PROCESS FOR TRANSFORMING PLASTIC INTO HYDROCARBON(S)
The electromagnetic induction heating process efficiently transforms plastic into high-value hydrocarbons like methane, addressing the inefficiencies of existing recycling methods by using a micrometric ferromagnetic heating element, achieving high yields and selectivity without catalysts.
Patent Information
- Application Number
- FR2023004642
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing plastic recycling processes are energy-intensive, expensive, and produce low-quality compounds, limiting their effectiveness and scalability, especially for commonly used plastics like polyethylene and polypropylene.
A process using electromagnetic induction heating with a micrometric ferromagnetic heating element transforms plastic into high-value hydrocarbons, such as methane, by heating the element in an oxygen-free atmosphere, allowing control over the reaction products without the need for catalysts.
The process achieves high yields and selectivity of hydrocarbons like methane efficiently, with low energy consumption, using simple steel wool as the heating element, and can produce hydrocarbons with controlled selectivity.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: PROCESS FOR THE TRANSFORMATION OF PLASTIC INTO HYDROCARBONS
[0001] The present invention falls within the general field of recycling plastic materials.
[0002] More particularly, the present invention relates to a method for transforming a plastic substrate or a heavy oil into hydrocarbon(s), using the electromagnetic induction heating technique. The invention also relates to the use, for such transformation, of a micrometric heating element formed from a ferromagnetic metal compound.
[0003] Plastic waste, a major cause of pollution in landfills and oceans, is a source of global concern, mainly due to the enormous production rate and the long lifespan of the materials from which it is made. For example, the global production capacity of polyethylene, the most widely used category of plastics, in a wide variety of fields ranging from garbage bags to bubble wrap to hip prostheses, is 80 million tons per year. Polyethylene molecules are, as their name suggests, composed of several ethylene molecules (C2H4). Polyethylene chains can be linear or branched, the degree of branching affecting the rigidity, density, and strength of the material. Generally speaking, the polyethylene produced is chemically inert and resistant to decomposition.It makes up about 60% of the plastics found in landfills, where it decomposes very slowly, if at all.
[0004] Several types of plastic recycling streams have been developed and are constantly being improved to cope with the enormous amount of plastic waste generated by industry.
[0005] Mechanical recycling currently efficiently processes collected plastic waste, it displays very good yields and benefits from a good establishment in the sorting sector. However, it has several limitations. On the one hand, it is not suitable for separating polymers from plastic components and their additives, for example dyes. On the other hand, although the sector is progressing rapidly, the physical characteristics of the material resulting from recycling are often degraded compared to the original material. Recycled plastic is therefore still often used for uses other than its initial use, particularly in the construction and building sector. The combination of these factors limits the scale at which plastic is recycled, especially since it is still often less expensive to use materials raw materials to produce plastic articles.
[0006] To take a step towards a circular economy, it is necessary to process the portion of collected plastics that mechanical recycling is unable to handle satisfactorily.
[0007] Several chemical recycling techniques, distinct in their method and the structure of the product obtained at the output, have been proposed in order to complement mechanical recycling and avoid resorting to incineration or landfilling. Among these techniques, we can cite: - dissolution, which allows the recovery, using a solvent, of polymer chains, which can be used to create new plastics, - chemical depolymerization, allowing a return to the monomer stage by using a chemical solvent, these monomers being able to be used subsequently to form new polymer chains, - biochemical conversion, which corresponds to a chemical depolymerization in which chemical agents are replaced by enzymes, - pyrolysis or gasification, i.e. thermal depolymerization, which allows hydrocarbons to be recovered in liquid and / or gaseous state, depending on the length of their chain, through heat treatment processes. Reinjected into a steam cracker, part of these hydrocarbons allows new plastics to be formed, by thermal cracking, catalytic cracking or hydrocracking, in the presence of a catalyst and hydrogen.
[0008] The transformation of plastic into fuel by pyrolysis is a known process that has been industrially developed for more than ten years. However, this process is energy-intensive and does not allow the selectivity of the products formed to be controlled.
[0009] Generally speaking, the processes for recycling plastics proposed by the prior art are expensive to implement and energy-intensive, and / or they produce low-quality compounds that are difficult to use. Their effectiveness may also be limited to certain plastics. For example, biochemical conversion, while effective for recycling polyethylene terephthalate, is much less so for the most commonly used plastics, namely polyethylene and polypropylene.
[0010] The present invention aims to overcome the drawbacks of the methods proposed by the prior art for recycling plastic waste, in particular the drawbacks set out above, by proposing such a method which makes it possible to produce high added value compounds, in an economical manner and in particular with low energy consumption.
[0011] It has now been discovered by the present inventors that such results can be achieved by a method implementing an electric induction heating mode. electromagnetic, in the presence of a micrometric-sized heating element mixed with the plastic substrate to be transformed. Such a process is particularly energy-efficient and has great versatility, in that it allows, by the choice of suitable operating conditions, to direct the transformation of plastics into different targeted reaction products, in particular into hydrocarbon(s) with a more or less long chain. Surprisingly, the present inventors have notably discovered that the implementation of such a process according to specific operating conditions also makes it possible to form methane with controlled selectivity, and in particular as the largely majority product of the reaction, this with a high yield, including in the absence of a catalyst compound for the plastic transformation reaction, and / or when the heating element is simple steel wool.
[0012] Thus, according to the present invention, there is proposed a method for transforming a solid or liquid substrate into hydrocarbon(s) chosen from substrates formed from plastic material(s) and heavy oils, by a transformation reaction occurring in a given temperature range. This method comprises steps of: - bringing this substrate into contact, in a reactor, with an element, called a heating element, in micrometric form, this element being formed from a ferromagnetic metallic compound, this under an atmosphere devoid of oxygen, - and, still under said oxygen-free atmosphere, heating this heating element by electromagnetic induction using a magnetic field inductor external to the reactor, this heating being carried out at a temperature within said temperature range.
[0013] In the present description, by external to the reactor, is meant the fact that the magnetic field inductor is not located in the atmosphere of the reactor, in the sense that it is located outside the reaction zone of the reactor, in which the substrate and the heating element are brought into contact with each other, under the oxygen-free atmosphere. The magnetic field inductor can be placed so as to surround the reactor or so as to be contained in the reactor (for an annular type reactor for example), as long as it remains external to the internal atmosphere of said reactor.
[0014] In the present description, micrometric shape means that the heating element is in the form of entity(ies) all of whose dimensions are greater than or equal to 1 μm, and at least one dimension is between 1 and 1000 μm.
[0015] The heating element used in the method according to the invention is formed from at least one, i.e. one or more, ferromagnetic metal compounds. It may further contain other compounds, which may or may not be inert with respect to the transformation reaction to be carried out. In alternative embodiments of the invention, the heating element consists of one or more, preferably a single, ferromagnetic metal compound(s).
[0016] A heavy oil is defined in the present description, in a conventional manner in itself, as a hydrocarbon or a mixture of hydrocarbons with a high boiling point, comprising at least 12 carbon atoms, such as octadecane. When the substrate is a heavy oil, its transformation according to the invention aims at the formation of so-called lower hydrocarbon(s), that is to say comprising a much smaller number of carbon atoms, in particular a number of carbon atoms between 1 and 4, with a much lower boiling point.
[0017] The type of reaction for transforming the substrate into hydrocarbon(s), which the method according to the invention makes it possible to carry out, varies depending on the operating conditions used, and in particular the atmosphere in the reactor during the heating step. As indicated above, this atmosphere is oxygen-free. The atmosphere in the reactor during the heating step may be of the inert type. The reaction for transforming the substrate, referred to as pyrolysis or thermolysis, is then caused solely by heat. Otherwise, the atmosphere in the reactor during the heating step may be of the reducing type, and in particular based on dihydrogen. The transformation reaction is in this case a hydrogenolysis, which may, depending on the operating conditions applied, be combined with pyrolysis. The reaction products obtained at the end of the transformation reaction are different depending on the type of reaction, and the mechanism(s) it implements.They also differ depending on whether or not the process according to the invention uses, in addition to the micrometric heating element, a catalyst for the transformation reaction. For example, a hydrogenolysis reaction of a plastic polymer, in the presence of a catalyst for this reaction, will lead to the production of a mixture of oligomers, alkanes, in particular methane, olefins, and coke, distributed in gaseous, liquid and solid phases. A pyrolysis reaction, thermal and / or catalytic, under an inert atmosphere, will lead to a mixture of gaseous alkanes, liquid fuels and carbonaceous materials.
[0018] The temperature range at which the transformation reaction occurs depends on the type of reaction, and in particular on the atmosphere used in the reactor and on the presence or absence therein of a reaction catalyst, as well as on the chemical nature of the substrate. It is within the skill of the person skilled in the art to know how to determine this temperature range depending on the particular substrate to be recycled and the desired reaction products (determining the type of transformation reaction to be carried out, pyrolysis and / or hydrogenolysis, and the choice of possible catalyst, or absence of catalyst). This temperature range is typically between 300 and 650°C. For any temperature range targeted, It is also within the skill of the person skilled in the art to know how to determine the operating parameters to be implemented for the application of the magnetic field in the reactor, so as to reach an adequate temperature in the latter, causing the transformation reaction to take place. For the determination of these operating parameters, the person skilled in the art will also take into account the characteristics of the particular heating element used, in particular its specific absorption rate (SAR) and its quantity present in the reactor. The SAR is a well-known parameter in itself, defining the heating capacity of a magnetic or electrically conductive material subjected to an alternating magnetic field.
[0019] In all its embodiments, whatever the type of transformation reaction, the process according to the invention advantageously makes it possible to obtain, from plastic material or heavy oil, one or more gaseous hydrocarbons, i.e. C1-C4, with high added value, and even more so in the case of methane. In this respect, the process according to the invention makes it possible in particular, in particular embodiments, to form, from plastic material or heavy oil, methane with a high yield, but also with very high selectivity, methane even being able, under certain conditions, to be the only gaseous product of the reaction.In particular, such selectivity with respect to methane can advantageously, and particularly surprisingly, be obtained without using a catalyst for the substrate transformation reaction, in the presence of a dihydrogen atmosphere, including using simple steel wool as a heating element. The process according to the invention also leads to the production of solid reaction product(s), and can lead, depending on the operating parameters applied, to the production of liquid reaction product(s). In particular embodiments of the invention, using a specific transformation reaction catalyst, such as ruthenium, the process according to the invention can advantageously make it possible to obtain saturated alkanes with a longer chain than gaseous hydrocarbons, typically C5-C30, in liquid form, also with high added value.
[0020] The method according to the invention is particularly energy-efficient, even when the transformation reaction only involves pyrolysis. In this respect, it takes advantage of the property of ferromagnetic metal compounds to rise in temperature when they are subjected to an electromagnetic field, under the effect of their own magnetic moment. When carrying out the heating step of the method according to the invention, only the heating element is heated. Under the effect of the electromagnetic field applied to the reactor, its temperature rises rapidly, locally reaching a temperature within the temperature range at which the transformation reaction according to the invention occurs. As indicated above, it is within the skills of a person skilled in the art to determine the characteristics of the magnetic field to be applied depending on the temperature range that is intended to be obtained (typically, a temperature range in the interval between 300 and 650 °C), as well as the particular ferromagnetic metal compound(s) used in the composition of the heating element used according to the invention, and the quantity of heating element used. Advantageously, the transformation reaction therefore occurs at the surface of the heating element, without the reaction medium as a whole reaching the temperature necessary for the intended transformation reaction, including when the substrate is initially in solid form (local heating at the surface of the heating element having the first effect of causing the solid plastic materials in contact with it to melt, with the consequence of increasing the contact surface between the heating element and the liquefied substrate).
[0021] The low energy consumption of the process according to the invention is advantageously proven even in the absence of a reducing atmosphere in the reactor, and in the absence of a catalyst. In such configurations, it is particularly inexpensive to implement, due to the low cost of reagents to be used.
[0022] Preferably, the reactor used in the method according to the invention is formed from a non-ferromagnetic material, for example glass, quartz, silicon carbide or any other non-metallic solid material compatible with exposure to a magnetic field and with the temperatures involved.
[0023] The method according to the invention may furthermore meet one or more of the characteristics described below, implemented in isolation or in each of their technically effective combinations.
[0024] The substrate that the method according to the invention aims to transform, when it is formed from plastic material(s), may initially be in solid form, in particular in the form of solid fragments, for example fragments of plastic bottles. It is preferably in liquefied form. Thus, the method according to the invention may comprise an initial step of liquefaction of the substrate, before its introduction into the reactor, or carried out directly in the reactor. Such a step may be carried out by any conventional heating technique in itself. By way of example, particularly advantageous from the point of view of the ecological footprint of the method, the liquefaction step may be carried out by heating with solar energy.The heating temperature to be applied depends on the particular plastic material to be liquefied, more specifically on its melting temperature, and its determination for each given substrate is within the skill of the person skilled in the art. Typically, the melting temperature of plastic materials is between 90 and 200 °C.
[0025] When formed from plastic material(s), the substrate may in particular be formed from polyolefin, such as polyethylene or polypropylene, from copolymer based on, that is to say comprising units of polyolefin, such as polyethylene terephthalate, polyester, polystyrene, or any of their mixtures. Of course, the reaction products in solid form, and where appropriate in liquid form, obtained at the end of the implementation of the process according to the invention, depend on the initial plastic material(s) used.
[0026] The micrometric heating element may be chosen from particle powders based on the ferromagnetic metal compound with a size between 1 and 1000 μm, and wires based on the ferromagnetic metal compound having a wire diameter between 1 and 1000 μm.
[0027] By particles of size between 1 and 1000 pm, it is meant that all the dimensions of the particles are between 1 and 1000 pm. Preferably, the particles are of size between 1 and 100 pm, more preferably between 1 and 50 pm, and preferentially between 1 and 10 pm. Each of the particles may be formed from one or more ferromagnetic metal compounds, and contain only this or these compounds, or may contain additional constituents, for example a catalyst for the targeted transformation reaction, such as cobalt, nickel, copper, ruthenium, rhodium, palladium, platinum or any other catalytic compound, or any alloy of one or more of these compounds.
[0028] Preferably, the heating element is a set of wires each formed from one or more ferromagnetic metal compounds, preferably composed for at least 90% by weight of one or more, preferably only one, ferromagnetic metal compound(s). In particular embodiments of the invention, each of these wires has a wire diameter of between 1 and 1000 μm, preferably between 10 and 1000 μm, more preferably between 20 and 500 μm, preferably between 50 and 200 μm, and for example between 50 and 100 μm, and a wire length preferably of a few centimeters. In preferred embodiments of the invention, the heating element is in the form of a straw, that is to say a tangle of such wires.
[0029] The ferromagnetic metal compound used in the method according to the invention, or each ferromagnetic metal compound used in the method according to the invention, is preferably chosen from those having a magnetic ani-sotropy less than or equal to 8.104 J.m3, preferably less than or equal to 3.104 Jm 3.
[0030] Each of these compounds is preferably chosen from iron, cobalt, nickel, and their oxides, carbides and / or alloys, as well as amorphous ferromagnetic materials.
[0031] In particular embodiments of the invention, the ferromagnetic metal compound is chosen from iron and its alloys, in particular iron alloys and of carbon, for example of the Fe / Cx type, such as Fe22C, Fe3C, Fe5C2, iron and cobalt alloys, and iron and nickel alloys. Alloys containing at least 50%, preferably at least 80%, by weight of iron are particularly preferred in the context of the invention, in particular in the context of an implementation of a heating element in the form of wires.
[0032] Otherwise, the ferromagnetic metal compound used according to the invention may, when it is in powder form, be chosen from iron oxides, such as magnetite or maghemite, or from ferromagnetic ceramics based on iron oxide(s).
[0033] In particularly preferred embodiments of the invention, the heating element is iron wool, in particular as commonly referred to as “superfine”, comprising an entanglement of wires composed of at least 90% by weight of iron, and the average wire diameter of which is between 10 and 1000 μm, preferably between 20 and 500 μm, more preferably between 50 and 200 μm, for example between 50 and 100 μm, and the length of the wires is a few centimeters, for example between 1 and 10 cm. In addition to constituting a high-performance heating element when subjected to a magnetic field, the iron wool has the advantages of low cost and a long service life. It is also easily recoverable, in particular separable from the other components in the reactor, and non-polluting.
[0034] In particular embodiments of the invention, the magnetic field generated by the magnetic field inductor, for the heating step of the method, has an amplitude of between 1 and 80 mT and a frequency of between 30 and 500 kHz.
[0035] The amplitude of the magnetic field is preferably between 1 and 50 mT, more preferably between 25 and 40 mT, preferably between 27 and 40 mT, even more preferably between 29 and 40 mT, and for example between 29 and 35 mT.
[0036] The power is preferably between 2 and 5 kW, preferably between 2 and 4 kW, and for example between 2.6 and 3.8 kW.
[0037] The frequency of the applied magnetic field is preferably between 50 and 400 kHz, more preferably between 100 and 300 kHz.
[0038] Such characteristics of the magnetic field advantageously make it possible to bring the heating element according to the invention to a temperature allowing the targeted substrate transformation reaction to occur.
[0039] As explained above, in particular embodiments of the invention, the atmosphere in the reactor, for the heating step, may be an inert atmosphere, for example an argon atmosphere, preferably at the pressure atmospheric. The process according to the invention can then be described as a process of pyrolysis, or thermolysis, of the substrate. Such an implementation method results in the production of gaseous hydrocarbons, in particular in the form of a mixture of methane, ethane and propane, and saturated liquid hydrocarbons, in particular C10-C40.
[0040] In alternative embodiments of the invention, the atmosphere in the reactor, for the heating step, is a reducing atmosphere. This atmosphere may in particular comprise dihydrogen. It preferably consists of dihydrogen. The process according to the invention can then be expressed in terms of a process of hydrogenolysis, where appropriate coupled with pyrolysis, of the substrate. The dihydrogen pressure in the reactor is then preferably at least 3 bars, preferably at least 5 bars, and for example between 5 and 10 bars. Generally speaking, a higher dihydrogen pressure in the reactor reduces the duration of the heating step necessary for the formation of the targeted products.
[0041] Implementing the process under a dihydrogen atmosphere leads in particular to the formation of a larger gaseous fraction of hydrocarbons than when the process is implemented under an inert atmosphere. In addition, it advantageously makes it possible to obtain methane with a high yield, as well as better control of the selectivity of the reaction with respect to the formation of methane, compared to the other gaseous hydrocarbons likely to be formed from the substrate.
[0042] In particular, in the embodiments of the method in which the atmosphere in the reactor is based on dihydrogen, this methane yield and this selectivity with respect to methane are all the higher, including when the reaction medium is devoid of catalyst for the transformation reaction, and including when the heating element consists of simple steel wool, when the mass ratio of the heating element relative to the substrate, in the reactor, is greater than or equal to 0.2.The selectivity with respect to methane, compared to other gaseous hydrocarbons, is particularly high, and may in particular be 100%, when the heating element / substrate mass ratio is greater than or equal to 0.25, preferably greater than or equal to 0.3, in particular when the reaction medium is free of catalyst for the transformation reaction and / or the heating element consists of steel wool, in particular as defined above.
[0043] The invention does not, however, exclude the possibility that the heating element / substrate mass ratio in the reactor is less than 0.2, the heating step then preferably being carried out in the presence, in the reactor, of a catalyst for the transformation reaction, in contact with the substrate and the heating element.
[0044] Generally speaking, a higher quantity of heating element in the reactor further reduces the duration of the heating step necessary for the formation of the targeted products.
[0045] In particular embodiments of the invention, a catalytic metal compound, catalyst for the transformation reaction, is brought into contact, in the reactor, with the substrate and the heating element during the heating step.
[0046] Such a catalytic metal compound may be chosen from manganese, cobalt, nickel, copper, zinc, rhodium, ruthenium, palladium, platinum, iridium and / or tin, or any alloy of one or more of these metals.
[0047] The mass rate of “catalytic metal compound / ferromagnetic metal compound”, for example “platinum / iron” (Pt / Fe), is then preferably between 0.1 and 2%.
[0048] The catalytic metal compound can be implemented as such, in powder form for example, or be deposited on a solid support, such as a support made of silicon, cerium, aluminum, titanium or zirconium oxide, or any of their mixtures. By way of example, the catalytic metal compound can be implemented deposited on a support based on silicon oxide and aluminum oxide, such as the product marketed under the name Siralox by the company Sasol.
[0049] In particular embodiments of the invention, the catalytic metal compound is platinum, preferably deposited on a solid support, in particular as defined above. Such a characteristic particularly promotes the production of gaseous hydrocarbon(s) from the substrate, and in particular methane, both in terms of yield and selectivity.
[0050] In alternative embodiments of the invention, the catalyst is ruthenium. Such a catalyst notably promotes the production of liquid hydrocarbon(s), in particular saturated hydrocarbons, from the substrate.
[0051] Alternatively, the reactor may be free of catalytic compound, in particular catalytic metal compound, capable of catalyzing the transformation reaction, by hydrogenolysis and / or pyrolysis, of the substrate into hydrocarbon(s). Preferably, no solid or liquid component other than one or more substrate(s) and one or more heating element(s), as defined above, is introduced, and therefore initially present, in the reactor at the time of starting the heating step. Such a characteristic does not exclude the possibility that a catalyst compound for the reaction may form spontaneously in the reactor during the heating step, in particular from the ferromagnetic metal compound(s) forming the heating element.
[0052] The absence of catalytic compound in the reactor during the heating step advantageously induces, in particular when the heating element is steel wool, the formation of gaseous hydrocarbons, to the detriment of the formation of liquid hydrocarbons, and mainly, or even only, methane.
[0053] The process according to the invention preferably comprises a final step of recovering the gaseous fraction contained in the reactor, and where appropriate the liquid fraction which may also be contained therein, after a determined time for carrying out the heating step (i.e., a reaction time). These fractions are advantageously rich in high added-value hydrocarbon(s), which can be used in numerous applications. The process may also comprise a step of recovering the solid fraction contained in the reactor at the end of the heating step.
[0054] The duration of the heating step is preferably greater than or equal to 2 hours, preferably greater than or equal to 5 hours, for example between 2 and 15 hours, preferably between 5 and 15 hours. It is within the competence of a person skilled in the art to determine this duration as a function of the specific characteristics of the substrate, the applied magnetic field, the heating element(s) and, where appropriate, the catalytic metal compound(s) used.
[0055] Another aspect of the invention relates to the use of an element, called a micrometric heating element, formed from one or more ferromagnetic metallic compound(s), to transform into hydrocarbon(s), by heating this heating element by electromagnetic induction, a solid or liquid substrate chosen from substrates formed from plastic material(s) and heavy oils.
[0056] This use may meet one or more of the characteristics described above with reference to the method according to the invention.
[0057] The characteristics and advantages of the invention will appear more clearly in the light of the following examples of implementation, provided for purely illustrative purposes and in no way limiting the invention, with the support of figures 1 to 4, in which:
[0058] [Fig-1] [Fig.l] schematically represents an example of a device for the implementation of a method according to the invention.
[0059] [Fig.2] [Fig.2] shows examples of transformation reactions that can be produced by a process according to the invention, from polyethylene.
[0060] [Fig.3] [Fig.3] shows graphs representing, as a function of reaction time, the respective contents of methane, ethane and propane obtained in the gaseous phase formed at the end of the implementation of a process in accordance with the invention for the transformation of low-density polyethylene, by magnetic induction at 29.3 mT, in the presence of steel wool (100 mg for 500 mg of polymer) and platinum catalyst supported on Siralox, and, in a / an argon atmosphere at atmospheric pressure, in b / an atmosphere of 3 bars of H2, and in c / an atmosphere of 5 bars of H2.
[0061] [Fig.4] [Fig.4] shows a bar graph representing, for different times of reaction, the material balance Bmatière (sum of the masses of the gaseous, liquid and solid fractions obtained at the end of the reaction, divided by the initial mass of polymer) at the result of implementing a process in accordance with the invention for transforming low-density polyethylene, by magnetic induction at 29.3 mT, in the presence of steel wool (100 mg for 500 mg of polymer) and platinum catalyst supported on Siralox, and an argon atmosphere at atmospheric pressure, 3 bars of H2 or 5 bars of H2.
[0062] An example of a device for implementing a method according to the invention is shown schematically in [Fig.l].
[0063] It comprises a reactor 10, formed from non-ferromagnetic material, for example glass, silicon, quartz or silicon carbide. It is in the form of a Fischer-Porter (FP) bottle in the embodiment shown in the figure.
[0064] In this reactor 10 are placed the substrate to be transformed, in solid or liquid form (solid fragments 11 in the embodiment shown in the figure), as well as a micrometric heating element 12 formed from a ferromagnetic metal compound. In the embodiment shown in the figure, the heating element 12 is in the form of steel wool pressed into a ball. A catalytic compound catalyzing the reaction of transformation of the substrate into hydrocarbon(s) (not shown in the figure) can also be placed in the reactor 10.
[0065] An annular connector 13 is fixed, in a fluid-tight manner, to the reactor 10, at the opening 102 of the latter. The fixing is for example carried out by screwing cooperating screw threads 101, 131 carried respectively by the reactor 10 and the connector 13. The sealing of the fixing can be ensured by any means, for example by a sealing washer 14 arranged in the screw thread 131 of the connector 13.
[0066] The connector 13 is hydraulically connected to a pipe 22, allowing the desired gas to be introduced into the reactor 10, or a gaseous fraction to be extracted therefrom. This pipe 22 is for example equipped with an opening / closing valve 15, a pressure gauge 16 and a safety bypass 17, closed during normal operation of the reactor.
[0067] The reactor 10 is arranged in an electromagnetic induction coil, also called a magnetic field inductor, 18. This is preferably a water-cooled coil capable of generating an alternating magnetic field (AMF), for example of a frequency of 300 kHz.
[0068] The electromagnetic induction coil 18 is connected to a generator 20, which is controlled by a control module 21, provided with a user interface 211, making it possible to control and adjust the operating parameters, and in particular the percentage of the maximum amplitude of the magnetic field. For the electromagnetic induction coil of frequency 300 kHz used for the examples described below, the relationship between percentage of the maximum magnetic field applied, power in kW and applied magnetic field amplitude in mT, is shown in Table 1.
[0069] [Tables 1] Percentage of maximum applied magnetic field (%) Power (kW) Magnetic field amplitude (mT) 5 0.8 17.5 9 1.4 22.2 15 2.2 27.4 18 2.6 29.3 20 2.8 30.6 25 3.5 33.8 27 3.8 35 30 4.2 36.6
[0070] Table 1 - Characteristics of the magnetic field that can be applied by the electromagnetic induction coil implemented in the examples
[0071] For the implementation of a method according to the invention, the substrate 11 to be transformed (plastic material in liquid or solid form or heavy oil), the heating element 12 and, where appropriate, the catalytic compound catalyzing the reaction, are placed in the reactor 10. After fixing the connector 13, the desired gas, for example dihydrogen or argon, is introduced, from the pipe 22, into the reactor 10, at the desired pressure, so as to constitute in the reactor an atmosphere 23 devoid of oxygen. The electromagnetic induction coil 18 is then activated, for the desired time to carry out the transformation of the substrate into hydrocarbon(s).
[0072] At the end of this substrate transformation reaction, the gaseous fraction formed, which may, depending on the operating conditions applied, be particularly rich in methane, can be recovered via pipe 22.
[0073] As examples, [Fig.2] shows transformation reactions that can be carried out by a process according to the invention from polyethylene, of formula (I):
[0074] [Chem.l]
[0075] in which, for these examples, n is approximately equal to 143, and using either platinum as a catalyst or no catalyst.
[0076] These transformation reactions, corresponding to the different examples which will be described below, lead to different products depending on the operating conditions applied: inert atmosphere (argon) or reducing atmosphere (hydrogen), and presence or absence of catalyst (for example platinum, “Pt Catalyst” in the figure). As can be seen in this figure, for each type of reaction, hydrogenolysis and / or pyrolysis, we obtain: - depending on the conditions, a liquid fraction, in the form of a pyrolyzed brown liquid, formed of hydrocarbon compounds of approximately C10-C40; - a gaseous fraction, composed, depending on the operating conditions used, of methane alone, or of a mixture mainly consisting of methane, ethane and propane; - and a solid fraction, formed of coke, where appropriate of iron carbide FexCy (non-stoichiometric carbide probably composed of Fe3C, Fe5C2 and Fe2.2C), possibly of amorphous carbides of formulation Fex with x between 0 and 1, in particular between 0 and 0.5, and of compound(s) of formula (II):
[0077] [Chem.2] (II)
[0078] in which, depending on the reaction, m can be: - significantly lower than 143 (“m “< 143”) (compounds insoluble in dichloromethane (DCM)), - much lower than 143 (“m “143”) (waxy compounds, soluble in DCM), - or lower than 143 (“m < 143”) (compounds insoluble in DCM). EXAMPLES
[0079] A / General Materials and Methods
[0080] Al / Chemicals and Materials
[0081] Tetrahydrofuran (THF, >99%) and toluene (>99%) were supplied by Carlo Erba and Fisher Scientific, respectively. The solvents were dried in a solvent purifier (by passing through an alumina-based desiccant) and degassed by bubbling argon (Ar) for 20 min before being transferred and stored in a glove box. HPLC-grade dichloromethane (DCM) was supplied by Aldrich and used without further purification.
[0082] Siralox (5 / 320) was obtained from Sasol. Tris(dibenzylideneacetone)diplatinum(0) (Pt2(dba)3, >98%) was purchased from NanoMePS.
[0083] Iron wool (trade name "FINE iron wool") was obtained from Gerlon and used without further purification. This iron wool is formed of iron micro-wires 50 to 100 pm in diameter and a few centimeters long. Its SAR at 93 kHz and 47 mT is 68 W.g1. This iron wool was pressed by hand, in order to give it the shape of a small sphere, for all reactions, in order to establish good contact with the other elements of the mixture.
[0084] Also obtained from Aldrich: - low density polyethylene (LDPE), with a low mass average molar mass (Mw) (mass average molar mass Mw of approximately 4000 g.mol1; number average molar mass Mn of approximately 1700 g.mol1; melting point 92°C; in powder form), - high mass average molar mass LDPE (melt index 25 g / 10 min (190°C / 2.16 kg); melting point 116°C, in pellet form), - high density polyethylene HDPE (flow index 12 g / 10 min (190°C / 2.16 kg)), - polypropylene (PP) (isotactic, Mw of approximately 12000 g.mol1; Mn of approximately 5000 g.mol1; melting point 157°C), - and polystyrene (PS) (Mw of approximately 35000 g.mol1; in powder form).
[0085] Plastic bottles made of grade 4 LDPE were purchased from VWR.
[0086] All experiments were carried out with the polymers as received, without further purification.
[0087] A.2 / Characterization
[0088] Powder X-ray Diffraction (XRD) patterns were obtained using a PANAlytical Empyrean diffractometer (with Cobalt source, Ka 1.79 Å).
[0089] The elemental analysis allowing the quantification of the Pt mass content of Pt / Siralox was obtained by inductively coupled plasma - atomic emission spectroscopy (ICP-AES) on an iCAP 6300 ICP Duo spectrometer.
[0090] Scanning electron microscopy (SEM) images were taken on a JEOL JSM-7800F microscope.
[0091] Elemental mapping by scanning electron microscopy coupled with an energy dispersive detection system (SEM-EDX), allowing the identification of the distribution of the elements, was obtained using a Bruker XFlash® EDX detector attached to the microscope.
[0092] Brightfield transmission electron microscopy (TEM) images were obtained on a JEOL JEM 1400 microscope (tungsten filament, operating voltage 120 kV).
[0093] ImageJ software was used to count the nanoparticles, the size distribution histograms having been obtained on the count of 150 particles.
[0094] High-resolution transmission electron microscopy (HR-STEM) images were recorded on a JEM-ARM200F microscope. The image resolution in STEM mode is 0.78 Å (STEM HAADF 200kV). Elemental mapping in STEM in High Angle Annular Dark Field (HAADF) mode was conducted to determine the elemental distribution at the nanoscale.
[0095] STEM-EDX mapping was obtained using a CENTURIO-X wide-angle SDD detector (129 eV resolution) attached to the microscope.
[0096] The specific surface area of the samples was obtained by measuring the isotherms using the Brunauer-Emmett-Teller (BET) method.
[0097] The solid residues obtained in the case of catalytic reactions using Pt / Siralox were characterized by DRX on powder, TEM and solid-state cross-polarization magic angle spinning 13C nuclear magnetic resonance (CP / MAS 13C-NMR).
[0098] In the case of reactions involving steel wool, the black residues obtained in certain experiments were characterized by powder XRD and Fourier transform Raman spectroscopy (FT-Raman).
[0099] During the reactions, the apparent temperatures at the surface of the FP bottle were measured and recorded after 10 min of reaction using a Testo 885 infrared (IR) camera.
[0100] A.3 / Gas chromatography and mass spectrometry
[0101] The obtained gas phase products were analyzed and quantified using a PerkinElmer Clarus® 580 gas chromatograph (GC). The instrument is equipped with a thermal conductivity detector (TCD) for product quantification. In addition, the instrument was connected to a Clarus® SQ-8T mass spectrometer, used for product identification. The initial oven temperature of 80°C was increased to 250°C with a ramp of 16°C / min, then held for 30 min at 250°C. The injection temperature was set at 200°C and the carrier gas (helium He) flow rate in the column was set at 1.8 mL / min. A Shin Carbon (ST 80 / 100) column was used (length of 2 m; internal diameter of 0.53 mm).The retention times under these conditions for the different compounds likely to be obtained at the end of the reactions are as follows: methane 1.82 min; ethylene 2.82 min; ethane 6.66 min; propene 12.51 min; propane 13.39 min; butene 30 min; n-butane 33 min.
[0102] B / Synthesis of the supported Pt / Siralox catalyst
[0103] The platinum (Pt) catalyst supported on SIRALOX was synthesized via decom position of an organometallic precursor. For this purpose, 56.8 mg of Pt2(dba)3 were mixed with 2 g of SIRALOX support (silicon and aluminum oxide from Sasol) in a Fischer-Porter (FP) bottle, followed by the addition of 20 mL of THF. The deep violet suspension was stirred for 15 h. Then, the FP bottle was charged at 3 bar with H2 and stirred vigorously for 24 h at room temperature. Instantly, the deep violet solution turned dark brown. After 24 h of stirring, the FP bottle was transferred to a glove box, where the residual pressure was released. After 1 h, a precipitate formed, the colorless supernatant was separated and the gray solid recovered, to be finally washed with 3x5 mL of toluene. The solid obtained was dried under vacuum for 4 h then transferred and stored in a glove box. The product obtained is named Pt / Siralox.
[0104] ICP-AES analysis showed a Pt mass content of 0.78%.
[0105] C / Example 1 - Transformation of LDPE in the presence of iron wool and catalyst Pt / Siralox
[0106] These experiments were carried out using low Mw LDPE.
[0107] All catalytic reactions were carried out in a device as described above. before, with FP bottles as reactors.
[0108] The following were introduced into each FP bottle, in the glove box: - 200 mg of Pt / Siralox,
[0109] - 500 mg of low Mw LDPE, - as well as, as a heating element 12, 100, 200 or 300 mg of the steel wool “FINE steel wool”.
[0110] The atmosphere of the FP bottle was evacuated and replaced with either dihydrogen H2, at a pressure of 3, 5 or 10 bars, or argon, at atmospheric pressure. Then, the FP bottle was placed in the center of the magnetic induction coil capable of generating an alternating magnetic field (AMF) with a frequency of 300 kHz, with a maximum field amplitude of 65 mT.
[0111] The catalytic reactions were carried out at 9, 18 or 27% of the maximum amplitude of the magnetic field, and for different reaction times (2 h, 5 h and 15 h).
[0112] After starting the magnetic induction coil, the polymer melted within a few minutes, and a release of white / grayish smoke was observed. The smoke release decreased sharply with the reaction time, until it disappeared. The melting of the polymer, the smoke release and its gradual cessation depend on many factors, such as the polymer mass / iron wool mass ratio, the amount of iron wool, the intensity of the applied magnetic field, etc.
[0113] The temperature of the external surface of the FP bottle wall was measured by IR camera, at a value of 180 to 280 °C depending on the operating conditions.
[0114] After completion of the reaction, the FP bottle was allowed to cool and, after After reaching room temperature, the FP bottle was connected to an injection device to the gas chromatograph, allowing the standardized injection at 1 bar of the gas phase contained in the FP bottle, for analysis and quantification of the products formed by GC-MS. The residual gas phase was evacuated and the dark brown / black residue at the bottom of the FP bottle was washed with 3x5 mL of DCM. The solid residue was filtered and then dried overnight while the liquid residue was collected after evaporation of the DCM.
[0115] Each reaction was repeated twice to ensure reproducibility of the experimental results.
[0116] The material balance was calculated by counting the mass of each fraction obtained at the end of the reaction (solid, liquid and gaseous fractions) weighted by the initial polymer mass, according to Equation 1:
[0117] [Math.l] _ ^solid ^leaves * ^*gas ^matter ~ * polymer (Equation 1)
[0118] in which Bmatière is the material balance (arbitrary unit), Msoiide is the mass of solid fraction obtained (g), Miiquide is the mass of liquid fraction obtained (g), Mgaz is the mass of gaseous fraction obtained (g) and Mpoiymère is the initial polymer mass (g)-
[0119] The yield (%) of methane (noted YCh4) was calculated taking into account the total quantity of polymer used for each reaction, according to Equation 2:
[0120] [Math.2] = ■---—---x 100 (Equation 2)
[0121] in which YCH4 is the methane yield of the reaction, molCH4 is the number of moles of methane obtained at the end of the reaction measured by GC-MS, PMCH4 is the molecular weight of methane (g / mol) and Mpolymer is the initial polymer mass (g).
[0122] The optimization of the catalytic transformations of low Mw LDPE in the presence of the Pt / Siralox catalyst was thus carried out by evaluating the effect, as indicated above: of the reaction time (2, 5 and 15 h), of the composition of the initial atmosphere (argon or dihydrogen), of the pressure of the initial gas phase (3, 5 and 10 bars of H2, or argon at atmospheric pressure), of the % of the maximum amplitude of the applied magnetic field (9, 18 and 27%, which is equivalent respectively to a magnetic field amplitude of 22.2, 29.3 and 35 mT, and to a power of 1.4, 2.6 and 3.8 kW), and of the amount of steel wool used (100, 200 and 300 mg).
[0123] The gas phase obtained at the end of each reaction was analyzed by GC-MS, and its respective methane, ethane and propane contents were determined. The results obtained are illustrated in [Fig.3], in a / for the argon atmosphere, in b / for the 3 bar H2 atmosphere and in c / for the 5 bar H2 atmosphere. As can be seen in this figure, methane is the predominantly formed product, and its production increases with the reaction time. Under an H2 atmosphere, the ethane and propane contents decrease with the reaction time, due to their hydrogenolysis. The quantity of methane produced is all the greater as the H2 pressure in the reactor is high.
[0124] The methane yields obtained for the different atmospheres and the different reaction times, for 100 mg of steel wool and 18% field amplitude (29.3 mT), as well as the temperatures of the external wall surface of the FP bottles recorded after 10 min of reaction, are indicated in Table 2.
[0125] [Tables2] Atmosphere Time (h) Ych4 (%) Temperature (°C) Argon (Patm) 2 6.6 150-160 5 10.7 150-160 15 22.5 160-170 H2 (3 bars) 2 14.6 150-160 5 26.6 155-160 15 46 160-165 H2 (5 bars) 2 27.2 150-155 5 41.2 160-165 15 61.9 160
[0126] Table 2 - Methane yields and temperatures recorded, for conditions of 100 mg of steel wool and 18% field amplitude
[0127] For each of the reactions, the masses of each of the gaseous, liquid and solid fractions formed were measured and the material balance Bmatière was calculated according to Equation 1. The results obtained are shown in [Fig.4]. As can be seen, for all the conditions tested, the material balance is particularly high, between 0.85 and 0.95.
[0128] The methane yields obtained for the different % of field amplitude, under 5 bars of H2, for 100 mg of steel wool and 15 h of reaction, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction are shown in Table 3.
[0129] [Tables3] % field amplitude (%) 9 18 27 Ych4 (%) 19.1 62 62.3 Temperature (°C) 140-150 160 150-160
[0130] Table 3 - Methane yields and temperatures recorded, for conditions of 5 bars of H2, 100 mg of steel wool and 15 h of reaction
[0131] The methane yield is substantially equivalent for the field amplitude % of 18% and 27%, and significantly higher than that obtained for 9% field amplitude.
[0132] The methane yields obtained for the different initial quantities of steel wool and the different reaction times, for 18% field amplitude and under 5 bars of H2, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction are indicated in Table 4.
[0133] [Tables4] Amount of steel wool (mg) Reaction time (h) Ych4 (%) Temperature (°C) 100 2 27.2 150-155 5 41.2 160-165 15 62 160 200 2 37.3 175-180 5 59 170-180 15 56.3 175-180 300 2 54.2 200-210 5 55.5 200-215
[0134] Table 4 - Methane yields and temperatures recorded, for conditions of 5 bars of H2 and 18% field amplitude
[0135] Increasing the amount of steel wool reduces the reaction time required to produce a substantially equivalent amount of methane. After 2 hours of reaction, the methane selectivity is greater the greater the amount of steel wool used. It is also observed that the higher the reactor temperature, the greater the amount of methane produced in the shorter reaction time.
[0136] D / Example 2 - Transformation of LDPE in the presence of steel wool without catalyst
[0137] Experiments were carried out with steel wool alone, in the absence of Pt / Siralox catalyst, according to a protocol similar to that described in Example 1, applied for: - 500 mg or 1 g of low Mw LDPE, - 100, 200 or 300 mg of steel wool “FINE steel wool” as described above, - an atmosphere of dihydrogen at 5 bars of H2 or argon at atmospheric pressure, - a reaction time of 2, 5 or 15 h, - 18% of the maximum amplitude of the magnetic field (29.3 mT, 2.6 kW).
[0138] The methane yields obtained for the different initial quantities of steel wool and the different reaction times, as well as the temperatures of the external wall surface of the FP bottles recorded after 10 min of reaction and the quantities of methane and ethane obtained at the end of the reaction (propane is not detected), for the initial condition of 500 mg of LDPE, are indicated in Table 5. In this table, the results obtained in Example 1 above, in the presence of the Pt / Siralox catalyst, for the same operating conditions, are also indicated.
[0139] [Tables5] Amount of steel wool (mg) Reaction time (h) Methane (mmol) Ethane (mmol) Ych4 (%) Temp. (°C) 100 2 (Example 1) 8.48 4.12 27.2 150-155 2 4.116 3.419 13.2 160 5 (Example 1) 12.857 0 41.2 160-165 5 5.977 3.404 19.2 160-165 200 2 (Example 1) 11.614 4.419 37.3 175-180 2 9.963 4.65 32 220-240 300 2 (Example 1) 16.881 0 54.2 200-210 2 14.884 0 47.7 250
[0140] Table 5 - Methane yields, quantities of methane and ethane produced, and temperatures recorded, for 0.5 g of LDPE
[0141] When the amount of iron wool is equal to 100 mg, the selectivity towards methane and the methane production rate are lower in the absence of the Pt / Siralox catalyst. Particularly surprisingly, when the amount of iron wool used is 200 mg or more (iron wool / initial polymer mass ratio greater than or equal to 0.4), the yield and the methane selectivity are substantially si- miliaries in the presence or absence of the Pt / Siralox catalyst.
[0142] The methane yields obtained for the different initial quantities of steel wool and the different reaction times, as well as the temperatures of the external wall surface of the FP bottles recorded after 10 min of reaction and the quantities of methane, ethane / ethylene and propane / propene obtained at the end of the reaction, for the initial condition of 1 g of LDPE, are indicated in Table 6.
[0143] [Tableauxô] Amount of steel wool (mg) Reaction time (h) Methane (mmol) Ethane / ethylene (mmol) Propane / propene (mmol) Ych4 (%) Temp. (°C) 100 2 6.15 4.22 / 0.9 1.30 / 1.8 9.9 210-220 5 8.36 4.42 / 1.0 1.58 / 1.8 13.4 180-200 15 12.55 5.18 / 0 1.87 / 1.3 20.1 200-210 200 2 10.98 6.40 / 0 2.10 / 1.7 17.6 200-215 5 15.64 6.80 / 0 3.88 / 0 24.1 200-210 15 32.16 7.19 / 0 0 51.6 220-230 300 2 29.05 0 0 46.6 265-370 5 32.35 0 0 51.9 250-275
[0144] Table 6 - Methane yields, quantities of methane, ethane / ethylene and propane / propene produced, and temperatures recorded, for the 1 g LDPE condition
[0145] It is observed that, for 100 mg of iron wool (iron wool / LDPE mass ratio of 0.1), the selectivity and the methane yield are low. For quantities greater than or equal to 200 mg of iron wool (iron wool / LDPE mass ratio greater than or equal to 0.2), the methane yield is much higher, and comparable to those obtained in the presence of Pt / Siralox catalyst.
[0146] For quantities greater than or equal to 300 mg of iron wool (iron wool / LDPE mass ratio greater than or equal to 0.3), the selectivity with respect to the formation of methane in the gas phase is particularly high.
[0147] An additional experiment was carried out with a different, thicker iron wool, formed of iron micro-wires of about 300 to 500 pm in diameter, and a few centimeters long. The protocol as described above was applied with: 1 g of low Mw LDPE, 300 mg of this iron wool, a dihydrogen atmosphere at 5 bars of H2, a reaction time of 2 h, 18% of the maximum amplitude of the magnetic field (29.3 mT, 2.6 kW). 27.68 mmol of methane were obtained, with a yield YCh4 = 44.4%. This experiment demonstrates that the dimensions of the micro iron wires do not modify the selectivity of the reaction towards methane and the methane yield.
[0148] E / Example 3 - Transformation of LDPE, HPDE and PP alone or in mixture with PS, in the presence of steel wool without catalyst
[0149] The operating protocol described in Example 1 was applied to different plastic materials (low Mw LDPE, high Mw LDPE, HDPE, PP) alone, or to an equimass mixture of low Mw LDPE, HDPE, PP and PS, or to fragments of 4 to 40 mm2 of LDPE bottle, using 1 g of polymer, mixture or fragments, and 300 mg of steel wool "FINE Steel Wool" as described above, without Pt / Siralox. The FP bottle was charged to a pressure of 5 bar in H2, then subjected to 18% of the maximum magnetic field amplitude, for 2 h or 5 h.
[0150] The results obtained, in terms of quantities of methane, ethane and propane obtained at the end of the reaction, and methane yields obtained, for 2 h of reaction, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction, are indicated in table 7.
[0151] [Tables?] Substrate Methane (mmol) Ethane (mmol) Propane (mmol) YcH4 (%) Temp. (°C) LDPE low Mw 29.04 0 0 46.6 265-270 LDPE high Mw 28.16 7.04 0 45.2 240-250 Bottle fragments LDPE 28.43 0 0 45.6 240-260 HDPE 20.08 6.92 4 32.2 260-280 PP 27.01 7.25 0 43.3 250-280 LDPE low Mw+ HDPE + PP + PS 27.22 7.14 0 43.7 240-260
[0152] Table 7 - Methane yields, quantities of methane, ethane and propane obtained at the end of the reaction, and temperatures recorded, for 2 h of reaction
[0153] It is observed that high methane yields, as well as good selectivity with respect to methane formation, are obtained for all substrates, including for the “LDPE low Mw + HDPE + PP + PS” mixture. A similar result is obtained for a “LDPE low Mw + HDPE + PP + PU” mixture (PU = polyurethane).
[0154] The results obtained, in terms of quantities of methane, ethane and propane obtained at the end of the reaction, methane yields obtained, for 5 h of reaction, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction, are shown in Table 8.
[0155] [Tables8] Substrate Methane (mmol) Ethane (mmol) Propane (mmol) YcH4 (%) Temp. (°C) LDPE low Mw 32.35 0 0 51.9 250-275 LDPE high Mw 31.83 7.12 0 51.1 240-250 Bottle fragments LDPE 28.43 0 0 51.6 240-260 HDPE 32.19 0 0 51.6 260-280 PP 33.92 0 0 54.4 250-280 LDPE low Mw+ HDPE + PP + PS 29.94 0 0 48.0 240-260
[0156] Table 8 - Methane yields, quantities of methane, ethane and propane obtained at the end of the reaction, and temperatures recorded, for 5 h of reaction
[0157] It is observed that the methane yield increases with the reaction time, as does the methane selectivity, a selectivity greater than 99% of methane being observed for all the substrates with the exception of high Mw LDPE, for which the selectivity of the reaction with respect to methane is still very high, greater than 80%.
[0158] F / Example 4 - Transformation of LPDE or octadecane, in the presence of steel wool without catalyst
[0159] The operating protocol described in Example 1 was applied to low Mw LDPE or octadecane (boiling temperature 317 °C), using 1 g of this substrate and 300 mg of “FINE Iron Wool” iron wool as described above, without Pt / Siralox. The FP bottle was charged to a pressure of 5 bar in H2, then subjected to 18% of the maximum magnetic field amplitude, for 2 h or 5 h.
[0160] The results obtained, in terms of quantities of methane, ethane and propane obtained at the end of the reaction, methane yields obtained, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction, are indicated in Table 9.
[0161] [Tables9] Substrate Reaction time (h) Methane (mmol) Ethane (mmol) Propane (mmol) YcH4 (%) Temp. (°C) LDPE 2 29.05 0 0 46.6 265-270 LDPE 5 32.35 0 0 51.9 250-275 Octadecane 2 34.60 8.4 0 55.5 200-225 Octadecane 5 32.34 0 0 51.9 220-240
[0162] Table 9 - Methane yields, quantities of methane, ethane and propane obtained at the end of the reaction, and temperatures recorded, for 2 h or 5 h of reaction
[0163] The results are particularly satisfactory for the two substrates tested.
[0164] G / Example 5 - Transformation of LDPE in the presence of iron wool without catalyst, for different quantities of iron wool
[0165] The operating protocol described in Example 1 was applied to low Mw LDPE using 1 g of this substrate and different quantities of iron wool "FINE iron wool" as described above (100, 200, 250, 300 and 350 mg), without Pt / Siralox. The FP bottle was charged to a pressure of 5 bar in H2, then subjected to 18% of the maximum magnetic field amplitude, for 2 h.
[0166] The results obtained, in terms of quantities of methane, ethane and propane obtained at the end of the reaction, methane yields obtained, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction, are indicated in table 10.
[0167] [TableauxlO] Quantity of steel wool (mg) Methane (mmol) Ethane / ethylene (mmol) Propane / propene (mmol) Ych4 (%) Temp. (°C) 100 6.15 4.22 / 0.89 1.30 / 1.78 9.9 210-220 200 10.98 6.40 / 0 2.10 / 1.69 17.6 200-215 250 26.57 7.87 / 0 0 42.6 220-240 300 29.05 0 0 46.6 265-270 350 29.66 0 0 47.6 250-285
[0168] Table 10 - Methane yields, quantities of methane, ethane and propane obtained at the end of the reaction, and temperatures recorded, for 2 h of reaction
[0169] The results, in terms of selectivity and methane yield, are excellent from 250 mg of iron wool, i.e. from a mass ratio of iron wool / polymer of 0.25. The selectivity towards methane is particularly important from 300 mg of steel wool, i.e. for steel wool / polymer mass ratios of 0.3 and above.
[0170] H / Example 6 - Transformation of LDPE in the presence of steel wool without catalyst, for different quantities of LDPE
[0171] The operating protocol described in Example 1 was applied to low Mw LDPE using different quantities (500, 1000 and 1500 mg) of this substrate and 300 mg of “FINE Iron Wool” iron wool as described above, without Pt / Siralox. The FP bottle was charged to a pressure of 5 bars in H2, then subjected to 18% of the maximum magnetic field amplitude, for 2 h or 5 h.
[0172] The results obtained, in terms of quantities of methane, ethane and propane obtained at the end of the reaction, methane yields obtained, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction, according to the reaction time, are indicated in Table 11.
[0173] [Tableauxll] Amount of LDPE (mg) Reaction time (h) Methane (mmol) Ethane (mmol) Propane (mmol) Ych4 (%) Temp. (°C) 500 2 14.88 0 0 47.7 250 1000 2 29.05 0 0 46.6 265-270 1000 5 32.35 0 0 51.9 250-275 1500 2 34.81 9.07 0 37.2 220-245 1500 5 43.30 9.29 0 46.3 230-240
[0174] Table 11 - Methane yields, quantities of methane, ethane and propane obtained at the end of the reaction, and temperatures recorded, for 300 mg of steel wool
[0175] The methane yield is excellent for all quantities of LDPE (iron wool / polymer mass ratios greater than or equal to 0.2). The selectivity towards methane is particularly important for 1000 mg of LDPE and less, that is to say for iron straw / polymer mass ratios greater than or equal to 0.3.
[0176] F Example 7 - Transformation of LDPE in the presence of iron in different forms, with Pt / Siralox catalyst
[0177] The operating protocol described in Example 1 was applied to low Mw LDPE (500 mg) and 200 mg of iron, either in the form of iron wool "FINE iron wool" as described above, or in the form of nanometric iron powder (average size 0.5 pm, SAR at 93 kHz and 47 mT of 1-10 W.g1), in the presence of 200 mg of Pt / Siralox. The FP bottle was charged at a pressure of 5 bars in H2, then subjected to 18% or 100% of the maximum magnetic field amplitude, for 2 hours.
[0178] The results obtained, in terms of quantities of methane, ethane and propane obtained at the end of the reaction, methane yields obtained, according to the reaction time, as well as the temperatures of the external surface of the wall of the FP bottles recorded after 10 min of reaction, are indicated in table 12.
[0179] [Tablesl2] Iron % field amplitude Methane (mmol) Ethane (mmol) Propane (mmol) Ych4 (%) Temp. (°C) Straw 18 11.61 4.42 0 37.3 175-180 Powder 100 neg. 0 0 0 150-200
[0180] Table 12 - Methane yields, quantities of methane, ethane and propane obtained at the end of the reaction, and temperatures recorded - "neg" means "negligible quantity"
[0181] The use of iron in the form of nanometric powder does not give rise to any production of methane, unlike micrometric iron wool.
Claims
Claims
1. Method for transforming a solid or liquid substrate (11) into hydrocarbon(s) chosen from substrates formed from plastic material(s) and heavy oils, by a transformation reaction occurring in a given temperature range, said method being characterized in that it comprises steps of: - bringing into contact, in a reactor (10), said substrate (11) and a micrometric heating element (12) formed from a ferromagnetic metal compound, under an atmosphere (23) devoid of oxygen, - and heating said heating element (12) by electromagnetic induction by means of a magnetic field inductor (18) external to said reactor (10), at a temperature included in said temperature range.
2. A method according to claim 1, wherein said substrate (11) is formed of solid or liquefied plastic material.
3. A method according to claim 1 or 2, wherein said substrate (11) is formed from polyolefin, polyolefin-based copolymer, polystyrene, or any mixture thereof.
4. Method according to any one of claims 1 to 3, according to which said heating element (12) is chosen from powders of particles based on said ferromagnetic metal compound with a size between 1 and 1000 pm, and wires based on said ferromagnetic metal compound having a wire diameter between 1 and 1000 pm.
5. Method according to any one of claims 1 to 4, according to which said ferromagnetic metallic compound is chosen from those having a magnetic anisotropy less than or equal to 8.104 J.m3.
6. A method according to any one of claims 1 to 5, wherein said ferromagnetic metal compound is selected from iron and its alloys.
7. A method according to any one of claims 1 to 6, wherein the magnetic field generated by said magnetic field inductor (18) has an amplitude of between 1 and 80 mT and a frequency of between 30 and 500 kHz.
8. A method according to any one of claims 1 to 7, wherein the atmosphere (23) in said reactor (10) is an inert atmosphere.
9. A method according to any one of claims 1 to 7, wherein the atmosphere (23) in said reactor (10) comprises dihydrogen.
10. A method according to any one of claims 1 to 9, wherein the mass ratio of said heating element (12) and said substrate (11), in said reactor (10), is greater than or equal to 0.
2.
11. A method according to any one of claims 1 to 10, wherein a catalytic metal compound catalyzing said transformation reaction is brought into contact with said substrate (11) and said heating element (12), in said reactor (10), during said heating step.
12. A method according to claim 11, wherein said catalytic metal compound is selected from platinum, ruthenium, manganese, cobalt, nickel, copper, zinc, rhodium, palladium, iridium and / or tin, or any alloy of one or more of these metals.
13. The method of claim 12, wherein said catalytic metal compound is platinum, deposited on a solid support.
14. A method according to any one of claims 1 to 13, wherein said reactor (10) is free of catalytic compound.
15. Method according to any one of claims 1 to 14, comprising a final step of recovering the gaseous fraction contained in the reactor (10).
16. Use of a micrometric heating element (12) formed from a ferromagnetic metal compound to transform into hydrocarbon(s), by heating said heating element (12) by electromagnetic induction, a solid or liquid substrate (11) chosen from substrates formed from plastic material(s) and heavy oils.
Citation Information
Patent Citations
Reactor and method for the at least partial decomposition, in particular depolymerization, and / or purification of plastic material
US20130303810A1
Process and apparatus for synthesizing multiwall carbon nanotubes from high molecular polymeric wastes
US20220055902A1
Low-temperature plastic depolymerization
WO2023064741A1