Polyimide fiber, fiber package, wiring board, and method for producing polyimide fiber
Patent Information
- Application Number
- JP2022028650
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-02-26
- Filing Date
- 2022-02-25
- Publication Date
- 2024-10-02
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing polyimide fibers using melt spinning face challenges such as high melting points, high melt viscosity leading to melt fracture, and difficulties in processing due to high processing temperatures, along with issues like yarn breakage and air bubbles during spinning, especially when using polyimide resins with chain aliphatic groups.
A polyimide fiber composition comprising specific structural units with a melting point of 280°C to 345°C, glass transition temperature of 150°C to 200°C, and controlled crystallization exothermic peak, allowing for stable fiberization with a melt spinning method that does not require solvent recovery, resulting in high-strength fibers with excellent dimensional and thermal stability.
The method produces polyimide fibers with high heat resistance, electrical insulation, and low coefficient of linear expansion, achieving stable fiberization at lower temperatures without the need for special spinning devices, and enabling easy post-processing and functionalization.
Abstract
Description
[Technical Field]
[0001] This invention relates to polyimide fibers, fiber packages, wiring boards, and methods for producing polyimide fibers. [Background technology]
[0002] Polyimide resins are useful engineering plastics with high thermal stability, high strength, and high solvent resistance due to the rigidity of their molecular chains, resonance stabilization, and strong chemical bonding, and are applied in a wide range of fields. Furthermore, crystalline polyimide resins can have their heat resistance, strength, and chemical resistance further improved, and are expected to be used as metal substitutes, etc. However, while polyimide resins have high heat resistance, they do not exhibit thermoplasticity and have the problem of poor moldability.
[0003] In particular, due to their rigid structure, polyimide resins typically do not have a melting point before their decomposition temperature, making it technically difficult to produce fibers using polyimide resins. Conventional methods for producing polyimide fibers involve dissolving them in a highly polar solvent and then spinning them using a wet-dry process. However, polyimide fibers produced by wet spinning require solvent recovery, which presents environmental and cost challenges. Therefore, in recent years, a method of converting polyimide resin into a thermoplastic resin and then using melt spinning to create fibers from it has attracted attention.
[0004] For example, Patent Document 1 (Japanese Patent Publication No. 2002-309441) proposes a polyimide fiber made of thermoplastic polyimide that can also be obtained by melt spinning, which has fine denier, high strength, and excellent properties such as dimensional stability and thermal stability, as well as a method for producing such a polyimide fiber. Patent Document 1 describes an invention of a crystallized polyimide fiber, which is a multifilament made of polyimide having 80 mol% or more of repeating units represented by a specific structural formula in the main chain, having a crystallinity of 20% or more, and an average fiber diameter of 20 μm or less per filament.
[0005] Patent Document 2 (Japanese Patent Publication No. 2004-176212) proposes a polyimide fiber with reduced yarn unevenness, made of thermoplastic polyimide obtained by melt spinning, having low yarn unevenness (C%) as a multifilament, low single filament fineness, and little variation in the fineness of each single filament constituting the multifilament, and a method for producing the same. Patent Document 2 describes an invention of a polyimide fiber with reduced yarn unevenness, characterized by a multifilament made of polyimide having 80 mol% or more of specific repeating units in the main chain, having 30 or more single filaments, a single filament fineness of 6 dtex or less, a multifilament thickness variation of 10% or less in Worcestershire normal C%, and a variation of the cross-sectional area of each single filament when the multifilament is cut perpendicular to the fiber axis direction of 20% or less.
[0006] Furthermore, Patent Document 3 (Japanese Unexamined Patent Publication No. 6-33316) proposes a method for producing polyimide fibers that are suitable as a base resin for fiber-reinforced composite materials and can be produced stably over a long period of time. Patent Document 3 describes an invention for a method of producing polyimide fibers in which, when melt spinning a thermoplastic polyimide with a melt viscosity of 7000 poise or less, the melting temperature of the resin, residence time, pressure, discharge linear velocity, die temperature, and ambient temperature of the heating cylinder are specified to prevent thickening, gel formation, or generation of decomposition gases.
[0007] Furthermore, Patent Document 4 (International Publication No. 2016 / 147996) describes a polyimide resin that includes repeating structural units represented by the following formula (1) and repeating structural units represented by the following formula (2), wherein the content ratio of the repeating structural units of formula (1) to the total of the repeating structural units of formula (1) and the repeating structural units of formula (2) is 20 mol% or more and less than 40 mol%, and satisfies predetermined conditions. JPEG2022132199000002.jpg3196
[0008] Furthermore, Patent Document 5 (International Publication No. 2015 / 020016) describes an invention of a polyimide resin that includes repeating structural units of the following formula (1), repeating structural units of the following formula (2), and repeating structural units of the following formula (A) or structural units of the following formula (B), wherein the content ratio of formula (1) to the total of formula (1) and formula (2) is 40 to 70 mol%, and the content ratio of formula (A) or formula (B) to the total of formula (1) and formula (2) is greater than 0 mol% and less than or equal to 25 mol%. JPEG2022132199000003.jpg54119 [Prior art documents] [Patent Documents]
[0009] [Patent Document 1] Japanese Patent Publication No. 2002-309441 [Patent Document 2] Japanese Patent Publication No. 2004-176212 [Patent Document 3] Japanese Patent Application Publication No. 6-33316 [Patent Document 4] International Publication No. 2016 / 147996 [Patent Document 5] International Publication No. 2015 / 020016 [Overview of the project] [Problems that the invention aims to solve]
[0010] Patent documents 1 to 3 disclose a method for producing polyimide fibers by melt spinning, using a thermoplastic polyimide resin. However, in the methods described in patent documents 1 to 3, the polyimide resin has a high melting point and high melt viscosity, and is prone to melt fracture, which limits the types of spinning machines that can be used and makes it difficult to produce polyimide fibers stably. In addition, the polyimide resin fibers obtained by the methods in patent documents 1 or 3 are difficult to process due to the high processing temperature, which also limits the types of machines that can be used.
[0011] One method for lowering the melting point of polyimide resin is to use long-chain aliphatic diamines as the raw material diamines. This method reduces the rigidity of the polyimide resin, thereby lowering the melting point. However, this method also lowers the glass transition temperature along with the melting point, raising concerns about a decrease in strength, especially at high temperatures. Furthermore, there has been the problem that synthesizing polyimide resin using raw material diamines mainly composed of aliphatic diamines is difficult. Patent documents 4 and 5 disclose a technique for improving the physical properties of a polyimide resin and producing a polyimide resin with good processing characteristics by using a polyimide resin containing specific chain-like aliphatic groups. However, when attempting to melt spin polyimide resins containing chain-like aliphatic groups as described in patent documents 4 and 5, problems such as yarn breakage and air bubble inclusion tend to occur during spinning, and there are drawbacks such as variations in the breaking strength of the fibers, making fiber formation difficult.
[0012] The present invention aims to solve the above-mentioned problems and provide polyimide fibers, fiber packages, wiring substrates, and a method for producing polyimide fibers that are highly strong and have excellent properties such as dimensional stability and thermal stability, by melt spinning. Another object of the present invention is to provide polyimide fibers that exhibit excellent post-processing properties, even if they have a very high melting point. Another object of the present invention is to provide a method for stably producing polyimide fibers with excellent heat resistance, dimensional stability, and electrical properties using a melt spinning method. [Means for solving the problem]
[0013] (1) Polyimide fibers conforming to a single plane are repeating structural units represented by the following formula (1) and the following formula (2): [ka] (R1 is a divalent group having 6 to 22 carbon atoms containing at least one alicyclic hydrocarbon structure. R2 is a divalent linear aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently tetravalent groups having 6 to 22 carbon atoms containing at least one aromatic ring.) The polyimide resin comprises a polyimide resin that satisfies the following conditions (a), (b), and (c), and has at least one physical property selected from the group consisting of physical properties (A), (B), and (C). The content ratio of repeating structural units of formula (1) to the total of repeating structural units of formula (2) is 20 mol% or more and less than 40 mol%, and the polyimide resin satisfies the following conditions (a), (b), and (c). Condition (a): Melting point (Tm) is between 280°C and 345°C. Condition (b): Glass transition temperature (Tg) is between 150°C and 200°C. Condition (c): The heat energy of the crystallization exothermic peak observed when the material is cooled at a rate of 20°C / min after melting, as measured by differential scanning calorimeter, is 17.0 mJ / mg or more. Physical property (A): The tensile strength of the polyimide fiber is 1.5 cN / dtex or higher. Physical property (B): The variation in the breaking strength of the polyimide fiber is within ±0.2 cN / dtex. Physical property (C): The elongation at break of the polyimide fiber is 20% or more.
[0014] According to the present invention, polyimide resin, which has excellent heat resistance, dimensional stability, and electrical properties, can be stably fiberized using a melt spinning method. This makes it possible to produce polyimide fibers that are particularly excellent in heat resistance, electrical insulation, low coefficient of thermal expansion, and strength. Furthermore, since fiberization can be performed at relatively low temperatures using a melt spinning method that does not require solvent recovery, special spinning equipment is not required, resulting in polyimide fibers that are excellent from the standpoint of the environment and cost. Furthermore, it is possible to create fibers with high breaking strength and high quality fibers with little variation in breaking strength. Furthermore, it is possible to create fibers with high elongation at break, and because they are easy to process in subsequent steps, they can be easily processed or given functions according to the product. Furthermore, because of its low glass transition temperature (Tg), it does not require a high-temperature environment in subsequent processes, making it possible to create a fiber that is easily processed or functionalized according to the product.
[0015] (2) The polyimide fiber according to the second invention is a polyimide fiber conforming to a single plane, wherein the melting point (Tm) of the polyimide resin is 310°C or higher and 335°C or lower, the glass transition temperature (Tg) is 170°C or higher and 190°C or lower, and the shear rate at 360°C is 100 s. -1 The melt viscosity may be 1050 Pa·s or less.
[0016] This makes it possible to produce polyimide fibers that are even stronger and have even better properties such as dimensional stability and thermal stability. Furthermore, even polyimide fibers with very high melting points can be produced that have excellent post-processing properties.
[0017] (3) The polyimide fiber according to the third invention is a polyimide fiber according to the first invention or the second invention, wherein R1 may be a divalent group represented by the following formula (R1-1) or (R1-2). [ka] (m 11 and m 12 Each of these is an integer between 0 and 2, independently of the others. 13 ~m 15 Each of these is an integer between 0 and 2, independently of the others.
[0018] This makes it possible to produce polyimide fibers that are even stronger and have even better properties such as dimensional stability and thermal stability. Furthermore, even polyimide fibers with very high melting points can be produced that have excellent post-processing properties.
[0019] (4) The polyimide fiber according to the fourth invention is, in one aspect, the polyimide fiber according to the third invention, and R1 may be a divalent group represented by the following formula (R1-3). [Chemical formula]
[0020] Thereby, it is possible to obtain a polyimide fiber having higher strength and also excellent properties such as dimensional stability and thermal stability. Further, even if the polyimide fiber has a very high melting point, it is possible to obtain a polyimide fiber having excellent post-processing properties.
[0021] (5) The polyimide fiber according to the fifth invention is, in one aspect, the polyimide fiber according to the fourth invention, and R2 may be an alkylene group having 7 to 12 carbon atoms.
[0022] Thereby, it is possible to obtain a polyimide fiber having higher strength and also excellent properties such as dimensional stability and thermal stability. Further, even if the polyimide fiber has a very high melting point, it is possible to obtain a polyimide fiber having excellent post-processing properties.
[0023] (6) The polyimide fiber according to the sixth invention is, in one aspect, the polyimide fiber according to the fifth invention, and X1 and X2 may each independently be a tetravalent group represented by any one of the following formulas (X-1) to (X-4).
[0024] [Chemical formula]
[0025] (R 11 ~R 18 are each independently an alkyl group having 1 to 4 carbon atoms. p 11 ~p 13 are each independently an integer of 0 to 2. p 14 p 15 p 16 and p18 Each of these is an integer between 0 and 3, independently of the others. 17 L is an integer between 0 and 4. 11 ~L 13 These are, independently, a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.
[0026] This makes it possible to produce polyimide fibers that are even stronger and have even better properties such as dimensional stability and thermal stability. Furthermore, even polyimide fibers with very high melting points can be produced that have excellent post-processing properties.
[0027] (7) Polyimide fibers following other orientations have a melting point (Tm) of 280°C to 345°C, a glass transition temperature (Tg) of 150°C to 200°C, and a shear rate of 100 s at 360°C. -1 The polyimide fiber comprises a thermoplastic dry polyimide resin having a melt viscosity of 1050 Pa·s or less, and possessing at least one physical property selected from the group consisting of the following physical properties (A), (B), and (C). Physical property (A): The tensile strength of the polyimide fiber is 1.5 cN / dtex or higher. Physical property (B): The tensile strength variation of the polyimide fiber is less than ±0.3 cN / dtex. Physical property (C): The elongation at break of the polyimide fiber is 10% or more.
[0028] In this invention, polyimide fibers can be produced using polyimide resin in accordance with a single plane. According to the present invention, polyimide resin, which has excellent heat resistance, dimensional stability, and electrical properties, can be stably fiberized using a melt spinning method. This makes it possible to produce polyimide fibers that are particularly excellent in heat resistance, electrical insulation, low coefficient of thermal expansion, and strength. Furthermore, since fiberization can be performed at relatively low temperatures using a melt spinning method that does not require solvent recovery, special spinning equipment is not required, resulting in polyimide fibers that are excellent from the standpoint of the environment and cost. Furthermore, it is possible to create fibers with high breaking strength and high quality fibers with little variation in breaking strength. Furthermore, it is possible to create fibers with high elongation at break, and because they are easy to process in subsequent steps, they can be easily processed or given functions according to the product. Furthermore, because of its low glass transition temperature (Tg), it does not require a high-temperature environment in subsequent processes, making it possible to create a fiber that is easily processed or functionalized according to the product.
[0029] (8) The polyimide fiber according to the eighth invention is a polyimide fiber conforming to the seventh aspect, having a melting point (Tm) of 310°C or more and 335°C or less, a glass transition temperature (Tg) of 170°C or more and 190°C or less, and having physical properties (A), (B), and (C).
[0030] This makes it possible to produce polyimide fibers that are even stronger and have even better properties such as dimensional stability and thermal stability. Furthermore, even polyimide fibers with very high melting points can be produced that have excellent post-processing properties.
[0031] (9) The fiber package according to the ninth invention may be a fiber package in which polyimide fibers according to the eighth invention are wound around a tube such as a paper tube.
[0032] This makes it possible to create fiber packages made of polyimide fibers that are high in strength and also have excellent properties such as dimensional stability and thermal stability.
[0033] (10) A wiring board following other aspects may include polyimide fibers according to the eighth invention from one aspect.
[0034] By using polyimide fibers, which have a low dielectric loss tangent and excellent heat resistance, as a material for semiconductor substrates, it is possible to create thin, miniaturized wiring substrates suitable for high-speed communication. In this case, it is preferable that the polyimide fibers have a single-fiber fineness of 2 dtex or less. This allows for the thinning and miniaturization of the circuit board.
[0035] (11) A method for producing polyimide fibers according to other aspects includes a drying step of drying a polyimide resin having a melting point (Tm) of 280°C to 345°C and a glass transition temperature (Tg) of 150°C to 200°C to obtain a dried polyimide resin with a moisture content of 50 ppm or less, and a spinning step of melting the dried polyimide resin while heating it using an extruder under the following conditions (a) to (c), and extruding it from a die to form spun yarn. Condition (a): Shear rate of dry polyimide resin at 360°C is 100 s. -1 The melt viscosity is 1050 Pa·s or less. Condition (b): Spinning temperature is between the melting point of the polyimide resin + 20°C and 380°C. Condition (c): Melt residence time is 12 minutes or less. The process includes a bundling step in which the spun yarn extruded from the die is gathered into a single filament, and a winding step in which the filament is wound onto a tube.
[0036] According to the present invention, polyimide resin, which has excellent heat resistance, dimensional stability, and electrical properties, can be stably fiberized using a melt spinning method. This makes it possible to produce polyimide fibers that are particularly excellent in heat resistance, electrical insulation, low coefficient of thermal expansion, and strength. Furthermore, since fiberization can be performed at relatively low temperatures using a melt spinning method that does not require solvent recovery, special spinning equipment is not required, making it possible to produce polyimide fibers that are excellent from the standpoint of the environment and cost. In addition, it is possible to produce fibers with high breaking strength and high quality fibers with little variation in breaking strength. Furthermore, it is possible to create fibers with high elongation at break, and because subsequent processing is easy, it is possible to create fibers that can be easily processed or given functions according to the product. Furthermore, because of its low glass transition temperature (Tg), it does not require a high-temperature environment in subsequent processes, making it possible to create a fiber that is easily processed or functionalized according to the product.
[0037] (12) The method for producing polyimide fibers according to the 12th invention is the method for producing polyimide fibers according to the 11th invention, which may further include a stretching step of stretching the bundled filaments while heating them at 150°C to 300°C.
[0038] This makes it possible to produce polyimide fibers with excellent post-processing properties, even if they have a very high melting point.
[0039] (13) The method for producing polyimide fibers according to the 13th invention is a method for producing polyimide fibers according to the 11th or 12th invention, wherein the spinning process satisfies the following conditions. Condition (d): Linear velocity is 5.0 m / min or more and 50.0 m / min or less. Condition (e): Shear rate is 700 s -1 More than 90,000s -1 below, Condition (f): The winding speed (spinning speed) during the winding process is 300 m / min or more and 3500 m / min or less.
[0040] This makes it possible to stably produce polyimide fibers with excellent heat resistance, dimensional stability, and electrical properties using the melt spinning method. [Brief explanation of the drawing]
[0041] [Figure 1] Figure 1 is a schematic diagram illustrating a method for producing polyimide fibers by melt-extruding and melt-spinning polyimide resin. [Modes for carrying out the invention]
[0042] The present invention will be described in detail below. The present invention relates to polyimide fibers that crystallize, have high strength, and exhibit excellent thermal stability and dimensional stability, etc., by using a thermoplastic polyimide resin having a specific chemical structure as a raw material and appropriately selecting the conditions for melt spinning and stretching, as well as a method for producing such polyimide fibers. According to the present invention, polyimide fibers with excellent heat resistance, dimensional stability, electrical properties, etc., can be stably produced using the melt spinning method.
[0043] [Polyimide resin] The polyimide resin used in this invention is formed by combining specific different polyimide constituent units in the specific ratios described above, and satisfies predetermined properties, thus providing a good balance between moldability and heat resistance. The polyimide fibers of the present invention consist of the following polyimide resins, or mainly contain the following polyimide resins. The polyimide resin contains repeating structural units represented by the following formula (1) and the following formula (2). [ka] R1 is a divalent group with 6 to 22 carbon atoms containing at least one alicyclic hydrocarbon structure. R2 is a divalent linear aliphatic group with 5 to 16 carbon atoms. X1 and X2 are each independently tetravalent groups with 6 to 22 carbon atoms containing at least one aromatic ring. The content ratio of the repeating constituent units of formula (1) to the total of the repeating constituent units of formula (2) is 20 mol% or more and less than 40 mol%, and the following conditions (a), (b), and (c) are satisfied. Condition (a): Melting point (Tm) is between 280°C and 345°C. Condition (b): Glass transition temperature (Tg) is 150°C or higher and 200°C or lower. Condition (c): The heat energy of the crystallization exothermic peak observed when the material is cooled at a rate of 20°C / min after melting, as measured by differential scanning calorimeter, is 17.0 mJ / mg or more. Such polyimide resins are thermoplastic, have excellent thermoprocessability, and possess crystalline properties.
[0044] (The constituent unit of polyimide resin) The repeating structural units of equation (1) are described in detail below. R1 is a divalent group having 6 to 22 carbon atoms that contains at least one alicyclic hydrocarbon structure. Here, an alicyclic hydrocarbon structure means a ring derived from an alicyclic hydrocarbon compound, which may be saturated or unsaturated, monocyclic or polycyclic.
[0045] Examples of alicyclic hydrocarbon structures include cycloalkane rings such as cyclohexane rings, cycloalkene rings such as cyclohexene, bicycloalkane rings such as norbornane rings, and bicycloalkene rings such as norbornene, but are not limited to these. Among these, cycloalkane rings are preferred, more preferably cycloalkane rings having 4 to 7 carbon atoms, and even more preferably cyclohexane rings.
[0046] The number of carbon atoms in R1 is 6 to 22, preferably 8 to 17. R1 contains at least one alicyclic hydrocarbon structure, preferably 1 to 3. R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2). [ka] (m 11 and m 12 Each of these is an integer between 0 and 2, preferably 0 or 1. 13 ~m 15 Each of these is an integer between 0 and 2, preferably 0 or 1. R1 is particularly preferably a divalent group represented by the following formula (R1-3). [ka]
[0047] In the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups with respect to the cyclohexane ring may be cis or trans, and the ratio of cis to trans may be any value.
[0048] X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monoring or a fused ring, and examples include, but are not limited to, a benzene ring, a naphthalene ring, anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. The carbon number of X1 is 6 to 22, preferably 6 to 18. X1 contains at least one aromatic ring, preferably 1 to 3. X1 is preferably a tetravalent group represented by any of the following formulas (X-1) to (X-4). [ka] (R 11 ~R 18 These are each independently alkyl groups having 1 to 4 carbon atoms. 11 ~p 13 Each of these is an integer between 0 and 2, preferably 0. 14 , p 15 , p 16 and p 18 Each of these is an integer between 0 and 3, preferably 0. 17 L is an integer between 0 and 4, preferably 0. 11 ~L 13 These are, independently, a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. Furthermore, since X1 is a tetravalent group with 6 to 22 carbon atoms containing at least one aromatic ring, R in equation (X-2) 12 , R 13 , p 12 and p 13 The carbon atoms of the tetravalent group represented by formula (X-2) are selected such that the number of carbon atoms falls within the range of 6 to 22.
[0049] Similarly, L in equation (X-3) 11 , R 14 , R 15 , p 14 and p 15 The number of carbon atoms in the tetravalent group represented by formula (X-3) is selected to fall within the range of 6 to 22, and L in formula (X-4) 12 , L 13 , R 16 , R 17 , R 18 , p 16 , p 17 and p 18 The carbon atoms in the tetravalent group represented by formula (X-4) are selected such that the number of carbon atoms falls within the range of 6 to 22.
[0050] X1 is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6). [ka]
[0051] Next, the repeating constituent units of equation (2) will be described in detail below. R2 is a divalent linear aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms. Here, a linear aliphatic group means a group derived from a linear aliphatic compound, and the linear aliphatic compound may be saturated or unsaturated, linear or branched, and may contain heteroatoms such as oxygen atoms.
[0052] R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, even more preferably an alkylene group having 7 to 12 carbon atoms, and most preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear alkylene group or a branched alkylene group, but a linear alkylene group is preferred.
[0053] R2 is preferably at least one selected from an octamethylene group and a decamethylene group, and is particularly preferably an octamethylene group. Another preferred form of R2 is a divalent linear aliphatic group having 5 to 16 carbon atoms and containing an ether group. The number of carbon atoms is preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10. Among these, a divalent group represented by the following formula (R2-1) or (R2-2) is preferred. [ka] (m 21 and m 22 Each of these is an integer between 1 and 15, preferably between 1 and 13, more preferably between 1 and 11, and even more preferably between 1 and 9. 23 ~m 25 Each of these is an integer between 1 and 14, preferably between 1 and 12, more preferably between 1 and 10, and even more preferably between 1 and 8.
[0054] Furthermore, since R2 is a divalent linear aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms), the m in formula (R2-1) 21 and m 22 The divalent group represented by formula (R2-1) is selected such that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). That is, m 21 +m 22 The value is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10).
[0055] Similarly, in equation (R2-2), m 23 ~m 25 The divalent group represented by formula (R2-2) is selected such that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). That is, m 23 +m 24 +m25 The carbon number is 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms).
[0056] X2 is defined in the same way as X1 in equation (1), and its preferred mode is also the same.
[0057] The content ratio of the repeating structural units of formula (1) to the total content of the repeating structural units of formula (2) is 20 mol% or more and less than 40 mol%. If this content ratio is less than 20 mol%, the melting point rises, and the spinnability decreases.
[0058] Furthermore, if the content ratio is less than 40 mol%, the amount of heat at the crystallization exothermic peak (hereinafter also referred to as "crystallization exothermic amount") increases, resulting in good heat resistance. When the content ratio of the repeating structural units in formula (1) is within the above range, it becomes possible to sufficiently crystallize the polyimide resin.
[0059] The ratio of the repeating structural units of formula (1) to the total of the repeating structural units of formula (2) is preferably 25 mol% or more, more preferably 30 mol% or more, and even more preferably 32 mol% or more, from the viewpoint of spinnability, and preferably 38 mol% or less, more preferably 37 mol% or less, and even more preferably 36 mol% or less, from the viewpoint of increasing the amount of heat generated during crystallization, i.e., heat resistance.
[0060] The content ratio of the total repeating units of formula (1) and formula (2) relative to the total repeating units constituting the polyimide resin is preferably 50 to 100 mol%, more preferably 75 to 100 mol%, even more preferably 80 to 100 mol%, and even more preferably 85 to 100 mol%.
[0061] The polyimide resin may further contain repeating structural units of formula (3) below. In this case, the content ratio of the repeating structural units of formula (3) to the total of the repeating structural units of formula (1) and formula (2) is preferably 25 mol% or less. On the other hand, there is no particular lower limit, and it is sufficient if it is greater than 0 mol%.
[0062] From the viewpoint of improving heat resistance, the aforementioned content ratio is preferably 5 mol% or more, more preferably 10 mol% or more, while from the viewpoint of maintaining crystallinity, it is preferably 20 mol% or less, more preferably 15 mol% or less. [ka] (R3 is a divalent group with 6 to 22 carbon atoms containing at least one aromatic ring. X3 is a tetravalent group with 6 to 22 carbon atoms containing at least one aromatic ring.)
[0063] R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monoring or a fused ring, and examples include, but is not limited to, a benzene ring, a naphthalene ring, anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.
[0064] The number of carbon atoms in R3 is 6 to 22, preferably 6 to 18. R3 contains at least one aromatic ring, preferably 1 to 3. Furthermore, the aromatic ring may have a monovalent or divalent electron-withdrawing group attached to it. Examples of monovalent electron-withdrawing groups include nitro groups, cyano groups, p-toluenesulfonyl groups, halogens, alkyl halides, phenyl groups, and acyl groups. Examples of divalent electron-withdrawing groups include alkylene fluorides (e.g., -C(CF3)2-, -(CF2)). p In addition to halogenated alkylene groups such as -(where p is an integer between 1 and 10), other examples include -CO-, -SO2-, -SO-, -CONH-, and -COO-.
[0065] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2). [ka] (m 31 and m 32 Each of these is an integer between 0 and 2, preferably 0 or 1. 33 and m 34 Each of these is an integer between 0 and 2, preferably 0 or 1. 21 , R 22 , and R 23 These are, independently, an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 , p 22 and p 23 L is an integer between 0 and 4, preferably 0. 21 (This refers to a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.)
[0066] Furthermore, since R3 is a divalent group with 6 to 22 carbon atoms that contains at least one aromatic ring, the m in formula (R3-1) 31 , m 32 , R 21 and p 21 The divalent group represented by formula (R3-1) is selected such that the number of carbon atoms falls within the range of 6 to 22.
[0067] Similarly, L in equation (R3-2) 21 , m 33 , m 34 , R 22 , R 23 , p 22 and p 23 The divalent group represented by formula (R3-2) is selected such that the number of carbon atoms falls within the range of 12 to 22. X3 is defined in the same way as X1 in equation (1), and the preferred mode is also the same.
[0068] The content ratio of the repeating structural unit of formula (3) to all the repeating structural units constituting the polyimide resin is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited, and it may exceed 0 mol%. From the viewpoint of improving heat resistance, the content ratio is preferably 5 mol% or more, more preferably 7 mol% or more. On the other hand, from the viewpoint of maintaining crystallinity, it is preferably 20 mol% or less, more preferably 15 mol% or less.
[0069] The polyimide resin may further contain a repeating structural unit represented by the following formula (4).
Chemical formula
[0070] There is no particular limitation on the terminal structure of the polyimide resin, but it is preferably a linear aliphatic group having 5 to 14 carbon atoms at the terminal. The linear aliphatic group may be saturated or unsaturated, and may be linear or branched. When the polyimide resin has the above specific group at the terminal, it has excellent heat aging resistance.
[0071] Examples of saturated chain aliphatic groups having 5 to 14 carbon atoms include n-pentyl group, n-hexyl group, n-heptyl group, n-octyl group, n-nonyl group, n-decyl group, n-undecyl group, lauryl group, n-tridecyl group, n-tetradecyl group, isopentyl group, neopentyl group, 2-methylpentyl group, 2-methylhexyl group, 2-ethylpentyl group, 3-ethylpentyl group, isooctyl group, 2-ethylhexyl group, 3-ethylhexyl group, isononyl group, 2-ethyloctyl group, isodecyl group, isododecyl group, isotridecyl group, isotetradecyl group, and so on. Examples of unsaturated linear aliphatic groups having 5 to 14 carbon atoms include 1-pentenyl group, 2-pentenyl group, 1-hexenyl group, 2-hexenyl group, 1-heptenyl group, 2-heptenyl group, 1-octenyl group, 2-octenyl group, nonenyl group, decenyl group, dodecenyl group, tridecenyl group, and tetradecenyl group. In particular, the above-mentioned linear aliphatic group is preferably a saturated linear aliphatic group, and more preferably a saturated linear aliphatic group. Furthermore, from the viewpoint of obtaining heat aging resistance, the above-mentioned linear aliphatic group preferably has 6 or more carbon atoms, more preferably 7 or more carbon atoms, even more preferably 8 or more carbon atoms, preferably 12 or fewer carbon atoms, more preferably 10 or fewer carbon atoms, and even more preferably 9 or fewer carbon atoms. The above-mentioned linear aliphatic group may be just one type or two or more types.
[0072] The above-mentioned linear aliphatic group is particularly preferably at least one selected from n-octyl group, isooctyl group, 2-ethylhexyl group, n-nonyl group, isononyl group, n-decyl group, and isodecyl group; more preferably at least one selected from n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, and isononylamine; and most preferably at least one selected from n-octyl group, isooctyl group, and 2-ethylhexyl group.
[0073] Furthermore, from the viewpoint of heat aging resistance, it is preferable that the polyimide resin has only linear aliphatic groups having 5 to 14 carbon atoms at its ends, in addition to terminal amino groups and terminal carboxyl groups. If other groups are present at the ends, their content is preferably 10 mol% or less, more preferably 5 mol% or less, relative to the linear aliphatic groups having 5 to 14 carbon atoms. From the viewpoint of exhibiting excellent heat aging resistance, the content of the above-mentioned chain-like aliphatic groups having 5 to 14 carbon atoms in the polyimide resin is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and even more preferably 0.2 mol% or more, based on 100 mol% of the total repeating structural units in the polyimide resin. Furthermore, in order to ensure a sufficient molecular weight and obtain good mechanical properties, the content of the above-mentioned chain-like aliphatic groups having 5 to 14 carbon atoms in the polyimide resin is preferably 10 mol% or less, more preferably 6 mol% or less, and even more preferably 3.5 mol% or less, based on 100 mol% of the total repeating structural units in the polyimide resin. The content of the above-mentioned chain-like aliphatic groups having 5 to 14 carbon atoms in the polyimide resin can be determined by depolymerizing the polyimide resin.
[0074] (Conditions for polyimide resin) The polyimide resin used in the present invention is characterized by satisfying the following conditions (a), (b), and (c). Condition (a): Melting point (Tm) is between 280°C and 345°C. Condition (b): Glass transition temperature (Tg) is 150°C or higher and 200°C or lower. Condition (c): The amount of heat from the crystallization exothermic peak observed when the material is cooled at a rate of 20°C / min after melting, as measured by differential scanning calorimeter, is 17.0 mJ / mg or greater.
[0075] Polyimide resins offer a good balance between spinnability and heat resistance by satisfying all of the above conditions (a) to (c). Furthermore, in general, crystalline resins with a high degree of crystallinity, i.e., those with a high heat generation during crystallization, exhibit good fluidity when heated above their melting point, resulting in improved spinnability. Generally, the crystalline portion of a crystalline resin melts when heated above its melting point, causing a rapid decrease in viscosity. Therefore, resins with a higher crystalline portion exhibit improved fluidity at temperatures above their melting point. In other words, polyimide resins that satisfy both conditions (a) and (c) also possess good spinnability.
[0076] With respect to condition (a), the melting point (Tm) of the polyimide resin is 280°C or higher, preferably 290°C or higher, more preferably 300°C or higher, from the viewpoint of exhibiting heat resistance, and 345°C or lower, preferably 340°C or lower, more preferably 335°C or lower, and even more preferably 330°C or lower, from the viewpoint of high spinnability. If the melting point (Tm) of polyimide resin is below 280°C, its heat resistance is insufficient, and if it exceeds 345°C, its spinnability is insufficient.
[0077] Regarding condition (b), the glass transition temperature (Tg) of the polyimide resin is preferably 150°C or higher from the viewpoint of heat resistance, and preferably higher than the Tg of polyetheretherketone (PEEK), which is highly regarded as a super engineering plastic (153°C). That is, the glass transition temperature (Tg) of the polyimide resin is preferably 160°C or higher, more preferably 170°C or higher, and even more preferably 180°C or higher, and from the viewpoint of exhibiting high spinnability, it is preferably 195°C or lower, more preferably 190°C or lower, and even more preferably 185°C or lower. If the glass transition temperature (Tg) of polyimide resin is below 150°C, its heat resistance is low and insufficient. The melting point and glass transition temperature of polyimide resin can both be measured using a differential scanning calorimeter, and specifically, they can be measured by the method described in the examples.
[0078] Furthermore, regarding condition (c), the crystallization heat observed when the polyimide resin is melted and then cooled at a cooling rate of 20°C / min is a value measured by a differential scanning calorimeter. Specifically, a sample of polyimide resin is taken, and the resin is heated at a constant rate using a differential scanning calorimeter to melt it. Then, the amount of exothermic crystallization is calculated from the area of the crystallization exothermic peak observed when the resin is cooled at a predetermined rate.
[0079] In the polyimide resin used in the present invention, the heat of crystallization is 17.0 mJ / mg or more. If the heat of crystallization is less than 17.0 mJ / mg, sufficient fiber processing characteristics cannot be obtained. From the viewpoint of obtaining sufficient fiber processing characteristics, the heat of crystallization is preferably 18.0 mJ / mg or more, more preferably 18.5 mJ / mg or more. The upper limit of the heat of crystallization is not particularly limited, but is usually 45.0 mJ / mg or less.
[0080] The logarithmic viscosity of a 0.5% by mass concentrated sulfuric acid solution of the polyimide resin used in the present invention at 30°C is preferably in the range of 0.2 to 2.0 dL / g, and more preferably in the range of 0.3 to 1.8 dL / g. If the logarithmic viscosity is 0.2 dL / g or higher, sufficient mechanical strength can be obtained when the material is fiberized, and if it is 2.0 dL / g or lower, the spinnability and handling properties are good.
[0081] The logarithmic viscosity μ is determined by measuring the flow time of concentrated sulfuric acid and the polyimide resin solution at 30°C using a Cannon-Fenske viscometer, and then using the following formula. μ = ln(ts / t0) / C t0: Time of flow of concentrated sulfuric acid ts: Flow time of the polyimide resin solution C: 0.5 (g / dL)
[0082] The polyimide resin used in this invention preferably has a heat deflection temperature (HDT) of 160°C to 180°C at a load of 1.80 MPa, and a specific gravity of 1.24 g / cm³. 3 More than 1.34g / cm 3 The following are preferred, and it is preferable that the water absorption rate (23°C, 24 hours) is 0.3% or less (all according to the JIS test method at the time of application).
[0083] [Method for producing polyimide resin] Polyimide resins can be produced by reacting a tetracarboxylic acid component with a diamine component. The tetracarboxylic acid component contains a tetracarboxylic acid and / or a derivative thereof that includes at least one aromatic ring, and the diamine component contains a diamine and a chain-like aliphatic diamine that include at least one alicyclic hydrocarbon structure.
[0084] Tetracarboxylic acids containing at least one aromatic ring are preferably compounds in which four carboxyl groups are directly bonded to the aromatic ring, and may contain alkyl groups in their structure. Tetracarboxylic acids are also preferably those with 6 to 26 carbon atoms. Preferred tetracarboxylic acids include pyromellitic acid, 2,3,5,6-toluenetetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, and 1,4,5,8-naphthalenetetracarboxylic acid. Among these, pyromellitic acid is more preferred.
[0085] Examples of tetracarboxylic acid derivatives containing at least one aromatic ring include anhydrides or alkyl esters of tetracarboxylic acids containing at least one aromatic ring. Tetracarboxylic acid derivatives are preferably those having 6 to 38 carbon atoms. Examples of tetracarboxylic acid anhydrides include pyromellitic monoanhydride, pyromellitic dianhydride, 2,3,5,6-toluenetetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid dianhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, and 1,4,5,8-naphthalenetetracarboxylic acid dianhydride. Examples of alkyl esters of tetracarboxylic acids include dimethyl pyromelliate, diethyl pyromelliate, dipropyl pyromelliate, diisopropyl pyromelliate, 2,3,5,6-toluenetetracarboxylate dimethyl, 3,3',4,4'-diphenylsulfonetetracarboxylate dimethyl, 3,3',4,4'-benzophenonetetracarboxylate dimethyl, 3,3',4,4'-biphenyltetracarboxylate dimethyl, and 1,4,5,8-naphthalenetetracarboxylate dimethyl. In the alkyl esters of the above tetracarboxylic acids, the number of carbon atoms in the alkyl group is preferably 1 to 3. A tetracarboxylic acid and / or derivative thereof containing at least one aromatic ring may be used as at least one compound selected from the above, or as a combination of two or more compounds.
[0086] The diamine containing at least one alicyclic hydrocarbon structure preferably has 6 to 22 carbon atoms, for example, 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 4,4'-methylenebis(2-methylcyclohexylamine), carbonediamine, limonenediamine, isophoronediamine, norbornanediamine, bis(aminomethyl)tricyclo[5.2.1.0 2,6] Decane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylpropane, etc. are preferred. These compounds may be used individually or in combination of two or more compounds selected from them. Of these, 1,3-bis(aminomethyl)cyclohexane can be preferably used. Diamines containing alicyclic hydrocarbon structures generally have structural isomers, but the cis / trans ratio is not limited.
[0087] The linear aliphatic diamine may be linear or branched, and the number of carbon atoms is preferably 5 to 16, more preferably 6 to 14, and even more preferably 7 to 12. Furthermore, if the number of carbon atoms in the chain portion is 5 to 16, it may contain ether bonds between them. Examples of preferred linear aliphatic diamines include 1,5-pentamethylenediamine, 2-methylpentane-1,5-diamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonameethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, and 2,2'-(ethylenedioxy)bis(ethyleneamine).
[0088] The linear aliphatic diamine may be used individually or in combination with others within the scope of the present invention. Of these, linear aliphatic diamines having 8 to 10 carbon atoms are preferably used, and at least one selected from 1,8-octamethylenediamine and 1,10-decamethylenediamine is particularly preferably used.
[0089] When manufacturing polyimide resin, the molar ratio of the amount of diamine containing at least one alicyclic hydrocarbon structure to the total amount of diamine containing at least one alicyclic hydrocarbon structure and linear aliphatic diamine is preferably 20 mol% or more and less than 40 mol%. The molar amount is preferably 25 mol% or more, more preferably 30 mol% or more, and even more preferably 32 mol% or more, and from the viewpoint of exhibiting excellent moldability, it is preferably less than 40 mol%, more preferably 38 mol% or less, even more preferably 37 mol% or less, and even more preferably 36 mol% or less.
[0090] Furthermore, the above-mentioned diamine component may contain a diamine containing at least one aromatic ring. The number of carbon atoms of the diamine containing at least one aromatic ring is preferably 6 to 22, and examples include orthoxylylenediamine, metaxylylenediamine, paraxylylenediamine, 1,2-diethynylbenzenediamine, 1,3-diethynylbenzenediamine, 1,4-diethynylbenzenediamine, 1,2-diaminobenzene, 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, α,α'-bis(4-aminophenyl)1,4-diisopropylbenzene, α,α'-bis(3-aminophenyl)-1,4-diisopropylbenzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,6-diaminonaphthalene, 1,5-diaminonaphthalene, and the like.
[0091] In the above, the molar ratio of the amount of diamine containing at least one aromatic ring to the total amount of diamine containing at least one alicyclic hydrocarbon structure and linear aliphatic diamine is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited and should be greater than 0 mol%. From the viewpoint of improving heat resistance, the molar ratio is preferably 5 mol% or more, more preferably 10 mol% or more, while from the viewpoint of maintaining crystallinity, it is preferably 20 mol% or less, more preferably 15 mol% or less. Furthermore, from the viewpoint of reducing the coloration of the polyimide resin, the molar ratio is preferably 12 mol% or less, more preferably 10 mol% or less, even more preferably 5 mol% or less, and even more preferably 0 mol%.
[0092] When manufacturing polyimide resin, the preferred ratio of tetracarboxylic acid component to diamine component is 0.9 to 1.1 moles of diamine component per mole of tetracarboxylic acid component.
[0093] The polymerization method for producing polyimide resin can be any known polymerization method for producing polyimide resin, and is not particularly limited, but examples include solution polymerization, melt polymerization, solid-phase polymerization, and suspension polymerization. Among these, suspension polymerization under high-temperature conditions using an organic solvent is particularly preferred. When performing suspension polymerization under high-temperature conditions, polymerization is preferably carried out at 150°C or higher, and more preferably at 180 to 250°C. The polymerization time is appropriately changed depending on the monomer used, but it is preferably carried out for about 0.1 to 6 hours.
[0094] A method for producing polyimide resin preferably includes a step of reacting a tetracarboxylic acid component and a diamine component in the presence of a solvent containing an alkylene glycol-based solvent represented by the following formula (I). This allows for obtaining a powdered polyimide resin.
[0095] This manufacturing method is preferable because, when a sieving test is performed according to the method of JIS K0069, polyimide resin powder with a passing rate of 90% by mass or more through a sieve with a nominal mesh opening of 500 μm for JIS testing is obtained, and polyimide resin powder with particle size distributions measured by a laser diffraction light scattering particle size analyzer, where D10 is 8 to 100 μm, D50 is 12 to 250 μm, and D90 is 20 to 500 μm, can be easily obtained. [ka] (Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, Ra2 is a linear alkylene group having 2 to 6 carbon atoms, and n is an integer from 1 to 3.) To obtain a uniform powdered polyimide resin, it is desirable that the solvent possesses two properties in a one-pot reaction: (1) uniformly dissolves the polyamic acid or uniformly disperses the nylon salt, and (2) does not dissolve or swell the polyimide resin at all. Solvents containing alkylene glycol-based solvents represented by the above formula (I) generally satisfy these two properties. From the viewpoint of enabling polymerization reactions at high temperatures under atmospheric pressure, alkylene glycol-based solvents preferably have a boiling point of 140°C or higher, more preferably 160°C or higher, and even more preferably 180°C or higher.
[0096] In formula (I), Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group or an ethyl group. In formula (I), Ra2 is a linear alkylene group having 2 to 6 carbon atoms, preferably a linear alkylene group having 2 to 3 carbon atoms, and more preferably an ethylene group.
[0097] In equation (I), n is an integer between 1 and 3, preferably 2 or 3. Specific examples of alkylene glycol solvents include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether (also known as 2-(2-methoxyethoxy)ethanol), triethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether (also known as 2-(2-ethoxyethoxy)ethanol), ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol, 1,3-propanediol, and the like. These solvents may be used individually, or two or more solvents selected from these may be used in combination. Of these solvents, 2-(2-methoxyethoxy)ethanol, triethylene glycol monomethyl ether, 2-(2-ethoxyethoxy)ethanol, and 1,3-propanediol are preferred, and 2-(2-methoxyethoxy)ethanol and 2-(2-ethoxyethoxy)ethanol are preferred.
[0098] The content of the alkylene glycol-based solvent in the solvent is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 75% by mass or more, and particularly preferably 95% by mass or more. The solvent may consist solely of the alkylene glycol-based solvent.
[0099] When the solvent includes alkylene glycol-based solvents and other solvents, specific examples of "other solvents" include water, benzene, toluene, xylene, acetone, hexane, heptane, chlorobenzene, methanol, ethanol, n-propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N-methylcaprolactam, hexameth Examples include phosphoramide, tetramethylene sulfone, dimethyl sulfoxide, o-cresol, m-cresol, p-cresol, phenol, p-chlorophenol, 2-chloro-4-hydroxytoluene, diglyme, triglyme, tetraglyme, dioxane, γ-butyrolactone, dioxolane, cyclohexanone, cyclopentanone, dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, dibromomethane, tribromomethane, 1,2-dibromoethane, and 1,1,2-tribromoethane. These solvents may be used individually or in combination of two or more selected solvents.
[0100] A suitable method for producing polyimide resin is, for example, to separately prepare a solution (a) containing a tetracarboxylic acid component in a solvent containing the alkylene glycol-based solvent, and a solution (b) containing a diamine component in a solvent containing the alkylene glycol-based solvent, then to prepare a solution (c) containing polyamic acid by adding solution (b) to solution (a) or by adding solution (a) to solution (b), and then to synthesize polyimide resin by imidizing the polyamic acid by heating solution (c).
[0101] The reaction between the tetracarboxylic acid component and the diamine component can be carried out under either atmospheric pressure or pressurized pressure, but it is preferable to carry it out under atmospheric pressure because it does not require a pressure-resistant container.
[0102] When using an end capping agent, it is preferable to mix solution (a) and solution (b), add the end capping agent to this mixture to prepare a solution (c) containing polyamic acid, and then heat solution (c). More preferably, it is preferable to add the end capping agent after adding solution (b) to solution (a) to prepare a solution (c) containing polyamic acid, and then heat solution (c).
[0103] Furthermore, from the viewpoint of reducing the amount of by-products in the polyimide resin, it is preferable that the method for producing the polyimide resin includes a tetracarboxylic acid component containing a tetracarboxylic acid dianhydride, and that the step of reacting the tetracarboxylic acid component with the diamine component includes a step (i) of preparing a solution (c) containing polyamic acid by adding a solution (b) containing a diamine component and an alkylene glycol-based solvent to a solution (a) containing a tetracarboxylic acid component and an alkylene glycol-based solvent, and a step (ii) of obtaining the polyimide resin by heating the solution (c) to imide the polyamic acid, wherein in step (i), it is preferable that the amount of diamine component added per unit time per 1 mol of tetracarboxylic acid component is 0.1 mol / min or less when adding solution (b) to solution (a).
[0104] Furthermore, the polyimide resin used in the present invention may contain, as needed, any components such as matting agents, nucleating agents, plasticizers, antistatic agents, color inhibitors, gelation inhibitors, and resin modifiers, provided that their properties are not impaired.
[0105] Furthermore, the polyimide resin may be a resin composition that incorporates at least one additive selected from fillers, flame retardants, colorants, sliding properties improvers, antioxidants, and conductive agents, in order to utilize the inherent physical properties of the polyimide resin while imparting desired performance.
[0106] The polyimide resin used in the present invention and the polyimide resin composition containing it can be melt-spun at a relatively low temperature of 290 to 350°C, thus enabling the easy and stable production of polyimide fibers. The melt-spinning temperature is preferably 310°C to 345°C.
[0107] [Melt spinning of polyimide resin] Next, we will explain the melt spinning method for polyimide resin. The polyimide resin obtained above, having a melting point (Tm) of 280°C to 345°C and a glass transition temperature (Tg) of 150°C to 200°C, is dried to obtain a dried polyimide resin with a moisture content of 50 ppm or less (drying step). Subsequently, the dried polyimide resin is melted and extruded from the die using extruder 1 under the following conditions (a) to (c) to form spun yarn (spinning process). Condition (a): Shear rate of dry polyimide resin at 360°C is 100 s. -1 The melt viscosity is 1050 Pa·s or less. Condition (b): Spinning temperature is between the melting point of the polyimide resin + 20°C and 380°C. Condition (c): Melt residence time is 12 minutes or less. Then, the spun yarn extruded from the die is bundled into a single filament (bundling process). Furthermore, the filaments obtained in the focusing process are wound onto a tube (winding process). Furthermore, a subsequent stretching process may be performed in which the bundled filaments are stretched while being heated at a temperature between 150°C and 300°C. Furthermore, as a subsequent process, the bundled filaments may be heated to a temperature between 150°C and 300°C, followed by a heat treatment process. The following provides a detailed explanation of each step.
[0108] (drying process) The polyimide resin obtained above is stored in a vacuum dryer and dried at a temperature of 100°C to 200°C for 10 to 30 hours. The moisture content of the polyimide resin shall be 50 ppm or less by means of a drying process. The moisture content of the polyimide resin is preferably 30 ppm or less, and more preferably 25 ppm or less. This can prevent the generation of bubbles during spinning. The polyimide resin may be in pellet form or powder form. In particular, it is preferably in pellet form. Drying may be carried out under a nitrogen flow, or fluidized drying may be performed using a tumbler or the like. When the moisture content of the polyimide resin exceeds 50 ppm, gas is generated by moisture during melting, and problems such as voids being contained in the spun yarn or gel-like insoluble substances being generated, making stable spinning impossible, occur, so it is not preferable.
[0109] (Spinning process) The melt extrusion of the polyimide resin in the present invention may be any suitable for melt spinning, and known methods may be used. For example, the polyimide resin is pelletized and melt extruded by an extruder-type extruder. FIG. 1 shows an example of a method for producing polyimide fibers by melt extruding a polyimide resin from an extruder 1 and melt spinning. The molten resin extruded from the extruder 1 passes through a pipe, is sent to a spinning head, is metered by a known metering device such as a gear pump 2, passes through a filter in a spinning pack 3, and then enters a spinneret 3a.
[0110] The spinning temperature in the present invention is the temperature of the molten resin from the pipe to the spinneret 3a, and is preferably not less than the melting point temperature of the polyimide resin and not more than 400 °C, and more preferably less than 390 °C. If the spinning temperature is lower than the lower limit, problems such as an increase in filtration pressure occur, and if it exceeds the upper limit, the quality of the fiber may deteriorate due to the influence of thermal decomposition. A suitable spinning temperature in the present invention is not less than the melting point + 20 °C and not more than 380 °C. Preferably, it is not less than 320 °C and not more than 370 °C, and most preferably not less than 340 °C and not more than 360 °C.
[0111] The melt viscosity of the polyimide resin in the present invention is at a shear rate of 100 s at 360 °C -1In this case, it is preferably 700 Pa·s or more, more preferably 750 Pa·s or more, and even more preferably 800 Pa·s or more. Furthermore, the melt viscosity of the polyimide resin in this invention is determined by a shear rate of 100 s at 360°C. -1 In this case, the pressure is 1050 Pa·s or less, preferably 1000 Pa·s or less, and more preferably 900 Pa·s or less. If the melt viscosity exceeds the upper limit, the spinnability during melt spinning deteriorates, and if the melt viscosity exceeds the lower limit, stable spinning becomes difficult.
[0112] In this invention, the shear rate in the spinneret hole is 700 sec. -1 Over 90,000 seconds -1 Preferably, the following is the case: 1,000 sec -1 Over 80,000 seconds -1 It is more preferable to do the following, for 3,000 seconds -1 Over 60,000 seconds -1 It is even more preferable to do the following: 5,000 sec -1 Over 50,000 seconds -1 The following is more preferable. The shear rate γ referred to in this invention is determined by the following formula. γ = 4Q / πr 3 (where r is the radius of the spinneret hole (cm) and Q is the polymer discharge rate per hole (cm) 3 / sec)) Within the above range, the fiber orientation is sufficient, making it easier to obtain fine-denier fibers and thus easier to achieve the desired physical properties.
[0113] In the present invention, the residence time of the molten resin is 12 minutes or less, preferably 10 minutes or less, and more preferably 9 minutes or less. In this invention, the residence time is the total time from when the resin is fed into the extruder 1 until it is discharged from the spinneret 3a. If the residence time is too long, the melt viscosity decreases due to the effects of thermal decomposition, bubbles are generated, the quality of the fibers deteriorates, and yarn breakage occurs.
[0114] In the present invention, the pore diameter D of the spinneret 3a is preferably 0.09 mm or more and 0.70 mm or less, and more preferably 0.12 mm or more and 0.45 mm or less. Furthermore, by installing a heater and a heat-retaining cylinder directly below the spinneret 3a, the diameter of the extruded fibers is stabilized, and changes in the surface temperature of the spinneret and the ambient temperature below the spinneret are suppressed by the outside air. This results in uniform finening due to the draft, and stable spinning without yarn breakage or fluffing.
[0115] In the present invention, the linear velocity of the spun fiber in the spinneret 3a is preferably 5.0 m / min or more and 50.0 m / min or less, and more preferably 10.0 m / min or more and 40.0 m / min or less. In this invention, the shear rate in the spinneret hole is 700 sec. -1 Over 90,000 seconds -1 Preferably, the following is the case: 1,000 sec -1 Over 80,000 seconds -1 It is more preferable to do the following, for 3,000 seconds -1 Over 60,000 seconds -1 It is even more preferable to do the following: 5,000 sec -1 Over 50,000 seconds -1 The following is more preferable. Furthermore, the focusing position is preferably 7 cm to 300 cm, and more preferably 20 cm to 200 cm. Furthermore, the winding speed (spinning speed) in the present invention is preferably 300 m / min or more and 3500 m / min, more preferably 300 m / min or more and 1700 m / min or less, and even more preferably 400 m / min or more and 1600 m / min or less. Furthermore, the ratio of winding speed to linear speed is preferably between 40 and 1600 times. This makes it possible to produce high-quality polyimide fibers using the melt spinning method.
[0116] (Focusing process) The spun yarn, extruded from the spinneret 3a, is coated with a predetermined oil by an oil application device and then bundled into a single filament. The polyimide fiber of the present invention is a filament, and may be either a monofilament or a multifilament. In the case of a multifilament, it is preferable that the number of single filaments be 6 or more. If the number of single filaments is less than 6, the strength of the multifilament itself will be weaker, making it difficult to stretch and wind it smoothly through the process, which may lead to yarn breakage and a decrease in productivity. Furthermore, the cross-sectional shape of each single filament is not particularly limited; it may be a round cross-section, or an irregular cross-section depending on the purpose and application.
[0117] (winding process) The polyimide fibers, which have become multifilaments after the bundling process, are then taken up by the first godet roll 4 and the second godet roll 5 and wound onto the winding bobbin 6. The winding speed is preferably 300 m / min to 3500 m / min, more preferably 300 m / min to 1700 m / min, and even more preferably 400 m / min to 1600 m / min. The spinning tension measured between the second godet roll 5 and the winding bobbin 6 is preferably between 4.7 cN and 47 cN. If the tension is less than 4.7 cN, the fibers will slacken, causing the yarn to wrap around the second godet roll 5 or resulting in a deformation of the winding bobbin 6. In this invention, the spinning tension refers to the tension applied when the yarn is wound onto the winding bobbin 6.
[0118] (Physical properties of polyimide fibers) The polyimide fibers obtained as described above are preferably given the following physical properties by adjusting the shear rate γ, pore size D, winding speed ratio, etc. In other words, the fineness of the polyimide fiber obtained by melt spinning is preferably 50 dtex or more as a total fineness, and preferably 100 dtex or more. As a single yarn fineness, it is preferably 1 dtex or more and about 12 dtex. Furthermore, the tensile strength of the polyimide fiber is preferably 1.5 cN / dtex or higher, more preferably 2.0 cN / dtex or higher, and even more preferably 2.2 cN / dtex or higher. Moreover, the variation in the tensile strength of the polyimide fiber is preferably less than ±0.3 cN / dtex, and more preferably within ±0.2 cN / dtex. Furthermore, the elongation at break of the polyimide fiber is preferably 10% to 90%, and more preferably 20% to 80%. Moreover, the elongation at break of the stretched polyimide fiber is more preferably 20% to 50%, and the elongation at break of the unstretched polyimide fiber is more preferably 50% to 80%. Furthermore, the strength of the polyimide fiber at 10% elongation (10%SS) is preferably 1.5 cN / dtex or more and 3.5 cN / dtex or less. Furthermore, the elastic modulus of the polyimide fiber is preferably 20 cN / dtex or higher. In the present invention, however, the upper limit is preferably 70 cN / dtex or lower. This makes it possible to produce polyimide fibers that are high in strength and also have excellent properties such as dimensional stability and thermal stability.
[0119] (Post-process: stretching process) The polyimide fibers of the present invention can be further stretched by a stretching process. The stretching process may be performed immediately after the bundling process, or it may be performed after the fibers have been wound in the winding process. In the drawing process, the multifilament may be preheated first at a temperature between Tg-100°C and Tg-30°C, which is the glass transition temperature of the polyimide resin. The preheating method is not limited, but it can be performed using a heated rotating roller or the like. Next, it is preferable to heat the polyimide resin at a temperature between Tg°C and Tg+100°C, and take up the polyimide resin with a take-up roller at a temperature between Tg-50°C and Tg+50°C, thereby stretching it to a stretch ratio of 1.2 to 5.0 times. If the heating temperature is below the Tg of the polyimide, yarn breakage is likely to occur during the stretching process, and if it exceeds Tg+100°C, the yarn will soften, and may break due to inability to withstand the stretching stress. Next, the heated multifilament is further stretched while being taken up by a take-up roller. The temperature of the take-up roller is preferably between Tg -50°C and Tg +50°C of the polyimide resin. The speed of the take-up roller should be 5.0 times or less. On the other hand, if the stretch ratio exceeds 5.0 times, yarn breakage occurs frequently during stretching, operability deteriorates, and the strength of the resulting fibers decreases, or fibers with single-fiber breakage occur.
[0120] (Post-process:) To further promote the crystallization of the polyimide fibers obtained as described above, they may be subjected to heat treatment for a certain period of time while under tension. The heating process is preferably carried out immediately after the stretching, and may be performed under an inert atmosphere such as nitrogen gas.
[0121] [Applications of polyimide fibers] Applications of the polyimide fibers of the present invention include bag filters and sports applications (life ropes, yacht sails), among others. For example, as it is a crystallized polyimide fiber, it can be used as a material for various industrial applications. For instance, it can be used as a long fiber, or woven into fabric, or as a short fiber into a nonwoven fabric, and is useful as a material for heat-resistant clothing, insulation materials, heat-resistant filters, insulating paper, and printed circuit board materials.
[0122] In particular, the polyimide fibers of the present invention have a low dielectric loss tangent of about 0.004 (10 GHz), excellent heat resistance (especially dimensional stability at high temperatures), and can be spun into finer fibers, making them suitable for use in thin and miniaturized wiring boards for high-speed communication. In this case, it is preferable that the polyimide fibers have a single-fiber fineness of 2 dtex or less. This allows for the wiring board to be made thinner and miniaturized. Furthermore, the polyimide fibers of the present invention may be processed into a fabric-like form (yarn-like, nonwoven fabric-like) and used as an impregnation material for prepregs (semi-cured resin materials). The wiring board may have one layer containing polyimide fibers or multiple layers. Furthermore, the polyimide fibers of the present invention have excellent processability, allowing them to be blended with multiple types of fibers to form commingled fibers or processed into fiber-reinforced plastics. Additionally, the polyimide fibers of the present invention can be used as short fibers to form nonwoven fabrics, nonwoven laminates, or fiber-reinforced plastics. Processed polyimide fiber products obtained in this way are lightweight due to their excellent strength and can withstand harsh environments, making them suitable for applications in aerospace, automotive, and other fields (structures, engine parts, etc.). [Examples]
[0123] The present invention will now be described in more detail with reference to examples, but the present invention is not limited thereto.
[0124] <Method for measuring polyimide resin> The melting point Tm, glass transition temperature Tg, crystallization temperature Tc, and heat generation during crystallization of the polyimide resin were measured using a differential scanning calorimeter (DSC-6220, manufactured by SII Nanotechnology Co., Ltd.). Under a nitrogen atmosphere, a polyimide resin was subjected to the following thermal history: first heating (heating rate 10°C / min), followed by cooling (cooling rate 20°C / min), and then a second heating (heating rate 10°C / min). The melting point was determined by reading the peak value of the endothermic peak observed during the second heating cycle. The glass transition temperature was determined by reading the value observed during the second heating cycle. The crystallization temperature was determined by reading the peak value of the exothermic peak observed during cooling. The heat of crystallization (mJ / mg) was calculated from the area of the crystallization heat of the peak observed during the cooling process described above.
[0125] <Examples of polyimide resin manufacturing> A method for producing a polyimide resin according to one embodiment is shown. The method for producing a polyimide resin of the present invention is not limited to the polyimide resin production examples shown below. In a 2 L separable flask equipped with a Dean-Stark apparatus, a Liebig condenser, a thermocouple, and four paddle blades, 600 g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Emulsifier Co., Ltd.) and 218.58 g (1.00 mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced. After nitrogen flow, the mixture was stirred at 150 rpm to obtain a homogeneous suspension solution. Meanwhile, in a 500 mL beaker, 49.42 g (0.347 mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd.) and 93.16 g (0.645 mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250 g of 2-(2-methoxyethoxy)ethanol to prepare a mixed diamine solution.
[0126] This mixed diamine solution is added gradually using a plunger pump. Nitrogen flow is maintained throughout the addition of the mixed diamine solution, and the impeller speed is set to 250 rpm. After the addition is complete, 130 g of 2-(2-methoxyethoxy)ethanol and 1.934 g (0.0149 mol) of n-octylamine (manufactured by Kanto Chemical Co., Ltd.), which is a terminal encapsulant, are added and the mixture is stirred further. At this stage, a pale yellow polyamic acid solution is obtained. Next, the stirring speed is set to 200 rpm, and the polyamic acid solution in the 2 L separable flask is heated to 190°C. During the heating process, precipitation of polyimide resin powder and dehydration due to imidization are observed between 120 and 140°C. After holding at 190°C for 30 minutes, the mixture is allowed to cool to room temperature and filtered. The obtained polyimide resin powder is washed with 300 g of 2-(2-methoxyethoxy)ethanol and 300 g of methanol, filtered, and then dried in a dryer at 180°C for 10 hours to obtain 316 g of polyimide resin powder (in the IR spectrum of the polyimide resin, ν(C=O)1768, 1697(cm) -1 Characteristic absorption of the imide ring was observed, and the logarithmic viscosity was 0.96 dL / g).
[0127] <Method for measuring polyimide fibers> The characteristic values in the examples were measured using the following method. 1. Melt viscosity The melt viscosity was measured using a Capillograph® (manufactured by Toyo Seiki Seisakusho, Model 1B), with a nozzle measuring 0.5 mm in diameter and 5 mm in length. The sample was heated to 360°C or spinning temperature, and the sample passed through the nozzle for 100 seconds. -1 It is defined as the viscosity when a shear rate is applied.
[0128] 2. Breaking strength, breaking elongation, elastic modulus, and variation in breaking strength 1) Tensile test (strength, elongation, 10% SS, modulus of elasticity) In accordance with the standard time test of JIS L 1013 (2010), a Shimadzu AGS-500NX tensile testing machine was used to determine the breaking strength, breaking elongation, and modulus of elasticity (initial tensile resistance) with a sample length of 200 mm and a tensile speed of 200 mm / min. The average of 10 points was used. The strength at 10% elongation was defined as 10%SS. The difference between the maximum and minimum values when the breaking strength was measured 50 times was defined as the breaking strength variability.
[0129] <Evaluation Method for Polyimide Fibers> 1. Evaluation of spinning status The spinning process after more than two hours was evaluated as follows. ○ Spinning was performed stably without any thread breakage. △ The yarn broke during the 2-hour spinning process. (Air bubbles: While it is possible to wrap the material, air bubbles, likely due to resin degradation, form directly beneath the nozzle, causing thread breakage and uneven strength.) Unable to wind: Frequent thread breakage prevented winding (either due to resin degradation causing thread breakage or increased filtration pressure making winding impossible). Spinning impossible: It was simply impossible to wind the yarn.
[0130] 2.250℃ dry heat shrinkage rate [Dry heat shrinkage rate] The dry heat shrinkage rate (%) was determined at 250°C using JIS-L1013 8.18.2 b) Filament shrinkage rate (Method B).
[0131] (Example 1) <Polyimide resin melt spinning process> As the polyimide resin, we used chips of Surprim® T O65 (manufactured by Mitsubishi Gas Chemical Company, Inc.). This polyimide resin has a melting point of 323°C, a glass transition temperature of 185°C, a crystallization heat of 23.7 mJ / mg, and a shear rate of 100 s at 360°C. -1 The melt viscosity was 1000 Pa·s. These chips were dried in a vacuum dryer at 140°C for 20 hours. The moisture content is shown in Table 1.
[0132] The chips were melted and extruded in extruder 1, weighed by gear pump 2, and supplied to spinning pack 3. The resin was melted while being heated using extruder 1. The spinning temperature was 370°C and the melt residence time was 7 minutes, and the material was extruded from spinneret 3a to form fibers. The spinneret had 24 holes, the linear velocity when extruded from spinneret 3a was 11.2 m / min, and the shear rate was 5976 s. -1 That was the case.
[0133] The spun yarn extruded from the spinneret 3a was lubricated once it had solidified, and then bundled into a single multifilament 30 cm directly below the spinneret. This was then wound onto a paper tube using a winder at a winding speed (spinning speed) of 650 m / min to obtain a polyimide fiber of 220 dtex / 24 f. The obtained physical properties and spinnability evaluation results are shown in Table 2.
[0134] (Example 2) Polyimide fibers were obtained in the same manner as in Example 1, except that the spinning conditions were as shown in Table 1. (Example 3) The spinning conditions were as shown in Table 1, the multifilament bundle was set to 100 cm directly below the spindle, and the shear rate was 31,857 s. -1 Except for the above, melt spinning was carried out in the same manner as in Example 1 to obtain polyimide fibers. The wound polyimide fibers were placed on a roller and unwound, then guided to a roll heater heated to 185°C, and then stretched to a stretch ratio of 2.3 times via a plate heater heated to 210°C. Finally, the fibers were wound onto a paper tube using a winder to obtain stretched yarn.
[0135] (Comparative Examples 1-8) The spinning process was carried out in the same manner as in Example 1, except that the spinning conditions were as shown in Table 1. Comparative Examples 1-5 had long residence times and could not be spun. Comparative Example 6 had a high moisture content, which caused air bubbles to form and prevented it from becoming thread. In Comparative Example 7, the spinning temperature was too high, resulting in excessively low viscosity, which caused air bubbles to form and prevented the material from becoming yarn. Comparative Example 8 was unusable because the spinning temperature was too low.
[0136] [Table 1]
[0137] [Table 2]
[0138] From the results in Tables 1 and 2, it was confirmed that the polyimide fibers of Examples 1 to 3 had a breaking strength of 1.5 cN / dtex or higher, a breaking strength variation of ±0.2 cN / dtex or less, and a breaking elongation of 20% or higher. [Explanation of symbols]
[0139] 1. Extruder 2 gear pump 3 Spinning pack 3a Spinner 4 First Godetroll 5. Second Godetroll 6. Winding bobbin
Claims
1. Repeating structural units shown in formula (1) and formula (2) below: 【Chemistry 1】 (R 1 R is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. 2 X is a divalent, chain-like aliphatic group having 5 to 16 carbon atoms. 1 and X 2 Each of these is independently a tetravalent group with 6 to 22 carbon atoms containing at least one aromatic ring. Includes, The content ratio of the repeating constituent units of formula (1) to the total of the repeating constituent units of formula (2) is 20 mol% or more and less than 40 mol%, and The material comprises a polyimide resin that satisfies the following conditions (a), (b), and (c): A polyimide fiber having at least one physical property selected from the group consisting of the following physical properties (A), (B), and (C). Condition (a): Melting point (Tm) is between 280°C and 345°C Condition (b): Glass transition temperature (Tg) is between 150°C and 200°C. Condition (c): The heat energy of the crystallization exothermic peak observed when the material is cooled at a rate of 20°C / min after melting, as measured by differential scanning calorimeter, is 17.0 mJ / mg or more. Physical property (A): The tensile strength of the polyimide fiber is 1.5 cN / dtex or higher. Physical property (B): The variation in the breaking strength of the polyimide fibers is within ±0.2 cN / dtex. Physical property (C): The elongation at break of the polyimide fiber is 20% or more.
2. The melting point (Tm) of the polyimide resin is 310°C or higher and 335°C or lower, the glass transition temperature (Tg) is 170°C or higher and 190°C or lower, and the shear rate at 360°C is 100 s. -1 The polyimide fiber according to claim 1, wherein the melt viscosity at 1050 Pa·s or less.
3. R 1 The polyimide fiber according to claim 1 or 2, wherein is a divalent group represented by the following formula (R1-1) or (R1-2). 【Chemistry 2】 (m 11 and m 12 are each independently an integer of 0 to 2. m 13 to m 15 are each independently an integer of 0 to 2.)
4. R 1 The polyimide fiber according to any one of claims 1 to 3, wherein is a divalent group represented by the following formula (R1-3). 【Transformation 3】
5. R 2 The polyimide fiber according to any one of claims 1 to 4, wherein is an alkylene group having 7 to 12 carbon atoms.
6. X 1 and X 2 The polyimide fiber according to any one of claims 1 to 5, wherein each is independently a tetravalent group represented by any one of the following formulas (X-1) to (X-4). 【Chemistry 4】 (R 11 ~R 18 These are each independently alkyl groups having 1 to 4 carbon atoms. 11 ~p 13 Each of these is an integer between 0 and 2, independently of the others. 14 , p 15 , p 16 and p 18 Each of these is an integer between 0 and 3, independently of the others. 17 L is an integer between 0 and 4. 11 ~L 13 These are, independently, a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.
7. Melting point (Tm) is between 280°C and 345°C, glass transition temperature (Tg) is between 150°C and 200°C, and shear rate at 360°C is 100 s. -1 It contains a thermoplastic polyimide resin having a melt viscosity of 1050 Pa·s or less. A polyimide fiber having at least one physical property selected from the group consisting of the following physical properties (A), (B), and (C). Physical property (A): The tensile strength of the polyimide fiber is 1.5 cN / dtex or higher. Physical property (B): The tensile strength variation of the polyimide fibers is less than ±0.3 cN / dtex. Physical property (C): The elongation at break of the polyimide fiber is 10% or more.
8. The melting point (Tm) is 310°C or higher and 335°C or lower, and the glass transition temperature (Tg) is 170°C or higher and 190°C or lower. The polyimide fiber according to claim 7, having the aforementioned physical properties (A), (B), and (C).
9. A fiber package comprising polyimide fibers according to any one of claims 1 to 8 wound around a tube.
10. A wiring board comprising polyimide fibers according to any one of claims 1 to 8.
11. A drying step to obtain a dried polyimide resin with a moisture content of 50 ppm or less by drying a polyimide resin having a melting point (Tm) of 280°C or more and 345°C or less and a glass transition temperature (Tg) of 150°C or more and 200°C or less, The aforementioned dried polyimide resin is melted while being heated using an extruder under the following conditions (a) to (c), and extruded from a die to form a spinning yarn, and Condition (a): Shear rate of the dry polyimide resin at 360°C is 100 s. -1 The melt viscosity is 1050 Pa·s or less. Condition (b): Spinning temperature is between the melting point of the polyimide resin + 20°C and 380°C. Condition (c): Melt residence time is 12 minutes or less. A bundling step in which the spun yarn extruded from the die is gathered into a single filament, A winding step of winding the filament onto a tube, A method for producing polyimide fibers, including [the specified element].
12. A method for producing polyimide fibers according to claim 11, further comprising a stretching step of stretching the bundled filaments while heating them at a temperature of 150°C to 300°C.
13. A method for producing polyimide fibers according to claim 11 or 12, wherein the spinning step satisfies the following conditions. Condition (d): Linear velocity is 5.0 m / min or more and 50.0 m / min or less. Condition (e): Shear rate is 700 s -1 More than 90,000s -1 below Condition (f): The winding speed of the winding process is 300 m / min or more and 3500 m / min or less.