A tire comprising a sidewall with at least one high-contrast sidewall element
A tire sidewall composition with specific elastomer and filler ratios maintains high contrast and resists ozone degradation, addressing the issue of reduced contrast over time in tire sidewalls.
Patent Information
- Application Number
- FR2023004436
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-03
AI Technical Summary
Existing tire sidewall designs with high-contrast elements suffer from reduced contrast over time due to chemical degradation, abrasion, and aging, leading to non-homogeneous coloring and dull appearance, which is particularly noticeable in sports or prestige vehicles.
A tire sidewall composition comprising an elastomeric matrix with specific ratios of isoprene and butadiene elastomers, reinforcing filler, anti-ozone wax, rubber crumb, and plasticizing agents, which maintains a high contrast by controlling brightness differences and resisting ozone attacks.
The solution maintains a durable high contrast between the sidewall element and adjacent surfaces throughout the tire's life, enhancing visual appeal and resisting ozone-induced cracks and efflorescence.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Tire comprising a sidewall with at least one high-contrast sidewall element
[0001] The present invention relates to a tire for a vehicle, comprising a sidewall with at least one high contrast sidewall element.
[0002] A tire comprises two sidewalls, a sidewall being the portion of the tire connecting one end of the tread, intended to come into contact with a ground, to a bead, intended to be mounted on a rim.
[0003] In the following, the external surface of a sidewall, in contact with atmospheric air, is designated, more simply, by the term "sidewall surface". A sidewall surface generally comprises at least one graphic element and / or, possibly, an aesthetic element. A graphic element, usually called marking and comprising letters, numbers or symbols, is generally intended to communicate technical, commercial or legal information.
[0004] By definition, a high-contrast sidewall element refers to a sidewall surface element, consisting of a specific texture different from that of the sidewall surface, which is most often smooth. This texture gives said high-contrast sidewall element a darker appearance than that of any portion of sidewall surface adjacent to said high-contrast sidewall element, such that this high-contrast sidewall element can be visually distinguished from any portion of adjacent sidewall surface. A high-contrast sidewall element may have as its object either a graphic element or an aesthetic element, or a portion of sidewall surface surrounding said graphic or aesthetic element, which makes said graphic or aesthetic element particularly visible on the sidewall surface.
[0005] Thus, whether for the enhancement of graphic elements or aesthetic elements of the sidewall surface, there is a constant concern among tire designers to produce sidewall elements with high contrast.
[0006] The contrast between a high-contrast sidewall element and a portion of sidewall surface adjacent to said high-contrast sidewall element is due to a difference in brightness between the two areas. An adjacent surface portion, which may be smooth or have a different texture, has a brightness greater than that of the texture of said high-contrast sidewall element, i.e. it appears visually lighter. This texture is made of a rubbery material, also called a rubber composition or elastomeric composition, identical to that of the portion of sidewall in contact with atmospheric air, since this texture is integral with the sidewall.
[0007] Brightness can be quantified by luminous luminance, expressed in candela / m2, which measures the luminous flux coming from an illuminated surface that is reflected in the eye of the observer. But the relationship between luminous luminance and the visual perception of brightness is not linear and is complex. This is the reason why, on a practical level, the International Commission on Illumination (CIE) has defined the brightness L*, a parameter that characterizes the capacity of a surface to reflect light, from the luminous luminance of the light produced by a primary or secondary source, expressed in candelas per square meter (cd / m2), relative to the luminous luminance of white taken as a reference. Thus, in what follows, the brightness L* is expressed according to a scale ranging from 0 to 100 in accordance with the L*a*b* colorimetric model adopted in 1976 by the International Commission on Illumination.The value 100 represents white or total reflection and the value 0 represents black or total absorption.
[0008] To calculate the difference between a first brightness L*1 of the texture of the high-contrast flank element and a second brightness L*2 of an adjacent flank surface portion, the first brightness L*1 and the second brightness L*2 must be measured respectively using a spectro-colorimeter, for example a KONICA-MINOLTA CM 700D spectro-colorimeter. To measure the first brightness L*1 of the texture, the spectro-colorimeter is positioned on the texture and this measurement is carried out with the SCI mode (Specular Reflection Included Mode) set at an angle of 8° and with a light setting of type D65 (setting defined according to the CIE). Similarly, to measure the second brightness L*2 of an adjacent flank surface portion, the spectro-colorimeter is positioned on said flank surface portion.In order to improve the determination of this second luminosity L*2, it is possible to carry out a plurality of luminosity measurements on several adjacent portions of flank surface, then to deduce an associated average luminosity.
[0009] High contrast sidewall elements, having a brightness difference substantially lower than that of an adjacent sidewall surface portion, have been described in WO 2016005572 A1 and WO 2011036061 A1 and WO 20174919 A1
[0010] It has been observed on tire sidewall surfaces, including high contrast sidewall elements, that the contrast between the high contrast sidewall elements and any adjacent sidewall surface portion changes over time.
[0011] The evolution of the contrast, over time, results from both the evolution of the texture and that of the visual appearance of the flank surface.
[0012] The evolution of the texture can result from its fouling, its at least partial abrasion or the aging of its constituent material.
[0013] The evolution of the visual appearance of the flank surface typically results in a evolution, at least locally, of its coloring (blueing, evolution towards a dark brown color, appearance of whitish spots), an evolution of its brightness (duller appearance) or the appearance of scratches or surface cracks.
[0014] More generally, the aging of the sidewall surface is linked to the elastomeric nature of its material. As is known, common rubber compositions include diene elastomers, natural or synthetic, whose molecular chains possess carbon-carbon double bonds. These double bonds are chemically more reactive than a single carbon-carbon bond and are therefore susceptible to deterioration more or less rapidly after prolonged exposure to the atmosphere, due to known oxidation and ozonolysis mechanisms. The action of ozone promotes the formation of cracks on the sidewall surface. These degradation mechanisms are further accelerated by the action of heat (thermo-oxidation) or by that of light (photo-oxidation).
[0015] To overcome the chemical degradation of the rubber composition by ozone, it is known to use anti-ozone agents, such as, for example, anti-ozone waxes. These anti-ozone waxes provide static protection by forming a protective coating on the surface. However, these anti-ozone waxes are characterized by their ability to migrate to the sidewall surface and to crystallize, which modifies the visual appearance of the sidewall surface, causing the appearance of stains or giving the sidewall a dull and gray appearance, or even causing a lighter coloring of the sidewall. This phenomenon is called "blooming". This phenomenon thus causes a non-uniform coloring and makes the sidewall surface, initially black and shiny, gray and dull.
[0016] Thus, a non-uniform coloring of the sidewall surface reduces the contrast effect of the high-contrast element and alters the visual and aesthetic appearance of the sidewall.
[0017] It therefore proves necessary, in order to obtain a sidewall element with high contrast that lasts throughout the life of the tire, to be able to reduce, or even eliminate, the alteration of the color and / or the brightness of the sidewall surface of the tire, while giving it a good capacity to resist ozone attacks that initiate cracks on the sidewall surface.
[0018] Increasing the durability of contrast is indeed an important commercial issue for a tire manufacturer. For example, when a user replaces only the tires mounted on the front of their vehicle, they may notice a significant difference in contrast between the new tires mounted on the front and the worn tires mounted on the rear. This difference in contrast between the front and rear tires may be considered unacceptable by the user, especially if their vehicle is a sports or luxury vehicle.
[0019] The inventors therefore set themselves the objective, for a tire comprising a sidewall with at least one high-contrast sidewall element, of increasing the durability over time of the contrast between said high-contrast sidewall element and the adjacent surface portion of the sidewall, using a suitable rubber composition of the sidewall, in particular close to the sidewall surface.
[0020] This objective has been achieved by a tire for a vehicle, comprising a sidewall with at least one high-contrast sidewall element: - the high contrast flank element being constituted by a texture having a first brightness L*1 at least equal to 1 and at most equal to 15, - any portion of flank surface adjacent to the high-contrast flank element, having a second brightness L*2 at least equal to L*l+5, -the sidewall comprising a rubber composition based on an elastomer matrix, at least one reinforcing filler, at least one crosslinking system, at least one plasticizing agent, at least one ozone-resistant wax and at least one rubber powder, -the elastomeric matrix comprising an isoprenoid elastomer at a rate of at least 35% and at most 65% and a butadiene elastomer at a rate of at least 35% and at most 65%, -the rate of reinforcing filler being at least equal to 5 pc and at most equal to 70 pc, -the rate of anti-ozone wax being at least equal to 1 pc and at most equal to 3 pc -and the rate of rubber powder being at least equal to 2 pc and at most equal to 30 pc.
[0021] According to the invention, the high-contrast flank element is constituted by a texture having a first brightness L*1 at least equal to 1 and at most equal to 15.
[0022] The lower the brightness of the high-contrast sidewall element in the new condition of the tire, the greater the contrast for a given brightness of an adjacent sidewall surface portion, and the more significant this contrast will remain over time on the aged tire. Indeed, over time, this first brightness L*1 of the texture of the high-contrast sidewall element tends to increase due, for example, to dust, dirt, or aging of the material. Furthermore, in this brightness range, there is good contrast with any adjacent sidewall surface portion, which, in conventional tire designs, has a brightness most often between 24 and 28. It should be noted that a texture with a first brightness L*1, typically at least equal to 9, is easier to produce, but the contrast is low.
[0023] According to the invention, any portion of flank surface adjacent to the high-contrast flank element has a second brightness L*2 at least equal to L*l+5.
[0024] The greater the difference in brightness between the high-contrast flanking element and any portion of The larger the adjacent sidewall surface, the greater the contrast. The greater this brightness difference is on the new tire, the more significant it will remain over time on the aged tire.
[0025] Also according to the invention, the sidewall comprises a rubber composition based on an elastomer matrix, at least one reinforcing filler, at least one crosslinking system, at least one plasticizing agent, at least one anti-ozone wax and at least one rubber powder.
[0026] The expression "rubber composition based on" means a rubber composition comprising the mixture and / or the in situ reaction product of the different constituents used, some of these constituents being able to react and / or intended to react with each other, at least partially, during the different phases of manufacturing the rubber composition, the rubber composition thus being able to be in a totally or partially crosslinked state or in a non-crosslinked state.
[0027] A rubber composition comprises at least one and often several elastomers, in particular several diene elastomers. This mixture of elastomers, particularly diene elastomers, is called an elastomer matrix. Preferably, the elastomer matrix comprises at least two different diene elastomers.
[0028] The term "elastomer" means a polymer, i.e. a homopolymer or a copolymer, having elastic properties obtained after crosslinking. The term rubber is a common synonym for elastomer.
[0029] By "diene elastomer" or indistinctly "diene rubber", whether natural or synthetic, is meant an elastomer consisting at least in part of diene monomer units (monomers carrying two carbon-carbon double bonds, conjugated or not). Diene elastomers are non-thermoplastic.
[0030] Diene elastomers can be classified into two categories: “essentially unsaturated” diene elastomers and “essentially saturated” diene elastomers. An “essentially unsaturated” diene elastomer is a diene elastomer derived at least in part from conjugated diene monomers, having a content of units or patterns of diene origin (conjugated dienes) which is greater than 15% (mol %). Thus, diene elastomers such as butyl rubbers or copolymers of dienes and alpha-olefins such as EPDM do not fall within the preceding definition and can be described in particular as “essentially saturated” diene elastomers (low or very low content of patterns of diene origin, always less than 15%).
[0031] The term diene elastomer capable of being used in the rubber compositions in accordance with the invention is particularly understood to mean: a. Any homopolymer of a diene monomer, conjugated or not, having from 4 to 18 carbon atoms; b. Any copolymer of a diene, conjugated or not, having from 4 to 18 carbon atoms and at least one other monomer; the other being ethylene, an olefin or a diene, conjugated or not.
[0032] Suitable conjugated dienes are conjugated dienes having from 4 to 12 carbon atoms, in particular 1,3-dienes, such as in particular 1,3-butadiene and isoprene.
[0033] Suitable as unconjugated dienes are unconjugated dienes having 6 to 12 carbon atoms, such as 1,4-hexadiene, ethylidene norbomene, dicyclo-pentadiene. Suitable olefins are vinylaromatic compounds having from 8 to 20 carbon atoms and aliphatic α-monoolefins having from 3 to 12 carbon atoms.
[0035] Suitable examples of vinylaromatic compounds include styrene, ortho-, meta-, para-methylstyrene, the commercial "vinyl-toluene" mixture, para-tert-butylstyrene.
[0036] As aliphatic α-monoolefins, acyclic aliphatic α-monoolefins having from 3 to 18 carbon atoms are particularly suitable.
[0037] More specifically, the diene elastomer is: a. Any homopolymer of a conjugated diene monomer, in particular any homopolymer obtained by polymerization of a conjugated diene monomer having 4 to 12 carbon atoms; b. Any copolymer obtained by copolymerization of one or more conjugated dienes with each other or with one or more vinylaromatic compounds having from 8 to 20 carbon atoms; c. Any copolymer obtained by copolymerization of one or more dienes, conjugated or not, with ethylene, an α-monoolefin or their mixture, such as, for example, elastomers obtained from ethylene, propylene with a non-conjugated diene monomer of the aforementioned type.
[0038] A reinforcing filler, intended to reinforce a rubber composition, may be an organic filler such as carbon black, or an inorganic filler such as silica or alumina in combination with a coupling agent between the inorganic filler and the diene elastomer, or a mixture of these types of fillers.
[0039] The crosslinking system may be any type of system known to those skilled in the art in the field of tire rubber compositions. It may in particular be based on sulfur, and / or peroxide and / or bismaleimides. Preferably, the crosslinking system is based on sulfur: this is then referred to as a vulcanization system. The sulfur may be provided in any form, in particular in the form of molecular sulfur, or a sulfur-donating agent. At least one vulcanization accelerator canization is also preferentially present, and, optionally, also preferentially, various known vulcanization activators may be used such as zinc oxide, stearic acid or an equivalent compound such as stearic acid salts and transition metal salts, guanidine derivatives (in particular diphenylguanidine), or known vulcanization retarders. Any compound capable of acting as a vulcanization accelerator of diene elastomers in the presence of sulfur may be used as an accelerator, in particular accelerators of the thiazole type and their derivatives, accelerators of the sulfenamide, thiuram, dithiocarbamate, dithiophosphate, thiourea and xanthate types.
[0040] A plasticizing agent is a common processing agent, known to those skilled in the art and usually used in rubber compositions. A plasticizing agent may be selected from the group consisting of plasticizing oils, high-temperature glass transition (Tg) plasticizing resins, and combinations thereof.
[0041] Any extender oil, whether aromatic or non-aromatic in nature and known for its plasticizing properties with respect to elastomers, can be used. At room temperature (23°C), these oils, more or less viscous, are liquids (that is to say, as a reminder, substances having the capacity to eventually take the shape of their container), in contrast in particular to high Tg hydrocarbon resins which are by nature solid at room temperature. The plasticizing oil generally has a glass transition temperature Tg, less than -20°C, preferably less than -40°C. The glass transition temperature Tg of the plasticizing oil is measured according to the ASTM D3418 (2008) standard.
[0042] By definition, a high Tg hydrocarbon resin, typically at least equal to 30°C, is solid at room temperature and pressure (23°C, 1 atm), while a plasticizing oil is liquid at room temperature and a low Tg hydrocarbon resin is viscous at room temperature. Hydrocarbon resins, also called hydrocarbon plasticizing resins, are polymers well known to those skilled in the art, essentially based on carbon and hydrogen but which may contain other types of atoms, for example oxygen, which can be used in particular as plasticizing agents or tackifying agents in polymer matrices. They are by nature at least partially miscible (i.e., compatible) at the rates used with the polymer compositions for which they are intended, so as to act as true diluting agents.As is known, these hydrocarbon resins can also be referred to as thermoplastic resins in that they soften upon heating and can thus be molded. The glass transition temperature Tg of the plasticizing resin is measured according to ASTM D3418 (2008).
[0043] As regards the anti-ozone waxes, they can be, for example, paraffin waxes, microcrystalline waxes or mixtures of paraffin and microcrystalline waxes. crystalline. They consist of a mixture of linear alkanes and non-linear alkanes (isoalkanes, cycloalkanes, branched alkanes) resulting from petroleum refining or the catalytic hydrogenation of carbon monoxide (Fisher Tropsch process) mainly comprising chains of at least 20 carbon atoms.
[0044] The determination of the distribution of alkanes is carried out by gas chromatography coupled with a flame ionization detector ("GC-FID"). The exploitation of the chromatogram is carried out according to the EWF ("European Wax Federation") method.
[0045] All known anti-ozonating waxes can be used, including natural waxes such as, for example, candelilla wax or carnauba wax. These waxes can also be used in cutting.
[0046] Anti-ozone waxes are commercially available such as, for example, "Varazon 4959", "Varazon 6500" and "Varazon 6810" from Sasol, "Ozoace 0355" from Nippon Seiro, "Negozone 9343" from H&R and "H3841" from Yanggu Huatai.
[0047] A rubber powder (also called “crumb rubber” in English) comes in the form of granules, possibly put in the form of a rubber plate.
[0048] Most often these rubber powders come from grinding or micronizing vulcanized rubber compositions already used for a first application, for example, in a tire, shoe soles, seals. They are therefore a product of recycling these materials.
[0049] In a known manner, rubber crumb can be obtained more particularly by reducing used tires into granules from which the reinforcing materials such as steel or textile fibers have been removed.
[0050] The rubber crumbs can be prepared by cryogenic grinding of used tires, for example according to the method described in document US 7,445,170, comprising successive and independent steps of granulation, separation of the metal and textile reinforcements, cooling and micronization in order to obtain a rough distribution of micron particles of vulcanized mixture (also called microparticles). This micronization can be carried out using a conical impact crusher as described in document US 7,861,958. The cryogenized input enters the crusher (for example, CUM150 crushers from the company Netzsch or CW250 crushers from the company Alpine can be used), then is transferred by gravity to a rotor rotating at high speed. The cryogenized input is thus projected onto the walls of the rotor chamber multiple times leading to its micronization.The particles may then pass through a series of two vibrating screens of the same size to separate the remaining non-vulcanized compound particles. A rough distribution of micron-sized vulcanized compound particles is obtained. By "microparticles" we mean particles that have a size, at . namely their diameter, in the case of spherical particles, or their largest dimension, in the case of anisometric particles, of a few tens or hundreds of microns. The size of the microparticles can be determined by techniques known to those skilled in the art such as, for example, microscopy.
[0051] Rubber crumbs can be simple ground or micronised rubber, without any other treatment. However, it is also known that rubber crumbs can undergo treatment in order to modify them. This treatment can consist of a chemical modification of functionalization or devulcanization. It can also be a thermomechanical, thermochemical or biological treatment.
[0052] According to the invention, the elastomer matrix comprises an isoprene elastomer at a rate at least equal to 35 pce and at most equal to 65 pce and a butadiene elastomer at a rate at least equal to 35 pce and at most equal to 65 pce.
[0053] By "isoprenic elastomer" is meant, in a known manner, a homopolymer or a copolymer of isoprene. In other words, an isoprene elastomer can be chosen from the group consisting of natural rubber (NR), synthetic polyisoprenes (IR), the various isoprene copolymers and the mixtures of these elastomers. Among the isoprene copolymers, mention will be made in particular of isobutene-isoprene (butyl rubber - IIR), isoprene-styrene (SIR), isoprene-butadiene (BIR) or isoprene-butadiene-styrene (SBIR) copolymers. Preferably, the isoprene elastomer can be chosen from the group consisting of natural rubber, synthetic cis-1,4 polyisoprenes, and combinations thereof.Even more preferably, the isoprene elastomer is chosen from the group consisting of natural rubber, synthetic polyisoprenes having a rate (mol%) of cis-1,4 bonds greater than 90% (even more preferably greater than 98%), and their combinations.
[0054] By "butadiene elastomer" is meant, in a known manner, a homopolymer or a copolymer of butadiene. In other words, a butadiene elastomer may be chosen from the group consisting of polybutadienes (BR), the various copolymers of butadiene and the mixtures of these elastomers. Among the copolymers of butadiene, mention will be made in particular of butadiene-styrene (SBR) or ethylene-butadiene (EBR) copolymers. Preferably, the butadiene elastomer may be a cis-1,4 polybutadiene; in particular a polybutadiene having a rate (mol%) of cis-1,4 bonds greater than 90%, more preferably still greater than 96%.
[0055] The unit "pce" or "parts per hundred of elastomer" represents the part by mass per hundred parts by mass of elastomer or rubber. In English, this unit is translated as "phr" ("parts per hundred of rubber"). The elastomers in the rubber crumb are excluded from the mass of elastomer in reference.
[0056] According to the invention, the reinforcing load ratio is at least equal to 5 parts per unit area and at most equal to 70 pce.
[0057] According to the invention, the rate of anti-ozone wax is at least equal to 1 pc and at most equal to 3 pc.
[0058] According to the invention, the proportion of rubber powder is at least equal to 2 pc and at most equal to 30 pc.
[0059] The inventors were able to verify that the combination of the respective previous levels of reinforcing filler, anti-ozone wax and rubber powder, for an elastomer matrix with the respective levels of isoprene elastomer and butadiene elastomer previously described, make it possible to obtain a satisfactory compromise between the reduction of efflorescence and the resistance to attack of the sidewall by ozone.
[0060] Advantageously, the anti-ozone wax content is at least equal to 1.2 pce and at most equal to 2.8 pce, preferably at least equal to 1.4 pce and at most equal to 2.6 pce and more preferably at least equal to 1.6 pce and at most equal to 2.4 pce.
[0061] Also advantageously the rubber powder content is at least equal to 5 pce and at most equal to 20 pce, preferably at least equal to 5.5 pce and at most equal to 19.5 pce, more preferably at least equal to 6 pce and at most equal to 19 pce and even more preferably at least equal to 6 pce and at most equal to 18 pce.
[0062] It should be noted that, within the meaning of the present invention, the rubber crumb is not considered to be a reinforcing filler. Consequently, the level of the rubber crumb is not included in the level of the reinforcing filler.
[0063] Advantageously, the rubber powder has a microparticle size distribution such that it comprises less than 1% by mass of particles not retained through a 600 µm sieve and less than 10% by mass of microparticles not retained through a 105 µm sieve, relative to the total mass of microparticles in the powder. Preferably, it has a microparticle size distribution such that it comprises less than 1% by mass of microparticles not retained through a 600 µm sieve and less than 10% by mass of microparticles not retained through a 149 µm sieve, relative to the total mass of microparticles in the rubber powder.More preferably, it has a microparticle size distribution such that it comprises less than 1% by mass of microparticles not retained through a 600 μm sieve and less than 10% by mass of microparticles not retained through a 177 μm sieve, relative to the total mass of microparticles in the rubber crumb. Even more preferably, it has a microparticle size distribution such that it comprises less than 1% by mass of microparticles not retained through a 400 μm sieve and less than 10% by mass of microparticles not retained through a 177 μm sieve relative to the total mass of microparticles in the rubber crumb. The distribution of microparticles in rubber crumb is de- . completed according to ASTM D5644-01 (2013).
[0064] To obtain such a rubber crumb having such distributions, an additional sieving step according to a size criterion was carried out. The sieving can be carried out by different technologies (vibration, centrifugation, suction) known to those skilled in the art. Preferably, this sieving step is carried out using a series of sieves stacked in order of size (sieves with calibrated mesh sizes such as the commercial products of the Gericke company, for example). Thus, the largest particles are retained on the sieve while the smallest pass to the lower stage on the next sieve. Those skilled in the art will understand that the distributions considered subsequently can be composed of all the particles passing a given sieve or all the particles retained between 2 stages.
[0065] Advantageously, the rubber crumb is a rubber crumb that has not undergone any modification by a treatment chosen from the group consisting of thermal, mechanical, biological and chemical treatments and their combinations.
[0066] Also advantageously the ratio between the rubber powder content, expressed in pce, and the anti-ozone wax content, expressed in pce, is at least equal to 5.50 and at most equal to 17.00, preferably at least equal to 6.00 and at most equal to 17.00 and more preferably at least equal to 6.50 and at most equal to 12.50.
[0067] Preferably the rate of reinforcing filler is at least equal to 10 pce and at most equal to 60 pce, preferably at least equal to 15 pce and at most equal to 55 pce, more preferably at least equal to 15 pce and at most equal to 50 pce and even more preferably at least equal to 15 pce and at most equal to 45 pce.
[0068] Advantageously, the sum of the reinforcing filler content and the rubber crumb content is at least equal to 30 pce and at most equal to 65 pce, preferably at least equal to 30 pce and at most equal to 60 pce and more preferably at least equal to 35 pce and at most equal to 50 pce.
[0069] Preferably the reinforcing filler consists mainly of carbon black.
[0070] When reference is made to a "major" compound, this means, for the purposes of the present invention, that this compound is the majority among the compounds of the same type in the composition; that is to say, it is the one that represents the greatest quantity by weight among the compounds of the same type, and preferably more than 50% by weight, more preferably more than 75% by weight. Thus, a "major" filler is the one that represents the greatest weight among the fillers in the composition.
[0071] Advantageously, the ratio between the level of reinforcing filler, expressed in pce, and the level of plasticizing agent, expressed in pce, is at least equal to 1.00 and at most equal to 5.00, preferably at least equal to 1.50 and at most equal to 4.50, more preferably at least equal to 1.00 and at most equal to 1.50. less than 2.00 and at most 4.00 and even more preferably at least 2.00 and at most 3.50.
[0072] When the plasticizing agent is a mixture of a hydrocarbon resin and an oil, the plasticizer content is the sum of the hydrocarbon resin content in pce and the oil content in pce, for the calculation of the ratio described above.
[0073] Advantageously, the at least one plasticizing agent of the rubber composition is chosen from the group consisting of plasticizing oils, plasticizing resins with a high glass transition temperature Tg, and combinations thereof.
[0074] The rubber composition described above, with all its embodiments, is, in particular, the constituent material of the high contrast sidewall element, made of material with the sidewall and consisting of a texture having a first brightness L*1 at least equal to 1 and at most equal to 15, any portion of sidewall surface adjacent to the high contrast sidewall element, having a second brightness L*2 at least equal to L*1+5.
[0075] Advantageously, the high-contrast flank element is constituted by a texture having a first brightness L*1 at least equal to 4 and at most equal to 13.
[0076] Also advantageously any portion of flank surface adjacent to the high contrast flank element has a second brightness L*2 at least equal to L*l+10, preferably at least equal to L*l+12.
[0077] Also advantageously, any portion of flank surface adjacent to the high-contrast flank element has a second brightness L*2 at least equal to 18, preferably at least equal to 22.
[0078] According to a first and a second preferred embodiment, the high-contrast sidewall element is constituted by a texture comprising protuberances, in relief relative to a sidewall surface, in contact with atmospheric air, and / or cavities, hollow relative to the sidewall surface.
[0079] According to a first variant of the first preferred embodiment, the high-contrast flank element is constituted by a texture comprising strand-shaped protuberances.
[0080] According to a second variant of the first preferred embodiment, the high-contrast flank element is constituted by a texture comprising blade-shaped protuberances.
[0081] The texture of a high-contrast sidewall element, according to the first and second preferred embodiments, is most often produced by molding during the tire curing process. The corresponding mold element, intended to produce the texture of the high-contrast sidewall element, is produced, by way of non-exhaustive examples, by machining or laser engraving. The texture of a high-contrast sidewall element can also be produced directly on the tire sidewall surface after cooking, for example by laser engraving. The texture is therefore made of the same material as the rest of the side.
[0082] The texture of the high-contrast side elements, comprising strand- or blade-shaped protrusions, absorbs a large portion of the incident light rays after one or more successive reflections off the walls of the protrusions. This gives the texture a darker appearance and, consequently, improves its contrast and therefore its visibility compared to any adjacent portion of the side surface. Furthermore, this particular texture provides a pleasant, velvety feel to the side surface. Finally, the texture has a water-repellent and slightly hydrophobic effect. In one particular embodiment, the texture can be positioned on a surface recessed from the side surface, so that it is embedded in the side, which has the advantage of protecting it, for example, against wear caused by the side surface rubbing against a curb.
[0083] Similarly, the texture of the high-contrast sidewall elements, comprising recesses relative to the sidewall surface, allows for the absorption of a large portion of the incident light rays after one or more successive reflections off the cavity walls. This specific texture has the advantage of being recessed relative to the sidewall surface, which ensures the durability of said texture by protecting it against wear caused by the sidewall surface rubbing against a curb. It also has the advantage of not disrupting the aerodynamic airflow near the sidewall surface during tire rolling.
[0084] The rubber composition described in the context of the present invention is illustrated by the following non-limiting examples.
[0085] In order to confirm the properties of the rubber composition of the present invention, ten rubber compositions (C1, C2, C3, C4 and C5: examples according to the invention, T1 and T3: references, and T2, T4 and T5: comparative examples) were used. Each of the formulations of the rubber compositions is presented in Tables 1 and 3 with the amounts of the various ingredients expressed in phr.
[0086] Each rubber composition was produced as follows: the reinforcing filler, the elastomer matrix, the ozone-blocking wax, the rubber powder (when present), the plasticizing agent, and the various other ingredients, with the exception of the vulcanizing system, were successively introduced into an internal mixer with an initial tank temperature of 60°C, the Banbury-type internal mixer being filled to approximately 70% of its volume. The thermomechanical work (non-productive phase) was then carried out in a single step lasting 3 to 4 minutes, until a maximum "drop" temperature was reached. of 165°C is reached. The mixture thus obtained was recovered and cooled, then the vulcanizing agent (sulfur) and the vulcanization accelerator (N-cyclohexyl-2-benzothiazolesulfenamide) of the crosslinking system were incorporated on an external mixer (homo-finisher) at a temperature of 30°C, the whole being mixed (productive phase) for a period of more than 5 minutes and less than 12 minutes.
[0087] The rubber compositions thus obtained were then calendered into sheets for the measurement of their ozone resistance properties and for the measurement of efflorescence according to the protocols below.
[0088] Concerning the measurement of ozone resistance, it is carried out according to the method described below. After curing at 150°C for 40 min in a bell press, then cooling at room temperature (23°C) for one day and then baking at 77°C in air for 28 days, 10 test pieces of each of the rubber compositions to be tested are placed on a trapezoid at different elongations ranging from 10% to 100% in steps of 10% elongation. The so-called "B15" test pieces come from an MFTR plate (called Monsanto) whose two beads located at the ends are used to hold the test piece. The so-called "B15" test pieces have the following dimensions: 78.5 mm * 15 mm * l.5 mm. After 192 hours of exposure to a temperature of 38°C and an ozone level of 50 ppm (parts per hundred million), each facies is noted according to the number and depth of the cracks.This subjective rating ranges from 0 to 5 (0: no cracks; 1 to 4: presence of increasingly significant and deep cracks; 5: rupture of the specimen). The average of the ratings of all deformations is used as the classification criterion. The lower the average, the better the ozone resistance performance.
[0089] The differences between the means of the notations of all the deformations of each sample (T2 and Cl to C3) and the reference (Tl) are presented in Table 2.
[0090] Similarly, Table 4 presents the differences between the averages of the ratings of all the deformations of each sample (T4, T5, C4 and C5) and the reference (T3)
[0091] A negative value in Tables 2 and 4 indicates an improvement in ozone resistance performance compared to the control reference T1 for Table 2 and the control reference T3 for Table 4.
[0092] The measurement of the “efflorescence” performance is carried out as follows. After a cutting operation of the plates of vulcanized rubber compositions, test pieces of thickness 2.5 mm are oven-dried at 70°C for 12 hours in air. They are then oven-dried at 40°C in air for 4 weeks. After removal from the oven and exposure to room temperature (23°C) for 15 min, a mechanical stimulus is applied in such a way as to reveal the efflorescence of the wax. In this case, the mechanical stimulus consists of scraping the test piece with a metal blade. The extent of the efflorescence phenomenon (white coloration of the surface) is then assessed using a subjective scale of values that is representative of the final appearance of the samples. The values of this subjective scale that were respectively obtained for the tested samples can vary from 0 to 3, and correspond to the “efflorescence rating”. These values, ranging from 0 to 3, correspond to the following aspects for the samples: 0 - No efflorescence. The scraped surface remains black. 1 - Slight efflorescence. 2 - Moderate efflorescence. 3 - Total efflorescence. The scraped surface is white.
[0093] The lower the scale value, i.e. the lower the efflorescence, the better the efflorescence performance.
[0094] The differences between the efflorescence values of each sample (T2 and C1 to C3) and the reference (T1) are presented in Table 2. Similarly, Table 4 presents the differences between the efflorescence values of each sample (T4, T5, C4 and C5) and the reference (T3). A negative value in Tables 2 and 4 indicates an improvement in efflorescence performance compared to each reference (T1, T3) respectively.
[0095] In the example of test 1, a rubber composition for a sidewall having a reference rubber composition (T1), not comprising rubber crumb, and compositions T2 (comparative) and C1 to C3 (according to the invention), as defined in table 1 below, is compared: [Tables 1] Composition Tl T2 Cl C2 C3 Isoprene elastomer (1) 35 60 60 60 60 Butadiene elastomer (2) 65 40 40 40 40 Reinforcing filler (3) 50 32 32 32 32 Rubber powder (4) (-) (-) 17 (-) (-) Rubber powder (5) (-) (-) (-) 17 (-) Rubber powder (6) (-) (-) (-) (-) 17 Anti-ozone wax (7) 2.0 2.0 2.3 2.3 2.3 Liquid plasticizer (8) 17.5 10 10 10 2 Plasticizer resin (9) (-) (-) (-) (-) 8 Antioxidant (10) 5.4 5.4 6.1 6.1 6.1 Stearic acid (11) 1.1 1.1 1.1 1.1 1.1 Zinc oxide (12) 2.5 2.5 2.5 2.5 2.5 Vulcanization accelerator (13) 1.5 1.5 1.7 1.7 1.7 Sulfur 1.5 1.5 1.7 1.7 1.7 1. Natural rubber; 2. Cis-1,4 polybutadiene synthesized with a neodymium catalyst having a cis-1,4 bonding ratio of at least 98 mol%; 3. Carbon black grade ASTM N550 according to ASTM D1765-14 having an STSA measured according to ASTM D6556-10 standard equal to 39 m2 / g, a CO AN index measured according to ASTM D3493-16 standard equal to 85 ml / 100g; 4. Rubber powder obtained by recycling (micronization of pneumatic), rubber powder marketed by Lehigh Technology of which the percentage of powder microparticles measured according to ASTM D5644-01 (2013) retained by a 400 pm sieve is less than 1% by weight and of which the percentage of powder particles retained by a 250 pm sieve is less than 12% by weight relative to the total weight of rubber powder particles, unmodified rubber powder; 5. Rubber crumb obtained by recycling (tire micronization), rubber crumb marketed by Lehigh Technology whose percentage of crumb microparticles measured according to standard ASTM D5644-01 (2013) retained by a 250 pm sieve is less than 1% by weight and of which the percentage of powder particles retained by a 177 pm sieve is less than 10% by weight relative to the total weight of rubber powder particles, unmodified rubber powder; 6. Rubber crumb obtained by recycling (tire micronization), rubber crumb marketed by Lehigh Technology whose percentage of crumb microparticles measured according to ASTM D5644-01 (2013) retained by a 600 pm sieve is less than 1% by weight and whose percentage of crumb particles retained by a 400 pm sieve is less than 12% by weight relative to the total weight of the rubber crumb particles, unmodified rubber crumb; 7. Anti-ozone wax marketed by Sasol under the commercial reference "Vazazon 4959"; 8. TDAE oil marketed by H&R under the commercial reference "VivaTec 500"; 9. C5 plasticizing hydrocarbon resin marketed by Exxon under the trade name "Escorez 1102"; 10. Mixture of 2 antioxidants: ((N-(l,3-dimethylbutyl) -N-phenyl-para-phenylenediamine marketed by Flexsys under the reference "Santaflex 6-PPD" and 2,2,4-trimethyl-l,2-dihydroquinolone marketed by Lanxess; 11. Stearic acid marketed by Uniquema under the reference "Pristerene 4931"; 12. Zinc oxide: commercial grade, marketed by Umicore; 13. N-dicyclohexyl-2-benzothiazolesulfenamide marketed by Flexsys under the reference “Sancure CBS”.
[0096] The performance results are presented in Table 2 below: [Tables2] Composition Tl T2 Cl C2 C3 Ozone resistance performance 0 -0.8 -0.3 -0.3 -0.1 Efflorescence performance 0 0 -2 -2 -2
[0097] The results in Table 2 show that only the rubber compositions C1, C2 and C3 according to the invention simultaneously exhibit better efflorescence performance and better ozone resistance performance, compared respectively to the reference rubber composition (T1) and to the com- rubber position of the comparative example (T2).
[0098] In the example of test 2, a rubber composition for a sidewall comprising a reference rubber composition (T3), not comprising rubber crumb, and compositions T4 and T5 (comparative) and C4 to C5 (according to the invention), as defined in table 3 below, is compared: [Tables 3] Composition T3 T4 T5 C4 C5 Isoprene elastomer (1) 53 53 53 53 53 Butadiene elastomer (2) 47 47 47 47 47 Reinforcing filler (3) 29 29 29 29 29 Rubber powder (4) (-) (-) (-) (-) (-) Rubber powder (5) (-) 17 17 17 (-) Rubber powder (6) (-) (-) (-) (-) 17 Anti-ozone wax (7) 2.0 1.0 3.1 2.3 2.3 Liquid plasticizer (8) 12 12 12 12 212 Plasticizer resin (9) (-) (-) (-) (-) (-) Antioxidant (10) 5.7 5.7 5.7 5.7 5.7 Stearic acid (11) 1.1 1.1 1.1 1.1 1.1 Zinc oxide (12) 2.5 2.5 2.5 2.5 2.5 Vulcanization accelerator (13) 1.7 1.7 1.7 1.7 1.7 Sulfur (14) 1.7 1.7 1.7 1.7 1.7 The ingredients in Table 3 are the same as those mentioned in Table 1.
[0099] The performances obtained are presented in table 4 below: [Tables4] Composition T3 T4 T5 C4 C5 Ozone resistance performance 0 +0.4 -0.9 -0.6 -0.1 Efflorescence performance 0 -2 0 -2 -2
[0100] The results in Table 4 also show that the examples (C4 and C5) according to the invention simultaneously exhibit better efflorescence performance and better ozone resistance performance than the reference rubber composition (T3) and the comparative rubber compositions (T4 and T5).
[0101] In conclusion, the rubber composition according to the invention makes it possible to obtain a sidewall exhibiting a good compromise of performance properties in terms of efflorescence and resistance to ozone, which makes it possible to have a sidewall element with high contrast that lasts over time, throughout the life of the tire.
[0102] The characteristics of a high-contrast flank element according to the invention are illustrated by schematic figures 1 to 5, not shown to scale: -[Fig.l]: Perspective view of a portion of a tire including a sidewall with high-contrast elements, -[Fig.2]: Half meridian section of a tire including a sidewall with a high contrast element, -[Fig.3]: Texture of a high-contrast element comprising strand-shaped protuberances, according to a first variant of the first preferred embodiment of the texture, -[Fig.4]: Texture of a high-contrast element comprising blade-shaped protrusions, according to a second variant of the first preferred embodiment of the texture, -[Fig.5]: Texture of a high contrast element comprising cavities, according to the second preferred embodiment of the texture.
[0103] Fig. 1 is a perspective view of a portion of a tire 1 comprising a sidewall 2 with high-contrast elements 3. Among the high-contrast elements 3 are two graphic elements 31, intended to communicate technical, commercial or legal information, and one aesthetic element 32.
[0104] [Fig.2] is a meridional half-section of a tire 1 comprising a sidewall 2 with a high-contrast element 3 consisting of a texture comprising protrusions 3, raised in relief from the surface of the sidewall 21. The protrusions 4 have a strand-like shape as shown in [Fig.3].
[0105] Figure 3 is a texture of a high-contrast element 3 comprising strand-shaped protrusions 4, according to a first variant of the first preferred embodiment of the texture. The strand-shaped protrusions 4, raised against a flank surface, have an average height H4. Average height is understood to be the arithmetic mean of the heights of all the protrusions. The strand-shaped protrusions 4 are spaced at an average pitch P4. The strand-shaped protrusions 4, having a diameter that varies along the entire height of the strand, have an average diameter D4. In the embodiment shown, the strand-shaped protrusions 4 have a diameter that decreases from a strand base, at the interface with the flank surface, and a free strand apex.
[0106] [Fig.4] is a texture of a high-contrast element 3 comprising blade-shaped protrusions 5, according to a second variant of the first mode of rea preferred texture layout. The blade-shaped protrusions 5, in relief relative to a flank surface, have an average height H5. By average height, we mean the arithmetic mean of the heights of all the protrusions. The blade-shaped protrusions 5 are distributed according to a pitch P5. The blade-shaped protrusions 5, having a width varying over the entire height of the blade, have an average width D5. In the embodiment shown, the blade-shaped protrusions 5 have a width that decreases from a blade base, in interface with the flank surface, and a free blade top.
[0107] [Fig. 5] is a texture of a high-contrast element 3 comprising cavities 6, according to the second preferred embodiment of the texture. The cavities 6, recessed relative to a flank surface, have an average depth. By average depth, we mean the arithmetic mean of the depths of all the cavities. A cavity 6 is constituted by a cavity interior 62, formed in the thickness of the flank, and an opening 61, opening into the surface of the flank. The openings 61 on the flank surface are spaced apart by a pitch P6. The openings 61 on the flank surface have an average diameter D6. By average diameter, we mean an arithmetic mean of the diameters, not necessarily identical, of the openings on the flank surface.
Claims
Claims
1. A tire (1) for a vehicle comprising a sidewall (2) with at least one high-contrast sidewall element (3): -the high-contrast sidewall element (3) being constituted by a texture having a first brightness L*1 at least equal to 1 and at most equal to 15, -any portion of sidewall surface (21) adjacent to the high-contrast sidewall element (3), having a second brightness L*2 at least equal to L*1+5, -the sidewall (2) comprising a rubber composition based on an elastomer matrix, at least one reinforcing filler, at least one crosslinking system, at least one plasticizing agent, at least one anti-ozone wax and at least one rubber crumb, characterized in that the elastomer matrix comprises an isoprene elastomer at a rate at least equal to 35 phr and at most equal to 65 phr and a butadiene elastomer at a rate at least equal to 35 pce and at most equal to 65 pce,in that the rate of reinforcing filler is at least equal to 5 pce and at most equal to 70 pce, in that the rate of anti-ozone wax is at least equal to 1 pce and at most equal to 3 pce and in that the rate of rubber powder is at least equal to 2 pce and at most equal to 30 pce.,
2. Tire (1) according to claim 1, in which the anti-ozone wax content is at least equal to 1.2 pce and at most equal to 2.8 pce, preferably at least equal to 1.4 pce and at most equal to 2.6 pce and more preferably at least equal to 1.6 pce and at most equal to 2.4 pce.
3. Tire (1) according to one of claims 1 or 2, in which the rubber crumb content is at least equal to 5 pce and at most equal to 20 pce, preferably at least equal to 5.5 pce and at most equal to 19.5 pce, more preferably at least equal to 6 pce and at most equal to 19 pce and even more preferably at least equal to 6 pce and at most equal to 18 pce.
4. Tire (1) according to any one of claims 1 to 3, in which the ratio between the rubber crumb content, expressed in pce, and the anti-ozone wax content, expressed in pce, is at least equal to 5.50 and at most equal to 17.00, preferably at least equal to 6.00 and at most equal to 17.00 and more preferably at least equal to 6.50 and at most equal to 12.
50.
5. Tire (1) according to any one of claims 1 to 4, in which the reinforcing filler content is at least equal to 10 pce and at most equal to 60 pce, preferably at least equal to 15 pce and at most equal to 55 pce, more preferably at least equal to 15 pce and at most equal to 50 pce and even more preferably at least equal to 15 pce and at most equal to 45 pce.
6. Tire (1) according to any one of claims 1 to 5, in which the sum of the reinforcing filler content and the rubber crumb content is at least equal to 30 pce and at most equal to 65 pce, preferably at least equal to 30 pce and at most equal to 60 pce and more preferably at least equal to 35 pce and at most equal to 50 pce.
7. A tire (1) according to any one of claims 1 to 6, wherein the reinforcing filler comprises mainly carbon black.
8. A tire according to any one of claims 1 to 7, in which the ratio between the level of reinforcing filler, expressed in pce, and the level of plasticizing agent, expressed in pce, is at least equal to 1.00 and at most equal to 5.00, preferably at least equal to 1.50 and at most equal to 4.50, more preferably at least equal to 2.00 and at most equal to 4.00 and even more preferably at least equal to 2.00 and at most equal to 3.
50.
9. Tire (1) according to any one of claims 1 to 8, in which the high-contrast sidewall element (3) is constituted by a texture having a first brightness L*1 at least equal to 4 and at most equal to 13.
10. A tire (1) according to any one of claims 1 to 9, wherein any portion of sidewall surface (21) adjacent to the high contrast sidewall element (3) has a second brightness L*2 at least equal to L*l+10, preferably at least equal to L*l+12.
11. A tire (1) according to any one of claims 1 to 10, wherein any portion of sidewall surface (21) adjacent to the high contrast sidewall element (3) has a second brightness L*2 of at least 18, preferably at least 22.
12. A tire (1) according to any one of claims 1 to 11, wherein the high-contrast sidewall element (3) is constituted by a texture comprising protuberances (4, 5), in relief relative to a sidewall surface (21), in contact with atmospheric air, and / or cavities (6), in hollow relative to the sidewall surface (21).
13. A tire (1) according to any one of claims 1 to 12, wherein the high contrast sidewall element (3) is constituted by a texture comprising strand-shaped protrusions (4).
14. A tire (1) according to any one of claims 1 to 12, wherein the high contrast sidewall element (3) is constituted by a texture comprising blade-shaped protrusions (4).
Citation Information
Patent Citations
Process and apparatus for manufacturing crumb and powder rubber
US7445170B2
Conical-shaped impact mill
US7861958B2
High-contrast tire pattern and method for producing same
WO2011036061A1
Core selection switch and optical node device
WO2020174919A1
Tyre provided with a texture on a sidewall
EP3592577B1