Preparation method of tin oxide nanowire and use thereof in gas detection

The method of preparing tin oxide nanowires with a soft structure and high diameter consistency addresses the challenges in gas sensing by producing a sensitive and responsive gas sensor, achieving effective detection of organic gases with a cost-effective and straightforward process.

GB2624048BActive Publication Date: 2024-11-13YANGTZE DELTA REGION INST OF UNIV OF ELECTRONIC SCI & TECH OF CHINA HUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
GB2022017452
Authority / Receiving Office
GB · GB
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-02
Filing Date
2022-11-22
Publication Date
2024-11-13
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

Existing methods for preparing tin oxide nanowires for gas sensing applications face challenges in achieving a soft structure and high diameter consistency, which are crucial for sensitive and responsive gas sensors, particularly for organic gases.

Method used

A method involving the deposition of a copper film on a silicon wafer, mixing tin oxide and carbon powders, and heating in a tubular furnace under controlled conditions to produce soft tin oxide nanowires, followed by gold film deposition for creating a sensitive gas sensor.

Benefits of technology

The method results in a tin oxide nanowire-based gas sensor with a soft structure, high diameter consistency, and enhanced sensitivity to organic gases, demonstrating application value with simple and cost-effective conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000001_0000
    Figure 00000001_0000
  • Figure 00000002_0000
    Figure 00000002_0000
Patent Text Reader

Abstract

A method of manufacturing a tin oxide nanowire-based gas sensor comprises using a pure copper target to deposit a copper film on a surface of a silicon wafer, placing a mixed powder of tin oxide and carbon in a high-temperature zone of a tubular furnace, placing the silicon wafer at an edge of the high-temperature zone, extracting air from the furnace, heating to a temperature of 1200°C to 1250°C and holding for 110 to 120 minutes, while flowing argon gas through the furnace, cooling to room temperature to obtain soft tin oxide nanowires, scraping the nanowires from the wafer into a high-purity alcohol, adding the resulting suspension onto a silicon wafer having a clean surface, evaporating the alcohol to obtain a silicon wafer with tin oxide nanowires, covering and fixing a surface of the silicon wafer using a mask, depositing a gold film on the surface, and removing the mask to obtain the tin oxide nanowire-based gas sensor.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure belongs to the field of oxide semiconductor gas sensing, and in particular relates to a preparation method of a tin oxide nanowire-based gas sensor. BACKGROUND

[0002] Nanomaterials have some properties that macroscopic materials do not have, such as small size effect, surface effect, quantum tunneling effect, and dielectric confinement effect. Therefore, the nanomaterials exhibit some physical characteristics different from those of the macroscopic materials, and thus have their unique applications.

[0003] Nanowires are the building blocks of some tiny circuit devices. Semiconductor nanowires have some special properties, including desirable optical properties, anisotropic conductivity and the like. Accordingly, it is of great application significance to develop the semiconductor nanowires to deal with the difficulties brought about by the limitation of material size in various periods.

[0004] Among many semiconductor materials, tin oxide, as an n-type semiconductor with a wide bandgap, has a bandgap width of 3.6 eV and exhibits excellent semiconductor properties. Moreover, tin oxide nanomaterials have been proved by a large number of facts to have the application background of gas detection. Therefore, a preparation method of a tin oxide nanowire and use thereof in gas detection facilitate the portable assembly of tin oxide semiconductors in gas sensing applications, especially in various flexible gas sensors. SUMMARY

[0005] Aiming at the above prior art, the present disclosure provides a preparation method of a tin oxide nanowire-based gas sensor. In the present disclosure, a tin oxide nanowire is prepared, which is easy to be separated and has a soft structure.

[0006] To achieve the above objective, the technical solution adopted in the first aspect is to provide a preparation method of a tin oxide nanowire-based gas sensor, comprising the following steps: SI: putting a silicon wafer into a gold-spraying instrument equipped with a pure copper target, and depositing a copper film on a surface of the silicon wafer at a current of 8 mA to 9 mA for 50 sec to 60 sec; S2: uniformly mixing a tin oxide powder and a carbon powder, placing a resulting mixed powder 16 11 23 in a high-temperature zone of a tubular furnace, and placing a metal copper-covered silicon wafer on an edge of the high-temperature zone of the tubular furnace; S3: extracting air from the tubular furnace such that the tubular furnace has an internal pressure of 10 Pa to 20 Pa; S4: heating a temperature control zone to l,200°C to l,250°C, and holding the temperature for 110 min to 120 min, while introducing argon gas at a flow rate of 25 seem to 30 seem as a protective gas, and cooling the tubular furnace to a room temperature to obtain a soft tin oxide nanowire on the silicon wafer; S5: scraping off the tin oxide nanowire on the silicon wafer into a high-purity alcohol, adding a resulting alcohol suspension of the tin oxide nanowire onto a silicon wafer with a clean surface, and completely evaporating the alcohol to obtain a silicon wafer with a separated tin oxide nanowire; and S6: covering and fixing a surface of the silicon wafer obtained in S5 using a mask, depositing 50 nm to 60 nm of a gold film on the surface, and removing the mask to obtain a tin oxide nanowirebased gas sensor.

[0007] In an embodiment, , the copper film is deposited on the surface of the silicon wafer at a current of 9 mA for 60 sec.

[0008] In an embodiment, the air is extracted from the tubular furnace such that the tubular furnace has an internal pressure of not more than 20 Pa; the temperature control zone is heated to l,250°C, and the temperature is held for 120 min, while the argon gas is introduced at a flow rate of 30 seem as the protective gas, and the tubular furnace is cooled to the room temperature to obtain the soft tin oxide nanowire on the silicon wafer.

[0009] . The tin oxide nanowire has obvious advantages in physical properties; the nanowire has a soft and fluffy structure, which is easy to be separated to prepare multiple or single nanowire devices. The tin oxide nanowire-based gas sensor is extremely sensitive and responsive to organic gases.

[0010] The present disclosure has the following beneficial effects: in the present disclosure, the preparation method has simple conditions, and a relatively low cost of required equipment and raw materials; the tin oxide nanowire prepared by the preparation method has a soft structure and a high diameter consistency, which is easy to be separated; and the tin oxide nanowire-based gas sensor is extremely sensitive and responsive to organic gases, showing a certain application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] FIG. 1 shows a scanning electron microscopy (SEM) image of a tin oxide nanowire; and

[0012] FIG. 2 shows a gas sensitivity diagram of a tin oxide nanowire-based gas sensor. 16 11 23 DETAILED DESCRIPTION OF THE EMBODIMENTS

[0013] The technical solutions of the embodiments of the present disclosure are clearly and completely described below with reference to the accompanying drawings. Apparently, the described embodiments are merely a part rather than all of the embodiments of the present disclosure. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present disclosure without creative efforts shall fall within the protection scope of the present disclosure.

[0014] The present disclosure provides a preparation method of a tin oxide nanowire-based gas sensor. The preparation method includes the following steps:

[0015] SI: putting a silicon wafer into a gold-spraying instrument equipped with a pure copper target, and depositing a copper film on a surface of the silicon wafer at a current of 8 mA to 9 mA for 50 sec to 60 sec;

[0016] S2: uniformly mixing a tin oxide powder and a carbon powder, placing a resulting mixed powder in a high-temperature zone of a tubular furnace, and placing a metal copper-covered silicon wafer on an edge of the high-temperature zone of the tubular furnace;

[0017] S3: extracting air from the tubular furnace such that the tubular furnace has an internal pressure of 10 Pa to 20 Pa;

[0018] S4: heating a temperature control zone to l,200°C to l,250°C, and holding the temperature for 110 min to 120 min, while introducing argon gas at a flow rate of 25 seem to 30 seem as a protective gas, and cooling the tubular furnace to a room temperature to obtain a soft tin oxide nanowire on the silicon wafer;

[0019] S5: scraping off the tin oxide nanowire on the silicon wafer into a high-purity alcohol, adding a resulting alcohol suspension of the tin oxide nanowire onto a silicon wafer with a clean surface, and completely evaporating the alcohol to obtain a silicon wafer with a separated tin oxide nanowire; and

[0020] S6: covering and fixing a surface of the silicon wafer obtained in S5 using a mask, depositing 50 nm to 60 nm of a gold film on the surface, and removing the mask to obtain a tin oxide nanowire-based gas sensor.

[0021] In an embodiment, the copper film is deposited on the surface of the silicon wafer at a current of 9 mA for 60 sec.

[0022] In an embodiment, the air is extracted from the tubular furnace such that the tubular furnace has an internal pressure of not more than 20 Pa; the temperature control zone is heated to l,250°C, and the temperature is held for 120 min, while the argon gas is introduced at a flow rate of 30 seem as the protective gas, and the tubular furnace is cooled to the room temperature to obtain the soft tin oxide nanowire on the silicon wafer.

[0023] In an embodiment, the surface of the silicon wafer obtained in S5 is covered and fixed using the mask, 60 nm of the gold film is deposited on the surface, and the mask is removed to obtain the tin oxide nanowire-based gas sensor.

[0024] Further, in the preparation method of the tin oxide nanowire-based gas sensor, the nanowire may have a uniform size and a diameter of 300 nm to 400 nm. The tin oxide nanowirebased gas sensor may be sensitive to organic gases, and exhibit a gas sensitivity of 2.1 to ethanol at a concentration of 10 ppm.

[0025] Although the specific implementation of the present disclosure has been described in detail in conjunction with the examples, it should not be construed as limiting the protection scope of the present disclosure. Within the scope described in the claims, various modifications and deformations that can be made by those skilled in the art without creative work still belong to the protection scope of the present disclosure. 16 11 23

Claims

1. A preparation method of a tin oxide nanowire-based gas sensor, comprising the following steps:SI: putting a silicon wafer into a gold-spraying instrument equipped with a pure copper target, and depositing a copper film on a surface of the silicon wafer at a current of 8 mA to 9 mA for 50 sec to 60 sec;S2: uniformly mixing a tin oxide powder and a carbon powder, placing a resulting mixed powder in a high-temperature zone of a tubular furnace, and placing a metal copper-covered silicon wafer on an edge of the high-temperature zone of the tubular furnace;S3: extracting air from the tubular furnace such that the tubular furnace has an internal pressure of 10 Pa to 20 Pa;S4: heating a temperature control zone to l,200°C to l,250°C, and holding the temperature for 110 min to 120 min, while introducing argon gas at a flow rate of 25 seem to 30 seem as a protective gas, and cooling the tubular furnace to a room temperature to obtain a soft tin oxide nanowire on the silicon wafer;S5: scraping off the tin oxide nanowire on the silicon wafer into a high-purity alcohol, adding a resulting alcohol suspension of the tin oxide nanowire onto a silicon wafer with a clean surface, and completely evaporating the alcohol to obtain a silicon wafer with a separated tin oxide nanowire; andS6: covering and fixing a surface of the silicon wafer obtained in S5 using a mask, depositing 50 nm to 60 nm of a gold film on the surface, and removing the mask to obtain the tin oxide nanowire-based gas sensor.

2. The preparation method of the tin oxide nanowire-based gas sensor according to claim 1, wherein the copper film is deposited on the surface of the silicon wafer at a current of 9 mA for 60 sec.

3. The preparation method of the tin oxide nanowire-based gas sensor according to claim 1, wherein the air is extracted from the tubular furnace such that the tubular furnace has an internal pressure of not more than 20 Pa; the temperature control zone is heated to l,250°C, and the temperature is held for 120 min, while the argon gas is introduced at a flow rate of 30 seem as the protective gas, and the tubular furnace iscooled to the room temperature to obtain the soft tin oxide nanowire on the silicon wafer.CXI