AI Technical Summary
Current adhesion technologies using catechol chemicals require complex modifications to the adhesive matrix, which alter physical properties and are costly and time-consuming, often failing to achieve durable adhesion under wet or humid conditions without compromising performance.
A polymer layer comprising catechol-containing polymers or oligomers, optionally with reactive species or catalysts, that self-react without altering the matrix, providing adhesion in dry, humid, wet, and underwater conditions without complex preparation processes.
The solution achieves durable adhesion across various environmental conditions without modifying the matrix, reducing costs and complexity, and maintaining the integrity of the adhesive properties.
Abstract
Description
Technical Field
[0001] Cross - Reference to Related Applications This application claims the benefit of U.S. Provisional Patent Application No. 63 / 083,894, filed on September 26, 2020, which is hereby incorporated by reference in its entirety.
[0002] The present disclosure relates to a thin layer comprising a catechol - containing polymer or oligomer that exhibits improved adhesion between two materials without substantially modifying the adhesive matrix. The present disclosure also relates to methods of making and using a thin layer comprising a catechol - containing polymer or oligomer.
Background Art
[0003] Industrial, economic, and facile use of catechol chemistry to improve adhesion, particularly to achieve long - term durable adhesion from one matrix to another under aqueous, moist, and humid conditions, has been a non - trivial endeavor.
[0004] Current technologies primarily describe the modification of entire matrices for use in any formulation, method, and application, relating to the use of catechol chemicals to improve adhesion, particularly in wet environments. Modifying an entire matrix with new, often highly variable, components dramatically alters the physical properties of the matrix in virtually all cases. Therefore, developing a completely new matrix is time-consuming, costly, complex, and often requires a significantly more stringent approval process by all necessary supervisory or licensing bodies compared to simply modifying methods that improve adhesion in other ways, leaving the matrix unchanged. In practice, such modifications can alter physical properties so significantly that a viable system may ultimately not be achieved, especially within the user's desired timeframe for successful commercial activity. It would be extremely useful if these limitations could be eliminated without compromising adhesion. There is also extensive research attempting to develop thin layers with highly specific structures, application methods, and complex chemical compositions using catechol chemicals to improve adhesion. Most typically, these include polymers containing dopamine, and / or polymers containing both catechol and another reactive species, particularly amines or acrylates, and typically polymers containing smaller amounts of epoxy or other reactive species, which also require complex preparation and application methods. Of particular importance, these polymers containing both amines and catechol require careful pH control, water as a solvent, and therefore long and complex preparations. Furthermore, amines tend to react with quinones resulting from the oxidation of catechol, leading to crosslinking that can interfere with subsequent physical and chemical interactions. Moreover, many of these preparations require the use of heating to complete a given structure. In fact, there is no practical method for heating a substrate in water, at any volume or rate.Therefore, if it does not have a complex chemical composition, does not require complex processes for thin film preparation or further matrix preparation, does not require heat, does not use water, does not contain self-reactive groups on the same structure except for catechol itself, and does not require cumulative capital costs and operating costs for developing resistance to water exposure under humid and simply wet bonding conditions, either before, during, or after bonding formation in water, it would be extremely useful.
[0005] Therefore, there is a need to use catechol-containing materials without problems to improve adhesion, specifically to improve adhesion under dry, humid, wet, and aquatic conditions, and there is a need to utilize catechol chemicals easily, effectively, and efficiently, in particular to store, handle, and reuse products in a space where they can be used in other ways as needed, easily and at low cost. [Overview of the Initiative]
[0006] This disclosure relates to a polymer layer comprising a catechol-containing polymer or oligomer, wherein the catechol exists as catechol and / or as semiquinone and / or quinone in the absence of a primary or secondary amine, and the polymer layer optionally comprises a) a reactive species separate from the catechol-containing polymer or oligomer and b) at least one of a catalyst, cocatalyst, or accelerator. This disclosure also relates to a method for preparing and using a polymer layer comprising a catechol-containing polymer or oligomer. In one embodiment, the catechol-containing polymer or oligomer is poly-catechol styrene (PCS). [Brief explanation of the drawing]
[0007] [Figure 1] This is a schematic diagram showing layers and layered articles described herein. Figure 1A shows an embodiment of the formulation of the present invention including a second layer. Figure 1B shows an embodiment of the formulation of the present invention not including a second layer. [Figure 2] This is a bar graph showing the average lap shear strength (PSI) of dry steel using epoxy 1 and epoxy 2, with the formulations of the present invention and comparative formulations. [Figure 3] This is a bar graph showing the average overlap shear strength (PSI) of dry aluminum using epoxy 1 and epoxy 2, with the formulations of the present invention and comparative formulations. [Figure 4] This bar graph shows the average tensile strength (PSI) of dry aluminum, dry anodized aluminum, and dry steel using the formulations of the present invention and comparative formulations, with Loctite epoxy. [Figure 5] This bar graph shows the average tensile strength (PSI) of wet aluminum, wet anodized aluminum, and wet steel using the formulations of the present invention and comparative formulations, with Loctite epoxy. [Figure 6] This is a bar graph showing the average overlap shear strength (PSI) of dry steel using Loctite epoxy with the formulations of the present invention and comparative formulations. [Figure 7] This bar graph shows the average lap shear strength (PSI) of wet aluminum, wet anodized aluminum, and wet steel using the formulations of the present invention and comparative formulations, with Loctite epoxy. [Figure 8] This bar graph shows the average overlap shear strength (PSI) of dry aluminum, dry anodized aluminum, and dry steel using the formulations of the present invention and comparative formulations, with a two-component Loctite epoxy. [Figure 9] This bar graph shows the average lap shear strength (PSI) of wet aluminum, wet anodized aluminum, and wet steel using the formulations of the present invention and comparative formulations, with a two-component Loctite epoxy. [Figure 10] This bar graph shows the average lap shear strength (PSI) of dry aluminum, dry anodized aluminum, and dry steel using a two-component urethane adhesive with the formulations of the present invention and comparative formulations. [Figure 11]This is a bar graph showing the average overlap shear strength (PSI) of dry aluminum using Marine Adhesive Sealant 5200, with the formulations of the present invention and comparative formulations. [Figure 12] This is a bar graph showing the average overlap shear strength (PSI) of wet aluminum using Marine Adhesive Sealant 5200, with the formulations of the present invention and comparative formulations. [Figure 13] This bar graph shows the average overlap shear strength (PSI) of dry phosphate-treated steel compared to as-received dry steel, using the formulations of the present invention and comparative formulations. [Figure 14] This bar graph shows the average overlap shear strength (PSI) of wet phosphate-treated steel compared to as-received wet steel, using the formulations of the present invention and comparative formulations. [Figure 15] This bar graph shows the average overlap shear strength (PSI) of old phosphated dry steel compared to new phosphated dry steel. [Figure 16] This bar graph shows the average overlap shear strength (PSI) of old phosphated wet steel compared to new phosphated wet steel. [Figure 17] This bar graph shows the average overlapping shear strength (PSI) of new dry steel containing F002 primer, compared to a sample without primer. [Figure 18] This bar graph shows the average lap shear strength (PSI) of a new wet steel containing F002 primer, compared to a sample without the primer. [Figure 19] This bar graph shows the average bond strength of aluminum joined using VHB adhesive tape under dry, wet, and low-temperature conditions. [Figure 20] This bar graph shows the average joint strength of aluminum joined using Flexcon (or Flexcon) tape under dry, wet, and low-temperature conditions. [Modes for carrying out the invention]
[0008] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in which the present invention pertains. The technical terms used herein are solely for the purpose of describing specific embodiments and are not intended to limit the disclosure.
[0009] The following terms are used to describe this disclosure. If a term is not specifically defined herein, it shall be given the meaning that is recognized in the art by those skilled in the art when applying that term in the context of describing this disclosure.
[0010] In this disclosure, the singular forms “a,” “an,” and “the” include multiple references, and references to specific numerical values include at least that specific value unless otherwise explicitly indicated by the context. Thus, for example, a reference to “material” is a reference to at least one such material and their equivalents known to those skilled in the art.
[0011] When a value is expressed as an approximate value using the descriptors “approximately” or “substantially,” that particular value is understood to form another embodiment. Generally, the use of the terms “approximately” or “substantially” refers to an approximate value that may vary depending on the desired characteristics that the disclosed subject matter seeks to achieve and should be interpreted on its function within the specific context in which it is used. Those skilled in the art will be able to interpret this as a matter of course. In some cases, the number of significant figures used for a particular value may be one non-restrictive way of determining the degree of the words “approximately” or “substantially.” In other cases, the gradual change used for a set of values may be used to determine the intended value available for the term “approximately” or “substantially” for each value. Where present, all ranges are inclusive and combinable; that is, a reference to a value stated in a range includes all values within that range.
[0012] When a list is presented, unless otherwise stated, it should be understood that each individual element of that list and any combination of that list should be construed as separate embodiments. For example, a list of embodiments presented as "A, B, or C" should be construed as including the embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".
[0013] It should be understood that certain features of the present disclosure described herein in the context of separate embodiments may sometimes be provided in combination in a single embodiment for clarity. That is, unless clearly contradictory or excluded, each individual embodiment is considered capable of being combined with any other embodiment, and such combinations are considered to be another embodiment. Conversely, the various features of the present disclosure described in the context of a single embodiment for brevity may sometimes be provided separately or in any partial combination. Further note that the claims can be drafted so as not to exclude any optional elements. Thus, the foregoing is intended to serve as a basis for the use of exclusive terms such as "merely", "only", etc. or the use of "negative" limitations with respect to the elaboration of the components of the claims. Finally, although an embodiment may be described as part of a series of steps or part of a more general structure, each such step may itself be considered an independent embodiment.
[0014] In one aspect, the present disclosure relates to a polymer layer comprising a catechol-containing polymer or oligomer, wherein the catechol is present as a catechol and / or as a semiquinone and / or as a quinone in the absence of a primary or secondary amine, and the polymer layer optionally comprises a) a reactive species separate from the catechol-containing polymer or oligomer and b) at least one of a catalyst, a co-catalyst, or an accelerator.
[0015] In some embodiments, the polymer layer comprises a catechol-containing polymer or oligomer, and the catechol is present as catechol and / or as semiquinone and / or as quinone in the absence of a primary or secondary amine.
[0016] In some embodiments, the polymer layer comprises a catechol-containing polymer or oligomer, and the catechol is present as catechol and / or as semiquinone and / or as quinone in the absence of a primary or secondary amine, and also includes a reactive species separate from the catechol-containing polymer or oligomer.
[0017] In some embodiments, the polymer layer comprises a catechol-containing polymer or oligomer, and the catechol is present as catechol and / or as semiquinone and / or as quinone in the absence of a primary or secondary amine. In some embodiments, the polymer layer comprises a catechol-containing polymer or oligomer, and the catechol is present as catechol and / or as semiquinone and / or as quinone in the absence of a primary or secondary amine, and also includes a catalyst, a cocatalyst, or an accelerator.
[0018] In some embodiments, the polymer layer comprises a catechol-containing polymer or oligomer, and the catechol is present as catechol and / or as semiquinone and / or as quinone in the absence of a primary or secondary amine. In some embodiments, the polymer layer comprises a catechol-containing polymer or oligomer, and the catechol is present as catechol and / or as semiquinone and / or as quinone in the absence of a primary or secondary amine, and also includes both a reactive species separate from the catechol-containing polymer or oligomer and a catalyst, a cocatalyst, or an accelerator.
[0019] Figure 1 shows a schematic diagram of a polymer layer 20 containing a catechol-containing polymer or oligomer and a layered article 100 containing the polymer layer described herein. The layered article 100 may include a substrate 10 disposed in contact with the polymer layer 20. The layered article 100 may also include a polymer matrix 30 disposed on and in contact with the polymer layer 20. The layered article 100 may also include a second polymer layer containing a catechol-containing polymer or oligomer 40 disposed in contact with the polymer matrix 30. The layered article 100 may also include a second substrate 50 disposed in contact with the second polymer layer 40.
[0020] In some embodiments, the catechol-containing polymer or oligomer in the polymer layer 20 is an oligomer. In some embodiments, the catechol-containing polymer or oligomer in the polymer layer 20 is a polymer.
[0021] In one embodiment, the polymer layer 20 contains a reactive species separate from the catechol-containing polymer or oligomer. In one embodiment, the reactive species is a urethane component, epoxy resin, acrylate monomer or oligomer, methacrylate monomer or oligomer, silane, or a combination thereof.
[0022] In some embodiments, the reactive species, separate from the catechol-containing polymer or oligomer, is a urethane component. In some embodiments, the urethane component is a polyol or an organic compound containing multiple hydroxyl groups, and the urethane is linear or branched.
[0023] In some embodiments, the urethane component is 1,6-hexanediol, glycerol, Stepanpol PDC-279®, or polycaprolactone triol.
[0024] In one embodiment, the reactive species, separate from the catechol-containing polymer or oligomer, is an epoxy resin. In some embodiments, the epoxy resin is an epoxy monomer, an epoxy oligomer, a polyepoxide, or a combination thereof, and the epoxy is linear or branched. In some embodiments, the epoxy resin is an epoxy monomer. In some embodiments, the epoxy resin is an epoxy oligomer. In some embodiments, the epoxy resin is a polyepoxide.
[0025] In some embodiments, the epoxy resin is bisphenol A diglycidyl ether, bisphenol A epoxy resin, bis(4-glycidyloxyphenyl)methane, bisphenol E diglycidyl ether (DGEBE), 2,2'-[1,1-ethanediylbis(4,1-phenyleneoxymethylene)]dioxirane, bisphenol F diglycidyl ether (DGEBF), poly(bisphenol A-co-epichlorohydrin), or a combination thereof.
[0026] In some embodiments, the epoxy resin is bisphenol A diglycidyl. In some embodiments, the epoxy resin is bisphenol A epoxy resin. In some embodiments, the epoxy is bis(4-glycidyloxyphenyl)methane. In some embodiments, the epoxy resin is bisphenol E diglycidyl ether (DGEBE). In some embodiments, the epoxy resin is 2,2'-[1,1-ethanediylbis(4,1-phenyleneoxymethylene)]dioxirane. In some embodiments, the epoxy resin is bisphenol F diglycidyl ether (DGEBF). In some embodiments, the epoxy resin is poly(bisphenol A-co-epichlorohydrin).
[0027] In one embodiment, the reactive species, separate from the catechol-containing polymer or oligomer, is an acrylate monomer or oligomer. In some embodiments, the acrylate monomer or oligomer is an acrylate monomer comprising a vinyl group and at least one of carboxylic acid esters and carboxylic acid nitriles, wherein the acrylate is linear or branched.
[0028] In some embodiments, the acrylate monomer or oligomer is ethyl acrylate, ethylene-methyl acrylate, methyl methacrylate, 2-chloroethyl vinyl ether, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, trimethylolpropane triacrylate (TMPTA), or a combination thereof.
[0029] In some embodiments, the acrylate monomer or oligomer is ethyl acrylate. In some embodiments, the acrylate monomer or oligomer is ethylene-methyl acrylate. In some embodiments, the acrylate monomer or oligomer is methyl methacrylate. In some embodiments, the acrylate monomer or oligomer is 2-chloroethyl vinyl ether. In some embodiments, the acrylate monomer or oligomer is 2-hydroxyethyl acrylate. In some embodiments, the acrylate monomer or oligomer is hydroxyethyl methacrylate. In some embodiments, the acrylate monomer or oligomer is butyl acrylate. In some embodiments, the acrylate monomer or oligomer is trimethylolpropane triacrylate (TMPTA).
[0030] In some embodiments, the reactive species distinct from the catechol-containing polymer or oligomer is a silane. In some embodiments, the reactive species distinct from the catechol-containing polymer or oligomer is a methacrylate monomer or oligomer. In some embodiments, the reactive species distinct from the catechol-containing polymer or oligomer is a methacrylate monomer. In some embodiments, the reactive species distinct from the catechol-containing polymer or oligomer is a methacrylate oligomer.
[0031] In one embodiment, the polymer layer 20 includes a catalyst, co-catalyst, or accelerator, wherein the catalyst, co-catalyst, or accelerator is a urethane catalyst that promotes a urethane polymerization reaction, an epoxy catalyst that promotes an epoxy polymerization reaction, an acrylate catalyst that promotes an acrylate polymerization reaction, or a combination thereof.
[0032] In some embodiments, the catalyst, co-catalyst, or accelerator is a urethane catalyst that promotes the urethane polymerization reaction. In some embodiments, the urethane catalyst is an aliphatic amine catalyst, an alicyclic amine catalyst, an alcohol amine catalyst, an aromatic amine catalyst, or an ether amine catalyst.
[0033] In some embodiments, the urethane catalyst is an aliphatic amine catalyst. In some embodiments, the aliphatic amine catalyst is N,N-dimethylcyclohexane, triethylenediamine, N,N,N,N-tetramethylalkylenediamine, N,N,N,N-pentamethyldiethylenetriamine, triethylamine, N,N-dimethylbenzylamine, N,N-dimethylhexadecylamine, N,N-dimethylbutylamine, or a combination thereof.
[0034] In some embodiments, the urethane catalyst is an alicyclic amine catalyst. In some embodiments, the alicyclic amine catalyst is triethylenediamine, N-ethylmorpholine, N-methylmorpholine, N,N-diethylpiperazine, N,N-bis-(α-hydroxypropyl)-2-methylpiperazine, N-hydroxypropyldimethylmorpholine, or a combination thereof.
[0035] In some embodiments, the urethane catalyst is an alcoholamine catalyst. In some embodiments, the alcoholamine catalyst is triethanolamine or N,N-dimethylethanolamine.
[0036] In some embodiments, the urethane catalyst is an aromatic amine catalyst. In some embodiments, the aromatic amine catalyst is pyridine or N,N-dimethylpyridine.
[0037] In some embodiments, the urethane catalyst is an etheramine catalyst. In some embodiments, the etheramine catalyst is BDMAEE.
[0038] In some embodiments, the urethane catalyst is 1,4-diazabicyclo[2.2.2]octane, K-KAT 6212, benzyldimethylamine, or a combination thereof. In some embodiments, the urethane catalyst is 1,4-diazabicyclo[2.2.2]octane. In some embodiments, the urethane catalyst is K-KAT 6212. In some embodiments, the urethane catalyst is benzyldimethylamine.
[0039] In some embodiments, the catalyst, co-catalyst, or accelerator is an epoxy catalyst that promotes epoxy polymerization.
[0040] Suitable catalysts, co-catalysts, or accelerators are substances that promote the reaction between an amino group and an epoxy group, such as an acid or a compound hydrolyzable to an acid. Suitable catalysts, co-catalysts, or accelerators, but not limited to, include: organic carboxylic acids such as acetic acid, benzoic acid, salicylic acid, 2-nitrobenzoic acid, and lactic acid; organic sulfonic acids such as methanesulfonic acid, p-toluenesulfonic acid, or 4-dodecylbenzenesulfonic acid; sulfonic acid esters; other organic or inorganic acids such as phosphoric acid, or mixtures of the aforementioned acids and acid esters; nitrates, particularly calcium nitrate; or tertiary amines such as 1,4-diazabicyclo[2.2.2]octane, benzyldimethylamine, α-methylbenzyldimethylamine, triethanolamine, and dimethylaminopropylamine.
[0041] In some embodiments, the epoxy catalyst is acetic acid, benzoic acid, salicylic acid, 2-nitrobenzoic acid, lactic acid, methanesulfonic acid, p-toluenesulfonic acid, 4-dodecylbenzenesulfonic acid, sulfonic acid esters, phosphoric acid, calcium nitrate, 1,4-diazabicyclo-[2.2.2]octane, benzyldimethylamine, α-methylbenzyldimethylamine, triethanolamine, dimethylaminopropylamine, N,N-dimethylpiperidine, triethylenediamine, 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), benzyldimethylamine (BDMA), 2-(dimethylaminomethyl)phenol (DMP-10), N,N-dimethylbenzylamine, (dimethylaminomethyl)phenol, or a combination thereof.
[0042] In some embodiments, the epoxy catalyst is 1,4-diazabicyclo[2.2.2]octane.
[0043] In some embodiments, the catalyst, co-catalyst, or accelerator is an acrylate catalyst that promotes acrylate polymerization. In some embodiments, the acrylate catalyst is an acrylic polymerization accelerator or a free radical polymerization accelerator.
[0044] In some embodiments, the acrylate catalyst is methyl 4-N,N-dimethylaminophenylacetate (methyl These are 4-N,N-dimethylaminophenylacetate (MDMAPA), N,N-dimethylaminoglutethimide (OMAG), N,N-dimethyl-p-toluidine (OMPT), N,N-di-2-hydroxyethyl-p-toluidine (DHEPT), N,N-di-2-hydroxypropyl-p-toluidine (DHPPT), N,N-dimethyl-sym-xylidine (DMSX), N,N-bis(3-p-tolyloxy-2-hydroxy-propyl)-m-xylidine (BTX), or combinations thereof.
[0045] In one embodiment, the polymer layer 20 has a thickness of about 10 nanometers to about 100 micrometers. In some embodiments, the polymer layer 20 has a thickness of about 15 nanometers to about 50 micrometers. In some embodiments, the polymer layer 20 has a thickness of about 15 nanometers to about 15 micrometers. In some embodiments, the polymer layer 20 has a thickness of about 150 nanometers to less than about 15 micrometers. In some embodiments, the polymer layer 20 has a thickness of about 150 nanometers to about 1.5 micrometers.
[0046] In some embodiments, the polymer layer 20 has a thickness of approximately 10 nanometers to approximately 100 micrometers; or approximately 10 nanometers to approximately 100 nanometers; or approximately 100 nanometers to approximately 150 nanometers; or approximately 150 nanometers to approximately 200 nanometers; or approximately 200 nanometers to approximately 250 nanometers; or approximately 250 nanometers to approximately 300 nanometers; or approximately 300 nanometers to approximately 350 nanometers; or approximately 350 nanometers to approximately 400 nanometers; or approximately 400 nanometers to approximately 450 nanometers; or approximately 450 nanometers to approximately 3350 nanometers to approximately 400 nanometers; or approximately 450 nanometers to approximately 450 nanometers. The range is approximately 500 nanometers; or approximately 500 nanometers to approximately 550 nanometers; or approximately 550 nanometers to approximately 600 nanometers; or approximately 600 nanometers to approximately 650 nanometers; or approximately 650 nanometers to approximately 700 nanometers; or approximately 700 nanometers to approximately 750 nanometers; or approximately 750 nanometers to approximately 800 nanometers; or approximately 800 nanometers to approximately 850 nanometers; or approximately 850 nanometers to approximately 900 nanometers; or approximately 900 nanometers to approximately 950 nanometers; or approximately 950 nanometers to approximately 1000 nanometers.
[0047] In some embodiments, the polymer layer 20 has a thickness of approximately 1 micrometer to approximately 1.5 micrometers; or approximately 1.5 micrometers to approximately 5 micrometers; or approximately 5 micrometers to approximately 10 micrometers; or approximately 10 micrometers to approximately 15 micrometers; or approximately 15 micrometers to approximately 20 micrometers; or approximately 20 micrometers to approximately 25 micrometers; or approximately 25 micrometers to approximately 30 micrometers; or approximately 30 micrometers to approximately 35 micrometers; or approximately 35 micrometers to approximately 40 micrometers; or approximately 40 micrometers to approximately 45 micrometers; or approximately The range is 45 micrometers to approximately 50 micrometers; or approximately 50 micrometers to approximately 55 micrometers; or approximately 55 micrometers to approximately 60 micrometers; or approximately 60 micrometers to approximately 65 micrometers; or approximately 65 micrometers to approximately 70 micrometers; or approximately 70 micrometers to approximately 75 micrometers; or approximately 75 micrometers to approximately 80 micrometers; or approximately 80 micrometers to approximately 85 micrometers; or approximately 85 micrometers to approximately 90 micrometers; or approximately 90 micrometers to approximately 95 micrometers; or approximately 95 micrometers to approximately 100 micrometers.
[0048] In one embodiment, the catechol-containing polymer or oligomer in the polymer layer 20 includes polycatecholstyrene (PCS).
[0049] In some embodiments, the PCS contains about 15% to about 50% catechol. In some embodiments, the PCS contains about 20% to about 40% catechol. In some embodiments, the PCS contains about 25% to about 35% catechol. In some embodiments, the PCS contains about 25% catechol. In some embodiments, the PCS contains about 35% catechol.
[0050] In some embodiments, the PCS includes approximately 20% to approximately 22% catechol; or approximately 22% to approximately 24% catechol; or approximately 24% to approximately 26% catechol; or approximately 26% to approximately 28% catechol; or approximately 28% to approximately 30% catechol; or approximately 30% to approximately 32% catechol; or approximately 32% to approximately 34% catechol; or approximately 34% to approximately 36% catechol; or approximately 36% to approximately 38% catechol; or approximately 38% to approximately 40% catechol.
[0051] In one embodiment, the polymer layer 20 is a continuous layer. In another embodiment, the polymer layer 20 is a discontinuous layer. In another embodiment, the polymer layer 20 is a patterned layer or a textured layer.
[0052] In one embodiment, the disclosure relates to a polymer layer 20 disposed on the surface of a substrate 10 as described herein. In some embodiments, the substrate 10 includes plastics, metals, minerals, composite materials, glass, silanes, concrete, ceramics, wood, recycled wood, asphalt, pitch, tar, bitumen, paper, molten materials, or agglomerating materials, and the substrate is wet, dry, semi-wet, or hydrated.
[0053] In some embodiments, the substrate 10 is wet. In some embodiments, the substrate 10 is dry. In some embodiments, the substrate 10 is semi-wet. In some embodiments, the substrate 10 is hydrated.
[0054] In some embodiments, the surface of the substrate 10 may be treated before the polymer layer is applied. In some embodiments, the surface of the substrate 10 is anodized. In some embodiments, the surface of the substrate 10 is phosphated.
[0055] In some embodiments, the substrate 10 includes a metal. In some embodiments, the metal is Ti, V, Cr, Mn, Fe, Co, Ni, Cu, W, Zr, Al, Au, Ag, or a combination thereof, or an alloy, blend, or oxide of any of these metals.
[0056] In some embodiments, the metal is Ti, a Ti-containing alloy, a Ti-containing blend, or a Ti-containing oxide. In some embodiments, the metal is V, a V-containing alloy, a V-containing blend, or a V-containing oxide. In some embodiments, the metal is Cr, a Cr-containing alloy, a Cr-containing blend, or a Cr-containing oxide. In some embodiments, the metal is Mn, a Mn-containing alloy, a Mn-containing blend, or a Mn-containing oxide. In some embodiments, the metal is Fe, an Fe-containing alloy, a Fe-containing blend, or a Fe-containing oxide. In some embodiments, the metal is Co, a Co-containing alloy, a Co-containing blend, or a Co-containing oxide. In some embodiments, the metal is Ni, a Ni-containing alloy, a Ni-containing blend, or a Ni-containing oxide. In some embodiments, the metal is Cu, a Cu-containing alloy, a Cu-containing blend, or a Cu-containing oxide. In some embodiments, the metal is W, a W-containing alloy, a W-containing blend, or a W-containing oxide. In some embodiments, the metal is Zr, a Zr-containing alloy, a Zr-containing blend, or a Zr-containing oxide. In some embodiments, the metal is Al, an Al-containing alloy, an Al-containing blend, or an Al-containing oxide. In some embodiments, the metal is Au, an Au-containing alloy, an Au-containing blend, or an Au-containing oxide. In some embodiments, the metal is Ag, an Ag-containing alloy, an Ag-containing blend, or an Ag-containing oxide.
[0057] In some embodiments, the substrate 10 includes a metal, including aluminum or steel. In some embodiments, the aluminum or steel is dry. In some embodiments, the aluminum or steel is wet. In some embodiments, the aluminum or steel is semi-wet. In some embodiments, the aluminum or steel is hydrated.
[0058] In some embodiments, aluminum includes anodized aluminum. In some embodiments, steel includes phosphated steel.
[0059] In some embodiments, the base material 10 includes plastic. In some embodiments, the base material 10 includes minerals. In some embodiments, the base material 10 includes ceramics. In some embodiments, the base material 10 includes glass. In some embodiments, the base material 10 includes silane. In some embodiments, the base material 10 includes concrete. In some embodiments, the base material 10 includes composite materials. In some embodiments, the base material 10 includes ceramics. In some embodiments, the base material 10 includes wood. In some embodiments, the base material 10 includes recycled wood. In some embodiments, the base material 10 includes asphalt. In some embodiments, the base material 10 includes pitch. In some embodiments, the base material 10 includes tar. In some embodiments, the base material 10 includes bitumen. In some embodiments, the base material 10 includes paper. In some embodiments, the base material 10 includes molten material. In some embodiments, the base material 10 includes agglomerating material.
[0060] To date, embodiments of the present invention have been described in relation to thin films on substrates. In one embodiment, the present invention relates to the coating of a thin film on a porous substrate. In other words, a thin film can be coated on the available surface of a porous surface, including the outer surface of such a porous structure as well as coating on pores and meandering channels within the porous substrate. A thin film is likely to only partially coat the available internal surface within the pores of the porous substrate. The present invention also relates to the coating of such porous substrates, wherein additives that alter viscosity, surface tension, and hydrophobicity are used to increase the available internal surface of such porous substrates.
[0061] In one embodiment, this disclosure relates to a polymer layer 20 in contact with a polymer matrix 30 as described herein. In some embodiments, the polymer matrix 30 is a bulk adhesive, sealant, coating, ink, pressure-sensitive adhesive (PSA), composite material, or film.
[0062] In some embodiments, the polymer matrix 30 is a bulk adhesive. In some embodiments, the polymer matrix 30 is a sealant. In some embodiments, the polymer matrix 30 is a coating. In some embodiments, the polymer matrix 30 is an ink. In some embodiments, the polymer matrix 30 is a pressure-sensitive adhesive (PSA). In some embodiments, the polymer matrix 30 is a composite material. In some embodiments, the polymer matrix 30 is a film.
[0063] In some embodiments, the polymer matrix 30 includes polyester. In some embodiments, the polymer matrix 30 includes urethane. In some embodiments, the polymer matrix 30 includes phenol. In some embodiments, the polymer matrix 30 includes epoxy, acrylic, or silane. In some embodiments, the polymer matrix 30 includes epoxy. In some embodiments, the polymer matrix 30 includes acrylic. In some embodiments, the polymer matrix 30 includes silane. In some embodiments, the polymer matrix 30 includes silicone.
[0064] In some embodiments, the polymer matrix 30 is a continuous layer. In some embodiments, the polymer matrix 30 is a discontinuous layer. In some embodiments, the polymer matrix 30 is a patterned or textured layer.
[0065] In some embodiments, the polymer layer 20 and the polymer matrix 30 form an interpenetrating polymer network (IPN). As used herein, IPN is interpreted to mean at least two polymer networks that are at least partially entangled at the molecular scale but are not covalently bonded to each other and cannot be separated unless the chemical bonds are broken.
[0066] In some embodiments, the polymer layer 20 and the polymer matrix 30 form a semi-interpenetrating polymer network (SIPN). As used herein, SIPN is interpreted to mean one or more polymer networks and one or more linear or branched polymers, characterized by molecular-scale intrusion of at least one of the networks by at least some of the linear or branched polymers.
[0067] In some embodiments, the polymer layer 20 and the polymer matrix 30 form a sequential interpenetrating polymer network (SeIPN). As used herein, SeIPN is interpreted to mean an interpenetrating polymer network prepared by a process in which a second component network is formed following the formation of a first component network.
[0068] In some embodiments, the polymer layer 20 and the polymer matrix 30 form a sequential semi-interpenetrating polymer network (SSeIPN). As used herein, SSeIPN is interpreted to mean a polymer network in which linear or branched components are formed after the completion of a reaction resulting in the formation of the network(s), or vice versa.
[0069] In some embodiments, the second substrate 50 is disposed on the polymer matrix 30. In some embodiments, the second substrate 50 is disposed in contact with the polymer matrix 30. In some embodiments, the second polymer layer 20 is disposed between the polymer matrix 30 and the second substrate 50.
[0070] In one embodiment, the present disclosure relates to a method for preparing a substrate, which includes distributing a polymer layer 20 as described herein onto the surface of a substrate 10. The method for distributing the polymer layer 20 as described herein is not particularly limited and will be recognized by those skilled in the art.
[0071] In some embodiments, the method for producing the substrate includes distributing a polymer layer 20 on a substrate 10 by methods such as spin coating, dipping coating, spray coating, inkjet printing, flood coating, brushing, and wiping. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by spin coating. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by dipping coating. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by spray coating. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by inkjet printing. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by flood coating. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by brushing. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 by wiping.
[0072] In some embodiments, the method for preparing the substrate includes distributing a polymer layer 20 on the substrate 10, wherein the polymer layer 20 is applied to the substrate 10 as a solution. In some embodiments, the solution contains about 0.001% to about 10% by weight of a catechol-containing polymer or oligomer. In some embodiments, the solution contains about 0.01% to about 5% by weight of a catechol-containing polymer or oligomer. In some embodiments, the solution contains about 0.01% to about 1% by weight of a catechol-containing polymer or oligomer. In some embodiments, the solution contains about 0.1% to about 1% by weight of a catechol-containing polymer or oligomer.
[0073] In some embodiments, the solution contains about 0.001% to about 0.005% by weight of a catechol-containing polymer or oligomer; or about 0.005% to about 0.01% by weight of a catechol-containing polymer or oligomer; or about 0.01% to about 0.02% by weight of a catechol-containing polymer or oligomer; or about 0.02% to about 0.03% by weight of a catechol-containing polymer or oligomer; or about 0.03% to about 0.04% by weight of a catechol-containing polymer or oligomer; or about 0.04% to about 0.05% by weight of a catechol-containing polymer or oligomer. Polymers or oligomers; or about 0.05% to about 0.06% by weight of catechol-containing polymers or oligomers; or about 0.06% to about 0.07% by weight of catechol-containing polymers or oligomers; or about 0.07% to about 0.08% by weight of catechol-containing polymers or oligomers; or about 0.08% to about 0.09% by weight of catechol-containing polymers or oligomers; or about 0.09% to about 0.1% by weight of catechol-containing polymers or oligomers; or about 0.1% to about 0.11% by weight of catechol-containing polymers or oligomers or oligomers; or about 0.11% to about 0.12% by weight of catechol-containing polymers or oligomers; or about 0.12% to about 0.13% by weight of catechol-containing polymers or oligomers; or about 0.13% to about 0.14% by weight of catechol-containing polymers or oligomers; or about 0.14% to about 0.15% by weight of catechol-containing polymers or oligomers; or about 0.15% to about 0.2% by weight of catechol-containing polymers or oligomers; or about 0.2% to about 0.25% by weight of catechol-containing polymers or oligomers Gomer; or approximately 0.25% to approximately 0.3% by weight of catechol-containing polymers or oligomers; or approximately 0.3% to approximately 0.35% by weight of catechol-containing polymers or oligomers; or approximately 0.35% to approximately 0.4% by weight of catechol-containing polymers or oligomers; or approximately 0.4% to approximately 0.45% by weight of catechol-containing polymers or oligomers; or approximately 0.45% to approximately 0.5% by weight of catechol-containing polymers or oligomers; or approximately 0.5% to approximately 0.75% by weight of catechol-containing polymers or oligomers; or approximately 0.It contains 75% to approximately 1% by weight of catechol-containing polymers or oligomers; or approximately 1.25% to approximately 1.5% by weight of catechol-containing polymers or oligomers; or approximately 1.5% to approximately 1.75% by weight of catechol-containing polymers or oligomers; or approximately 1.75% to approximately 2% by weight of catechol-containing polymers or oligomers.
[0074] In some embodiments, the catechol-containing polymer or oligomer used in the solution is polycatecholstyrene (PCS). In some embodiments, the solution contains about 0.001% to about 10% by weight of PCS. In some embodiments, the solution contains about 0.01% to about 5% by weight of PCS. In some embodiments, the solution contains about 0.01% to about 1% by weight of PCS. In some embodiments, the solution contains about 0.1% to about 1% by weight of PCS.
[0075] In some embodiments, the solution is approximately 0.001% to approximately 0.005% by weight of PCS; or approximately 0.005% to approximately 0.01% by weight of PCS; or approximately 0.01% to approximately 0.02% by weight of PCS; or approximately 0.02% to approximately 0.03% by weight of PCS; or approximately 0.03% to approximately 0.04% by weight of PCS; or approximately 0.04% to approximately 0.05% by weight of PCS; or approximately 0.05 PCS of weight % to approximately 0.06 weight %; or approximately 0.06 weight % to approximately 0.07 weight %; or approximately 0.07 weight % to approximately 0.08 weight %; or approximately 0.08 weight % to approximately 0.09 weight %; or approximately 0.09 weight % to approximately 0.1 weight %; or approximately 0.1 weight % to approximately 0.11 weight %; or approximately 0.11 weight % to approximately 0.12 weight %; or approximately 0.12 weight % PCS of approximately 0.13% by weight; or approximately 0.13% to approximately 0.14% by weight; or approximately 0.14% to approximately 0.15% by weight; or approximately 0.15% to approximately 0.2% by weight; or approximately 0.2% to approximately 0.25% by weight; or approximately 0.25% to approximately 0.3% by weight; or approximately 0.3% to approximately 0.35% by weight; or approximately 0.35% to approximately 0. Includes 4% by weight PCS; or approximately 0.4% to approximately 0.45% by weight PCS; or approximately 0.45% to approximately 0.5% by weight PCS; or approximately 0.5% to approximately 0.75% by weight PCS; or approximately 0.75% to approximately 1% by weight PCS; or approximately 1.25% to approximately 1.5% by weight PCS; or approximately 1.5% to approximately 1.75% by weight PCS; or approximately 1.75% to approximately 2% by weight PCS.
[0076] In some embodiments, the solution also includes an aqueous solvent or organic solvent for dissolving the catechol-containing polymer or oligomer. In some embodiments, the organic solvent is acetone, toluene, chloroform, dichloromethane (DCM), ethyl acetate, methyl ethyl ketone (MEK), or a combination thereof.
[0077] In some embodiments, the organic solvent is acetone. In some embodiments, the organic solvent is toluene. In some embodiments, the organic solvent is chloroform. In some embodiments, the organic solvent is dichloromethane (DCM). In some embodiments, the organic solvent is ethyl acetate. In some embodiments, the organic solvent is methyl ethyl ketone (MEK). In some embodiments, the organic solvent is a combination of acetone and toluene. In some embodiments, the organic solvent is acetone, and the catechol-containing polymer or oligomer is PCS. In some embodiments, the organic solvent is toluene, and the catechol-containing polymer or oligomer is PCS. In some embodiments, the organic solvent is a combination of acetone and toluene, and the catechol-containing polymer or oligomer is PCS.
[0078] The pH of the solution is not particularly limited. In some embodiments, the pH of the solution is about 3; or about 3.5; or about 4; or about 4.5; or about 5; or about 5.5; or about 6; or about 6.5; or about 7; or about 7.5; or about 8; or about 8.5; or about 9; or about 9.5; or about 10; or about 10.5; or about 11.
[0079] In some embodiments, the pH of the solution is approximately 3-3.5; or approximately 3.5-4; or approximately 4-4.5; or approximately 4.5-5; or approximately 5-5.5; or approximately 5.5-6; or approximately 6-6.5; or approximately 6.5-7; or approximately 7-7.5; or approximately 7.5-8; or approximately 8-8.5; or approximately 8.5-9; or approximately 9-9.5; or approximately 9.5-10; or approximately 10-10.5; or approximately 10.5-11.
[0080] In some embodiments, a method for producing a substrate includes arranging a polymer layer 20 on a substrate 10, wherein the substrate 10 includes plastic, metal, mineral, composite material, glass, silane, concrete, ceramic, wood, recycled wood, asphalt, pitch, tar, bitumen, paper, molten material, or agglomerating material, and the substrate is wet, dry, semi-wet, or hydrated.
[0081] In some embodiments, the method for producing the base material 10 includes distributing a polymer layer 20 on a base material 10 containing plastic. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing metal. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing minerals. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing composite material. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing glass. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing silane. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing concrete. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing ceramic. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing wood. In some embodiments, the method includes distributing a polymer layer 20 on a base material 10 containing recycled wood. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing asphalt. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing pitch. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing tar. In some embodiments, the method includes distributing a polymer layer on a substrate containing bitumen. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing paper. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing a molten material. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing an agglomerating material.
[0082] In some embodiments, the method for preparing the substrate includes distributing a polymer layer 20 on a wet substrate 10. In some embodiments, the method includes distributing a polymer layer 20 on a dry substrate 10. In some embodiments, the method includes distributing a polymer layer 20 on a semi-wet substrate 10. In some embodiments, the method includes distributing a polymer layer 20 on a water-containing substrate 10.
[0083] In some embodiments, the method for preparing the substrate includes treating the surface of the substrate 10 before applying the polymer layer described herein. In some embodiments, the method includes anodizing the surface of the substrate 10 before applying the polymer layer. In some embodiments, the method includes phosphate treatment of the surface of the substrate 10 before applying the polymer layer.
[0084] In some embodiments, the method for preparing the substrate includes distributing a polymer layer 20 on a substrate 10 containing a metal. In some embodiments, the metal is Ti, V, Cr, Mn, Fe, Co, Ni, Cu, W, Zr, Al, or a combination thereof, or an alloy, blend, or oxide of any of these metals.
[0085] In some embodiments, the method for producing a substrate includes distributing a polymer layer 20 on a substrate 10 containing Ti, a Ti-containing alloy, a Ti-containing blend, or a Ti-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing V, a V-containing alloy, a V-containing blend, or a V-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Cr, a Cr-containing alloy, a Cr-containing blend, or a Cr-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Mn, a Mn-containing alloy, a Mn-containing blend, or a Mn-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Fe, an Fe-containing alloy, a Fe-containing blend, or an Fe-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Co, a Co-containing alloy, a Co-containing blend, or a Co-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Ni, a Ni-containing alloy, a Ni-containing blend, or a Ni-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Cu, a Cu-containing alloy, a Cu-containing blend, or a Cu-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing W, a W-containing alloy, a W-containing blend, or a W-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Zr, a Zr-containing alloy, a Zr-containing blend, or a Zr-containing oxide. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing Al, an Al-containing alloy, an Al-containing blend, or an Al-containing oxide.
[0086] In some embodiments, the method for producing a substrate includes distributing a polymer layer 20 on a substrate 10 containing aluminum or steel. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing dry aluminum or dry steel. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing semi-moist aluminum or semi-moist steel. In some embodiments, the method includes distributing a polymer layer 20 on a substrate 10 containing hydrated aluminum or hydrated steel.
[0087] In some embodiments, the method for producing the substrate includes distributing a polymer layer 20 on a substrate 10 containing anodized aluminum. In some embodiments, the method for producing the substrate includes distributing a polymer layer 20 on a substrate 10 containing phosphated steel.
[0088] In some embodiments, the method for producing the substrate includes distributing a polymer layer 20 on the substrate 10 in a dry environment. In some embodiments, the method includes distributing a polymer layer 20 on the substrate 10 in an ambient environment. In some embodiments, the method includes distributing a polymer layer 20 on the substrate 10 in a humid environment. In some embodiments, the method includes distributing a polymer layer 20 on the substrate 10 in an aqueous environment. In some embodiments, the method includes distributing a polymer layer 20 on the substrate 10 in an underwater environment.
[0089] In some embodiments, the method for producing the substrate includes arranging a polymer layer 20 as a continuous layer on the substrate 10. In some embodiments, the method for producing the substrate includes arranging a polymer layer 20 as a discontinuous layer on the substrate 10. In some embodiments, the method for manufacturing the substrate includes arranging a polymer layer 20 as a patterned layer or a textured layer on the substrate 10.
[0090] In one embodiment, the present disclosure relates to a method for preparing a substrate, the method comprising distributing a polymer layer 20 as described herein on the surface of a substrate 10, and further comprising distributing a polymer matrix 30 on the polymer layer 20. The method for distributing the polymer matrix 30 as described herein is not particularly limited and will be recognized by those skilled in the art.
[0091] In some embodiments, the method for producing the substrate includes distributing a polymer matrix 30 on a polymer layer 20 by methods such as spin coating, dipping coating, spray coating, inkjet printing, flood coating, brushing, and wiping. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by spin coating. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by dipping coating. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by spray coating. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by inkjet printing. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by flood coating. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by brushing. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 by wiping.
[0092] In some embodiments, the polymer matrix 30 is a bulk adhesive, sealant, coating, ink, pressure-sensitive adhesive (PSA), composite material, or film.
[0093] In some embodiments, the method for producing a substrate includes distributing a bulk adhesive 30 on a polymer layer 20. In some embodiments, the method includes distributing a sealant 30 on a polymer layer 20. In some embodiments, the method includes distributing a coating 30 on a polymer layer 20. In some embodiments, the method includes distributing an ink 30 on a polymer layer 20. In some embodiments, the method includes distributing a pressure-sensitive adhesive (PSA) 30 on a polymer layer 20. In some embodiments, the method includes distributing a composite material 30 on a polymer layer 20. In some embodiments, the method includes distributing a film 30 on a polymer layer 20.
[0094] In some embodiments, the polymer matrix 30 includes polyester, urethane, phenol, epoxy, acrylic, silane, or silicone.
[0095] In some embodiments, the method for producing the substrate includes distributing polyester on the polymer layer 20. In some embodiments, the method includes distributing urethane on the polymer layer 20. In some embodiments, the method includes distributing phenol on the polymer layer 20. In some embodiments, the method includes distributing epoxy, acrylic, or silane on the polymer layer 20. In some embodiments, the method includes distributing epoxy on the polymer layer 20. In some embodiments, the method includes distributing acrylic on the polymer layer 20. In some embodiments, the method includes distributing silane on the polymer layer 20. In some embodiments, the method includes distributing silicone on the polymer layer 20.
[0096] In some embodiments, the method for producing the substrate includes distributing a polymer matrix 30 on a polymer layer 20 in a dry environment. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 in an ambient environment. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer in a humid environment. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 in an aqueous environment. In some embodiments, the method includes distributing a polymer matrix 30 on a polymer layer 20 in an underwater environment.
[0097] In some embodiments, the method for producing a substrate includes arranging a polymer matrix 30 as a continuous layer on a polymer layer 20 on the substrate. In some embodiments, the method includes arranging a polymer matrix 30 as a discontinuous layer on the polymer layer 20. In some embodiments, the method includes arranging a polymer matrix 30 as a patterned layer or a textured layer on the polymer layer 20.
[0098] In some embodiments, a method for arranging the polymer matrix 30 as a discontinuous layer, or a method for arranging the polymer layer 20 as a discontinuous layer, includes arranging the layers in an ordered pattern or a disordered pattern.
[0099] In some embodiments, the ordered pattern includes stripes, grids, concentric circles, or dot patterns. In some embodiments, the method includes arranging the polymer matrix 30 and / or polymer layer 20 as stripes. In some embodiments, the method includes arranging the polymer matrix 30 and / or polymer layer 20 as a grid. In some embodiments, the method includes arranging the polymer matrix 30 and / or polymer layer 20 as concentric circles. In some embodiments, the method includes arranging the polymer matrix 30 and / or polymer layer 20 as a dot pattern.
[0100] In some embodiments, the method includes distributing the polymer matrix 30 and / or polymer layer 20 in a disordered manner.
[0101] The polymer matrix 30 and / or polymer layer 20 can be arranged in a specific shape or in an amorphous manner. In some embodiments, the method includes arranging the polymer matrix 30 and / or polymer layer 20 as dots, circles, squares, rectangles, pentagons, hexagons; or in an amorphous shape.
[0102] In one embodiment, the polymer matrix 30 and / or polymer layer 20 are dot-shaped. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are circular. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are elliptical. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are triangular. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are square. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are rectangular. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are pentagonal. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are hexagonal. In one embodiment, the polymer matrix 30 and / or polymer layer 20 are irregularly shaped.
[0103] In some embodiments, the method includes arranging the polymer matrix 30 and / or polymer layer 20 as grid lines, cross lines, random lines, concentric circles, eccentric circles, spaghetti patterns, and flat strips.
[0104] In one embodiment, the polymer matrix 30 and / or polymer layer 20 have a grid pattern. In one embodiment, the polymer matrix 30 and / or polymer layer 20 have a cross pattern. In one embodiment, the polymer matrix 30 and / or polymer layer 20 have a random line pattern. In one embodiment, the polymer matrix 30 and / or polymer layer 20 have a concentric circle pattern. In one embodiment, the polymer matrix 30 and / or polymer layer 20 have an eccentric circle pattern. In one embodiment, the polymer matrix 30 and / or polymer layer 20 have a spaghetti pattern pattern. In one embodiment, the polymer matrix 30 and / or polymer layer 20 have a flat strip pattern.
[0105] In one embodiment, the present disclosure relates to a layered structure comprising a polymer layer 20 as described herein.
[0106] In one embodiment, the present disclosure relates to a layered structure comprising a polymer layer 20 described herein disposed on a substrate 10.
[0107] In one embodiment, the present disclosure relates to a layered structure comprising a polymer layer 20 described herein disposed between a substrate 10 and a polymer matrix 30.
[0108] In one embodiment, the present disclosure relates to a layered structure comprising a polymer layer 20 disposed between a substrate 10 and a polymer matrix 30, and further comprising a second substrate 50 disposed on the polymer matrix 30.
[0109] In one embodiment, the present disclosure relates to a layered structure comprising a polymer layer 20 disposed between a substrate 10 and a polymer matrix 30, and further comprising a second polymer layer 20 disposed on the polymer matrix 30.
[0110] In one embodiment, the present disclosure relates to a layered structure comprising a polymer layer 20 disposed between a substrate 10 and a polymer matrix 30, and further comprising a second polymer layer 20 disposed between a second substrate 50 and a polymer matrix 30.
[0111] In one embodiment, the present disclosure relates to an article comprising a polymer layer 20 as described herein.
[0112] In one embodiment, the present disclosure relates to an article comprising a polymer layer 20 described herein disposed on a substrate 10.
[0113] In one embodiment, the present disclosure relates to an article comprising a polymer layer 20 described herein disposed between a substrate 10 and a polymer matrix 30.
[0114] In one embodiment, the present disclosure relates to an article comprising a polymer layer 20 disposed between a substrate 10 and a polymer matrix 30, and further comprising a second substrate 50 disposed on the polymer matrix 30.
[0115] In one embodiment, the present disclosure relates to an article comprising a polymer layer 20 disposed between a substrate 10 and a polymer matrix 30, and further comprising a second polymer layer 20 disposed on the polymer matrix 30.
[0116] In one embodiment, the present disclosure relates to an article comprising a polymer layer 20 disposed between a substrate 10 and a polymer matrix 30, and further comprising a second polymer layer 20 disposed between a second substrate 50 and a polymer matrix 30.
[0117] The following examples are provided to illustrate some of the concepts described herein. While the examples are intended to provide embodiments, they should not be considered to limit the more general embodiments described herein. [Examples]
[0118] Example 1: Effect of poly(catechol-styrene)PCS-based primer on the adhesion performance of two-component isocyanate (urethane) on dry steel and dry aluminum. The performance of the epoxy resin (poly(bisphenol A-co-epichlorohydrin)) was tested by adding it to the PCS primer at various concentrations (1%, 5%, and 10%). Next, the epoxy catalyst (1,4-diazabicyclo[2.2.2]octane) was added to the PCS primer alone at a concentration of 1:100 (catalyst to PCS). The epoxy resin at a 10% concentration (relative to PCS) and the catalyst at a 1% concentration (relative to PCS) were added together to the primer formulation. Stock solutions of F0043 and F0044 were prepared as follows: ●F0043: Store 0.1% by weight of poly(bisphenol A-co-epichlorohydrin) in toluene. ●F0044: Store 0.1% by weight of 1,4-diazabicyclo[2.2.2]octane in toluene.
[0119] Four primer solutions (F0046, F0047, F0048, F0053) were prepared. The primer solutions were tested against two different types of epoxy adhesives, using both dry steel and dry aluminum as substrates. 120 dry steel samples and 120 dry aluminum samples were prepared and washed. The primer solutions were applied to the dry steel and aluminum samples, left for 24 hours, and then either epoxy 1 or epoxy 2 was applied. Details of the primers used are shown in Table 1 below.
[0120] [Table 1]
[0121] Single-lap joint adhesive bonded metal specimens (ASTM D1002) were tested using steel (A366-1008) and aluminum (5086). The average overlap shear strength (PSI) results for dry steel and dry aluminum using epoxy 1 and epoxy 2 are shown in Table 2 below. The results are also presented graphically for dry steel (Figure 2) and dry aluminum (Figure 3). The standard deviations of the results in Table 2 are shown in Table 3 below.
[0122] [Table 2]
[0123] [Table 3]
[0124] Example 2: Effect of PCS-based primer on the adhesion performance of isocyanates (urethanes) on aluminum, anodized aluminum, and steel. The objective of this experiment was to test the performance of PCS primers using isocyanate (urethane) adhesives. The tests were performed on single-lap joint bonded metal specimens (ASTM D1002) using steel (A366-1008), aluminum (5086), and anodized aluminum. Samples were bonded in both dry and aquatic environments. Various primers were tested using two different PCS polymers with different catechol content (25% and 35%). For each polymer, PCS was tested at concentrations of 1% (wt%) and 0.1% (wt%) in acetone. As controls, lap shear specimens without primer and lap shear specimens with 0.1% polystyrene primer were tested. The effect of the PCS primers on the overall bond strength was determined by comparing the forces required to break each joint.
[0125] Metal samples (4 inches x 1 inch) were cleaned by wiping with acetone (aluminum and anodized aluminum) or toluene (steel). Five separate primer solutions (and one control without primer) were tested. Details of the primers used are listed in Table 4 below.
[0126] [Table 4]
[0127] Each individual metal sample was pre-coated by applying 0.1 mL of primer solution (both sides that would come into contact with the adhesive were pre-coated), and the solution was then spread evenly across the entire metal sample using a plastic pipette. The solvent was evaporated, leaving a thin film of primer on the surface.
[0128] After priming, the samples were left to stand for 24 hours before bonding. To bond the samples, isocyanate adhesive (Loctite 8x) was applied using a wooden applicator stick. The adhesive was spread over a 1-inch area, and then the second sample was bonded to the first sample to obtain a 1-inch x 1-inch overlap. The samples were prepared in a dry state or bonded in water. In the case of underwater bonding, the adhesive was applied to the metal sample below the line corresponding to the water surface. The samples were cured (in air for dry samples, and in water for underwater samples), and then pulled using a tensile strength measuring device to measure the force required to break the bond. The samples were pulled according to ASTM D1002.
[0129] The average tensile strength (PSI) results for dry aluminum, dry anodized aluminum, and dry steel are shown in Table 5 below. The results are also shown in graph form (Figure 4). The standard deviations of the results in Table 5 are shown in Table 6 below.
[0130] [Table 5]
[0131] [Table 6]
[0132] The average tensile strength (PSI) results for wet aluminum, wet anodized aluminum, and wet steel are shown in Table 7 below. The results are also presented in graph form (Figure 5). The standard deviations of the results in Table 7 are shown in Table 8 below.
[0133] [Table 7]
[0134] [Table 8]
[0135] Example 3: Effect of additives to PCS-based primers on the adhesion performance of isocyanates (urethanes) on aluminum, anodized aluminum, and steel. The purpose of this experiment was to test the performance of PCS primers using isocyanate (urethane) adhesives, both with and without various additives. Single-lap joint bonded metal specimens (ASTM D1002) using steel (A366-1008), aluminum (5086), and anodized aluminum were tested. The specimens were bonded in both dry environments (steel only for dry specimens) and underwater environments (all three metals). Three compounds (1,6-hexanediol, a urethane catalyst from King Industries (K-Cat 6212), and 1,4-diazabicyclo[2.2.2]octane (DABCO)) were added to the PCS primer of the present invention and tested. Each additive was tested individually, and then hexanediol and each catalyst compound were combined to form a single primer formulation which was tested again. For dry steel samples, a 0.1% (35% catechol) PCS primer solution was used as the base for all catechol primers. For wet samples, a 0.1% (25% catechol) PCS primer solution was used as the base for all catechol primers. For controls, lap shear specimens without primer and lap shear specimens with 0.1% polystyrene primer were used. By comparing the force required to break each joint, the effect of PCS primers with and without additives on the overall joint strength can be determined.
[0136] Metal samples (4 inches x 1 inch) were cleaned by wiping with acetone (aluminum and anodized aluminum) or toluene (steel). Five separate primer solutions (and one control without primer) were tested. Details of the primers used are listed in Table 9 below for dry primers and in Table 10 below for wet primers.
[0137] [Table 9]
[0138] [Table 10]
[0139] Each individual metal sample was pre-coated by applying 0.1 mL of primer solution (both sides that would come into contact with the adhesive were pre-coated), and the solution was then spread evenly across the entire metal sample using a plastic pipette. The solvent was evaporated, leaving a thin film of primer on the surface.
[0140] After priming, the samples were left to stand for 24 hours before bonding. To bond the samples, isocyanate adhesive (Loctite 8x) was applied using a wooden applicator stick. The adhesive was spread over a 1-inch area, and then the second sample was bonded to the first sample, resulting in a 1-inch x 1-inch overlap. The samples were then clamped together for the curing time. Samples were prepared either dry or underwater. For underwater bonding, the adhesive was applied to the metal sample below the line corresponding to the water surface. The samples were cured (in air for dry samples, and in water for underwater samples), and then pulled using a tensile strength measuring device to measure the force required to break the bond. The samples were pulled according to ASTM D1002.
[0141] The average lap shear strength (PSI) results for dry steel are shown in Table 11 below. The results are also shown in graph format (Figure 6). The standard deviations of the results in Table 11 are shown in Table 12 below.
[0142] [Table 11]
[0143] [Table 12]
[0144] The average lap shear strength (PSI) results for wet aluminum, wet anodized aluminum, and wet steel are shown in Table 13 below. The results are also shown in graph form (Figure 7). The standard deviations for the results in Table 13 are shown in Table 14 below.
[0145] [Table 13]
[0146] [Table 14]
[0147] Example 4: Effect of PCS-based primer on the adhesive performance of a two-component urethane adhesive The objective of this experiment was to test the performance of PCS primers using two-component urethane adhesives. Single-lap joint bonded metal specimens (ASTM D1002) using steel (A366-1008), aluminum (5086), and anodized aluminum were tested. The specimens were bonded in both dry and aquatic environments. Various primers using two different PCS polymers with different catechol content (25% and 35%) were tested. For each polymer, PCS at a concentration of 0.1% (wt%) in acetone was tested. As controls, lap shear specimens without primer and lap shear specimens with 0.1% polystyrene primer were tested. The effect of the PCS primer on the overall bond strength could be determined by comparing the forces required to break each joint.
[0148] Metal samples (4 inches x 1 inch) were cleaned by wiping with acetone (aluminum and anodized aluminum) or toluene (steel). Three separate primer solutions (and one control without primer) were tested. Details of the primers used are listed in Table 15 below.
[0149] [Table 15]
[0150] Each individual metal sample was pre-coated by applying 0.1 mL of primer solution (both sides that would come into contact with the adhesive were pre-coated), and the solution was then spread evenly across the entire metal sample using a plastic pipette. The solvent was evaporated, leaving a thin film of primer on the surface.
[0151] After priming, the samples were left to stand for 24 hours before bonding. A two-component urethane adhesive (Loctite UK U-09FL) was applied using a wooden applicator stick for bonding. The adhesive was spread over a 1-inch area, and then the second sample was bonded to the first sample, resulting in a 1-inch x 1-inch overlap. The two samples were then clamped together for the curing time. Samples were prepared either dry or underwater. For underwater bonding, the adhesive was applied to the metal sample below the water level line. The samples were cured (in air for dry samples and underwater for underwater samples), and then pulled using a tensile strength measuring device to measure the force required to break the bond. The samples were pulled according to ASTM D1002.
[0152] The average tensile strength (PSI) results for dry aluminum, dry anodized aluminum, and dry steel are shown in Table 16 below. The results are also shown in graph form (Figure 8). The standard deviations for the results in Table 16 are shown in Table 17 below.
[0153] [Table 16]
[0154] [Table 17]
[0155] The average tensile strength (PSI) results for wet aluminum, wet anodized aluminum, and wet steel are shown in Table 18 below. The results are also presented in graph form (Figure 9). The standard deviations for the results in Table 18 are shown in Table 19 below.
[0156] [Table 18]
[0157] [Table 19]
[0158] Example 5: Effect of additives to PCS-based primers on the adhesive performance of two-component urethane adhesives The purpose of this experiment was to test the performance of PCS primer using a two-component urethane adhesive, both with and without various additives. Single-lap joint bonded metal specimens (ASTM D1002) using steel (A366-1008), aluminum (5086), and anodized aluminum were tested. The specimens were bonded only in a dry state due to the insufficient performance of this adhesive in aquatic environments. Three compounds (1,6-hexanediol, a urethane catalyst from King Industries (K-Cat 6212), and 1,4-diazabicyclo[2.2.2]octane (DABCO)) were added to the PCS primer of the present invention and tested. Each additive was tested individually, and then hexanediol and each catalyst compound were combined to form a single primer formulation which was tested again. A 0.1% (25% catechol) PCS primer solution was used as the base for all catechol primers. As controls, lap shear specimens without primer and lap shear specimens with 0.1% polystyrene primer were tested. By comparing the force required to break each bond, the effect of PCS primers with and without additives on the overall bond strength can be determined.
[0159] Metal samples (4 inches x 1 inch) were cleaned by wiping with acetone (aluminum and anodized aluminum) or toluene (steel). Seven separate primer solutions (and one control without primer) were tested. Details of the primers used are listed in Table 20 below.
[0160] [Table 20]
[0161] Each individual metal sample was pre-coated by applying 0.1 mL of primer solution (both sides that would come into contact with the adhesive were pre-coated), and the solution was then spread evenly across the entire metal sample using a plastic pipette. The solvent was evaporated, leaving a thin film of primer on the surface.
[0162] After priming, the samples were left to stand for 24 hours before bonding. A two-component urethane adhesive (Loctite UK U-09FL) was applied using a wooden applicator stick for bonding. The adhesive was spread over a 1-inch area, and then the second sample was bonded to the first sample, resulting in a 1-inch x 1-inch overlap. The two samples were then clamped together for the curing time. Samples were prepared either dry or underwater. For underwater bonding, the adhesive was applied to the metal sample below the water level line. The samples were cured (in air for dry samples, and underwater for underwater samples), and then pulled using a tensile strength measuring device to measure the force required to break the bond. The samples were pulled according to ASTM D1002.
[0163] The average lap shear strength (PSI) results for dry aluminum, dry anodized aluminum, and dry steel are shown in Table 21 below. The results are also shown in graph form (Figure 10). The standard deviations for the results in Table 21 are shown in Table 22 below.
[0164] [Table 21]
[0165] [Table 22]
[0166] Example 6: Effect of additives to PCS-based primers on the performance of 3M Marine Adhesive Sealant (or Marine Sealant Adhesive) 5200 The objective of this experiment was to test the performance of PCS primers against 3M Marine Adhesive Sealant 5200, both with and without various additives. Single-lap joint adhesive bonded metal specimens (ASTM D1002) were tested using aluminum (5086). Samples were bonded in both dry and underwater environments. The base primer was 0.1 wt% PCS with a 25% catechol content, diluted with acetone. Four compounds—1,6-hexanediol, a urethane catalyst from King Industries (K-Cat 6212), 1,4-diazabicyclo[2.2.2]octane (DABCO), and polycaprolactone triol (PCL)—were added to the PCS-based primer of the present invention and tested. The combination of K-Cat 6212 and 1,6-hexanediol was also analyzed. Lap shear test specimens without primer and lap shear test specimens with 0.1% polystyrene primer were used as controls. All samples were bonded with 3M 5200 and cured. The effect of the PCS primer on the overall bond strength was determined by comparing the force required to break each bond.
[0167] 140 aluminum metal samples (4 inches x 1 inch) were prepared by wiping with acetone. Seven different primer solutions were tested. Details of the primers used are listed in Table 23 below.
[0168] [Table 23]
[0169] Each individual metal sample was pre-coated by applying 0.1 mL of primer solution (both sides that would come into contact with the adhesive were pre-coated), and the solution was then spread evenly across the entire metal sample using a plastic pipette. The solvent was evaporated, leaving a thin film of primer on the surface.
[0170] After priming, the samples were left for 24 hours before bonding. Next, 3M Marine Adhesive Sealant 5200 was applied using a wooden applicator stick. For samples without primer, the adhesive was spread over a 1-inch segment at the end of the metal sample. A second sample without primer was bonded to the first sample, resulting in a 1-inch x 1-inch overlap. For samples with primer, the adhesive was applied over the primer in the same 1-inch segment. Next, the second sample was bonded to the first sample, ensuring that the primer-coated portion of the second sample adhered securely to the adhesive-coated portion of the first sample. A 1-inch x 1-inch overlap was obtained. In all cases, the adhesive was applied to dry aluminum samples in an air-exposed environment. Adhesive was also applied to wet samples while submerged in water. All bonded samples were clamped together, and any excess adhesive was wiped off.
[0171] The samples were cured in their respective environments. Wet samples were submerged in water, and dry samples were cured in air. Then, 70 bonded samples were pulled using an Instron according to ASTM D1002. The force required to break the bond (in psi) was recorded.
[0172] The average overlap shear strength (PSI) results for dry aluminum are shown in Table 24 below. The results are also presented in graph format (Figure 11).
[0173] [Table 24]
[0174] The average lap shear strength (PSI) results for wet aluminum are shown in Table 25 below. The results are also presented in graph format (Figure 12).
[0175] [Table 25]
[0176] Example 7: Phosphate surface treatment A phosphate chloride coating was formed on steel by immersing the samples in a heated bath of manganese dioxide, phosphoric acid, and water for 1 hour. These samples were primed with F0012 (0.1% PCS (25% catechol)) and F0053 (0.1% PCS (25% catechol), 0.001% 1,4-DIAZABICLO, and 0.01% poly(bisphenol Aco-epichlorohydrin)). Along with a control without primer, lap shear test specimens were prepared using Loctite E120HP two-component epoxy on mixed chips in both wet and dry environments. A control set of uncoated lap shear test specimens was also prepared in the same manner as the coated lap shear test specimens.
[0177] As shown in Figure 13, the phosphate coating significantly increased the strength of the dry lap shear specimens compared to the untreated lap shear specimens. However, as shown in Figure 14, the treated wet lap shear specimens showed a decrease in strength compared to the untreated lap shear specimens. This decrease in strength was mitigated by the use of a primer, allowing the treated lap shear specimens to recover strength exceeding that of the uncoated lap shear specimens. The internal stress state of lap shear specimens is complex, and therefore any description made when analyzing the strain of lap shear specimens is questionable. However, it should be noted that the epoxy in the treated dry samples appeared to yield before fracture, which was not observed in the untreated samples, and this is evidence of increased joint strength.
[0178] The control group with primer F0002 (0.1% polystyrene) was tested on new steel lap shear specimens, presumably with different compositions. The phosphate-treated samples without primer were then repeated to investigate any differences in the phosphate-based coating. It was thought that the strength of the control samples without primer would change when the coatings were different. The results are shown in Figure 15 (dry, no primer comparison) and Figure 16 (wet, no primer comparison).
[0179] Observing the difference in strength between phosphate-treated and unphosphate-treated steel samples in Figures 13 and 14, the phosphate-treated steel was stronger in the dry state and weaker in the wet state. This clearly indicates that the phosphate coating is less pronounced in newer steel samples than it was in older compositions.
[0180] Figures 17 and 18 show that the inclusion of F0002 reduces the lap shear strength. This decrease in strength contradicts the conventional hypothesis that the hydrophobicity of the primer plays a role in increasing the wet bond strength, and indicates that catechol plays a role in this increase.
[0181] Based on the above observations, the following conclusions can be drawn: 1) the method used to prepare the phosphated coating is functional; 2) the primer appears to increase the strength of the treated wet sample; and 3) the composition of the steel plays a role in the phosphated coating.
[0182] Example 8: Effect of PCS-based primer on the performance of VHB adhesive tape The objective of this experiment was to test the performance of PCS primer using VHB tape adhesive. The tests were conducted using aluminum single-lap joint bonded metal specimens (ASTM D1002). The PCS polymer was prepared by Purdue Lab. A pure primer containing 0.1 wt / vol% PCS in acetone was tested. Lap shear test specimens without primer and lap shear test specimens with 0.1% polystyrene primer were used as controls. All samples were bonded with VHB adhesive tape. Bonding was performed under dry, wet, and low-temperature conditions. The effect of PCS on bond strength was determined by comparing the forces required to break each bond.
[0183] Sixty aluminum metal samples (5 inches x 1 inch) were prepared by wiping with Kimtech wipes and acetone. Two primer solutions were prepared. Details of the primers used are shown in Table 26 below.
[0184] [Table 26]
[0185] Metal specimens were primed by applying 0.1 mL of each primer solution to aluminum lap shear specimens. Using a plastic pipette, the solution was spread evenly across the entire 1-inch segment on the end of the metal specimen. After the solvent evaporated, a thin film remained on the metal surface. The specimens were primed and left to stand for 4 hours before bonding. For the dry conditions, 1-inch segments of VHB tape adhesive were then applied to each segment of the lap shear specimen. The red film protecting the adhesive on the opposite side of the tape was removed, and the top of the lap shear specimen was placed on top of the tape. The combined lap shear specimen pair was squeezed together by the operator, and the specimens were not clamped. For the wet conditions, the primed specimens were placed on a sheet of brown paper. Next, using a spray bottle filled with tap water, the specimens were sprayed 4-5 times from a distance of about 3 feet. This simulates wet or rainy conditions. Then, the VHB tape was immediately applied in the same manner as in the dry conditions. For the low-temperature conditions, the primer-coated sample and VHB tape were placed in a laboratory refrigerator and cooled for 3 hours. Then, the VHB tape was immediately applied.
[0186] Since the tape is 0.75 inches wide, the overlap area for all samples is, instead of the usual 1.0 inch, * Please note that the calculation was performed using 0.75 inches. As a result, the average overlapping area was approximately 0.75 in².
[0187] The samples were left standing for 24 hours. Next, 30 bonded samples were pulled using an Instron according to ASTM D1002. The force required to break the bond (in lbs) was recorded. This force was converted to PSI by calculating as described above and dividing by the overlapping area. The results are shown in Table 19.
[0188] These results indicate that PCS did not cause significant changes under either dry or low-temperature conditions, but significantly preserved the performance of the VHB tape under wet conditions. Under dry conditions, lap shear specimens primered with F0012 performed slightly better than lap shear specimens without primer, but the results were not significant due to overlapping standard deviations. Under wet conditions, 0.1% PCS primer (F0012) allowed the bonding strength to remain the same as under dry conditions. In contrast, the strength of the unprimed sample decreased to 27.7 PSI. This means that PCS enables a 64.4% improvement compared to wet conditions without primer. No significant improvements or decreases were observed under other conditions.
[0189] These experiments on VHB adhesive tapes using 0.1% PCS primer under dry, wet, and low-temperature conditions demonstrate that PCS primer significantly preserves performance under wet or rainy conditions. Wet samples with primer exhibited significantly superior bonding strength compared to wet samples without primer. No significant performance improvement compared to the dry control was observed under any of the conditions.
[0190] Example 9: Effect of PCS-based primer on the performance of Flexcon (or Flexcon) PSA tape The objective of this experiment was to test the performance of PCS primer using Flexcon PSA tape. The PCS polymer was prepared by Purdue Lab. A pure primer containing 0.1 wt / vol% PCS in acetone was tested. Aluminum lap shear specimens without primer and aluminum lap shear specimens with 0.1% polystyrene primer were used as controls. All samples were bonded with Flexcon PSA tape. Bonding was performed under dry, wet, and low-temperature conditions. Bonding strength to aluminum was measured by the 180-degree peel strip strength of adhesive bonds as specified in ASTM D903. Measuring the force required to peel the Flexcon PSA tape from the aluminum substrate allowed for the determination of the effect of PCS on bond strength.
[0191] Forty-five aluminum metal samples (5 inches x 1 inch) were prepared by wiping them with Kimtech wipes and acetone. Two primer solutions were prepared. Details of the primers used are shown in Table 27 below.
[0192] [Table 27]
[0193] Aluminum lap shear specimens were primed by applying 0.5 mL of each primer solution to each specimen via a micropipette. Using a plastic micropipette tip, the solution was spread evenly over the entire length of the metal lap shear specimen, covering 5 square inches. After the solvent evaporated, a thin film remained on the metal surface. The specimens were primed and left to stand for 4 hours before bonding. Flexcon tape bonding was performed as follows: Strips 1 inch wide and approximately 10 inches long were cut for preparation, the protective film was removed, and the strips of tape were placed over the entire lap shear specimen, leaving approximately 5 inches of overhang. The strips were applied under dry conditions. Under wet conditions, the specimens were placed on a sheet of brown paper. Then, using a spray bottle filled with tap water, the specimens were sprayed 4-5 times from a distance of approximately 3 feet. This simulates wet or rainy conditions. The Flexcon tape was then immediately applied using the same procedure as under dry conditions. For the low-temperature conditions, the lap shear test specimens and Flexcon tape were placed in a laboratory refrigerator and cooled for 3 hours. The tape was then immediately applied. For all conditions, after the tape was attached to the metal lap shear test specimen, uniform pressure was applied to the tape using the flat end of a Sharpie pen.
[0194] The samples were left standing for 24 hours. Then, 45 bonded samples were pulled with an Instron (or Instron) according to ASTM D903, the 180-degree peel strip strength for adhesive bonds. The force required to peel the tape from the aluminum (in lbs) was recorded. This was converted to scattering peel and peel strength using the Testworks (or Testworks) peel test method. The results are shown in Table 20.
[0195] These results indicate that primer F12 provided a statistically significant improvement in performance under dry and low-temperature conditions. While improvement was observed under wet conditions, it is unclear whether this improvement was statistically significant. From these results, the percentage improvement relative to the control could be calculated and summarized in Table 28 below.
[0196] [Table 28]
[0197] F0012 showed the greatest improvement in peel strength compared to dry conditions, at 122%, or more than double. Under low temperature conditions, the strength increased by 84%. Under wet conditions, the strength increased by 20%, but this is not considered statistically significant due to the variability of the results. Under all conditions, the polystyrene control performed the same as or worse than the control without primer. It is also noteworthy that the samples primered with F0012 showed a much greater change in those results than the samples without primer or with F002 as the primer. Nevertheless, the F0012 samples still performed better than the other conditions in all cases.
[0198] These experiments on Flexcon adhesive tapes using 0.1% PCS primer under dry, wet, and low-temperature conditions demonstrate that PCS primer can significantly improve the performance of the tape under dry and low-temperature conditions.
Claims
1. A polymer layer comprising a catechol-containing polymer or oligomer, the catechol exists as a catechol and / or as a semiquinone and / or as a quinone in the absence of a primary or secondary amine; the polymer layer optionally comprises a) a reactive species separate from the catechol-containing polymer or oligomer, and b) at least one of a catalyst, a co-catalyst, or an accelerator; The polymer layer has a thickness of from 10 nanometers to 100 micrometers.
2. 2. The polymer layer of claim 1, wherein the polymer layer comprises the reactive species separate from the catechol-containing polymer or oligomer, the reactive species being a urethane component, an epoxy resin, an acrylate monomer or oligomer, a methacrylate monomer or oligomer, a silane, or a combination thereof.
3. the reactive species is a urethane component; Optionally, the urethane component is a polyol or an organic compound containing multiple hydroxyl groups, and the urethane is linear or branched; or The polymer layer of claim 2, wherein the urethane component is 1,6-hexanediol, glycerol, Stepanpol PDC-279®, or polycaprolactone triol.
4. the reactive species is an epoxy resin; 3. The polymer layer of claim 2, optionally wherein: (a) the epoxy resin is an epoxy monomer, an epoxy oligomer, a polyepoxide, or a combination thereof, and the epoxy is linear or branched; or (b) the epoxy resin is bisphenol A diglycidyl ether, bisphenol A epoxy resin, bis(4-glycidyloxyphenyl)methane, bisphenol E diglycidyl ether (DGEBE), 2,2'-[1,1-ethanediylbis(4,1-phenyleneoxymethylene)]dioxirane, bisphenol F diglycidyl ether (DGEBF), poly(bisphenol A-co-epichlorohydrin), or a combination thereof.
5. the reactive species is an acrylate monomer or oligomer; Optionally, (a) the acrylate monomer or oligomer is an acrylate monomer comprising a vinyl group and at least one of a carboxylic acid ester and a carboxylic acid nitrile, the acrylate being linear or branched; or 3. The polymeric layer of claim 2, wherein (b) the acrylate monomer or oligomer is ethyl acrylate, ethylene-methyl acrylate, methyl methacrylate, 2-chloroethyl vinyl ether, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, trimethylolpropane triacrylate (TMPTA), or a combination thereof.
6. the polymer layer comprises the catalyst, co-catalyst, or accelerator, the catalyst, co-catalyst, or accelerator being a urethane catalyst for promoting a urethane polymerization reaction, an epoxy catalyst for promoting an epoxy polymerization reaction, an acrylate catalyst for promoting an acrylate polymerization reaction, or a combination thereof; Optionally, the catalyst, cocatalyst, or promoter is (a) a urethane catalyst that promotes a urethane polymerization reaction, optionally the urethane catalyst being 1,4-diazabicyclo[2.2.2]octane, K-KAT 6212, benzyldimethylamine, or a combination thereof; or (b) an epoxy catalyst that promotes an epoxy polymerization reaction, optionally wherein the epoxy catalyst is 1,4-diazabicyclo[2.2.2]octane; or The polymer layer of any one of claims 1 to 5, wherein (c) an acrylate catalyst that promotes an acrylate polymerization reaction, optionally said acrylate catalyst being an acrylic polymerization promoter or a free radical polymerization promoter. (a) the polymer layer has a thickness of 15 nanometers to 50 micrometers, optionally the polymer layer has a thickness of 15 nanometers to 15 micrometers, optionally the polymer layer has a thickness of 150 nanometers to less than 15 micrometers, optionally the polymer layer has a thickness of 150 nanometers to 1.5 micrometers, and / or 7. The polymer layer of any one of claims 1 to 6, wherein (b) the catechol-containing polymer or oligomer comprises polycatecholstyrene (PCS), optionally the PCS comprises 25% catechol to 35% catechol, optionally (i) the PCS comprises 25% catechol, or (ii) the PCS comprises 35% catechol.
8. A substrate comprising a polymer layer according to any one of claims 1 to 7 disposed on a surface of the substrate, Optionally, the substrate comprises a plastic, a metal, a mineral, a composite material, a glass, a silane, a concrete, a ceramic, wood, reclaimed wood, asphalt, pitch, tar, bitumen, paper, a molten material, or an aggregate material; the substrate is wet, dry, semi-wet or hydrous; Optionally, the substrate comprises a metal; Optionally, the metal comprises aluminum or steel, and optionally (a) the aluminium or steel is dry; or (b) the aluminum or steel is wet; or (c) the aluminum comprises anodized aluminum; or (d) the substrate, wherein the steel comprises phosphate treated steel.
9. A polymer matrix in contact with the polymer layer of any one of claims 1 to 7, optionally the polymer matrix being a bulk adhesive, a sealant, a coating, an ink, a pressure sensitive adhesive (PSA), a composite, or a film; Optionally, the polymer matrix is a bulk adhesive.
10. A method of making a substrate, comprising disposing a polymer layer according to any one of claims 1 to 7 on a surface of the substrate.
11. The substrate comprises a plastic, a metal, a mineral, a composite, a glass, a silane, a concrete, a ceramic, a wood, a reclaimed wood, an asphalt, a pitch, a tar, a bitumen, a paper, a molten material, or an aggregate material; the substrate is wet, dry, semi-wet or hydrous; Optionally, the substrate comprises a metal; Further optionally, the metal comprises aluminum or steel; Optionally, (a) the aluminium or steel is dry; or (b) the aluminum or steel is wet; or (c) the aluminum comprises anodized aluminum; or (d) the steel comprises phosphated steel.
12. The disposing step comprises: (a) disposing in a dry environment, Optionally, the dry environment is an ambient environment; and optionally, the ambient environment is humid; or (b) disposing in an aqueous environment, Optionally, the aqueous environment is an underwater environment. The method of claim 10, comprising:
13. further comprising disposing a polymer matrix over the polymer layer; Optionally, (a) the polymer matrix is a bulk adhesive, a sealant, a coating, an ink, a pressure sensitive adhesive (PSA), a composite, or a film, and further optionally, the polymer matrix is a bulk adhesive; or (b) the disposing includes disposing in a dry environment, optionally the dry environment is an ambient environment, and further optionally the ambient environment is humid; or 11. The method of claim 10, wherein (c) said disposing comprises disposing in an aqueous environment, and further optionally, said aqueous environment is an underwater environment.
14. A layered structure comprising a polymer layer according to any one of claims 1 to 7 disposed between a substrate and a polymer matrix.