Gasket member for polymer electrolyte fuel cell, electrode-electrolyte membrane laminate with gasket member, and polymer electrolyte fuel cell
Patent Information
- Application Number
- JP2022176376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-02-10
- Filing Date
- 2022-11-02
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2042-02-10
AI Technical Summary
Gasket members in polymer electrolyte fuel cells lack sufficient hydrolysis resistance in high-temperature environments, leading to potential leakage issues.
A laminate structure comprising a base material layer and adhesive layers on both sides, with a breaking elongation retention rate of 60% or more after 300 hours in water at 120°C, using materials like polysulfone and acid-modified polyolefin to enhance hydrolysis resistance.
The gasket member exhibits excellent hydrolysis resistance in high-temperature environments, preventing leakage and ensuring the integrity of the fuel cell.
Smart Images

Figure 00000017_0000 
Figure 00000017_0001 
Figure 00000017_0002
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a gasket member for a polymer electrolyte fuel cell, an electrode-electrolyte membrane laminate with a gasket member, and a polymer electrolyte fuel cell. [Background technology]
[0002] A fuel cell is a battery in which electrodes are placed on both sides of an electrolyte, and electricity is generated by the electrochemical reaction of hydrogen and oxygen, producing only water during power generation. Unlike conventional internal combustion engines, it does not generate environmentally harmful gases such as carbon dioxide, and is therefore expected to become widespread as a next-generation clean energy system. Among these, polymer electrolyte fuel cells in particular have a relatively low operating temperature, low electrolyte resistance, and use a highly active catalyst, allowing them to achieve high output even in a small size, and are expected to be put into practical use in household cogeneration systems and other applications in the near future.
[0003] In this polymer electrolyte fuel cell, first, a proton-conducting polymer electrolyte membrane is prepared. An anode catalyst layer is formed on one side of this electrolyte membrane, and a cathode catalyst layer is formed on the other side to create a catalyst layer-electrolyte membrane laminate. Furthermore, a gas diffusion layer is formed on each catalyst layer to create an electrode-electrolyte membrane laminate. Finally, gaskets and separators are installed on this electrode-electrolyte membrane laminate to complete the polymer electrolyte fuel cell (see, for example, Patent Document 1). [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2013-218876 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] In a fuel cell, it operates in a humidified atmosphere to improve the proton conductivity of the electrolyte membrane. Further, since water is generated by the power generation reaction, high hydrolysis resistance is also required for the members constituting the fuel cell. Also, since the output density can be improved by increasing the operating temperature of the fuel cell, use in a high-temperature environment (for example, 100°C or higher) is required from the viewpoint of miniaturizing the fuel cell.
[0006] However, among the members constituting the fuel cell, the gasket member does not necessarily have sufficient hydrolysis resistance in a high-temperature environment. When the fuel cell is used in a high-temperature environment, if the hydrolysis resistance of the gasket member in the high-temperature environment is not sufficient, problems such as hydrolysis of the gasket member and leakage of fuel may occur.
[0007] Under such circumstances, the main object of the present disclosure is to provide a gasket member for a solid polymer fuel cell having excellent hydrolysis resistance in a high-temperature environment.
Means for Solving the Problems
[0008] The inventors of the present disclosure have conducted intensive studies to solve the above problems. As a result, it is composed of a laminate including a base material layer and adhesive layers disposed on both sides of the base material layer, and the laminate has an elongation at break retention rate of 60% or more after being left standing in water at 120°C for 300 hours. It has been found that such a laminate has excellent hydrolysis resistance in a high-temperature environment and can be suitably used as a gasket member for a solid polymer fuel cell.
[0009] The present disclosure has been completed by further studies based on such new findings. That is, the present disclosure provides an invention in the following aspects. It is composed of a laminate including a base material layer and adhesive layers disposed on both sides of the base material layer, The laminate has an elongation at break retention rate of 60% or more after being left standing in water at 120°C for 300 hours, and is a gasket member for a solid polymer fuel cell.
Effects of the Invention
[0010] This disclosure provides a gasket member for polymer electrolyte fuel cells that exhibits excellent hydrolysis resistance in high-temperature environments. Furthermore, this disclosure also provides an electrode-electrolyte membrane laminate with the gasket member and a polymer electrolyte fuel cell utilizing the said gasket member. [Brief explanation of the drawing]
[0011] [Figure 1] This is a schematic diagram showing an example of the cross-sectional structure of a gasket member for a polymer electrolyte fuel cell according to the present disclosure. [Figure 2] This is a schematic diagram showing an example of the cross-sectional structure of a gasket member for a polymer electrolyte fuel cell according to the present disclosure. [Figure 3] This is an example of a schematic plan view of a gasket member for a polymer electrolyte fuel cell according to the present disclosure. [Figure 4] This is a schematic diagram showing an example of the cross-sectional structure of the electrode-electrolyte membrane laminate with gasket member of the present disclosure. [Figure 5] This is an example of a schematic plan view of the electrode-electrolyte membrane laminate with gasket member according to the present disclosure. [Figure 6] This is a schematic diagram showing an example of the cross-sectional structure of the polymer electrolyte fuel cell described herein. [Figure 7] This is a schematic diagram showing an example of the cross-sectional structure of the polymer electrolyte fuel cell described herein. [Modes for carrying out the invention]
[0012] The gasket member for polymer electrolyte fuel cell according to this disclosure is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, wherein the laminate is characterized in that it retains a fracture elongation rate of 60% or more after being left standing in water at 120°C for 300 hours. The gasket member for polymer electrolyte fuel cell according to this disclosure has excellent hydrolysis resistance in high-temperature environments.
[0013] The gasket member for polymer electrolyte fuel cells disclosed herein is a gasket member that is placed between the electrolyte membrane and the separator of a polymer electrolyte fuel cell, as described below, and can be applied to a wide range of polymer electrolyte fuel cells.
[0014] The gasket members for polymer electrolyte fuel cells described herein will be described in detail below. In this specification, numerical ranges indicated by "~" mean "greater than or equal to" and "less than or equal to". For example, the notation 2~15mm means 2mm or more and 15mm or less.
[0015] 1. Laminated structure and physical properties of gasket components for polymer electrolyte fuel cells The gasket member 10 for polymer electrolyte fuel cell (hereinafter sometimes referred to as gasket member 10) of this disclosure is composed of a laminate comprising at least a base layer 1 and adhesive layers 2 arranged on both sides of the base layer 1, as shown in Figure 1, for example. That is, the gasket member 10 is composed of a laminate in which at least the adhesive layer 2, base layer 1, and adhesive layer 2 are laminated in this order. The adhesive layers 2 on both sides of the gasket member 10 each constitute the outermost layer of the gasket member 10, with one adhesive layer 2 positioned on the electrolyte membrane 21 side and the other adhesive layer 2 positioned on the separator 25 side (see Figure 6).
[0016] As described later, the gasket member 10 is installed, for example, to surround the electrode-electrolyte membrane laminate (see schematic diagrams of the electrode-electrolyte membrane laminate with gasket member in Figures 4 and 5). Accordingly, such a gasket member 10 has an opening 11 for inserting the catalyst layers 22, 23 and the gas diffusion layer 24 (see Figure 3).
[0017] The gasket member 10 may have an anchor coat layer 3 on at least one side of the surface of the base layer 1, as shown in Figure 2, for example. For example, if the base layer 1 is formed of a film, the adhesion between the base layer 1 and the adhesive layer 2 can be improved by providing the anchor coat layer 3 between the base layer 1 and the adhesive layer 2. It is preferable to provide the anchor coat layer 3 on both sides of the surface of the base layer 1. That is, it is more preferable that the gasket member 10 is composed of a laminate in which at least the adhesive layer 2, anchor coat layer 3, base layer 1, anchor coat layer 3, and adhesive layer 2 are laminated in this order.
[0018] The thickness (total thickness) of the laminate constituting the gasket member 10 is adjusted according to the size of the polymer electrolyte fuel cell and is not particularly limited, but examples include approximately 300 μm or less, approximately 200 μm or less, approximately 100 μm or less, approximately 50 μm or less, or, for example, approximately 30 μm or more, approximately 100 μm or more, approximately 200 μm or more, and approximately 250 μm or more. Preferred ranges for the thickness (total thickness) of the laminate constituting the gasket member 10 include approximately 30 to 300 μm, approximately 30 to 200 μm, approximately 30 to 100 μm, approximately 30 to 50 μm, approximately 100 to 300 μm, approximately 100 to 200 μm, approximately 200 to 300 μm, and approximately 250 to 300 μm.
[0019] For example, as shown in Figure 7, when a single gasket member 10 is installed to surround the electrode-electrolyte membrane laminate, the thickness (total thickness) of the laminate constituting the gasket member 10 is preferably about 400 μm or less, more preferably about 300 μm or less, and also preferably about 30 μm or more, more preferably about 50 μm or more, even more preferably more than 50 μm, and even more preferably about 100 μm or more. Preferred ranges include about 30 to 400 μm, about 30 to 30 μm, about 50 to 400 μm, about 50 to 300 μm, about 50 to 400 μm or less, about 50 to 300 μm or less, about 100 to 400 μm, and about 100 to 300 μm. In this case, the thickness of the base layer 1 is preferably about 300 μm or less, more preferably about 200 μm or less, and also preferably about 20 μm or more, more preferably about 30 μm or more, and even more preferably 50 μm or more. Preferred ranges include about 20-300 μm, about 20-200 μm, about 30-300 μm, about 30-200 μm, about 50-300 μm, and about 50-200 μm. The thickness of the adhesive layer 2 is preferably about 200 μm or less, more preferably about 100 μm or less, and also preferably about 10 μm or more, more preferably about 30 μm or more. Preferred ranges include about 10-200 μm, about 10-100 μm, about 30-200 μm, and about 30-100 μm.
[0020] Furthermore, as shown in Figure 6, for example, when two gasket members 10 are installed to surround the electrode-electrolyte membrane laminate, the thickness (total thickness) of the laminate constituting each gasket member 10 is preferably about 200 μm or less, more preferably about 150 μm or less, and also preferably about 25 μm or more, more preferably about 50 μm or more, with preferred ranges including about 25 to 200 μm, about 25 to 150 μm, about 50 to 200 μm, and about 50 to 150 μm. In this case, the thickness of the base layer 1 is preferably about 200 μm or less, more preferably about 150 μm or less, and also preferably about 10 μm or more, more preferably about 15 μm or more, with preferred ranges including about 10 to 200 μm, about 10 to 150 μm, about 15 to 200 μm, and about 15 to 150 μm. Furthermore, the thickness of the adhesive layer 2 is preferably about 100 μm or less, more preferably about 50 μm or less, and also preferably about 3 μm or more, more preferably about 15 μm or more. Preferred ranges include about 3 to 100 μm, about 3 to 50 μm, about 15 to 100 μm, and about 15 to 50 μm.
[0021] In this disclosure, whether to use one gasket member 10 or two gasket members 10 can be appropriately selected depending on the specifications of the polymer electrolyte fuel cell 30. Furthermore, the total thickness of the gasket member 10 and the thickness of each layer can also be appropriately selected depending on the thickness of the polymer electrolyte fuel cell 30.
[0022] In the gasket member 10, the ratio of the total thickness of the base layer 1, adhesive layer 2, and optionally provided anchor coat layer 3 to the total thickness of the laminate constituting the gasket member 10 is preferably 90% or more, more preferably 95% or more, even more preferably 98% or more, and even more preferably 100%. For example, if the gasket member 10 of this disclosure includes a base layer 1 and an adhesive layer 2, the ratio of the total thickness of each of these layers to the total thickness of the laminate constituting the gasket member 10 is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more. Also, if the gasket member 10 of this disclosure is a laminate including a base layer 1, an adhesive layer 2, and an anchor coat layer 3, the ratio of the total thickness of each of these layers to the total thickness of the laminate constituting the gasket member 10 is, for example, 80% or more, preferably 90% or more, more preferably 95% or more, even more preferably 98% or more, and even more preferably 100%.
[0023] The laminate constituting the gasket member 10 of this disclosure has a fracture elongation retention rate of 60% or more after being left standing in water at 120°C for 300 hours. This provides excellent hydrolysis resistance in high-temperature environments. The method for measuring the fracture elongation retention rate of the gasket member 10 is as follows.
[0024] <Method for measuring the elongation retention rate at break> The elongation retention rate at break was determined by the following method. Specifically, the sample was immersed in water at 120°C and left to stand for 300 hours. After that, the elongation at break of the sample was measured, and the obtained measurement value was divided by the elongation at break before the durability test (initial elongation at break) to determine the elongation retention rate at break. The elongation at break was measured by cutting the film into strips with a width (TD) of 15 mm and a length (MD) of 50 mm, and pulling them using a tensile testing machine at a tensile speed of 200 mm / min and a gauge length of 20 mm. The elongation at break was measured. The test environment was 23°C, and the average of three measurements was used. Breaking elongation retention rate (%) = Breaking elongation after durability test ÷ Breaking elongation before durability test (initial breaking elongation) × 100
[0025] Furthermore, one method for confirming the MD (Mass Distribution) of a gasket component involves observing the cross-section of the gasket component (for example, the cross-section of the first adhesive layer, the substrate, or the second adhesive layer) with an electron microscope to confirm the sea-island structure. In this method, the direction parallel to the cross-section where the average diameter of the island shapes perpendicular to the thickness direction of the gasket component is maximized can be determined as the MD. Specifically, the sea-island structure is confirmed by observing electron microscope images of each of the 10 cross-sections (a total of 10 cross-sections) from the cross-section in the longitudinal direction to the direction perpendicular to the cross-section in 10-degree increments. Next, the shape of each individual island is observed in each cross-section. For each island shape, the diameter y is defined as the straight-line distance connecting the leftmost point perpendicular to the thickness direction of the gasket component and the rightmost point perpendicular to that point. In each cross-section, the average of the top 20 island shapes with the largest diameter y is calculated. The direction parallel to the cross-section with the largest average diameter y is determined as the MD.
[0026] From the viewpoint of exhibiting superior properties due to hydrolysis resistance in high-temperature environments, the fracture elongation retention rate of the laminate constituting the gasket member 10 is 60% or more, preferably 65% or more, more preferably 70% or more, even more preferably 75% or more, even more preferably 80% or more, and particularly preferably 85% or more.
[0027] Effective methods for increasing the fracture elongation retention rate of the laminate constituting the gasket member 10 to 60% or more include, for example, using a resin or metal described later as the material for forming the base layer 1, or using a resin with a high glass transition temperature (Tg) among these materials. In addition, it is also effective to use a polyolefin resin (especially acid-modified polyolefin) for the adhesive layer 2 and to provide an anchor coat layer 3 in conjunction with this method. That is, it is effective to use a heat-resistant resin as the base layer 1, and then use an acid-modified polyolefin for the adhesive layer 2 or provide an anchor coat layer 3 to improve adhesion with the heat-resistant resin.
[0028] From the viewpoint of exhibiting superior properties in hydrolysis resistance in high-temperature environments, the hot shrinkage rate of the laminate constituting the gasket member 10 when left standing in a 150°C environment for 30 minutes is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less. Similarly, from the same viewpoint, the hot shrinkage rate of the laminate constituting the gasket member 10 when left standing in a 180°C environment for 30 minutes is preferably 30% or less, more preferably 20% or less, even more preferably 10% or less, even more preferably 3% or less, even more preferably 1% or less, and even more preferably 0.5% or less. The method for measuring the hot shrinkage rate of the gasket member 10 is as follows.
[0029] <Method for measuring hot shrinkage rate at 150°C or 180°C> The hot shrinkage rate is calculated by cutting a gasket material into a test piece measuring 10 cm (MD) x 10 cm (TD), heating it in an oven at 150°C or 180°C for 30 minutes, determining the dimensional change rate before and after heating in the longitudinal and transverse directions (two orthogonal directions) of the test piece based on the following formula (I), and then taking the absolute value of the dimensional change rates in the two directions as the average value. Hot shrinkage rate (%) = {(XY) / X} × 100 ... (I) [X: Dimensions before heating in the oven, Y: Dimensions after heating in the oven]
[0030] 2. Each layer forming the gasket component for polymer electrolyte fuel cell [Base material layer 1] In this disclosure, the base layer 1 is a layer provided for purposes such as enabling the gasket member 10 to function as a base material. The base layer 1 is located between the two adhesive layers 2.
[0031] The base layer 1 is preferably formed from a material with excellent hydrolysis resistance, and preferably contains polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyimide, polyetheretherketone, polymethylterpene, polyphenylene oxide, polyphenylene sulfide, fluororesin, metal, etc. When these materials are used to form the base layer 1, the base layer 1 may contain one type of these material or two or more types.
[0032] Examples of polyolefins include polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; ethylene-α-olefin copolymers; polypropylene such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymer of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymer of propylene and ethylene); propylene-α-olefin copolymers; and ethylene-butene-propylene terpolymers. Among these, polypropylene is preferred. When polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer. Furthermore, the polyolefin resin may be an acid-modified polyolefin. When the base layer 1 contains polyolefin, the base layer 1 may contain only one type of polyolefin or two or more types.
[0033] Acid-modified polyolefins are polymers modified by block polymerization or graft polymerization of polyolefins with an acid component. As the polyolefin to be acid-modified, the above-mentioned polyolefins, copolymers obtained by copolymerizing the above-mentioned polyolefins with polar molecules such as acrylic acid or methacrylic acid, or polymers such as cross-linked polyolefins can also be used. Examples of acid components used for acid modification include carboxylic acids or their anhydrides, such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride. Preferred acid-modified polyolefins include polyolefins modified with carboxylic acids or their anhydrides, polypropylenes modified with carboxylic acids or their anhydrides, maleic anhydride-modified polyolefins, and maleic anhydride-modified polypropylenes. When the base layer 1 contains an acid-modified polyolefin, the base layer 1 may contain only one type of acid-modified polyolefin or two or more types.
[0034] Specifically, polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (where I represents isophthalic acid and T represents terephthalic acid), which contain constituent units derived from terephthalic acid and / or isophthalic acid; aromatic polyamides such as polyamide MXD6 (polymetaxylylene adipamide); alicyclic polyamides such as polyamide PACM6 (polybis(4-aminocyclohexyl)methaneadipamide); polyamides copolymerized with lactam components or isocyanate components such as 4,4'-diphenylmethane-diisocyanate; polyesteramide copolymers and polyether esteramide copolymers, which are copolymers of copolymerized polyamides with polyester or polyalkylene ether glycol; and other polymers of these polyamides. If the base layer 1 contains polyamide, the base layer 1 may contain only one type of polyamide, or it may contain two or more types.
[0035] The polyamide is preferably one that has an α-crystal structure, and specifically, examples include aliphatic polyamides such as nylon 6, nylon 66, nylon 46, and copolymers of nylon 6 and nylon 66.
[0036] Examples of metals include aluminum alloys, copper, zinc, titanium, and stainless steel.
[0037] In this disclosure, from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in a high-temperature environment, the base layer 1 preferably contains polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, or polyolefin, more preferably contains polyethersulfone, polyphenylsulfone, or polyarylate, and even more preferably contains polyphenylsulfone. The base layer 1 is preferably formed of at least one of these resins, and is particularly preferably formed of polyphenylsulfone.
[0038] Furthermore, in this disclosure, from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in a high-temperature environment, the base layer 1 is preferably formed of a resin with excellent heat resistance, and the glass transition temperature (Tg) of the resin forming the base layer 1 is preferably about 160°C or higher, more preferably about 180°C or higher, and even more preferably about 200°C or higher. The upper limit of the glass transition temperature (Tg) is, for example, about 450°C or lower. The glass transition temperature (Tg) refers to the baseline displacement point of the DSC curve measured by a differential scanning calorimeter (DSC).
[0039] The base layer 1 may be a film or a nonwoven fabric. For example, if the base layer 1 is a film, it can be suitably formed from the aforementioned resin or metal film. Also, if the base layer 1 is a nonwoven fabric, it can be suitably formed from the aforementioned resin or metal nonwoven fabric. When the base layer 1 is a nonwoven fabric, the adhesive layer 2 can be impregnated into the gaps of the nonwoven base layer 1, thereby increasing the physical adhesion between the base layer 1 and the adhesive layer 2. Therefore, when the base layer 1 is a nonwoven fabric, the anchor coat layer 3, described later, may be provided on the surface of the base layer 1, but the adhesion between the base layer 1 and the adhesive layer 2 can be sufficiently increased even without providing the anchor coat layer 3. On the other hand, when the base layer 1 is a film, it is preferable to provide the anchor coat layer 3 on the surface of the base layer 1 from the viewpoint of increasing the adhesion between the base layer 1 and the adhesive layer 2.
[0040] The base layer 1 may be a single layer or may consist of two or more layers. If the base layer 1 consists of two or more layers, the materials and thicknesses of each layer may be the same or different.
[0041] Furthermore, at least one of the surface and interior of the base layer 1 may contain additives such as fillers, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents. Specific examples of additives include metal oxide particles such as alumina, silica, and titania. Only one type of additive may be used, or two or more types may be mixed and used.
[0042] In the present disclosure, the thickness of the base material layer 1 is appropriately adjusted according to the size of the solid polymer fuel cell and the like. From the viewpoint of suitably enhancing the hydrolysis resistance of the gasket member 10 in a high-temperature environment, it is preferably about 20 μm or more, more preferably about 40 μm or more, still more preferably about 50 μm or more, and even more preferably 100 μm or more. Also, it is preferably about 200 μm or less, more preferably about 150 μm or less, still more preferably about 100 μm or less. Preferred ranges of the thickness of the base material layer 1 include about 20 to 200 μm, about 20 to 150 μm, about 20 to 100 μm, about 40 to 200 μm, about 40 to 150 μm, about 40 to 100 μm, about 100 to 200 μm, and about 100 to 150 μm.
[0043] When the base material layer 1 is in the form of a non-woven fabric, the basis weight of the base material layer 1 is appropriately adjusted according to the size of the solid polymer fuel cell and the like. From the viewpoint of suitably enhancing the hydrolysis resistance of the gasket member 10 in a high-temperature environment, it is preferably about 5 g / m 2 or more, more preferably about 10 g / m 2 or more, still more preferably about 15 g / m 2 or more. Also, it is preferably about 50 g / m 2 or less, more preferably about 40 g / m 2 or less, still more preferably about 30 g / m 2 or less. When the base material layer 1 is in the form of a non-woven fabric, preferred ranges of the basis weight of the base material layer 1 include about 5 to 50 g / m 2 level, about 5 to 40 g / m 2 level, about 5 to 30 g / m 2 level, about 10 to 50 g / m 2 level, about 10 to 40 g / m 2 level, about 10 to 30 g / m 2 level, about 15 to 50 g / m 2 level, about 15 to 40 g / m 2 level, about 15 to 30 g / m 2 level.
[0044] [Adhesive layer 2] In the gasket member 10, the adhesive layers 2 are arranged on both sides of the base layer 1. The adhesive layers 2 on both sides of the gasket member 10 constitute the outermost layer of the gasket member 10, with one adhesive layer 2 positioned on the electrolyte membrane 21 side and the other adhesive layer 2 positioned on the separator 25 side (see Figure 6). The adhesive layer 2 positioned on the electrolyte membrane 21 side and the adhesive layer 2 positioned on the separator 25 side may be the same in material, thickness, etc., or they may be different. In addition, at least one of the surface and interior of the adhesive layer 2 may contain additives such as fillers, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents. Specific examples of additives include metal oxide particles such as alumina, silica, and titania. Only one type of additive may be used, or two or more types may be mixed and used.
[0045] The adhesive layer 2 is preferably formed from a resin that has excellent adhesion to the separator 25 and the electrolyte membrane 21. Examples of resins used to form the adhesive layer 2 include polyolefin resins, adhesives (acrylic resins, aliphatic polyamides, etc.), and thermosetting resins (epoxy resins, phenolic resins, etc.). The adhesive layer 2 may contain only one type of resin or two or more types.
[0046] Examples of polyolefin resins include those exemplified for the base layer 1. Among these, the adhesive layer 2 preferably contains at least one of acid-modified polyolefin, imine-modified polyolefin, or carbodiimide-modified polyolefin, and is more preferably formed of acid-modified polyolefin, due to its excellent adhesion to the metal separator 25. Furthermore, among acid-modified polyolefins, acid-modified polypropylene is preferred. In this disclosure, by using acid-modified polyolefin, the hydrolysis resistance of the gasket member 10 in high-temperature environments can be suitably improved together with the base layer 1.
[0047] The adhesive layer 2 may be a single layer or may consist of two or more layers. If the adhesive layer 2 consists of two or more layers, the materials and thicknesses of each layer may be the same or different. Even when the adhesive layer 2 consists of two or more layers, the outermost layer of the gasket member 10 preferably contains an acid-modified polyolefin, and more preferably is formed from an acid-modified polyolefin, because it has excellent adhesion to the metal separator 25.
[0048] The thickness of the adhesive layer 2 is adjusted as appropriate depending on the size of the polymer electrolyte fuel cell, but from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in a high-temperature environment, it is preferably about 10 μm or more, more preferably about 15 μm or more, even more preferably about 20 μm or more, and also preferably about 100 μm or less, more preferably about 80 μm or less, and even more preferably about 60 μm or less. Preferred ranges for the thickness of the adhesive layer 2 include about 10 to 100 μm, about 10 to 80 μm, about 10 to 60 μm, about 15 to 100 μm, about 15 to 80 μm, about 15 to 60 μm, about 20 to 100 μm, about 20 to 80 μm, and about 20 to 60 μm.
[0049] The laminate of the base layer 1 and the adhesive layers 2 on both sides can be manufactured, for example, by extruding the resin that forms the adhesive layers 2 onto both sides of a pre-prepared base layer 1, or by simultaneously extruding the resin that forms the base layer 1 and the resin that forms the adhesive layers 2. Alternatively, the base layer 1 can be manufactured by extruding it between pre-prepared adhesive layers 2. The resin extrusion and lamination method is not particularly limited, but known methods such as the extrusion lamination method, T-die method, inflation method, and thermal lamination method can be applied. When providing the anchor coat layer 3 described later, the resin that forms the anchor coat layer 3 can be applied to at least one side of the surface of the base layer 1, and the adhesive layers can be laminated on top of that.
[0050] [Anchor Coat Layer 3] The anchor coat layer 3 is a layer provided on at least one side of the surface of the base layer 1, as needed, for the purpose of improving the adhesion between the base layer 1 and the adhesive layer 2. Preferably, the anchor coat layer 3 is provided on both sides of the base layer 1.
[0051] As described above, the base layer 1 is preferably made of a resin with excellent heat resistance, but resins with excellent heat resistance generally have low adhesion to other resins. Therefore, when using a highly heat-resistant resin film with a glass transition temperature (Tg) of approximately 160°C or higher for the base layer 1, it is effective to provide an anchor coat layer 3 from the viewpoint of improving the adhesion between the base layer 1 and the adhesive layer 2.
[0052] The material used to form the anchor coat layer 3 is not particularly limited as long as it enhances the adhesion between the base layer 1 and the adhesive layer 2, but isocyanate-based, polyethyleneimine-based, polyester-based, polyurethane-based, polyvinyl butyral-based, acrylic-based, aminoethylated acrylic polymer-based, styrene / maleic acid copolymer-based, rubber-based, epoxy-based resins are preferred. One or more of these resins can be used in combination.
[0053] While there are no particular limitations on the compound having an isocyanate group, polyfunctional isocyanate compounds are preferred from the viewpoint of effectively improving the adhesion between the substrate layer 1 and the adhesive layer 2. The polyfunctional isocyanate compound is not particularly limited as long as it is a compound having two or more isocyanate groups. Specific examples of polyfunctional isocyanate curing agents include pentane diisocyanate (PDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), m-xylylene diisocyanate (XDI), polymerized or nurated versions thereof, mixtures thereof, and copolymers with other polymers. Adducts, burettes, and isocyanurates are also examples. Other examples of triisocyanates include triphenylmethane-4,4',4"-triisocyanate and tris(p-isocyanatephenyl)thiophosphorate. The compound having an isocyanate group used to form the anchor coat layer 3 may be one type or two or more types.
[0054] Examples of polyurethane-based materials include two-component mixtures of polyester resin and polyfunctional isocyanate compounds, and two-component mixtures of polycarbonate diol and polyfunctional isocyanate compounds. Specific examples of polyurethane-based materials include two-component mixtures of polyester resin and hexamethylene diisocyanate, and two-component mixtures of polycarbonate diol and polymethylene polyphenyl polyisocyanate.
[0055] The thickness of the anchor coat layer 3 is adjusted as appropriate depending on the size of the polymer electrolyte fuel cell, but from the viewpoint of suitably improving the hydrolysis resistance of the gasket member 10 in high-temperature environments, it is preferably about 0.02 g / m². 2 More preferably 0.05 g / m 2 More preferably, about 0.1 g / m 2 More preferably, about 0.3 g / m 2 More preferably, about 0.5 g / m 2The above is true, and preferably about 5 g / m 2 More precisely, approximately 4 g / m 2 More preferably, about 3 g / m 2 The following is a preferred range for the thickness of the anchor coat layer 3: 0.02 to 5 g / m². 2 degree, 0.02~4g / m 2 degree, 0.02~3g / m 2 degree, 0.05~5g / m 2 degree, 0.05~4g / m 2 degree, 0.05~3g / m 2 degree, 0.1~5g / m 2 degree, 0.1~4g / m 2 degree, 0.1~3g / m 2 degree, 0.3~5g / m 2 degree, 0.3~4g / m 2 degree, 0.3~3g / m 2 degree, 0.5~5g / m 2 degree, 0.5~4g / m 2 degree, 0.5~3g / m 2 The degree can be described as follows.
[0056] 3. Electrode-electrolyte membrane laminate with gasket component The electrode-electrolyte membrane laminate 20 with gasket member of this disclosure is an electrode-electrolyte membrane laminate to which the gasket member 10 of this disclosure is attached (see Figure 4). Specifically, the electrode-electrolyte membrane laminate 20 with gasket member of this disclosure comprises an electrode-electrolyte membrane laminate in which catalyst layers 22, 23 and a gas diffusion layer 24 are arranged on both sides of an electrolyte membrane 21, and a frame-shaped gasket member 10 arranged to cover the outer peripheral edge of the electrode-electrolyte membrane laminate. The gasket member 10 is composed of a laminate comprising at least a base layer 1 and adhesive layers 2 arranged on both sides of the base layer 1, and the laminate is characterized in that it retains a break elongation rate of 60% or more after being left standing in water at 120°C for 300 hours.
[0057] The gasket member 10 of this disclosure may be a pair of members bonded together, arranged to cover the outer peripheral edge of the electrode-electrolyte membrane laminate from one side and the other side, as shown in Figure 4, or it may be a single gasket member 10 that covers the outer peripheral edge of the electrode-electrolyte membrane laminate, as shown in Figure 7.
[0058] The electrolyte membrane 21 is not particularly limited and may be, for example, one used in a known polymer electrolyte fuel cell. The electrolyte membrane 21 is formed, for example, by coating a substrate with a solution containing a hydrogen ion conductive polymer electrolyte and drying it. Examples of hydrogen ion conductive polymer electrolytes include perfluorosulfonic acid-based fluorine ion exchange resins, and more specifically, perfluorocarbon sulfonic acid-based polymers (PFS polymers) in which the CH bonds of a hydrocarbon-based ion exchange membrane are replaced with fluorine. By introducing highly electronegative fluorine atoms, chemical stability is achieved, the degree of dissociation of sulfonic acid groups is high, and high ionic conductivity can be realized. Specific examples of such hydrogen ion conductive polymer electrolytes include "Nafion" (registered trademark) from DuPont, "Flemion" (registered trademark) from Asahi Glass Co., Ltd., "Aciplex" (registered trademark) from Asahi Kasei Corporation, and "GoreSelect" (registered trademark) from Gore. The concentration of the hydrogen ion-conducting polymer electrolyte in the hydrogen ion-conducting polymer electrolyte-containing solution is typically about 5 to 60% by weight, preferably about 20 to 40% by weight. The thickness of the electrolyte membrane 21 is typically about 3 to 50 μm, preferably about 5 to 20 μm. Although not shown in the figures, the end face of the electrolyte membrane 21 does not need to be aligned with the end faces of the catalyst layers 22 and 23. For example, the end face of the electrolyte membrane 21 may protrude beyond the end faces of the catalyst layers 22 and 23, and the adhesive layer 2 of the gasket member 10 may cover the protruding portion of the electrolyte membrane 21.
[0059] Specifically, catalyst layers 22 and 23 consist of an anode catalyst layer and a cathode catalyst layer. Catalyst layers 22 and 23 are not particularly limited and may be, for example, those used in known polymer electrolyte fuel cells. Catalyst layers 22 and 23 are, for example, platinum-containing catalyst layers. Catalyst layers 22 and 23 contain, for example, carbon particles supporting catalyst particles and a hydrogen ion-conducting polymer electrolyte. Examples of catalyst particles include platinum and platinum compounds. Examples of platinum compounds include alloys of platinum with at least one metal selected from the group consisting of ruthenium, palladium, nickel, molybdenum, iridium, iron, etc. Typically, the catalyst particles in the cathode catalyst layer are platinum, and the catalyst particles in the anode catalyst layer are alloys of the aforementioned metal and platinum. Furthermore, the same material used for the electrolyte membrane 21 can be used as the hydrogen ion-conducting polymer electrolyte.
[0060] The size and shape of the electrolyte membrane 21 and catalyst layers 22 and 23 are adjusted according to the size of the polymer electrolyte fuel cell, and the size and shape of the gasket member 10 of this disclosure are also adjusted appropriately according to their size so that they function as a gasket member (i.e., they have mechanical strength to withstand hot pressing and exhibit gas barrier properties sufficient to prevent leakage of fuel and oxidizer to the outside).
[0061] 4. Polymer electrolyte fuel cell The polymer electrolyte fuel cell 30 of this disclosure is a polymer electrolyte fuel cell utilizing the gasket member 10 of this disclosure. That is, the polymer electrolyte fuel cell 30 of this disclosure comprises an electrode-electrolyte membrane laminate 20 with a gasket member of this disclosure.
[0062] The polymer electrolyte fuel cell 30 comprises a catalyst layer-electrolyte membrane laminate, and an electrode-electrolyte membrane laminate is formed by forming gas diffusion layers 24 on the catalyst layers 22 and 23 of the catalyst layer-electrolyte membrane laminate, respectively. The catalyst layers 22 and 23 and the gas diffusion layer 24 constitute electrodes (anode and cathode electrodes), respectively. The gasket member 10 of this disclosure is placed on the outer edge of the electrolyte membrane 21 so as to surround these electrodes. Furthermore, a separator 25 with a gas flow path 26 is installed so as to sandwich the electrode-electrolyte membrane laminate on which the gasket member 10 is installed from above and below.
[0063] The gas diffusion layer 24 is not particularly limited and may be, for example, one used in a known polymer electrolyte fuel cell. That is, the gas diffusion layer 24 can be any gas diffusion layer that constitutes the anode or cathode electrode, and is made of a porous conductive substrate in order to efficiently supply the fuel gas and oxidizer gas to the catalyst layers 22 and 23. Examples of porous conductive substrates include carbon paper and carbon cloth.
[0064] The separator 25 is not particularly limited and may be, for example, one used in a known polymer electrolyte fuel cell. The separator 25 can be any conductive plate that is stable in the environment inside the fuel cell, and generally, a metal plate such as titanium, aluminum, copper, or stainless steel with a gas channel 26 formed on it is used. Alternatively, the separator 25 may be made of the above metals, and a coating made of a conductive material such as carbon, silver, chromium nitride, platinum group metals or their oxides, or a conductive polymer may be formed on the surface of the metal.
[0065] The operating temperature of the polymer electrolyte fuel cell 30 of this disclosure is not particularly limited, but since the gasket member 10 has excellent hydrolysis resistance in high-temperature environments, it may be used at operating temperatures of, for example, 60°C or higher, and even 100°C or higher. Increasing the operating temperature of the fuel cell can increase the power density. The upper limit of the operating temperature of the polymer electrolyte fuel cell 30 of this disclosure is, for example, 150°C or lower. [Examples]
[0066] The present disclosure will be described in detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the examples.
[0067] <Manufacturing of gasket components for solid polymer fuel cells> (Example 1) A polysulfone (PSU) film (100 μm thick, Tg 180°C) was prepared as the base layer. Next, a resin composition containing a compound having an isocyanate group (a two-component mixture of polyester resin and hexamethylene diisocyanate) was applied to both sides of the base layer to form an anchor coat layer (0.5 g / m² thick). 2 A layer was formed. Furthermore, an adhesive layer was formed on the surface of each of the anchor coat layers by melt-extruding maleic anhydride-modified polypropylene (PPa) to a thickness of 50 μm, resulting in an adhesive layer (thickness 50 μm) / anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0068] (Example 2) Except for using a polyethersulfone (PESU) film (100 μm thick, Tg 220°C) instead of a polysulfone (PSU) film as the base layer, the procedure was the same as in Example 1, with an adhesive layer (50 μm thick) and an anchor coat layer (0.5 g / m² thick). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0069] (Example 3) Except for using a polyphenylsulfone (PPSU) film (100 μm thick, Tg 220°C) instead of a polysulfone (PSU) film as the base layer, the procedure was the same as in Example 1, with an adhesive layer (50 μm thick) and an anchor coat layer (0.5 g / m² thick). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0070] (Example 4) Except for using a "two-component urethane (a two-component mixture of polycarbonate diol and polymethylene polyphenyl polyisocyanate)" instead of the "resin composition containing a compound having an isocyanate group (a two-component mixture of polyester resin and hexamethylene diisocyanate)" as the resin composition forming the anchor coat layer (anchor coat material), the process was the same as in Example 3, with an adhesive layer (thickness 50 μm) and an anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0071] (Example 5) Except for using "triphenylmethane-4,4',4"-triisocyanate (one-component curing type)" instead of "a resin composition containing a compound having an isocyanate group (a two-component mixture of polyester resin and hexamethylene diisocyanate)" as the resin composition (anchor coat material) for forming the anchor coat layer, the procedure was the same as in Example 3, with an adhesive layer (thickness 50 μm) and an anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0072] (Example 6) Except for using "polymethylene polyphenyl polyisocyanate (one-component curing type)" instead of "resin composition containing a compound having an isocyanate group (polyester resin and hexamethylene diisocyanate two-component mixture)" as the resin composition (anchor coat material) for forming the anchor coat layer, the procedure was the same as in Example 3, with an adhesive layer (thickness 50 μm) and an anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0073] (Example 7) Except for using "polyisocyanate of hexamethylene diisocyanate (one-component curing type)" instead of "resin composition containing a compound having an isocyanate group (two-component mixture of polyester resin and hexamethylene diisocyanate)" as the resin composition (anchor coat material) for forming the anchor coat layer, the procedure was the same as in Example 3, with an adhesive layer (thickness 50 μm) and an anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0074] (Comparative Example 1) Except for using polyethylene naphthalate (PEN) film (thickness 100 μm, Tg 155℃), which is commonly used as the base layer for gasket components for polymer electrolyte fuel cells, instead of polysulfone (PSU) film as the base layer, the procedure was the same as in Example 1, with an adhesive layer (thickness 50 μm) and an anchor coat layer (thickness 0.5 g / m²). 2 ) / Substrate layer (thickness 100 μm) / Anchor coat layer (thickness 0.5 g / m 2 A gasket member (200 μm thick) for a polymer electrolyte fuel cell was obtained by sequentially laminating adhesive layers (50 μm thick).
[0075] <Elongation retention rate at break (evaluation of hydrolysis resistance in high-temperature environments)> For the solid polymer fuel cell gasket members manufactured in the examples and comparative examples, the retention rate of elongation at break (%) was measured after being left to stand for 300 hours in 120°C water (in a heat-resistant and pressure-resistant container) under the following measurement conditions. The results are shown in Table 1. After being immersed in 120°C water and left to stand for 300 hours, the elongation at break of the sample was measured, and the retention rate of elongation at break was calculated by dividing the obtained measurement value by the elongation at break before the durability test (initial elongation at break). Elongation at break was measured by cutting the film into strips with a width (TD) of 15 mm and a length (MD) of 50 mm, and pulling them using a tensile testing machine at a tensile speed of 200 mm / min and a gauge length of 20 mm. The elongation until breakage was measured. The test environment was 23°C, and the average value of three measurements was used. Breaking elongation retention rate (%) = Breaking elongation after durability test ÷ Breaking elongation before durability test (initial breaking elongation) × 100
[0076] <Adhesion strength to separators> The adhesive strength (N) of the solid polymer fuel cell gasket members manufactured in the examples and comparative examples was measured against a stainless steel plate (SUS304) used as a separator, under the following measurement conditions. The results are shown in Table 1. In accordance with the provisions of JIS K7127:1999, the peel strength in a 25°C environment was measured as follows. A sample was cut from the sample into strips with a width of 15 mm in the TD direction, and the metal-adhesive layer was bonded by hot pressing to create a sample for measurement. Next, the sample for measurement was attached to a tensile testing machine, and the adhesive strength (peel strength) between the metal layer and the adhesive layer was measured under the conditions of a tensile speed of 300 mm / min and a gauge length of 50 mm. The maximum strength at the time of peeling was defined as the seal strength (N / 15 mm). The average value of three measurements was used. The hot pressing conditions were fixed at a temperature of 170°C, a surface pressure of 1 MPa, and a pressing time of 20 seconds (s), and measurements were taken by changing the temperature. The peeling direction was set to 180°, and the size of the bonded area of the stainless steel plate (SUS304) used for measurement was 15 mm in width and 30 mm in length.
[0077] <Measurement of hot shrinkage rate at 180℃> The hot shrinkage rate was calculated by cutting a gasket material into a 10cm x 10cm (MD) test piece, heating it in a 180°C oven for 30 minutes, and determining the dimensional change rate before and after heating in the longitudinal and transverse directions (two orthogonal directions) of the test piece based on the following formula (I). The absolute value of the dimensional change rates in the two directions was then used as the average value. Hot shrinkage rate (%) = {(XY) / X} × 100 ... (I) [X: Dimensions before heating in the oven, Y: Dimensions after heating in the oven]
[0078] [Table 1]
[0079] The gasket members of Examples 1 to 7 were composed of a laminate comprising a base layer and adhesive layers arranged on both sides of the base layer. After being left to stand in water at 120°C for 300 hours, they maintained a break elongation rate of 60% or more, demonstrating excellent hydrolysis resistance in high-temperature environments. Furthermore, the gasket members of Examples 1 to 7 also exhibited good adhesion to the separator.
[0080] As described above, this disclosure provides inventions in the following embodiments. Item 1. It is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, The laminate is a gasket member for a polymer electrolyte fuel cell, wherein the elongation retention rate at break after being left standing in water at 120°C for 300 hours is 60% or more. Item 2. The gasket member for polymer electrolyte fuel cell according to Item 1, wherein the base layer comprises at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyimide, polyetheretherketone, polymethylterpene, polyphenylene oxide, polyphenylene sulfide, fluororesin, and metal. Item 3. The gasket member for a polymer electrolyte fuel cell according to item 1 or 2, wherein the base layer is a nonwoven fabric. Item 4. A gasket member for a polymer electrolyte fuel cell according to any one of items 1 to 3, comprising an anchor coat layer on at least one side of the surface of the base material layer. Item 5. A gasket member for a polymer electrolyte fuel cell according to any one of items 1 to 4, wherein the thickness of the base material layer is 20 μm or more and 200 μm or less. Item 6. A gasket member for a polymer electrolyte fuel cell according to any one of items 1 to 5, wherein the thickness of the adhesive layer is 10 μm or more and 100 μm or less. Item 7. An electrode-electrolyte membrane laminate in which a catalyst layer and a gas diffusion layer are arranged on both sides of the electrolyte membrane, A frame-shaped gasket member is positioned to cover the outer edge of the electrode-electrolyte membrane laminate, Equipped with, The gasket member is composed of a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer. The laminate is an electrode-electrolyte membrane laminate with a gasket member, wherein the elongation retention rate at break after being left standing in water at 120°C for 300 hours is 60% or more. Item 8. The electrode-electrolyte membrane laminate with gasket member according to Item 7, wherein the substrate layer comprises at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyimide, polyetheretherketone, polymethylterpene, polyphenylene oxide, polyphenylene sulfide, fluororesin, and metal. Item 9. The electrode-electrolyte membrane laminate with gasket member according to item 7 or 8, wherein the base layer is a nonwoven fabric. Item 10. An electrode-electrolyte membrane laminate with a gasket member according to any one of items 7 to 9, comprising an anchor coat layer on at least one side of the surface of the base layer. Item 11. An electrode-electrolyte membrane laminate with a gasket member according to any one of items 7 to 10, wherein the thickness of the substrate layer is 20 μm or more and 200 μm or less. Item 12. An electrode-electrolyte membrane laminate with a gasket member according to any one of items 7 to 11, wherein the thickness of the adhesive layer is 10 μm or more and 100 μm or less. Item 13. A polymer electrolyte fuel cell comprising an electrode-electrolyte membrane laminate with a gasket component as described in any one of items 7 to 12. Item 14. A method for manufacturing a gasket member for a polymer electrolyte fuel cell, comprising a laminate comprising at least a base layer and adhesive layers disposed on both sides of the base layer, The process includes laminating the adhesive layer on both sides of the base material layer. A method for manufacturing a gasket member for a polymer electrolyte fuel cell, wherein the laminate has a fracture elongation retention rate of 60% or more after being left standing in water at 120°C for 300 hours. [Explanation of symbols]
[0081] 1 Base material layer 2 Adhesive layer 3. Anchor Coat Layer 10 Gasket components 11 Opening 20 Electrode-electrolyte membrane laminate with gasket component 21 Electrolyte membrane 22,23 Catalyst layer 24 Gas diffusion layer 25 Separators 26 Gas flow path 30 Polymer electrolyte fuel cell
Claims
1. The laminate includes at least a base layer and an adhesive layer disposed on both sides of the base layer, the substrate layer contains at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyetheretherketone, polymethyltempene, polyphenylene oxide, polyphenylene sulfide, and metal; The laminate has a breaking elongation retention rate of 80% or more after being left to stand in water at 120° C. for 300 hours.
2. The gasket member for a polymer electrolyte fuel cell according to claim 1 , wherein the base layer is a nonwoven fabric.
3. 3. The gasket member for a polymer electrolyte fuel cell according to claim 1, further comprising an anchor coat layer on at least one side of a surface of the base layer.
4. 4. The gasket member for a polymer electrolyte fuel cell according to claim 1, wherein the thickness of the base layer is 20 μm or more and 200 μm or less.
5. 5. The gasket member for a polymer electrolyte fuel cell according to claim 1, wherein the adhesive layer has a thickness of 10 μm or more and 100 μm or less.
6. an electrode-electrolyte membrane laminate in which a catalyst layer and a gas diffusion layer are disposed on both sides of an electrolyte membrane; A frame-shaped gasket member arranged to cover the outer peripheral edge of the electrode-electrolyte membrane stack; Equipped with The gasket member is composed of a laminate including at least a base material layer and adhesive layers disposed on both sides of the base material layer, the substrate layer contains at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyetheretherketone, polymethyltempene, polyphenylene oxide, polyphenylene sulfide, and metal; The laminate is an electrode-electrolyte membrane laminate with a gasket member, the laminate having a breaking elongation retention rate of 80% or more after being left to stand in water at 120° C. for 300 hours.
7. 7. The electrode-electrolyte membrane laminate with gasket member according to claim 6, wherein the base material layer is a nonwoven fabric.
8. 8. The electrode-electrolyte membrane laminate with gasket member according to claim 6, further comprising an anchor coat layer on at least one side of the surface of the base layer.
9. 9. The electrode-electrolyte membrane laminate with gasket member according to claim 6, wherein the thickness of the substrate layer is from 20 μm to 200 μm.
10. 10. The electrode-electrolyte membrane laminate with a gasket member according to claim 6, wherein the adhesive layer has a thickness of 10 μm or more and 100 μm or less.
11. A polymer electrolyte fuel cell comprising the gasket member-attached electrode-electrolyte membrane laminate according to any one of claims 6 to 10.
12. A method for producing a gasket member for a polymer electrolyte fuel cell, the gasket member being constituted by a laminate including at least a base layer and adhesive layers disposed on both sides of the base layer, the method comprising the steps of: The method includes a step of laminating the adhesive layer on both sides of the base material layer, the substrate layer contains at least one selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylate, polyolefin, polyamide, polyetheretherketone, polymethyltempene, polyphenylene oxide, polyphenylene sulfide, and metal; The laminate has a breaking elongation retention rate of 80% or more after being left in water at 120° C. for 300 hours.