Toner compositions and additives
Patent Information
- Application Number
- JP2021176078
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-02
- Filing Date
- 2021-10-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Toner compositions are sensitive to environmental conditions such as humidity, leading to issues like excessive background in images due to charge instability, especially in extreme weather conditions.
Incorporation of polymeric toner additives comprising a fluorinated monomer with less than 10% crosslinking and optionally 0.1% to 1.5% nitrogen-containing groups, which are applied to the toner surface to enhance charge stability and humidity sensitivity.
The polymeric additives improve charge stability and reduce image background issues by providing better coverage and embedding on the toner surface, enhancing performance across varying environmental conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure generally relates to toner compositions, and more specifically toner compositions comprising polymer additives. [Background technology]
[0002] Electrophotographic printing utilizes toner particles that can be produced by various processes. One such process involves an emulsion aggregation ("EA") process in which a surfactant is used to form a latex emulsion that forms toner particles. For example, see U.S. Patent No. 6,120,967, the disclosure of which is incorporated herein by reference in its entirety.
[0003] A combination of amorphous and crystalline polyesters can be used in the EA process. This resin combination can provide high gloss and relatively low melting point characteristics (sometimes called low melting, ultra-low melting, or ULM), enabling higher energy efficiency and faster printing. The use of additives containing EA toner particles may be important for achieving optimal toner performance, especially in the charged region. [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] One potential problem with toner is its sensitivity to environmental conditions, including humidity. For example, in summer, high temperatures and humidity can lead to user complaints about the background of images. In winter, cold and dry conditions can result in complaints about overly bright images. In some cases, excessive background blur can occur due to a decrease in the charge level caused by changes in the developer over time.
[0005] There is an ongoing need to improve the additives used in the formation of EA ULM toner. There is also a need to improve the sensitivity of the toner composition to environmental conditions, including relative humidity.
[0006] According to various embodiments, a toner composition is provided, comprising toner particles of at least one resin, an optional colorant, an optional wax, and a polymer toner additive on at least a portion of the outer surface of the toner particles. The polymer toner additive comprises a polymer resin containing a fluorinated monomer, wherein the polymer resin is crosslinked by less than 10% by weight, and an optionally nitrogen-containing charge control agent in an amount of 0.1% to 1.5% by weight of the polymer resin.
[0007] Developers comprising toner compositions and toner carriers are provided according to various embodiments. The toner composition comprises toner particles comprising at least one resin, an optional colorant, an optional wax, and a polymer toner additive on at least a portion of the outer surface of the toner particles. The polymer toner additive comprises a polymer resin comprising a fluorinated monomer, wherein the polymer resin is crosslinked by less than 10% by weight, and an optionally nitrogen-containing charge control agent in an amount of 0.1% to 1.5% by weight of the polymer resin.
[0008] This specification discloses toner additives comprising a polymer resin. The polymer resin comprises less than 10% by weight of a crosslinked fluorinated monomer and optionally 0.1% to 1.5% by weight of a charge control agent containing nitrogen groups of the polymer resin. [Brief explanation of the drawing]
[0009] The accompanying drawings incorporated herein and constituting part of this specification illustrate several embodiments of this teaching and, together with the descriptions, serve to illustrate the principles of this teaching.
[0010] [Figure 1] Figure 1 shows the charge of a single additive formulated on the surface of the toner at a surface area coverage (SAC) of 17% according to various embodiments disclosed herein.
[0011] [Figure 2]Figure 2 shows DVB 0% TFEMA latex on cyan parent toner after 15 minutes of developer aging according to various embodiments disclosed herein.
[0012] [Figure 3] Figure 3 shows Comparative Example 3, which uses a cross-linked TFEMA latex with 30% DVB on a cyan parent toner after 120 minutes of developer aging.
[0013] Please note that some details in these figures have been simplified, and strict structural accuracy, detail, and scale are not maintained; they are drawn to facilitate understanding of the embodiments. [Modes for carrying out the invention]
[0014] This disclosure provides polymer additives for use with toner particles.
[0015] The resulting polymer may be used as an additive to the toner composition, thereby increasing the sensitivity of the resulting toner to relative humidity and charge stability. The polymer additives herein can be used at lower densities compared to other additives, and require far less material by weight to cover a comparable surface area compared to inorganic additives containing oxides such as titania and silica. The polymer additives herein can also provide toner particles with a wide range of properties, such as hydrophobicity and charge controllability, depending on the monomer used to form the polymer.
[0016] In one embodiment, the toner additive is a non-crosslinked emulsion polymerized organic polymer latex-based toner additive containing a fluorinated monomer. This non-crosslinked polymer additive can be added to other toner surface additives and compounded onto the toner surface, where the additive is planarized and embedded in the toner surface. The resulting toner may provide better blocking than the case without the non-crosslinked fluorinated polymer. One embodiment is a poly(trifluoroethyl methacrylate) polymer.
[0017] Suitable fluorinated monomers that can be used to form polymer additives include, for example, 2,4,6-fluorophenyl acrylate, pentafluorophenyl acrylate, hexafluoroisopropyl methacrylate, 1H,1H,3H-hexafluorobutyl methacrylate, 2,2,2-trifluoroethyl acrylate, 2,2,2-trifluoroethyl methacrylate, 1H,1H,2H,2H-heptadecafluorodecyl methacrylate (HDFDMA), 1H,1H,5H-octafluoropentyl methacrylate, and 2,2 ,3,3,4,4,5,5,6,6,7,7-Dodecafluoroheptyl acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,12-Heneicosafluorododecyl acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,10-Heptadecafluorodecyl methacrylate, 2,2,3,3,4,4,4-Heptafluorobutyl acrylate, 2,2,3,3,4,4,4-Heptafluorobutyl methacrylate, 2,2,3,4,4,4-Hexafluorobutyl methacrylate Safluorobutyl acrylate, 2,2,3,4,4,4-Hexafluorobutyl methacrylate, 1,1,1,3,3,3-Hexafluoroisopropyl acrylate, 1,1,1,3,3,3-Hexafluoroisopropyl methacrylate, 2,2,3,3,4,4,5,5-Octafluoropentyl methacrylate, 2,2,3,3,3-Pentafluoropropyl acrylate, 2,2,3,3,3-Pentafluoropropyl methacrylate, 1H,1H,2H,2H-Perfluorodecyl acrylate, 2,2,3,3-Tetra Examples include fluoropropyl methacrylate, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl methacrylate, 2,2,2-trifluoroethyl methacrylate, 2-[(1',1',1'-trifluoro-2'-(trifluoromethyl)-2'-hydroxy)propyl]-3-norbornyl methacrylate, perfluorocyclohexyl (meth)acrylate, and any combination thereof. In embodiments, the crosslinking agent may be fluorinated.Suitable fluorinated crosslinking agents include fluorinated divinyl crosslinking agents such as 1,8-divinylperfluoro(octane), 1,6-divinylperfluoro(hexane), and 1,4-divinylperfluoro(butane) and perfluorocyclohexyl (meth)acrylate.
[0018] The polymer additive is not crosslinked.
[0019] The fluorinated acrylic monomer may be present in the polymer additive in an amount of about 5 wt% to about 90 wt% of the polymer additive, in embodiments about 20 wt% to about 92 wt% of the polymer additive.
[0020] In embodiments, charge control agent monomers include, but are not limited to, nitrogen-containing groups such as dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, dipropylaminoethyl methacrylate, diisopropylaminoethyl methacrylate, dibutylaminoethyl methacrylate, and combinations thereof.
[0021] The charge control agent monomer contains 0.1 wt% to 1.5 wt%, about 0.6 wt% to 1.2 wt%, or about 0.7 wt% to about 1.1 wt% nitrogen-containing groups in the polymer additive.
[0022] In embodiments, methods of forming the polymer additive include emulsion polymerization of monomers utilized to form the polymer additive.
[0023] In the polymerization process, the reactants may be added to a suitable reactor such as a mixing vessel. An appropriate amount of starting materials may optionally be dissolved in a solvent, an optional initiator added to the solution, and contacted with at least one surfactant to form an emulsion. The polymer additive may be formed in the emulsion, which may then be recovered and used as the polymer additive for the toner composition.
[0024] Suitable solvents for use include, but are not limited to, water and / or organic solvents, such as toluene, benzene, xylene, tetrahydrofuran, acetone, acetonitrile, carbon tetrachloride, chlorobenzene, cyclohexane, diethyl ether, dimethyl ether, dimethylformamide, heptane, hexane, methylene chloride, pentane, and combinations thereof.
[0025] In embodiments, the latex for forming the polymer additive may be optionally prepared under an inert gas such as nitrogen in an aqueous phase containing a surfactant or co-surfactant. The surfactant may be used together with the resin to form the latex dispersion and may be an ionic or nonionic surfactant in an amount of about 0.01 to about 15 weight percent of the solid, and in embodiments, about 0.1 to about 10 weight percent of the solid.
[0026] Examples of anionic surfactants that can be used include sulfates and sulfonates, sodium dodecyl sulfate (SDS) known as sodium lauryl sulfate (SLS), sodium dodecylbenzenesulfonate, sodium dodecylnaphthalene sulfate, dialkylbenzenealkyl sulfates and sulfonates, acids such as abietic acid available from Aldrich, Neogen® and Neogen SC from Daiichi Kogyo Seiyaku Co., Ltd., and combinations thereof. Other suitable anionic surfactants, in embodiments, include DOWFAX® 2A1, alkyldiphenyl oxide disulfonate from Dow Chemical Company, and / or Teika Power BN2060 from Teika Co., Ltd. (Japan), which are branched sodium dodecylbenzenesulfonate. Combinations of these surfactants with any of the aforementioned anionic surfactants may be used in embodiments.
[0027] Examples of cationic surfactants, though not limited to them, include ammonium, such as alkylbenzyldimethylammonium chloride, dialkylbenzenealkylammonium chloride, lauryltrimethylammonium chloride, alkylbenzylmethylammonium chloride, alkylbenzyldimethylammonium bromide, benzalkonium chloride, C 12 ,C 15 ,C 17 Examples include trimethylammonium bromide and combinations thereof. Other cationic surfactants include cetylpyridinium bromide, quaternary polyoxyethylalkylamine halogen salts, dodecylbenzyltriethylammonium chloride, MIRAPOL and ALKAQUAT available from Alkaril Chemical Company, sanisol (benzalkonium chloride) available from Kao Chemicals, and combinations thereof. In embodiments, a preferred cationic surfactant is SANISOL B-50 available from Kao Corp., which is mainly benzyldimethylalkonium chloride.
[0028] Examples of nonionic surfactants include, but are not limited to, alcohols, acids, and ethers, such as polyvinyl alcohol, polyacrylic acid, metalrose, methylcellulose, ethylcellulose, propylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, and combinations thereof. In the embodiments, commercially available surfactants from Rhone-Poulenc, such as IGEPAL CA-210(trademark), IGEPAL CA-520(trademark), IGEPAL CA-720(trademark), IGEPAL CO-890(trademark), IGEPAL CO-720(trademark), IGEPAL CO-290(trademark), IGEPAL CA-210(trademark), ANTAROX 890(trademark), and ANTAROX 897(trademark), can be used.
[0029] The selection of specific surfactants or combinations thereof, as well as the respective amounts used, are within the scope of knowledge of those skilled in the art.
[0030] In embodiments, reaction initiators may be added to form latex used in the formation of polymer additives. Examples of suitable reaction initiators include water-soluble reaction initiators, such as ammonium persulfate, sodium persulfate and potassium persulfate, and organic solvent-soluble reaction initiators, such as organic peroxides, and azo compounds, such as VAZO 64®, 2-methyl-2-2'-azobispropannitrile, VAZO 88®, 2-2'-azobisisobutylamide anhydride, and combinations thereof. Other water-soluble initiators that can be used include azoamidine compounds, such as 2,2'-azobis(2-methyl-N-phenylpropionamidine)dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine]tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine]dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine]dihydrochloride, and 2,2'-azobis[N-(2-hydroxy-ethyl)-2-methylpropionamidine]dihydrochloride. [Amidine]dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepine-2-yl)propane]dihydrochloride, 2,2'-azobis[2- Examples include (3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, and combinations thereof.
[0031] The reaction initiator can be added in a suitable amount, for example, about 0.1 to about 8 weight percent of the monomer, and in embodiments, about 0.2 to about 5 weight percent.
[0032] When forming the emulsion, starting materials, surfactants, optionally solvents, and optionally initiators can be combined using any means within the understanding of those skilled in the art. In embodiments, the reaction mixture may be mixed for about 1 minute to about 72 hours, or in specific embodiments about 4 hours to about 24 hours, while maintaining the temperature at about 10°C to about 100°C, about 20°C to about 90°C in certain embodiments, and about 45°C to about 75°C in other specific embodiments.
[0033] Those skilled in the art will understand that by optimizing the reaction conditions, temperature, and initiator load, polymers of various molecular weights can be produced, and that structurally related starting materials can be polymerized using equivalent techniques.
[0034] The average particle size of polymer nanoparticles was measured by dynamic light scattering using a Nanotrac252 instrument (Microtrac, Inc.).
[0035] In this specification, the term “average particle size” refers to the diameter value of particles that constitute 50% (by volume unless otherwise specified) of the sample, in which case the diameter is less than that value. The average particle size may also be referred to as “D50”.
[0036] The particle size of latex particles ranging from 0.0008 to 6.54 micrometers is measured using the Nanotrac 252 instrument. This instrument employs laser light scattering techniques to measure the Doppler shift light generated from each particle during its motion (Brownian motion). The signals generated by these shifts are proportional to the particle size. The signals are mathematically converted into particle size and particle size distribution. The analysis can be performed using an external probe or by inserting the probe into a fixed sample chamber.
[0037] For light scattering techniques, NIST polystyrene nanosphere control samples with diameters in the range of 15 nm to 150 nm can be used under the trademark name NIST Traceable Reference Material for Nanotrac Particle Size Analyzers, obtained from Microtrac.
[0038] The resulting latex has the polymer additives of the present disclosure and can be applied to toner particles by any means within the intent of those skilled in the art. In embodiments, toner particles may be immersed in or sprayed with the latex containing the polymer additives, and thus coated, and the coated particles can then be dried to leave the polymer coating on top.
[0039] In other embodiments, once the polymer additive for the toner is formed, it can be recovered from the latex by any technique within the scope of the intent of those skilled in the art, including filtration, drying, centrifugation, spray drying, and combinations thereof.
[0040] In embodiments, the polymer additive, once obtained and used as a toner additive, can be dried into a powder form by any method within the intent of those skilled in the art, including, for example, freeze-drying, optionally spray-drying in a vacuum, or a combination thereof. The dried polymer additive of the present disclosure can then be applied to toner particles by any means within the intent of those skilled in the art, including, but not limited to, mechanical impact and / or electrostatic attraction. An example of a mechanical mixing apparatus is the Henschel FM high-strength mixer from Zeppelin Systems, but other mixing apparatuses may also be used in embodiments.
[0041] The polymer additive particles may have an average or medium particle size (D50) of approximately 20 nanometers to 250 nanometers in diameter, and in embodiments, approximately 40 nanometers to 150 nanometers in diameter.
[0042] In the embodiment, the polymer additive used as a polymer additive soluble in a solvent such as tetrahydrofuran (THF) has a number average molecular weight (M) measured by gel permeation chromatography (GPC) using a polystyrene standard, for example, about 40,000 to about 280,000 daltons, and in the embodiment, about 60,000 to about 170,000 daltons. n ), and when measured by gel transmission chromatography, for example, a weight-average molecular weight (M) of about 200,000 to about 800,000 daltons, and in embodiments, about 400,000 to about 600,000 daltons. w ) may have. In the embodiment, the solubility of the crosslinked resin is limited by crosslinking, so it may be impossible to measure the molecular weight by any method.
[0043] The polymer or polymer additive used as a polymer additive may have a glass transition temperature (Tg) of about 85°C to about 140°C, and in embodiments, about 100°C to about 130°C. In embodiments, it may be impossible to determine the Tg due to crosslinking of the resin, which may make detection of the Tg difficult. In embodiments, the A-zone charge of the toner containing the polymer additive of the present disclosure may be about -15 to about -80 microcoulombs per gram, and in embodiments, about -20 to about -60 microcoulombs per gram, while the C-zone charge of the toner containing the polymer additive of the present disclosure may be about -15 to about -80 microcoulombs per gram, and in embodiments, about -20 to about -60 microcoulombs per gram.
[0044] The polymer additives of this disclosure may be combined with toner particles in an amount of about 0.1% by weight to about 5% by weight of the toner particles, and in embodiments, about 0.2% by weight to about 2% by weight of the toner particles.
[0045] Therefore, the polymer additive compositions and processes of this disclosure allow for the formulation of developers having selected high triboelectric charging properties and / or conductivity values by utilizing several different combinations. toner
[0046] The polymer additive thus produced may then be optionally combined with a toner resin having a colorant to form the toner of the present disclosure. resin
[0047] Any toner resin can be used when forming the toner of the present disclosure. Such a resin may then be prepared by any suitable monomer or any suitable polymerization method with any suitable monomer. In embodiments, the resin may be prepared by a method other than emulsion polymerization. In further embodiments, the resin may be prepared by condensation polymerization.
[0048] The toner compositions of this disclosure, in embodiments, include an amorphous resin. The amorphous resin may be linear or branched. In embodiments, the amorphous resin may include at least one low molecular weight amorphous polyester resin. Low molecular weight amorphous polyester resins, available from numerous sources, may have a variety of glass transition temperatures, for example, about 30°C to about 80°C, and in embodiments about 35°C to about 75°C. When used herein, the low molecular weight amorphous polyester resin has a number average molecular weight (M) of, for example, about 1,000 to about 10,000, in embodiments about 2,000 to about 8,000, in embodiments about 3,000 to about 7,000, and in embodiments about 4,000 to about 6,000, as measured by gel permeation chromatography (GPC). n ) has. The weight-average molecular weight (M) of the resin. w The molecular weight distribution (M) of low molecular weight amorphous resins is less than or equal to 50,000 when determined by GPC using polystyrene standards, for example, in embodiments, about 2,000 to about 50,000, in embodiments, about 3,000 to about 40,000, in embodiments, about 10,000 to about 30,000, and in embodiments, about 18,000 to about 21,000. w / Mn ) is, for example, from about 2 to about 6, and in an embodiment from about 3 to about 4. The low molecular weight amorphous polyester resin may have an acid value of from about 8 to about 20 mg KOH / g, in an embodiment from about 9 to about 16 mg KOH / g, and in an embodiment from about 10 to about 14 mg KOH / g.
[0049] Examples of linear amorphous polyester resins that can be utilized include poly(propoxylated bisphenol A cofumarate), poly(ethoxylated bisphenol A cofumarate), poly(butyloxylated bisphenol A cofumarate), poly(copropoxylated bisphenol A coethoxylated bisphenol A cofumarate), poly(1,2-propylene fumarate), poly(propoxylated bisphenol A comalate), poly(ethoxylated bisphenol A comalate), poly(butyloxylated bisphenol A comalate), poly(copropoxylated bisphenol A coethoxylated bisphenol A comalate), poly(1,2-propylene maleate), poly(propoxylated bisphenol A coitaconate), poly(ethoxylated bisphenol A coitaconate), poly(butylenated bisphenol A coitaconate), poly(copropoxylated bisphenol A coethoxylated bisphenol A coitaconate), poly(1,2-propylene itaconate), and combinations thereof.
[0050] In an embodiment, suitable amorphous resins can include alkoxylated bisphenol A fumarate / terephthalate-based polyester and copolyester resins. In an embodiment, a suitable amorphous polyester resin can be a copoly(propoxylated bisphenol A cofumarate)-copoly(propoxylated bisphenol A coterephthalate) resin having the following formula (I),
Chemical formula
[0051] In embodiments, the low molecular weight amorphous polyester resin may be a saturated or unsaturated amorphous polyester resin. Exemplary examples of saturated and unsaturated amorphous polyester resins selected for the processes and particles of this disclosure include: polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polypentylene terephthalate, polyhexylene terephthalate, polyheptadene terephthalate, polyoctalene terephthalate, polyethylene isophthalate, polypropylene isophthalate, polybutylene isophthalate, polypentylene isophthalate, and polyhexylene isophthalate. Polyheptadene-isophthalate, polyoctalene-isophthalate, polyethylene-sebacate, polypropylene-sebacate, polybutylene-sebacate, polyethylene-aziperte, polypropylene-aziperte, polybutylene-aziperte, polypentylene-aziperte, polyhexylene-aziperte, polyheptadene-aziperte, polyoctalene-aziperte, polyethylene-glutarate, polypropylene-glutarate, polybutylene-glutarate, polypentylene-glutarate, polyhexylene- Glutarate, polyheptadene-glutarate, polyoctalene-glutarate, polyethylene-pimelate, polypropylene-pimelate, polybutylene-pimelate, polypentylene-pimelate, polyhexylene-pimelate, polyheptadene-pimelate, poly(ethoxylated bisphenol A-fumarate), poly(ethoxylated bisphenol A-succinate), poly(ethoxylated bisphenol A-azipart), poly(ethoxylated bisphenol A-glutarate), poly(ethoxylated bisphenol A-fumarate), Poly(ethoxylated bisphenol A-terephthalate), poly(ethoxylated bisphenol A-isophthalate), poly(ethoxylated bisphenol A-dodecenyl succinate), poly(propoxylated bisphenol A-fumarate), poly(propoxylated bisphenol A-succinate), poly(propoxylated bisphenol A-aziperte), poly(propoxylated bisphenol A-glutarate), poly(propoxylated bisphenol A-terephthalate), poly(propoxylated bisphenol A-isophthalate),Examples of various amorphous polyesters include poly(propoxylated bisphenol A-dodecenyl succinate), SPAR (Dixie Chemicals), BECKOSOL (Reichhold Inc.), ARAKOTE (Ciba-Geigy Corporation), HETRON (Ashland Chemical), PARAPLEX (Rohm & Haas), POLYLITE (Reichhold Inc.), PLASTHALL (Rohm & Haas), CYGAL (American Cyanamide), ARMCO (Armco Composites), ARPOL (Ashland Chemical), CELANEX (Celanese Eng), RYNITE (DuPont), STYPOL (Freeman Chemical Corporation), and combinations thereof. The resins may also be functionalized, such as carboxylation, sulfonation, or, if particularly desired, sodium sulfonation.
[0052] Examples of polycondensation catalysts suitable for any low molecular weight amorphous polyester resin include tetraalkyl titanates, dialkyltin oxides such as dibutyltin oxide, tetraalkyltins such as dibutyltin dilaurate, dialkyltin oxide hydroxides such as butyltin oxide hydroxide, aluminum alkoxides, alkylzincs, dialkylzincs, zinc oxide, stannous oxide, or mixtures thereof. This catalyst can be used in amounts of, for example, about 0.01 mol% to about 5 mol%, based on the diacid or diester used as the starting material for producing the polyester resin.
[0053] Low molecular weight amorphous polyester resins may also be branched resins. As used herein, the terms "branched" or "branched" include branched resins and / or crosslinked resins.
[0054] The resulting unsaturated polyester is reactive (e.g., crosslinkable) in two leading parts: (i) unsaturated sites (double bonds) along the polyester chain, and (ii) functional groups suitable for acid-base reactions, such as carboxyl groups and hydroxyl groups. In embodiments, the unsaturated polyester resin is prepared by melt polycondensation or other polymerization processes using diacids and / or anhydrides and diols.
[0055] In embodiments, the low molecular weight amorphous polyester resin or combination of low molecular weight amorphous resins may have a glass transition temperature of about 30°C to about 80°C, and in embodiments, about 35°C to about 70°C. In further embodiments, the combined amorphous resins have a glass transition temperature of about 10 to about 1,000,000 Pa at about 130°C. * S, in the embodiment, approximately 50 to approximately 100,000 Pa * It may have a melting viscosity of S.
[0056] The amount of low molecular weight amorphous polyester resin in the toner particles of the present disclosure may be present in any core, any shell, or both in amounts of 25 to about 50% by weight, in embodiments about 30 to about 45% by weight, and in embodiments about 35 to about 43% by weight of toner particles (i.e., toner particles excluding external additives and water).
[0057] In embodiments, the toner composition comprises at least one crystalline resin. As used herein, “crystalline” refers to polyester having a three-dimensional order. As used herein, “semi-crystalline resin” refers to a resin having a crystallinity of, for example, about 10 to about 90%, and in embodiments, about 12 to about 70%. Furthermore, as used below, “crystalline polyester resin” and “crystalline resin” encompass both crystalline and semi-crystalline resins unless otherwise specified.
[0058] In this embodiment, the crystalline polyester resin is either a saturated crystalline polyester resin or an unsaturated crystalline polyester resin.
[0059] Crystalline polyester resins, available from many sources, can have a variety of melting points, for example, from about 30°C to about 120°C, and in embodiments, from about 50°C to about 90°C. When measured, for example, by gel permeation chromatography (GPC), the number average molecular weight (M) of the crystalline resin is, for example, from about 1,000 to about 50,000, in embodiments, from about 2,000 to about 25,000, in embodiments, from about 3,000 to about 15,000, and in embodiments, from about 6,000 to about 12,000. n ) may have. Molecular weight distribution of crystalline resin (M w / M n The acid value is, for example, about 2 to about 6, and in embodiments, about 3 to about 4. The crystalline polyester resin may have an acid value of about 2 to about 20 mg KOH / g, in embodiments, about 5 to about 15 mg KOH / g, and in embodiments, about 8 to about 13 mg KOH / g.
[0060] Examples of crystalline polyester resins include poly(ethylene-adipate), poly(propylene-adipate), poly(butylene-adipate), poly(pentylene-adipate), poly(hexylene-adipate), poly(octylene-adipate), poly(ethylene-succinate), poly(propylene-succinate), poly(butylene-succinate), poly(pentylene-succinate), poly(hexylene-succinate), poly(octylene-succinate), poly(ethylene-sevacate), and poly(propylene-sevacate). Poly(butylene-sebacate), Poly(pentylene-sebacate), Poly(hexylene-sebacate), Poly(octylene-sebacate), Poly(nonylene-sebacate), Poly(decylene-sebacate), Poly(undecylene-sebacate), Poly(dodecylene-sebacate), Poly(ethylene-dodecanediote), Poly(propylene-dodecanediote), Poly(butylene-dodecanediote), Poly(pentylene-dodecanediote), Poly(hexylene-dodecanediote), Poly(octylene-dodecanediote) Poly(nonylene-dodecanediote), poly(decylene-dodecanediote), poly(undecylene-dodecanediote), poly(dodecylene-dodecanediote), poly(ethylene-fumarate), poly(propylene-fumarate), poly(butylene-fumarate), poly(pentylene-fumarate), poly(hexylene-fumarate), poly(octylene-fumarate), poly(nonylene-fumarate), poly(decylene-fumarate), copoli(5-sulfoisophthaloyl)-copoly(ethylene-aziparte), copoli( 5-Sulfoisophthaloyl)-copoly(propylene-adipate), copoly(5-sulfoisophthaloyl)-copoly(butylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(pentylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(hexylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(octylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(ethylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(propylene-adipate),Copoly(5-sulfo-isophthaloyl)-copoly(butylene-adipate), Copoly(5-sulfo-isophthaloyl)-copoly(pentylene-adipate), Copoly(5-sulfo-isophthaloyl)-copoly(hexylene-adipate), Copoly(5-sulfo-isophthaloyl)-copoly(octylene-adipate), Copoly(5-sulfoisophthaloyl)-copoly(ethylene-succinate), Copoly(5-sulfoisophthaloyl)-copoly( Propylene succinate), copoli(5-sulfoisophthaloyl)-copoly(butylene succinate), copoli(5-sulfoisophthaloyl)-copoly(pentylene succinate), copoli(5-sulfoisophthaloyl)-copoly(hexylene succinate), copoli(5-sulfoisophthaloyl)-copoly(octylene succinate), copoli(5-sulfo-isophthaloyl)-copoly(ethylene sebacate), copoli(5-sulfo (5-isophthaloyl)-copoly(propylene-sebacate), (5-sulfo-isophthaloyl)-copoly(butylene-sebacate), (5-sulfo-isophthaloyl)-copoly(pentylene-sebacate), (5-sulfo-isophthaloyl)-copoly(hexylene-sebacate), (5-sulfo-isophthaloyl)-copoly(octylene-sebacate), (5-sulfo-isophthaloyl) Examples of various crystalline polyesters include -copoly(ethylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(propylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(butylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(pentylene-adipate), copoly(5-sulfo-isophthaloyl)-copoly(hexylene-adipate), and any combination thereof.
[0061] Crystalline resins can be prepared by a polycondensation process involving the reaction of a suitable organic diol with a suitable organic diacid in the presence of a polycondensation catalyst.
[0062] Examples of organic diols selected for the preparation of crystalline polyester resins include aliphatic diols having approximately 2 to 36 carbon atoms.
[0063] Examples of organic diacids or diesters selected for the preparation of crystalline polyester resins include oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, naphthalene-2,7-dicarboxylic acid, cyclohexanedicarboxylic acid, malonic acid and mesaconic acid, their diesters or anhydrides; and alkali sulfo-organic diacids, such as dimethyl-5-sulfo-isophthalate and dialkyl-5-sulfo-isophthalate-4-sulfo-1,8-naphthalic acid. Examples include aqueous solutions, 4-sulfophthalic acid, dimethyl-4-sulfophthalate, dialkyl-4-sulfophthalate, 4-sulfophenyl-3,5-dicarbomethoxybenzene, 6-sulfo-2-naphthyl-3,5-dicarbomethoxybenzene, sulfo-terephthalic acid, dimethyl-sulfo-terephthalate, 5-sulfo-isophthalic acid, dialkyl-sulfo-terephthalate, sulfo-p-hydroxybenzoic acid, sodium, lithium, or potassium salts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, or mixtures thereof. Organic diacids may be selected in amounts of, for example, about 40 to about 50 mole percent of the resin, and alkali sulfoaliphatic diacids may be selected in amounts of about 1 to about 10 mole percent of the resin.
[0064] In the embodiment, the preferred crystalline resin may include a resin made of ethylene glycol or nonanediol, and a mixture of dodecanediic acid and fumaric acid comonomer having the following formula (II): [ka] In the formula, b is approximately 5 to approximately 2000, and d is approximately 5 to approximately 2000.
[0065] When semicrystalline polyester resins are used herein, the semicrystalline resins include poly(3-methyl-1-butene), poly(hexamethylene carbonate), poly(ethylene-p-carboxyphenoxybutyrate), poly(ethylene vinyl acetate), poly(docosyl acrylate), poly(dodecyl acrylate), poly(octadecyl acrylate), poly(octadecyl methacrylate), poly(behenyl polyethoxyethyl methacrylate), poly(ethylene adipate), poly(decamethylene adipate), poly(decamethylene azelaate), poly(hexamethylene oxalate), poly(decamethylene oxalate), poly(ethylene oxide), poly(propylene oxide), poly(butadiene oxide), poly(decamethylene oxide), poly(decamethylene sulfide), poly(decamethylene disulfide), and poly(ethylene seba Poly(decamethylene sebacate), poly(ethylene sverate), poly(decamethylene succinate), poly(eicosamethylene malonate), poly(ethylene-p-carboxyphenoxy undecanoate), poly(ethylenedithion ethophthalate), poly(methylethylene terephthalate), poly(ethylene-p-carboxyphenoxy valerate), poly(hexamethylene-4,4'-oxydibenzoate), poly Possible examples include poly(10-hydroxycapric acid), poly(isophthalaldehyde), poly(octamethylene dodecanediate), poly(dimethylsiloxane), poly(dipropylsiloxane), poly(tetramethylenephenylenediacetate), poly(tetramethylene trithiodicarboxylate), poly(trimethylene dodecanediate), poly(m-xylene), poly(p-xylylenepimeramide), and combinations thereof.
[0066] The amount of crystalline polyester resin in the toner particles of this disclosure may be present in the core, shell, or both in amounts of 1 to about 15% by weight, in embodiments about 5 to about 10% by weight, and in embodiments about 6 to about 8% by weight of toner particles (i.e., toner particles excluding external additives and water).
[0067] In embodiments, the toner of the present disclosure may also contain at least one high molecular weight branched or crosslinked amorphous polyester resin. Examples of such high molecular weight resins in embodiments include branched amorphous resins or amorphous polyesters, crosslinked amorphous resins or amorphous polyesters, or mixtures thereof, or crosslinked non-crosslinked amorphous polyester resins. According to the present disclosure, about 1% to about 100% by weight of the high molecular weight amorphous polyester resin may be branched or crosslinked, and in embodiments, about 2% to about 50% by weight of the high molecular weight amorphous polyester resin may be branched or crosslinked.
[0068] When used herein, high molecular weight amorphous polyester resins have a number average molecular weight (M) of approximately 1,000 to approximately 10,000, as measured by, for example, gel permeation chromatography (GPC). n ) may have. High molecular weight amorphous resins available from numerous sources may have a variety of glass transition onset temperatures (Tg) when measured by differential scanning calorimeter (DSC), for example, about 40°C to about 80°C, in embodiments about 50°C to about 70°C, and in embodiments about 54°C to about 68°C. In embodiments, linear and branched amorphous polyester resins may be saturated or unsaturated resins.
[0069] High molecular weight amorphous polyester resins can be prepared by branching or crosslinking linear polyester resins. Branching agents such as trifunctional or polyfunctional monomers can be used, and these agents typically increase the molecular weight and polydispersity of the polyester. Suitable branching agents include glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, diglycerol, trimellitic acid, trimellitic anhydride, pyromellitic acid, pyromellitic anhydride, 1,2,4-cyclohexanetricarboxylic acid, 2,5,7-naphthalentricarboxylic acid, 1,2,4-butanetricarboxylic acid, and combinations thereof. These branching agents can be used in effective amounts of about 0.1 mol% to about 20 mol%, based on the diacid or diester used as the starting material for the resin.
[0070] In some embodiments, the crosslinked polyester resin may be made from a linear amorphous polyester resin containing unsaturated moieties that can react under free radical conditions. In some embodiments, suitable unsaturated polyester resins can be prepared from diacids and / or anhydrides such as maleic anhydride, terephthalic acid, trimellitic acid, fumaric acid, and combinations thereof, and diols such as bisphenol A ethylene oxide adduct, bisphenol A-propylene oxide adduct, and combinations thereof. In some embodiments, a suitable polyester is poly(propoxylated bisphenol A co-fumaric acid).
[0071] In embodiments, crosslinked branched polyesters may be used as high molecular weight amorphous polyester resins. Examples of such polyesters and methods for synthesizing them are disclosed in U.S. Patent No. 6,592,913, the entire disclosure of which is incorporated herein by reference.
[0072] Suitable polyols contain about 2 to about 100 carbon atoms and may have at least two or more hydroxyl groups, or esters thereof. Examples of polyols include glycerol, pentaerythritol, polyglycol, polyglycerol, or mixtures thereof. The polyol may contain glycerol. Suitable esters of glycerol include glycerol palmitate, glycerol sebacate, glycerol azipart, and triacetin trippropionine. The polyol may be present in an amount of about 20% to about 30% by weight of the reaction mixture, and in embodiments, about 22% to about 26% by weight of the reaction mixture.
[0073] In embodiments, the crosslinked branched polyester of the high molecular weight amorphous polyester resin may include those resulting from the reaction of dimethyl terephthalate, 1,3-butanediol, 1,2-propanediol, and pentaerythritol.
[0074] In embodiments, a high molecular weight resin, such as a branched polyester, may be present on the surface of the toner particles of the present disclosure. The high molecular weight resin on the surface of the toner particles may also be particulate, and may be high molecular weight resin particles having a diameter of about 100 nanometers to about 300 nanometers, and in embodiments, about 110 nanometers to about 150 nanometers.
[0075] The amount of high molecular weight amorphous polyester resin in the toner particles of this disclosure may be about 25% to about 50% by weight of the toner in any core, any shell, or both; in embodiments, about 30% to about 45% by weight; in other embodiments, or about 40% to about 43% by weight of the toner (i.e., toner particles excluding external additives and water).
[0076] The ratio of crystalline resin to low molecular weight amorphous resin to high molecular weight amorphous polyester resin may range from approximately 1:1:98 to approximately 98:1:1 to approximately 1:98:1, approximately 1:5:5 to approximately 1:9:9 in embodiments, and approximately 1:6:6 to approximately 1:8:8 in embodiments. surfactant
[0077] In the embodiment, the resin, wax, and other additives used to form the toner composition may be in a dispersion containing a surfactant. Furthermore, the toner particles may be formed by an emulsion flocculation method, in which the resin and other components of the toner are placed in one or more surfactants to form an emulsion, the toner particles are agglomerated and bonded, and optionally washed, dried, and recovered.
[0078] One, two, or more surfactants may be used. The surfactants may be selected from ionic surfactants and nonionic surfactants. Anionic surfactants and cationic surfactants are included in the term "ionic surfactants". In embodiments, the surfactant may be used in an amount of about 0.01% to about 5% by weight of the toner composition, for example, about 0.75% to about 4% by weight of the toner composition, and in embodiments, about 1% to about 3% by weight of the toner composition.
[0079] Examples of nonionic surfactants that can be used include, for example, polyacrylic acid, metalrose, methylcellulose, ethylcellulose, propylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, and IGEPAL CA-210(trademark), IGEPAL CA-520(trademark), IGEPAL CA-720(trademark), IGEPAL CO-890(trademark), IGEPAL CO-720(trademark), IGEPAL CO-290(trademark), IGEPAL CA-210(trademark), ANTAROX 890(trademark), and ANTAROX 897(trademark), all available from Rhone-Poulenc. Other examples of suitable nonionic surfactants include polyethylene oxide and polypropylene oxide block copolymers, including Synperonic PE / F, which in some embodiments is commercially available as Synperonic PE / F 108.
[0080] The anionic surfactants that can be used include those mentioned above. Examples of cationic surfactants include those mentioned above. Coloring agents
[0081] The latex particles produced as described above can be added to a colorant to produce toner. In embodiments, the colorant may be in the form of a dispersion. The colorant dispersion may contain, for example, submicron colorant particles having a volume average diameter of about 50 to about 500 nanometers, and in embodiments, a volume average diameter of about 100 to about 400 nanometers. The colorant particles may be suspended in an aqueous phase containing an anionic surfactant, a nonionic surfactant, or a combination thereof. Suitable surfactants include any of the surfactants described above. In embodiments, the surfactant may be ionic and may be present in the dispersion in an amount of about 0.1 to about 25% by weight of the colorant, and in embodiments, about 1 to about 15% by weight of the colorant.
[0082] Colorants useful for toner formation according to this disclosure include pigments, dyes, mixtures of pigments and dyes, mixtures of pigments, and mixtures of dyes. The colorants may be, for example, carbon black, cyan, yellow, magenta, red, orange, brown, green, blue, violet, or mixtures thereof.
[0083] In embodiments where the coloring agent is a pigment, the pigment may be, for example, carbon black, phthalocyanine, quinacridone or rhodamine B(trademark), red, green, orange, brown, violet, yellow, a fluorescent coloring agent, or the like.
[0084] If desired, stirring the resulting latex and colorant dispersion in the dispersion and heating it to a temperature of about 35°C to about 70°C, or in embodiments, about 40°C to about 65°C, may yield toner aggregates with a volume average diameter of about 2 micrometers to about 10 micrometers, or in embodiments, about 5 micrometers to about 8 micrometers. wax
[0085] Optionally, wax may also be combined with resin to form toner particles. If included, the wax may be present in an amount of, for example, about 1% to about 25% by weight of the toner particles, and in embodiments, about 5% to about 20% by weight of the toner particles.
[0086] Examples of waxes that can be selected include waxes having a weight-average molecular weight of about 500 to about 20,000, and in embodiments, about 1,000 to about 10,000. Examples of waxes that can be used include polyolefins such as polyethylene, polypropylene, and polybutene wax; plant-based waxes such as carnauba wax, rice wax, candelilla wax, wood wax, and jojoba oil; animal-based waxes such as beeswax; mineral waxes and petroleum-based waxes such as montan wax, ozokerite, ceresin, paraffin wax, microcrystalline wax, and Fischer-Tropsch wax; ester waxes obtained from higher fatty acids and higher alcohols such as stearyl stearate and behenyl behenate; butyl stearate; propyl oleate. Examples include ester waxes obtained from higher fatty acids such as glyceride monostearate, glyceride distearate, and pentaerythritol tetrabehenate and monohydric or polyhydric lower alcohols; ester waxes obtained from higher fatty acids such as diethylene glycol monostearate, dipropylene glycol distearate, diglyceryl distearate, and triglyceryl tetrastearate and polyhydric alcohol multimers; sorbitan higher fatty acid ester waxes such as sorbitan monostearate; and cholesterol higher fatty acid ester waxes such as cholesteryl stearate. Toner preparation
[0087] Toner particles can be prepared by any method within the intent of those skilled in the art. Embodiments relating to the production of toner particles are described below with respect to emulsion agglomeration processes, but any suitable method for preparing toner particles may be used, including chemical processes such as suspension and encapsulation methods, the respective disclosures of which are incorporated herein in their entirety by reference. In embodiments, toner compositions and toner particles may be prepared by agglomeration and bonding processes, in which small-particle resin particles are agglomerated to a suitable toner particle size and then bonded to achieve the final shape and form of toner particles.
[0088] In embodiments, the toner composition may be prepared by an emulsion flocculation process, such as a process comprising flocculating an emulsion containing the resin in the surfactant with a mixture of an optional wax and any other desired or required additive, and then bonding the flocculated mixture. The mixture may also be prepared by adding an optional wax or other material (which may be in a dispersion(or more) containing a surfactant) to an emulsion (which may be a mixture of two or more emulsions containing a resin). The pH of the resulting mixture can be adjusted with an acid, for example, acetic acid or nitric acid. In embodiments, the pH of the mixture can be adjusted to about 2 to about 4.5. In addition, in embodiments, the mixture may be homogenized. If the mixture is homogenized, homogenization may be achieved by mixing at about 600 to about 6,000 revolutions per minute. Homogenization may be achieved by any preferred means, for example, an IKA ULTRA TURRAX T50 probe homogenizer.
[0089] Following the preparation of the above mixture, a flocculant may be added to the mixture. Toner may be formed using any suitable flocculant. Suitable flocculants include, for example, aqueous solutions of divalent or polyvalent cationic materials. The flocculant may be, for example, a polyaluminum halide such as polyaluminum chloride (PAC), or a corresponding bromide, fluoride, or iodide, or an aluminum polysilicate such as polyaluminum sulfosilicate (PASS), and a water-soluble metal salt containing aluminum chloride, aluminum nitrite, aluminum sulfate, aluminum sulfate, calcium chloride, calcium nitrite, calcium oxyate, calcium sulfate, magnesium acetate, magnesium nitrate, magnesium sulfate, zinc acetate, zinc nitrate, zinc sulfate, zinc chloride, zinc bromide, magnesium bromide, copper chloride, copper sulfate, and combinations thereof. In the embodiment, the flocculant may be added to the mixture at a temperature below the glass transition temperature (Tg) of the resin.
[0090] The flocculant may be added to the mixture used to form the toner in an amount of about 0.1% to about 8% by weight of the resin in the mixture, about 0.2% to about 5% by weight in an embodiment, and about 0.5% to about 5% by weight in other embodiments. This provides a sufficient amount of the agent for flocculation. Shell resin
[0091] In this embodiment, the shell may be applied to the aggregated particles after aggregation but before cementation.
[0092] Examples of resins that can be used to form the shell include, but are not limited to, the amorphous resins used for the core. Such amorphous resins may be low molecular weight resins, high molecular weight resins, or combinations thereof. In embodiments, an example of an amorphous resin that can be used to form the shell according to this disclosure is the amorphous polyester of formula I described above.
[0093] In some embodiments, the amorphous resin used to form the shell may be crosslinked. For example, crosslinking can be achieved by combining the amorphous resin with a crosslinking agent, sometimes referred to herein as a reaction initiator in embodiments. Examples of suitable crosslinking agents include, but are not limited to, the above-mentioned organic peroxides and azo compounds, which are suitable for forming a gel within the core, as free radicals or thermal reaction initiators.
[0094] The crosslinking agent and amorphous resin may be combined for a sufficient time and temperature to form a crosslinked polyester gel. In embodiments, the crosslinking agent and amorphous resin may be heated to a temperature of about 25°C to about 99°C, or in embodiments, about 30°C to about 95°C, for a period of about 1 minute to about 10 hours, or in embodiments, about 5 minutes to about 5 hours, to form a crosslinked polyester resin or polyester gel suitable for use as a shell.
[0095] When used, the crosslinking agent may be present in an amount of about 0.001% to about 5% by weight of the resin, and in embodiments, about 0.01% to about 1% by weight of the resin. The amount of CCA can be reduced in the presence of the crosslinking agent or reaction initiator. Fusion
[0096] Following aggregation to a desired particle size and the application of an optional shell, the particles may then be cemented into a desired final shape, which is achieved by heating the mixture to a temperature of, for example, about 45°C to about 100°C, and in embodiments, about 55°C to about 99°C (this temperature may be above the glass transition temperature of the resin used to form the toner particles), and / or reducing the stirring to, for example, about 100 rpm to about 400 rpm, and in embodiments, about 200 rpm to about 300 rpm. The cemented particles can be measured for shape factor or roundness using an analyzer such as a SYSMEX FPIA 2100 until the desired shape is achieved.
[0097] Bonding may be achieved over a period of approximately 0.01 to 9 hours, or in some embodiments, approximately 0.1 to 4 hours. Subsequent processing
[0098] In embodiments, after aggregation and / or bonding, the pH of the mixture can be lowered to about 3.5 to about 6, and in embodiments to about 3.7 to about 5.5, for example, with an acid, in order to further bond the toner aggregates. Suitable acids include, for example, nitric acid, sulfuric acid, hydrochloric acid, citric acid, and / or acetic acid. The amount of acid added may be about 0.1 to about 30 weight percent of the mixture, and in embodiments to about 1 to about 20 weight percent of the mixture.
[0099] The mixture may be cooled, washed, and dried. Cooling may take place at a temperature of about 20°C to about 40°C, or in embodiments, about 22°C to about 30°C, for about 1 hour to about 8 hours, or in embodiments, about 1.5 hours to about 5 hours.
[0100] In embodiments, cooling of the cemented toner slurry may include rapid cooling by adding a cooling medium such as ice or dry ice and rapidly cooling to a temperature of about 20°C to about 40°C, or in embodiments, about 22°C to about 30°C. Rapid cooling may be feasible for small amounts of toner, for example, less than about 2 liters, or in embodiments, about 0.1 liters to about 1.5 liters. For larger-scale processes, such as those exceeding about 10 liters in size, rapid cooling of the toner mixture may not be feasible or practical, whether by introducing a cooling medium into the toner mixture or by using reactor cooling with a jacket.
[0101] Next, the toner slurry may be washed. The washing may be carried out at a pH of about 7 to about 12, and in embodiments, at a pH of about 9 to about 11. The washing may be carried out at a temperature of about 30°C to about 70°C, and in embodiments, at a temperature of about 40°C to about 67°C. The washing may include filtering and re-slurring the filtration cake containing toner particles in deionized water. The filtration cake may be washed once or more times with deionized water, or the pH of the slurry may be adjusted with acid to a pH of about 4 and washed once with deionized water, followed optionally by one or more more washes with deionized water.
[0102] Drying may be carried out by any method within the scope of intent of those skilled in the art. Any suitable method for drying toner particles may be used, including freeze-drying, spray drying, and instantaneous airflow drying such as Aljet dryers. Drying may be continued until the moisture level of the particles falls below the set target of about 1% by weight, or in embodiments, about 0.7% by weight. additives
[0103] In embodiments, the toner particles may contain the polymer additives of the present disclosure described above, as well as any other additives, if desired or as needed. For example, the toner may contain a positive or negative charge regulator in an amount of about 0.1 to about 10% by weight of the toner, or in embodiments, about 1 to about 3% by weight of the toner. Examples of suitable charge regulators include quaternary ammonium compounds containing alkylpyridinium halides, disulfates, alkylpyridinium compounds, organic sulfates and sulfonates, including those disclosed in U.S. Patent No. 4,298,672, which is incorporated entirely herein by reference, and those disclosed in U.S. Patent No. 4,338,390, which is incorporated entirely herein by reference.
[0104] Furthermore, after formation, the toner particles may be compounded with external additive particles containing flow aid additives, and these additives may be present on the surface of the toner particles. Examples of these additives include metal oxides such as titanium dioxide, silicon dioxide, aluminum oxide, cerium oxide, tin oxide, and mixtures thereof; metal salts and fatty acid metal salts containing colloidal silica and amorphous silica such as AEROSIL®, zinc stearate, calcium stearate, or long-chain alcohols such as UNILIN 700, and mixtures thereof.
[0105] Generally, silica may be applied to the toner surface for toner flow, triboelectric charging enhancement, mixing control, improved development and transfer stability, and higher toner blocking temperature. TiO2 may be applied for improved relative humidity (RH) stability, triboelectric charging control, and improved development and transfer stability. Zinc stearate, calcium stearate, and / or magnesium stearate may be used as external additives to provide lubrication properties, developer conductivity, and triboelectric charging enhancement, thereby enabling higher toner charge and charge stability by increasing the number of contacts between the toner and carrier particles. In embodiments, commercially available zinc stearate known as Zinc Stearate L, available from Ferro Corporation, may be used. External surface additives may be used with or without the coating.
[0106] Each of these external additives may be present in an amount of about 0% to about 3% by weight of the toner, or in embodiments, about 0.25% to about 2.5% by weight of the toner, although the amount of additives may be outside these ranges. In embodiments, the toner may contain, for example, about 0% to about 3% by weight of titania, about 0% to about 3% by weight of silica, and about 0% to about 3% by weight of zinc stearate.
[0107] In embodiments, in addition to the polymer additives of the present disclosure, the toner particles may also contain silica in an amount of about 0.1% to about 5% by weight, and in embodiments, about 0.2% to about 2% by weight, of the toner particles, and titania in an amount of about 0% to about 3% by weight, and in embodiments, about 0.1% to about 1% by weight, of the toner particles. Developer
[0108] The toner particles formed in this way can be incorporated into a developer composition. By mixing the toner particles with carrier particles, a two-component developer composition can be obtained. The toner concentration in the developer may be about 1% by weight to about 25% by weight of the total weight of the developer, and in embodiments, about 2% by weight to about 15% by weight of the total weight of the developer. Career
[0109] Examples of carrier particles that can be used for mixing with toner include particles that can acquire a charge of opposite polarity to that of the toner particles through triboelectric means. Exemplary examples of suitable carrier particles include granular zircon, granular silicon, glass, steel, nickel, ferrite, iron ferrite, and silicon dioxide. Other carriers are disclosed in U.S. Patents No. 3,847,604, No. 4,937,166, and No. 4,935,326.
[0110] In embodiments, a suitable carrier may include a steel core, for example, with a diameter of about 25 to about 100 μm, or in embodiments, about 50 to about 75 μm, coated using the processes described in U.S. Patent Nos. 5,236,629 and 5,330,874, with a conductive polymer mixture containing, for example, methyl acrylate and carbon black, in about 0.5% to about 10% by weight, or in embodiments, about 0.7% to about 5% by weight, using a conductive polymer mixture containing, for example, methyl acrylate and carbon black.
[0111] The carrier particles can be mixed with toner particles in various suitable combinations. The concentration may be about 1% to 20% by weight of the toner composition. However, by using different percentages of toner and carrier, a developer composition with desired properties can be obtained. imaging
[0112] Toners can be used in electrostatic copying or electrophotographic processes, including those disclosed in U.S. Patent No. 4,295,990, which is incorporated herein by reference in its entirety. In embodiments, any known type of developing system may be used in developing apparatuses, including, for example, magnetic brush developing, jumping single-component developing, and hybrid scavengeless developing (HSD). These and similar developing systems are within the intent of those skilled in the art.
[0113] Once an image is formed with toner / developer via a preferred developing method such as one of the methods described above, the image can then be transferred to an image-receiving medium such as paper. In some embodiments, toner may be used for development in a developing device that utilizes a fuser roll member.
[0114] The following examples are provided to illustrate embodiments of the present disclosure. These examples are for illustrative purposes only and are not intended to limit the scope of the present disclosure. Unless otherwise stated, proportions and percentages are given by weight. [Examples]
[0115] Preparation of fluorinated latex.
[0116] All fluorinated organic-added latexes used herein were prepared on a 2L bench scale. Numerous latexes were used. All latexes were prepared using the same general process and formulation filler amounts, except for variations in monomer ratios. Details are shown in Table 1 below.
[0117] Example 1: Synthesis of fluorinated organic-added latex with 0% DVB.
[0118] In a 2 L Bucher reactor equipped with a P4 impeller, 6.5 g of Calfoam SLS surfactant (30% solid) was added to 816 g of deionized water (DIW). The reactor was deoxygenated by passing a nitrogen stream through it during the reaction. The reactor was heated to 77°C and the rpm was set to 400. Separately, in a 1 L glass container equipped with two P4 impellers, a monomer emulsion was prepared by mixing 319.5 g of trifluoroethyl methacrylate (TFEMA), 6.5 g of Calfoam SLS surfactant (30% solid), and 416 g of DIW together (at 450 rpm). 37.1 g of seed was taken from the monomer emulsion and pumped into the 2 L reactor at 77°C. A reaction initiator solution prepared from 1.22 g of ammonium persulfate in 34.3 g of DIW was added over 20 minutes after the seed emulsion was added. The remaining monomer emulsion was supplied to the reactor over 120 minutes. When half of the monomer emulsion had been added, the reactor speed was increased to 450 rpm. At the end of the monomer supply, the latex was post-treated using a protocol of 77°C for 1 hour, followed by heating to 87°C for 2 hours and holding at 87°C for 1 hour to reduce residual monomer at the end of the emulsion polymerization process. As a result, a latex with an average particle size of 99 nm and containing 20% solid was obtained.
[0119] Example 2: Synthesis of fluorinated organic-added latex with 0% DVB. Same process and formulation as above.
[0120] Comparative Example 1: Synthesis of fluorinated organic-added latex using DVB. The procedure was the same as in Example 2, except that 10% DVB and 90% TFEMA were used.
[0121] Comparative Example 2: Synthesis of fluorinated organic-added latex using DVB. The procedure was the same as in Example 2, except that 20% DVB and 80% TFEMA were used.
[0122] Comparative Example 3: Synthesis of fluorinated organic-added latex using DVB. The procedure was the same as in Example 2, except that 30% DVB and 70% TFEMA were used.
[0123] Comparative Example 4: Synthesis of fluorinated organic-added latex using CHMA and DVB. This is the same as Example 2, except that 30% DVB, 35% TFEMA, and 35% CHMA were used. Since DVB contains impurities, in all of the above examples and comparative examples, the actual DVB content is 55% of the amount added to the resin. The following table shows the amount of DVB added to the formulation and the actual DVB content, which is approximately 0.55 times the amount added to the formulation. The majority of the impurities in DVB are ethyl vinylbenzene, which is also incorporated into polymer additives.
[0124] Comparative Example 5: Synthesis of non-fluorinated organically added latex prepared using CHMA and 25% DVB with 0.8% DMAEMA. In a 300 Gal reactor equipped with two P4 impellers and a condenser, 0.942 kg of Calfoam SLS surfactant (30% solid) was added to 444 kg of DIW. The reactor was deoxygenated by passing a nitrogen stream through it during the reaction, and the condenser was used. The reactor was heated to 77°C and the rpm was set to 59. Separately, in a 100 Gal reactor equipped with one P4 impeller, a monomer emulsion was prepared by mixing 126 kg of CHMA, 42.45 kg of DVB, 1.358 kg of DMAEMA, 5.92 kg of Calfoam SLS surfactant (30% solid) and 221.1 kg of DIW together (at 28 rpm). 0.369 kg of seed was removed from the monomer emulsion and pumped into a 300 Gal reactor at 77°C. An initiator solution prepared from 0.645 kg of ammonium persulfate in 7.045 kg of DIW was added over 15 minutes after the seed emulsion was added. The remaining monomer emulsion was supplied to the 300 Gal reactor over 120 minutes. When half of the monomer emulsion had been added, the reactor rpm was increased to 66 rpm. The condenser was turned off at the end of the monomer supply. The latex underwent a post-treatment protocol at 77°C for 1 hour, followed by heating to 87°C for 2 hours and holding at 87°C for 1 hour to reduce residual monomer at the end of the emulsion polymerization process. During the post-treatment protocol, the pH of the latex was adjusted to ≥6.0 every 30 minutes using a 0.1 wt% NaOH solution. As a result, a latex with an average particle size of 98 nm and containing 20% solid was obtained and filtered through a 25 micrometer filter bag. The latex was spray-dried to form the final dried powder.
[0125] In all examples and comparative examples, DVB contains impurities; therefore, in all of the above examples and comparative examples, the actual DVB content is 55% of the amount added to the resin. The table below shows the amount of DVB added to the formulation and the actual DVB content, which is approximately 0.55 times the amount added to the formulation. The majority of the impurities in DVB are ethyl vinylbenzene, which is also incorporated into polymer additives. [Table 1] ND = Not detected Toner additive change over time: Planarization test
[0126] Each additive was individually compounded in a laboratory SKM mill at 18% SAC (Surface Area Coverage) in the cyan ecotoner, which is the base material for the Xerox 700 Digital Color Press. The general ideal formula for the surface area coverage (%) of spherical organic surface additives on the surface of toner particles is given by (100%·w·D·P) / (0.363·d·p), where D is the average D50 size in micrometers for the toner and P is grams / cm². 3 This is the true density, and for organic emulsion polymerized latex, d is the average D50 size in nanometers, and p is the gram / cm³. 3 This is the true density, where w is the weight added to the mixture in pph units. Table 2 shows the weight percentage of the fill amount corresponding to 18% SAC. [Table 2]
[0127] For each toner, 30 g of Xerox 700 Digital Color Press carrier was used together with 1.50 g of formulated toner in a 60 mL glass vial. This resulted in a toner concentration of 5%, i.e., TC. The sample was prepared in the J zone and then mixed on a Turbula mixer for a total of 2 hours, with samples for SEM taken at 15 minutes, 30 minutes, 1 hour, and 2 hours. The SEM images were examined, and failure was evaluated if the organic polymer additive had flattened and was no longer spherical. The survival time was then defined as the longest time the particles remained spherical. Therefore, if the particles flattened at 2 hours, the survival time was 1 hour. As shown in Figure 1, increasing the DVB to 30% by weight increased the survival time. Toners with non-crosslinked TFEMA polymer additives were already flattened on the toner surface before the developer aging test, i.e., flattened during the toner formulation process. [Table 3] Single-additive electrostatic test with a single additive containing 17% SAC
[0128] The electrostatic properties in the J zone were evaluated for each of the toners listed in Table 2, formulated with 18% SAC. Samples were taken at 15 minutes and 120 minutes during the above time-course test. The results are shown in Table 3 and Figure 1. It is very clear from the data that the charge decreases with increasing crosslinking. For crosslinking additives that are not planarized or affected, it is theorized that the charge originates almost entirely from the uncovered parent surface, as the additives have only a small surface coverage, and therefore the additives have only a small effect on the charge. Since the non-crosslinking additives are completely planarized, it was expected that these additives would be completely embedded in the toner even at time zero in this time-course test, and thus provide even less charge benefit. However, these examples without crosslinking are far more negatively charged. Non-crosslinking TFEMA particles during planarization cover more of the toner surface, increasing the cross-sectional area covered on the surface.
[0129] Figure 2 shows Example 2, which is 0% DVB non-crosslinked TFEMA latex on cyan parent toner after 15 minutes of developer aging (first aging point). The majority of the additive has been planarized on the toner surface and is visible as flakes of flat particles and merged particles, except for protective areas in deep toner gaps. Thus, the additive does not remain spherical at the first aging point of 15 minutes, and its lifespan is 0 minutes.
[0130] Figure 3 shows Comparative Example 3, which has DVB 30% cross-linked TFEMA latex on cyan parent toner, after 120 minutes of developer aging (the last aging point tested). Some of the additive is embedded in the toner surface, but the additive particles remain spherical after 120 minutes. Thus, the survival time of the additive is at least 120 minutes. [Table 4]
[0131] Since the non-crosslinked additive was thus planarized, and therefore its surface coverage was higher than that of the crosslinked version, the non-crosslinked additive was evaluated for its effects on charge, flow, and blocking in addition to the Pinot surface additive design shown in Table 4. Both toners had the same additive package shown in Table 4, except that one toner contained 1.3 wt% non-crosslinked TFEMA latex in a 16% SAC mixture. Surprisingly, as shown in Table 5, there was no effect on charge, flow cohesive force increased somewhat, but blocking was significantly improved. [Table 5] [Table 6] The non-crosslinked TFEMA polymer had a measured Tg of 67°C. Due to the low Tg, the additive is very easily planarized. Furthermore, because the Tg is not significantly higher than that of the resin, any effect on melting is small, less than that of the same filler weights of silica and titania, and less than, for example, the effect of using CHMA or PMMA polymers, both of which have Tg > 100°C. On the other hand, fluorination gives the polymer a lower surface energy, which helps with blocking.
[0132] By using TFEMA non-crosslinked latex in the additive formulation, blocking can be improved without affecting the charge and with minimal impact on flow cohesive forces.
[0133] The polymer resins disclosed herein do not contain a substantial amount of crosslinking and comprise a fluorinated monomer and a charge control agent optionally containing 0.1% to 1.5% by weight of nitrogen-containing groups of the polymer resin. In embodiments, the crosslinking of the polymer resin is less than 10% by weight of the polymer resin. In embodiments, the crosslinking is less than about 5% by weight of the polymer resin. In embodiments, the crosslinking is less than about 2% by weight of the polymer resin. In embodiments, the crosslinking is less than about 1% by weight of the polymer resin. This low amount of crosslinking does not hinder the planarization of the polymer additive.
[0134] It will be understood that variations of the above-disclosed features and functions, or substitutes thereof, may be combined into other different systems or applications. Various substitutes, modifications, variations, or improvements not currently anticipated or anticipated may be subsequently made by those skilled in the art, and these are also covered by the following claims.
Claims
1. 1. A toner composition comprising: emulsion aggregation toner particles comprising at least one amorphous polyester resin and one crystalline polyester resin; A surfactant, an optional colorant; and an optional wax; a polymeric toner additive on at least a portion of an outer surface of said emulsion aggregation toner particles; The polymeric toner additive is a polymeric resin comprising a fluorinated monomer consisting of trifluoromethacrylate, said polymeric resin being less than 10% by weight crosslinked; and optionally 0.1% to 1.5% by weight of said polymeric resin of a charge control agent comprising a nitrogen-containing group monomer; Toner Composition.
2. The toner composition of claim 1 , wherein the charge control agent monomer comprises an acrylate monomer or a methacrylate monomer.
3. The toner composition of claim 1 , wherein the polymeric resin further comprises a non-fluorinated hydrophobic monomer.
4. The toner composition of claim 1 , wherein the polymeric resin further comprises cyclohexyl methacrylate.
5. The toner composition of claim 1 , wherein the polymer resin is leveled on the surface of the toner particles.
6. 10. The toner composition of claim 1, further comprising at least one additive selected from the group of silica, titania, alumina, and crosslinked non-fluorinated organic surface additives.
7. 10. The toner composition of claim 1, wherein said emulsion aggregation toner particles have a size of from about 4 micrometers to about 10 micrometers.
8. 10. The toner composition of claim 1, further comprising a cleaning additive selected from the group consisting of stearates, cerium oxide, and strontium titanate.
9. 2. The toner composition of claim 1, wherein said polymeric additive comprises from 0.1 weight percent to 5 weight percent of said toner composition.
10. 2. The toner composition of claim 1, wherein the polymeric additive has a size of from 25 nanometers to 250 nanometers.
11. a developer comprising a toner composition and a toner carrier; The toner composition comprises emulsion aggregation toner particles comprising at least one amorphous polyester resin and one crystalline polyester resin; A surfactant, an optional colorant; and an optional wax; a polymeric toner additive on at least a portion of an outer surface of said emulsion aggregation toner particles; The polymeric toner additive is a polymeric resin comprising a fluorinated monomer consisting of trifluoromethacrylate, the polymeric resin being less than 10% by weight crosslinked; and 0.1% to 1.5% by weight of the polymeric resin of a charge control agent comprising a nitrogen-containing group. Developer.
12. The developer of claim 11 , wherein the charge control agent monomer comprises an acrylate monomer or a methacrylate monomer.
13. The developer of claim 11 , wherein the polymeric resin further comprises a non-fluorinated hydrophobic monomer.
14. The developer of claim 11 , wherein the polymer resin further comprises cyclohexyl methacrylate.
15. The developer of claim 11 , wherein the polymer resin is leveled on the surface of the toner particles.
16. 12. The developer of claim 11 further comprising an additive selected from the group of silica, titania, alumina, and bridged non-fluorinated organic surface additives.
17. 1. A toner additive composition comprising: emulsion aggregation toner particles comprising at least one amorphous polyester resin and one crystalline polyester resin; A surfactant, a polymeric resin comprising a fluorinated monomer consisting of trifluoromethacrylate, the polymeric resin being less than 10% crosslinked by weight; and 0.1% to 1.5% by weight of the polymeric resin of a charge control agent monomer comprising a nitrogen-containing group; Toner additive compositions.
18. 20. The toner composition of claim 17, wherein said emulsion-polymerized polymer resin comprises a size range of 25 nanometers to 250 nanometers.