporated on an external mixer (homo-finisher) at a temperature of 30°C, the whole being mixed (productive phase) for a period of more than 5 minutes and less than 12 minutes.
[0082] The rubber compositions thus obtained were then calendered in the form of sheets for the measurement of their ozone resistance properties and for the measurement of efflorescence according to the protocols below.
[0083] The measurement of the ozone resistance is carried out according to the method described below. After curing at 150°C for 40 min in a bell press, then cooling at room temperature (23°C) for one day and then baking at 77°C in air for 28 days, 10 test pieces of each of the rubber compositions to be tested are placed on a trapezoid at different elongations ranging from 10% to 100% in steps of 10% elongation. The so-called "B15" test pieces come from an MFTR plate (called Monsanto) whose two beads located at the ends are used to hold the test piece. The so-called "B15" test pieces have the following dimensions: 78.5 mm * 15 mm * l.5 mm. After 192 hours of exposure to a temperature of 38°C and an ozone level of 50 ppm (parts per hundred million), each facies is noted according to the number and depth of cracks.This subjective rating ranges from 0 to 5 (0: no cracks; 1 to 4: presence of increasingly significant and deep cracks; 5: rupture of the specimen). The average of the ratings of all deformations is used as the classification criterion. The lower the average, the better the ozone resistance performance.
[0084] The measurement of the “efflorescence” performance is carried out as follows. After an operation of cutting the plates of the vulcanized rubber compositions, 2.5 mm thick test pieces are oven-dried at 70°C for 12 hours in air. They are then oven-dried at 40°C in air for 4 weeks. After removal from the oven and exposure to room temperature (23°C) for 15 minutes, a mechanical stimulus is applied to reveal the wax efflorescence. In this case, the mechanical stimulus consists of scraping the test piece with a metal blade. The extent of the efflorescence phenomenon (white coloration of the surface) is then evaluated using a subjective scale of values that is representative of the final appearance of the samples. The values of this subjective scale that were respectively obtained for the tested samples can vary from 0 to 3, and correspond to the "efflorescence rating". These values, ranging from 0 to 3, correspond to the following aspects for the samples: 0 - No efflorescence. The scraped surface remains black. 1 - Slight efflorescence. 2 - Moderate efflorescence. 3 - Total efflorescence. The scraped surface is white.
[0085] The lower the scale value, i.e. the lower the efflorescence, the better the efflorescence performance.
[0086] The formulations of the rubber compositions (C1, C2, C3, C4, C5) are presented in Table 1 below: [Tables 1] Composition Cl C2 C3 C4 C5 Isoprene elastomer (1) (expressed as % by weight, relative to the total weight of the rubber composition) 30.64 30.64 30.64 30.57 29.18 Butadiene elastomer (2) (expressed as % by weight, relative to the total weight of the rubber composition) 27.18 27.18 27.18 27.11 25.87 Anti-ozone wax (3) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.32 1.32 1.32 1.56 1.65 Other additives (4) (expressed as % by weight, relative to the total weight of the rubber composition) 31.02 31.02 31.02 30.95 29.54 Rubber crumb 1 (5) (expressed as % by weight, relative to the total weight of the rubber composition) 9.83 (-) (-) (-) (-) Rubber crumb 2 (6) (expressed as % by weight, relative to the total weight of the rubber composition) (-) 9.83 (-) 9.81 13.76 Rubber crumb 3 (7) (expressed as % by weight, relative to the total weight of the rubber composition) (-) (-) 9,83 (-) (-) Microparticle having a size less than 74 pm in the rubber crumb (expressed in % by weight, relative to the total weight of the rubber crumb) - B 1.18 2.36 9.83 2.35 3.30 Ratio B / A 0.89 1.79 7.45 1.51 2.00 , 1. Natural rubber; 2. Cis-1,4 polybutadiene synthesized with a neodymium catalyst having a cis-1,4 bonding rate of at least 98 mol%; 3. Anti-ozone wax marketed by Sasol under the commercial reference “Vazazon 4959”; 4. Other ingredients: mixture comprising carbon black, TDAE oil marketed by H&R under the commercial reference “VivaTec 500”, ((N-(1,3-dimethylbutyl)-N-phenyl-para-phenylenediamine marketed by Flexsys under the reference “Santoflex 6-PPD”, 2,2,4-trimethyl-1,2-dihydroquinolone marketed by Lanxess; stearic acid marketed by Uniquema under the reference “Pristerene 4931”; zinc oxide: commercial quality, marketed by Umicore; N-dicyclohexyl-2-benzothiazolesulfenamide marketed by Flexsys under the reference “Santocure CBS” and sulfur; 5. Unmodified rubber crumb 1 obtained by recycling (micronization of used tires) marketed by Lehigh Technology, the percentage by weight of crumb microparticles having a particle size less than 74 pm of which is 12%, relative to the total weight of the rubber crumb microparticles, and the percentage by weight of microparticles with a particle size greater than 74 pm of which is 88%, relative to the total weight of the rubber crumb microparticles; the percentage by weight of microparticles is measured according to ASTM D5644-01 (2013); 6. Unmodified rubber crumb 2 obtained by recycling (tire micronization) marketed by Lehigh Technology, the percentage by weight of crumb microparticles having a particle size less than 74 pm of which is 24%, relative to the total weight of the rubber crumb microparticles, and the percentage by weight of microparticles with a particle size greater than 74 pm of which is 76% by weight, relative to the total weight of the rubber crumb microparticles; the percentage by weight of microparticles is measured according to ASTM D5644-01 (2013); 7. Unmodified rubber crumb 3 obtained by recycling (tire micronization) marketed by Lehigh Technology, the weight percentage of crumb microparticles having a particle size less than 74 pm of which is 100%, relative to the total weight of rubber crumb microparticles; the weight percentage of microparticles is measured according to ASTM D5644-01 (2013).
[0087] The formulations of the rubber compositions (T1, T2, T3, T4, T5, T6, T7) are presented in Table 2 below: [Tables 2] Composition Tl T2 T3 T4 T5 T6 T7 Isoprene elastomer (1) (expressed as % by weight, relative to the total weight of the rubber composition) 34.05 32.73 30.64 30.64 26.02 30.50 30.87 Butadiene elastomer (2) (expressed as % by weight, relative to the total weight of the rubber composition) 30.20 29.02 27.18 27.18 31.80 27.05 27.38 Anti-ozone wax (3) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.28 1.42 1.33 1.33 1.33 1.78 0.59 Other additives (4) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.28 1.42 1.33 1.33 1.33 1.78 0.59 Other additives (5) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.28 1.42 1.33 1.33 1.33 1.78 0.59 Other additives (6) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.28 1.42 1.33 1.33 1.33 1.78 0.59 Other additives (7) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.28 1.42 1.33 1.33 1.33 1.78 0.59 Other additives (8) (expressed as % by weight, relative to the total weight of the rubber composition) -A 1.28 1.42 1.33 1.33 relative to the total weight of the rubber composition) 34.47 33.13 31.02 31.02 31.02 30.89 31.26 Rubber crumb 1 (5) (expressed in % by weight, relative to the total weight of the rubber composition) (-) 3.70 (-) (-) (-) (-) (-) Rubber crumb 2 (6) (expressed in % by weight, relative to the total weight of the rubber composition) (-) (-) (-) (-) 9.83 9.78 9.90 Rubber crumb 4 (8) (expressed in % by weight,relative to the total weight of the rubber composition) (-) (-) 9.83 (-) (-) (-) (-) Rubber crumb 5 (9) (expressed in % by weight, relative to the total weight of the rubber composition) (-) (-) (-) 9.83 (-) (-) (-) , Microparticle having a size less than 74 pm in the rubber crumb (expressed in % by weight, relative to the total weight of the rubber composition) - B 0 0.44 0 0 2.36 2.35 2.38 Ratio B / A (-) 0.31 (-) (-) 1.77 1.32 4.03 Ingredients (1) to (6) in Table 2 are the same as those mentioned in Table 1. (8) unmodified rubber crumb 4 manufactured by Lehigh Technology Company from micronization of used tires and screening; the rubber crumb not having microparticles having a size less than 74 pm and whose percentage by weight of microparticles having a particle size greater than 74 pm and less than 180 pm is 100%, relative to the total weight of the rubber crumb microparticles; the percentage by weight of microparticles is measured according to ASTM D5644-01 (2013); (9) unmodified rubber crumb 5 manufactured by Lehigh Technology Company from tire micronization and screening; the crumb not having microparticles having a size less than 74 pm and whose weight percentage of microparticles having a particle size greater than 74 pm and less than 850 pm is 100%, relative to the total weight of the rubber crumb microparticles; the weight percentage of microparticles is measured according to ASTM D5644-01 (2013).
[0088] The results of the ozone resistance and efflorescence performance measurements are presented in Tables 3 and 4, as differences between the averages of the ratings of all deformations of each sample and the reference TL. A negative value in Tables 3 and 4 indicates an improvement in performance, either with respect to ozone resistance or efflorescence.
[0089] The results of the ozone resistance performance and bloom performance measurements for the rubber compositions (Cl, C2, C3, C4, C5) are shown in Table 3 below: [Tables3] Composition Cl C2 C3 C4 C5 Ozone resistance performance -0.1 -0.6 -0.8 -0.8 -0.4 Efflorescence performance -2 -2 -2 -1 -2
[0090] The results of the ozone resistance performance and bloom performance measurements for the rubber compositions (T1, T2, T3, T4, T5, T6, T7) are shown in Table 4 below: [Tables4] Composition Tl T2 T3 T4 T5 T6 T7 Ozone resistance performance 0 +0.1 -0.3 -0.2 -0.5 -0.9 +0.4 Efflorescence performance 0 0 0 0 0 0 -2
[0091] The results in Table 3 show that the compositions (C1, C2, C3, C4, C5) according to the invention make it possible to improve at the same time the efflorescence performance and the ozone resistance performance; compared to the reference composition T1, whereas the comparative compositions (T2, T3, T4, T5, T6, T7), according to the results in Table 4, do not show, compared to the reference composition T1, any improvement in the efflorescence performance and / or an ozone resistance performance which can be improved or degraded.
[0092] In conclusion, the rubber composition according to the invention makes it possible to obtain a sidewall having a good compromise of performance properties in terms of efflorescence and ozone resistance, which makes it possible to have a sidewall element with high contrast that is durable over time, throughout the entire service life of the tire.
[0093] The characteristics of a high-contrast flank element according to the invention are illustrated by schematic figures 1 to 5, not shown to scale: -[Fig.l]: Perspective view of a portion of a tire including a sidewall with high-contrast elements, -[Fig.2]: Half meridian section of a tire including a sidewall with a high contrast element, -[Fig.3]: Texture of a high-contrast element comprising strand-shaped protuberances, according to a first variant of the first preferred embodiment of the texture, -[Fig.4]: Texture of a high-contrast element comprising blade-shaped protrusions, according to a second variant of the first preferred embodiment of the texture, -[Fig.5]: Texture of a high contrast element comprising cavities, according to the second preferred embodiment of the texture.
[0094] [Fig.l] is a perspective view of a portion of tire 1 comprising a sidewall 2 with high-contrast elements 3. Among the high-contrast elements 3 are represented two graphic elements 31, intended to communicate information technical, commercial or legal, and an aesthetic element 32.
[0095] [Fig. 2] is a half-meridian section of a tire 1 comprising a sidewall 2 with a high-contrast element 3 consisting of a texture comprising protuberances 3, in relief relative to the surface of the sidewall 21. The protuberances 4 have the shape of strands as shown in [Fig. 3].
[0096] [Fig. 3] is a texture of a high-contrast element 3 comprising strand-shaped protrusions 4, according to a first variant of the first preferred embodiment of the texture. The strand-shaped protrusions 4, in relief relative to a flank surface, have an average height H4. By average height is meant the arithmetic mean of the heights of all the protrusions. The strand-shaped protrusions 4 are spaced apart by an average pitch P4. The strand-shaped protrusions 4, having a diameter varying over the entire height of the strand, have an average diameter D4. In the embodiment shown, the strand-shaped protrusions 4 have a diameter which decreases from a strand base, in interface with the flank surface, and a free strand top.
[0097] [Fig. 4] is a texture of a high-contrast element 3 comprising blade-shaped protrusions 5, according to a second variant of the first preferred embodiment of the texture. The blade-shaped protrusions 5, in relief relative to a flank surface, have an average height H5. By average height is meant the arithmetic mean of the heights of all the protrusions. The blade-shaped protrusions 5 are distributed according to a pitch P5. The blade-shaped protrusions 5, having a width varying over the entire height of the blade, have an average width D5. In the embodiment shown, the blade-shaped protrusions 5 have a width which decreases from a blade base, in interface with the flank surface, and a free blade top.
[0098] [Fig. 5] is a texture of a high-contrast element 3 comprising cavities 6, according to the second preferred embodiment of the texture. The cavities 6, recessed relative to a flank surface, have an average depth. By average depth, we mean the arithmetic mean of the depths of all the cavities. A cavity 6 is constituted by a cavity interior 62, formed in the thickness of the flank, and an opening 61, opening into the surface of the flank. The openings 61 on the flank surface are spaced apart by a pitch P6. The openings 61 on the flank surface have an average diameter D6. By average diameter, we mean an arithmetic mean of the diameters, not necessarily identical, of the openings on the flank surface.
Claims
Claims
1. Tire (1) for a vehicle comprising a sidewall (2) with at least one high-contrast sidewall element (3): -the high-contrast sidewall element (3) being constituted by a texture having a first brightness L*1 at least equal to 1 and at most equal to 15, -any portion of sidewall surface (21) adjacent to the high-contrast sidewall element (3), having a second brightness L*2 at least equal to L*1+5, -the sidewall (2) comprising a rubber composition based on an elastomer matrix comprising an isoprene elastomer, at least one reinforcing filler, at least one crosslinking system, at least one anti-ozone wax and at least one rubber crumb comprising microparticles having a size less than 74 μm, characterized in that the content of isoprene elastomer is at least equal to 27.00% by weight relative to the total weight of the rubber composition, in that the anti-ozone wax content is at least equal to 0,60% and at most equal to 1.70% by weight relative to the total weight of the rubber composition, and in that a weight ratio between the rate of microparticles of rubber crumb having a size less than 74 pm and the rate of anti-ozone wax, these rates being expressed as a percentage by weight relative to the total weight of the rubber composition, is at least equal to 0.50.,
2. Tire (1) according to claim 1, in which the rate of isoprene elastomer is at least equal to 28.00% by weight and at most equal to 34.00% by weight, preferably at least equal to 28.50% by weight and at most equal to 34.00% by weight, relative to the total weight of the rubber composition.
3. Tire (1) according to one of claims 1 or 2, in which the anti-ozone wax content is at least equal to 0.70% by weight and at most equal to 1.68% by weight, preferably at least equal to 0.90% by weight and at most equal to 1.65% by weight, relative to the total weight of the rubber composition.
4. Tire (1) according to any one of claims 1 to 3, in which the weight ratio between the rate of microparticles of rubber crumb having a size less than 74 pm and the rate of antiozonant wax, expressed as a percentage by weight relative to the total weight of the rubber composition, is at least equal to 0.65 and at most equal to 4.00, preferably at least equal to 0.70 and at most equal to 2.
50.
5. Tire (1) according to any one of claims 1 to 4, in which the rate of microparticles having a size less than 74 pm is at least equal to 0.90% by weight, preferably at least equal to 0.95% by weight, more preferably at least equal to 1.00% by weight, relative to the total weight of the rubber composition.
6. A tire (1) according to any one of claims 1 to 5, wherein the isoprene elastomer is selected from the group consisting of natural rubber, synthetic polyisoprenes, isoprene copolymers, and mixtures of these elastomers, preferably from the group consisting of natural rubber, synthetic polyisoprenes and mixtures of these elastomers.
7. Tire (1) according to any one of claims 1 to 6, in which the isoprene elastomer is chosen from the group consisting of natural rubber, synthetic cis-1,4 polyisoprenes, preferably those having a molar rate of cis-1,4 bonds greater than 90%, preferably greater than 98%.
8. A tire (1) according to any one of claims 1 to 7, wherein the rubber composition comprises a butadiene elastomer.
9. Tire (1) according to claim 8, in which the butadiene elastomer content is at least equal to 23.00% by weight and at most equal to 31.00% by weight, preferably at least equal to 24.00% by weight and at most equal to 30.00% by weight, more preferably at least equal to 25.00% by weight and at most equal to 29.00% by weight, relative to the total weight of the rubber composition.
10. A tire (1) according to any one of claims 8 or 9, wherein the butadiene elastomer is selected from the group consisting of polybutadienes, butadiene copolymers, and combinations of these elastomers, more preferably is a polybutadiene, preferably a polybutadiene having a molar rate of cis-1,4 bonds greater than 90%, preferably greater than 96%.
11. A tire according to any one of claims 1 to 10, wherein the rubber crumb is a rubber crumb that has not undergone any modification by a treatment selected from the group consisting of thermal, mechanical, biological and chemical treatments and their combinations.
12. Tire (1) according to any one of claims 1 to 11, in which the high-contrast sidewall element (3) is constituted by a texture having a first brightness L*1 at least equal to 4 and at most equal to 13.
13. A tire (1) according to any one of claims 1 to 12, wherein any portion of sidewall surface (21) adjacent to the high contrast sidewall element (3) has a second brightness L*2 at least equal to L*l+10, preferably at least equal to L*l+12.
14. A tire (1) according to any one of claims 1 to 13, wherein any portion of sidewall surface (21) adjacent to the high contrast sidewall element (3) has a second brightness L*2 of at least 18, preferably at least 22.
15. A tire (1) according to any one of claims 1 to 14, wherein the high-contrast sidewall element (3) is constituted by a texture comprising protuberances (4, 5), in relief relative to a sidewall surface (21), in contact with atmospheric air, and / or cavities (6), in hollow relative to the sidewall surface (21).
16. A tire (1) according to any one of claims 1 to 15, wherein the high contrast sidewall element (3) is constituted by a texture comprising strand-shaped protrusions (4).
17. A tire (1) according to any one of claims 1 to 15, wherein the high contrast sidewall element (3) is constituted by a texture comprising blade-shaped protrusions (4).
Citation Information
Patent Citations
Process and apparatus for manufacturing crumb and powder rubber
US7445170B2
Conical-shaped impact mill
US7861958B2
High-contrast tire pattern and method for producing same
WO2011036061A1
Core selection switch and optical node device
WO2020174919A1
Tyre provided with a texture on a sidewall
EP3592577B1