Method for manufacturing a part in a biodegradable mold containing lanthanum oxide

The use of lanthanum oxide or lanthanum hydroxide molds in a water vapor environment addresses the challenges of shaping and demolding complex parts by ensuring homogeneous densification and preventing carbon contamination, enabling easy part retrieval.

FR3157237B1Active Publication Date: 2026-10-30COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2023014575
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2026-10-30
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

The shaping of complex-shaped parts and the removal of these parts from molds, particularly in foundry work, is challenging due to issues like carbon contamination and part breakage during demolding, which existing molds made of graphite cannot adequately address.

Method used

A method involving the use of a mold containing lanthanum oxide or lanthanum hydroxide, which undergoes hydrolysis in a water vapor environment, leading to mold degradation and allowing for easy recovery of the part without demolding, while maintaining the integrity of the part.

Benefits of technology

Enables the efficient shaping and easy removal of complex-shaped parts by ensuring homogeneous densification and preventing carbon contamination, with the mold degrading into a powder form, facilitating part retrieval.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000013_0000
    Figure 00000013_0000
  • Figure 00000013_0001
    Figure 00000013_0001
  • Figure 00000013_0002
    Figure 00000013_0002
Patent Text Reader

Abstract

A process for manufacturing a part, the process comprising the following successive steps: a) shaping the part by: - ​​solidifying a liquid bath contained in a sintered mold containing lanthanum oxide, or - sintering a charge to be sintered contained in a mold containing lanthanum hydroxide or in a sintered mold containing lanthanum oxide, b) cooling the part in the mold, and c) maintaining the assembly formed by the part and the mold in a gaseous medium containing water vapor for a holding time suitable for degrading the mold under the effect of the hydrolysis of the lanthanum oxide by the water contained in the gaseous medium. No abbreviated figure
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for manufacturing a part in a biodegradable mold containing lanthanum oxide. Technical field

[0001] The present invention relates to the shaping of cast or sintered parts. More particularly, it relates to the implementation of a mold adapted to this shaping. Previous technique

[0002] Uniaxial sintering allows the production of complex-shaped parts. A complex-shaped part has at least one of the following characteristics: hole in the compression axis, portions of the part extending at different heights measured along the compression axis, inclined faces not parallel and not perpendicular to the compression axis, absence of an axis of revolution, non-planar faces.

[0003] The shaping of complex shaped parts requires the use of suitable molds in order to obtain homogeneous densification of the sintered part, easy demolding, and which also prevent carbon contamination of at least the portion of the part in contact with the tooling which is generally made of graphite which provides carbon.

[0004] Moreover, in the field of foundry work, removing a part from the foundry mold can be complex and lead to breakage of the part.

[0005] There is a permanent need to facilitate the shaping of complex-shaped parts and the removal of these parts from the mold. Description of the invention

[0006] The invention proposes a method for manufacturing a part, the method comprising the following successive steps: a) shaping the part by: - solidification of a liquid bath contained in a sintered mold containing lanthanum oxide, or - sintering of a sintering charge contained in a mold containing lanthanum hydroxide or in a sintered mold containing lanthanum oxide, b) cooling of the part in the mold, and c) maintaining the assembly consisting of the part and the mold in a gaseous medium containing water vapor for a holding period suitable for degrading the mold under the effect of the hydrolysis of lanthanum oxide by the water contained in the gaseous medium.

[0007] The invention essentially eliminates the demolding step, as the degraded mold no longer has its own integrity due to the hydrolysis of lanthanum oxide. The hydrolysis of lanthanum oxide to lanthanum hydroxide induces a volume change that generates a progressive pulverization of the mold into a powder of lanthanum hydroxide particles during the holding period. The molded part can thus be recovered directly. Detailed description

[0008] The mold comprises lanthanum oxide or lanthanum hydroxide.

[0009] The mold may further comprise a refractory compound selected from BN, Si3N4, Al2O3, ZrO2, HfO2, SiC, and mixtures thereof. The refractory compound provides thermal stability suitable for shaping the part, particularly by melting and solidification. It can thus be adapted to the specific properties of the part's constituent material and, in particular, is preferably chemically inert with respect to the part's constituent material. Moreover, advantageously, the refractory compound is inert with respect to lanthanum oxide and therefore does not hinder the degradation of lanthanum oxide in step c). In addition, the refractory compound makes it possible to increase the temperature range for using the mold to manufacture the part.

[0010] According to a first embodiment, the mold is sintered.

[0011] The mold may consist of lanthanum oxide, the refractory compound and less than 1% of other constituents. Preferably, it consists of lanthanum oxide and the refractory compound.

[0012] Throughout this description, "other constituents" means all constituents other than La2O3, La(OH)3, BN, Si3N4, Al2O3, ZrO2, HfO2, and SiC. For example, other constituents are impurities, meaning they are introduced unintentionally and necessarily with the raw materials. Impurities are not necessary constituents, but merely tolerated.

[0013] Furthermore, the mold preferably comprises more than 10%, and preferably more than 25%, lanthanum oxide. An increase in the lanthanum oxide content accelerates the degradation of the mold after the part has cooled.

[0014] According to a second embodiment, the mold includes lanthanum hydroxide and the part is shaped by sintering.

[0015] The mold may consist of lanthanum hydroxide and less than 1% of other constituents. It may consist of lanthanum hydroxide.

[0016] Alternatively, the mold consists of lanthanum hydroxide, the refractory compound, and less than 1% of other constituents. Preferably, it consists of lanthanum hydroxide and the refractory compound.

[0017] Preferably, the mold is preformed and comprises agglomerated particles, optionally bonded by means of a binder. The agglomerated particles are bonded together by contact with each other. They are not bonded together by a common material bridge, as is the case in a sintered part. A preformed mold exhibits low tensile strength, but preferably sufficient for handling. Preferably, the preformed mold is obtained by compressing a starting charge comprising particles made of the mold's constituent material. The mold is preferably manufactured by the production method according to the invention described below.

[0018] Preferably, the mold is sintered during the sintering of the part, at a temperature above the reaction temperature of lanthanum hydroxide to lanthanum oxide, preferably at 900°C or more.

[0019] Furthermore, the mold has a cavity to receive the liquid bath or the charge to be sintered.

[0020] According to one embodiment, the process involves shaping the mold by solidifying the liquid bath. The process includes filling the mold by pouring the liquid bath into the cavity.

[0021] According to another embodiment, the process involves shaping the material to be sintered by sintering. The material to be sintered is in the form of particles after the mold has been filled. During sintering, the particles are bonded together by the action of heat to form the part. Preferably, the sintering process involves applying uniaxial compression to densify the part by reducing the porosity between the particles.

[0022] The part can be made of a ceramic or metallic material. Preferably, the part is made of a metallic material. For example, the metallic material is chosen from steels, aluminum alloys, copper alloys and titanium alloys.

[0023] In step b), the part and the mold are preferably cooled to a temperature below 100 °C, preferably below 50 °C, in particular between 20 °C and 30 °C.

[0024] In step c), the gaseous medium is preferably air, the humidity level of which is preferably greater than 40%. Such a humidity level allows handling of the assembly formed by the part and the mold, for example between the part forming device and a storage location, without damage to the mold, while allowing for mold degradation during handling.

[0025] Furthermore, the gaseous medium may be at atmospheric pressure.

[0026] The retention time may in particular depend on the mass content of oxide of lanthanum in the mold. Preferably, it is less than 15 days, or even less than 5 days.

[0027] At the end of the holding period, the mold is sufficiently degraded for the part to be removed from the mold. Preferably, at the end of the holding period, the mold is disintegrated and in powder form.

[0028] Subsequent to step c), the process may include a part cleaning step. For example, the part may be brushed to recover portions of the degraded mold and / or sodium hydroxide dust in contact with the part.

[0029] The constituent contents of the mold are expressed as percentages by mass based on the mass of the mold.

[0030] Furthermore, the process may include, prior to step a) and / or subsequent to step c), a step of implementing the method of producing the mold according to the invention which will be described below.

[0031] The invention further relates to a method for producing a mold, in particular for implementing the manufacturing process according to the invention, the method comprising the steps of: - preparation of a starting charge consisting of lanthanum hydroxide particles, optionally of particles made of a refractory compound chosen from BN, Si3N4, Al2O3, ZrO2, HfO2, SiC and mixtures thereof, and less than 1% of other constituents, preferably free of other constituents, - payment of the initial charge in a counterform, - shaping the initial charge against the counter-form, so as to pre-form a mold, - optionally, sintering of the preformed mold.

[0032] The lanthanum hydroxide particles can originate from the degradation of the sintered mold in step c) of the manufacturing process according to the invention. It is thus possible to recycle an old mold to manufacture a new one by taking advantage of the reversible nature of the lanthanum oxide hydrolysis reaction.

[0033] Preferably, the starting charge consists of lanthanum hydroxide particles and particles made of a refractory compound selected from BN, Si3N4, Al2O3, ZrO2, HfO2, SiC and mixtures thereof.

[0034] Preferably, the starting charge comprises by volume at least 10%, or at least 20%, or at least 30%, or at least 40%, or even at least 50% of lanthanum hydroxide.

[0035] The refractory compound is preferably as described above.

[0036] The entire set of lanthanum hydroxide particles can have a median size D50 between 100 nm and 500 pm, for example equal to 300 nm. The size of a particle can be measured by laser granulometry.

[0037] The starting charge may consist of lanthanum hydroxide particles and less than 1% by volume of other constituents. Preferably, the starting charge consists of lanthanum hydroxide particles. Furthermore, the sintering temperature of the preformed mold and / or the sintering temperature of the part in step a) of the manufacturing process according to the invention may be between 900 °C and 1300 °C.

[0038] The starting charge may consist of lanthanum hydroxide particles, Si3N4 particles, and less than 1% by volume of other constituents, the mass content of lanthanum oxide particles preferably being at least 10%. Preferably, the starting charge consists of lanthanum hydroxide particles and Si3N4 particles. Furthermore, the sintering temperature of the preformed mold and / or the sintering temperature of the part in step a) of the manufacturing process according to the invention may be between 1265 °C and 1760 °C.

[0039] The starting charge may consist of lanthanum hydroxide particles, Al₂O₃ particles, and less than 1% by volume of other constituents, the mass content of lanthanum oxide particles preferably being at least 50%. Preferably, the starting charge consists of lanthanum hydroxide particles and Al₂O₃ particles. Furthermore, the sintering temperature of the preformed mold and / or the sintering temperature of the part in step a) of the manufacturing process according to the invention may be between 920 °C and 1420 °C.

[0040] The starting charge may consist of lanthanum hydroxide particles, SiC particles, and less than 1% by volume of other constituents, the mass content of lanthanum oxide particles preferably being at least 50%. Preferably, the starting charge consists of lanthanum hydroxide particles and SiC particles. Furthermore, the sintering temperature of the preformed mold and / or the sintering temperature of the part in step a) of the manufacturing process according to the invention may be between 1400 °C and 1700 °C.

[0041] The starting charge may consist of lanthanum hydroxide particles, BN particles, and less than 1% by volume of other constituents, the mass content of lanthanum oxide particles preferably being at least 10%. Preferably, the starting charge consists of lanthanum hydroxide particles and BN particles. Furthermore, the sintering temperature of the preformed mold and / or the sintering temperature of the part in step a) of the manufacturing process according to the invention may be between 1300 °C and 1850 °C.

[0042] Furthermore, the shaping of the starting load may involve the compression, preferably uniaxial, of the starting load against the counterform.

[0043] The method may include, after the preforming of the mold and, if necessary, before the sintering of the preformed mold, an optional step of demolding of the preformed mold and / or a drying step of the preformed mold, in particular until the residual moisture is between 0 and 0.5%.

[0044] Compression, particularly uniaxial compression, of the preformed mold can be implemented during the sintering of the preformed mold. The compression can be between 35 MPa and 500 MPa. Brief description of the drawings

[0045] The invention will be better understood by reading the examples presented by way of illustration and not limitation, and the accompanying drawing in which: - [[Fig.1]] is a group of photographs of an example of an assembly consisting of a part obtained by the process according to the invention and a mold used in the process, at different stages of maintenance in the gaseous medium, - [[Fig.2]] are diffractograms of samples made of lanthanum oxide, taken from the mold immediately after cooling of the part and the mold, and then 48 h after holding the mold in open air respectively, according to an example of implementation of the process, and - [[Fig.3]] is a set of photographs of pellets made of BN and La2O3 for, on the x-axis, different mass contents of La2O3 expressed as lanthanum hydroxide La(OH)3 contents in the starting charge and, in the column, after manufacture, after 3 days of maintenance in open air and after 13 days of maintenance in open air. Example 1

[0046] A starting charge consisting of lanthanum hydroxide particles was poured into a counterform. The starting charge was compacted to preform a preformed pellet.

[0047] Particles of a tungsten-cobalt carbide cermet (WC / Co) were arranged on the pre-formed pellet in order to manufacture a part.

[0048] The assembly was then heated at a rate of 100 K / min to a temperature suitable for sintering the pellet 1 and a part 2 made of the cermet. A photograph of the sintered assembly, obtained after cooling to room temperature, is shown in [Fig. 1] a).

[0049] The assembly consisting of the part and the mold was then kept for several days at ambient temperature and humidity, in the open air.

[0050] Photographs b) to e) of [Fig. 1] illustrate the progressive degradation of the mold upon contact with atmospheric humidity. At the end of the holding period, the WC / Co cermet part can be recovered directly without demolding, as the mold is completely pulverized ([Fig. 1] e)). Only a few traces of lanthanum oxide remain on the surface of the part.

[0051] The degradation of the mold by transformation of lanthanum oxide into lanthanum hydroxide was confirmed by means of the diffractograms illustrated in [Fig. 2], in which the square and round markers correspond to the theoretical positions of the peaks of lanthanum oxide and lanthanum hydroxide, respectively. After sintering and then cooling of the part and the mold, the diffractogram (shown at the top of [Fig. 2]) corresponds to the diffractogram of lanthanum oxide, while after 48 hours, a mixture of the peaks of lanthanum oxide and lanthanum hydroxide is observed (diffractogram shown at the bottom of [Fig. 2]). Example 2

[0052] Lanthanum hydroxide particle powder, as described in Example 1, and Carbotherm reference boron nitride particle powder, marketed by Saint Gobain, were available. Different starting loads were prepared by varying the respective mass proportions of said powders.

[0053] Preformed pellets were then obtained by compacting the initial charges and subsequently sintered according to the temperatures and proportions indicated in Table 1 below. The sintering temperature was reached via a ramp of 100 K / min. Once the sintering temperature was reached, the pellet was removed from the furnace.

[0054] [Tables 1] Sample Content in L a(OH)3 (% by volume) Sintering Temperature (°C) Appearance after 3 days in open air Appearance after 13 days in open air 1 1 1890 not degraded not degraded 2 2 1800 not degraded not degraded 3 5 1800 not degraded slightly degraded 4 10 1470 slightly degraded pulverized 5 25 1400 Highly degraded pulverized 6 40 1350 Highly degraded pulverized 7 50 1300 Highly degraded pulverized 8 60 1300 Highly degraded pulverized 9 99 1850 pulverized pulverized

[0055] Sintered pellets were thus obtained, which were then left in open air for 13 days. The visual condition of each pellet was assessed after sintering, and then at 3 and 13 days of exposure to open air. Photographs of the different samples are shown in [Fig. 3].

[0056] The following criteria listed in Table 2 were used to qualify the state of a pellet:

[0057] [Tables2] Criterion Definition Non-degraded No visible cracks and handling without risk of pellet breakage Slightly degraded Visible cracks and / or pellet crumbling during handling Severely degraded Pellet broken into several pieces or pellet rupture during handling Pulverized Pellet reduced to a powder

[0058] A faster degradation is observed with an increase in the mass content of La(OH)3 in the starting feed, and therefore of the content of lanthanum oxide La2O3 in the sintered pellet. Example 3

[0059] Lanthanum hydroxide particle powder, as described in Example 1, and silicon carbide particle powders commercially available from Kyocera, grades UF 05, UF 10, UF 15, and UF 25, had median particle sizes D50 of 2.2 pm, 0.9 pm, 0.75 pm, and 0.65 pm, respectively. Different starting loads were formed by varying the respective mass proportions of said powders.

[0060] Preformed pellets were then obtained by compacting the starting charges and were then sintered according to the temperatures and proportions indicated in Table 3 below.

[0061] The visual condition was then determined after 1 day of maintenance in open air.

[0062] [Tables3 Sample La(OH)3 content (% by volume) Sintering temperature (°C) Appearance after 1 day in open air 10 90 1750 Sprayed 11 50 1470 Sprayed Example 4

[0063] A lanthanum hydroxide particle powder was available, as in Example 1, and an alumina particle powder was available, marketed by the Baikowski company under the reference BMA 15 and having a median size D50 of 0.17 pm. Different starting charges were formed by varying the respective mass proportions of said powders.

[0064] Preformed pellets were then obtained by compacting the starting charges and were then sintered according to the temperatures and proportions indicated in Table 4 below.

[0065] The visual condition was then determined after 1 day of maintenance in open air.

[0066] [Tables4] Sample La(OH)3 content (% by volume) Sintering temperature (°C) Appearance after 1 day in open air 12 90 1350 Not degraded 13 50 1420 Sprayed Example 5

[0067] Lanthanum hydroxide particle powder, as described in Example 1, and grade 7 silicon nitride particle powder, commercially available from HC Starck, were used. Different starting loads were formed by varying the respective mass proportions of said powders.

[0068] Preformed pellets were then obtained by compacting the starting charges and were then sintered according to the temperatures and proportions indicated in Table 5 below.

[0069] The visual condition was then determined after 1 day of maintenance in open air.

[0070] [Tables5] Sample La(OH)3 content (% by volume) Sintering temperature (°C) Appearance after 1 day in open air 14 90 1760 Sprayed 15 50 1710 Sprayed

Claims

Demands

1. A method for manufacturing a part, the method comprising the following successive steps: a) shaping the part by: - ​​solidification of a liquid bath contained in a sintered mold comprising lanthanum oxide, or - sintering of a charge to be sintered contained in a mold comprising lanthanum hydroxide or in a sintered mold comprising lanthanum oxide, b) cooling the part in the mold, and c) maintaining the assembly formed of the part and the mold in a gaseous medium containing water vapor for a holding time suitable to degrade the mold under the effect of the hydrolysis of the lanthanum oxide by the water contained in the gaseous medium.

2. Method according to claim 1, the mold further comprising a refractory compound selected from BN, Si3N4, A12O3, ZrO2, HfO2, SiC and mixtures thereof.

3. A method according to any one of claims 1 and 2, the mold being sintered and consisting of lanthanum oxide and the refractory compound.

4. A method according to any one of claims 1 and 2, the part being shaped by sintering and the mold being made up of lanthanum hydroxide and the refractory compound.

5. A method according to any one of the preceding claims, the gaseous medium being air, preferably with a humidity level greater than 40%.

6. A method according to any one of the preceding claims, the holding period being less than 15 days, or even less than 5 days.

7. Method according to any one of the preceding claims, the part being metallic.

8. Method for producing a mold, in particular for implementing the process according to any one of the preceding claims, the method comprising the steps of: - preparing a starting charge consisting of lanthanum hydroxide particles, optionally of particles made of a refractory compound selected from BN, Si3N4, Al2O3, ZrO2, HfO2, SiC and their mixtures, and less than 1% of other constituents, preferably free of other constituents, and - pouring the starting charge into a counterform, - shaping the starting charge against the counterform, so as to preform a mold, and - optionally, sintering the preformed mold.

9. Method according to the preceding claim, the lanthanum hydroxide particles resulting from the degradation of the sintered mold in step c) of the process according to any one of claims 1 to 7

10. / . Method according to any one of claims 8 and 9, the starting charge comprising by volume, at least 10%, or at least 20%, or at least 30%, or at least 40%, or at least 50% of lanthanum hydroxide.

11. Method according to any one of claims 8 to 10, the starting charge consisting of lanthanum hydroxide particles and less than 1% by volume of other constituents and the sintering temperature of the preformed mold preferably being between 900 °C and 1300 °C.

12. Method according to any one of claims 8 to 10, the starting charge consisting of lanthanum hydroxide particles, Si3N4 particles and less than 1% by volume of other constituents, the mass content of lanthanum hydroxide particles preferably being at least 10% and the sintering temperature of the preformed mold preferably being between 1265 °C and 1760 °C.

13. Method according to any one of claims 8 to 10, the starting charge consisting of lanthanum hydroxide particles, A12O3 particles and less than 1% by volume of other constituents, the mass content of lanthanum hydroxide particles preferably being at least 50% and the sintering temperature of the preformed mold preferably being between 920 °C and 1420 °C.

14. Method according to any one of claims 8 to 10, the starting charge consisting of lanthanum hydroxide particles, SiC particles and less than 1% by volume of other constituents, the mass content of lanthanum hydroxide particles preferably being at least 50% and the sintering temperature of the preformed mold preferably being between 1400 °C and 1700 °C.

15. Method according to any one of claims 8 to 10, the starting charge consisting of lanthanum hydroxide particles, BN particles and less than 1% of other constituents, the mass content of lanthanum hydroxide particles preferably being at least 10% and the sintering temperature of the preformed mold preferably being between 1300 °C and 1850 °C.