Polyfunctional (meth)acrylate coating liquid, coating film, and laminate

JP2023084663A5Inactive Publication Date: 2024-12-05TOYO INK MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022161216
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-10-05
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing antireflection films lack sufficient scratch resistance against both rigid fibers like steel wool and flexible fibers like gauze, compromising surface smoothness and antifouling properties.

Method used

A coating liquid for forming a low refractive index layer containing specific particle sizes and compositions of inorganic oxide fine particles, polyfunctional (meth)acrylate, and fluorine-containing (meth)acrylate, which results in a layer with enhanced scratch resistance and antifouling properties.

Benefits of technology

The solution provides an antireflection film with improved scratch resistance against various abrasives and excellent antifouling properties, maintaining surface smoothness and transparency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a low refractive index layer formation coating liquid for a reflection preventing film which is excellent in the resistance to abrasion by various different polishing materials and is also excellent in the resistance to fouling.SOLUTION: A low refractive-index layer formation coating liquid for a reflection preventing film includes: hollow particles (A) with particle diameters (D50) of 150nm or less; inorganic oxide fine particles (B) with particle diameters (D50) of 10-90 nm and particle diameters (D99) of 150-300 nm [excluding the hollow particles (A)]; and polyfunctional (meta) acrylate (C), the liquid containing 0.5-15 pts.mass of the inorganic oxide fine particles (B) with respect to 100 pts.mass of the hollow particles (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a coating liquid for forming a low refractive index layer, a low refractive index layer, and an antireflection film. [Background technology]

[0002] BACKGROUND ART In order to suppress reflection of external light, an anti-reflection film or an anti-glare film having a low refractive index layer is provided on the image display surface of an image display device such as a liquid crystal display, an organic EL display, or a touch panel.

[0003] An anti-reflection film reduces reflectance by the light interference effect of light reflected from the surface of a low refractive index layer and light reflected from the interface between the low refractive index layer and a layer adjacent to the low refractive index layer (e.g., a hard coat layer or a high refractive index layer).

[0004] Anti-reflection films are often laminated on the outermost surface of displays, and are required to be scratch-resistant and wear-resistant.

[0005] In Patent Document 1, convex portions are formed on the surface of the low refractive index layer by adding inorganic oxide particles having an average particle diameter larger than the average thickness of the low refractive index layer to the low refractive index layer. The convex portions on the surface improve scratch resistance against steel wool. Since robust inorganic particles are less susceptible to scratches than soft organic polymer resins, forming convex portions on the surface using inorganic particles makes it more difficult for abrasives to come into contact with the surface layer of the polymer resin, improving the scratch resistance of the entire layer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2021 / 020504 Summary of the Invention [Problem to be solved by the invention]

[0007] In addition, anti-reflection films are used in various image display devices such as displays, and therefore require surface anti-fouling properties and easy wiping of stains. When wiping off stains, gauze or cloth impregnated with alcohol such as ethanol is often used, and the film must be scratch-resistant against the gauze.

[0008] However, when the low refractive index layer described in Patent Document 1 has an uneven surface, rigid fiber abrasives such as steel wool will contact the convex parts of the surface layer when a load is applied, and will not easily contact the polymer resin surface layer, whereas highly flexible fibers such as gauze or cotton cloth such as metal cloth will tend to contact not only the convex parts of the surface layer but also the concave parts. Therefore, although the abrasion resistance to steel wool can be improved, the reduced surface smoothness reduces the slipperiness to the abrasive, resulting in poor abrasion resistance to gauze and the like.

[0009] Therefore, the present invention aims to achieve both surface smoothness and robustness due to inorganic fine particles in order to form a low refractive index layer that has high scratch resistance against both rigid fibers such as steel wool and soft fibers such as gauze, and also aims to achieve the transparency, low reflectance, and antifouling properties required for an antireflection film.

[0010] That is, the problem to be solved by the present invention is to provide a coating liquid for forming a low refractive index layer for an antireflection film which has excellent scratch resistance against various abrasives and also has excellent antifouling properties. [Means for solving the problem]

[0011] The present inventors have conducted extensive research to solve the above problems and have come up with the following inventions. 50 ) is 150 nm or less hollow particles (A) and particle diameter (D 50 ) is 10 to 90 nm, and the particle diameter (D 99The coating liquid for forming a low refractive index layer contains inorganic oxide fine particles (B) (excluding hollow particles (A)) having a size of 150 to 300 nm, and a polyfunctional (meth)acrylate (C), and contains 0.5 to 15 parts by mass of the inorganic oxide fine particles (B) per 100 parts by mass of the hollow particles (A).

[0012] A second invention relates to the coating liquid for forming a low refractive index layer, which further contains a fluorine-containing (meth)acrylate (D).

[0013] The third invention relates to the coating liquid for forming a low refractive index layer, wherein the content of the fluorine-containing (meth)acrylate (D) is 0.5 to 10 mass % relative to 100 mass % of the nonvolatile content of the coating liquid for forming a low refractive index layer.

[0014] A fourth invention relates to the coating liquid for forming a low refractive index layer, wherein the polyfunctional (meth)acrylate (C) contains a polyfunctional (meth)acrylate having a silicone chain.

[0015] The fifth invention relates to a low refractive index layer formed from the coating liquid for forming a low refractive index layer.

[0016] The sixth invention is directed to a surface having a water contact angle of 90° or more and a steel wool contact strength of 200 g / cm 2 The low refractive index layer has a change in haze of 0.1 or less when subjected to 10 reciprocating motions under a load.

[0017] The seventh invention relates to an antireflection film comprising the above-mentioned low refractive index layer on a transparent substrate.

[0018] An eighth aspect of the present invention relates to the antireflection film, wherein the luminous reflectance is 1.5% or less. [Effects of the Invention]

[0019] The present invention has made it possible to provide a coating liquid for forming a low refractive index layer for an antireflection film that has excellent scratch resistance against various abrasives and also has excellent antifouling properties. DETAILED DESCRIPTION OF THE INVENTION

[0020] Hereinafter, embodiments of the present invention will be described, but first, the terms used in this specification will be explained. In this specification, unless otherwise specified, when "(meth)acrylic", "(meth)acrylo", "(meth)acrylic acid", "(meth)acrylate", and "(meth)acryloyloxy" are written, they respectively mean "acrylic or methacrylic", "acrylo or methacrylo", "acrylic acid or methacrylic acid", "acrylate or methacrylate", and "acryloyloxy or methacryloyloxy". In addition, "particle diameter (D 50 ) is 150 nm or less. 50 ) is 10 to 90 nm, and the particle diameter (D 99 ) is 150 to 300 nm" are sometimes referred to as "inorganic oxide fine particles (B)." In the present invention, a low refractive index means a refractive index of 1.45 or less. In addition, the particle diameter (D 50 ) and particle size (D 99 ) represent the particle sizes at which the cumulative values ​​are 50% and 99%, respectively, in the volume-based particle size distribution obtained from particle size distribution measurements, and can be determined using a Nanotrac particle size distribution analyzer that uses dynamic light scattering. The luminous reflectance is determined in accordance with JIS Z8722. Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a mixture of two or more types.

[0021] <Coating liquid for forming low refractive index layer> The coating liquid for forming the low refractive index layer has a particle diameter (D 50 ) is 150 nm or less (A) and particle diameter (D 50 ) is 10 to 90 nm, and the particle diameter (D 99 ) contains inorganic oxide fine particles (B) having a particle size of 150 to 300 nm and a polyfunctional (meth)acrylate (C), The inorganic oxide fine particles (B) are contained in an amount of 0.5 to 15% by mass relative to 100% by mass of the hollow particles (A).

[0022] <Hollow particle (A)> The hollow particles (A) have a particle diameter (D 50 ) are hollow particles having a diameter of 150 nm or less, and hollow particles include hollow silica particles, hollow polymer particles, etc., which have voids inside. Examples of polymers constituting the hollow polymer particles include crosslinked acrylic polymers, crosslinked styrene polymers, vinyl polymers, etc. Crosslinked acrylic polymers are preferred from the viewpoint of achieving a low refractive index. Commercially available hollow silica particles include Surulia 4320 (particle diameter (D 50 ) 60nm, JGC Catalysts and Chemicals), hollow polymer particles Techpolymer XX5964Z (particle diameter (D 50 )80nm, Sekisui Chemical Co., Ltd.) etc.

[0023] Particle diameter (D 50 ) is 150 nm or less, and preferably 80 nm or less from the viewpoint of haze and gauze resistance. The lower limit is not particularly limited, but is preferably 40 nm or more in order to improve the refractive index. The particle diameter of the hollow particles (D 50 ) can be determined using a Nanotrac particle size distribution analyzer that utilizes dynamic light scattering. An example of the Nanotrac particle size distribution measuring device is the "Nanotrac UPA" manufactured by Nikkiso Co., Ltd. Specifically, it can be added to a dilution solution so that the loading index value in the analysis software "Microtrac" becomes 1.0, and then measured. The diluent preferably uses the same dispersion solvent as the main component of the dispersion solvent for the hollow particles, and examples thereof include methyl isobutyl ketone, methyl ethyl ketone, and propylene glycol monomethyl ether.

[0024] In order to reduce the refractive index, the content of hollow particles is preferably 10 to 80 mass % and more preferably 15 to 70 mass % in 100 mass % of the nonvolatile content of the coating liquid for forming the low refractive index layer.

[0025] <Inorganic oxide fine particles (B)> The inorganic oxide particles (B) have a particle diameter (D 50 ) is 10 to 90 nm, and the particle diameter (D 99 ) are inorganic oxide fine particles having a diameter of 150 to 300 nm, excluding hollow particles (A). This can reduce haze and coloring, resulting in a low refractive index layer with excellent transparency. In addition, in order to achieve both transparency and scratch resistance, the particle diameter (D 99 ) is preferably 180 to 280 nm, more preferably 200 to 250 nm. In order to improve the scratch resistance of the low refractive index layer, the particle diameter (D 50 ) is preferably 50 to 90 nm, more preferably 65 to 90 nm. The dispersed particle size of the inorganic oxide fine particles can be determined by a microtrack particle size distribution measuring device or the like that utilizes dynamic light scattering. An example of a microtrack particle size distribution measuring device is "Nanotrack UPA" manufactured by Nikkiso Co., Ltd. Specifically, the loading index can be measured by adding an inorganic oxide fine particle dispersion prepared by dispersing inorganic oxide fine particles in a solvent to a dilution solution so that the loading index value becomes 1.0. The diluent preferably uses the same dispersion solvent as the main component of the dispersion solvent for the inorganic oxide fine particles, and examples thereof include methyl isobutyl ketone, methyl ethyl ketone, and propylene glycol monomethyl ether.

[0026] The inorganic oxide fine particles to be used are not particularly limited, but from the viewpoint of transparency and scratch resistance, aluminum oxide (Al2O3) or silica (SiO2) fine particles can be used. From the viewpoint of transparency and scratch resistance, aluminum oxide fine particles are preferred, and further, in order to improve scratch resistance, the aluminum oxide fine particles preferably have a θ-type and / or α-type crystal structure.

[0027] From the viewpoint of achieving both scratch resistance, a low refractive index, and transparency, the content of inorganic oxide fine particles (B) is preferably 0.3 to 5 mass %, more preferably 0.4 to 3 mass %, based on 100 mass % of the nonvolatile content of the coating liquid for forming the low refractive index layer.

[0028] The content of the inorganic oxide fine particles (B) is 0.5 to 15 parts by mass, preferably 1 to 10 parts by mass, and more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the hollow particles (A).Within this range, both scratch resistance and transparency can be achieved.

[0029] <Polyfunctional (meth)acrylate (C)> The polyfunctional (meth)acrylate (C) is not limited as long as it is a compound having two or more (meth)acrylate groups. Examples of the polyfunctional (meth)acrylate (C) include polyol poly(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; Trimers (isocyanurates) of (meth)acrylates having an isocyanate group, such as tris(2-acryloxyethyl) isocyanurate, EO-modified tris(2-acryloxyethyl) isocyanurate, PO-modified tris(2-acryloxyethyl) isocyanurate, and ε-caprolactone-modified tris(2-acryloxyethyl) isocyanurate; Other examples include, but are not limited to, polyacrylates of polymer polyols such as polyacrylic poly(meth)acrylates, polyurethane poly(meth)acrylates, and polyester (meth)acrylates having three or more (meth)acryloyl groups; polyepoxy (meth)acrylates; and the like.

[0030] In addition, from the viewpoint of scratch resistance and stain resistance, the polyfunctional (meth)acrylate (C) is preferably a polyfunctional (meth)acrylate having a silicone chain. The silicone chain in the present invention is a skeleton having a siloxane bond.

[0031] Commercially available products of the polyfunctional (meth)acrylate (C) include, but are not limited to, tris(2-acryloxyethyl)isocyanurate (e.g., FANCRYL FA-731A manufactured by Hitachi Chemical Co., Ltd., NEW FRONTIER TEICA (GX-8430) manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), EO-modified tris(2-acryloxyethyl)isocyanurate (e.g., ARONIX M-313 and M-315 manufactured by Toagosei Co., Ltd., NK Ester A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., and SARTOMER SR-368 manufactured by ARKEMA), PO-modified tris(2-acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris(2-acryloxyethyl)isocyanurate (e.g., NK Ester A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0032] From the viewpoint of achieving both scratch resistance and a low refractive index, the content of the polyfunctional (meth)acrylate (C) is preferably 10 to 90 mass %, more preferably 20 to 80 mass %, of 100 mass % of the nonvolatile content of the coating liquid for forming the low refractive index layer.

[0033] <Fluorine-containing (meth)acrylate (D)> The fluorine-containing (meth)acrylate (D) is not limited as long as it is a (meth)acrylate having a fluorine atom, and examples thereof include (meth)acrylates having a perfluoropolyether skeleton. Commercially available products include FLUOROLINK AD1700 (manufactured by Solvay) and Megafac RS-90 (manufactured by DIC).

[0034] By including the fluorine-containing (meth)acrylate (D), it is possible to improve the water contact angle of the surface and thereby improve the antifouling properties. The content of the fluorine-containing (meth)acrylate is preferably 1 to 11 mass %, more preferably 1.4 to 8 mass %, based on 100 mass % of the nonvolatile content of the coating liquid for forming the low refractive index layer.

[0035] <Optional ingredients> The low refractive index forming coating liquid of the present invention may further contain various additives, such as a photopolymerization initiator, a thermosetting resin, a polymerization inhibitor, a leveling agent, a slip agent, an antifoaming agent, a surfactant, an antibacterial agent, an antiblocking agent, a plasticizer, an ultraviolet absorber, an infrared absorber, an antioxidant, a silane coupling agent, a conductive agent, and an inorganic filler.

[0036] <Anti-reflective film> The anti-reflection film of the present invention has a low refractive index layer formed on a transparent substrate using the low refractive index forming coating liquid of the present invention. This makes it possible to provide an anti-reflection film that is excellent in abrasion resistance against various abrasives and in anti-fouling properties. The antireflection film may further have another cured film layer such as a hard coat layer or an optical adjustment layer, and preferably has a hard coat layer and a low refractive index layer in this order on the transparent substrate. Another cured film layer may be further provided between the transparent substrate layer and the hard coat layer or between the hard coat layer and the low refractive index layer. It is also preferable to have a hard coat layer, an optical adjustment layer, and a low refractive index layer in this order on the transparent substrate. The luminous reflectance of the antireflection film of the present invention is 1.5% or less, and from the viewpoint of antireflection properties, it is preferably 1.2% or less, and more preferably 1% or less.

[0037] [Low refractive index layer] The low refractive index layer is formed from the coating liquid for forming a low refractive index layer of the present invention, and can be obtained, for example, by applying the coating liquid for forming a low refractive index layer onto a hard coat layer or the like, drying it, and then curing it.

[0038] The low refractive index layer has a refractive index of 1.45 or less, and in order to reduce reflectance, the refractive index is preferably 1.41 or less. The thickness of the low refractive index layer is preferably 80 to 150 nm, more preferably 100 to 140 nm, in order to reduce reflectance.

[0039] The water contact angle is preferably 90° or more, which allows the anti-reflection film to have excellent anti-fouling properties. Furthermore, the higher the water contact angle, the higher the anti-fouling properties, so the water contact angle is preferably 100° or more, and more preferably 110° or more.

[0040] [Transparent base material] The transparent substrate is not particularly limited as long as it is a substrate having optical transparency, and examples thereof include glass, synthetic resin moldings, and films. The thickness of the substrate is not particularly limited, but is usually about 50 to 200 μm.

[0041] Examples of synthetic resin moldings include moldings of synthetic resins such as polymethyl methacrylate resin, copolymer resins containing methyl methacrylate as the main component, polystyrene resin, styrene-methyl methacrylate copolymer resin, styrene-acrylonitrile copolymer resin, polycarbonate resin, cellulose acetate butyrate resin, polyallyl diglycol carbonate resin, polyvinyl chloride resin, and polyester resin.

[0042] Examples of films include polyester films, polyethylene films, polypropylene films, cellophane films, diacetyl cellulose films, triacetyl cellulose (TAC) films, acetyl cellulose butyrate films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, ethylene vinyl alcohol films, polyolefin films, polystyrene films, polycarbonate films, polymethylpentel films, polysulfone films, polyether ether ketone films, polyether sulfone films, polyether imide films, polyimide films, fluororesin films, nylon films, and acrylic films.

[0043] [Hard coat layer] The hard coat layer can be formed using a conventionally known coating liquid for forming a hard coat layer, and is not particularly limited. For example, the hard coat layer can be obtained by laminating a conventional coating liquid for forming a hard coat layer containing an active energy ray-curable resin, a photopolymerization initiator, and the like, on a substrate. The hard coat layer usually has a thickness of about 0.5 μm to 5 μm, preferably about 3 to 5 μm for scratch resistance, and has a refractive index of about 1.5 to 1.8. From the viewpoint of anti-reflection, the refractive index is preferably 1.50 or more, and more preferably 1.60 or more.

[0044] [Optical adjustment layer] The optical adjustment layer can be formed using a conventionally known coating liquid for forming an optical adjustment layer, and is not particularly limited, but can be obtained, for example, by laminating a conventional coating liquid for forming an optical adjustment layer containing an active energy ray-curable resin, a photopolymerization initiator, etc., and high refractive index fine particles on the substrate or the hard coat layer. The optical adjustment layer usually has a thickness of about 30 to 500 nm, preferably about 50 to 300 nm from the viewpoint of anti-reflection.The refractive index is about 1.60 to 1.9, preferably 1.65 or more from the viewpoint of anti-reflection.

[0045] [Anti-reflection film manufacturing method] The method for producing an antireflection film is not particularly limited, but for example, an antireflection film can be obtained by forming a low refractive index layer on a substrate using a coating liquid for forming a low refractive index layer. Furthermore, when a hard coat layer is provided, for example, an antireflection film can be obtained by forming a hard coat layer on a substrate and then laminating a low refractive index layer on the hard coat layer. In addition, another cured film layer such as an optical adjustment layer may be further provided between the substrate layer and the hard coat layer or between the hard coat layer and the low refractive index layer. The thickness of the anti-reflection film is usually about 50 to 200 μm. [Example]

[0046] The present invention will be explained in more detail below with reference to examples and comparative examples, but the following examples are not intended to limit the technical scope of the present invention in any way. The blending amounts in the table are in mass %, and values ​​other than the solvent are calculated as non-volatile content. Note that blank spaces in the table indicate that no blending was performed. The average particle diameters of the hollow particles and inorganic oxide fine particles and the film thickness of the low refractive index layer were measured by the following methods.

[0047] <Average particle size of hollow particles and inorganic oxide particles> Measurements were carried out using a Nanotrac particle size distribution measuring device, "Nanotrac UPA" manufactured by Nikkiso Co., Ltd., which utilizes dynamic light scattering. Measurements were performed by adding hollow particles and inorganic oxide fine particles to a dilution solution so that the loading index value was 1.0. The dilution solution used was the same as the dispersion solvent that was the main component, depending on the dispersion solvent for the hollow particles and inorganic oxide fine particles.

[0048] <Thickness of low refractive index layer> The film thickness of the low refractive index layer was measured using an optical non-contact film thickness meter (FILMETRICS, Inc., F20 film thickness measuring device).

[0049] <Production of polyfunctional polyester acrylate> (Production of multifunctional polyester acrylate PE1) A four-neck flask equipped with a stirrer, reflux condenser, dry air inlet tube, and thermometer was charged with 80.0 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 250.0 parts of pentaerythritol triacrylate (manufactured by Nippon Kayaku Co., Ltd., pentaerythritol triacrylate trade name: KAYARAD PET-30, containing pentaerythritol tetraacrylate as a by-product) having a hydroxyl value of 122 mg KOH / g, 0.24 parts of methylhydroquinone, and 217.8 parts of cyclohexanone, and the mixture was heated to 60 ° C. Next, 1.65 parts of 1,8-diazabicyclo[5.4.0]-7-undecene was added as a catalyst, and the mixture was stirred at 90 ° C. for 8 hours. Next, 78.3 parts of methacrylic glycidyl ether and 54.0 parts of cyclohexanone were added, followed by 2.65 parts of dimethylbenzylamine as a catalyst. The mixture was stirred at 100°C for 6 hours, and the acid value of the reaction mixture was measured periodically while the reaction continued. When the acid value reached 5.0 mgKOH / g or less, the mixture was cooled to room temperature to terminate the reaction. The resulting resin varnish was pale yellow and transparent, and a 60% solids mixture of polyester acrylate and pentaerythritol tetraacrylate (solids mass ratio: polyester acrylate:pentaerythritol tetraacrylate = 76:24) was obtained as a multifunctional polyester acrylate PE1 solution. The multifunctional polyester acrylate PE1 had 8 functional groups and a weight-average molecular weight of 3,500.

[0050] 《Inorganic oxide fine particles (B)》 <Production of Aluminum Oxide Fine Particle Dispersion> [Aluminum oxide fine particle dispersion (1)] 35 parts of aluminum oxide (1) (θ-type crystals, primary particle diameter 10 nm), 14 parts of multifunctional polyester acrylate PE1 in solid content, 25.5 parts of methyl ethyl ketone as organic solvents, and 25.5 parts of methoxybutanol were mixed, stirred with a disperser, and then dispersed with a sand mill to obtain a uniform aluminum oxide particle dispersion (1) containing θ-type crystalline aluminum oxide particles (B-1). The aluminum oxide particles (B-1) had a particle diameter (D 50 ) is 80 nm, particle diameter (D 99 ) was 200 nm.

[0051] [Aluminum oxide fine particle dispersion (2)] A dispersion treatment was carried out in the same manner as in Production Example 1, except that 14.3 parts of aluminum oxide (1), 5.7 parts of multifunctional polyester acrylate PE1 in terms of solid content, and 40 parts of methyl ethyl ketone and 40 parts of methoxybutanol were mixed as organic solvents, to obtain a uniform aluminum oxide fine particle dispersion (2) containing θ-type crystalline aluminum oxide fine particles (B-2). The aluminum oxide fine particles (B-2) had a particle diameter (D 50 ) is 60 nm, particle diameter (D 99 ) was 160 nm.

[0052] [Aluminum oxide fine particle dispersion (3)] A dispersion treatment was carried out in the same manner as in Production Example 1, except that aluminum oxide (2) (θ-type crystals, primary particle diameter 30 nm) was used, to obtain a uniform aluminum oxide particle dispersion (3) containing θ-type crystalline aluminum oxide particles (B-3). The aluminum oxide particles (B-3) had a particle diameter (D 50 ) is 90 nm, particle diameter (D 99 ) was 280 nm.

[0053] [Aluminum oxide fine particle dispersion (4)] A dispersion treatment was carried out in the same manner as in Production Example 2, except that aluminum oxide (3) (α-type crystal, primary particle diameter 30 nm) was used, to obtain a uniform aluminum oxide particle dispersion (4) containing α-type crystalline aluminum oxide particles (B-4). The aluminum oxide particles (B-4) had a particle diameter (D 50 ) is 80 nm, particle diameter (D 99 ) was 200 nm.

[0054] [Aluminum oxide fine particle dispersion (5)] A uniform alumina dispersion (5) containing γ-type crystalline aluminum oxide fine particles (B-5) was obtained by dispersing the aluminum oxide (4) (γ-type crystal, primary particle diameter 10 nm) in the same manner as in Production Example 1. The aluminum oxide fine particles (B-5) had a particle diameter (D 50 ) is 80 nm, particle diameter (D 99) was 200 nm.

[0055] [Aluminum oxide fine particle dispersion (6)] A dispersion treatment was carried out in the same manner as in Production Example 2, except that aluminum oxide (5) (α-type crystal, primary particle diameter 50 nm) was used, to obtain a uniform aluminum oxide particle dispersion (6) containing α-type crystalline aluminum oxide particles (B'-1). The aluminum oxide particles (B'-1) had a particle diameter (D 50 ) is 110 nm, particle diameter (D 99 ) was 280 nm.

[0056] [Aluminum oxide fine particle dispersion (7)] A dispersion treatment was carried out in the same manner as in Production Example 1, except that aluminum oxide (3) (α-type crystal, primary particle diameter 30 nm) was used, to obtain a uniform aluminum oxide particle dispersion (5) containing α-type crystalline aluminum oxide particles (B'-2). The aluminum oxide particles (B'-2) had a particle diameter (D 50 ) is 90 nm, particle diameter (D 99 ) was 320 nm.

[0057] [Aluminum oxide fine particle dispersion (8)] A uniform alumina dispersion (8) containing γ-type crystalline aluminum oxide fine particles (B'-3) was obtained by dispersing the aluminum oxide fine particles (4) (γ-type crystals, primary particle diameter 10 nm) in the same manner as in Production Example 2. The aluminum oxide fine particles (B'-3) had a particle diameter (D 50 ) is 60 nm, particle diameter (D 99 ) was 140 nm.

[0058] <Silica fine particles> Inorganic oxide particles (B-6): MEK-AC-2140Z (Nissan Chemical Co., Ltd., silica particles, particle size (D 50 ) is 20 nm, particle diameter (D 99 ) is 150nm)

[0059] The types, crystal systems, and average particle sizes of the inorganic oxide fine particles are summarized below.

[0060] [Table 1]

[0061] <Preparation of Coating Liquid for Forming Hard Coat Layer or Optical Adjustment Layer> [Coating liquid 1 for forming hard coat layer or optical adjustment layer (Coating liquid 1)] Coating liquid 1 for forming a hard coat layer or an optical adjustment layer (coating liquid 1) was obtained by mixing 100 parts of zirconium oxide particles, 155.4 parts of multifunctional polyester acrylate PE1, 4.6 parts of ESACURE ONE (manufactured by IGM RESINS Co., Ltd.) as a photopolymerization initiator, and propylene glycol monomethyl ether as an organic solvent, adjusted to a non-volatile concentration of 40%.

[0062] [Coating liquid 2 for forming hard coat layer or optical adjustment layer (Coating liquid 2)] Coating liquid 2 for forming a hard coat layer or optical adjustment layer (coating liquid 2) was obtained by mixing 155.4 parts of multifunctional polyester acrylate PE1, 4.6 parts of ESACURE ONE (manufactured by IGM RESINS Co., Ltd.) as a photopolymerization initiator, and propylene glycol monomethyl ether as an organic solvent, adjusted to a non-volatile concentration of 40%.

[0063] [Coating liquid 3 for forming hard coat layer or optical adjustment layer (Coating liquid 3)] Coating liquid 3 for forming a hard coat layer or optical adjustment layer (coating liquid 3) was obtained by mixing 100 parts of titanium oxide particles, 60 parts of multifunctional polyester acrylate PE1, 3 parts of ESACURE ONE (manufactured by IGM RESINS Co., Ltd.) as a photopolymerization initiator, and propylene glycol monomethyl ether as an organic solvent, adjusted to a non-volatile concentration of 40%.

[0064] The materials used in the production of the examples and comparative examples are as follows. <Hollow particles> Hollow particles (A-1); Techpolymer XX-5964Z (hollow polymer particles, cross-linked acrylic resin, particle diameter (D 50)80nm, hollow rate 43%, solid content 10%, manufactured by Sekisui Plastics Co., Ltd.) Hollow particles (A-2); hollow polymer particles, vinyl resin, particle diameter (D 50 )150nm, solid content 10% Hollow particles (A-3); Surulia 4320 (hollow silica particles, particle diameter (D 50 ) 60 nm, particle refractive index 1.30, solid content 20.5%, manufactured by JGC Catalysts and Chemicals Co., Ltd. Hollow particles (A'-1); hollow silica particles, particle diameter (D 50 ) 200nm, solid content 20.5%

[0065] <Polyfunctional (meth)acrylate (C)> SIU2400: Miramer SIU2400 (10-functional urethane acrylate containing silicone chains, molecular weight 8000, manufactured by Miwon) DPHA-2C: KAYARAD DPHA-2C (a mixture of dipentaerythritol hexaacrylate and pentaerythritol tetraacrylate, manufactured by Nippon Kayaku Co., Ltd.) Multifunctional polyester acrylate PE1

[0066] <Fluorine-containing (meth)acrylate (D)> Fluorine-containing (meth)acrylate (D-1); FLUOROLINK AD1700 (perfluoropolyether urethane acrylate, solids content 65%, manufactured by Solvay) Fluorine-containing (meth)acrylate (D-2); Megafac RS-90 (fluorine-containing UV-reactive oligomer, solid content 10%, manufactured by DIC)

[0067] <Photopolymerization initiator> OMNIRAD907 (IGM RESINS Co., Ltd.)

[0068] [Example 1] <Preparation of Coating Liquid for Forming Low Refractive Index Layer> 100 parts (based on 100% solids) of hollow particles (A-1) (Techpolymer XX-5964Z, hollow polymer particles, crosslinked acrylic resin, average particle diameter 80 nm, manufactured by Sekisui Plastics Co., Ltd.) as hollow particles (A), 100 parts of Miramer SIU2400 (manufactured by Miwon) as polyfunctional (meth)acrylate (C), 15 parts (based on 100% solids) of fluorine-containing (meth)acrylate (D-1) (FLUOROLINK AD1700 (manufactured by Solvay)) as fluorine-containing (meth)acrylate (D), 4 parts of alumina dispersion (1), and 5 parts of OMNIRAD907 (manufactured by IGM Resins Co., Ltd.) as a photopolymerization initiator were thoroughly mixed, and propylene glycol monomethyl ether was used as an organic solvent to adjust the nonvolatile content to 4%, to obtain low refractive index layer-forming coating liquid X1. Since the aluminum fine particles (B-1) are contained in the alumina dispersion (1) at 25 mass %, the ratio of the hollow particles (A-1) to the alumina fine particles (B-1) is 100:1. The fluorine-containing (meth)acrylate (D) was contained in an amount of 6.78 mass % in the nonvolatile matter. The polyfunctional polyester acrylate PE1 is contained in the alumina dispersion (1) in an amount of 10 mass %.

[0069] <Production of anti-reflection film> On a 50 μm thick polyethylene terephthalate (PET) film ("Lumirror UH-13" manufactured by Toray Industries, Inc.), hard coat layer forming coating liquid 1 (coating liquid 1) was applied using a bar coater so that the film thickness after drying would be 3.0 μm, and then the hard coat layer was coated with 400 mJ / cm from a high-pressure mercury lamp. 2 The obtained low refractive index layer-forming coating liquid X1 was applied onto the hard coat layer using a bar coater so that the film thickness after drying would be 100 nm, and then irradiated with 400 mJ / cm 2 of ultraviolet light from a high-pressure mercury lamp in a nitrogen atmosphere with an oxygen concentration of 500 ppm or less. 2 The film was irradiated with ultraviolet light of 1000 kJ / cm to form a low refractive index layer, thereby obtaining an anti-reflection film.

[0070] [Examples 2 to 19, Comparative Examples 1 to 7] Coating liquids X2 to X26 for forming low refractive index layers, each having a nonvolatile content of 4%, were obtained in the same manner as in Example 1, except that the compositions and blending amounts (calculated as nonvolatile content) shown in Tables 1 to 3 were used. Subsequently, antireflection films were obtained in the same manner as in Example 1, except that low refractive index layer-forming coating liquids X2 to X26 were used.

[0071] [Examples 20, 21, and 28] In the same manner as in Example 1, a low refractive index layer-forming coating liquid X1 was obtained. As shown in Table 5, hard coat layer-forming coating solutions 1 to 3 (coating solutions 1 to 3) were applied to a 50 μm-thick polyethylene terephthalate (PET) film ("Lumirror UH-13" manufactured by Toray Industries, Inc.) or an 80 μm-thick triacetyl cellulose (TAC) film ("Fujitack" manufactured by Fujifilm Corporation) using a bar coater so that the film thickness after drying would be 3.0 μm. Then, the coating solution was exposed to 400 mJ / cm with a high-pressure mercury lamp. 2 The obtained low refractive index layer-forming coating liquid X1 was applied onto the hard coat layer using a bar coater so that the film thickness after drying would be 100 nm, and then irradiated with 400 mJ / cm 2 of ultraviolet light from a high-pressure mercury lamp in a nitrogen atmosphere with an oxygen concentration of 500 ppm or less. 2 The film was irradiated with ultraviolet light of 1000 kJ / cm to form a low refractive index layer, thereby obtaining an anti-reflection film.

[0072] [Example 22] In the same manner as in Example 1, a low refractive index layer-forming coating liquid X1 was obtained. The obtained low refractive index layer-forming coating liquid X1 was applied to a 50 μm-thick polyethylene terephthalate (PET) film ("Lumirror UH-13" manufactured by Toray Industries, Inc.) using a bar coater so that the film thickness after drying would be 100 nm, and then the coating liquid was irradiated with 400 mJ / cm 2 using a high-pressure mercury lamp in a nitrogen atmosphere such that the oxygen concentration was 500 ppm or less. 2 The film was irradiated with ultraviolet light of 1000 kJ / cm to form a low refractive index layer, thereby obtaining an anti-reflection film.

[0073] [Examples 23 and 24] In the same manner as in Example 1, a low refractive index layer-forming coating liquid X1 was obtained. As shown in Table 5, coating solution 1 or 3 was applied to a 50 μm thick polyethylene terephthalate (PET) film ("Lumirror UH-13" manufactured by Toray Industries, Inc.) using a bar coater so that the film thickness after drying would be 100 nm. Then, the coating solution was applied to a 50 μm thick polyethylene terephthalate (PET) film ("Lumirror UH-13" manufactured by Toray Industries, Inc.) using a high-pressure mercury lamp at 400 mJ / cm 2 The obtained low refractive index layer-forming coating liquid X1 was applied onto the optical adjustment layer using a bar coater so that the film thickness after drying would be 100 nm, and then irradiated with 400 mJ / cm 2 of ultraviolet light from a high-pressure mercury lamp in a nitrogen atmosphere such that the oxygen concentration was 500 ppm or less. 2 The film was irradiated with ultraviolet light of 1000 kJ / cm to form a low refractive index layer, thereby obtaining an anti-reflection film.

[0074] [Examples 25 to 27] In the same manner as in Example 1, a low refractive index layer-forming coating liquid X1 was obtained. As shown in Table 5, coating solution 1 or 2 was applied to a 50 μm thick polyethylene terephthalate (PET) film ("Lumirror UH-13" manufactured by Toray Industries, Inc.) using a bar coater so that the film thickness after drying would be 3.0 μm. Then, the coating solution was applied to the film using a high-pressure mercury lamp at 400 mJ / cm. 2 Coating Solution 1 or 3 was applied onto the hard coat layer using a bar coater so that the film thickness after drying would be 100 nm, and then irradiated with 400 mJ / cm 2 of ultraviolet light from a high-pressure mercury lamp in a nitrogen atmosphere with an oxygen concentration of 800 ppm or less. 2 The obtained low refractive index layer-forming coating liquid X1 was applied onto the optical adjustment layer using a bar coater so that the film thickness after drying would be 100 nm, and then irradiated with 400 mJ / cm 2 of ultraviolet light from a high-pressure mercury lamp in a nitrogen atmosphere such that the oxygen concentration was 500 ppm or less. 2 The film was irradiated with ultraviolet light of 1000 kJ / cm to form a low refractive index layer, thereby obtaining an anti-reflection film.

[0075] [Example 29] In the same manner as in Example 1, a low refractive index layer-forming coating liquid X1 was obtained. As shown in Table 5, on a 50-μm-thick polyethylene terephthalate (PET) film (「Lumirror UH-13」manufactured by Toray Industries, Inc.), coating liquid 1 for forming a hard coat layer (coating liquid 1) was applied using a bar coater so that the film thickness after drying would be 3.0 μm, and then irradiated with ultraviolet rays of 400 mJ / cm 2 using a high-pressure mercury lamp to form a hard coat layer. On the hard coat layer, the obtained coating liquid X1 for forming a low refractive index layer was applied using a bar coater so that the film thickness after drying would be 140 nm, and then irradiated with ultraviolet rays of 400 mJ / cm 2 using a high-pressure mercury lamp in a nitrogen atmosphere where the oxygen concentration was 500 ppm or less to form a low refractive index layer, obtaining an antireflection film.

[0076] [Evaluation Items and Evaluation Methods] The evaluation methods for the obtained low refractive index layer and antireflection film are as follows. The results are shown in Tables 2 to 5.

[0077] <Measurement of Refractive Index> Using a 「Prism Coupler Model 2010」manufactured by Metricon Corporation, the refractive indices of the low refractive index layer, hard coat layer, and optical adjustment layer at a wavelength of 594 nm were determined.

[0078] <HZ; Measurement of Haze Value> For the produced antireflection film, the haze value (HZ) of the surface of the low refractive index layer was measured using a 「Haze Meter SH7000」manufactured by Nippon Denshoku Industries Co., Ltd. Note that △ and ○ are at levels with no practical problems. [Evaluation Criteria] · ○: 1.5% or less · △: More than 1.5% and 2.0% or less · ×: More than 2.0%

[0079] <SW Resistance; Abrasion Resistance> For the produced antireflection film, the abrasion resistance was evaluated using a 「Gakushin-type Friction Fastness Tester」manufactured by Tester Sangyo Co., Ltd. A friction element with a load of 200 g attached (surface area 1 cm 2The surface of the hard coat layer (1 cm x 15 cm) was reciprocated 10 times with steel wool #0000 attached to the anti-reflection film. Thereafter, the haze value of the anti-reflection film was measured and evaluated according to the following criteria. [Evaluation criteria] ◎: ΔHz is 0.05% or less (very good) 〇: ΔHz is over 0.05% and 0.1% or less (good) △: ΔHz is greater than 0.1% and less than 0.2% (acceptable) ×: ΔHz exceeds 0.2% (bad) Here, ΔHz = haze value after scratch test - haze value before scratch test.

[0080] <Gauze resistance> The anti-reflection films thus prepared were evaluated for scratch resistance using a Gakushin-type abrasion fastness tester manufactured by Tester Sangyo Co., Ltd. A friction element (surface area 1 cm) with a load of 500 g was attached. 2 Gauze (Iwatsuki gauze, 100% cotton) was attached to the anti-reflection film, and the surface of the hard coat layer (1 cm x 15 cm) was rubbed back and forth 100 times. Thereafter, the haze value of the anti-reflection film was measured and evaluated according to the following criteria. [Evaluation criteria] 〇: ΔHz is 0.05% or less (very good) △: ΔHz is over 0.05% and 0.1% or less (good) ×: ΔHz exceeds 0.1% (bad)

[0081] <Stain resistance> The antifouling property was evaluated based on the water contact angle. The larger the contact angle, the easier it is to repel water and the less likely it is to get dirty. The water contact angle was measured using a fully automatic contact angle meter DM-701 manufactured by Kyowa Interface Science Co., Ltd., and the contact angle value on the surface of the low refractive index layer of the obtained anti-reflection film was determined. [Evaluation criteria] · 〇: Contact angle is 100° or more (very good) ·△: Contact angle is 90° or more and less than 100° (good) ×: Contact angle is less than 90° (bad) △ and ◯ are at levels that present no practical problems.

[0082] <Measurement of visual reflectance> Measurements were taken in accordance with JIS Z8722 using a Hitachi High-Tech Science Corporation "Spectrophotometer U4100" and "5-degree regular reflection accessory." The surface of the film opposite the anti-reflection layer was sanded with sandpaper, and then black ink was applied and allowed to dry, minimizing the influence of light reflection from the backside. △ and ◯ indicate levels that are acceptable for practical use. [Evaluation criteria] ◎: 0.5% or less 〇: Over 0.5% and 1.0% or less (very good) ·△: More than 1.0% and less than 1.5% (good) ·×: Exceeded by 1.5% (defective)

[0083] [Table 2]

[0084] [Table 3]

[0085] [Table 4]

[0086] [Table 5]

[0087] As shown in Tables 2 to 5, it has been revealed that the low refractive index layer formed using the coating liquid for forming a low refractive index layer of the present invention has high scratch resistance against both rigid fibers such as steel wool and soft fibers such as gauze, and also provides an antireflection film with excellent antifouling properties.

Claims

1. A coating liquid for forming a low refractive index layer provided in an anti-reflection film provided on an image display surface of an image display device, comprising: Particle diameter (D 50 ) is 150 nm or less, and hollow particles (A) having a particle diameter (D 50 ) is 10 to 90 nm, and the particle diameter (D 99 The polyfunctional (meth)acrylate coating liquid contains inorganic oxide fine particles (B) (excluding hollow particles (A)) having a size of 150 to 300 nm, and a polyfunctional (meth)acrylate (C), and contains 0.5 to 15 parts by mass of the inorganic oxide fine particles (B) per 100 parts by mass of the hollow particles (A).

2. The polyfunctional (meth)acrylate coating liquid according to claim 1 , further comprising a fluorine-containing (meth)acrylate (D).

3. The polyfunctional (meth)acrylate coating liquid according to claim 1 or 2, wherein the hollow particles (A) have a particle diameter (D50) of 80 nm or less and comprise at least one type selected from the group consisting of hollow silica particles and hollow polymer particles, and the inorganic oxide fine particles (B) comprise aluminum oxide fine particles.

4. A coating film which is formed from the polyfunctional (meth)acrylate coating liquid according to any one of claims 1 to 3 and provides a low refractive index layer.

5. The water contact angle of the surface is 90° or more, and the steel wool test shows a water contact angle of 200 g / cm 2 5. The coating film according to claim 4, which has a change in haze of 0.1 or less when subjected to 10 reciprocating motions under a load.

6. A laminate providing an anti-reflection film, comprising a transparent substrate and a low refractive index layer, the low refractive index layer being the coating film according to claim 4 or 5.

7. The laminate according to claim 6, which has a luminous reflectance of 1.5% or less.

8. A laminate comprising a transparent substrate, at least one of a hard coat layer and an optical adjustment layer, and a low refractive index layer having a thickness of 80 to 150 nm, the low refractive index layer having a visual reflectance of 1.5% or less, providing an anti-reflection film, the low refractive index layer being a coating film as described in claim 4 or 5.