Method for manufacturing sheet made of collection of flat powder by joining gap between flat surfaces of flat powder made of metal, alloy, metal oxide, or inorganic compound with collection of metal or metal oxide nanoparticles

By bonding flat powder surfaces using methanol-dispersed organometallic compounds to form metal or metal oxide nanoparticles, the method addresses the issue of ineffective bonding in flat powder sheets, achieving improved electromagnetic noise absorption and magnetic shielding with reduced material usage and costs.

JP2023160276A5Active Publication Date: 2024-11-06小林 博
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022070517
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-04-22
Publication Date
2024-11-06
Estimated Expiration
2042-04-22

AI Technical Summary

Technical Problem

Existing methods for forming sheets from flat powders of metals, alloys, or metal oxides fail to effectively bond the flat surfaces together, leading to reduced performance in electromagnetic noise absorption and magnetic shielding due to the use of dissimilar materials or excessive stress, which compromises the inherent properties of the flat powders.

Method used

A method involving the use of organometallic compounds dispersed in methanol to separate and bond flat powder surfaces via metal or metal oxide nanoparticles using frictional heat, ensuring the flat surfaces are joined without excessive stress or loss of properties, utilizing a low-viscosity, low-density liquid to facilitate separation and bonding.

Benefits of technology

This method allows for the production of sheets with enhanced bonding strength and preservation of the flat powders' properties, enabling effective electromagnetic noise absorption and magnetic shielding across a wide frequency band while reducing material usage and manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a sheet made of a collection of soft magnetic flat powder.SOLUTION: In a method, a raw material for a substance that joins flat surfaces of flat powder is liquefied into a low-viscosity, low-density liquid, the flat surfaces of the flat powder are overlapped through the liquid, the flat surfaces is transformed into a nano-sized substance that joins the flat surfaces, the nano-sized substance is changed to the substance that joins flat surfaces, and after this, the flat surfaces are joined together by the collection of the substance, an organometallic compound that precipitates metal or metal oxides through thermal decomposition is dispersed in methanol, the methanol dispersion is interposed between the flat surfaces of the flat powder, the methanol is vaporized, the collection of fine crystals of the organometallic compound is deposited in the gaps between the flat surfaces of the flat powder, compressive stress is applied to the collection of flat powder to thermally decompose the fine crystals of the organometallic compound, the collection of metal or metal oxide nanoparticles is deposited, and the flat surfaces of the flat powder are joined together via the collection of nanoparticles joined together by frictional heat.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to Excluding tin and zinc The gaps between the flat surfaces of flat powder made of metal, alloy, metal oxide, or inorganic compound are joined via a collection of nanoparticles of metal or metal oxide that are joined by frictional heat. Ta The present invention relates to a method for producing a sheet made of a collection of the flat powder. Powders with a large aspect ratio, which is the ratio of the average value of the major axis and minor axis to the thickness, are variously described as flat powder, flake powder, scale powder, thin plate powder, disk powder, and thin plate powder, but in the present invention, they are described as flat powder. On the other hand, flat powders made of soft metals or glass are generally described as flake powder, and are described as flake powder. The present invention first involves dispersing an organometallic compound, which is capable of precipitating a metal or a metal oxide upon thermal decomposition, in methanol having a low viscosity and density, and then dispersing the compound in the form of a dispersion. Excluding tin and zinc A suspension in which flat surfaces of flat powder made of any one of metals, alloys, metal oxides, and inorganic compounds are overlapped is produced in a container. Next, methanol is evaporated from the suspension in the container, and a collection of fine crystals of an organometallic compound is precipitated in the gaps between the flat surfaces of the flat powder and on the surface of the collection of flat powder. Furthermore, a plate material is placed over the entire surface of the collection of flat powder, and the entire surface of the plate material is evenly compressed, and the collection of fine crystals of the organometallic compound is crushed into a collection of finer crystals. After this, the container is heated while applying a compressive load evenly to the entire plate material, and the organometallic compound is thermally decomposed, and a collection of nanoparticles of metal or metal oxide is precipitated simultaneously in the gaps between the flat surfaces of the flat powder and on the surface of the collection of flat powder. Furthermore, the nanoparticles are bonded to the flat surfaces by frictional heat, and the nanoparticles are bonded to each other by frictional heat. As a result, a sheet in which the flat surfaces of the flat powder are bonded to each other through the collection of nanoparticles bonded by frictional heat is produced in the container. In addition, if the flat powder is a soft magnetic flat powder of a metal or alloy, and the material of the nanoparticles has a certain relative magnetic permeability, and at least one of the magnetic permeability loss in the complex magnetic permeability and the dielectric loss in the complex dielectric constant has a certain size, a sheet in which the flat surfaces of the flat powder are bonded together through a collection of nanoparticles can be used as a sheet with high electromagnetic wave reception sensitivity, absorbing electromagnetic noise, and as a sheet with a high magnetic shielding effect. In addition, if the flat powder is a flake powder of a metal or alloy, a sheet in which the flat surfaces of the metal or alloy flake powder are bonded together through a collection of metal nanoparticles with high electrical conductivity and thermal conductivity can be used as an antistatic sheet, an electromagnetic wave shielding sheet, a thermally conductive sheet, a sheet made of a metal or alloy with excellent surface lubricity, wiring for electrical equipment, an electrode, etc. In addition, if the flat surfaces of the flake powder of a metal or alloy are bonded together with nickel or aluminum nanoparticles with excellent transparency, a sheet with the gloss of the metal or alloy can be obtained without losing the color of the metal or alloy. Furthermore, if the flat powder is an insulating flat powder made of glass, alumina, or hematite, a sheet in which the flat surfaces of the flat powder are bonded together via a collection of insulating metal oxide nanoparticles can be used as an insulating sheet with high insulation properties. Also, if the flat surfaces of an inorganic luster pigment in which the surface of a flat powder made of glass or aluminum is covered with a coating made of a metal or metal oxide are bonded together using transparent nickel or aluminum nanoparticles, a sheet with the luster of the inorganic luster pigment can be obtained without losing the color of the inorganic luster pigment. The present inventor has filed a patent application for a method for producing a paste consisting of a collection of flat powders in which the flat surfaces of the flat powders overlap each other through a solution of an organic compound having a certain viscosity, as Patent Application No. 2020-139002. In other words, the flat surfaces of the flat powders are overlapped each other through a solution of an organic compound, and then the solution of the organic compound is vaporized to create a collection of flat powders in which the flat surfaces of the flat powders overlap each other. Furthermore, one surface of the collection of flat powders is evenly compressed, and the flat surfaces of the flat powders are joined together by frictional heat to produce a sheet consisting of the collection of flat powders. In contrast, the present invention produces a sheet in which the flat surfaces of the flat powder are bonded together through a collection of nanoparticles of metal or metal oxide bonded by frictional heat. For this purpose, an organometallic compound that precipitates metal or metal oxide by thermal decomposition is dispersed in methanol, which has both low viscosity and density, and the flat surfaces of the flat powder are overlapped together through the methanol dispersion. After this, the collection of flat powder is compressed, and the organometallic compound is further thermally decomposed, and the flat surfaces of the flat powder are bonded together through a collection of nanoparticles of metal or metal oxide bonded together by frictional heat. In other words, since the flat surfaces of the flat powder are not completely flat, even if the collection of flat powder in which the flat surfaces are overlapped is compressed evenly, the flat powders are not bonded together by frictional heat over the entire surface of the flat surface, but are bonded together by frictional heat in a part of the flat surface. Therefore, the lower the flatness of the flat powder, the weaker the bonding force between the flat surfaces. In contrast, in the present invention, the entire surfaces of the flat powder are bonded together with a collection of nanoparticles that are two or more orders of magnitude smaller than the area of ​​the flat powder. Therefore, even if the flatness of the flat powder is low or the flat powder has irregularities, the nanoparticles are nearly two orders of magnitude smaller than the irregularities of the flat powder, so regardless of the flatness of the flat powder and the irregularities of the surface, the entire surfaces of the flat powder are bonded together with the collection of nanoparticles, and the bonding strength between the flat powder particles is increased. Furthermore, in the bonding of the flat surfaces in the present invention, the size of the nanoparticles precipitated in the gaps between the flat surfaces is small, about 10 nm, and the deposition density of the nanoparticles is high, so that when a compressive stress is applied to the collection of nanoparticles, the nanoparticles are difficult to move, and the strength of the nanoparticles bonded to the flat surfaces and the bonding strength between the nanoparticles themselves are increased. For this reason, in the present invention, the collection of fine crystals of the organometallic compound precipitated in the gaps between the flat surfaces is once crushed to a limit size, and the collection of finer crystals is stacked at high density in the gaps between the flat surfaces. After this, a compressive load is applied to the entire collection of flat powder with overlapping flat surfaces, and the finer crystals of the organometallic compound are thermally decomposed, and nanoparticles of metal or metal oxide with a size of about 10 nm are precipitated simultaneously in the gaps between the flat surfaces, overlapping with high density, and further, when stress is applied to the collection of nanoparticles, the nanoparticles are bonded to the flat surfaces by frictional heat, and the nanoparticles are bonded to each other by frictional heat. This results in a sheet with various properties made of a collection of flat powder particles with increased bonding strength between the flat powder particles. [Background technology]

[0002] There are four types of powders with flake-shaped or flat surfaces made of either metal, alloy, metal oxide, or inorganic compound: soft magnetic flat powder made of metal or alloy, flake powder made of metal or alloy, insulating flat powder made of metal oxide or inorganic compound, and inorganic luster pigments in which the surface of flat powder made of glass or aluminum is coated with a coating made of metal or metal oxide. First, the background art related to soft magnetic flat powder made of metal or alloy will be described. If the flat surfaces of soft magnetic flat powder can be joined together, a sheet made of a collection of flat powder can be formed, and by utilizing the complex permeability of the flat powder, it can become a sheet that absorbs electromagnetic noise. In addition, by utilizing the relative permeability of the flat powder, it can become a sheet that shields magnetism. Meanwhile, in recent years, electronic devices that use high-frequency signals, such as mobile phones and personal computers, have become increasingly popular. For example, some mobile phones and wireless LANs use high-frequency signals ranging from several GHz to 10 GHz. Furthermore, as electronic devices use higher frequencies, and as they become smaller, thinner, and more powerful, malfunctions caused by electromagnetic interference within the electronic devices and interference caused by noise radiated to the outside of the devices have become problems. For this reason, the CISPR22 standard issued by the International Special Committee on Radio Interference (CISPR) in 2005 regulates electromagnetic noise up to 6 GHz.

[0003] The absorbed energy P of electromagnetic noise is given by Equation 1. The first term is the absorption of electromagnetic noise based on the properties of soft magnetism, where magnetic loss occurs depending on the magnitude of the imaginary part μ” of the complex permeability and the frequency, and this magnetic loss is converted into heat. The second term is the absorption of electromagnetic noise based on the properties of a dielectric material, where dielectric loss occurs depending on the magnitude of the imaginary part ε” of the complex permittivity and the frequency, and this dielectric loss also converts into heat. The third term is the absorption of electromagnetic noise based on electrical conductivity, where a conductive current flows on the surface due to the skin effect of the high-frequency electric field, forming a resistive film, and this resistive film generates a resistive loss depending on the magnitude of the electrical conductivity σ, and this resistive loss also converts into heat. Therefore, if an electromagnetic noise absorbing sheet has a certain imaginary part μ” of the complex permeability in the frequency band of electromagnetic noise, or if it has a certain imaginary part ε” of the complex permittivity, then electromagnetic noise in a certain frequency band will be absorbed. In formula 1, E is the magnitude of the electric field in the electromagnetic noise, H is the magnitude of the magnetic field in the electromagnetic noise, f is the frequency of the electromagnetic noise, and σ is the conductivity. When a magnetic material receives an alternating magnetic field in electromagnetic noise, a phase lag occurs in the change in magnetic flux density, and the magnetic permeability is given by μ'-jμ”, which is the difference between the real part μ' and the imaginary part μ”. Alternatively, when a dielectric material receives an alternating electric field in electromagnetic noise, a phase lag occurs in the change in electric flux density, and the dielectric constant is given by the difference ε'-jε”. (Number 1) P = πfμ”H 2 +πfε”E 2 +1 / 2 σE 2

[0004] Conventionally, the performance of a sheet that absorbs electromagnetic noise has been determined based on the magnetic permeability of the soft magnetic material that forms the sheet. In other words, for electromagnetic noise up to around 100 MHz, the magnetic flux convergence effect due to the real part μ' of the complex permeability of the soft magnetic material shields the magnetic field and provides a magnetic shielding effect. In addition, the magnetic loss effect due to the imaginary part μ” of the complex permeability absorbs electromagnetic noise and converts it to heat, suppressing the electromagnetic noise. However, for many soft magnetic materials, the real part of the complex permeability decreases from frequencies just before 100 MHz, and the larger the value of the real part, the more rapidly it decreases. This phenomenon is known as the snake limit, where the larger the real part of the complex permeability of ferrite is, the lower the real part becomes when it exceeds 10 MHz. On the other hand, the imaginary part of the complex permeability increases rapidly from the frequency just before the frequency at which the real part shows a peak value, shows a peak value at a certain frequency, decreases the further it gets from the frequency at which the peak value is reached, and does not have the necessary magnitude in the frequency band above 500 MHz.

[0005] On the other hand, if the imaginary part of the complex dielectric constant in the properties of the dielectric has a certain magnitude in the frequency band above 500 MHz, the electromagnetic noise in the frequency band above 500 MHz will be absorbed by the dielectric loss of the dielectric material based on Equation 1. In other words, the dipoles of the dielectric (called orientation polarization) cannot follow the change in the electric field above 500 MHz, and dielectric dispersion occurs, in which the dielectric constant of the dielectric decreases. This phenomenon is a phenomenon in which a phase delay occurs in the change in electric flux density in the alternating electric field of the electromagnetic noise described in paragraph 3. However, in the frequency band above 500 MHz, the value of the imaginary part of the complex dielectric constant of most solid dielectrics is small. This will be explained below using the value of the imaginary part of the complex dielectric constant of a dielectric at 2.45 GHz microwaves used in microwave ovens. The imaginary part of the complex permittivity of polymeric materials at 2.45 GHz is 0.2-0.5 for phenolic resin, 0.16-0.23 for urea resin, 0.08-0.25 for polyvinyl chloride resin, 0.12-0.28 for polyamide resin, 0.03-0.42 for cellulose resin, 0.027-0.03 for synthetic rubber, and 1.2×10 for polyethylene resin. -3 And polypropylene resin is 4 x 10 -4The imaginary part of the complex dielectric constant of all polymeric materials is small. On the other hand, the imaginary part of the complex dielectric constant of water, a typical polar molecule, is large at 22.0. For this reason, the magnitude of the imaginary part of the complex dielectric constant of water at 2.45 GHz is used as the principle behind heating food in microwave ovens. In other words, when food is irradiated with microwaves of 2.45 GHz, the water molecules contained in the food are unable to keep up with the change in the electric field, and instead absorb the microwaves due to dielectric loss and convert them into heat. On the other hand, the imaginary part of the complex dielectric constant of ice at 2.45 GHz is 2.8×10 -4 is small. For this reason, ice does not melt when exposed to microwaves. In this way, except for liquids made of polar molecules such as water, alcohol, and acetone, the imaginary part of the complex dielectric constant of many substances in the frequency band above 500 MHz is small, and they cannot absorb electromagnetic noise in the frequency band above 500 MHz.

[0006] By the way, electromagnetic waves have a skin depth. The skin depth is the distance at which the electromagnetic field of the electromagnetic waves incident on a sheet made of a soft magnetic material attenuates to 1 / e (equivalent to 0.368). The skin depth is inversely proportional to the square root of the product of the frequency of the electromagnetic waves, the complex permeability of the flat powder, and the conductivity of the flat powder. Therefore, the higher the frequency of the electromagnetic waves, the higher the complex permeability of the flat powder, and the higher the conductivity of the flat powder, the shallower the skin depth. For this reason, if the skin effect is utilized, the thickness of the sheet made of the soft magnetic material will be thin and the sheet will be light. Therefore, if the thickness of the sheet made of the soft magnetic material is changed according to the frequency band of the electromagnetic waves to be absorbed and the sheet is constructed with the required thickness, the amount of soft magnetic material used will be small and the sheet will be light. Similarly, for a sheet that shields magnetism, if the thickness of the sheet made of the soft magnetic material is changed according to the frequency band of the electromagnetic waves to be shielded and the sheet is constructed with the required thickness, the amount of soft magnetic material used will be small and the sheet will be light.

[0007] Patent Document 1 discloses a sheet made of a new material composition as a sheet that absorbs electromagnetic waves. That is, the sheet absorbs electromagnetic waves by fine particles of a magnetic material, and includes a first magnetic layer made of a polymeric material in which the fine particles of a magnetic material are dispersed, a non-magnetic layer made of a polymeric material formed on the first magnetic layer, and a second magnetic layer made of a polymeric material in which fine particles of a magnetic material are dispersed, formed on the non-magnetic layer, in which the direction of the easy axis of magnetization in the first magnetic layer is different from the direction of the easy axis of magnetization in the second magnetic layer. In other words, this is an electromagnetic wave absorbing sheet designed to efficiently absorb electromagnetic waves by using a second magnetic layer having an easy axis direction different from that of the first magnetic layer, even if electromagnetic waves are radiated in a direction that cannot be efficiently absorbed by the first magnetic layer. However, if the magnetic material that absorbs electromagnetic waves is not a fine particle but a flat powder with a certain area, then a sheet can be formed by randomly joining the flat surfaces in the direction of the easy axis of magnetization, eliminating the need to form the three layers described in Patent Document 1, and making it possible to produce an inexpensive sheet.

[0008] Patent Document 2 discloses a flat powder of an alloy having even higher magnetic permeability by intentionally deviating from the composition of an Fe-9.6%Si-5.4%Al alloy, which is an alloy powder having high magnetic permeability. Patent Document 2 describes an example of a sheet using flat powder of this alloy, in which chlorinated polyethylene is dissolved in toluene, the flat powder of the alloy powder is mixed into this solution, and then the solution is coated on polyester resin and dried, and then pressed at 130°C under a pressure of 15 MPa to produce a composite sheet, which is a highly magnetic permeable sheet. However, chlorinated polyethylene resin is a non-magnetic material and does not contribute to electromagnetic wave absorption or magnetic shielding. Therefore, the electromagnetic wave absorption performance and magnetic shielding performance of the composite sheet decrease depending on the volume ratio of the non-magnetic chlorinated polyethylene resin. It is also described that alloy flat powder has high magnetic permeability when the flatness ratio is 15 or more. However, in order to reflect the magnetic permeability characteristics of flat powder with a large flatness ratio in the composite sheet, the flat planes must be aligned and overlapped in the same direction as the sheet surface, so that the collection of flat powder efficiently contributes to electromagnetic wave absorption and magnetic shielding. However, simply mixing flat powder with a size of tens of microns or less into a solution of chlorinated polyethylene and applying this mixture does not align the flat planes of the flat powder in the same direction as the sheet surface. In this way, even if the magnetic permeability characteristics of a soft magnetic material are excellent, unless the magnetic permeability characteristics of the soft magnetic material are reflected in the sheet structure, the sheet will not reflect the magnetic permeability characteristics.

[0009] Next, the background art related to flake powder made of metal or alloy will be described. If flat surfaces of flake powder made of metal or alloy can be joined together to form a sheet made of a collection of flake powder, it can be used for antistatic sheets, electromagnetic shielding sheets, wiring for electrical devices, electrodes, etc. To form such conductive sheets, a conductive paste is used to form a conductive film. Conventional conductive pastes are composed of a fluid composition in which conductive fillers made of metal or alloy are dispersed in a vehicle made of a resin binder and a solvent. When the conductive paste is printed by a method such as screen printing, the conductive fillers are reflected on the printed material through the liquid substance, and the liquid substance made of a resin binder and a solvent plays a role in carrying the conductive fillers, so the liquid substance is called a vehicle. These conductive pastes are divided into two types: a resin-curing type in which the conductive fillers are bonded together through the hardening of the resin, forming an electrical path through the conductive filler; and a fired type in which the organic components are volatilized by firing, sintering the conductive fillers together, and the sintered conductive filler forms an electrical path. Resin-curing conductive paste is a paste-like composition consisting of a conductive filler made of metal powder or alloy powder and an organic binder in which a thermosetting resin such as epoxy resin is dissolved. When heat is applied, the thermosetting resin hardens and shrinks together with the conductive filler, and the conductive fillers are pressed together through the hardened resin to come into contact with each other, providing conductivity. This resin-curing conductive paste is heated at a low temperature of about 200°C, so it is less susceptible to heat damage and is used to form wiring on printed wiring boards and circuit boards made of heat-sensitive synthetic resins. On the other hand, the sinterable conductive paste is a paste-like composition in which a conductive filler made of metal powder or alloy powder and glass frit are dispersed in an organic vehicle, and is sintered at a high temperature of about 900°C to volatilize the organic vehicle, melt the glass frit, and sinter the metal powders or alloy powders together to provide conductivity. At this time, the glass frit bonds the conductive film made of metal powder or alloy powder to the substrate, and the organic vehicle makes the metal powder or alloy powder and the glass frit into a liquid medium that makes printing possible. The sinterable conductive paste cannot be used for printed wiring boards or circuit boards made of synthetic resin because of its high sintering temperature, but the metal powder or alloy powder is sintered and integrated, which allows for low resistance, and is used, for example, for internal electrodes of multilayer ceramic capacitors.

[0010] The conductive paste is composed of a dispersion liquid in which a metal powder or an alloy powder is used as a conductive filler, and the metal powder or the alloy powder, or the metal powder or the alloy powder and the glass frit, are dispersed in a vehicle consisting of a resin binder and an organic solvent. The conductive film formed by this conductive paste has various problems due to the use of the metal powder or the alloy powder as the conductive filler and the dispersion of this metal powder or the alloy powder. The first problem is that the resistance of the conductive film formed by the heat treatment of the conductive paste is higher than that of the metal powder or alloy powder. That is, in the resin-curing conductive paste, the insulating thermosetting resin prevents the metal powders or alloy powders from directly contacting each other. In the sintering conductive paste, the glass frit, which has low conductivity, prevents the metal powders or alloy powders from sintering each other. This increases the electrical resistance of the wiring, electrodes, electromagnetic shielding film, antistatic film, etc. of the electric circuit formed by the heat treatment of the conductive paste, resulting in loss of electrical energy and heat generation, which causes malfunctions. The second problem is the dispersibility of the metal or alloy powder. In other words, if the dispersibility of the metal or alloy powder aggregates in the vehicle is poor, the metal or alloy powder will be unevenly distributed after heat treatment and will not be able to directly contact each other. As a result, as in the above, the electrical resistance of the wiring, electrodes, electromagnetic shielding film, and antistatic film of the electric circuit formed by heat treatment of the conductive paste will increase. The third problem is that when metal powders or alloy powders are sintered together, the metal powders or alloy powders shrink, which can cause structural defects in the internal electrodes of multilayer ceramic capacitors, such as delamination between the electrodes and the dielectric and cracks in the electrode layers. The fourth problem is that metal powders or alloy powders aggregate together. Furthermore, the finer the powder, the more likely it is to aggregate. When powder aggregates, the dispersibility of the powder in the vehicle deteriorates, and as a result, the electrical resistance of the conductive film formed by heat treatment of the conductive paste increases. All four of the above problems are caused by the use of metal powder or alloy powder as the conductive filler and the dispersion medium that disperses the aggregates of this metal powder or alloy powder, and therefore it is difficult to fundamentally solve them.

[0011] Various attempts have been made to solve the problems associated with conductive films using conductive pastes. For example, Patent Document 3 describes a conductive paste that does not contain a resin component as a binder, and is composed of a metal powder filler in which a metal powder of a relatively base metal is coated with a relatively noble metal, metal nanoparticles coated with a coating agent, and an organic solvent. In order to disperse the metal nanoparticles in the conductive paste, the metal nanoparticles are coated with an alkylamine that has affinity for the organic solvent and has a boiling point close to that of the organic solvent. When the applied conductive paste is heat-treated, the metal nanoparticles precipitate, and the metal filler is bonded by the metal nanoparticles to form a conductive film that does not contain a resin component. However, metal nanoparticles are very prone to aggregation, and once aggregated, they are nano-sized particles, so it is difficult to release the aggregation, and they are fine particles that are difficult to handle. Furthermore, when generating metal nanoparticles, the generated metal nanoparticles easily aggregate with each other. For this reason, it is not possible to adsorb alkylammine to the generated metal nanoparticles, and metal nanoparticles coated with alkylammine are produced by precipitating metal nanoparticles in a liquid containing alkylammine, covering the metal nanoparticles with alkylamine, and evaporating the liquid components other than alkylammine. For this reason, the manufacturing cost of coating metal nanoparticles with alkylamine is much higher than the cost of producing conductive paste. Therefore, versatile conductive films such as wiring for electric circuits, electrodes, electromagnetic shielding films, and antistatic films become expensive films. It should be noted that Patent Document 3 describes the use of metal nanoparticles coated with alkylammine as a conductive paste, but does not describe a manufacturing method for coating metal nanoparticles with alkylamine.

[0012] Patent Document 4 describes a conductive paste made of silver oxide and fatty acid silver salt having one or more amino groups. In other words, when a coating film coated with the conductive paste is heat-treated, the fatty acid silver salt is decomposed into silver by the heat treatment, and the fatty acid or its decomposition products produced by the decomposition are volatilized, while a part of the fatty acid produced by the decomposition reacts with silver oxide to generate fatty acid silver salt again, and this fatty acid silver salt is decomposed into silver and fatty acid, repeating this cycle to form a conductive film made of silver. However, fatty acid silver having one or more amino groups is produced by dissolving at least one hydroxyl-containing α-amino acid, consisting of 2-aminoisobutyric acid, DL-threonine, DL-serine, DL-norvaline, and 6-aminohexane, in a solvent consisting of butyl carbitol, methyl ethyl ketone, isophorone, α-terpineol, etc., adding silver oxide powder to the solution, and reacting it at room temperature for a long time. Therefore, the cost of producing fatty acid silver using the above-mentioned special chemicals is much higher than the cost of producing a conductive paste. Therefore, as in the above-mentioned Patent Document 3, versatile conductive films such as wiring for electric circuits, electrodes, electromagnetic wave shielding films, and antistatic films become expensive films.

[0013] Next, the background art related to insulating flat powder made of glass, alumina, or hematite will be described. When describing flat glass powder as one type of insulating flat powder, it is described as flat glass powder, and when describing flat glass powder as an individual flat powder, it is described as glass flake powder. This is because flat glass powder is generally called glass flake powder. Since flat silica powder has a thickness of 0.1 μm or less, it is likely to be crushed when flat surfaces are bonded together with a collection of metal oxide nanoparticles, so it was excluded from the insulating flat powder. In addition, flat mica and boron nitride powders were excluded from the insulating flat powder because the interlayer bonds of the crystals are easily broken by shear stress, and crystal pieces are peeled off from the flat powder when flat surfaces are bonded together. The electrical resistivity of the flat powder made of glass and alumina is 10 14 It has a high insulation of more than Ωcm. Therefore, if the flat surfaces of the flat powder can be bonded together with a collection of highly insulating metal oxide nanoparticles, an insulating sheet with extremely high insulation resistance will be formed. Of the glass flake powder, only soda-lime glass has a high insulation resistance of 10 12 The electrical resistivity of hematite (a substance made of the alpha phase of ferric oxide Fe2O3) is 10 8However, if the thickness of the flat powder is submicron and the cross-sectional area of ​​the flat powder of hematite is 0.3 μm × 10 μm, the electrical resistance per unit length of the flat powder is 3.3 × 10 16 On the other hand, the electrical resistance of a collection of flat powders where the flat surfaces overlap each other is such that the electrical resistance of a very large number of flat powders forms series and parallel connections, and an insulating film made of a collection of hematite flat powders exhibits high insulation. Hematite flat powder is a red pigment called red iron oxide, and is a general-purpose flat powder. On the other hand, when excessive compressive stress is applied to the flat surfaces of many insulating flat powders, the flat powder does not undergo plastic deformation but undergoes brittle fracture. For this reason, when joining flat surfaces together, it is necessary to join them in a way that does not apply excessive stress to the flat surfaces. In addition, it is necessary that the material that joins the flat surfaces together does not reduce the insulating properties of the flat powder. As described above, flat powders made of glass, alumina, or hematite are excellent raw materials for forming insulating sheets. However, there have been no cases to date where flat surfaces of insulating flat powders are joined together in a manner that does not apply excessive stress to the flat surfaces and does not reduce the insulating properties of the flat powder. In addition, there are inorganic luster pigments with excellent luster, in which the surface of flat powder made of glass or aluminum is coated with metals such as gold, silver, and nickel, or metal oxides such as titanium oxide and iron oxide, by electroless plating. However, up to now, inorganic luster pigments have only been used as pigments. In contrast, if the flat surfaces of the flat powder of the inorganic luster pigment can be bonded together with a transparent material, a sheet made of a collection of flat powder of the inorganic luster pigment can be created without losing the color reflected from the luster pigment. Furthermore, if a sheet made of a collection of flat powder of multiple types of luster pigments is created using multiple types of luster pigments that reflect different colors, the color tone reflected by the sheet can be changed to various colors by combining multiple types of luster pigments. However, there has been no case to date in which the flat surfaces of the flat powder of the inorganic luster pigment can be bonded together with a transparent material in a manner that does not damage the coating of metal oxides such as titanium oxide and iron oxide. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2008-198873 A [Patent Document 2] JP 2007-118114 A [Patent Document 3] JP 2014-035974 A [Patent Document 4] JP 2010-102884 A [Non-patent literature]

[0015] [Non-Patent Document 1] Sanyo Special Steel Technical Report, VOl.13, No.1, 53-61 Summary of the Invention [Problem to be solved by the invention]

[0016] First, a problem that arises when forming a sheet made of an assembly of flat powder in which the flat surfaces of soft magnetic flat powder are joined together will be described. It is known that when soft magnetic powder is flattened in the plane direction, which is the easy axis of magnetization, the demagnetizing factor becomes smaller, and the larger the flattening ratio, the larger the imaginary part μ" of the complex permeability. In addition, soft magnetic powder is made of metal or alloy, except for ferrite, and is therefore conductive. For this reason, the imaginary part μ" of the complex permeability and the electrical conductivity of conductive soft magnetic flat powder contribute to absorbing electromagnetic noise in formula 1 described in paragraph 3. Furthermore, the flattening process of soft magnetic powder does not rely on long batch processing using a ball mill, but on atomized soft magnetic powder or reduced soft magnetic powder being attrited using a media stirring mill, so that flat powder can be obtained continuously in a short time and is manufactured using inexpensive processing. On the other hand, a sheet made of a collection of flat powders in which the flat surfaces of soft magnetic flat powders are overlapped and the overlapping flat surfaces are joined with a substance having a constant value for at least one of the imaginary part of the complex permeability or the imaginary part of the complex permittivity, can be formed into a sheet with a large area using a small amount of flat powder. In addition, since the flat surfaces form the sheet surface, all of the flat surfaces participate in absorbing electromagnetic waves, resulting in a sheet with high electromagnetic wave reception sensitivity and high electromagnetic wave absorption performance. This sheet maximizes the flat effect of the soft magnetic flat powder. Furthermore, if the thickness of the sheet can be freely changed according to the frequency band of the electromagnetic waves to be absorbed, the skin effect can be utilized, and a lighter sheet can be formed using less flat powder. On the other hand, the magnitude of the imaginary part of the complex permeability of the soft magnetic flat powder depends on the frequency band of the electromagnetic wave. In addition, the magnitude of the imaginary part of the complex permeability of the flat powder and the frequency characteristics of the imaginary part of the complex permeability change depending on the material of the soft magnetic powder. Therefore, if multiple types of soft magnetic flat powders have a constant magnitude of the imaginary part of the complex permeability in different frequency bands, and the frequency characteristics of the imaginary part of the complex permeability of each flat powder are complementary to each other in different frequency ranges, the flat surfaces of the multiple types of flat powders can be overlapped and the overlapping flat surfaces can be joined to absorb electromagnetic noise in a wide frequency band. Furthermore, a sheet made of a collection of flat powders in which the flat surfaces of soft magnetic flat powders are overlapped and the overlapping flat surfaces are joined with a material having a certain magnetic permeability becomes a sheet that shields magnetism. In other words, the higher the magnetic permeability of the flat powder in a direct current magnetic field and the lower the magnetic resistance, the easier it is for the magnetic lines to flow through the sheet, and a greater magnetic shielding effect can be obtained. On the other hand, since magnetic resistance is inversely proportional to magnetic permeability, a sheet made by overlapping flat surfaces of soft magnetic flat powders with a high relative magnetic permeability and joining the overlapping flat surfaces becomes a sheet with a high magnetic shielding effect. Furthermore, a sheet with a large area can be formed with a small amount of flat powder, and since the flat surfaces form the sheet surface, all the flat powder participates in the magnetic shielding, enhancing the effect of the magnetic shielding. Furthermore, by changing the thickness of the sheet according to the frequency band of the electromagnetic waves to be shielded, the skin effect can be utilized, and a lighter sheet can be obtained with less flat powder used. In this way, a collection of flat powders in which flat surfaces of soft magnetic flat powders are bonded together provides excellent effects as a sheet that absorbs electromagnetic noise and as a shielding film that shields magnetism. However, there have been no cases in which flat surfaces of soft magnetic flat powders are bonded together with a material in which at least one of the imaginary part of the complex permeability or the imaginary part of the complex permittivity has a constant value, or in which they are bonded with a material that has a constant magnetic permeability. As described in Patent Document 2, the conventional sheet is a sheet made of a composite material in which the organic solvent in the binder is evaporated and the flat powder is bonded to each other through the bonding of the solid polymer material. However, since the polymer material has different properties from the soft magnetic flat powder, the properties of the polymer material are reflected in the sheet. In this way, when the soft magnetic flat powder is bonded to each other through the bonding of solid dissimilar materials that occupy a certain volume, the properties of the dissimilar materials are reflected and the inherent properties of the soft magnetic flat powder are sacrificed. In addition, the flat surface does not form the sheet surface. On the other hand, if a sheet can be formed from a collection of flat powders in which the flat surfaces of soft magnetic flat powders are joined together, the amount of flat powder used to form the sheet can be reduced, and the characteristics of the soft magnetic flat powder and the flat surfaces can be reflected in the sheet. Furthermore, if the flat surfaces form the sheet surface, all the flat powder can participate in absorbing electromagnetic waves, or all the flat powder can participate in magnetic shielding, resulting in a sheet that best reflects the magnetic characteristics of the soft magnetic flat powder. This makes it an ideal sheet that can maximize the performance of the soft magnetic flat powder.

[0017] Next, a description will be given of problems that arise when forming a sheet made of an assembly of metal flake powder in which flat surfaces of the flake powder are joined together. The four problems in forming the conductive film described in paragraph 10 can be fundamentally solved if no conductive filler is used when forming the sheet. Therefore, if the flat surfaces of the metal flake powder can be bonded together with a substance that has metallic properties, the four problems can be fundamentally solved. Furthermore, when joining the flat surfaces of a flat powder made of an insulating metal oxide, it is sufficient that the flat surfaces can be joined together with an insulating material in a manner that does not apply excessive stress to the flat surfaces and does not reduce the insulating properties of the flat powder. Furthermore, if the flat surfaces of the inorganic luster pigment flake powder can be joined together with a transparent substance without damaging the coating of metal oxides such as titanium oxide and iron oxide, a sheet consisting of a collection of inorganic luster pigment flake powder can be created without losing the color reflected from the luster pigment. Therefore, the objective of forming a sheet in which flat surfaces of soft magnetic flake powder are joined together is to overlap the flat surfaces of the flat powder and join the overlapping flat surfaces with a material having at least one of a constant value of the imaginary part of the complex permeability or the imaginary part of the complex permittivity, or with a material having a constant relative permeability. The objective of forming a sheet in which flat surfaces of metal flake powder are joined together is to overlap the flat surfaces of the flat powder and join the overlapping flat surfaces with a material having metallic properties. Furthermore, the insulating flat powder may be joined together with an insulating material in a manner that does not apply excessive stress to the flat surfaces. Furthermore, the inorganic luster pigment flat powder may be joined together with a transparent material without damaging the metal oxide coating. On the other hand, even if the flatness of the flat powder is poor or the flat planes are uneven, if the material that bonds the flat planes is composed of a collection of nano-sized materials, the flat planes are bonded to each other through the collection of nano-sized materials on the entire surface of the overlapping flat planes regardless of the state of the flat planes, and the bonding force between the flat powders is increased. Furthermore, if the thickness of the collection of nano-sized materials that bonds the flat planes of the flat powders is thinner than the thickness of the flat powder, the area of ​​the flat powder is more than two orders of magnitude larger than the size of the nano-sized material, so that the properties of the sheet made of the collection of flat powder are dominated by the properties of the flat powder. Furthermore, when the flat planes are bonded to each other through the collection of nano-sized materials, the contact area where the nano-sized material comes into contact with the flat planes is extremely small. Therefore, when the nano-sized material comes into contact with the flat planes, excessive load is not applied to the flat planes. In addition, the coating provided on the flat planes is not damaged. As a result, even if the flat powder is prone to brittle fracture, the flat planes are not damaged. In addition, there is no need for a process such as stress relief annealing to eliminate distortion caused by stress. Furthermore, the brilliance of the inorganic luminous pigment is not lost. Therefore, it is necessary to overlap the flat surfaces of the flat powder through the raw material of nano-sized substances. On the other hand, it is possible to separate flat powder with flat surfaces directly overlapping each other into individual flat powders in a liquid. Furthermore, it is easy to overlap the flat surfaces of the flat powder through a liquid. This is because liquids have energy that allows molecules to move freely, and the shape of the liquid can change freely. For this reason, it is possible to generate a shock wave in the liquid, apply the shock wave through the liquid to the flat powder directly overlapping each other, and separate them into individual flat powders in the liquid. In addition, if a moving load is applied to the liquid, flat powder with a large aspect ratio will move in the liquid with the flat surface side up, and the flat surfaces of the flat powder separated into individual flat powders can be overlapped through the liquid. Furthermore, if the liquid is low viscosity and low density, shock waves can easily be transmitted through the liquid, and the flat surfaces can easily move within the liquid, making it easy to overlap the flat surfaces of flat powder that have been separated into individual pieces of flat powder with a low viscosity and low density liquid in between.For this reason, the nano-sized material that bonds the flat surfaces must first be liquefied as a low-viscosity, low-density liquid, secondly separated into individual flat powders in the low-viscosity, low-density liquid, thirdly stacked together the flat surfaces of the flat powder in the low-viscosity, low-density liquid, and the liquefied nano-sized material must be interposed between the flat surfaces of the flat powder. Fourthly, a nano-sized material is produced from the liquefied nano-sized material, fifthly, a collection of nano-sized materials is interposed between the flat surfaces of the flat powder, and sixthly, if the flat surfaces can be bonded together by the collection of nano-sized materials, a sheet made of a collection of flat powder is produced. To achieve this, the following six processes are required. The goal is to find a way to easily implement the six processes. First, the raw material of the nano-sized material that bonds the flat surfaces of the flat powder is liquefied into a low-viscosity, low-density liquid. Second, the flat powder is separated into individual flat powder sheets using a low-viscosity, low-density liquid, and each sheet of flat powder is covered with a low-viscosity, low-density liquid. Third, the flat powder sheets are overlapped with each other through a low-viscosity, low-density liquid. Fourth, the low-viscosity, low-density liquid that exists in the gaps between the flat powder sheets is converted into a nano-sized material that bonds the flat surfaces. Fifth, the nano-sized material is converted into a material that bonds the flat surfaces. Sixth, the flat surfaces are bonded with a nano-sized material to produce a sheet consisting of a collection of flat powder. [Means for solving the problem]

[0018] In the present invention Excluding tin and zinc A method for producing a sheet made of an assembly of flat powder in which flat surfaces of the flat powder made of any one of a metal, an alloy, a metal oxide, and an inorganic compound are bonded to each other via an assembly of nanoparticles of a metal or a metal oxide is provided, Organometallic compounds that precipitate metals or metal oxides upon thermal decomposition In molecular state The organometallic compound is dispersed in methanol, and the methanol dispersion of the organometallic compound is filled into a container. Thereafter, Excluding tin and zinc Metals, alloys, metal oxides, or inorganic compounds 1 typeA mass of flat powder made of the material is weighed out at a weight less than the weight of the methanol multiplied by the ratio of the density of the flat powder to the density of the methanol used, the weighed mass of flat powder is put into the container, and the mass of flat powder is stirred in the methanol dispersion of the organometallic compound; a homogenizer device is placed in the container, and the homogenizer device is operated in the container to repeatedly apply shock waves to the mass of flat powder through the methanol dispersion of the organometallic compound; The collection of flat powders, The mixture is separated into individual flat powders through the methanol dispersion of the organometallic compound, and the separated flat powders are covered with the methanol dispersion of the organometallic compound. After this, the homogenizer device is removed from the container. Furthermore, the container is covered in three directions, i.e., front-back, left-right, and up-down. impact Acceleration is applied repeatedly, and finally impact Acceleration is applied to allow the methanol dispersion of the organometallic compound to penetrate into the gaps between the flat surfaces of the flat powder, and the flat powder is formed into a collection of flat powder in which the flat surfaces of the flat powder overlap each other through the methanol dispersion of the organometallic compound, forming a shape of the bottom surface of the container. Thereafter, the temperature of the container is raised to the boiling point of methanol, and methanol is evaporated from the methanol dispersion of the organometallic compound. Consists of a size smaller than 100 nm A collection of microcrystals is precipitated in the gaps between the flat surfaces of the flat powder and on the surface of the collection of flat powder. A plate material that covers the entire surface of the collection of flat powder is placed over the entire surface of the collection of flat powder, and the entire surface of the plate material is uniformly compressed to precipitate the microcrystals of the organometallic compound. The size is about 20 nm, which is about 1 / 5 of the size of the original. crushing into fine crystals, Furthermore, a compressive load is evenly applied to the entire surface of the plate material, and the container is heated to the thermal decomposition temperature of the organometallic compound to thermally decompose the fine crystals of the organometallic compound. This causes metal or metal oxide to form in the gaps between the flat surfaces of the flat powder and on the surfaces of the collection of flat powder. Consists of a size of about 10 nmThe nanoparticle clusters overlap and precipitate simultaneously, and the nanoparticle clusters are compressed, and the nanoparticle clusters are bonded to the flat surfaces of the flat powder by frictional heat, and the nanoparticles are bonded to each other by frictional heat. As a result, a sheet made of the flat powder clusters, in which the flat surfaces of the flat powder clusters are bonded to each other via the nanoparticle clusters bonded by frictional heat, is placed in the container. The shape of the bottom of the container is After that, the container is impact Acceleration is applied to peel off the sheet made of the collection of flat powder from the bottom surface of the container, and the sheet is removed from the container. Excluding tin and zinc Metals, alloys, metal oxides, or inorganic compounds 1 type A method for producing a sheet consisting of a collection of flat powder in which the flat surfaces of the flat powder made of the above material are joined together via a collection of metal or metal oxide nanoparticles.

[0019] The method for producing a sheet made of a collection of flat powder of the present invention is a method of consecutively carrying out the following eight simple processes. This produces a sheet made of a collection of flat powder in which the flat surfaces of the flat powder are bonded together via a collection of nanoparticles bonded by frictional heat. The first process is a process of dispersing an organometallic compound, which is thermally decomposed to precipitate a metal or a metal oxide, in methanol to prepare a methanol dispersion of the organometallic compound, and filling a container with the methanol dispersion of the organometallic compound. Excluding tin and zinc A collection of flat powders made of any one of metals, alloys, metal oxides, and inorganic compounds is weighed out to a weight less than the weight of methanol multiplied by the ratio of the density of the flat powders used to the density of the methanol, and the weighed collection of flat powders is placed in a container and stirred in a methanol dispersion of an organometallic compound. The third process is a process in which a homogenizer device is placed in the container and operated within the container. The fourth process is a process in which a homogenizer device is placed in the container in three directions and a homogenizer device is operated within the container. impact Acceleration is applied repeatedly, and finally impactWhen these four processes are carried out in succession, a collection of flat powder particles, in which the flat surfaces of the flat powder particles overlap each other, is formed on the bottom surface of the container in the shape of the bottom surface through the methanol dispersion of the organometallic compound. The fifth process is to heat the container to the boiling point of methanol. The sixth process is to cover the entire surface of the flat powder in the container with a plate material, and evenly compress the entire surface of the plate material to crush the fine crystals of the organometallic compound into finer crystals. As a result, the finer crystals of the organometallic compound are piled up and accumulated at a high density in the gaps between the overlapping flat surfaces of the flat powder and on the entire surface of the flat powder. The seventh treatment is to apply a compressive load evenly to the surface of the plate, raise the temperature of the container to the thermal decomposition temperature of the organometallic compound, and thermally decompose the fine crystals of the organometallic compound. The eighth treatment is to apply pressure to the container in three directions, front-back, left-right, and up-down. impact This is a process in which acceleration is applied and the sheet made of the collection of flat powder is peeled off from the bottom surface of the container. As a result, a sheet made of the collection of flat powder is obtained in which the flat surfaces of the flat powder are bonded together via a collection of metal or metal oxide nanoparticles bonded by frictional heat. All eight of the processes are simple. In addition, the organometallic compounds are general-purpose industrial chemicals. This allows for inexpensive production of sheets made of a collection of flat powder in which the flat surfaces of the powder are bonded together via a collection of metal or metal oxide nanoparticles. The highest thermal decomposition temperature of organometallic compounds is 330°C in air. On the other hand, among soft metals, tin has an extremely low melting point of 232°C, and exhibits low-temperature brittleness at around -40°C. Similarly, zinc also exhibits low-temperature brittleness. On the other hand, the melting point of any flat powder of metals, alloys, metal oxides, or inorganic compounds other than tin and zinc is higher than 330°C, and does not exhibit low-temperature brittleness, making it possible to use it at extremely low temperatures. Therefore, a sheet made of a collection of flat powders in which the flat surfaces of the flat powders are joined together can be used in harsh environments such as high temperatures, extremely low temperatures, vacuum, and high pressure. For this reason, flat powders made of metals, alloys, metal oxides, or inorganic compounds other than tin and zinc can be used as raw materials for manufacturing sheets made of a collection of flat powders. Here, the phenomena occurring in each process and the effects of each process will be described. In the first treatment, when an organometallic compound that precipitates a metal or metal oxide by thermal decomposition is dispersed in methanol, the organometallic compound becomes a molecular state and disperses in methanol. In contrast, when an organometallic compound dissolves in methanol, the metal that constitutes the organometallic compound becomes a metal ion and dissolves in methanol, and the dissolved organometallic compound cannot be returned to the organometallic compound before dissolution. For this reason, when methanol is evaporated from a methanol solution of an organometallic compound, the organometallic compound before dissolution does not precipitate. Therefore, an organometallic compound that does not dissolve in methanol and disperses in methanol is used as the organometallic compound that precipitates a metal or metal oxide by thermal decomposition. In the second process, Excluding tin and zinc A collection of flat powders made of any one of a metal, alloy, metal oxide, and inorganic compound is weighed out to a weight less than the weight of methanol multiplied by the ratio of the density of the flat powder used to the density of the methanol, and the weighed collection of flat powders is placed in a container. Excluding tin and zinc Among flat powders made of metals, alloys, metal oxides, or inorganic compounds, permalloy has the highest density. The density of permalloy with a nickel content of 45% is 8.25 g / cm 3 On the other hand, the density of methanol is 0.792 g / cm 3Therefore, the density of permalloy is 10 times higher than that of methanol. Also, organometallic compounds can be dispersed in methanol to a concentration of about 10% by weight, but the density of organometallic compounds is 1 g / cm 3 The density of the organometallic compound in methanol is close to that of methanol. The viscosity of the organometallic compound in methanol, where the organometallic compound is dispersed in methanol to about 10% by weight, is close to that of methanol. The viscosity of methanol is extremely low at 0.59 mPa·sec. Therefore, when using flat powder of permalloy, the weight of the collection of flat powder of permalloy is less than 1 / 10 of the weight of the organometallic compound in methanol. On the other hand, the density of permalloy is 10 times the density of methanol. Therefore, the volume ratio of the organometallic compound in methanol dispersion is larger than the volume ratio of the volume theoretically calculated from the weight of the collection of flat powder of permalloy. Therefore, when the collection of flat powder of permalloy is stirred in the organometallic compound in methanol dispersion with a large volume ratio, the flat powder of permalloy is well dispersed in the low density and low viscosity organometallic compound in methanol dispersion, and is evenly mixed in the methanol dispersion. On the other hand, Excluding tin and zinc Among flat powders made of metals, alloys, metal oxides, or inorganic compounds, the lowest density flat powder has a density of 2.7 g / cm 3The aluminum flake powder is composed of aluminum flakes. Therefore, when using aluminum flake powder, the weight of the aluminum flake powder cluster is less than 1 / 3 of the weight of the organometallic compound methanol dispersion. On the other hand, the density of aluminum is 3.4 times the density of methanol. Therefore, the volume ratio of the organometallic compound methanol dispersion becomes larger than the volume ratio consisting of the volume theoretically calculated from the weight of the aluminum flake powder cluster. Therefore, when the aluminum flake powder cluster is stirred in the organometallic compound methanol dispersion with a large volume ratio, the aluminum flake powder disperses well in the low-density and low-viscosity organometallic compound methanol dispersion and is evenly mixed in the methanol dispersion. In this way, the collection of flat powder is weighed out at a weight less than the weight of methanol multiplied by the ratio of the density of the flat powder used to the density of the methanol, and the weighed collection of flat powder is put into a methanol dispersion of an organometallic compound.When the collection of flat powder is stirred in the methanol dispersion of an organometallic compound, since the volume ratio of the methanol dispersion of an organometallic compound is large, all of the flat powder disperses well in the low-viscosity, low-density methanol dispersion of an organometallic compound regardless of the difference in density of the flat powder, and is evenly mixed in the methanol dispersion, so that all of the flat powder is covered with the methanol dispersion of an organometallic compound. In the third process, a homogenizer is placed in the container and operated in the container. At this time, since the methanol dispersion of the organometallic compound is a liquid with low viscosity and low density, the shock waves generated by the homogenizer are consumed at a low rate when exciting the methanol dispersion, and the shock waves are efficiently and repeatedly applied to the collection of flat powder through the methanol dispersion. As a result, shock waves are repeatedly applied to all the flat powder through the methanol dispersion of the organometallic compound. On the other hand, even in the flat powder with a relatively high density, an extremely thick flat powder, and the largest flat powder size, i.e., a density of 7.8 g / cm 3 The weight of a single flat piece of reduced iron powder with a particle size of 100 μm and a thickness of 15 μm is only 1×10 -6g. Therefore, even if the flat powder has flat surfaces overlapping each other in a complex manner, the shock waves are repeatedly applied to the extremely lightweight flat powder, and the flat powder with overlapping flat surfaces is separated into individual flat powder pieces, and the separated flat powder pieces are covered with the methanol dispersion of the organometallic compound. That is, flat powder has flat surfaces with a large aspect ratio, which is the ratio of the average value of the major axis and minor axis to the thickness. Furthermore, even if the flat powder is the same type, there is variation in the size and thickness of the flat surfaces. When such a collection of flat powder is handled in an air atmosphere, the flat surfaces overlap each other in a complex manner. On the other hand, when a sheet made of a collection of flat powder is formed using flat powder with flat surfaces directly overlapping each other, the flat powder with flat surfaces directly overlapping each other forms a part of the sheet with weak mechanical strength. In addition, if all the overlapping flat powders can be separated into individual flat powder sheets, the amount of flat powder used to form the sheet can be reduced. Therefore, a process is required to reliably separate flat powder with overlapping flat surfaces. On the other hand, when trying to separate flat powder with overlapping flat surfaces in an air atmosphere, frictional forces are generated on the overlapping flat surfaces, making separation difficult. In addition, it is difficult to identify whether the flat surfaces overlap each other. In contrast, the methanol dispersion of the organometallic compound is a low-viscosity, low-density liquid, and furthermore, as described above, the volume ratio of the methanol dispersion of the organometallic compound is greater than the volume ratio of the theoretically calculated volume from the weight of the collection of flat powder. Therefore, when the collection of flat powder is stirred in the methanol dispersion of the organometallic compound, the flat powder is well dispersed in the methanol dispersion of the organometallic compound regardless of the density, thickness, and size of the flat powder, and is evenly mixed in the methanol dispersion. When shock waves are repeatedly generated in this mixture by a homogenizer device, the shock waves spread throughout the entire methanol dispersion of the organometallic compound, the energy of the shock waves is consumed in the methanol dispersion at a low rate, the shock waves are efficiently and repeatedly applied to the flat powder, and the shock waves are also repeatedly applied to the parts where the flat planes of the flat powder overlap, and since the flat powder is extremely light, the overlapping flat planes are easily separated from each other. As a result, the flat powder with overlapping flat planes is reliably separated into individual flat powder sheets. When an ultrasonic homogenizer is used as the homogenizer, the generation and disappearance of a huge number of bubbles, each of which is two orders of magnitude smaller than the flat surfaces of the flat powder, is repeated in the methanol dispersion of the organometallic compound (this phenomenon is called cavitation), and shock waves generated when the bubbles burst are continuously generated throughout the methanol dispersion of the organometallic compound, causing the flat powder with overlapping flat surfaces to separate into individual pieces of flat powder in a short period of time. As a result, all of the flat powder is covered with the methanol dispersion of the organometallic compound. The homogenizer is then removed from the container. In the fourth process, the container is impact Acceleration is applied repeatedly, and finally impact Acceleration is applied. In other words, by processing with a homogenizer device, all the flat powder is covered with a methanol dispersion of a low-viscosity, low-density organometallic compound, and dispersed in the methanol dispersion. This mixture is subjected to three directions of acceleration. impact When acceleration is applied, a methanol dispersion of a low-viscosity, low-density organometallic compound disperses into flat powder. impact The powder is repeatedly moved in the direction of acceleration. Since the flat powder has a flat surface with a large aspect ratio, the flat surface is placed on top together with a methanol dispersion of an organometallic compound. impactThe particles move repeatedly in the direction of acceleration. The flat powder particles also rearrange and overlap with the flat surface facing up in the methanol dispersion of the organometallic compound. As a result, the collection of flat powder particles, with their flat surfaces overlapping each other through the methanol dispersion of the organometallic compound, spreads over the entire bottom surface of the container. Finally, the particles move in the vertical direction. impact Acceleration is applied, and the vibration of the container is stopped. As a result, the collection of flat powder, whose flat surfaces overlap each other via the methanol dispersion of the organometallic compound, spreads over the entire bottom surface of the container and forms the shape of the bottom surface of the container. In the fifth treatment, the container is heated to the boiling point of methanol. Consists of size Clusters of fine crystals of the organometallic compound are deposited in the gaps between the overlapping flat surfaces of the flat powder and on the entire surface of the cluster of flat powder. In other words, in the methanol dispersion of the organometallic compound, the organometallic compound is dispersed in the methanol in a molecular state, so when the methanol is evaporated, the organometallic compound before dispersion is dispersed into small particles smaller than 100 nm. Consists of size It precipitates as a collection of fine crystals. On the other hand, since the dispersion concentration of the organometallic compound in the methanol dispersion of the organometallic compound is low and the volume ratio of the organometallic compound in the methanol dispersion is greater than the volume ratio of the volume theoretically calculated from the weight of the collection of flat powder, when the excess methanol evaporates, the thickness of the collection of fine crystals precipitated between the flat surfaces and on the surface of the collection of flat powder is thin, with a thickness of submicron. On the other hand, since the organometallic compound dispersed in a molecular state precipitates as fine crystals, the fine crystals are a collection of crystals in which crystals forming single molecules of the organometallic compound are accumulated. For this reason, when stress is applied to the fine crystals, the fine crystals are easily crushed. However, the finer the fine crystals are, the more difficult it is to apply stress to them, and there is a limit to how fine the fine crystals can be. In addition, the evaporated methanol is recovered by a recovery machine and reused. In the sixth process, a plate material covering the entire surface of the flat powder collection in the container is placed over the entire surface of the flat powder collection, and the entire surface of the plate material is compressed evenly. At this time, the gaps where the flat surfaces of the flat powder overlap and the collection of fine crystals that have precipitated overlapping on the entire surface of the flat powder collection are crushed into finer crystals. Since the relatively larger the size of the fine crystals, the easier they are to crush, the relatively larger fine crystals are crushed first, and the crushing of the fine crystals progresses while the compression load is applied. On the other hand, when the fine crystals are crushed, new voids are formed in the collection of fine crystals, and the collection of crushed and finer crystals moves into the voids and fills the voids. As the crushing of the fine crystals progresses, the crushed and finer crystals overlap at a high density in the gaps where the flat surfaces of the flat powder overlap and on the entire surface of the collection of flat powder, and the collection of finer crystals accumulates at a high density, forming a very thin layer of crystals. When the crystals reach their limit of crushing size, the crushing of the fine crystals does not progress even when a compressive load is applied to the plate material, and the plate material to which the compressive load is applied no longer moves, and the repulsive force from the plate material increases. At this point, the process of compressing the plate material surface is stopped. As a result, the size of the fine crystals is reduced to approximately 20 nm, which is nearly 1 / 5 of the size at the time of precipitation, and the thickness of the fine crystals of approximately 20 nm that are piled up at a high precipitation density in the gaps between the flat surfaces and on the surfaces of the flat powder clusters is 120-1 6 The thickness of the plate is about 20 nm. The compressive load applied to the plate is equivalent to 10-100 kg, depending on the size of the container and the amount of microcrystals. The impact acceleration applied to the container is 0.2-1.0 G, depending on the size of the container and the amount of microcrystals. As a result, clusters of organometallic compound crystals with a size of about 20 nm are densely stacked in the gaps between the overlapping flat surfaces of the flat powder, and on the entire surface of the cluster of flat powder. In the seventh treatment, a compressive load is evenly applied to the entire surface of the plate material, the container is heated to the thermal decomposition temperature of the organometallic compound, and the fine crystals of the organometallic compound are thermally decomposed. First, the moisture adsorbed on the flat powder and the foreign matter consisting of compounds having hydroxyl groups are vaporized. Next, the thermal decomposition of the fine crystals of the organometallic compound begins, the organometallic compound is thermally decomposed into organic molecules and metal molecules or metal oxide molecules, and when the vaporization of the organic molecules is completed, the metal or metal oxide molecules gather together to form granular nanoparticles made of metal or metal oxide having a size of about 10 nm, and 6-8 of the granular nanoparticles overlap and precipitate simultaneously, and the collection of the nanoparticles forms a thickness of 60-80 nm. The metal or metal oxide nanoparticles do not contain any impurities and are precipitated as genuine metal or metal oxide nanoparticles. In addition, since the metal nanoparticles are precipitated as nanoparticles of active metal, adjacent metal nanoparticles are metallically bonded at the contact area. After this, the metal nanoparticles that have been metallically bonded are rejoined by frictional heat. Meanwhile, as the thermal decomposition of the fine crystals progresses, the foreign matter consisting of organic matter adsorbed to the flat powder vaporizes. This cleans the flat surface of the flat powder, and a collection of nanoparticles of genuine metal or genuine metal oxide precipitates on the cleaned flat surface, increasing the bonding strength of the nanoparticles of metal or metal oxide bonded to the flat surface by frictional heat. In addition, the bonding strength between the nanoparticles of genuine metal or metal oxide due to frictional heat is also increased. In addition, since the granular nanoparticles of metal or metal oxide are small, around 10 nm, and the contact area of ​​the granular nanoparticles with the flat surface is extremely small, when the granular nanoparticles of metal or metal oxide are bonded to the flat surface by frictional heat, the flat surface does not undergo plastic deformation, and no stress distortion occurs on the flat surface. For this reason, there is no need to anneal the sheet consisting of a collection of flat powder to remove distortion. In the eighth process, the container is impactAcceleration is applied and the sheet made of the flat powder is peeled off from the bottom of the container. As a result, a sheet made of the flat powder is obtained. The layer of nanoparticles formed on the surface of the flat powder and in the gaps between the flat particles is a very thin bonding layer with a thickness of 60-80 nm, which corresponds to a collection of 6-8 nanoparticles, and the size of the nanoparticles, which are about 10 nm in size, is more than two orders of magnitude smaller than the flat surface of the flat powder. For this reason, the properties of the flat powder dominate in the sheet made of the flat powder. Here, the method of producing a sheet made of a collection of flat powder in the present invention provides the following effects. First, the substance that bonds the flat surfaces of the flat powder is a nanoparticle of metal or metal oxide, and further, the raw material of the nanoparticles of metal or metal oxide is liquefied as a methanol dispersion in which an organometallic compound is dispersed in methanol. Since this liquid has low viscosity and density, by continuously carrying out the second and third processes, it is possible to interpose the methanol dispersion of the organometallic compound in the gaps between the flat surfaces of the separated flat powder. This solves the first problem described in paragraph 16. Secondly, the homogenizer device is operated in the container, and the shock waves generated by the homogenizer device are consumed in a small proportion when exciting the methanol dispersion of the organometallic compound because the methanol dispersion of the organometallic compound has a low viscosity and density, and most of the impact energy is efficiently and repeatedly transmitted to the collection of flat powder. Since the flat powder is extremely light, even flat powder that is overlapped in a complex manner is reliably separated into individual flat powder pieces, and the methanol dispersion of the organometallic compound comes into contact with the surface of all the flat powder pieces regardless of the material, shape, and particle size distribution of the flat powder. This solves the second problem described in paragraph 16. In addition, the surfaces of the flat powders are all hydrophobic and do not react with the methanol dispersion of the organometallic compound, and the methanol dispersion of the organometallic compound comes into contact with the surface of the flat powder. Thirdly, the container has three directions: left and right, front and back, and top and bottom. Impact force Repeatedly add, and finally add Impact forceAt this time, since the methanol dispersion of the organometallic compound has low viscosity and low density, the methanol dispersion of the organometallic compound is mixed with the flat powder. impact The powder repeatedly moves in three directions of acceleration, and the flat surfaces repeatedly overlap and rearrange in the methanol dispersion of the organometallic compound. As a result, the flat powder spreads over the entire bottom surface of the container, and a collection of flat powder with flat surfaces overlapping each other through the methanol dispersion of the organometallic compound is formed on the bottom surface of the container in the shape of the bottom surface. This solves the third problem described in paragraph 16. Fourth, the flat powder separated into individual pieces is stacked together with the flat surfaces interposed in a methanol dispersion of an organometallic compound, so the larger the aspect ratio of the flat powder, the less flat powder is used. Therefore, even if the flat powder is expensive, a sheet made of a collection of flat powders stacked together with the flat surfaces overlapping each other can be produced inexpensively. Fifth, methanol is evaporated from the collection of flat powders whose flat surfaces overlap each other through a methanol dispersion of an organometallic compound, and a collection of fine crystals of the organometallic compound is precipitated in the gaps between the flat surfaces and on the surface of the collection of flat powders. Furthermore, the entire surface of the collection of flat powders is evenly compressed. As a result, the fine crystals are crushed to about 1 / 5 of their original size, and the crushed crystals are piled up in the gaps between the flat surfaces and on the surface of the collection of flat powders, with a high precipitation density. These crushed fine crystals having a size of about 20 nm become the raw material for the collection of nanoparticles of metal or metal oxide that join the flat surfaces of the flat powders. This solves the fourth problem described in paragraph 16. Sixth, the entire surface of the flat powder is heated while being compressed evenly, and the crushed microcrystals are thermally decomposed. At this time, a collection of metal or metal oxide nanoparticles is precipitated simultaneously at high density in the gaps between the flat surfaces and on the surface of the flat powder. Furthermore, the entire surface of the flat powder is compressed evenly, and the collection of metal or metal oxide nanoparticles precipitated at high density are bonded to the flat surfaces by frictional heat, and the nanoparticles are bonded to each other by frictional heat. In other words, since the collection of metal or metal oxide nanoparticles is precipitated overlapping each other at high density, it becomes difficult for the compressed nanoparticles to move in the nanoparticle collection, and frictional heat is instantly generated at the contact points of the nanoparticles in contact with the flat surfaces and at the contact points between the nanoparticles, and the nanoparticles are bonded to the flat surfaces by the bonding force due to the frictional heat, and the nanoparticles are bonded to each other by the bonding force due to the frictional heat. This solves the fifth and sixth problems described in paragraph 16, and all of the problems described in paragraph 16 are solved. Seventh, flat powders made of metals, alloys, metal oxides, or inorganic compounds other than tin and zinc can be used as flat powders when manufacturing a sheet made of a collection of flat powders. In other words, the thermal decomposition temperature of organometallic compounds, which has the highest thermal decomposition temperature, is 330°C in the air. On the other hand, among soft metals, the melting point of tin is as low as 232°C, and it becomes brittle at low temperatures at around -40°C. Zinc also becomes brittle at low temperatures. In contrast, the melting point of flat powders made of metals, alloys, metal oxides, or inorganic compounds other than tin and zinc is higher than 330°C, and they do not have low-temperature brittleness, making them usable at extremely low temperatures. Therefore, a sheet made of a collection of flat powders in which the flat surfaces of the flat powders are joined together can be used in harsh environments such as high temperatures, extremely low temperatures, vacuum, and high pressure. Eighth, the organometallic compound precipitates metals or metal oxides of various materials by thermal decomposition, so that the material of the nanoparticles that connect the flat surfaces of the flat powders can be the most suitable metal or metal oxide nanoparticle material for exhibiting the properties of the sheet made of the flat powders. Ninth, the sheet made of a collection of flat powder can be produced at low cost using inexpensive materials. In other words, the organometallic compound and the flat powder are general-purpose industrial materials, and the amounts of the organometallic compound and the flat powder used are small. In addition, all of the eight processes for producing the sheet are extremely simple. For this reason, the production cost of the sheet is low. As described above, the sheet produced by this manufacturing method is made up of a collection of flat powder, with the flat surfaces of the separated flat powder joined together via a collection of metal or metal oxide nanoparticles, resulting in a sheet made of a collection of flat powder that has revolutionary effects not found in conventional collections of flat powder.

[0020] The method for producing a sheet made of a collection of flat powder described in paragraph 18 is a method for producing a sheet made of a collection of soft magnetic flat powder, and the method for producing a sheet made of a collection of soft magnetic flat powder includes: The flat powder described in paragraph 18 is either iron, permalloy, silicon steel, sendust, or magnetic stainless steel. 1 type The organometallic compound described in paragraph 18 is nickel octylate which precipitates nickel by thermal decomposition, and any of the above 1 type A method for producing a sheet consisting of a collection of soft magnetic flat powder, comprising using a soft magnetic flat powder made of the material described above as the flat powder described in paragraph 18, using the nickel octylate as the organometallic compound described in paragraph 18, and producing a sheet consisting of a collection of flat powder in which the flat surfaces of the soft magnetic flat powder are joined together via collections of nickel nanoparticles, according to the method for producing a sheet consisting of a collection of flat powder described in paragraph 18.

[0021] First, the properties of soft magnetic flat powders of iron, permalloy, silicon steel, sendust, or magnetic stainless steel will be described. The soft magnetic flat powder made of iron and permalloy has a large initial relative permeability and a large maximum relative permeability, and a sheet made of a collection of flat powders in which the flat surfaces of the soft magnetic flat powder are bonded together with a collection of nanoparticles is effective as a sheet for shielding magnetism.In addition, the soft magnetic flat powder made of iron, permalloy, silicon steel, sendust, or electromagnetic stainless steel has a constant value of the imaginary part of the complex permeability in a specific frequency band, so that a sheet made of a collection of flat powders in which the flat surfaces of these soft magnetic flat powders are bonded together with a collection of nanoparticles is effective as a sheet for absorbing electromagnetic noise or preventing interference of electromagnetic noise in a specific frequency band. Here, we will explain about iron flake powder. Electromagnetic soft iron, which has magnetic properties similar to those of pure iron, has an initial relative permeability of 150 in a DC magnetic field and a maximum relative permeability of 1×10 4The relative permeability in an AC magnetic field of 100 kHz is 100. The saturation magnetic flux density of electromagnetic soft iron is 2.2 Tesla, the largest among soft magnetic materials. Therefore, a sheet of flat iron powder overlapping flat surfaces effectively acts as a shielding film to shield magnetism. It is particularly effective as a magnetic shield for devices that generate strong magnetic fields, such as MRI (Magnetic Resonance Imaging) and power transformers. On the other hand, iron has a Vickers hardness of 110 Hv and is a relatively hard metal. There are reduced iron powder and atomized iron powder, and reduced iron powder has many voids and is easier to flatten than atomized iron powder, but the thickness of the flat powder is thicker due to its high hardness. Therefore, the flat powder of reduced iron powder has a larger flatness ratio than atomized iron powder, and the imaginary part of the complex permeability has a certain magnitude in the frequency band of 100 kHz to 10 MHz. Therefore, a sheet made of reduced iron powder acts as a sheet for absorbing electromagnetic noise in the frequency band of 100 kHz to 10 MHz or for preventing interference with electromagnetic noise. The skin depth of the electromagnetic waves of reduced iron powder at 100 kHz is 50 μm. Therefore, the flat powder made of reduced iron powder exhibits excellent performance as a magnetic shield for devices that generate strong magnetic fields. It is also effective in a limited frequency band as a sheet for absorbing electromagnetic noise or for preventing interference with electromagnetic noise. For this reason, when the flat powder of reduced iron powder is used as the flat powder made of metal described in paragraph 17 and a sheet made of a collection of flat powders in which the flat surfaces of the reduced iron powder are joined together is formed according to the method described in paragraph 17, it can be used as a sheet for shielding magnetism and as a sheet for absorbing electromagnetic noise or for preventing interference with electromagnetic noise. In contrast, permalloy is a soft magnetic material made of an alloy with high magnetic permeability. The higher the magnetic permeability of the flat powder and the lower the magnetic resistance, the greater the magnetic shielding effect. Since magnetic resistance is inversely proportional to the permeability, a sheet made of permalloy flat powder with high magnetic permeability has a high magnetic shielding effect. For example, permalloy, which is 45% nickel, has an initial relative permeability of 2.5 x 10 in a DC magnetic field. 3 The maximum relative permeability is 2.5×10 4However, its saturation magnetic flux density is 0.9 Tesla, which is smaller than that of soft magnetic iron. On the other hand, permalloy, which is made of 79% nickel and 4% molybdenum, has an initial relative permeability of 2×10 4 , the maximum relative permeability is 2×10 5 is extremely large. However, the higher the nickel content, the more expensive the permalloy becomes, so the nickel content is preferably 50% or less. Therefore, a sheet made by overlapping flat surfaces of permalloy powder is an excellent sheet for shielding magnetism. For this reason, in areas where the external magnetic field is relatively small, such as leakage magnetic fields from electrical equipment, AC magnetic fields from current transmission and distribution lines, urban magnetic noise, and environmental magnetic fields, a sheet made of permalloy flat powder is effective as a sheet for shielding magnetism. According to Non-Patent Document 1, permalloy flat powder containing 50% nickel has an aspect ratio of 38 and an average particle size of 14 μm. In addition, the imaginary part of the complex permeability rises sharply from around 100 MHz, has a peak value of 8.8 at 3.3 GHz, decreases from around 4 GHz, and has a value of 3.5 at 10 GHz. Therefore, the permalloy flat powder has a complex permeability with an imaginary part of 5 or more in the frequency band of 1-8 GHz, and a sheet formed by overlapping flat surfaces of the permalloy flat powder acts as a sheet for absorbing electromagnetic noise or preventing electromagnetic noise interference in this frequency band. In this way, a sheet formed by overlapping flat surfaces of the permalloy flat powder exhibits excellent performance as a magnetic shielding sheet in an area where the external magnetic field is relatively small. It is also effective in a limited frequency band as a sheet for absorbing electromagnetic noise or preventing electromagnetic noise interference. For this reason, when the permalloy flat powder is used as the flat powder made of the alloy described in paragraph 17 and a sheet made of a collection of flat powders in which the flat surfaces of the flat powders are joined together according to the method described in paragraph 17 is formed, it can be used as a magnetic shielding sheet and as a sheet for absorbing electromagnetic noise or preventing electromagnetic noise interference. On the other hand, soft magnetic alloy materials include silicon steel, which is made by adding a small amount of silicon to iron, permalloy, which is made by adding nickel to iron, sendust, which is made by adding silicon and aluminum to iron, permendur, which is made by adding cobalt to iron, and electromagnetic stainless steel, which is made by adding chromium and silicon to iron. Of these, silicon steel becomes brittle as the amount of silicon added increases, and the amount of silicon that can be flattened is less than 10%. A slight difference in the amount of silicon added can greatly change the permeability characteristics of silicon steel. Also, the more nickel added to permalloy, the higher the manufacturing cost, but if the amount of nickel added is small, the permeability decreases, so it is desirable to keep the amount of nickel added to about 50%. Also, sendust is hard and brittle, but if a small amount of nickel is added and the amount of silicon added is reduced, flattening becomes possible. Furthermore, permendur is an alloy with cobalt, so the manufacturing cost is high and it is not suitable as flat powder to be used in sheets that absorb electromagnetic noise or prevent electromagnetic noise interference. In addition, the flattening process of electromagnetic stainless steel becomes easier when aluminum is added. Therefore, the four types of alloys except for permendur can be used as soft magnetic flat powder. The thickness of the flat powder made of the four types of alloys is in the range of 1-1.5 μm. In contrast, the hardness of the reduced iron powder is higher than that of the four types of alloys, so the thickness of the flat powder made of reduced iron powder is as thick as 10-20 μm. On the other hand, as explained in paragraph 16, the larger the flatness of the flat powder, the larger the imaginary part of the complex permeability. Also, as shown in formula 1 described in paragraph 3, the absorption of electromagnetic noise depends on the magnitude of the imaginary part of the complex permeability of the flat powder and the magnitude of the electrical conductivity. Therefore, for sheets used to absorb electromagnetic noise or prevent interference from electromagnetic noise, flat powder of silicon steel with less than 10% silicon added, flat powder of permalloy with nickel added to nearly 50%, flat powder of sendust with a small amount of nickel added and a reduced amount of silicon added, and flat powder of electromagnetic stainless steel with aluminum added can be used. However, the complex permeability of flat powders made of these four types of alloys changes when the composition of the components other than iron changes slightly. Also, since the hardness of the four types of alloys is different, the flatness of the flat powder is different for each of the four types of alloys, and the magnitude of the imaginary part of the complex permeability is different for each of the four types of alloys. Furthermore, the frequency characteristics of the imaginary part of the complex permeability are significantly different for the four types of alloys, and even for the same type of alloy, the characteristics are different for the components other than iron. Therefore, when making a sheet made of a collection of alloy flat powders used for absorbing electromagnetic noise or preventing electromagnetic noise interference, the characteristics of the imaginary part of the complex permeability of the soft magnetic flat powder made of alloy can be utilized by using different soft magnetic flat powders made of alloys according to the frequency band of the electromagnetic waves to be absorbed. Therefore, when the soft magnetic flat powder made of alloy is used as the flat powder made of alloy described in paragraph 18, and a sheet made of a collection of flat powders in which the flat surfaces of the flat powders are joined together according to the method described in paragraph 18 is formed, it can be used as a sheet that absorbs electromagnetic noise or prevents electromagnetic noise interference. However, the hardness of soft magnetic flat powders varies, so the thickness of the flat powder varies depending on the material. For example, the thickness of flattened reduced iron powder, which has high hardness and is difficult to flatten, is as thick as 10-20 μm. In contrast, the thickness of flattened powder, which is made easier to flatten by adding a small amount of nickel to sendust, a ternary alloy consisting of iron, silicon, and aluminum, and reducing the amount of silicon added, is as thin as 1-1.5 μm. The weight of the flattened powder also varies greatly depending on the particle size and density of the flattened powder, as well as the thickness of the flattened powder. For example, the weight of flattened reduced iron powder with a particle size of 100 μm and a thickness of 15 μm is 0.927 × 10 -6In contrast, the weight of Sendust flakes with a particle size of 40 μm and a thickness of 1 μm is 0.86 × 10 -8 g, and is even lighter. The density of iron is 7.8 g / cm 3 The density of sendust is 7.6 g / cm 3 The densities of the two are close. Therefore, the reason why the weight of the reduced iron powder flakes is two orders of magnitude larger than that of the Sendust powder is due to the difference in the thickness and particle size of the flat powder. However, the weight of one piece of soft magnetic flat powder is extremely small, even for reduced iron powder flakes. The density of soft magnetic flat powder made of metal or alloy is 7.7-8.3g / cm 3 is within the range. On the other hand, in the method for manufacturing a sheet consisting of an assembly of flat powder in which the flat surfaces of the flat powder are bonded together via an assembly of nanoparticles as described in paragraph 18, the assembly of flat powder is weighed to a weight less than the weight obtained by multiplying the weight of methanol by the ratio of the density of the flat powder used to the density of the methanol, and the weighed assembly of flat powder is mixed with a methanol dispersion of a low-viscosity, low-density organic compound, and a homogenizer is operated in the mixture. When the homogenizer is operated in the mixture, since the methanol dispersion of the organometallic compound is a low-viscosity, low-density liquid, the shock waves generated by the homogenizer are efficiently and repeatedly applied to the assembly of soft magnetic flat powder through the methanol dispersion without exciting the methanol dispersion. Because each sheet of soft magnetic flat powder is extremely light, even if the weight, thickness, size, and density of the soft magnetic flat powder are different, the overlapping soft magnetic flat powder can be easily separated into individual flat powder sheets via the methanol dispersion of the organometallic compound, and the separated soft magnetic flat powder is covered with the methanol dispersion of the organometallic compound. After this, the container is impact Acceleration is applied repeatedly, and finally impact Acceleration was applied. Through the treatment using the homogenizer device, all of the soft magnetic flaky powder was covered with the low-viscosity, low-density methanol dispersion of the organometallic compound and dispersed in the methanol dispersion. impactWhen acceleration is applied, the methanol dispersion of the organometallic compound is low in viscosity and density, and each sheet of soft magnetic flat powder is extremely light, so even if the weight, thickness, size, and density of the soft magnetic flat powder are different, the methanol dispersion of the organometallic compound moves along with the soft magnetic flat powder. impact The soft magnetic powder moves in the direction of acceleration. Since the soft magnetic powder has a flat surface with a large aspect ratio, the flat surface is placed on top. impact The phenomenon in which the flat powder is repeatedly moved in the direction of acceleration, rearranged with the flat surface facing up, and overlaps with each other progresses in the methanol dispersion of the organometallic compound, and the flat surfaces overlap with each other through the methanol dispersion of the organometallic compound. As a result, even if the weight, thickness, size, and density of the soft magnetic flat powder are different, the collection of flat powder with the flat surfaces overlapping with each other through the methanol dispersion of the organometallic compound spreads over the entire bottom surface of the container. Therefore, there are no restrictions on the material, thickness, size, particle size distribution, and hardness of the soft magnetic flat powder used. Next, the material of the nano-sized substance that bonds the flat surfaces of the soft magnetic flat powder made of any of the above-mentioned iron, permalloy, silicon steel, sendust, or electromagnetic stainless steel will be described. As explained in paragraph 18, the thickness of the layer of the nano-sized substance that bonds the flat surfaces of the flat powder is thin, at 60-80 nm. In addition, nanoparticles with a size of about 10 nm are two orders of magnitude smaller than the area of ​​the flat surfaces of the soft magnetic flat powder. For this reason, the sheet in which the flat surfaces of the soft magnetic flat powder are bonded together by a collection of nanoparticles has the properties of the soft magnetic flat powder. However, if the material of the nanoparticles is a ferromagnetic material with soft magnetic properties, it does not hinder the soft magnetic properties of the sheet made of the collection of soft magnetic flat powder. Nickel is one such ferromagnetic material. Nickel has a maximum relative magnetic permeability of 600. In addition, its complex permeability at 2.45 GHz and 50°C is 1.592 in real part and 1.349 in imaginary part. Therefore, nickel is a ferromagnetic material among metals and metal oxides, with both the maximum relative magnetic permeability and complex permeability having a certain value. The maximum relative magnetic permeability is 1×10 that of iron. 4 On the other hand, nickel has an electrical resistance of 69.3×10 -9 100 x 10 of the electrical resistivity of iron in Ω m-9 Since nickel has a lower permeability than iron, it has a higher electromagnetic wave reflection loss and absorption loss than iron, making it effective for electromagnetic wave shielding. Furthermore, nickel has a certain complex permeability in the high frequency band, so it has a magnetic shielding effect and a certain effect of absorbing electromagnetic noise in the high frequency band. Nickel also has a Vickers hardness of 400-500HV, which is higher than 120-160HV of PB permalloy, which is the softest magnetic material with the lowest hardness. However, nickel nanoparticles are small, about 10nm, and the contact area formed when they come into contact with the flat surface of the permalloy powder is extremely small. Therefore, when a collection of nickel nanoparticles comes into contact with the flat surface of the permalloy, the very small contact area of ​​the permalloy flat surface is slightly elastically deformed, and no stress distortion occurs on the flat surface of the permalloy. At this time, the frictional heat generated in the very small contact area between the two bonds the nickel nanoparticles to the flat surface of the permalloy. Based on this idea, we decided to join the flat surfaces of the soft magnetic flat powder with a collection of nickel nanoparticles. Here, we will explain a method for producing a sheet made of a collection of soft magnetic flat powder in which the flat surfaces of the powder are joined together via a collection of nickel nanoparticles, following the eight steps described in paragraph 18. In the first process, nickel octylate is dispersed in methanol up to a maximum of 10% by weight to prepare a methanol dispersion of nickel octylate, and the methanol dispersion is filled into a container. In the second process, a collection of soft magnetic flat powder made of any one of iron, permalloy, silicon steel, sendust, and electromagnetic stainless steel is weighed out to a weight less than the weight of methanol multiplied by the ratio of the density of the flat powder used to the density of the methanol, the collection of flat powder is poured into a container, and the soft magnetic flat powder is stirred. In the third process, a homogenizer device is placed in the container, and the homogenizer device is operated within the container. In the fourth process, a homogenizer device is placed in the container in three directions, and the container is filled with a 3-axis homogenizer. impact Acceleration is applied repeatedly, and finally impact By carrying out these four processes in succession, a collection of flat powder particles, with the flat surfaces of the flat powder overlapping each other, is formed on the bottom surface of the container in the shape of the bottom surface through the methanol dispersion of nickel octylate. In the fifth process, the container is heated to the boiling point of methanol. In the sixth process, a plate material that covers the entire surface of the flat powder collection in the container is placed over the entire surface of the flat powder collection, and the entire surface of the plate material is evenly compressed to crush the fine crystals of nickel octylate into even finer crystals. As a result, the even finer crystals of nickel octylate are piled up and accumulated at a high density in the gaps between the overlapping flat surfaces of the flat powder and on the entire surface of the flat powder collection. In the seventh process, a compressive load is evenly applied to the surface of the plate material, and the container is heated to 290°C at which the thermal decomposition of nickel octylate is completed, causing the nickel octylate to thermally decompose. In the eighth process, the container is rotated in three directions: front-back, left-right, and top-bottom. impact Acceleration is applied and the sheet consisting of the collection of flat powder is peeled off from the bottom of the container. As a result, a sheet consisting of a collection of flat powder is obtained in which the flat surfaces of the flat powder are bonded together via a collection of nickel nanoparticles of about 10 nm in size that are bonded by frictional heat. The thermal decomposition temperature of nickel octylate in a nitrogen atmosphere is 340°C, which is 50°C higher than in air. Here, we will explain the phenomena that occur in the eight processes and the effects that each process brings about. In the first process, nickel octylate is dispersed in methanol, and the nickel octylate becomes molecular and disperses in the methanol. This causes the raw material for nickel nanoparticles to be liquid-phase. Since nickel octylate does not dissolve in methanol, when methanol is evaporated from the nickel octylate, fine crystals of nickel octylate are precipitated. In the second process, a collection of soft magnetic flat powder made of any one of iron, permalloy, silicon steel, sendust, or electromagnetic stainless steel is weighed out to a weight less than the weight of methanol multiplied by the ratio of the density of the flat powder used to the density of the methanol, and the collection of soft magnetic flat powder is placed in a container and stirred. On the other hand, since the hardness of the soft magnetic flat powder differs depending on the material, the thickness of the flat powder varies depending on the material. Reduced iron powder, which is the hardest of all soft magnetic flat powders and difficult to flatten, is flattened to a thickness of 10-20 μm. The weight of the flat powder of reduced iron powder with a particle size of 100 μm and a thickness of 15 μm is 0.927 × 10 -6 g. In contrast, when a small amount of nickel is added to sendust, a ternary alloy of iron, silicon, and aluminum, and the amount of silicon added is reduced to make flattening easier, the thickness of the flattened powder is as thin as 1-1.5 μm. The weight of sendust flattened powder with a particle size of 40 μm and a thickness of 1 μm is 0.86×10 -8 g. The density of iron is 7.8 g / cm 3 The density of sendust is 7.6 g / cm 3 The reason why the weight of the reduced iron powder flakes is two orders of magnitude larger than that of the sendust flakes is due to the difference in the thickness and particle size of the flakes. On the other hand, the density of methanol is 0.792 g / cm 3 The density of nickel octylate is 1.08g / cm 3Therefore, the density of the methanol dispersion of nickel octylate is close to 1 / 10 of the density of the soft magnetic flat powder. Therefore, the weight of the soft magnetic flat powder used is less than 10 times the weight of the methanol in which nickel octylate is dispersed. On the other hand, the density of the methanol dispersion of nickel octylate is close to 1 / 10 of the density of the soft magnetic flat powder. Therefore, the theoretical volume calculated from the weight and density of the soft magnetic powder mass is less than the volume of the methanol dispersion of nickel octylate. However, the weight of one sheet of soft magnetic flat powder is extremely small. Furthermore, the dispersion concentration of nickel octylate in methanol is low, about 10% by weight. Therefore, the viscosity of the methanol dispersion of nickel octylate is close to the viscosity of methanol. The viscosity of methanol is extremely low, at 0.59 mPa·sec. Therefore, when a collection of soft magnetic flat powder is weighed out to a weight less than 1 / 10 of the weight of methanol and mixed with a methanol dispersion of nickel octylate, and the collection of soft magnetic flat powder is stirred in the methanol dispersion of nickel octylate, the weight of a single piece of soft magnetic flat powder is extremely small, so the soft magnetic flat powder disperses well in the low-density and low-viscosity methanol dispersion of nickel octylate, and the soft magnetic flat powder is evenly mixed in the methanol dispersion. As a result, even if the weight, thickness, size, and density of the soft magnetic flat powder are different, all of the soft magnetic flat powder is covered with the methanol dispersion of nickel octylate. In the third process, a homogenizer is placed in the container and operated in the container. At this time, since the methanol dispersion of nickel octylate is a low viscosity and low density liquid, the proportion of shock waves generated by the homogenizer that are consumed when exciting the methanol dispersion is small, and shock waves are efficiently and repeatedly applied to the collection of soft magnetic flat powder via the methanol dispersion. As a result, shock waves are repeatedly applied to all of the soft magnetic flat powder via the methanol dispersion of nickel octylate. On the other hand, when the density is 7.8 g / cm 3 Even for flat reduced iron powder with a large particle size of 100 μm and an extremely thick thickness of 15 μm, the weight is only 1×10 -6Therefore, even if the flat surfaces of the soft magnetic flake powder overlap each other in a complex manner, the shock waves are repeatedly applied to the extremely lightweight soft magnetic flake powder, and the flat surfaces overlap each other and are separated into individual flat powder pieces, which are then covered with a methanol dispersion of nickel octylate. In the fourth process, the container is impact Acceleration is applied repeatedly, and finally impact Acceleration is applied. In other words, the soft magnetic flat powder overlapping on the flat surface is separated into individual soft magnetic flat powder sheets by the homogenizer device, and all the soft magnetic flat powder sheets are covered with a low-viscosity, low-density methanol dispersion of nickel octylate, and are evenly dispersed in the methanol dispersion. This collection of soft magnetic flat powder sheets is subjected to three-way acceleration. impact When acceleration is applied repeatedly, the soft magnetic flaky powder is extremely light, so the low viscosity, low density methanol dispersion of nickel octylate is absorbed by the flaky powder. impact The soft magnetic powder is repeatedly moved in the direction of acceleration. Since the soft magnetic powder has a flat surface with a large aspect ratio, the flat surface is placed on top together with a methanol dispersion of nickel octylate. impact It moves repeatedly in the direction of acceleration. As the soft magnetic flat powder repeatedly moves in the methanol dispersion of nickel octylate, the flat powder particles rearrange themselves with the flat surfaces facing up and overlap, a phenomenon that progresses in the methanol dispersion of nickel octylate. In this way, the flat surfaces of the soft magnetic flat powder overlap each other via the methanol dispersion of nickel octylate. As a result, the collection of flat powder particles with overlapping flat surfaces spreads across the entire bottom surface of the container, forming the shape of the bottom surface, via the methanol dispersion of nickel octylate. Finally, in the vertical direction, impact Acceleration is applied to the container. Application of impact force Stop. In the fifth treatment, the container is heated to the boiling point of methanol. Consists of sizeClusters of nickel octylate microcrystals are deposited in the gaps between the overlapping flat surfaces of the soft magnetic flaky powder and on the entire surface of the clusters of soft magnetic flaky powder. In other words, in the methanol dispersion of nickel octylate, nickel octylate is dispersed in the methanol in a molecular state, so when the methanol is evaporated, the nickel octylate before dispersion is dispersed into particles smaller than 100 nm. Consists of size It precipitates as a collection of fine crystals. The concentration of nickel octylate in the methanol dispersion of nickel octylate is low, and excess methanol evaporates. At this time, the thickness of the fine crystals that precipitate in the gaps between the flat surfaces and on the surfaces of the collection of flat powder is thin, being submicron thick. On the other hand, since nickel octylate that was dispersed in a molecular state precipitates as fine crystals, the fine crystals are a collection of crystals in which crystals that form single molecules of nickel octylate are accumulated. For this reason, when stress is applied to the fine crystals, the fine crystals are easily crushed. However, the finer the fine crystals are, the more difficult it is to apply stress to them, and there is a limit to how fine the fine crystals can be. In addition, the evaporated methanol is recovered by a recovery machine and reused. In the sixth process, a plate material that covers the entire surface of the soft magnetic flat powder in the container is placed over the entire surface of the soft magnetic flat powder, and the entire surface of the plate material is compressed evenly. At this time, the gaps between the overlapping flat surfaces of the soft magnetic flat powder and the collection of nickel octylate fine crystals that are overlapping and precipitated over the entire surface of the soft magnetic flat powder are crushed into finer crystals. Since the relatively larger the size of the fine crystals, the easier they are to crush, the relatively larger fine crystals are crushed first, and the crushing of the fine crystals progresses while the compressive load is applied. On the other hand, when the fine crystals are crushed, new voids are formed in the collection of fine crystals, and the crushed and finer crystal collections move into the voids to fill them. As the crushing of the fine crystals progresses, the crushed and finer crystals overlap at a high density in the gaps between the overlapping flat surfaces of the soft magnetic flat powder and on the entire surface of the soft magnetic flat powder cluster, and the finer crystal clusters accumulate at a high density, forming a thin layer due to the crystal clusters. When the crushing of the nickel octylate crystals reaches its limit, the crushing of the fine crystals does not progress even when a compressive load is applied to the plate material, and the plate material to which the compressive load is applied no longer moves, and the repulsive force from the plate material increases. At this point, the process of compressing the plate material surface is stopped. As a result, the size of the fine crystals is reduced to about 20 nm, which is nearly 1 / 5 of the size at the time of precipitation, and the thickness of the nickel octylate fine crystals of about 20 nm, which overlap at a high precipitation density in the gaps between the soft magnetic flat surfaces and on the surface of the soft magnetic flat powder cluster, becomes 120-180 nm thick. The compressive load applied to the plate is equivalent to 10-100 kg depending on the size of the container and the amount of microcrystals. The impact acceleration applied to the container is 0.2-1.0 G depending on the size of the container and the amount of microcrystals. This causes clusters of nickel octylate crystals with a size of about 20 nm to overlap at high density in the gaps between the overlapping flat surfaces of the soft magnetic flat powder and on the entire surface of the cluster of flat powder. In the seventh process, a compressive load is evenly applied to the entire surface of the plate material, and the container is heated to 290°C at which the thermal decomposition of nickel octylate is completed, and the fine crystals of nickel octylate are thermally decomposed. First, the moisture adsorbed on the flat powder and foreign matter consisting of compounds with hydroxyl groups are vaporized. Next, the thermal decomposition of the fine crystals of nickel octylate begins, and nickel octylate is thermally decomposed into octylic acid and nickel. When the vaporization of the octylic acid molecules is completed, the nickel molecules gather to form granular nickel nanoparticles with a size of about 10 nm, and 6-8 of the granular nickel nanoparticles overlap and precipitate simultaneously. The nickel nanoparticles do not contain any impurities and precipitate as genuine nickel nanoparticles. In addition, the nickel nanoparticles precipitate as nanoparticles in an activated state. Therefore, adjacent nickel nanoparticles are metallically bonded at the contact area. After this, the metallically bonded nickel nanoparticles are rejoined by frictional heat. On the other hand, as the thermal decomposition of the fine crystals of nickel octylate progresses, the foreign matter consisting of organic matter adsorbed to the soft magnetic flat powder vaporizes. This cleans the flat surface of the soft magnetic flat powder, and a collection of genuine nickel nanoparticles precipitates on the cleaned flat surface, increasing the bonding strength of the nickel nanoparticles bonded to the flat surface by frictional heat. In addition, the bonding strength between the genuine nickel nanoparticles due to frictional heat also increases. In addition, since the nickel nanoparticles are small, around 10 nm, and the contact area of ​​the granular nanoparticles with the flat surface is extremely small, no stress distortion occurs on the flat surface when the granular nickel nanoparticles are bonded to the flat surface by frictional heat. For this reason, there is no need to anneal the sheet consisting of a collection of soft magnetic flat powder to relieve distortion. In the eighth process, the container is impactAcceleration is applied, and the sheet consisting of the soft magnetic flat powder is peeled off from the bottom of the container. As a result, a sheet consisting of the soft magnetic flat powder is obtained. The layer of nickel nanoparticles formed on the surface of the flat powder and in the gaps between the flat powders is a very thin layer with a thickness of 60-80 nm, which corresponds to a collection of 6-8 nanoparticles, and the size of the nickel nanoparticles, which is about 10 nm in size, is more than two orders of magnitude smaller than the flat surface of the flat powder. For this reason, the sheet consisting of the soft magnetic flat powder has the properties of the soft magnetic flat powder. Here, when soft magnetic flat powder is used as the flat powder described in paragraph 18, nickel octylate is used as the organometallic compound described in paragraph 18, and a sheet consisting of a collection of soft magnetic flat powder in which the flat surfaces of the soft magnetic flat powder are bonded together via a collection of nickel nanoparticles according to the method described in paragraph 18, provides the following effects. First, the material that bonds the flat surfaces of the soft magnetic flat powder is a collection of nickel nanoparticles, and then nickel octylate, the raw material for the nickel nanoparticles, is dispersed in methanol to create a liquid phase. Because this liquid has low viscosity and density, by continuously carrying out the second and third processes, it becomes possible to interpose the methanol dispersion of nickel octylate in the gaps between the flat surfaces of the soft magnetic flat powder that have been separated into individual sheets. Secondly, the homogenizer is operated in the container, and the shock waves generated by the homogenizer are consumed in small proportions when exciting the methanol dispersion of nickel octylate because the methanol dispersion of nickel octylate has low viscosity and low density, and most of the impact energy is efficiently and repeatedly transmitted to the collection of soft magnetic flat powder. Therefore, even if the soft magnetic flat powder has complex overlapping flat surfaces, the soft magnetic flat powder is extremely light, so it is reliably separated into individual flat powder sheets, and the methanol dispersion of nickel octylate comes into contact with the surface of all the flat powder regardless of the material, shape, and particle size distribution of the flat powder. In addition, the surfaces of the soft magnetic flat powder are all hydrophobic and do not react with the methanol dispersion of nickel octylate, and the methanol dispersion of nickel octylate comes into contact with the surface of the soft magnetic flat powder. Thirdly, the container has three directions: left and right, front and back, and top and bottom. Impact force Repeatedly add, and finally add Impact force At this time, since the methanol dispersion of nickel octylate has low viscosity and low density, and the soft magnetic flaky powder is extremely light, the methanol dispersion of nickel octylate is mixed with the soft magnetic flaky powder. impact The object is repeatedly moved in the direction of acceleration. This causes the soft magnetic flaky powder to rearrange and overlap with the flat surface facing up in the methanol dispersion of nickel octylate. As a result, the soft magnetic flaky powder spreads over the entire bottom surface of the container, and a collection of flat powder with overlapping flat surfaces through the methanol dispersion of nickel octylate forms the shape of the bottom surface of the container. Fourth, the soft magnetic flake powder separated into individual pieces is stacked with the flat surfaces facing each other via a methanol dispersion of nickel octylate, so the larger the aspect ratio of the soft magnetic flake powder is, the less soft magnetic flake powder is used. Therefore, even if the soft magnetic flake powder is expensive, a sheet made of a collection of soft magnetic flake powder with the flat surfaces stacked together can be produced inexpensively. Fifth, methanol is evaporated from the flat powder clusters whose flat surfaces overlap each other through a methanol dispersion of nickel octylate, and clusters of nickel octylate microcrystals are precipitated in the gaps between the flat surfaces and on the surface of the flat powder clusters. Furthermore, the entire surface of the soft magnetic flat powder cluster is evenly compressed. This causes the microcrystals to be crushed to about 1 / 5 of their original size, and the crushed crystal clusters are overlapped and accumulated at high density in the gaps between the flat surfaces and on the surface of the flat powder clusters. These crushed nickel octylate microcrystals, which are about 20 nm in size, become the raw material for clusters of nickel nanoparticles, which are about 10 nm in size, that connect the flat surfaces of the flat powder. Sixth, the soft magnetic flat powder is heated while being compressed evenly, and the crushed nickel octylate microcrystals are thermally decomposed. At this time, the nickel nanoparticles are piled up and precipitated at high density in the gaps between the flat surfaces and on the surface of the flat powder. Furthermore, the soft magnetic flat powder is compressed evenly, and the nickel nanoparticles precipitated at high density are bonded to the flat surfaces by frictional heat, and the nickel nanoparticles are bonded to each other by frictional heat. In other words, since the nickel nanoparticles are piled up and precipitated at high density, it becomes difficult for the compressed nanoparticles to move in the nanoparticles, and frictional heat is generated at the contact points of the nanoparticles in contact with the flat surfaces and at the contact points between the nanoparticles, and the nickel nanoparticles are bonded to the flat surfaces by the bonding force due to the frictional heat, and the nickel nanoparticles are bonded to each other by the bonding force due to the frictional heat. Seventh, soft magnetic flat powder made of iron, permalloy, silicon steel, sendust, or electromagnetic stainless steel can be used as the flat powder when manufacturing a sheet made of a collection of flat powders. In other words, the thermal decomposition temperature of nickel octylate is 290°C in the air atmosphere. On the other hand, the melting points of any of the soft magnetic flat powders made of iron, permalloy, silicon steel, sendust, or electromagnetic stainless steel are significantly higher than 290°C, and none of the soft magnetic flat powders have low-temperature brittleness, making them usable at extremely low temperatures. Therefore, a sheet made of a collection of flat powders in which the flat surfaces of the soft magnetic flat powders are joined together can be used in harsh environments such as high temperatures, extremely low temperatures, vacuum, and high pressure. The thermal decomposition temperature of nickel octylate in a nitrogen atmosphere is 340°C, which is 50°C higher than that of the air atmosphere, but is significantly lower than the melting point of the soft magnetic flat powder. Eighth, the flat surfaces of the soft magnetic flat powder are joined together with a collection of nickel nanoparticles. Nickel has a maximum relative magnetic permeability of 600. In addition, at 2.45 GHz, the complex permeability is 1.592 in real part and 1.349 in imaginary part. Therefore, nickel is a ferromagnetic material with a constant maximum relative magnetic permeability and complex permeability among metals and metal oxides. Although its magnetic shielding performance is inferior to iron, its complex permeability has a constant value in the high frequency band. For this reason, the nickel nanoparticles do not inhibit the permeability characteristics of the soft magnetic flat powder in the sheet in which the flat surfaces of the soft magnetic flat powder are joined together. Ninth, nickel octylate is a general-purpose industrial chemical. Also, since the flat surfaces of the flat powder are bonded together, the amount of flat powder used is small. Furthermore, all eight processes for bonding the flat surfaces together with a collection of nickel nanoparticles are simple processes. Therefore, a sheet made of a collection of soft magnetic flat powder can be manufactured using inexpensive materials at low cost. As described above, the sheet made of a collection of soft magnetic flat powder produced by this manufacturing method has flat surfaces bonded together with collections of nickel nanoparticles, making it a sheet made of a collection of soft magnetic flat powder that has revolutionary effects not found in conventional collections of soft magnetic flat powder.

[0022] The method for producing a sheet made of an aggregate of soft magnetic flat powder described in paragraph 20 is a method for producing a sheet made of an aggregate of soft magnetic flat powder of a plurality of types of alloys, and the method for producing a sheet made of an aggregate of soft magnetic flat powder of a plurality of types of alloys is as follows: The soft magnetic flat powder described in paragraph 20 is a soft magnetic flat powder made of a plurality of alloys other than iron described in paragraph 20, and the frequency characteristics of the imaginary part of the complex permeability of the soft magnetic flat powder made of the plurality of alloys are each Made of alloy The soft magnetic flat powders are different from each other, and each of the above Made of alloyA method for producing a sheet made of an assembly of soft magnetic flat powders of multiple types of alloys, the method comprising using the soft magnetic flat powder made of multiple types of alloys as the flat powder described in paragraph 18, using nickel octylate described in paragraph 20 as the organometallic compound described in paragraph 18, and producing a sheet made of an assembly of flat powders of multiple types of alloys in which the flat surfaces of the soft magnetic flat powders of the multiple types of alloys are bonded to each other via a cluster of nickel nanoparticles, in accordance with the method for producing a sheet made of an assembly of flat powders of the multiple types of alloys, the frequency characteristics of the imaginary part of the complex permeability of the soft magnetic flat powder being such that the imaginary parts of the complex permeability complement each other in different frequency ranges. 。

[0023] As described in paragraph 16, when soft magnetic powder is flattened in the plane direction, which is the direction of the easy axis of magnetization, the demagnetizing factor becomes smaller, and the greater the flatness, the greater the imaginary part μ" of the complex permeability. In addition, the frequency characteristics of the imaginary part of the complex permeability of the flattened powder vary greatly depending on the material of the soft magnetic flat powder. Therefore, if multiple types of soft magnetic flat powder made of metal or alloy have different frequency characteristics of the imaginary part of the complex permeability and the frequency characteristics of the imaginary part of each complex permeability are complementary to each other in different frequency ranges, then if multiple types of soft magnetic flat powder made of such metal or alloy are used and the multiple types of flat powder are randomly joined together with their flat surfaces to form a sheet, the characteristics of the imaginary part of the complex permeability of the multiple types of flat powder will be reflected in the sheet, and the sheet will absorb electromagnetic noise over a wide frequency band. In addition, the sheet prevents electromagnetic noise interference caused by electromagnetic waves interfering with each other. However, among the multiple types of soft magnetic flat powders made of metals or alloys, only the flat powder of reduced iron powder has a higher hardness than the other soft magnetic flat powders, and therefore the thickness of the flat powder is extremely thick at 10-20 μm. In contrast, the composition of the other soft magnetic flat powders is finely adjusted to reduce the hardness and enable flattening, and the thickness deviation is within the range of 1-1.5 μm. Therefore, when a collection of flat powders in which the flat powder of reduced iron powder is mixed with flat powders made of other materials is treated by the method described in paragraph 20, the flat surfaces of all the flat powders do not overlap with each other through the methanol dispersion of nickel octylate. Therefore, when a sheet is manufactured using soft magnetic flat powders made of multiple types of metals or alloys, the flat powder of reduced iron powder is excluded from the soft magnetic flat powder made of metals or alloys described in paragraph 20. Therefore, the multiple types of soft magnetic flat powders become multiple types of soft magnetic flat powders made of alloys. As a result, the multiple types of soft magnetic flat powder described in paragraph 20 can be combined to have three characteristics: first, flat powder made of multiple types of alloys excluding flat powder made of reduced iron powder; second, the frequency characteristics of the imaginary part of the complex permeability of the flat powder made of the multiple types of alloys are different from each other; and third, the frequency characteristics of the imaginary part of the complex permeability of each flat powder have frequency characteristics of the imaginary part of the complex permeability that complement each other in different frequency ranges. Furthermore, when the soft magnetic flat powder made of multiple types of alloys having the three characteristics is used as the soft magnetic flat powder described in paragraph 20 and the eight processes are performed according to the method described in paragraphs 20-21, a sheet consisting of a collection of soft magnetic flat powders randomly bonded together by the flat surfaces of the soft magnetic flat powder made of multiple types of alloys is produced. This sheet reflects the characteristics of the imaginary part of the complex permeability of soft magnetic flat powder made up of multiple types of alloys with three characteristics, and the imaginary part of the complex permeability has a constant magnitude over a wider frequency band that was difficult to achieve with a single type of flat powder, making it a sheet that can absorb electromagnetic noise over a wide frequency band or prevent electromagnetic noise interference, which was previously difficult to achieve. On the other hand, as described in paragraph 16, the flat powder is produced by attriting the atomized soft magnetic powder or the reduced soft magnetic powder with a media stirring mill. Therefore, if the material of the flat powder is different, the shape, structure and hardness of the atomized soft magnetic powder or the reduced soft magnetic powder will change, so not only the flatness but also the shape, particle size distribution and hardness of the flat powder will be different. However, as described above, the thickness deviation is narrow at 1-1.5 μm and the thickness is thin. Furthermore, the manufacturing method of the sheet made of a collection of soft magnetic flat powder consists of the eight processes described in paragraphs 20-21. On the other hand, even if the soft magnetic flat powder made of multiple types of alloys other than reduced iron powder is a flat powder made of multiple types of alloys with different flatness, shape, particle size distribution and hardness, the eight processes are possible. Therefore, a sheet can be produced in which the flat surfaces of a collection of soft magnetic flat powder made of multiple types of alloys excluding reduced iron powder are randomly bonded together with a collection of nickel nanoparticles. This sheet provides the following effects similar to those described in paragraph 21: First, in a collection of soft magnetic flat powders made of multiple alloys, 6-8 nickel nanoparticles are piled up and precipitated in the gaps between the flat surfaces of the flat powder, forming a bonding layer with a very thin thickness of 60-80 nm, randomly bonding the flat surfaces together. Since the size of the nickel nanoparticles is more than two orders of magnitude smaller than the area of ​​the flat powder, the sheet made of multiple alloys has the properties of the flat powder of multiple alloys. Secondly, since the sheet is formed on the bottom surface of the container in the shape of the bottom surface, there are no restrictions on the area and shape of the sheet. In addition, even if the soft magnetic flat powder made of multiple types of alloys other than reduced iron powder is a flat powder made of multiple types of alloys with different flatness, shape, particle size distribution, and hardness, eight processes for forming a sheet are possible, so a sheet can be manufactured in which the flat surfaces of the flat powder made of multiple types of alloys other than reduced iron powder are bonded together with a collection of nickel nanoparticles. Therefore, the manufacturing method of this sheet can be used to form a sheet with versatility for soft magnetic flat powders other than flat reduced iron powder. Thirdly, a sheet made by overlapping flat surfaces of soft magnetic flat powder made of multiple types of alloys with high relative magnetic permeability has a high magnetic shielding effect. Furthermore, if the thickness of the sheet is close to the skin depth of the flat powder, a sheet with a large area can be formed using a small amount of flat powder, and all the flat powder will participate in the magnetic shielding, improving the magnetic shielding effect. Fourth, if the soft magnetic flat powders made of multiple alloys have different frequency characteristics of the imaginary part of the complex permeability, and the frequency characteristics of the imaginary part of each complex permeability are complementary to each other in different frequency ranges, a sheet formed using a collection of soft magnetic flat powders made of multiple alloys will absorb electromagnetic noise in a wide frequency band that was previously difficult. Also, if the thickness of the sheet is made close to the skin depth of the flat powders of multiple alloys, a sheet with a large area can be formed using a small amount of flat powder, and all the flat powders will participate in absorbing electromagnetic noise, improving the electromagnetic noise absorption effect. As described above, the sheet made by this manufacturing method, which is made of a collection of soft magnetic flat powder of multiple types of alloys, has the flat surfaces of the soft magnetic flat powder of multiple types of alloys randomly bonded together with a collection of nickel nanoparticles, and therefore has the functional effects of soft magnetic flat powder of multiple types of alloys that are not found in collections of conventional soft magnetic flat powder.

[0024] The method for producing a sheet made of a collection of flat powder described in paragraph 18 is a method for producing a sheet made of a collection of flake powder of a metal or alloy, and the method for producing a sheet made of a collection of flake powder of a metal or alloy is as follows: The flat powder described in paragraph 18 is made of silver, copper, brass, nickel, or aluminum. 1 type The metal or alloy flake powder is made of the material described above, and the organometallic compound described in paragraph 18 is either copper octylate, aluminum octylate, or nickel octylate. 1 type Any of the above metal octylate compounds is used. 1 typeas the flat powder described in paragraph 18, and any of the above metal octylate compounds as the organometallic compound described in paragraph 18, according to a method for producing a sheet consisting of an assembly of the flat powder described in paragraph 18, 1 type The flat surfaces of the metal or alloy flake powder made of the above material are bonded together via a collection of nanoparticles made of copper, aluminum, or nickel. Either one of the following Metal or If Method for producing a sheet made of an aggregate of gold flake powder, and method for producing a sheet made of an aggregate of metal or alloy flake powder 。

[0025] First, a method for producing the flake powder made of a metal or alloy used in the present invention will be described. Flake powder made of silver, copper, brass, or nickel, excluding aluminum, is produced by pounding metal or alloy powder made of silver, copper, brass, or nickel with a stamp mill using a number of metal pestles, stretching the powder into thin flakes, and flattening the powder into thin flakes. ofBrass flake powder is sometimes called brass flake powder. When this metal or alloy flake powder is pounded with a number of metal pestles, undulations are formed on the surface, and the flatness of the flake powder is not high. On the other hand, for aluminum, the fine particles are highly active, so the fine particles produced by the atomization method are flattened in a wet ball mill to produce scaly flake powder. This aluminum flake powder has a surface roughness due to the flattening process using a wet ball mill. These metal or alloy flake powders have a high aspect ratio, which is the ratio of the thickness to the long axis. Therefore, by overlapping the flat surfaces together, a sheet with a certain area can be formed from a small amount of flake powder. In addition, since the surface of the flake powder is smooth, the friction coefficient of the surface is small, at 0.20-0.25. For this reason, the metal or alloy flake powder has a lubricating surface, electrical and thermal conductivity based on the material, and the color and luster inherent to the metal or alloy. Among soft metals, the melting point of tin is 232°C, which is lower than the thermal decomposition temperature of metal octylate compounds, and it becomes brittle at low temperatures around -40°C. Similarly, zinc also becomes brittle at low temperatures. For this reason, flake powder made of tin and zinc was excluded from the raw materials used to create sheets made of a collection of flake powder. Next, the material of the nanoparticles that bond the flat surfaces of the metal or alloy flake powder together will be described. If the material of the nanoparticles is excellent in electrical conductivity and thermal conductivity, a sheet consisting of a collection of flake powders bonded with a collection of metal nanoparticles will be a sheet with excellent electrical conductivity and thermal conductivity with a wide area that cannot be obtained with flat powder. Also, if the nanoparticles are made of a transparent material, a sheet consisting of a collection of flake powders bonded with a collection of transparent nanoparticles will be a sheet with the inherent color and luster of metals or alloys. On the other hand, the electrical conductivity of metals is best in the order of silver, copper, gold, aluminum, calcium, and magnesium. Also, the thermal conductivity of metals is best in the order of silver, copper, gold, aluminum, magnesium, and zinc. Furthermore, it is desirable that the octylate metal compound, which is the raw material of the nanoparticles, is relatively inexpensive. Therefore, when manufacturing a sheet with excellent electrical conductivity and thermal conductivity, it is appropriate to bond the flat surfaces of the flake powders together with nanoparticles made of copper or aluminum. On the other hand, when manufacturing a sheet with the inherent color and luster of metals or alloys, it is appropriate to bond the flat surfaces of the flake powders together with a collection of transparent nanoparticles. Since the collection of nanoparticles made of aluminum or nickel has transparency, the collection of flake powder bonded with the collection of nanoparticles made of aluminum or nickel becomes a sheet having the inherent color and luster of the flake powder. Here, transparent nanoparticles are explained. A transparent substance must have a first characteristic that the refractive index in the wavelength region of visible light is 0.4 or more and 2.4 or less, and a second characteristic that the size is a fine particle that is one order of magnitude smaller than the wavelength of visible light. That is, when the flat surfaces of flake powder are joined together using a substance with a refractive index of 0.4 or more and 2.4 or less, the refractive index is close to the refractive index of air, which is 1, so that more than 70% of the visible light is incident on the flat surface of the flake powder due to the surface reflectance and total light transmittance of the light. Note that the surface reflectance and total light transmittance will be explained in paragraph 27. Furthermore, if the size of the fine particles is one order of magnitude smaller than the wavelength of visible light, the visible light is hardly scattered by the collection of fine particles, and the visible light is transmitted with high transparency. As a result, when a collection of nanoparticles with a refractive index of 0.4 or more and 2.4 or less and a size nearly two orders of magnitude smaller than the wavelength of visible light is formed on the surface of the flake powder, the visible light is transmitted through the collection of nanoparticles. In addition, when flat surfaces are joined together through a collection of nanoparticles, visible light passes through the gaps between the flat surfaces. The scattering of light in a collection of fine particles is explained in paragraph 27. Nanoparticles made of nickel or aluminum are transparent materials that have both of these characteristics. Nickel or aluminum has a refractive index of 0.4 or more and 2.4 or less in the visible light wavelength range (380-750 nm). That is, the refractive index of nickel is 1.61 at 380 nm, and increases with increasing wavelength, being 1.75 at 539 nm, 2.21 at 709 nm, 2.28 at 729 nm, and 2.34 at 750 nm. Therefore, light is reflected by the difference in refractive index between air and nickel at the surface of the nickel nanoparticle cluster covering the surface made of the flake powder cluster, and at the surface of the bonding layer made of the nickel nanoparticle cluster bonding the flat surfaces of the flake powder. In this case, the light transmittance is 89% at 380 nm, 86% at 539 nm, 74% at 709 nm, 72% at 729 nm, and 70% at 750 nm. Therefore, a part of the red visible light component is reflected by the surface of the nickel nanoparticle cluster. In addition, the size of the nickel nanoparticles is nearly two orders of magnitude smaller than the wavelength of visible light. Therefore, the light that enters the nickel nanoparticle cluster passes through the nickel nanoparticle cluster with almost no scattering. In contrast, the refractive index of aluminum is a maximum of 2.80 at 800 nm, and decreases rapidly as the wavelength becomes shorter, reaching 2.40 at 750 nm, 1.91 at 708 nm, and closest to the refractive index of air of 1 at 560 nm, 0.620 at 450 nm, and 0.45 at 380 nm. Therefore, light is reflected on the surface of the aluminum nanoparticles due to the difference in the refractive index between air and aluminum. In this case, the light transmittance is 69% at 750 nm, 81% at 708 nm, 100% at 560 nm, 89% at 450 nm, and 73% at 380 nm. Therefore, part of the red and purple visible light is reflected on the surface of the aluminum nanoparticles. In addition, the size of the aluminum nanoparticles is nearly two orders of magnitude smaller than the wavelength of visible light. Therefore, the light that enters the aluminum nanoparticles passes through the aluminum nanoparticles with almost no scattering. As explained above, in a group of aluminum nanoparticles, some of the light rays that make up visible light are reflected on the surface of the group of aluminum nanoparticles, and emit a color corresponding to this light, but the group of aluminum nanoparticles is transparent. In addition, in a group of nickel nanoparticles, the group of nickel nanoparticles is nearly colorless and also transparent. As explained above, the group of nanoparticles made of aluminum or nickel bonds the flat surfaces of the flake powder together while maintaining transparency. Therefore, the color and luster reflected by the flake powder are not lost. Next, we will explain the phenomenon that occurs when flat surfaces of flake powder made of metal or alloy are bonded together with a collection of nanoparticles. The Mohs hardness of silver, copper, brass, nickel, or aluminum that make up the flake powder is 2.7 for silver, 2.9 for aluminum, 3.0 for copper, 3-4 for brass, and 3.5 for nickel. The Young's modulus is 69 GPa for aluminum, 82.7 GPa for silver, 130 GPa for copper, 103 GPa or 110 GPa for brass, and 204 GPa for nickel. Therefore, the Mohs hardness of all the metals or alloys that make up the flake powder is low. On the other hand, since the nanoparticles are about 10 nm in size, the thickness of the thinnest flake powder is 20 times the size of the nanoparticle, and the area of ​​the flat powder with the smallest surface area is 1000 times the size of the nanoparticle. The contact area of ​​the nanoparticles with the flat surfaces of such flake powder is extremely small. In addition, the contact area between the nanoparticles is also extremely small. On the other hand, as described above, the Young's modulus of metals or alloys other than nickel is small, and they are excellent in ductility and malleability. Therefore, when the flat surfaces of flake powder of a metal or alloy other than nickel are joined together with a collection of nanoparticles made of copper or aluminum, the nanoparticles made of copper or aluminum contact the flat surfaces, and localized parts of the contact area on the flat surfaces are elastically deformed. At this time, frictional heat is generated at the localized parts of the contact area. On the other hand, since the nanoparticles are also made of copper or aluminum, which has a small Young's modulus, localized parts of the contact area on the nanoparticles are elastically deformed. At this time, frictional heat is generated at the localized parts of the contact area. Due to the frictional heat between the two, the flat surfaces of the flake powder made of a metal or alloy are joined together with a collection of nanoparticles made of copper or aluminum. In addition, localized parts of the contact area between the nanoparticles made of copper or aluminum are elastically deformed, and frictional heat is generated at the localized parts of the contact area. As a result, the copper or aluminum nanoparticles are bonded together by frictional heat. Meanwhile, when the copper or aluminum nanoparticles come into contact with the flat surface of the nickel flake powder, the localized area of ​​the contact area of ​​the nanoparticles is elastically deformed. At this time, frictional heat is generated at the localized area of ​​the contact area.On the other hand, nickel flake powder has a large Young's modulus, so localized areas of contact on the flat surfaces do not elastically deform, but frictional heat is generated. The frictional heat between the two also bonds the flat surfaces of the nickel flake powder together with a collection of nanoparticles made of copper or aluminum. Localized areas of contact between nanoparticles made of copper or aluminum also elastically deform, and frictional heat is generated at the localized areas of contact. As a result, nanoparticles made of copper or aluminum are bonded together by frictional heat. In contrast, when a nickel nanoparticle comes into contact with a flat surface of a metal or alloy flake powder, a localized portion of the contact area on the flat surface is preferentially elastically deformed. At this time, frictional heat is generated at the localized portion of the contact area. On the other hand, since the nickel nanoparticles have a large Young's modulus, the localized portion of the contact area on the nanoparticles does not elastically deform, but frictional heat is generated. Therefore, the flat surfaces of the metal or alloy flake powder are bonded together by a collection of nickel nanoparticles due to the frictional heat between the two. In addition, frictional heat is generated at the localized portion of the contact area between the nickel nanoparticles. As a result, the nickel nanoparticles are bonded together by the frictional heat. As a result, the flat surfaces of the metal or alloy flake powder are bonded together by the collection of nanoparticles made of copper, aluminum, or nickel. The nanoparticles are also bonded together by frictional heat. The heat resistance of metal or alloy flake powder is determined by its softening point, with the lowest softening point being 350°C for aluminum. In addition, metals or alloys made of silver, copper, brass, nickel, or aluminum do not have low-temperature brittleness, making them usable at extremely low temperatures. For this reason, a sheet made of a collection of flake powder in which the flat surfaces of the flake powder are bonded together can be used in harsh environments such as high temperatures, extremely low temperatures, ultra-vacuum, and ultra-high pressure, where oil lubrication cannot be applied. In addition, the load resistance is high at 600 MPa or more. For this reason, when a collection of flake powder is compressed, the flat surfaces of the flake powder can withstand the compressive stress. As mentioned above, the softening point of aluminum is low at 350°C. On the other hand, when flat surfaces of aluminum flake powder are joined together with a collection of copper, aluminum, or nickel nanoparticles, the contact area of ​​the copper, aluminum, or nickel nanoparticles with the flat surfaces is extremely small. Therefore, even when flat surfaces of aluminum flake powder are joined together with a collection of aluminum nanoparticles, the contact area between the aluminum flat surfaces and the aluminum nanoparticles does not soften. In addition, the metal or alloy flake powder has a smooth surface, but the surface is not flat and has its own undulations. On the other hand, the size of the copper, aluminum, or nickel nanoparticles is nearly two orders of magnitude smaller than the unevenness of the flat surfaces. Therefore, regardless of the flatness of the flat surfaces and the unevenness of the surface, the entire surfaces of the flat surfaces are bonded together through a collection of copper, aluminum, or nickel nanoparticles. In addition, the aluminum flake powder has unevenness formed on its surface by flattening processing using a wet ball mill. However, the size of the copper, aluminum, or nickel nanoparticles is more than two orders of magnitude smaller than the unevenness of the flat surfaces. Therefore, regardless of the unevenness of the flat surfaces of the aluminum flake powder, the entire surfaces of the flat surfaces are bonded together through a collection of copper, aluminum, or nickel nanoparticles. The thickness of metal or alloy flake powder varies from 0.2 to 1 μm depending on the material, but within the grade of the product used, the thickness deviation is within 0.1 μm. Even if the material of the flake powder is the same, the grain size varies depending on the product because the flattening conditions differ for each product. On the other hand, the density of metals or alloys varies greatly depending on the material. Aluminum has a density of 2.7 g / cm3. 3 And silver is 10.5g / cm 3 And copper is 9.0g / cm 3 And brass is 8.7g / cm 3 And nickel is 8.9g / cm 3 However, even in the case of flake powders with the highest density and relatively large flat powder, that is, the density is 10.5 g / cm 3Even if the silver flake powder has a particle size of 100 μm and a thickness of 0.5 μm, the weight of the flake powder is only 4.5 × 10 -8 g. Next, an octylic acid metal compound that precipitates a metal by thermal decomposition will be described. In a carboxylate metal compound that combines the first characteristic that the oxygen ion that constitutes the carboxyl group of the carboxylic acid is covalently bonded to the metal ion and the second characteristic that the carboxylic acid is a saturated fatty acid, the metal ion is the largest ion, and the distance between the oxygen ion that constitutes the carboxyl group and the metal ion is longer than the distance between the other ions. When a carboxylate metal compound having such molecular structure characteristics is heat-treated in an air atmosphere, when the temperature exceeds the boiling point of the carboxylic acid, the bond between the oxygen ion that constitutes the carboxyl group and the metal ion is first broken, and the carboxylic acid and the metal are separated. When the carboxylic acid is composed of a saturated fatty acid, since it does not have an unsaturated structure in which carbon atoms are in excess of hydrogen atoms, the carboxylic acid absorbs the heat of vaporization and vaporizes according to the molecular weight and number of the carboxylic acid, and the metal is precipitated when the vaporization is completed. In addition, the carboxylate metal compound disperses in methanol to nearly 10% by weight and does not dissolve in methanol. Therefore, a carboxylate metal compound that combines the two characteristics can be used as the organometallic compound described in paragraph 17. Such metal carboxylate compounds include metal octylate compounds, metal laurate compounds, and metal stearates. The boiling points of octylate, laurate, and stearic acid are 228°C, 296°C, and 361°C, respectively. Therefore, these metal carboxylate compounds are thermally decomposed in an air atmosphere of 290-430°C. Among the metal carboxylate compounds, the metal octylate compounds have the lowest thermal decomposition temperature, making them the most desirable metal carboxylate compounds. When the metal octylate compounds are thermally decomposed in a nitrogen atmosphere, the progress of the thermal decomposition reaction in the nitrogen atmosphere is delayed, and the thermal decomposition temperature rises to 340°C. Furthermore, metal carboxylate compounds are inexpensive industrial chemicals that can be easily synthesized. That is, when carboxylic acid, the most widely used organic acid, is reacted with a strong alkali, an alkali metal carboxylate compound is produced, and when an alkali metal carboxylate compound is reacted with an inorganic metal compound, a metal carboxylate compound made of various metals is synthesized. Therefore, it is the cheapest organometallic compound among organometallic compounds. Next, the present invention describes the various phenomena that occur when a flake powder made of a metal or alloy is used as the flat powder described in paragraph 18, and copper octylate, aluminum octylate, or nickel octylate is used as the organometallic compound described in paragraph 17, and when a sheet is produced according to the method for producing a sheet consisting of a collection of flat powders described in paragraph 18, and the effects and advantages that each phenomenon brings about. First, the material that bonds the flat surfaces of the flake powder is a collection of nanoparticles of copper, aluminum, or nickel, and then the raw material of the nanoparticles, a metal octylate compound, is dispersed in methanol to create a liquid phase. Because this liquid has low viscosity and density, by continuously carrying out the second and third processes, it becomes possible to interpose the methanol dispersion of the metal octylate compound in the gaps between the flat surfaces of the flake powder that have been separated into individual pieces. Secondly, a homogenizer is operated in the container, and shock waves are repeatedly generated by the homogenizer. On the other hand, since the methanol dispersion of the metal octylate compound has low viscosity and low density, the proportion of shock waves consumed when exciting the methanol dispersion of the metal octylate compound is small, and most of the impact energy is efficiently and repeatedly transmitted to the collection of flake powder. Also, as described above, the weight of one flake powder is extremely light. Therefore, even if the flake powder has flat surfaces overlapping each other in a complex manner, when a shock wave is applied to the flake powder, the flake powder is reliably separated into individual flake powder sheets, and the methanol dispersion of the metal octylate compound contacts the surface of all the flake powder regardless of the material, shape, and particle size distribution of the flake powder. In addition, the surfaces of the flake powder are all hydrophobic and do not react with the methanol dispersion of the metal octylate compound, and the methanol dispersion of the metal octylate compound contacts the surface of the flake powder. Thirdly, the container has three directions: left and right, front and back, and top and bottom. Impact force Repeatedly add, and finally add Impact force At this time, since the methanol dispersion of the metal octylate compound has low viscosity and low density, and each flake powder is extremely light, the methanol dispersion of the metal octylate compound is mixed with the flake powder. impact It moves repeatedly in the direction of acceleration. When this phenomenon is repeated in three directions, left and right, front and back, and up and down, the soft magnetic flaky powder rearranges with the flat surfaces facing up, and the flat surfaces overlap each other, a phenomenon that progresses in the methanol dispersion of the metal octylate compound. As a result, the flake powder spreads over the entire bottom surface of the container, and a collection of flat powder with overlapping flat surfaces is formed on the bottom surface of the container as the shape of the bottom surface through the methanol dispersion of the metal octylate compound. Fourth, the flake powder separated into individual pieces is stacked with the flat surfaces of the flake powder interposed between them via a methanol dispersion of a metal octylate compound, so the larger the aspect ratio of the flake powder is, the less flake powder is used. Therefore, even if the flake powder is expensive, the amount of flake powder used is small, so a sheet made of a collection of flake powder can be produced inexpensively. Fifth, the flat surfaces of the flake powder are overlapped with each other through a methanol dispersion of the metal octylate compound, and methanol is evaporated from the flake powder collection, and a collection of fine crystals of the metal octylate compound is precipitated in the gaps between the flat surfaces and on the surface of the flake powder collection. Furthermore, the entire surface of the flake powder collection is evenly compressed. As a result, the fine crystals are crushed to about 1 / 5 of their original size, and the crushed crystal collections are overlapped and accumulated at high density in the gaps between the flat surfaces and on the surface of the flake powder collection. The crushed fine crystals of the metal octylate compound, which are about 20 nm in size, become the raw material for the collection of copper, aluminum, or nickel nanoparticles, which are about 10 nm in size, that join the flat surfaces of the flake powder. Sixth, the entire surface of the flake powder is heated while being compressed evenly, and the crushed fine crystals of the octylate metal compound are thermally decomposed. At this time, a group of copper, aluminum, or nickel nanoparticles having a size of about 10 nm are overlapped and precipitated simultaneously at high density in the gaps between the flat surfaces of the flake powder and on the surface of the flake powder. Furthermore, the entire surface of the flake powder is compressed evenly, and the group of copper, aluminum, or nickel nanoparticles precipitated at high density are bonded to the flat surfaces by frictional heat, and the copper, aluminum, or nickel nanoparticles are bonded to each other by frictional heat. In other words, because the clusters of copper, aluminum, or nickel nanoparticles are precipitated in a high density overlapping relationship, the compressed nanoparticles have difficulty moving within the cluster of nanoparticles, and frictional heat is generated at the contact points of the nanoparticles with the flat surface and at the contact points between the nanoparticles, and the bonding force generated by the frictional heat bonds the copper, aluminum, or nickel nanoparticles to the flat surface, and also bonds the copper, aluminum, or nickel nanoparticles to each other. Seventh, flake powder made of silver, copper, brass, nickel, or aluminum can be used as flat powder when manufacturing a sheet made of a collection of flake powder. That is, the thermal decomposition temperature of the octylate metal compound is 290°C in the air atmosphere. On the other hand, the softening point of any of the flat powders of silver, copper, brass, nickel, or aluminum is higher than 290°C, and none of the flake powders has low-temperature brittleness, making it possible to use them at extremely low temperatures. Therefore, a sheet made of a collection of flake powders in which the flat surfaces of the flake powders are bonded together can be used in harsh environments such as high temperatures, extremely low temperatures, vacuum, and high pressure. The thermal decomposition temperature of the octylate metal compound in a nitrogen atmosphere is 340°C, which is 50°C higher than that of the air atmosphere. On the other hand, among flake powders made of metals or alloys, the softening point of aluminum is the lowest at 350°C. Therefore, even if the octylate metal compound is thermally decomposed in a nitrogen atmosphere, the aluminum does not soften. Eighth, the flat surfaces of the flake powder are joined together with a collection of copper, aluminum, or nickel nanoparticles. Both copper and aluminum are metals that have excellent electrical conductivity and thermal conductivity among metals and alloys. Therefore, the copper or aluminum nanoparticles do not inhibit the electrical conductivity and thermal conductivity of the flake powder made of a metal or alloy in a sheet in which the flat surfaces of the flake powder are joined together. In addition, the nickel or aluminum nanoparticles have transparency. Therefore, the nickel or aluminum nanoparticles do not lose the color and luster inherent to the flake powder made of a metal or alloy in a sheet in which the flat surfaces of the flake powder are joined together. Ninth, the metal octylate compound is a general-purpose industrial chemical. Also, since the flat surfaces of the flake powder are bonded together, the amount of flake powder used is small. Furthermore, all eight processes for bonding the flat surfaces together with a collection of copper, aluminum, or nickel nanoparticles are simple processes. Therefore, a sheet made of a collection of flake powder can be manufactured using inexpensive materials at low cost. The sheet made of an aggregate of flake powder produced by the eight processes described above provides the following effects. First, in a group of flake powders made of metals or alloys, 6-8 nanoparticles of copper, aluminum, or nickel with a size of about 10 nm are stacked to bond the flat surfaces of the flake powders together. Since the size of the nanoparticles is two orders of magnitude smaller than the particle size of the flake powder, the properties of the flake powder are dominant in the sheet. In addition, both copper and aluminum are metals with excellent electrical conductivity and thermal conductivity among metals and alloys. Therefore, the bonding layer formed by the group of nanoparticles does not inhibit the electrical conductivity and thermal conductivity of the flake powder made of metals or alloys in the sheet made of the flake powder. In addition, nickel or aluminum nanoparticles have excellent transparency. Therefore, the bonding layer formed by the group of nanoparticles does not lose the inherent color and luster of the flake powder of metals or alloys in the sheet made of the flake powder. Secondly, since the sheet is formed on the bottom surface of the container in the shape of the bottom surface, there are no restrictions on the area and shape of the sheet. In addition, the above-mentioned eight processes are possible for all flake powders made of metals or alloys, regardless of differences in the flatness, shape, and particle size distribution of the flake powders. Therefore, for all flake powders made of metals or alloys, a sheet can be produced in which the flat surfaces of the flake powders are bonded together with a collection of nanoparticles of copper, aluminum, or nickel. Therefore, the sheet production method of this sheet can be used for flake powders made of metals or alloys to form a sheet made of a collection of flake powders with versatility. As explained above, the sheet made of the flake powder produced by this production method can be formed into a sheet with a large area using a small amount of flake powder. This sheet has excellent electrical and thermal conductivity, and has the color and gloss unique to the flake powder, and can also be used as an antistatic sheet, an electromagnetic wave shielding sheet, or a sheet with an excellent surface lubricity.

[0026] Surface reflectance and total light transmittance are explained below. When light enters a substrate, surface reflection occurs depending on the difference in refractive index between air and the substrate. Therefore, even transparent glass experiences loss due to surface reflection, and the total light transmittance does not reach 100%. Incidentally, for a 2mm thick float glass, the total light transmittance is about 90% in the visible light wavelength range. The surface reflectance R of the surface of light that enters the substrate perpendicularly is calculated by Equation 2, which consists of the refractive index n of the substrate and the refractive index m of air. The total light transmittance T is calculated by Equation 3, which consists of the surface reflectance R. Therefore, when the refractive index of the metal is 0.4, the total light transmittance entering the conductive layer is 67%, and when the refractive index of the metal is 2.4, the total light transmittance entering the conductive layer is 69%, and more than 70% of the visible light enters the conductive layer. (Number 2) R = (n-m) 2 / (n+m) 2 (Number 3) T = (1-R) 2

[0027] Next, the scattering of light is explained. When visible light is irradiated onto a collection of particles, the Rayleigh scattering formula shown in Equation 4 can be applied to the scattering of light. In Equation 4, S is the scattering coefficient, which means the ratio of scattering, λ is the wavelength of visible light, D is the particle diameter, m is the refractive index of the particle, and π is the circular constant. Therefore, the magnitude of the scattering coefficient S depends on the fourth power of the ratio D / λ of the particle diameter D to the wavelength λ of visible light, and also depends on the square of the particle diameter D and the refractive index m. Since the size D of the nanoparticles is nearly two orders of magnitude smaller than the wavelength λ of visible light, the ratio D / λ is small, and the particle diameter D is also sufficiently small. Furthermore, the refractive index m of the metal is 0.4 or more and 2.4 or less. Therefore, the scattering coefficient S is extremely small, and the conductive layer exhibits high transparency. (Number 4) S=4 / 3·π 5 / λ 4 D 6 {(m 2 -1) / (m 2 +1)} 2

[0028] The method for producing a sheet made of an aggregate of flat powder described in paragraph 18 is a method for producing a sheet made of an aggregate of insulating flat powder made of a metal oxide or an inorganic compound, and the method for producing a sheet made of an aggregate of insulating flat powder made of a metal oxide or an inorganic compound is as follows: The flat powder described in paragraph 18 is glass, alumina or hematite. 1 type The insulating flat powder is made of a metal oxide or an inorganic compound, and the organometallic compound described in paragraph 18 is made of the metal oxide or The above A complex made of a metal carboxylate compound that precipitates an insulating metal oxide having a hardness lower than that of the insulating flat powder made of an inorganic compound by thermal decomposition, 1 type The present invention relates to a method for producing a sheet comprising an assembly of flat powders, the method comprising the steps of: using an insulating flat powder comprising a metal oxide or an inorganic compound comprising the above-mentioned material as the flat powder described in paragraph 18; using a complex comprising a metal carboxylate compound as the organometallic compound described in paragraph 18; and manufacturing the sheet comprising the assembly of flat powders described in paragraph 18 by using the above-mentioned metal oxide or The above The flat surfaces of insulating flat powder made of inorganic compounds are bonded to each other. Applicable A method for producing a sheet made of an assembly of insulating flat powder made of a metal oxide or an inorganic compound, the insulating flat powder being bonded via an assembly of nanoparticles made of an insulating metal oxide having a hardness lower than that of the insulating flat powder, and a method for producing a sheet made of an assembly of insulating flat powder made of a metal oxide or an inorganic compound. 。

[0029] First, the insulating flat powder made of a metal oxide or an inorganic compound used in the present invention will be described. The electrical resistivity of the flat powder made of glass and alumina is 10 14 It has a high insulating property of more than Ωcm. Therefore, if the flat surfaces of flat powders made of these metal oxides or inorganic compounds are joined together with a collection of nanoparticles made of insulating metal oxides, an insulating sheet with extremely high insulating resistance is formed. The main components of glass are silicon dioxide and boron oxide, and since silicon and boron are semi-metallic elements, silicon dioxide and boron oxide are inorganic compounds. Other components include metal oxides such as alumina, lead oxide, sodium oxide, potassium oxide, and calcium oxide. For this reason, glass consists of a mixture of metal oxides and inorganic compounds. Of the glass flake powders, only soda-lime glass has a low insulating property of 10 12 The electrical resistivity of hematite (a substance made of the alpha phase of ferric oxide Fe2O3) is 10 8 However, if the thickness of the hematite flakes is submicron and the cross-sectional area of ​​the flakes is 0.3 μm × 10 μm, the electrical resistance per unit length of the flakes is 3.3 × 10 16Ω / cm. The electrical resistance of the sheet in which the flat surfaces of the hematite powder are joined together by a collection of nanoparticles made of insulating metal oxide forms an insulating sheet with extremely large insulation resistance. That is, the collection of nanoparticles made of an extremely large number of insulating metal oxides that join the flat surfaces of the hematite powder forms an electrical resistance in which the collection of nanoparticles made of insulating metal oxides are connected in series. In addition, the flat powder in which the flat surfaces of the hematite are joined together through this collection of nanoparticles has an electrical resistance in which the electrical resistance of the flat powder and the electrical resistance of the collection of nanoparticles are connected in parallel. When the flat powder connected through such a collection of nanoparticles forms a sheet with a huge number of flat powders, the flat powder forms an electrical parallel connection and a series connection and is joined, so that the sheet made of the collection of flat powder in which the flat powder of hemite is joined together through a collection of nanoparticles made of insulating metal oxide becomes an insulating sheet with extremely large insulation resistance. Similarly, a sheet made by bonding flat powders made of glass or alumina together via a collection of nanoparticles made of insulating metal oxide also becomes an insulating sheet with extremely high insulation resistance. Incidentally, flat powder of hematite is a red pigment called red iron oxide, and is a general-purpose flat powder. As explained above, flat powder made of glass, alumina or hematite is an excellent raw material for an insulating sheet having extremely high insulation resistance. Here, the characteristics of the insulating flat powder made of glass, alumina, and hematite will be described. Glass flake powder has an average thickness of 2-5μm and a particle size of 10-4000μm. Fine flake powder with an average thickness of 0.4-1.0μm is also available. The Mohs hardness is 5-6. The glass material is C glass or E glass. Flat powder made of alumina is produced by heating scaly flat powder of boehmite, an alumina hydrate, to 500℃ or higher. Three types of flat powder with an aspect ratio of 20-40 and average particle sizes of 2μm, 5μm, and 9μm are available. The specific gravity is 3.98g / cm 3 The Mohs hardness is high at 9. The specific gravity of the flat powder made of hematite is 5.2 g / cm3 Flat powders with an average particle size of 10-20μm and an average particle thickness of 0.1-0.4μm are commercially available. The Mohs hardness is 5.5. Even E-glass flat powder, which has an extremely large particle size of 4000μm and a relatively thick thickness of 2μm, weighs only 1.7×10 -6 g. On the other hand, when an excessive compressive stress is applied to the flat surfaces of insulating flat powder, the flat powder does not undergo plastic deformation and undergoes brittle fracture. For this reason, when joining flat surfaces with a collection of insulating nanoparticles made of metal oxide, the thinner the flat powder is, the more likely it is to undergo brittle fracture. Therefore, the nanoparticles are made of a metal oxide whose hardness is lower than that of the flat powder, so that excessive compressive stress is not applied to the flat surfaces when the collection of nanoparticles comes into contact with the flat surfaces. Here, the hardness of metal oxides will be described. The hardness of metal oxide particles increases in the order of aluminum oxide Al2O3, silicon oxide SiO2, tin oxide SnO2, chromium oxide Cr2O3, magnesium oxide MgO, and titanium oxide TiO2. Furthermore, the hardness increases in the order of manganese oxide MnO2, copper oxide CuO, nickel oxide NiO, and zinc oxide ZnO. Therefore, the nanoparticles that bond the flat glass powders together may be made of insulating metal oxides that are lower in hardness than tin oxide and have a Mohs hardness lower than 5. Furthermore, the nanoparticles that bond the flat alumina powders together may be made of insulating metal oxides that are lower in hardness than aluminum oxide and have a Mohs hardness lower than 9. Furthermore, the nanoparticles that bond the flat hematite powders together may be made of insulating metal oxides that are lower in hardness than chromium oxide and have a Mohs hardness lower than 5.5. Next, a complex made of a metal carboxylate compound that precipitates a metal oxide by thermal decomposition will be described. When a complex made of a metal carboxylate compound is heat-treated in an air atmosphere at a temperature of 180-330°C, it precipitates a metal oxide. On the other hand, among flat powders made of glass, alumina, or hematite, the flat powder with the lowest softening point is glass flat powder, and further, the softening point of glass, which has the lowest softening point among flat powders of glass, is 355°C. Therefore, the thermal decomposition temperature of a complex made of a metal carboxylate compound is lower than the softening point of flat powder made of glass, alumina, or hematite. In addition, a complex made of a metal carboxylate compound disperses in methanol and does not dissolve in methanol. Therefore, a complex made of a metal carboxylate compound can be used as the organometallic compound described in paragraph 18. That is, the carboxylate anion of carboxylic acid (R-COO - A complex consisting of a carboxylate metal compound in which the ligand approaches and coordinates with a metal ion is formed by bonding the carboxylate anion (R-COO - ) approach each other and form a coordinate bond, shortening the distance between them. This allows the carboxylate anion (R-COO - ) is at the longest distance from the ion covalently bonded to the opposite side of the metal ion. When the boiling point of the carboxylic acid is exceeded, the carboxylate anion (R-COO - ) is first broken at the bond with the ion covalently bonded on the opposite side of the metal ion, and decomposed into a metal oxide, which is a compound of a metal ion and an oxygen ion, and a carboxylic acid. If the temperature is further increased, the carboxylic acid absorbs the heat of vaporization and vaporizes, and the vaporization of the carboxylic acid proceeds according to the molecular weight of the carboxylic acid and the number of carboxylic acids in the coordinate bond. When the vaporization is complete, the metal oxide is precipitated and the thermal decomposition is completed. Metal carboxylate compounds with these molecular structural characteristics include, in order of decreasing thermal decomposition temperature, metal acetate compounds, metal caprylate compounds, metal benzoate compounds, and metal naphthenate compounds. Complexes made of these metal carboxylate compounds decompose thermally in air at temperatures between 180-330°C, depending on the boiling point of the carboxylic acid. In other words, the boiling point of acetic acid is 118°C, that of caprylic acid is 237°C, and that of benzoic acid is 249°C. On the other hand, naphthenic acid is a mixture of saturated fatty acids with five-membered rings, and has the general formula C n H 2n-1 It is represented by COOH, and its main component is CH with a boiling point of 268°C and a molecular weight of 170. 17 It is composed of COOH. Therefore, the thermal decomposition temperature of metal naphthenate compounds is high at 330°C among complexes composed of metal carboxylate compounds. Therefore, metal acetate compounds, metal caprylate compounds, metal benzoate compounds, or metal naphthenate compounds can be used as the organometallic compounds described in paragraph 17. In addition, flat powders composed of glass, alumina, or hematite are inorganic compounds composed of metal oxides or semimetal oxides, so they do not oxidize even when heated to 330°C in the air. On the other hand, among the metal acetate compounds, there are metal acetate compounds that dissolve in methanol. There are also metal acetate compounds that precipitate amorphous metal oxides by thermal decomposition. The composition of the amorphous metal oxides is not constant. Such metal acetate compounds cannot be used as raw materials for metal oxide fine particles. Furthermore, among the metal acetate compounds or metal caprylic acid compounds, there are metal acetate compounds or metal caprylic acid compounds that precipitate amorphous metal oxides by thermal decomposition. Such metal acetate compounds or metal caprylic acid compounds cannot be used as raw materials for metal oxide fine particles. Furthermore, among the metal acetate compounds, metal caprylic acid compounds, and metal benzoic acid compounds, oxygen ions approach metal ions and form coordinate bonds to form binuclear complex salts, but there are metal acetate compounds, metal caprylic acid compounds, and metal benzoic acid compounds that are unstable substances during the thermal decomposition and are difficult to handle during the thermal decomposition. Among such metal carboxylate compounds, metal naphthenic acid compounds are used as raw materials for insulating metal oxide fine particles. Therefore, depending on the substance that precipitates by thermal decomposition, a complex made of a metal carboxylate compound is used as the raw material for the microcrystals. Furthermore, complexes made of metal carboxylate compounds are inexpensive industrial chemicals that can be easily synthesized. That is, when a carboxylic acid is reacted with a strong alkali, an alkali metal carboxylate compound is produced. When the alkali metal carboxylate compound is then reacted with an inorganic metal compound, a complex made of metal carboxylate compounds made of various metals is synthesized. In addition, the raw material carboxylic acid is an inexpensive organic acid. Therefore, it is the cheapest organometallic compound among all organometallic compounds. Here, the effects of using a flat powder made of glass, alumina or hematite as the flat powder described in paragraph 18, changing the metal or metal oxide nanoparticles described in paragraph 18 to nanoparticles made of insulating metal oxide having a hardness lower than that of the flat powder, and producing a sheet consisting of a collection of flat powders according to the method of producing a sheet consisting of a collection of flat powders described in paragraph 18 are described. First, the material that bonds the flat surfaces of the flat powder is a collection of insulating metal oxide nanoparticles with a hardness lower than that of the flat powder, and then a complex made of a metal carboxylate compound, which is the raw material for the nanoparticles, is dispersed in methanol to create a liquid phase. Because this liquid has low viscosity and density, by continuously carrying out the second and third processes, it becomes possible to interpose the methanol dispersion of the complex made of a metal carboxylate compound between the gaps between the flat surfaces of the flat powder that have been separated into individual sheets. Secondly, the homogenizer is operated in the container, and shock waves are repeatedly generated by the homogenizer. On the other hand, since the methanol dispersion of the complex made of the carboxylic acid metal compound has a low viscosity and a low density, the proportion of shock waves consumed when exciting the methanol dispersion of the complex made of the carboxylic acid metal compound is small, and most of the shock energy is efficiently and repeatedly transmitted to the collection of flat powder. In addition, as described above, the weight of one flat powder is extremely light. Therefore, even if the flat powder has flat surfaces overlapping each other in a complex manner, when a shock wave is applied to the flat powder, it is reliably separated into individual flat powder sheets. As a result, regardless of the material, shape, and particle size distribution of the flat powder, the methanol dispersion of the complex made of the carboxylic acid metal compound contacts the surface of all the flat powder. In addition, the flat surfaces of all the flat powders are hydrophobic and do not react with the methanol dispersion of the complex made of the carboxylic acid metal compound, and the methanol dispersion of the complex made of the carboxylic acid metal compound contacts the flat surfaces. Thirdly, the container has three directions: left and right, front and back, and top and bottom. Impact force Repeatedly add, and finally add Impact force At this time, since the methanol dispersion of the complex made of the carboxylic acid metal compound has low viscosity and low density, and each flat powder is extremely light, the methanol dispersion of the complex made of the carboxylic acid metal compound is mixed with the flat powder. impactIt moves repeatedly in the direction of acceleration. When this phenomenon is repeated in three directions, left and right, front and back, and up and down, the flat powder rearranges and overlaps with the flat surface facing up in the methanol dispersion of the complex made of the carboxylate metal compound. As a result, the flat powder spreads over the entire bottom surface of the container, and a collection of flat powder with flat surfaces overlapping each other through the methanol dispersion of the complex made of the carboxylate metal compound forms the shape of the bottom surface of the container. Fourth, the flat powder separated into individual pieces is stacked on top of each other with the flat surfaces of the flat powder interposed between them via a methanol dispersion of a complex made of a carboxylate metal compound, so the larger the aspect ratio of the flat powder, the less the amount of flat powder used. Therefore, even if the flat powder is expensive, the amount of flat powder used is small, so a sheet made of a collection of flat powder can be produced inexpensively. Fifth, methanol is evaporated from the flat powder collection in which the flat surfaces of the flat powder are stacked together through a methanol dispersion of a complex made of a metal carboxylate compound, and a collection of fine crystals of the complex made of a metal carboxylate compound is precipitated in the gaps between the flat surfaces and on the surface of the collection of flat powder. Furthermore, the entire surface of the collection of flat powder is evenly compressed. As a result, the fine crystals are crushed to about 1 / 5 of their original size, and the crushed crystals are piled up and accumulated at high density in the gaps between the flat surfaces and on the surface of the collection of flat powder. The crushed fine crystals of the complex made of a metal carboxylate compound, which are about 20 nm in size, become the raw material for the collection of metal oxide nanoparticles, which are about 10 nm in size, that connect the flat surfaces of the flat powder. Sixth, the entire surface of the flat powder is heated while being compressed evenly, and the fine crystals of the complex made of the crushed carboxylate metal compound are thermally decomposed. At this time, a collection of nanoparticles of metal oxides having a size of about 10 nm is overlapped and precipitated simultaneously at high density in the gaps between the flat surfaces of the flat powder and on the surface of the flat powder collection. Furthermore, the entire surface of the flat powder collection is compressed evenly, and the collection of metal oxide nanoparticles precipitated at high density are bonded to the flat surfaces by frictional heat, and the metal oxide nanoparticles are bonded to each other by frictional heat. In other words, since the collection of metal oxide nanoparticles is overlapped and precipitated at high density, it becomes difficult for the compressed nanoparticles to move in the nanoparticle collection, and frictional heat is generated at the contact points of the nanoparticles in contact with the flat surfaces and at the contact points between the nanoparticles, and the metal oxide nanoparticles are bonded to the flat surfaces by the bonding force due to the frictional heat, and the metal oxide nanoparticles are bonded to each other by the bonding force due to the frictional heat. In addition, since the nanoparticles are composed of insulating metal oxides having a hardness lower than that of the flat powder, when the nanoparticles contact the flat surface, the contact portion of the nanoparticles is preferentially elastically deformed very slightly, and excessive compressive stress is not applied to the flat surface. Therefore, the flat powder does not break brittle. In addition, when the nanoparticles contact each other, the contact portion of the nanoparticles is elastically deformed very slightly, and excessive compressive stress is not applied to the contact portion of the nanoparticles. Therefore, the collection of nanoparticles is not destroyed. In addition, when the entire surface of the collection of flat powder is compressed, the nanoparticles are bonded to the flat surface by frictional heat, and after the nanoparticles are bonded to each other by frictional heat, if further compressive stress is applied to the collection of flat powder, a repulsive force is generated in the plate material to which the compressive stress is applied, since the nanoparticles are miniaturized to the limit size, and at this point, the compressive stress applied to the collection of flat powder is stopped. Seventh, the flat powder made of glass, alumina or hematite can be used as the flat powder when manufacturing a sheet made of a collection of flat powders. That is, the thermal decomposition temperature of the complex made of a carboxylate metal compound is 330°C, which is the highest temperature of the air atmosphere. On the other hand, among the flat powders made of glass, alumina or hematite, the flat powder with the lowest softening point is the flat powder of glass, and further, the softening point of glass, which has the lowest softening point among the flat powders of glass, is 355°C. Therefore, the thermal decomposition temperature of the complex made of a carboxylate metal compound is lower than the softening point of the flat powder. For this reason, a sheet made of a collection of flat powders in which the flat surfaces of the flat powders are joined together can be used in harsh environments such as high temperatures, extremely low temperatures, vacuum, and high pressure. Incidentally, among the flat powders made of glass, alumina or hematite, the flat powder with the lowest melting point is the flake powder of glass, and the melting point of the flake powder of glass is high, at 1200°C or higher. In addition, even if a sheet made of a collection of flat powder is heated above the softening point of the flat powder, as long as no stress that deforms the flat powder is applied to the sheet, the sheet made of a collection of flat powder will retain its original properties when the sheet made of a collection of flat powder is returned to its original temperature. For this reason, a sheet made of a collection of flat powder can be used at very high temperatures. In addition, the metal oxide with the lowest melting point among metal oxides and nanoparticles is tin oxide, which has a melting point of 1630°C. Eighth, the flat surfaces of the flat powder are joined together by a collection of insulating metal oxide nanoparticles. The collection of nanoparticles made of an extremely large number of insulating metal oxides that join the flat surfaces of the flat powder together forms an electrical resistance in which the collection of nanoparticles made of insulating metal oxides are connected in series. In addition, the flat powder in which the flat surfaces are joined together through the collection of nanoparticles has an electrical resistance in which the electrical resistance of the flat powder and the electrical resistance of the collection of nanoparticles are connected in parallel. When the flat powder connected through such a collection of nanoparticles forms a sheet with a huge number of flat powders, the flat powders form electrical parallel and series connections and are joined, so that the sheet made of the collection of flat powders becomes an insulating sheet with an extremely large insulation resistance. Ninth, the complex made of a metal carboxylate compound is a general-purpose industrial chemical. In addition, since the flat surfaces of the flat powder are bonded together, the amount of flat powder used is small. Furthermore, all eight processes for bonding the flat surfaces together with a collection of metal oxide nanoparticles are simple. Therefore, an insulating sheet with high insulation resistance made of a collection of flat powder can be manufactured using inexpensive materials at low cost. The sheet made of the flake powder described above provides the following effects. First, in a group of flat powders made of glass, alumina, or hematite, 6-8 insulating metal oxide nanoparticles, which have a hardness lower than that of the flat powder, are stacked on top of each other to bond the flat surfaces of the powder. Since the size of the nanoparticles is more than two orders of magnitude smaller than the particle size of the flat powder, the properties of the sheet are dominated by the properties of the flake powder. In addition, the bonding layer formed by the group of nanoparticles forms an insulating layer with high insulation resistance. Therefore, in a sheet made of a group of insulating flat powders, the metal oxide nanoparticles contribute to further increasing the insulation resistance of the sheet. Secondly, since the sheet is formed on the bottom surface of the container in the shape of the bottom surface, there are no restrictions on the area and shape of the sheet. In addition, the above-mentioned eight processes are possible for all flat powders made of glass, alumina or hematite, regardless of the flatness, shape, and particle size distribution of the flat powder, so that for all flat powders, a sheet can be produced in which the flat surfaces of the flat powder are bonded together with a collection of nanoparticles made of insulating metal oxide. Therefore, the manufacturing method of this sheet can form an insulating sheet with high insulation resistance made of a collection of flat powders with versatility for flat powders made of glass, alumina or hematite. As described above, the sheet made of the aggregate of flat powder produced by the present production method can be formed into a sheet with a large area using a small amount of flat powder. This sheet becomes an insulating sheet with high insulation resistance.

[0030] The method for producing a sheet consisting of a collection of flat powder described in paragraph 18 is a method for producing a sheet consisting of a collection of inorganic luster pigments in which the surface of flat powder consisting of glass or aluminum is covered with a coating consisting of a metal or a metal oxide, and the method for producing a sheet consisting of a collection of inorganic luster pigments is as follows: A method for producing a sheet consisting of an aggregate of inorganic luster pigments, the flat powder described in paragraph 18 being an inorganic luster pigment in which the surface of a flat powder consisting of glass or aluminum is coated with a coating consisting of a metal or a metal oxide, and the organometallic compound described in paragraph 18 being aluminum octylate which is precipitated by thermal decomposition of aluminum, the method for producing a sheet consisting of an aggregate of inorganic luster pigments comprising using the inorganic luster pigment as the flat powder described in paragraph 18 and using the aluminum octylate as the organometallic compound described in paragraph 18, and producing a sheet consisting of an aggregate of inorganic luster pigments in which the flat surfaces of the inorganic luster pigments are bonded to each other via aggregates of nanoparticles consisting of aluminum, according to the method for producing a sheet consisting of an aggregate of inorganic luster pigments described in paragraph 18. 。

[0031] First, an inorganic bright pigment in which the surface of a flat powder made of glass or aluminum used in the present invention is coated with a film made of a metal or a metal oxide will be described. There are inorganic luster pigments with excellent luster, in which the surface of flat powder made of glass or aluminum is coated with metals such as gold, silver, or nickel, or metal oxides such as titanium oxide or iron oxide, by electroless plating. Luster pigments made of glass flake powder coated with titanium oxide are commercialized as luster pigments that reflect five colors, white, yellow, red, blue, and green, depending on the thickness of the titanium oxide coating on glass flake powder with a plate thickness of 1 μm and an average particle size of 20-80 μm. In addition, luster pigments that reflect silver are commercialized by coating the surface of glass flake powder with a plate thickness of 1 to 5 μm and an average particle size of 25-480 μm with a silver coating. Furthermore, a glittering pigment made of glass flake powder coated with iron oxide (hematite made of α-Fe2O3) has been commercialized as a glittering pigment that reflects five colors, yellow, bronze, copper, and russet, depending on the thickness of the iron oxide coating on the glass flake powder with a plate thickness of 1 μm and an average particle size of 30 μm and 80 μm. A glittering pigment that reflects gold has been commercialized as a glittering pigment made of glass flake powder with a plate thickness of 1 μm and an average particle size of 30 μm and 80 μm, coated with a gold coating. Furthermore, a glittering pigment made of aluminum flat powder coated with titanium oxide has been commercialized as a glittering pigment that reflects four colors, yellow, red, orange, and green, depending on the thickness of the titanium oxide coating, just like the glittering pigment made of glass flake powder coated with titanium oxide. The weight of the flat powder of these inorganic glittering pigments is extremely light in all cases. If the flat surfaces of the inorganic luster pigment flake powder can be joined together with a transparent material without damaging the coating made of metal or metal oxide, a sheet made of an aggregate of inorganic luster pigment flake powder can be created without losing the color reflected from the luster pigment. Furthermore, if multiple types of luster pigments that reflect different colors are used and the flat surfaces of the multiple types of luster pigment flake powder can be joined together with a transparent material, the color tone emitted by the aggregate of the multiple types of luster pigment flake powder can be changed to various colors by combining multiple types of luster pigments. Such transparent nanoparticles include the nickel and aluminum nanoparticles described in paragraph 25. In an aggregate of aluminum nanoparticles, part of the light rays that make up visible light are reflected by the surface of the aggregate of aluminum nanoparticles, and the color corresponding to this light is emitted, but the aggregate of aluminum nanoparticles has transparency. In an aggregate of nickel nanoparticles, nickel The cluster of nanoparticles is nearly colorless and transparent. The cluster of nanoparticles made of aluminum or nickel maintains its transparency and bonds the flat surfaces of the inorganic luster pigment flake powder together. Therefore, the color reflected by the inorganic luster pigment is not lost. Next, the material of the nanoparticles that bond the flat surfaces of the flat powder of the inorganic bright pigment will be described. The coating that covers the surface of the flat powder made of glass or aluminum is made of metals such as gold, silver, and nickel, or metal oxides such as titanium oxide and iron oxide. Among the substances that form these coatings, gold has the lowest hardness, with a Mohs hardness of 2.5, and silver has a Mohs hardness of 2.7. Titanium oxide has a Mohs hardness of 5.5-6, and hematite has a Mohs hardness of 5.5. In contrast, aluminum has a Mohs hardness of 2.9, and nickel has a Mohs hardness of 3.5. On the other hand, the Young's modulus is 78 GPa for gold, 82.7 GPa for silver, 69 GPa for aluminum, 204 GPa for nickel, 300 GPa for titanium oxide, and 160 GPa for hematite. By the way, when a collection of nanoparticles contacts the flat surface of a flat powder covered with a metal or metal oxide coating, the nanoparticles are small, about 10 nm, but the thickness of the flake powder, which is the thinnest among the flat powders, is 100 times the size of the nanoparticles, and the area of ​​the flat powder with the smallest surface area is 2000 times the size of the nanoparticles. Therefore, the contact area where the nanoparticles contact the flat surface of the flat powder is extremely small. In addition, the contact area between the nanoparticles is also extremely small. On the other hand, gold, silver, and aluminum are soft metals with excellent ductility and malleability. For this reason, the Young's modulus of soft metals is small. Therefore, when the gold or silver coating comes into contact with the nanoparticles, the localized area of ​​the contact area in the gold or silver coating is elastically deformed. At this time, frictional heat is generated at the localized area of ​​the contact area. On the other hand, if the nanoparticles are made of aluminum, aluminum is also a soft metal with a small Young's modulus, so the localized area of ​​the contact area in the nanoparticles is elastically deformed. At this time, frictional heat is generated at the localized area of ​​the contact. The gold or silver coating and the aluminum nanoparticles are bonded by the frictional heat between the two. In addition, the Mohs hardness of nickel is higher than that of aluminum, and the Young's modulus of nickel is higher than that of aluminum. Therefore, when the nanoparticles are subjected to stress, the aluminum nanoparticles are more likely to elastically deform than the nickel nanoparticles. For this reason, when the flat surfaces of flat powders covered with a nickel coating are bonded together with a collection of aluminum nanoparticles, the localized area of ​​the contact in the nanoparticles is preferentially elastically deformed. At this time, frictional heat is generated at the localized area of ​​the contact.In contrast, localized areas of the contact area in the nickel coating generate heat without elastic deformation. The frictional heat between the two bonds the nickel coating and the aluminum nanoparticles. Furthermore, in the case of a coating made of titanium oxide or iron oxide, like the coating made of nickel, when flat surfaces of flat powders covered with a coating of titanium oxide or iron oxide are bonded with a collection of aluminum nanoparticles, localized areas of the contact area in the nanoparticles are preferentially elastically deformed. At this time, frictional heat is generated at localized areas of the contact area. In contrast, localized areas of the contact area in the coating of titanium oxide or iron oxide generate heat without elastic deformation. The frictional heat between the two bonds the coating of titanium oxide or iron oxide and the aluminum nanoparticles. Note that when flat surfaces of flat powders covered with a coating of titanium oxide or iron oxide are bonded with a collection of nickel nanoparticles, the Young's modulus of nickel is greater than that of aluminum, and is also greater than that of iron oxide, so the amount of elastic deformation in the nickel nanoparticles is smaller than the amount of elastic deformation in the aluminum nanoparticles. For this reason, the possibility of damaging the iron oxide coating cannot be denied. Therefore, when bonding flat surfaces of flat powders made of glass or aluminum together via a collection of nanoparticles without damaging the coating made of metal or metal oxide, it is preferable to bond them using a collection of transparent aluminum nanoparticles that have low hardness and a small Young's modulus. Here, the effects of using a flat powder of an inorganic lustrous pigment as the flat powder described in paragraph 18, changing the metal or metal oxide nanoparticles described in paragraph 18 to aluminum nanoparticles, and producing a sheet consisting of a collection of flat powders according to the method described in paragraph 18 will be described. First, the material that bonds the flat surfaces of the inorganic luster pigment flake powder is a collection of aluminum nanoparticles, and aluminum octylate, the raw material of the nanoparticles, is dispersed in methanol to create a liquid phase. Because this liquid has low viscosity and density, by continuously carrying out the second and third processes, it becomes possible to interpose the methanol dispersion of aluminum octylate in the gaps between the flat surfaces of the inorganic luster pigment flake powder that have been separated into individual sheets. Secondly, a homogenizer is operated in the container, and shock waves are repeatedly generated by the homogenizer. On the other hand, since the methanol dispersion of aluminum octylate has low viscosity and low density, the proportion of shock waves consumed when exciting the methanol dispersion of aluminum octylate is low, and most of the shock energy is efficiently and repeatedly transmitted to the collection of flat powder of the inorganic luster pigment. In addition, the weight of each flat powder is extremely light. Therefore, even if the flat powder has flat surfaces overlapping each other in a complex manner, when a shock wave is applied to the flat powder, it is reliably separated into individual flat powder sheets. As a result, the methanol dispersion of aluminum octylate comes into contact with the surface of the coating of all the flat powder, regardless of the material of the inorganic luster pigment flat powder, the material and thickness of the coating, the shape and particle size distribution of the flat powder. In addition, the coating on the flat surfaces of all the flat powders is hydrophobic and does not react with the methanol dispersion of aluminum octylate, and the methanol dispersion of aluminum octylate comes into contact with the coating on the flat surfaces. Thirdly, the container has three directions: left and right, front and back, and top and bottom. Impact force Repeatedly add, and finally add Impact force At this time, since the methanol dispersion of aluminum octylate has low viscosity and low density, and each flat powder is extremely light, the methanol dispersion of aluminum octylate is mixed with the flat powder. impact It moves repeatedly in the direction of acceleration. When this phenomenon is repeated in three directions, left and right, front and back, and up and down, the flat powder rearranges and overlaps with the flat surface facing up in the methanol dispersion of aluminum octylate. As a result, the flat powder of the inorganic luster pigment spreads over the entire bottom surface of the container, and a collection of flat powder of the inorganic luster pigment with the flat surfaces overlapping each other through the methanol dispersion of aluminum octylate forms the shape of the bottom surface of the container. Fourth, the flat powder separated into individual pieces is stacked with the flat surfaces of the flat powder interposed between them in a methanol dispersion of aluminum octylate, so the larger the aspect ratio of the flat powder, the less the amount of flat powder used. Therefore, even if the flat powder is expensive, the amount of flat powder used is small, so a sheet made of a collection of flat powder can be produced inexpensively. Fifth, the methanol is evaporated from the flat powder aggregate, in which the flat surfaces of the flat powder are overlapped, through a methanol dispersion of aluminum octylate, and aggregates of aluminum octylate fine crystals are precipitated in the gaps between the flat surfaces and on the surface of the aggregate of flat powder. Furthermore, the entire surface of the aggregate of flat powder is evenly compressed. As a result, the fine crystals are crushed to about 1 / 5 of their original size, and the aggregates of crushed crystals are overlapped and accumulated at high density in the gaps between the flat surfaces and on the surface of the aggregate of flat powder. These crushed aluminum octylate fine crystals, which are about 20 nm in size, become the raw material for the aggregate of aluminum nanoparticles, which are about 10 nm in size, that join the flat surfaces of the flat powder. Sixth, the entire surface of the flat powder is heated while being compressed evenly, and the crushed aluminum octylate microcrystals are thermally decomposed. At this time, a collection of aluminum nanoparticles having a size of about 10 nm is overlapped and precipitated simultaneously at high density in the gaps between the flat surfaces of the flat powder and on the surface of the flat powder collection. Furthermore, the entire surface of the flat powder collection is compressed evenly, and the collection of aluminum nanoparticles precipitated at high density are bonded to the flat surfaces by frictional heat, and the aluminum nanoparticles are bonded to each other by frictional heat. In other words, since the collection of aluminum nanoparticles is precipitated overlapping each other at high density, it becomes difficult for the compressed nanoparticles to move in the collection of nanoparticles, and frictional heat is generated at the contact points of the nanoparticles in contact with the flat surfaces and at the contact points between the nanoparticles, and the aluminum nanoparticles are bonded to the flat surfaces by the bonding force due to the frictional heat, and the aluminum nanoparticles are bonded to each other by the bonding force due to the frictional heat. In addition, since the nanoparticles are made of aluminum, which has low hardness and a small Young's modulus, when the nanoparticles contact the flat surface, the contact portion of the nanoparticles elastically deforms very slightly, and excessive compressive stress is not applied to the coating surface of the flat surface. Therefore, the coating is not damaged. In addition, when the nanoparticles contact each other, the contact portion of the nanoparticles elastically deforms very slightly, and excessive compressive stress is not applied to the contact portion of the nanoparticles. Therefore, the collection of nanoparticles is not damaged. In addition, when the entire surface of the collection of flat powder is compressed, the nanoparticles are bonded to the flat surface by frictional heat, and after the nanoparticles are bonded to each other by frictional heat, if further compressive stress is applied to the collection of flat powder, a repulsive force is generated in the plate material to which the compressive stress is applied, since the nanoparticles are miniaturized to the limit size, and at this point, the compressive stress applied to the collection of flat powder is stopped. Seventh, the inorganic luster pigment flake powder can be used as the flake powder when manufacturing a sheet consisting of a collection of flake powders. In other words, the thermal decomposition temperature of aluminum octylate is 290°C in the air. On the other hand, the heat resistance of the coating formed on the surface of the inorganic luster pigment flake powder, which is made of metals such as gold, silver, and nickel, or metal oxides such as titanium oxide and iron oxide, is significantly higher than 290°C. For this reason, a sheet consisting of a collection of flake powders in which the flat surfaces of the flake powders are bonded together can be used in harsh environments such as high temperatures, extremely low temperatures, vacuum, and high pressure. Eighth, the flat surfaces of the inorganic luster pigment flat powder are joined together by a collection of aluminum nanoparticles that are transparent, have low hardness, and have a small Young's modulus. Therefore, the flat surfaces of the inorganic luster pigment flat powder can be joined together by a collection of aluminum nanoparticles without damaging the coating made of metal or metal oxide. This makes it possible to create a sheet made of a collection of inorganic luster pigment flat powder without losing the color reflected from the luster pigment. Furthermore, by using multiple types of luster pigments that reflect different colors from each other, and joining the flat surfaces of the flat powder of the multiple types of luster pigments together by a collection of aluminum nanoparticles, the color tone emitted by the collection of flat powder of the multiple types of luster pigments can be changed to various colors by combining multiple types of luster pigments. Ninth, aluminum octylate is a general-purpose industrial chemical. Also, since the flat surfaces of the flat powder are bonded together, the amount of flat powder used is small. Furthermore, all eight processes for bonding the flat surfaces together with a collection of aluminum nanoparticles are simple processes. Therefore, a sheet made of a collection of flat powder of inorganic photoluminescent pigment can be manufactured using inexpensive materials at low cost without losing the color reflected from the photoluminescent pigment. Furthermore, when the flat surfaces of the inorganic luster pigment powder are bonded together with a collection of aluminum nanoparticles, a further effect is obtained. First, the surface of the aggregate of flat powder of the inorganic luster pigment is uneven based on the size of the nanoparticles. The total surface area of ​​the uneven surface is huge because the number of nanoparticles is enormous, and it is close to a so-called fractal surface. When a liquid droplet comes into contact with the surface of such an aggregate of flat powder of the inorganic luster pigment, the liquid cannot enter the unevenness of the nanoparticle size due to the surface tension of the droplet, and the liquid surface of the droplet comes into point contact with the protrusions of the enormous number of nanoparticles. As a result, the surface of the aggregate of flat powder of the inorganic luster pigment exhibits super water repellency with a contact angle of nearly 180 degrees, resulting in water repellency, oil repellency, and antifouling properties. Secondly, the surface of the aggregate of flat powder of the inorganic luster pigment has electrical conductivity and thermal conductivity similar to that of the aluminum that constitutes the nanoparticles, so that the aggregate of flat powder of the inorganic luster pigment has antistatic properties, electromagnetic wave shielding properties, and heat dissipation properties. As described above, the surface of the clusters of flat powder of the inorganic luster pigment is covered with clusters of aluminum nanoparticles, providing the sheet with excellent functional effects based on the size and material of the aluminum nanoparticles that cannot be obtained with inorganic luster pigments. [Brief description of the drawings]

[0032] [Figure 1] 1 is an explanatory diagram showing a schematic side view of a sheet made of a collection of flat iron powder particles in which the flat iron powder particles are directly bonded together at their opposing faces. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Example 1 In this embodiment, a flat iron powder obtained by flattening reduced iron powder is used as the soft magnetic flat powder, and a sheet is produced from a collection of reduced iron powder in which the flat surfaces of the flat iron powder are bonded together via a collection of nickel nanoparticles. The flat iron powder used is flat iron powder MG150D manufactured by JFE Steel Corporation. This flat iron powder has a large average particle size of 100 μm and an extremely thick thickness of 10-20 μm. This is because the particles of the reduced iron powder are relatively large, but the Vickers hardness of the reduced iron powder is high at 160-200 HV, making it difficult to flatten. First, nickel octylate Ni(CH 1542 g (equivalent to 0.12 moles) of nickel octoate (COO)2 (e.g., a product of Fujifilm Wako Pure Chemical Industries, Ltd.) was dispersed in methanol at a weight ratio of 10%. The methanol dispersion of nickel octoate was then filled into a container measuring 20 cm x 20 cm x 1.5 cm (depth), and 40 g of flat iron powder was added to the container. Then, ultrasonic vibrations of 20 kHz were applied to the methanol dispersion of nickel octoate in the container for 2 minutes using an ultrasonic homogenizer device (e.g., LUH300, a product of Yamato Scientific Co., Ltd.). The ultrasonic homogenizer device was then removed from the container, and a three-way vibration of 0.3 G was applied. impact Acceleration was repeatedly applied to the container to create a mass of flat iron powder in the container, with the flat surfaces of the flat iron powder overlapping each other via the methanol dispersion of nickel octylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of nickel octylate, and crystals of nickel octylate were precipitated on the surface of the flat iron powder and in the gaps between the flat surfaces of the flat iron powder. After this, a plate material measuring 20 cm x 20 cm x 2 mm (thickness) was placed on the surface of the flat iron powder, and five weights of 10 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way bending with 0.4 G. impact By applying acceleration, the collection of flat iron powder inside the container was pulled away from the container. Next, the surface and side of the sample were observed using an electron microscope. An extremely low accelerating voltage SEM from JFE Techno-Research Corporation was used as the electron microscope. This device allows surface observation at extremely low accelerating voltages starting from 100V, and has the advantage of being able to directly observe the surface of the sample without forming a conductive coating on the sample. First, the secondary electron beam between 900-1000V of the reflected electron beam was extracted and image processing was performed. Three flat surfaces of 10-20μm thick flat powder were stacked together to form a 20cm x 20cm sheet with a thickness of about 45μm. In addition, six nanoparticles with a size of about 10nm were stacked on the surface of the flat powder collection and in the gaps between the flat powder flat surfaces. Furthermore, the energy between 900-1000V of the reflected electron beam was extracted and image processing was performed, and the material was observed based on the shade of the image. Since no shade was observed, it was found that both the flat powder and the nanoparticles were formed from a single element. Next, the energy and intensity of the characteristic X-rays were image processed and the elements were analyzed. It was found that the flat powder was iron atoms and the nanoparticles were nickel atoms. Therefore, the flat iron powder collection was joined by the flat surfaces through the nickel nanoparticle collection, and the flat iron powder collection formed a sheet. The skin depth of electromagnetic waves from reduced iron powder at 100 kHz is 50 μm. For this reason, a sheet with a thickness of around 45 μm effectively absorbs electromagnetic noise at around 100 kHz using a small amount of flat powder made of reduced iron powder. Figure 1 shows a schematic of part of the side of a sheet made of a collection of flat iron powder particles bonded together at their flat surfaces via a collection of nickel nanoparticles. 1 is the flat iron powder and 2 is the nickel nanoparticle. Furthermore, the magnetic shielding performance of the prepared sheet was evaluated. For comparison, a cold-rolled steel sheet with a thickness of 45 μm was used. A shielding box with a rectangular parallelepiped shape with a side length of 100 mm was prepared using both the sheet and the cold-rolled steel sheet. The above-mentioned shielding box was placed in a Helmholtz coil placed in a magnetically shielded room, and the external magnetic field generated by the Helmholtz coil and the internal magnetic field at the center of the shielding box were measured, and the magnetic shielding performance S was evaluated using Equation 5. A magnetic sensor for measuring the magnetic field was installed in the shielding box through a hole provided in the shielding box. The sample had a magnetic shielding performance S value of 7 dB, which was about 3 dB better than that of the cold-rolled steel sheet. As a result, it was found that the prepared sheet had an excellent magnetic shielding effect. (Number 5) S=20·log((external magnetic field) / (internal magnetic field)) Next, the sheet's performance in absorbing electromagnetic noise was evaluated. A microstrip line measuring 220 mm in length, 30 mm in width, and with a characteristic impedance adjusted to 50 Ω was installed on a board, and the sheet was aligned in the length direction of the microstrip line and positioned so that their centers were aligned, creating a magnetic sheet that absorbs noise. After this, the S parameters were measured using a network analyzer (Agilent Technologies, Inc. product N5230A) connected to the microstrip line. The S parameter S due to reflection was 11 and the S-parameter S due to transmission 12 Therefore, the transmission loss in the microstrip line becomes the amount of electromagnetic wave absorption according to the following formula 6. The measurement results showed that the absorption rate was 12% at 100 kHz, 24% at 800 kHz, and 13% at 10 MHz. The sheet had an absorption rate of more than 12% in the frequency range from 100 kHz to 10 MHz. (Number 6) Reflection amount (dB)=20·log|S 11 | Transmission amount (dB)=20·log|S 12 | Absorption amount (%) = (1-|S 11 | 2 -|S 12 | 2 ) x 100

[0034] Example 2 In this embodiment, a flat permalloy powder is used as the soft magnetic flat powder, and a sheet is manufactured from a collection of flat permalloy powder in which the flat surfaces of the flat permalloy powder are bonded together via a collection of nickel nanoparticles. The flat permalloy powder is a flat permalloy powder containing 50% nickel (for example, a product developed by Sanyo Special Steel). The flatness of this flat powder is 38, and the average particle size is 14 μm. Thus, the average thickness of the flat permalloy powder is extremely thin, and the average particle size is also small. In addition, the imaginary part of the complex permeability rises sharply from around 100 MHz, has a peak value of 8.8 at 3.3 GHz, decreases from around 4 GHz, and has a value of 3.5 at 10 GHz. Therefore, in the frequency band of 1 to 8 GHz, the imaginary part of the complex permeability has a value of 5 or more. In contrast, in a direct current magnetic field, the initial relative permeability is 1×10 4 The maximum relative permeability is 1.4×10 5 and has a large value. First, 21 g (corresponding to 0.08 moles) of the nickel octylate used in Example 1 was dispersed in methanol at a weight ratio of 10%. The methanol dispersion of nickel octylate was then filled into a container measuring 12 cm x 12 cm x 2 cm (depth), and 18 g of flat permalloy powder was added to the container. Then, ultrasonic vibrations of 20 kHz were applied to the methanol dispersion of nickel octylate in the container for 2 minutes using the ultrasonic homogenizer device used in Example 1. The ultrasonic homogenizer device was then removed from the container, and three-way vibrations of 0.2 G were applied. impact Acceleration was repeatedly applied to the container, creating a mass of flat permalloy powder in the container in which the flat surfaces of the flat permalloy powder overlapped each other via a methanol dispersion of nickel octylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of nickel octylate, and crystal clusters of nickel octylate were precipitated on the surfaces of the clusters of flat permalloy powder and in the gaps between the flat surfaces of the flat permalloy powder. After this, a plate material measuring 12 cm x 12 cm x 3 cm (thickness) was placed on the surface of the clusters of flat iron powder, and five weights weighing 6 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way impact By applying acceleration, the collection of flat iron powder inside the container was pulled away from the container. Next, the surface and side of the sheet were observed with an electron microscope in the same manner as in Example 1. A material having a thickness of 0.4-0.5 μm was laminated in 10 layers via a collection of nanoparticles having a size of about 10 nm. This material was composed of nickel atoms and iron atoms, so it was permalloy. Also, the nanoparticles were composed of nickel atoms, so they were nickel nanoparticles. Since the skin depth of permalloy at 1 GHz is 5.0 μm, a sheet having a thickness of 4-5 μm effectively absorbs electromagnetic noise around 1 GHz using a small amount of flat powder made of permalloy. Furthermore, the magnetic shielding performance of the sheet was evaluated in the same manner as in Example 1. For comparison, a sheet of 5 μm thick made of permalloy containing 47% nickel was used. As in Example 1, a rectangular parallelepiped shielding box with a side length of 100 mm was created using each of the sheet and the permalloy sheet. The sample had a magnetic shielding performance S value of 40 dB, which was about 5 dB better than the 47Ni permalloy sheet. As a result, the sample provides an excellent magnetic shielding effect. Next, the sheet's electromagnetic noise absorption performance was evaluated in the same manner as in Example 1. The absorption rate was 8% at 1 GHz, 10% at 3 GHz, and 8% at 6.8 GHz. Thus, the sample had an absorption rate of 8% or more in the frequency band from 1 GHz to 7 GHz. However, the absorption rate of electromagnetic waves was low. This is due to the small average particle size of the flattened powder of permalloy and the low flatness.

[0035] Example 3 In this embodiment, flat sendust powder is used as the soft magnetic flat powder, and a sheet is produced consisting of an aggregate of flat sendust powder in which the flat surfaces of the flat sendust powder are bonded together via aggregates of nickel nanoparticles. The flat powder of sendust is a product of Sanyo Special Steel's high magnetic permeability type A, which has a relatively large average particle size of 50 μm or less, a thickness of about 1 μm, and an aspect ratio of close to 50. This flat powder contains a small amount of nickel and a reduced amount of silicon compared to conventional sendust, which makes the flattening process easier and increases the particle size of the flat powder, thereby significantly improving the complex permeability characteristics. The imaginary part of the complex permeability has a value of 60 or more in the frequency band of 10-70 MHz and a value of 30 or more in the frequency band of 3-100 MHz. Compared to the flat powder of permalloy used in Example 2, the particle size of the flat powder is larger and the thickness is also thicker. Furthermore, the aspect ratio is large, and the frequency band where the value of the imaginary part of the complex permeability exceeds 10 times the value extends to 3-100 MHz. In addition, the real part of the complex permeability has a large value of 200 at 1-3 MHz. Therefore, it is effective in suppressing electromagnetic noise in the frequency band of 3 MHz or more. On the other hand, the magnetic permeability in a DC magnetic field is two orders of magnitude smaller than that of the permalloy used in Example 2, so the magnetic shielding effect is low. The skin depth of the flat sendust powder at 3 MHz is 20 μm. First, 42 g (equivalent to 0.12 moles) of the nickel octylate used in Example 1 was dispersed in methanol at a weight ratio of 10%. The flat powder of sendust is thicker and has a larger average particle size than the flat permite. The methanol dispersion of nickel octylate was then filled into a container measuring 20 cm x 20 cm x 1.5 cm (depth), and 40 g of flat sendust powder was added to the container. Then, ultrasonic vibrations of 20 kHz were applied to the methanol dispersion of nickel octylate in the container for 2 minutes using the ultrasonic homogenizer device used in Example 1. The ultrasonic homogenizer device was then removed from the container, and three-directional vibrations of 0.3 G were applied. impact Acceleration was repeatedly applied to the container, and a mass of the flat sendust powder was formed in the container in which the flat surfaces of the flat sendust powder were overlapped with each other via the methanol dispersion of nickel octylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of nickel octylate, and crystal clusters of nickel octylate were precipitated on the surface of the cluster of flat sendust powder and in the gaps between the flat surfaces of the flat sendust powder. After this, a plate material measuring 20 cm x 20 cm x 2 mm (thickness) was placed on the surface of the cluster of flat sendust powder, and five weights each weighing 8 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way bending with 0.4 G. impact Acceleration was applied, causing the mass of flat Sendust powder inside the container to be torn away from the container. Next, the surface and side of the sheet were observed with an electron microscope in the same manner as in Example 1. A material with a thickness of 1 μm was laminated into 20 layers through a collection of nanoparticles with a size of about 10 nm. This material is closer to super sendust than sendust because iron atoms account for the majority, followed by silicon atoms, aluminum atoms, and a small amount of nickel atoms were observed. In addition, the nanoparticles were composed of nickel atoms, so they were nickel nanoparticles. Since the skin depth of flat sendust powder at 3 MHz is 20 μm, a sheet with a thickness of 20 μm effectively absorbs electromagnetic noise around 3 MHz using a small amount of flat sendust powder. Furthermore, the electromagnetic noise absorption performance of the prepared sheet was evaluated in the same manner as in Example 2. The absorption rate was 28% at 3 MHz, 38% at 10 MHz, 42% at 20 MHz, 38% at 50 MHz, and 28% at 100 MHz. Therefore, the prepared sheet had an absorption rate of 28% or more in the frequency band of 3-100 MHz. Compared to Example 4, the absorption rate of electromagnetic waves was significantly increased. This is due to the fact that the particle size and flatness of the sendust flat powder are larger than those of the permalloy flat powder.

[0036] Example 4 In this embodiment, flat powder made of three types of alloys whose imaginary parts of complex permeability have peak values ​​in different frequency bands is used, and a sheet is produced consisting of an assembly of the three types of flat powder, with the flat surfaces of the three types of flat powder joined together via clusters of nickel nanoparticles. The three types of alloy flat powders were the permalloy flat powder used in Example 2, plus a silicon steel flat powder containing 3% silicon, and a magnetic stainless steel flat powder. The flat powder made of silicon steel containing 3% silicon (for example, a product developed by Sanyo Special Steel) has an aspect ratio of 34 and an average particle size of 9 μm. In contrast to the flat powder of permalloy in Example 2, the imaginary part of the complex permeability has a required size in the high frequency band. That is, it gradually increases from around 10 MHz, has a value of 2.3 at 1 GHz, intersects with the value of the imaginary part of the complex permeability of permalloy at 4.7 GHz, shows a peak value of 8.7 at 5.9 GHz, gradually decreases from around 6.3 GHz, has a value of 5.9 even at 10 GHz, and has a value of 3.7 at 12 GHz. Therefore, at 4.7 GHz or higher, the value of the imaginary part of the complex permeability is larger than that of the flat powder of permalloy. Flat powder made of electromagnetic stainless steel with 7% chromium, 1% silicon, and 1.6% aluminum added to iron (for example, a product developed by Sanyo Special Steel) has an aspect ratio of 29 and an average particle size of 12 μm. The imaginary part of the complex permeability increases sharply from around 10 MHz, has a value of 3.4 at 1 GHz, intersects with the imaginary part of silicon steel with 3% silicon at 4.2 GHz, shows a peak value of 7.5 at 4.8 GHz, and gradually decreases from around 5.5 GHz, has a value of 4.8 even at 10 GHz, and has a value of 3.1 at 12 GHz. Therefore, when three types of flat powders, namely, permalloy flat powder, silicon steel flat powder with 3% silicon, and electromagnetic stainless steel flat powder, are used to form a sheet by randomly overlapping the flat surfaces of the three types of flat powder, the imaginary part of the complex permeability of the sheet becomes the sum of the imaginary part of the complex permeability of the three types of flat powder, and the performance of absorbing electromagnetic noise in the intermediate frequency band from 2 to 8 GHz is improved. In particular, the performance of absorbing electromagnetic noise in the frequency band from 3.3 GHz, where the imaginary part of the complex permeability of permalloy shows a peak value, to 4.8 GHz, where the imaginary part of the complex permeability of silicon steel with 3% silicon shows a peak value, is improved. First, 32 g (equivalent to 0.09 moles) of the nickel octylate used in Example 1 was dispersed in methanol at a weight ratio of 10%. After this, the methanol dispersion of nickel octylate was filled into a container measuring 15 cm x 15 cm x 1.5 cm (depth). Next, 8 g of flat powder of permalloy, 7 g of flat powder of silicon steel, and 15 g of flat powder of electromagnetic stainless steel were added to the container. After this, ultrasonic vibrations of 20 kHz were applied for 2 minutes to the methanol dispersion of nickel octylate in the container using the ultrasonic homogenizer device used in Example 1. Furthermore, the ultrasonic homogenizer device was removed from the container, and three-directional vibrations of 0.3 G were applied. impact Acceleration was repeatedly applied to the container, creating a collection of flat powders made of the three types of alloys in which the flat surfaces of the powders overlapped each other through a methanol dispersion of nickel octylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of nickel octylate, and crystals of nickel octylate were precipitated on the surface of the collection of flat powders made of the three types of alloys and in the gaps between the flat surfaces of the flat powders made of the three types of alloys. After this, a plate material measuring 15 cm x 15 cm x 2 mm (thickness) was placed on the surface of the collection of flat powders made of the three types of alloys, and five weights of 6 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment chamber in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way 0.4G. impactBy applying acceleration, a collection of flat powder made up of three types of alloys inside the container was pulled away from the container. Next, the front and side surfaces of the sheet were observed under an electron microscope in the same manner as in Example 1. A substance having a thickness of 0.4-0.6 μm was laminated into 10 layers, interposed between a collection of nanoparticles having a size of about 10 nm. Furthermore, the electromagnetic noise absorbing performance of the prepared sheet was evaluated in the same manner as in Example 1. The absorption rate was 8% at 1 GHz, 10% at 3.3 GHz, 9% at 4.7 GHz, 10% at 5.9 GHz, and 8% at 10 GHz. As a result, the absorption rate was 8% or more in the wide frequency band of 1-10 GHz. However, the absorption rate of electromagnetic waves was low. This is because the average particle size of the three types of alloys was small and the flatness was low compared to the flat powder of sendust used in Example 3. In addition, the case of combining soft magnetic flat powders made of multiple types of alloys is not limited to Example 4. In other words, by combining flat powders made of multiple types of alloys and adjusting the amount of each flat powder used so that the imaginary part of the complex permeability has a constant value in a wide frequency band, the collection of flat powders in which the flat surfaces made of multiple types of alloys overlap and bond with each other will show the characteristics of the imaginary part of the complex permeability of each flat powder, which is added according to the amount of each flat powder used, and as a result, a sheet that absorbs electromagnetic noise in a wide frequency band can be realized.

[0037] Example 5 In this embodiment, flake copper powder is used to produce a sheet consisting of an aggregate of flake copper powder in which the flat surfaces of the flake copper powder are bonded together via an aggregate of copper nanoparticles. The flake copper powder used was MS-800 manufactured by Fukuda Metal Foil and Powder Co., Ltd. The particle size distribution of this flake copper powder is such that flake powder larger than 75 μm accounts for more than 4%, flake powder larger than 45 μm accounts for more than 25%, and flake powder smaller than 45 μm accounts for more than 75%. The thickness is around 0.5 μm, so the aspect ratio is large. In addition, the apparent density is 0.6-1.0 g / cm 3 The raw material for copper nanoparticles is copper octylate, Cu(C7H15 COO)2 (e.g., a product of Mitsuwa Pharmaceutical Co., Ltd.) was used. First, 12 g (corresponding to 0.035 moles) of copper octylate was dispersed in methanol at a weight ratio of 10%. The methanol dispersion of copper octylate was then filled into a container measuring 8 cm x 8 cm x 2 cm (depth), and 9 g of flake copper powder was added to the container. Then, ultrasonic vibrations of 20 kHz were applied to the methanol dispersion of copper octylate in the container for 2 minutes using the ultrasonic homogenizer device used in Example 1. The ultrasonic homogenizer device was then removed from the container, and a three-way vibration of 0.2 G was applied. impact Acceleration was repeatedly applied to the container, creating an aggregate of flake copper powder in which the flat surfaces of the flake copper powder overlapped each other via the methanol dispersion of copper octylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of copper octylate, and copper octylate crystals were precipitated on the surface of the flake copper powder and in the gaps between the flat surfaces of the flake copper powder. After this, a plate material measuring 8 cm x 8 cm x 2.5 mm (thickness) was placed on the surface of the flake copper powder, and five weights weighing 4 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way impact By applying acceleration, the collection of flake copper powder inside the container was torn off from the container. Next, the surface and sides of the sheet were observed with an electron microscope in the same manner as in Example 1. Copper flake powder with a thickness of about 0.5 μm was stacked into six layers, with copper nanoparticles with a size of about 10 nm in between. Furthermore, the electrical resistance of the sample was measured using a DC resistance meter (for example, Tsuruga Electric Co., Ltd.'s DC resistance meter model 356H). Terminals were attached to four points on the sample, and a DC current was passed through the sample in different directions. The voltage was measured twice at the two inner terminals, and the resistance value calculated by dividing the difference between these two voltage values ​​by the current value measured at the two outer terminals showed a volume resistivity close to that of copper. Therefore, the sample produced is a sheet with excellent thermal conductivity and electrical conductivity.

[0038] Example 6 In this example, flake copper powder is used to produce a sheet consisting of an aggregate of flake copper powder in which the flat surfaces of the flake copper powder are bonded together via an aggregate of nickel nanoparticles. The flake copper powder used in Example 5 was used. The raw material for the nickel nanoparticles was nickel octylate Ni(CH 15 COO)2 (e.g., a product of Fujifilm Wako Pure Chemical Industries, Ltd.) was used. First, 12 g (corresponding to 0.035 moles) of the nickel octylate used in Example 1 was dispersed in methanol at a weight ratio of 10%. The methanol dispersion of nickel octylate was then filled into a container measuring 8 cm x 8 cm x 2 cm (depth), and 9 g of flake copper powder was added to the container. Then, ultrasonic vibrations of 20 kHz were applied to the methanol dispersion of nickel octylate in the container for 2 minutes using the ultrasonic homogenizer device used in Example 1. The ultrasonic homogenizer device was then removed from the container, and a three-way vibration of 0.2 G was applied. impact Acceleration was repeatedly applied to the container, creating a mass of flake copper powder in the container in which the flat surfaces of the flake copper powder overlapped each other with the methanol dispersion of nickel octylate interposed therebetween. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of nickel octylate, and crystal clusters of nickel octylate were precipitated on the surface of the cluster of flake copper powder and in the gaps between the flat surfaces of the flake copper powder. After this, a plate material measuring 8 cm x 8 cm x 3 mm (thickness) was placed on the surface of the cluster of flake copper powder, and five weights weighing 4 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way impact By applying acceleration, the collection of flake copper powder inside the container was torn off from the container. Next, the surface and sides of the sheet were observed with an electron microscope in the same manner as in Example 1. Copper flake powder with a thickness of about 0.5 μm was stacked into six layers, with nickel nanoparticles with a size of about 10 nm in between. Furthermore, the electrical resistance of the sample was measured using the DC resistance meter used in Example 5. The sample showed a volume resistivity close to that of copper. Furthermore, the sample showed a sheet with the reddish dark yellow-brown color inherent to copper. Therefore, the fabricated sample has excellent thermal conductivity and electrical conductivity, and is a sheet with the reddish dark yellow-brown color inherent to copper.

[0039] Example 7 In this embodiment, alumina flake powder is used as a flat powder with excellent insulating and lubricating properties, and a sheet is manufactured consisting of an alumina flake powder aggregate bonded via an aggregate of magnesium oxide nanoparticles. The alumina flake powder (BMF-B, a product of Kawai Lime Industry Co., Ltd.) has an aspect ratio of about 40, an average particle size of 9 μm, and a density of 3.98 g / cm. 3 The flake-like boehmite powder (product BMF) consisting of the above is heat-treated at a temperature of 500°C or higher to obtain alumina flake powder with a shape similar to that of boehmite. First, 22g (equivalent to 0.07 moles) of magnesium caprylate Mg(CH3(CH2)6COO)2 (imported product) was dispersed in methanol at a weight ratio of 10%. After this, the methanol dispersion of magnesium caprylate was filled into a container of 11cm x 11cm x 2cm (depth), and 40g of alumina scale powder was added to the container. After that, ultrasonic vibrations of 20 kHz were applied for 2 minutes to the methanol dispersion of nickel octylate in the container by the ultrasonic homogenizer device used in Example 1. Furthermore, the ultrasonic homogenizer device was removed from the container, and the three-direction vibrations of 0.3 G were applied to the dispersion of nickel octylate in methanol in the container. impact Acceleration was repeatedly applied to the container, and an aggregate of the alumina flake powder was formed in the container in which the flat surfaces of the alumina flake powder overlapped each other via the methanol dispersion of magnesium caprylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of magnesium caprylate, and crystals of magnesium caprylate were precipitated on the surface of the alumina flake powder and in the gaps between the flat surfaces of the alumina flake powder. After this, a plate material measuring 11 cm x 11 cm x 3 mm (thickness) was placed on the surface of the alumina flake powder, and five weights of 5 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way impact By applying acceleration, the alumina flakes inside the container were torn off. Next, the surface and sides of the sheet were observed under an electron microscope in the same manner as in Example 1. It was found that 0.2-0.3 μm thick flat powder of alumina was laminated into 10 layers, with aggregates of magnesium oxide nanoparticles with a size of about 10 nm in between. After this, when the surface resistance of the sample was measured at multiple points with an insulation resistance meter, the needle swung to the extreme and the resistance value was greater than 100 MΩ. Next, the static and dynamic friction coefficients of the multiple surfaces of the sample were measured using a measuring device (a friction coefficient measuring device consisting of a Shimadzu Corporation tabletop precision universal testing machine Autograph AGS-X). The static friction coefficient was 0.15±0.03, and the dynamic friction coefficient was 0.10±0.02. Both friction coefficients were small.

[0040] Example 8 In this example, colored flake powder is used as the flat powder, and the flat surfaces of the flake powder are bonded together via a cluster of aluminum nanoparticles to produce a sheet consisting of a cluster of colored flake powder. As the colored flake powder, colored flake powder (Metashine, a product of Nippon Sheet Glass Co., Ltd.) in which glass flake powder is coated with titanium oxide was used. Two types of glass flake powder, colored red (E025RR) and blue (E025RB), were mixed in equal amounts. The colored flake powder had a thickness of 0.5 μm, an average particle size of 25 μm, and a density of 2.6 g / cm. 3 It is. First, aluminum octylate Al (CH 15 23g (equivalent to 0.05 moles) of aluminum octoate (COO)3 (imported product) was dispersed in methanol at a weight ratio of 10%. The methanol dispersion of aluminum octoate was then filled into a container measuring 12cm x 12cm x 2cm (depth), and 65g of colored flake powder was added to the container. Thereafter, ultrasonic vibrations of 20 kHz were applied for 2 minutes to the methanol dispersion of aluminum octylate in the container by the ultrasonic homogenizer device used in Example 1. Furthermore, the ultrasonic homogenizer device was removed from the container, and the homogenizer device was subjected to three-way vibrations of 0.2 G. impact Acceleration was repeatedly applied to the container, and an aggregate of colored flake powder was formed in the container in which the flat surfaces of the colored flake powder overlapped each other via the methanol dispersion of aluminum octylate. Next, the container was heated to 65°C, methanol was evaporated from the methanol dispersion of aluminum octylate, and aluminum octylate crystals were precipitated on the surface of the colored flake powder and in the gaps between the flat surfaces of the colored flake powder. After this, a plate material measuring 12 cm x 12 cm x 3 cm (thickness) was placed on the surface of the colored flake powder, and five weights weighing 4 kg were placed at equal intervals on the plate material. The container was then placed in a heat treatment device in an air atmosphere, heated to 290° C., and left at 290° C. for 1 minute. After this, the container was subjected to three-way impact By applying acceleration, the collection of flake copper powder inside the container was torn off from the container. First, the spectral reflectance of the sample was measured using a spectrophotometer (CM-700d, manufactured by Konica Minolta Japan, Inc.) The spectral reflectance was highest around 470 nm, which emits a blue hue, and around 700 nm, which emits a red hue. Next, the side of the sample was observed and analyzed using an electron microscope in the same manner as in Example 1. As a result, the flat surface of the glass flake powder was found to be stacked into 10 layers of glass flake powder with a thickness of 0.5 μm, with agglomerations of aluminum nanoparticles with a size of about 10 nm in between. On the other hand, the base material of the flat powder is transparent, flat glass flake powder, and the flat surfaces of this glass flake powder are bonded together via clusters of transparent aluminum nanoparticles, so the coating emits a reddish-purple color that combines a strong luster, transparency, and high brightness. From the above results, it was found that the flat surfaces of colored glass flake powder coated with titanium oxide were overlapped and bonded together in 10 layers to form a sheet made of glass flake powder. This sheet had excellent colorability. 31 By using the flake powders colored in the various colors described in the paragraph or a plurality of types of colored flake powders, a colored sheet emitting various colors can be formed. [Explanation of symbols]

[0041] 1. Reduced iron powder 2. Nickel nanoparticles

Claims

1. A method for producing a sheet consisting of an assembly of flat powder made of any one of a metal, alloy, metal oxide, and inorganic compound other than tin and zinc, in which the flat surfaces of the flat powder are bonded together via an assembly of nanoparticles of the metal or metal oxide, comprising: An organometallic compound that precipitates a metal or metal oxide upon thermal decomposition is dispersed in a molecular state in methanol, and the methanol dispersion of the organometallic compound is filled into a container. Thereafter, a collection of flat powders made of any one of metals, alloys, metal oxides, and inorganic compounds excluding tin and zinc is weighed out to a weight less than the weight of the methanol multiplied by the ratio of the density of the flat powder to the density of the methanol used, and the weighed collection of flat powders is poured into the container and stirred in the methanol dispersion of the organometallic compound. Furthermore, a homogenizer is placed in the container and operated in the container to mix the methanol of the organometallic compound. Shock waves are repeatedly applied to the collection of flat powder through the methanol dispersion liquid, and the collection of flat powder is separated into individual flat powder sheets through the methanol dispersion liquid of the organometallic compound, and the separated flat powder is covered with the methanol dispersion liquid of the organometallic compound. After this, the homogenizer device is removed from the container. Furthermore, impact accelerations in three directions, front and back, left and right, and up and down, are repeatedly applied to the container, and finally, impact acceleration in the up and down direction is applied, so that the methanol dispersion liquid of the organometallic compound enters into the gaps between the flat surfaces of the flat powder, and the collection of flat powder in which the flat surfaces of the flat powder overlap each other is formed on the bottom surface of the container in the shape of the bottom surface through the methanol dispersion liquid of the organometallic compound. After this, the container is heated to the boiling point of methanol, methanol is evaporated from the methanol dispersion of the organometallic compound, and a collection of fine crystals of the organometallic compound having a size smaller than 100 nm is precipitated in the gaps between the flat surfaces of the flat powder and on the surface of the collection of flat powder.Furthermore, a plate material that covers the entire surface of the collection of flat powder is placed over the entire surface of the collection of flat powder, and the entire surface of the plate material is evenly compressed to crush the fine crystals of the organometallic compound into fine crystals having a size of approximately 20 nm, which is close to 1 / 5 of the size. Furthermore, a compressive load is evenly applied to the entire surface of the plate material, and the container is heated to the thermal decomposition temperature of the organometallic compound to thermally decompose the fine crystals of the organometallic compound. As a result, clusters of nanoparticles of metal or metal oxide having a size of about 10 nm are deposited simultaneously in the gaps between the flat surfaces of the flat powder and on the surfaces of the clusters of flat powder, and the clusters of nanoparticles are compressed and bonded to the flat surfaces of the flat powder by frictional heat, and the nanoparticles are bonded to each other by frictional heat. As a result, the clusters of nanoparticles bonded by frictional heat A sheet consisting of a collection of flat powder in which the flat surfaces of the flat powder are joined together via a ball is produced within the container in the shape of the bottom of the container; then, impact acceleration is applied to the container in three directions, front-to-back, left-to-right, and up-to-down, to peel the sheet consisting of the collection of flat powder from the bottom of the container, and the sheet is removed from the container; a method for producing a sheet consisting of a collection of flat powder in which the flat surfaces of the flat powder made of one type of material selected from the group consisting of metals, alloys, metal oxides, and inorganic compounds excluding tin and zinc are joined together via collections of metal or metal oxide nanoparticles.

2. The method for producing a sheet made of a collection of flat powder according to claim 1 is a method for producing a sheet made of a collection of soft magnetic flat powder, and the method for producing a sheet made of a collection of soft magnetic flat powder is as follows: A method for producing a sheet consisting of a collection of soft magnetic flat powder, comprising: the flat powder described in claim 1 is a soft magnetic flat powder made of one of the following materials: iron, permalloy, silicon steel, sendust, or electromagnetic stainless steel; the organometallic compound described in claim 1 is nickel octylate, which precipitates nickel by thermal decomposition; the soft magnetic flat powder made of one of the above-mentioned materials is used as the flat powder described in claim 1; the nickel octylate is used as the organometallic compound described in claim 1; and a method for producing a sheet consisting of a collection of soft magnetic flat powder, comprising the steps of: producing a sheet consisting of a collection of flat powder in which the flat surfaces of the soft magnetic flat powder made of one of the above-mentioned materials are joined together via a collection of nickel nanoparticles, according to the method for producing a sheet consisting of a collection of soft magnetic flat powder described in claim 1.

3. The method for producing a sheet made of an aggregate of soft magnetic flat powder according to claim 2 is a method for producing a sheet made of an aggregate of soft magnetic flat powder of a plurality of types of alloys, and the method for producing a sheet made of an aggregate of soft magnetic flat powder of a plurality of types of alloys is as follows: The soft magnetic flat powder described in claim 2 is a soft magnetic flat powder made of a plurality of types of alloys excluding iron described in claim 2, and the frequency characteristics of the imaginary part of the complex permeability of the soft magnetic flat powder made of the plurality of types of alloys are different from each other in the soft magnetic flat powder made of each of the alloys, and the frequency characteristics of the imaginary part of the complex permeability of the soft magnetic flat powder made of each of the alloys have a frequency characteristic of the imaginary part of the complex permeability in which the imaginary parts of the complex permeability complement each other in different frequency ranges. The soft magnetic flat powder made of the plurality of types of alloys is used as the flat powder described in claim 1, and the nickel octylate described in claim 2 is used as the organometallic compound described in claim 1. According to the method for manufacturing a sheet made of a collection of flat powder described in claim 1, a sheet made of a collection of flat powder of the plurality of types of alloys is manufactured in which the flat surfaces of the soft magnetic flat powder of the plurality of types of alloys are joined together via a collection of nickel nanoparticles. A method for manufacturing a sheet made of a collection of soft magnetic flat powder of a plurality of types of alloys.

4. The method for producing a sheet made of a collection of flat powder according to claim 1 is a method for producing a sheet made of a collection of flake powder of a metal or alloy, and the method for producing a sheet made of a collection of flake powder of a metal or alloy includes the following steps: The flat powder described in claim 1 is a flake powder of metal or alloy made of any one of silver, copper, brass, nickel, and aluminum, and the organometallic compound described in claim 1 is a metal octylate compound of any one of copper octylate, aluminum octylate, and nickel octylate. The flake powder of metal or alloy made of any one of the materials is used as the flat powder described in claim 1, and the metal octylate compound of any one of the materials is used as the organometallic compound described in claim 1. A method for producing a sheet consisting of a collection of metal or alloy flake powder, in which the flat surfaces of the flake powder of metal or alloy made of any one of the materials are bonded together via a collection of nanoparticles made of copper, aluminum, or nickel, according to the method for producing a sheet consisting of a collection of flat powder described in claim 1.

5. The method for producing a sheet made of an aggregate of flat powder according to claim 1 is a method for producing a sheet made of an aggregate of insulating flat powder made of a metal oxide or an inorganic compound, and the method for producing a sheet made of an aggregate of insulating flat powder made of a metal oxide or an inorganic compound is as follows: The flat powder described in claim 1 is an insulating flat powder made of a metal oxide or an inorganic compound made of one of glass, alumina, or hematite, and the organometallic compound described in claim 1 is a complex made of a carboxylate metal compound that precipitates an insulating metal oxide having a hardness lower than that of the insulating flat powder made of the metal oxide or the inorganic compound by thermal decomposition. The insulating flat powder made of a metal oxide or an inorganic compound made of any one of the materials is used as the flat powder described in claim 1, and the complex made of the carboxylate metal compound is used as the organometallic compound described in claim 1. A method for manufacturing a sheet made of an insulating flat powder made of a metal oxide or an inorganic compound, in which the flat surfaces of the insulating flat powder made of the metal oxide or the inorganic compound are bonded to each other via a collection of nanoparticles made of an insulating metal oxide having a hardness lower than that of the insulating flat powder, according to the method for manufacturing a sheet made of an insulating flat powder made of a metal oxide or an inorganic compound.

6. The method for producing a sheet made of an aggregate of flat powder according to claim 1 is a method for producing a sheet made of an aggregate of inorganic luster pigments in which the surface of flat powder made of glass or aluminum is covered with a coating made of a metal or a metal oxide, and the method for producing a sheet made of an aggregate of inorganic luster pigments is as follows: A method for producing a sheet consisting of an aggregate of inorganic luster pigments, comprising: the flat powder described in claim 1 is an inorganic luster pigment in which the surface of a flat powder consisting of glass or aluminum is coated with a coating consisting of a metal or a metal oxide; the organometallic compound described in claim 1 is aluminum octylate which precipitates by thermal decomposition of aluminum; the inorganic luster pigment is used as the flat powder described in claim 1, and the aluminum octylate is used as the organometallic compound described in claim 1; and a method for producing a sheet consisting of an aggregate of inorganic luster pigments in which the flat surfaces of the inorganic luster pigments are joined together via an aggregate of aluminum nanoparticles, according to the method for producing a sheet consisting of an aggregate of flat powders described in claim 1.

Citation Information

Patent Citations

  • Stopping device for robot

    JP2007118114A

  • Electromagnetic wave absorbing sheet and manufacturing method therefor

    JP2008198873A

  • Conductive composition, base material with conductive film, and its manufacturing method

    JP2010102884A

  • Electroconductive metal paste

    JP2014035974A