In-line lamination process for producing decorative thermoplastic composite panels

JP2023550718A5Inactive Publication Date: 2024-11-20AZDEL INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023528306
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-05-13
Filing Date
2021-11-12
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Manufacturing decorative panels is time-consuming and tedious, often requiring separate processes and locations for different components.

Method used

An in-line lamination process combining reinforcing materials and thermoplastic materials in an aqueous solution, forming a web with an open cell structure, drying and heating to create a porous core layer, and applying skin layers with or without adhesive to produce a thermoplastic composite article.

Benefits of technology

The process results in a lightweight, durable, and aesthetically pleasing composite panel with improved surface smoothness and enhanced properties such as flame retardancy and acoustic performance, reducing the likelihood of delamination and increasing strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

An in-line system and method for manufacturing lightweight, reinforced thermoplastic composite panels are described. The in-line system and method can be used to manufacture composite panels with smoother surfaces and enhanced properties in an automated manner. The manufactured composite panels can include a decorative layer that can provide an overall smoother panel surface compared to a composite panel lacking the decorative layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Priority Claim

[0002] This application claims priority and interest in U.S. Patent Application No. 63 / 112,914, filed November 12, 2020, U.S. Patent Application No. 63 / 145,073, filed February 3, 2021, and U.S. Patent Application No. 63 / 188,358, filed May 13, 2021. The entire disclosures of each of these applications are incorporated herein by reference.

[0003] Technical field

[0004] The specific configurations described herein relate to in-line lamination processes that can manufacture decorative panels. In some examples, the decorative panels can be used for recreational vehicles or building applications. [Overview of the project] [Problems that the invention aims to solve]

[0005] background

[0006] The manufacturing of decorative panels can be time-consuming and cumbersome. Often, the different components of a panel are manufactured using different processes or in different locations. [Means for solving the problem]

[0007] overview

[0008] This document describes specific aspects, configurations, embodiments, and examples of inline processes that can be used to manufacture decorative panels that can be used in recreational vehicles or architectural applications.

[0009] In one embodiment, a process for manufacturing a thermoplastic composite article using an in-line system is described. In a particular configuration, the in-line process includes combining a reinforcing material and a thermoplastic material in an aqueous solution. The in-line process may also include placing the aqueous solution of the mixed reinforcing material and thermoplastic material onto a mobile support. The in-line process may also include removing water from the placed aqueous solution on the mobile support to form a web containing an open-cell structure formed from the reinforcing material and thermoplastic material. The in-line process may also include drying the web on the mobile support to provide a porous core layer. The in-line process may also include heating the dried porous core layer on the mobile support to melt the thermoplastic material of the heated porous core layer. The in-line process may also include placing a first skin layer on a first surface of the heated porous core layer on the mobile support. The in-line process may also include placing a second skin layer on a second surface of the heated porous core layer on the mobile support. The in-line process may also include applying pressure to the heated porous core layer, including the first skin layer and the second skin layer placed on the mobile support, to provide a thermoplastic composite article.

[0010] In certain embodiments, the porous core layer is heated to a first temperature higher than the melting point of the thermoplastic material and lower than the melting point of the reinforcing material. In some embodiments, the in-line process may include adding a foam to an aqueous solution of the reinforcing material and the thermoplastic material. In other embodiments, the in-line process may include adding a lofting agent to an aqueous solution of the reinforcing material and the thermoplastic material. In additional embodiments, the in-line process may include configuring the first skin layer as a scrim. In some embodiments, the in-line process may include configuring the second skin layer as a patterned layer. In certain embodiments, the pattern of the patterned layer may include one or more of the following: wood grain pattern, marble pattern, tile pattern, random pattern, pinwheel pattern, herringbone pattern, brick pattern, offset alternating brick pattern, offset pattern, lattice pattern, laminated vertical pattern, French pattern, basket weave pattern, diamond pattern, or chevron pattern. In other embodiments, the thermoplastic material includes polyolefin and the reinforcing material includes inorganic fibers.

[0011] In some cases, the surface roughness (Ra) of thermoplastic composite articles is less than 3 microns in both the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other cases, the surface roughness (Ra) of thermoplastic composite articles is less than 2 microns in both the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997.

[0012] In some embodiments, the first skin layer is placed on the heated porous core layer without using an adhesive between the first skin layer and the heated porous core layer. In certain embodiments, the inline process includes placing an adhesive on the second surface of the heated porous core layer before placing the second skin layer on the second surface. In some embodiments, the adhesive includes polyolefin or polyurethane. In certain examples, the inline process includes cutting a groove at the first end of the thermoplastic composite panel. In other examples, the inline process includes cutting a tongue at the second end of the thermoplastic composite panel.

[0013] In some embodiments, the inline process includes compacting the heated porous core layer before placing the first skin layer on the first surface and before placing the second skin layer on the second surface.

[0014] In certain examples, the in-line process includes heating the thermoplastic composite article after compacting it in order to increase the overall thickness of the thermoplastic composite article.

[0015] In an additional example, the inline process includes printing a pattern on the second skin layer before placing the second skin layer on the second surface of the heated porous core layer.

[0016] In other embodiments, the inline process includes placing a second skin layer on a second surface of a heated porous core layer, and then printing a pattern on the second skin layer.

[0017] In other embodiments, the inline process includes compressing the side edges of a heated porous core layer, the compressed side edges of the heated porous core layer having a thickness thinner than the thickness of the central region of the heated porous core layer.

[0018] In another embodiment, an in-line system configured for manufacturing a thermoplastic composite article is provided. In a particular embodiment, the in-line system comprises a fluid reservoir configured to receive an aqueous solution, a thermoplastic material, and a reinforcing material, the fluid reservoir configured to mix the thermoplastic material and the reinforcing material in the aqueous solution to provide a homogeneous dispersion of the thermoplastic material and the reinforcing material in the aqueous solution. In another embodiment, the in-line system comprises a mobile support fluidly coupled to the fluid reservoir and configured to receive a homogeneous dispersion from the fluid reservoir and hold the homogeneous dispersion on the mobile support. In some examples, the in-line system comprises a pressure device configured to remove water from the homogeneous dispersion on the mobile support to provide a web containing an open-cell structure formed from the reinforcing material and the thermoplastic material. In a particular example, the in-line system comprises a device configured to dry and heat the web on the mobile support to provide a porous core layer on the mobile support. Separate drying and heating devices may also be used as needed. In another example, the in-line system comprises a heating device configured to heat the porous core layer on the mobile support to melt the thermoplastic material of the porous core layer. In an additional example, the inline system comprises a first feeder configured to receive a first skin material, the first feeder configured to provide the first skin material as a first skin layer on a first surface of the porous core layer on a moving support. In another embodiment, the inline system comprises a second feeder configured to receive a second skin material, the second feeder configured to provide the second skin material as a second skin layer on a second surface of the porous core layer on a moving support. In an additional configuration, the inline system comprises a compaction device configured to compact the heated porous core layer with the positioned first skin layer and the positioned second skin layer by applying pressure to the heated porous core layer and the positioned first skin layer and the positioned second skin layer to provide a substantially flat thermoplastic composite article.

[0019] In certain embodiments, a first feeder is configured to receive a roll of first skin material. In other embodiments, a second feeder is configured to receive a roll of second skin material. In additional embodiments, the inline system further includes a device configured to cut the thermoplastic composite article into individual sheets as the thermoplastic composite article leaves the moving support. In some examples, the inline system includes a second heating device located after the compaction device, which is configured to heat the thermoplastic composite article to increase the overall thickness of the thermoplastic composite after compaction. In other configurations, the inline system includes a sprayer fluid-coupled to a fluid reservoir, which is configured to spray a uniform dispersion onto the moving support. In some embodiments, the inline system includes an adhesive reservoir configured to place an adhesive on the second surface of a heated porous core layer before placing the second skin layer on the second surface of the heated porous core layer.

[0020] In certain configurations, the inline system includes a printer configured to print a pattern on the second skin layer after the second skin layer has been placed on the second surface of the heated porous core layer. In other embodiments, the inline system includes a printer configured to print a pattern on the second skin material before the second skin layer has been placed on the second surface of the heated porous core layer. In some embodiments, the inline system includes a processor configured to control the movement of a moving support.

[0021] In another embodiment, the recreation vehicle (RV) wall includes a first laminated lightweight-reinforced thermoplastic composite article comprising a porous core layer, a first skin layer on a first surface of the porous core layer, and a patterned second skin layer on a second surface of the porous core layer. In some examples, the RV wall includes a foam layer bonded to the first laminated lightweight-reinforced thermoplastic composite article at a first surface of the foam layer, the foam layer being bonded to the first laminated lightweight-reinforced thermoplastic composite article via a first skin layer of the first laminated lightweight-reinforced thermoplastic composite article, and as a result, the patterned second skin layer is located on the inner surface of the recreation vehicle wall. In other embodiments, the RV wall includes a support structure bonded to a second surface of the foam layer at a first surface of the support structure. In further examples, the RV wall includes a second laminated lightweight-reinforced thermoplastic composite article bonded to a second surface of the support structure, the second laminated lightweight-reinforced thermoplastic composite article comprising a porous core layer, a first skin layer on a first surface of the porous core layer, and a second skin layer on a second surface of the porous core layer. In some embodiments, the RV wall includes an exterior panel bonded to a second laminated lightweight reinforced thermoplastic composite article. In some examples, the exterior panel includes fiberglass or aluminum. In other examples, the support structure includes tubes or a network.

[0022] In certain embodiments, the patterned second skin layer includes one or more of a wood grain pattern, a marble pattern, a tile pattern, a random pattern, a whirl pattern, a herringbone pattern, a brick pattern, an offset brick pattern, an offset pattern, a lattice pattern, a stacked vertical pattern, a French pattern, a basket weave pattern, a diamond pattern, or a chevron pattern. In some embodiments, the first skin layer of the first laminated lightweight reinforced thermoplastic composite article includes a scrim. In other embodiments, the porous core layer of the first laminated lightweight reinforced thermoplastic composite article includes a web including a continuous cellular structure formed from reinforcing fibers held together by a thermoplastic material. In other configurations, the porous core layer of the second laminated lightweight reinforced thermoplastic composite article includes a web including a continuous cellular structure formed from reinforcing fibers held together by a thermoplastic material. In a particular example, the thermoplastic material in each porous core layer independently includes a polyolefin. In some embodiments, the reinforcing material of each porous core layer includes glass fibers. In other embodiments, the thermoplastic material in each porous core layer is polypropylene.

[0023] In another aspect, a recreational vehicle includes a roof, sidewalls coupled to the roof, and a floor coupled to the sidewalls to provide an interior space within the recreational vehicle, wherein at least one of the sidewalls comprises a wall panel of the recreational vehicle described herein. In some embodiments, the recreational vehicle includes wheels to enable towing or operation of the recreational vehicle.

[0024] Further aspects, configurations, embodiments and examples are described below. [[ID=…]]

[0025] [[ID=…]] Brief description of some of the views of the drawings

[0026] To facilitate a better understanding of the technology described herein, specific specific exemplifications are described below with reference to the accompanying drawings.

Brief description of the drawings

[0027] [Figure 1] This is a simplified diagram showing the side wall of a recreation vehicle according to several embodiments. [Figure 2] A block diagram showing specific steps of an inline process that can be used, according to several embodiments. [Figure 3] This figure shows specific components that can be used to add materials to a mixing tank, according to a particular example. [Figure 4A] This is a diagram of a movable support according to several embodiments. [Figure 4B] This is a diagram of a movable support according to several embodiments. [Figure 5A] This figure shows a drying apparatus according to a specific embodiment. [Figure 5B] This figure shows a drying apparatus according to a specific embodiment. [Figure 5C] This figure shows a drying apparatus according to a specific embodiment. [Figure 6A] This figure shows the application of a skin layer to a core layer according to a specific embodiment. [Figure 6B] This figure shows the application of a skin layer to a core layer according to a specific embodiment. [Figure 7] This figure shows an adhesive layer reservoir that can be used to apply adhesive to the surface of a core layer, with several examples. [Figure 8A] This figure shows rollers that can be used in inline processes, with several examples. [Figure 8B] This figure shows rollers that can be used in inline processes, with several examples. [Figure 9] This figure shows a cutting device that can be used to cut a moving composite material article into individual composite material articles, according to a specific embodiment. [Figure 10A] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10B] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10C] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10D] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10E] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10F] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10G] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10H] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10I] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10J] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10K] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10L] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10M] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10N] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 10O] Several examples illustrate the different patterns that can exist on a patterned skin layer. [Figure 11A] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 11B] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 11C]This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 11D] This is a diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 12] Another diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 13] Another diagram of a system that can be used to perform an inline process according to a specific embodiment. [Figure 14] This is a diagram of the wall of a recreational vehicle (RV) according to several embodiments. [Figure 15] This is a diagram of a recreational vehicle that may include the RV wall described herein, by some example. [Figure 16A] This is a photograph showing a wood grain pattern. [Figure 16B] This is a photograph showing a marble pattern. [Figure 17A] This figure shows a test specimen used in a flat tensile test according to a specific embodiment. [Figure 17B] This figure shows a test specimen used in a flat tensile test according to a specific embodiment. [Figure 18A] This figure shows the peak loading of a specific test specimen. [Figure 18B] This figure shows the bending gradient of a specific test specimen. [Figure 19A] The sound absorption test results for the test sample and reference sample are shown. [Figure 19B] The sound absorption test results for the test sample and reference sample are shown. [Modes for carrying out the invention]

[0028] Detailed explanation

[0029] Given the advantages of this specification, it will be recognized by those skilled in the art that the different layers described herein are not necessarily shown to a constant scale. Unless specifically indicated in the description relating to its particular configuration, no material is intended to be required for any single layer. The thickness, arrangement, and end use of the decorative panels may vary.

[0030] In certain embodiments, the processes described herein can be used to manufacture decorative panels for use in building applications, vehicles such as recreational vehicles, and other applications. Recreational vehicles (RVs), including campervans and towed vehicles, can reduce weight by incorporating lightweight fiberglass-reinforced thermoplastic composite panels into sidewalls, ceilings, roof panels, or floor components. Compared to traditionally used wood composites, i.e., plywood, polymer composites offer a wealth of advantages, including better durability due to formaldehyde-free properties, lighter weight for fuel efficiency, improved acoustic performance, water and mold resistance, and flame retardancy derived from the advanced functional integration of the glass and thermoplastic resin matrices. In some configurations, reinforcing fibers, such as glass fibers, can favorably impart to the modulus of elasticity of the resin matrix, resulting in enhanced properties with minimal weight increase. The performance of the resulting composite may depend, at least in part, on the core composition (fiber / resin ratio), weight per unit area (surface density), panel application thickness, and functional skin material.

[0031] In certain embodiments, a decorative layer, sometimes referred to herein as a decorator, can be used to cover / hide the porous and rough texture of the underlying material, providing a more natural material appearance. For example, the decorative skin can be bonded to the underlying web or core layer in an online process, so it is generally not separable from the composite core. The resulting composite article can exhibit high tensile strength and eliminate the problem of delamination of the decorative skin / / core at the interlayer interface within the RV sidewall structure. The decorative skin material can also improve the bending stiffness of the board, particularly in the longitudinal direction. The patterned panel can also pass the ASTM E84 Class A flame retardancy classification.

[0032] In certain embodiments, lightweight reinforced thermoplastic (LWRT) composites can be used for RV sidewall and roofing applications. RV sidewall structures typically include an exterior wall material, foam insulation (e.g., PET, EPS, or honeycomb foam), and an interior wall layer, all of which are laminated or bonded together and then installed as roofing and flooring to provide strength to the entire unit. Referring, for example, to Figure 1, a simplified diagram shows an RV 100 and an RV sidewall 110. An exploded view of the sidewall 110 includes a fiberglass exterior 112, an LWRT layer 114, a chassis 116 (e.g., a metal cage or tubular structure), a foam 118, and another LWRT 120, typically located on the interior surface of the RV. The LWRT 120 may include a decorative pattern on the interior surface of the RV, visible to people inside the RV. As described below, the LWRT 120 may include a decorative skin and, optionally, a porous web in combination with additional skin layers. Conventional manufacturing methods involve applying decorative paper or vinyl film offline onto a substrate (typically plywood). However, in recent years, concerns about formaldehyde emissions, the poor durability of plywood, and the high cost of the offline lamination process due to the use of polyurethane (PUR) adhesives to bond decorative materials to plywood have stimulated interest in developing products by inline laminating decorative materials onto durable composite panels. Inline laminated decorative composite panels can offer similar or better quality surfaces, gloss, and colors compared to offline laminated plywood / decor panels, depending on the design / pattern.

[0033] In certain embodiments, an in-line process for manufacturing a decorative panel may include a number of steps controlled in an automated manner, typically using a processor or computer, as will be described in more detail below. Specific aspects of the process and the various materials used / manufactured by each step are shown by the block diagram in Figure 2. The LWRT layer is prepared by combining a thermoplastic material (TP), e.g., a thermoplastic resin, and a reinforcing material (RM) to form a dispersion or mixture 202. This mixture can then be deposited onto a suitable mobile support to provide a web 204 formed of the reinforcing material and the thermoplastic resin. The resulting web may include an open-cell structure of reinforcing fibers held in place by the thermoplastic material. The resulting web can be heated and dried to soften or melt the thermoplastic resin and form a porous core layer 206. One or more skin layers can then be applied to the surface of the formed and heated porous core layer. For example, a decorative layer can be applied to form an LWRT composite article 208. The resulting LWRT composite can be compacted into a flat sheet 210, which can be used to form an RV panel or other composite panel. For example, a flat sheet 210 on a movable support can be cut to provide individual LWRT composite articles 212. Various examples of process conditions, steps, and materials are described in more detail below.

[0034] As shown in Figure 3, the thermoplastic material may be present in reservoir 302, and the reinforcing fibers (or other reinforcing materials) may be present in a second reservoir 304. Each of the thermoplastic material and the reinforcing fibers can be introduced by metering, spraying, or other means into an aqueous solution in a mixing tank 306 containing water, liquid, or aqueous solution. If necessary, foams or other additives (described later) may be present in the mixing tank 306. The thermoplastic material and the reinforcing fibers can be mixed for an appropriate time and at an appropriate temperature to provide a substantially homogeneous aqueous dispersion of the fibers and thermoplastic material. For example, the materials may be mixed at room temperature, e.g., about 25 degrees Celsius, or above or below room temperature by heating or cooling the mixing tank. In some embodiments, as described later, the materials can be continuously added to the mixing tank 306 to continuously deposit the dispersion onto a moving support. The exact mixing time may vary depending on the materials used, but exemplary mixing times include 10 seconds to about 10 minutes, more specifically about 30 seconds to about 5 minutes. However, as described above, mixing is always occurring when the materials are continuously added to the mixing tank 306. The mixing tank 306 may include a paddle mixer, an impeller, or other devices to facilitate mixing.

[0035] In certain embodiments, referring to Figure 4A, the dispersion in the mixing tank 306 can be sprayed, dripped, or otherwise deposited onto the mobile support 410. Although the mobile support 410 is shown as a single segment in certain figures provided herein, the mobile support 410 can be divided into two or more individual segments as needed. The mixing tank 306 can be fluidly coupled to a plurality of spray heads 402 that can spray the dispersion onto the surface of the mobile support 410. As shown in Figure 4B, the mobile support 410 may be porous or may contain a mesh that can receive the dispersion. The exact deposition rate used may vary depending on the amount of material deposited per square meter. The mobile support 410 can be moved at a continuous and constant speed to allow continuous spraying of the dispersion along the upper surface of the mobile support 410. The area of ​​the mobile support 410 below the spray heads may be heated, cooled, or present at room temperature during the deposition of the dispersion. Different areas of the mobile support 410 may have different temperatures, as will be discussed later. The exact dimensions of the moving support 410 may vary, but typically the moving support is about 4 feet wide and can include a mesh or pore size of about 60 openings / square inch to about 80 openings / square inch. The moving support 410 allows for the receiving of dispersed material and the movement of the received dispersed material to additional locations or stations in the inline system. At the ends of the moving support 410, formed LWRT articles can be cut and stacked. The moving support 410 allows for the continuous formation of LWRT articles. In certain embodiments, the moving support 410 can be divided into two or more separate sections or segments. For example, a wet mat may be formed on the former belt and then, for example, manually or automatically, transferred to a separate dryer belt where it can pass through an oven or other drying device.

[0036] In certain embodiments, referring to Figure 5A, a mobile support 410 containing a dispersion of thermoplastic material and reinforcing fibers can be moved to a drying apparatus 510. The drying apparatus 510 can provide heat and / or negative pressure (vacuum) to remove water from the web 502 on the mobile support, leaving the reinforcing fibers and thermoplastic material on the mobile support 510. This process can form a highly porous core layer 512 (see Figure 5B) containing an open-cell structure formed from the reinforcing fibers held in place by the thermoplastic material. Other materials may also be present in the core layer or sprayed onto the core layer 512, as needed. For example, an adhesive from a reservoir can be sprayed onto the surface of the formed core layer 512. The exact temperature used to heat the web 502 and / or core layer 512 may vary, preferably higher than the melting point of the thermoplastic material and lower than the melting point of the reinforcing fibers. In some examples, the mobile support 410 itself can be heated, while in other examples, the drying apparatus 510 may include a heating element or be configured as an oven or other heating device. If necessary, both the drying apparatus 510 and the moving support 410 can supply heat to the web 502 on the moving support 410. In some cases, the moving support 410 may include a thermally conductive material that can retain heat from the drying apparatus 510 to help maintain the core layer 512 in a softened form during the application of the skin layer or other material. In some examples, a separate pressure apparatus 520 may be present (see Figure 5C). For example, a vacuum can be applied to the web 502 to remove water from the web, leaving the reinforcing material and thermoplastic material. The pressure apparatus 520 is typically located upstream of the drying apparatus 510 and is designed to remove at least 40% of the volume of water from the web 502, more specifically about 60% of the volume of water from the web 502. If necessary, another pressure apparatus (not shown) may be located downstream of the pressure apparatus 520.

[0037] In certain embodiments, when the core layer 512 exits the drying apparatus 510, one or more skin layers can be applied to the surface of the core layer in an automated manner. Referring to Figure 6A, a diagram is shown in which a skin layer 610 is applied to the core layer 512 as the core layer 512 exits the moving support 410. For example, the skin layer 610 may exist as a roll of skin layer material 605 that is unfolded and continuously applied to one surface of the core layer 512. As shown in Figure 6B, a second skin layer 620 can be applied to the second surface of the core layer 512 from a second roll 615 containing the second skin material. The skin layers 610, 620 can be applied at room temperature, even if the core layer 512 may still be heated, otherwise they are above room temperature on the moving support 410. Alternatively, the rolls 605, 615 or the skin layers 610, 620, or both, can be heated before being applied to the surface of the core layer 512. The skin layers 610 and 620 can generally be applied sequentially to form a thermoplastic composite article comprising a core layer 512, a first skin layer 610, and optionally a second skin layer 620. Although not shown, additional skin layers can be applied on top of the skin layers 610 and 620 using a similar process.

[0038] In some embodiments, it may be desirable to apply an adhesive layer on the core layer 512 before applying the skin layer 610 to the core layer 512. In such cases, an adhesive reservoir 720 (see Figure 7) is present and can be used to spray adhesive onto the surface of the core layer 512 before applying the skin layer 610, so that an adhesive layer 722 is present on the surface of the core layer 512. The exact adhesive used may differ from thermoplastic adhesives, thermosetting adhesives, or combinations thereof. Although not shown, adhesive may also be applied to the opposite surface of the core layer 512 before applying the skin layer 620 to the core layer 512. Exemplary adhesives include polyolefin adhesives, polyurethane adhesives, and combinations thereof.

[0039] In certain embodiments, the resulting thermoplastic composite article can be compacted by applying pressure to the surface of the composite article. For example, referring to Figure 8A, the composite article can be compressed by passing it between rollers 810, 812, thereby strengthening the bond between the skin layers 610, 620 and the core layer 512. The exact distance or gap between rollers 810, 812 may vary depending on the desired pressure applied and the desired final thickness of the composite article. Generally, the overall thickness of the composite article decreases after passing through rollers 810, 812. The rollers 810, 812 can operate at room temperature, above room temperature, or below room temperature. Multiple sets of rollers 810, 812 may be present as needed. For example, referring to Figure 8B, a second set of rollers 820, 822 is shown. The gaps between different sets of rollers may differ. For example, the first set of rollers 810, 812 may have a first gap smaller than the gap between rollers 820, 822. The gaps between the various rollers may be fixed or variable. For example, it may be desirable to compress certain areas of the composite article more strongly to reduce the thickness of these compressed areas. In some cases, the edges of the composite article may be compressed more so that the thickness at the side edges of the composite article is lower. Three, four or more roller sets may be present as needed. The rollers may be placed in an oven or heating device as needed to maintain the core layer in a softened state during the compaction of the composite article.

[0040] In certain embodiments, once the composite article is compacted, the continuous sheet of compacted composite article can be cut or shredded into individual sheets using a cutting device 910 (see Figure 9). The resulting individual composite articles can be stacked or palletized for shipment, for example, on a pallet 915, as shown in the stack 920. The dimensions of the composite articles in Figure 9 have been intentionally enlarged to show the stack, as the composite articles tend to be stacked as individual thin sheets having thicknesses of, for example, 1 mm to about 30 mm. The exact size of the individual composite articles can vary from about 2 feet to about 8 feet wide and from about 4 feet to about 16 feet long. In some embodiments, the individual composite articles may be about 4 feet wide and about 8 feet long, resulting in dimensions similar to plywood panels commonly used in recreational vehicles.

[0041] In certain configurations, core layers manufactured using an in-line process may include reinforcing fibers in combination with a thermoplastic resin. For example, a core layer can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic resin material. The core layer typically contains a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, porous core layers may have percentages of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, 20-60%, 20-70% This may include %, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges.

[0042] In certain embodiments, the thermoplastic material used to form the core layer described herein may include one or more polyolefins (e.g., polyethylene, polypropylene, etc.), polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and unplasticized, as well as blends of these materials with each other or other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic material used to form the core layer may be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein and, for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the core layer may vary, with exemplary amounts ranging from approximately 20% to approximately 80% by weight, for example, 30-70% or 35-65% by weight, based on the total weight of the core layer. Those skilled in the art will recognize that the total weight percentage of all materials used in the core layer can increase to 100% by weight.

[0043] In other embodiments, the reinforcing fibers of the core layer may include glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, such as para- and meta-aramid fibers, nylon fibers, polyester fibers, high melt flow index resins suitable for use as fibers (e.g., 100 g / 10 min MFI or higher), basalt, mineral wool (e.g., rock or slag wool), mineral fibers such as wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents or both. The fiber content in the core layer may independently be about 20% to about 90% of the weight of the core layer, more specifically about 30% to about 70% of the weight of the core layer. The specific size and / or orientation of the fibers used may depend, at least in part, on the desired properties of the thermoplastic material and / or core layer used. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally other additives to provide the core layer may generally have a diameter greater than about 5 microns, more specifically about 5 to about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0044] In certain embodiments, other additives may also be present in the mixture containing the thermoplastic resin and reinforcing fibers. For example, lofting agents, flame retardants, colorants, smoke suppressants, surfactants, foams, or other materials may be present. In some examples, the core layer may be substantially halogen-free or halogen-free to meet the limitations of hazardous substance requirements for a particular application. In other examples, the core layer may contain halogenated flame retardants, such as halogenated flame retardants containing one or more of F, Cl, Br, I, and At, or compounds containing such halogens, such as tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some cases, the thermoplastic material used for the core layer may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. If halogenated flame retardants are present, the flame retardant is preferably present in an amount that can vary depending on the other components present. For example, halogenated flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the core layer), more specifically, about 1% to about 13% by weight based on the weight of the core layer, for example, about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may also contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the core layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more core layers described herein.In certain cases, one or more core layers described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the core layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component), or they can be added after the layer has been formed. In some examples, the flame retardant material may contain one or more of the following: expandable graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0045] In certain embodiments, the skin layers 610 and 620 may be the same or different. For example, skin layer 610 may be a cosmetic layer or a patterned layer, and skin layer 620 may be a cosmetic layer, a patterned layer, or another type of skin layer. If one or both of skin layers 610 and 620 are patterned layers, the patterns may be the same or different in different regions of the skin layer. In some embodiments, the skin layer may include patterns that are one or more of the following: wood grain pattern (Figure 10A), marble pattern (Figure 10B), tile pattern (Figure 10C), random pattern (Figure 10D), pinwheel pattern (Figure 10E), herringbone pattern (Figure 10F), brick pattern (Figure 10G), offset alternating brick pattern (Figure 10H), offset pattern (Figure 10I), grid pattern (Figure 10J), laminated vertical pattern (Figure 10K), basket weave pattern (Figure 10L), diamond pattern (Figure 10M), chevron pattern (Figure 10N), or French pattern (Figure 10O). Other patterns are also possible. In some embodiments, the pattern may already be present on the skin layer material when it is on roll 605 or roll 615. In other examples, the pattern can be printed on the skin layer before applying the skin layer to the core layer. Diagrams of systems that include a printer for printing patterns on the skin layer are described in more detail below. If one of the skin layers 610, 620 is a patterned skin layer, the other skin layer may be, for example, a thermoplastic film, a polyolefin film, an elastomer film, etc. In a particular configuration, the film includes at least one of the following: polyolefin, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone.In other examples, the other skin layer may be, for example, a frim (film + scrim), a scrim (e.g., fiber-based scrim), foil, woven fabric, nonwoven fabric, or may exist as an inorganic coating, organic coating, or thermosetting coating. In other examples, the other skin layer may contain a limiting oxygen index greater than about 22, as measured according to ISO 4589 1996. If a fibrous scrim exists as (or as part of) another skin layer, the fibrous scrim may include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallated synthetic fibers, and metallated inorganic fibers. If necessary, the scrim may include materials or fibers manufactured from one or more of the thermoplastic materials described above in relation to the core layer. If a thermosetting coating exists as (or as part of) another skin layer, the coating may include at least one of unsaturated polyurethanes, vinyl esters, phenols, and epoxys. If an inorganic coating is present as (or as part of) another skin layer, the inorganic coating may contain minerals containing cations selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or it may contain at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as (or as part of) another skin layer, the nonwoven fabric may contain thermoplastic materials, thermosetting binders, inorganic fibers, metallic fibers, metallized inorganic fibers, and metallized synthetic fibers. If necessary, the other skin layer may also contain lofting agents, expandable graphite materials, flame retardants, fibers, etc.

[0046] In certain embodiments, the composite articles described herein may have desired surface properties on at least one surface. For example, the core layer of the article described herein may be rough due to the presence of reinforcing fibers. By adding a patterned layer to the core layer, the overall surface roughness can be reduced and / or the roughness of the core layer can be masked. Surface roughness can be measured in many ways, but three roughness parameters can be used as measures of surface roughness: the mean arithmetic deviation of the profile (Ra), the root mean square of the profile height (Rq), and the maximum height (Rt). Ra is the average distance from the profile to the mean line over the evaluation length, Rq is the mean root mean square of the profile height over the evaluation length, and Rt is the vertical distance between the highest and lowest points of the profile within the evaluation length. See, for example, L. Mummery (1990), Surface Texture Analysis: Handbook, Hommelwerke, p. 106. The results are shown in Table 2 below. Surface roughness can be measured using a stylus shape measuring device, generally conforming to JIS (JIS-B0601-2001, JIS-B0601-1994, JIS B0601-1982), VDA, ISO 4287:1997, and ANSI standards. The parameters (Ra, Rq, Rz, and Rt) can be characterized according to ISO 4287:1997.

[0047] In certain embodiments, the surface roughness (Ra) of at least one surface of a composite article, for example, a surface including a patterned layer, may be less than 10, 8, 8, 7, 6, 5, 4, or 3 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the surface roughness (Ra) of a surface of a thermoplastic composite article, including a patterned layer, is less than 2 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other examples, the mean RMS profile height (Rq) of at least one surface of a composite article, for example, a surface including a patterned layer, may be less than 12, 11, 10, 9, 8, 7, 6, or 5 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the average RMS profile height (Rq) of the surface of the thermoplastic composite article, including the patterned layer, is less than 4 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other examples, the maximum height (Rt) of at least one surface of the composite article, for example, the surface including the patterned layer, may be less than 80, 70, 60, 50, 40, 35, or 30 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997. In other embodiments, the maximum height (Rt) of the surface of the thermoplastic composite article, including the patterned layer, is less than 30 microns in the longitudinal and transverse directions, as measured by a stylus shape measuring device according to ISO 4287:1997.

[0048] In certain configurations, the system can be used to carry out an inline process. A diagram of the system components is shown in Figure 11A. System 1100 includes reservoirs 1102 and 1104. Reservoir 1102 can accept thermoplastic material, and reservoir 1104 can accept reinforcing fibers. Reservoirs 1102 and 1104 can supply material to a mixing tank 1106. The mixing tank 1106 can be fluidly coupled to a spray head or nozzle 1108 to spray the mixed dispersion onto a moving support 1110. The web 1115 on the moving support 1110 can move through a vacuum or other pressure device 1120 which can remove liquid from the web 1115 to form a core layer 1122. The core layer 1122 can pass through a drying device 1125 to dry and heat the core layer. Skin layers 1130 and 1140 can be applied, respectively, from a feeder or rolls 1135 and 1145 onto the opposite surface of the core layer 1122 to provide a composite article. The composite article can pass through a set of rollers 1160 and 1162 to compact it. The compacted composite article can be cut into individual articles by a cutting device 1170 as the moving sheet of compacted thermoplastic composite article passes through the cutting device 1170. For example, a processor 1180 is shown that can control the movement of the moving support 1110, the spraying of material onto the moving support 1110, and other devices and parameters used by the system 1100.

[0049] In certain examples, system 1100 may include other components that may be located before or after the cutting device 1170. For example, system 1100 may include another cutting station 1175 (Figure 11B) designed to cut a tongue into one edge of the composite article and a groove into the opposite edge of the composite article. This carving allows different individual panels to interlock with each other when in use, thus resulting in some overlap of panels at the joint. In other examples, system 1100 may include another heating device 1185 (Figure 11C) that can be used to loft or increase the thickness of the composite article. The heating device 1185 may be located before or after the cutting device 1170 as desired. An optional adhesive reservoir 1190 (Figure 11D) may be present to provide adhesive to the core layer before applying the skin layer 1130. A second adhesive reservoir (not shown) may also be present to provide adhesive to the core layer before applying the skin layer 1140.

[0050] In some embodiments, the system 1200 may include multiple sets of different rollers, including rollers 1160, 1162 and rollers 1212, 1214, as shown in Figure 12. Different rollers may exist at different temperatures or provide different gap thicknesses to compress the composite article before it exits the moving support. In some examples, rollers 1212, 1214 may be used to compress the edges of the composite article more highly, resulting in an overall thickness at the edges of the composite article being lower than in the central region of the composite article. The thicknesses at different edges may be the same or different.

[0051] In other embodiments, the system may include a printer 1310 that can print a pattern onto the skin layer before applying the skin layer to the core layer, as shown in Figure 13. A printer 1305 can spray, print, or deposit ink and other materials, such as fibers, particles, powders, etc., onto the surface of the skin layer before or after the skin layer has been applied to the core layer. The printer 1305 may be positioned near the roll 1335 to print a pattern onto the surface of the skin layer 1330 as it unfolds from the roll 1335. Although not shown, the printer may be positioned to apply the patterned layer to the skin layer 1340 after the patterned layer has been applied to the surface of the core layer 1122. The exact pattern provided by the printer may vary and may differ in different areas of the skin layer. For example, the pattern printed on the skin layer may be one or more of the following: wood grain pattern, marble pattern, tile pattern, random pattern, pinwheel pattern, herringbone pattern, brick pattern, offset alternating brick pattern, offset pattern, grid pattern, layered vertical pattern, French pattern, basket weave pattern, diamond pattern, or chevron pattern.

[0052] In certain embodiments, sidewalls can be manufactured using the in-line processes and in-line systems described herein. Sidewalls may be present in recreational vehicles or other vehicles, cubicles, office walls, residential walls, or other environments. An example of an RV wall 1400 is shown in Figure 14, which includes a first laminated lightweight reinforced thermoplastic composite article 1410 comprising a porous core layer 1412, a first skin layer 1414 on a first surface of the porous core layer 1412, and a patterned second skin layer 1416 on a second surface of the porous core layer. The patterned skin layer 1416 is typically positioned to face the interior of the space formed by the RV wall 1400. The RV wall 1400 may also include a foam layer 1420 bonded to the first laminated lightweight reinforced thermoplastic composite article 1410 at a first surface of the foam layer. For example, the foam layer 1420 can be bonded to the first laminated lightweight reinforced thermoplastic composite article 1410 via the first skin layer 1414 of the first laminated lightweight reinforced thermoplastic composite article 1410, such that a patterned second skin layer 1416 is present on the inner surface of the RV wall 1400. The RV wall 1400 also includes a support structure 1430, which can typically take the form of a chassis, tube, cage, or other structure. The support structure 1430 typically includes a metal or multiple metals, such as steel or aluminum. The support structure 1430 can be bonded to a second surface of the foam layer 1420 at a first surface of the support structure 1430. The second laminated lightweight reinforced thermoplastic composite article 1440 can be bonded to a second surface of the support structure 1430. The second laminated lightweight reinforced thermoplastic composite article 1440 includes a porous core layer 1442, a first skin layer 1444 on a first surface of the porous core layer 1442, and a second skin layer 1446 on a second surface of the porous core layer 1442. To form an RV wall 1400, an exterior panel 1450 can be bonded to the second laminated lightweight reinforced thermoplastic composite article 1440. In some examples, the exterior panel 1450 contains glass fiber or aluminum.

[0053] As described herein, the patterned second skin layer 1416 may include a pattern that is one or more of the following: wood grain pattern, marble pattern, tile pattern, random pattern, pinwheel pattern, herringbone pattern, brick pattern, offset alternating brick pattern, offset pattern, lattice pattern, laminated vertical pattern, French pattern, basket weave pattern, diamond pattern, or chevron pattern. In certain embodiments, the first skin layer 1414 of the first laminated lightweight reinforced thermoplastic composite article 1410 includes a scrim. In certain examples, the porous core layer 1412 of the first laminated lightweight reinforced thermoplastic composite article 1410 may include a web that includes an open-cell structure formed from reinforcing fibers held together by the thermoplastic material as described above. In some examples, the porous core layer 1442 of the second laminated lightweight reinforced thermoplastic composite article includes a web that includes an open-cell structure formed from reinforcing fibers held together by the thermoplastic material. In some configurations, the thermoplastic material of each porous core layer 1410, 1440 independently comprises a thermoplastic material as described herein, for example, a polyolefin such as polypropylene or polyethylene. In some embodiments, the reinforcing material of each porous core layer comprises a reinforcing fiber as described herein, for example, glass fiber.

[0054] In certain embodiments, the RV wall may be located within a recreation vehicle, including a roof, side walls coupled to the roof, and a floor coupled to the side walls to provide interior space within the recreation vehicle, one example of which is shown in Figure 15, where RV 1500 includes an RV wall 1510, which may be similar to the RV wall 1400 described above. RV 1500 also includes a roof 1512, another side wall 1514, and a floor 1516. RV 1500 may include wheels 1552, 1554 to enable the towing of the RV, and / or an engine, electric motor or other power source to enable the independent movement of the RV.

[0055] In certain examples, the inline methods and inline systems described herein may be controlled using one or more processors, which may be part of the inline system, or otherwise electrically coupled to the inline system via relevant devices, such as a computer, laptop, or mobile device. For example, a processor can be used to control the mixing rate of materials, the speed of a moving support, the pressure used to remove liquid from a placed dispersion, the temperature of a heating device, the pressure applied to the material, and other parameters of the process and system. Such processes may be performed automatically by the processor without requiring user intervention, or the user may input parameters via a user interface. In certain configurations, the processor may reside in one or more computer systems and / or common hardware circuits, including, for example, a microprocessor and / or appropriate software for operating the system, to control various fluid reservoirs, mixing tanks, pressure devices, temperatures, etc. The processor may be integrated with the inline system, or it may reside on one or more accessory boards, printed circuit boards, or computers electrically coupled to components of the inline system. Typically, the processor is electrically coupled to one or more memory units to receive data from other components of the system and to allow adjustment of various system parameters as needed or desired.The processor may be part of a general-purpose computer, including processors designed by Apple, such as Unix®, Intel PENTIUM® processors, Intel Core® processors, Intel Xeon® processors, AMD Ryzen® processors, AMD Athlon® processors, AMD FX® processors, Motorola PowerPC, Sun UltraSPARC, Hewlett-Packard PA-RISC processors, Apple A14 Bionic processors, A13 Bionic processors, A12 processors, Apple A11 processors, etc., or based on any other type of processor. According to various embodiments of this technology, one or more of any type of computer system may be used. Furthermore, the system may be connected to a single computer or distributed across multiple computers connected by a communication network. If necessary, different components of the inline system may be controlled by separate processors or computers, distinct from the processors or computers used to control the other components of the inline system. Other functions, including network communication, may be performed, and it should be understood that this technology is not limited to having any particular function or set of functions. Various embodiments may be implemented as dedicated software running on a general-purpose computer system. A computer system may include a processor connected to one or more memory devices, such as disk drives, memory, or other devices for storing data. Memory is typically used to store programs, temperatures, moving support speeds, and other values ​​used in inline processes. Components of a computer system may be connected by interconnectors, which may include one or more buses (e.g., between components integrated within the same machine) and / or networks (e.g., between components residing in separate individual machines). Interconnectors provide communication (e.g., signals, data, instructions) exchanged between components of the system.A computer system is typically capable of receiving and / or issuing commands within processing times of, for example, milliseconds or less, to enable rapid control of the system. The processor is typically electrically coupled to a power source, which can be, for example, a DC source, an AC source, a battery, a solar cell, a fuel cell, or other power sources, or a combination of power sources. The power source may be shared by other components of the system. The system may also include one or more input devices, such as a keyboard, mouse, trackball, microphone, touchscreen, manual switch (e.g., override switch), and one or more output devices, such as a printing device, display screen, or speaker. Furthermore, the system may include one or more communication interfaces that connect the computer system to a communication network (in addition to or as a substitute for an interconnector). The system may also include appropriate circuits for converting signals received from various electrical devices present within the system. Such circuits may reside on a printed circuit board, or on a separate board or device electrically coupled to the printed circuit board via a suitable interface, such as a Serial ATA interface, ISA interface, PCI interface, USB interface, Fibre Channel interface, Firewire interface, M.2 connector interface, PCIe interface, mSATA interface, etc., or via one or more wireless interfaces, such as Bluetooth, Wi-Fi, near-field communication, or other wireless protocols and / or interfaces.

[0056] In certain embodiments, the storage system used in the systems described herein typically includes a computer-readable and writable non-volatile recording medium that can store software code that can be used by programs executed by the processor, or information to be processed by programs stored on or within the medium. The medium may be, for example, a hard disk, a solid-state drive, or flash memory. Programs or instructions executed by the processor may be located locally or remotely and may be retrieved by the processor by interconnection mechanisms, communication networks, or other means as desired. Typically, during operation, the processor loads data from the non-volatile recording medium into another memory that allows the processor to access the information faster than the medium. This memory is typically a volatile random-access memory, such as dynamic random-access memory (DRAM) or static memory (SRAM). This may be located within the storage system or memory system. The processor generally manipulates data in integrated circuit memory and then copies the data to the medium after processing is complete. Various mechanisms for managing data movement between the medium and integrated circuit memory elements are known and are not limited to these. The technology is also not limited to a particular memory system or storage system. In certain embodiments, the system may also include specially programmed, dedicated hardware such as application-specific integrated circuits (ASICs), microprocessor units (MPUs), or field-programmable gate arrays (FPGAs), or combinations thereof. Embodiments of this technology can be implemented in software, hardware, or firmware, or any combination thereof. Furthermore, such methods, operations, systems, system elements, and their components may be implemented as part of the systems described above, or as independent components. While a particular system is described as an example of one type of system capable of implementing various embodiments of this technology, it should be understood that embodiments are not limited to being implemented on the described system.Various embodiments can be implemented on one or more systems having different architectures or components. A system may comprise a general-purpose computer system programmable using a high-level computer programming language. The system may also be implemented using specially programmed, dedicated hardware. In the system, the processor is typically a commercially available processor, such as a well-known microprocessor available from Intel, AMD, Apple, etc. Many other processors are also commercially available. Such processors typically run an operating system that may be, for example, Windows 7, Windows 8, or Windows 10 operating systems available from Microsoft, MAC OS® X such as Snow Leopard, Lion, Mountain Lion, Mojave, High Sierra, or El Capitan, or other versions available from Apple, the Solaris operating system available from Sun Microsystems, or UNIX or Linux® operating systems available from various sources. Many other operating systems may be used, and in certain embodiments, a simple set of commands or instructions may function as the operating system.

[0057] In certain examples, the processor and operating system together may define a platform on which application programs in a high-level programming language can be written. It should be understood that this technology is not limited to a specific system platform, processor, operating system, or network. Furthermore, given the merits of this disclosure, it will be apparent to those skilled in the art that this technology is not limited to a specific programming language or computer system. It should also be understood that other suitable programming languages ​​and other suitable systems may be used. In certain examples, the hardware or software may be configured to implement a cognitive architecture, a neural network, or other suitable implementation. If desired, one or more parts of a computer system may be distributed across one or more computer systems coupled to a communication network. These computer systems may also be general-purpose computer systems. For example, various embodiments may be distributed across one or more computer systems configured to provide services (e.g., servers) to one or more client computers, or to perform an entire task as part of a distributed system. For example, various embodiments may run on a client-server or multi-tier system including components distributed across one or more server systems performing various functions according to various embodiments. These components may be executable code, intermediate code (e.g., IL), or interpreted code (e.g., Java) that communicates over a communication network (e.g., the Internet) using a communication protocol (e.g., TCP / IP). It should also be understood that this technology is not limited to running on any particular system or group of systems. Furthermore, it should be understood that this technology is not limited to any particular distributed architecture, network, or communication protocol.

[0058] In some cases, various embodiments can be programmed using object-oriented programming languages ​​such as SQL, SmallTalk, Basic, Java, Javascript, PHP, C++, Ada, Python, iOS / Swift, Ruby on Rails, or C# (C-Sharp). Other object-oriented programming languages ​​may also be used. Alternatively, functions, scripts, and / or logic programming languages ​​may be used. Various configurations can be implemented in an unprogrammed environment (e.g., a document created in HTML, XML, or another format that renders a graphical user interface (GUI) or performs other functions when displayed in a browser program window). A particular configuration may be implemented as programmed or unprogrammed elements, or any combination thereof. In some examples, the system may have a remote interface, such as one residing on a mobile device, tablet, laptop computer, or other portable device, which can communicate via a wired or wireless interface and, if desired, allows for remote control of the inline system.

[0059] In certain examples, the processor may also have, or be able to access, a database of information about specific items to be manufactured. For example, specific parameters used to manufacture a core layer of a desired thickness and composition can be retrieved from the database and used by the inline system. Instructions stored in memory can execute software modules or control routines for the system, and in practice, can provide a controllable model of the inline system. The processor can use information accessed from the database, along with one or more software modules running within the processor, to determine control parameters or values ​​for different components of the system, such as different temperatures, different pressures, different consolidation devices, etc. Using input interfaces for receiving control instructions and output interfaces linked to different system components within the system, the processor can perform active control over the system.

[0060] Specific examples of LWRT articles manufactured and tested using an in-line process are described below. [Examples]

[0061] Example 1

[0062] LWRT articles were prepared by adding chopped glass fibers (e.g., 30-70% by weight) to a polypropylene (PP) resin matrix as a reinforcing material in the in-line process described herein to form a web or core. First skin (23 gsm or g / m²) 2 A nonwoven scrim with a basis weight of 105 g / m² is added to one surface of the core, and a second skin (with a marble or wood grain pattern) is applied. 2 The LWRT article was formed by adding the skin to the opposite surface using an inline process along with inline calendaring, and then pressing the skin onto the core. [Examples]

[0063] Example 2

[0064] Various physical and analytical tests were performed on a 99 mm diameter disc cut from the LWRT article of Example 1. The surface density (g / m²) of the laminated decorative panel was also measured. 2 Alternatively, gsm (5-unit grid), ash content (%), density (g / cm³). 3 The thickness (mm, 5-strand) and the as-manufactured thickness (mm, 5-strand) were measured. The results are shown in Table 1 below. Table 1. Physical properties of inline laminated LWRT composite decorative panels. TIFF2023550718000002.tif32151

[0065] The PP / glass LWRT composite substrate has a porous structure with a high void content, resulting in a remarkably low density. The densities for the two samples were 0.35 and 0.36 g / cm³, respectively. 3 These LWRT composites are approximately 50% lighter than regular plywood and comparable to modified plywood. The surface density and ash content of the two finished LWRT / decor samples are very close, with standard deviations within ±5% of the mean, indicating that these in-line laminated decorative composite panels are very uniform. The thickness of these in-line laminated decorative panels meets the 2.9 ± 0.2 mm flatness requirement for these decorative panels used in the interior layers of RV sidewalls. Photographs of wood grain (Figure 16A) and marble pattern (Figure 16B) are shown. [Examples]

[0066] Example 3

[0067] LWRT test specimens measuring 75 mm × 75 mm were cut from the LWRT article of Example 1 by an in-line lamination process from LWRT boards without a surface skin and LWRT boards laminated with decor (wood grain and marble). The surface roughness of 10 samples was measured. A stylus shape measuring device (Mitutoyo Surftest SJ-210) was used to perform one measurement on each surface roughness test specimen along the longitudinal (MD) and transverse-longitudinal (CD) directions. The trace speed, stylus tip diameter, and tip angle were 10 mm / min, 4 mm, and 90 degrees, respectively. Three roughness parameters were recorded: the mean arithmetic deviation of the profile (Ra), the root mean square of the profile height (Rq), and the maximum height (Rt). Ra is the average distance from the profile to the mean line over the evaluation length, Rq is the root mean square of the profile height over the evaluation length, and Rt is the vertical distance between the highest and lowest points of the profile within the evaluation length. For example, see L. Mummery (1990), Surface Texture Analysis: Handbook, Hommelwerke, p. 106. The results are shown in Table 2 below. Table 2 Surface roughness parameters of inline laminated decorative panels. TIFF2023550718000003.tif43151

[0068] The exposed surface of the PP / glass LWRT composite has Ra, Rq, and Rt values ​​of 13.6, 16.9, and 100.0 microns in the longitudinal (MD) direction and 18.4, 22.6, and 139 microns in the transverse (CD) direction. The surface roughness is higher in the CD direction than in the MD direction, indicating better alignment of glass fibers in the longitudinal direction than in the transverse direction during the in-line lamination process. In both the MD and CD directions, the Ra, Rq, and Rt values ​​of both decorative patterns are significantly lower than those of the exposed PP / glass LWRT surface, further indicating that laminating these types of decors onto the LWRT composite substrate can cover the porous structure of the LWRT core board, thereby efficiently improving surface smoothness and appearance. For example, Ra significantly decreases to 1.4 microns in both the MD and CD directions from the exposed surface of the PP / glass LWRT to the surface of the wood grain pattern decor panel, which is lower than the surface roughness (Ra) of plywood. These results are consistent with the decorative layer, particularly the wood grain pattern, and are thick enough to adequately cover the core texture of the LWRT composite. [Examples]

[0069] Example 4

[0070] Two laminated decorative samples with woodgrain or marble patterns were subjected to 180-degree peel tests on the decor and scrim surfaces using an MTS tester equipped with a 250N load cell according to ASTM standard D 903-2004. Ten rectangular (25mm × 100mm) test specimens were cut from the manufacturing sheet in the MD and CD directions. The crosshead speed, span, anvil diameter, and nose diameter were 15mm / min, 64mm, 6.4mm, and 6.4mm, respectively. The results are shown in Table 3. Table 3. Adhesion strength between decor or scrim and LWRT composite core substrate. TIFF2023550718000004.tif40151 Neither the decor nor the scrim could be separated from the composite core substrate, and under ambient conditions, they showed good interfacial bonding between the skin material and the PP / glass LWRT core substrate. [Examples]

[0071] Example 5

[0072] Flat tensile (FWT) tests were performed on two samples (Woodgrain and Marble) of as-manufactured decorative panels using an MTS mechanical testing machine according to ASTM C297-04. Ten test specimens (51 mm × 51 mm) were cut from the manufactured panel in the CD direction. The crosshead speed was 50 mm / min and the load cell was 5 kN. Each test specimen was applied to the tensile jig / end tabs (top and bottom) with urethane adhesive (3M Scotch-Weld 3535, base-to-accelerator weight ratio 100:105, density approximately 1.29 g / cm³). 3 The samples were bonded together and left in the air for 24 hours to allow the adhesive to fully cure. Flat tensile strength (FWT) is a desirable criterion for flat panels used in RV sidewall applications. The results are shown in Figure 17A (wood grain veneer skin) and Figure 17B (marble veneer skin).

[0073] Photographs of the tested specimens show that almost all specimens failed either on the surface of the decor at the interface between the decor and the test fixture, or due to adhesive failure. The mean peak loading values ​​for the Woodgrain and Marble samples were 1545 and 1172 N, respectively, which are significantly higher than the majority of FWT peak loading values ​​for EPS foam reported in the literature (less than 700 N), and EPS foam is one of the most commonly used insulating foams in RV sidewall structures. These results are consistent with the fact that as-manufactured decorative panels are much stronger in the z direction compared to EPS foam, reducing the likelihood that finished RV sidewall panels will not delaminate within the decorative panels. [Examples]

[0074] Example 6

[0075] Bending (three-point bending) tests were performed on as-manufactured laminated panels (Woodgrain and Marble) according to ASTM D790-2007. Ten rectangular specimens (25 mm × 100 mm) were cut from the panels in both MD and CD directions. The tests were performed using an MTS mechanical testing machine with a 250 N load cell, with the scrim or decor surface of the sample facing the load. The crosshead speed, span, anvil diameter, and nose diameter were set to 15 mm / min, 64 mm, 6.4 mm, and 6.4 mm, respectively. The significance of bending strength and modulus was statistically analyzed using one-way analysis of variance (ANOVA) with software R version Ri386-3.5.0 (The R Foundation, https: / / www.r-project.org / ) at an α level of 0.05 using Tukey's test. The results are shown in Figure 18A (peak load) and Figure 18B (modulus).

[0076] When bending strength (peak load) with the scrim surface facing the load (or upward) during the bending test, the wood grain sample exhibits significantly higher strength (20% higher) than the MD marble sample. With the decor or scrim surface facing upward, the stiffness of the wood grain sample exhibits significantly higher values ​​than the MD marble sample. For example, the gradient values ​​of the wood grain sample are 26% and 40% higher than the marble sample when the scrim and decor surfaces are facing upward, respectively, during the test. The overall trend for both samples is that MD has better bending strength and stiffness than CD, which is also due to the better glass orientation in MD than in CD. Furthermore, in both MD and CD of both samples, the decor surface facing upward during the test can exhibit higher strength and stiffness than the scrim surface facing upward. This suggests that laminating a decor skin layer on top of an LWRT composite improves the overall strength and stiffness of the resulting decorative panel compared to LWRT with both sides as scrim, as used in RV sidewall structures. [Examples]

[0077] Example 7

[0078] Flammability performance was evaluated according to two standards: the Federal Motor Vehicle Safety Standard (FMVSS 302-03) and ASTM E84. While FMVSS 302 is more commonly accepted for automotive interior applications, performance tested by the ASTM E84 method provides more insight into the performance expected by the building and construction industries, including the RV industry. Test specimens were cut to 304.8 mm × 25.4 mm and tested horizontally based on FMVSS 302. For the ASTM E84 test, both samples (Woodgrain and Marble) were cut to 0.61 m × 1.83 m to classify the material as Class A, B, or C, and evaluated for the Flame Propagation Index (FSI) and Smoke Emission Index (SDI). The results are shown in Table 4. Table 4. Combustion performance of the two decorative panels. TIFF2023550718000005.tif29151 From the FMVSS 302 test, the woodgrain sample burned 30% slower than the marble sample. The woodgrain sample had a flame propagation index (FSI) of 25, meeting Class A performance (FSI ≤ 25), and a smoke emission index (SDI) of 50, significantly lower than the requirements for Class A, B, or C (SDI ≤ 450). In contrast, the marble sample had an FSI of 125 and an SDI of 30, meeting Class C requirements. The only difference between these two samples was the decorative pattern of the decorative material. Therefore, the better FR performance of the woodgrain sample may be due to the difference between the marble-like pattern and the wood-grain pattern. However, the marble sample already meets the FR requirements for single-component RV sidewalls of ASTM E84 Class C. [Examples]

[0079] Example 8

[0080] For the article of Example 1 and the Luan / NPP decorative panel, according to the ASTM E1050-98 standard, the sound absorption characteristics and sound absorption coefficient were determined using the two-microphone transfer function method. A Luan plywood panel was laminated using decorative paper with an NPP pattern by a secondary lamination process. The frequency range for the evaluation was from 100 to 6500 Hz. All samples were tested with the decorative surface or the scrim surface (the exposed Luan surface of the Luan / NPP panel) facing the sound source. The results are shown in Fig. 19A (the decorative surface facing the sound source) and Fig. 19B (the scrim surface facing the sound source).

[0081] Different test samples containing the following compositions: ST-13792 included a LWRT core layer having a basis weight of 1200 g / m 2 , a thickness of 3.6 mm, 45 wt% polypropylene and 55 wt% glass fiber. ST-13793 included a LWRT core layer having a basis weight of 1670 g / m 2 , a thickness of 4.7 mm, 50 wt% polypropylene and 50 wt% glass fiber. All other test samples had a LWRT core layer having a basis weight of 960 g / m 2 , a thickness of 2.7 mm, 45 wt% polypropylene and 55 wt% glass fiber. The overall dimensions of each sheet sample produced were approximately 1219 mm in width × 2438 mm in length (about 4 feet × 8 feet). Sample ST-13378 included a marble-patterned layer on the outer surface. Samples ST-13794 and ST-13882 included a fabric-patterned layer on the outer surface. The remaining samples included a wood-grain-patterned layer on the outer surface.

[0082] The evaluation of the acoustic properties of the materials was based on the sound absorption coefficient α. This parameter is the ratio of the absorbed sound intensity to the incident sound intensity on the surface. When the α value is close to 1 and there is an absorption plateau at this value over a wide frequency range, this material can be considered to have good sound absorption characteristics. The sound absorption ability of LWRT articles can be affected by various factors such as the surface density, density, thickness, and filler (type and content).

[0083] Across the entire frequency range (100-6500Hz), the sound absorption coefficient of the test samples was significantly higher than that of the Luang / NPP decorative panel, regardless of which surface faced the sound source. When the decorative paper surface faced the sound source, the coefficient varied from 0.1 to 0.5, compared to approximately 0.1-0.2 for the Luang / NPP panel. When the scrim surface faced the sound source, the coefficient values ​​varied from 0.1 to 0.9 for the RVX 3.6 core (ST-13792) and RVZ 4.7 core (ST-13793) based samples. The RVX 2.7 core based sample showed a coefficient in the range of 0.1 to 0.7, while the Luang / NPP sample only had values ​​in the range of 0.1-0.2. LWRT panels can significantly reduce sound / noise reflection compared to Luang / NPP panels. Thicker substrates can improve sound absorption performance.

[0084] When introducing elements of the examples disclosed herein, the articles “a,” “an,” “the,” and “said” are intended to mean that there are one or more elements. The terms “comprising,” “including,” and “having” are intended to be open-ended, meaning that additional elements other than those enumerated may exist. In light of the merits of this disclosure, it will be recognized by those skilled in the art that various components of the examples can be interchanged or substituted with various components of other examples.

[0085] While specific aspects, configurations, examples, and embodiments have been described above, those skilled in the art will recognize that, in consideration of the interests of this disclosure, additions, substitutions, modifications, and changes are possible to the disclosed exemplary aspects, configurations, examples, and embodiments.

Claims

1. 1. An in-line process for manufacturing a thermoplastic composite article using an in-line system, comprising: mixing a reinforcing material and a thermoplastic material in an aqueous solution; placing the aqueous solution of the reinforcing material and the thermoplastic material on a moving support; removing water from the aqueous solution disposed on the moving support to form a web including an open cell structure formed from the reinforcing material and the thermoplastic material; drying the web on the moving support to provide a porous core layer; heating the dried porous core layer on the moving support to melt the thermoplastic material of the heated porous core layer; disposing a first skin layer on a first surface of the heated porous core layer on the moving support; disposing a second skin layer on a second surface of the heated porous core layer on the moving support; and applying pressure to the heated porous core layer including the disposed first skin layer and the disposed second skin layer on the moving support to provide a thermoplastic composite article.

2. The in-line process of claim 1 , wherein the porous core layer is heated at a first temperature above the melting point of the thermoplastic material and below the melting point of the reinforcing material.

3. 10. The in-line process of claim 1, further comprising adding a foam to the aqueous solution in which the reinforcing material and the thermoplastic material are mixed.

4. 10. The in-line process of claim 1, further comprising adding a lofting agent to the aqueous solution in which the reinforcing material and the thermoplastic material are mixed.

5. The in-line process of claim 1 further comprising configuring the first skin layer as a scrim.

6. The in-line process of claim 5 further comprising configuring the second skin layer as a patterned layer.

7. 7. The in-line process of claim 6, wherein the pattern of the patterned layer is one or more of a wood grain pattern, a marble pattern, a tile pattern, a random pattern, a pinwheel pattern, a herringbone pattern, a brick pattern, an offset staggered brick pattern, an offset pattern, a lattice pattern, a stacked vertical pattern, a French pattern, a basket weave pattern, a diamond pattern, or a chevron pattern.

8. 8. The in-line process of claim 7, wherein the thermoplastic material comprises a polyolefin and the reinforcing material comprises inorganic fibers.

9. The surface roughness (R a 2. The in-line process of claim 1, wherein the thickness of the coating is less than 3 microns in the longitudinal and transverse directions as measured by a stylus profilometer in accordance with ISO 4287:1997.

10. The surface roughness (R a 2. The in-line process of claim 1, wherein the thickness of the coating is less than 2 microns in the longitudinal and transverse directions as measured by a stylus profilometer in accordance with ISO 4287:1997.

11. 10. The in-line process of claim 1, wherein the first skin layer is disposed on the heated porous core layer without the use of an adhesive between the first skin layer and the heated porous core layer.

12. 10. The in-line process of claim 1, further comprising disposing an adhesive on the second surface of the heated porous core layer prior to disposing the second skin layer on the second surface.

13. The in-line process of claim 12 , wherein the adhesive comprises a polyolefin or a polyurethane.

14. The in-line process of claim 1 further comprising cutting a groove in a first end of the thermoplastic composite panel.

15. 15. The in-line process of claim 14, further comprising cutting a tongue into a second end of the thermoplastic composite panel.

16. 10. The in-line process of claim 1, further comprising consolidating the heated porous core layer prior to disposing the first skin layer on the first surface and prior to disposing the second skin layer on the second surface.

17. 10. The in-line process of claim 1, further comprising heating the thermoplastic composite article after consolidating the thermoplastic composite article to increase an overall thickness of the thermoplastic composite article.

18. 10. The in-line process of claim 1, further comprising printing a pattern on the second skin layer prior to disposing the second skin layer on the second surface of the heated porous core layer.

19. 10. The in-line process of claim 1, further comprising printing a pattern on the second skin layer after disposing the second skin layer on the second surface of the heated porous core layer.

20. 2. The in-line process of claim 1, further comprising compressing side edges of the heated porous core layer, the compressed side edges of the heated porous core layer having a thickness less than a thickness of a central region of the heated porous core layer.