In-line lamination process for producing thermoplastic composite panels with textured film layers

JP2023550325A5Inactive Publication Date: 2024-11-20AZDEL INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023528325
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-05-13
Filing Date
2021-11-12
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Manufacturing decorative panels is time-consuming and tedious due to the use of different components being processed separately, which can lead to inefficiencies and potential delamination issues.

Method used

An in-line process for manufacturing thermoplastic composite panels with textured film layers, involving the mixing of reinforcing materials and thermoplastic materials in an aqueous solution, forming a web with an open cell structure, and applying textured film layers to a heated porous core layer without adhesives, followed by consolidation to create a composite article.

Benefits of technology

The process results in lightweight, waterproof, and flame-retardant panels with enhanced adhesion and stiffness, suitable for recreational vehicles and wet applications, while reducing manufacturing time and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

An in-line system and method are described that can be used to provide lightweight reinforced thermoplastic composite articles that include a textured film layer. The textured film layer can provide one or more of water resistance, flame retardancy, a desired surface roughness, or other desired properties. The lightweight reinforced thermoplastic composite articles that include the textured film layer can be used in construction applications, recreational vehicle applications, and other applications as desired.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Priority Claim

[0002] This application claims the priority and benefit of each of U.S. Patent Application No. 63 / 112,914, filed on November 12, 2020, U.S. Patent Application No. 63 / 145,073, filed on February 3, 2021, and U.S. Patent Application No. 63 / 188,358, filed on May 13, 2021. The entire disclosure of each of these applications is incorporated herein by reference.

[0003] Technical Field

[0004] The specific configurations described herein relate to an in-line lamination process capable of manufacturing thermoplastic composite panels including a textured film layer. In some examples, the panels can be used in architectural applications, recreational vehicles, and other areas where waterproof panels may be desired.

Summary of the Invention

Problems to be Solved by the Invention

[0005] Background

[0006] The manufacture of decorative panels can be time-consuming and cumbersome. In many cases, the different components of the panel are manufactured in different processes or at different locations.

Means for Solving the Problems

[0007] Summary

[0008] Specific aspects, configurations, embodiments, and examples of an in-line process that can be used to manufacture panels including a textured film layer for use in recreational vehicles, architectural applications, wet applications, and other areas are described.

[0009] In one embodiment, an in-line process for manufacturing a thermoplastic composite article using an in-line system is described. In a particular embodiment, the in-line process includes: mixing a reinforcing material and a thermoplastic material in an aqueous solution; placing the aqueous solution of the reinforcing material and the thermoplastic material on a mobile support; removing water from the placed aqueous solution on the mobile support to form a web including an open-cell structure formed from the reinforcing material and the thermoplastic material; drying the web on the mobile support to provide a porous core layer; heating the dried porous core layer on the mobile support to melt the thermoplastic material of the heated porous core layer; placing a first textured film layer on a first surface of the heated porous core layer on the mobile support; and applying pressure to the heated porous core layer including the placed first textured film layer on the mobile support to provide a thermoplastic composite article.

[0010] In certain configurations, the porous core layer is heated to a first temperature higher than the melting point of the thermoplastic material and lower than the melting point of the reinforcing material. In some examples, the method includes adding a foam to an aqueous solution of the reinforcing material and the thermoplastic material. In other examples, the method includes adding a lofting agent to an aqueous solution of the reinforcing material and the thermoplastic material. In some embodiments, the method includes configuring the first textured film layer as a polyolefin film. In certain examples, the method includes configuring the polyolefin film to have a maximum height surface roughness (Rt) of at least 8 microns, as measured using a stylus shape measuring device.

[0011] In additional examples, the first textured film layer further includes a pattern. In some embodiments, the pattern includes one or more of the following: wood grain patterns, marble patterns, tile patterns, random patterns, pinwheel patterns, herringbone patterns, brick patterns, offset alternating brick patterns, offset patterns, grid patterns, stacked vertical patterns, French patterns, basket weave patterns, diamond patterns, or chevron patterns.

[0012] In some embodiments, the thermoplastic material includes a polyolefin, and the reinforcing material includes inorganic fibers.

[0013] In other embodiments, the method includes stretching the first textured film layer before placing the first textured film layer on the first surface of the heated porous core layer on the moving support.

[0014] In additional embodiments, the first textured film layer is stretched in the longitudinal direction.

[0015] In certain embodiments, the first textured film layer is placed on the heated porous core layer without using an adhesive between the first textured film layer and the heated porous core layer.

[0016] In some embodiments, the method includes placing a skin layer on a second surface of a heated porous core layer on a moving support.

[0017] In certain examples, the method includes placing an adhesive on the second surface of a heated porous core layer before placing a skin layer on the second surface.

[0018] In some embodiments, the method includes constructing a thermoplastic composite article to meet the Class B standard tested by ASTM E84 2009.

[0019] In other embodiments, the method includes constructing a thermoplastic composite article to meet the Class A standard tested by ASTM E84 2009.

[0020] In certain embodiments, the method includes compacting a heated porous core layer before placing a first textured film layer on a first surface. In some examples, the method includes heating the thermoplastic composite article after compaction in order to increase the overall thickness of the thermoplastic composite article.

[0021] In other embodiments, the method includes placing a first textured film layer on a first surface of a heated porous core layer, and then printing a pattern on the first textured film layer.

[0022] In additional embodiments, the method includes placing a first textured film layer on a first surface of a heated porous core layer, and then embossing the first textured film layer.

[0023] In some examples, the method includes placing a non-porous layer on a first surface of a heated porous core layer before placing a first textured film layer.

[0024] In another aspect, an in-line system configured to manufacture a thermoplastic composite article is described. In a specific example, the in-line system includes a fluid reservoir configured to receive an aqueous solution, a thermoplastic material, and a reinforcing material, and the fluid reservoir is configured to mix the thermoplastic material and the reinforcing material in the aqueous solution to provide a uniform dispersion of the thermoplastic material and the reinforcing material in the aqueous solution. The in-line system can also include a moving support fluid-coupled to the fluid reservoir and configured to receive the uniform dispersion from the fluid reservoir and hold the uniform dispersion on the moving support. Optionally, the moving support can include two or more separate sections or segments. In some cases, the in-line system can also include a pressure device configured to remove water from the uniform dispersion on the moving support to provide a web including a continuous cellular structure formed from the reinforcing material and the thermoplastic material. The in-line system can also include a device configured to dry and heat the web on the moving support to provide a porous core layer on the moving support. The in-line system can also include a first supply device configured to receive a first film material, and the first supply device is configured to provide the first film material as a first film layer on a first surface of the porous core layer on the moving support. The in-line system can also include a consolidation device configured to consolidate the heated porous core layer with the disposed first film layer by applying pressure to the heated porous core layer and the disposed first film layer to provide a substantially flat thermoplastic composite article.

[0025] In a particular embodiment, the first supply device is configured to receive a roll of the first film material.

[0026] In other embodiments, the in-line system can include a texturing device configured to impart texture to the first film layer before disposing the first film layer on the heated porous core layer.

[0027] In some embodiments, the inline system can include a texturing apparatus configured to impart texture to a first film layer after disposing the first film layer on a heated porous core layer.

[0028] In certain examples, the inline system can also include a densification apparatus.

[0029] In certain embodiments, the inline system can include a second heating apparatus disposed after the densification apparatus, the second heating apparatus being configured to heat a thermoplastic composite article to increase the overall thickness of the thermoplastic composite after densification.

[0030] In certain examples, the inline system can include a nebulizer fluidly coupled to a fluid reservoir, the nebulizer being configured to spray a uniform dispersion onto a moving support.

[0031] In certain embodiments, the inline system can include a second supply apparatus configured to receive a feed or non-porous material, the second supply apparatus being configured to provide the non-porous material as a non-porous layer on a first surface of the porous core layer on the moving support before disposing the first film layer on the heated porous core layer.

[0032] In some embodiments, the inline system can include a printer configured to print a pattern onto the first film layer after the first film layer is disposed on a second surface of the heated porous core layer.

[0033] In certain configurations, the inline system can include an embosser configured to provide a pattern onto the first film layer.

[0034] In some embodiments, the inline system can include a processor configured to control the movement of the moving support of the inline system and optionally the movement of other components.

[0035] In additional embodiments, the recreation vehicle (RV) ceiling includes a first laminated lightweight reinforced thermoplastic composite article comprising a porous core layer, a first skin layer on a first surface of the porous core layer, and a textured and patterned film layer on a second surface of the porous core layer. The RV ceiling may also include a support structure bonded to the first skin layer. For example, the support structure may include tubes or a network.

[0036] In certain embodiments, the RV ceiling includes exterior panels coupled to a support structure. In other embodiments, the exterior panels include fiberglass or aluminum.

[0037] In some embodiments, the RV ceiling includes a foam layer bonded to a first skin layer and positioned between a first laminated lightweight reinforced thermoplastic composite article and a support structure.

[0038] In some embodiments, the textured and patterned film layer includes a polyolefin film. For example, the polyolefin film may include one or more polypropylene, polyethylene, or blends or copolymers thereof.

[0039] In certain examples, the porous core layer of the first laminated lightweight reinforced thermoplastic composite article includes a web comprising an open-cell structure formed from reinforcing fibers held together by the thermoplastic material. In other embodiments, the thermoplastic material in the porous core layer includes polyolefin. In some embodiments, the reinforcing material in the porous core layer includes glass fibers. In additional embodiments, the recreation ceiling panel is waterproof.

[0040] In another embodiment, the recreation vehicle comprises a ceiling, side walls coupled to the roof, and a floor coupled to the side walls to provide interior space within the recreation vehicle, wherein the ceiling of the recreation vehicle comprises a textured film layer as described herein. In some examples, the RV comprises wheels that enable the towing of the recreation vehicle.

[0041] In an additional embodiment, the waterproof panel includes a first laminated lightweight reinforced thermoplastic composite article comprising a porous core layer, a first skin layer on a first surface of the porous core layer, and a textured and patterned film layer on a second surface of the porous core layer, and a substrate bonded to the first laminated lightweight reinforced thermoplastic composite article via the first skin layer.

[0042] In certain embodiments, the waterproof panel meets the Class B standard as tested by ASTM E84 2009. In other embodiments, the waterproof panel meets the Class A standard as tested by ASTM E84 2009.

[0043] In some embodiments, the waterproof panel includes a non-porous layer between the second surface of the porous core layer and the textured and patterned film layer.

[0044] In some examples, the textured and patterned film layer includes microspikes on the surface of the film layer that bond to the first surface of the porous core layer in order to enhance the adhesion of the textured and patterned film layer to the first surface of the porous core layer.

[0045] In certain embodiments, the textured and patterned film layer is 80 gsm (g / m²). 2 ) Includes a basis weight of ~250 gsm. In other embodiments, the textured and patterned film layer includes multiple film layers.

[0046] In some examples, waterproof panels include a thermosetting top coating on a textured and patterned film layer, such as a thermosetting material coating on a textured and patterned film layer.

[0047] In some embodiments, the waterproof panel does not contain cellulose.

[0048] In another embodiment, the shower panel comprises a lightweight reinforced thermoplastic article including a textured film layer as described herein, for example, the article comprising a porous core layer, a first skin layer on a first surface of the porous core layer, a textured and patterned film layer on a second surface of the porous core layer, and an optional substrate bonded to a first laminated lightweight reinforced thermoplastic composite article via the first skin layer.

[0049] In an additional embodiment, the shower enclosure comprises a shower pan, a rear wall coupled to the shower pan, and a side wall coupled to the shower pan and the rear wall, wherein at least one of the shower pan, the rear wall, and the side wall comprises at least one side of a lightweight reinforced thermoplastic article including the textured film layer described herein, for example, the rear wall or pan comprises a porous core layer, a first skin layer on a first surface of the porous core layer, a textured and patterned film layer on a second surface of the porous core layer, and an optional substrate bonded to a first laminated lightweight reinforced thermoplastic composite article via the first skin layer.

[0050] Further aspects, configurations, embodiments, and examples are described below.

[0051] A brief overview of some of the drawings.

[0052] To facilitate a better understanding of the technology described herein, with reference to the attached drawings, certain specific examples are given below. [Brief explanation of the drawing]

[0053] [Figure 1] This is a simplified diagram showing the ceiling of a recreation vehicle according to several embodiments. [Figure 2] A block diagram showing specific steps of an inline process that can be used, according to several embodiments. [Figure 3] This figure shows specific components that can be used to add materials to a mixing tank, according to a particular example. [Figure 4A] This is a diagram of a movable support according to several embodiments. [Figure 4B] This is a diagram of a movable support according to several embodiments. [Figure 5A] This figure shows a drying apparatus according to a specific embodiment. [Figure 5B] This figure shows a drying apparatus according to a specific embodiment. [Figure 5C] This figure shows a drying apparatus according to a specific embodiment. [Figure 6A] This figure shows the application of a textured film layer and / or skin layer to the core layer according to a specific embodiment. [Figure 6B] This figure shows the application of a textured film layer and / or skin layer to the core layer according to a specific embodiment. [Figure 7] This figure shows an adhesive layer reservoir that can be used to apply adhesive to the surface of a core layer, with several examples. [Figure 8A] This figure shows rollers that can be used in inline processes, with several examples. [Figure 8B] This figure shows rollers that can be used in inline processes, with several examples. [Figure 9] This figure shows a cutting device that can be used to cut a moving composite material article into individual composite material articles, according to a specific embodiment. [Figure 10A] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10B] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10C] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10D] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10E]Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10F] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10G] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10H] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10I] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10J] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10K] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10L] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10M] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10N] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 10O] Several examples illustrate the different patterns that can exist on a textured film layer. [Figure 11A] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 11B] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 11C] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 11D] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 12] This is a diagram of the ceiling of a recreational vehicle (RV) according to several embodiments. [Figure 13] This is a diagram of a recreational vehicle that may include an RV roof as described herein, by some examples. [Figure 14A] This is a diagram of a shower enclosure according to several embodiments. [Figure 14B] This is a diagram of a shower enclosure according to several embodiments. [Figure 15A] This is a diagram of a siding panel according to a specific embodiment. [Figure 15B] This is a diagram of a roof panel according to a specific embodiment. [Figure 16] This table shows the various films and materials present in the tested LWRT articles. [Figure 17A] This figure shows different patterns and textures on the surface of the film. [Figure 17B] This figure shows different patterns and textures on the surface of the film. [Figure 17C] This figure shows different patterns and textures on the surface of the film. [Figure 17D] This figure shows different patterns and textures on the surface of the film. [Figure 17E] This figure shows different patterns and textures on the surface of the film. [Figure 17F] This figure shows different patterns and textures on the surface of the film. [Figure 17G] This figure shows different patterns and textures on the surface of the film. [Figure 17H] This figure shows different patterns and textures on the surface of the film. [Figure 17I] This figure shows different patterns and textures on the surface of the film. [Figure 18] This is a table showing the LWRT items that have been tested. [Figure 19]This is a table showing surface roughness measurements. [Figure 20] This is a table showing flame retardancy measurements. [Figure 21] This table shows the measured characteristics of the tested samples. [Figure 22] This table shows the measured characteristics of the tested samples. [Modes for carrying out the invention]

[0054] Detailed explanation

[0055] Given the advantages of this specification, it will be recognized by those skilled in the art that the different layers described herein are not necessarily shown to a constant scale. Unless specifically indicated in the description relating to its particular configuration, no material is intended to be required for any single layer. The thickness, arrangement, and end use of the decorative panels may vary.

[0056] In certain embodiments, the processes described herein can be used to manufacture panels for use in building applications, vehicles such as recreational vehicles, wet applications, and other applications. Recreational vehicles (RVs), including campervans and towed vehicles, can have their weight reduced by incorporating lightweight fiberglass-reinforced thermoplastic composite panels into the ceiling or other components. Compared to traditionally used wood composites, i.e., plywood, polymer composites offer a wealth of advantages, including better durability due to formaldehyde-free properties, lighter weight for better fuel efficiency, improved acoustic performance, water resistance or waterproofing, mold resistance, and flame retardancy derived from the advanced functional integration of the glass and thermoplastic resin matrices. In some configurations, reinforcing fibers, such as glass fibers, can be advantageously imparted to the modulus of elasticity of the resin matrix, resulting in enhanced properties with minimal weight increase. The performance of the resulting composite may depend at least in part on the core composition (fiber / resin ratio), weight per unit area (surface density), panel application thickness, and textured film layer.

[0057] In certain examples, the outer surface of the panel may include a textured film layer having a "deep" or high surface roughness. For example, the textured film can be bonded to the underlying web or core layer in an in-line process so that it is generally not separable from the composite core. The resulting composite article can exhibit strong tensile strength and eliminate the problem of delamination of the decor / core at the interlayer interface in RV ceiling structures. The textured film can also improve the bending stiffness of the substrate, particularly in the longitudinal direction. The textured panel can also pass ASTM E84 Class A flame retardancy classification 2009 or ASTM E84 Class B flame retardancy classification 2009, depending on the film used. Class A classification generally means a flame propagation index of -25 and a smoke emission index of 450 or less. Class B classification generally means a flame propagation index of 26-75 and a smoke emission index of 450 or less. In some embodiments, the textured film and other layers can provide a waterproof panel that can be used as a shower wall, shower pan, or other wet applications, such as a roof or roof panel. In some embodiments, flame retardancy can also be measured using the FMVSS 302 standard. The FMVSS 302 test is sometimes referred to as the SAE J369 test standard. These tests are generally equivalent and are used to determine the burning rate measurement. Briefly, the test uses a horizontal flame chamber, a ventilation hood, a tote large enough to handle a test specimen about 12 inches long, a water source, a timer, a lighter, and a ruler. The test specimens are about 4 inches x about 12 inches in size, and typically five or more specimens are tested. The adhesive surfaces of the test specimens are typically exposed to the flame. For the FMVSS 302 test, the ventilation hood is typically opened wide enough to provide an airflow of about 150 cubic feet / minute. For the SAE J369 test, for example, the ventilation hood may be opened to provide the same airflow or may be fully open. Unless otherwise specified herein, the FMVSS 302 test is interchangeable with the SAE J369 test. The results of these tests can be classified in several ways, including DNI, SE / 0, SE / NBR, SE / B, B, and RB.DNI refers to materials that do not support combustion during or after a 15-second ignition period, and / or materials that do not propagate the flame front across any surface to a selected distance. SE / 0 refers to materials that ignite on a surface, but the flame extinguishes before traveling the selected distance. SE / NBR refers to materials that cease burning before 60 seconds from the start of timing and do not burn beyond approximately 50 mm from the start of timing. SE / B refers to a preceding flame front that travels a selected distance but extinguishes before reaching a second distance. B refers to materials that burn the entire distance. RB refers to materials that burn so rapidly that the burning rate cannot be measured. One or more of the following can also be measured: burning distance, burning time, burning rate, and whether the material is self-extinguishing. A test specimen may be considered "compliant" or "pass" the FMVSS 302 or SAE J369 test if the flame travels at less than approximately 102 mm / min. If the test specimen burns faster than 102 mm per minute, it may fail the test.

[0058] In certain embodiments, the articles described herein may include a textured film on their outer surface. In some embodiments, the textured film may include patterns, embossing, or other features that generally provide some depth to the film and result in a rough surface. The overall basis weight of the film is approximately 50 grams per square meter (gsm or g / m²). 2The thickness can vary from approximately 0.1 mm to approximately 0.5 mm, more specifically from approximately 0.15 mm to approximately 0.30 mm. The surface roughness value can be used as a measure of the film's depth. For example, the maximum height surface roughness (Rt) on at least one surface of the film can be measured by a stylus shape measuring device according to ISO 4287:1997 and be 8 microns or more, 10 microns or more, 15 microns or more, or more than 20 microns in the longitudinal and transverse directions. In other examples, the maximum height (Rt) can be measured by a stylus shape measuring device according to ISO 4287:1997 and be 30 microns or more in the longitudinal and transverse directions. In other embodiments, the maximum height (Rt) can be measured by a stylus shape measuring device according to ISO 4287:1997 and be 30 microns or more in the longitudinal and transverse directions. In certain embodiments, the maximum height (Rt) may exceed 50 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In some embodiments, the maximum height (Rt) may exceed 60 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the maximum height (Rt) may exceed 70 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In some cases, microspikes (or other non-planar structures) on the surface of the film layer bonded to the first surface of the porous core layer can enhance the adhesion of the textured film layer to the first surface of the porous core layer.

[0059] In certain embodiments, the textured film surface of an LWRT article described herein may have low or zero water absorption, as tested by a Cobb test. Water absorption or retention is generally a measure of the mass of water absorbed over a given time by a given area of ​​an LWRT article in contact with water. For example, water absorption can be measured by punching out a disc of material and clamping the punched disc with the textured film surface facing upwards. The clamp can surround the top surface of the disc to form a cylindrical wall capable of receiving water. Water is then poured into the cylinder, and after waiting for one minute, the water is removed and the test piece is weighed to determine how much water was absorbed, for example, to determine the weight gain rate. If the surface layer is porous or not water-resistant, water may penetrate and saturate the test piece, which results in a higher water retention rate or increased weight gain rate. In certain embodiments, the textured film surface of an LWRT may have a water absorption rate of less than 1%, more specifically less than 0.5%, or even 0%. As used herein, percentages refer to the percentage of weight increase after exposure to water. For example, the textured film surface of an LWRT article may be waterproof so that water or moisture cannot penetrate the surface, or is substantially impervious to it. As will be described in more detail below, the textured film layer may be used in combination with a non-porous layer or non-porous coating to further enhance the water resistance of the LWRT article.

[0060] In some examples, the materials used in the film may vary, and typically, the film is manufactured using polyolefins or combinations of polyolefins. For example, the film may include one or more polyethylene, polypropylene, combinations of polyethylene and polypropylene, and copolymers of polyethylene and polypropylene. In some embodiments, the textured film may be a homopolymer film, while in other embodiments, the textured film may contain two or more different polymers, for example, a copolymer film. If desired, different regions of the textured film may contain different polymer materials. The textured film may also contain colorants, additives, fibers, or other materials as needed.

[0061] In certain embodiments, the textured film may also include patterns or embossing on its surface. These patterns or embossings may be provided before or after the film is placed on the core layer. Patterns can be applied to the surface of the textured film by printing, embossing, etching, pressing, or other means in many different ways. Exemplary patterns include, but are not limited to, one or more of the following: square patterns, wood grain patterns, marble patterns, tile patterns, random patterns, pinwheel patterns, herringbone patterns, brick patterns, offset alternating brick patterns, offset patterns, grid patterns, laminated vertical patterns, French patterns, basket weave patterns, diamond patterns, or chevron patterns.

[0062] In other embodiments, the textured film can be used in combination with a topcoat of material added to the outer surface of the textured film by spraying, coating, or other means. The topcoat material can be varied and include thermoplastic and thermosetting materials, but typical topcoat materials include, but are not limited to, epoxy resins, acrylic resins, polyester resins, polycarbonate resins, melamine-formaldehyde resins, polyurethane resins, and other thermosetting or thermoplastic resins. In some examples, the resin may include polymers crosslinked by the use of aminoplasts. Such resins are commercially available, and exemplary resins / coatings are described, for example, in U.S. Patent Application Publication No. 20030055145. The exact thickness of the topcoat can vary and is typically much thinner than the overall film thickness. The topcoat is generally optically clear but may be colored if necessary. In some embodiments, the topcoat may also provide some degree of abrasion resistance according to ISO 9352:2012 Plastics - Determination of abrasion resistance by polishing wheel.

[0063] In some configurations, the textured film may also provide some degree of chemical resistance. For example, the textured film can be used to clean composite articles containing the textured film using conventional household cleaning agents, such as mild bleaches, quaternary amines, and alcohols, without damaging the textured film or removing any color or design. In certain embodiments, lightweight reinforced thermoplastic (LWRT) composites can be used as RV ceiling panels or RV ceilings. Figure 1 shows one figure in which RV 100 includes a ceiling panel comprising a core layer 110, a textured film 130, and a skin layer 120. The textured film 130 generally faces the interior space of RV 100, and the skin layer 120 can be bonded to other components of RV 100, as will be described in more detail below. The RV may include other layers or components. For example, an RV sidewall structure typically includes an exterior wall material, foam insulation (e.g., PET, EPS, or honeycomb foam), and an interior wall layer, all of which are laminated or bonded together and then installed as a roof and floor to provide strength to the entire unit. The roof or ceiling may include one or more foam layers, panels shown in Figure 1 bonded to RV structural components, etc. As will be discussed later, the core layer 110 may include a textured film layer and a porous web used in combination with optionally additional skin layers. Conventional manufacturing methods involve bonding the material offline onto a substrate (typically plywood) for use in RV ceilings. However, in recent years, concerns about formaldehyde emissions, the poor durability of plywood, and the high cost of the offline lamination process due to the use of polyurethane (PUR) adhesives to bond the material to the plywood have stimulated interest in developing products by in-line laminating textured film onto durable composite panels. In-line laminated textured film composite panels can provide similar or better quality surface, gloss, and color compared to offline laminated plywood panels, depending on the design / pattern.

[0064] In certain embodiments, an in-line process for manufacturing a panel having a textured film may include a number of steps controlled in an automated manner, typically using a processor or computer, as will be described in more detail below. Specifics of the process and the various materials used / manufactured by each step are shown by the block diagram in Figure 2. The LWRT layer is prepared by combining a thermoplastic material (TP), e.g., a thermoplastic resin, and a reinforcing material (RM) to form a dispersion or mixture 202. This mixture can then be deposited onto a suitable mobile support to provide a web 204 formed of the reinforcing material and the thermoplastic resin. The resulting web 204 may include an open-cell structure of reinforcing fibers held in place by the thermoplastic material. The resulting web 204 can be heated and dried to soften or melt the thermoplastic resin and form a porous core layer 206. One or more layers, e.g., a textured film layer, can then be applied to the surface of the formed and heated porous core layer 206. For example, a textured film layer can be applied to form an LWRT composite article 208. Although not shown, an impermeable layer or coating can be applied between the core layer 206 and the textured film to further make the assembly water-resistant or waterproof. The resulting LWRT composite can be compacted into flat sheets 210 that can be used when forming RV ceilings or other composite panels. For example, the flat sheets 210 on a movable support can be cut to provide individual LWRT composite articles 212. Various examples of process conditions, steps, and materials are described in more detail below.

[0065] As shown in Figure 3, the thermoplastic material may be present in reservoir 302, and the reinforcing fibers (or other reinforcing materials) may be present in a second reservoir 304. Each of the thermoplastic material and the reinforcing fibers can be introduced by metering, spraying, or other means into an aqueous solution in a mixing tank 306 containing water, liquid, or aqueous solution. If necessary, foams or other additives (described later) may be present in the mixing tank 306. The thermoplastic material and the reinforcing fibers can be mixed for an appropriate time and at an appropriate temperature to provide a substantially homogeneous aqueous dispersion of the fibers and thermoplastic material. For example, the materials may be mixed at room temperature, e.g., about 25 degrees Celsius, or above or below room temperature by heating or cooling the mixing tank. In some embodiments, as described later, the materials can be continuously added to the mixing tank 306 to continuously deposit the dispersion onto a moving support. The exact mixing time may vary depending on the materials used, but exemplary mixing times include 10 seconds to about 10 minutes, more specifically about 30 seconds to about 5 minutes. However, as described above, mixing is always occurring when the materials are continuously added to the mixing tank 306. The mixing tank 306 may include a paddle mixer, an impeller, or other devices to facilitate mixing.

[0066] In certain embodiments, referring to Figure 4A, the dispersion in the mixing tank 306 can be sprayed, dripped, or otherwise deposited onto the mobile support 410. Although the mobile support 410 is shown as a single segment in certain figures provided herein, the mobile support 410 can be divided into two or more individual segments as needed. The mixing tank 306 can be fluidly coupled to a plurality of spray heads 402 that can spray the dispersion onto the surface of the mobile support 410. As shown in Figure 4B, the mobile support 410 may be porous or may contain a mesh that can receive the dispersion. The exact deposition rate used may vary depending on the amount of material deposited per square meter. The mobile support 410 can be moved at a continuous and constant speed to allow continuous spraying of the dispersion along the upper surface of the mobile support 410. The area of ​​the mobile support 410 below the spray heads may be heated, cooled, or present at room temperature during the deposition of the dispersion. Different areas of the mobile support 410 may have different temperatures, as will be discussed later. The exact dimensions of the moving support 410 may vary, but typically the moving support is about 4 feet wide and can include a mesh or pore size of about 60 openings / square inch to about 80 openings / square inch. The moving support 410 allows for the receiving of dispersed material and the movement of the received dispersed material to additional locations or stations in the inline system. At the ends of the moving support 410, formed LWRT articles can be cut and stacked. The moving support 410 allows for the continuous formation of LWRT articles. In certain embodiments, the moving support 410 can be divided into two or more separate sections or segments. For example, a wet mat may be formed on the former belt and then, for example, manually or automatically, transferred to a separate dryer belt where it can pass through an oven or other drying device.

[0067] In certain embodiments, referring to Figure 5A, the mobile support 410 containing a dispersion of thermoplastic material and reinforcing fibers can be moved to a dryer 510. Alternatively, as described above, the dryer 510 may be positioned adjacent to a separate dryer belt that can receive the formed mat. The dryer 510 can provide heat and / or negative pressure (vacuum) to remove water from the web 502 on the mobile support 410, leaving the reinforcing fibers and thermoplastic material on the mobile support 410. This process can form a highly porous core layer 512 (see Figure 5B) containing an open-cell structure formed from the reinforcing fibers held in place by the thermoplastic material. Other materials may also be present in the core layer or sprayed onto the core layer 512, as needed. For example, an adhesive from a reservoir can be sprayed onto the surface of the formed core layer 512. In another example, a coating can be sprayed onto the core layer 512 to act as a non-porous layer, thereby increasing the water resistance of the final LWRT article. The exact temperature used to heat the web 502 and / or core layer 512 may vary, preferably higher than the melting point of the thermoplastic material and lower than the melting point of the reinforcing fibers. In some examples, the mobile support 410 itself may be heated, while in others, the drying apparatus 510 may include a heating element or be configured as an oven or other heating device. Although not shown, heated or cooled air may be blown across the top surface of the web 502 or core 512. If necessary, both the drying apparatus 510 and the mobile support 410 may supply heat to the web 502 on the mobile support 410. In some cases, the mobile support 410 may include a thermally conductive material that can retain heat from the drying apparatus 510 to help maintain the core layer 512 in a softened form during the application of the textured film layer or other material. In some examples, a separate pressure device 520 may be present (see Figure 5C). For example, a vacuum can be applied to the web 502 to remove water from it, leaving the reinforcing material and thermoplastic material.The pressure device 520 is typically located upstream of the dryer 510 and is designed to remove at least 40% of the volume of water from the web 502, more specifically about 60% of the volume of water from the web 502. If necessary, another pressure device (not shown) may be located downstream of the pressure device 520 or downstream of the dryer 510.

[0068] In certain embodiments, as the core layer 512 exits the drying apparatus 510, one or more skin layers can be applied to the surface of the core layer in an automated manner. As described herein, the outer skin layer typically takes the form of a textured film that imparts some surface roughness and / or pattern, embossing, etc., to the outer surface of the LWRT article. Referring to Figure 6A, a diagram is shown in which a textured film layer 610 is applied to the core layer 512 as the core layer 512 exits the moving support 410. For example, the textured film layer 610 may exist as a roll of film layer material 605 that is unfolded and continuously applied to one surface of the core layer 512. Although not shown in Figure 6A, the textured film layer material 605 can be stretched or elongated before the film layer 610 is applied to the surface of the core layer 512. In some examples, the textured film layer material 605 can be stretched longitudinally, for example in the direction of movement of the moving support, or transversely, for example in a direction perpendicular to the longitudinal direction. The degree of stretching depends on the specific material present in the textured film layer material 605, but in some embodiments, the film can be stretched by applying a stretching force of about 60 N to about 250 N to stretch the film layer material 605. The exact force applied may vary with thicker films, typically using a higher force to stretch the film. When a stretching force is applied, it is selected to be less than the elongation force at break so that the film does not tear during stretching. If necessary, the film layer material 605 can be stretched between multiple rollers before being applied to the core layer 512. The textured film layer 610 can be applied at room temperature, even if the core layer 512 may still be heated or otherwise present above room temperature on the moving support 410.

[0069] In some embodiments, the final LWRT article includes a textured film layer 610 on the surface of the core layer 512. A nonporous layer or nonporous material may be present between the surface of the core layer 512 and the textured film layer 610. For example, the porosity of the nonporous layer may be less than 5%, or even less than 1% or 0%, in order to provide an LWRT article that is inherently waterproof and can be used in wet environments such as shower walls, shower receptacles, RV shower walls, roof panels, exterior panels or siding, or other building and vehicle applications where the article may be exposed to water.

[0070] In a particular embodiment shown in Figure 6B, a second skin layer 620 can be applied to the second surface of the core layer 512 from a second roll 615 containing the second skin material. The skin layer 620 can be applied at room temperature, even if the core layer 512 may still be heated, otherwise it is present on the moving support 410 above room temperature. Alternatively, the rolls 605, 615 or layers 610, 620, or both, can be heated before being applied to the surface of the core layer 512. Layers 610, 620 can generally be applied sequentially to form a thermoplastic composite article comprising the core layer 512, the textured film layer 610, and optionally the second skin layer 620. Although not shown, an additional skin layer can be applied on top of the skin layer 620 using a similar process, although the textured film layer 610 tends to be the outer layer of the LWRT article facing the environment of use. However, if necessary, another layer, such as a second textured film layer, can be applied on top of the textured film layer 610.

[0071] In some embodiments, it may be desirable to apply an adhesive layer on the core layer 512 before applying layer 610 to the core layer 512. In such cases, an adhesive reservoir 720 (see Figure 7) is present and can be used to spray adhesive onto the surface of the core layer 512 before applying the film layer 610, so that an adhesive layer 722 is present on the surface of the core layer 512. The exact adhesive used may differ from thermoplastic adhesives, thermosetting adhesives, or combinations thereof. Although not shown, adhesive may also be applied to the opposite surface of the core layer 512 before applying the skin layer 620 to the core layer 512. Exemplary adhesives include polyolefin adhesives, polyurethane adhesives, and combinations thereof.

[0072] In certain embodiments, the resulting thermoplastic composite article can be compacted by applying pressure to the surface of the composite article. For example, referring to Figure 8A, the composite article can be compressed by passing it between rollers 810, 812, thereby strengthening the bond between layers 610, 620 and the core layer 512. The exact distance or gap between rollers 810, 812 may vary depending on the desired pressure applied and the desired final thickness of the composite article. Generally, the overall thickness of the composite article decreases after passing through rollers 810, 812. Rollers 810, 812 can operate at room temperature, above room temperature, or below room temperature. Roller 810 can also be kept at a temperature lower or higher than the temperature of roller 812. For example, it may be desirable to heat roller 812 to strengthen the adhesion of the film layer 610 to the surface of the core layer 512 while cooling roller 810 to maintain the core layer 512 in a more cured or solid form. Multiple sets of rollers 810, 812 may be present as needed. For example, referring to Figure 8B, a second set of rollers 820, 822 is shown. The gaps between different roller sets may differ. For example, the rollers 810, 812 of the first set may have a first gap smaller than the gap between rollers 820, 822. The gaps between different rollers may be fixed or varied. For example, it may be desirable to compress certain areas of the composite article more strongly to reduce the thickness of these compressed areas. In some cases, the edges of the composite article may be compressed more so that the thickness at the side edges of the composite article is lower. There may be three, four or more roller sets as needed. The rollers may be placed in an oven or heating device as needed to maintain the core layer in a softened state during the consolidation of the composite article. Alternatively, the temperature of each individual roller may be controlled independently to provide heat or cooling to specific surfaces of the article.

[0073] In certain embodiments, once the composite article is compacted, the continuous sheet of compacted composite article can be cut or shredded into individual sheets using a cutting device 910 (see Figure 9). The resulting individual composite articles can be stacked or palletized for shipment, for example, on a pallet 915, as shown in the stack 920. The dimensions of the composite articles in Figure 9 have been intentionally enlarged to show the stack, as the composite articles tend to be stacked as individual thin sheets having thicknesses ranging from, for example, 1 mm to about 30 mm. The exact size of the individual composite articles can vary from about 2 feet to about 8 feet wide and from about 4 feet to about 16 feet long. In some embodiments, the individual composite articles may be about 4 feet wide and about 8 feet long, resulting in dimensions similar to plywood panels commonly used in recreational vehicles and construction applications.

[0074] In certain configurations, core layers manufactured using an in-line process may include reinforcing fibers in combination with thermoplastic resin. For example, the core layer can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic resin material. For example, the core layer typically contains a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, porous core layers may have percentages of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, 20-60%, 20-70% This may include %, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges.

[0075] In certain embodiments, the thermoplastic material used to form the core layer described herein may include one or more polyolefins (e.g., polyethylene, polypropylene, etc.), polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and unplasticized, as well as blends of these materials with each other or other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic material used to form the core layer may be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein and, for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the core layer may vary, with exemplary amounts ranging from approximately 20% to approximately 80% by weight, for example, 30-70% or 35-65% by weight, based on the total weight of the core layer. Those skilled in the art will recognize that the total weight percentage of all materials used in the core layer can increase to 100% by weight.

[0076] In other embodiments, the reinforcing fibers of the core layer may include glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, e.g., para- and meta-aramid fibers, nylon fibers, polyester fibers, high melt flow index resins suitable for use as fibers (e.g., 100 g / 10 min MFI or higher), basalt, mineral wool (e.g., rock or slag wool), mineral fibers such as wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In certain embodiments, the fibers used may not contain cellulose to avoid or reduce the possibility of mold or other microorganism growth. In some embodiments, the fibers in the core may be two-component fibers, e.g., core-sheath fibers, as described, for example, in U.S. Patent Application Publication No. 20180162107, published June 14, 2018. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents, or both. The fiber content in the core layer may vary from about 20% to about 90% of the weight of the core layer, more specifically from about 30% to about 70% of the weight of the core layer. The specific size and / or orientation of the fibers used may depend, at least in part, on the desired properties of the thermoplastic material and / or core layer used. For example, the fibers may be randomly oriented or may have a specific selected orientation as desired. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally other additives to provide the core layer may generally have a diameter greater than about 5 microns, more specifically from about 5 microns to about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 microns to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0077] In certain embodiments, other additives may also be present in the mixture containing the thermoplastic resin and reinforcing fibers. For example, lofting agents, flame retardants, colorants, smoke suppressants, surfactants, foams, or other materials may be present. In some examples, the core layer may be substantially halogen-free or halogen-free to meet the limitations of hazardous substance requirements for a particular application. In other examples, the core layer may contain halogenated flame retardants, such as halogenated flame retardants containing one or more of F, Cl, Br, I, and At, or compounds containing such halogens, such as tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some cases, the thermoplastic material used for the core layer may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. If halogenated flame retardants are present, the flame retardant is preferably present in an amount that can vary depending on the other components present. For example, halogenated flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the core layer), more specifically, about 1% to about 13% by weight based on the weight of the core layer, for example, about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may also contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the core layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more core layers described herein.In certain cases, one or more core layers described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the core layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component), or they can be added after the layer has been formed. In some examples, the flame retardant material may contain one or more of the following: expandable graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0078] In certain embodiments, the skin layers 610 and 620 may be the same or different. For example, each of layers 610 and 620 may be a textured film layer, or one of layers 610 and 620 may be a textured film layer and the other layer may be a material or layer other than a textured film layer. In one example, skin layer 610 may be a cosmetic, embossed, or patterned film layer, and skin layer 620 may be a cosmetic, patterned layer, or other type of skin layer. If one or both of skin layers 610 and 620 include a pattern, the pattern may be the same or different in different areas of the skin layer. In some embodiments, the textured film layer or skin layer may include patterns that are one or more of the following: wood grain pattern (Figure 10A), marble pattern (Figure 10B), tile pattern (Figure 10C), random pattern (Figure 10D), pinwheel pattern (Figure 10E), herringbone pattern (Figure 10F), brick pattern (Figure 10G), offset alternating brick pattern (Figure 10H), offset pattern (Figure 10I), grid pattern (Figure 10J), laminated vertical pattern (Figure 10K), basket weave pattern (Figure 10L), diamond pattern (Figure 10M), chevron pattern (Figure 10N), or French pattern (Figure 10O). Other patterns are also possible. In some embodiments, the pattern may already be present on the textured film layer or skin layer material when it is on roll 605 or roll 615. In other examples, the pattern may be printed or embossed on the film layer or skin layer before applying the film layer or skin layer to the core layer. A diagram of a system that may include a printer for printing patterns onto the skin layer is described in more detail below. If one of layers 610 or 620 contains a pattern or embossing, the other layer may be, for example, a thermoplastic film, polyolefin film, elastomer film, scrim, frim, web, etc.In certain configurations, if the other layer takes the form of a thermoplastic film, the thermoplastic film includes at least one of the following: polyolefins, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone. In other examples, the other layer may be, for example, a frim (film + scrim), a scrim (e.g., fiber-based scrim), foil, woven fabric, nonwoven fabric, or exist as an inorganic coating, organic coating, or thermosetting coating. In other examples, the other skin layer may contain a limiting oxygen index greater than about 22, as measured according to ISO 4589 1996. If a fibrous scrim is present as (or as part of) another skin layer, the fibrous scrim may include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallated synthetic fibers, and metallated inorganic fibers. Optionally, the scrim may include materials or fibers manufactured from one or more of the thermoplastic materials described above in relation to the core layer. If a thermosetting coating is present as (or as part of) another skin layer, the coating may include at least one of unsaturated polyurethanes, vinyl esters, phenols, and epoxys. If an inorganic coating is present as (or as part of) another skin layer, the inorganic coating may include minerals containing cations selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as (or as part of) another skin layer, the nonwoven fabric may include thermoplastic materials, thermosetting binders, inorganic fibers, metal fibers, metallated inorganic fibers, and metallated synthetic fibers.If necessary, other skin layers may also include lofting agents, expandable graphite materials, flame retardants, fibers, etc. As described herein, if the LWRT article is intended for use in wet applications, it may be desirable to select other skin layers that do not contain cellulose to avoid microbial growth.

[0079] In certain embodiments, the composite articles described herein may have desired surface properties on at least one surface. For example, the core layer of an article described herein may have some inherent roughness due to the presence of reinforcing fibers. This roughness can be increased by selecting appropriate fibers having appropriate lengths. The substrate roughness of the core layer can be used in combination with the surface roughness of a textured film layer to impart overall roughness to the surface of the LWRT article. Surface roughness can be measured in many ways, but three roughness parameters can be used as measures of surface roughness: the mean arithmetic deviation of the profile (Ra), the root mean square of the profile height (Rq), and the maximum height (Rt). Ra is the average distance from the profile to the mean line over the evaluation length, Rq is the mean root mean square of the profile height over the evaluation length, and Rt is the vertical distance between the highest and lowest points of the profile within the evaluation length. See, for example, L. Mummery (1990), Surface Texture Analysis: Handbook, Hommelwerke, p. 106. Surface roughness can be measured using a stylus shape measuring device, generally conforming to JIS (JIS-B0601-2001, JIS-B0601-1994, JIS B0601-1982), VDA, ISO 4287:1997, and ANSI standards. The parameters (Ra, Rq, Rz, and Rt) can be characterized according to ISO 4287:1997.

[0080] In certain embodiments, the surface roughness (Ra) of at least one surface of an LWRT composite article, for example, a surface including a patterned layer, can exceed 7 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the surface roughness (Ra) of a surface of a thermoplastic composite article, including a textured film layer, can exceed 10 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other examples, the average RMS profile height (Rq) of at least one surface of a composite article, for example, a surface including a textured film layer, can exceed 1 micron in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the average RMS profile height (Rq) of a surface of a thermoplastic composite article, including a textured film layer, can exceed 12 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other examples, the maximum height (Rt) of at least one surface of a composite article, for example, a surface including a textured film layer, may be greater than 10 microns or greater than 20 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the maximum height (Rt) of a surface of a thermoplastic composite article including a textured film layer is greater than 30 microns or greater than 40 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997.

[0081] In certain configurations, the system can be used to carry out an inline process. A diagram of the system components is shown in Figure 11A. System 1100 includes reservoirs 1102 and 1104. Reservoir 1102 can accept thermoplastic material, and reservoir 1104 can accept reinforcing fibers. Reservoirs 1102 and 1104 can supply material to a mixing tank 1106. The mixing tank 1106 can be fluidly coupled to a spray head or nozzle 1108 to spray the mixed dispersion onto a moving support 1110. The web 1115 on the moving support 1110 can move through a vacuum or other pressure device 1120 which can remove liquid from the web 1115 to form a core layer 1122. The core layer 1122 can pass through a drying device 1125 to dry and heat the core layer. The textured film layer 1130 and the skin layer 1140 can be applied, respectively, from a feeder or rolls 1135, 1145 onto the opposite surface of the core layer 1122 to provide a composite article. The composite article can pass through a set of rollers 1160, 1162 to compact it. The compacted composite article can be cut into individual articles by a cutting device 1170 as the moving sheet of compacted thermoplastic composite article passes through the cutting device 1170. For example, a processor 1180 is shown that can control the movement of the moving support 1110, the spraying of material onto the moving support 1110, and other devices and parameters used by the system 1100.

[0082] In certain examples, system 1100 may include other components that may be located before or after the cutting device 1170. For example, system 1100 may include another cutting station 1175 (Figure 11B) designed to cut a tongue into one edge of the composite article and a groove into the opposite edge of the composite article. This recess allows different individual panels to interlock with each other when in use, and thus there is some overlap of panels at the joint. The overlap at the joint may be particularly desirable in wet applications to prevent water from penetrating behind the surface of the panels. In other examples, system 1100 may include another heating device 1185 (Figure 11C) that can be used to loft or increase the thickness of the composite article. The heating device 1185 may be located before or after the cutting device 1170 as desired. An optional adhesive reservoir 1190 (Figure 11D) may be present to provide adhesive to the core layer before applying the skin layer 1130. A second adhesive reservoir (not shown) may also be present to provide adhesive to the core layer before applying the skin layer 1140. If necessary, physical processes can be applied to the surface of the composite article, for example, by polishing, etching, or embossing the textured film layer to change the surface roughness or to impart a desired pattern or texture to the film layer.

[0083] In some embodiments, the system may include multiple sets of rollers. Different rollers may be present at different temperatures or provide different gap thicknesses to compress the composite article before it exits the moving support. In some examples, rollers may be used to compress the edges of the composite article more highly, resulting in an overall thickness at the edges of the composite article being lower than in the central region of the composite article. The thicknesses at different edges may be the same or different.

[0084] In other embodiments, the system may include a printer capable of printing a pattern onto the skin layer before applying the skin layer to the core layer. The printer can spray, print, or deposit ink and other materials, such as fibers, particles, powders, etc., onto the surface of the skin layer before or after the skin layer has been applied to the core layer. For example, the printer may be positioned near the roll 1135 of the film layer to print a pattern onto the surface of the skin layer 1130 as it unfolds from the roll 1135. Alternatively, the printer may print a pattern onto the skin layer 1130 after the pattern has been applied to the surface of the core layer. The exact pattern provided by the printer may vary and may differ in different areas of the skin layer. For example, the pattern printed on the skin layer may be one or more of the following: wood grain pattern, marble pattern, tile pattern, random pattern, pinwheel pattern, herringbone pattern, brick pattern, offset alternating brick pattern, offset pattern, grid pattern, laminated vertical pattern, French pattern, basket weave pattern, diamond pattern, or chevron pattern. In other examples, an embosser may be present and used to impart a pattern or texture to the film layer. The embosser may be used, for example, after the LWRT article has left the moving support. The LWRT article can be compressed between multiple plates to impart a pattern to one or more surfaces of the LWRT article from the plates.

[0085] In certain embodiments, ceiling panels can be manufactured using the in-line processes and in-line systems described herein. The ceiling panels may be present in recreational vehicles or other vehicles, commercial and residential structures or other environments. Figure 12 shows an example in which the RV ceiling 1200 includes a first laminated lightweight reinforced thermoplastic composite article 1210 comprising a porous core layer 1212, a first skin layer 1214 on a first surface of the porous core layer 1212, and a textured film layer 1216 on a second surface of the porous core layer 1212. The textured film layer 1216 is typically positioned to face the interior of the space formed by the RV. The RV ceiling 1200 may also include an optional foam layer 1220 bonded to the first laminated lightweight reinforced thermoplastic composite article 1210 at a first surface of the foam layer 1220. For example, the foam layer 1220 can be bonded to the first laminated lightweight reinforced thermoplastic composite article 1210 via the first skin layer 1214 of the first laminated lightweight reinforced thermoplastic composite article 1210, such that the textured film layer 1216 is located on the inner surface of the RV ceiling 1200. The RV ceiling 1200 also includes a support structure 1230, which can typically take the form of a chassis, tube, cage, or other structure. The support structure 1230 typically includes a metal such as steel, aluminum, or metal. The support structure 1230 can be bonded to a second surface of the foam layer 1220 at a first surface of the support structure 1230. Any second laminated lightweight reinforced thermoplastic composite article 1240 can be bonded to a second surface of the support structure 1230. The second laminated lightweight reinforced thermoplastic composite article 1240 includes a porous core layer 1242, a first skin layer 1244 on the first surface of the porous core layer 1242, and a second skin layer 1246 on the second surface of the porous core layer 1242. To form the RV ceiling 1200, exterior panels 1250 can be bonded to the second laminated lightweight reinforced thermoplastic composite article 1240. Alternatively, the LWRT article 1240 can be omitted, and the exterior panels 1250 can be directly bonded to the support structure 1230. In some examples, the exterior panels 1250 include glass fiber or aluminum.

[0086] As described herein, the textured film layer 1216 may include a pattern that is one or more of the following: wood grain pattern, marble pattern, tile pattern, random pattern, pinwheel pattern, herringbone pattern, brick pattern, offset alternating brick pattern, offset pattern, lattice pattern, laminated vertical pattern, French pattern, basket weave pattern, diamond pattern, or chevron pattern. In certain embodiments, the first skin layer 1214 of the first laminated lightweight reinforced thermoplastic composite article 1210 includes a scrim. In certain examples, the porous core layer 1212 of the first laminated lightweight reinforced thermoplastic composite article 1210 may include a web that includes an open-cell structure formed from reinforcing fibers held together by the thermoplastic material as described above. In some examples, the porous core layer 1242 of the second laminated lightweight reinforced thermoplastic composite article includes a web that includes an open-cell structure formed from reinforcing fibers held together by the thermoplastic material. In some configurations, the thermoplastic material of each porous core layer 1210, 1240 independently includes the thermoplastic materials described herein, for example, polyolefins such as polypropylene and polyethylene. In some embodiments, the reinforcing material for each porous core layer includes reinforcing fibers as described herein, such as glass fibers.

[0087] In certain embodiments, the RV ceiling may be present within the RV, including a roof, side walls coupled to the roof, and a floor coupled to the side walls to provide interior space within the recreation vehicle. An example of RV 1300 including an RV ceiling 1312 is shown in Figure 13, which may be similar to the RV ceiling 1200 described above. RV 1300 also includes side walls 1313, 1314 and a floor 1316. RV 1300 may include wheels 1352, 1354 to enable the towing of the RV and / or an engine, electric motor or other power source to enable the independent movement of the RV.

[0088] In certain embodiments, panels comprising the textured film layer described herein may be particularly suitable for use in wet applications where the panel is exposed to water. This water may be present in an internal environment, such as a shower or RV shower, or in an external environment, such as a roof panel or building siding. An example of a shower is shown in Figure 14A, where the shower stall 1410 can be configured as a stall comprising one or more panels comprising an LWRT panel comprising the textured film described herein. The shower stall 1410 has three panels, one or more of which may be LWRT panels comprising the textured film. Although not shown, the shower stall 1410 is typically used with a shower pan or receptacle that together provides a nearly watertight shower enclosure suitable for use in residential applications. If necessary, the shower may be configured as a single piece of material, as shown in Figure 14B. The shower enclosure 1450 has an integrated shower pan or receptacle, side walls, and a rear wall. Any one or more surfaces of the enclosure 1450 may be manufactured using LWRT articles having the textured films described herein. In certain wet bath RV applications, the shower enclosure 1450 may also include a toilet or be designed to accommodate a toilet.

[0089] Referring to Figure 15A, a side view of the siding panel 1500 is shown. The panel 1500 may include a core layer 1510 in combination with a textured film layer 1520 and a skin layer 1530. In some examples, the siding panel 1500 may be composed of a flame retardant or may be flame retardant in general. For example, the siding panel 1500, tested according to ASTM E84 2009, has a flame propagation index of less than 25 and a smoke index of less than 150. In some cases, there may be butt joints, overlapping joints, etc., that can interlock two siding panels horizontally with each other.

[0090] In certain examples, one or more of the LWRT panels having the textured films described herein may be configured as roof panels or shingles attached to buildings such as residential or commercial buildings. Roof panels can be used, for example, to cover attics, to be attached to roof trusses, or to cover flat roofs, such as those commonly found on commercial buildings. If necessary, roof panels may be bonded to another substrate, such as oriented strand boards, plywood, or solar cells, which are attached to and function as roof coverings. Referring to Figure 15B, a perspective view of roof panel 1560 attached to house 1550 is shown. In some examples, roof panel 1560 contains a flame retardant or is flame retardant itself and is bonded to an underlying roof board substrate. If necessary, roof panel 1560 may be tested according to ASTM E84 2009 and contain a flame propagation index of less than 25 and a smoke emission index of less than 150. Alternatively, roof panel 1560 may be configured as a shingle that can be nailed to an underlying roof substrate or bonded in another manner. In some cases, there may be butt joints, overlapping joints, or other connections that allow two roof panels or shingles to be locked together horizontally.

[0091] In certain examples, the inline methods and inline systems described herein may be controlled using one or more processors, which may be part of the inline system, or otherwise electrically coupled to the inline system via relevant devices, such as a computer, laptop, or mobile device. For example, a processor can be used to control the mixing rate of materials, the speed of a moving support, the pressure used to remove liquid from a placed dispersion, the temperature of a heating device, the pressure applied to the material, and other parameters of the process and system. Such processes may be performed automatically by the processor without requiring user intervention, or the user may input parameters via a user interface. In certain configurations, the processor may reside in one or more computer systems and / or common hardware circuits, including, for example, a microprocessor and / or appropriate software for operating the system, to control various fluid reservoirs, mixing tanks, pressure devices, temperatures, etc. The processor may be integrated with the inline system or reside on one or more accessory boards, printed circuit boards, or computers electrically coupled to components of the inline system. Typically, the processor is electrically coupled to one or more memory units to receive data from other components of the system and to allow adjustment of various system parameters as needed or desired.The processor may be part of a general-purpose computer, including processors designed by Apple, such as Unix®, Intel PENTIUM® processors, Intel Core® processors, Intel Xeon® processors, AMD Ryzen® processors, AMD Athlon® processors, AMD FX® processors, Motorola PowerPC, Sun UltraSPARC, Hewlett-Packard PA-RISC processors, Apple A14 Bionic processors, A13 Bionic processors, A12 processors, Apple A11 processors, etc., or based on any other type of processor. According to various embodiments of this technology, one or more of any type of computer system may be used. Furthermore, the system may be connected to a single computer or distributed across multiple computers connected by a communication network. If necessary, different components of the inline system may be controlled by separate processors or computers, distinct from the processors or computers used to control the other components of the inline system. Other functions, including network communication, may be performed, and it should be understood that this technology is not limited to having any particular function or set of functions. Various embodiments may be implemented as dedicated software running on a general-purpose computer system. A computer system may include a processor connected to one or more memory devices, such as disk drives, memory, or other devices for storing data. Memory is typically used to store programs, temperatures, moving support speeds, and other values ​​used in inline processes. Components of a computer system may be connected by interconnectors, which may include one or more buses (e.g., between components integrated within the same machine) and / or networks (e.g., between components residing in separate individual machines). Interconnectors provide communication (e.g., signals, data, instructions) exchanged between components of the system.A computer system is typically capable of receiving and / or issuing commands within processing times of, for example, milliseconds or less, to enable rapid control of the system. The processor is typically electrically coupled to a power source, which can be, for example, a DC source, an AC source, a battery, a solar cell, a fuel cell, or other power sources, or a combination of power sources. The power source may be shared by other components of the system. The system may also include one or more input devices, such as a keyboard, mouse, trackball, microphone, touchscreen, manual switch (e.g., override switch), and one or more output devices, such as a printing device, display screen, or speaker. Furthermore, the system may include one or more communication interfaces that connect the computer system to a communication network (in addition to or as a substitute for an interconnector). The system may also include appropriate circuits for converting signals received from various electrical devices present within the system. Such circuits may reside on a printed circuit board, or on a separate board or device electrically coupled to the printed circuit board via a suitable interface, such as a Serial ATA interface, ISA interface, PCI interface, USB interface, Fibre Channel interface, Firewire interface, M.2 connector interface, PCIe interface, mSATA interface, etc., or via one or more wireless interfaces, such as Bluetooth, Wi-Fi, near-field communication, or other wireless protocols and / or interfaces.

[0092] In certain embodiments, the storage system used in the systems described herein typically includes a computer-readable and writable non-volatile recording medium that can store software code that can be used by programs executed by the processor, or information to be processed by programs stored on or within the medium. The medium may be, for example, a hard disk, a solid-state drive, or flash memory. Programs or instructions executed by the processor may be located locally or remotely and may be retrieved by the processor by interconnection mechanisms, communication networks, or other means as desired. Typically, during operation, the processor loads data from the non-volatile recording medium into another memory that allows the processor to access the information faster than the medium. This memory is typically a volatile random-access memory, such as dynamic random-access memory (DRAM) or static memory (SRAM). This may be located within the storage system or memory system. The processor generally manipulates data in integrated circuit memory and then copies the data to the medium after processing is complete. Various mechanisms for managing data movement between the medium and integrated circuit memory elements are known and are not limited to these. The technology is also not limited to a particular memory system or storage system. In certain embodiments, the system may also include specially programmed, dedicated hardware such as application-specific integrated circuits (ASICs), microprocessor units (MPUs), or field-programmable gate arrays (FPGAs), or combinations thereof. Embodiments of this technology can be implemented in software, hardware, or firmware, or any combination thereof. Furthermore, such methods, operations, systems, system elements, and their components may be implemented as part of the systems described above, or as independent components. While a particular system is described as an example of one type of system capable of implementing various embodiments of this technology, it should be understood that embodiments are not limited to being implemented on the described system.Various embodiments can be implemented on one or more systems having different architectures or components. A system may comprise a general-purpose computer system programmable using a high-level computer programming language. The system may also be implemented using specially programmed, dedicated hardware. In the system, the processor is typically a commercially available processor, such as a well-known microprocessor available from Intel, AMD, Apple, etc. Many other processors are also commercially available. Such processors typically run an operating system that may be, for example, Windows 7, Windows 8, or Windows 10 operating systems available from Microsoft, MAC OS® X such as Snow Leopard, Lion, Mountain Lion, Mojave, High Sierra, or El Capitan, or other versions available from Apple, the Solaris operating system available from Sun Microsystems, or UNIX or Linux® operating systems available from various sources. Many other operating systems may be used, and in certain embodiments, a simple set of commands or instructions may function as the operating system.

[0093] In certain examples, the processor and operating system together may define a platform on which application programs in a high-level programming language can be written. It should be understood that this technology is not limited to a specific system platform, processor, operating system, or network. Furthermore, given the merits of this disclosure, it will be apparent to those skilled in the art that this technology is not limited to a specific programming language or computer system. It should also be understood that other suitable programming languages ​​and other suitable systems may be used. In certain examples, the hardware or software may be configured to implement a cognitive architecture, a neural network, or other suitable implementation. If desired, one or more parts of a computer system may be distributed across one or more computer systems coupled to a communication network. These computer systems may also be general-purpose computer systems. For example, various embodiments may be distributed across one or more computer systems configured to provide services (e.g., servers) to one or more client computers, or to perform an entire task as part of a distributed system. For example, various embodiments may run on a client-server or multi-tier system including components distributed across one or more server systems performing various functions according to various embodiments. These components may be executable code, intermediate code (e.g., IL), or interpreted code (e.g., Java) that communicates over a communication network (e.g., the Internet) using a communication protocol (e.g., TCP / IP). It should also be understood that this technology is not limited to running on any particular system or group of systems. Furthermore, it should be understood that this technology is not limited to any particular distributed architecture, network, or communication protocol.

[0094] In some cases, various embodiments can be programmed using object-oriented programming languages ​​such as SQL, SmallTalk, Basic, Java, Javascript, PHP, C++, Ada, Python, iOS / Swift, Ruby on Rails, or C# (C-Sharp). Other object-oriented programming languages ​​may also be used. Alternatively, functions, scripts, and / or logic programming languages ​​may be used. Various configurations can be implemented in an unprogrammed environment (e.g., a document created in HTML, XML, or another format that renders a graphical user interface (GUI) or performs other functions when displayed in a browser program window). A particular configuration may be implemented as programmed or unprogrammed elements, or any combination thereof. In some examples, the system may have a remote interface, such as one residing on a mobile device, tablet, laptop computer, or other portable device, which can communicate via a wired or wireless interface and, if desired, allows for remote control of the inline system.

[0095] In certain examples, the processor may also have, or be able to access, a database of information about specific items to be manufactured. For example, specific parameters used to manufacture a core layer of a desired thickness and composition can be retrieved from the database and used by the inline system. Instructions stored in memory can execute software modules or control routines for the system, and in practice, can provide a controllable model of the inline system. The processor can use information accessed from the database, along with one or more software modules running within the processor, to determine control parameters or values ​​for different components of the system, such as different temperatures, different pressures, different consolidation equipment, etc. Using input and output interfaces for receiving control instructions linked to different system components within the system, the processor can perform active control over the system.

[0096] Specific examples of LWRT articles manufactured and tested using an in-line process are described below. [Examples]

[0097] Example 1

[0098] LWRT articles were prepared by adding chopped glass fibers (e.g., 30-70 wt%) to a polypropylene (PP) resin matrix as a reinforcing material using the in-line process described herein to form a web or core. A textured film layer was added to one surface of the core, and a second skin (23 gsm water-repellent black scrim) was added to the opposite surface using the in-line process along with in-line calendering, pressing the skin onto the core to form an LWRT article. Various properties of the films and LWRT articles are shown in Table 1 of Figure 16. Six different textured films were used with basis weights ranging from 110 gsm to 166 gsm. Film thicknesses varied from 0.17 mm to 0.30 mm. Different films contained different decorations / textures.

[0099] Film #1 included both printing and embossing, along with a random square pattern (see Figure 17A). Film #2 included deep embossing and a white wood grain pattern (see Figure 17B). Film #3 included printing and embossing, along with a dark wood grain pattern (see Figure 17C). Film #4 included printing with deep embossing, rough / coarse spikes on the reverse side of the film, and a dark fabric pattern (see Figure 17D (A or front) and Figure 17E (B or back)). Film #5 included printing and shallow embossing, along with a gray fabric pattern (see Figure 17F (A or front) and Figure 17G (B or back)). Film #6 included shallow embossing printed with a rough fabric and pattern (see Figure 17H ​​(A or front) and Figure 17I (B or back)). If the top thermosetting coating is shown in Table 1 (Film 3), the top thermosetting coating may be one or more of the following: epoxy resin, acrylic resin, polyester resin, polycarbonate resin, melamine-formaldehyde resin, or polyurethane resin. As a representative film, Film #3 was tested for its ability to meet indoor air quality tests. Film #3 passed indoor air quality tests for all volatile organic compounds, toluene, and formaldehyde.

[0100] These films were used with a 23gsm water-repellent scrim and a polypropylene glass fiber core (45 wt% PP and 55 wt% glass fiber) to achieve a yield of 960 g / m², as shown in Table 2 of Figure 18. 2 We provided LWRT articles having a basis weight of [specified value]. [Examples]

[0101] Example 2

[0102] Surface roughness (Rt) measurements were performed on various LWRT articles and films used in Example 1. The results are shown in Table 3 of Figure 19. The longitudinal direction refers to the same direction of movement as the moving support, and the transverse direction is perpendicular to the longitudinal direction. Roughness can indirectly indicate the level of emboss depth retention, with higher Rt values ​​suggesting a deeper texture. Depending on whether the film is embossed only or "embossed + top coating", some texture depths, namely films #2 and ST-13636, can be retained better, while other patterns such as films #4, #5, and #6 may lose 50% of the texture depth. Therefore, various levels of texture depth can be adopted depending on the application and preference. Films #1-4 provided a relatively much deeper / rougher texture compared to films #5 and 6. [Examples]

[0103] Example 3

[0104] Flame retardancy tests were performed on various samples according to the FMVSS 302 standard. FMVSS 301 is equivalent to ASTM E84. During the tests, the textured film surface was exposed to flames.

[0105] The results are shown in Table 4 of Figure 20. For comparison, a similar core with 23gsm scrim on both sides has a burning rate value of 2.1 inches / min according to FMVSS 302. Only sample ST-13928 has a higher burning rate than the reference scrim / core / scrim / board, indicating that most boards with film provided better flame retardancy than the reference board. These results are consistent with LWRT articles that meet Class A or Class B standards under ASTM E84. [Examples]

[0106] Example 4

[0107] Further properties of the board, including ash content, thickness, basis weight, density, scrim adhesion, film adhesion, bending peak load, bending stiffness, water retention, surface energy, and flat tensile peak load, were also measured for the articles. The results are shown in Tables 5 and 6 in Figures 21 and 22.

[0108] The presence of a textured film generally increases the rigidity of LWRT boards. While the film surface is highly water-resistant, the scrim surface also provides good water resistance. Flat tensile test results show that these in-line laminates are significantly stronger than EPS or other insulating foams, suggesting that these in-line laminates will not fail before the foams do.

[0109] The adhesive (hot melt) layers of films #1-3 can help them adhere well to the LWRT composite core. Deeply embossed films like film #4 (ST-13799) can also be useful for mechanical bonding to the LWRT composite core. Films #5 and #6 do not have a hot melt adhesive layer on the back, and their embossing type falls into the category of shallow embossing. Therefore, their film / core adhesion is not as good as the other four samples.

[0110] When introducing elements of the examples disclosed herein, the articles “a,” “an,” “the,” and “said” are intended to mean that there are one or more elements. The terms “comprising,” “including,” and “having” are intended to be open-ended, meaning that additional elements other than those enumerated may exist. In light of the merits of this disclosure, it will be recognized by those skilled in the art that various components of the examples can be interchanged or substituted with various components of other examples.

[0111] While specific aspects, configurations, examples, and embodiments have been described above, those skilled in the art will recognize that, in consideration of the interests of this disclosure, additions, substitutions, modifications, and changes are possible to the disclosed exemplary aspects, configurations, examples, and embodiments.

Claims

1. 1. An in-line process for manufacturing a thermoplastic composite article using an in-line system, comprising: mixing a reinforcing material and a thermoplastic material in an aqueous solution; placing the aqueous solution of the reinforcing material and the thermoplastic material on a moving support; removing water from the aqueous solution disposed on the moving support to form a web including an open cell structure formed from the reinforcing material and the thermoplastic material; drying the web on the moving support to provide a porous core layer; heating the dried porous core layer on the moving support to melt the thermoplastic material of the heated porous core layer; placing a first textured film layer on a first surface of the heated porous core layer on the moving support; and applying pressure to the heated porous core layer including the first textured film layer disposed on the moving support to provide a thermoplastic composite article.

2. The in-line process of claim 1 , wherein the porous core layer is heated at a first temperature above the melting point of the thermoplastic material and below the melting point of the reinforcing material.

3. 10. The in-line process of claim 1, further comprising adding a foam to the aqueous solution in which the reinforcing material and the thermoplastic material are mixed.

4. 10. The in-line process of claim 1, further comprising adding a lofting agent to the aqueous solution in which the reinforcing material and the thermoplastic material are mixed.

5. 10. The in-line process of claim 1, further comprising configuring the first textured film layer as a polyolefin film.

6. 6. The in-line process of claim 5, further comprising configuring the polyolefin film to include a maximum height surface roughness (Rt) of at least 8 microns as measured using a stylus profilometer.

7. The in-line process of claim 6 , wherein the first textured film layer further comprises a pattern.

8. 8. The in-line process of claim 7, wherein the pattern is one or more of a wood grain pattern, a marble pattern, a tile pattern, a random pattern, a pinwheel pattern, a herringbone pattern, a brick pattern, an offset staggered brick pattern, an offset pattern, a lattice pattern, a laminated vertical pattern, a French pattern, a basket weave pattern, a diamond pattern, or a chevron pattern, the thermoplastic material comprises a polyolefin, and the reinforcing material comprises inorganic fibers.

9. 10. The in-line process of claim 1, further comprising stretching the first textured film layer prior to disposing the first textured film layer on the first surface of the heated porous core layer on the moving support.

10. 10. The in-line process of claim 9, wherein the first textured film layer is stretched in the machine direction.

11. 10. The in-line process of claim 1 , wherein the first textured film layer is disposed on the heated porous core layer without the use of an adhesive between the first textured film layer and the heated porous core layer.

12. The in-line process of claim 1 further comprising disposing a skin layer on the second surface of the heated porous core layer on the moving support.

13. 13. The in-line process of claim 12, further comprising disposing an adhesive on the second surface of the heated porous core layer prior to disposing the skin layer on the second surface.

14. 10. The in-line process of claim 1, further comprising configuring the thermoplastic composite article to meet Class B standards as tested by ASTM E84, 2009.

15. 15. The in-line process of claim 14, further comprising configuring the thermoplastic composite article to meet Class A standards as tested by ASTM E84, 2009.

16. 10. The in-line process of claim 1, further comprising consolidating the heated porous core layer prior to disposing the first textured film layer on the first surface.

17. 20. The in-line process of claim 16, further comprising heating the thermoplastic composite article after consolidating the thermoplastic composite article to increase an overall thickness of the thermoplastic composite article.

18. 10. The in-line process of claim 1, further comprising printing a pattern onto the first textured film layer after disposing the first textured film layer on the first surface of the heated porous core layer.

19. 10. The in-line process of claim 1, further comprising embossing the first textured film layer after disposing the first textured film layer on the first surface of the heated porous core layer.

20. 10. The in-line process of claim 1, further comprising disposing a non-porous layer on the first surface of the heated porous core layer prior to disposing the first textured film layer.