Sealing compound for aluminum parts and their alloys
A sealing composition using silicate, organosilane, and phosphate salts, combined with a chromium (III)/zirconium (IV) process, addresses the challenge of achieving high corrosion resistance and adhesion without hexavalent chromium, ensuring compliance with environmental regulations and broad applicability across aluminum alloys.
Patent Information
- Application Number
- FR2023005282
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Existing sealing technologies for aluminum alloys, particularly in the aeronautics sector, face challenges in achieving high corrosion resistance and adhesion of coatings while avoiding the use of toxic hexavalent chromium, and are not universally applicable across various alloy types.
A sealing composition comprising silicate salt, functional organosilane, and phosphate salt, combined with a chromium (III)/zirconium (IV) impregnation process, forms a silica gel and polymer network to enhance corrosion resistance and adhesion without using hexavalent chromium, suitable for all types of aluminum alloys.
The composition achieves corrosion protection exceeding 500 hours and excellent coating adhesion, meeting aeronautical industry standards, and is compatible with REACH regulations, applicable to a wide range of aluminum alloys.
Abstract
Description
Title of the invention: Sealing composition for aluminum parts and their alloys
[0001] The present invention belongs to the field of surface treatment of metal parts, and more particularly to treatments for the protection of the surfaces of aluminum and aluminum alloy parts.
[0002] It relates to a sealing composition used to obtain a corrosion-resistant coating in aggressive environments. It also relates to a process for treating aluminum or aluminum alloy parts using this composition.
[0003] Aluminum and its alloys are materials of choice widely used in the aeronautical field because, while they allow for a reduction in the mass of aircraft structures and therefore the energy consumption of aircraft, they can also offer excellent mechanical performance. Obtaining alloys with high mechanical properties that meet the requirements of this industrial sector requires the implementation of effective corrosion protection methods to ensure their durability. Several processes are generally combined to achieve optimal protection. A commonly used protection scheme involves the formation of an oxide layer on the metal surface by chemical or electrochemical conversion, before the application of an external coating (often a primer and a topcoat for protective and / or decorative purposes).
[0004] Chemical conversion coatings allow the development of a protective layer on the surface of the alloy, through chromating or phosphating. Chromating involves Cr₂O₇²⁻ ions, forming a layer rich in hexavalent chromium (Cr(VI)) and trivalent chromium (Cr(III)), which provides good corrosion resistance. This technology was widely used in the aerospace industry but raises pollution concerns. It is now prohibited and subject to authorization by the ECHA (European Chemicals Agency), so the number of treated parts is decreasing daily. In the following description, in accordance with standard chemical notation, hexavalent chromium refers to chromium in the +6 oxidation state, and trivalent chromium to chromium in the +3 oxidation state.
[0005] Anodizing (or anodic oxidation) is an electrochemical conversion process that increases the thickness of the oxide layer naturally present on the surface of aluminum alloys. Among the oldest processes is chromic anodic oxidation (COO), still used today, although some are not yet fully developed. particularly by aircraft manufacturers, despite the presence of hexavalent chromium in the baths. We also know sulfuric anodic oxidation (SAO), currently the most widespread process in the industrial sector, sulfo-tartaric anodic oxidation (SAO) carried out in a bath containing both sulfuric acid and tartaric acid, and phosphoric anodic oxidation (PAO) used mainly in the United States for aeronautical applications.
[0006] Regardless of the anodic oxidation technique used, it results in the formation of an aluminum oxide layer (or anodic layer) a few microns thick. The high porosity of this layer promotes the adhesion of organic, inorganic, or hybrid coatings (such as paints, adhesives, and sol-gels), but it does not provide good corrosion resistance. Indeed, due to its high porosity, and despite its thickness, the anodic layer is very sensitive to the surrounding atmosphere and external aggressions, leading to premature degradation. To increase its corrosion resistance, it is important to reduce its porosity through a complementary sealing operation.
[0007] For years, sealing has commonly been carried out by immersing the part to be anodized in an aqueous solution containing hexavalent chromium via a sodium or potassium dichromate solution, which may also contain other additives, for a fixed time and temperature. The mechanism involved is complex. It is generally stated in the literature that the aluminum oxides formed during anodizing are hydrated and converted into oxyhydroxide, a mineral similar to boehmite. The reaction is accompanied by swelling of the layer, resulting in the partial closure of the pores. Corrosion resistance and adhesion of the external coating are then generally of a good standard.
[0008] However, hexavalent chromium is harmful to the environment and to health due to its CMR (Carcinogenic, Mutagenic and Reprotoxic) nature and must be eliminated from industrial processes. Therefore, since 2007, with the REACH regulation (Registration, Evaluation and Authorisation of Chemicals), new sealing processes have been developed to replace those using Cr(VI)-based compounds.
[0009] In particular, processes have been proposed in which an impregnation step is carried out using a chromium(III) / zirconium(IV) solution, followed by a sealing step with nearly boiling water. These impregnation solutions, commercially available, for example under the brand names Surtec 650, Lanthane 613.3, SOCOSURF TCS, etc., have been successfully tested according to standard qualification methods on alloys of various grades (2024T451 and 7175T73), but nevertheless, relatively few have been tested. susceptible to corrosion. These impregnation solutions combined with water sealing do not allow the expected anti-corrosion performance to be achieved on much more sensitive wrought alloys (for example of type 2219T851, 2214T6, 2618AT8, 2219T6), nor on casting alloys such as those of type AS7G0.6T6, AS7U1GT6 and AU5NKZrT6.
[0010] Numerous other studies have been conducted over the past fifteen years to develop alternative techniques, as evidenced by the article "The Sealing Step in Aluminum Anodizing: A Focus on Sustainable Strategies for Enhancing Both Energy Efficiency and Corrosion Resistance", Ofoegbu SU et al., Coatings 2020, 10, 226; doi: 10.3390 / coatings 10030226. Examples include those based on the use of rare earths, particularly cerium salts; molybdate salts; hybrid solutions obtained from sol-gel, triethanolamine; potassium permanganates; rare earths associated with strong oxidants that convert oxides; or various electrophoretic solutions. Solutions based on PTFE (polyethylene terephthalate) polymers and copolymers exist but are not applicable to sealing all anodized areas and cannot receive a coating.
[0011] None of these techniques has been able to meet a broad range of specifications. None is suitable for treating all grades of aluminum alloys and can be used in conjunction with REACH-compliant anodizing techniques to achieve excellent corrosion resistance combined with coating adhesion. Thus, despite the significant amount of research on the subject, no technology currently appears sufficiently effective given the level of requirements of manufacturers, particularly in the aerospace sector.
[0012] As a result, potassium dichromate sealing in addition to anodizing treatments by OAS or TSA, still remains the reference as an anti-corrosion treatment for aluminum alloy parts, and is still used for the manufacture of aluminum parts intended for use in fields where parts are subjected to high stresses with regard to corrosion (braking systems in extreme environments, underwater drilling ...).
[0013] There is therefore a pressing need to develop new technologies for the protection of aluminum alloys that do not use toxic elements. In particular, the development of hexavalent chromium-free sealing compositions is a major objective for the aerospace, space, and other sectors.
[0014] An aluminum alloy is defined as an alloy in which aluminum is the predominant component (by mass), with at least 80% aluminum, but generally more than 90% and often more than 95%. The alloying elements can be metals of all kinds, including copper, magnesium, manganese, iron, nickel, titanium, Chromium and silicon metals are present in varying concentrations and combinations depending on the desired properties. The different types of alloys are classified into series and grades, the designations of which are standardized and well-known to professionals in the field.
[0015] According to a first aspect, the present invention aims to provide a sealing solution whose chemical composition complies with REACH regulations, in particular one that is free of chromium (VI). Such a composition must be usable in a sealing process compatible with the usual anodizing treatments for aluminum alloy parts. Another objective of the invention is to provide a sealing composition for aluminum alloys that achieves corrosion protection performance of more than 500 hours, and potentially up to 1000 hours, after exposure to neutral salt spray (NSS). A further objective is to provide a sealing composition that ensures good adhesion of paints used as external coatings, including the new non-chromate paints now available.Another objective is to have a sealing composition that can be used with all types of aluminum alloys, including those that have atypical behaviors compared to most others.
[0016] According to a second aspect, the invention aims to provide a sealing process for aluminum alloys that is effective in terms of corrosion protection and coating adhesion, and thereby complies with environmental standards. The process according to the invention must prevent the formation of chromium(VI) both in the sealing composition and in residual form on the treated parts. Another objective of the invention is to have a universal treatment, that is to say, one that can be used in conjunction with all anodizing processes used in industry, and one that is suitable for a wide range of aluminum alloy grades. Aluminum alloys used in the civil and military aeronautics, space, and defense sectors are particularly targeted. Finally, an objective of the invention is to have a process that is not difficult to master industrially.
[0017] It is to meet these needs and objectives that the composition which is the subject of this application was developed. It essentially comprises three compounds whose combined action makes it possible to overcome the drawbacks mentioned above. The first two are silica compounds, one of which is mineral and the other organic, and the third compound is a phosphate additive.
[0018] More specifically, the present invention relates to a sealing composition for the treatment of aluminum or aluminum alloy parts, comprising, in aqueous solution: - a silicate salt; - a functional organosilane belonging to the alkoxysilane family with the formula: (Ri-O)3 - Si - R2 (I) or (RrO)3 - Si - (CH2)n- O - R2 (II) in which Ri represents a linear or branched alkyl radical with 1 to 5 carbon atoms; n is an integer that can take the values from 0 to 5; R2 represents an alkyl radical, an amine radical or an epoxy radical; and - a phosphate salt.
[0019] The silicate salt's role is to form a silica gel within the pores of the anodic layer, where it then performs a sealing function. The transition from the soluble basic silicate form, SiO32, to the form of a silica precipitate, Si(OH)4, and then SiO2, in a gel state, results from the acidification of the sealing composition in the vicinity of the anodic layer and the pores. The silica gel is a good sealing agent because it is insoluble and exhibits good chemical inertness. However, due to its high hydrophilicity, it tends to absorb water and swell when in contact with a humid environment, which causes blistering of the external coatings and, more generally, leads to adhesion problems.
[0020] However, unexpectedly, its use in a mixture with a second sealing agent chosen from among the silicon organic compounds proved capable of preventing this phenomenon: the adhesion of the paints is significantly improved, without negatively affecting the corrosion resistance properties. This silicon organic compound (or organosilane) is more specifically chosen from the family of functional trialkoxysilanes.
[0021] It has also been observed that adding a phosphate additive to these two sealing agents further enhances the adhesion properties of the sealing composition. This phosphate compound is a phosphate salt whose action has been elucidated: it is capable of forming a precipitate with aluminum ions present in the anodic layer, in an AlPO4-type form with low solubility (solubility product Ks = 10¹⁹²). This additional precipitation during sealing is the proposed explanation for the marked strengthening of the adhesion of the sealing layer during its formation.
[0022] We thus have a sealing composition made up of three compounds acting in synergy, so that it offers corrosion resistance and adhesion properties at unsurpassed levels, without resorting to harmful and prohibited ingredients such as Cr(VI).
[0023] According to a preferred feature of the composition of the invention, the silicate salt is chosen from sodium silicate, potassium silicate, or lithium silicate. It can be supplied indifferently in solid form or as a solution of defined concentration, possibly in a mixture.
[0024] According to a further preferred feature of the composition that is the subject of the invention, the Silicate salt is sodium silicate present at a concentration ranging from 7 g / L to 20 g / L.
[0025] According to the invention, the composition comprises an alkoxysilane of formula (I) or (II), having three identical alkoxy (-ORi) substituents, in which the Ri group is an alkyl radical, which may be linear or branched, and which comprises from 1 to 5 carbon atoms. Advantageously, Ri comprises 1 or 2 carbons, forming methoxyl or ethoxyl groups with the oxygen. Thus, according to a preferred feature of the sealing composition, Ri is a methyl or ethyl radical.
[0026] The fourth substituent of silicon is a functional group that can be in two forms, namely a radical R2 directly linked to silicon (compound (I)), or separated from it by an oxygen atom accompanied or not by a hydrocarbon chain (compound (II)).
[0027] According to a first embodiment, the sealing composition according to the invention comprises an organosilane of formula (I), wherein R2 is an alkyl radical having from 1 to 10 carbon atoms, or a primary amine radical, or an epoxy radical. R2 may, in particular, be an ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, or aminoethyl, aminopropyl, or aminobutyl radical. Preferably, the primary amine function is in the terminal position.
[0028] According to a second embodiment, the sealing composition according to the invention comprises an organosilane of formula (II), in which n can take the values from 0 to 3 and R2 is an alkyl radical having from 1 to 5 carbon atoms or an epoxy radical. The oxygen atom can be directly bonded to the silicon, in which case n = 0. The R2 group can be, in particular, a methyl, ethyl, propyl, butyl, or glycidyl radical.
[0029] In a preferred embodiment, the composition according to the invention comprises an organosilane selected from (3-glycidyloxypropyl)-trimethoxysilane, (3-aminopropyl)-triethoxysilane, tetraethoxysilane, octyl-trimethoxysilane or OTMS.
[0030] (3-glycidyloxypropyl)-trimethoxysilane, abbreviated as GPTMS, is an organosilane of formula (II) in which Ri = - CH3, n = 3 and R2 = - C3H5O.
[0031] (3-aminopropyl)-triethoxysilane, abbreviated as APTES, is an organosilane of formula (I) in which Ri = - CH2- CH3 and R2 = - (CH2)3 - NH2.
[0032] Tetraethoxysilane, abbreviated as TEOS, is an organosilane of formula (II) in which - CH2- CH3, n = 0 and R2 = - CH2- CH3.
[0033] Octyl-trimethoxysilane, also designated OTMS, is an organosilane of formula (I) in which Ri = - CH2- CH3 and R2 = - (CH2)7- CH3.
[0034] According to a preferred feature of the sealing composition, the organosilane is (3-glycidyloxypropyl)-trimethoxysilane present at a concentration ranging from 0.5 g / L to 1.5 g / L. It is introduced into the sealing composition via a solution of purity greater than 95%, commercially available.
[0035] In an advantageous embodiment, the composition according to the invention may comprise from 7 g / L to 15 g / L of sodium silicate, and from 0.7 g / L to 1.3 g / L of GPTMS. In a preferred embodiment, the composition according to the invention may comprise from 8 g / L to 12 g / L of sodium silicate, and from 0.8 g / L to 1.2 g / L of GPTMS.
[0036] In general, care will be taken to ensure that, whatever the respective concentrations retained for the sealing agents, the silicate salt and the GPTMS are in a defined mass ratio, which can range from 20:1 to 1:1, and more commonly from 20:1 to 5:1.
[0037] The sealing composition comprises a phosphate salt capable of precipitating aluminum ions from the substrate. Various salts may be used, provided that their solubility in the sealing composition is sufficient to perform their function without affecting the process. Sodium or potassium phosphates may be used, while lithium salts are unsuitable.
[0038] Therefore, according to a preferred feature of the composition of the invention, the phosphate salt is selected from disodium phosphate (Na2HPO4), trisodium phosphate (Na3PO4), dipotassium phosphate (K2HPO4), tripotassium phosphate (K3HPO4), or a mixture of at least two of them. Even more preferably, the sealing composition according to the invention comprises disodium phosphate at a concentration ranging from 0.1 g / L to 5 g / L. Even more preferably, the composition comprises from 0.3 g / L to 0.7 g / L of disodium phosphate.
[0039] The composition according to the invention may include a fourth compound, in this case lithium hydroxide (LiOH). The addition of a small amount of lithium hydroxide makes it possible to obtain excellent corrosion resistance for all the alloys tested. Indeed, for certain grades of aluminum alloys treated with a sealing composition lacking this compound, slight defects may appear after corrosion tests. Therefore, in a particular embodiment, the composition according to the invention also includes lithium hydroxide at a concentration ranging from 0.005 g / L to 0.2 g / L.
[0040] To perform their function effectively, the compounds in the sealing composition must be in a distinctly basic environment. Therefore, said composition includes at least one basic compound in sufficient quantity to bring its pH to a value ranging from 10 to 12. Preferably, a pH of 10.5 to 11.5 is chosen, and even more preferably, the pH of the composition is adjusted to between 11 and 11.5. It goes without saying that the nature of the base and its concentration will be taken into account in order to determine the quantity to be added to bring the pH of the sealing composition to the desired value. The pH adjustment can be carried out by means of various bases known to those skilled in the art, alone or possibly in mixtures. Sodium hydroxide is conveniently used, but it is also advantageous to use lithium hydroxide here, since it may be present elsewhere in the composition, as explained previously.
[0041] Thus, advantageously, the composition according to the invention comprises at least one basic compound selected from sodium hydroxide, potassium hydroxide, lithium hydroxide, or a mixture thereof.
[0042] The sealing composition described above achieves unprecedented performance levels that fully meet the requirements of aircraft manufacturers' specifications, both in terms of corrosion resistance and coating adhesion. This result is based on the simultaneous use of two sealing agents, one of which forms a silica gel and the other creates a polymer network that prevents the silica from swelling, along with the introduction of a precipitating agent with the aluminum.
[0043] Aluminum and aluminum alloy parts can advantageously undergo a surface treatment using this sealing composition, by a process that is also the subject of the present invention. The sealing process is carried out on parts whose surface has a porous aluminum oxide layer obtained beforehand by an anodic oxidation operation, according to one of the techniques known in the prior art.
[0044] The sealing process for aluminum alloy parts according to the invention then takes place in two essential steps. The first step consists of impregnating the parts with a chromium(III) / zirconium(IV) solution, so that the porous layer takes on an acidic character. The second step allows for the actual sealing, by immersing the parts in a sealing composition as described above.
[0045] The present invention thus relates to a method for sealing the porous layer of aluminum or aluminum alloy parts that have undergone prior surface treatment (by anodizing), comprising the steps of: a) - immerse the parts in a chromium (III) / zirconium (IV) bath to impregnate the porous layer of the parts, then b) - immerse said parts in a sealing composition as described above, to seal said porous layer.
[0046] Zirconium is present in the impregnation bath in the +4 oxidation state, for example in the form of sodium hexafluorozirconate (Na2ZrF6) or potassium hexafluorozirconate (K2ZrF6), while chromium(III) is supplied by solubilized chromium sulfate (Cr2(SO4)3) producing hydrated chromium(III) ions Cr(H2O)63+, more simply denoted Cr3+. Solutions based on trivalent chromium and Tetravalent zirconium, free of CMR compounds, are also offered in manufacturers' catalogues.
[0047] According to a preferred embodiment of the sealing process according to the invention, the chromium(III) / zirconium(IV) bath is prepared from hexafluorozirconate and chromium oxide. This impregnation step is responsible for acidifying the surface of the parts.
[0048] The impregnation step can be carried out according to different protocols. According to the invention, this first impregnation step (step a) is generally carried out at a temperature of 30°C to 45°C for a treatment time of approximately 3 to 20 minutes. The concentrations used are those recommended by the suppliers, in accordance with the manufacturers' requirements. A draining and / or drying operation may be required.
[0049] In the second step of the claimed process (step b), the parts are immersed in a sealing composition as described above. According to a preferred embodiment, during this step, the parts remain in the sealing composition, maintained at a temperature between 94°C and 98°C, for 15 to 60 minutes. In a preferred embodiment, the parts may remain in the sealing composition for 30 minutes at a temperature of 97°C.
[0050] The inventive process described above, with implementation of the sealing composition as defined above, thus provides a sealing technology for aluminum and aluminum alloy parts that is free of chromium VI and compatible with anodizing treatments authorized by REACH regulations. This technology achieves corrosion protection performance of over 500 hours and up to 1000 hours after exposure to salt spray, as well as grade 0 dry and wet paint adhesion, particularly with new non-chromate paints. Furthermore, it achieves the same performance with the various impregnating products used prior to sealing. To date, no solution providing such performance had been proposed.
[0051] The present invention will be better understood and relevant details thereof will become apparent in light of the following description of various embodiments. EXAMPLE 1: Sealing composition Cl
[0052] A sealing composition Cl with the following formula was prepared: - Na2SiO3: 10 g / L - (3-glycidoxypropyl)-trimethoxysilane: 1 g / L - Na2HPO4: 0.5 g / L - LiOH: 0.2 g / L
[0053] On an industrial scale, a 360 L bath is prepared by putting into aqueous solution: - 9.5 kg of a sodium silicate solution; - 3.6 kg of a commercial solution comprising 3-GPTMS and LiOH; - 0.18 kg of sodium phosphate in solid form.
[0054] The sodium silicate source used is a 38-39% sodium silicate solution with a density of 1.38 and a %SiO2 / %Na2O ratio between 2.9 and 3.2. The pH is between 11 and 11.5. EXAMPLE 2: C2 Sealing Composition
[0055] A C2 sealing composition of the following formula was prepared, using the same reagents as before: - Na2SiO3: 15 g / L - (3-glycidoxypropyl)-trimethoxysilane: 1.3 g / L - Na2HPO4: 0.7 g / L - LiOH: 0.2 g / L EXAMPLE 3: C3 Sealing Composition
[0056] A C3 sealing composition of the following formula was prepared, using the same reagents as before, except for LIOH which is absent: - Na2SiO3: 10 g / L - (3-glycidoxypropyl)-trimethoxysilane: 1 g / L - Na2HPO4: 0.5 g / L
[0057] EXAMPLE 4: Impregnation and sealing treatment of parts
[0058] Impregnation stage
[0059] The first step of the process according to the invention is impregnation of the parts in an acid bath. In this way, the silica gel can form in the spores of the surface of the treated parts even though the silicate salt of the sealing composition from which it originates is basic.
[0060] Its mechanism is explained in the following sequence of reactions, taking place in the vicinity of the aluminum hydroxide layer A1(OH)3 present on the surface of the parts: 1) Recovery of hydroxides associated with Al3+ by Cr3+ and precipitation of Cr(OH)3 Cr3++ 3OH -> Cr(OH)3 (s) 2) Reaction between Al3+ and ZrF62, release of ZU+ ions Al3+ + ZrF62 -> A1F63 + ZU+ 3) Recovery of hydroxides by ZrF62 ZrF62 (aq) + 4OH -> ZrO2-2H2O (s) + 6F (aq)
[0061] The consumption of hydroxide ions is responsible for the acidification of the layer at the level of the pores.
[0062] The impregnation bath was prepared from a commercial product containing chromium (III) and zirconium (IV) (Lanthane 613.3 distributed by COVENTYA). The impregnation is carried out at a pH of 3.9 at a temperature of 35°C + / - 5°C for 5 to 15 minutes, generally for 10 minutes. The parts are then drained and dried before carrying out the sealing step.
[0063] Sealing step
[0064] The sealing step itself was carried out by immersing the parts in the Cl, C2, or C3 compositions described above, at a pH of 11 to 11.5, for 30 min, at a temperature of 97°C.
[0065] EXAMPLE 5: Performance of composition Cl with regard to corrosion
[0066] Tests were carried out to show the effectiveness of sealing by a composition according to the invention, as well as the influence of the impregnation step, on the level of performance in terms of corrosion resistance obtained on anodized layers of different grades of aluminum alloy.
[0067] The parts underwent anodizing using one of the known techniques: conventional sulfuric acid anodic oxidation (SAA) or new generation sulfuric acid anodic oxidation (NGA), long cycle sulfotartaric acid anodic oxidation (TS CL) or short cycle sulfotartaric acid anodic oxidation (TSA CC). Impregnation with a commercial Cr(III) / Zr(IV) solution, marketed under the name Lanthane 613.3, was carried out on some of them. Finally, sealing with the Cl composition shown in Example 1 was performed.
[0068] Corrosion resistance performance was evaluated by a salt spray test (defined by the international standard EN ISO 9227), by counting the number of pits per dm² appearing on the part. The conformity criterion meeting the specifications is a number of pits less than 5 after 500 h of exposure to salt spray. The results are presented in Table 1. They are rated according to the number of pits observed (piq), as compliant (++) for piq < 5, average (+ / -) for 5 < piq < 10, or non-compliant (—) for piq > 10.
[0069] [Tables 1] Anodizing Impregnation Solution Alloy 2024 2618 7175 AU5NKZr TSA CL Lanthanum 613.3 ++ ++ ++ ++ OAS NG Lanthanum 613.3 ++ ++ ++ + / - TSA CC ___ + / - ++ OAS ___ — — + / - —
[0070] It has been observed that, in the absence of treatment with a sealing composition, corrosion resistance is very insufficient, even poor. However, the results are good when the samples have been pre-sealed with Lanthanum 613.3 solution, then sealed with composition CL. This highlights that The impregnation step is essential. The determining role of treatment with a sealing composition Cl according to the invention is clearly demonstrated, on different types of anodizing and on different aluminum substrates, including on alloys very sensitive to corrosion such as FAU5NKZR.
[0071] EXAMPLE 6: Performance of composition Cl with regard to adhesion
[0072] Tests were carried out to demonstrate the effectiveness of sealing with the Cl composition according to the invention, on the performance obtained in terms of coating adhesion to anodized layers of different grades of aluminum alloy. As before, the parts underwent anodizing using one of the known techniques. They were then impregnated in a Cr(III) / Zr(IV) bath as described in Example 4, followed by sealing with the Cl composition. Finally, a coating was applied to the parts. The paints used were water-based and solvent-based, chromated and non-chromated.
[0073] Adhesion was evaluated for each test according to ISO 2409, in dry conditions (without aging) and in wet conditions (after 14 days of immersion in an aqueous solution). The results are noted on a scale of 0 to 5, where grade 0 corresponds to the best level of adhesion. They are presented in Tables 2a and 2b (dry adhesion and wet adhesion, respectively).
[0074] [Tables2a] Dry adhesion Alloy 2024 2618 7175 AU5NKZr TSA CL 0 0 0 0 OAS NG 0 0 0 0 TSA CC 0 0 0 0 OAS 0 0 0 0
[0075] [Tables2b] Wet adhesion Alloy 2024 2618 7175 AU5NKZr TSA CL 0 0 0 0 OAS NG 0 0 0 0 TSA CC 0 0 0 0 OAS 0 0 0 0
[0076] It is necessary to achieve grades 0 or 1 to comply with the criteria required by aircraft manufacturers. All samples are graded at grade 0, which shows that they exhibit excellent coating adhesion, and this on the different substrates tested.
[0077] The two examples above show that the sealing composition Cl according to the invention achieves very good performance in terms of both corrosion resistance and paint adhesion. It thus surpasses existing treatments and meets the stringent specifications of the aerospace industry. EXAMPLE 7: Performance of composition C2
[0078] The formula of composition C2 is identical to that of Cl in its components but differs in their concentration. Samples of the same aluminum alloys were treated in the same way as before. The pH, temperature, and treatment time conditions are unchanged.
[0079] The performance of this C2 composition was studied according to identical protocols. The number of pits on the samples after 500 hours of exposure to salt spray remained below 15: the corrosion resistance performance therefore remains very high and in accordance with the specifications. Paint adhesion is also satisfactory, with a grade of 0 observed for the 4 alloys tested. The results are essentially the same as those obtained for composition CL. EXAMPLE 8: Performance of composition C3
[0080] The formula of composition C3 is identical to that of Cl, its first three components being present at the same concentrations. The fourth component, lithium hydroxide, is not present. Samples of aluminum alloys underwent anodizing by OAS, followed by impregnation with a chromium(III) solution, marketed under the name TCS / PACS by the company Socomore. Sealing was carried out in the same manner as before. The pH, concentration, temperature, and treatment time conditions were adapted to comply with the conditions recommended by the suppliers of the impregnation solutions: TCS (temperature: 35-45°C, immersion time: 18-22 minutes); PACS (temperature: 15-30°C, immersion time: 4-6 minutes). The thickness of the coatings obtained ranges from 3 µm to 12 µm (depending on the alloys treated), which corresponds to the manufacturers' requirements for aeronautical applications.
[0081] Corrosion resistance and paint adhesion were tested according to ISO 9227. The results are presented in Table 3.
[0082] [Tables3] Alloy Thickness (pm) Clogging (grade) BS Exposure Test (pits / dm2) 24 h 48 h 96 h 192 h 384 h 480 h 576 h 2024 10.2 0 0 0 0 0 0 0 0 2618 8.2 0 0 0 0 0 0 0 3-4 7175 7.2 0 0 0 0 0 0 0 AU5NKZ r 9.8 0 0 0 0 0 0 < 10 < 10
[0083] The performance of the sealing composition remains satisfactory and meets the required level, despite a slight decrease in corrosion resistance for the 2618 and AU5NKZr alloys around 500 hours of salt spray (BS) exposure. This decrease is limited, remaining below 10 pits after 500 hours of BS exposure. Paint adhesion is also good, with a grade of 0 for all four alloys tested. The results obtained are thus of an excellent overall standard, demonstrating the feasibility of using the compositions according to the invention in conjunction with various anodizing techniques. EXAMPLE 9: C4 Sealing Composition
[0084] A C4 sealing composition was prepared, based on the Cl composition of Example 1, in which LiOH and Na2HPO4 were replaced by Li2HPO4. Since the active species are HPO42 and Li+, the use of this compound could be chemically equivalent, although its cost is very high compared to that of LiOH and Na2HPO4. Furthermore, its solubility is very low (less than 0.25 g / L), so the concentration introduced cannot be equivalent to those used in the CL composition.
[0085] The formula for composition C4 is as follows: - Na2SiO3: 10 g / L - (3-glycidoxypropyl)-trimethoxysilane: 1 g / L - Li2HPO4: 0.25 g / L
[0086] Aluminum alloy parts were treated with various types of anodizing and impregnation, followed by sealing with composition C4. Salt spray tests were performed. The corrosion resistance performance of the coating obtained with this composition is described in Table 4. The part is considered compliant (C) if it exhibits fewer than 5 pits after 500 h of salt spray exposure; otherwise, it is considered non-compliant (NC).
[0087] [Tables4] Anodizing Impregnation solution Alloy 2024 2618 7175 AU5NKZr OAS fine TCS / PACS (Socomore) CCC NC TSA CL Lanthanum 613.3 (Coventya) CCC NC OAS Lanthanum 613.3 (Coventya) NC C c NC OAS Surtec 650 (SURTEC) NC cc C
[0088] It is observed that the performance does not meet the previous results. In particular, corrosion resistance is not compliant on two alloys (grades 2024 and AU5NKZr). Furthermore, it is noted that different types of anodizing and impregnation are involved prior to sealing by composition C4. Therefore, this composition does not possess the desired universal properties.
Claims
Claims
1. Sealing composition for the treatment of aluminum or aluminum alloy parts, characterized in that it comprises, in aqueous solution: - a silicate salt, - a functional organosilane belonging to the family of alkoxysilanes of formula: (Ri-O)3 - Si - R2 (I) or (RrO)3 - Si - (CH2)n- 0 - R2 (II) in which Ri represents a linear or branched alkyl radical containing from 1 to 5 carbon atoms; n is an integer which can take the values from 0 to 5; R2 represents an alkyl radical, an amine radical or an epoxy radical; and - a phosphate salt.
2. Sealing composition according to claim 1, characterized in that the silicate salt is chosen from sodium silicate, potassium silicate, lithium silicate.
3. Sealing composition according to claim 1 or 2, characterized in that the silicate salt is sodium silicate present at a concentration ranging from 7 g / L to 20 g / L.
4. Sealing composition according to one of the preceding claims, characterized in that Ri is a methyl or ethyl radical.
5. Sealing composition according to one of the preceding claims, characterized in that it comprises an organosilane of formula (I), in which R2 is an alkyl radical having from 1 to 10 carbon atoms, or a primary amine radical, or an epoxy radical.
6. Sealing composition according to one of claims 1 to 4, characterized in that it comprises an organosilane of formula (II), in which n can take the values from 0 to 3 and R2 is an alkyl radical having from 1 to 5 carbon atoms or an epoxy radical.
7. Sealing composition according to one of claims 1 to 4, characterized in that it comprises an organosilane chosen from (3-glycidyloxypropyl)-trimethoxysilane, (3-aminopropyl)-triethoxysilane, tetraethoxysilane, roctyl-trimethoxysilane.
8. Sealing composition according to the preceding claim, characterized in that the organosilane is (3-glycidyloxypropyl)-trimethoxysilane present at a concentration ranging from 0.5 g / L to 1.5 g / L.
9. Sealing composition according to one of the preceding claims, characterized in that it comprises from 7 g / L to 15 g / L of sodium silicate, and from 0.7 g / L to 1.3 g / L of (3-glycidyloxypropyl)-trimethoxysilane.
10. Sealing composition according to one of the preceding claims, characterized in that the phosphate salt is chosen from disodium phosphate, trisodium phosphate, dipotassium phosphate, tripotassium phosphate, or a mixture of at least two of them.
11. Sealing composition according to the preceding claim, characterized in that it comprises from 0.1 g / L to 5 g / L of disodium phosphate.
12. Sealing composition according to any one of the preceding claims, characterized in that it comprises lithium hydroxide at a concentration ranging from 0.005 g / L to 0.2 g / L.
13. Sealing composition according to one of the preceding claims, characterized in that it further comprises at least one basic compound in a quantity sufficient to bring the pH of the composition to a value ranging from 10 to 12.
14. Sealing composition according to the preceding claim, characterized in that said at least one basic compound is chosen from sodium hydroxide, potassium hydroxide, lithium hydroxide, or a mixture thereof.
15. Method for sealing the porous layer of aluminum or aluminum alloy parts having undergone a prior surface treatment, characterized in that it comprises the steps consisting of: a) - immersing the parts in a chromium (III) / zirconium (IV) bath to impregnate the porous layer of the parts, then b) - immersing said parts in a sealing composition according to one of the preceding claims to seal said porous layer.
Citation Information
Patent Citations
Hole sealing agent and method for aluminum and aluminum alloy anode oxide film aftertreatment
CN106400085A
Method for sealing aluminum alloys
US20230059040A1
Cited By
A PROCESS FOR SEALABLES OF ALUMINUM ALLOYS USING A SILANE AND A PART BASED ON ALUMINUM OR AN ALUMINUM ALLOY OBTAINED BY THIS PROCESS
FR3162446A1
Method for sealing aluminum alloys using a silane and aluminum-based or aluminum alloy-based part obtained by this method
WO2025242997A1