Methods for producing iron electrodes and articles and systems made from such electrodes

JP2023549670A5Active Publication Date: 2024-11-12FORM ENERGY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023525614
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-05-26
Filing Date
2021-11-10
Publication Date
2024-11-12
Estimated Expiration
2041-11-10

AI Technical Summary

Technical Problem

Existing methods for producing iron electrodes for energy storage applications face challenges in creating electrically conductive and low-cost electrodes with low packaging costs, while maintaining high microporosity and microporosity, which limits electron transport and increases production costs.

Method used

A method involving high-temperature thermomechanical processing of porous particulate iron materials to form metallurgical bonds between particles, creating electrodes with conductive connections that are low-cost, mechanically robust, and scalable for mass production, eliminating the need for external current collectors.

Benefits of technology

The method produces electrodes suitable for long-term energy storage, achieving high performance and scalability, reducing production costs, and enabling grid-scale energy storage solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Iron electrode materials, iron electrodes, and methods for making the iron electrode materials and iron electrodes by high-temperature thermomechanical processing of porous particulate iron materials are described. For example, as part of iron electrode manufacturing, a particulate iron material may be provided to an apparatus, and pressure and / or heat may be applied to the particulate iron material within the apparatus for a period of time to form an electrode having conductive connections between particles of the particulate iron material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 112,539, entitled "METHOD OF IRON ELECTRODE MANUFACTURE AND ARTICLES AND SYSTEMS THEREFROM," filed November 11, 2020, and U.S. Provisional Patent Application No. 63 / 193,424, entitled "METHOD OF IRON ELECTRODE MANUFACTURE AND ARTICLES AND SYSTEMS THEREFROM," filed May 26, 2021, the entire contents of both applications being incorporated herein by reference for all purposes. [Background technology]

[0002] Energy storage technologies are playing an increasingly important role in the power grid. At the most basic level, these energy storage assets provide smoothing to better match generation and demand on the distribution grid. The services performed by energy storage devices benefit the power grid over multiple timescales, from milliseconds to years. Today, energy storage technologies exist that can support timescales from milliseconds to hours, but long-term and ultra-long-term (collectively, >8 hours) energy storage systems are needed.

[0003] Direct reduced iron (DRI) is an inexpensive form of iron produced by reducing iron ore to a primarily metallic oxidation state. DRI is primarily available in pellet or lump form, with characteristic sizes ranging from 6 to 16 mm, depending on the pellets and lumps fed into the reduction process.

[0004] Iron negative electrodes (i.e., battery anodes) for energy storage applications require a high level of microporosity (typically greater than about 40% by volume), a high specific surface area (typically about 0.05 m² / g), and reasonably high purity (typically greater than 80% by weight iron). Direct reduced iron satisfies all of the above material property requirements at an attractive price.

[0005] Other methods for producing highly porous iron materials (e.g., sponge iron) exist, often at prices that are quite attractive for the production of battery electrodes. These sponge irons may be produced in particulate form. The teachings of this disclosure may be useful for the consolidation of any iron-containing particulate electrode material that would benefit from making electrical connections between particles for battery applications. Hereinafter, the term porous particulate iron will be used to describe any material with a high level of microporosity that can be usefully arranged for electrical connections to form battery materials.

[0006] To function, battery electrodes must be both ionically and electrically conductive. While porous particulate iron in particulate form offers advantages for bulk handling and manufacturing processes, the size and shape of the particulates can present challenges when attempting to form a conductive mass of material while substantially maintaining the internal porosity and microstructure of the porous particulate iron. That is, electron transport through porous particulate iron-based electrodes can be difficult enough that electron transport through the electrode limits the electrode's performance, for example, due to point contact resistance. In many cases, electron transport through these electrodes can be enhanced by an appropriate combination of conductive additives, compression to reduce contact resistance, or other techniques. However, these techniques for enhancing electrical conduction within and across the electrode are often so expensive that attractive applications of iron electrodes are no longer technically and economically attractive. Therefore, an economical technique for providing electrical connections between porous particulate iron particles for iron battery electrodes is needed. Summary of the Invention [Problem to be solved by the invention]

[0007] Successful techniques for connecting particles within an electrode not only produce electrically conductive, low-cost electrodes, but also produce electrodes with low packaging costs, low current collector costs, and provide sufficiently robust batteries that they exhibit sufficient life spans for a variety of applications. The methods, systems, and articles disclosed herein have the unique potential to simultaneously address the above needs.

[0008] The foregoing background introduces various aspects of the art that may be of interest to embodiments of the present disclosure. As such, the foregoing discussion is intended to provide a framework for better understanding the various aspects of the disclosure herein, and should not be construed as admissions of prior art. [Means for solving the problem]

[0009] Without being limited to any particular theory or model regarding the reactivity of iron electrodes, a possible scheme for the oxidation of iron electrodes in alkaline electrolytes can proceed according to the following two reaction steps: Reaction 1 and Reaction 2. Although additional or different reaction products may occur (one of which is described below in Reaction 3), the characteristics of the volume change via the reaction may be common to all oxidation products for metallic iron. Reaction 1: Fe + 2OH - →Fe(OH)2+2e - E 0 =-0.88V vs SHE Reaction 2: 3Fe(OH)2 + 2OH - →Fe3O4+4H2O+2e - E 0 =-0.76V vs SHE Reaction 3: Fe(OH)2 + OH - →FeOOH+H2O+e - E 0 =-0.61V vs SHE

[0010] Various embodiments include iron electrode materials, iron electrodes, and methods of fabricating the iron electrode materials and electrodes by high-temperature thermomechanical processing of porous particulate iron materials. Generally, the techniques involve feeding, providing, or otherwise receiving a porous particulate iron material into an apparatus. Pressure and / or heat may be applied to the porous particulate iron material within the apparatus for a period of time to form an electrode having conductive connections between particles of the particulate iron material. In some embodiments, the apparatus may simultaneously apply pressure and high temperature to the material to create strong conductive connections between particles via metallurgical bonding. This thermomechanical processing may result in a material comprised of porous particulate iron with metallurgical bonds at the contact points between the particles. Materials produced by the disclosed methods can be used as components of battery electrodes. Electrodes produced by this method can be low-cost, mechanically robust, scalable to mass production, and high-performance. Materials and electrodes produced by the methods disclosed herein are particularly suitable for use in iron batteries for grid-scale energy storage, potentially enabling the large-scale adoption of renewable energy from intermittent energy sources such as wind and solar. Electrodes produced by these methods may be particularly attractive for commercial applications in long-term energy storage due to the small number of parts required for electrode assembly. Under appropriate processing conditions, electrodes produced by these methods may not require external current collection or packaging, but rather may be utilized as ready-to-use assemblies in electrochemical systems, saving parts and assembly costs compared to conventional electrode designs. In some embodiments, the disclosed methods can be scaled to very high production volumes with minor modifications to existing manufacturing equipment currently installed, with potential production volumes of millions of tons per year per plant. This level of productivity is unattainable with other battery electrode manufacturing methods. The combination of cost, performance, and manufacturing scalability of the disclosed methods entitles these battery electrodes to be used to store energy at the scale of hundreds of gigawatt hours with existing manufacturing equipment, representing a fast track to true grid-scale energy storage.

[0011] Various embodiments include an iron electrode comprising metallurgically bonded sponge iron particles, wherein the sponge iron particles have a microporosity of >50% by volume and a particle size of >100 μm.

[0012] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate exemplary embodiments of the claims and, together with the general description set forth above and the detailed description set forth below, serve to explain the features of the claims. [Brief explanation of the drawings]

[0013]

[0014]

[0015]

[0016]

[0017]

[0018]

[0019]

[0020]

[0021]

[0022]

[0023]

[0024]

[0025]

[0026] [Figure 1] A comparison of the levels of deformation is shown. [Figure 2] 1 illustrates an embodiment of hot roll consolidation that produces a mechanically and electrically connected material. [Figure 3] An example of a comparison between unimodal and bimodal filling is shown. [Figure 4]1 illustrates the relationship between electrode thickness, DRI pellet size, and layer size. [Figure 5] FIG. 1 is an Ellingham diagram of various elements. [Figure 6] Iron-carbon phase diagram. [Figure 7] 10A-10C illustrate examples of tooling and pressing operations to form channeled electrodes, according to various embodiments. [Figure 8] 10A-10C illustrate examples of tooling and pressing operations to form channeled electrodes, according to various embodiments. [Figure 9] 1 shows an example of a toothed roller that may be suitable for forming a channeled electrode, according to various embodiments. [Figure 10] 1 shows an overview of an example of a channeled electrode, according to various embodiments. [Figure 11] An example of a textured roller and an example of a procedure for using such a textured roller to form a channeled electrode according to various embodiments is provided. [Figure 12] FIG. 10 shows a side view of one example of a cutting or separation mechanism being used to separate sheets of formed electrodes. [Figure 13] 10 illustrates examples of electrode connections according to various embodiments. [Figure 14] 1 is an example of a structural facing application in accordance with various embodiments. [Figure 15] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 16] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 17] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 18]1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 19] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 20] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 21] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 22] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. [Figure 23] 1A-1C illustrate various exemplary systems in which one or more aspects of various embodiments may be used as part of a bulk energy storage system. DETAILED DESCRIPTION OF THE INVENTION

[0027] Various embodiments will be described in detail with reference to the accompanying drawings. Wherever possible, the same reference numbers will be used throughout the drawings to refer to the same or like parts. References to specific examples and implementations are for illustrative purposes only and are not intended to limit the scope of the claims. The following description of embodiments of the invention is not intended to limit the invention to those embodiments, but rather to enable one of ordinary skill in the art to make and use the invention. Unless otherwise noted, the accompanying drawings are not drawn to scale.

[0028] As used herein, unless otherwise specified, room temperature is 25° C. and standard temperature and pressure are 25° C. and 1 atmosphere. Unless expressly stated otherwise, all tests, test results, physical properties, and values ​​that are temperature-dependent, pressure-dependent, or both, are provided at standard ambient temperature and pressure.

[0029] In general, the term "about" and the symbol "about," as used herein, unless otherwise specified, are meant to encompass a variation or range of ±10%, the experimental or instrumental error associated with obtaining a stated value, preferably whichever is greater.

[0030] As used herein, unless otherwise stated, the recitation of ranges of values ​​herein is merely intended to serve as a shorthand method of referring individually to each separate value falling within the range. Unless otherwise indicated herein, each separate value within a range is incorporated herein as if it were individually recited herein.

[0031] As used herein, unless otherwise specified, the terms "%," "wt. %," and "mass %" are used interchangeably and refer to the weight of a first component as a percentage of the weight of a total, e.g., formulation, mixture, particle, pellet, agglomerate, material, structure, or product. As used herein, unless otherwise specified, "volume %" and "% volume" and similar such terms refer to the volume of a first component as a percentage of the volume of a total, e.g., formulation, mixture, particle, pellet, agglomerate, material, structure, or product.

[0032] The term "microporous," as used herein, refers to materials that have pores (i.e., porosity) with characteristic length scales of tens of microns or less.

[0033] The expression "volume percent microporosity within a particle," as used herein, refers to the volume fraction of three-dimensionally permeating voids within a particle that is microporous (i.e., the geometric envelope of the particle). After thermomechanical processing, the term is used to mean the volume fraction of three-dimensionally permeating voids within the region occupied by the material of the original particle after deformation. More simply stated, although the particle is deformed, in most cases, some degree of discernment of the original single particle is possible where the deformation is not particularly severe. The volume percent microporosity within a particle after thermomechanical processing is the porosity within the discernible region of the original particle.

[0034] The following examples are provided to illustrate various embodiments of the present systems and methods of the present invention. These examples are intended to be illustrative and may be prophetic, and should not be considered limiting or in any way restrict the scope of the invention.

[0035] It should be noted that there is no requirement to provide or express the theory underlying any novel and innovative process, material, performance, or other beneficial features and characteristics that are the subject of or associated with embodiments of the present invention. Nevertheless, various theories are provided herein to further advance the art. The theories presented herein are not intended to limit, restrict, or narrow in any way the scope of protection afforded to the claimed invention, unless expressly stated otherwise. Such theories may not be necessary for the utilization of the present invention or may not be put into practice. Furthermore, it is understood that the present invention may rely on new and previously unknown theories to explain the function-characteristics of embodiments of the methods, articles, materials, devices, and systems of the present invention. Such subsequently developed theories shall not limit the scope of protection afforded to the present invention.

[0036] The various embodiments of the systems, equipment, techniques, methods, activities, and operations described herein can be used in a variety of other activities and fields in addition to those described herein. In addition, such embodiments can be used, for example, with other equipment or activities that may be developed in the future and with existing equipment or activities that may be modified based on the teachings herein. Furthermore, the various embodiments and examples described herein can be used with each other, in whole or in part, and in various different combinations. Thus, the configurations provided in the various embodiments herein can be used with each other. For example, elements of an embodiment having A, A', and B and elements of an embodiment having A", C, and D can be used with each other in various combinations, e.g., A, C, D, and A, A", C, D, etc., in accordance with the teachings herein. Thus, the scope of protection afforded the present invention should not be limited to the specific embodiments, configurations, or arrangements shown in the specific embodiments, examples, or in the specific illustrated embodiments.

[0037] As used herein, unless otherwise specified, the term "specific gravity," also called apparent density, should be given the broadest possible meaning and generally refers to the weight per unit volume of a structure, e.g., a volumetric form of a material. This property will include the internal porosity of a particle as part of its volume. It can be measured, among other techniques, with a low viscosity fluid wetting the particle surface.

[0038] As used herein, unless otherwise specified, the term "actual density," which may also be referred to as true density, should be given the broadest possible meaning and generally refers to the weight per unit volume of a material if no voids were present in that material. This measurement and property essentially excludes internal porosity from the material, e.g., does not include any voids in the material.

[0039] Therefore, a collection of porous foam balls (e.g., Nerf® balls) can be used to illustrate the relationship between the three density properties: The weight of the ball filling a container would be the bulk density of the ball.

number

[0040] The weight of a single ball per spherical volume of the ball would be its apparent density.

number

[0041] The weight of the material that makes up the ball's skeleton, i.e., the ball with all void volume removed, per remaining volume of that material would be the skeleton density.

number

[0042] As used herein, unless otherwise specified, the terms agglomerate and agglomerate should be given the broadest possible meaning and generally refer to an aggregation of powder-like particles.

[0043] Embodiments of the present invention include devices, systems, and methods for long-term and ultra-long-term low-cost energy storage. As used herein, "long-term" and "ultra-long-term" and similar such terms shall be given the broadest possible meaning unless expressly stated otherwise and shall include energy storage periods of 8 hours or longer, such as an 8-hour energy storage period, an energy storage period ranging from 8 hours to 20 hours, a 20-hour energy storage period, an energy storage period ranging from 20 hours to 24 hours, a 24-hour energy storage period, an energy storage period ranging from 24 hours to one week, and an energy storage period ranging from one week to one year (e.g., from days to weeks, to months, etc.), and shall include LODES systems. Furthermore, the terms "long-term" and "ultra-long-term," "energy storage cell," including "electrochemical cell," and similar such terms shall be given the broadest possible interpretation unless expressly stated otherwise and shall include electrochemical cells that may be configured to store energy for time periods of days, weeks, or seasons.

[0044] Generally, in embodiments, the long-term energy storage cell may be a long-term electrochemical cell. Generally, this long-term electrochemical cell can store electricity generated by a power generation system when: (i) the power source or fuel for that generation is available, abundant, inexpensive, and combinations and variations thereof; (ii) the power needs or demands of the power grid, customers, or other users are less than the amount of electricity generated by the power generation system, the price paid to provide such power to the power grid, customers, or other users is below the economically efficient point for generating such power (e.g., when the cost of generation exceeds the market price for electricity), and combinations and variations thereof; and (iii) combinations and variations of (i) and (ii), and other reasons. This electricity stored in the long-term electrochemical cell can then be distributed to the power grid, customers, or other users when economical or otherwise needed. For example, the electrochemical cell may be configured to store energy generated by solar cells during summer months when sunlight is abundant and solar power generation exceeds grid needs, and to discharge the stored energy during winter months when sunlight may be insufficient to meet grid needs.

[0045] Various embodiments are discussed regarding the use of direct reduced iron (DRI) as a battery (or cell) material, as a battery (or cell) component, and combinations and variations thereof. In various embodiments, DRI may be produced from or be material obtained from the reduction of natural or processed iron ore, where such reduction is carried out without reaching the melting temperature of iron. In various embodiments, the iron ore may be taconite, magnetite, hematite, goethite, or the like. In various embodiments, DRI may be in the form of pellets, which may be spherical or substantially spherical. In various embodiments, DRI may be porous and contain open and / or closed pores. In various embodiments, DRI may include material that has been further processed by hot or cold briquetting. In various embodiments, DRI is produced by reducing iron ore pellets to produce iron metal (Fe 0DRI can be produced by forming more metallic (more reduced, less oxidized) materials such as iron ore taconite, wüstite (FeO), or composite pellets containing iron metal and residual oxide phases. In various non-limiting embodiments, DRI may be reduced iron ore taconite, direct reduced (“DR”) taconite, reduced “blast furnace (BF) grade” pellets, reduced “electric arc furnace (EAF) grade” pellets, “cold direct reduced iron (CDRI)” pellets, DRI pellets, hot briquette iron (HBI), or any combination thereof. In the iron and steel industry, DRI is sometimes referred to as “sponge iron,” and its use is particularly common in India. Iron material embodiments, including exemplary embodiments of DRI materials for use in various embodiments described herein, including use as electrode materials, may have one, more than one, or all of the material properties as set forth in Table 1 below. As used herein, including in Table 1, the following terms have the following meanings unless expressly stated otherwise: "specific surface area" means the total surface area of ​​a material per unit mass, including the surface area of ​​pores in a porous structure; "carbon content" or "carbon (wt%)" means the mass of total carbon as a percentage of the total mass of the DRI; "cementite content" or "cementite (wt%)" means the mass of FeC as a percentage of the total mass of the DRI; "total Fe (wt%)" means the mass of all iron as a percentage of the total mass of the DRI; "metallic Fe (wt%)" means the mass of Fe as a percentage of the total mass of the DRI. 0 "Metallization" means the mass of iron in the Fe state as a percentage of the total mass of iron; 0 As used herein, weight and volume percentages and apparent densities are understood to exclude any pore-infiltrating electrolyte or transient additives within the pores, unless otherwise stated. [Table 1]

[0046] *The specific surface area is preferably determined by the Brunauer-Emmett-Teller adsorption method ("BET"), more preferably BET as set forth in ISO 9277, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as methylene blue (MB) staining, ethylene glycol monoethyl ether (EGME) adsorption, electrokinetic analysis of complex ion adsorption, and protein retention (PR) methods, can be used to provide results that can be correlated with BET results.

[0047] ** Actual density is preferably determined by helium (He) pycnometer method, more preferably as set forth in ISO 12154, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Actual density is sometimes also referred to in the art as "true density" or "skeletal density."

[0048] *** Apparent density is preferably determined by immersion in water, more preferably as set forth in ISO 15968, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Porosity can be defined as the ratio of apparent density to actual density.

number

[0049] **** d 孔、90%容積 is preferably determined by mercury (Hg) intrusion porosimetry, more preferably as set forth in ISO 15901-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as gas adsorption, can be used to provide results that can be correlated with Hg intrusion results. 孔、90%容積is the pore diameter above which 90% of the total pore volume resides.

[0050] ***** d 孔、50%表面積 is preferably determined by mercury (Hg) intrusion porosimetry, more preferably as set forth in ISO 15901-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as gas adsorption, can be used to provide results that can be correlated with Hg intrusion results. 孔、50%表面積 is the pore diameter above which 50% of the free surface area resides.

[0051] #Total Fe (wt%) is preferably determined by dichromate titration, more preferably as set forth in ASTM E246-10, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as tin(II) chloride reduction followed by titration, titanium(III) chloride reduction followed by titration, and inductively coupled plasma (ICP) spectroscopy, can be used to provide results that can be correlated to the dichromate titration method.

[0052] ##Metallic Fe (wt%) is preferably determined by iron(III) chloride titration, more preferably as set forth in ISO 16878, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as bromine-methanol titration, can be used to provide results that can be correlated to iron(III) chloride titration.

[0053] ### Metallization (%) is preferably determined by the ratio of metallic Fe to total Fe, each preferably determined by the method described above.

[0054] #### Carbon (wt%) is preferably determined by infrared absorption after induction furnace firing, more preferably as set forth in ISO 9556, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as various combustion and inert gas fusion techniques such as those set forth in ASTM E1019-18, can be used to provide results that can be correlated to infrared absorption after induction furnace firing.

[0055] #####Fe 2+ (wt %) is preferably determined by titration, more preferably as set forth in ASTM D3872-05, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as Mössbauer spectroscopy, X-ray absorption spectroscopy, and the like, can be used to provide results that can be correlated to titration.

[0056] $Fe 3+ (wt%) is preferably total Fe (wt%), metallic Fe (wt%), Fe 2+ (wt%), and Fe 3+ It is determined by the mass balance relationship between or within these (wt%). Specifically, total Fe (wt%) = metallic Fe (wt%) + Fe 2+ (Weight%)+Fe 3+ (wt%) must be true due to the law of conservation of mass, so Fe 3+ (wt%) is Fe 3+ (wt%) = total Fe (wt%) - metallic Fe (wt%) - Fe 2+ It can be calculated as a percentage by weight.

[0057] $$SiO2 (wt%) is preferably determined gravimetrically, more preferably as set forth in ISO 2598-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as reduced molybdosilicate spectrophotometry, X-ray diffraction (XRD), and the like, can be used to provide results that can be correlated to gravimetric methods. In certain methods, SiO2 wt% is not determined directly; rather, the Si concentration (including neutral and ionic species) is measured and SiO2 wt% is calculated assuming SiO2 stoichiometry, i.e., a molar ratio of Si:O of 1:2 is assumed.

[0058] $$$Ferrite (wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0059] $$$$Wüstite (FeO, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0060] $$$$$Goethite (FeOOH, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0061] + Cementite (Fe3C, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0062] Additionally, embodiments of iron materials (e.g., including embodiments of DRI materials) for use in various embodiments described herein, including for use as electrode materials, may have one or more of the following properties, characteristics, or features, as shown in Table 2 (note that values ​​in one row or one column may be present with values ​​in different rows or columns): [Table 2]

[0063] Total Fe (wt%) is preferably determined by dichromate titration, more preferably as set forth in ASTM E246-10, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as tin(II) chloride reduction titration, titanium(III) chloride reduction titration, and inductively coupled plasma (ICP) spectroscopy, can be used to provide results that can be correlated to the dichromate titration method.

[0064] !!SiO2 (wt%) is preferably determined gravimetrically, more preferably as set forth in ISO 2598-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as reduced molybdosilicate spectrophotometry, X-ray diffraction (XRD), and the like, can be used to provide results that can be correlated to gravimetric methods. In certain methods, SiO2 wt% is not determined directly; rather, the Si concentration (including neutral and ionic species) is measured and SiO2 wt% is calculated assuming SiO2 stoichiometry. That is, a molar ratio of Si:O of 1:2 is assumed.

[0065] Al2O3 (wt%) is preferably determined by flame atomic absorption spectrometry, more preferably as set forth in ISO 4688-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as X-ray diffraction (XRD), can be used to provide results that can be correlated to flame atomic absorption spectrometry. In certain methods, Al2O3 wt% is not determined directly; rather, the Al concentration (including neutral and ionic species) is measured and Al2O3 wt% is calculated assuming Al2O3 stoichiometry; that is, a molar ratio of Al:O of 2:3 is assumed.

[0066] !!!!MgO (wt%) is preferably determined by flame atomic absorption spectrometry, more preferably as set forth in ISO 10204, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as X-ray diffraction (XRD), can be used to provide results that can be correlated to flame atomic absorption spectrometry. In certain methods, MgO wt% is not determined directly; rather, the Mg concentration (including neutral and ionic species) is measured and the MgO wt% is calculated assuming MgO stoichiometry; that is, a 1:1 molar ratio of Mg:O is assumed.

[0067] !!!!!CaO (wt%) is preferably determined by flame atomic absorption spectrometry, more preferably as set forth in ISO 10203, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as X-ray diffraction (XRD), can be used to provide results that can be correlated to flame atomic absorption spectrometry. In certain methods, CaO wt% is not determined directly; rather, the Ca concentration (including neutral and ionic species) is measured and CaO wt% is calculated assuming CaO stoichiometry; that is, a 1:1 molar ratio of Ca:O is assumed.

[0068] & TiO2 (wt%) is preferably determined by diantipyrylmethane spectrophotometry, more preferably as set forth in ISO 4691, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as X-ray diffraction (XRD), can be used to provide results that can be correlated to diantipyrylmethane spectrophotometry. In certain methods, TiO2 wt% is not determined directly; rather, the Ti concentration (including neutral and ionic species) is measured and TiO2 wt% is calculated assuming TiO2 stoichiometry; that is, a molar ratio of Ti:O is assumed to be 1:2.

[0069] && Actual density is preferably determined by helium (He) pycnometer method, more preferably as set forth in ISO 12154, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Actual density is sometimes also referred to in the art as "true density" or "skeletal density."

[0070] &&& Apparent density is preferably determined by immersion in water, more preferably as set forth in ISO 15968, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results.

[0071] Bulk density (kg / m 3 ) is preferably determined by measuring the mass of a test portion introduced into a container of known volume until its surface is filled to the brim, more preferably as set forth in Method 2 of ISO 3852, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with those of gravimetric methods.

[0072] &&&&& The porosity is preferably determined by the ratio of the apparent density to the actual density.

number

[0073] Also, the properties shown in Table 1 may be present in embodiments along with, in addition to, or instead of the properties in Table 2. Also, greater and lesser values ​​of such properties may be present in various embodiments.

[0074] In an embodiment, the specific surface area of ​​the pellet is about 0.05 m 2 / g ~ approx. 35m 2 / g, approx. 0.1m 2 / g~about 5m 2 / g, approx. 0.5m 2 / g~about 10m 2 / g, approx. 0.2m 2 / g~about 5m 2 / g, approx. 1m 2 / g~about 5m 2 / g, approx. 1m 2 / g~about 20m 2 / g, and about 1m 2 / g, and may be greater than about 2m 2 / g, and may be greater than about 5m 2 / g, and may be less than about 15m 2 / g, and may be less than about 20m 2 / g, as well as combinations and variations thereof, and larger and smaller values.

[0075] Generally, iron ore pellets are produced by crushing, grinding, or milling iron ore into a fine, powder-like form, which is then concentrated by removing impurity phases (so-called "gangue") liberated by the grinding operation. Generally, grinding the ore to a finer (smaller) particle size increases the purity of the resulting concentrate. The concentrate is then formed into pellets by a pelletizing or balling process (e.g., using a drum or disc pelletizer). Producing higher purity ore pellets generally requires a greater energy input. Iron ore pellets are generally commercially or sold in two main categories: blast furnace (BF)-grade pellets and direct reduction (DR-grade) (sometimes also referred to as electric arc furnace (EAF)-grade), with the primary difference being the content of SiO2 and higher amounts of other impurity phases in BF-grade pellets compared to DR-grade pellets. Typical critical specifications for DR grade pellets or feedstock are a total Fe content by mass in the range of 63-69 wt%, such as 67 wt%, and a SiO2 content by mass of less than 3 wt%, such as 1 wt%. Typical critical specifications for BF grade pellets or feedstock are a total Fe content by mass in the range of 60-67 wt%, such as 63 wt%, and a SiO2 content by mass in the range of 2-8 wt%, such as 4 wt%.

[0076] In certain embodiments, DRI can be produced by the reduction of "blast furnace" pellets, in which case the resulting DRI may have material properties as set forth below in Table 3. The use of reduced BF grade DRI can be advantageous because less input energy is required to produce the pellets, which translates to a lower cost of the finished product. [Table 3]

[0077] *The specific surface area is preferably determined by the Brunauer-Emmett-Teller adsorption method ("BET"), more preferably BET as set forth in ISO 9277, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as methylene blue (MB) staining, ethylene glycol monoethyl ether (EGME) adsorption, electrokinetic analysis of complex ion adsorption, and protein retention (PR) methods, can be used to provide results that can be correlated with BET results.

[0078] ** Actual density is preferably determined by helium (He) pycnometer method, more preferably as set forth in ISO 12154, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Actual density is sometimes also referred to in the art as "true density" or "skeletal density."

[0079] *** Apparent density is preferably determined by immersion in water, more preferably as set forth in ISO 15968, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Porosity can be defined as the ratio of apparent density to actual density.

number

[0080] **** d 孔、90%容積 is preferably determined by mercury (Hg) intrusion porosimetry, more preferably as set forth in ISO 15901-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as gas adsorption, can be used to provide results that can be correlated with Hg intrusion results. 孔、90%容積is the pore diameter above which 90% of the total pore volume resides.

[0081] ***** d 孔、50%表面積 is preferably determined by mercury (Hg) intrusion porosimetry, more preferably as set forth in ISO 15901-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as gas adsorption, can be used to provide results that can be correlated with Hg intrusion results. 孔、50%表面積 is the pore diameter above which 50% of the free surface area resides.

[0082] #Total Fe (wt%) is preferably determined by dichromate titration, more preferably as set forth in ASTM E246-10, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as tin(II) chloride reduction followed by titration, titanium(III) chloride reduction followed by titration, and inductively coupled plasma (ICP) spectroscopy, can be used to provide results that can be correlated to the dichromate titration method.

[0083] ##Metallic Fe (wt%) is preferably determined by iron(III) chloride titration, more preferably as set forth in ISO 16878, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as bromine-methanol titration, can be used to provide results that can be correlated to iron(III) chloride titration.

[0084] ### Metallization (%) is preferably determined by the ratio of metallic Fe to total Fe, each preferably determined by the method described above.

[0085] #### Carbon (wt%) is preferably determined by infrared absorption after induction furnace firing, more preferably as set forth in ISO 9556, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as various combustion and inert gas fusion techniques such as those set forth in ASTM E1019-18, can be used to provide results that can be correlated to infrared absorption after induction furnace firing.

[0086] #####Fe 2+ (wt %) is preferably determined by titration, more preferably as set forth in ASTM D3872-05, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as Mössbauer spectroscopy, X-ray absorption spectroscopy, and the like, can be used to provide results that can be correlated to titration.

[0087] Fe 3+ (wt%) is preferably total Fe (wt%), metallic Fe (wt%), Fe 2+ (wt%), and Fe 3+ It is determined by the mass balance relationship between or within these (wt%). Specifically, total Fe (wt%) = metallic Fe (wt%) + Fe 2+ (Weight%)+Fe 3+ (wt%) must be true due to the law of conservation of mass, so Fe 3+ (wt%) is Fe 3+ (wt%) = total Fe (wt%) - metallic Fe (wt%) - Fe 2+ It can be calculated as a percentage by weight.

[0088] $$SiO2 (wt%) is preferably determined gravimetrically, more preferably as set forth in ISO 2598-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as reduced molybdosilicate spectrophotometry, X-ray diffraction (XRD), and the like, can be used to provide results that can be correlated to gravimetric methods. In certain methods, SiO2 wt% is not determined directly; rather, the Si concentration (including neutral and ionic species) is measured and SiO2 wt% is calculated assuming SiO2 stoichiometry, i.e., a molar ratio of Si:O of 1:2 is assumed.

[0089] $$$Ferrite (wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0090] $$$$Wüstite (FeO, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0091] $$$$$Goethite (FeOOH, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0092] + Cementite (Fe3C, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0093] Also, the properties shown in Table 3 may be present in embodiments along with, in addition to, or instead of the properties in Tables 1 and / or 2. Also, greater and lesser values ​​of such properties may be present in various embodiments.

[0094] In certain embodiments, DRI can be produced by reduction of DR grade pellets, in which case the resulting DRI may have material properties as set forth below in Table 4. The use of reduced DR grade DRI can be advantageous due to the higher Fe content in the pellets, which increases the energy density of the battery. [Table 4]

[0095] * The specific surface area is preferably determined by the Brunauer-Emmett-Teller adsorption method ("BET"), more preferably BET as set forth in ISO 9277, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as methylene blue (MB) staining, ethylene glycol monoethyl ether (EGME) adsorption, electrokinetic analysis of complex ion adsorption, and protein retention (PR) methods, can be used to provide results that can be correlated with BET results.

[0096] ** Actual density is preferably determined by helium (He) pycnometer method, more preferably as set forth in ISO 12154, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Actual density is sometimes also referred to in the art as "true density" or "skeletal density."

[0097] *** Apparent density is preferably determined by immersion in water, more preferably as set forth in ISO 15968, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests can be used to provide results that can be correlated with He pycnometer results. Porosity can be defined as the ratio of apparent density to actual density.

number

[0098] **** d 孔、90%容積is preferably determined by mercury (Hg) intrusion porosimetry, more preferably as set forth in ISO 1 5901-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as gas adsorption, can be used to provide results that can be correlated with Hg intrusion results. 孔、90%容積 is the pore diameter above which 90% of the total pore volume resides.

[0099] ***** d 孔、50%表面積 is preferably determined by mercury (Hg) intrusion porosimetry, more preferably as set forth in ISO 15901-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as gas adsorption, can be used to provide results that can be correlated with Hg intrusion results. 孔、50%表面積 is the pore diameter above which 50% of the free surface area resides.

[0100] #Total Fe (wt%) is preferably determined by dichromate titration, more preferably as set forth in ASTM E246-10, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as tin(II) chloride reduction followed by titration, titanium(III) chloride reduction followed by titration, and inductively coupled plasma (ICP) spectroscopy, can be used to provide results that can be correlated to the dichromate titration method.

[0101] ##Metallic Fe (wt%) is preferably determined by iron(III) chloride titration, more preferably as set forth in ISO 16878, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as bromine-methanol titration, can be used to provide results that can be correlated to iron(III) chloride titration.

[0102] ### Metallization (%) is preferably determined by the ratio of metallic Fe to total Fe, each preferably determined by the method described above.

[0103] #### Carbon (wt%) is preferably determined by infrared absorption after induction furnace firing, more preferably as set forth in ISO 9556, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as various combustion and inert gas fusion techniques such as those set forth in ASTM E1019-18, can be used to provide results that can be correlated to infrared absorption after induction furnace firing.

[0104] #####Fe 2+ (wt %) is preferably determined by titration, more preferably as set forth in ASTM D3872-05, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as Mössbauer spectroscopy, X-ray absorption spectroscopy, and the like, can be used to provide results that can be correlated to titration.

[0105] $Fe 3+ (wt%) is preferably total Fe (wt%), metallic Fe (wt%), Fe 2+ (wt%), and Fe 3+ The mass balance relationship between and within these (wt%) is determined by: Total Fe (wt%) = Metallic Fe (wt%) + Fe 2+ (Weight%)+Fe 3+ (wt%) must be true due to the law of conservation of mass, so Fe 3+ (wt%) is Fe 3+ (wt%) = total Fe (wt%) - metallic Fe (wt%) - Fe 2+ It can be calculated as a percentage by weight.

[0106] $$SiO2 (wt%) is preferably determined gravimetrically, more preferably as set forth in ISO 2598-1, the disclosure of which is incorporated herein by reference in its entirety. It is recognized that other tests, such as reduced molybdosilicate spectrophotometry, X-ray diffraction (XRD), and the like, can be used to provide results that can be correlated to gravimetric methods. In certain methods, SiO2 wt% is not determined directly; rather, the Si concentration (including neutral and ionic species) is measured and SiO2 wt% is calculated assuming SiO2 stoichiometry, i.e., a molar ratio of Si:O of 1:2 is assumed.

[0107] $$$Ferrite (wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0108] $$$$Wüstite (FeO, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0109] $$$$$Goethite (FeOOH, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0110] + Cementite (Fe3C, wt%, XRD) is preferably determined by X-ray diffraction (XRD).

[0111] Also, the properties shown in Table 4 may be present in an embodiment along with, in addition to, or instead of the properties in Tables 1, 2, and / or 3. Also, greater and lesser values ​​of such properties may be present in various embodiments.

[0112] Electrochemical cells, such as batteries, store electrochemical energy by using differences in electrochemical potential to generate a voltage difference between positive and negative electrodes. When the electrodes are connected by a conductive element, this voltage difference produces an electric current. In a battery, the negative and positive electrodes are connected in parallel by external and internal conductive elements. Generally, the external element conducts electrons, and the internal element (electrolyte) conducts ions. Because no charge imbalance is allowed between the negative and positive electrodes, the two must supply ions and electrons at the same rate. During operation, the electronic current can be used to power an external device. Rechargeable batteries can be recharged by applying an opposite voltage difference, which drives the electronic and ionic currents to flow in the opposite direction to that of a discharging battery during use.

[0113] Generally, electrodes and electrode materials that are low cost and easy to manufacture are desirable, especially for long-term storage applications. Production and / or manufacturing processes can be evaluated and selected based on several criteria, including capital costs, material supply capabilities, operating costs, number of unit operations, number of material transfers, number of material handling steps, required energy inputs, amount of waste and / or by-products generated, etc.

[0114] Electrochemical cells, such as batteries, store electrochemical energy by exploiting differences in electrochemical potential to create a voltage difference between positive and negative electrodes. When the electrodes are connected by a conductive element, this voltage difference generates an electric current. In a battery, the negative and positive electrodes are connected in parallel by external and internal conductive elements. Generally, the external element conducts electrons, and the internal element (electrolyte) conducts ions. Because no charge imbalance is allowed between the negative and positive electrodes, the two must supply ions and electrons at the same rate. During operation, the electronic current can be used to power an external device. Rechargeable batteries can be recharged by applying an opposite voltage difference, which drives the electronic and ionic currents to flow in the opposite direction to that of a discharging battery during use.

[0115] Iron is an ideal electrode material due to its low cost, very high production yield, recyclability, and high theoretical and practical energy storage capacity in terms of stored energy per unit mass of material. The low material cost and high energy storage capacity result in a large amount of stored energy per unit mass of raw material. These factors, particularly the cost per unit mass of stored energy and production, are critical for long-term, grid-scale energy storage applications that are cost-sensitive and require the storage of very large amounts of energy. Iron is also inherently electrically conductive, which can simplify the problems encountered in many battery systems with charge uptake and release from battery electrode materials.

[0116] A central concern in the design of all battery electrodes is enabling the transport of electrons and ions to and from reaction sites. Generally, this requires interconnected porosity and a permeable, electrically conductive network for the electrolyte to transport the ions. In the iron battery electrodes disclosed herein, porous particulate iron provides the pores that are filled with caustic electrolyte. The permeable, electrically conductive network is provided by the iron material itself, with conductive metallurgical bonds formed by thermomechanical processing. The metallurgical bonds can occur through a combination of solid-state diffusion and bonding due to mechanically induced plasticity. Iron, in particular, forms much larger amounts of discharge products than iron metal itself. Therefore, to accommodate the microscopic formation of large amounts of discharge products, iron electrodes generally need a large amount of microporosity (>40%, with even larger amounts being preferred). Porous particulate iron materials satisfy the requirements of being inherently conductive and having a larger amount of microporosity. The methods described herein describe how to effectively bond these materials together to achieve high-performance electrodes at low cost.

[0117] The ideal electrical conductor for iron electrodes is iron itself, as its use as a conductor does not involve additional parts, assemblies, joints, or other design elements that add cost and complexity to the material. A central problem with forming metallurgical bonds between porous particulate iron materials is that many techniques used to join these metals are either poorly suited to joining porous materials or cause densification of microporosity or have other related issues. For example, arc welding results in vaporization of the porous iron material, sintering results in overall densification and the resulting loss of microporosity, and low-temperature mechanical compaction can result in poor electrical connection due to densification of the material and a lack of interdiffusion between particles. The problems associated with low-temperature mechanical compaction increase as the particle size of the particulate material increases, due to the material's greater tendency to flow / decompaction. High-temperature thermomechanical processing is uniquely suited to joining porous particulate iron particles for battery applications, as stress concentrations at the interparticle contacts can localize deformation (and the resulting bond) while simultaneously creating a metallurgical bond. The localized deformation avoids the loss of microporosity at points away from the contact points between particles.

[0118] Several forms of high temperature thermomechanical processing are already in use on a large scale, examples of which include uniaxial hot pressing, hot briquetting, and hot isostatic pressing.

[0119] Generally, high temperature thermomechanical processing involves the simultaneous application of high temperature and pressure to materials to deform and / or consolidate them. In this context, high temperature and pressure are used to achieve a metallurgical bond between porous particulate iron materials. For an exemplary embodiment, the process conditions are shown in Table 5 below, along with the ranges of the process parameters. [Table 5]

[0120] Similarly, a variety of material inputs are possible. These generally inherit their material composition and properties from the processing techniques used to produce them. For example, direct reduced iron materials have 50-70% volume porosity within the particles and ≥85% iron content by weight. High purity is generally preferred for more consistent, higher performance electrodes. Porous particulate iron materials have a reasonably high specific surface area (>0.003 m). 2 / g is preferred), high values ​​are preferred up to a point. A very high surface area can lead to excessive reactivity both during processing and use, and a specific surface area >3m 2 / g is too high. In contrast, sponge iron used in powder metallurgy automotive part manufacturing has much higher purity but substantially less porosity. Generally, electrode materials produced by the methods described herein can produce satisfactory performance when the final manufactured part contains >50% total microporosity. This porosity may be derived from microporosity within the particles fed into the high-temperature thermomechanical process, or it may result from a combination of intra-particle microporosity and microporosity resulting from inter-particle bond formation.

[0121] Guidance on adjusting process parameters based on material input characteristics and process changes

[0122] Due to the variety of mechanical properties achievable in porous particulate iron materials and the degree to which these properties can vary with thermomechanical processing, those skilled in the art will understand that the pressure and temperature ranges set forth herein may need to be modified based on the particular material being used. Some guidance is provided herein to assist with process modifications. If the porous particulate iron contains hardening phases or elements, such as carbon, the pressure required may be higher than those set forth herein to overcome the increased yield stress. The pressure generally scales with the yield of the material at the processing temperature and / or the indentation hardness of the material. Similarly, less porosity in a porous particulate iron material may require higher stresses for consolidation.

[0123] Preferred compact morphology

[0124] The deformation required for sufficient interparticle bonding varies depending on the type of input material used. For materials input as relatively large particles (>1 mm), the microporosity created by particle bonding can be negligible compared to the intraparticle microporosity. This is the case, for example, with direct reduced iron materials. In this case, to maintain sufficient porosity within the material, the consolidation process can be controlled so that the volumetric loss of porosity is low enough that the material maintains >50% intraparticle microporosity by volume after the consolidation process. Initially, this can be calculated from basic volume conservation and the volumetric engineering strain applied to the material. Thus, input materials with high initial intraparticle porosity can accommodate large deformations while maintaining >50% intraparticle microporosity by volume. In many cases, particles do not have sufficient initial porosity to allow the particles to undergo large bulk deformations. If excessive bulk deformation is undesirable, appropriate adjustments to the process can result in deformation only at the contact points, as outlined in Figures 1(A), 1(B), and 1(C).

[0125] Highly preferred inert atmosphere

[0126] In many cases, porous particulate iron can be insulating when handled as a bulk particulate. It may be preferable to preheat the material in equipment designed to uniformly heat the insulating material (a heated kiln or blender). In other cases, porous particulate iron may be produced using high-temperature processes, and the already hot material may be fed to a consolidation device. Such heating and feeding equipment may contain a substantially non-oxidizing atmosphere.

[0127] In many cases, the high surface area of ​​porous particulate iron allows undesirable oxidation to occur when the material is exposed to oxygen or other oxidizing agents at high temperatures. Therefore, a non-oxidizing atmosphere (e.g., an inert or reducing atmosphere) may be preferred during any portion of the process that occurs at high temperatures, and the fabricated part is typically cooled to a temperature where the reaction is slow (e.g., below 100°C) before being exposed to oxygen or other oxidizing agents. In some cases, it may be useful to passivate the material by exposing it to a small amount of oxygen before exposure to a larger amount of oxygen occurs. It should be further noted that the electrical connection between particles also serves as the thermal connection between particles. Thus, while a compacted body may be effectively convectively cooled from one side after fabrication (e.g., by passing it under a fan), one-sided convection is not a useful cooling technique for bulk particulate materials that are not in thermal communication with each other. Thus, in some embodiments, parts may be fabricated in an inert or reducing atmosphere, transferred to a belt after fabrication, and cooled by convection while maintaining a substantially non-oxidizing atmosphere. Passivation can occur simultaneously with or after cooling occurs. In some embodiments, the produced compacted body may be discharged at a high temperature into a storage chamber or other container filled with a substantially non-oxidizing atmosphere, cooled, and optionally passivated.

[0128] In some cases, it may not be possible to prevent oxidation during or after high-temperature thermomechanical processing to the desired extent. In such cases, oxidation may be removed from these surfaces by suitable means after electrode formation. For example, in some embodiments, surface oxides formed during or after processing may be electrochemically reduced within the battery system before or during cycling. In some embodiments, surface oxides formed during or after processing may be thermochemically reduced in a reducing gas stream before incorporation into the battery system. In some embodiments, surface oxides may be chemically reduced by the introduction of a suitable reducing solution. Suitable acids for reducing iron surface oxides include acids used in etching or pickling steel, such as solutions containing nitric acid, sulfuric acid, and acetic acid.

[0129] High temperature thermomechanical processing may be carried out by suitable application. Thus, in various embodiments, pressure and / or heat may be applied by one or more of the following processing techniques: hot isostatic pressing (HIP), uniaxial hot pressing, hot roll consolidation (which may be uniaxial or biaxial), hot briquetting (using rolling in some embodiments, and possibly uniaxial consolidation), or hot forging. Specific methods for producing geometries suitable for use as battery electrodes are discussed below for each processing technique, with particular attention to electrodes suitable for long-term energy storage.

[0130] Using hot isostatic pressing, large billets of material can be economically produced with precise levels of compaction by appropriate selection of time-temperature-pressure schedules. The application of HIP differs in that in this context, full or near-full densification is not the goal, but rather the consolidation of material in an economical manner. In some embodiments, the electrode shape is constructed into the can used to consolidate the material, and the output of the HIP process yields a useful electrode. In some embodiments, to reduce the cost of can manufacturing, very large cans are produced and cut from the billet resulting from the HIP process. The temperature and pressure conditions described above can be used as a starting point for tailoring the HIP process to a given material and electrode application.

[0131] Uniaxial hot pressing can be used to produce large billets when low compaction pressures are required. In many cases, the compaction pressures required, as well as the temperatures required, are much lower than in typical hot pressing applications. Therefore, the unit cost of hot pressing can be substantially reduced compared to typical applications. In some embodiments, a steel hot press may be inserted, material may be metered into the press, and the material may be automatically pressed. This process may resemble uniaxial hot pressing in terms of the size of the articles produced, but may resemble hot briquetting in terms of parts produced per unit time and the time scale required for pressing. In some embodiments, particulate materials may be consolidated at high speeds and in very short periods of time, making the hot uniaxial compaction process most similar to hot forging.

[0132] Integrated Technology

[0133] Thermal spraying

[0134] Thermal spraying may be used to produce large billets from particles. The bonding, density, and other properties of the resulting compact can be advantageously adjusted by controlling process parameters such as speed, temperature, and direction, as well as the deposition rate of the sprayed particles. In one embodiment, the porous particulate iron particles are sprayed onto a substrate. The substrate can function as a current collector or structural reinforcement for the resulting billet. In another embodiment, to bond the porous particulate iron particles, bonding particles can be sprayed together with the porous particulate iron particles or onto a bed of prepared DRI particles.

[0135] Additive manufacturing using DRI laser sintering or laser melting (e.g., direct metal laser sintering (DMLS)) may be used to bond porous particulate iron particles together, thereby forming or adding to a large billet. In some embodiments, a layer-by-layer process may be used, in which one or more layers of particulate material are deposited and laser energy is applied to the entire layer or to selected areas within the layer. In some embodiments, one or more galvanometers, positioning systems, and / or optical components may be used to direct the laser energy to desired areas. In some embodiments, other directed energy deposition strategies, such as digital light processing (DLP) projection technology, microwave radiation, resistive heating, and electric arc heating, may be used instead of or in conjunction with a laser. Such methods may also be used for localized modification of one or more areas of an existing billet.

[0136] welding technology

[0137] In some embodiments, one or more welding techniques may be used to connect or consolidate the porous particulate iron particles (e.g., by forming a metallurgical bond between the particles of porous particulate iron, thereby forming the particles into a mechanically and / or electrically continuous billet). Such methods include alternating current (AC) resistance welding, direct current (DC) resistance welding, arc welding, explosion welding, forge welding, radio frequency (HF) welding, capacitive discharge welding, friction stir welding, and other conventional fusion welding techniques. In some embodiments, filler and / or flux materials may be used, for example, to enhance the bond or reduce or eliminate oxidation tendencies in the weld.

[0138] Ultrasonic compaction vibration includes ultrasonic vibration and may be used alone or in conjunction with other heating and agitation methods herein as one method of thermally or mechanically agitating the porous particulate iron. Vibration may also be used in combination with other pressing processes to aid in consistency, speed, bond strength, or other aspects of the compaction process.

[0139] Fabrication of Larger or Simpler Consolidated Bodies and Their Slicing or Post-Machining: In some embodiments, the formed billet may be larger than or otherwise different from the desired geometry of the electrode or its component, and the billet may then be sectioned, machined, assembled, or otherwise processed to a suitable intermediate or end-use shape. This can be advantageous in that tailoring the billet's morphology to suit the consolidation method used allows for low cost and high throughput when the billet is formed. Such billets may be formed using one or more suitable consolidation methods. The initial morphology may be similar to or substantially different from the desired morphology. In some embodiments, the initial morphology may include some of the desired geometry extending in one or more axes (e.g., a 2D profile extending in a third dimension), such that the desired shape is achieved by cutting the billet into slices. In other embodiments, the billet may require only localized machining or reshaping to achieve the desired shape. This sectioning or shaping may be achieved by using one or more cutting, splitting, milling, or crushing processes. Such processes include cutting by water jet, plasma, laser, oxy-fuel torch, and / or mechanical sawing. The billet material may also be chopped, sheared, scraped, snapped, bent, or formed into advantageous geometries. The resulting geometries may represent one or more complete electrodes, or electrode components, one or more of which may be assembled with other components to form an electrode.

[0140] Cold Consolidation. In some embodiments, the consolidation processes described above, particularly roll consolidation, isostatic pressing, and uniaxial pressing, may be carried out at room temperature or at temperatures substantially lower than those typically used in industry for a given consolidation process. Such low-temperature billet formation is advantageous in that it reduces or eliminates the complexity and cost associated with heating materials to high temperatures and the equipment required for high-temperature processing. This low-temperature processing may be achieved by appropriate adjustment of process parameters such as time or pressure, and by the incorporation or other modification of porous particulate iron. In some embodiments, the composition, microstructure, and / or shape of the iron particles may be formulated to facilitate billet formation at lower temperatures. In some embodiments, physical, chemical, or other surface treatments may be used to facilitate billet formation at lower temperatures.

[0141] As an alternative to cold bonding, cold extrusion can be used to create shapes designed to enhance electrode performance by increasing the available area of ​​the electrode. Cold extrusion can be used to create 3D serpentine blocks from ore slurry. The slurry passes as a block through a DRI reactor and is reduced to a high-surface-area iron block. The shape can be a sphere, cylinder, or any 3D shape that flows freely through the reduction reactor. Surface area can be further increased by adding holes or surface textures such as dimples and ribs. In some embodiments, additive materials, such as binders, that burn off at high temperatures during reduction may be used.

[0142] Alternatively, the iron oxide may be reduced to iron and then cold extrusion may be used to form the shapes described above.

[0143] Another method for creating complex 3D shapes with added porosity is to dry a slurry of iron ore using techniques common in the ceramics industry, such as plaster casting or mold casting, and then harden it in a high temperature oven. In other embodiments, such techniques can be used with reduced iron.

[0144] Non-uniform compaction temperature

[0145] In some embodiments, one or more regions of the material are at one or more different temperatures, potentially having large regions of higher and lower temperatures at different points in time and shape. This non-uniform temperature profile can be used to modify the behavior and properties of the porous iron material in ways that are advantageous for promoting favorable bonding, porosity, deformation, or other important properties. In some embodiments, the material is hottest on the surface of the flat electrode, thereby producing maximum strength at the edges and only minor deformation in the interior. The resulting electrode exhibits a useful combination of high bending strength from deformation near the hot surface while preserving the cooler interior porosity away from the surface.

[0146] Combining multiple billets, adding particles to an existing billet. In some embodiments, consolidation and bonding methods, including those described herein as methods for consolidating porous particulate iron, can also be applied to that billet, or some combination of porous particulate iron and that billet. Such methods can be used, for example, to bond one or more billets to another billet, or to bond additional porous particulate iron to an existing billet. Any such heating, pressing, welding, spraying, or other technique may be used one or more times in various sequences.

[0147] Electrode or billet shape

[0148] Any billet or electrode must have sufficient mechanical and electrical robustness to avoid damage throughout its entire life cycle, including any manufacturing, assembly, transportation, operation, service, and disposal procedures. The electrode or billet geometry may be selected in a manner that promotes that robustness. In some embodiments, the dimensions, thickness, and aspect ratio of the billet or electrode may be selected so that the geometry is sufficiently robust against various forms of fracture or degradation.

[0149] Channeled electrodes with enhanced performance characteristics

[0150] Generally, for many battery electrodes, especially thick-format electrodes, ion transport can limit the rate capacity of the electrode. In hot-consolidated, pressed, and sintered electrodes, particles deform to form a dense structure, resulting in reduced macroporosity for ion transport through the thickness of the anode. Furthermore, the resulting macroporosity can have high tortuosity and unfavorable alignment relative to the direction of ion transport. Therefore, there is a need for equipment designs and processing methods that enhance ion transport through the thickness of the electrode. Furthermore, in some hot-rolling processes for porous electrodes, it can be difficult to provide a surface for pressing the material against the electrode grips when low compaction is desired. Protruding features can mechanically interlock the rollers and material, allowing rolling to occur with less force. Textured or channeled electrodes with varying degrees of compaction and / or metallurgical bonding across the electrode area can usefully exhibit enhanced mechanical robustness and electrical conductivity properties.

[0151] Similar patterns of variable thickness channels and other engineered shapes in metallurgically bonded electrodes can be formed in a variety of ways.

[0152] The tool for manufacturing the electrode may be patterned with a plurality of protruding features (spikes, cones, rods, etc.), which eliminate material during the pressing process, resulting in macroporosity extending through the electrode thickness. This tool may then be used to press, roll, or otherwise mechanically manufacture the electrode. The electrode may be pressed for subsequent sintering, with the tool remaining on the electrode for at least a portion of the sintering process, or the tool may be used to press (in a hot or cold pressing operation) the electrode for subsequent use. In some embodiments, the area ratio and spacing of the protruding features may be optimally calculated to provide an optimal rate capacity / area capacity compromise for a particular application. In some embodiments, a rolling consolidation process may be used. The rolling consolidation process may use high temperatures above 300°C to metallurgically bond the electrode materials. The input material for electrode manufacturing may be iron or its derivatives. The electrode material may more specifically be sponge iron, direct reduced iron, or any other similar highly porous metallic iron material. Conical protrusions may be used to ensure adequate material flow around the protrusions and minimize tool wear. The angle of the protrusion may be selected or otherwise optimized to provide a pressing surface. Figures 7, 8(A), and 8(B) show examples of tooling and pressing operations to form channeled electrodes, according to various embodiments.

[0153] Toothed rollers can also be used to create patterns with channels in the electrode. Figure 9 shows an example of a toothed roller that may be suitable for forming channeled electrodes, according to various embodiments.

[0154] In a hot rolling press, rollers may be textured to intentionally increase the density of the hot-compressed material in specific locations. Increasing the material density serves two functions: (1) adding areas of high strength, improving handling, and (2) adding areas of high conductivity, providing a highway for electron flow. These features act as built-in / formed bus bars. Steel bus bars can then be welded directly to these areas to carry the current out of the electrode. FIG. 10(A) shows an overview of an example channeled electrode according to various embodiments. FIG. 10(B) shows a cross-section of a portion of the example channeled electrode of FIG. 10(A). FIG. 11(A) shows an example textured roller, and FIG. 11(B) shows an example operation of using two of the textured rollers of FIG. 11(A) to form a channeled electrode according to various embodiments. In a hot rolling press, rollers may be textured to intentionally increase the density of the hot-compressed material in specific locations. Increasing the material density serves two functions. These features can act as integrated / formed busbars. For example, steel busbars can then be welded directly to these areas to carry the current out of the electrode.

[0155] In a roll-consolidation process, the electrode may be separated into sheets by cutting or separating features built into the rollers, which impart features to the continuous sheet for periodic cutting or later separation of the sheet. The rollers may be compaction rollers, and the applied pressure may be generated at least in part by the compaction rollers. Figures 12(A)-12(C) show side views of an example of a cutting or separating mechanism used to separate sheets of formed electrodes. In Figures 12(A)-12(C), the formed electrode sheet is fed between rollers (downward in the direction shown). Figure 12(A) shows the formed electrode sheet being initially fed between the rollers. Figure 12(B) shows a cutting mechanism where two rollers rotate in opposite directions and meet to cut the formed electrode. Figure 12(C) shows the formed electrode sheet still being fed between the rollers, but now the section below the rollers has been cut.

[0156] In some embodiments, hot-roll consolidation or hot briquetting using rollers may be used to bond porous particulate iron material into a sheet of electrically conductive material. For example, FIG. 2 illustrates an embodiment of hot-roll consolidation, which produces a mechanically and electrically connected material. According to various embodiments, an electrode may be provided to an electrochemical system without applying an external current collector or filling the electrode. The sheet may be patterned or cut during the rolling process either to create a desired geometry for incorporation into a battery electrode or to aid in the subsequent formation of said geometry. Hot-roll consolidation techniques, such as hot briquetting, are used to produce densified briquettes from porous particulate iron, particularly DRI. The process of hot-briquetting DRI is referred to as the hot-briquette iron (HBI) process. In the HBI process, the goal is to densify DRI as much as possible (i.e., increase its density) to reduce the amount of microporosity for safer shipping and handling, thereby reducing the reactivity of the material. To create battery materials, it may be useful to reverse the concept of densifying HBI: such a briquetting process minimizes material densification while still achieving a strong, conductive metallurgical bond between the materials. This modification of the hot briquetting iron process has several important advantages. First, in the case of an in-line briquetting unit in a DRI plant, the material is already hot and in a reducing / protective atmosphere. This essentially eliminates the costs associated with these aspects of thermomechanical processing. Second, the process is continuous and high-throughput (some HBI plants produce >1 million tons of HBI per year). Third, the briquetting process is inexpensive, adding only a small amount to the cost of steelmaking inputs. Finally, hot briquetting machines already incorporate a cutting mechanism to convert the continuous sheet of briquette material into a set of discrete electrodes. To avoid collapse of the microporosity, the briquetting process generally occurs at operating conditions different from those typically applied to the production of high-density HBI products. The parameters are specific to the electrode geometry being fabricated and the material being consolidated, but may be found empirically.First, the DRI temperature during pressing may be reduced to limit softening of the iron and maintain internal porosity. Second, the pressure applied to the rolls may be reduced or even varied to a certain limit. Third, the rolling speed may be reduced to increase the time the iron is under pressure and enhance its ability to form interparticle bonds. Fourth, the gap between the rolls may be controlled to a higher tolerance to produce a uniform thickness in the compacted electrode.

[0157] Material handling and modification before integration of iron electrodes

[0158] Material handling for producing metallurgically bonded iron electrodes presents several challenges. First, the materials must be blended and maintained throughout feeding. Second, the weight and volume of the materials must be controlled to minimize heterogeneity within and between electrodes. Third, the materials must be properly processed and prepared for bonding via any applicable heating and desired chemical reactions. Fourth, any other applicable materials required for inclusion in the electrode must be fed into an appropriate device for bonding particulate materials.

[0159] Surface Preparation: The surface of the material may optionally be prepared by the following surface preparation methods. Surface preparation may be performed at numerous points during material processing and handling. To achieve the desired bonding between the iron particles, it may be necessary to remove impurities or detrimental phases from the surface that interfere with, delay, or prevent metallurgical bonding. Of particular importance are oxide coatings often associated with DRI manufacturing; these inorganic compounds are designed to prevent adhesion during DRI manufacturing and therefore interfere with bonding in subsequent operations. Commonly used techniques, such as solvent cleaning, acid etching, and sand / shot blasting, may be used prior to heating and consolidation.

[0160] Heating: In many consolidation and / or metallurgical joining processes, it may be desirable or necessary to heat the materials prior to the joining or consolidation step itself. For example, temperatures >400°C are often required to achieve a metallurgical bond via a hot consolidation process. Similarly, in many welding processes (e.g., resistance welding), preheating the material enhances the consistency and quality of the bond. Ferrous materials can be heated in a number of ways. In some cases, porous ferrous materials may be heated by radiant and / or electric heaters, by inductive coupling to the porous ferrous material itself, or by being placed in the presence of a combustion gas atmosphere. Porous ferrous materials may also self-heat by the introduction of oxygen into the process atmosphere and its reaction with the porous ferrous material. Mechanical actions such as crushing, rotating, stirring, ultrasonic agitation, etc. can also be used as a means of heating, regardless of whether other purposes are achieved using these actions. Materials may additionally or alternatively be preheated and stored in bulk in insulated storage containers to maintain moisture-free conditions and eliminate the need for rapid heating. Heating may be carried out in a continuous furnace such as a rotary hearth furnace, rotary kiln, linear hearth furnace, tunnel furnace, or linear grate furnace. In some cases, the heating atmosphere may be devised to achieve a chemical transformation of the porous ferrous material.

[0161] Particle Size Control and Blending: Porous particulate iron materials may be size reduced, classified by size, and blended to achieve optimal particle characteristics for the formation of metallurgically bonded electrodes. Particle size reduction may occur via any one of the techniques known in the art for particle size reduction of particulate materials, including, but not limited to, high-pressure grinding rolls, jaw crusher processing, gyratory milling, and / or hammer milling. In some cases, porous particulate iron materials may be combined from two separate sources or manufacturing processes to produce an optimal blend or particle size distribution. Also, in some cases, a single input material may be divided into various portions, which may undergo different size reduction and classification processes to achieve the desired size distribution. Appropriate size distribution may be ensured by the use of sieves, air classifiers, or other particle sizing and classification techniques known in the art for handling particulate metal materials. Such sizing operations may be operated continuously in-line with material processing or in separate batches. Blending or homogenization may be performed to ensure product quality and uniformity. Blending may be accomplished via various blending and portioning techniques appropriate to the particle size used. For example, finer particulate materials may be blended in a double cone or V-blender, while coarser particulate materials may be better blended by a series of riffling and mixing steps.

[0162] Metering, Conveying, and Dosing: The porous particulate iron material may be conveyed, metered, and dosed by techniques appropriate for the particle size and mass throughput involved. In some embodiments, a screw conveyor or other volumetric technology may be used to provide a uniform volumetric flow rate of material. In some embodiments, a vibratory gravimetric feeder or loss-in-weight feeder may be used to provide a constant input per unit time. In some instances, volumetric and gravimetric conveying may be combined at various points in the material feeding process. Where flow rate control is not critical, pneumatic, magnetic, or slurry-based conveying may be utilized between various processing units. Blending may be performed at the beginning of a conveyance, at the end of a conveyance, or periodically throughout the material transport to ensure material homogeneity.

[0163] Processing and Upgrading of Materials During Transportation: In some instances, dust associated with the material may interfere with bonding during subsequent processing. In such cases, the porous particulate ferrous material may be de-dusted. In some embodiments, de-dusting may be performed by jet-blasting air onto the particles. In some embodiments, de-dusting may be performed by feeding the material through a chamber with sufficient air velocity to allow for transport and removal of the generated dust; for example, a vibrating surface may mechanically remove dust from the surface by agitation, removing it from certain porous ferrous materials.

[0164] Customization of material shape and material properties in the integration process: In some cases, the material used for metallurgical bonding to the iron electrode may have a shape different from the spherical shape often used in direct reduction processes. In such cases, a more suitable shape can be created by extrusion, modified pelleting techniques, pressing, or other suitable processes. Cylindrical, hexagonal, octagonal, or other shapes can be used to produce porous particulate materials.

[0165] Use of particle size reduction techniques in the manufacture of iron electrodes.

[0166] Metallurgical joining of DRI can be challenging because the pellets are often coated to prevent sticking during the various heating, handling, and reduction processes used to produce DRI. This joining process can also be achieved by applying increased amounts of heat, temperature, pressure, or other suitable process variables—essentially, increasing the degree of melting, deformation, or microstructural modification that ultimately results in a satisfactory bond. However, microstructural modification through welding typically results in a decrease in electrochemical performance due to the densification and subsequent loss of microporosity and specific surface area necessary for electrode performance.

[0167] The inventors have found that some particle size reduction processes result in porous particulate iron materials retaining a large proportion of their microporosity. In reducing the particle size of a material, fresh surface areas are exposed that are not covered by the anti-stick coating used in previous processing steps to prevent material adhesion. This fresh surface area can then be metallurgically joined relatively easily. A very large particle size reduction is not necessary to have a significant impact on adhesion enhancement. As a very rough approximation, assume a spherical particle at that particle size with 75% of its surface uncoated. A quarter-fold particle size reduction results in 93.75% of the surface area being uncoated. Therefore, even a small reduction in particle size can result in a significant change in material behavior during metallurgical joining.

[0168] The use of the necessary particle size reduction techniques not only usefully enhances the quality of the electrode's adhesion and electrical connection, but also ensures that the electrode is less susceptible to upstream process variations from suppliers, and broadens the pool of suppliers that can supply materials for the electrode because regulations and constraints on coating type and amount are relaxed. Thus, the use of reduced particle sizes usefully enhances process robustness, reduces electrode variability, and enhances supplier flexibility in material production.

[0169] Particle size reduction techniques include jaw crushing, hammer milling, gyratory milling, and parallel plate milling.

[0170] Metallurgical joining techniques may include welding, sintering, or pressing, or combinations of these with other techniques and combinations between the listed techniques. Welding may include DC resistance welding and AC high frequency resistance welding. Sintering may include sintering under a small amount of pressure and pressing before sintering. Pressing may include hot or cold pressing. Pressing may include the application of pressure along one or more axes.

[0171] Use of broad or engineered size distributions for iron electrode production

[0172] Several considerations motivate the use of engineered size distributions in iron electrodes made from porous particulate materials. First, battery electrodes require active materials to maintain electrical connection with the current collector so that the electrode can pass through an external circuit. Electrical insulation of active materials is a major form of capacity loss in many battery systems. This is particularly important in metal electrode systems, where the active material often acts as its own current collector through the thickness of the electrode. Therefore, systems or methods that ensure increased contact or increased robustness of electrical contact between active materials in metal electrodes would be useful for enhancing the robustness of battery electrodes in terms of mishandling and / or active material degradation. Second, compression and / or consolidation of porous metal materials is one method for producing electrically connected, highly porous materials for battery electrodes. However, such consolidation processes are inherently limited in that porosity is desirable for battery electrodes, and consolidation processes often result in mechanical degradation due to densification or plastic deformation and rearrangement of the particles being consolidated. At the same time, battery electrodes must be mechanically robust so that they can be handled, installed into assemblies, and maintain excellent performance and connectivity throughout their lifespan. While mechanical robustness increases with increasing compaction, battery performance often decreases with increasing compaction. These two desirable battery characteristics are in direct conflict in electrode manufacturing processes using compaction. Therefore, methods and / or systems to avoid this technological tradeoff would be highly useful in the manufacture of compressed metal electrodes.

[0173] Broad and / or engineered particle size distributions, including multimodal packings, can often increase contact per unit volume within the particle packing and increase the packing density of the materials contained within the packing compared to narrower particle size distributions. Broad and engineered particle size distributions are therefore useful for engineering robustness of particles in contact with compacted electrodes (where the active material is also the conductive phase, simultaneously increasing packing density). Higher packing density reduces thickness and reduces overall system cost (e.g., due to less electrolyte required in the cell).

[0174] A problem posed by extensive and / or engineered particle packing is the possibility of small particles rattling within the interstitial spaces of larger particles. The volume fraction of these rattling particles is strongly related to the particle size distribution, shape, and packing method of the material, suggesting that extensive and engineered packing can result in a lack of reproducibility in electrode properties from batch to batch and run to run. However, the spaces within which these particles move are often quite small, often less than 1% of the particle diameter.

[0175] Therefore, electrode reproducibility and performance can be significantly enhanced by combining a broad and / or engineered particle size distribution with an electrode consolidation method that can achieve uniaxial plastic deformation >1%. By applying a small amount of densification (approximately 1%), plastic deformation can induce a significant increase in the number and weight fraction of interconnected active materials, greatly increasing the robustness of the connections between them. For iron electrode materials made from materials with high internal porosity (e.g., iron sponge powder), this deformation can be achieved either by applying very large forces (approximately 0.5–50 MPa) near room temperature, or by hot consolidation of the iron at somewhat lower pressures (approximately 0.1–10 MPa) but at significantly higher temperatures (>400°C and <1200°C). Of course, there is a continuum of temperature and pressure combinations between these two extremes. Consolidation techniques other than uniaxial consolidation are possible.

[0176] It has further been discovered that when broad and / or engineered particle size distributions are used as feedstocks for the consolidation process, the mechanical robustness of the resulting electrode material is much greater at the same degree of consolidation (e.g., the same applied pressure and / or the same densification uniaxial strain).

[0177] Therefore, the use of broad and / or engineered particle size distributions is useful for 1) creating a more robust conductive network between particles, 2) enhancing packing density and reducing electrode thickness and system cost, and 3) enhancing the mechanical robustness of the resulting product. Figures 3(A) and 3(B) illustrate an example comparison between unimodal packing, shown in Figure 3(A), and bimodal packing, shown in Figure 3(B), where the bimodal packing has a different particle size distribution, with smaller particles filling the gaps between the larger particles.

[0178] Some non-limiting considerations regarding size ranges associated with various forms of DRI and methods of making them are provided below. An important consideration is maintaining the microporosity of sponge iron while reducing particle size. These particle size reduction techniques have been shown to work to reduce particle size while substantially preserving the internal microporosity of sponge iron. As one non-limiting example, DRI may be in the form of whole pellet DRI, e.g., pellets of about 6 mm to 20 mm formed from a shaft furnace. Other processes may have different preferred size ranges. For example, some DRI processes, such as fluidized bed processes, inherently produce smaller DRI particles. As one non-limiting example, a fluidized bed may be used to obtain particles exclusively having a size less than 6 mm. As one non-limiting example, DRI may be in the form of crushed DRI, which may typically be less than half the size of whole pellet DRI (e.g., about 3 mm to about 10 mm), and often at least one-third to one-fifth the size (e.g., 1 mm to 6 mm). As non-limiting examples, such DRI may be formed using methods such as jaw crushers, gyratory crushers, high-pressure grinding rolls, and / or low-energy hammer mills. In some cases, the particle size of the DRI may be reduced using non-contact or limited-contact methods, such as spinning the DRI at high speeds to break it down. As one non-limiting example, the DRI may be in the form of finely ground or pulverized DRI, such as those having a size of about 0.1 mm to about 2 mm. As one non-limiting example, such DRI may be produced using higher-energy hammer mills, vertical grinding mills, and / or other finer grinding processes. As another non-limiting example, other forms of sponge iron may also be used, such as sponge iron produced for the powder metallurgy industry by the Höganäs sponge iron production process. Some specific details of embodiments of the engineered size distribution include whole pellet DRI mixed with crushed DRI and / or mixed with DRI fines, where the crushed DRI is 3 to 7 times finer than the whole pellet DRI.Some specific details of embodiments of the engineered size distribution include whole pellet DRI mixed with crushed DRI and / or mixed with DRI fines, where the DRI fines are waste products from DR facilities that could not proceed to an electric arc furnace. Some specific details of embodiments of the engineered size distribution include whole pellet DRI from a shaft furnace mixed with much finer sized fluidized bed DRI. Some specific details of embodiments of the engineered size distribution include crushed DRI that achieves different particle size distributions by incorporating DRI crushed by different processes. Some specific details of embodiments of the engineered size distribution include a crushing process, where the crushing process is inherently designed to have a broad size distribution.

[0179] In some embodiments, a target electrode thickness may be desirable. In such configurations, particle size may be selected so that the particle size is either much smaller than the overall thickness of the electrode or so that the particles form an integer number of layers across the thickness of the electrode. This is shown in Figure 4, which illustrates desirable (solid horizontal lines) and undesirable (dashed horizontal lines) anode thicknesses for integer increments of layers of porous particulate iron (e.g., DRI) particles. To ensure consistent packing within the anode, it may be beneficial to coordinate the anode thickness with the particle diameter of the porous particulate iron. Furthermore, adding a percentage of crushed porous particulate iron mediates this effect by reducing the incrementality of the desired thickness, regardless of the overall pellet diameter. Figure 4 also illustrates examples of desirable (horizontal lines 2 and 4) and undesirable (dashed lines 1 and 3) anode thicknesses for integer increments of layers of DRI particles. To ensure consistent packing within the anode, it may be beneficial to coordinate the anode thickness with the DRI particle diameter. Furthermore, adding a percentage of crushed DRI acts to mediate this effect by reducing the desired thickness gradient regardless of overall pellet diameter.

[0180] In certain embodiments, the iron electrode materials and iron electrodes disclosed in the present invention can be used as the negative electrode in alkaline electrochemical cells or Fe-air batteries, such as Fe—Ni, Fe—MnO2, and other positive electrodes known to those skilled in the art may be paired with the iron (negative) electrode.

[0181] Reheating and controlled cooling of DRI to achieve phase separation

[0182] While DRI and other porous particulate iron materials represent an inexpensive form of iron for use in iron negative electrodes in batteries, DRI and other porous particulate iron materials often contain large amounts of iron carbide (often called cementite). Cementite and iron have complex electrochemical behavior when galvanically coupled, and as a result, fabricating steel-based iron negative electrodes from both iron and cementite starting materials has proven difficult, whereas electrodes with similar amounts of graphite may be easier to fabricate due to a simpler reaction pathway. Such low-cementite electrodes may actually offer higher performance.

[0183] The inventors have discovered that the metastability of iron carbide can be exploited to design higher-performance carbon-containing iron electrodes. More specifically, cementite-containing porous particulate iron materials can be heated to temperatures at which the iron carbide decomposes to form iron and graphite, thereby improving the performance of the porous particulate iron material. The general heating requirement is to maintain the material at a temperature high enough to convert the metastable iron carbide phase to iron and graphite. The kinetics of this decomposition reaction are complex but have been thoroughly studied in the steelmaking field. Temperature and time can be manipulated to control the microstructural length scales of the iron and graphite phases. In general, the length scale of phase separation can be a function of the battery electrode's application, with lower temperatures favoring finer phase separation and higher temperatures favoring coarser microstructures. Generally, processing temperatures should range from about 300°C to around the iron-carbon eutectoid temperature of 727°C. Above this temperature, significant amounts of carbon become soluble in iron, thereby limiting the amount of cementite that can phase separate. The preferred temperature range is 500 to 650°C depending on the material used.

[0184] To phase separate the cementite in the porous particulate iron material without the need for reheating, or to reduce the time and energy required to reheat the material to the phase separation temperature, the porous particulate iron material can also be held at an elevated temperature after being discharged from the reduction furnace. This process is sometimes referred to as "hot discharge." The concepts of hot discharge and reheating can be combined: the porous particulate iron material can be cooled to an intermediate temperature, reheated, and held at the reheat temperature to achieve phase separation. The cooling profile of the process may also be controlled to control the microstructural characteristics of the remaining cementite.

[0185] Method for purifying carbon from iron electrodes

[0186] At the broadest level, reducing the impurity levels in secondary battery electrodes is often important to improve electrode performance, but this generally comes at a cost, for example, through additional processing. A low-cost method for purifying electrodes is important for many types of electrodes. In some embodiments, it can be advantageous to have low levels of carbon in iron anodes for secondary storage applications. This can be for example for electrochemical or cell performance reasons, or for manufacturability reasons, such as the ability to integrate and bond the DRI to the anode by hot compaction. The final carbon content of the DRI can vary depending on the input materials, and it would be desirable to be able to reduce the level of carbon in the DRI through manipulation of processing parameters and / or additional processes.

[0187] Chemical reactions of the porous particulate ferrous material involving gaseous atmospheres can be used to alter the carbon content of the ferrous material, some of which are described below. These reactions may occur via selective modification of the treatment atmosphere in a reduction process, a sintering process, or as a separate, dedicated chemical treatment process.

[0188] Use of Trace Oxygen to Reduce the Carbon Content of Porous Particulate Iron Materials: One potential method for reducing the carbon levels of porous particulate iron materials is to intentionally expose the sponge iron to an oxygen-containing atmosphere while it is at high temperature, for example, by having trace amounts of oxygen present in the atmosphere surrounding the DRI. The goal is to oxidize the carbon in the sponge iron so that carbon is removed from the sponge iron material. The reaction that occurs is either C + O → CO or 2C + O → CO. According to the Ellingham diagram in Figure 5, the temperature at which the initiation of these reactions becomes spontaneous is approximately 700°C (depending on the purity of the atmosphere). The free energies of oxidation of carbon and iron intersect near this temperature (approximately 700°C), indicating that carbon can reduce iron as long as carbon-containing gaseous byproducts are blown away as the reduction reaction proceeds. The reaction is of the form: Fe3O4 + 4C → 3Fe + 4CO (or Fe3O4 + 2C → 3Fe + 2CO2, depending on the temperature; similar reduction reactions exist for other iron oxides). This reaction produces gaseous by-products, either CO2 or CO, which must be blown away for the reduction reaction to continue.

[0189] The use of oxygen in DRI for carbon removal in porous particulate iron: If the temperature is appropriately selected, carbon can reduce iron oxide, even when both are in the solid state. This typically occurs above approximately 700°C, at which point carbon oxidation becomes thermodynamically favorable compared to iron oxidation, resulting in reactions of the form FeO + CFe + CO₂ or 2FeO + CFe + CO₂,g. This results in the removal of carbon impurities from the porous particulate iron and the production of more metallic iron instead of iron oxide, both of which are desirable from an electrochemical perspective. A flow of an inert gas, such as argon or nitrogen, is required to properly drive the reduction reaction. The amount of flow can be selected based on the amount of gaseous products that need to be removed as the reduction process progresses. Using oxygen already present in the porous particulate iron is advantageous in that the reaction is self-limiting and therefore easily controlled, without the need for strict control of the total oxygen content of the atmosphere. Because no oxygen is introduced, unwanted iron oxidation is essentially avoided.

[0190] The preferred temperature range for this method of removing carbon from iron may be selected so that the solubility of carbon in iron is high and therefore the rate of dissolution of FeC and graphite is rapid (i.e., above about 723°C for Fe-C co-deposition). The upper limit of the temperature range is limited by heating costs, densification, and the adhesion of porous particulate iron in the material feed that can occur at high temperatures. Therefore, a temperature not so high as to allow for these phenomena is desirable. Generally, the optimum operating temperature is about 700°C to about 900°C for decarburization of iron by its own oxides.

[0191] In some embodiments, sponge iron may be used directly from a DRI manufacturing plant to take advantage of the latent heat trapped in the material. In such cases, additional inert gas supply and heating may be used to adjust the temperature and atmosphere of the material to enable decarburization.

[0192] The iron-carbon phase diagram is shown in Figure 6. Below the Fe-C codeposition at approximately 723 °C, the rate-limiting step in the FeO-C reduction reaction is the dissolution and diffusion of carbon in the iron, such that the carbon reaches and reduces adjacent oxides. To allow this reduction to proceed more rapidly, the material must be heated above codeposition, where the solubility of carbon in iron increases by approximately 40 times, allowing for much faster diffusion of carbon into the oxides in sponge iron and the resulting reduction.

[0193] In some situations, the use of chemically active gases with low oxidizing power to promote decarburization without oxidizing the iron can make it difficult to achieve sufficient decarburization without oxidizing the sponge iron. In such situations, a third method for achieving decarburization is to add a chemically active gas to the atmosphere holding the sponge iron to remove carbon. In some cases, this is preferable because it has a lower tendency to oxidize the iron than pure iron. In some embodiments, hydrogen can be used to remove carbon via the following reaction: Cs + 2H2,g → CH4,g (which is effective for both cementitious and graphitic carbon). The kinetics and thermodynamics of this reaction are most effective at intermediate temperatures between 300 and 800°C, with the decarburization reaction being stoichiometrically limited at high temperatures (>800°C) and kinetically slow at low temperatures (<300°C). In some embodiments, carbon dioxide can be used to decarburize sponge iron at high temperatures (typically above 700°C). The temperature and partial pressure at which CO causes decarburization have been well studied in steelmaking and are governed by the Boudouard reaction: CO2,g + Cs ←→ 2COg. Addition of CO2 drives this reaction to the right, forming CO through the oxidation of carbon. CO2 has a lower oxidizing activity compared to oxygen, which typically limits the amount of iron oxidation that occurs. In some embodiments, water can be used as a decarburization gas to achieve a reaction of the form Cs + H2Og → COg + H2,g. Water is a kinetically more effective decarburization agent than hydrogen, and its reaction with carbon results in the production of a reducing gas that can limit or prevent iron oxidation and, in some cases, reduce iron oxide. Water can be added as an effective decarburization agent at a temperature range similar to that used for hydrogen. The concentration of water can be controlled by bubbling the gas into a water column at a controlled temperature, thereby controlling the dew point.

[0194] The inventors have found that some forms of carbon present in DRI exhibit faster decarburization rates than other forms of carbon. In some cases, DRI with a high graphitic carbon content may decarburize faster than DRI with a high cementitious carbon content but approximately the same total carbon. Therefore, DRI with a high graphitic carbon content is typically used as input for the decarburization process to minimize the amount of gas, time, and temperature required for processing. Decarburization reactions that can be more easily driven to completion (or where the reaction can be reasonably expected to proceed to completion) exhibit more stable product properties and uniformity. Uniformity of material properties between and within powder particles is a highly advantageous attribute for battery active materials, and a uniform starting composition prevents current crowding and accelerated degradation at specific points in the electrode. In some embodiments, the decarburized material is included in a metallurgically connected electrode. In some embodiments, the decarburized material is included in a non-metallurgically bonded electrode, but may also be included in designs with active material compressed between two current collectors, for example.

[0195] In some embodiments, a combination of process gases may be used to control the chemical reactions. For example, H / H0 and CO / CO mixtures may be used for controlled decarburization of porous particulate iron materials. Such mixtures may, for example, set the oxygen potential of the process atmosphere so that the oxygen can oxidize carbon present in the iron without oxidizing the iron itself. The composition of such process gases may be calculated from thermodynamic data or determined empirically.

[0196] Decarburization may be carried out in a variety of material processing equipment such as a kiln, tunnel furnace, pusher furnace, or rotary hearth furnace.

[0197] Post-treatment of metallurgically bonded electrodes:

[0198] Following bonding and decarburization, the formed electrode may undergo a series of processes including: (1) quenching, (2) cutting, (3) surface cleaning, and (4) application of a protective layer.

[0199] Various techniques can be applied to quench the consolidated electrode. Quenching is preferred to minimize the risk of reoxidation and phase transformation that may occur during cooling. In some embodiments, blasting with cooling air or inert gas can be performed, where the flow of gaseous species is at a volume and velocity sufficient to enhance the heat transfer of the gas from the consolidated electrode. If necessary, the gas can be recycled via a heat exchanger or other means, and the heat extracted from the consolidated anode can be reused. Other embodiments include liquid cooling, such as spraying or immersion in a tank; continuous operation requires transport in and out of the liquid cooling area by means such as a gravity gradient, conveyor belt, or other commonly used methods. The liquid must be selected to enhance cooling and prevent oxidation of the electrode, either through chemical incompatibility or by exceeding the oxidation kinetics; liquids such as water, oil, nitrogen, or battery electrolytes can be used alone or in combination. In some embodiments, the cooling liquid can also function as a protective coating.

[0200] After cooling, the electrode dimensions may need to be adjusted to fit the tolerances of the battery.

[0201] Surface cleaning of the formed electrodes may be required to remove any residue from the compact and for subsequent processing. Commonly used techniques such as solvent washing, acid etching, and sand / shot blasting may be used prior to heating and consolidation.

[0202] The final step in anode processing is to coat the electrode with a protective layer to prevent reoxidation of the electrode during shipping, storage, handling, and battery assembly. In some embodiments, the coating can consist of forming a thin iron oxide layer (also known as passivation) in a controlled, oxidizing atmosphere. Other embodiments include spraying or immersing the compacted anode in a corrosion inhibitor or a liquid compatible with the electrolyte. Other embodiments include applying a sealing film or casing under vacuum.

[0203] Handling and automation of handling

[0204] Due to their mechanical properties, integrated porous particulate iron electrodes tend to have limited strength and increased mass and bulk, depending on the carbon content and integration process. This limited strength means that these materials can be difficult to handle, potentially requiring new features, processes, and mechanisms for handling battery electrodes. Means can be used to enhance the electrode's strength and handling, such as a material backing bonded to one or both sides of the electrode. The backing may be a permeable iron-containing material that acts as a secondary conductive substrate. The backing material may be located in the center of the electrode, with porous particulate iron material integrated on both sides. There may be dense, specially fabricated areas of the integrated electrode that are patterned to enhance strength at load-bearing locations to facilitate current flow and provide increased strength and conductivity. Protective frames may be applied to one or more edges of the electrode, which may provide locations for electrical connections as well as increase handling strength. The electrode itself or these protective frames may have features that allow the electrode to be fixed, positioned, restrained, or suspended within an electrochemical assembly. These features can be manifested by holes, grooves, tracks, or ledges, and can allow the electrode to only contact its mechanical support and current-conducting path via the protective frame, and not the DRI-derived material itself. The electrode design can also include specific features that allow the electrodes to be densely and tightly packed in shipping containers that are later returned to the manufacturing site for reuse. Electrode consolidation can also be performed at the site of material reduction or decarburization, and the electrodes can be cooled and passivated by immersion in the electrolyte itself, within a container that serves as the liquid containment for the electrochemical device.

[0205] A method for separating metallurgically bonded iron electrode units.

[0206] Processing thick or brittle electrodes presents several challenges. This is because such electrodes cannot be tightly packaged by cellophane rolling or other similar techniques (such as those used in lithium-ion batteries) due to bending or other reasons. Therefore, thick or brittle electrodes must be cut or cut to the desired size and shape. Such a process must produce electrodes of consistent shape and weight. Continuous processing presents challenges because brittle materials must be cut and shaped without damaging the rest of the electrode. Such cutting processes are even more difficult when the brittle electrodes are made from metallurgically bonded metal particles, such as metals, especially iron. While such metallurgically bonded electrodes tend to be made of microscopically hard and heat-resistant materials, they can be macroscopically brittle, for example, due to the size of the contact points between particles being substantially smaller than the flow support and the resulting stress concentrations at the contact points. The microstructure of metallurgically bonded metal electrodes tends to be highly engineered to achieve the appropriate combination of porosity, surface area, and mechanical robustness for a given application. A cutting method that preserves this engineered microstructure in as many electrodes as possible is desirable to minimize material loss or underutilized material.

[0207] System Architecture: In some cases, metallurgically bonded electrodes may be manufactured in such a way that they are formed in the desired shape and size during the bonding operation, thereby eliminating the need for further separation. In some cases, the production of individual electrodes may be accomplished during the bonding operation itself through any number of incorporated cutting, stress concentration, or other operations, such as stress concentration features included in the rollers used in hot briquetting of direct reduced iron. In some cases, electrodes may be continuously formed and separated at a later stage in the process. When electrodes are continuously formed, the electrodes can be brought to the desired size by cutting or otherwise separating operations positioned along the electrode path. The separating operations may be stationary or may move in series with the electrodes using infrastructure such as a cam system.

[0208] Separation Mechanism: In some cases, metallurgically bonded iron electrodes may be cut or separated by any method common to cutting metals and other materials, especially brittle materials, including, but not limited to, shearing or other pressing actions, abrasive saws, diamond saws, chainsaws or other rotary cutting tools, water jets, bead blast streams, torches, lasers, or through scraping and snapping. In some cases, a combination of these cutting or separation methods may be used, for example, a rotary cutter may be used to scrape the electrode followed by a snapping mechanism. In some cases, electrodes may be separated by the use of high-velocity fluids, such as air knives or oxygen knives, designed to achieve specific mechanical and / or thermal conditions on the electrode. In some cases, electrodes may be designed with a thermal profile favorable for cutting or separation through methods including, but not limited to, the introduction of oxygen into the electrode. In some cases, oxygen may be introduced into the cutting process to cause a localized heating reaction when the reaction of the electrode metal with the oxygen results in heating. In some cases, oxygen introduction or other heat source may be used to create a thermal gradient and local softening of the electrode at the point that typically results in separation, for example by cracking, melting, or a combination thereof.

[0209] Strengthening: In some cases, the cutting mechanism can strengthen the electrode, which can occur through thermal or mechanical means. In some cases, the strengthening step may be included before, during, or after cutting.

[0210] System architecture of hot compaction anode manufacturing equipment

[0211] Hot-pressed electrodes can be produced at very low cost and in high-throughput equipment. This is especially true when the equipment is integrated into a DRI manufacturing facility. TDRI can be transferred directly from the DRI furnace to the hot-pressing equipment. This interface is very similar to the DRI furnace-HBI interface (where hot material flows directly from the furnace to the hot briquetting). This arrangement eliminates the need to reheat the DRI before entering the hot-pressing equipment. This saves cost, energy, and ultimately increases the throughput of the manufacturing equipment.

[0212] Hot-compressed anodes can be produced at very low cost and with high-throughput equipment. To reduce shipping and handling costs during production, the hot-compressed anode production line can be co-located with the DRI production facility. However, the hot-compressed anode equipment does not need to be integrated into the DRI production equipment. It can be advantageous to separate the two sets of equipment to allow for pre-treatment of the DRI before it goes into the hot-compression equipment to improve material properties related to porosity, shape, and adhesion.

[0213] Hot-compressed anode manufacturing equipment can be designed to be containerized (i.e., modular and portable). This can be highly advantageous, as the cost of the equipment can be quite high. It is likely to be used for a specific project, receiving DRI from the nearest DRI plant to reduce shipping and handling costs. Containerized hot-compressed anode manufacturing equipment can be described, but is not limited to, as follows: a heating, pressing, or rolling system secured within a standard 40-foot container(s), manufacturing equipment within a 45-foot container(s), which may be equipped with standard interfaces for integration into DRI furnaces, DRI handling equipment, and hot-compressed anode handling automation equipment. This allows for land or sea transportation to the project or DRI manufacturing site. The equipment can be easily shipped to a DRI manufacturing site as close as possible to Form Energy's energy storage facility. This containerized equipment may include decarburization capabilities.

[0214] The mechanism used in the hot compaction anode manufacturing apparatus can be described as a design methodology including, but not limited to: A continuous roller system similar to that found in hot briquetting apparatus architectures may be used; A quasi-continuous process such as a uniaxial press system may be used; This may include automated material handling at the inlet and outlet of the uniaxial press to increase the throughput of the apparatus; The press system may utilize the following actuation systems: hydraulic or air driven piston; cam driven actuation; lead screw driven actuation, electromagnetic actuation; The mechanism may include guided parallel plates to ensure dimensional uniformity and stability of the compact.

[0215] The mechanisms used in hot pressing anode manufacturing equipment can be described as follows, but are not limited to: A conveyor belt-like drive mechanism can be used to feed material into the press, which can be a stand-alone conveyor or a conveyor belt that is later incorporated into the anode electrode and used for current collection.

[0216] The mechanisms used in hot-compression anode manufacturing equipment can be described as, but not limited to, the following design methodologies: Linear or rotary press equipment (similar to pill press equipment) using multiple hot-press zones and material handling to accommodate multiple parallel or staged hot-press zones. This equipment can produce electrodes in form factors or small (10 cm x 10 cm) tiles or large (100 cm x 100 cm) panels.

[0217] The anode assembly may include an integrated current collector.

[0218] The actuation method for pressing the materials together can also serve as the actuation method for severing the integrated current collector from the continuous sheet.

[0219] System Architecture for Hot-Compressed Anode Embodiments

[0220] The reactor architecture ideally uses large-area (approximately 1 m²) metallurgically bonded anode electrodes fabricated directly from DRI or upstream steelmaking process materials. Large-area electrodes are difficult to fabricate by press or roller manufacturing processes, requiring very large and rigid presses. It may be advantageous to construct large-area electrodes from smaller pieces fabricated with simpler automated equipment. Hot-pressed anodes may be assembled using smaller hot-pressed anode units that are subsequently bonded. Assembly methods include, but are not limited to, electromechanical welding, forging, thermal bonding, and electrochemical sintering directly to either the DRI compact or the embedded and / or protruding current collectors.

[0221] Anode electrodes can be produced in panels or small pieces (30 cm x 30 cm) using the hot roller process, using large rollers with cutting features to form the compact into sheets. The material forms in the gaps between the roller cuts. As the rollers rotate and cut off segments at the ends of the rollers, the compact is "snipped" and cut into sheets.

[0222] The above method can also be used to create anode assemblies where multiple DRI compacts are formed and connected to a single steel mesh current collector. This string assembly can then be handled in continuous form or cut at a later stage for easier handling.

[0223] Conversely, a continuous process can produce a continuous sheet of material that can be continuously pulled through a continuous or semi-continuous press system and cut at a later processing step in the manufacturing process line.

[0224] Containing DRI can be difficult and costly, and a simple way to circumvent this problem is to create small packets of DRI for easy handling and containment. These packets can then be directly compressed in a hot press. These packets can be made from either a metal mesh-like material or a plastic material. If made from plastic, the packet casing can be thermally burned off later in the anode manufacturing process.

[0225] Method for collecting current from metallurgically bonded electrodes

[0226] Current collection from some metallurgically bonded iron electrode architectures, particularly those fabricated by welding or hot compaction, can be challenging. More specifically, the high currents generated by such electrodes often require welded connections, which can be difficult to achieve directly on electrodes made of highly porous iron materials. In some instances, current collecting materials that can be easily connected to bus bars or terminals can be embedded within or on the surface of the electrode, or at the ends of the electrode that must be connected to an external circuit. The current collecting materials may be comprised of metal strips, mesh sheets, perforated sheets, heterogeneous branched metal fabrics, or wires. In some embodiments, the current collecting materials may be incorporated into the electrode during the same metallurgical bonding process that bonds the porous particulate iron material to itself, while in other embodiments, the current collector may be incorporated into or bonded to the electrode in a second bonding step. The current collecting materials may be comprised of any material suitable in the art for manufacturing current collectors for electrodes. In some embodiments, the current collectors are made of steel, nickel, and / or copper. In some embodiments, less expensive current collector materials, such as nickel-plated steel, may be coated with a corrosion-resistant material.

[0227] In some embodiments, the current collector material can extend across the entire surface of the electrode, but in other embodiments, the current collector can be embedded only near the electrode's terminal to facilitate welding to adjacent external circuit elements. When the current collector is embedded in only a portion of the electrode, it can be embedded on the side of the electrode produced by the rolling process, and the electrode can be connected to external circuitry via the embedded current collector on this side, as shown in Figure 13, for example. A hopper can be installed above the roller, and slots can be created to allow the passage of the "tab-strand." The tab-strand can be compressed with iron in the nip at the desired frequency. A downstream slitter can also remove the carrier. If the tab-strand needs to be the length of the slab, a similar cutout can be made on the opposite side.

[0228] In some embodiments, the metallurgically bonded electrodes may have holes for attaching bolts and ring terminals for current collection.

[0229] In some embodiments, the busbar is metallurgically bonded directly to the metallurgically bonded electrode.

[0230] In some embodiments, the current collector can act as a basket to contain the material during the pressing or welding operation, allowing for material containment and further bonding of the current collector to the active material.

[0231] In some embodiments, a structural surface layer 1410 may be applied to one or both sides of the anode. This is similar to the paper surface on a drywall panel; without it, the drywall sheet would be very weak and nearly impossible to handle. The surface layer 1410 may be made from a suitable metallic material (such as steel or nickel) in a suitable format (such as wire mesh, expanded metal, or perforated sheet). In some cases, the surface layer 1410 may be made of plastic or another non-metallic material. The surface layer 1410 may be bonded to the DRI 1420 as part of the bonding process (whether using a roller 1430, a uniaxial press, or another process), so that the surface layer is integrally bonded to the surface of the anode. The surface layer 1410 may be inspired by the potential need for additional mechanical robustness, but it may also serve as a current collector. Additionally, it can function as a retaining screen to ensure that loose particles of DRI 1420 (whether they failed to bond during hot compaction or became loose after cycling) do not migrate from the anode envelope and disrupt cell function. Surface layer 1410 can also serve as a mechanical interface structure, allowing the anode to be attached to other elements of the cell during assembly. Surface layer 1410 can function during anode fabrication, for example, by operating as a conveyor that can meter and transport DRI 1420 to the compaction step. In some embodiments, perforated steel mesh can be bonded to both sides of the electrode, forming a sandwich structure with current-collecting structural elements on the surface that simultaneously enhance current collection, mechanical integrity, and handling. The structural surface of the electrode need not be a current-collecting element and can be made of plastic or other suitable material. An example of how a structural surface can be applied to an electrode is shown in FIG. 14.

[0232] Various embodiments may provide devices and / or methods for use in bulk energy storage systems, such as long-term energy storage (LODES) systems and short-term energy storage (SDES) systems. As an example, various embodiments may provide batteries for bulk energy storage systems, such as batteries for LODES systems. Renewable energy sources are becoming increasingly prevalent and cost-effective. However, many renewable energy sources face intermittency issues that hinder their adoption. The impact of renewable energy sources' tendency toward intermittency can be mitigated by pairing them with bulk energy storage systems, such as LODES systems and SDES systems. To support the adoption of combined generation, transmission, and storage systems (e.g., renewable generation sources paired with bulk energy storage systems, and power plants with transmission facilities at either the power plant and / or bulk energy storage system), devices and methods are needed to support the design and operation of such combined generation, transmission, and storage systems, such as the various embodiment devices and methods described herein.

[0233] An integrated generation, transmission, and storage system may be a power plant that includes one or more power generation sources (e.g., one or more renewable power generation sources, one or more non-renewable power generation sources, a combination of renewable and non-renewable power generation sources, etc.), one or more transmission facilities, and one or more bulk energy storage systems. The transmission facilities in either the power plant and / or the bulk energy storage systems may be co-optimized with the power generation and storage systems or may impose constraints on the design and operation of the power generation and storage systems. Integrated generation, transmission, and storage systems can be configured to meet various output targets under various design and operational constraints.

[0234] 15-23 illustrate various exemplary systems in which one or more aspects of various embodiments can be used as part of a bulk energy storage system, such as a LODES system, an SDES system, etc. For example, various embodiments described herein with reference to FIGS. 1-32 can be used as batteries for bulk energy storage systems, such as a LODES system, an SDES system, etc., and / or various electrodes described herein can be used as components of a bulk energy storage system. As used herein, the term "LODES system" refers to a bulk energy storage system configured to have a rated duration (energy / power ratio) of 24 hours (h) or longer, such as a 24-hour duration, a 24-50 hour duration, a longer duration than 50 hours, a 24-150 hour duration, a longer duration than 150 hours, a 24-200 hour duration, a longer duration than 200 hours, a 24-500 hour duration, or a longer duration than 500 hours.

[0235] FIG. 15 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiments of batteries described herein, various electrodes described herein, etc. The LODES system 1504 may be electrically connected to a wind farm 1502 and one or more transmission facilities 1506. The wind farm 1502 may be electrically connected to the transmission facility 1506. The transmission facility 1506 may be electrically connected to an electrical grid 1508. The wind farm 1502 may generate electrical power, and the wind farm 1502 may output the generated electrical power to the LODES system 1504 and / or the transmission facility 1506. The LODES system 1504 may store electrical power received from the wind farm 1502 and / or the transmission facility 1506. The LODES system 1504 can output the stored power to a transmission facility 1506. The transmission facility 1506 can output power received from one or both of the wind farm 1502 and the LODES system 1504 to a power grid 1508 and / or can receive power from the power grid 1508 and output the power to the LODES system 1504. The wind farm 1502, the LODES system 1504, and the transmission facility 1506 can together comprise a power plant 1500, which may be an integrated power, transmission, and storage system. The power generated by the wind farm 1502 may be fed directly to the power grid 1508 via the transmission facility 1506 or may first be stored in the LODES system 1504. In certain cases, the power supplied to the power grid 1508 may be entirely from the wind farm 1502, entirely from the LODES system 1504, or from a combination of the wind farm 1502 and the LODES system 1504.The distribution of power from the combined wind farm 1502 and LODES system 1504 power plant 1500 may be controlled according to a predetermined long-term (multi-day or even multi-year) schedule, or may be controlled according to a day-ahead (15-hour notice) market, or may be controlled according to an hour-ahead market, or may be controlled in response to actual pricing factors.

[0236] In one example of the operation of the power plant 1500, the LODES system 1504 can be used to reshape and "stabilize" the power produced by the wind farm 1502. In one such example, the wind farm 1502 may have a peak power output (capacity) of 260 megawatts (MW) and a capacity factor (CF) of 41%. The LODES system 1504 may have a power rating (capacity) of 106 MW, a rated duration (energy / power ratio) of 150 hours (h), and a rated energy of 15,900 megawatt-hours (MWh). In another such example, the wind farm 1502 may have a peak power output (capacity) of 300 MW and a capacity factor (CF) of 41%. The LODES system 1504 may have a power rating (capacity) of 106 MW, a rated duration (energy / power ratio) of 200 hours, and a rated energy of 21,200 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 176 MW and a capacity factor (CF) of 53%. The LODES system 1504 may have a power rating (capacity) of 88 MW, a rated duration (energy / power ratio) of 150 hours, and a rated energy of 13,200 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 277 MW and a capacity factor (CF) of 41%. The LODES system 1504 may have a power rating (capacity) of 97 MW, a rated duration (energy / power ratio) of 50 hours, and a rated energy of 4,850 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 315 MW and a capacity factor (CF) of 41%. The LODES system 1504 may have a power rating (capacity) of 110 MW, a rated duration (energy / power ratio) of 25 hours, and a rated energy of 2,750 MWh.

[0237] FIG. 16 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiments of batteries described herein, various electrodes described herein, etc. The system of FIG. 16 may be similar to the system of FIG. 15, except that a photovoltaic (PV) station 1602 may be used instead of the wind farm 1502. The LODES system 1504 may be electrically connected to the PV station 1602 and one or more transmission facilities 1506. The PV station 1602 may be electrically connected to the transmission facility 1506. The transmission facility 1506 may be electrically connected to a power grid 1508. The PV station 1602 may generate power, and the PV station 1602 may output the generated power to the LODES system 1504 and / or the transmission facility 1506. The LODES system 1504 can store power received from the PV station 1602 and / or the transmission facility 1506. The LODES system 1504 can output the stored power to the transmission facility 1506. The transmission facility 1506 can output power received from one or both of the PV station 1602 and the LODES system 1504 to the power grid 1508 and / or can receive power from the power grid 1508 and output the power to the LODES system 1504. The PV station 1602, the LODES system 1504, and the transmission facility 1506 can together comprise a power plant 1600, which may be an integrated power, transmission, and storage system. Power generated by the PV station 1602 may be fed directly to the power grid 1508 via the transmission facility 1506 or may first be stored in the LODES system 1504. In certain cases, the power supplied to the power grid 1508 may be entirely from the PV station 1602, entirely from the LODES system 1504, or from a combination of the PV station 1602 and the LODES system 1504.The distribution of power from the combined PV station 1602 and LODES system 1504 power plant 1600 may be controlled according to a predetermined long-term (multi-day or even multi-year) schedule, or may be controlled according to a day-ahead (24-hour advance notice) market, or may be controlled according to an hour-ahead market, or may be controlled in response to real-time pricing signals.

[0238] As one example of the operation of the power plant 1600, the LODES system 1504 can be used to reshape and “balance” the power produced by the PV station 1602. In one such example, the PV station 1602 may have a peak power output (capacity) of 490 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 340 MW, a rated duration (energy / power ratio) of 150 hours, and a rated energy of 51,000 MWh. In another such example, the PV station 1602 may have a peak power output (capacity) of 680 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 410 MW, a rated duration (energy / power ratio) of 200 hours, and a rated energy of 82,000 MWh. In another such example, the PV station 1602 may have a peak power output (capacity) of 330 MW and a capacity factor (CF) of 31%. The LODES system 1504 may have a power rating (capacity) of 215 MW, a rated duration (energy / power ratio) of 150 hours, and a rated energy of 32,250 MWh. In another such example, the PV station 1602 may have a peak power output (capacity) of 510 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 380 MW, a rated duration (energy / power ratio) of 50 hours, and a rated energy of 19,000 MWh. In another such example, the PV station 1602 may have a peak power output (capacity) of 630 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 380 MW, a rated duration (energy / power ratio) of 25 hours, and a rated energy of 9,500 MWh.

[0239] FIG. 17 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, the bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiments of batteries described herein, various electrodes described herein, etc. The system of FIG. 17 may be similar to the systems of FIGS. 15 and 16, except that the wind farm 1502 and the photovoltaic (PV) farm 1602 may both be power generating devices operating together in a power generation plant 1700. The PV farm 1602, the wind farm 1502, the LODES system 1504, and the transmission facility 1506 may together comprise the power generation plant 1700, which may be a combined power generation, transmission, and storage system. Electricity generated by the PV sites 1602 and / or wind farms 1502 may be fed directly into the grid 1508 via the transmission facility 1506, or may first be stored in the LODES system 1504. In certain cases, the electricity supplied to the grid 1508 may be fed entirely from the PV sites 1602, entirely from the wind farms 1502, entirely from the LODES system 1504, or from a combination of the PV sites 1602, the wind farms 1502, and the LODES system 1504. The distribution of electricity from the combined wind farms 1502, the PV sites 1602, and the LODES system 1504 power plant 1700 may be controlled according to a predetermined long-term (multi-day or even multi-year) schedule, or according to a day-ahead (24-hour advance notice) market, or according to an hour-ahead market, or in response to real-time pricing signals.

[0240] As one example of the operation of the power plant 1700, the LODES system 1504 may be used to reshape and "stabilize" the power produced by the wind farm 1502 and the PV farm 1602. In one such example, the wind farm 1502 may have a peak power output (capacity) of 126 MW and a capacity factor (CF) of 41%, and the PV farm 1602 may have a peak power output (capacity) of 126 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 63 MW, a rated duration (energy / power ratio) of 150 hours, and a rated energy of 9,450 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 170 MW and a capacity factor (CF) of 41%, and the PV farm 1602 may have a peak power output (capacity) of 110 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 57 MW, a rated duration (energy / power ratio) of 200 hours, and a rated energy of 11,400 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 105 MW and a 51% capacity factor (CF), and the PV farm 1602 may have a peak power output (capacity) of 70 MW and a 31% capacity factor (CF). The LODES system 1504 may have a power rating (capacity) of 61 MW, a rated duration (energy / power ratio) of 150 hours, and a rated energy of 9,150 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 135 MW and a capacity factor (CF) of 41%, and the PV farm 1602 may have a peak power output (capacity) of 90 MW and a capacity factor (CF) of 24%. The LODES system 1504 may have a power rating (capacity) of 68 MW, a rated duration (energy / power ratio) of 50 hours, and a rated energy of 3,400 MWh. In another such example, the wind farm 1502 may have a peak power output (capacity) of 144 MW and a capacity factor (CF) of 41%, and the PV farm 1602 may have a peak power output (capacity) of 96 MW and a capacity factor (CF) of 24%.The LODES system 1504 may have a power rating (capacity) of 72 MW, a rated duration (energy / power ratio) of 25 hours, and a rated energy of 1,800 MWh.

[0241] FIG. 18 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiments of batteries described herein, various electrodes described herein, etc. The LODES system 1504 may be electrically connected to one or more transmission facilities 1506. In this manner, the LODES system 1504 may operate in a “standalone” manner to arbitrate energy near market prices and / or avoid transmission constraints. The LODES system 1504 may be electrically connected to one or more transmission facilities 1506. The transmission facilities 1506 may be electrically connected to a power grid 1508. The LODES system 1504 may store power received from the transmission facilities 1506. The LODES system 1504 may output the stored power to the transmission facilities 1506. The power transmission facility 1506 may output power received from the LODES system 1504 to the power distribution grid 1508 and / or may receive power from the power distribution grid 1508 and output the power to the LODES system 1504 .

[0242] The LODES system 1504 and the transmission facility 1506 together may comprise a power generation plant 900. As an example, the power generation plant 900 may be located downstream of a transmission constraint, close to the power consumption. In such an exemplary downstream power generation plant 1800, the LODES system 1504 may have a duration of 24 to 500 hours and may fully discharge once or multiple times per year to support peak power consumption when transmission capacity is insufficient to serve customers. Additionally, in such an exemplary downstream power generation plant 1800, the LODES system 1504 may arbitrage the difference between nighttime and daytime electricity prices and perform several shallow discharges (daily or more frequently) to reduce the overall cost of electricity service to customers. As a further example, the power generation plant 1800 may be located upstream of a transmission constraint, close to the power generation. In such an exemplary upstream power plant 1800, the LODES system 1504 may have a duration of 24 to 500 hours and may undergo one or more full charges per year to absorb excess generation at times when transmission capacity is insufficient to distribute electricity to customers. Additionally, in such an exemplary upstream power plant 1800, the LODES system 1504 may undergo several shallow charge / discharge cycles (daily or more frequently) to arbitrage the difference between nighttime and daytime electricity prices and maximize the value of the power generation facility's output.

[0243] FIG. 19 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiment batteries described herein, various electrodes described herein, etc. The LODES system 1504 may be electrically connected to commercial and industrial (C&I) customers 1902, such as data centers, factories, etc. The LODES system 1504 may be electrically connected to one or more transmission facilities 1506. The transmission facilities 1506 may be electrically connected to a distribution grid 1508. The transmission facilities 1506 may receive power from the distribution grid 1508 and output the power to the LODES system 1504. The LODES system 1504 may store the power received from the transmission facilities 1506. The LODES system 1504 may output the stored power to the C&I customers 1902. In this manner, the LODES system 1504 can operate to reshape the power purchased from the grid 1508 to match the consumption patterns of the C&I customers 1902 .

[0244] The LODES system 1504 and the transmission facility 1506 together can comprise a power generation plant 1900. As an example, the power generation plant 1900 may be located near the electricity consumption, i.e., near the C&I customers 1902, such as between the power distribution grid 1508 and the C&I customers 1902. In such an example, the LODES system 1504 may have a duration of 24 hours to 500 hours and may purchase electricity from the market at times when electricity is cheaper, thereby charging the LODES system 1504. The LODES system 1504 may then discharge and provide electricity to the C&I customers 1902 at times when market prices are higher, thus offsetting the C&I customers' 1902 market purchases. In an alternative configuration, the power generation plant 1900 may be located not between the power distribution grid 1508 and the C&I customers 1902, but between a renewable resource, such as a PV farm or a wind farm, and the transmission facility 1506, which may be connected to the renewable resource. In such an alternative example, the LODES system 1504 may have a duration of 24 hours to 500 hours, and the LODES system 1504 may be charged at times when renewable output may be available. The LODES system 1504 may then discharge to cover some or all of the C&I customer's 1902 power needs and provide the C&I customer's 1902 with renewable generated electricity.

[0245] FIG. 20 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, a bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiment batteries described herein, various electrodes described herein, etc. The LODES system 1504 may be electrically connected to a wind farm 1502 and one or more transmission facilities 1506. The wind farm 1502 may be electrically connected to the transmission facility 1506. The transmission facility 1506 may be electrically connected to C&I customers 1902. The wind farm 1502 may generate power, and the wind farm 1502 may output the generated power to the LODES system 1504 and / or the transmission facility 1506. The LODES system 1504 may store the power received from the wind farm 1502.

[0246] The LODES system 1504 can output the stored power to the transmission facility 1506. The transmission facility 1506 can output the power received from one or both of the wind farm 1502 and the LODES system 1504 to the C&I customers 1902. The wind farm 1502, the LODES system 1504, and the transmission facility 1506 can together comprise a power plant 2000, which may be an integrated power, transmission, and storage system. The power generated by the wind farm 1502 can be delivered directly to the C&I customers 1902 via the transmission facility 1506 or can first be stored in the LODES system 1504. In certain cases, the power supplied to the C&I customers 1902 can be delivered entirely from the wind farm 1502, entirely from the LODES system 1504, or from a combination of the wind farm 1502 and the LODES system 1504. The LODES system 1504 may be used to reshape the electricity generated by the wind farm 1502 to match the consumption patterns of the C&I customers 1902. In one such example, the LODES system 1504 may have a duration of 24 hours to 500 hours and may charge when renewable generation by the wind farm 1502 exceeds the C&I customers 1902 load. Then, when renewable generation by the wind farm 1502 falls below the C&I customers 1902 load, the LODES system 1504 may discharge to provide the C&I customers 1902 with a stable renewable profile that offsets some or all of the C&I customers 1902 electricity consumption.

[0247] FIG. 21 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, the bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiments of batteries described herein, various electrodes described herein, etc. The LODES system 1504 may integrate a large amount of renewable power generation into a microgrid, for example, by integrating renewable power output from the PV site 1602 and wind power site 1502 with existing thermal power generation from, for example, a thermal power plant 2102 (e.g., a gas plant, a coal plant, a diesel generator set, etc., or a combination of thermal generation methods), and may be part of a power plant 2100 in which the renewable and thermal power supply C&I customer 1902 loads when availability is high. A microgrid, such as the microgrid comprised of the power plant 2100 and the thermal power plant 2102, may provide an availability factor of 90% or higher. The power generated by the PV site 1602 and / or wind farm 1502 may be delivered directly to the C&I customers 1902 or may first be stored in the LODES system 1504 .

[0248] In one particular case, the power supplied to the C&I customers 1902 may be entirely from the PV sites 1602, entirely from the wind farms 1502, entirely from the LODES systems 1504, entirely from the thermal power plants 2102, or from any combination of the PV sites 1602, the wind farms 1502, the LODES systems 1504, and / or the thermal power plants 2102. As an example, the LODES systems 1504 of the power plant 2100 may have a duration between 24 hours and 500 hours. As a specific example, the C&I customers 1902 load may have a peak of 100 MW, the LODES systems 1504 may have a power rating of 14 MW and a duration of 150 hours, the cost of natural gas may be $6 / million British thermal units (MMBTU), and the renewable occupancy may be 58%. As another specific example, the C&I customer 1902 load may be 100 MW peak, the LODES system 1504 may have a power rating of 25 MW and a duration of 150 hours, the cost of natural gas may be $8 / million British thermal units (MMBTU), and the renewable occupancy may be 65%.

[0249] FIG. 22 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, the bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include the batteries of various embodiments described herein, the various electrodes described herein, etc. The LODES system 1504 can be used to enhance a nuclear power plant 2202 (or other inflexible power generation facilities, such as thermal, biomass, and / or any other type of power plant with a ramp rate of less than 50% of rated power per hour and a capacity factor of 80% or higher) to add flexibility to the combined output of a power plant 2200 comprised of the combined LODES system 1504 and the nuclear power plant 2202. The nuclear power plant 2202 can operate at a high capacity factor and at its highest efficiency point, and the LODES system 1504 can charge and discharge to effectively reshape the output of the nuclear power plant 2202 to match customer electricity consumption and / or the market price of electricity. As an example, the LODES system 1504 of the power plant 2200 may have a duration of 24 hours to 500 hours. In one specific example, the nuclear power plant 2202 may have a rated output of 1000 MW, and the nuclear power plant 2202 may be forced to operate at minimum stable power generation or even shut down for an extended period of time due to a drop in the market price of electricity. The LODES system 1504 can charge during the market price drop, avoiding facility shutdown, and then the LODES system 1504 can discharge during a rise in market price, restoring total power generation.

[0250] FIG. 23 illustrates an exemplary system in which one or more aspects of various embodiments can be used as part of a bulk energy storage system. As a specific example, the bulk energy storage system incorporating one or more aspects of various embodiments may be a LODES system 1504. By way of example, the LODES system 1504 may include various embodiments of batteries described herein, various electrodes described herein, etc. The LODES system 1504 may operate in conjunction with an SDES system 2302. The LODES system 1504 and the SDES system 2302 may together comprise a power plant 2300. By way of example, the LODES system 1504 and the SDES system 2302 may be co-optimized, thereby enabling the LODES system 1504 to provide various services, including long-term backup and / or bridging, across multi-day variations (e.g., multi-day variations in market prices, renewable generation, electricity consumption, etc.). The SDES system 2302 can provide various services, including rapid support services (e.g., voltage control, frequency regulation, etc.) and / or bridging across diurnal variations (e.g., diurnal variations in market prices, renewable generation, electricity consumption, etc.). The SDES system 2302 may have a duration of less than 10 hours and a round-trip efficiency of greater than 80%. The LODES system 1504 may have a duration of 24 to 500 hours and a round-trip efficiency of greater than 40%. In one such example, the LODES system 1504 may have a duration of 150 hours and can support customer electricity consumption for up to a week of renewable generation shortages. The LODES system 1504 can also support customer electricity consumption during daytime generation shortage events, enhancing the capacity of the SDES system 2302. Additionally, the SDES system 2302 can supply customers during daytime generation shortage events and provide quality services such as power conditioning and voltage control and frequency regulation.

[0251] Various embodiments may include a battery including a first electrode, an electrolyte, and a second electrode, wherein at least one of the first electrode and the second electrode includes an iron agglomerate. In some embodiments, the electrolyte includes a soluble sulfide. In some embodiments, at least one of the first electrode and the second electrode further includes a solid sulfide. In some embodiments, at least one of the first electrode or the second electrode is under a compressive load. In some embodiments, the compressive load is applied to one side of at least one of the first electrode or the second electrode by a current collecting member. In some embodiments, the iron agglomerate includes at least one of magnetite, hematite, or wustite. In some embodiments, the electrolyte includes a corrosion inhibitor. In some embodiments, the iron agglomerate has an average length ranging from about 50 um to about 50 mm. In some embodiments, the iron agglomerate has an average internal porosity ranging from about 10% to about 90% by volume. In some embodiments, the iron agglomerate has a thickness of about 0.1 m. 2 / g ~ approx. 25m 2 / g。 In some embodiments, the electrolyte is infiltrated between the iron agglomerates. In some embodiments, the electrolyte includes 1-octanethiol. In some embodiments, the electrolyte includes molybdate anions and sulfide anions. In some embodiments, the iron agglomerates are supported within a woven metal mesh that provides compressive force and current collection for the iron agglomerates. In some embodiments, the iron agglomerates are bonded to each other and to a current collector.

[0252] Various embodiments may include a battery including a first electrode, an electrolyte, and a second electrode, wherein at least one of the first electrode and the second electrode comprises an atomized metal powder. In some embodiments, the electrolyte comprises a soluble sulfide. In some embodiments, at least one of the first electrode and the second electrode further comprises a solid sulfide. In some embodiments, at least one of the first electrode or the second electrode is under a compressive load. In some embodiments, the compressive load is applied to one side of at least one of the first electrode or the second electrode by a current collecting member. In some embodiments, the atomized metal powder comprises at least one of magnetite, hematite, or wustite. In some embodiments, the electrolyte comprises a corrosion inhibitor. In some embodiments, the electrolyte is infiltrated between the atomized metal powder. In some embodiments, the electrolyte comprises 1-octanethiol. In some embodiments, the electrolyte comprises molybdate anions and sulfide anions. In some embodiments, the atomized metal powder is supported within a woven metal mesh that provides a compressive force and current collection for the atomized metal powder, hi some embodiments, the atomized metal powder is bonded together and to a current collector.

[0253] Various embodiments may be methods for fabricating an electrode that include electrochemically producing a metal powder and forming the metal powder into an electrode. In some embodiments, the electrochemical production of the metal powder includes electrochemically producing the metal powder at least in part using molten salt electrochemistry. In some embodiments, the electrochemical production of the metal powder includes electrochemically producing the metal powder at least in part using gas atomization. In some embodiments, the electrochemical production of the metal powder includes electrochemically producing the metal powder at least in part using water atomization.

[0254] Various embodiments may include a bulk energy storage system including one or more batteries, at least one of which includes a first electrode, an electrolyte, and a second electrode, wherein at least one of the first electrode and the second electrode includes an iron agglomerate. In some embodiments, the bulk energy storage system is a long-term energy storage (LODES) system. In some embodiments, the electrolyte includes a soluble sulfide. In some embodiments, at least one of the first electrode and the second electrode further includes a solid sulfide. In some embodiments, at least one of the first electrode or the second electrode is subjected to a compressive load. In some embodiments, the compressive load is applied to one side of at least one of the first electrode or the second electrode by a current collecting member. In some embodiments, the iron agglomerate includes at least one of magnetite, hematite, or wustite. In some embodiments, the electrolyte includes a corrosion inhibitor. In some embodiments, the iron agglomerate has an average length ranging from about 50 μm to about 50 mm. In some embodiments, the iron agglomerates have an average internal porosity ranging from about 10% to about 90% by volume. 2 / g ~ approx. 25m 2 / g。 In some embodiments, the electrolyte is infiltrated between the iron agglomerates. In some embodiments, the electrolyte includes 1-octanethiol. In some embodiments, the electrolyte includes molybdate anions and sulfide anions. In some embodiments, the iron agglomerates are supported within a woven metal mesh that provides compressive force and current collection for the iron agglomerates. In some embodiments, the iron agglomerates are bonded to each other and to a current collector.

[0255] Various embodiments may include a bulk energy storage system including one or more batteries, at least one of which includes a first electrode, an electrolyte, and a second electrode, wherein at least one of the first electrode and the second electrode includes an atomized metal powder. In some embodiments, the bulk energy storage system is a long-term energy storage (LODES) system. In some embodiments, the electrolyte includes a soluble sulfide. In some embodiments, at least one of the first electrode and the second electrode further includes a solid sulfide. In some embodiments, at least one of the first electrode or the second electrode is under a compressive load. In some embodiments, the compressive load is applied to one side of at least one of the first electrode or the second electrode by a current collecting member. In some embodiments, the atomized metal powder includes at least one of magnetite, hematite, or wustite. In some embodiments, the electrolyte includes a corrosion inhibitor. In some embodiments, the electrolyte is infiltrated between the atomized metal powder. In some embodiments, the electrolyte includes 1-octanethiol. In some embodiments, the electrolyte includes molybdate anions and sulfide anions. In some embodiments, the atomized metal powder is supported within a woven metal mesh that provides a compressive force and current collection for the atomized metal powder. In some embodiments, the atomized metal powder is bonded together and to a current collector.

[0256] Example implementations are described in the following paragraphs. While some of the example implementations below are described with respect to example methods, further example implementations may include the example methods discussed in the following paragraphs implemented to form iron electrodes and / or electrochemical systems.

[0257] Example 1. A method of manufacturing an iron electrode, comprising providing a particulate iron material to an apparatus, and applying pressure and / or heat to the particulate iron material in the apparatus for a time to form an electrode having conductive connections between particles of the particulate iron material.

[0258] Example 2. The method of Example 1, further comprising providing the electrode in an electrochemical system without applying an external current collector or filling the electrode.

[0259] Example 3. The method of example 1 or 2, wherein the apparatus includes a compaction roller and the applied pressure is generated at least in part by the compaction roller.

[0260] Example 4. The method of example 1 or 2, wherein the pressure and / or heat is applied in a hot isostatic pressing (HIP) process, a uniaxial hot pressing, a hot roll consolidation process, a hot briquetting process, or a hot forging process.

[0261] Example 5. The method of any one of Examples 1-4, wherein the applied heat results in a high temperature in the range of about 300 to about 1000°C; the applied pressure is in the range of about 0.1 to about 200 MPa; the applied pressure is applied by uniaxial, biaxial, triaxial, isostatic pressure and / or roller method; and / or the time is in the range of about 1 second to about 24 hours.

[0262] Example 6. The method of Example 5, wherein the applied pressure is in the range of about 1 to about 100 MPa.

[0263] Example 7. The method of any one of Examples 1-6, wherein greater than 50% by volume microporosity within the particles of the particulate iron material is maintained after application of pressure and elevated temperature.

[0264] Example 8. The method of any one of Examples 1-7, wherein the electrode has greater than 50% by volume microporosity within the particles of the particulate iron material after application of pressure and elevated temperature.

[0265] Example 9. The method of any one of Examples 1-8, wherein the pressure and / or heat is applied in a non-oxidizing atmosphere.

[0266] Example 10. The method of any one of Examples 1-8, further comprising removing oxidation after forming the electrode.

[0267] Example 11. The method of any one of Examples 1-10, further comprising forming a texture on the iron electrode.

[0268] Example 12. The method of example 11, wherein the texture comprises channels of variable thickness.

[0269] Example 13. The method of any one of Examples 1-12, wherein the device comprises a tool portion having a conical protrusion.

[0270] Example 14. The method of any one of Examples 1-12, wherein the apparatus comprises a toothed roller.

[0271] Example 15. The method of any one of Examples 1-12, wherein the apparatus comprises a textured roller.

[0272] Example 16. The method of any one of Examples 1-15, further comprising the step of performing a surface cleaning of the particulate ferrous material prior to providing the particulate ferrous material to the apparatus.

[0273] Example 17. The method of any one of Examples 1-16, further comprising preheating the particulate ferrous material and / or mechanically modifying one or more aspects of the particulate ferrous material prior to providing the particulate ferrous material to the apparatus.

[0274] Example 18. The method of any one of Examples 1-17, further comprising controlling the particle size of the particulate ferrous material prior to providing the particulate ferrous material to the apparatus.

[0275] Example 19. The method of example 18, wherein controlling the particle size of the particulate iron material comprises reducing the particle size of the particulate iron from a first particle size to a second particle size.

[0276] Example 20. The method of Example 19, wherein the second particle size is one-half the first particle size.

[0277] Example 21 The method of Example 19, wherein the second particle size is one-quarter the first particle size.

[0278] Example 22. The method of any one of Examples 19-21, wherein the particle size reduction technique comprises one or more of jaw crushing, hammer milling, gyratory milling, and parallel plate pulverizer grinding.

[0279] Example 23. The method of any one of Examples 1-22, wherein the step of providing the particulate ferrous material to the apparatus at least partially comprises a thermal spray process that deposits a portion of the particulate ferrous material onto the substrate and / or bed of the DRI.

[0280] Example 24. The method of any one of Examples 1-22, wherein providing the particulate ferrous material to the device comprises, at least in part, using an additive manufacturing process.

[0281] Example 25. The method of any one of Examples 1-24, wherein the step of forming the electrode further comprises at least one of ultrasonic consolidation / vibration, slicing, machining, cold consolidation, cold extrusion, casting, differential temperature consolidation, and bonding and consolidation to at least partially form the electrode.

[0282] Example 26. The method of any one of Examples 1-25, wherein the step of applying pressure and / or heat comprises applying a pressure of about 0.5-50 MPa at room temperature or about 0.1-10 MPa at a temperature >400°C and <1200°C.

[0283] Example 27. The method of any one of Examples 1-26, comprising applying heat to the particulate iron material, wherein the iron carbide decomposes to produce iron and graphite.

[0284] Example 28. The method of Example 27, wherein the applied heat is at a temperature of 300 to 727°C.

[0285] Example 29. The method of any one of Examples 1-28, further comprising applying pressure and / or heat in an oxygen atmosphere at a temperature between 700 and 900°C.

[0286] Example 30. An iron electrode produced by the method described in any of Examples 1-29.

[0287] Example 31. An iron electrode comprising metallurgically bonded sponge iron particles, wherein the sponge iron particles have a microporosity of >50% by volume and a particle size of >100 μm.

[0288] Example 32. The iron electrode described in Example 31, prepared by the method described in any one of Examples 1-29.

[0289] Example 33. An electrochemical system comprising an iron electrode produced by the method of any one of Examples 1-29 and / or the iron electrode of any one of Examples 30-32.

[0290] Example 34. The electrochemical system of Example 33, which is a long-term energy storage system.

[0291] The above method descriptions are provided merely as illustrative examples and are not intended to require or imply that the steps of the various embodiments must be performed in the order presented. As one skilled in the art will understand, the order of steps in the above embodiments can be performed in any order. Words such as "then," "then," and "next" are not necessarily intended to limit the order of steps; such words may be used to guide the reader through the method description. Furthermore, any reference to a claim element in the singular, for example, using the article "a," "an," or "the," should not be construed as limiting the element to the singular. Furthermore, any step of any embodiment described herein can be used in any other embodiment.

[0292] The foregoing description of the disclosed embodiments is provided to enable any person skilled in the art to make or use the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the basic principles defined herein may be applied to other embodiments without departing from the scope of the present invention. Thus, the present invention is not intended to be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for producing an iron electrode, comprising: providing a particulate ferrous material to an apparatus; applying pressure to the particulate ferrous material in the apparatus for a time to form electrodes having conductive connections between particles of the particulate ferrous material; A method comprising:

2. The method of claim 1 , wherein the apparatus includes compaction rollers and the pressure applied to the apparatus is generated at least in part by the compaction rollers.

3. The applied pressure is in the range of 0.1 to 200 MPa, The pressure applied to the device may be applied by uniaxial, biaxial, triaxial, isostatic pressure and / or roller methods; The method of claim 1.

4. The method of claim 3, wherein the pressure applied to the device is in the range of 1 to 100 MPa.

5. 10. The method of claim 1, wherein the electrode has greater than 50 volume percent microporosity within the particles of the particulate iron material after application of the pressure and elevated temperature.

6. The method of claim 1 , wherein the pressure is applied in a non-oxidizing atmosphere.

7. The method of claim 1 further comprising removing oxidation after forming the electrode.

8. 10. The method of claim 1, further comprising forming a texture on the iron electrode.

9. The method of claim 8 , wherein the texture comprises channels of variable thickness.

10. The method of claim 1 , wherein the apparatus comprises a tool portion having a conical protrusion, a toothed roller, or a textured roller.

11. The method of claim 1 , further comprising the step of performing a surface cleaning of said particulate ferrous material prior to applying said pressure to said particulate ferrous material in said apparatus.

12. 10. The method of claim 1, further comprising the steps of preheating the particulate ferrous material and controlling the particle size of the particulate ferrous material prior to providing the particulate ferrous material to the apparatus.

13. The method of claim 1 , further comprising the step of controlling a particle size of the particulate ferrous material prior to providing the particulate ferrous material to an apparatus.

14. 14. The method of claim 13, wherein controlling the particle size of the particulate ferrous material comprises reducing the particle size of the particulate ferrous material from a first particle size to a second particle size.

15. 15. The method of claim 14, wherein the second particle size is one-quarter the size of the first particle size.

16. 15. The method of claim 14, wherein the particle size reduction of the particulate ferrous material comprises one or more of jaw crushing, hammer milling, gyratory milling, and grinding with a parallel plate grinder.

17. 10. The method of claim 1, wherein providing the particulate ferrous material to the apparatus comprises, at least in part, a thermal spray process that deposits a portion of the particulate ferrous material onto a bed of direct reduced iron and / or onto a substrate.

18. The method of claim 1, wherein the step of applying pressure and / or heat comprises application of a pressure of 0.5-50 MPa at room temperature or application of 0.1-10 MPa at a temperature >400°C and <1200°C.

19. An iron electrode, 1. An iron electrode comprising metallurgically bonded sponge iron particles, the sponge iron particles having a microporosity of greater than 50 volume percent and a particle size of greater than 100 μm.