Windows for chemical vapor deposition systems and related methods

JP2023539137A5Active Publication Date: 2024-11-01GLOBALWAFERS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023512164
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-08-18
Filing Date
2021-08-13
Publication Date
2024-11-01
Estimated Expiration
2041-08-13

AI Technical Summary

Technical Problem

Conventional chemical vapor deposition (CVD) systems face challenges in achieving uniform gas flow distribution within the process chamber, leading to non-uniform film thickness and increased processing time due to turbulent gas flows and reduced growth rates.

Method used

A top window with a convex first surface and a radially outer and inner circumferential surface of different curvatures is used to direct gas flow uniformly across the substrate, creating a laminar flow and minimizing deposition dips.

Benefits of technology

The solution enhances film thickness uniformity and reduces processing time by maintaining uniform gas flow distribution across the substrate, even at higher flow rates, improving the efficiency and lifespan of semiconductor wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A system for depositing a layer on a substrate includes a process chamber defining a gas inlet for introducing gas into the process chamber and a gas outlet for allowing the gas to exit the process chamber. A substrate support is disposed within the process chamber and configured to receive a substrate. A transparent top window includes a convex first surface spaced apart from the substrate support and defining an air gap therebetween. The top window is disposed within the process chamber and directs gas from the gas inlet through the air gap to the gas outlet. The first surface includes a radially outer peripheral surface and a radially inner peripheral surface tangent to the outer peripheral surface. The outer peripheral surface has a first radius of curvature, and the inner peripheral surface has a second radius of curvature different from the first radius of curvature.
Need to check novelty before this filing date? Find Prior Art

Description

Cross - reference to related applications

[0001] This application claims priority to U.S. Provisional Patent Application No. 62 / 706,452, filed on August 18, 2020, the entire disclosure of which is incorporated herein by reference.

Technical Field

[0002] This field generally relates to the use of chemical vapor deposition systems in the processing of semiconductor wafers, and more specifically, to windows and methods for controlling the uniformity of gas flow within a chemical vapor deposition process chamber.

Background Art

[0003] In a chemical vapor deposition (CVD) process including epitaxial growth, the uniformity of the film thickness of the deposited film on a substrate depends on, among other things, the uniformity of the gas flow rate distribution within the process chamber. As the requirement for film thickness uniformity becomes more stringent, it has become desirable for the gas flow rate distribution within the process chamber to be more uniform.

[0004] In a conventional CVD apparatus, source gas is introduced into the process chamber through a gas manifold and is guided through a defined gap between an upper window of the process chamber and a substrate disposed on a substrate support. The upper window of a conventional CVD apparatus cannot direct a uniform gas flow distribution onto the substrate surface within the process chamber.

[0005] For example, some conventional upper windows include a curved surface that spans the process chamber and faces the substrate, which may be a convex surface that depresses towards the center of the substrate. However, with such conventional upper windows, a turbulent gas flow may occur on the substrate, and dips or depressions may occur in the epitaxy deposited on the substrate.

[0006] Furthermore, some conventional CVD systems attempt to minimize the dip depth of the epitaxy thickness profile by operating at a reduced growth rate (for example, by lowering the deposition temperature in the process chamber and / or reducing the gas flow rate). However, in such operating systems, even a slight change in the depth of the deposited epitaxy dip can lead to increased process time.

[0007] Therefore, an upper window is required that can guide a more uniform flow distribution across the substrate surface within the process chamber.

[0008] This background section is intended to introduce readers to various aspects of the technology that may be relevant to the various aspects of the disclosure described and / or claimed below. This discussion is intended to be useful in providing readers with background information to facilitate a better understanding of the various aspects of the disclosure. Therefore, it should be understood that these disclosures should be read in this context and do not constitute an admission of prior art. [Overview of the project]

[0009] One aspect of the present disclosure relates to a system for depositing layers on a substrate. The system includes a process chamber that defines a gas inlet for introducing a gas into the process chamber and a gas outlet for allowing the gas to exit the process chamber. A substrate support is positioned within the process chamber and configured to receive the substrate. A transparent upper window includes a convex first surface positioned at a distance from the substrate support, with an air gap defined between them. The upper window is positioned within the process chamber and guides the gas from the gas inlet through the air gap to the gas outlet. The first surface includes a radial outer surface and a radial inner surface circumscribing the outer surface. The outer surface has a first radius of curvature, and the inner surface has a second radius of curvature different from the first radius of curvature.

[0010] Another aspect of the present disclosure relates to a window for a substrate processing system. The window includes a frame for mounting the window to a process chamber of the substrate processing system, and a transparent body connected to the frame. The body extends between a convex first surface and a second surface opposite to it. The first surface includes a radial outer surface and a radial inner surface circumscribing the outer surface. The outer surface extends radially from the frame to the inner surface, and the inner surface extends radially inward from the outer surface to the radial center of the window. The outer surface has a first radius of curvature, and the inner surface has a second radius of curvature different from the first radius of curvature.

[0011] A further aspect of the present disclosure relates to a method for depositing a layer on a substrate. The method includes providing a substrate on a substrate support within a process chamber. The process chamber includes a gas inlet and a gas outlet. The method further includes providing an upper window in the process chamber. The upper window is transparent to allow light from radiant heat to pass through. The upper window includes a convex first surface positioned at a distance from the substrate, defining an air gap between them. The first surface includes a radial outer surface and a radial inner surface circumscribing the outer surface. The outer surface has a first radius of curvature, and the inner surface has a second radius of curvature different from the first radius of curvature. The method further includes directing a gas flow through the gas inlet into the air gap between the first surface and the substrate and to the gas outlet.

[0012] Various improvements to the features pointed out in relation to the embodiments described above exist. Similarly, further features can be incorporated in the embodiments described above. These improvements and additional features may exist individually or in any combination. For example, the various features described below in relation to any of the illustrated embodiments can be incorporated into any of the embodiments described above, either individually or in any combination. [Brief explanation of the drawing]

[0013] [Figure 1]This is a cross-sectional view of a chemical vapor deposition system including an upper window in one embodiment of the present disclosure. [Figure 2] This is an enlarged cross-sectional view of the chemical vapor deposition system in Figure 1, with a portion removed for illustrative purposes. [Figure 3] Figure 2 is a bottom view of the upper window. [Figure 4] This is an enlarged cross-sectional view of a portion of the upper window shown in Figure 2. [Figure 5] This graph shows the thickness profile of epitaxy deposited on the substrate surface in a CVD system using a single upper window with a large curvature. [Figure 6] This graph shows the thickness profile of epitaxy deposited on the substrate surface in a CVD system using a single upper window with a small curvature. [Figure 7] This graph shows the thickness profile of epitaxy deposited on the substrate surface in a CVD system using the first double-curved upper window. [Figure 8] This graph shows the thickness profile of epitaxy deposited on the substrate surface in a CVD system using a second double curvature upper window.

[0014] Similar reference numerals used in various drawings indicate similar elements. [Modes for carrying out the invention]

[0015] The chemical vapor deposition (CVD) system, also referred to herein as the “substrate processing system,” is shown as a 100 in Figure 1. While the illustrated system is a single-substrate system, the systems and methods disclosed herein are suitable for use in other system designs, such as multi-substrate systems, to provide a more uniform gas flow distribution. An example of a CVD system suitable for use according to this disclosure is the Applied Materials EPI Centura 300.

[0016] In this specification, "curvature" refers to the amount by which a curve of a surface and / or plane deviates from a plane, and "radius of curvature" refers to the radius of a circle or sphere whose outer circumference has a curvature that matches the curvature of the surface and / or plane. For example, a surface and / or plane with relatively large curvature will have a large deviation from the plane at every point of the curve and a relatively small radius of curvature. Similarly, a surface or plane with relatively small curvature will have a relatively small deviation from the plane at every point of the curve and a relatively large radius of curvature.

[0017] The CVD system 100 includes a reaction chamber or process chamber 102 for depositing and / or growing a thin film on a substrate 104 (e.g., a semiconductor wafer), a gas introduction port 106 located at one end of the process chamber 102, and a gas exhaust port 108 located at the opposite end of the process chamber 102. A gas manifold 140, located between the gas introduction port 106 and the process chamber 102, is used to guide incoming gas 110 through the gas introduction port 106 into the process chamber 102, which is enclosed by an upper window 112 and a lower window 114. The gas manifold 140 includes an injection baffle or gas distribution plate located between the gas introduction port 106 and the process chamber 102, and an injection insert liner assembly 170 located upstream of the process chamber 102 adjacent to the baffle plate. During operation, the incoming process gas 110 passes through the gas manifold 140 and flows into the process chamber 102 from the gas introduction port 103. The gas 110 then flows over the substrate surface 116 and reacts with the substrate surface 116 or the precursor placed thereon, depositing a film on the substrate surface 116. The gas 110 then flows out of the process chamber 102 and out of the gas discharge port 108.

[0018] The deposited substrate 104 is supported by a susceptor 120 within a process chamber 102. The susceptor 120 is connected to a shaft 122, which is connected to a motor of a rotation mechanism (not shown) for rotating the substrate 104, around the vertical axis X of the CVD system 100. The outer edge 124 of the susceptor 120 and the inner edge of the preheating ring 126 (for heating the incoming gas 110 before contact with the substrate 104) are separated by a gap to allow rotation of the susceptor 120. Rotating the substrate 104 prevents excessive material deposition at the leading edge of the wafer and provides a more uniform epitaxial layer.

[0019] The incoming gas 110 may be heated before contacting the substrate 104. Both the preheating ring 126 and the susceptor 120 are typically opaque to absorb radiant heating light (e.g., infrared light) generated by a high-intensity radiant heating lamp 128 that may be positioned above or below the process chamber 102. It is also possible to supply heat to the process chamber 102 using equipment other than the high-intensity lamp 128, such as resistance heaters or induction heaters. By maintaining the preheating ring 126 and the susceptor 120 at a temperature above the ambient temperature, the preheating ring 126 and the susceptor 120 transfer heat to the incoming gas 110 as it passes over them. The diameter of the substrate 104 may be smaller than the diameter of the susceptor 120 so that the susceptor 120 can heat the incoming gas 110 before contacting the substrate 104. The preheating ring 126 and the susceptor 120 may be made of opaque graphite coated with silicon carbide.

[0020] The upper and lower chamber walls 130 and 132 define the outer periphery of the process chamber 102 and are in contact with the gas inlet port 106 and the gas outlet port 108.

[0021] The CVD system 100 may include an upper liner 134 and a lower liner 136 disposed within the process chamber to prevent reactions between the gas 110 and the chamber walls 130, 132, which are typically made of a metallic material such as stainless steel. The liners 134, 136 can be made of a suitable non-reactive material such as quartz.

[0022] The upper window 112 and the lower window 114 each consist of a generally annular body 142 made of a transparent material such as quartz, allowing radiant heating light to pass into the process chamber 102 to irradiate the preheat ring 126, the susceptor 120, and the substrate 104. The windows 112, 114 may be planar, or as shown in FIG. 1, the windows 112, 114 may have a generally dome-shaped configuration and / or an inwardly recessed configuration. In particular, referring to the embodiment shown in FIG. 1, the lower window 114 has a generally dome-shaped configuration and the upper window has an inwardly recessed configuration. The upper window 112 and the lower window 114 are each coupled or connected (terms used interchangeably herein) to the upper chamber wall 130 and the lower chamber wall 132 of the process chamber 102. In particular, the upper window 112 includes a rim 138 attached to the upper chamber wall 130, or more generally, a frame. Alternatively, the upper window 112 may not include the rim 138 and may be coupled to the upper chamber wall 130 in any manner that allows the upper window 112 to function as described herein.

[0023] The upper window 112 is attached to or optionally connected to the rim 138 and further includes a transparent body 142 that extends between an upper concave surface 144 and a lower convex surface 146 of the upper window 112. The upper surface 144 and the lower surface 146 each circumscribe the inside of the rim 138. The upper surface 144 faces away from the substrate 104. The lower surface 146 is oriented to face the substrate 104. As shown in FIG. 1, the upper surface 144 is substantially curved corresponding to the lower surface 146. Alternatively, the upper concave surface 144 is formed in any way that allows the upper window 112 to function as described herein. For example, without limitation, in some alternative embodiments, the upper surface 144 can have a generally planar and / or dome-shaped configuration.

[0024] A longitudinal gap, indicated generally at 147, can be defined between the lower surface 146 of the upper window 112 and the susceptor 120. The gap 147 is sized to direct the gas 110 entering from the gas inlet 103 along the substrate surface 116 to the gas outlet 105 when the substrate is disposed within the susceptor. In an exemplary embodiment, the gap 147 is about 20 millimeters at its narrowest point. In other embodiments, the gap is any size that allows the CVD system to operate as described herein. As will be explained in more detail below, the lower surface 146 is formed to direct the process gas 110 onto the substrate during operation of the CVD system and provide substantially uniform deposition on the substrate 104.

[0025] FIG. 2 is an enlarged view of a portion of the CVD system 100, and FIG. 3 is a bottom view of the upper window 112. FIG. 4 is an enlarged cross-sectional view of a portion of the upper window 112 shown in FIG. 2. Referring now to FIG. 2, in which a portion of the CVD system 100 has been removed for purposes of illustration, the shape of the upper window 112 is shown in more detail. The dimensions of the upper window 112 are not drawn to scale in FIG. 2, and more particularly, it will be understood that the curvature of the upper window 112 is exaggerated for purposes of explanation.

[0026] As shown in Figure 2, the bottom surface 146 defines the lowest point, which is denoted by 148. In particular, as described herein, the lowest point 148 of the bottom surface 146 is the point where the gap 147 defined between the bottom surface 146 and the substrate surface 116 is narrowest. For example, as shown in Figure 2, the lowest point 148 is separated from the substrate 104 by a gap distance indicated by G1. As shown in Figure 3, the lowest point 148 of the bottom surface 146 may also be located at the center of the radiation line of the bottom surface 146, more generally, at the center of the radiation line of the upper window 112. Alternatively, the upper window 112 may be shaped such that its lowest point is spaced apart from the center of the radiation line of the upper window 112. Furthermore, as shown in Figure 2, the lowest point 148 may be aligned perpendicular to the radial center of the substrate 104.

[0027] The lower surface 146 of the upper window 112 includes a radial outer surface 150 and a radial inner surface 152 circumferentially located within the outer surface 150. More specifically, as shown in the embodiment of Figure 2, the outer surface 150 extends radially inward from the rim 138 to the inner surface 152 by a first radial distance indicated by R1. The outer surface 150 is also curved such that the entire surface extends from the rim 138 to the inner surface 152 by a height indicated by H1. More specifically, in the exemplary embodiment, the outer surface 150 of the lower surface 146 has a constant curvature between the rim 138 and the inner surface 152. Alternatively, the outer surface 150 may include multiple surfaces having varying curvatures from one another.

[0028] The inner circumferential surface 152 of the lower surface 146 extends a second radial distance between the outer circumferential surface 150 and the lowest point 148 of the upper window 112, in a plane tangent to the lowest point 148 (which, in the exemplary embodiment, is also the "radial center" of the upper window), denoted by R2. The radius R2 of the inner circumferential surface 152 may be between 5 millimeters and 200 millimeters, between 25 millimeters and 125 millimeters, between 50 millimeters and 100 millimeters, or between 70 millimeters and 90 millimeters. In the embodiment of Figure 2, the radius R2 of the inner circumferential surface 152 is approximately 75 millimeters. The inner circumferential surface 152 may also be curved to extend a height denoted by H2 between the outer circumferential surface 150 and the lowest point 148 (i.e., the radiation center) of the upper window 112. As shown in the embodiment of Figure 2, the inner circumferential surface 152 has a constant curvature from the outer circumferential surface 150 to the lowest point 148, and from the lowest point 148 to the portion of the outer circumferential surface 150 that is diametrically opposed. Alternatively, the inner circumferential surface 152 may include a plurality of surfaces having varying curvatures relative to each other.

[0029] The lower surface 146 extends from the rim 138 to the lowest point 148 for an overall height indicated by H3. More specifically, in the embodiment shown in Figure 2, the overall height H3 is equal to the sum of the height H1 of the outer surface 150 and the height H2 of the inner surface 152. The overall height H3 may be between 6 and 20 millimeters, 8 and 16 millimeters, or 9 and 12 millimeters. In the embodiment of Figure 2, the overall height H3 of the lower surface 146 is approximately 10 millimeters.

[0030] As shown in Figures 2 and 4, in exemplary embodiments, the outer circumferential surface 150 has a greater curvature than the inner circumferential surface 152, such that the inner circumferential surface 152 has a larger radius of curvature than the outer circumferential surface 150. As a result, as shown in Figures 3 and 4, the lower surface 146 defines a curved boundary 149 extending circumferentially from the lower surface 146 at the intersection of the inner circumferential surface 152 and the outer circumferential surface 150. The outer circumferential surface 150 can have a radius of curvature that is at least twice the radius of curvature of the inner circumferential surface 152. The radius of curvature of the outer circumferential surface 150 is preferably 700 to 1,500 mm, 800 to 1,400 mm, or 900 to 1,300 mm. In the embodiment shown in Figure 2, the radius of curvature of the outer circumferential surface 150 is 1,260 mm. The radius of curvature of the inner circumferential surface 152 is preferably 3,000 to 13,000 mm, 6,000 to 10,000 mm, or 7,000 to 9,000 mm. In the embodiment shown in Figure 2, the radius of curvature of the inner circumferential surface 152 is 8,000 mm. The ratio of the radius of curvature of the inner circumferential surface 152 to the radius of curvature of the outer circumferential surface 150 is preferably 100 to 1.1:1, 20 to 2:1, 13 to 4:1, or 10:1 to 5:1. In the embodiment shown in Figure 2, the ratio of the radius of curvature of the inner circumferential surface 152 to the radius of curvature of the outer circumferential surface 150 is approximately 6:1.

[0031] The upper window 112 is preferably sized such that at least a portion of the outer surface 150 and at least a portion of the inner surface 152 vertically cover (i.e., vertically align) the substrate surface 116. In particular, the ratio of the radius of the substrate 104 to the radius R2 of the inner surface 152 is 4: to 5:1, 3:1 to 1:1, or 2.5:1 to 1.5:1. In the embodiment shown in Figure 2, the ratio of the radius of the substrate 104 to the radius R2 of the inner surface 152 is about 2:1. More specifically, the radius R2 of the inner surface 152 is about 75 millimeters, and the radius of the substrate 104 is about 150 millimeters. In one alternative embodiment, the radius R2 of the inner surface 152 is about 100 millimeters, and the radius of the substrate 104 is about 150 millimeters. In an alternative embodiment, the upper window 112 can be sized such that its outer peripheral surface 150 is radially spaced away from the substrate 104, and only its inner peripheral surface 152 vertically covers the substrate surface 116.

[0032] During operation, gas 110 is introduced into the CVD system 100 from the gas introduction port at a selected flow rate. The gas can then flow into an air gap 147 defined between the bottom surface 146 and the susceptor 120 and / or substrate 104. More specifically, at least a portion of the gas may flow along the outer circumferential surface 150 of the bottom surface 146 to the inner circumferential surface 152. The gas 110 can then flow into the narrow portion of the gap 147 between the inner circumferential surface and the substrate 104. Due at least in part to the configuration of the outer circumferential surface 150 and the inner circumferential surface 152, the gap 147 may be narrower at the center of the substrate 104, while the curvature of the inner circumferential surface 152 may be relatively small compared to at least some conventional upper windows (i.e., the radius of curvature of the inner circumferential surface 152 may be relatively large). Combined with the relatively small curvature of the upper window 112 located near the center of the substrate 104, the narrow gap 147 at the center of the substrate facilitates the provision of layered gas flow around the center of the substrate 104, preventing the formation of “dips” or depressions in the epitaxial deposition surrounding the center of the substrate 104.

[0033] Examples The window for the CVD systems of this disclosure is further illustrated by the following embodiments. These examples should not be taken as limiting.

[0034] Example 1: Variation in thickness profile In the first example, the thickness profiles of epitaxy deposition on a substrate were measured for different upper windows with different bottom surfaces. Specifically, a large curvature window, a small curvature window, and two windows with double curvature bottom surfaces were tested using a CVD system. Specifically, each window was tested using an Applied Materials EPI Centura 300 system. The CVD system was controlled to deposit epitaxy films on a cylindrical substrate with a diameter of 300 mm. In particular, the CVD system was controlled to deposit films on the substrate at a growth rate of approximately 1.4 μm / min (microns / min) in each test window. Thickness change values ​​were measured by determining the difference between the maximum and minimum thicknesses in the radial range of the substrate. For example, the radial ranges of the substrate were -100 mm to -50 mm, -50 mm to 0 mm, 0 mm to 50 mm, and 50 mm to 100 mm, with 0 mm representing the radial center of the substrate. A representative dip value for each test was calculated by averaging the thickness change values ​​in each substrate diameter range.

[0035] As shown in Table 1 below, the large curvature window had a bottom surface with a single radius of curvature of 3,556 mm, the small curvature window had a bottom surface with a single radius of curvature of 8,070 mm, the first double curvature window had a bottom surface with an outer surface having a radius of curvature of 1,260 mm and an inner surface having a radius of curvature of 8,000 mm, the second double curved window had a bottom surface with an outer surface having a radius of curvature of 910 mm and an inner surface having a radius of curvature of 8,000 mm. The inner surface of the first double curved window had a radius of 75 mm, and the inner surface of the second double curved window had a radius of 100 mm.

[0036] The large curvature window was positioned within the CVD system such that the gap between the large curvature window and the substrate (e.g., the same as the gap 147 described above in relation to Figure 1) was approximately 23 millimeters at its narrowest point. In other words, the distance between the lowest point of the upper window (e.g., the same as point 148 described above in relation to Figures 2 and 3) and the substrate was approximately 23 millimeters. The first and second double curvature windows were positioned substantially at the same locations as the large curvature windows. Due to the large curvature of the outer surface of the double curvature windows, the gap between the substrate and the double curvature window was approximately 20 millimeters at its narrowest point. The windows with smaller curvature were positioned so that the gap between the substrate and the window was approximately 20 millimeters at its narrowest point.

[0037] Table 1: Epitaxy Profile Test Window 1-4 TIFF2023539137000002.tif159163

[0038] As shown in Table 1 provided above, each of the first and second double curvature windows results in lower relative thickness variation (i.e., improved thickness uniformity) than both the large curvature window and the small curvature window combined. Furthermore, each of the first and second double curvature windows resulted in smaller typical dips than the large curvature window. The "relative thickness variation" of the deposited layer is determined by measuring the difference between the maximum and minimum layer thicknesses and dividing this difference by the average layer thickness. The resulting value is multiplied by 100 to calculate the percentage. This percentage is the "relative thickness variation" disclosed herein.

[0039] Figures 5-8 are graphs showing the measured thickness profiles of epitaxy deposited on the substrate surface for each test window. The Y-axis of the graph represents the thickness of epitaxy deposited on the substrate surface in nanometers, with zero being adjusted to the lowest thickness measured on the substrate. The X-axis of the graph represents the distance from the radial center of the substrate. More specifically, Figure 5 shows the measured thickness profile 402 from the above-mentioned test performed on a large curvature window, as described in Table 1. Figure 6 shows the measured thickness profile 502 from the above-mentioned test performed on a small curvature window. Figure 7 shows the measured thickness profile 602 from the above-mentioned test performed on a first double curvature window with an inner radius of 75 mm. Figure 8 shows the measured thickness profile 702 from the above-mentioned test performed on a second double curvature window with an inner radius of 100 mm.

[0040] As shown in Figure 5, due to the large curvature window, a large dip 404 occurred in the epitaxy thickness profile at approximately one-third of the radial distance from the center of the substrate (i.e., at ±50 millimeters from the center of the substrate). Furthermore, as shown in Figure 6, the dip 504 around the ±50 mm portion of the substrate was less pronounced in the small curvature window compared to the large curvature window. However, in the small curvature window, high edge rise 506 occurred in the ranges of -150 mm to -125 mm and 125 mm to 150 mm on the substrate.

[0041] Referring to Figures 7 and 8, epitaxy deposited on the substrate using both the first and second double curvature windows showed reduced dips 604 and 704 in the ±50 mm radius range compared to the large curvature window. Furthermore, epitaxy deposited on the substrate surface showed reduced edge rises 606 and 706 between -150 mm and -125 mm, and between 125 mm and 150 mm, compared to the small curvature window. As a result, as shown in Table 1 above, the double curvature windows each produced epitaxial deposition profiles with smaller relative thickness variations compared to the large curvature upper window and the small curvature upper window, respectively.

[0042] Example 2: Comparison of growth rates In the second example, a test window was used to measure the effects of operating the CVD system at different flow rates. In each test, the process chamber temperature was maintained at 1100°C.

[0043] In the initial tests, the large curvature window, small curvature window, and first double-curvature upper window were tested in a CVD system, introducing a trichlorosilane-hydrogen mixture into the CVD system at a flow rate of 8.5 standard liters / minute. The average film thickness and deposition time of the epitaxy film were measured, and the growth rate per minute was determined in microns. The test results are shown in Table 2 below.

[0044] Table 2: Comparison of growth rates at a flow rate of 8.5 slm TIFF2023539137000003.tif34146

[0045] As shown in Table 2 above, the first double curvature window resulted in an increased growth rate compared to the large curvature window.

[0046] In the second test, the first and second double curvature windows were tested using a CVD system, introducing a trichlorosilane-hydrogen mixture into the CVD system at a flow rate of 7.6 standard liters / minute. The average film thickness and deposition time of the epitaxy film were measured, and the growth rate per minute was determined in microns. The test results are shown in Table 3 below.

[0047] Table 3: Comparison of growth rates at a flow rate of 7.6 slm TIFF2023539137000004.tif27146

[0048] As shown in Table 3 provided above, the second double curvature window showed improved growth rates compared to the first double curvature window. Furthermore, the growth rate of the first double curvature window used at a flow rate of 7.6 standard liters / min was approximately the same as the resulting growth rate of the large curvature window operating at an increased flow rate of 8.5 standard liters / min, as measured in the initial test.

[0049] In CVD systems including the upper window described herein, uniformity of gas flow distribution across the substrate surface can be maintained across different gas flow velocities, compared to conventional CVD systems. For example, process gases such as trichlorosilane-hydrogen mixtures can be introduced into the CVD system at flow rates of at least approximately 5 standard liters / min, at least approximately 10 standard liters / min, and even at least approximately 15 standard liters / min, while maintaining relative layer thickness variations of less than approximately 4%, less than approximately 2%, and even less than approximately 1% across the entire substrate surface. Carrier gases such as hydrogen can also be introduced at higher flow velocities, such as at least approximately 70 standard liters / min, at least approximately 80 standard liters / min, or at least approximately 90 standard liters / min, while maintaining relative layer thickness variations of less than approximately 4%, less than approximately 2%, or less than approximately 1% across the entire substrate surface. Because uniformity of gas flow distribution across the substrate surface can be maintained even at higher gas flow velocities, the rate at which predetermined films or layers are deposited on the substrate can be increased while maintaining uniform layer thickness. For example, epitaxial layers can be deposited on silicon wafers having a diameter of at least about 150 mm, at least about 200 mm, or at least about 300 mm, while maintaining relative layer thickness variations of less than about 4% across the wafer diameter, less than about 2% across the wafer diameter, or less than 1% across the wafer diameter.

[0050] In this specification, the term "standard liter" means one liter of reference gas at 0°C and 101.3 kPa (1013 millibars).

[0051] The described examples are suitable for processing semiconductor wafers such as silicon wafers, but can also be used for other applications. Some of the examples are particularly suitable for use in atmospheric pressure silicon-on-silicon chemical vapor deposition using a gas mixture containing hydrogen, trichlorosilane, and diborane. Other silicon precursors besides trichlorosilane can also be used, such as higher-order silane precursors like dichlorosilane, silane, trisilane, tetrachlorosilane, methylsilane, pentasilane, and neopentasilane. Other precursors besides silicon can also be used, such as germanium precursors like Germann and Digermann. Other dopant gas species besides diborane may also be used, such as phosphine and arsine. Furthermore, the described examples can be used in processes other than atmospheric pressure silicon-on-silicon epitaxy, such as reduced pressure epitaxy (e.g., pressures between approximately 10 Torr and approximately 750 Torr), silicon-germanium epitaxy, carbon-doped silicon epitaxy, and non-epitaxial chemical vapor deposition. Furthermore, this embodiment can also be used for processing wafers other than silicon wafers, such as wafers containing germanium, gallium arsenide, indium phosphide, and silicon carbide.

[0052] As described above, the process chamber including the upper window of the present disclosure offers improvements over known process chambers. The upper window of the present disclosure includes two surfaces having different curvatures, which facilitates directing the process flow during operation to provide a laminar flow of process gas across the substrate. As a result, the uniformity of the gas flow distribution on the substrate surface can be improved. More specifically, the CVD system including the upper window of the present disclosure offers the following advantages over several conventional CVD systems: 1) reduced epitaxial dips on the substrate, 2) reduced epitaxial rises on the substrate near the periphery of the substrate, 3) reduced processing time for epitaxial growth on the substrate, and 4) improved semiconductor wafer life.

[0053] When describing elements or embodiments of the present disclosure, the articles “a,” “an,” “the,” and “said” are intended to mean that there is one or more of those elements. The terms “comprising,” “including,” and “having” are intended to mean comprehensive and that there may be additional elements other than those described.

[0054] Various modifications can be made to the above-described structures and methods without departing from the scope of this disclosure, so all matters included in the above description and shown in the accompanying drawings are intended to be illustrative and not limiting.

Claims

1. 1. A system for depositing a layer on a substrate, comprising: a process chamber having a gas inlet for introducing gas into the process chamber and a gas outlet for exhausting gas from the process chamber; a substrate support disposed within the process chamber and configured to receive the substrate; a top window that is transparent to allow radiant heating light to pass therethrough, the top window having a first surface spaced apart from the substrate support and defining an air gap therebetween, the top window being positioned within the process chamber to direct gas from a gas inlet, through the air gap, to a gas outlet, the first surface including a radially outer peripheral surface and a radially inner peripheral surface tangent to the outer peripheral surface, the outer peripheral surface having a first radius of curvature, the inner peripheral surface having a second radius of curvature different from the first radius of curvature, the outer peripheral surface and the inner peripheral surface each being convex, the top window including a transparent body, the transparent body including the inner peripheral surface and the outer peripheral surface; A system including:

2. 2. The system of claim 1, wherein the inner periphery is disposed to be vertically aligned with the substrate when the substrate is received on the substrate support, and the second radius of curvature is greater than the first radius of curvature.

3. 3. The system of claim 2, wherein a ratio of the second radius of curvature to the first radius of curvature is from 100:1 to 1.1:

1.

4. 4. The system of claim 3, wherein the ratio is from 10:1 to 5:

1.

5. The system of claim 1 , wherein the inner periphery and the outer periphery are each positioned to be vertically aligned with at least a portion of the substrate when the substrate is received on the substrate support.

6. 2. The system of claim 1, wherein the upper window further comprises a rim surrounding the first surface and configured to be coupled to the process chamber, the outer circumferential surface extending from the rim to the inner circumferential surface with a first radius of curvature.

7. 7. The system of claim 6, wherein the inner periphery extends from the outer periphery to the radial center of the upper window at a second radius of curvature.

8. The system of claim 7 , wherein the air gap is reduced between the outer periphery and the inner periphery.

9. 2. The system of claim 1, wherein the inner periphery defines a radius extending in a plane tangent to a radial center of the upper window, the radius extending from the radial center to the outer periphery, the radius of the inner periphery being between 5 millimeters and 200 millimeters.

10. 10. The system of claim 1, wherein the upper window further includes a second side opposite the first side and a body extending between the first side and the second side, the second side having a concave curvature.

11. 2. The system of claim 1, wherein the upper window further comprises a rim surrounding the first surface and configured to be coupled to the process chamber, the outer circumferential surface extending at a first height between the rim and the inner circumferential surface, the inner circumferential surface extending at a second height between the outer circumferential surface and a linear center of the upper window, the first height being greater than the second height.

12. A chemical vapor deposition system comprising: a chamber wall at least partially defining a process chamber; a substrate support disposed in the process chamber and configured to receive a substrate thereon; A window, a frame for mounting the window to the chamber wall; and a window including: a transparent body connected to the frame, the body extending between a first surface and an opposing second surface, the first surface being positioned to face the substrate support when the frame is attached to the chamber wall, the first surface including a radially outer peripheral surface and a radially inner peripheral surface tangent to the outer peripheral surface, the outer peripheral surface extending radially from the frame to the inner peripheral surface, the inner peripheral surface extending radially inward from the outer peripheral surface to a linear center of the window, the outer peripheral surface having a first radius of curvature and the inner peripheral surface having a second radius of curvature different from the first radius of curvature, the outer peripheral surface and the inner peripheral surface each being convex, the transparent body including the inner peripheral surface and the outer peripheral surface; 1. A chemical vapor deposition system comprising:

13. The chemical vapor deposition system of claim 12 , wherein the second radius of curvature is greater than the first radius of curvature.

14. 14. The chemical vapor deposition system of claim 13, wherein a ratio between the second radius of curvature and the first radius of curvature is from 100:1 to 1.1:

1.

15. 13. The chemical vapor deposition system of claim 12, wherein the outer periphery extends from the frame to the inner periphery with a first radius of curvature, and the inner periphery extends from the outer periphery to the linear center of the window with a second radius of curvature.

16. 13. The chemical vapor deposition system of claim 12, wherein the inner periphery defines a radius extending in a plane tangent to a radial center of the window, the radius extending from the radial center to the outer periphery, the radius of the inner periphery being between 5 millimeters and 200 millimeters.

17. The chemical vapor deposition system of claim 12 , wherein the second surface has a concave curvature.

18. 1. A method for depositing a layer on a substrate, comprising the steps of: providing a substrate on a substrate support in a process chamber, the process chamber including a gas inlet and a gas outlet; providing a top window in the process chamber, the top window being transparent to allow radiant heating light to pass therethrough, the top window having a first surface spaced from the substrate to define an air gap therebetween, the first surface including an outer radial surface and an inner radial surface tangent to the outer radial surface, the outer radial surface having a first radius of curvature and the inner radial surface having a second radius of curvature different from the first radius of curvature, the outer radial surface and the inner radial surface each being convex, the top window including a transparent body, the transparent body including the inner and outer radial surfaces; directing a flow of gas through a gas inlet, into an air gap between the first surface and the substrate, and to a gas outlet; The method includes:

19. 20. The method of claim 18, wherein the gas flow is provided at a flow rate of greater than 2 standard liters per minute and the variation in relative thickness of the deposited layer on the substrate is less than about 2%.

20. The system of claim 1, wherein the upper window includes a transparent body, the transparent body including an inner surface and an outer surface.