Method for preparing a catalyst comprising at least one metal of group VIB, at least one metal of group VIIIB and a support based on oxide(s)
Patent Information
- Application Number
- JP2023535801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-15
- Filing Date
- 2021-12-02
- Publication Date
- 2024-12-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for recycling metals from used hydroprocessing catalysts are complex and inefficient, requiring numerous operations and not suitable for industrial-scale implementation, leading to reduced catalyst activity and increased environmental impact.
A method involving the use of an extraction solution with a common solvent for both extraction and impregnation steps, utilizing organic compounds with complexing and acidic properties to dissolve metals from spent catalysts, followed by impregnation onto a support, without intermediate solid-phase treatments, to produce new catalysts.
This method simplifies the recycling process, allowing for high metal recovery and production of catalysts with performance comparable to fresh catalysts, reducing operational complexity and environmental footprint.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to the production of catalysts comprising at least one metal from Group VIB, at least one metal from Group VIIIB, and a support based on metal and / or silicon oxides. These catalysts are intended, among other things, to be used in units for the hydrogenation or hydrogenation of hydrocarbons. [Background technology]
[0002] The term "hydrogenation" refers to all purification methods that enable the removal of various impurities contained in hydrocarbon feedstock through the action of hydrogen. Hydrogenation methods make it possible to remove impurities present in the feedstock, such as nitrogen (referred to as hydrodenitrification), sulfur (referred to as hydrodesulfurization), oxygen (referred to as hydrodeoxygenation), and compounds containing metals that can inhibit the action of catalysts and cause problems in downstream operations (referred to as hydrodemetallation), through the action of hydrogen. Hydrogenation thus makes it possible to make petroleum products, such as hydrocarbons, meet the specifications required for a given application (automotive fuel, gasoline or diesel fuel, household fuel oil, etc.) (sulfur content, aromatic compound content, etc.). Automotive standards, in particular, impose very strict reductions in sulfur in diesel and gasoline fuels, and hydrogenation thus makes it possible to make these products meet the required specifications.
[0003] Hydrogenation thus improves the quality of hydrocarbons by reducing the content of certain compounds and elements considered to be impurities. This also makes it possible to reduce the content of aromatic hydrocarbons and, consequently, improve the cetane number of hydrocarbons. Small amounts of fuel gas and light fractions, such as LPG (Liquefied Petroleum Gas) and naphtha, can also be produced during the hydrogenation process.
[0004] The hydrocarbon feedstock targeted by this type of processing includes, among other things, hydrocarbons (sometimes as mixtures) derived from coal or natural gas, or hydrocarbon fractions derived from biomass. They may also be heavy synthetic fractions or petroleum fractions, such as kerosene, gas oil, or distillates resulting from atmospheric and vacuum distillation, which can produce upgraded kerosene, gas oil, or vacuum distillates. These are placed in storage units (pools) that accept the same type of product, or sent to downstream units, such as catalytic cracking units, where the feedstock is "cracked" to produce hydrocarbons with shorter chains. Often, the hydrogenation method is actually a preliminary step to processing the feedstock by a hydrogenation / hydrocracking type method.
[0005] It is worth noting that the hydrocracking of heavy petroleum fractions (also referred to under the term hydroconversion) is a key refining method that enables the production of lighter fractions, such as gasoline, jet fuel, and light gas oil, from surplus and slightly upgradeable heavy feedstock, which refineries desire to adapt to the production of fractions in demand. Several hydrocracking methods also make it possible to obtain highly refined residues that can constitute an excellent base for oil.
[0006] The feedstocks used in the hydrogenation process are, more specifically, gasoline, gas oil, vacuum gas oil, atmospheric residue, vacuum residue, atmospheric distillates, vacuum distillates, heavy fuel oil, waxes and paraffins, spent oil, de-asphalt residue or crude oil, feedstocks resulting from thermal or contact conversion methods, lignocellulosic feedstocks, or, more generally, feedstocks resulting from biomass, such as vegetable oils, which are used individually or in mixtures. The feedstocks to be processed, particularly the feedstocks mentioned above, generally contain heteroatoms, such as sulfur, oxygen and nitrogen, and in the case of heavy feedstocks, they usually also contain metals.
[0007] For example, Patent Document 1 may be mentioned, which describes a hydrotreatment and hydroconversion facility, with general fractionation, and is intended for the production of at least one of the following products: (light and / or heavy) naphtha, diesel, kerosene, distillates and residues.
[0008] Similarly, Patent Document 2 may be mentioned, which describes a method having at least one hydrogenation step, encompassing various alternative forms. These include hydrogenation, hydrocracking, hydrogenation and subsequent hydrocracking without separation between hydrogenation and hydrocracking (also called single-step hydrocracking), hydrogenation and subsequent hydrocracking with intermediate separation, or hydrogenation and subsequent treatment of the unconverted fraction by a first hydrocracking, separation of products and another hydrocracking (also called two-step hydrocracking). This patent recommends recycling a portion of the hydrogenated or hydrocracking effluent, along with nitrogenous feedstock, back into the hydrogenation or hydrocracking step after stripping with hydrogen or other inert gas.
[0009] Similarly, Patent Document 3 may be mentioned, which describes the hydrogenation of two hydrocarbon fractions, each containing a sulfur and nitrogen compound, using different or the same catalyst for each fraction, and recycling the recovered hydrogen into two hydrogenated effluents to hydrogenate one of the two fractions.
[0010] Conventional hydrogenation catalysts generally comprise an oxide support and an active phase based on metals from Group VIB and Group VIII, and also phosphorus, in oxide form. The preparation of these catalysts typically involves impregnation of the support with metal and phosphorus, followed by drying and calcination steps, which allow for the acquisition of the active phase in oxide form. Prior to their use in hydrogenation and / or hydrocracking reactions, these catalysts are generally subjected to sulfidation as well.
[0011] It is known that the activity of hydrogenation catalysts can be improved by adding organic additives, and this is especially true for catalysts prepared by impregnation and subsequent drying (without subsequent calcination). These catalysts are often referred to as "additive-impregnated dried catalysts."
[0012] The catalysts used in hydrocracking are of the dual-function type, that is, they combine an acidic functional group with a hydrogenation functional group. The acidic functional group has a high specific surface area (generally 150-800 m²). 2 ·g -1 Supports having high acidity, such as halogenated (particularly chlorinated or fluorinated) alumina, combinations of boron and aluminum oxides, amorphous silica-alumina, and zeolites. The hydrogenation functional group is given by one or more metals from Group VIII of the periodic table, or a combination of at least one metal from Group VIB and at least one metal from Group VIII of the periodic table, used in the presence of sulfur. The balance between these two, the acidic functional group and the hydrogenation functional group, determines the activity and selectivity of the catalyst.
[0013] During the operation of hydrogenation and / or hydrocracking methods, the catalyst is deactivated by the accumulation of coke and / or sulfur-based compounds or compounds containing other heteroatoms on its surface. After a certain period, it is therefore necessary to replace it.
[0014] To overcome these disadvantages, the regeneration (also known as gentle calcination) of hydrogenation catalysts is an advantageous method from an economic and environmental perspective. This is because it allows these catalysts to be reused in industrial units, rather than being buried in landfills or recycled (metal recovery). Regeneration generally consists of heat treatment at 350°C to 550°C in the presence of high-purity or diluted oxygen, with the aim of removing at least some of the coke present on the spent catalyst by combustion. This regeneration allows the catalyst, called the "regenerated" catalyst, to regain its hydrogenosulfurization activity. However, regenerated catalysts are generally less active than the starting catalyst, also called the "fresh" catalyst. As a result, their cycle time in hydrogenation units is reduced compared to that of fresh catalysts. In some cases, they can be reused in applications with lower demand.
[0015] To overcome the shortcomings in the hydrogenosulfurization activity of regenerated catalysts, an additional treatment called "rejuvenation" can be applied. Rejuvenation methods consist of re-impregnating the already regenerated catalyst with a solution containing organic or inorganic additives and / or metal precursors. These "rejuvenation" methods are well known, particularly in the field of intermediate distillates. While more effective than simple regeneration, catalyst rejuvenation often results in catalysts with lower activity than fresh catalysts. Finally, some spent catalysts cannot be reused even after regeneration or reactivation, either because their integrity is compromised (they are extremely small in size or have extremely low mechanical strength) or because they contain excessively large amounts of contaminants. In such cases, the performance of the regenerated or reactivated product will be insufficient.
[0016] Generally, metals contained in spent hydrogenation or hydrogenation catalysts are not industrially recycled today for the purpose of manufacturing new catalysts. They are essentially reused in the manufacture of special alloys, but this requires complex purification operations, and in particular, compounds considered to be contaminants, such as arsenic, or compounds considered problematic given the target application, such as phosphorus, whose presence would impair the properties of, for example, chromium steel alloys, must be removed from the recovered metals.
[0017] Further developments have been made to recover metals from catalysts and recycle them for the production of new catalysts. This is the case, for example, in the method described in Patent Document 4, which provides for the recovery of molybdenum from spent catalysts to make new catalysts. To do this, according to this method, the spent catalyst is dispersed in a basic solution and contaminants / compounds contained in the spent catalyst that are to be removed (arsenic, phosphorus) are extracted from the solution. These extractions are carried out by precipitating them and then filtering the solution. Molybdenum is then precipitated by modifying the pH of the solution toward an acidic pH. The molybdenum precipitate is filtered off and made reusable by dispersion in an impregnation solution further containing precursors of other metals, e.g., precursors of cesium, antimony, or vanadium, and precursors of other components necessary to constitute a new catalyst by impregnation of a support.
[0018] Patent Document 5 provides a highly similar method aimed at selectively recovering metals from Group VIB and Group VIII from spent catalysts containing metals from Group VIB and Group VIII, and reusing them for the purpose of producing new catalysts. The provided method consists of oxidizing the spent catalyst by calcination at 600°C, physically separating the oxides of Group VIB metals from the oxides of Group VIII metals, then dissolving the oxides of Group VIB metals in an alkaline solution, oxidizing the solution with a peroxide-type oxidizing agent, precipitating the oxides of Group VIB metals by adding alkaline earth metal ions, filtering the precipitate, and then converting it into a solid metal compound by adding an acid. This solid metal compound is subsequently dissolved in an impregnation solution also containing the compound of Group VIII metals, impregnating a carrier, and thus producing a new catalyst.
[0019] These methods are technically advantageous, however, they are not without drawbacks. The reason is that they involve a large number of operations and the extraction of the target metals from the used catalyst and their reuse in a new catalyst remains complex, thus making them complex to implement and not very beneficial as a result.
[0020] The object of the present invention is, therefore, to provide a method for recycling the metals contained in a used catalyst to produce a new catalyst. The present invention relates to the development of an improved method which is particularly simpler to implement on an industrial scale while enabling a high recovery rate of the metals.
Prior Art Documents
Patent Documents
[0021]
Patent Document 1
Patent Document 2
Patent Document 3
Patent Document 4
Patent Document 5
Summary of the Invention
Means for Solving the Problems
[0022] (Summary of the Invention) The subject of the present invention is, firstly, a method for producing a recycled catalyst comprising a carrier based on at least one metal M1 from Group VIB and / or at least one metal M2 from Group VIII, optionally phosphorus and / or sulfur, and one or more oxides, characterized in that it comprises recycling at least a portion of one or more metals of a source catalyst containing metal M1 and / or metal M2 common to the recycled catalyst to be produced, the method comprising: - extracting metal M1 and / or metal M2 from the source catalyst with an extraction solution to obtain a solution of the extracted metal(s); - then impregnating a carrier with an impregnation solution obtained from the solution of the extracted metal(s), to obtain an impregnated substrate, wherein the extracted metal(s) remain in the liquid phase from extraction to impregnation.
[0023] According to the present invention, it is understood that "resulting" of the extract solution from the extract solution means that there will be no intermediate processing in which the extracted metal(s) are in a solid phase, and there will be no liquid / liquid extraction process.
[0024] To do this, the impregnation solution and the extraction solution preferably share at least one solvent.
[0025] These may have one solvent or a mixture of several solvents, and if a mixture, the proportions of each solvent may be the same or different. For example, this could relate to a mixture of several solvents, including water or a solvent that is primarily or essentially aqueous.
[0026] According to the present invention, "extraction" is understood to mean the fact that there is an extraction step, but the extraction can be performed by a single extraction operation or by multiple consecutive extraction operations.
[0027] According to the present invention, "impregnation" is understood to mean the fact that there is an impregnation step, but impregnation can be carried out by a single impregnation or a series of consecutive impregnation operations.
[0028] According to the present invention, the “source” catalyst is understood to mean a spent catalyst, i.e., a catalyst that has already been used in the manufacturing process, particularly in equipment for hydrocracking-type hydrotreatment or hydroconversion. This catalyst may, in some cases, have already been regenerated and reactivated prior to its recycling. The term is also understood to mean a catalyst that has not yet been used in the manufacturing process but is substandard, for example, because it contains one or more metals in insufficient proportions, or because it is smaller than the required size (e.g., “fine particles” of catalyst particles).
[0029] According to the present invention, the term "carrier" (which will be impregnated with an impregnation solution derived from a solution of one or more extracted metals) means a "new" oxide carrier, but is also understood to mean a carrier that has already been impregnated with another impregnation solution (a pre-impregnated carrier is mentioned), or in fact a catalyst carrier (a carrier comprising multiple metals) that contains an insufficient amount of metal, such as a spent catalyst or a regenerated catalyst.
[0030] The present invention is advantageously applicable to the recycling of metals from hydrogenation catalysts.
[0031] Preferably, the extraction solution and / or impregnation solution is an acidic medium.
[0032] If these media are aqueous, their acidity is expressed by their pH value, which is at most 6, for example, 0.5 to 6. If these media are organic, their acidity can be expressed by the content of inorganic or organic acids.
[0033] Advantageously, the impregnation solution does not contain alkali metal elements (column IA of the periodic table according to Chemical Abstract Service nomenclature, corresponding to column 1 according to IUPAC nomenclature). This is because alkali metals have been found to tend to behave as poisons in hydrogenation catalysts.
[0034] According to one embodiment, the present invention extracts only a single metal M1 or metal M2 from the catalyst, particularly when it contains only metal M1 or only metal M2. According to another embodiment, the spent catalyst contains both at least one metal M1 and at least one metal M2, and according to the present invention, either only one of the type M1 or type M2 metals is extracted, or both type M1 and type M2 metals are extracted.
[0035] The present invention therefore provides a novel method in which the metal derived from the source catalyst is dissolved and remains in the solution until it is reused as a replenishment of the impregnation solution for producing a fresh / new catalyst. Unlike the prior art, the present invention does not attempt to recover the metal from the source catalyst, which is in the form of a solid and monometallic substance, thus saving a number of precipitation / filtration type operations themselves. The method of the present invention is therefore easier to implement on an industrial scale. It is further simplified when the extraction solution and the impregnation solution have a common solvent (or mixture of solvents), in particular when the solvents of the two solutions are identical (or, for example, similar except for the proportion of solvents in the case of a mixture of solvents).
[0036] Preferably, the extraction is carried out with a solution containing a solvent, particularly an aqueous solvent, and at least one organic compound having complexing properties and, optionally, acidic properties.
[0037] This is because adding organic compounds to a solution (generally aqueous) has proven to be very effective in extracting metals that are to be recycled by passing them through the liquid phase, while the support of the source catalyst and other optional compounds of the spent catalyst remain in the solid phase and are therefore easily removed.
[0038] It should be emphasized that the organic compounds that yield the most favorable results are those possessing acidic and complexing properties. This is because organic acids allow for the protonation of metal oxides, thereby limiting their interaction with the support and promoting their dissolution in the extract. Complexing agents, in part, enable the formation of soluble metal complexes in the extract. The combination of acidic and complexing properties is thus particularly advantageous. The use of organic compounds possessing these two properties, or combinations of acidic and complexing organic compounds, is therefore particularly indicated.
[0039] This organic compound, or if there are several organic compounds, at least one of them may contain one or more chemical functional groups selected from carboxylic acids, phosphoric acids, sulfonic acids, alcohols, thiols, thioethers, sulfones, sulfoxides, ethers, aldehydes, ketones, esters, carbonates, amines, nitriles, imides, oximes, ureas, and amides, or a compound containing a furan ring, or a sugar.
[0040] The organic compound (or, if there are several organic compounds, at least one of them) may be selected from at least one of the following compounds: formic acid, acetic acid, oxalic acid, malonic acid, glutaric acid, glycolic acid, lactic acid, tartaric acid, citric acid, tartaric acid, pyruvic acid, γ-ketovaleric acid, succinic acid, acetoacetic acid, gluconic acid, ascorbic acid, phthalic acid, salicylic acid, maleic acid, malic acid, fumaric acid, acrylic acid, thioglycolic acid, 2-hydroxy-4-methylthiobutanoic acid, glutamic acid, N-acetylglutamic acid, alanine, glycine, cysteine, histidine, aspartic acid, N-acetylaspartic acid, 4-aminobutanoic acid, 1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid (EDTA), nitrilotriacetic acid (NTA), iminodiacetic acid Acids: IDA), N-(2-hydroxyethyl)ethylenediamine-N,N',N'-triacetic acid (HEDTA), diethylenetriaminepentaacetic acid (DTPA), bicine, tricine, 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP or etidronic acid), nitrilotris (methylenephosphonic acid), diethylenetriaminepentakis (methylenephosphonic acid), 4-sulfophthalic acid, 3-(N-morpholino)-2-hydroxy-1-propanesulfonic acid (MOPSO), 2-(4-pyridinyl)ethanesulfonic acid, phenol-4-sulfonic acid, thiodiacetic acid, and diglycolic acid.
[0041] This is because the chemical compounds in this group exhibit both acidic and complexing properties.
[0042] The organic compound (or at least one of several organic compounds) may be selected from at least one of the following compounds: dimethylglyoxime, methyl acetoacetate, ethyl acetoacetate, ethyl lactate, methyl glycolate, ethyl glycolate, dimethyl malate, diethyl malate, dimethyl tartrate, diethyl tartrate, ethyl 3-hydroxybutanoate, ethyl 3-ethoxypropanoate, methyl 3-methoxypropanoate, methyl 3-(methylthio)propanoate, ethyl 3-(methylthio)propanoate, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol (molecular weight 200-1500 g / mol), propylene glycol, glycerol, 2-butoxyethanol, 2-(2-butoxyethoxy)ethanol, 2-(2-methoxyethoxy)ethanol, triethylene glycol dimethyl Tyl ether, crown ether, acetophenone, 2,4-pentanedione, pentanone, glucose, fructose, sucrose, sorbitol, xylitol, mannitol, γ-valerolactone, propylene carbonate, octylamine, N,N-diethylformamide, N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, propanamide, 1-methyl-2-pyrrolidinone, tetramethylurea, N,N'-dimethylurea, acetonitrile, lactamide, furflore, 2-fluoraldehyde, 5-hydroxymethylfurfural, 3-hydroxybutanoate ethyl, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidinone, N,N,N',N'-tetramethyltartrate, 3-hydroxypropionitrile, and N,N'-bis(2-hydroxyethyl)ethylenediamine.
[0043] This is because the chemical compounds in this group exhibit complexing properties.
[0044] Advantageously, the extraction solution also contains at least one inorganic acid, particularly phosphoric acid, nitric acid, or boric acid. This combination of complexing organic compounds and inorganic acids has proven to be highly effective, enabling the efficient extraction of the target metal in a single step, especially by creating a sufficiently acidic environment, which is particularly advantageous. This is especially true if the impregnation of the support with this solution must be carried out in an acidic medium, and if the final catalyst must contain phosphorus, and if phosphoric acid is chosen.
[0045] Once the concentration of each organic compound in the extract solution is defined, the concentration of the organic compound (one or more) in the extract solution is defined, and as a result, the molar ratio of organic compound / extracted metal (one or more) is set to 0.2 to 25, preferably 0.2 to 11, preferably 0.2 to 5, preferably 0.4 to 2, and most preferably 0.4 to 1.2 for each organic compound (one or more) if there are multiple organic compounds.
[0046] Advantageously, the recycling according to the present invention may include at least one step of treating the source catalyst prior to extraction by liquid route, selected from at least one of the following treatments: decoking, separation of compounds of the type of contaminants / impurities, or mechanical grinding. The purpose of these pretreatments is to make the extraction more effective by mechanical, physical, or chemical treatment: grinding reduces the particle size of the source catalyst particles and increases the contact surface area of the particles / extraction solution. Removing coke and other contaminants or reducing their amounts proceeds in the same direction, which is done by improving / increasing the contact between the extraction solution and the metal to be extracted, which is contained in the source catalyst.
[0047] Advantageously, the recycling may include at least one step of treating the solution of one or more extracted metals prior to impregnation, selected from at least one of the following treatments: concentration, dilution, or modification of the composition of the solution by the complete or partial addition or removal of at least one compound. According to one embodiment, this or these treatment steps are selected solely from concentration, dilution, or modification of the composition of the solution by the complete or partial addition or removal of at least one compound.
[0048] The purpose of these post-treatments is to place the extract solution under the conditions desired for it to function as an impregnation solution. Concentration by thus removing at least a portion of the solvent / nonmetallic compound from the solution will make it more efficient and bring it closer to the concentration required to carry out impregnation in conventional methods for impregnating fresh catalysts. This can also be achieved, for example, by contributing the constituent elements of the catalyst to be produced to this solution, in particular at least one metal that is not present in the solution or is present in insufficient amounts.
[0049] The impregnation of the carrier can therefore be carried out starting from a solution of one or more extracted metals, supplementation of at least one of the metals M1 and M2, possibly supplementation of phosphorus, and possibly supplementation of one or more organic additives. This is because the addition of organic additives to hydrogenation catalysts has been recommended by those skilled in the art to improve their activity. The supplementation can be added in advance to the solution of one or more extracted metals for premixing, or it can be added separately to the device on which the carrier impregnation is carried out. The supplementation can be in liquid or non-liquid form; if added separately, it will rather be in liquid form, and if added to the solution of one or more extracted metals prior to appropriate impregnation, it can be in liquid or solid form.
[0050] In some cases, the method according to the present invention may also include a step of sulfidation of the impregnated substrate: if the catalyst to be produced must contain sulfur, it is known that sulfur may be introduced, in whole or in part, just at the end of the production method, ex situ on the line for the production of the catalyst, or in situ in the hydrogenation reactor on the hydrogenation facility, particularly during the startup phase of the facility.
[0051] The method according to the present invention may also include one or more steps of heat treatment of the carrier after impregnation. It generally includes at least one heat treatment of the drying type. It may also include calcination.
[0052] In known methods for producing new catalysts, the following is generally provided after impregnation: - Aging stages depending on the case, - Drying or firing, - Depending on the circumstances, the addition of organic additives, - In the case of adding organic additives, further drying and - Ultimately, sulfidation may occur depending on the circumstances.
[0053] These steps, in particular the post-impregnation of organic additives, can thus be carried out in a manner similar to that of the method for the recycled catalyst of the present invention.
[0054] According to the present invention, after impregnation of the carrier, at least a portion of the impregnation solution can be reused, in particular, as a replenishment for the extraction solution. This thus limits the consumption of the solvent and (optional) organic compounds in the method.
[0055] According to the present invention, a solution of one or more extracted metals may be concentrated, and at least a portion of the solvent and, optionally, at least a portion of any selected organic compounds contained therein may be withdrawn from it, and thereafter, at least a portion of the solvent / organic compounds thus withdrawn is reused as replenishment for the extract solution. Here again, this reuse makes it possible to limit the consumption of the solvent / organic compounds in the present method.
[0056] According to one embodiment, the method according to the present invention includes the following (sequential, but not necessarily sequential) steps: - At least one step of processing the source catalyst (a1, a2, a3), - Extraction step (b) with an extraction solution of one or more metals of the source catalyst; to obtain a solution of one or more extracted metals, - At least one optional step (c) of purifying the solution of one or more metals extracted in step (b); removing all or part of any possible impurities therefrom. - At least one optional step (d) of concentrating the solution of one or more extracted metals, - At least one optional step (e) of adjusting the composition of the solution of one or more extracted metals resulting from step (b), (c), or (d), - Impregnation of the carrier via a liquid route by an impregnation solution obtained from the solution of one or more extracted metals obtained in step (b), (c), (d), or (e), optionally supplementing with an optional supply of one or more metals, phosphorus and organic additives (one or more); obtaining an impregnated substrate, wherein the extracted one or more metals remain in the liquid phase from extraction to impregnation (depending on whether steps (c), (d), and (e) are performed or not, and the order in which they are performed). - Optional sulfidation (g) of the impregnated carrier obtained in step (f).
[0057] It should be noted that step (b) is performed before step (f) and sulfidation (g) is performed after step (f). The optional steps (c), (d) and (e) are preferably performed in the order described above for the steps, i.e., step (c), then step (d), then step (e), but they may also be performed in a different order (e.g., (d), (c), (e), (c), (e), (d), or (e), (c), (d)).
[0058] As described above, the method according to the present invention is more specifically aimed at producing catalysts for hydrogenation or hydrocracking.
[0059] The spent catalyst used in the recycling method according to the present invention can be regenerated or reactivated before recycling by liquid extraction of the metal.
[0060] The metal M1 of the catalyst to be produced is preferably Mo and / or W, and the metal M2 of the catalyst is preferably Ni and / or Co. The support is preferably based on silicon and / or aluminum oxide, which preferably contains phosphorus and optionally sulfur. The source catalyst is of the same type and contains at least the same metal M1 and / or the same metal M2 as the catalyst to be produced.
[0061] In the method according to the present invention, the only thing that may be provided is a carrier, on which impregnation is carried out with an impregnation solution obtained from a solution of one or more extracted metals to be impregnated with a (conventional) impregnation solution. After impregnation with the impregnation solution according to the present invention, the carrier may also be post-impregnated with a conventional impregnation solution. The term “conventional” impregnation solution is understood to mean a “fresh” solution containing, in known ways, precursors of the components of the active phase of the catalyst, very specifically precursors of the metal components. The purpose of this pre-impregnation and / or post-impregnation of the carrier is, among other things, to adjust the amount of metal as needed so that the catalyst ultimately has the desired composition.
[0062] In the context of this invention, the support may also be a metal-depleted spent catalyst of the regenerated / reactivated type.
[0063] The present invention also relates to catalysts produced by the above method, which may therefore contain, as a whole, one or more recycled metals, or partially, one or more recycled metals and "fresh" metals.
[0064] The present invention also relates to a catalyst for any hydrogenation or hydrocracking, the catalyst comprising a mixture of fresh catalyst particles (which are obtained without recycling according to the present invention) and catalyst particles obtained by the recycling method of the present invention. [Modes for carrying out the invention]
[0065] (List of drawings) Figure 1 shows a block diagram of a first-choice configuration of equipment for carrying out the method according to the present invention.
[0066] Figure 2 shows a block diagram of a second-option configuration of equipment for carrying out the method according to the present invention.
[0067] The figures are highly schematic and do not necessarily represent all possible operations that may be involved in the methods according to the present invention. Reference numerals identical from one figure to the other relate to the same operation / same component / same device.
[0068] (Description of the embodiment) (definition) The groups of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, published by CRC Press, editor-in-chief Dr. Lide, 81st edition, 2000-2001). For example, Group VIII according to the CAS classification corresponds to the metals in columns 8, 9, and 10 of the new IUPAC classification.
[0069] (Source catalyst) In the non-limiting examples and in the detailed description of the present invention, the specifications and formulations of the catalyst to be produced by recycling are considered to correspond to the formulation of the “source” catalyst (minus contaminants, coke, and other substances that would gradually deactivate the catalyst).
[0070] Naturally, this remains within the scope of the present invention for producing a recycled catalyst from a source catalyst, and the source catalyst contains the following: - At least one type of metal; which is common to it, but not all metals are likely to be common to it, and / or - One or more types of metals; common but in different concentrations, or further, - One or more common metals and one or more additional metals; these will not form part of the composition of the recycled catalyst produced.
[0071] Therefore, as long as they share at least one common metal, it is possible to use a source catalyst that does not have the same function as the recycling catalyst to be manufactured (hydrogenation catalyst, hydrocracking catalyst, Fischer-Tropsch catalyst), or a source catalyst that has the same function (for example, a hydrogenation catalyst in both cases).
[0072] This is because, as understood above, the following is that the method according to the present invention allows for the adjustment of the composition of the catalyst produced by an optional adjustment step, and the extraction step according to the present invention can be selected selectively, that is, operated to extract only one or more metals common to the catalyst to be produced from the source catalyst.
[0073] The specifications are as follows:
[0074] The source catalyst of the method according to the present invention is a catalyst comprising at least one oxide support and at least one metal, preferably multiple metals. The term "source" according to the present invention is as defined above.
[0075] The source catalyst comprises at least one metal belonging to Group VIII and / or at least one metal belonging to Group VIB, an oxide support, and optionally phosphorus. It may also contain, but is not limited to, coke and / or sulfur, as described below.
[0076] Discharge of spent catalyst from a hydrogenation and / or hydrocracking method is preferably preceded by a de-oiling step. The de-oiling step generally involves contacting the spent catalyst, at least partially, with a flow of inert gas (i.e., essentially oxygen-free), such as nitrogen, at a temperature of 300°C to 400°C, preferably 300°C to 350°C. The flow rate of the inert gas is 5 to 150 SL·h over 3 to 7 hours with respect to the flow rate per unit volume of catalyst. -1 In an alternative form, the de-oiling step may be carried out by light hydrocarbons, by steam treatment, or by any other similar method.
[0077] The oxide support of the source catalyst in the method according to the present invention is typically a porous solid selected from the group consisting of: alumina, silica, silica-alumina, and also an oxide of titanium or magnesium (used alone or as a mixture with alumina or silica-alumina).
[0078] In another preferred case, the oxide present in the support of the source catalyst of the method according to the present invention is silica-alumina containing at least 50% by weight of alumina relative to the total weight of the composite support. The silica content in the support is at most 50% by weight, generally 45% by weight or less, and preferably 40% by weight or less, relative to the total weight of the support.
[0079] In a particularly preferred alternative form, the support for the source catalyst consists of alumina, silica, or silica-alumina.
[0080] The oxide support may also advantageously further contain 0.1% to 80% by weight, preferably 0.1% to 50% by weight, of zeolite relative to the total weight of the support. In this case, all known sources of zeolite and all associated preparation methods may be incorporated. Preferably, the zeolite is selected from the group FAU, BEA, ISV, IWR, IWW, MEI, UWY, and preferably, the zeolite is selected from the group FAU and BEA, for example, zeolite Y and / or beta-zeolite, particularly preferably, for example, USY and / or beta-zeolite.
[0081] The carrier is advantageously provided in the form of beads, extruded materials, pellets, or irregular and non-spherical aggregates, the particular shape of which may result from the grinding stage.
[0082] The active phase of the source catalyst preferably comprises at least one metal from Group VIB and at least one metal from Group VIII. The Group VIB metal present in the active phase of the catalyst is preferably selected from molybdenum and tungsten, or a mixture of these two elements. The Group VIII metal present in the active phase of the catalyst is preferably selected from cobalt, nickel, and a mixture of these two elements. The active phase of the catalyst is preferably selected from the group formed by combinations of elements such as nickel-molybdenum, cobalt-molybdenum, nickel-cobalt-molybdenum, nickel-tungsten, nickel-molybdenum-tungsten, and nickel-cobalt-tungsten.
[0083] The metal content from Group VIII is 1% to 10% by weight, preferably 1.5% to 9% by weight, and preferably 2% to 8% by weight, relative to the total weight of the dry catalyst. When the metal is cobalt or nickel, the metal content is expressed as CoO and NiO, respectively.
[0084] The metal content from Group VIB is 5% to 40% by weight, preferably 8% to 35% by weight, and very preferably 10% to 30% by weight, of the metal oxide from Group VIB relative to the total weight of the dry catalyst. When the metal is molybdenum or tungsten, the metal content is expressed as MoO3 and WO3, respectively.
[0085] The molar ratio of metals from Group VIII to metals from Group VIB in the catalyst is preferably 0.1 to 0.8, more preferably 0.15 to 0.6, more preferably 0.2 to 0.6, or also 0.3 to 0.5, when it contains both types of metals.
[0086] The source catalyst of the method according to the present invention may also contain phosphorus as a dopant. The dopant is an additional element that does not exhibit any catalytic properties on its own, but enhances the catalytic activity of the active phase.
[0087] The phosphorus content in the source catalyst, expressed as P2O5, is preferably 0.1% to 20% by weight, preferably 0.2% to 15% by weight, and most preferably 0.3% to 8% by weight, based on the total weight of the dry catalyst.
[0088] The molar ratio of phosphorus to elements from Group VIB in the catalyst is 0.05 or higher, preferably 0.07 or higher, preferably 0.08 to 1, preferably 0.01 to 0.9, and very preferably 0.15 to 0.6.
[0089] The source catalyst of the method according to the present invention may contain sulfur. The sulfur content in the source catalyst is expressed as an element relative to the total weight of the dry catalyst, preferably 1% to 15% by weight, preferably 2% to 12% by weight, and most preferably 4% to 10% by weight. The sulfur content is measured by elemental analysis according to ASTM D5373.
[0090] The source catalyst of the method according to the present invention may include coke, in particular if it has not been regenerated. It should be noted that in this patent application, the term "coke" refers to a hydrocarbon-based substance deposited on its surface during the use of the catalyst, which is a highly cyclized and condensed substance and has an appearance similar to graphite.
[0091] The coke content is expressed as a weight percent of carbon and can be 5% to 20% by weight, preferably 6% to 16% by weight, and particularly 7% to 14% by weight, relative to the total weight of the dry catalyst. The coke content is determined according to the ASTM D5373 method.
[0092] In some cases, the source catalyst may further exhibit low levels of contaminants, such as silicon, arsenic, iron, sodium, or chlorine, or even sulfur, resulting from the feedstock treated with the fresh catalyst from which the source catalyst originates.
[0093] Preferably, the silicon content of the source catalyst (apart from any silicon that may be present on fresh catalyst) is less than 2% by weight, and more preferably less than 2000 ppm by weight, relative to the total weight of the source catalyst.
[0094] Preferably, the arsenic content is less than 2000 ppm by weight relative to the total weight of the source catalyst, and more preferably less than 500 ppm by weight.
[0095] Preferably, the chlorine content is less than 2000 ppm by weight relative to the total weight of the regenerated catalyst, and more preferably less than 500 ppm by weight.
[0096] Preferably, the sulfur content is less than 2% by weight of the total weight of the source catalyst, and more preferably less than 2000 ppm by weight.
[0097] Preferably, if the source catalyst is a regenerated catalyst, it is uncontaminated, i.e., it contains less than 100 ppm by weight of silicon (except what may be present on a fresh catalyst), 100 ppm by weight of sodium (except what may be present on a fresh catalyst), 50 ppm by weight of arsenic, 50 ppm by weight of iron, and 50 ppm by weight of chlorine.
[0098] According to one embodiment of the present invention, the source catalyst of the method according to the present invention may include or consist of particulate matter generated during the operation of discharging the spent catalyst from an industrial unit from which the spent catalyst is extracted, or during regeneration.
[0099] According to another embodiment, the source catalyst of the method according to the present invention comprises or consists of substandard fine particles and / or products arising from various unit operations of the production of the new catalyst.
[0100] (Step of the method for producing a recycled metal-based catalyst according to the present invention) (Stage (a) (Optional): The stage before extraction (one or more times)) If the source catalyst is a spent catalyst, this is generated during the hydrogenation of hydrocarbon fractions containing sulfur and other contaminants, such as silicon, arsenic, chlorine, iron, sodium, or nitrogen, particularly during methods of hydrodesulfurization or hydroconversion. The formation of coke and / or the accumulation of contaminants converts the fresh catalyst into a spent catalyst, at least partially.
[0101] An optional step (a) is to remove all or part of one or more impurities that may be present in the source catalyst by any method known to those skilled in the art, prior to the metal extraction step (b). Preferably, step (a) includes a regeneration step to remove all or part of coke, sulfur and / or chlorine, or a heat treatment step under a gas flow containing hydrogen sulfide, which is carried out in particular to remove arsenic.
[0102] (Example of stage (a1): Playback) The catalyst, at least partially used, is subjected to a stage of coke and sulfur removal: a regeneration stage, which makes it possible to remove all or part of the coke, sulfur, and / or chlorine that may have accumulated on the catalyst.
[0103] Even if this were possible, regeneration is preferably not carried out by maintaining the catalyst loaded in the hydrogenation reactor (on-site regeneration). Preferably, the catalyst, at least partially used, is therefore extracted from the reactor and sent to a regeneration plant for on-site regeneration (off-site regeneration).
[0104] The regeneration stage is generally carried out in a gas stream containing oxygen, typically in air. The water content in the gas is generally 0% to 50% by weight. The gas flow rate with respect to the flow rate per unit volume of at least partially used catalyst is preferably 20 to 2000 SL·h -1 Comfortable 30-1000 SL·h -1 Particularly preferred is 40-500 SL·h -1 The duration of the regeneration is preferably 2 hours or more, more preferably 2.5 hours or more, and particularly preferably 3 hours or more. The temperature at which the regeneration of at least partially used catalyst is generally performed is 320 to 550°C, preferably 360 to 500°C.
[0105] The regenerated source catalyst consists of an oxide support from the source catalyst, an active phase formed from at least one metal from Group VIB and at least one metal from Group VIII, and optionally phosphorus. The regenerated catalyst has a surface area of 20 to 300 m 2 / g, preferably 30 to 280 m 2 / g, preferably 40 to 260 m 2 / g, most preferably 80 to 250 m 2 / g.
[0106] (The source catalyst (used and then regenerated here)) generally has a pore volume of 0.1 cm 3 / g to 1.3 cm 3 / g, preferably 0.2 cm 3 / g to 1.1 cm 3 / g.
[0107] The regenerated catalyst obtained in the regeneration step contains residual carbon at a content of less than 3% by weight, preferably 0% to 2.9% by weight, preferentially 0% to 2.0% by weight, and particularly preferably 0% to 1.0% by weight, based on the total weight of the regenerated catalyst. It should be noted that in this patent application, the term "residual carbon" means carbon (coke) remaining in the regenerated catalyst after the regeneration of the used hydrotreating catalyst. The content of this residual carbon in the regenerated hydrotreating catalyst is measured according to the ASTM D5373 method.
[0108] (Example of step (a2): Heat treatment under a gas stream containing hydrogen sulfide (optionally in a cumulative manner together with the regeneration in the preceding step (a1))) All or part of the elemental arsenic or arsenic compounds that may be present in the source catalyst can be removed by passing a stream of hydrogen sulfide and an inert gas through the solid at a temperature of 300°C to 750°C. During this process, the arsenic present in the source catalyst forms arsenic sulfide (formula As2S3) and is volatilized from the solid. This reaction is preferably carried out by fluidizing the solid in a stream of hydrogen sulfide and an inert gas. When a mixture of hydrogen sulfide and an inert gas is used, the inert gas is preferably nitrogen, carbon dioxide, or a combustion gas.
[0109] (Example of stage (a3): Optional preliminary crushing) The source catalyst can, advantageously, undergo an optional grinding step prior to extraction to facilitate the dynamics of metal extraction during the extraction step (b) of the method according to the present invention. In this case, this step includes a first optional phase (a3) that conditions the source catalyst by grinding at least once to obtain source catalyst particles having a maximum size of 1 mm. Naturally, several successive grinding steps can be performed to reach the target particle size. Any method known to those skilled in the art can be used to perform this crushing or grinding step, such as a ball mill or a rotary cutter mill. Preferably, the size of the source catalyst used during the extraction step (b) according to the present invention is 1 to 1000 micrometers (1 mm), preferably 80 to 500 micrometers, and more preferably 100 to 400 micrometers. Most frequently, the ground source catalyst is transported to the extraction zone by any means known to those skilled in the art, in particular by a screw conveyor or by pneumatic transport.
[0110] (Extraction stage (b)) In this stage, the source catalyst is brought into contact with the extraction solution. The extraction solution contains at least one organic compound, preferably having complexing properties and optionally acidic properties (for example, at least one compound having both properties, or a combination of at least one acidic compound and at least one complexing compound, or at least one complexing compound alone).
[0111] The extraction solution according to the present invention may contain any polar protic solvent known to those skilled in the art. Preferably, the polar protic solvent is selected from the group formed by methanol, ethanol, and water, or a mixture of water-ethanol or water-methanol, and this is used. Much preferably, the solvent used in the impregnation solution is water. In the case of an aqueous solution, the pH of the solution can be modified by the addition of an optional acid or base. The pH of the extraction solution is generally 0.1 to 8.5, preferably 0.5 to 6, and more preferably 1 to 4.
[0112] Generally, organic compounds are compounds containing one or more chemical functional groups selected from carboxylic acids, phosphoric acids, sulfonic acids, alcohols, thiols, thioethers, sulfones, sulfoxides, ethers, aldehydes, ketones, esters, carbonates, amines, nitriles, imides, oximes, ureas, and amides, or compounds containing furan rings, or sugars.
[0113] Examples of complexing organic compounds, as well as organic compounds possessing both complexing and acidic properties, have already been listed above; therefore, the list will not be repeated here.
[0114] The concentration of each organic compound in the extraction solution is determined so that the molar ratio of organic compound to extracted metal is 0.2 to 25, preferably 0.2 to 11, preferably 0.2 to 5, preferably 0.4 to 2, and most preferably 0.4 to 1.2.
[0115] When several organic compounds are present, various molar ratios are applied to each of the organic compounds present.
[0116] In one embodiment of the present invention, the extraction solution may also contain phosphorus. The presence of phosphorus in the extraction solution promotes the extraction of metals, particularly molybdenum, due to the high stability of the heteropolyanion formed by this metal together with phosphorus. The addition of phosphorus in the form of phosphoric acid (H3PO4) can also lower the pH of the solution, which is generally beneficial for the extraction of metals contained in the source catalyst. Inorganic acids other than phosphoric acid, particularly nitric acid or boric acid, can also be used.
[0117] A suitable phosphorus precursor is H3PO4 phosphoric acid, but its esters and salts, such as ammonium phosphate, are also suitable, as are polyphosphates. Without being bound by any particular theory, it appears that the combination of phosphoric acid with an organic acid with an acidity constant pKa greater than 1.5, i.e., a weak acid, allows for the observation of synergistic effects at a level of metal extraction that is unpredictable when phosphoric acid or the organic acid is used alone. Extraction in the presence of two specific acids enables very good dissolution of the metal phase.
[0118] In one embodiment of the present invention, the extraction solution may also contain an oxidizing agent to promote the extraction of metals. Preferably, the oxidizing agent contained in the extraction solution is hydrogen peroxide. When an oxidizing agent is present, the concentration is generally 0.1 to 5.0 mol·L -1 That is the case.
[0119] Generally, the operating conditions in step (b) are selected to maximize the extraction of the metal contained in the source catalyst, while minimizing the dissolution of the metal(s) contained in the support of the source catalyst, and limiting the amount of organic compounds so that the amount of organic compounds does not exceed the optimal amount of organic compounds required in the impregnation step, thereby obtaining a high-performance catalyst. It is also required to minimize the amount of extraction solution to be used, and to obtain the most concentrated metal solution possible at the end of the extraction: or, as an impregnation solution, the need to concentrate the solution in the impregnation solution or before using it as an impregnation solution is thus limited.
[0120] The contact procedure is performed using the extraction solution under the following conditions: - Temperature: 10-150℃, especially 15-95℃, - Pressure: Between atmospheric pressure and 20 bar, especially atmospheric pressure or up to 10 bar. - Duration: 1 minute to 20 hours, preferably 5 to 300 minutes, more preferably 5 to 180 minutes.
[0121] Preferably, the device(s) on which the contact operation is performed does not have a heating device, and the temperature of the contact operation is regulated by the temperature of the extraction solution. The temperature of the extraction solution may be between 15°C, 20°C, or 25°C and 95°C, preferably 30°C to 90°C, and more preferably 50°C to 85°C. Thus, for this particular contact stage, it may be ambient temperature or heated. It may also be a temperature above a given temperature, particularly the ambient temperature, because it is at least in part due to the recycling of liquid spills that occur in the method according to the present invention and are already in this temperature range.
[0122] The amount of extraction solution used for this step is, as described above, preferably as small as possible to obtain the desired effect. Preferably, this step (b) is carried out by contacting the source catalyst with the solution in a volume of 1.5 to 60 times the volume of the source catalyst. Preferably, the volume of the solution is 2 to 30 times the volume of the source catalyst, more preferably 2 to 20 times the volume of the source catalyst.
[0123] All modes of contact in a single step or several steps in the manner of parallel, countercurrent, or crosscurrent flow are possible for the implementation of step (b) in a continuous manner. Batch contact operations may also be provided. For example, contact operations may be carried out by immersion or otherwise by dropping the extract solution onto a moving source catalyst, for example, under a flow of the extract solution.
[0124] At the end of step (b), the solution is separated from the solid residue, yielding the leached catalyst on the one hand and the metal solution on the other, which will be used in the subsequent steps (c), (d), (e), or (f). Preferably, the residual metal content of the leached catalyst (the sum of the individual metal contentes contained in the leached catalyst, expressed as oxides) is less than 10% by weight, preferably less than 5% by weight, and very preferably less than 2% by weight. Any method of liquid / solid separation can be used, for example, by filtration or drainage, for example by gravity. Preferably, the separation step is carried out using a filter press type device.
[0125] (Stage (c) (Optional): Purification) The role of the optional step (c) of purifying the metal solution produced in step (b) is to remove all or part of any impurities that may be present in the metal solution. These impurities may arise particularly from impurities potentially present on the source catalyst or from the partial dissolution of the catalyst support. Step (c) may be carried out in a single step or in several consecutive steps.
[0126] At the end of step (b), if the metal solution after the separation step contains suspended solids, any known method for removing these suspended solids may be used during this step (c). Preferably, this removal is carried out by filtration (e.g., microfiltration and ultrafiltration on a cross-flow filter). Other methods include centrifugation or coagulation.
[0127] All known methods for removing dissolved impurities, such as arsenates or arsenites, may be used during this step (c), and in particular and preferably, adsorption on a solid, precipitation with a solvent, and extraction may be used, while at the same time care is taken not to remove the target metal from which extraction has been performed.
[0128] (Stage (d) (Optional): Concentration) Step (d) consists of concentrating the metal solution obtained from step (b) or (c). This is done by removing part of the solvent and all or part of the organic compounds contained in the metal solution. This step may be necessary if the metal concentration is too low for the concentration required for impregnation. Any known method for removing part of the solvent from the solution is assumed. Step (d) may be carried out in a single step or in several consecutive steps. All or part of the solvent, with or without organic compounds, extracted from the metal solution in step (d) may be recycled to extraction step (b).
[0129] Preferably, and especially when the metal solution is an aqueous solution, step (d) is carried out by evaporation and concentration. In this case, neutralization takes precedence, and as a result, the effluent enters the evaporator at a pH in the range of 5 to 7. Unless co-distillation is required for the simultaneous removal of the solvent and some of the organic compounds, this regulation of pH also makes it possible to limit the phenomenon of co-distillation in order to avoid precipitation of metal oxides as much as possible. Preferably, all or part of the distillate is recycled to the extraction step (b).
[0130] When only partial removal of the solvent is desired, apart from evaporation and concentration, suitable techniques are membrane technologies, and more preferably, nanofiltration, reverse osmosis and permeation vaporization, solvent extraction, or cryogenic concentration.
[0131] When solvents and organic compounds (one or more) are used and it is desired to remove them, a preferred technique is evaporation and concentration.
[0132] (Step (e) (Optional) for adjusting the composition of the metal solution) Step (e) consists of modifying the metal solution obtained from steps (b), (c), or (d) by adding (one or more) and / or removing (one or more) predetermined components. Metal precursors and / or phosphorus precursors and / or organic additives may be added. Organic compounds used for metal extraction may also be extracted, in whole or in part, if necessary. The objective is to obtain a metal solution whose composition corresponds to a desired composition as an impregnation solution used for the synthesis of the catalyst according to the present invention in impregnation step (f).
[0133] (Examples involving metals) Even if it is desired that the catalyst according to the present invention has the same formulation as the source catalyst, the ratio of each metal in the metal solution will potentially be altered. This is because, on the one hand, the purification of the catalyst—step (a)—may alter the initial content of each metal in the source catalyst, and on the other hand, the extraction step (b) may result in different extraction rates for each metal.
[0134] The ratio between each metal is adjusted by either adding a supplemental solution containing one or more of the aforementioned metals, or by directly dissolving one or more metal precursors in the metal solution obtained from step (b), (c), or (d), with direct dissolution being the preferred option. The molar ratio of metals from Group VIII to metals from Group VIB in the metal solution obtained from step (e) has already been specified above, but is generally 0.1 to 0.8, preferably 0.15 to 0.6.
[0135] Examples of metal precursors that may be used include, among sources of molybdenum, oxides and hydroxides, molybdic acid and its salts, in particular ammonium salts, such as ammonium molybdate or ammonium heptamolybdate, phosphomolybdic acid (H3PMo). 12 O 40 ) and their salts, depending on the case, silicic acid (H4SiMo 12 O 40 ) and its salts. The source of molybdenum can be any of the following heteropoly compounds: Keggin, deficient Keggin, substituted Keggin, Dawson, Anderson, or Strandberg. Preferably used are molybdenum trioxide, as well as heteropoly compounds of the Keggin, deficient Keggin, substituted Keggin, and Strandberg types.
[0136] The tungsten precursors that can be used are also well known to those skilled in the art. For example, among the sources of tungsten that may be used are oxides and hydroxides, tungstic acid and its salts, in particular ammonium salts, such as ammonium tungstate or ammonium metatungstate, phosphotungstic acid and its salts, and possibly silitungstic acid (H4SiW 12 O 40 ) and its salts. The source of tungsten can be any heteropoly compound of the type Keggin, deficient Keggin, substituted Keggin, or Dawson. Preferably used are oxides and ammonium salts, such as ammonium metatungstate, or heteropolyanions of the type Keggin, deficient Keggin, or substituted Keggin.
[0137] The cobalt precursors that can be used are advantageously selected from, for example, oxides, hydroxides, hydroxycarbonates, carbonates, and nitrates. Cobalt hydroxide and cobalt carbonate are preferred for use. Cobalt acetoacetate may also be involved.
[0138] The nickel precursors that can be used are advantageously selected from oxides, hydroxides, hydroxycarbonates, carbonates, and nitrates, for example. Nickel acetoacetate may also be involved.
[0139] (The case of phosphorus) A phosphorus precursor may be used in the extraction step (b). If the phosphorus / metal ratio of the metal solution obtained from steps (b), (c), or (d) is lower than that desired for the impregnation solution in step (f), then the same or a different phosphorus precursor as optionally used in step (b) may be added to the metal solution during step (e). This is particularly likely to apply if no phosphorus compound / precursor is added in step (b), or if the carrier contains alumina and the carrier consumes it, at least partially, to form an aluminophosphate. In this case, the molar ratio of phosphorus to metal from group VIB is 0.1 to 2.5 mol / mol, preferably 0.1 to 2.0 mol / mol, more preferably 0.1 to 1.0 mol / mol, or 0.15 to 0.8 mol / mol, or also 0.2 to 0.6 mol / mol.
[0140] A suitable phosphorus precursor is H3PO4 phosphate, but its esters and salts, such as ammonium phosphate, are also suitable, as are polyphosphates. Phosphorus can also be introduced simultaneously with one or more elements from Group VIB in the form of Keggin, deficient Keggin, substituted Keggin, or Strandberg-type heteropolyanions.
[0141] (Examples of organic additives) The addition of organic additives to hydrogenation catalysts has been recommended by those skilled in the art, as it improves their activity. They are known to improve the dispersibility of metals on the surface of the support and / or play a beneficial role during the sulfidation of the catalyst. Thus, one or more organic additives well known to those skilled in the art may be advantageously added at this stage. Generally, the amount of each organic additive added is specified such that the additive / metal molar ratio in the impregnation solution is 0.1 to 1.
[0142] Patent FR 3 083 134 describes an example of an organic additive. This organic additive may be suitable, may be used in aqueous form, and therefore may be added to the impregnation solution (in step (e) or step (f)). Patent FR 3 083 131 also describes an example of an organic additive, which may be suitable, but instead would be added separately in the pre-impregnation or post-impregnation of the carrier.
[0143] (Examples of organic compounds used for metal extraction) The metal solution obtained from step (b), (c), or (d) may contain an excess of organic compound relative to the desired impregnation solution. The ratio of organic compound to metal can be adjusted in two ways. The first method involves adding a concentrated solution of metal precursors or directly dissolving these metal precursors to achieve the desired ratio. In this case, the resulting final catalyst will contain a mixture of recycled metal and new metal.
[0144] If the excess of organic compounds is too high to use the first method (i.e., the amount of recycled metal incorporated into the final catalyst is insufficient, for example, less than 5% of the total amount of metal), the second method consists of removing all or part of the excess organic compounds from the metal solution. In this case, the organic compounds can be recycled to step (b). For this purpose, any method known to those skilled in the art for separating organic molecules from the metal solution is conceivable.
[0145] (Stage (f): Impregnation) According to step (f), a porous support or a catalyst already containing one or more metals (the “support” as defined above) is brought into contact with the solution obtained in step (b), (c), (d), or (e). According to step (f), the operation of bringing the porous support or the catalyst into contact with the metal salt in the solution can be carried out by any known method, such as ion exchange, dry impregnation, over-impregnation, vapor deposition, etc. The contact operation can be carried out in a single step or in several consecutive steps.
[0146] In a preferred configuration, the step (f) of bringing the carrier into contact with the metal solution is carried out by over-impregnation or dry impregnation.
[0147] Equilibrium or over-impregnation involves immersing a support or catalyst in a solution that is larger (often considerably larger) than the pore volume of the support or catalyst. Dry impregnation involves introducing, in part, an impregnation solution in a volume equal to or slightly smaller than the pore volume of the support or catalyst. Dry impregnation allows for the deposition of all components of the impregnation solution onto a given support or catalyst.
[0148] Step (f) may be advantageously carried out by one or more over-impregnations of the solution, or preferably by one or more dry impregnations, and for example by a single over-impregnation, using an impregnation solution.
[0149] Stage (f) is generally carried out at a temperature of 10°C to 95°C, a pressure between atmospheric pressure and 20 bar, preferably atmospheric pressure, and preferably over a period of 1 minute to 20 hours, preferably 1 to 300 minutes. Stage (f) is preferably carried out at a temperature of 10°C to 60°C, preferably at ambient temperature.
[0150] Advantageously, after each impregnation step, the impregnated support or catalyst is allowed to mature. This maturation process allows the impregnation solution to be uniformly dispersed within the support or catalyst.
[0151] Any maturation step described in this invention is advantageously carried out at atmospheric pressure, in a water-saturated atmosphere, at a temperature of 17°C to 50°C, preferably at ambient temperature. Generally, a maturation time of 10 minutes to 48 hours, preferably 30 minutes to 6 hours, is sufficient.
[0152] Advantageously, after step (f), the drying step is carried out at a temperature of less than 200°C, preferably 50–180°C, more preferably 70–150°C, and very preferably 75–130°C. The drying step is preferably carried out over a period of 10 minutes to 24 hours. Longer periods are not ruled out, but do not necessarily result in any improvement. The drying step can be carried out by any known technique. It is advantageously carried out under atmospheric pressure or reduced pressure. Preferably, this step is carried out under atmospheric pressure. It is advantageously carried out using hot air or any other hot gas. Preferably, the gas used is air or an inert gas, such as argon or nitrogen. Very preferably, the drying is carried out in the presence of nitrogen and / or air, and advantageously, on a transverse floor.
[0153] According to the alternative configuration, drying is advantageously carried out to preferably retain at least 30% by weight of the organic additive introduced between steps (e) and / or (f). Preferably, this amount is greater than 50% by weight, and more preferably greater than 70% by weight, calculated based on the carbon remaining on the catalyst.
[0154] In the alternative form, drying is advantageously carried out to preferably retain at least 30% by weight of the organic extractant compound introduced during step (f); preferably, this amount is greater than 50% by weight, and more preferably greater than 70% by weight, calculated based on the carbon remaining on the catalyst.
[0155] In some cases, a calcination step may be performed after drying. This may be done, for example, when it is desired to remove all or part of one or more organic extractants. According to this alternative form, at the end of the drying step, the calcination step is performed at a temperature of 200°C to 600°C, preferably 250°C to 550°C, under an inert atmosphere (e.g., nitrogen) or an oxygen-containing atmosphere (e.g., air). The duration of this heat treatment is generally 0.5 to 16 hours, preferably 1 to 5 hours. After this treatment, the active phase is therefore generally found in oxide form; heteropolyanions are therefore converted to oxides. Similarly, the catalyst no longer contains organic extractants and / or organic additives, or contains only very small amounts of organic extractants and / or organic additives. However, the introduction of organic additives during its preparation makes it possible to improve the dispersibility of the active phase, thereby resulting in a more active catalyst.
[0156] Preferably, the catalyst is not subjected to calcination.
[0157] In embodiments in which step (f) is carried out over at least two impregnation cycles, after each impregnation, advantageously, drying and optional firing are performed.
[0158] The oxide support used in step (f) of the method according to the present invention is typically a porous solid selected from the group consisting of: alumina, silica, silica-alumina, and also an oxide of titanium or magnesium (used alone or as a mixture with alumina or silica-alumina).
[0159] The total pore volume favorably exhibited by the oxide support is 0.1 to 1.5 mL / g, preferably 0.4 to 1.1 mL / g.
[0160] The specific surface area of the oxide support is advantageously 5 to 400 m². 2 ·g -1 Preferably 10-350m 2 ·g -1More preferably 40-350m 2 ·g -1 The specific surface area is determined in this invention by the BET method in accordance with standard ASTM D3663.
[0161] The oxide support of the recycled catalyst according to the present invention may have the same properties as the support of the source catalyst, and this has already been described above.
[0162] It is preferably selected from the group consisting of: silica, the transition alumina family, and silica-alumina. Much preferably, the oxide support is composed essentially of at least one transition alumina, i.e., it contains at least 51% by weight, preferably at least 60% by weight, much preferably at least 80% by weight, and indeed even at least 90% by weight of transition alumina. It preferably consists only of transition alumina. Preferably, the oxide support of the catalyst in the method according to the present invention is γ-phase alumina.
[0163] In another preferred case, the oxide present in the catalyst support of the method according to the present invention is silica-alumina containing at least 50% by weight of alumina relative to the total weight of the composite support. The silica content in the support is at most 50% by weight, generally 45% by weight or less, and preferably 40% by weight or less, relative to the total weight of the support.
[0164] Sources of silicon are well known. Examples that may be mentioned include silicic acid, silica in powder or colloidal form (silica sol), or tetraethyl orthosilicate Si(OEt)4.
[0165] If the support for the catalyst is silica-based, it contains more than 50% by weight of silica relative to the total weight of the support, and generally, it contains only silica.
[0166] In a particularly preferred alternative form, the carrier consists of alumina, silica, or silica-alumina.
[0167] The oxide support may also advantageously further contain 0.1% to 80% by weight, preferably 0.1% to 50% by weight, of zeolite relative to the total weight of the support. In this case, any source of zeolite known to those skilled in the art and any related preparation method may be incorporated. Preferably, the zeolite is selected from the group FAU, BEA, ISV, IWR, IWW, MEI, UWY, and preferably, the zeolite is selected from the group FAU and BEA, for example, zeolite Y and / or beta-zeolite, particularly preferably, for example, USY and / or beta-zeolite.
[0168] The carrier may also contain, in addition to those that may be introduced between steps (e) and / or (f), at least some of the metals (one or more) of Groups VIB and VIII and / or at least some of the phosphorus and / or sulfur and / or at least some of the organic additives (one or more). These are introduced, for example, during the preparation of the carrier. This is referred to as a “pre-impregnated” carrier.
[0169] It is also possible to add one or more types of metals to a carrier that has already been impregnated with the impregnation solution according to the present invention. This is referred to as a "post-impregnation" carrier.
[0170] In both the case of “pre-impregnation” and “post-impregnation” carriers, the objective is the same: it is the issue of adjusting the metal content of the final catalyst by either adding a certain amount of metal (one or more) present in the impregnation solution according to the present invention, or by adding one or more other metals in another step, in particular, with another impregnation solution, before and / or after step (f) of impregnating with the impregnation solution of the present invention.
[0171] The support can even be a catalyst, which will therefore be further "filled" with metal. It could be a metal-depleted catalyst, and in particular, it could be the spent catalyst itself, which may have been regenerated and then possibly reactivated.
[0172] The carrier is preferably provided in the form of beads, extruded materials, pellets, or irregular and non-spherical aggregates, the particular shape of which may be derived from the grinding stage.
[0173] The active phase of the recycled catalyst targeted by the method according to the present invention is generally of the type of active phase already described above for “spent” catalysts. It is also possible to seek to produce a recycled catalyst according to the present invention that contains a lower packing amount of metal than the spent catalyst used, in particular if this does not make it possible to concentrate the extraction solution before impregnation. The recycled catalyst may be used differently (on different hydrocarbon feedstocks) from the spent catalyst from which the recycled catalyst is derived (for example, a catalyst having 20% by weight of Mo expressed as MoO3 relative to the weight of the dry catalyst may be used for the hydrogenation of distillates, while a catalyst containing a lower packing amount of Mo, 10% by weight of Mo expressed as MoO3, may be used for the hydrogenation of naphtha).
[0174] The amount of recycled metal contained in the catalyst according to the present invention is 1% to 100% by weight of the metal contained in the catalyst produced by the present invention, preferably 10% to 100% by weight, more preferably 20% to 100% by weight, and even more preferably 50% to 100% by weight of the metal contained in the catalyst according to the present invention.
[0175] It should be emphasized that the catalyst produced by the present invention can have a different formulation from the spent catalyst used to recover the metal, and can have different amounts of metal and different ratios of metals: therefore, as described above, a spent catalyst containing a high packing amount of metal can be used by the present invention to produce a catalyst containing a lower packing amount of metal (and vice versa). This makes it possible, if appropriate, to avoid the step of concentrating the post-extraction solution at the end of step (b), or at least reduce its intensity / duration.
[0176] It should also be noted that the catalyst produced according to the present invention may be post-additivated, that is, it may be possible to further impregnate it with one or more organic additives, the function of which is to increase the catalytic activity of the non-additivated catalyst before the final sulfidation step (g), and preferably the calcination step is not performed after its introduction.
[0177] (Stage (g) (Optional): Sulfidation) Prior to use, the catalyst produced by the method according to the present invention may undergo an optional sulfidation step. Sulfidation is preferably carried out in a sulfo-reducing medium, i.e., in the presence of H2S and hydrogen, to convert the metal oxide into sulfides, such as MoS2 and Co9S8. Sulfidation is carried out by injecting the catalyst with a stream containing H2S and hydrogen, or with a sulfur compound that can decompose in the presence of the catalyst and hydrogen to yield H2S. Polysulfides, such as dimethyl disulfide (DMDS), are H2S precursors commonly used to sulfid the catalyst. Sulfur may also be derived from the feedstock. The temperature is controlled so that H2S reacts with the metal oxide to form a metal sulfide. This sulfidation may be carried out in or out of the reactor (inside or outside the reactor) of the hydrogenation treatment or hydrogenation conversion method according to the present invention at a temperature of 200–600°C, more preferably 300–500°C.
[0178] Figure 1 shows a block diagram illustrating a first alternative embodiment of the method according to the present invention.
[0179] The source catalyst is sent via line (1) to the purification unit (2): optional step (a1). Fluid containing contaminants is removed via line (3), while the purified catalyst is withdrawn via line (4) and sent to the mill (5): optional step (a3). The pulverized catalyst (6) is sent to the extraction unit (9) to recover a metal-rich metal solution (11): this is the extraction step (b). For this, an extraction solution (8) containing organic compounds is used. This extraction solution (8) may be a mixture of recycled extraction solution (13) and supplemental extraction solution (7), which allows for adjustment of the composition of the catalyst to be produced, particularly the ratio and amount of metals. The extraction unit (9) is operated in a temperature range of 10–150°C, particularly 10–95°C, and a pressure range of 1–20 bar.
[0180] Unit (9) also produces effluent (10). The effluent (10) contains, in particular, the source / used catalyst support and residual metal. The metal solution (11) is sent to a concentration unit (12); this is an optional concentration step (d), which makes it possible to obtain a solution (14) with a higher filler weight of metal. The concentration unit (12) also makes it possible to recover the metal-depleted fraction, which is recycled through line (13) (for example, obtained by condensation of the evaporated fraction in cases where concentration is performed by evaporative concentration which constitutes part of the extract solution (8)). A supplement solution (16), which may contain metal, phosphorus and organic additives, is added to the solution (14) to adjust the metal solution composition: this is the adjustment step (e). The mixture constituting the impregnation solution and the catalyst support (15) are then used in the impregnation unit (17) to deposit metal onto the catalyst support: This is the impregnation stage (f). After optional maturation, heat treatment and optional post-addition stages known to those skilled in the art, the impregnated catalyst (18) may finally be sent to a sulfidation unit (19) which enables the conversion of metal oxides into their sulfide forms: this is the sulfidation stage (g), which may be carried out in some cases (it may also be carried out later, in situ, in a hydrogenation / hydrogenation reactor). The catalyst (20) is finally produced.
[0181] Figure 2, in block diagram form, represents a second alternative form of the method according to the present invention. It is similar to the first alternative form; there are only two differences from the first alternative form, which are shown below: - The step (d) of concentrating the metal extract solution is omitted. - The outlet solution of the impregnation unit (17) is reused to constitute part, in particular, most or most of, the extraction solution (8).
[0182] (Example 1) The starting material was a spent "CoMoP" catalyst containing molybdenum, cobalt, and phosphorus, which were deposited on an alumina support used in the hydrogenation process. It was pre-regenerated at 450°C for 4 hours under a flow of dry air.
[0183] The regenerated catalyst contains molybdenum, phosphorus, and cobalt. The catalyst composition is expressed in oxide form and relative to the weight of the dry catalyst: 21.6 wt% MoO3 (14.4 wt% molybdenum), 3.7 wt% CoO (2.9 wt% cobalt, i.e., Co / Mo molar ratio equal to 0.33), and 3.2 wt% P2O5 (1.4 wt% phosphorus, i.e., P / Mo molar ratio equal to 0.3).
[0184] The extraction of metallic molybdenum and cobalt from this regenerated catalyst is performed on a laboratory scale: The regenerated catalyst (known as the source catalyst) is pre-ground to a particle size of 100-300 microns, and 40 g of this regenerated catalyst and 200 g of the extraction solution are introduced into a round-bottom flask. The extraction solution is an aqueous solution containing 4 wt% glutaric acid. The pH of the mixture is adjusted to 2.0 by adding phosphoric acid. The amounts of one organic acid (glutaric acid) and the other inorganic acid (phosphoric acid) were chosen so that they would not need to be subsequently removed / reduced in the extraction solution, which would function as the impregnation solution. The round-bottom flask, equipped with a reflux condenser to limit water loss by evaporation, is then placed in a water bath heated to 85°C, and the mixture is stirred at 200 rpm for 6 hours via a magnetic bar. The mixture is then filtered on sintered glass with a porosity of 5, recovering the polymetallic solution on one side and the solid residue on the other. Analysis of the solution reveals that it contains 25.9 g / L of molybdenum and 4.6 g / L of cobalt. The extraction rates of Mo and Co are calculated to be 90% and 80%, respectively.
[0185] The glutaric acid / Mo ratio and Co / Mo ratio of the polymetallic solution are adjusted to obtain a solution that can be used for impregnation of the new support.
[0186] For this purpose, the polymetallic solution is first concentrated by evaporation. In this way, 80% of the solvent (water) is removed, thereby obtaining 40 mL of a solution containing 13.0% by weight of molybdenum. The concentrated solution exhibits a glutaric acid / Mo molar ratio of 1.1, which is suitable for the impregnation solution. The Co / Mo molar ratio is 0.3. A sufficient amount of cobalt precursor Co(OH)2, i.e., 180 mg, is therefore added to adjust the ratio to 0.4.
[0187] Finally, 40 mL (pH 1.3) of the obtained impregnation solution was used to impregnate 10 g of alumina support via an over-impregnation method at ambient temperature for 3 hours. After aging at ambient temperature in a humid atmosphere for 16 hours and drying at 120°C for 2 hours, the composition of the obtained recycled catalyst was 1.1% by weight of MoO3, 3.6% by weight of CoO, and 3.3% by weight of P2O, containing 100% recycled Mo.
[0188] Catalysts manufactured in this way from recycled metals exhibit performance levels substantially equivalent to those of fresh catalysts that do not contain recycled metals. [Brief explanation of the drawing]
[0189] [Figure 1] This diagram shows a block diagram of a first-choice configuration of equipment for carrying out the method according to the present invention. [Figure 2] This diagram shows a block diagram of a second-choice configuration of equipment for carrying out the method according to the present invention.
Claims
1. A method for the preparation of a recycled catalyst comprising at least one metal M1 from group VIB and / or at least one metal M2 from group VIII, optionally phosphorus and / or sulfur, and one or more oxide-based supports, characterized in that it comprises the recycling of at least a portion of the metal or metals of a source catalyst comprising the metal M1 and / or the metal M2 common to the recycled catalyst to be prepared, - extracting the metal M1 and / or metal M2 from said source catalyst with an extraction solution to obtain a solution of extracted metal(s), then impregnating the support with the impregnation solution resulting from said solution of the extracted metal or metals to obtain an impregnated substrate; wherein said extracted one or more metals remain in the liquid phase from extraction to impregnation.
2. 2. The method of claim 1, wherein the extraction solution and the impregnation solution have at least one solvent in common.
3. 3. The method according to claim 1 or 2, characterized in that the extraction solution and the impregnation solution are in an acidic medium.
4. 4. The method according to claim 3, characterized in that the extraction is carried out with a solution comprising a solvent, in particular an aqueous solvent, and at least one organic compound having complexing properties and possibly also acid properties.
5. 5. The method according to claim 4, characterized in that the extraction solution contains an inorganic acid, in particular phosphoric acid, nitric acid or boric acid.
6. 6. The method of claim 5, wherein the organic compound comprises one or more chemical functional groups selected from carboxylic acid, phosphate, sulfonic acid, alcohol, thiol, thioether, sulfone, sulfoxide, ether, aldehyde, ketone, ester, carbonate, amine, nitrile, imide, oxime, urea and amide groups, or a compound containing a furan ring, or a sugar.
7. The method according to any one of claims 4 to 6, characterized in that the organic compound is selected from at least one of the following compounds: formic acid, acetic acid, oxalic acid, malonic acid, glutaric acid, glycolic acid, lactic acid, tartronic acid, citric acid, tartaric acid, pyruvic acid, γ-keto valeric acid, succinic acid, acetoacetic acid, gluconic acid, ascorbic acid, phthalic acid, salicylic acid, maleic acid, malic acid, fumaric acid, acrylic acid, thioglycolic acid, 2-hydroxy-4-methylthiobutanoic acid, glutamic acid, N-acetylglutamic acid, alanine, glycine, cysteine, histidine, aspartic acid, N-acetylaspartic acid, 4-aminobutanoic acid, 1,2-cyclohexanediaminetetraacetic acid, ethylene ... ethylenediaminetetraacetic acid (EDTA), nitrilotriacetic acid (NTA), iminodiacetic acid (IDA), N-(2-hydroxyethyl)ethylenediamine-N,N',N'-triacetic acid (HEDTA), diethylenetriaminepentaacetic acid (DTPA), bicine, tricine, 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP or etidronic acid), nitrilotris(methylenephosphonic acid), diethylenetriaminepentakis(methylenephosphonic acid), 4-sulfophthalic acid, 3-(N-morpholino)-2-hydroxy-1-propanesulfonic acid (MOPSO), 2-(4-pyridinyl)ethanesulfonic acid, phenol-4-sulfonic acid, thiodiacetic acid, and diglycolic acid.
8. The method according to any one of claims 4 to 6, characterized in that the organic compound is selected from at least one of the following compounds: dimethylglyoxime, methyl acetoacetate, ethyl acetoacetate, ethyl lactate, methyl glycolate, ethyl glycolate, dimethyl malate, diethyl malate, dimethyl tartrate, diethyl tartrate, ethyl 3-hydroxybutanoate, ethyl 3-ethoxypropanoate, methyl 3-methoxypropanoate, methyl 3-(methylthio)propanoate, ethyl 3-(methylthio)propanoate, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol (molecular weight is 200 to 1500 g / mol), propylene glycol, glycerol, 2-butoxyethanol, 2-(2-butoxyethoxy)ethanol, 2-(2-methoxyethoxy)ethanol, triethylene glycol dimethyl ether, crown ether, acetophenone, 2,4-pentanedione, pentanone, glucose, fructose, sucrose, sorbitol, xylitol, mannitol, γ-valerolactone, propylene carbonate, octylamine, N,N-diethylformamide, N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, propanamide, 1-methyl-2-pyrrolidinone, tetramethylurea, N,N'-dimethylurea, acetonitrile, lactamide, furfurol, 2-furaldehyde, 5-hydroxymethylfurfural, ethyl 3-hydroxybutanoate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidinone, N,N,N',N'-tetramethyltartaric acid amide, 3-hydroxypropionitrile, and N,N'-bis(2-hydroxyethyl)ethylenediamine.
9. 9. The method according to any one of claims 4 to 8, characterized in that the concentration of each organic compound or compounds in the extraction solution is defined in such a way that the molar ratio organic compound / extracted metal or metals is between 0.2 and 25, preferably between 0.2 and 11, preferably between 0.2 and 5, preferably between 0.4 and 2, suitably between 0.4 and 1.2, for the organic compound or for each of the organic compounds.
10. The method according to any one of claims 1 to 9, characterized in that the recycling comprises at least one stage of treatment of the source catalyst prior to extraction by the liquid route, chosen from at least one of the following treatments: decoking, separation of contaminant / impurity type compounds, mechanical comminution.
11. The method according to any one of claims 1 to 10, characterized in that the recycling comprises at least one stage of treatment of the solution of the extracted metal or metals, prior to impregnation, chosen from at least one of the following treatments: concentrating, diluting, modifying the composition of the solution by complete or partial addition or removal of at least one compound.
12. 12. The method according to claim 1, wherein the impregnation of the support is carried out starting from a solution of the extracted metal or metals, a supply of at least one of the metals M1, M2, optionally a supply of phosphorus, and optionally a supply of one or more organic additives.
13. 13. A method according to any one of the preceding claims, comprising a step of sulphurising the impregnated substrate.
14. 14. The method according to any one of claims 1 to 13, characterized in that at least a part of the impregnation solution is reused after impregnation of the support, in particular as a make-up for the extraction solution.
15. 15. The method according to any one of the preceding claims, characterized in that the solution of the extracted metal(s) is concentrated and at least a part of the solvent and, optionally, at least a part of the optional organic compound(s) it contains is extracted therefrom, and at least a part of the solvent / organic compound(s) thus extracted is reused as make-up for the extraction solution.
16. A method according to any one of claims 1 to 15, characterized in that it comprises the steps of: - at least one stage (a1, a2, a3) of treatment of the source catalyst, - (b) extracting said source catalyst with an extraction solution of one or more metals; obtaining a solution of the extracted one or more metals; at least one optional step (c) of purification of the solution of extracted metal(s) resulting from step (b); extracting therefrom all or part of possible impurities, - at least one optional step (d) of concentrating the solution of the extracted metal or metals, at least one optional step (e) of adjusting the composition of the solution of extracted metal(s) resulting from step (b), (c) or (d), - impregnation (f) by liquid route of the support with an impregnation solution resulting from said solution of extracted metal(s) obtained in step (b), (c), (d) or (e), with optional supplementation of metal(s), phosphorus and one or more organic additives; obtaining an impregnated substrate, said extracted metal(s) remaining in the liquid phase from extraction to impregnation, - optional sulfurization (g) of the impregnated support obtained in step (f).
17. 17. The method according to any one of claims 1 to 16, wherein the source catalyst is a spent catalyst that has previously been regenerated or reactivated.
18. 18. The method according to any one of the preceding claims, characterized in that the support impregnated with the impregnation solution resulting from a solution of the extracted metal or metals is pre- or post-impregnated with the impregnation solution or is a metal-depleted catalyst of the spent catalyst type, possibly regenerated / reactivated.