Manufacturing method of photomask blank and manufacturing method of photomask
Patent Information
- Application Number
- JP2021183761
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-11-10
AI Technical Summary
Conventional photomask manufacturing methods face challenges in achieving precise dimensional accuracy of the light shielding portion due to differing etching rates between the phase shift film and light shielding film, leading to edge roughness and prolonged etching times.
A method for manufacturing photomask blanks involves forming a first and second functional film on a transparent substrate, where the films are aligned on the same plane with their edges in contact, and using Cr-based materials for both films to ensure similar etching characteristics, thereby eliminating laminated portions and reducing edge roughness.
This approach enhances pattern dimension control and improves accuracy by minimizing edge roughness and shortening etching time, resulting in high-precision patterning of the photomask.
Smart Images

Figure 00000000_0000_ABST 
Figure 00000000_0001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a photomask blank and a method for manufacturing a photomask.
Background Art
[0002] As photolithography techniques, phase shift masks and halftone masks are known. A phase shift mask is a photomask having a phase shift film on a part of a transparent substrate, and has functions of improving resolution and improving depth of focus (DOF) by changing the phase and intensity of light passing through this part. A halftone mask is a photomask having a halftone film on a part of a transparent substrate, and has a function of realizing multi-tone of three or more tones by changing the intensity of light passing through this part.
[0003] This type of photomask is manufactured through the following steps: i) preparing a photomask blank in which a light-shielding film is formed on a transparent substrate; ii) forming a resist film on the light-shielding film; iii) drawing a predetermined resist pattern on the resist film, removing the unnecessary resist film by development, and forming a predetermined resist pattern; iv) using the resist pattern as a mask to remove the exposed portion of the light-shielding film by etching; v) removing the remaining resist film; vi) forming a phase shift film or a halftone film on the exposed portion of the transparent substrate from which the light-shielding film has been removed and on the light-shielding film; vii) forming a resist film on the phase shift film or the halftone film; viii) drawing a predetermined resist pattern on the resist film, removing the unnecessary resist film by development, and forming a predetermined resist pattern; ix) using the resist pattern as a mask to remove the exposed portions of the phase shift film or the halftone film and the exposed portion of the light-shielding film by etching; x) removing the remaining resist film. For example, Patent Document 1 describes a method for manufacturing a photomask in which a halftone film is formed as step vi).
Prior Art Documents
Patent Documents
[0004] [Patent Document 1] Japanese Patent Publication No. 2005-257712 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] According to the conventional photomask manufacturing method described above, the light-shielding portion is composed of a laminated portion of a light-shielding film and a phase-shift film or halftone film. Therefore, when patterning the light-shielding portion, it is necessary to etch both the phase-shift film or halftone film and the light-shielding film. However, if the etching rates of the two differ, a difference in the amount of side etching occurs between the phase-shift film or halftone film and the light-shielding film. As a result, edge roughness occurs at the edges of the light-shielding portion, making it difficult to finish the dimensional accuracy of the light-shielding portion (edge position accuracy of the light-shielding portion relative to the transparent portion) as intended. In addition, because it is a laminated portion, the etching time may be longer than in the case of a single layer, making dimensional control of the light-shielding portion (edge position control of the light-shielding portion relative to the transparent portion (CD (Critical Dimension) control)) difficult.
[0006] Therefore, the present invention has been made in view of these circumstances, and aims to provide a method for manufacturing photomask blanks and a method for manufacturing photomasks that facilitates the control of pattern dimensions during the manufacturing of photomasks and improves the dimensional accuracy of patterns in the photomasks. [Means for solving the problem]
[0007] The method for manufacturing photomask blanks according to the present invention is: A method for manufacturing photomask blanks, wherein the surface of a transparent substrate is divided into a region of a first pattern and a region of a second pattern, a first functional film is formed in the region of the first pattern, and a second functional film is formed in the region of the second pattern, A photomask blank preparation step involves preparing a primary photomask blank in which a first functional film is formed on a transparent substrate, A first patterning step involves patterning a first functional film with a pattern corresponding to the region of the first pattern, and removing the first functional film in the region of the second pattern. A functional film formation step in which a second functional film is formed on the exposed portion of the transparent substrate from which the first functional film has been removed and on the first functional film, The method comprises a second patterning step of patterning a second functional film with a pattern corresponding to the region of the second pattern, and removing the second functional film in the region of the first pattern. This is a method for manufacturing photomask blanks.
[0008] Here, as one embodiment of the method for manufacturing photomask blanks according to the present invention, As the first photomask blank, a photomask blank is used in which a first functional film is formed on a transparent substrate, and an interlayer having different etching characteristics from the first functional film is formed on top of the first functional film. As the second functional film, a film having the same etching characteristics as the first functional film is used. This configuration can be adopted.
[0009] in this case, The first and second functional films are made of Cr-based material. This configuration can be adopted.
[0010] Furthermore, as another embodiment of the method for manufacturing photomask blanks according to the present invention, As the first functional film, a film having the function of adjusting the optical properties of exposure light is used. As the second functional film, a film is used that has a function different from the first functional film, namely, a function to adjust the optical properties of the exposure light. This configuration can be adopted.
[0011] in this case, As either the first functional film or the second functional film, a phase-shift film or a halftone film is used. A light-shielding film is used as the other of either the first or second functional film. This configuration can be adopted.
[0012] Furthermore, the method for manufacturing a photomask according to the present invention is: A photomask blank preparation step involves preparing a photomask blank manufactured by one of the above methods for manufacturing photomask blanks, The process includes a patterning step for patterning a first functional film and a second functional film in a predetermined pattern. This is a method for manufacturing photomasks. [Effects of the Invention]
[0013] According to the present invention, a composite photomask blank is manufactured in which a first functional film and a second functional film are formed on a transparent substrate so that their edges are touching and they are arranged on the same plane. In this photomask blank, there is no substantial laminated portion of the first and second functional films, and the edges of the photomask pattern are defined on the first and second functional films, which are substantially single layers, respectively. This means that edge roughness is less likely to occur at the edges of the photomask pattern, and the etching time is shortened. Therefore, according to the present invention, it is possible to easily control the dimensions of the pattern during the manufacturing of the photomask and to improve the dimensional accuracy of the pattern in the photomask. [Brief explanation of the drawing]
[0014] [Figure 1] Figure 1(a) is an enlarged plan view of the main part of a photomask according to one embodiment of the present invention. Figure 1(b) is a cross-sectional view taken along line AA of Figure 1(a). [Figure 2] Figure 2(a) is a photomask blank according to one embodiment of the present invention, and is an enlarged plan view of the main part of the photomask blank that serves as the basis for the photomask in Figure 1. Figure 2(b) is a cross-sectional view of Figure 2(a) along line BB. [Figure 3]Figs. 3(a) to 3(d) are explanatory diagrams of a method for manufacturing a photomask blank according to Embodiment 1 of the present invention. [Figure 4] Figs. 4(a) to 4(c) are explanatory diagrams that continue the explanation of Fig. 3. [Figure 5] Figs. 5(a) to 5(d) are explanatory diagrams that continue the explanation of Fig. 4. [Figure 6] Figs. 6(a) to 6(d) are explanatory diagrams that continue the explanation of Fig. 5. [Figure 7] Figs. 7(a) to 7(d) are explanatory diagrams of a method for manufacturing a photomask blank according to Embodiment 2 of the present invention. [Figure 8] Figs. 8(a) to 8(c) are explanatory diagrams that continue the explanation of Fig. 7. [Figure 9] Figs. 9(a) to 9(d) are explanatory diagrams that continue the explanation of Fig. 8. [Figure 10] Figs. 10(a) to 10(d) are explanatory diagrams that continue the explanation of Fig. 9. [Figure 11] Figs. 11(a) to 11(d) are explanatory diagrams of a method for manufacturing a photomask blank according to Embodiment 3 of the present invention. [Figure 12] Figs. 12(a) to 12(b) are explanatory diagrams that continue the explanation of Fig. 11. [Figure 13] Figs. 13(a) to 13(d) are explanatory diagrams that continue the explanation of Fig. 12. [Figure 14] Figs. 14(a) to 14(c) are explanatory diagrams that continue the explanation of Fig. 13. [Figure 15] Figs. 15(a) to 15(d) are explanatory diagrams of a method for manufacturing a photomask according to an embodiment of the present invention. [Figure 16] Figs. 16(a) to 16(d) are explanatory diagrams that continue the explanation of Fig. 15. [Figure 17] Figs. 17(a) to 17(d) are supplementary explanatory diagrams of Step 3 in Fig. 15(c). [Figure 18] Fig. 18 is a partially enlarged cross-sectional view of Fig. 1(b) and Fig. 16(d). [Figure 19] Figs. 19(a) to 1(c) are explanatory diagrams of a method for manufacturing a photomask blank according to another embodiment of the present invention.
Mode for Carrying Out the Invention
[0015] <Photomask configuration> First, the configuration of the photomask according to one embodiment of the present invention will be described.
[0016] As shown in Figure 1, the photomask 1 is a 3-level multi-gradation photomask comprising a transparent area (white area), a semi-transparent area (hatched area), and a light-shielding area (black area). The transparent area is composed of a transparent substrate 3, the semi-transparent area is composed of a semi-transparent film 4, and the light-shielding area is composed of a light-shielding film 5. That is, the exposed parts of the transparent substrate 3 where the semi-transparent film 4 and light-shielding film 5 are not laminated become the transparent areas, the parts on the transparent substrate 3 where the semi-transparent film 4 is laminated become the semi-transparent areas, and the parts on the transparent substrate 3 where the light-shielding film 5 is laminated become the light-shielding areas.
[0017] The semi-transparent portion is formed in the form of an island pattern in which unit elements (islands) of a predetermined shape (rectangular in this embodiment) are arranged in two dimensions with predetermined intervals between them. The light-shielding portion is formed to fill the area other than the semi-transparent portion. The transparent portion is formed in the form of a hole pattern 7 in which unit elements (holes 7A, 7B) of a predetermined shape (rectangular in this embodiment) are arranged in two dimensions with predetermined intervals between them and are contained within the semi-transparent portion and the light-shielding portion, respectively.
[0018] The transparent substrate 3 is a substrate such as synthetic quartz glass. The transparent substrate 3 has a transmittance of 95% or more for representative wavelengths (e.g., i-line, h-line, or g-line) included in the exposure light used in the exposure process using the photomask 1. The exposure light may be, for example, i-line, h-line, or g-line, or it may be a mixed light containing at least two of these lights. Alternatively, the exposure light may have a wavelength band shifted or extended to the shorter wavelength side and / or longer wavelength side relative to these lights. As an example, the wavelength band of the exposure light can be extended from a broadband of 365 nm to 436 nm to 300 nm to 450 nm. However, the exposure light is not limited to these.
[0019] The semipermeable film 4 is made of a Cr-based material from among known materials such as Cr or Cr-based compounds, Ni or Ni-based compounds, Ti or Ti-based compounds, Si-based compounds, and metal silicide compounds. In this embodiment, a Cr-based compound is used for the semipermeable film 4. The semipermeable film 4 is a phase-shift film. Alternatively, the semipermeable film 4 may be a halftone film. The semipermeable film 4 has a transmittance lower than that of the transparent substrate 3 and higher than that of the light-shielding film 5 with respect to a representative wavelength included in the exposure light, and is set to have a transmittance of 5% to 70% with respect to the representative wavelength. The semipermeable film 4 may also be a semipermeable metal film in which the transmittance distribution within the plane of the photomask 1 is improved by adjusting the nitrogen content. Furthermore, the optical density (OD value) in the semipermeable portion of the semipermeable film 4 can be changed by including other elements. The semipermeable film 4 is formed on the transparent substrate 3 by sputtering, vapor deposition, or the like.
[0020] The light-shielding film 5 is made of the same material as the semi-permeable film 4. In this embodiment, a Cr-based compound is used for the light-shielding film 5. The light-shielding film 5 has a transmittance of 1% or less with respect to the representative wavelength included in the exposure light. Alternatively, it is sufficient if the optical density (OD value) in the light-shielding portion is 2.7 or higher. As an example, the light-shielding film 5 has a laminated structure comprising a first film-forming layer and a second film-forming layer. The first film-forming layer is composed of a Cr film and is intended for light shielding. The second film-forming layer is composed of a chromium oxide film and is intended for reflection suppression. In this case, even if the transmittance of the first film-forming layer is higher than 1%, it is sufficient if the combined transmittance of the first and second film-forming layers is 1% or less. The light-shielding film 5 is formed on the transparent substrate 3 by sputtering, vapor deposition, or the like.
[0021] The semipermeable film 4 and the light-shielding film 5 have the same etching properties because they are made of the same material. However, the semipermeable film 4 and the light-shielding film 5 have different etching properties from the interlayer film 6, which will be described later, because they are made of different materials. That is, the semipermeable film 4 and the light-shielding film 5 have etching selectivity with respect to the interlayer film 6, and the interlayer film 6 has etching selectivity with respect to the semipermeable film 4 and the light-shielding film 5.
[0022] <Composition of photomask blanks> Next, we will describe the configuration of a photomask blank that serves as the basis for photomask 1, according to one embodiment of the present invention.
[0023] As shown in Figure 2, the photomask blank 2 is in the state before the hole pattern 7 of the photomask 1 is formed. That is, the photomask blank 2 is formed so that the semi-permeable film 4 and the light-shielding film 5 are aligned on the same plane with their edges touching, without having a transparent area across the entire surface (effective area) of the transparent substrate 3. However, although they are aligned on the same plane, the thicknesses of the semi-permeable film 4 and the light-shielding film 5 are not necessarily the same. For example, it is certainly possible that the thickness of the semi-permeable film 4 is smaller than the thickness of the light-shielding film 5, or vice versa.
[0024] <First method for manufacturing photomask blanks> Next, a method for manufacturing a photomask blank 2 according to Embodiment 1 of the present invention (a first method for manufacturing a photomask blank 2) will be described.
[0025] In general terms, the manufacturing method is a method for manufacturing a photomask blank 2 in which the surface of a transparent substrate 3 is divided into a region of a first pattern and a region of a second pattern, a first functional film is formed in the region of the first pattern, and a second functional film is formed in the region of the second pattern, wherein the region of the first pattern is the region of a semipermeable film 4, the region of the second pattern is the region of a light-shielding film 5, the first functional film is the semipermeable film 4, and the second functional film is the light-shielding film 5. A functional film is a film that has the function of adjusting the optical properties of exposure light. Functional films include phase-shift films that have the function of changing the phase of exposure light, semipermeable films that have the function of adjusting the transmittance of exposure light, and light-shielding films that have the function of blocking exposure light.
[0026] Specifically, the manufacturing method in question is: i) Photomask blank preparation process (Step 1) ii) Resist film formation process (Step 2) iii) Drawing process (process 3) iv) Development process (Step 4) v) Interlayer etching process (Step 5) vi) Semipermeable film etching process (step 6) vii) Resist film removal process (Step 7) viii) Light shielding film formation process (process 8) ix) Resist film formation process (Step 9) x) Drawing process (Step 10) xi) Development process (Step 11) xii) Light-shielding film etching process (step 12) xiii) Interlayer etching process (step 13) xiv) Resist film removal process (step 14) xv) Finishing process (Step 15) It is equipped with.
[0027] The process from the resist film formation process (step 2) to the resist film removal process (step 7), and the process from the resist film formation process (step 9) to the resist film removal process (step 14), are collectively referred to as patterning processes. In the former patterning process, the semi-permeable film 4 of the photomask blank 2 is patterned, and in the latter patterning process, the light-shielding film 5 of the photomask blank 2 is patterned.
[0028] In the photomask blank preparation step (step 1), as shown in Figure 3(a), a semipermeable film 4 is formed on a transparent substrate 3, and an interlayer film (etching stopper film) 6 is formed on the semipermeable film 4. This prepares a photomask blank (first photomask blank) in which the semipermeable film 4 and the interlayer film 6 are laminated on the transparent substrate 3. The interlayer film 6 is made of a non-Cr material. In this embodiment, the interlayer film 6 is made of Ni, Ti, or a molybdenum silicide compound. The semipermeable film 4 and the interlayer film 6 are formed by sputtering, vapor deposition, or the like, respectively.
[0029] In the first resist film formation step (step 2), as shown in Figure 3(b), the resist is uniformly applied onto the interlayer film 6 to form the resist film 8. The resist is applied by coating or spraying.
[0030] In the first drawing process (step 3), as shown in Figure 3(c), exposure light is irradiated onto the resist film 8 using the electron beam or laser of the drawing apparatus, and a resist pattern corresponding to the area of the semi-permeable film 4 of the photomask blanks 2 is drawn. In addition to drawing the resist pattern, alignment marks are also drawn in the first drawing process (step 3) to align the drawing position in the second drawing process (step 10). Although not shown, alignment marks are formed, for example, at three or four appropriate locations in the outer region surrounding the resist pattern.
[0031] In the first development step (step 4), as shown in Figure 3(d), the unnecessary resist film 8 (part 8a) is removed by development, and a resist pattern is formed. Development is performed by immersion in a developer solution. The drawing step (step 3) and the development step (step 4) together are called the resist pattern formation step.
[0032] In the interlayer etching process (step 5), as shown in Figure 4(a), the resist pattern is used as an etching mask, and the exposed portions of the interlayer 6 are removed by etching. Etching can be done by either dry etching or wet etching, but wet etching is preferred for large-sized photomasks. Etching solutions or etching gases are used. In any case, an etchant that has etching selectivity for the interlayer 6 (an etchant that does not etch the semipermeable film 4) is used.
[0033] In the semipermeable film etching process (step 6), as shown in Figure 4(b), the exposed portion of the semipermeable film 4 is removed by etching using the interlayer film 6 as an etching mask. Etching can be done by either dry etching or wet etching, but wet etching is preferred for large-sized photomasks. Etching solutions or etching gases are used. In any case, an etchant that has etching selectivity for the semipermeable film 4 (an etchant that does not etch the interlayer film 6) is used.
[0034] In the first resist film removal step (step 7), the resist film 8 is removed as shown in Figure 4(c). The resist film 8 is removed by ashing or by immersion in a resist stripping solution.
[0035] In the light-shielding film formation step (step 8), as shown in Figure 5(a), a light-shielding film 5 is formed on the exposed portion of the transparent substrate 3 from which the semi-permeable film 4 has been removed, and on the semi-permeable film 4. The light-shielding film 5 is formed by sputtering, vapor deposition, or the like.
[0036] In the second resist film formation step (step 9), similar to the first resist film formation step (step 2), a resist is applied to the light-shielding film 5, as shown in Figure 5(b), to form a resist film 8. The resist is applied by coating or spraying.
[0037] In the second drawing process (step 10), as in the first drawing process (step 3), exposure light is irradiated onto the resist film 8 using the electron beam or laser of the drawing apparatus, as shown in Figure 5(c), and a resist pattern corresponding to the area of the light-shielding film 5 of the photomask blanks 2 is drawn. The drawing apparatus is the same apparatus used in the first drawing process (step 3). In the second drawing process (step 10), the drawing apparatus detects the alignment marks formed in the first drawing process (step 3) and aligns the transparent substrate 3.
[0038] However, even with improved alignment accuracy, completely eliminating alignment errors is extremely difficult. Therefore, in the second drawing process (step 10), a resist pattern is set that takes alignment errors into account. Specifically, by offsetting the edge of the light-shielding film 5 of the photomask blanks 2 outward (+offset), a resist pattern is set that overlaps (overlaps) with an overlap amount L at the edges of the laminated portion of the semi-permeable film 4, the interlayer film 6, and the light-shielding film 5. The overlap amount L is, for example, a value between 0.3 μm and 0.5 μm.
[0039] In the second development step (step 11), as in the first development step (step 4), as shown in Figure 5(d), the unnecessary resist film 8 (part 8a) is removed by development, and a resist pattern is formed. Development is performed by immersion in a developer solution. The drawing step (step 10) and the development step (step 11) together are called the resist pattern formation step.
[0040] In the light-shielding film etching process (step 12), as shown in Figure 6(a), the resist pattern is used as an etching mask, and the exposed portions of the light-shielding film 5 are removed by etching. Etching can be done by either dry etching or wet etching, but wet etching is preferred for large-sized photomasks. Etching solutions or etching gases are used. In any case, an etchant that has etching selectivity for the light-shielding film 5 (an etchant that does not etch the interlayer film 6) is used.
[0041] In the interlayer etching process (step 13), as shown in Figure 6(b), the light-shielding film 5 (or the resist pattern if the light-shielding film 5 is not present) is used as an etching mask, and the exposed portion of the interlayer 6 is removed by etching. Etching can be done by either dry etching or wet etching, but wet etching is preferred for large-sized photomasks. Etching solutions or etching gases are used. In any case, an etchant that has etching selectivity for the interlayer 6 (an etchant that does not etch the semipermeable film 4) is used.
[0042] In the second resist film removal step (step 14), the resist film 8 is removed in the same way as in the first resist film removal step (step 7), as shown in Figure 6(c). The resist film 8 is removed by ashing or by immersion in a resist stripping solution.
[0043] In the finishing process (step 15), as shown in Figure 6(d), the residue 9 of the interlayer 6 and light-shielding film 5 remaining after the lapping is removed. Since the residue 9 is narrow and has low rigidity, it can be easily removed by washing or the like. Alternatively, if the light-shielding film 5 is side-etched in the light-shielding film etching process (step 12) and the interlayer 6 is side-etched in the interlayer etching process (step 13), and no residue 9 remains, then the finishing process (step 15) is unnecessary.
[0044] After going through steps 1 through 15 described above, the second photomask blank, photomask blank 2, is completed.
[0045] <Second method for manufacturing photomask blanks> Next, a method for manufacturing the photomask blank 2 according to Embodiment 2 of the present invention (a second method for manufacturing the photomask blank 2) will be described.
[0046] In general terms, the manufacturing method is a method for manufacturing a photomask blank 2 in which the surface of a transparent substrate 3 is divided into a region of a first pattern and a region of a second pattern, a first functional film is formed in the region of the first pattern, and a second functional film is formed in the region of the second pattern, wherein the region of the first pattern is the region of a light-shielding film 5, the region of the second pattern is the region of a semi-permeable film 4, the first functional film is the light-shielding film 5, and the second functional film is the semi-permeable film 4.
[0047] Specifically, the manufacturing method in question is: i) Photomask blank preparation process (Step 1) ii) Resist film formation process (Step 2) iii) Drawing process (process 3) iv) Development process (Step 4) v) Interlayer etching process (Step 5) vi) Light-shielding film etching process (step 6) vii) Resist film removal process (Step 7) viii) Semi-permeable membrane formation process (Step 8) ix) Resist film formation process (Step 9) x) Drawing process (Step 10) xi) Development process (Step 11) xii) Semipermeable film etching process (step 12) xiii) Interlayer etching process (step 13) xiv) Resist film removal process (step 14) xv) Finishing process (Step 15) It is equipped with.
[0048] The process from the resist film formation process (step 2) to the resist film removal process (step 7), and the process from the resist film formation process (step 9) to the resist film removal process (step 14), are collectively referred to as patterning processes. In the former patterning process, the light-shielding film 5 of the photomask blank 2 is patterned, and in the latter patterning process, the semi-permeable film 4 of the photomask blank 2 is patterned.
[0049] The difference between the second manufacturing method and the first manufacturing method is that in the first method, the semipermeable film 4 is patterned first and the light-shielding film 5 is patterned later, whereas in the second method, the light-shielding film 5 is patterned first and the semipermeable film 4 is patterned later. Aside from this difference, the two methods are identical. Therefore, the following will describe the differences, while the similarities will be omitted, as they are the same as those described for the first manufacturing method.
[0050] In the photomask blank preparation process (step 1), as shown in Figure 7(a), a light-shielding film 5 is formed on the transparent substrate 3, and an interlayer film (etching stopper film) 6 is formed on the light-shielding film 5. This prepares a photomask blank (first-stage photomask blank) in which the light-shielding film 5 and the interlayer film 6 are laminated on the transparent substrate 3.
[0051] In the first drawing process (step 3), as shown in Figure 7(c), a resist pattern corresponding to the area of the light-shielding film 5 on the photomask blank 2 is drawn.
[0052] In the interlayer etching process (step 5), as shown in Figure 8(a), the resist pattern is used as an etching mask, and the exposed portion of the interlayer 6 is removed by etching. The etchant used is one that has etching selectivity for the interlayer 6 (an etchant that does not etch the light-shielding film 5).
[0053] In the light-shielding film etching process (step 6), as shown in Figure 8(b), the exposed portion of the light-shielding film 5 is removed by etching using the interlayer film 6 as an etching mask. The etchant used is one that has etching selectivity for the light-shielding film 5 (an etchant that does not etch the interlayer film 6).
[0054] In the semi-permeable film formation step (step 8), as shown in Figure 9(a), a semi-permeable film 4 is formed on the exposed portion of the transparent substrate 3 from which the light-shielding film 5 has been removed and on the light-shielding film 5.
[0055] In the second drawing process (step 10), a resist pattern corresponding to the area of the semipermeable film 4 on the photomask blank 2 is drawn, as shown in Figure 9(c). However, the resist pattern is such that it overlaps (overlaps) with an overlap amount L on the edges of the laminated portion of the light-shielding film 5, the interlayer film 6, and the semipermeable film 4 by offsetting the edges of the semipermeable film 4 on the photomask blank 2 outward (+offset).
[0056] In the semipermeable film etching process (step 12), as shown in Figure 10(a), the resist pattern is used as an etching mask, and the exposed portion of the semipermeable film 4 is removed by etching. The etchant used is one that has etching selectivity for the semipermeable film 4 (an etchant that does not etch the interlayer 6).
[0057] In the interlayer etching process (step 13), as shown in Figure 10(b), the semipermeable film 4 (or the resist pattern if the semipermeable film 4 is not present) is used as an etching mask, and the exposed portion of the interlayer 6 is removed by etching. The etchant used is one that has etching selectivity for the interlayer 6 (an etchant that does not etch the light-shielding film 5).
[0058] <Third method for manufacturing photomask blanks> Next, a method for manufacturing the photomask blanks 2 according to Embodiment 3 of the present invention (a third method for manufacturing the photomask blanks 2) will be described.
[0059] In general terms, the manufacturing method is a method for manufacturing a photomask blank 2 in which the surface of a transparent substrate 3 is divided into a region of a first pattern and a region of a second pattern, a first functional film is formed in the region of the first pattern, and a second functional film is formed in the region of the second pattern, wherein the region of the first pattern is a region of a semipermeable film 4, the region of the second pattern is a region of a light-shielding film 5, the first functional film is a semipermeable film 4, and the second functional film is a light-shielding film 5.
[0060] Specifically, the manufacturing method in question is: i) Photomask blank preparation process (Step 1) ii) Resist film formation process (Step 2) iii) Drawing process (process 3) iv) Development process (Step 4) v) Semipermeable film etching process (Step 5) vi) Resist film removal process (step 6) vii) Light shielding film formation process (process 7) viii) Resist film formation process (step 8) ix) Drawing process (process 9) x) Development process (Step 10) xi) Light-shielding film etching process (Step 11) xii) Resist film removal process (step 12) xiii) Finishing process (Step 13) It is equipped with.
[0061] The process from the resist film formation process (step 2) to the resist film removal process (step 6), and the process from the resist film formation process (step 8) to the resist film removal process (step 12), are collectively referred to as patterning processes. In the former patterning process, the semi-permeable film 4 of the photomask blank 2 is patterned, and in the latter patterning process, the light-shielding film 5 of the photomask blank 2 is patterned.
[0062] The differences between the third manufacturing method and the first manufacturing method are that, in the third manufacturing method, i) the interlayer film 6 is not laminated, and a photomask blank in which only a semi-permeable film 4 is formed on the transparent substrate 3 is used as the primary photomask blank, and consequently, the interlayer etching step (step 5) and the interlayer etching step (step 13) of the first manufacturing method are omitted; and ii) either the semi-permeable film 4 or the light-shielding film 5 is made of a Cr-based material, for example, and the other is made of a non-Cr-based material, resulting in different etching characteristics between the semi-permeable film 4 and the light-shielding film 5 due to the difference in materials, and consequently, different etchants are used. Aside from matters related to these, the two methods are the same. Therefore, the description of the third manufacturing method is the same as that of the first manufacturing method, and is omitted.
[0063] <Fourth method for manufacturing photomask blanks> Next, a method for manufacturing the photomask blanks 2 according to Embodiment 4 of the present invention (a fourth method for manufacturing the photomask blanks 2) will be described.
[0064] In general terms, the manufacturing method is a method for manufacturing a photomask blank 2 in which the surface of a transparent substrate 3 is divided into a region of a first pattern and a region of a second pattern, a first functional film is formed in the region of the first pattern, and a second functional film is formed in the region of the second pattern, wherein the region of the first pattern is the region of a light-shielding film 5, the region of the second pattern is the region of a semi-permeable film 4, the first functional film is the light-shielding film 5, and the second functional film is the semi-permeable film 4.
[0065] Specifically, the manufacturing method in question is: i) Photomask blank preparation process (Step 1) ii) Resist film formation process (Step 2) iii) Drawing process (process 3) iv) Development process (Step 4) v) Light-shielding film etching process (Step 5) vi) Resist film removal process (step 6) vii) Semi-permeable membrane formation process (Step 7) viii) Resist film formation process (step 8) ix) Drawing process (process 9) x) Development process (Step 10) xi) Semipermeable film etching process (Step 11) xii) Resist film removal process (step 12) xiii) Finishing process (Step 13) It is equipped with.
[0066] The process from the resist film formation process (step 2) to the resist film removal process (step 6), and the process from the resist film formation process (step 8) to the resist film removal process (step 12), are collectively referred to as patterning processes. In the former patterning process, the light-shielding film 5 of the photomask blank 2 is patterned, and in the latter patterning process, the semi-permeable film 4 of the photomask blank 2 is patterned.
[0067] The difference between the fourth manufacturing method and the third manufacturing method is that in the third method, the semipermeable film 4 is patterned first and the light-shielding film 5 is patterned later, whereas in the fourth method, the light-shielding film 5 is patterned first and the semipermeable film 4 is patterned later. Aside from matters related to this, the two methods are the same. Therefore, the description of the fourth manufacturing method is omitted, as it is the same as the description of the first and second manufacturing methods.
[0068] <Method for manufacturing a photomask> Next, a method for manufacturing a photomask 1 according to one embodiment of the present invention will be described.
[0069] The manufacturing method is i) Photomask blank preparation process (Step 1) ii) Resist film formation process (Step 2) iii) Drawing process (process 3) iv) Development process (Step 4) v) Film etching process (Step 5) vi) Resist film removal process (step 6) It is equipped with.
[0070] The process from the resist film formation step (step 2) to the resist film removal step (step 7) is called the patterning process. In the patterning process, the transparent areas of photomask 1 are patterned.
[0071] In the photomask blank preparation step (step 1), as shown in Figure 15(a), a photomask blank 2 (second photomask blank) manufactured by one of the above methods for manufacturing the photomask blank 2 is prepared.
[0072] In the resist film formation step (step 2), as shown in Figure 15(b), the resist is uniformly applied to the semipermeable film 4 and the light-shielding film 5 to form the resist film 8. The resist is applied by coating or spraying.
[0073] In the drawing process (step 3), as shown in Figure 15(c), exposure light is irradiated onto the resist film 8 using the electron beam or laser of the drawing apparatus, and a resist pattern corresponding to the transparent area (hole pattern 7) of the photomask 1 is drawn.
[0074] However, even though the semipermeable film 4 and the light-shielding film 5 have the same etching characteristics, if their etching rates differ, a difference in the amount of side etching occurs between the semipermeable film 4 and the light-shielding film 5 during the film etching process (step 5). As a result, the dimensional accuracy of at least one of the holes 7A, ... located in the semipermeable region or the holes 7B, ... located in the light-shielding region of the hole pattern 7 of the photomask 1 (edge position accuracy relative to at least one of the semipermeable or light-shielding regions of the photomask 1) deteriorates. Therefore, in the drawing process (step 3), a resist pattern is set that takes into account the difference in etching rates. Specifically, for example, if the semi-permeable film 4 has a higher etching rate than the light-shielding film 5, while the holes 7A and 7B shown in Figures 17(a) and (b) have their original dimensions and shapes, a resist pattern is set such that, as shown in Figure 17(c), the edges of the holes 7A, ... located in the semi-permeable region are offset inward (-offset), or as shown in Figure 17(d), the edges of the holes 7B, ... located in the light-shielding region are offset outward (+offset). Of course, if the etching rates of the semi-permeable film 4 and the light-shielding film 5 are the same or approximate, the offset process is unnecessary.
[0075] Another approach to the etching rate is to form (deposit) the semipermeable film 4 and the light-shielding film 5 so that their etching rates are the same or approximately the same. This involves changing the composition ratio of the compounds contained in the semipermeable film 4 in the film thickness direction during the manufacturing stage of the photomask blanks 2, thereby adjusting the etching rate through a compositional gradient. For example, it is possible to slow down the etching rate by increasing the etching difficulty in the direction in which etching progresses along the film thickness direction. Alternatively, the reverse adjustment method is also possible.
[0076] In the development step (step 4), as shown in Figure 15(d), the unnecessary resist film 8 (part 8a) is removed by development, and a resist pattern is formed. Development is performed by immersion in a developer solution. The drawing step (step 3) and the development step (step 4) together are called the resist pattern formation step.
[0077] In the film etching process (step 5), as shown in Figure 16(a), the resist pattern is used as an etching mask, and the exposed portions of the semi-permeable film 4 and the light-shielding film 5 are removed by etching. Etching can be done by either dry etching or wet etching, but wet etching is preferred for large-sized photomasks. Etching is performed using an etching solution or etching gas.
[0078] However, in the case of photomask blanks 2 manufactured by the third and fourth manufacturing methods described above, the semipermeable film 4 and the light-shielding film 5 have different etching characteristics and use different etchants. Therefore, the film etching process (step 5) is divided into a semipermeable film etching process (step 5-1) as shown in Figure 16(b) and a light-shielding film etching process (step 5-2) as shown in Figure 16(c). The order in which these steps are performed does not matter.
[0079] In the resist film removal step (step 6), the resist film 8 is removed as shown in Figure 16(d). The resist film 8 is removed by ashing or by immersion in a resist stripping solution.
[0080] After going through steps 1 through 6 described above, photomask 1 is completed.
[0081] <Effects of the Embodiment> According to the above manufacturing methods for the photomask blanks 2, a composite type of photomask blanks 2 is manufactured in which a semi-permeable film 4 and a light-shielding film 5 are formed on a transparent substrate 3 so that their edges touch each other and they are arranged on the same plane. In this photomask blanks 2, there is no substantial layering of the semi-permeable film 4 and the light-shielding film 5, and the edges of the photomask 1 pattern are defined on the semi-permeable film 4 and the light-shielding film 5, which are substantially single layers, respectively. In other words, the photomask 1 pattern is patterned on a photomask blanks 2 with a small overall film thickness and a small aspect ratio (ratio of pattern dimensions to height). This means that edge roughness is less likely to occur at the edges of the photomask 1 pattern, and the etching time is shortened. Therefore, it is possible to easily control the dimensions of the pattern during the manufacturing of the photomask 1 and to improve the dimensional accuracy of the pattern in the photomask 1.
[0082] Specifically, as shown in Figure 18, the semipermeable film 4 and the light-shielding film 5 are each substantially single layers, and the holes 7A,... of the hole pattern 7 of the photomask 1 are formed in the region of the semipermeable film 4, while the holes 7B,... are formed in the region of the light-shielding film 5. Therefore, in the photomask 1, the dimensions SA of each hole 7A and the dimensions SB of each hole 7B are finished to be faithful to the design. As a result, the dimensional accuracy of each hole 7A, 7B can be improved compared to when the hole pattern is formed in the laminated portion, and a highly accurate hole pattern 7 that is faithful to the design can be patterned.
[0083] Furthermore, according to the manufacturing method of the photomask 1 described above, the patterning of holes 7A,... on the semipermeable film 4 and the patterning of holes 7B,... on the light-shielding film 5 are performed in a single patterning process, rather than in separate patterning processes. Therefore, alignment errors naturally cannot occur, and the relative positional relationship of each hole 7A, 7B, such as the distance D between adjacent holes 7A, 7B, in the photomask 1 is faithful to the design. This improves the positional accuracy of each hole 7A, 7B, and in this respect as well, it is possible to pattern a highly accurate hole pattern 7 that is faithful to the design.
[0084] Furthermore, according to the first and second manufacturing methods of the photomask blanks 2 described above, films made of Cr-based material are used as the semipermeable film 4 and the light-shielding film 5. Cr-based materials have resistance to high pressure and chemicals, and possess film strength. Therefore, cleaning resistance equivalent to that of general photomasks can be obtained.
[0085] <Other Embodiments> It should be noted that the present invention is not limited to the embodiments described above, and various modifications are possible without departing from the spirit of the invention.
[0086] In the first and second methods for manufacturing the photomask blanks 2 described above, the first functional film and the second functional film are selected to have the same etching properties (in this document, when the etching properties are "the same" and the film material is "the same", this includes the concept of "approximation"). However, the present invention is not limited thereto. For example, i) the first functional film may be selected to have different etching properties from the second functional film and the interlayer, and the second functional film may be selected to have different etching properties from the first functional film and the interlayer. Or, ii) the first functional film may be selected to have different etching properties from the second functional film and the interlayer, and the second functional film may be selected to have different etching properties from the first functional film but the same etching properties as the interlayer.
[0087] Furthermore, in each of the above-described manufacturing methods for the photomask blanks 2, the residue 9 is removed so that the laminated portion is completely eliminated. However, the present invention is not limited thereto. For example, in areas of the photomask where the pattern edges do not overlap (pass through), the laminated portion 10 may be left as shown in Figure 19. In this case, the overlap amount L is set to a larger value, for example, 1 μm or more and 10 μm or less. Figure 19 is a drawing corresponding to the first manufacturing method of the photomask blanks 2 described above.
[0088] Furthermore, the photomask blank may also have a semipermeable film with a different transmittance formed on top of the photomask blank 2. In this case, the transmittance of the lower semipermeable film 4 (first semipermeable film) is readjusted by the upper semipermeable film (second semipermeable film). That is, the second semipermeable film functions as a transmittance adjusting film.
[0089] Furthermore, the photomask blank may be one in which a phase-shift film is formed on the photomask blank 2 described above. In this case, the lower semipermeable film 4 may be set to such an extent that it does not affect the phase-shift effect, that is, the phase shift amount may be set to 0 degrees or more and 20 degrees or less.
[0090] Furthermore, in the above embodiment, the pattern of the photomask 1 is a hole pattern 7. However, the hole pattern is merely an example, and the present invention is not limited thereto. The photomask pattern can include both patterns in which the edges of the pattern do not pass through the boundary between the region of the first functional film (region of the first pattern) and the region of the second functional film (region of the second pattern), and are set within each region of the first functional film and the second functional film, and patterns in which the edges of the pattern pass through the boundary between the region of the first functional film and the second functional film, and are set spanning the region of the first functional film and the second functional film. Various patterns can be used as appropriate.
[0091] Furthermore, in the above embodiment, either the first functional film or the second functional film is a semipermeable film 4, and the other is a light-shielding film 5. However, the present invention is not limited thereto. Appropriate functional films can be selected from various functional films as the first and second functional films. For example, a phase-shift film that is not intended for use as a semipermeable film may also be used.
[0092] Furthermore, as long as there is no physical interference, it is naturally possible to apply the technical elements described above to other embodiments or examples, to substitute the technical elements described above with technical elements relating to other embodiments or examples, and to combine the technical elements described above with each other, and this is naturally intended by the present invention. [Explanation of symbols]
[0093] 1...Photomask, 2...Photomask blanks, 3...Transparent substrate, 4...Semi-transparent film, 5...Light-shielding film, 6...Interlayer (etching stopper film), 7...Hole pattern, 7A...Hole in semi-transparent area, 7B...Hole in light-shielding area, 8...Resist film, 8a...Part, 9...Residue, 10...Laminated section
Claims
1. A method for manufacturing a photomask blank, comprising the steps of: partitioning a surface of a transparent substrate into a first pattern region and a second pattern region; forming a first functional film in the first pattern region; and forming a second functional film in the second pattern region, the method comprising the steps of: a photomask blanks preparation step of preparing a first photomask blank having a first functional film formed on a transparent substrate; a first patterning step of patterning a first functional film with a pattern corresponding to a region of a first pattern and removing the first functional film in a region of a second pattern; a functional film forming step of forming a second functional film on the exposed portion of the transparent substrate from which the first functional film has been removed and on the first functional film; and a second patterning step of patterning the second functional film with a pattern corresponding to the region of the second pattern and removing the second functional film in the region of the first pattern. A method for manufacturing photomask blanks.
2. The second patterning step comprises: a resist film forming step of forming a resist film on the second functional film; a resist pattern forming step of forming a resist pattern corresponding to a region of the second pattern, the resist pattern overlapping an edge portion of a laminated portion of the first functional film and the second functional film by offsetting an edge position of the resist pattern outward, with a predetermined overlap amount; and an etching step of removing the exposed portion of the second functional film in the region of the first pattern by etching using the resist pattern as a mask. The method for producing the photomask blank according to claim 1 .
3. The method further includes a finishing step of removing residue of the second functional film remaining due to a predetermined amount of overlap. The method for producing the photomask blanks according to claim 2 .
4. As a first photomask blank, a photomask blank in which a first functional film is formed on a transparent substrate and an intermediate film having etching characteristics different from those of the first functional film is formed on the first functional film is used; The second functional film is a film having the same etching characteristics as the first functional film. A method for producing the photomask blank according to any one of claims 1 to 3.
5. The first and second functional films are made of a material selected from the group consisting of Cr-based, Ni-based, Ti-based, Si-based, metal silicide-based, and metals with adjusted nitrogen content. The method for producing the photomask blanks according to claim 4 .
6. A photomask blank having a first functional film formed on a transparent substrate is used as a first photomask blank, The second functional film is a film having etching characteristics different from those of the first functional film. A method for producing the photomask blank according to any one of claims 1 to 3.
7. As the first functional film, a film having a function of adjusting the optical characteristics of the exposure light is used, As the second functional film, a film having a function of adjusting the optical characteristics of the exposure light and a function different from that of the first functional film is used. A method for producing a photomask blank according to any one of claims 1 to 6.
8. A phase shift film or a halftone film is used as either the first functional film or the second functional film, A light-shielding film is used as either the first functional film or the second functional film. The method for producing the photomask blanks according to claim 7 .
9. Either one or both of the first functional film and the second functional film are adjusted so that the etching rate is the same as that of the other of the first functional film and the second functional film. A method for producing a photomask blank according to any one of claims 1 to 8.
10. A photomask blanks preparation step of preparing a photomask blank manufactured by the method for manufacturing a photomask blank according to any one of claims 1 to 9; A patterning step of patterning the first functional film and the second functional film into a predetermined pattern. A method for manufacturing a photomask.
11. The patterning process includes only one drawing process. The method for producing a photomask according to claim 10 .
12. The patterning step comprises: a resist film forming step of forming a resist film on a surface of the photomask blank; a resist pattern forming step of forming a resist pattern according to a predetermined pattern, the resist pattern being determined in consideration of a difference in etching rate between the first functional film and the second functional film; and an etching step of removing exposed portions of the first functional film and the second functional film by etching using the resist pattern as a mask. The method for manufacturing a photomask according to claim 10 or 11.