Oxygen evolution reaction catalyst and method for producing same

The oxygen evolution reaction catalyst with yttrium and iridium, optimized for high surface area and particle size, addresses the slow reaction rate and iridium scarcity issues, achieving efficient hydrogen production and improved fuel cell durability with reduced iridium consumption.

GB2630471APending Publication Date: 2024-11-27FURUYA KINZOKU KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
GB2024008993
Authority / Receiving Office
GB · GB
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-25
Filing Date
2022-11-25
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

The high demand for hydrogen production through water electrolysis is hindered by the slow oxygen evolution reaction rate and the scarcity of iridium, necessitating a catalyst with high oxygen evolution activity and durability using minimal iridium content.

Method used

Development of an oxygen evolution reaction catalyst comprising an oxide with yttrium and iridium, having a BET specific surface area of 50 m2/g or more and an average particle diameter of 100 nm or less, supported on a carrier with a proton transport agent and an ion exchange polymer electrolyte membrane, produced through a method involving high-temperature and high-pressure treatment with an oxidizing agent.

Benefits of technology

The catalyst exhibits high oxygen evolution ability with reduced iridium usage, enhancing the efficiency of water electrolysis and fuel cell performance while preventing oxidative corrosion in fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

[Problem] To provide a catalyst for electrolysis, the catalyst being suppressed in the amount of iridium used therefor, while enabling a high oxygen evolution reaction. [Solution] An oxygen evolution reaction catalyst which contains an oxide that contains yttrium and iridium, while having a BET specific surface area of 50 m2 / g or more.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to an oxygen evolution reaction catalyst, and more particularly, the present invention relates to an oxygen evolution reaction catalyst used for electrolysis of water. Furthermore, the present invention relates to a method for producing an oxide contained in the oxygen evolution reaction catalyst. BACKGROUND ART

[0002] Hydrogen has high energy conversion efficiency and does not generate carbon dioxide when burned, so it is attracting attention as an energy source due to the global trend toward eliminating carbon dioxide. Known methods for producing hydrogen include methods for producing it by reforming hydrocarbons, methods for producing it from methanol and the like produced from biomass, methods for using by-products produced in processes such as steel manufacturing, and methods for obtaining hydrogen from renewable energy. Among these methods, the method of electrolyzing water using electricity generated from the renewable energy such as solar power generation and wind power generation is attracting attention as a preferred method for producing hydrogen because it does not generate carbon dioxide. Further, by electrolyzing water and storing energy as hydrogen, surplus electricity can be used effectively. Excess electricity can be converted into hydrogen, stored as a gas or a liquid, and immediately used as fuel. Additionally, hydrogen can be converted into other compounds such as ammonia or chemicals such as methanol for industrial use. Therefore, the production of hydrogen by electrolysis of water is attracting attention also from the point of view of effective use of energy.

[0003] As methods of electrolysis of water (hereinafter also referred to as "water electrolysis"), an alkaline water electrolysis system and a solid molecular membrane (hereinafter also referred to as "PEM") type water electrolysis system are being studied. The PEM type water electrolysis system allows a higher current to flow in the same area than the alkaline water electrolysis system, so the electrolyzer can be made smaller, and it has good followability for renewable energies and other energy sources with wildly fluctuating voltages. Therefore, there is an advantage that the hydrogen generated by electrolysis has high purity. [0004 ] A PEM type water electrolysis cell has a membrane electrode assembly (hereinafter also abbreviated as MEA) as one structural unit, consisting of a catalyst coated membrane (hereinafter also abbreviated as CCM) in which a cation exchange polymer electrolyte membrane such as Nafion (registered trademark) is sandwiched between an anode catalyst layer and a cathode catalyst layer and both sides of the catalyst coated membrane are further sandwiched between gas diffusion layers, and the PEM type water electrolysis cell is constructed by connecting a plurality of the membrane electrode assemblies in series via separators. When water is supplied to the anode catalyst layer, the reaction of the following formula (1) occurs in the anode catalyst layer, and the reaction of the following formula (2) occurs in the cathode catalyst layer, and oxygen (O2) is generated on the anode side and hydrogen (H2) is generated on the cathode side. H20    1 / 202(g)+2H++2e-    (1) 2H + + 2e“     H2 (g) ( 2) A rate-determining step in the overall reaction is oxidation of water on the anode side and the oxygen evolution reaction, and mass activity of the oxygen evolution reaction (hereinafter also referred to as "OER") of the anode catalyst is an important factor that determines the efficiency of the system.

[0005] The oxygen evolution reaction at the anode of the PEM type water electrolysis system has a slow reaction rate, and it is necessary to apply a high voltage to generate more oxygen. For this reason, a catalyst containing an iridium oxide or iridium, which has electrical conductivity and high durability under a highly oxidizing environment or a high voltage environment, has been used in the anode of the PEM type water electrolysis system. On the other hand, since an annual production of iridium is small and it is highly rare, there has been a demand for a catalyst with a lower iridium content that exhibits a high oxygen evolution reaction and has high durability under a highly oxidizing environment or a high voltage environment.

[0006] Patent Document 1 discloses an electrode catalyst composition in which iridium-ruthenium oxide is supported on 2 tin oxide.

[0007] Patent Document 2 proposes a core-shell type oxygen evolution reaction catalyst comprising a core and a shell covering the surface of the core wherein the core contains ruthenium oxide or metal ruthenium at least on the surface and the shell contains titania or a composite oxide of titanium and ruthenium.

[0008] Patent Document 3 proposes a catalyst membrane containing an electrolysis catalyst containing platinum or platinum alloyed with one or more other metals and an oxygen evolution reaction catalyst, and it has been reported that the oxygen evolution reaction catalyst has a high oxygen evolution reaction mass activity.

[0009] Non-Patent Document 1 has reported yttrium and iridium oxide having a BET specific surface area of 21 m2 / g or more, a particle size of about 200 nm and a pyrochlore crystal structure.

[0010] Non-Patent Document 2 has reported yttrium and iridium oxide having a BET specific surface area of 7.3 m2 / g or more, a particle size of about 200 nm and a pyrochlore crystal structure. PRIOR ART DOCUMENT PATENT DOCUMENT

[0011] Patent Document 1: JP-A-202 0 - 500692 Patent Document 2: Japanese Patent No. 6763009 Patent Document 3: Japanese Patent No. 5978224

[0012] Non-patent Document 1: Highly Active and Stable Iridium Pyrochlores for Oxygen Evolution Reaction, Chemistry of Materials. 2017, 29, 5182-5191 Non-patent Document 2: Single Phase Pyrochlore Y2Ir2O7 Electrocatalyst on the Activity of Oxygen Evolution Reaction, APPLIED ENERGY MATERIALS. 2018, 1, 8, 3992-3998 SUMMARY OF THE INVENTION PROBLEM TO BE SOLVED BY THE INVENTION

[0013] If the practical application of hydrogen production technology through water electrolysis accelerates in the future, it is expected that large amounts of iridium will be used. On the other hand, the annual production of iridium is approximately 9 tons, and as it is highly rare, there is a need to reduce the amount of iridium used and to develop an oxygen evolution reaction catalyst for water electrolysis that exhibits a high oxygen evolution 3 reaction . MEANS FOR SOLVING THE PROBLEM [0014 ] The present inventors conducted intensive studies to solve the above problems, and as a result, completed the present invention. That is, the present invention has the following aspects.

[0015] [1] An oxygen evolution reaction catalyst comprising an oxide containing yttrium and iridium and having a BET specific surface area of 50 m2 / g or more. [2] The oxygen evolution reaction catalyst in the above-mentioned item [1], wherein the oxide has an average particle diameter of 100 nm or less. [3] An oxygen evolution reaction catalyst layer comprising the oxygen evolution reaction catalyst in the above-mentioned item [1] or [2] and a proton transport agent . [4] An electrolysis cell comprising the oxygen evolution reaction catalyst layer in the above-mentioned item [3] and an ion exchange polymer electrolyte membrane. [5] The electrolysis cell in the above-mentioned item [4], wherein the ion exchange polymer electrolyte membrane is a cation exchange polymer electrolyte membrane.

[0016] Further, the present invention has the following aspects . [6] A method for producing the oxide in the above-mentioned item [1], the method comprising: a step A of (1) dispersing yttrium nanoparticles and iridium nanoparticles or yttrium hydroxide particles and iridium hydroxide particles in a dispersion medium to obtain a dispersion liquid or (2) dissolving an yttrium compound and an iridium compound in a solvent to obtain a solution; a step B of increasing a temperature of water to 100°C or higher and a pressure of the water to higher than 0.1 MPa; and a step C of mixing the dispersion liquid or the solution obtained in the step A and the high-temperature and high-pressure water obtained in the step B. [7] The method for producing the oxide in the above-mentioned item [6] , wherein the step B includes a step of adding an oxidizing agent. [8] The method for producing the oxide in the above-mentioned item [7], wherein the oxidizing agent is an oxidizing agent that releases oxygen atoms. [9] The method for producing the oxide in the above-mentioned item [8], wherein the step B includes any one of (1) a step of adding the oxidizing agent that releases the 4 oxygen atoms to the water and then increasing the temperature of the water to 100°C or higher and the pressure of the water to higher than 0.1 MPa, (2) a step of adding the oxidizing agent that releases the oxygen atoms to the water after increasing the temperature of the water to 100°C or higher and the pressure of the water to higher than 0.1 MPa, or (3) a step of adding the oxidizing agent that releases the oxygen atoms to the water, increasing the temperature of the water to 100°C or higher and the pressure of the water to higher than 0.1 MPa and then further adding the oxidizing agent that releases the oxygen atoms. EFFECTS OF THE INVENTION

[0017] According to the present invention, there is provided a catalyst for water splitting, particularly for water electrolysis, which has a high oxygen evolution ability even with a small amount of iridium used. BRIEF DESCRITION OF THE DRAWINGS

[0018] FIG. 1 is an example of an apparatus for producing an oxide of yttrium and iridium according to the present embodiment . FIG. 2 is an X-ray diffraction pattern in Example 1. FIG. 3 is an X-ray diffraction pattern in Comparative Example 1. FIG. 4 is an X-ray diffraction pattern of iridium oxide of Comparative Example 2. FIG. 5 is a TEM image of Example 1. MODE FOR CARRYING OUT THE INVENTION

[0019] Hereinafter, the present invention will be described in detail by showing embodiments, but the present invention should not be interpreted as being limited to these descriptions. The embodiments may be modified in various ways as long as the effects of the present invention are achi eved.

[0020] An oxygen evolution reaction catalyst of the present invention (hereinafter also referred to as the present catalyst) comprises an oxide containing yttrium and iridium and having a BET specific surface area of 50 m2 / g or more (hereinafter also referred to as "the present oxide").

[0021] The present oxide may contain yttrium oxide or iridium oxide, a mixture of yttrium oxide and iridium oxide, or a composite oxide of yttrium and iridium represented by the general formula YxIryOz. The present oxide may also contain a mixture of these. The present oxide preferably contains a composite oxide of yttrium and iridium from the viewpoint of oxygen evolution reaction activity. In addition, in the said general formula, the subscripts x, y and z usually satisfy the following. 0 . 1 < x < 3 0.1 < y < 3 1 < z < 10 When the present oxide contains the composite oxide of yttrium and iridium, it is more preferable to contain the composite oxide in which x, y and z satisfy the following ranges . 0 . 2 < x < 2 0.2 < y < 2 2 < z < 8 When the present oxide contains the composite oxide, it is more preferable that the composite oxide is the main component. The composite oxide being the main component means that when X-ray diffraction of powder of the present oxide is measured, diffraction peaks attributed to yttrium oxide and iridium oxide are below a detection limit.

[0022] The present oxide may contain other metals in addition to yttrium and iridium. Examples of the other metals include platinum, ruthenium, rhodium, palladium, nickel, aluminum, strontium, bismuth, titanium, tin, zinc, iron, copper, silver, gold, lanthanum and antimony. These metals may be oxides of each metal or may be other than oxides, such as halides and hydroxides. Further, yttrium, iridium or a composite oxide of both may be used.

[0023] From the viewpoint of oxygen evolution reaction activity, an elemental ratio of yttrium and iridium in the present oxide is preferably 40 to 60 atm% for yttrium and 60 to 40 atm% for iridium, more preferably 50 atm% for yttrium and 50 atm% for iridium, assuming that the total elemental amount of yttrium and iridium is 100 atm% . [0024 ] The BET specific surface area of the present oxide is more preferably 100 m2 / g or more, and even more preferably 150 m2 / g or more, from the viewpoint of oxygen evolution reaction . The BET specific surface area is determined by the BET method by low-temperature physical adsorption of an inert gas and is the specific surface area determined from the obtained adsorption isotherm.

[0025] An average particle diameter of the present oxide is preferably 100 nm or less. The average particle diameter is more preferably 50 nm or less. The average particle size can be measured with a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM). As the average particle diameter becomes smaller, the number of active sites in the catalyst increases, and it is expected that the OER mass activity will improve. The average particle diameter is measured according to the method described in JIS H 7804:2005. That is, 200 or more primary particles are selected from among the metal particles shown in the image taken by TEM, and the longest length of these particles is visually measured as the particle diameter. The average particle diameter is determined by dividing the :otal particle diameter of each particle by the number of particles whose particle diameter was measured. The field of view is photographed in areas containing 200 or more primary particles. The number of primary particles to be measured is not particularly limited as long as it is 200 or more, but it is usually 300 or less, about 200 to 300.

[0026] A shape of the present oxide may be spherical, ellipsoidal, columnar or irregular, but a spherical or nearly spherical shape is preferred from the viewpoint of handling . Note that the average particle size of the present oxide is a value obtained by measuring the long diameter when observed by TEM or STEM.

[0027] The present catalyst may be the above-mentioned present oxide itself or may contain other components. For example, the present catalyst may be prepared by supporting the present oxide on a carrier. As the carrier, corrosion-resistant carbon powder such as graphitized carbon black or acetylene black or a conductive oxide powder carrier such as H4O7 is preferably used.

[0028] When the present catalyst is prepared by supporting the present oxide on the carrier, a content of the present oxide in the present catalyst is preferably 20% by mass or more, more preferably 30% by mass or more, based on the total mass of the present oxide and the carrier as 10 0 % by mas s. In addition to the above-mentioned carrier, the present catalyst may contain other components such as a stabilizer as neces sary.

[0029] Since the present catalyst has a high oxygen evolution ability, it can be used as a catalyst layer such as an oxygen evolution reaction catalyst layer in a water electrolysis system. As mentioned above, in the water electrolysis system, when water supplied from an outside is supplied to an anode catalyst layer, which is an oxygen evolution reaction catalyst layer, a reaction of the following formula (1) occurs in the anode catalyst layer, and the water is converted into oxygen and hydrogen ions (protons). The hydrogen ions move through a proton transport agent to a cathode catalyst layer, which is a hydrogen evolution reaction catalyst layer, a reaction of the following formula (2) occurs in the cathode catalyst layer, and oxygen (O2) is generated on the anode side and hydrogen (H2) is generated on the cathode side. H20    1 / 202(g)+2H++2e“    (1) 2H + + 2e-     H2 (g) ( 2 ) In the PEM type water electrolysis system, through the above-mentioned reaction, protons generated by water splitting in the MEA are transported from the anode catalyst layer to the cathode catalyst layer through the ion exchange polymer electrolyte membrane, and at the same time, electrons generated in the anode catalyst layer are transferred to the cathode catalyst layer through an external circuit.

[0030] Therefore, by using the present catalyst together with a proton transport agent, it can be used as an oxygen evolution reaction catalyst layer, that is, an anode catalyst layer, of the water electrolysis system. The proton transport agent has a role of conducting protons and may have a function of transporting protons to a vicinity of the catalyst in the catalyst layer for the electrolysis reaction and a function of a binder that fixes the catalyst to a base material. By attaching catalyst particles to each other using the proton transport agent, the proton transport agent is an important factor in improving catalyst performance because the proton transport agent can change a proton transport path and a packing structure of the catalyst. Examples of the proton transport agent  include perfluor0sulfonic  acid-based proton transport  agents, sulfonated polyethylene ether ketone-based proton transport agents, and sulfonated  po1ybenzimidaz01e-based proton transport agents. Among them, Nation (registered trademark, manufactured by DuPont), Flemion (registered trademark, 8 manufactured by AGC), Aciplex (registered trademark, manufactured by Asahi Kasei), Fumion (registered trademark, manufactured by Fumatech), Aquivio (registered trademark, manufactured by Solvay) and the like, which are perfluorosulfonic acid-based proton transport agents, are preferred.

[0031] The present catalyst can be used as an electrolytic cell of the water splitting system by further using an ion exchange polymer electrolyte membrane. As the ion exchange polymer membrane, a cation exchange polymer electrolyte membrane is usually used. The cation exchange polymer electrolyte membrane has physical strength and low gas permeability and is preferably in the form of a membrane. A cation-exchange polymer electrolyte is usually used to be sandwiched between a cathode catalyst layer and an anode catalyst layer, so it has a membrane-1ike shape. A catalyst coated membrane (CCM) used in the water electrolysis system can be obtained by forming a multilayer structure by providing the cation exchange polymer electrolyte membrane and the oxygen evolution reaction catalyst layer and the hydrogen evolution reaction catalyst layer on both sides thereof. Materials constituting the cation exchange polymer electrolyte membrane include the same materials as those constituting the proton transport agent.

[0032] The oxygen evolution reaction catalyst layer and the electrolytic cell can be obtained, for example, by coating the present catalyst on the proton transport agent or the cation exchange polymer electrolyte membrane. Ink used for coating may be prepared by stirring and mixing the proton transport agent and the present catalyst in a solvent. A ratio of the catalyst to the proton transport agent is not particularly limited, but the ratio is preferably from 1:0.2 to 1:0.05, more preferably from 1:0.15 to 1:0.07. The solvent is not particularly limited, but water or a mixture of water and a lower aliphatic alcohol such as ethanol, propanol or butanol is preferably used. When applying the present catalyst to the cation exchange polymer membrane, a coating amount of the catalyst is preferably 0.001 mg / cm2 to 4 mg / cm2 , more preferably 0.1 mg / cm2 to 2 mg / cm2 per unit area of the cation exchange polymer electrolyte membrane.

[0033] The electrolytic cell has a cathode layer, which is the hydrogen evolution reaction catalyst layer, on the surface of the cation exchange polymer electrolyte membrane 9 opposite to the present catalyst. Platinum is usually used as a hydrogen evolution reaction catalyst in the cathode layer . An MEA is formed by sandwiching both outer sides of the catalyst layer of the electrolytic cell between diffusion layers. This is considered as one structural unit, and when a plurality of these are connected in series through separators and water is supplied to the anode catalyst layer, which is the oxygen evolution reaction catalyst layer, the reaction of the above formula (1) occurs in the anode catalyst layer, the reaction of the above formula (2) occurs in the cathode catalyst layer, and oxygen is generated on the anode side and hydrogen is generated on the cathode side. [0034 ] The present catalyst can also be used in the anode of a fuel cell. In the fuel cell, hydrogen molecules supplied from the outside separate two electrons at the anode and become hydrogen ions (protons) . The electrons that leave the hydrogen flow as a current through an external circuit to the opposite cathode, where electricity is generated.

[0035] At the cathode, oxygen molecules taken in from the air receive electrons returned from an external circuit and become oxygen ions. Oxygen ions combine with hydrogen ions that have migrated through the proton transport agent to form water .

[0036] Chemical reaction on the anode side can be represented by the following formula (3), chemical reaction on the cathode side can be represented by the following formula (4), and the overall reaction can be represented by the following formula (5). 2H2 - 4H+ + 4e~    (3) 4H+ + 02 + 4e~ 2H2O (4) 2H2 + 02 2H2O (5) When starting or stopping the fuel cell, if there is insufficient hydrogen supply to the anode side, a fuel starvation state occurs and a reverse potential occurs where current is forced to flow from other cells connected in series to this fuel starved cell. As a result, the reaction of the following formula (6) occurs. Since a platinum-supported carbon-based electrode catalyst is normally used in the anode catalyst layer of the fuel cell, the carbon of the anode catalyst is oxidized and corroded due to the 10 following formula (6), resulting in severe deterioration of the fuel cell. C + 2H2O C02 + 4H + + 4e~    (6) 2H2O 02 + 4H+ + 4e“    (7) By using the electrolytic catalyst that electrolyzes water on the anode side of the fuel cell by the reaction of formula (7) under such reverse potential conditions, oxidative corrosion of the carbon carrier by water can be suppre s s ed. Therefore, when the present catalyst with high oxygen evolution reaction ability and an anode catalyst containing p1 atinum-supported carbon are used as the anode of the fuel cell, the reaction of formula (7) proceeds, and deterioration of the catalyst due to hydrogen deficiency in the anode of the fuel cell can be prevented.

[0037] Further, the present catalyst can be used as a cocatalyst for phot0cata1ysts. Known photocatalyst materials include gallium phosphide, gallium arsenide, cadmium sulfide, strontium titanate, titanium oxide, zinc oxide, iron oxide, tungsten oxide, and tin oxide. The water splitting reaction by a photocatalyst begins when the photocatalyst absorbs light with energy above the band gap and generates excited electrons in the conduction band and holes in the valence band. Then, water is reduced and oxidized by excited electrons and holes to generate hydrogen and oxygen, and a phot0cata1ytic reaction progresses . On the other hand, there are very few metal oxides that can be used as photocatalysts that can respond to visible light, making it difficult to efficiently produce hydrogen, and improvements in performance are being considered by using hydrogen evolution reaction catalysts and oxygen evolution reaction catalysts as cocatalysts. By using the present catalyst as an oxygen evolution reaction catalyst, hydrogen can be efficiently produced. In this case, examples of the hydrogen evolution reaction catalyst include fine metal particles such as platinum, rhodium, iridium, ruthenium, nickel and gold.

[0038] The present catalyst can be used as an electrode by using a metal plate. The obtained electrode can be suitably used as a cathode in the soda industry. When using the present catalyst with the metal plate to form the electrode, the catalyst can be applied to the metal plate to form the electrode. Regarding the amount of 11 application, the content of the present oxide in the present catalyst is preferably 1 mg / cm2 to 3 mg / cm2, more preferably 2 mg / cm2 to 3 mg / cm2 per unit area of the metal plate.

[0039] The soda industry produces caustic soda, chlorine and hydrogen by electrolyzing salt water. Chlorine is used for disinfection and sterilization, for bleaching paper and pulp and as a raw material for synthetic resins such as vinyl chloride resin, epoxy resin, silicone resin, and fluororesin, chlorinated solvents, refrigerants, agricultural chemicals, pharmaceuticals and various other chemical products. Further, the caustic soda is also used as a raw material for bleaching paper and pulp, chemical fibers, detergents and soaps, raw materials for industrial chemicals, seasonings and other products essential to daily life.

[0040] Industrially established electrolysis methods include the mercury method, diaphragm method and ion exchange membrane method, but the electrode containing the present catalyst and the metal plate is suitable for use in the ion exchange membrane method, which is superior in environmental impact and cost. In the ion exchange membrane method, a cathode chamber and an anode chamber of the electrolytic cell are separated by a cation exchange polymer electrolyte membrane, and the cathode uses a metal electrode such as titanium, and the anode uses a metal electrode such as nickel.

[0041] In particular, DSA (registered trademark: Dimensionally Stable Anode), which is based on titanium and coated with a mixed oxide layer containing a platinum group metal oxide, is used for the cathode. Since DSA (registered trademark) has many excellent properties, such as high electrochemical catalytic activity for oxygen and chlorine evolution, high electrical conductivity, good processing properties, corrosion resistance, energy saving and light weight, it has been widely used. Regarding the platinum group metal oxide coated on the surface of the DSA (registered trademark), iridium is widely used due to its durability or the like, but by using the platinum group metal oxide coated on the surface of DSA (registered trademark) as the catalyst of the present invention, the amount of iridium used can be suppressed and caustic soda, chlorine and hydrogen can be efficiently produced.

[0042] The method for producing the present oxide will 12 be described below. A method for producing the present oxide (hereinafter also referred to as the present production method) comprises a step A of (1) dispersing yttrium nanoparticles and iridium nanoparticles or yttrium hydroxide particles and iridium hydroxide particles in a dispersion medium to obtain a dispersion liquid (hereinafter also referred to as "present dispersion liquid") or (2) dissolving an yttrium compound and an iridium compound in a solvent to obtain a solution (hereinafter also referred to as "present solution"), a step B of increasing a temperature of water to 100°C or higher and a pressure of the water to higher than 0.1 MPa and a step C of mixing the dispersion liquid or the solution obtained in the step A and the high-temperature and high-pressure water obtained in the step B.

[0043] Here, an example of a production apparatus of the oxide will be described with reference to FIG. 1. The production apparatus 100 for the present oxide includes a first supply source 1 that supplies the present dispersion liquid or the present solution, a second supply source 2 that supplies water and a heating unit 3 for heating the water supplied from the second supply source 2. The water supplied from the second supply source 2 is heated by the heating unit 3 to a temperature of 100°C or higher. Moreover, the pressure of the water becomes higher than 0.1 MPa due to a pressure adjusting mechanism 10, which will be described later. Further, the production apparatus 100 has a reaction unit 4 in which the present dispersion liquid or the present solution and the water heated to a temperature of 100°C or higher and adjusted to a pressure of higher than 0.1 MPa in the step B (hereinafter also referred to as "present high-temperature water") are combined. The water supplied from the second supply source 2 may contain an oxidizing agent, which will be described later, if necessary. The first supply source 1 and the reaction unit 4 are connected by a liquid feeding route 5, and the present dispersion liquid or the present solution is sent from the first supply source 1 to the reaction unit 4 through the liquid feeding route 5. The second supply source 2 and the reaction unit 4 are connected by a liquid feeding route 6, and a liquid containing water is sent from the second supply source 2 to the reaction unit 4 through the liquid supply route 6. The oxidizing agent may be added to the water at any point along the liquid feeding route 6, if necessary. [0044 ] Further, the reaction unit 4 is connected to a collection unit 8 for collecting the generated reactant by 13 a liquid feeding route 7, and a cooling unit 9 is arranged around the liquid feeding route 7 between the reaction unit 4 and the collection unit 8. Thereby, the reactant produced in the reaction unit 4 is cooled by the cooling unit 9 when passing through the liquid feeding route 7 and is sent to the collection unit 8. Furthermore, the production apparatus 100 has a pressure adjusting mechanism 10 for the purpose of setting the reaction unit to a high pressure condition. The pressure adjusting mechanism 10 may be connected to the collection unit 8 as shown in FIG. 1 or may be connected between the cooling unit 9 and the collection unit 8 via the liquid feeding route 7. As the pressure adjusting mechanism, a plunger, a cylinder and a regulator can be considered, but a cylinder is preferable from the viewpoint of clogging or wear and tear .

[0045] The liquid feeding routes 5 to 7 are formed by, for example, piping. According to the production apparatus 100, the oxide of yttrium and iridium can be stably produced.

[0046] In the reaction unit 4, by mixing the present dispersion liquid or the present solution with the present high-temperature water, yttrium and iridium in the present dispersion liquid or the present solution are oxidized to produce the oxide containing yttrium and iridium. Although yttrium and iridium may be oxidized using only the present high-temperature water, yttrium and iridium can be oxidized more efficiently by adding an oxidizing agent to the present high-temperature water. In this regard, the present high-temperature water is obtained by the heating unit 3 and the pressure adjusting mechanism 10. The pressure adjusting mechanism 10 is located downstream of the production device 100, and since the pressure adjusting mechanism 10 is connected to the reaction unit 4, the liquid feeding route 5, the liquid feeding route 6 and the liquid feeding route 7, it has a function of adjusting the overall pressure of the production apparatus 100. The pressure adjusting mechanism 10 adjusts the pressures of the reaction unit and all of the liquid feeding routes and obtains the high-temperature water at the above-mentioned temperature and pressure. The oxidizing agent is preferably an oxidizing agent that releases oxygen, and preferably an oxidizing agent that releases oxygen such as oxygen, hydrogen peroxide or ozone. When using oxygen gas as the oxidizing agent, it is preferable to bring the water to a saturated oxygen 14 concentration to a high temperature and high pressure state. [0047 ] The liquid feeding route 5 connecting the first supply source 1 and the reaction unit 4 has a liquid feeding means. An example of the liquid feeding means for the present dispersion liquid or the present solution is a liquid feeding means that arranges the first supply source 1 at a higher position than the reaction unit 4 and utilizes a height difference. In this case, the present dispersion liquid or the present solution can be sent from the first supply source 1 to the reaction unit 4 by connecting with piping. At this time, a flow rate adjusting means such as a needle valve or a stop valve may be arranged in the liquid feeding route 5 to adjust the flow rate.

[0048] The liquid feeding route 6 connecting the second supply source 2 and the reaction unit 4 has a liquid feeding means. An example of the liquid feeding means of the present high-temperature water is a liquid feeding means that arranges the second supply source 1 at a higher position than the reaction unit 4 and utilizes the height difference. In this case, the liquid containing water and the present high-temperature water can be sent from the second supply source 2 to the reaction unit 4 by connecting them with piping. At this time, similarly to the liquid feeding route 5, a means for adjusting the flow rate, such as a needle valve or a stop valve, may be arranged in the liquid feeding route 6.

[0049] The production apparatus of the oxide according to the present embodiment may include flow rate adjusting mechanisms 11 and 12 that send the liquid flowing in one direction to either the liquid feeding route 5 or the liquid feeding route 6 or both. The production apparatus 100 of the oxide of yttrium and iridium shown in FIG. 1 has an embodiment in which in addition to the first supply source 1, the second supply source 2, the heating unit 3, the reaction unit 4, the liquid feeding route 5, the liquid feeding route 6, the liquid feeding route 7, the collection unit 8, the cooling unit 9 and the pressure adjusting mechanism 10, the liquid feeding route 5 and the liquid feeding route 6 are provided with the flow rate adjusting mechanisms 11 and 12, respectively. In this embodiment, since it is possible to stably control the flow rate and flow velocity of the present dispersion liquid or the present solution in the liquid feeding route 5 and the flow rate and flow velocity of the liquid containing water in the liquid feeding route 6, respectively, the oxide can be stably produced. Examples of the mechanisms 11 and 12 example, plungers, cylinders or regulators. include, for

[0050] The dispersion medium used in the present dispersion liquid is a medium for dispersing yttrium nanoparticles and iridium nanoparticles or yttrium hydroxide particles and iridium hydroxide particles. Examples of the dispersion medium include water and organic solvents. The solvent used in the present dispersion liquid is a solvent that dissolves the yttrium compound and the iridium compound and is liquid at normal temperature. Examples of the solvent include water and organic solvents. In this embodiment, normal temperature is 15°C to 30°C, preferably 20°C to 25°C.

[0051] When obtaining the dispersion liquid of the yttrium nanoparticles and the iridium nanoparticles in the item (1) of the step A, the average particle size of the yttrium nanoparticles or the iridium nanoparticles is usually 100 nm or less, preferably 3 nm or less, and more preferably 2.5 nm or less. If the average particle size of the yttrium nanoparticles and the iridium nanoparticles is too large, the particle size of the oxide containing yttrium and iridium may become too large when yttrium and iridium are reacted with oxygen, and oxidation may become insufficient in the oxidation reaction described below. As the yttrium nanoparticles and the iridium nanoparticles, for example, yttrium nanoparticles and iridium nanoparticles that have a desired average particle size by particle sizing or the like may be used. Note that the method for measuring the average particle diameter is the same as described above.

[0052] When obtaining the dispersion liquid of the yttrium hydroxide particles and the iridium hydroxide particles in the item (1) of the step A, the average particle size of the yttrium hydroxide particles or the iridium hydroxide particles is usually 100 nm or less, preferably 3 nm or less, and more preferably 2.5 nm or less. If the average particle size of the yttrium hydroxide particles and the iridium hydroxide particles is too large, the particle size of the oxide containing yttrium and iridium may become too large when the yttrium hydroxide particles and the iridium hydroxide particles are reacted with oxygen, and oxidation may become insufficient in the oxidation reaction described below. As the yttrium hydroxide particles and the iridium hydroxide particles, for example, yttrium hydroxide particles and iridium hydroxide particles that have a 16 desired average particle size by particle classification or the like may be used. Note that the method for measuring the average particle diameter is the same as described above.

[0053] The present dispersion liquid can be obtained by adding the above-mentioned yttrium nanoparticles and iridium nanoparticles or yttrium hydroxide particles and iridium hydroxide particles to the dispersion medium. Examples of the dispersion medium include water and ethanol. [0054 ] In the item (2) of the step A, examples of the yttrium compound include yttrium-containing salts such as yttrium nitrate, yttrium acetate, yttrium sulfate and yttrium chloride, and metal complexes such as yttrium acetylacetonate and yttrium carbonyl. Among these compounds, yttrium nitrate compounds, yttrium sulfate compounds and yttrium acetate compounds are preferred.

[0055] Examples of the iridium compound include iridium-containing salts such as iridium nitrate compounds, iridium sulfate compounds, iridium acetate compounds and iridium chloride, and metal complexes such as iridium acetylacetonate and iridium carbonyl. Among these compounds, iridium nitrate compounds, iridium sulfate compounds and iridium acetate compounds are preferred. The present solution can be obtained by adding the above-mentioned yttrium compound and iridium compound to the solvent. Examples of the solvent include water for yttrium-containing salts or iridium-containing salts, and ethanol, ethyl acetate and the like for yttrium-containing metal complexes or iridium-containing metal complexes. When the salt and the complex are mixed, the solvent may be water, ethanol, ethyl acetate or the like. In the item (2) of the step A, it is preferable to dissolve the yttrium compound or the iridium compound in the solvent at room temperature, for example from 15°C to 30°C.

[0056] In the step B, the temperature of the water is increased to 100°C or higher and the pressure of the water is increased to higher than 0.1 MPa to obtain the present high-temperature water. The temperature of the present high-temperature water is preferably 150°C or higher, more preferably 374°C or higher, for example about 400°C. The pressure of the present high-temperature water is preferably 0.5 MPa or more, more preferably 22.1 MPa or more, for example about 30 MPa. Pure water is preferable as the water for obtaining the high-temperature water. An oxidizing agent such as oxygen, 17 hydrogen peroxide or ozone may be added to the water in advance . From the viewpoint of setting the BET specific surface area within the range of the present oxide, the temperature of the present high-temperature water is preferably 100°C or higher and the pressure is preferably 0.5 MPa or higher, more preferably the temperature is 374°C or higher and the pressure is 22.1 MPa or higher, and even more preferably the present high-temperature water is in a supercritical state .

[0057] In order to efficiently carry out the oxidation reaction in the step C, which will be described later, the step B preferably further includes a step of adding the oxidizing agent, and more preferably includes a step of adding an oxidizing agent that releases oxygen atoms. More preferably, the step of adding the oxidizing agent that releases oxygen atoms includes any one of a step (1) of adding the oxidizing agent that releases oxygen atoms to the water to obtain the present high-temperature water that satisfies the above-mentioned temperature and pressure, a step (2) of adding the oxidizing agent that releases oxygen atoms after the water is made into the present high-temperature water that satisfies the above-mentioned temperature and pressure, or a step (3) of making the water into the present high-temperature water that satisfies the above-mentioned temperature and pressure after adding the oxidizing agent that releases oxygen atoms to the water, and further adding the oxidizing agent that releases oxygen atoms .

[0058] In the step C, the present dispersion liquid or the solution obtained in the step A and the present high-temperature water obtained in the step B are mixed. In the step C, iridium and yttrium contained in the present dispersion liquid or the solution are oxidized to become the oxide. When using the production apparatus 100 of the present oxide, the conditions for mixing are as follows: by merging the liquid feeding route 5 through which the present dispersion liquid or the present solution obtained in the step A is sent and the liquid feeding route 6 through which the present high-temperature water obtained in the step B is sent, the present dispersion liquid or the present solution and the present high-temperature water are mixed, so that the dispersion liquid in which the oxide containing yttrium and iridium is dispersed in the present high-temperature water can be obtained. In FIG. 1, they are mixed in the reaction unit 4.

[0059] The dispersion liquid obtained in the step C is cooled in the cooling unit 9 shown in FIG. 1, and then collected in the collection section 8. Thereafter, a sample is separated and washed by filtration, centrifugation or the like and dehydrated in a dryer to obtain the present oxide containing yttrium and iridium.

[0060] Other than the above method, for example, by putting the present dispersion liquid or the solution obtained in the step A and the present hi gh-1 empe r a t ur e water obtained in the step B in the same container and mixing by stirring and the like to perform the oxidation reaction, the dispersion liquid in which the present oxide containing yttrium and iridium is dispersed in the present high-temperature water can be obtained. In this case, the water may be brought to the above-mentioned temperature and pressure in a separate container, and the resulting present high-temperature water may be added to the container containing the present dispersion liquid or the present solution, or the present dispersion liquid or the present solution liquid may be added to a container containing the present high-temperature water, or the present dispersion liquid or the present solution and the present high-temperature water may be put in one container at the same time. The addition may be continuous or intermittent.

[0061] In order to set the BET specific surface area of the present oxide to 50 m2 / g by the above method, for example, it is preferable that using the above-mentioned present high-temperature water, the present dispersion liquid or the present solution obtained in the step A and the present high-temperature water are mixed in the shortest possible time in the step C and then the mixture is cooled as quickly as possible after the step C. In particular, if the present high-temperature water is in a supercritical state, yttrium ions and iridium ions in the present dispersion liquid or the present solution are directly oxidized, and the particle size of the resulting oxide becomes small. It is considered that by further cooling in a short time, the BET specific surface area of the obtained oxide containing yttrium and iridium can be set within a desired range.

[0062] The production method using the liquid feeding routes as shown in FIG. 1 is preferable because the present oxide can be produced continuously and the average particle size of the obtained oxide can be made small. In the case of the production method using the liquid feeding routes as shown in Figure 1, by controlling the metal concentration, the liquid feeding rate, the temperature of the reaction unit, the cooling rate and the like of the present dispersion liquid or the present solution of the first supply source, the average particle size of the obtained present oxide can be controlled within the preferred range mentioned above. For example, the mixing time in the step C varies depending on the size of the production apparatus used, the material of the apparatus or the like, but is, for example, 0.1 seconds to 60 seconds. The cooling time after the step C also varies depending on the size of the production apparatus used, the material of the apparatus or the like, but is, for example, 1 second to 60 seconds.

[0063] When the present oxide contains a metal other than yttrium and iridium, metal particles or a metal compound containing the desired metal may be added separately in the step A or the step C. Further, when supporting the present oxide on the carrier, the present oxide may be isolated and then supported on the carrier by a conventional method. Furthermore, if necessary, the present oxide may be mixed with other components such as a stabilizer to form the present catalyst. Further, the obtained catalyst can be applied to the proton transport agent or the cation exchange polymer electrolyte membrane to form the oxygen evolution reaction catalyst layer and the electrolytic cell. Application methods include metal mask printing method, electrostatic coating method, dip coating method, spray coating method, roll coating method, doctor blade method, gravure coating method, screen printing method, or the like.

[0064] The present catalyst and the method for producing the present oxide has been described above. However, the present invention is not limited to the configuration of the above embodiment . For example, in the configuration of the abovedescribed embodiment, the present catalyst may additionally include any other configuration in the configuration of the embodiment or may be replaced with any other configuration that exhibits the same function. Further, the method for producing the present oxide may additionally include any other process in the configuration of the embodiment or may be replaced with any process that produces the same effect. EXAMPLES

[0065] Hereinafter, the present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0066] ( Examp1e 1) Production of oxide containing yttrium and iridium (YI- Iridium nitrate solution containing 1.92 g of iridium weight (manufactured by Furuya Metal Co., Ltd.) and 3.84 g of yttrium nitrate hydrate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were added to 2.8 L of water to form a mixture, and then the mixture was stirred and subjected to ultrasonication. Thereby, a metal compound mixed solution containing a homogeneous iridium compound and a homogeneous yttrium compound was obtained. Next, 10 mL of 30% hydrogen peroxide aqueous solution was added to 10 L of water at room temperature (25°C), and then the water temperature was adjusted to 430 °C and the water pressure was adjusted to 29 MPa to obtain high-temperature and high-pressure water. Next, the metal compound mixed solution obtained above was flowed into the reaction unit at a rate of 30 ml / min by the liquid feeding route, and the high-temperature and high-pressure water obtained above was flowed into the reaction unit at a rate of 2 00 ml / min through the liquid feeding route. Thereby, mixing was performed to obtain a dispersion liquid of an oxide containing iridium and yttrium. Thereafter, the mixed dispersion liquid of the oxide containing iridium and yttrium was adjusted to 1 atmosphere in the cooling unit, cooled to 20°C and collected in the collection unit. Thereafter, after filtration with a membrane filter, the filter cake was dried in an electric dryer at 80°C for 4 hours to obtain an oxide containing yttrium and iridium.

[0067] (Comparative Example 1) Preparation of oxide containing yttrium and iridium (YI-2) In a 1 L Teflon (registered trademark, the same applies hereinafter) beaker, iridium (IV) chloride containing 1.46 g of iridium weight (H21rCle • nH20 manufactured by Furuya Metal Co., Ltd.) and yttrium chloride hexahydrate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were added and 170 mL of pure water was added to form a mixture. Thereafter, the mixture was stirred at 200 rpm for 1 hour while raising the liquid temperature to 80°C to prepare an iridium chloride-yttrium chloride mixed solution. 21 Next, 25 g of sodium hydroxide was weighed out and dissolved in 250 mL of pure water to prepare a 10% sodium hydroxide solution, which was added dropwise to the iridium chlorideyttrium chloride mixed solution at a rate of 3 mL / min until the pH reached 11. After the dropwise addition was completed, the iridium chioride-y11rium chloride mixed solution was further stirred for 5 hours while maintaining the liquid temperature at 80°C.

[0068] The resulting slurry was allowed to cool down to room temperature and then allowed to stand, and the supernatant liquid was decanted. 300 mL of pure water was added to the Teflon beaker containing the remaining slurry, and the obtained mixture was stirred for 1 hour while raising the temperature thereof to 80°C again. After cooling the obtained mixture to room temperature, it was allowed to stand and the supernatant liquid was again decanted. Such decantation washing was carried out until the conductivity of the supernatant liquid did not change. Filtration was then carried out to obtain a filter cake. This filter cake was dried in an electric dryer at 60°C for 20 hours and then baked in the air at 1 000 ° for 10 hours in an electric furnace to obtain an oxide containing yttrium and iridium.

[0069] (Comparative Example 2) Preparation of iridium oxide (10-1) In a 5 L Teflon beaker, iridium chloride tetravalent preparation containing 50 g of iridium weight (H21rCle • nH20 manufactured by Furuya Metal Co., Ltd.)was added and 1.6 L of pure water was added to form a mixture. Thereafter, the mixture was stirred at 200 rpm for 1 hour while raising the liquid temperature to 80°C to prepare an iridium chloride solution . Next, 70 g of sodium hydroxide was weighed out and dissolved in 700 mL of pure water to prepare a 10% sodium hydroxide solution, which was added dropwise to the iridium chloride solution at a rate of 12 mL / min. After the dropwise addition was completed, the iridium chloride solution was further stirred for 10 hours while maintaining the liquid temperature at 80°C.

[0070] The resulting slurry was allowed to cool down to room temperature and then allowed to stand, and the supernatant liquid was decanted. 1300 mL of pure water was added to the Teflon beaker containing the remaining slurry, and the obtained mixture was stirred for 1 hour while raising the temperature thereof to 80°C again. After cooling the obtained mixture to room temperature, it was allowed to 22 stand and the supernatant liquid was again decanted. Such decantation washing was carried out until the conductivity of the supernatant liquid did not change. Filtration was then carried out to obtain a filter cake. This filter cake was dried in an electric dryer at 60°C for 20 hours and then baked in the air at 400° for 10 hours in an electric furnace to obtain iridium oxide. 70 g of zirconia balls with a diameter of 0.65 mm, 16 g of pure water, and 7 g of the iridium oxide were weighed into a 45 cc zirconia container, and the mixture was put in a planetary ball mill P-6 manufactured by Fritsche and pulverized at 500 rpm for 7.5 minutes. The iridium oxide slurry after pulverization was separated into zirconia balls having a diameter of 0.65 mm, and the iridium oxide slurry was filtered. The filter cake was dried in an electric dryer at 60°C for 20 hours, and the iridium oxide was pulverized in an agate mortar to obtain iridium oxide.

[0071] Powder X-ray diffraction was performed on the oxides containing yttrium and iridium obtained in Example 1 (YI-1), Comparative Example 1 (YI-2) and Comparative Example 2 ( IO-1) . The powder X-ray diffraction measurement method was performed using an X-ray diffraction (hereinafter referred to as XRD) device (Rigaku, Ultima IV). As specific measurement conditions, using CuKa radiation, the diffraction angle was first adjusted so that the diffraction angle 20 of Si (2,2,0) was 4 8.28 in an RSRP-Si standard powder sample. A glass substrate was filled with the obtained oxide, and XRD measurement was performed by first sweeping 20=10 to 90° at a sampling interval of 0.02° 20 and a scan speed of 10° 20 / min. The results are shown in FIGS. 2, 3 and 4.

[0072] As a result of powder X-ray diffraction, the catalyst of Example 1 (YI-1) has a broad peak around 30° to 35° at 20 and no other unique peaks, so the catalyst of Example 1 (YI-1) is considered to have an amorphous structure without a specific crystal structure. On the other hand, in the catalyst of Comparative Example 1 (YI-2), 29.5°, 34.3°, 49.2° and 58.4° were detected at 20, which are characteristic peaks of pyrochlore type Y2Ir2O7, so the catalyst of Comparative Example 1 (YI-2) is considered to be a pyrochlore type Y2lr2O?.

[0073] The specific surface areas of the catalysts of Example 1   (YI-1), Comparative Example 1   (YI-2) and Comparative Example 2 (10-1) were measured by a nitrogen adsorption method using a specific surface area / pore distribution measuring device, BELSORP-mini II. In addition, the data of the obtained adsorption isotherm was analyzed by the BET method of the analysis software BEL Master built into the specific surface area / pore distribution measuring device to determine the specific surface area. The results are shown in Table 1.

[0074] [Table 1] BET (mVg) Example 1 (YI-1) 152.2 Comparative Example 1 (YI-2) 18.5 Comparative Example 2 (10-1) 55.0 From Table 1, it was confirmed that the BET specific surface area of Example 1 was 50 m2 / g or more.

[0075] STEM observation of Example 1 (YI-1) was performed. In the measurement, a JEOL Ltd. model JEM-ARM200CF was used, and the STEM photograph image was shown in FIG. 5 at an acceleration voltage of 200 kV. As is clear from FIG. 5, it was confirmed that the particle size of the oxide containing yttrium and iridium obtained in Example 1 was 100 nm or less.

[0076] Oxygen evolution reaction evaluation (OER) mass activity Using the oxides containing yttrium and iridium obtained in Example 1 (YI-1) and Comparative Examples 1 and 2 (YI-2 and 10-1) as oxygen evolution reaction catalysts, 14.7 mg of each was weighed into a mixed solution of 15 mL of ultrapure water, 10 mL of 2-propanol (hereinafter referred to as IPA) and 0.1 mL of a 5 wt% Nation dispersion solution and dispersed using ultrasound. The obtained dispersion liquid was added onto a gold electrode on a rotating disk using a micropipette to prepare an electrode coated with a catalyst of 30 pg / cm2 . The thus prepared electrode was subjected to a rectangular wave durability test using an electrochemical measurement system (HZ-7000, manufactured by Hokuto Denko Co., Ltd.) . A 60 wt % perchloric acid solution (reagent for precision analysis, manufactured by Kanto Kagaku Co., Ltd.) was prepared to a concentration of 0.1 M, degassed with Ar gas and used as the electrolytic solution. A three-e1ectrode method was adopted as the measurement method, a hydrogen reference electrode in which hydrogen gas was passed through platinum black was used as the reference electrode, and the measurement was at 25°C. carried out in a constant temperature bath

[0077] Oxygen evolution reaction (hereinafter referred to as OER) mass activity was evaluated by sweeping the voltage range of 1.0 V to 1.8 V at a rate of 10 mV / sec and calculating the current density at 1.5 V (mA / cm2) by dividing the amount of catalyst applied to the electrode (30 pg / cm2) . The results are shown in Table 2. Example 1 (YI-1) and Comparative Example 1 (YI-2) are both oxides containing yttrium and iridium, but when the OER mass activity at 1.5V was compared based on the total metal amount of yttrium and iridium coated on the electrode, it was found that Example 1 (YI-1) was 1.8 times higher. When the OER mass activity was calculated based on the amount of iridium applied to the electrode, it was confirmed that Example 1 (YI-1) was about 3.9 times higher. In addition, in a comparison between Example 1 (YI-1) and Comparative Example 2 (10-1) , when comparing the OER mass activity at 1.5 V with the total amount of metal applied to the electrode, it was found that Example 1 (YI-1) was approximately 2.5 times higher than Comparative Example 2 (10-1) . Further, when the OER mass activity was calculated based on the amount of iridium applied to the electrode, it was found that Example 1 (YI-1) was approximately 3.9 times higher.

[0078] [Table 2] Amount of catalyst applied (pg / crrP! Iridium weigfit (u g / cmc OER mass'activity at 1.5 V (mA / mg-lr) OER ?nass activity at 1.5 V (mA / mg) Example 1 Vl-1) 29.86 16.55 42.14 76.06 Comparative Example 1 (Yi-2) 30.02 7.77 10.8 41.74 Comparative Example 2 (10-1) 30.37 25.86 1'6.5 19.3

[0079] As is clear from the above results, the catalyst containing the present oxide has an iridium single catalyst and a pyrochlore-type composite oxide of yttrium and iridium in terms of OER mass activity, but the catalyst showed higher performance than a catalyst having a BET specific surface area of less than 50 m2 / g. Therefore, by using the present oxide, an electrolysis catalyst can be provided that suppresses the amount of iridium used and has high oxygen evolution mass activity. REFFERENCE SIGNS LIST

[0080] 1 : First supply source 2: Second supply source 3: Heating unit 4: Reaction unit 5 : Liquid feeding route 6 : Liquid feeding route 7 : Liquid feeding route 8 : Collection unit 9 : Cooling unit 1 0 : Pressure adjusting mechanism 11 : Flow rate adjusting means 12 : Flow rate adjusting means 100 : Production apparatus

Claims

1. An oxygen evolution reaction catalyst comprising an oxide containing yttrium and iridium and having a BET specific surface area of 50 m2 / g or more.

2. The oxygen evolution reaction catalyst as claimed in claim 1, wherein the oxide has an average particle diameter of 100 nm or less.

3. An oxygen evolution reaction catalyst layer comprising the oxygen evolution reaction catalyst as claimed in claim 1 or 2 and a proton transport agent.

4. An electrolysis cell comprising the oxygen evolution reaction catalyst layer as claimed in claim 3 and an ion exchange polymer electrolyte membrane.

5. The electrolysis cell as claimed in claim 4, wherein the ion exchange polymer electrolyte membrane is a cation exchange polymer electrolyte membrane.

6. A method for producing the oxide as claimed in claim 1, the method comprising:a step A of (1) dispersing yttrium nanoparticles and iridium nanoparticles or yttrium hydroxide particles and iridium hydroxide particles in a dispersion medium to obtain a dispersion liquid or (2) dissolving an yttrium compound and an iridium compound in a solvent to obtain a solution;a step B of increasing a temperature of water to 100°C or higher and a pressure of the water to higher than 0.1 MPa; anda step C of mixing the dispersion liquid or the solution obtained in the step A and the high-temperature and high-pressure water obtained in the step B.

7. The method for producing the oxide as claimed in claim 6, wherein the step B includes a step of adding an oxidizing agent .

8. The method for producing the oxide as claimed in claim 7, wherein the oxidizing agent is an oxidizing agent that releases oxygen atoms.

9. The method for producing the oxide as claimed in claim 8, wherein the step B includes any one of (1) a step of adding the oxidizing agent that releases the oxygen atoms to the water and then increasing the temperature of the water to 100°C or higher and the pressure of the water to 27higher than 0.1 MPa, (2) a step of adding the oxidizing agent that releases the oxygen atoms to the water after increasing the temperature of the water to 100°C or higher and the pressure of the water to higher than 0.1 MPa, or (3) a step of adding the oxidizing agent that releases the oxygen atoms to the water, increasing the temperature of the water to 100°C or higher and the pressure of the water to higher than 0.1 MPa and then further adding the oxidizing agent that releases the oxygen atoms.

Citation Information

Patent Citations

  • Catalyst layer

    JP2014504433A

  • Electrocatalysts for efficient water electrolysis

    WO2016156599A1