Gasket member for polymer electrolyte fuel cell, electrode-electrolyte membrane laminate with gasket member, and polymer electrolyte fuel cell

JP2022190083A5Active Publication Date: 2024-10-07DAI NIPPON PRINTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022176378
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-10
Filing Date
2022-11-02
Publication Date
2024-10-07
Estimated Expiration
2042-02-10

AI Technical Summary

Technical Problem

Fuel cell gasket members lack sufficient hydrolysis resistance in high-temperature environments, leading to potential leakage issues.

Method used

A gasket member composed of a laminate structure with a base layer containing a resin with a glass transition temperature of 160°C or higher, and adhesive layers made of imine-modified or carbodiimide-modified polyolefin, ensuring high adhesion and hydrolysis resistance.

Benefits of technology

The gasket member exhibits excellent hydrolysis resistance and adhesion in high-temperature environments, preventing leakage and enhancing the performance of polymer electrolyte fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000018_0000
    Figure 00000018_0000
  • Figure 00000018_0001
    Figure 00000018_0001
  • Figure 00000018_0002
    Figure 00000018_0002
Patent Text Reader

Abstract

Provided is a gasket member for a polymer electrolyte fuel cell that has high adhesion between a heat-resistant substrate layer and an adhesive layer, and has excellent hydrolysis resistance in a high-temperature environment. [Solution] The laminate is made up of at least a base material layer and adhesive layers disposed on both sides of the base material layer, the substrate layer contains a resin having a glass transition temperature of 160°C or higher, The adhesive layer comprises at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to a gasket member for a polymer electrolyte fuel cell, an electrode-electrolyte membrane laminate with a gasket member, and a polymer electrolyte fuel cell. [Background technology]

[0002] A fuel cell is a battery in which electrodes are placed on both sides of an electrolyte, and electricity is generated by the electrochemical reaction of hydrogen and oxygen, producing only water during power generation. Unlike conventional internal combustion engines, it does not generate environmentally harmful gases such as carbon dioxide, and is therefore expected to become widespread as a next-generation clean energy system. Among these, polymer electrolyte fuel cells in particular have a relatively low operating temperature, low electrolyte resistance, and use a highly active catalyst, allowing them to achieve high output even in a small size, and are expected to be put into practical use in household cogeneration systems and other applications in the near future.

[0003] In this polymer electrolyte fuel cell, first, a proton-conducting polymer electrolyte membrane is prepared. An anode catalyst layer is formed on one side of this electrolyte membrane, and a cathode catalyst layer is formed on the other side to create a catalyst layer-electrolyte membrane laminate. Furthermore, a gas diffusion layer is formed on each catalyst layer to create an electrode-electrolyte membrane laminate. Finally, gaskets and separators are installed on this electrode-electrolyte membrane laminate to complete the polymer electrolyte fuel cell (see, for example, Patent Document 1). [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2013-218876 [Overview of the project] [Problems that the invention aims to solve]

[0005] Fuel cells operate in a humidified atmosphere to improve the proton conductivity of the electrolyte membrane, and since water is generated during the power generation reaction, the components of the fuel cell must have high hydrolysis resistance. In addition, since the power density can be improved by increasing the operating temperature of the fuel cell, use in high-temperature environments (e.g., above 100°C) is required from the perspective of miniaturizing fuel cells.

[0006] However, among the components that make up a fuel cell, the gasket component does not necessarily have sufficient hydrolysis resistance in high-temperature environments. When a fuel cell is used in a high-temperature environment, if the gasket component does not have sufficient hydrolysis resistance in high-temperature environments, problems such as the gasket component hydrolyzing and fuel leakage may occur.

[0007] Under these circumstances, the main objective of this disclosure is to provide a gasket component for polymer electrolyte fuel cells that exhibits excellent hydrolysis resistance in high-temperature environments. [Means for solving the problem]

[0008] The inventors of this disclosure have diligently studied to solve the above-mentioned problems. As a result, they have found that a gasket member comprising a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, wherein the base layer contains a resin having a glass transition temperature of 160°C or higher, and the adhesive layer contains at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, is suitable for use as a gasket member for polymer electrolyte fuel cells because it exhibits excellent adhesion between the heat-resistant base layer and the adhesive layer, and excellent hydrolysis resistance in high-temperature environments.

[0009] This disclosure was completed by further consideration based on such novel findings. Specifically, this disclosure provides inventions in the following embodiments. It is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, The substrate layer contains a resin having a glass transition temperature of 160°C or higher. The gasket member for a solid polymer fuel cell, wherein the adhesive layer contains at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin.

Advantages of the Invention

[0010] According to the present disclosure, it is possible to provide a gasket member for a solid polymer fuel cell having high adhesiveness between the base material layer and the adhesive layer and excellent hydrolysis resistance in a high-temperature environment. Further, according to the present disclosure, it is also possible to provide an electrode-electrolyte membrane laminate with a gasket member and a solid polymer fuel cell using the gasket member.

Brief Description of the Drawings

[0011] [Figure 1] It is a schematic diagram showing an example of a cross-sectional structure of the gasket member for a solid polymer fuel cell of the present disclosure. [Figure 2] It is a schematic diagram showing an example of a cross-sectional structure of the gasket member for a solid polymer fuel cell of the present disclosure. [Figure 3] It is an example of a schematic plan view of the gasket member for a solid polymer fuel cell of the present disclosure. [Figure 4] It is a schematic diagram showing an example of a cross-sectional structure of the electrode-electrolyte membrane laminate with a gasket member of the present disclosure. [Figure 5] It is an example of a schematic plan view of the electrode-electrolyte membrane laminate with a gasket member of the present disclosure. [Figure 6] It is a schematic diagram showing an example of a cross-sectional structure of the solid polymer fuel cell of the present disclosure. [Figure 7] It is a schematic diagram showing an example of a cross-sectional structure of the solid polymer fuel cell of the present disclosure.

Embodiments for Carrying Out the Invention

[0012] The gasket member for polymer electrolyte fuel cell according to this disclosure is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, wherein the base layer contains a resin having a glass transition temperature of 160°C or higher, and the adhesive layer contains at least one of imine-modified polyolefin and carbodiimide-modified polyolefin. The gasket member for polymer electrolyte fuel cell according to this disclosure has excellent adhesion between the heat-resistant base layer and the adhesive layer, and excellent hydrolysis resistance in high-temperature environments.

[0013] The gasket member for polymer electrolyte fuel cells disclosed herein is a gasket member that is placed between the electrolyte membrane and the separator of a polymer electrolyte fuel cell, as described below, and can be applied to a wide range of polymer electrolyte fuel cells.

[0014] The gasket members for polymer electrolyte fuel cells described herein will be described in detail below. In this specification, numerical ranges indicated by "~" mean "greater than or equal to" and "less than or equal to". For example, the notation 2~15mm means 2mm or more and 15mm or less.

[0015] 1. Laminated structure and physical properties of gasket components for polymer electrolyte fuel cells The gasket member 10 for polymer electrolyte fuel cell (hereinafter sometimes referred to as gasket member 10) of this disclosure is composed of a laminate comprising at least a base layer 1 and adhesive layers 2 arranged on both sides of the base layer 1, as shown in Figure 1, for example. That is, the gasket member 10 is composed of a laminate in which at least the adhesive layer 2, base layer 1, and adhesive layer 2 are laminated in this order. The adhesive layers 2 on both sides of the gasket member 10 each constitute the outermost layer of the gasket member 10, with one adhesive layer 2 positioned on the electrolyte membrane 21 side and the other adhesive layer 2 positioned on the separator 25 side (see Figure 6).

[0016] As described later, the gasket member 10 is installed, for example, to surround the electrode-electrolyte membrane laminate (see schematic diagrams of the electrode-electrolyte membrane laminate with gasket member in Figures 4 and 5). Accordingly, such a gasket member 10 has an opening 11 for inserting the catalyst layers 22, 23 and the gas diffusion layer 24 (see Figure 3).

[0017] The gasket member 10 may have an anchor coat layer 3 on at least one side of the surface of the base layer 1, as shown in Figure 2, for example. For example, if the base layer 1 is formed of a film, the adhesion between the base layer 1 and the adhesive layer 2 can be improved by providing the anchor coat layer 3 between the base layer 1 and the adhesive layer 2. That is, the gasket member 10 may be composed of a laminate in which at least the adhesive layer 2, anchor coat layer 3, base layer 1, anchor coat layer 3, and adhesive layer 2 are laminated in this order. However, as described later, the gasket member 10 of this disclosure has an adhesive layer 2 that includes at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin which have excellent adhesion to the base layer 1, so the base layer 1 and the adhesive layer 2 may be in direct contact without providing the anchor coat layer 3.

[0018] As described below, the adhesive layer may have a laminated structure of two or more layers comprising a layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin and a layer containing acid-modified polyolefin, or it may have a laminated structure of three or more layers comprising a layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, a layer containing polyolefin and a layer containing acid-modified polyolefin.

[0019] The thickness (total thickness) of the laminate constituting the gasket member 10 is adjusted according to the size of the polymer electrolyte fuel cell and is not particularly limited, but examples include approximately 300 μm or less, approximately 200 μm or less, approximately 100 μm or less, approximately 50 μm or less, or, for example, approximately 30 μm or more, approximately 100 μm or more, approximately 200 μm or more, and approximately 250 μm or more. Preferred ranges for the thickness (total thickness) of the laminate constituting the gasket member 10 include approximately 30 to 300 μm, approximately 30 to 200 μm, approximately 30 to 100 μm, approximately 30 to 50 μm, approximately 100 to 300 μm, approximately 100 to 200 μm, approximately 200 to 300 μm, and approximately 250 to 300 μm.

[0020] For example, as shown in Figure 7, when a single gasket member 10 is installed to surround the electrode-electrolyte membrane laminate, the thickness (total thickness) of the laminate constituting the gasket member 10 is preferably about 400 μm or less, more preferably about 300 μm or less, and also preferably about 30 μm or more, more preferably about 50 μm or more, even more preferably more than 50 μm, and even more preferably about 100 μm or more. Preferred ranges include about 30 to 400 μm, about 30 to 30 μm, about 50 to 400 μm, about 50 to 300 μm, about 50 to 400 μm or less, about 50 to 300 μm or less, about 100 to 400 μm, and about 100 to 300 μm. In this case, the thickness of the base layer 1 is preferably about 300 μm or less, more preferably about 200 μm or less, and also preferably about 20 μm or more, more preferably about 30 μm or more, and even more preferably 50 μm or more. Preferred ranges include about 20-300 μm, about 20-200 μm, about 30-300 μm, about 30-200 μm, about 50-300 μm, and about 50-200 μm. The thickness of the adhesive layer 2 is preferably about 200 μm or less, more preferably about 100 μm or less, and also preferably about 10 μm or more, more preferably about 30 μm or more. Preferred ranges include about 10-200 μm, about 10-100 μm, about 30-200 μm, and about 30-100 μm.

[0021] Furthermore, as shown in Figure 6, for example, when two gasket members 10 are installed to surround the electrode-electrolyte membrane laminate, the thickness (total thickness) of the laminate constituting each gasket member 10 is preferably about 200 μm or less, more preferably about 150 μm or less, and also preferably about 25 μm or more, more preferably about 50 μm or more, with preferred ranges including about 25 to 200 μm, about 25 to 150 μm, about 50 to 200 μm, and about 50 to 150 μm. In this case, the thickness of the base layer 1 is preferably about 200 μm or less, more preferably about 150 μm or less, and also preferably about 10 μm or more, more preferably about 15 μm or more, with preferred ranges including about 10 to 200 μm, about 10 to 150 μm, about 15 to 200 μm, and about 15 to 150 μm. Furthermore, the thickness of the adhesive layer 2 is preferably about 100 μm or less, more preferably about 50 μm or less, and also preferably about 3 μm or more, more preferably about 15 μm or more. Preferred ranges include about 3 to 100 μm, about 3 to 50 μm, about 15 to 100 μm, and about 15 to 50 μm.

[0022] In this disclosure, whether to use one gasket member 10 or two gasket members 10 can be appropriately selected depending on the specifications of the polymer electrolyte fuel cell 30. Furthermore, the total thickness of the gasket member 10 and the thickness of each layer can also be appropriately selected depending on the thickness of the polymer electrolyte fuel cell 30.

[0023] In the gasket member 10, the ratio of the total thickness of the base layer 1, adhesive layer 2, and optionally provided anchor coat layer 3 to the total thickness of the laminate constituting the gasket member 10 is preferably 90% or more, more preferably 95% or more, even more preferably 98% or more, and even more preferably 100%. For example, if the gasket member 10 of this disclosure includes a base layer 1 and an adhesive layer 2, the ratio of the total thickness of each of these layers to the total thickness of the laminate constituting the gasket member 10 is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more. Also, if the gasket member 10 of this disclosure is a laminate including a base layer 1, an adhesive layer 2, and an anchor coat layer 3, the ratio of the total thickness of each of these layers to the total thickness of the laminate constituting the gasket member 10 is, for example, 80% or more, preferably 90% or more, more preferably 95% or more, even more preferably 98% or more, and even more preferably 100%.

[0024] The laminate constituting the gasket member 10 of this disclosure preferably has a fracture elongation retention rate of 60% or more after being left standing for 300 hours in water at 120°C (inside a heat-resistant and pressure-resistant container). This allows for the desirable expression of excellent hydrolysis resistance in high-temperature environments. The method for measuring the fracture elongation retention rate of the gasket member 10 is as follows.

[0025] <Method for measuring the elongation retention rate at break> The elongation retention rate at break is determined by the following method. Specifically, the sample is immersed in water at 120°C and left to stand for 300 hours. After that, the elongation at break of the sample is measured, and the obtained measurement value is divided by the elongation at break before the durability test (initial elongation at break) to determine the elongation retention rate at break. The elongation at break is measured by cutting the film into strips with a width (TD) of 15 mm and a length (MD) of 50 mm, and pulling them using a tensile testing machine at a tensile speed of 200 mm / min and a gauge length of 20 mm, measuring the elongation until breakage. The test environment is 23°C, and the average of three measurements is used. Breaking elongation retention rate (%) = Breaking elongation after durability test ÷ Breaking elongation before durability test (initial breaking elongation) × 100

[0026] Furthermore, one method for confirming the MD (Mass Distribution) of a gasket component involves observing the cross-section of the gasket component (for example, the cross-section of the first adhesive layer, the substrate, or the second adhesive layer) with an electron microscope to confirm the sea-island structure. In this method, the direction parallel to the cross-section where the average diameter of the island shapes perpendicular to the thickness direction of the gasket component is maximized can be determined as the MD. Specifically, the sea-island structure is confirmed by observing electron microscope images of each of the 10 cross-sections (a total of 10 cross-sections) from the cross-section in the longitudinal direction to the direction perpendicular to the cross-section in 10-degree increments. Next, the shape of each individual island is observed in each cross-section. For each island shape, the diameter y is defined as the straight-line distance connecting the leftmost point perpendicular to the thickness direction of the gasket component and the rightmost point perpendicular to that point. In each cross-section, the average of the top 20 island shapes with the largest diameter y is calculated. The direction parallel to the cross-section with the largest average diameter y is determined as the MD.

[0027] From the viewpoint of exhibiting superior properties in terms of hydrolysis resistance in high-temperature environments, the fracture elongation retention rate of the laminate constituting the gasket member 10 is 60% or more, preferably 65% ​​or more, more preferably 70% or more, even more preferably 75% or more, even more preferably 80% or more, and particularly preferably 85% or more.

[0028] An effective method for increasing the fracture elongation retention rate of the laminate constituting the gasket member 10 to 60% or more is to use, for example, a resin with a particularly high glass transition temperature (Tg) as the material for forming the base layer 1.

[0029] From the viewpoint of exhibiting superior properties in hydrolysis resistance in high-temperature environments, the hot shrinkage rate of the laminate constituting the gasket member 10 when left standing in a 150°C environment for 30 minutes is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less. Similarly, from the same viewpoint, the hot shrinkage rate of the laminate constituting the gasket member 10 when left standing in a 180°C environment for 30 minutes is preferably 30% or less, more preferably 20% or less, even more preferably 10% or less, even more preferably 3% or less, even more preferably 1% or less, and even more preferably 0.5% or less. The method for measuring the hot shrinkage rate of the gasket member 10 is as follows.

[0030] <Method for measuring hot shrinkage rate at 150°C or 180°C> The hot shrinkage rate is calculated by cutting a gasket material into a test piece measuring 10 cm (MD) x 10 cm (TD), heating it in an oven at 150°C or 180°C for 30 minutes, determining the dimensional change rate before and after heating in the longitudinal and transverse directions (two orthogonal directions) of the test piece based on the following formula (I), and then taking the absolute value of the dimensional change rates in the two directions as the average value. Hot shrinkage rate (%) = {(XY) / X} × 100 ... (I) [X: Dimensions before heating in the oven, Y: Dimensions after heating in the oven]

[0031] 2. Each layer forming the gasket component for polymer electrolyte fuel cell [Base material layer 1] In this disclosure, the base layer 1 is a layer provided for purposes such as enabling the gasket member 10 to function as a base material. The base layer 1 is located between the two adhesive layers 2.

[0032] In this disclosure, the glass transition temperature (Tg) of the resin forming the substrate layer 1 is 160°C or higher, preferably about 165°C or higher, more preferably about 170°C or higher, and even more preferably about 175°C or higher. The upper limit of the glass transition temperature (Tg) is, for example, about 450°C or lower. The glass transition temperature (Tg) refers to the baseline displacement point of the DSC curve measured by a differential scanning calorimeter (DSC).

[0033] The base layer 1 is preferably formed from a material that satisfies the glass transition temperature and has excellent hydrolysis resistance, and preferably contains, for example, polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyimide, polyetheretherketone, polymethylterpene, polyphenylene oxide, polyphenylene sulfide, fluororesin, metal, etc. When these materials are used to form the base layer 1, the base layer 1 may contain one type of these material or two or more types.

[0034] Examples of polyolefins include polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; ethylene-α-olefin copolymers; polypropylene such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymer of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymer of propylene and ethylene); propylene-α-olefin copolymers; and ethylene-butene-propylene terpolymers. Among these, polypropylene is preferred. When polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer. Furthermore, the polyolefin resin may be an acid-modified polyolefin. When the base layer 1 contains polyolefin, the base layer 1 may contain only one type of polyolefin or two or more types.

[0035] Acid-modified polyolefins are polymers modified by block polymerization or graft polymerization of polyolefins with an acid component. As the polyolefin to be acid-modified, the above-mentioned polyolefins, copolymers obtained by copolymerizing the above-mentioned polyolefins with polar molecules such as acrylic acid or methacrylic acid, or polymers such as cross-linked polyolefins can also be used. Examples of acid components used for acid modification include carboxylic acids or their anhydrides, such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride. Preferred acid-modified polyolefins include polyolefins modified with carboxylic acids or their anhydrides, polypropylenes modified with carboxylic acids or their anhydrides, maleic anhydride-modified polyolefins, and maleic anhydride-modified polypropylenes. When the base layer 1 contains an acid-modified polyolefin, the base layer 1 may contain only one type of acid-modified polyolefin or two or more types.

[0036] Specifically, polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (where I represents isophthalic acid and T represents terephthalic acid), which contain constituent units derived from terephthalic acid and / or isophthalic acid; aromatic polyamides such as polyamide MXD6 (polymetaxylylene adipamide); alicyclic polyamides such as polyamide PACM6 (polybis(4-aminocyclohexyl)methaneadipamide); polyamides copolymerized with lactam components or isocyanate components such as 4,4'-diphenylmethane-diisocyanate; polyesteramide copolymers and polyether esteramide copolymers, which are copolymers of copolymerized polyamides with polyester or polyalkylene ether glycol; and other polymers of these polyamides. If the base layer 1 contains polyamide, the base layer 1 may contain only one type of polyamide, or it may contain two or more types.

[0037] The polyamide is preferably one that has an α-crystal structure, and specific examples include aliphatic polyamides such as nylon 6, nylon 66, nylon 46, and copolymers of nylon 6 and nylon 66.

[0038] Examples of metals include aluminum alloys, copper, zinc, titanium, and stainless steel.

[0039] In this disclosure, from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in a high-temperature environment, the base layer 1 preferably contains polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, or polyolefin, more preferably polysulfone, polyethersulfone, or polyphenylsulfone, and even more preferably polyphenylsulfone. The base layer 1 is preferably formed of at least one of these resins, and particularly preferably polyphenylsulfone. As described later, polysulfone-based resins such as polysulfone, polyethersulfone, and polyphenylsulfone have excellent adhesion to the adhesive layer 2 which contains at least one of imine-modified polyolefin and carbodiimide-modified polyolefin.

[0040] The base layer 1 may be a film or a nonwoven fabric. For example, if the base layer 1 is a film, it can be suitably formed from the aforementioned resin film. Alternatively, if the base layer 1 is a nonwoven fabric, it can be suitably formed from the aforementioned resin nonwoven fabric. When the base layer 1 is a nonwoven fabric, the adhesive layer 2 can be impregnated into the gaps of the nonwoven fabric base layer 1, thereby improving the physical adhesion between the base layer 1 and the adhesive layer 2.

[0041] The base layer 1 may be a single layer or may consist of two or more layers. If the base layer 1 consists of two or more layers, the materials and thicknesses of each layer may be the same or different.

[0042] In addition, additives such as fillers, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents may be present on at least one of the surface and inside of the base material layer 1. Specific examples of the additives include, for example, metal oxide particles such as alumina, silica, and titania. Only one type of additive may be used, or two or more types may be mixed and used.

[0043] In the present disclosure, the thickness of the base material layer 1 is appropriately adjusted according to the size of the solid polymer fuel cell and the like. From the viewpoint of suitably enhancing the hydrolysis resistance of the gasket member 10 in a high-temperature environment, it is preferably about 20 μm or more, more preferably about 40 μm or more, still more preferably about 50 μm or more, and still more preferably 100 μm or more. Also, it is preferably about 200 μm or less, more preferably about 150 μm or less, still more preferably about 100 μm or less. Preferred ranges of the thickness of the base material layer 1 include about 20 to 200 μm, about 20 to 150 μm, about 20 to 100 μm, about 40 to 200 μm, about 40 to 150 μm, about 40 to 100 μm, about 100 to 200 μm, and about 100 to 150 μm.

[0044] When the base material layer 1 is in the form of a non-woven fabric, the basis weight of the base material layer 1 is appropriately adjusted according to the size of the solid polymer fuel cell and the like. From the viewpoint of suitably enhancing the hydrolysis resistance of the gasket member 10 in a high-temperature environment, it is preferably about 5 g / m 2 or more, more preferably about 10 g / m 2 or more, still more preferably about 15 g / m 2 or more. Also, it is preferably about 50 g / m 2 or less, more preferably about 40 g / m 2 or less, still more preferably about 30 g / m 2 or less. When the base material layer 1 is in the form of a non-woven fabric, preferred ranges of the basis weight of the base material layer 1 include about 5 to 50 g / m 2 or so, about 5 to 40 g / m 2 or so, about 5 to 30 g / m 2 or so, about 10 to 50 g / m 2 or so, about 10 to 40 g / m 2 or so, about 10 to 30 g / m 2degree, 15~50g / m 2 degree, 15~40g / m 2 degree, 15~30g / m 2 The degree can be described as follows.

[0045] [Adhesive layer 2] In the gasket member 10, the adhesive layers 2 are arranged on both sides of the base layer 1. The adhesive layers 2 on both sides of the gasket member 10 constitute the outermost layer of the gasket member 10, with one adhesive layer 2 positioned on the electrolyte membrane 21 side and the other adhesive layer 2 positioned on the separator 25 side (see Figure 6). The adhesive layer 2 positioned on the electrolyte membrane 21 side and the adhesive layer 2 positioned on the separator 25 side may be the same in material, thickness, etc., or they may be different. In addition, at least one of the surface and interior of the adhesive layer 2 may contain additives such as fillers, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents. Specific examples of additives include metal oxide particles such as alumina, silica, and titania. Only one type of additive may be used, or two or more types may be mixed and used.

[0046] The adhesive layer 2 comprises at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin. Both the imine-modified polyolefin and the carbodiimide-modified polyolefin exhibit excellent adhesion to resins having a high glass transition temperature (160°C or higher) used in the base layer 1, and thus exhibit excellent adhesion between the base layer 1 and the adhesive layer 2. Therefore, the gasket member 10 of this disclosure exhibits excellent hydrolysis resistance in high-temperature environments. Since the imine-modified polyolefin and the carbodiimide-modified polyolefin exhibit particularly excellent adhesion to polysulfone-based resins such as polysulfone, polyethersulfone, and polyphenylsulfone, it is especially effective to use a polysulfone-based resin such as polysulfone, polyethersulfone, and polyphenylsulfone in the base layer 1. Furthermore, the imine-modified polyolefin and the carbodiimide-modified polyolefin also exhibit good adhesion to the separator 25 and the electrolyte membrane 21.

[0047] Furthermore, the adhesive layer 2 may have a laminated structure of two or more layers, comprising, in order from the base layer 1 side, a layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, and a layer containing acid-modified polyolefin; or it may have a laminated structure of three or more layers, comprising, in order from the base layer 1 side, a layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, a layer containing polyolefin, and a layer containing acid-modified polyolefin. As described above, imine-modified polyolefin and carbodiimide-modified polyolefin have excellent adhesion to resins having a high glass transition temperature used in the base layer 1, and acid-modified polyolefin has excellent adhesion to the separator 25 made of metal, so these laminated structures are preferable. In addition, by providing a layer containing polyolefin between the layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin and the layer containing acid-modified polyolefin, the acid-base reaction caused by direct contact between the layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin and the layer containing acid-modified polyolefin can be suppressed. When the adhesive layer 2 comprises a layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, and a layer containing acid-modified polyolefin, it is preferable that the layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin constitutes the surface on the substrate layer 1 side, and the layer containing acid-modified polyolefin constitutes the surface on the separator 25 side. Furthermore, in these laminated configurations of the adhesive layer 2, it is particularly preferable that the layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, the layer containing polyolefin, and the layer containing acid-modified polyolefin are, respectively, a layer formed from at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, a layer formed from polyolefin, and a layer formed from acid-modified polyolefin.

[0048] Imine-modified polyolefins are preferably obtained by grafting a polyimine compound having multiple imino groups onto a polyolefin in the presence of a radical generator. From the viewpoint of suitably improving hydrolysis resistance in high-temperature environments, the imine-modified polyolefin is preferably imine-modified polypropylene.

[0049] Carbodiimide-modified polyolefins are obtained by reacting a polyolefin having a group that reacts with a carbodiimide group with a carbodiimide group-containing compound, preferably at a temperature of 230°C or higher. Specifically, carbodiimide-modified polyolefins can be obtained by melt kneading, such as by melt modification, but are not limited to this method. From the viewpoint of suitably improving hydrolysis resistance in high-temperature environments, carbodiimide-modified polyolefins are preferably carbodiimide-modified polypropylenes.

[0050] Furthermore, the same examples as those exemplified for the base layer 1 are used for the acid-modified polyolefin and polyrheofin. Among acid-modified polyolefins, acid-modified polypropylene is preferred. Among polyolefins, polypropylene is preferred. In this disclosure, by using acid-modified polyolefin for the adhesive layer 2, adhesion with the separator 25 is improved, and the hydrolysis resistance of the gasket member 10 in high-temperature environments can be suitably enhanced.

[0051] The thickness of the adhesive layer 2 is adjusted as appropriate depending on the size of the polymer electrolyte fuel cell, but from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in a high-temperature environment, it is preferably about 10 μm or more, more preferably about 15 μm or more, even more preferably about 20 μm or more, and also preferably about 100 μm or less, more preferably about 80 μm or less, and even more preferably about 60 μm or less. Preferred ranges for the thickness of the adhesive layer 2 include about 10 to 100 μm, about 10 to 80 μm, about 10 to 60 μm, about 15 to 100 μm, about 15 to 80 μm, about 15 to 60 μm, about 20 to 100 μm, about 20 to 80 μm, and about 20 to 60 μm.

[0052] When the adhesive layer 2 has the aforementioned laminated structure of two or more layers, the preferred thickness range for the layer containing at least one of the imine-modified polyolefin and the carbodiimide-modified polyolefin is approximately 5 to 50 μm. The preferred thickness range for the layer containing the acid-modified polyolefin is also approximately 5 to 50 μm. The preferred thickness range for the layer containing the polyolefin is also approximately 5 to 50 μm. The composition and thickness of the adhesive layers 2 on both sides may be the same or different.

[0053] The laminate of the base layer 1 and the adhesive layers 2 on both sides can be manufactured, for example, by extruding the resin that forms the adhesive layers 2 onto both sides of a pre-prepared base layer 1, or by extruding the resin that forms the base layer 1 and the resin that forms the adhesive layers 2. The resin extrusion and lamination method is not particularly limited, but known methods such as extrusion lamination, T-die lamination, inflation lamination, and thermal lamination can be applied. When providing the anchor coat layer 3 described later, the resin that forms the anchor coat layer 3 can be applied to at least one side of the surface of the base layer 1, and the adhesive layers can be laminated on top of that.

[0054] [Anchor Coat Layer 3] The anchor coat layer 3 is a layer provided on at least one side of the surface of the base layer 1, as needed, for the purpose of further enhancing the adhesion between the base layer 1 and the adhesive layer 2.

[0055] As described above, the gasket member 10 of this disclosure includes an adhesive layer 2 containing at least one imine-modified polyolefin and a carbodiimide-modified polyolefin that have excellent adhesion to the base layer 1. Therefore, the base layer 1 and the adhesive layer 2 may be in direct contact without the provision of an anchor coat layer 3.

[0056] The material used to form the anchor coat layer 3 is not particularly limited as long as it enhances the adhesion between the base layer 1 and the adhesive layer 2, but isocyanate-based, polyethyleneimine-based, polyester-based, polyurethane-based, polyvinyl butyral-based, acrylic-based, aminoethylated acrylic polymer-based, styrene / maleic acid copolymer-based, rubber-based, epoxy-based resins are preferred. One or more of these resins can be used in combination.

[0057] While there are no particular limitations on the compound having an isocyanate group, polyfunctional isocyanate compounds are preferred from the viewpoint of effectively improving the adhesion between the substrate layer 1 and the adhesive layer 2. The polyfunctional isocyanate compound is not particularly limited as long as it is a compound having two or more isocyanate groups. Specific examples of polyfunctional isocyanate curing agents include pentane diisocyanate (PDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), m-xylylene diisocyanate (XDI), polymerized or nurated versions thereof, mixtures thereof, and copolymers with other polymers. Adducts, burettes, and isocyanurates are also examples. Other examples of triisocyanates include triphenylmethane-4,4',4"-triisocyanate and tris(p-isocyanatephenyl)thiophosphorate. The compound having an isocyanate group used to form the anchor coat layer 3 may be one type or two or more types.

[0058] Examples of polyurethane-based materials include two-component mixtures of polyester resin and polyfunctional isocyanate compounds, and two-component mixtures of polycarbonate diol and polyfunctional isocyanate compounds. Specific examples of polyurethane-based materials include two-component mixtures of polyester resin and hexamethylene diisocyanate, and two-component mixtures of polycarbonate diol and polymethylene polyphenyl polyisocyanate.

[0059] The thickness of the anchor coat layer 3 is adjusted as appropriate depending on the size of the polymer electrolyte fuel cell, but from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in high-temperature environments, it is preferably about 0.02 g / m². 2 More preferably 0.05 g / m 2 More preferably, about 0.1 g / m 2 More preferably, approximately 0.3 g / m 2 More preferably, about 0.5 g / m 2 The above is true, and preferably about 5 g / m 2 More precisely, approximately 4 g / m 2 More preferably, about 3 g / m 2 The following is a preferred range for the thickness of the anchor coat layer 3: 0.02 to 5 g / m². 2 degree, 0.02~4g / m 2 degree, 0.02~3g / m 2 degree, 0.05~5g / m 2 degree, 0.05~4g / m 2 degree, 0.05~3g / m 2 degree, 0.1~5g / m 2 degree, 0.1~4g / m 2 degree, 0.1~3g / m 2 degree, 0.3~5g / m 2 degree, 0.3~4g / m 2 degree, 0.3~3g / m 2 degree, 0.5~5g / m 2 degree, 0.5~4g / m 2 degree, 0.5~3g / m 2 The degree can be described as follows.

[0060] 3. Electrode-electrolyte membrane laminate with gasket component The electrode-electrolyte membrane laminate 20 with gasket member of this disclosure is an electrode-electrolyte membrane laminate to which the gasket member 10 of this disclosure is attached (see Figure 4). Specifically, the electrode-electrolyte membrane laminate 20 with gasket member of this disclosure comprises an electrode-electrolyte membrane laminate in which catalyst layers 22, 23 and a gas diffusion layer 24 are arranged on both sides of an electrolyte membrane 21, and a frame-shaped gasket member 10 arranged to cover the outer peripheral edge of the electrode-electrolyte membrane laminate. The gasket member 10 is composed of a laminate comprising at least a base layer 1 and adhesive layers 2 arranged on both sides of the base layer 1, wherein the base layer 1 contains a resin having a glass transition temperature of 160°C or higher, and the adhesive layer 2 contains at least one of imine-modified polyolefin and carbodiimide-modified polyolefin.

[0061] The gasket member 10 of this disclosure may be a pair of members bonded together, arranged to cover the outer peripheral edge of the electrode-electrolyte membrane laminate from one side and the other side, as shown in Figure 4, or it may be a single gasket member 10 that covers the outer peripheral edge of the electrode-electrolyte membrane laminate, as shown in Figure 7.

[0062] The electrolyte membrane 21 is not particularly limited and may be, for example, one used in a known polymer electrolyte fuel cell. The electrolyte membrane 21 is formed, for example, by coating a substrate with a solution containing a hydrogen ion conductive polymer electrolyte and drying it. Examples of hydrogen ion conductive polymer electrolytes include perfluorosulfonic acid-based fluorine ion exchange resins, and more specifically, perfluorocarbon sulfonic acid-based polymers (PFS polymers) in which the CH bonds of a hydrocarbon-based ion exchange membrane are replaced with fluorine. By introducing highly electronegative fluorine atoms, chemical stability is achieved, the degree of dissociation of sulfonic acid groups is high, and high ionic conductivity can be realized. Specific examples of such hydrogen ion conductive polymer electrolytes include "Nafion" (registered trademark) from DuPont, "Flemion" (registered trademark) from Asahi Glass Co., Ltd., "Aciplex" (registered trademark) from Asahi Kasei Corporation, and "GoreSelect" (registered trademark) from Gore. The concentration of the hydrogen ion-conducting polymer electrolyte in the hydrogen ion-conducting polymer electrolyte-containing solution is typically about 5 to 60% by weight, preferably about 20 to 40% by weight. The thickness of the electrolyte membrane 21 is typically about 3 to 50 μm, preferably about 5 to 20 μm. Although not shown in the figures, the end face of the electrolyte membrane 21 does not need to be aligned with the end faces of the catalyst layers 22 and 23. For example, the end face of the electrolyte membrane 21 may protrude beyond the end faces of the catalyst layers 22 and 23, and the adhesive layer 2 of the gasket member 10 may cover the protruding portion of the electrolyte membrane 21.

[0063] Specifically, catalyst layers 22 and 23 consist of an anode catalyst layer and a cathode catalyst layer. Catalyst layers 22 and 23 are not particularly limited and may be, for example, those used in known polymer electrolyte fuel cells. Catalyst layers 22 and 23 are, for example, platinum-containing catalyst layers. Catalyst layers 22 and 23 contain, for example, carbon particles supporting catalyst particles and a hydrogen ion-conducting polymer electrolyte. Examples of catalyst particles include platinum and platinum compounds. Examples of platinum compounds include alloys of platinum with at least one metal selected from the group consisting of ruthenium, palladium, nickel, molybdenum, iridium, iron, etc. Typically, the catalyst particles in the cathode catalyst layer are platinum, and the catalyst particles in the anode catalyst layer are alloys of the aforementioned metal and platinum. Furthermore, the same material used for the electrolyte membrane 21 can be used as the hydrogen ion-conducting polymer electrolyte.

[0064] The size and shape of the electrolyte membrane 21 and catalyst layers 22 and 23 are adjusted according to the size of the polymer electrolyte fuel cell, and the size and shape of the gasket member 10 of this disclosure are also adjusted appropriately according to their size so that they function as a gasket member (i.e., they have mechanical strength to withstand hot pressing and exhibit gas barrier properties sufficient to prevent leakage of fuel and oxidizer to the outside).

[0065] 4. Polymer electrolyte fuel cell The polymer electrolyte fuel cell 30 of this disclosure is a polymer electrolyte fuel cell utilizing the gasket member 10 of this disclosure. That is, the polymer electrolyte fuel cell 30 of this disclosure comprises an electrode-electrolyte membrane laminate 20 with a gasket member of this disclosure.

[0066] The polymer electrolyte fuel cell 30 comprises a catalyst layer-electrolyte membrane laminate, and an electrode-electrolyte membrane laminate is formed by forming gas diffusion layers 24 on the catalyst layers 22 and 23 of the catalyst layer-electrolyte membrane laminate, respectively. The catalyst layers 22 and 23 and the gas diffusion layer 24 constitute electrodes (anode and cathode electrodes), respectively. The gasket member 10 of this disclosure is placed on the outer edge of the electrolyte membrane 21 so as to surround these electrodes. Furthermore, a separator 25 with a gas flow path 26 is installed so as to sandwich the electrode-electrolyte membrane laminate on which the gasket member 10 is installed from above and below.

[0067] The gas diffusion layer 24 is not particularly limited and may be, for example, one used in a known polymer electrolyte fuel cell. That is, the gas diffusion layer 24 can be any gas diffusion layer that constitutes the anode or cathode electrode, and is made of a porous conductive substrate in order to efficiently supply the fuel gas and oxidizer gas to the catalyst layers 22 and 23. Examples of porous conductive substrates include carbon paper and carbon cloth.

[0068] The separator 25 is not particularly limited and may be, for example, one used in a known polymer electrolyte fuel cell. The separator 25 can be any conductive plate that is stable in the environment inside the fuel cell, and generally, a metal plate such as titanium, aluminum, copper, or stainless steel with a gas channel 26 formed on it is used. Alternatively, the separator 25 may be made of the above metals, and a coating made of a conductive material such as carbon, silver, chromium nitride, platinum group metals or their oxides, or a conductive polymer may be formed on the surface of the metal.

[0069] The operating temperature of the polymer electrolyte fuel cell 30 of this disclosure is not particularly limited, but since the gasket member 10 has excellent hydrolysis resistance in high-temperature environments, it may be used at operating temperatures of, for example, 60°C or higher, and even 100°C or higher. Increasing the operating temperature of the fuel cell can increase the power density. The upper limit of the operating temperature of the polymer electrolyte fuel cell 30 of this disclosure is, for example, 150°C or lower. [Examples]

[0070] The present disclosure will be described in detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the examples.

[0071] <Manufacturing of gasket components for solid polymer fuel cells> (Example 1) A polysulfone (PSU) film (100 μm thick, Tg 180°C) was prepared as the base layer. Next, an adhesive layer was formed on both sides of the base layer by melt-extruding imine-modified polypropylene to a thickness of 50 μm, thereby obtaining a solid polymer fuel cell gasket member (200 μm thick) in which the adhesive layer (50 μm thick) / base layer (100 μm thick) / adhesive layer (50 μm thick) were laminated in that order.

[0072] (Example 2) A polyethersulfone (PESU) film (100 μm thick, Tg 220°C) was prepared as the base layer. Next, an adhesive layer was formed on both sides of the base layer by melt-extruding imine-modified polypropylene to a thickness of 50 μm, thereby obtaining a solid polymer fuel cell gasket member (200 μm thick) in which the adhesive layer (50 μm thick) / base layer (100 μm thick) / adhesive layer (50 μm thick) were laminated in that order.

[0073] (Example 3) Except for using a polyphenylsulfone (PPSU) film (100 μm thick, Tg 220°C) as the base layer instead of a polyethersulfone (PESU) film, a gasket member for a polymer electrolyte fuel cell (200 μm thick) was obtained in the same manner as in Example 1, with an adhesive layer (50 μm thick) / base layer (100 μm thick) / adhesive layer (50 μm thick) laminated in that order.

[0074] (Example 4) Except for the fact that, instead of imine-modified polypropylene as the adhesive layer, imine-modified polypropylene (20 μm thick) and maleic anhydride-modified polypropylene (PPa, 30 μm thick) were melt-extruded onto both sides of a polyphenylsulfone (PPSU) film (with the imine-modified polypropylene on the substrate layer side), a gasket member for polymer electrolyte fuel cell (200 μm thick) was obtained in the same manner as in Example 3, with the adhesive layer (50 μm thick) / substrate layer (100 μm thick) / adhesive layer (50 μm thick) being laminated in that order.

[0075] (Example 5) Except for the fact that, instead of imine-modified polypropylene as the adhesive layer, imine-modified polypropylene, polypropylene, and maleic anhydride-modified polypropylene (PPa) were melt-extruded onto both sides of a polyphenylsulfone (PPSU) film (the imine-modified polypropylene (20 μm thick) was on the substrate layer side, the maleic anhydride-modified polypropylene (20 μm thick) was on the opposite side from the substrate layer, and the polypropylene (10 μm thick) was between the imine-modified polypropylene and the acid-modified polypropylene), a gasket member for polymer electrolyte fuel cell (200 μm thick) was obtained in the same manner as in Example 3, with adhesive layer (50 μm thick) / substrate layer (100 μm thick) / adhesive layer (50 μm thick) laminated in that order.

[0076] (Example 6) Except for the fact that, instead of imine-modified polypropylene, carbodiimide-modified polypropylene (20 μm thick) and maleic anhydride-modified polypropylene (PPa, 30 μm thick) were melt-extruded onto both sides of a polyphenylsulfone (PPSU) film as adhesive layers (carbodiimide-modified polypropylene on the substrate layer side), a gasket member for polymer electrolyte fuel cell (200 μm thick) was obtained in the same manner as in Example 3, with adhesive layer (50 μm thick) / substrate layer (100 μm thick) / adhesive layer (50 μm thick) laminated in that order.

[0077] (Example 7) Except for the fact that, instead of imine-modified polypropylene, carbodiimide-modified polypropylene, polypropylene, and maleic anhydride-modified polypropylene (PPa) were melt-extruded onto both sides of a polyphenylsulfone (PPSU) film as adhesive layers (the carbodiimide-modified polypropylene (20 μm thick) was on the substrate layer side, the maleic anhydride-modified polypropylene (20 μm thick) was on the opposite side from the substrate layer, and the polypropylene (10 μm thick) was between the carbodiimide-modified polypropylene and the acid-modified polypropylene), a gasket member for polymer electrolyte fuel cell (200 μm thick) was obtained in the same manner as in Example 3, with adhesive layer (50 μm thick) / substrate layer (100 μm thick) / adhesive layer (50 μm thick) laminated in that order.

[0078] (Comparative Examples 1 and 2) Except for using polyethylene naphthalate (PEN) film (thickness 100 μm, Tg 155°C), which is commonly used as the base layer for polymer electrolyte fuel cell gasket members, instead of polysulfone (PSU) film as the base layer, a polymer electrolyte fuel cell gasket member (thickness 200 μm) was obtained in the same manner as in Example 1, with an adhesive layer (thickness 50 μm) / base layer (thickness 100 μm) / adhesive layer (thickness 50 μm) laminated in that order. The polymer electrolyte fuel cell gasket members in Comparative Examples 1 and 2 are the same, the only difference being that the temperature condition for <adhesion temperature to the separator> described later was evaluated at 170°C for Comparative Example 1 and 230°C for Comparative Example 2.

[0079] (Comparative Example 3) Instead of a polysulfone (PSU) film, a polyethylene naphthalate (PEN) film (100 μm thick, Tg 155°C), commonly used as the base layer for gasket components of polymer electrolyte fuel cells, was used. Next, a resin composition containing a compound having an isocyanate group (a two-component mixture of polyester resin and hexamethylene diisocyanate) was applied to both sides of the base layer to form an anchor coat layer (0.5 g / m² thick). 2A layer was formed. Furthermore, an adhesive layer was formed on the surface of each of the anchor coat layers by melt-extruding maleic anhydride-modified polypropylene (PPa) to a thickness of 50 μm, resulting in an adhesive layer (thickness 50 μm) / anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).

[0080] <Elongation retention rate at break (evaluation of hydrolysis resistance in high-temperature environments)> For the solid polymer fuel cell gasket members manufactured in the examples and comparative examples, the retention rate of elongation at break (%) was measured after being left to stand in 120°C water for 300 hours (in a heat-resistant and pressure-resistant container) under the following measurement conditions. The results are shown in Table 1. After being immersed in 120°C water and left to stand for 300 hours, the elongation at break of the sample was measured, and the retention rate of elongation at break was determined by dividing the obtained measurement value by the elongation at break before the durability test (initial elongation at break). Elongation at break was measured by cutting the film into strips with a width (TD) of 15 mm and a length (MD) of 50 mm, and pulling them using a tensile testing machine at a tensile speed of 200 mm / min and a gauge length of 20 mm. The elongation at break was measured. The test environment was 23°C, and the average of three measurements was used. Breaking elongation retention rate (%) = Breaking elongation after durability test ÷ Breaking elongation before durability test (initial breaking elongation) × 100

[0081] <Adhesion strength to separators> The adhesive strength (N) of the solid polymer fuel cell gasket members manufactured in the examples and comparative examples was measured against a stainless steel plate (SUS304) used as a separator, under the following measurement conditions. The results are shown in Table 1. In accordance with the provisions of JIS K7127:1999, the peel strength in a 25°C environment was measured as follows. A sample was cut from the sample into strips with a width of 15 mm in the TD direction, and the metal-adhesive layer was bonded by hot pressing to create a sample for measurement. Next, the sample for measurement was attached to a tensile testing machine, and the adhesive strength (peel strength) between the metal layer and the adhesive layer was measured under the conditions of a tensile speed of 300 mm / min and a gauge length of 50 mm. The maximum strength at the time of peeling was defined as the seal strength (N / 15 mm). The average value of three measurements was used. For the hot pressing conditions, the surface pressure was fixed at 1 MPa and the pressing time at 20 seconds (s), and the temperature was changed for measurement. Specifically, the bonding temperature was increased in 10°C increments, and the bonding strength was measured when the bonded sample was strong enough to be grasped by hand (as shown in Table 1). As mentioned above, the solid polymer fuel cell gasket members for Comparative Examples 1 and 2 were the same, and the bonding strength was evaluated under different temperature conditions: 170°C for Comparative Example 1 and 230°C for Comparative Example 2. The bonding strength of Comparative Example 1 was too low to be measured at 170°C.

[0082] <Adhesion temperature to separators> In the measurement of the adhesive strength described above, the temperature at which the polymer electrolyte fuel cell gasket member was bonded to the stainless steel plate (SUS304) was measured. The results are shown in Table 1. As mentioned above, the polymer electrolyte fuel cell gasket members for Comparative Examples 1 and 2 were the same, but the temperature conditions were 170°C for Comparative Example 1 and 230°C for Comparative Example 2.

[0083] [Table 1]

[0084] *1 In Comparative Example 3, an anchor coat layer is provided between the substrate layer and the adhesive layer.

[0085] The gasket members of Examples 1 to 7 had a base layer containing a resin with a glass transition temperature of 160°C or higher, and an adhesive layer containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, exhibiting excellent hydrolysis resistance in high-temperature environments. Among these, Examples 3 to 7, which used PPSU for the base layer, showed an even higher retention rate of elongation at break and particularly excellent hydrolysis resistance in high-temperature environments. In Comparative Example 1, at an adhesive temperature of 170°C, delamination occurred at the separator (SUS304)-adhesive layer interface, making strength measurement impossible. In Comparative Example 2, where the adhesive temperature was raised to 230°C, cohesive failure of the adhesive layer occurred, confirming adhesion. Furthermore, in Examples 4 to 7, which used gasket members in which layers containing at least one of imine-modified polyolefin and carbodiimide-modified polyolefin, and an acid-modified polyolefin were laminated on both sides of the base layer, in order from the base layer side, in addition to excellent hydrolysis resistance in high-temperature environments, the adhesive temperature to the separator could be further reduced. Lowering the bonding temperature to the separator reduces the thermal load on the electrode-electrolyte membrane laminate and also improves productivity.

[0086] As described above, this disclosure provides inventions in the following embodiments. Item 1. It is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, The substrate layer contains a resin having a glass transition temperature of 160°C or higher. The adhesive layer comprises at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, and is a gasket member for a polymer electrolyte fuel cell. Item 2. The gasket member for polymer electrolyte fuel cell according to Item 1, wherein the base layer comprises at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyimide, polyetheretherketone, polymethylterpene, polyphenylene oxide, polyphenylene sulfide, and fluororesin. Item 3. The gasket member for polymer electrolyte fuel cell according to item 1 or 2, wherein the adhesive layer comprises, in order from the substrate layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, and a layer containing an acid-modified polyolefin. Item 4. The adhesive layer comprises, in order from the substrate layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, a layer containing a polyolefin, and a layer containing an acid-modified polyolefin, the gasket member for a polymer electrolyte fuel cell according to any one of items 1 to 3. Item 5. A gasket member for a polymer electrolyte fuel cell according to any one of items 1 to 4, wherein the thickness of the base material layer is 20 μm or more and 200 μm or less. Item 6. A gasket member for a polymer electrolyte fuel cell according to any one of items 1 to 5, wherein the thickness of the adhesive layer is 10 μm or more and 100 μm or less. Item 7. An electrode-electrolyte membrane laminate in which a catalyst layer and a gas diffusion layer are arranged on both sides of the electrolyte membrane, A frame-shaped gasket member is positioned to cover the outer edge of the electrode-electrolyte membrane laminate, Equipped with, The gasket member is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer. The substrate layer contains a resin having a glass transition temperature of 160°C or higher. The adhesive layer comprises at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, and is an electrode-electrolyte membrane laminate with a gasket member. Item 8. The electrode-electrolyte membrane laminate with gasket member according to Item 7, wherein the substrate layer comprises at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyimide, polyetheretherketone, polymethylterpene, polyphenylene oxide, polyphenylene sulfide, carbodiimide-modified polyolefin, and fluororesin. Item 9. The electrode-electrolyte membrane laminate with gasket member according to item 7 or 8, wherein the adhesive layer comprises, in order from the substrate layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, and a layer containing an acid-modified polyolefin. Item 10. The electrode-electrolyte membrane laminate with a gasket member according to any one of items 7 to 9, wherein the adhesive layer comprises, in order from the substrate layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, a layer containing a polyolefin, and a layer containing an acid-modified polyolefin. Item 11. An electrode-electrolyte membrane laminate with a gasket member according to any one of items 7 to 10, wherein the thickness of the substrate layer is 20 μm or more and 200 μm or less. Item 12. An electrode-electrolyte membrane laminate with a gasket member according to any one of items 7 to 11, wherein the thickness of the adhesive layer is 10 μm or more and 100 μm or less. Item 13. A polymer electrolyte fuel cell comprising an electrode-electrolyte membrane laminate with a gasket component as described in any one of items 7 to 12. Item 14. A method for manufacturing a gasket member for a polymer electrolyte fuel cell, comprising a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, The process includes laminating the adhesive layer on both sides of the base material layer. The substrate layer contains a resin having a glass transition temperature of 160°C or higher. The adhesive layer comprises an imine-modified polyolefin, and the method for manufacturing a gasket member for a polymer electrolyte fuel cell. [Explanation of Symbols]

[0087] 1 Base material layer 2 Adhesive layer 3. Anchor Coat Layer 10 Gasket components 11 Opening 20 Electrode-electrolyte membrane laminate with gasket component 21 Electrolyte membrane 22,23 Catalyst layer 24 Gas diffusion layer 25 Separators 26 Gas flow path 30 Polymer electrolyte fuel cell

Claims

1. The laminate includes at least a base layer and an adhesive layer disposed on both sides of the base layer, The substrate layer contains a resin having a glass transition temperature of 180° C. or higher, the base layer contains at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyetheretherketone, polymethyltempene, polyphenylene oxide, and polyphenylene sulfide; The gasket member for a polymer electrolyte fuel cell, wherein the adhesive layer contains at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin.

2. 2. The gasket member for a polymer electrolyte fuel cell according to claim 1, wherein the adhesive layer comprises, in order from the base layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, and a layer containing an acid-modified polyolefin.

3. 3. The gasket member for a polymer electrolyte fuel cell according to claim 1 or 2, wherein the adhesive layer comprises, in order from the base layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, a layer containing a polyolefin, and a layer containing an acid-modified polyolefin.

4. 4. The gasket member for a polymer electrolyte fuel cell according to claim 1, wherein the thickness of the base layer is 20 μm or more and 200 μm or less.

5. 5. The gasket member for a polymer electrolyte fuel cell according to claim 1, wherein the adhesive layer has a thickness of 10 μm or more and 100 μm or less.

6. an electrode-electrolyte membrane laminate in which a catalyst layer and a gas diffusion layer are disposed on both sides of an electrolyte membrane; A frame-shaped gasket member arranged to cover the outer peripheral edge of the electrode-electrolyte membrane stack; Equipped with The gasket member is composed of a laminate including at least a base material layer and adhesive layers disposed on both sides of the base material layer, The substrate layer contains a resin having a glass transition temperature of 180° C. or higher, the base layer contains at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyetheretherketone, polymethyltempene, polyphenylene oxide, and polyphenylene sulfide; The adhesive layer comprises at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin.

7. 7. The gasket member-attached electrode-electrolyte membrane laminate according to claim 6, wherein the adhesive layer comprises, in this order from the base material layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, and a layer containing an acid-modified polyolefin.

8. 8. The electrode-electrolyte membrane laminate with gasket member according to claim 6, wherein the adhesive layer comprises, in this order from the base material layer side, a layer containing at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin, a layer containing a polyolefin, and a layer containing an acid-modified polyolefin.

9. 9. The electrode-electrolyte membrane laminate with gasket member according to claim 6, wherein the thickness of the substrate layer is from 20 μm to 200 μm.

10. 10. The electrode-electrolyte membrane laminate with gasket member according to claim 6, wherein the adhesive layer has a thickness of 10 μm or more and 100 μm or less.

11. A polymer electrolyte fuel cell comprising the gasket member-attached electrode-electrolyte membrane laminate according to any one of claims 6 to 10.

12. A method for producing a gasket member for a polymer electrolyte fuel cell, the gasket member being constituted by a laminate including at least a base layer and adhesive layers disposed on both sides of the base layer, the method comprising the steps of: The method includes a step of laminating the adhesive layer on both sides of the base material layer, The substrate layer contains a resin having a glass transition temperature of 180° C. or higher, the base layer contains at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyetheretherketone, polymethyltempene, polyphenylene oxide, and polyphenylene sulfide; The method for producing a gasket member for a polymer electrolyte fuel cell, wherein the adhesive layer contains at least one of an imine-modified polyolefin and a carbodiimide-modified polyolefin.