Method for manufacturing vapor deposition mask
Patent Information
- Application Number
- JP2021183562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-11-10
AI Technical Summary
The manufacturing process of vapor deposition masks faces challenges in accurately measuring the shrinkage rate of the plating layer, leading to displacement of the opening region from the desired position due to stress, which cannot be measured until the plating layer is separated from the supporting substrate, and using dummy substrates results in inaccurate evaluations.
A method is developed to measure the warp and internal stress of the supporting substrate during the manufacturing process, allowing for the calculation of the shrinkage rate of the mask body without separating it from the substrate, and adjusting the drawing coordinates to ensure the shrinkage rate falls within a predetermined range, thereby improving positional accuracy.
This method enables accurate prediction and control of the shrinkage rate, reducing the number of defective masks and improving yield by allowing early feedback and correction of manufacturing conditions, ensuring precise alignment of the opening regions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a vapor deposition mask. In particular, the present invention relates to a method for manufacturing a vapor deposition mask provided with a thin film mask body on a mask frame.
[0002] As an example of a flat panel display device, a liquid crystal display device and an organic EL display device can be mentioned. These display devices are structures in which thin films containing various materials such as insulators, semiconductors, and conductors are laminated on a substrate. These thin films are appropriately patterned and connected to realize the function as a display device.
[0003] The methods for forming thin films are roughly classified into a vapor phase method, a liquid phase method, and a solid phase method. The vapor phase method is classified into a physical vapor phase method and a chemical vapor phase method. As a typical example of the physical vapor phase method, a vapor deposition method is known. The simplest method among the vapor deposition methods is the vacuum vapor deposition method. In the vacuum vapor deposition method, by heating a material under high vacuum, the material is sublimated or evaporated to generate a vapor of the material (hereinafter, these are collectively referred to as vaporization). In the region for depositing this material (hereinafter, the vapor deposition region), the vaporized material solidifies and deposits to obtain a thin film of the material. In order to selectively form a thin film on the vapor deposition region and prevent the material from depositing on other regions (hereinafter, the non-vapor deposition region), vacuum vapor deposition is performed using a mask (vapor deposition mask) (see Patent Documents 1 and 2).
[0004] The vapor deposition mask has a mask frame for fixing the mask body joined to the mask body on which a vapor deposition pattern is formed. The mask body is formed by using a photoresist layer having a predetermined pattern formed on a support substrate via a metal layer as a mask, forming a plating film, joining the frame, and then separating the mask body from the support substrate and the underlying metal layer.
Prior Art Documents
Patent Documents
[0005]
Patent Document 1
[0006] In the manufacturing process of the mask body, when the plating layer, which consists of a fine pattern formed by electroplating on a support substrate, is separated from the support substrate, the plating layer shrinks due to stress. This causes the opening area to shift from the desired position, making it crucial to control the shrinkage rate of the plating layer. However, since the shrinkage rate of the plating layer cannot be measured without separating it from the support substrate, it took several days to feed back the measured shrinkage rate of the plating layer into the fine pattern formation process and the plating layer formation process.
[0007] On the other hand, there is a method to measure the shrinkage rate of the plating layer by forming the plating layer on a dummy support substrate, immediately peeling it off, and then measuring the shrinkage rate of the plating layer. In this case, the plating layer needs to be formed thickly so that it is not damaged or deformed when peeled off on its own. However, the state of the plating layer peeled off from the dummy support substrate is different from the plating layer that makes up the actual mask body, so it was not possible to accurately evaluate the shrinkage rate.
[0008] In view of the above problems, one of the objectives of one embodiment of the present invention is to provide a method for manufacturing a vapor deposition mask with improved positional accuracy of the aperture region. [Means for solving the problem]
[0009] A method for manufacturing a vapor deposition mask according to one embodiment of the present invention involves forming a photoresist layer with a predetermined pattern on a support substrate via a base metal layer, positioning the support substrate so that its first surface is perpendicular to the horizontal plane, measuring the first amount of warpage of the support substrate, forming a mask body by electroforming metal into areas of the base metal layer where the photoresist layer is not formed, positioning the support substrate so that its first surface is perpendicular to the horizontal plane, measuring the second amount of warpage of the support substrate, calculating the shrinkage rate of the mask body based on the change in warpage calculated based on the first and second amounts of warpage and the internal stress of the support substrate calculated based on the change in warpage, and changing the drawing coordinates of each predetermined pattern in the next mask body to be manufactured according to the shrinkage rate of the mask body. [Brief explanation of the drawing]
[0010] [Figure 1A] This is a plan view of a vapor deposition mask relating to one embodiment of the present invention. [Figure 1B] This is a plan view of a vapor deposition mask relating to one embodiment of the present invention. [Figure 1C] This is a cross-sectional view of a vapor deposition mask according to one embodiment of the present invention. [Figure 2] This is a flowchart illustrating the outline of the manufacturing process for a vapor deposition mask according to one embodiment of the present invention. [Figure 3] This is a flowchart illustrating the process of adjusting the shrinkage rate of the mask body. [Figure 4A] This is a cross-sectional view showing the manufacturing method of the mask body. [Figure 4B] This is a cross-sectional view showing the manufacturing method of the mask body. [Figure 4C] This is a cross-sectional view showing the manufacturing method of the mask body. [Figure 5] This is a simulation result of the amount of warping when a plating layer is formed on a SUS substrate. [Figure 6]The simulation results of the warpage amount when a plating layer is formed on a glass substrate. [Figure 7] It is a diagram schematically showing regions 301 to 305 shown in FIG. 5 on a support substrate. [Figure 8] It is an example of a photoresist layer after adjusting the magnification of a predetermined pattern based on the shrinkage rate of the mask body obtained in FIG. 5. [Figure 9A] It is a cross-sectional view showing a method of forming a mask frame on a mask body. [Figure 9B] It is a cross-sectional view showing a method of forming a mask frame on a mask body. [Figure 9C] It is a cross-sectional view showing a method of forming a mask frame on a mask body. [Figure 9D] It is a cross-sectional view showing a method of forming a mask frame on a mask body. [Figure 9E] It is a cross-sectional view showing a method of forming a mask frame on a mask body.
Embodiments for Carrying Out the Invention
[0011] Hereinafter, each embodiment of the present invention will be described with reference to the drawings and the like. However, the present invention can be implemented in various modes without departing from the gist thereof, and is not to be construed as being limited to the description content of the embodiments illustrated below.
[0012] For the sake of clearer explanation, the drawings may schematically represent the width, thickness, shape, etc. of each part compared to the actual mode. However, the examples shown in the drawings are merely examples, and unless otherwise specifically described for the illustrated mode, they do not limit the interpretation of the present invention. In this specification and each figure, the same components as those described above for the previously presented figures may be denoted by the same reference numerals, and detailed description may be omitted as appropriate.
[0013] In this specification and the claims, when expressing the aspect where another structure is disposed on a certain structure, if simply denoted as "on", unless otherwise specified, it is defined to include both the case where another structure is disposed directly above the certain structure so as to be in contact with the certain structure, and the case where another structure is disposed above the certain structure with yet another structure intervening therebetween.
[0014] (First Embodiment) The configuration of the vapor deposition mask according to an embodiment of the present invention will be described with reference to FIGS. 1A to 1C.
[0015] FIGS. 1A and 1B are plan views of a vapor deposition mask 10 according to an embodiment of the present invention. Specifically, FIG. 1A is a plan view seen from the first surface 110a of the mask body 110 of the vapor deposition mask 10, and FIG. 1B is a plan view seen from the second surface 110b on the opposite side of the first surface 110a of the mask body 110 of the vapor deposition mask 10. Further, FIG. 1C is a cross-sectional view of the vapor deposition mask 10 according to an embodiment of the present invention. Specifically, FIG. 1C is a cross-sectional view of the vapor deposition mask 10 cut along the line A1 - A2 shown in FIG. 1A or FIG. 1B.
[0016] The vapor deposition mask 10 includes a mask body 110, a mask frame 120, and a connection portion 130. The mask body 110 has a first surface 110a and a second surface 110b. As shown in FIGS. 1A and 1B, the mask frame 120 and the connection portion 130 are provided on the first surface 110a of the mask body 110. Also, in a plan view, the mask frame 120 and the connection portion 130 overlap the mask body 110. As shown in FIG. 1A, in a plan view seen from the first surface 110a of the mask body 110, the mask frame 120 and the connection portion 130 are exposed from the mask body 110. On the other hand, as shown in FIG. 1B, in a plan view seen from the second surface 110b of the mask body 110, the mask frame 120 and the connection portion 130 are not exposed from the mask body 110. In other words, in a plan view seen from the second surface 110b of the mask body 110, it can also be said that the mask frame 120 and the connection portion 130 are covered by the mask body 110.
[0017] The mask body 110 includes an open region 111 and a non-open region 112. The open region 111 is provided with an opening 113 that penetrates the mask body 110 and corresponds to the deposition pattern. On the other hand, the non-open region 112 does not have an opening 113. The boundary between the open region 111 and the non-open region 112 is not always clear. However, in many cases, the openings 113 are provided according to the deposition pattern, so the distance between two adjacent openings 113 has a predetermined pitch. Therefore, it is possible to distinguish between the open region 111 and the non-open region 112 based on a predetermined pitch of the deposition pattern.
[0018] The thickness of the mask body 110 is, for example, 1 μm to 10 μm. Furthermore, it is preferable that the mask body 110 is formed from a material used in electroforming (or electroplating). The mask body 110 is formed by electroforming from a material such as nickel or a nickel alloy.
[0019] When performing a deposition process using a deposition mask 10, the substrate to be deposited is placed on the second surface 110b of the mask body 110. As the substrate to be deposited, for example, a circuit board on which transistors, etc., are formed is used. The deposition mask 10 is fixed inside the chamber of the deposition apparatus by being attracted by magnets provided in the deposition apparatus, with the substrate to be deposited sandwiched between them. In the deposition apparatus, a deposition source is provided on the first surface 110a side of the mask body 110. When the deposition source is heated, the organic material is heated and sublimated or evaporated. In such a deposition process, the organic material is deposited by passing only through the openings 113 of the mask body 110. As a result, a pattern (deposition pattern) corresponding to the openings 113 is formed on the substrate to be deposited. The openings 113 can be provided, for example, in correspondence with the arrangement of pixels of a display device and can be arranged in a matrix. The openings 113 are arranged in the x-axis direction (also called the first direction) and the y-axis direction (also called the second direction). In Figure 1A, if the center of the mask body 110 is taken as the reference point, and the reference point is set to coordinate O(0,0), then the four corners of the substrate will be coordinates A(-x,y), B(-x,-y), C(x,-y), and D(x,-y).
[0020] The mask frame 120 includes a frame portion 121 located on the outer circumference of the deposition mask 10 and a crossbar portion 122 located inside the frame portion 121. The inside of the frame portion 121 of the mask frame 120 is open, but this opening is partitioned by the crossbar portion 122 arranged in a grid pattern. When the size of the mask frame 120 increases, it may be difficult to maintain the parallelism of the mask frame 120 to a predetermined standard due to warping or twisting of the frame portion 121. In the deposition mask 10, the crossbar portion 122 increases the rigidity of the frame portion 121, thereby maintaining the parallelism of the mask frame 120 to a predetermined standard. However, if the size of the deposition mask 10 is small and the rigidity of the frame portion 121 is sufficiently high, the crossbar portion 122 may not be provided.
[0021] The mask frame 120 may be formed by integrating the frame portion 121 and the crossbar portion 122, or the frame portion 121 and the crossbar portion 122 may be manufactured separately and then welded together.
[0022] In Figure 1A, the mask frame 120 is divided into 12 openings by the crossbars 122, but the number of divided openings is not limited to this. The number of divided openings can be appropriately determined according to the size of the substrate to be deposited and the deposition pattern. Also, the arrangement of the crossbars 122 is not limited to a grid. If the mask frame 120 is a rectangle with short sides and long sides, warping or twisting is more likely to occur on the long sides than on the short sides. For this reason, it is preferable to provide the crossbars 122 so as to connect opposite long sides. Furthermore, the arrangement of the crossbars 122 may be in a shape that corresponds to the deposition pattern.
[0023] The width of the frame portion 121 and the width of the crossbar portion 122 can be appropriately determined according to the size of the deposition mask 10. In order to maximize the area of the deposition pattern, it is preferable that the width of the crossbar portion 122 be smaller than the width of the frame portion 121.
[0024] The thickness of the mask frame 120 is, for example, 10 μm to 2000 μm. Furthermore, it is preferable that the mask frame 120 be made of a material with a low coefficient of thermal expansion. The mask frame 120 can be made of materials such as Invar containing iron and nickel, or SuperInvar containing iron, nickel, and cobalt.
[0025] The connecting portion 130 can connect the mask body 110 and the mask frame 120. As shown in Figure 1C, the mask body 110 and the mask frame 120 are in direct contact, but they are not glued or joined together. By joining the connecting portion 130 to the mask body 110 and the mask frame 120, the mask body 110 and the mask frame 120 are connected and fixed together via the connecting portion 130.
[0026] The connecting portion 130 only needs to be provided on at least a part of the side surface of the frame portion 121 or the crossbar portion 122 of the mask frame 120. However, in order to increase the bonding strength between the mask body 110 and the mask frame 120, it is preferable that the connecting portion 130 is provided on more than half of the side surface of the frame portion 121 or the crossbar portion 122, and it is even more preferable that it is provided on the entire side surface of the frame portion 121 or the crossbar portion 122. Furthermore, it is preferable that the connecting portion 130 is formed from a material used in electroforming. For example, the connecting portion 130 is formed from a material such as nickel or a nickel alloy. The material of the connecting portion 130 may be the same as or different from the material of the mask body 110.
[0027] As described above, in the vapor deposition mask 10, the mask body 110 and the mask frame 120 are in direct contact, but the mask body 110 and the mask frame 120 are not directly fixed to each other. Therefore, even if the mask body 110 and the mask frame 120 are made of materials with different coefficients of thermal expansion, the stress on the mask body 110 or the mask frame 120 can be distributed. Alternatively, the mask body 110 and the mask frame 120 may not be in direct contact, and a gap may be provided between them. In this case as well, the stress on the mask body 110 or the mask frame 120 can be distributed.
[0028] In the manufacturing process of the mask body, when the plating layer, which consists of fine patterns formed by electroplating, is separated from the plating support substrate, the plating layer shrinks due to stress. This causes the opening area to shift from the desired position, making it crucial to control the shrinkage rate of the plating layer. However, since the shrinkage rate of the plating layer cannot be measured until the plating layer is separated from the support substrate, it takes several days to feed back the measured shrinkage rate of the plating layer into the fine pattern formation process and the plating layer formation process.
[0029] On the other hand, there is a method to measure the shrinkage rate of the plating layer by forming the plating layer on a dummy support substrate, immediately peeling it off, and then measuring the shrinkage rate of the plating layer. In this case, the plating layer needs to be formed thickly so that it is not damaged or deformed when peeled off on its own. However, the state of the plating layer peeled off from the dummy support substrate is different from the plating layer that makes up the actual mask body, so it is not possible to accurately evaluate the shrinkage rate.
[0030] In view of the above problems, one of the objectives of one embodiment of the present invention is to provide a method for manufacturing a vapor deposition mask with improved positional accuracy of the aperture region.
[0031] In one embodiment of the present invention, an in-line inspection of the shrinkage rate of the mask body is performed during the manufacturing process of the vapor deposition mask, and the inspection results are fed back to the preceding process. This allows the shrinkage rate of the mask body to be inspected at the stage when the mask body is formed, before the vapor deposition mask is completed, and the inspection results can be fed back at an earlier stage. In addition, the number of vapor deposition masks manufactured with a large shrinkage rate and low positional accuracy of the opening area can be reduced. In other words, the yield of usable vapor deposition masks can be improved.
[0032] A method for manufacturing a vapor deposition mask according to one embodiment of the present invention will be described below with reference to Figures 2 to 9E.
[0033] Figure 2 is a flowchart illustrating the general method for manufacturing a vapor deposition mask. In this embodiment, the vapor deposition mask 10 is manufactured as follows. First, when the manufacturing process for the vapor deposition mask 10 is started, it is determined whether or not the manufacturing process termination conditions are met (step S401). If the termination conditions are met, the process proceeds to (step S401; Yes), and if the termination conditions are not met, the process proceeds to (step S401; No), and the process of adjusting the shrinkage rate of the mask body is performed (step S402). Next, it is determined whether or not the loop termination conditions are met (step S403). If the loop termination conditions are not met (step S403; No), the process proceeds to the mask body formation process (step S404) and the mask frame formation process (step S405), and then returns to step S403 to repeatedly execute the loop process. If the loop termination conditions are met (step S403; Yes), the process returns to step S401. In the following explanation, the vapor deposition masks 10 will be referred to as vapor deposition masks 10-1, 10-2, and 10-3 in the order they are manufactured, and will be referred to as vapor deposition mask 10 when the manufacturing order is not distinguished. The same applies to the components of vapor deposition mask 10. The following describes each step shown in steps S401 to S405 in detail.
[0034] The termination condition in step S401 is, for example, whether a predetermined number of deposition masks 10 have been manufactured, or whether an operation to terminate the manufacturing of deposition masks has been performed. Here, we will explain the case in which the first deposition mask 10-1 is manufactured, so we proceed to step S402 assuming that the termination condition is not met (step S401; No).
[0035] The process of adjusting the shrinkage rate of the mask body in step S402 will be explained with reference to Figures 3 and 4A to 4C.
[0036] Figure 3 is a flowchart illustrating the process of adjusting the shrinkage rate of the mask body 110. First, a photoresist layer 230 having a predetermined pattern is formed on a support substrate 210 that forms the Nth mask body (step S411 shown in Figure 3). Here, we will explain assuming N=1. The predetermined pattern is an opening pattern formed on the mask body. Figure 4A shows the process of forming a metal layer 220 on the support substrate 210 and forming a photoresist layer 230 having a predetermined pattern on the metal layer 220. The support substrate 210 has a first surface 210a and a second surface 210b. The metal layer 220 is formed on the first surface 210a side. In plan view, the shape of the pattern of the photoresist layer 230 is, for example, approximately rectangular. In this case, the pattern arrangement is provided in correspondence with the pixel arrangement of the display device and is arranged in a matrix. When manufacturing the first deposition mask 10-1, the pattern arrangement may be a pattern designed without the influence of mask body shrinkage, or it may be a pattern designed from the beginning considering the influence of mask body shrinkage.
[0037] The support substrate 210 supports each layer in the manufacturing process of the vapor deposition mask 10. Therefore, it is preferable that the support substrate 210 be a rigid substrate. The manufacturing process of the vapor deposition mask 10 includes a step of heating the support substrate 210. When the support substrate 210 expands or contracts due to the heating treatment, not only does the positional displacement of the photoresist layer 230 formed on the support substrate 210 occur, but it may also peel off due to stress. Therefore, in order to stabilize the manufacturing process of the vapor deposition mask 10, it is even more preferable that the support substrate 210 be a rigid substrate with a small coefficient of thermal expansion. Examples of materials for the support substrate 210 include stainless steel (such as SUS304 or SUS430), 42 alloy, Invar, Super Invar, or stainless Invar. Alternatively, a glass substrate may be used as the support substrate 210.
[0038] The metal layer 220 functions as the base metal in the first electroforming process. The material of the metal layer 220 is, for example, nickel or a nickel alloy. The metal layer 220 is formed by sputtering, electroforming, or electroless plating.
[0039] The metal layer 220 is ultimately separated and removed. Therefore, a conductive layer may be provided on the metal layer 220 to facilitate separation of the metal layer 220 from the support substrate 210. In this case, the metal layer 220 can be easily separated from the support substrate 201 by peeling off the conductive layer.
[0040] The vapor deposition mask 10 may be manufactured using electroless plating instead of electroforming. When using electroless plating, an insulating layer may be used instead of the metal layer 220.
[0041] The photoresist layer 230 functions as a mask in the first electroforming process. The photoresist layer 230 is formed by placing a photoresist on the metal layer 220 to have a predetermined film thickness and then developing it to form the desired shape. The photoresist may be a dry film resist that is in film form and can be applied and processed, or a liquid coating-type resist. Furthermore, the photosensitive properties may be either positive or negative. In the following description, an example using a negative-type photosensitive dry film will be explained.
[0042] The photoresist layer 230 has a pattern that corresponds to the opening pattern of the mask body 110 of the deposition mask 10. The pattern of the photoresist layer 230 is formed by photolithography. That is, the pattern of the photoresist layer 230 is formed by adhering a photomask to a dry film resist, irradiating the dry film with ultraviolet light to expose it, and dissolving and removing the unexposed areas.
[0043] Next, the amount of warpage of the support substrate 210 on which the metal layer 220 and the photoresist layer 230 are formed is measured (see step S412 shown in Figure 3). The amount of warpage of the support substrate 210 is measured, for example, using a laser displacement sensor. The laser displacement sensor measures the amount of warpage by irradiating the support substrate 210 with laser light and imaging the reflected light with a CMOS sensor. The laser displacement sensor provides data on the amount of warpage of the support substrate 210 in the XY plane. The amount of warpage acquired for each coordinate in the XY plane of the support substrate 210 is called the amount of warpage data. The number of points for acquiring the amount of warpage is set appropriately according to the area of the support substrate 210.
[0044] When measuring the amount of warpage of the support substrate 210, it is preferable to position the support substrate 210 so that its first surface 210a is perpendicular to the horizontal plane, and then measure the amount of warpage of the support substrate 210. If the support substrate 210 is positioned so that its first surface 210a is parallel to the horizontal plane, the amount of warpage will decrease due to the weight of the support substrate 210, making it impossible to accurately measure the amount of warpage. By positioning the support substrate 210 so that its first surface 210a is perpendicular to the horizontal plane, the influence of the weight of the support substrate 210 can be reduced, and thus the amount of warpage of the support substrate 210 can be accurately measured. If the influence of the weight of the support substrate 210 is small, the first surface 210a of the support substrate 210 may be tilted by ±20° from perpendicular to the horizontal plane.
[0045] Next, a first plating layer 240 is formed on the support substrate 210 (see step S413 shown in Figure 3). Figure 4B shows the process of forming the first plating layer 240 using the photoresist layer 230 as a mask. The first plating layer 240 is formed by electroforming (plating).
[0046] Plating solutions used in electroforming typically consist of a solvent in which one or more metal salts, organic electrolytes, acids such as phosphoric acid, alkalis, and other electrolytes are dissolved. Examples of solvents include water, alcohols such as methanol and ethanol, cyclic carbonates such as ethylene carbonate and propylene carbonate, linear carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, or mixtures thereof.
[0047] The metal salt should be appropriately selected considering the metal, alloy, etc. to be precipitated. Examples of metals used in the metal salt include Cu, Zn, Ga, As, Cr, Se, Mn, Fe, Co, Ni, Ag, Cd, In, Sn, Sb, Te, Ru, Rh, Pd, Au, Hg, Tl, Pb, Bi, W, Po, Re, Os, Ir, and Pt. Among these, Ni, Ag, Au, Cd, Co, Cr, Cu, Fe, Sn, and Zn are preferred, and Ni is particularly preferred. These metals may be used individually or in combination of two or more.
[0048] Specific examples of metal salts that are the main components of the plating solution include, for example, nickel sulfate, nickel chloride, nickel sulfamate, and nickel chloride in a nickel plating solution. These metal salts may be used individually or in combination of two or more in the plating solution. A plating solution to which cobalt sulfamate has been added to the above-mentioned nickel plating solution may also be used.
[0049] The first electroforming step involves placing the metal layer 220 and the photoresist layer 230 into an electroforming bath prepared with the aforementioned plating solution under predetermined conditions. Then, a metal plating is formed from the surface of the metal layer 220 that is not covered by the photoresist layer 230 up to the height of the photoresist layer 230. Examples of materials for the first plating layer 240 include nickel or a nickel alloy.
[0050] In this embodiment, nickel sulfamate is preferably used as the metal salt. By using nickel sulfamate as the metal salt and adjusting the current density, the internal stress of the deposited nickel film can be adjusted. Alternatively, the internal stress may be reduced by adding a stress-reducing agent such as saccharin to the plating solution.
[0051] Furthermore, the internal stress of the nickel film can be adjusted by adding impurities to the nickel plating solution. Compressive stress can be generated in the nickel film by adding, for example, a compound containing a sulfur atom in its molecule as an organic chemical species to the nickel plating solution. Tensile stress can be generated in the nickel film by adding, for example, iron(II,III) ions, zinc ions and their hydroxides, chromate ions as inorganic chemical species, or 2-butyn-1,4-diol and 2-propyne-1-ol, which have a double bond in their molecules, as organic chemical species to the nickel plating solution. When applying compressive stress to the nickel film, it is preferable to add an impurity that generates compressive stress to the nickel plating solution. In addition, to adjust the stress of the nickel film, an impurity that generates tensile stress may be added in addition to the impurity that generates compressive stress.
[0052] Next, the amount of warpage of the support substrate 210 on which the first plating layer 240 is formed is measured (see step S414 shown in Figure 3). The method for measuring the amount of warpage in step S414 is the same as the method for measuring the amount of warpage in step S412. The coordinates of the amount of warpage measured in step S414 correspond to the coordinates of the amount of warpage measured in step S412. This provides data on the amount of warpage in the XY plane. In the following explanation, the amount of warpage measured before the formation of the first plating layer 240 will be called the first amount of warpage, and the amount of warpage measured after the formation of the first plating layer 240 will be called the second amount of warpage.
[0053] Next, the change in warpage δ is calculated based on the first and second warpage amounts before and after the formation of the first plating layer 240. The change in warpage δ can be calculated by subtracting the first warpage amount from the second warpage amount for each coordinate. Next, the internal stress σ of the first plating layer 240 is calculated based on the change in warpage δ (step S415 shown in Figure 3). The internal stress σ of the first plating layer 240 is calculated by the following equation (1).
[0054]
number
[0055] In equation (1), Es is the Young's modulus of the support substrate 210, b is the thickness of the support substrate 210, ν is the Poisson's ratio of the support substrate 210, L is the distance of the support substrate 210 from the reference point, and d is the thickness of the first plating layer 240. Based on equation (1), the internal stress σ can be calculated for each coordinate in the XY plane. The internal stress σ calculated for each coordinate in the XY plane of the support substrate 210 is called the internal stress data. The internal stress data for each coordinate has a one-to-one relationship with the amount of warpage at that coordinate, but it may be calculated for all coordinates, or, based on the assumption that the amount of change in stress in the plane of the support substrate is constant, the stress values at other coordinates may be approximated based on the relationship between the stress values and the amount of warpage at several points sampled from within the plane.
[0056] Next, the shrinkage rate ε of the first plating layer 240 is calculated based on the internal stress σ of the first plating layer 240 (step S416 shown in Figure 3). The shrinkage rate ε of the first plating layer 240 is calculated by the following equation (2).
number
[0057] By performing the above calculations on the internal stress data in the XY plane, data on the shrinkage rate ε of the first plating layer 240 in the XY plane can be obtained.
[0058] Next, it is determined whether the shrinkage rate ε of the first plating layer 240 falls within a predetermined range (step S417). The predetermined range of the allowable shrinkage rate ε varies depending on the material of the support substrate, for example, Young's modulus, thickness, etc. For example, if the shrinkage rate ε falls within the predetermined range at all four corner coordinates of the support substrate 210, it may be determined that the shrinkage rate ε falls within the predetermined range. For example, if the shrinkage rate ε falls within the predetermined range at predetermined coordinates other than the four corner coordinates of the support substrate 210, it may be determined that the shrinkage rate ε falls within the predetermined range. If it is determined that the shrinkage rate ε falls within the predetermined range (step S417; Yes), the process proceeds to step S422, and the photoresist layer 230 is removed. Figure 4C shows the process of peeling the photoresist layer 230 from the surface of the metal layer 220. The photoresist layer 230 is peeled off, for example, with an amine-based peeling solution. This forms the first plating layer 240 having an open region 111 and a non-open region 112.
[0059] Before removing the photoresist layer 230, the first plating layer 240 formed by electroforming may be polished. By polishing the first plating layer 240, the surface of the first plating layer 240 can be flattened.
[0060] The first plating layer 240 corresponds to the mask body 110 of the deposition mask 10. Therefore, for convenience, the first plating layer 240 will be described as the mask body 110 below.
[0061] Next, the mask frame formation process is performed (step S423). The mask frame formation process will be explained in detail later. Once the mask frame formation is complete, the manufacturing of the vapor deposition mask 10-1 is complete. After the shrinkage rate adjustment process of the mask body 110 is completed, the process proceeds to step S403 shown in Figure 2.
[0062] In the manufacturing process of the vapor deposition mask 10-1, if it is determined in step S417 that the shrinkage rate is not within a predetermined range (step S417; No), the process proceeds to step S418. For example, if the shrinkage rate ε is not within a predetermined range at any of the coordinates of the four corners of the support substrate 210, it may be determined that the shrinkage rate ε is not within a predetermined range. For example, even if the coordinates of the four corners of the support substrate 210 are within a predetermined range, if the shrinkage rate ε is not within a predetermined range at any other predetermined coordinates, it may be determined in step S417 that the shrinkage rate ε is not within a predetermined range. In step S418, it is determined whether the shrinkage rate is greater than or equal to the first threshold or less than or equal to the second threshold. Here, the first threshold is a value smaller than the lower limit of the predetermined range, and the second threshold is a value larger than the upper limit of the predetermined range. Similar to the predetermined range, the first and second thresholds of the allowable shrinkage rate differ depending on the material of the support substrate, such as Young's modulus and thickness. Therefore, in a pattern of multiple display devices arranged on a surface, the first and second thresholds are defined as the values at which the aperture pattern with the largest misalignment is shifted by approximately ±1 / 2 of the pixel pitch relative to the original aperture pattern, relative to a certain point where the misalignment is zero. Here, the deposition mask has the relationship: shrinkage rate ∝ stress ∝ tension. If the tension is too high, the deformation of the deposition mask becomes large, making adjustment in the pattern difficult. Also, if the tension is too low, the mask body expands when the mask temperature rises during the deposition process, resulting in zero tension and sagging.
[0063] If it is determined that the shrinkage rate is above the first threshold or below the second threshold (step S418; Yes), the drawing coordinates of the predetermined pattern of the N+1th photoresist layer are adjusted so that the calculated shrinkage rate falls within a predetermined range (step S419). Here, since N=1, the drawing coordinates of the predetermined pattern of the photoresist layer in the next manufacturing process of the deposition mask 10-2 are adjusted. If the center of the support substrate 210 is taken as the reference point, the shrinkage rate tends to increase toward the peripheral region of the support substrate 210. In this case, the magnification of the drawing of the predetermined pattern may be increased as one moves toward the peripheral region from the reference point (coordinate O) of the support substrate 210. In other words, the magnification of the drawing of the predetermined pattern may be increased linearly as one moves toward the peripheral region from the reference point on the support substrate 210. The drawing coordinates are changed by increasing the magnification of the drawing of the predetermined pattern. In addition, the uniformity of the film thickness of the first plating layer 240 in the XY plane affects the shrinkage rate in the XY plane. Therefore, in the XY plane, the magnification for drawing a predetermined pattern may be increased in areas with relatively high shrinkage rates, and decreased in areas with relatively low shrinkage rates. Alternatively, the support substrate 210 may be divided into multiple regions, and a predetermined pattern magnification may be set for each region. Furthermore, the reference point of the support substrate 210 does not have to be the center of the support substrate 210; the reference point may be the point or region with the smallest shrinkage rate among the shrinkage rate data of the first plating layer 240 in the XY plane. Once the drawing coordinates of the predetermined pattern of the (N+1)th photoresist layer are adjusted, the process in step S402 is completed. After that, in order to manufacture the (N+1)th mask body, the process in step S402 may be started again from step S411.
[0064] In step S418, if it is determined that the shrinkage rate ε in the two-dimensional data is less than the first threshold or exceeds the second threshold (step S418; No), the conditions of the first electroforming process are adjusted so that the calculated shrinkage rate falls within a predetermined range of shrinkage rate ε (step S420). Here, since N=1, the drawing of a predetermined pattern on the photoresist layer in the next manufacturing process of the deposition mask 10-2 is adjusted. Because the shrinkage rate of the mask body 110 is large, a stress-reducing agent may be added to the plating solution in the first electroforming process, for example. Alternatively, nickel sulfamate may be used as the metal salt in the plating solution to adjust the current density. Furthermore, if a nickel plating solution is used as the plating solution, impurities may be added. Another method of stress adjustment is to adjust the stress by raising or lowering the temperature of the plating solution. In addition, multiple stress adjustment means may be used in combination. The processing time of the first electroforming process may also be adjusted. After adjusting the conditions of the (N+1)th first electroforming process, the process in step S402 is completed. Subsequently, in order to manufacture the N+1th (in this case, the 2nd) mask body, the process in step S402 should be started from step S411.
[0065] By performing steps S411 to S420, the shrinkage rate of the Nth manufactured mask body can be used to feed back the predetermined pattern formation process of the photoresist layer for the N+1th mask body to be manufactured, as well as the first electroforming process. This improves the accuracy of the opening position of the mask body 110 and stabilizes the manufacturing process.
[0066] In step S403, it is determined whether the loop termination condition is met. The loop termination condition is whether a predetermined number of deposition masks 10 have been manufactured. Here, the predetermined number in step S403 is smaller than the predetermined number in step S401. The predetermined number in step S403 is, for example, the number required to return to the process of adjusting the shrinkage rate of the mask body (step S402) after repeatedly performing the cycle of manufacturing deposition masks 10 (steps S404 and S405). After manufacturing the predetermined number of deposition masks 10, the shrinkage rate of the mask body 110 is checked for any abnormalities. If there is an abnormality in the shrinkage rate of the mask body 110, the shrinkage rate can be adjusted early. Therefore, if the predetermined number of deposition masks 10 is reached (step S403; Yes), the process returns to step S402 to check for any abnormalities in the shrinkage rate of the mask body 110. If the predetermined number of deposition masks 10 has not been reached (step S403; No), the process from steps S404 to S405 is repeated.
[0067] The vapor deposition mask 10 can be manufactured through the above process.
[0068] In a method for manufacturing a vapor deposition mask according to one embodiment of the present invention, instead of forming a plating layer on a dummy support substrate for measurement, peeling it off the support substrate, and then measuring the shrinkage rate, the shrinkage rate of the first plating layer 240 (mask body 110) to be used as the product can be calculated after forming the first plating layer 240 without peeling it off the support substrate. This allows measurement at the same thickness as the plating layer constituting the mask body 110. Therefore, the shrinkage rate can be evaluated more accurately than when measuring the shrinkage rate using a dummy substrate. Furthermore, since the conditions of a predetermined pattern or the conditions of the first electroforming process can be corrected from the calculated shrinkage rate, early feedback can be provided.
[0069] In a method for manufacturing a vapor deposition mask according to one embodiment of the present invention, the conditions of a predetermined pattern may be changed, or the electroforming conditions may be changed. If the electroforming conditions are changed each time the shrinkage rate of the mask body 110 is adjusted, it may take time to obtain the desired accuracy or for the plating solution to stabilize. This reduces the productivity of vapor deposition masks. Therefore, instead of changing the electroforming conditions each time the shrinkage rate of the mask body 110 is adjusted, the shrinkage rate of the mask body 110 is adjusted by changing the conditions of a predetermined pattern of the photoresist layer 230. In areas where the shrinkage rate of the first plating layer 240 is large, the drawing coordinates may be corrected so that the area of the predetermined pattern is large. This improves the positional accuracy of the opening area of the first plating layer 240. Furthermore, when the shrinkage rate of the mask body 110 is large and correction is difficult by changing the predetermined pattern, the time required to determine the conditions can be significantly reduced by changing the electroforming conditions.
[0070] After manufacturing the mask body 110, only the mask bodies 110 that have achieved the desired shrinkage rate can be sent to the mask frame formation process. By manufacturing the vapor-deposited mask 10 in this manner, it is possible to determine whether or not a mask should be sent to the mask frame formation process, thereby reducing the number of defective masks that result from high shrinkage of the mask body 110 and low positional accuracy of the opening area after mask frame formation. In other words, the yield of the final shipped product can be improved.
[0071] Figure 5 shows the simulation results of the amount of warpage when the mask body 110 is formed using a SUS substrate as the support substrate. Figure 6 shows the simulation results of the amount of warpage when the mask body is formed using a glass substrate as the support substrate. The conditions used in the calculations are shown below.
[0072] The support substrate was a stainless steel substrate with a Young's modulus Es = 200 GPa, a thickness b = 1 mm, and a size of 1000 mm × 800 mm. The first plating layer formed on the support substrate was a nickel alloy with a thickness d = 5 μm and an internal stress σ = 40 MPa (tensile). The internal stress σ was calculated at 10 mm intervals in the X direction and 10 mm intervals in the Y direction, with the center of the support substrate as coordinate O(0,0).
[0073] The support substrate was a glass substrate with a Young's modulus Es = 77 GPa, a thickness b = 0.5 mm, and a size of 1000 mm × 800 mm. The first plating layer formed on the support substrate was a Ni alloy with a thickness d = 5 μm and an internal stress σ = 40 MPa (tensile). The internal stress σ was calculated at 10 mm intervals in the X direction and 10 mm intervals in the Y direction, with the center of the support substrate as coordinate O(0,0).
[0074] Figures 5 and 6 show the XY plane of the support substrate. Coordinate O(0,0) is the reference point of the support substrate. In Figure 5, region 301 is the region where the change in warpage is 0 to 0.2, region 302 is the region where the change in warpage is 0.2 to 0.4, region 303 is the region where the change in warpage is 0.4 to 0.6, region 304 is the region where the change in warpage is 0.6 to 0.8, and region 305 is the region where the change in warpage is 0.8 to 1.0. Also, in Figure 6, region 311 is the region where the change in warpage is 0 to 2, region 312 is the region where the change in warpage is 2 to 4, region 313 is the region where the change in warpage is 4 to 6, region 314 is the region where the change in warpage is 6 to 8, and region 315 is the region where the change in warpage is 8 to 10. Because glass substrates have a lower Young's modulus than stainless steel substrates, the change in warpage is larger.
[0075] As shown in Figures 5 and 6, the change in warpage δ increases from the reference point O(0,0) of the substrate towards the four corners A(-400,500), B(-400,-500), C(400,-500), and D(400,500). In other words, the amount of warpage increases from the reference point O(0,0) of the substrate towards the four corners A(-400,500), B(-400,-500), C(400,-500), and D(400,500).
[0076] Figure 7 is a schematic representation of regions 301 to 305 shown in Figure 5 on a support substrate. The amount of change in warpage increases towards the four corners of the support substrate. Although not shown, if regions 311 to 315 shown in Figure 6 are also schematically represented on a support substrate, the distribution of the amount of change in warpage will be the same as in Figure 7. Therefore, as the shrinkage rate of the mask body 110 increases, the area of the opening region of the mask body 110 decreases, and the position (coordinates) of the opening region tends to shift. By measuring the shrinkage rate of the mask body 110, the trend of the area of the opening region in the mask body 110 can be predicted. To correct the decrease in area and position (coordinates) of the opening region of the mask body 110, either a predetermined pattern of the photoresist layer or the conditions of the plating solution should be adjusted.
[0077] Figure 8 shows an example of photoresist layers 331-335 after adjusting the magnification of a predetermined pattern based on the shrinkage rate of the mask body obtained in Figure 5. The photoresist layers 331-335 shown in Figure 8 are only partially shown; in reality, the photoresist layer is formed over the entire support substrate. When changing the magnification of the drawing of a predetermined pattern, for example, the drawing magnification can be set so that, in a plan view, the drawing magnification increases from region 301 to region 305. Thus, the area increases from photoresist layers 331 to 335. In addition, in a plan view, the drawing coordinates of each predetermined pattern are changed so that the area of each predetermined pattern in the peripheral region of the support substrate is larger than the area of each predetermined pattern near the reference point of the support substrate. As a result, when manufacturing the next deposition mask 10, it is possible to form a photoresist layer in which the area of a predetermined pattern changes according to the amount of warping of the mask body 110, thereby improving the accuracy of the shape and positional accuracy of the opening region of the mask body 110 in the XY plane.
[0078] Next, the mask frame formation process will be explained with reference to Figures 9A to 9E.
[0079] Figures 9A and 9B illustrate the process of attaching the mask frame. As shown in Figure 9A, a protective layer 250 is formed on the opening region 111 of the mask body 110. The protective layer 250 prevents particles generated by the process described later from entering the opening 113 of the opening region 111 and blocking the opening 113. The protective layer 250 can also function as a mask in the second electroforming process described later. The same material as the photoresist layer 230 is used for the protective layer 250.
[0080] Next, as shown in Figure 9B, an adhesive layer 280 is provided on the non-opening region 112 of the mask body 110, and the mask frame 120 is bonded to the adhesive layer 280. The adhesive layer 280 does not need to be completely cured as it will be removed in a later step. As the material for the adhesive layer 280, for example, vinyl acetate resin, ethylene vinyl acetate resin, epoxy resin, cyanoacrylate resin, or acrylic resin can be used.
[0081] Figure 9C illustrates the second electroforming process. As shown in Figure 9C, a second plating layer 270 is formed to connect the mask body 110 and the mask frame 120. The second plating layer 270 can be formed by electroforming, which involves energizing the metal layer 220 or the mask frame 120. The second plating layer 270 can be formed in the same manner as the first plating layer 240. Since the second plating layer 270 is provided to fill the openings of the non-opening region 112, the second plating layer 270 is in contact with the metal layer 220. The second plating layer 270 also connects the upper and side surfaces of the non-opening region 112 of the mask body 110 to the mask frame 120. In other words, the second plating layer 270 corresponds to the connection portion 130 of the vapor deposition mask 10. For convenience, the second plating layer 270 will be described below as the connection portion 130.
[0082] Figures 9D and 9E illustrate the process of separating the support substrate. As shown in Figure 9D, the protective layer 250 is peeled off. The protective layer 250 can be peeled off in the same manner as the photoresist layer 230.
[0083] Next, as shown in Figure 9E, the support substrate 210 and the metal layer 220 are separated from the mask body 110. The support substrate 210 and the metal layer 220 may be separated at the same time, or the metal layer 220 may be separated after the support substrate 210 has been separated.
[0084] Through the above process, a vapor deposition mask 10 can be manufactured in which the mask frame 120 and the connecting portion 130 are superimposed on the mask body 110.
[0085] The order of steps in the manufacturing method of the vapor deposition mask 10 is not limited to those described above. For example, the formation of the protective layer 250 shown in Figure 9A may be performed after the mask frame 120 shown in Figure 9B is brought into close contact with the mask body. Also, the peeling off of the protective layer 250 shown in Figure 9D may be performed after the separation of the support substrate 210 shown in Figure 9E.
[0086] In this embodiment, a method for forming the mask body 110 by electroplating has been described, but the embodiment of the present invention is not limited thereto. The mask body 110 can also be applied to films formed by other metal foil film formation techniques, such as films formed by electroless plating or films formed by sputtering. The film used as the mask body 110 may be patterned by etching as appropriate.
[0087] The embodiments described above as embodiments of the present invention can be combined and implemented as appropriate, insofar as they do not contradict each other. Furthermore, any additions, deletions, or design changes to components, or additions, omissions, or changes to processes based on these embodiments, made by those skilled in the art, are also included within the scope of the present invention, as long as they retain the essence of the present invention.
[0088] Any effects or benefits other than those brought about by the embodiments described above, if they are clear from the description herein or easily predictable to a person skilled in the art, are naturally considered to be brought about by the present invention. [Explanation of Symbols]
[0089] 10, 10-1~10-3: Evaporation mask, 110: Mask body, 110-1: Mask body, 110-2: Mask body, 110a: First surface, 110b: Second surface, 111: Opening area, 112: Non-opening area, 113: Opening, 120: Mask frame, 121: Frame part, 122: Cross part, 130: Connection part, 210: Support substrate, 210a: First surface, 210b: Second surface, 220: Metal layer, 230: Photoresist layer, 240: First plating layer, 250: Protective layer, 270: Second plating layer, 280: Adhesive layer, 301~305: Area, 311~315: Area
Claims
1. forming a photoresist layer having a predetermined pattern on a support substrate via a base metal layer; placing the support substrate so that a first surface of the support substrate is perpendicular to a horizontal plane, and measuring a first warpage amount of the support substrate; forming a mask body by depositing metal by electroforming in an area of the base metal layer where the photoresist layer is not formed; the support substrate is disposed so that a first surface of the support substrate is perpendicular to a horizontal plane, and a second warpage amount of the support substrate is measured; calculating a shrinkage rate of the mask body based on a change in the amount of warpage calculated based on the first amount of warpage and the second amount of warpage and an internal stress of the support substrate calculated based on the change in the amount of warpage; a method for manufacturing a deposition mask, wherein when the shrinkage rate of the mask body is smaller than a lower limit value of a predetermined range and is equal to or larger than a first threshold value, or when the shrinkage rate of the mask body is larger than an upper limit value of a predetermined range and is equal to or smaller than a second threshold value, the method changes drawing coordinates of each of the predetermined patterns on a mask body to be manufactured next according to the shrinkage rate of the mask body.
2. 2. The method for manufacturing a deposition mask according to claim 1, wherein when the shrinkage rate of the mask body is smaller than the lower limit of the predetermined range and is less than the first threshold value, or when the shrinkage rate of the mask body is larger than the upper limit of the predetermined range and exceeds the second threshold value, the electroforming conditions of the mask body to be manufactured next are changed.
3. The method for manufacturing a deposition mask according to claim 1 , further comprising the steps of: peeling off the photoresist layer and forming a mask frame on the mask body when the shrinkage rate of the mask body is within the predetermined range.
4. 2. The method for manufacturing a deposition mask according to claim 1, wherein the drawing coordinates are changed so that an area of the predetermined pattern increases radially from a reference point on the support substrate toward a peripheral region in a plan view.
5. The method for manufacturing a deposition mask according to claim 1 , further comprising changing the drawing coordinates so that an area of the predetermined pattern in a peripheral region of the support substrate is larger than an area of the predetermined pattern in the vicinity of a reference point on the support substrate in a plan view.