Toner compositions and additives

JP2022074081A5Active Publication Date: 2024-11-01XEROX CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021176043
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-02
Filing Date
2021-10-28
Publication Date
2024-11-01
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

Toner compositions are sensitive to environmental conditions such as humidity, leading to issues like image background problems in hot and humid conditions and bright images in cold and dry conditions, and there is a need to improve additives for enhanced sensitivity and charge stability.

Method used

A toner composition containing polymeric additives with a polymeric resin comprising fluorinated acrylic monomers, cross-linking monomers with two or more vinyl groups, and a nitrogen-containing group charge control agent, which are applied to the toner particles to enhance sensitivity to relative humidity and charge stability.

Benefits of technology

The polymeric additives provide improved toner performance by reducing sensitivity to environmental conditions, allowing for better charge stability and hydrophobicity, and can be used at lower densities with comparable surface coverage, enhancing triboelectric charging properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To improve additives used in formation of EA ULM toners, and to improve sensitivity of toner compositions to environmental conditions including relative humidity.SOLUTION: A toner composition, a developer, and an additive for a toner composition are disclosed. The toner composition comprises toner particles containing at least one type of resin, an optional colorant, an optional wax, and a polymeric toner additive provided on at least portions of external surfaces of the toner particles. The polymeric toner additive comprises a polymeric resin containing a fluorinated acrylic monomer, a cross-linkable monomer containing two or more vinyl groups at 8 wt.% to 40 wt.% of the polymeric resin, and optionally a charge control agent consisting of a nitrogen-containing group at 0.1 wt.% to 1.5 wt.% of the polymeric resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure generally relates to toner compositions, and more specifically toner compositions comprising polymer additives. [Background technology]

[0002] Electrophotographic printing utilizes toner particles that can be produced by various processes. One such process involves an emulsion aggregation ("EA") process in which a surfactant is used to form a latex emulsion that forms toner particles. For example, see U.S. Patent No. 6,120,967, the disclosure of which is incorporated herein by reference in its entirety.

[0003] A combination of amorphous and crystalline polyesters can be used in the EA process. This resin combination can provide high gloss and relatively low melting point characteristics (sometimes called low melting, ultra-low melting, or ULM), enabling higher energy efficiency and faster printing. The use of additives containing EA toner particles may be important for achieving optimal toner performance, especially in the charged region. [Overview of the project] [Problems that the invention aims to solve]

[0004] One potential problem with toner is its sensitivity to environmental conditions, including humidity. For example, in summer, high temperatures and humidity can lead to user complaints about the background of images. In winter, cold and dry conditions can result in complaints about overly bright images. In some cases, excessive background blur can occur due to a decrease in the charge level caused by changes in the developer over time.

[0005] There is an ongoing need to improve the additives used in the formation of EA ULM toner. There is also a need to improve the sensitivity of the toner composition to environmental conditions, including relative humidity.

[0006] According to various embodiments, a toner composition is described, comprising toner particles containing at least one resin, an optional colorant, an optional wax, and a polymer toner additive on at least a portion of the outer surface of the toner particles. The polymer toner additive comprises a polymer resin having a fluorinated acrylic monomer, 8% to 40% by weight of the polymer resin of a crosslinkable monomer containing two or more vinyl groups, and optionally 0.1% to 1.5% by weight of the polymer resin of a nitrogen-containing charge control agent.

[0007] According to various embodiments, a developer is provided. The developer comprises a toner composition and a toner carrier. The toner composition comprises toner particles having at least one resin, an optional colorant, an optional wax, and a polymer toner additive on at least a portion of the outer surface of the toner particles. The polymer toner additive comprises a polymer resin having a fluorinated acrylic monomer, 8% to 40% by weight of the polymer resin of a crosslinkable monomer containing two or more vinyl groups, and optionally 0.1% to 1.5% by weight of the polymer resin of a charge-controlling agent monomer containing nitrogen groups.

[0008] This specification discloses a toner additive comprising a polymer resin containing a fluorinated acrylic monomer, a crosslinkable monomer containing two or more vinyl groups in an amount of 8% to 40% by weight of the polymer resin, and optionally 0.1% to 1.5% by weight of nitrogen-containing groups of the polymer resin. [Modes for carrying out the invention]

[0009] This disclosure provides polymer additives for use with toner particles.

[0010] The resulting polymer may be used as an additive to the toner composition, thereby increasing the sensitivity of the resulting toner to relative humidity and charge stability. The polymer additives of this disclosure can be used at lower densities in terms of specific gravity compared to other additives, and require far less material by weight to cover a comparable surface area compared to inorganic additives containing oxides such as titania and silica. The polymer additives of this disclosure can also provide toner particles with a wide range of properties, such as hydrophobicity and charge controllability, depending on the monomer used to form the polymer.

[0011] In the embodiment, the toner composition comprises toner particles of at least one resin. The toner composition may optionally contain a colorant. The toner composition may optionally contain a wax. The toner composition contains a polymer toner additive on at least a portion of the outer surface of the toner particles. The polymer toner additive comprises a polymer resin containing a fluorinated acrylic monomer, 8% to 40% by weight of the polymer resin of a crosslinkable monomer containing two or more vinyl groups, and optionally 0.1% to 1.5% by weight of the polymer resin of a charge control agent monomer consisting of nitrogen-containing groups. The polymer toner additive has a size of 25 nanometers to about 250 nanometers. The filling amount of the polymer toner additive is 0.1% to 5% by weight of the toner composition.

[0012] Suitable fluorinated acrylic monomers that can be used to form polymer additives include, for example, 2,4,6-trifluorophenyl acrylate, pentafluorophenyl acrylate, hexafluoroisopropyl methacrylate, 1H,1H,3H-hexafluorobutyl methacrylate, 2,2,2-trifluoroethyl acrylate, 2,2,2-trifluoroethyl methacrylate, 1H,1H,2H,2H-heptadecafluorodecyl methacrylate (HDFDMA), and 1H,1H,5H-octafluoropentyl methacrylate. 2,2,3,3,4,4,5,5,6,6,7,7-Dodecafluoroheptyl acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,12-Heneicosafluorododecyl acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,10-Heptadecafluorodecyl methacrylate, 2,2,3,3,4,4,4-Heptafluorobutyl acrylate, 2,2,3,3,4,4,4-Heptafluorobutyl methacrylate, 2,2,3,4,4,4 -Hexafluorobutyl acrylate, 2,2,3,4,4,4-Hexafluorobutyl methacrylate, 1,1,1,3,3,3-Hexafluoroisopropyl acrylate, 1,1,1,3,3,3-Hexafluoroisopropyl methacrylate, 2,2,3,3,4,4,5,5-Octafluoropentyl methacrylate, 2,2,3,3,3-Pentafluoropropyl acrylate, 2,2,3,3,3-Pentafluoropropyl methacrylate, 1H,1H,2H,2H-Perfluorodecyl acrylate, 2,2,3,3-Tet Examples include lafluoropropyl methacrylate, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl methacrylate, 2,2,2-trifluoroethyl methacrylate, 2-[(1',1',1'-trifluoro-2'-(trifluoromethyl)-2'-hydroxy)propyl]-3-norbornyl methacrylate, perfluorocyclohexyl (meth)acrylate, and any combination thereof.

[0013] Polymer additives also include crosslinkable monomers having at least two vinyl groups. Suitable monomers having at least two vinyl groups for use in polymer additives include, for example, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2'-bis(4-(acrylooxy / diethoxy)phenyl)propane, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, ethylene glycol dimethacrylate, and diethylene glycol dimethacrylate. Examples include dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, polypropylene glycol dimethacrylate, 2,2'-bis(4-(methacryloxy / diethoxy)phenyl)propane, 2,2'-bis(4-(methacryloxy / polyethoxy)phenyl)propane, trimethylolpropane trimethacrylate, tetramethylolmethane tetramethacrylate, divinylbenzene, divinylnaphthalene, divinyl ether, and combinations thereof. In embodiments, the crosslinking agent may be fluorinated. Suitable fluorinated crosslinking agents include fluorinated divinyl crosslinking agents, such as 1,8-divinylperfluoro(octane), 1,6-divinylperfluoro(hexane), and 1,4-divinylperfluoro(butane).

[0014] The fluorinated acrylic monomer may be present in the polymer additive in an amount of about 5% by weight of the copolymer to about 90% by weight of the polymer additive, and in embodiments, about 20% by weight to about 92% by weight of the polymer additive.

[0015] A crosslinkable monomer having at least two vinyl groups may be present in such polymer additives in an amount of about 8.0% by weight to about 40% by weight of the polymer additive, and in embodiments, about 10% by weight to about 25% by weight of the copolymer.

[0016] In the embodiments, examples of charge control monomers containing nitrogen groups include, but are not limited to, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, dipropylaminoethyl methacrylate, diisopropylaminoethyl methacrylate, dibutylaminoethyl methacrylate, and combinations thereof.

[0017] The charge-controlling monomer containing nitrogen-containing groups in the polymer additive is present in an amount of 0.1% to 1.5% by weight, about 0.6% to 1.2% by weight, or about 0.7% to about 1.1% by weight of the polymer additive.

[0018] One method for forming a polymer additive, in this embodiment, is emulsion polymerization of monomers used to form the polymer additive.

[0019] In the polymerization process, the reactants may be added to a suitable reactor, such as a mixing vessel. Appropriate amounts of the starting materials may be optionally dissolved in a solvent, and optional initiators may be added to the solution and brought into contact with at least one surfactant to form an emulsion. The copolymer may be formed in the emulsion, which can then be recovered and used as a polymer additive for toner compositions.

[0020] Suitable solvents for use include, but are not limited to, water and / or organic solvents, such as toluene, benzene, xylene, tetrahydrofuran, acetone, acetonitrile, carbon tetrachloride, chlorobenzene, cyclohexane, diethyl ether, dimethyl ether, dimethylformamide, heptane, hexane, methylene chloride, pentane, and combinations thereof.

[0021] In an embodiment, the latex for forming the polymer additive may be prepared in an aqueous phase containing a surfactant or a co-surfactant, optionally under an inert gas such as nitrogen. The surfactant that may be used together with the resin to form the latex dispersion may be an ionic or non-ionic surfactant in an amount of about 0.01 to about 15 weight percent of the solid, and in an embodiment, about 0.1 to about 10 weight percent of the solid.

[0022] Examples of anionic surfactants that can be used include sulfates and sulfonates, sodium dodecyl sulfate (SDS) known as sodium lauryl sulfate (SLS), sodium dodecylbenzene sulfonate, sodium dodecylnaphthalene sulfate, dialkylbenzene alkyl sulfates and sulfonates, acids such as abietic acid available from Aldrich, Neogen R (trademark) and Neogen SC (trademark) obtained from Dai-ichi Kogyo Seiyaku Co., Ltd., combinations thereof, and the like. Other suitable anionic surfactants include, in an embodiment, DOWFAX (trademark) 2A1, an alkyldiphenyloxide disulfonate from Dow Chemical Company, and / or Teika Power BN2060 from Teika Corporation (Japan), which are sodium branched dodecylbenzene sulfonates. Combinations of these surfactants with any of the aforementioned anionic surfactants may be used in an embodiment.

[0023] Examples of cationic surfactants include, but are not limited to, ammonium, such as alkylbenzyldimethylammonium chloride, dialkylbenzene alkylammonium chloride, lauryltrimethylammonium chloride, alkylbenzylmethylammonium chloride, alkylbenzyldimethylammonium bromide, benzalkonium chloride, C 12 ,C 15 ,C 17Examples include trimethylammonium bromide, combinations thereof, and the like. Other cationic surfactants include cetylpyridinium bromide, halide salts of quaternized polyoxyethylalkylamines, dodecylbenzyltriethylammonium chloride, MIRAPOL and ALKAQUAT available from Alkaril Chemical Company, Sanizol (benzalkonium chloride) available from Kao Chemicals, combinations thereof, and the like. In an embodiment, a suitable cationic surfactant includes SANISOL B-50 available from Kao Corp., which is mainly benzyl dimethyl alkonium chloride.

[0024] Examples of nonionic surfactants include, but are not limited to, alcohols, acids, and ethers, such as polyvinyl alcohol, polyacrylic acid, metarose, methyl cellulose, ethyl cellulose, propyl cellulose, hydroxyl ethyl cellulose, carboxymethyl cellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octyl phenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonyl phenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, combinations thereof, and the like. In an embodiment, surfactants commercially available from Rhone-Poulenc, such as IGEPAL CA-210 (trademark), IGEPAL CA-520 (trademark), IGEPAL CA-720 (trademark), IGEPAL CO-890 (trademark), IGEPAL CO-720 (trademark), IGEPAL CO-290 (trademark), IGEPAL CA-210 (trademark), ANTAROX 890 (trademark), and ANTAROX 897 (trademark) can be used.

[0025] The selection of specific surfactants or combinations thereof, as well as the respective usage amounts, are within the knowledge of those skilled in the art.

[0026] In embodiments, reaction initiators may be added for the formation of latex used in the formation of polymer additives. Examples of suitable reaction initiators include water-soluble reaction initiators, such as ammonium persulfate, sodium persulfate and potassium persulfate, and organic solvent-soluble reaction initiators, such as organic peroxides, and azo compounds, such as VAZO 64®, 2-methyl-2-2'-azobispropannitrile, VAZO 88®, 2-2'-azobisisobutylamide anhydride, and combinations thereof. Other water-soluble initiators that can be used include azoamidine compounds, such as 2,2'-azobis(2-methyl-N-phenylpropionamidine)dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine]tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine]dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine]dihydrochloride, and 2,2'-azobis[N-(2-hydroxy-ethyl)-2-methylpropionamidine]dihydrochloride. [Amidine]dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepine-2-yl)propane]dihydrochloride, 2,2'-azobis[2- Examples include (3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, and combinations thereof.

[0027] The initiator can be added in a suitable amount, for example, about 0.1 to about 8 weight percent of the monomer, and in some embodiments, about 0.2 to about 5 weight percent.

[0028] When forming the emulsion, starting materials, surfactants, optionally solvents, and optionally initiators can be combined using any means within the understanding of those skilled in the art. In embodiments, the reaction mixture may be mixed for about 1 minute to about 72 hours, or in embodiments about 4 hours to about 24 hours, while maintaining the temperature at about 10°C to about 100°C, in embodiments about 20°C to about 90°C, and in other embodiments about 45°C to about 75°C.

[0029] Those skilled in the art will understand that by optimizing the reaction conditions, temperature, and initiator load, polymers of various molecular weights can be produced, and that structurally related starting materials can be polymerized using equivalent techniques.

[0030] The resulting latex has the polymer additives of the present disclosure and can be applied to toner particles by any means within the intent of those skilled in the art. In embodiments, toner particles may be immersed in or sprayed with the latex containing the polymer additives, and thus coated, and the coated particles can then be dried to leave the polymer coating on top.

[0031] In other embodiments, once the polymer additive for the toner is formed, it can be recovered from the latex by any technique within the scope of the intent of those skilled in the art, including filtration, drying, centrifugation, spray drying, and combinations thereof.

[0032] In embodiments, the copolymer obtained, which is to be used as a toner additive, can be dried into a powder form by any method within the intent of those skilled in the art, including, for example, freeze-drying, optionally spray-drying in a vacuum, or a combination thereof. The dried polymer additive of the present disclosure can then be applied to toner particles by any means within the intent of those skilled in the art, including, but not limited to, mechanical impact and / or electrostatic attraction. An example of a mechanical mixing apparatus is the Henschel FM high-strength mixer from Zeppelin Systems, but other mixing apparatuses may also be used in embodiments.

[0033] Copolymer particles may have an average or medium particle size (D50) of approximately 20 nanometers to 250 nanometers in diameter, and in embodiments, approximately 40 nanometers to 150 nanometers in diameter. The particle size of suspended particles ranging in size from 0.0008 to 6.54 micrometers is measured using a Nanotrac 252 instrument. This instrument uses laser light scattering techniques to measure the Doppler shift light generated from each particle in motion (Brownian motion). The signals generated by these shifts are proportional to the particle size. The signals are mathematically converted into particle size and particle size distribution. The analysis may be performed using an external probe or by inserting the probe into a fixed sample chamber. As used herein, the term “D50” refers to the diameter (by volume, unless otherwise specified) in which 50% of the sample consists of particles with a diameter less than that value. D50 may also be referred to as “average particle size.” For light scattering techniques, NIST polystyrene nanosphere control samples with diameters in the range of 15 mm to 150 mm can be used under the trademark name NIST Traceable Reference Material for Nanotrac Particle Size Analyzers, obtained from Microtrac.

[0034] Copolymers used as polymer additives, which in embodiments are soluble in solvents such as tetrahydrofuran (THF), have a number-average molecular weight (M) of, for example, about 40,000 to about 280,000 daltons, and in embodiments, about 60,000 to about 170,000 daltons, when measured by gel permeation chromatography (GPC) using a polystyrene standard. n ), and when measured by gel transmission chromatography, for example, a weight-average molecular weight (M) of about 200,000 to about 800,000 daltons, and in embodiments, about 400,000 to about 600,000 daltons. w ) may have. In the embodiment, the solubility of the crosslinked resin is limited by crosslinking, so it may be impossible to measure the molecular weight by any method.

[0035] Copolymers used as polymer additives may have a glass transition temperature (Tg) of about 85°C to about 140°C, and in embodiments, about 100°C to about 130°C. In embodiments, it may be impossible to determine the Tg due to crosslinking of the resin, which may make detection of the Tg difficult. In embodiments, the A-zone charge of a toner containing the polymer additive of this disclosure may be about -15 to about -80 microcoulombs per gram, and in embodiments, about -20 to about -60 microcoulombs per gram, while the J-zone charge of a toner containing the polymer additive of this disclosure may be about -15 to about -80 microcoulombs per gram, and in embodiments, about -20 to about -60 microcoulombs per gram.

[0036] The polymer additives of this disclosure may be combined with toner particles in an amount of about 0.1% by weight to about 5% by weight of the toner particles, and in embodiments, about 0.2% by weight to about 2% by weight of the toner particles.

[0037] Therefore, the polymer additive compositions and processes of this disclosure allow for the formulation of developers having selected high triboelectric charging properties and / or conductivity values ​​by utilizing several different combinations. toner

[0038] The polymer additive thus produced may then be optionally combined with a toner resin having a colorant to form the toner of the present disclosure. resin

[0039] Any toner resin can be used when forming the toner of the present disclosure. Such a resin may then be prepared by any suitable monomer or any suitable polymerization method with any suitable monomer. In embodiments, the resin may be prepared by a method other than emulsion polymerization. In further embodiments, the resin may be prepared by condensation polymerization.

[0040] The toner compositions of this disclosure, in embodiments, include an amorphous resin. The amorphous resin may be linear or branched. In embodiments, the amorphous resin may include at least one low molecular weight amorphous polyester resin. Low molecular weight amorphous polyester resins, available from numerous sources, may have a variety of glass transition temperatures, for example, about 30°C to about 80°C, and in embodiments about 35°C to about 75°C. When used herein, the low molecular weight amorphous polyester resin has a number average molecular weight (M) of, for example, about 1,000 to about 10,000, in embodiments about 2,000 to about 8,000, in embodiments about 3,000 to about 7,000, and in embodiments about 4,000 to about 6,000, as measured by gel permeation chromatography (GPC). n ) has. The weight-average molecular weight (M) of the resin. w The molecular weight distribution (M) of low molecular weight amorphous resins is less than or equal to 50,000 when determined by GPC using polystyrene standards, for example, in embodiments, about 2,000 to about 50,000, in embodiments, about 3,000 to about 40,000, in embodiments, about 10,000 to about 30,000, and in embodiments, about 18,000 to about 21,000. w / Mn ) is, for example, from about 2 to about 6, and in an embodiment from about 3 to about 4. The low molecular weight amorphous polyester resin may have an acid value of from about 8 to about 20 mg KOH / g, in an embodiment from about 9 to about 16 mg KOH / g, and in an embodiment from about 10 to about 14 mg KOH / g.

[0041] Examples of linear amorphous polyester resins that can be used include poly(propoxylated bisphenol A cofumarate), poly(ethoxylated bisphenol A cofumarate), poly(butyloxylated bisphenol A cofumarate), poly(copropoxylated bisphenol A coethoxylated bisphenol A cofumarate), poly(1,2-propylene fumarate), poly(propoxylated bisphenol A comalate), poly(ethoxylated bisphenol A comalate), poly(butyloxylated bisphenol A comalate), poly(copropoxylated bisphenol A coethoxylated bisphenol A comalate), poly(1,2-propylene maleate), poly(propoxylated bisphenol A coitaconate), poly(ethoxylated bisphenol A coitaconate), poly(butylenated bisphenol A coitaconate), poly(copropoxylated bisphenol A coethoxylated bisphenol A coitaconate), poly(1,2-propylene itaconate), and combinations thereof.

[0042] In an embodiment, suitable amorphous resins can include alkoxylated bisphenol A fumarate / terephthalate-based polyester and copolyester resins. In an embodiment, a suitable amorphous polyester resin can be a copoly(propoxylated bisphenol A cofumarate)-copoly(propoxylated bisphenol A coterephthalate) resin having the following formula (I),

Chemical formula

[0043] In embodiments, the low molecular weight amorphous polyester resin may be a saturated or unsaturated amorphous polyester resin. Exemplary examples of saturated and unsaturated amorphous polyester resins selected for the processes and particles of this disclosure include: polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polypentylene terephthalate, polyhexylene terephthalate, polyheptadene terephthalate, polyoctalene terephthalate, polyethylene isophthalate, polypropylene isophthalate, polybutylene isophthalate, polypentylene isophthalate, and polyhexylene isophthalate. Polyheptadene-isophthalate, polyoctalene-isophthalate, polyethylene-sebacate, polypropylene-sebacate, polybutylene-sebacate, polyethylene-aziperte, polypropylene-aziperte, polybutylene-aziperte, polypentylene-aziperte, polyhexylene-aziperte, polyheptadene-aziperte, polyoctalene-aziperte, polyethylene-glutarate, polypropylene-glutarate, polybutylene-glutarate, polypentylene-glutarate, polyhexylene- Glutarate, polyheptadene-glutarate, polyoctalene-glutarate, polyethylene-pimelate, polypropylene-pimelate, polybutylene-pimelate, polypentylene-pimelate, polyhexylene-pimelate, polyheptadene-pimelate, poly(ethoxylated bisphenol A-fumarate), poly(ethoxylated bisphenol A-succinate), poly(ethoxylated bisphenol A-azipart), poly(ethoxylated bisphenol A-glutarate), poly(ethoxylated bisphenol A-fumarate), Poly(ethoxylated bisphenol A-terephthalate), poly(ethoxylated bisphenol A-isophthalate), poly(ethoxylated bisphenol A-dodecenyl succinate), poly(propoxylated bisphenol A-fumarate), poly(propoxylated bisphenol A-succinate), poly(propoxylated bisphenol A-aziperte), poly(propoxylated bisphenol A-glutarate), poly(propoxylated bisphenol A-terephthalate), poly(propoxylated bisphenol A-isophthalate),Examples of various amorphous polyesters include poly(propoxylated bisphenol A-dodecenyl succinate), SPAR (Dixie Chemicals), BECKOSOL (Reichhold Inc.), ARAKOTE (Ciba-Geigy Corporation), HETRON (Ashland Chemical), PARAPLEX (Rohm & Haas), POLYLITE (Reichhold Inc.), PLASTHALL (Rohm & Haas), CYGAL (American Cyanamide), ARMCO (Armco Composites), ARPOL (Ashland Chemical), CELANEX (Celanese Eng), RYNITE (DuPont), STYPOL (Freeman Chemical Corporation), and combinations thereof. The resins may also be functionalized, such as carboxylation, sulfonation, or, if particularly desired, sodium sulfonation.

[0044] Examples of polycondensation catalysts suitable for any low molecular weight amorphous polyester resin include tetraalkyl titanates, dialkyltin oxides such as dibutyltin oxide, tetraalkyltins such as dibutyltin dilaurate, dialkyltin oxide hydroxides such as butyltin oxide hydroxide, aluminum alkoxides, alkylzincs, dialkylzincs, zinc oxide, stannous oxide, or mixtures thereof. This catalyst can be used in amounts of, for example, about 0.01 mol% to about 5 mol%, based on the diacid or diester used as the starting material for producing the polyester resin.

[0045] Low molecular weight amorphous polyester resins may also be branched resins. As used herein, the terms "branched" or "branched" include branched resins and / or crosslinked resins.

[0046] The resulting unsaturated polyester is reactive (e.g., crosslinkable) in two leading parts: (i) unsaturated sites (double bonds) along the polyester chain, and (ii) functional groups suitable for acid-base reactions, such as carboxyl groups and hydroxyl groups. In embodiments, the unsaturated polyester resin is prepared by melt polycondensation or other polymerization processes using diacids and / or anhydrides and diols.

[0047] In embodiments, the low molecular weight amorphous polyester resin or combination of low molecular weight amorphous resins may have a glass transition temperature (Tg) of, for example, about 30°C to about 80°C, and in embodiments, about 35°C to about 70°C, when measured by DSC. In further embodiments, the combined amorphous resins have a glass transition temperature of about 10 to about 1,000,000 Pa at about 130°C. * S, in the embodiment, approximately 50 to approximately 100,000 Pa * It may have a melting viscosity of S.

[0048] The amount of low molecular weight amorphous polyester resin in the toner particles of the present disclosure may be present in any core, any shell, or both in amounts of 25 to about 50% by weight, in embodiments about 30 to about 45% by weight, and in embodiments about 35 to about 43% by weight of toner particles (i.e., toner particles excluding external additives and water).

[0049] In embodiments, the toner composition comprises at least one crystalline resin. As used herein, “crystalline” refers to polyester having a three-dimensional order. As used herein, “semi-crystalline resin” refers to a resin having a crystallinity of, for example, about 10 to about 90%, and in embodiments, about 12 to about 70%. Furthermore, as used below, “crystalline polyester resin” and “crystalline resin” encompass both crystalline and semi-crystalline resins unless otherwise specified.

[0050] In this embodiment, the crystalline polyester resin is either a saturated crystalline polyester resin or an unsaturated crystalline polyester resin.

[0051] Crystalline polyester resins, available from many sources, can have a variety of melting points, for example, from about 30°C to about 120°C, and in embodiments, from about 50°C to about 90°C. When measured, for example, by gel permeation chromatography (GPC), the number average molecular weight (M) of the crystalline resin is, for example, from about 1,000 to about 50,000, in embodiments, from about 2,000 to about 25,000, in embodiments, from about 3,000 to about 15,000, and in embodiments, from about 6,000 to about 12,000. n ) may have. Molecular weight distribution of crystalline resin (M w / M n The acid value is, for example, about 2 to about 6, and in embodiments, about 3 to about 4. The crystalline polyester resin may have an acid value of about 2 to about 20 mg KOH / g, in embodiments, about 5 to about 15 mg KOH / g, and in embodiments, about 8 to about 13 mg KOH / g.

[0052] Examples of crystalline polyester resins include poly(ethylene-adipate), poly(propylene-adipate), poly(butylene-adipate), poly(pentylene-adipate), poly(hexylene-adipate), poly(octylene-adipate), poly(ethylene-succinate), poly(propylene-succinate), poly(butylene-succinate), poly(pentylene-succinate), poly(hexylene-succinate), poly(octylene-succinate), poly(ethylene-sevacate), and poly(propylene-sevacate). Poly(butylene-sebacate), Poly(pentylene-sebacate), Poly(hexylene-sebacate), Poly(octylene-sebacate), Poly(nonylene-sebacate), Poly(decylene-sebacate), Poly(undecylene-sebacate), Poly(dodecylene-sebacate), Poly(ethylene-dodecanediote), Poly(propylene-dodecanediote), Poly(butylene-dodecanediote), Poly(pentylene-dodecanediote), Poly(hexylene-dodecanediote), Poly(octylene-dodecanediote) Poly(nonylene-dodecanediote), poly(decylene-dodecanediote), poly(undecylene-dodecanediote), poly(dodecylene-dodecanediote), poly(ethylene-fumarate), poly(propylene-fumarate), poly(butylene-fumarate), poly(pentylene-fumarate), poly(hexylene-fumarate), poly(octylene-fumarate), poly(nonylene-fumarate), poly(decylene-fumarate), copoli(5-sulfoisophthaloyl)-copoly(ethylene-aziparte), copoli( 5-Sulfoisophthaloyl)-copoly(propylene-adipate), copoly(5-sulfoisophthaloyl)-copoly(butylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(pentylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(hexylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(octylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(ethylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(propylene-adipate),Copoly(5-sulfo-isophthaloyl)-copoly(butylene-adipate), Copoly(5-sulfo-isophthaloyl)-copoly(pentylene-adipate), Copoly(5-sulfo-isophthaloyl)-copoly(hexylene-adipate), Copoly(5-sulfo-isophthaloyl)-copoly(octylene-adipate), Copoly(5-sulfoisophthaloyl)-copoly(ethylene-succinate), Copoly(5-sulfoisophthaloyl)-copoly( Propylene succinate), copoli(5-sulfoisophthaloyl)-copoly(butylene succinate), copoli(5-sulfoisophthaloyl)-copoly(pentylene succinate), copoli(5-sulfoisophthaloyl)-copoly(hexylene succinate), copoli(5-sulfoisophthaloyl)-copoly(octylene succinate), copoli(5-sulfo-isophthaloyl)-copoly(ethylene sebacate), copoli(5-sulfo (5-isophthaloyl)-copoly(propylene-sebacate), (5-sulfo-isophthaloyl)-copoly(butylene-sebacate), (5-sulfo-isophthaloyl)-copoly(pentylene-sebacate), (5-sulfo-isophthaloyl)-copoly(hexylene-sebacate), (5-sulfo-isophthaloyl)-copoly(octylene-sebacate), (5-sulfo-isophthaloyl) Examples of various crystalline polyesters include -copoly(ethylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(propylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(butylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(pentylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(hexylene-adipate), and any combination thereof.

[0053] Crystalline resins can be prepared by a polycondensation process involving the reaction of a suitable organic diol with a suitable organic diacid in the presence of a polycondensation catalyst.

[0054] Examples of organic diols selected for the preparation of crystalline polyester resins include aliphatic diols having approximately 2 to 36 carbon atoms.

[0055] Examples of organic diacids or diesters selected for the preparation of crystalline polyester resins include oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, naphthalene-2,7-dicarboxylic acid, cyclohexanedicarboxylic acid, malonic acid and mesaconic acid, their diesters or anhydrides; and alkali sulfo-organic diacids, such as dimethyl-5-sulfo-isophthalate and dialkyl-5-sulfo-isophthalate-4-sulfo-1,8-naphthalic acid. Examples include aqueous solutions, 4-sulfophthalic acid, dimethyl-4-sulfophthalate, dialkyl-4-sulfophthalate, 4-sulfophenyl-3,5-dicarbomethoxybenzene, 6-sulfo-2-naphthyl-3,5-dicarbomethoxybenzene, sulfo-terephthalic acid, dimethyl-sulfo-terephthalate, 5-sulfo-isophthalic acid, dialkyl-sulfo-terephthalate, sulfo-p-hydroxybenzoic acid, sodium, lithium, or potassium salts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, or mixtures thereof. Organic diacids may be selected in amounts of, for example, about 40 to about 50 mole percent of the resin, and alkali sulfoaliphatic diacids may be selected in amounts of about 1 to about 10 mole percent of the resin.

[0056] In the embodiment, the preferred crystalline resin may include a resin made of ethylene glycol or nonanediol, and a mixture of dodecanediic acid and fumaric acid comonomer having the following formula (II): [ka] In the formula, b is approximately 5 to approximately 2000, and d is approximately 5 to approximately 2000.

[0057] When semicrystalline polyester resins are used herein, the semicrystalline resins include poly(3-methyl-1-butene), poly(hexamethylene carbonate), poly(ethylene-p-carboxyphenoxybutyrate), poly(ethylene vinyl acetate), poly(docosyl acrylate), poly(dodecyl acrylate), poly(octadecyl acrylate), poly(octadecyl methacrylate), poly(behenyl polyethoxyethyl methacrylate), poly(ethylene adipate), poly(decamethylene adipate), poly(decamethylene azelaate), poly(hexamethylene oxalate), poly(decamethylene oxalate), poly(ethylene oxide), poly(propylene oxide), poly(butadiene oxide), poly(decamethylene oxide), poly(decamethylene sulfide), poly(decamethylene disulfide), and poly(ethylene seba Poly(decamethylene sebacate), poly(ethylene sverate), poly(decamethylene succinate), poly(eicosamethylene malonate), poly(ethylene-p-carboxyphenoxy undecanoate), poly(ethylenedithion ethophthalate), poly(methylethylene terephthalate), poly(ethylene-p-carboxyphenoxy valerate), poly(hexamethylene-4,4'-oxydibenzoate), poly Possible examples include poly(10-hydroxycapric acid), poly(isophthalaldehyde), poly(octamethylene dodecanediate), poly(dimethylsiloxane), poly(dipropylsiloxane), poly(tetramethylenephenylenediacetate), poly(tetramethylene trithiodicarboxylate), poly(trimethylene dodecanediate), poly(m-xylene), poly(p-xylylenepimeramide), and combinations thereof.

[0058] The amount of crystalline polyester resin in the toner particles of this disclosure may be present in the core, shell, or both in amounts of 1 to about 15% by weight, in embodiments about 5 to about 10% by weight, and in embodiments about 6 to about 8% by weight of toner particles (i.e., toner particles excluding external additives and water).

[0059] In embodiments, the toner of the present disclosure may also contain at least one high molecular weight branched or crosslinked amorphous polyester resin. Examples of such high molecular weight resins in embodiments include branched amorphous resins or amorphous polyesters, crosslinked amorphous resins or amorphous polyesters, or mixtures thereof, or crosslinked non-crosslinked amorphous polyester resins. According to the present disclosure, about 1% to about 100% by weight of the high molecular weight amorphous polyester resin may be branched or crosslinked, and in embodiments, about 2% to about 50% by weight of the high molecular weight amorphous polyester resin may be branched or crosslinked.

[0060] When used herein, high molecular weight amorphous polyester resins have a number average molecular weight (M) of approximately 1,000 to approximately 10,000, as measured by, for example, gel permeation chromatography (GPC). n ) may have. High molecular weight amorphous resins available from numerous sources may have a variety of glass transition onset temperatures (Tg) when measured by differential scanning calorimeter (DSC), for example, about 40°C to about 80°C, in embodiments about 50°C to about 70°C, and in embodiments about 54°C to about 68°C. In embodiments, linear and branched amorphous polyester resins may be saturated or unsaturated resins.

[0061] High molecular weight amorphous polyester resins can be prepared by branching or crosslinking linear polyester resins. Branching agents such as trifunctional or polyfunctional monomers can be used, and these agents typically increase the molecular weight and polydispersity of the polyester. Suitable branching agents include glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, diglycerol, trimellitic acid, trimellitic anhydride, pyromellitic acid, pyromellitic anhydride, 1,2,4-cyclohexanetricarboxylic acid, 2,5,7-naphthalentricarboxylic acid, 1,2,4-butanetricarboxylic acid, and combinations thereof. These branching agents can be used in effective amounts of about 0.1 mol% to about 20 mol%, based on the diacid or diester used as the starting material for the resin.

[0062] In some embodiments, the crosslinked polyester resin may be made from a linear amorphous polyester resin containing unsaturated moieties that can react under free radical conditions. In some embodiments, suitable unsaturated polyester resins can be prepared from diacids and / or anhydrides such as maleic anhydride, terephthalic acid, trimellitic acid, fumaric acid, and combinations thereof, and diols such as bisphenol A ethylene oxide adduct, bisphenol A-propylene oxide adduct, and combinations thereof. In some embodiments, a suitable polyester is poly(propoxylated bisphenol A co-fumaric acid).

[0063] In embodiments, crosslinked branched polyesters may be used as high molecular weight amorphous polyester resins. Examples of such polyesters and methods for synthesizing them are disclosed in U.S. Patent No. 6,592,913, the entire disclosure of which is incorporated herein by reference.

[0064] Suitable polyols contain about 2 to about 100 carbon atoms and may have at least two or more hydroxyl groups, or esters thereof. Examples of polyols include glycerol, pentaerythritol, polyglycol, polyglycerol, or mixtures thereof. The polyol may contain glycerol. Suitable esters of glycerol include glycerol palmitate, glycerol sebacate, glycerol azipart, and triacetin trippropionine. The polyol may be present in an amount of about 20% to about 30% by weight of the reaction mixture, and in embodiments, about 22% to about 26% by weight of the reaction mixture.

[0065] In embodiments, the crosslinked branched polyester of the high molecular weight amorphous polyester resin may include those resulting from the reaction of dimethyl terephthalate, 1,3-butanediol, 1,2-propanediol, and pentaerythritol.

[0066] In embodiments, a high molecular weight resin, such as a branched polyester, may be present on the surface of the toner particles of the present disclosure. The high molecular weight resin on the surface of the toner particles may also be particulate, and may be high molecular weight resin particles having a diameter of about 100 nanometers to about 300 nanometers, and in embodiments, about 110 nanometers to about 150 nanometers.

[0067] The amount of high molecular weight amorphous polyester resin in the toner particles of this disclosure may be about 25% to about 50% by weight of the toner in any core, any shell, or both; in embodiments, about 30% to about 45% by weight; in other embodiments, or about 40% to about 43% by weight of the toner (i.e., toner particles excluding external additives and water).

[0068] The ratio of crystalline resin to low molecular weight amorphous resin to high molecular weight amorphous polyester resin may range from approximately 1:1:98 to approximately 98:1:1 to approximately 1:98:1, approximately 1:5:5 to approximately 1:9:9 in embodiments, and approximately 1:6:6 to approximately 1:8:8 in embodiments. surfactants

[0069] In the embodiment, the resin, wax, and other additives used to form the toner composition may be in a dispersion containing a surfactant. Furthermore, the toner particles may be formed by an emulsion flocculation method, in which the resin and other components of the toner are placed in one or more surfactants to form an emulsion, the toner particles are agglomerated and bonded, and optionally washed, dried, and recovered.

[0070] One, two, or more surfactants may be used. The surfactants may be selected from ionic surfactants and nonionic surfactants. Anionic surfactants and cationic surfactants are included in the term "ionic surfactants". In embodiments, the surfactant may be used in an amount of about 0.01% to about 5% by weight of the toner composition, for example, about 0.75% to about 4% by weight of the toner composition, and in embodiments, about 1% to about 3% by weight of the toner composition.

[0071] Examples of nonionic surfactants that can be used include, for example, polyacrylic acid, metalrose, methylcellulose, ethylcellulose, propylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, and IGEPAL CA-210(trademark), IGEPAL CA-520(trademark), IGEPAL CA-720(trademark), IGEPAL CO-890(trademark), IGEPAL CO-720(trademark), IGEPAL CO-290(trademark), IGEPAL CA-210(trademark), ANTAROX 890(trademark), and ANTAROX 897(trademark), all available from Rhone-Poulenc. Other examples of suitable nonionic surfactants include block copolymers of polyethylene oxide and polypropylene oxide, including Synperonic PE / F, which in some embodiments is commercially available as Synperonic PE / F 108.

[0072] The anionic surfactants that can be used include those mentioned above. Examples of cationic surfactants include those mentioned above. Coloring agents

[0073] The latex particles produced as described above can be added to a colorant to produce toner. In embodiments, the colorant may be in the form of a dispersion. The colorant dispersion may contain, for example, submicron colorant particles having a volume average diameter of about 50 to about 500 nanometers, and in embodiments, a volume average diameter of about 100 to about 400 nanometers. The colorant particles may be suspended in an aqueous phase containing an anionic surfactant, a nonionic surfactant, or a combination thereof. Suitable surfactants include any of the surfactants described above. In embodiments, the surfactant may be ionic and may be present in the dispersion in an amount of about 0.1 to about 25% by weight of the colorant, and in embodiments, about 1 to about 15% by weight of the colorant.

[0074] Colorants useful for toner formation according to this disclosure include pigments, dyes, mixtures of pigments and dyes, mixtures of pigments, and mixtures of dyes. The colorants may be, for example, carbon black, cyan, yellow, magenta, red, orange, brown, green, blue, violet, or mixtures thereof.

[0075] In embodiments where the coloring agent is a pigment, the pigment may be, for example, carbon black, phthalocyanine, quinacridone or rhodamine B(trademark), red, green, orange, brown, violet, yellow, a fluorescent coloring agent, or the like.

[0076] If desired, stirring the resulting latex and colorant dispersion in the dispersion and heating it to a temperature of about 35°C to about 70°C, or in embodiments, about 40°C to about 65°C, may yield toner aggregates with a volume average diameter of about 2 micrometers to about 10 micrometers, or in embodiments, about 5 micrometers to about 8 micrometers. wax

[0077] Optionally, wax may also be combined with resin to form toner particles. If included, the wax may be present in an amount of, for example, about 1% to about 25% by weight of the toner particles, and in embodiments, about 5% to about 20% by weight of the toner particles.

[0078] Examples of waxes that can be selected include waxes having a weight-average molecular weight of about 500 to about 20,000, and in embodiments, about 1,000 to about 10,000. Examples of waxes that can be used include polyolefins such as polyethylene, polypropylene, and polybutene wax; plant-based waxes such as carnauba wax, rice wax, candelilla wax, wood wax, and jojoba oil; animal-based waxes such as beeswax; mineral waxes and petroleum-based waxes such as montan wax, ozokerite, ceresin, paraffin wax, microcrystalline wax, and Fischer-Tropsch wax; ester waxes obtained from higher fatty acids and higher alcohols such as stearyl stearate and behenyl behenate; butyl stearate; propyl oleate. Examples include ester waxes obtained from higher fatty acids such as glyceride monostearate, glyceride distearate, and pentaerythritol tetrabehenate and monohydric or polyhydric lower alcohols; ester waxes obtained from higher fatty acids such as diethylene glycol monostearate, dipropylene glycol distearate, diglyceryl distearate, and triglyceryl tetrastearate and polyhydric alcohol multimers; sorbitan higher fatty acid ester waxes such as sorbitan monostearate; and cholesterol higher fatty acid ester waxes such as cholesteryl stearate. Toner preparation

[0079] Toner particles can be prepared by any method within the intent of those skilled in the art. Embodiments relating to the production of toner particles are described below with respect to emulsion agglomeration processes, but any suitable method for preparing toner particles may be used, including chemical processes such as suspension and encapsulation methods, the respective disclosures of which are incorporated herein in their entirety by reference. In embodiments, toner compositions and toner particles may be prepared by agglomeration and bonding processes, in which small-particle resin particles are agglomerated to a suitable toner particle size and then bonded to achieve the final shape and form of toner particles.

[0080] In embodiments, the toner composition may be prepared by an emulsion flocculation process, such as a process comprising flocculating an emulsion containing the resin in the surfactant with a mixture of optionally selected wax and any other desired or required additives, and then bonding the flocculated mixture. The mixture may also be prepared by adding optionally selected wax or other material (which may be in a dispersion(or more) containing the surfactant) to an emulsion (which may be a mixture of two or more emulsions containing the resin). The pH of the resulting mixture can be adjusted with an acid, for example, acetic acid or nitric acid. In embodiments, the pH of the mixture can be adjusted to about 2 to about 4.5. In addition, in embodiments, the mixture may be homogenized. If the mixture is homogenized, homogenization may be achieved by mixing at about 1,000 to about 6,000 revolutions per minute. Homogenization may be achieved by any preferred means, for example, an IKA ULTRA TURRAX T50 probe homogenizer.

[0081] Following the preparation of the above mixture, a flocculant may be added to the mixture. Toner may be formed using any suitable flocculant. Suitable flocculants include, for example, aqueous solutions of divalent or polyvalent cationic materials. The flocculant may be, for example, a polyaluminum halide such as polyaluminum chloride (PAC), or a corresponding bromide, fluoride, or iodide, or an aluminum polysilicate such as polyaluminum sulfosilicate (PASS), and a water-soluble metal salt containing aluminum chloride, aluminum nitrite, aluminum sulfate, aluminum sulfate, calcium chloride, calcium nitrite, calcium oxyate, calcium sulfate, magnesium acetate, magnesium nitrate, magnesium sulfate, zinc acetate, zinc nitrate, zinc sulfate, zinc chloride, zinc bromide, magnesium bromide, copper chloride, copper sulfate, and combinations thereof. In the embodiment, the flocculant may be added to the mixture at a temperature below the glass transition temperature (Tg) of the resin.

[0082] The flocculant may be added to the mixture used to form the toner in an amount of about 0.1% to about 8% by weight of the resin in the mixture, about 0.2% to about 5% by weight in an embodiment, and about 0.5% to about 5% by weight in another embodiment. This provides a sufficient amount of the agent for flocculation. Shell resin

[0083] In this embodiment, the shell may be applied to the aggregated particles after aggregation but before cementation.

[0084] Examples of resins that can be used to form the shell include, but are not limited to, the amorphous resins used for the core. Such amorphous resins may be low molecular weight resins, high molecular weight resins, or combinations thereof. In embodiments, an example of an amorphous resin that can be used to form the shell according to this disclosure is the amorphous polyester of formula I described above.

[0085] In some embodiments, the amorphous resin used to form the shell may be crosslinked. For example, crosslinking can be achieved by combining the amorphous resin with a crosslinking agent, sometimes referred to herein as a reaction initiator in embodiments. Examples of suitable crosslinking agents include, but are not limited to, the above-mentioned organic peroxides and azo compounds, which are suitable for forming a gel within the core, as free radicals or thermal reaction initiators.

[0086] The crosslinking agent and amorphous resin may be combined for a sufficient time and temperature to form a crosslinked polyester gel. In embodiments, the crosslinking agent and amorphous resin may be heated to a temperature of about 25°C to about 99°C, or in embodiments, about 30°C to about 95°C, for a period of about 1 minute to about 10 hours, or in embodiments, about 5 minutes to about 5 hours, to form a crosslinked polyester resin or polyester gel suitable for use as a shell.

[0087] When used, the crosslinking agent may be present in an amount of about 0.001% to about 5% by weight of the resin, and in embodiments, about 0.01% to about 1% by weight of the resin. The amount of CCA can be reduced in the presence of the crosslinking agent or reaction initiator. Fusion

[0088] Following aggregation to a desired particle size and the application of an optional shell, the particles may then be cemented into a desired final shape, which is achieved by heating the mixture to a temperature of, for example, about 45°C to about 100°C, and in embodiments, about 55°C to about 99°C (this temperature may be above the glass transition temperature of the resin used to form the toner particles), and / or reducing the stirring to, for example, about 100 rpm to about 400 rpm, and in embodiments, about 200 rpm to about 300 rpm. The cemented particles can be measured for shape factor or roundness using an analyzer such as a SYSMEX FPIA 2100 until the desired shape is achieved.

[0089] Bonding may be achieved over a period of approximately 0.01 to 9 hours, or in some embodiments, approximately 0.1 to 4 hours. Subsequent processing

[0090] In embodiments, after aggregation and / or bonding, the pH of the mixture can be lowered to about 3.5 to about 6, and in embodiments to about 3.7 to about 5.5, for example, with an acid, in order to further bond the toner aggregates. Suitable acids include, for example, nitric acid, sulfuric acid, hydrochloric acid, citric acid, and / or acetic acid. The amount of acid added may be about 0.1 to about 30 weight percent of the mixture, and in embodiments to about 1 to about 20 weight percent of the mixture.

[0091] The mixture may be cooled, washed, and dried. Cooling may take place at a temperature of about 20°C to about 40°C, or in embodiments, about 22°C to about 30°C, for about 1 hour to about 8 hours, or in embodiments, about 1.5 hours to about 5 hours.

[0092] In embodiments, cooling of the cemented toner slurry may include rapid cooling by adding a cooling medium such as ice or dry ice and rapidly cooling to a temperature of about 20°C to about 40°C, or in embodiments, about 22°C to about 30°C. Rapid cooling may be feasible for small amounts of toner, for example, less than about 2 liters, or in embodiments, about 0.1 liters to about 1.5 liters. For larger-scale processes, such as those exceeding about 10 liters in size, rapid cooling of the toner mixture may not be feasible or practical, whether by introducing a cooling medium into the toner mixture or by using reactor cooling with a jacket.

[0093] Next, the toner slurry may be washed. The washing may be carried out at a pH of about 7 to about 12, and in embodiments, at a pH of about 9 to about 11. The washing may be carried out at a temperature of about 30°C to about 70°C, and in embodiments, at a temperature of about 40°C to about 67°C. The washing may include filtering and re-slurring the filtration cake containing toner particles in deionized water. The filtration cake may be washed once or more times with deionized water, or the pH of the slurry may be adjusted with acid to a pH of about 4 and washed once with deionized water, followed optionally by one or more more washes with deionized water.

[0094] Drying may be carried out by any method within the scope of intent of those skilled in the art. Any suitable method for drying toner particles may be used, including freeze-drying, spray drying, and instantaneous airflow drying such as Aljet dryers. Drying may be continued until the moisture level of the particles falls below the set target of about 1% by weight, or in embodiments, about 0.7% by weight. additives

[0095] In embodiments, the toner particles may contain the polymer additives of the present disclosure described above, as well as any other additives, if desired or as needed. For example, the toner may contain a positive or negative charge regulator in an amount of about 0.1 to about 10% by weight of the toner, or in embodiments, about 1 to about 3% by weight of the toner. Examples of suitable charge regulators include quaternary ammonium compounds containing alkylpyridinium halides, disulfates, alkylpyridinium compounds, organic sulfates and sulfonates, including those disclosed in U.S. Patent No. 4,298,672, which is incorporated entirely herein by reference, and those disclosed in U.S. Patent No. 4,338,390, which is incorporated entirely herein by reference.

[0096] Furthermore, after formation, the toner particles may be compounded with external additive particles containing flow aid additives, and these additives may be present on the surface of the toner particles. Examples of these additives include metal oxides such as titanium dioxide, silicon dioxide, aluminum oxide, cerium oxide, tin oxide, and mixtures thereof; metal salts and fatty acid metal salts containing colloidal silica and amorphous silica such as AEROSIL®, zinc stearate, calcium stearate, or long-chain alcohols such as UNILIN 700, and mixtures thereof.

[0097] Generally, silica may be applied to the toner surface for toner flow, triboelectric charging enhancement, mixing control, improved development and transfer stability, and higher toner blocking temperature. TiO2 may be applied for improved relative humidity (RH) stability, triboelectric charging control, and improved development and transfer stability. Zinc stearate, calcium stearate, and / or magnesium stearate may be used as external additives to provide lubrication properties, developer conductivity, and triboelectric charging enhancement, thereby enabling higher toner charge and charge stability by increasing the number of contacts between the toner and carrier particles. In embodiments, commercially available zinc stearate known as Zinc Stearate L, available from Ferro Corporation, may be used. External surface additives may be used with or without the coating.

[0098] Each of these external additives may be present in an amount of about 0% to about 3% by weight of the toner, or in embodiments, about 0.25% to about 2.5% by weight of the toner, although the amount of additives may be outside these ranges. In embodiments, the toner may contain, for example, about 0% to about 3% by weight of titania, about 0% to about 3% by weight of silica, and about 0% to about 3% by weight of zinc stearate.

[0099] In embodiments, in addition to the polymer additives of the present disclosure, the toner particles may also contain silica in an amount of about 0.1% to about 5% by weight, and in embodiments, about 0.2% to about 2% by weight, of the toner particles, and titania in an amount of about 0% to about 3% by weight, and in embodiments, about 0.1% to about 1% by weight, of the toner particles. Developer

[0100] The toner particles formed in this way can be incorporated into a developer composition. By mixing the toner particles with carrier particles, a two-component developer composition can be obtained. The toner concentration in the developer may be about 1% by weight to about 25% by weight of the total weight of the developer, and in embodiments, about 2% by weight to about 15% by weight of the total weight of the developer. Career

[0101] Examples of carrier particles that can be used for mixing with toner include particles that can acquire a charge of opposite polarity to that of the toner particles through triboelectric means. Exemplary examples of suitable carrier particles include granular zircon, granular silicon, glass, steel, nickel, ferrite, iron ferrite, and silicon dioxide. Other carriers are disclosed in U.S. Patents No. 3,847,604, No. 4,937,166, and No. 4,935,326.

[0102] In embodiments, a suitable carrier may include a steel core, for example, with a diameter of about 25 to about 100 μm, or in embodiments, about 50 to about 75 μm, coated using the processes described in U.S. Patent Nos. 5,236,629 and 5,330,874, with a conductive polymer mixture containing, for example, methyl acrylate and carbon black, in about 0.5% to about 10% by weight, or in embodiments, about 0.7% to about 5% by weight, using a conductive polymer mixture containing, for example, methyl acrylate and carbon black.

[0103] The carrier particles can be mixed with toner particles in various suitable combinations. The concentration may be about 1% to 20% by weight of the toner composition. However, by using different percentages of toner and carrier, a developer composition with desired properties can be obtained. imaging

[0104] Toners can be used in electrostatic copying or electrophotographic processes, including those disclosed in U.S. Patent No. 4,295,990, which is incorporated herein by reference in its entirety. In embodiments, any known type of developing system may be used in developing apparatuses, including, for example, magnetic brush developing, jumping single-component developing, and hybrid scavengeless developing (HSD). These and similar developing systems are within the intent of those skilled in the art.

[0105] Once an image is formed with toner / developer via a preferred developing method such as one of the methods described above, the image can then be transferred to an image-receiving medium such as paper. In some embodiments, toner may be used for development in a developing apparatus that utilizes a fuser roll member.

[0106] The following examples are provided to illustrate embodiments of the present disclosure. These examples are for illustrative purposes only and are not intended to limit the scope of the present disclosure. Unless otherwise stated, proportions and percentages are given by weight. [Examples]

[0107] Preparation of fluorinated latex. All fluorinated organic-added latexes used herein were prepared on a 2L bench scale. Numerous latexes were used in this implementation. All latexes were prepared using the same general process and formulation filler amounts, except for variations in monomer ratios. Details are shown in Table 1 below.

[0108] Comparative Example 1: Synthesis of fluorinated organic-added latex using 0% divinylbenzene (DVB).

[0109] In a 2 L Bucher reactor equipped with a P4 impeller, 6.5 g of 30% solid Calfoam SLS (sodium lauryl sulfate) surfactant was added to 816 g of deionized water (DIW). The reactor was deoxygenated by passing a nitrogen stream through it during the reaction. The reactor was heated to 77°C and the rpm was set to 400. Separately, in a 1 L glass container equipped with two P4 impellers, a monomer emulsion was prepared by mixing 319.5 g of trifluoroethyl methacrylate (TFEMA), 6.5 g of Calfoam SLS surfactant (30% solid), and 416 g of DIW together (at 450 rpm). 37.1 g of the monomer emulsion was taken and pumped into the 2 L reactor at 77°C. A reaction initiator solution prepared from 1.22 g of ammonium persulfate in 34.3 g of DIW was added over 20 minutes after the seed emulsion was added. The remaining monomer emulsion was supplied to the reactor over 120 minutes. When half of the monomer emulsion had been added, the reactor speed was increased to 450 rpm. At the end of the monomer supply, the latex was post-treated at 77°C for 1 hour, followed by heating to 87°C for 2 hours and holding at 87°C for 1 hour to reduce residual monomer at the end of the emulsion polymerization process. As a result, a latex containing 20% ​​solid particles with a particle size of 99 nm was obtained.

[0110] Comparative Example 2: Synthesis of fluorinated organic-added latex with 0% DVB. The same process and formulation as in Comparative Example 1.

[0111] Comparative Example 3: Synthesis of non-fluorinated organically added latex prepared using CHMA and 25% DVB with 0.8% DMAEMA. In a 300 Gal reactor equipped with two P4 impellers and a condenser, 0.942 kg of Calfoam SLS surfactant (30% solid) was added to 444 kg of DIW. The reactor was deoxygenated by passing a nitrogen stream through it during the reaction, and the condenser was also used. The reactor was heated to 77°C and the rpm was set to 59. Separately, in a 100 Gal reactor equipped with one P4 impeller, a monomer emulsion was prepared by mixing 126 kg of CHMA, 42.45 kg of DVB, 1.358 kg of DMAEMA, 5.92 kg of Calfoam SLS surfactant (30% solid) and 221.1 kg of DIW together (at 28 rpm). 0.369 kg of monomer emulsion was taken and pumped into a 300 Gal reactor at 77°C. A reaction initiator solution prepared from 0.645 kg of ammonium persulfate in 7.045 kg of DIW was added over 15 minutes after the seed emulsion was added. The remaining monomer emulsion was supplied to the 300 Gal reactor over 120 minutes. When half of the monomer emulsion had been added, the reactor rpm was increased to 66 rpm. The condenser was turned off at the end of the monomer supply. The latex underwent a post-treatment process at 77°C for 1 hour, followed by heating to 87°C for 2 hours and holding at 87°C for 1 hour to reduce residual monomer at the end of the emulsion polymerization process. Also, during the post-treatment protocol, the pH of the latex was adjusted to ≥6.0 every 30 minutes using a 0.1 wt% NaOH solution. As a result, a latex containing 20% ​​solid particles with a particle size of 98 nm was obtained and filtered through a 25 micrometer filter bag. The latex was spray-dried for 3D powder coating.

[0112] Example 2: Synthesis of fluorinated organic-added latex using DVB. This is the same as Comparative Example 1 above, except that 20% DVB and 80% TFEMA were used.

[0113] Example 3: Synthesis of fluorinated organic-added latex using DVB. This is the same as Comparative Example 1 above, except that 30% DVB and 70% TFEMA were used.

[0114] Example 4: Synthesis of fluorinated organic-added latex using CHMA and DVB. This is the same as Comparative Example 1 above, except that 30% DVB, 35% TFEMA, and 35% CHMA were used.

[0115] Because DVB contains impurities, in all of the above examples and comparative examples, the actual DVB content is 55% of the amount added to the resin. The table below shows the amount of DVB added to the formulation and the actual DVB content, which is approximately 0.55 times the amount added to the formulation. The majority of the impurities in DVB are ethyl vinylbenzene, which is also incorporated into the copolymer. [Table 1] NA = Not applicable, nd = Not detected Planarization test due to changes in toner additives over time.

[0116] Each additive was individually compounded in a laboratory-grade SKM mill at a 20% SAC (Surface Area Coverage) in cyan ecotoner, the base material for the Xerox 700 Digital Color Press. Table 2 shows the weight percentage of the fill amount corresponding to 20% SAC. [Table 2]

[0117] For each toner, 30 g of Xerox 700 Digital Color Press carrier was used together with 1.50 g of formulated toner in a 60 mL glass vial. This resulted in a toner concentration of 5%, i.e., TC. The samples were prepared in the J zone at 21.1°C and 10% RH, then mixed on a Turbula mixer for a total of 2 hours, and samples for SEM were taken at 15 minutes, 30 minutes, 1 hour, and 2 hours. SEM images were examined, and failure was judged if the organic polymer additive had flattened and was no longer spherical. The survival time was then defined as the longest time the particles remained spherical. Therefore, if the particles flattened at 2 hours, the survival time was 1 hour. As shown in Table 3, the survival time increased up to the addition of 30% DVB. Since the maximum time the toner was expected to remain in the xerography developing housing was 120 minutes, the test was not continued beyond 120 minutes. For use as a toner additive, approximately 20% by weight of DVB at 55% purity, or 11% by weight of DVB, is required to make the fluorinated polymer additive sufficiently robust for xerography applications. For best performance, approximately 30% by weight of DVB at 55% purity, or 16.5% by weight of DVB, may be required. [Table 3] Electrostatic charge test with a single additive.

[0118] As described above, toners were formulated, using 100% SAC of each additive in the formulation. In this case, the toner surface is completely coated with the additives, so the toner's performance depends on the surface additives. In this way, a direct comparison of the relative performance of each additive was obtained. The electrostatic properties, blocking, and cohesiveness of each toner were evaluated and are shown in Table 4.

[0119] RX50 is a typical medium-particle silica toner additive included herein for reference. In the J zone, the charge is very good negative, but the RH sensitivity is very high. The ratio of the A zone is only 0.35 of the J zone value, so the A zone retains only 35% of the J zone's charge. Thus, silica alone is an unacceptable additive, although it exhibits good flowability and provides very good blocking initiation, with very good low cohesive force.

[0120] The non-fluorinated additive in Comparative Example 3, which is CHMA / 25%DVB / 0.8%DMAEMA, is a positively charged additive. The charge is very similar in both zones and shows better RH sensitivity. The RH ratio is quite similar due to the very low values. The fluid cohesive force of this additive is not good due to its size, as larger additives have worse fluidity than smaller primary additives. Blocking is also very good.

[0121] The TFEMA polymer organic additive is very highly negatively charged, nearly twice the J-zone charge of silica and nearly four times the A-zone charge. Despite the extremely high negative charge, the RH ratio is very good, maintaining 75% of the charge from the J-zone to the A-zone. Furthermore, despite its large size, the fluidity is actually slightly better than RX50, and blocking is also considerably improved. [Table 4]

[0122] The TFEMA polymer additive alone in Example 3 is clearly more negatively charged than silica, and more negatively charged than those typically used in electrophotographic printers, and there are many ways to use this additive to provide a lower charge.

[0123] For example, fluorinated polymer additives can be used in smaller SACs, resulting in a reduction in charge.

[0124] As mentioned above, by utilizing copolymers of TFEMA and non-fluorinated polymer additives such as CHMA, it is possible to adjust the charge to any desired level between, for example, the very negative charge of TFEMA and the slightly positive charge of CHMA. This charge can also replace silica with better RH sensitivity when charged, or directly replace silica / titania combinations with better RH sensitivity and lower charge.

[0125] As another option that provides a charge similar to RX50 silica, a charge between these two additives can be obtained by mixing a smaller SAC fluorinated additive with a smaller SAC non-fluorinated CHMA additive, with a total filling volume of 60% to approximately 130%.

[0126] Alternatively, the fluorinated polymer additive may be mixed with positive silica, such as H2O50.

[0127] Fluorinated polymer additives may be mixed with alumina additives, which are highly effective in reducing electric charge.

[0128] In addition, U.S. Patent No. 8,663,886 states that it is possible to reduce the charge of polymer additives such as DMAEMA used with CHMA by adding positively charged monomers such as amines.

[0129] It will be understood that variations of the above-disclosed features and functions, or substitutes thereof, may be combined into other different systems or applications. Various substitutes, modifications, variations, or improvements not currently anticipated or anticipated may be subsequently made by those skilled in the art, and these are also covered by the following claims.

Claims

1. 1. A toner composition comprising: emulsion aggregation toner particles comprising at least one amorphous polyester resin and one crystalline polyester resin; a surfactant; an optional colorant; an optional wax; and a polymeric toner additive on at least a portion of an exterior surface of said emulsion aggregation toner particles, said polymeric toner additive comprising: A toner composition comprising: a polymer resin comprising a fluorinated acrylic monomer; 8% to 40% by weight of said polymer resin of a crosslinking monomer containing two or more vinyl groups; and 0.1% to 1.5% by weight of said polymer resin of a charge control agent monomer comprising a nitrogen-containing group.

2. The toner composition of claim 1 , wherein the fluorinated acrylic monomer comprises a fluorinated acrylate monomer or a fluorinated methacrylate monomer.

3. 2. The toner composition of claim 1, wherein the charge control agent monomer comprises an acrylate monomer or a methacrylate monomer.

4. The toner composition of claim 1 , wherein the polymeric resin further comprises a non-fluorinated hydrophobic monomer.

5. The toner composition of claim 1 , wherein the polymeric resin further comprises cyclohexyl methacrylate.

6. The toner composition of claim 1 , wherein the crosslinking monomer comprises divinylbenzene.

7. 10. The toner composition of claim 1, further comprising at least one additive selected from the group of silica, titania, alumina, and crosslinked non-fluorinated organic surface additives.

8. 10. The toner composition of claim 1, wherein said emulsion aggregation toner particles comprise a size of from about 4 micrometers to about 10 micrometers.

9. 10. The toner composition of claim 1, further comprising a cleaning additive selected from the group consisting of stearates, cerium oxide, and strontium titanate.

10. 2. The toner composition of claim 1, wherein said polymeric additive comprises from 0.1 weight percent to 5 weight percent of said toner composition.

11. 10. The toner composition of claim 1, wherein the polymer additive comprises a size between 25 nanometers and 250 nanometers.

12. 1. A developer comprising: a toner composition; a toner carrier; said toner composition comprising emulsion aggregation toner particles comprising at least one amorphous polyester resin and one crystalline polyester resin; a surfactant; an optional colorant; an optional wax; and a polymeric toner additive on at least a portion of an outer surface of said toner particles, said polymeric toner additive comprising:

1. A developer comprising: a polymer resin comprising a fluorinated acrylic monomer; 8% to 40% by weight of said polymer resin of a crosslinking monomer containing two or more vinyl groups; and 0.1% to 1.5% by weight of said polymer resin of a charge control agent monomer comprising a nitrogen-containing group.

13. The developer of claim 12 , wherein the fluorinated acrylic monomer comprises a fluorinated acrylate monomer or a fluorinated methacrylate monomer.

14. The developer of claim 12 , wherein the charge control agent monomer comprises an acrylate monomer or a methacrylate monomer.

15. The developer of claim 12 , wherein the polymeric resin further comprises a non-fluorinated hydrophobic monomer.

16. The developer of claim 12 , wherein the polymer resin further comprises cyclohexyl methacrylate.

17. The developer of claim 12 , wherein the crosslinking monomer comprises divinylbenzene.

18. 13. The developer of claim 12 further comprising an additive selected from the group of silica, titania, alumina, and bridged non-fluorinated organic surface additives.

19. A toner composition comprising emulsion aggregation toner particles comprising at least one amorphous polyester resin and one crystalline polyester resin; a surfactant; and 1. A toner composition comprising: a polymer resin comprising a fluorinated acrylic monomer, the polymer resin comprising from 8% to 40% by weight of said polymer resin of a crosslinking monomer containing two or more vinyl groups; and from 0.1% to 1.5% by weight of said polymer resin of a charge control agent monomer having a nitrogen-containing group.

20. 2. The toner composition of claim 1, wherein said emulsion-polymerized polymer resin comprises a size range of 25 nanometers to 250 nanometers.