Powder for ceramic shaping, ceramic shaped article, and method for manufacturing the same
Patent Information
- Application Number
- JP2023190897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-07-14
- Filing Date
- 2023-11-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2038-07-10
AI Technical Summary
Ceramic modeling faces challenges in achieving uniform melting and high precision due to light diffusion in powder beds, leading to non-uniform sintered regions and reduced modeling accuracy, especially with laser wavelengths like Nd:YAG (approximately 1 μm), which do not show clear absorption in materials like Al2O3-ZrO2 eutectic systems.
Incorporating a ceramic modeling powder with a composition that includes an absorber with relatively higher absorption to laser light, which changes into a composition with lower absorption post-irradiation, reducing light diffusion and enhancing modeling accuracy by local heating and minimizing reabsorption effects.
The use of this powder enables high molding accuracy by reducing light diffusion and reabsorption, resulting in narrow sintered areas and improved precision in ceramic objects.
Smart Images

Figure 00000022_0000 
Figure 00000022_0001 
Figure 00000022_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder used in forming a ceramic object by laser irradiation and a manufacturing method using the powder. [Background technology]
[0002] In recent years, additive manufacturing technology has developed, and in the metal field in particular, powder bed fusion has produced dense and diverse objects. The denseness is due to the fact that the object is obtained as a solidified structure by effectively melting it. In this situation, the possibility of applying this technology to ceramics molding has also been discussed, and many efforts have been reported. In order to melt ceramics in the same way as metals, a certain amount of energy must be input, but unlike metals, light diffusion within the powder makes it difficult to achieve uniform melting, making it difficult to obtain molding accuracy. For this reason, objects were formed by sintering without melting in order to ensure molding accuracy, but they lacked density.
[0003] In this situation, for example, in Non-Patent Document 1, 2 O 3 -ZrO 2 A method has been proposed in which the melting point is lowered by using a eutectic system, and when melted and solidified, a microstructure specific to the eutectic system is formed, realizing high mechanical strength. However, although this method succeeded in improving the density of the molded object, numerous protrusions were generated on the surface of the molded object, and the molding precision was not sufficient. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Physics Procedia 5 (2010) 587-594 Summary of the Invention [Problem to be solved by the invention]
[0005] The wavelength of the laser light is Nd:YAG (approximately 1 μm), and even if the melting point is reduced in the eutectic system, the Al 2 O 3 ZrO 2 Since the material does not show clear absorption, a certain amount of energy is required to melt and solidify the material system. In such a system, light diffusion occurs in the powder, which causes problems such as uneven melting in the desired shaped area and uneven sintering in a wide area around it.
[0006] Furthermore, there was a problem that areas where the process had already been completed, such as nearby areas during laser scanning or in the stacking direction, could be processed again due to the absorption of laser light, which could have a negative impact on the accuracy of the modeling.
[0007] Therefore, in order to improve the molding accuracy, there was a need for a material that could suppress light diffusion in the powder, absorb the laser wavelength, and reduce or eliminate the absorption effect in areas that had already been molded so as not to be affected by re-absorbing the laser light. [Means for solving the problem]
[0008] The ceramic molding powder of the present invention is a ceramic molding powder for obtaining a molded object by repeatedly successively sintering or melting and solidifying the powder in the laser light irradiated area, characterized in that the powder contains a plurality of compositions, at least one of the compositions is an absorber that exhibits relatively higher absorption of the laser light than other compositions, and at least a portion of the absorber is changed to another composition that exhibits relatively lower absorption of the laser light upon irradiation with the laser light.
[0009] In addition, in the manufacture of a ceramic object by repeatedly sintering or melting and solidifying powder in an irradiated area of a laser beam, (i) placing the ceramic shaping powder in a laser irradiation section; (ii) irradiating the powder for ceramics molding with a laser based on three-dimensional modeling data, thereby sintering or melting the powder for ceramics molding and then solidifying it; and (iii) repeating steps (i) and (ii) to produce a shaped object; The present invention is characterized by having the following. Effect of the Invention
[0010] When the ceramic shaping powder of the present invention is used, a part of the absorber changes to another composition that has a relatively low absorption of the laser light upon irradiation with a laser beam, so that the region after sintering or melting is less susceptible to the effects of the laser irradiation during subsequent shaping. In addition, the absorber has a relatively higher absorption of the laser beam than the other compositions that make up the powder, so light diffusion can also be reduced. As a result, it is possible to manufacture a ceramic shaped object with high shaping accuracy. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing an example of a molding apparatus to which the powder of the present invention can be applied. [Diagram 2] FIG. 13 is a diagram showing another example of a molding apparatus to which the powder of the present invention can be applied. [Diagram 3] FIG. 2 is a conceptual diagram showing the temperature rise process of a powder containing the absorbent of the present invention and a reference powder not containing the absorbent. [Figure 4] FIG. 13 is a diagram showing the measurement results of the amplitude of the contour of the boundary between a laser irradiated region and a non-irradiated region. [Diagram 5] FIG. 2 is a diagram showing a process of irradiating the powders of Examples 8 to 25 of the present invention with laser light. [Figure 6] FIG. 2 is a diagram showing objects formed using the powders of Examples 8 to 25 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiment for carrying out the present invention will be described with reference to the drawings. First, the powder, composition, and absorber in the present invention will be described. The powder is an aggregate of particles that can be recognized as isolated grains. The powder is composed of a plurality of compositions. The composition is composed of a plurality of components (elements or compounds). The powder is composed of a plurality of compositions means that many types of particles made of one type of composition are mixed, or one type or many types of particles made of multiple types of compositions are mixed. The absorber is defined as a composition that has a relatively high absorption capacity for the laser light used compared to other compositions that make up the powder. In other words, the absorber has the highest absorption capacity for laser light among the compositions contained in the powder. At least one composition that makes up the powder of the present invention is an absorber that has the ability to absorb laser light. The absorption capacity of the absorber is preferably 10% or more for the laser light of the wavelength used. It is more preferable that the absorption rate is 40% or more, and most preferably 60% or more. The absorptance of the absorber alone can be measured using a general spectrometer, and an integrating sphere is used to irradiate the absorber alone filled in a sample dish with light of the expected wavelength (near the laser wavelength used in manufacturing) and measure it. The absorptance is calculated from the ratio of the data without the sample as the reference data.
[0013] (powder) The powder of the present invention is composed of two or more types of compositions, and the compositions include at least one type of composition that is an absorbent. Each particle constituting the powder may be composed of a single composition, or one particle may be composed of multiple compositions. The cases are divided and explained in order below.
[0014] First, the powder is composed of particles of a single composition. For example, multiple compositions may be present, such as Al 2 O 3 , ZrO 2 , Tb 4 O 7 (absorber), Al 2 O 3 Particles, ZrO 2particles, Tb 4 O 7 An example of such a state is when each type of particle exists and the powder is made up of a mixture of these particles.
[0015] Next, the powder contains particles composed of two or more compositions. For example, the composition is Al 2 O 3 , ZrO 2 , Tb 4 O 7 (absorber), Al 2 O 3 -ZrO 2 -Tb 4 O 7 A state in which the particles consist only of Al 2 O 3 -ZrO 2 particles, Tb 4 O 7 As the particle, Al 2 O 3 -ZrO 2 In particular, when the absorbent is contained in the same particle as another composition, the absorbent of the present invention is an example of the absorbent of the present invention. 4 O 7 In the case of Tb 4 O 7 Furthermore, it is preferable that the composition serving as the absorbent is in a state where it constitutes particles by itself, regardless of how the other compositions are constituted.
[0016] In addition, for the powder of the present invention, the fluidity of the powder is important when forming a powder bed layer using a recoater in the powder bed fusion method, or when spraying powder from a nozzle in the cladding method. It is preferable to use a powder that satisfies a fluidity index of 40 [sec / 50g] or less. In order to ensure fluidity, it is preferable that the particles are spherical. However, as long as the above fluidity index is satisfied, it is not essential that the particles are spherical.
[0017] Furthermore, the particle size of the composition constituting the absorbent (the particle size is not that of a single particle but the median value of a group of particles having the same composition) is preferably 1 / 5 or less of the particle size of the composition other than the absorbent. Therefore, since the particle size of the particles constituting the absorbent is preferably 1 μm or more and 10 μm or less, it is important that the particle size of the composition other than the absorbent is 5 μm or more to satisfy the above condition.
[0018] In addition, the powder of the present invention preferably does not contain a resin binder. If a resin binder is contained, a process of explosive burning may occur due to laser irradiation, which may cause voids and the like to be present in the modeling region. Furthermore, if carbon is contained, it will combine with oxygen to become gas, and the volume occupied by the carbon component may become voids, so it is preferable that the carbon content is small. Therefore, the carbon content is preferably 1000 ppm or less in molar ratio with respect to the metal elements of the multiple compositions constituting the powder. Furthermore, if carbon is contained, it will oxidize and gasify upon laser irradiation, which will have a detrimental effect on shaping, so it is preferable that it is incorporated into the shaped object, as in the absorber of the present invention, and changes into a different composition upon laser irradiation.
[0019] Although the absorber, composition, and particles have been described so far, the powder for ceramic molding in the present invention does not matter whether it is in a crystalline or amorphous state, or a mixture thereof. In addition, the composition does not need to be completely the same between the powder and the molded object, and differences in particular in the oxidation state and nitridation state may be acceptable. Therefore, it is also preferable to control the atmosphere during the molding process, and it is preferable to use not only an air atmosphere, but also an inert state such as a nitrogen or other rare gas atmosphere, a state that is easily reduced by partially containing hydrogen or reducing pressure, or even an oxygen atmosphere. By controlling the atmosphere in this way, it is not excluded to include a composition in a partially metallic state as the raw material powder.
[0020] Although the present invention is a powder for ceramic molding, it is not limited to a state in which the molded object is composed of 100% crystalline ceramics. As long as the desired physical properties are obtained, a part or majority of the molded object may contain amorphous regions or regions that have been reduced to a metallic state.
[0021] (Absorbent) The absorber suitable for the present invention absorbs the laser light, and converts the powder at the irradiated portion of the laser light into a solidified body by sintering or melting it with the heat of the laser light, and the absorber itself remains in the molded object. At that time, a part of the absorber changes to another composition having a relatively low absorption ability for the laser light, and is incorporated into the molded object. Therefore, the area converted into the solidified body has a lower absorption of the laser light than when it was a powder before the irradiation of the laser light.
[0022] The action and effect of the absorbent body of the present invention will now be described in detail. The first effect is that as an absorber, it efficiently absorbs the laser light used during manufacturing, and by heating itself up, it spreads to other compositions present within an area equivalent to the focal size of the laser light, causing an increase in temperature. This realizes effective local heating, and clarifies the interface between the process area (area irradiated with laser light) and the non-process area (area not irradiated with laser light), improving modeling accuracy.
[0023] The second effect is that the area where the modeling process is completed by irradiating the laser light has low absorption, so that adjacent areas and areas below the area where the process is about to be performed can be prevented from absorbing the laser light again and becoming altered. In addition, since the influence on adjacent areas and areas below that have already been modeled is suppressed, a wide process margin can be set for the laser irradiation conditions, and the adverse effect on modeling accuracy due to fluctuations in the irradiation conditions can be reduced.
[0024] When the ceramic shaping powder of the present invention is used to perform shaping by selective irradiation with laser light, shaping with high precision can be achieved due to the above-mentioned first and second effects.
[0025] Such a situation will be explained with reference to the conceptual diagram of FIG. 3. The horizontal axis indicates the laser irradiation time, and the vertical axis indicates the temperature of the laser irradiation area. In lines A and B in FIG. 3, line A indicates the characteristics of a powder that does not contain an absorbent. In line A, the temperature starts to rise due to laser irradiation, and the powder melts linearly beyond the melting point, and reaches the molding temperature indicated by the dashed line. On the other hand, line B indicates the characteristics of a powder that contains the absorbent of the present invention. In line B, the temperature starts to rise rapidly due to the light absorption effect of the absorbent due to laser irradiation, and the effect of the absorbent decreases just before melting, resulting in a temperature rise rate similar to that of line A when no absorbent is contained.
[0026] Powders that exhibit the characteristics of line A have poor heating efficiency, and a wide, low-density sintered area is formed at the boundary between the powder and the melted and solidified part in the area irradiated by the laser light, which has a wide effect on the adjacent powder parts, making it impossible to achieve spatial modeling precision.
[0027] On the other hand, powders that exhibit the characteristics of line B have good heating efficiency and can achieve localized heating. Therefore, when a laser irradiation area is formed, the temperature difference with the adjacent area is sufficiently ensured, so that only a narrow sintered area is generated at the boundary between the molten and solidified part and the powder, and good molding accuracy is obtained. Furthermore, since the finished part of the model after the laser irradiation does not absorb and exhibits characteristics like line A, even if the process conditions change and the laser light affects the existing modeling area, the temperature rise due to the laser light is relatively small, and the influence can be avoided. In addition, the area being irradiated with the laser and the area that has already been irradiated are bonded by fusion due to thermal conduction between the two areas, so the connection and strength of the boundary between the laser-drawn lines are maintained. In this way, when the characteristics of line B of the present invention are present, the two effects described above can be obtained.
[0028] The absorber of the present invention can be any material that changes at least partially into another composition with relatively low absorption upon laser irradiation, but is preferably selected from metal oxides. This is because some metal oxides change the valence of the metal element due to the release of oxygen as the temperature rises, and change into another metal oxide with relatively low absorption of laser light (for example, Tb 4 O 7 →Tb 2 O 3 , Tb 3+ GdAlO 3 This is because there are some that are prone to undergoing substitutions (such as substitution of the Gd (gadolinium) site in the SiO2 site). In addition, they have a high affinity with other components that make up the ceramics, making it possible to incorporate them into objects.
[0029] Metal oxides in which a change in valence functions as a change in absorptivity for various laser wavelengths are preferably oxides of metals selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Hf, Ta, W, In, Sn, Bi, Ce, Pr, Sm, Eu, Tb, and Yb. For the Nd:YAG laser (1070 nm), which is a typical laser used for modeling, it is preferable to use oxides of Tb and Pr, and the oxidation state is Tb. 4 O 7 OrPr 6 O 11 However, the present invention is not limited to the above ratio (composition ratio) of the molecular formula, and other ratios or mixtures thereof may be used as long as the desired absorption effect is obtained.
[0030] Next, the most preferred terbium oxide as the composition of the absorber of the present invention will be described in detail as an example. Terbium oxide can take various forms, and a representative example is Tb 4 O 7 This state and Tb 2 O 3 The molecular formula is Tb 4 O 7 However, it is not limited to being strictly 4:7. In this case, Tb 4 O7 is Tb 4+ and Tb 3+ It is a material composed of half and half of Tb 2 O 3 So, Tb 3+ This consists of only Tb 4 O 7 The high infrared absorption rate of Tb is remarkable around 1070 nm of Nd:YAG laser, exceeding 60% and sometimes reaching 70%. 4+ As the absorption rate decreases, the Tb 3+ Tb consisting of only 2 O 3 In this state, it is about 7%. 4+ Since it is clear that the absorption rate decreases with the decrease in 4 O 7 ) is a suitable composition for realizing the present invention.
[0031] In addition, to obtain an absorption rate of 10% (when measured with the absorber alone), Tb 4+ is Tb 3+ and Tb 4+ It is sufficient that the amount of valence is about 10% of the total amount. Here, X-ray Absorption Fine Structure (XAFS) can be applied as a method for evaluating the valence. Since the rising energy of the absorption edge differs for each valence, it can be evaluated from the ratio. In addition, evaluation can be performed by making full use of general evaluation methods such as X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectroscopy or ESCA: Electron Spectroscopy for Chemical Analysis) and electron spin resonance (ESR).
[0032] In addition, in oxides with a metal element to oxygen ratio of 2:3, the metal element is stabilized with a valence of 3+, so after conversion to a solid, it is possible to obtain other compositions (for example, Y 2 O 3 or Gd 2 O 3 , Other R 2 O3 (R: metallic element)) in a solid solution state. Therefore, the area that has been converted into a solidified body after molding does not show a large absorption. 3+ In compounds where is stable, the same state can be achieved by substituting Tb for the R site. 2 In this case, it is dissolved and contributes to stabilizing the fluorite structure, and the valence is also 3+. In this way, the absorbent of the present invention also functions as a material for forming a shaped object.
[0033] In order to obtain the effects of the present invention, it is preferable that the difference in absorptance between before and after the process by irradiation with laser light is 1.2 times or more, and more preferably 2 times or more. Alternatively, it is preferable that the absorptance is 50% or more before the process and 40% or less after the process. Alternatively, it is preferable that the absorptance is 60% or more before the process and 20% or less after the process. Tb, which is an example of an absorber, 4 O 7 It is preferable to achieve this condition by using the composition. Note that this absorption rate is for the absorbent body alone.
[0034] The absorbent can have its effect if it is contained in multiple compositions, but it is more preferable that the absorbent composition is contained in the powder at 0.5 vol% to 53 vol%. Here, vol% is used because it is important to know how much area the absorbent occupies relative to the irradiation size (focus size) of the laser light, and if the composition that makes up the powder changes, the mol% expression cannot be used.
[0035] The above lower limit of the absorber content is determined by the necessity of containing at least one particle of the absorber within the laser focus size. The upper limit is determined by the effect on the main composition constituting the shaped object. When the laser focus size is 10 μm, the melted region of the laser can be regarded as a hemisphere with a diameter of 10 μm, and the state in which one particle of the absorber with a diameter of 1 μm exists in that region is about 0.5 vol%, so the lower limit of the absorber composition is preferably 0.5 vol% or more.
[0036] In addition, the upper limit is based on the general-purpose Al as a structural ceramic. 2 O 3 In contrast, Tb 4 O 7 When Tb is added, 3 Al 5 O 12 Al is formed. 2 O 3 Taking advantage of the properties of ceramics, Tb 3 Al 5 O 12 To construct a composite system with Tb 4 O 7 In this case, Tb 3 Al 5 O 12 The main phase contains a small amount of Al. 2 O 3 Since a state in which the content of Mn is dispersed at the grain boundaries is realized, the upper limit is preferably 53 vol%.
[0037] The particle size of the absorbent is also important, and is preferably 10 μm or less, more preferably 1 μm to 10 μm, and most preferably 1 μm to 5 μm. Here, the particle size in the present invention specifies the range of the median particle size distribution of particles made of the same composition, and does not mean that particles with particle sizes outside the range are not included. Furthermore, the measurement of particle size is applied not only to particles in a single crystal state, but also to particles in a polycrystalline state and an aggregated state. The composition that is the absorbent may be composed of particles in a single unit.
[0038] In the case where the absorbent composition is composed of particles by itself, when the absorbent is contained at 0.5 vol%, the particle size is 1 μm, and the packed bulk density of the powder layer is 50% of the true density, a laser focal size of 10 μm corresponds to a state in which one particle is contained within the heated area (hemispherical volume consisting of the focal size diameter), and the absorbent effect is obtained. In addition, when the particle size is 10 μm, a laser focal size of 100 μm corresponds to a state in which one particle is contained within the heated area, so it is important to select the particle size of the absorbent according to the laser focal size.
[0039] From the viewpoint of uniformity, it is more preferable that at least two or more absorber particles are included within the laser focus size. The particle interval between each absorber is preferably 100 μm or less, and more preferably 50 μm or less. It is also preferable to adjust the laser focus size so that such a situation can be realized. As described above, assuming that the laser focus size is up to 100 μm from the viewpoint of modeling accuracy, it is preferable that the particle size of the absorber is 1 μm or more and 10 μm or less as described above. However, the laser focus size may be 100 μm or more according to the desired modeling accuracy.
[0040] On the other hand, from the viewpoint of ensuring the fluidity of the powder, it is desirable that the median value of the particle size distribution of the particles of the composition that is the base material of the shaped object and is not the absorbent is 5 μm or more and the shape is spherical. In addition, the particle size of the absorbent is in the range of 1 μm to 10 μm, but it is preferable that the particle size is as small as possible. This is from the viewpoint of the dispersibility of the absorbent in the powder and high packing density. In addition, in the present invention, the particle size of the absorbent is preferably 1 / 5 or less of the particle size of the composition other than the absorbent.
[0041] (Composition other than absorbent) The composition other than the absorber is a composition that is the main component of the ceramic structure. Since such a composition greatly contributes to the properties such as strength of the final product, it should be selected appropriately according to the application. Therefore, by determining the absorber for the wavelength of the laser light used in the production, it is preferable to select one or more main components from metal oxides with relatively low absorption effect, and it is also preferable to select their compounds or mixtures. In particular, aluminum oxide and zirconium oxide (stabilized / semi-stabilized) can be used as general-purpose structural ceramics. Furthermore, silicon oxide, silicon nitride, and aluminum nitride can also be used. Although silicon nitride exhibits a laser absorption effect, its absorptivity does not change before and after the process, so it does not function as an absorber in the present invention. Furthermore, cordierite (2MgO·2Al2 O 3 5SiO 2 ), zircon (ZrO 2 SiO 2 ), Mullite (3Al 2 O 3 2SiO 2 It is also possible to select ceramic materials such as tantalum oxide, yttrium oxide, aluminum titanate, etc. Also, a mixture of the above materials may be used.
[0042] The main composition may further contain small-sized silicon oxide particles having a particle size of less than 5 μm. The function of the silicon oxide particles will be described in detail below.
[0043] When the powder for ceramic molding is irradiated with a laser beam, the absorber in the irradiated area absorbs the energy and generates heat. Since small-diameter silicon oxide has a small particle size of less than 5 μm and is easily melted, the heat of the absorber first melts the small-diameter silicon oxide particles present around the absorber. The melted small-diameter silicon oxide particles then transfer heat to other relatively large-diameter particles, which melt. The small-diameter silicon oxide particles melted in the area irradiated with the laser beam soften and deform, contacting other relatively large-diameter particles over a wide area and efficiently transferring heat to the particle surfaces. This allows heat to be transferred more evenly to other relatively large-diameter particles compared to when the powder does not contain small-diameter silicon oxide particles. As a result, the temperature distribution in the powder for ceramic molding during melting is reduced, and the cooling rate during solidification is uniform depending on the location. This reduces thermal stress, suppresses the occurrence of microcracks during solidification, and results in a ceramic molded product with fewer microcracks. Another effect is that when a silicon oxide component is contained in the powder or forms a compound with another composition that is the main component during solidification, the thermal conductivity becomes relatively low, rapid cooling during solidification is mitigated, and the occurrence of microcracks is suppressed. Ceramic shaped objects with few microcracks have high mechanical strength and low water absorption, making them applicable to components that require strength and low water absorption, such as vacuum device parts.
[0044] As mentioned above, the particle size of the small-diameter silicon oxide particles is smaller than that of the particles of other compositions, and the diameter is preferably less than 5 μm. When the powder is composed of multiple types of particles, the particle size of the small-diameter silicon oxide particles is preferably smaller than that of each of the multiple types of particles. This is because the small particle size makes it easier to lead the melting together with the absorber, and the softened small-diameter silicon oxide particles are distributed more evenly than other particles, so that the temperature distribution in the powder for ceramic molding during melting can be further reduced. The small-diameter silicon oxide particles are preferably spherical from the viewpoint of fluidity, but may be anisotropic shapes such as amorphous, plate-like, and needle-like. The small-diameter silicon oxide particles preferably have a narrow particle size distribution. This is because the uniform particle size allows them to be uniformly dispersed in the powder for ceramic molding, and when softened, they can be distributed more uniformly on the surface of the particles of other compositions.
[0045] The mass of small-diameter silicon oxide particles contained in the powder for ceramic shaping is preferably 0.04% or more and 5.0% or less with respect to the mass of the absorber particles. 2 The inclusion of particles is desirable because it reduces the water absorption rate to 1.0% or less.
[0046] In addition, when the mass of the small-diameter silicon oxide particles is 5.0% or less relative to the mass of the absorber particles, almost all of the small-diameter silicon oxide particles present between the particles of the composition as the main component are melted. This is more preferable because no unmelted residue that may reduce the mechanical strength of the ceramic molded product is generated. In addition, after the small-diameter silicon oxide particles are melted by irradiation with laser light and play the role of a heat transfer medium, some of them become glass and are distributed on the surface and inside of the ceramic molded product. If a large amount of small-diameter silicon oxide particles are contained in the powder when the powder for ceramic molding solidifies, many glass regions originating from the small-diameter silicon oxide particles are formed in the ceramic molded product, which may reduce the mechanical strength of the ceramic molded product. Therefore, it is more preferable that the mass of the small-diameter silicon oxide particles is 1.0% or less relative to the mass of the particles consisting of the composition as the main component.
[0047] The powder of the present invention is composed of a plurality of compositions, and preferably contains at least one component as an absorber and at least one component of aluminum oxide, zirconium oxide, or silicon oxide as a main component forming a ceramic structure. Aluminum oxide, zirconium oxide, and silicon oxide are preferable because they have a lower absorption capacity than the absorber, and they form eutectic systems with many materials, and by expressing their microstructure, they can maintain high strength and also obtain the effect of lowering the melting point. For example, in aluminum oxide, the absorber Tb 4 O 7 When the two types are mixed, Tb 4 O 7 With a change from Tb 3 Al 5 O 12 and TbAlO 3 On the other hand, in zirconium oxide, Tb 3+ In this state, it plays a role in stabilizing zirconium oxide in a tetragonal state. It is also preferable that aluminum oxide and zirconium oxide are simultaneously included in the composition, and that the absorber is composed of three components. 2 O 3 :ZrO 2 It is also possible to select a ratio of 85:15wt% or 70:30wt%. It is preferable that the silicon oxide is configured as a shaped object regardless of whether it is amorphous or crystalline. Furthermore, it is preferable that the silicon oxide is configured as a 3-component or 4-component composition including zirconium oxide, aluminum oxide, etc., in addition to a 2-component composition with an absorber. Furthermore, the shaped object containing silicon oxide may contain zircon, mullite, silicate with an absorber, etc.
[0048] Although not limited in the present invention, it is preferable that the plurality of compositions are contained in a relationship that forms a eutectic composition. The eutectic composition is the composition at the eutectic point shown in the eutectic phase diagram, but the shaping process using the laser beam of the present invention is significantly far from the equilibrium state because heating and cooling states are repeated very quickly. Therefore, it is more preferable to define the eutectic composition as the composition range in which a eutectic structure is formed, and a range of ±10 mol% from the eutectic composition in the eutectic phase diagram is allowed.
[0049] Next, preferably, at least one rare earth oxide that is not an absorber is included. The metal element of the rare earth oxide is preferably selected from Sc, Y, La, Ce, Nd, Sm, Eu, Gd, Dy, Ho, Er, Tm, Yb, and Lu. In this case, depending on the composition, R 2 O 3 (In some cases, RO 2 ) for RAlO 3 Or R 3 Al 5 O 12 In some cases, it is also preferable that the composition is a eutectic composition. 3+ ,Pr 3+ A material system consisting of the above is also applicable.
[0050] (Use of the ceramic molding powder of the present invention) The ceramic shaping powder of the present invention is used in a manufacturing process (manufacturing method) of a shaped object by irradiation with a laser beam. The manufacturing process includes the steps of (i) arranging the ceramic shaping powder of the present invention in a laser beam irradiation area, (ii) irradiating the ceramic shaping powder with a laser beam based on three-dimensional modeling data to sinter or melt the ceramic shaping powder and then solidifying it, and (iii) repeating the steps (i) and (ii) to form a shaped object.
[0051] The terms "sintering" or "melting and solidifying" in the present invention are not unique in that they mean sintering when no powder is melted, and melting when no powder remains. Recently, the term "liquid phase sintering" has also been used, and the boundaries between these terms have become unclear. Therefore, the terms "sintering" do not exclude sintering that only bonds powders together, liquid phase sintering in which molten material exists surrounding the powders, and even melting in which some powder remains unmelted.
[0052] In the manufacturing process of the present invention, it is also preferable to carry out a heat treatment after the step of forming the shaped object, if necessary. In this case, there is no limitation on the heating means, and it is possible to select and use a resistance heating method, an induction heating method, an infrared lamp method, a laser method, an electron beam method, etc. according to the purpose. The heat treatment is also suitable for adjusting the crystal grain size of the shaped object in order to improve the density and strength of the shaped object. It is also preferable to impregnate or coat the shaped object with a glaze, whether organic or inorganic, during the heat treatment.
[0053] In the above-mentioned method of use of the present invention, the steps (i) and (ii) may be carried out by spreading the powder of the present invention evenly and then irradiating the powder with a laser beam. Also, the steps (i) and (ii) may be carried out by spraying the powder of the present invention at a predetermined location and irradiating the predetermined location with a laser beam.
[0054] Specifically, the method of obtaining a molded object by repeatedly sintering or melting and solidifying in the irradiated area of the laser light is called the powder bed fusion method or the cladding method. There is no limit to the wavelength of the laser light used, but it is preferable to use a lens or fiber adjusted to a desired focal size such as 10 μm to 2 mm. The focal size is one of the parameters that affect the molding accuracy, and in order to achieve a molding accuracy of 0.1 mm, it is preferable that the line width is about the same, depending on the situation, and the focal size is preferably 100 μm or less. It does not matter whether the laser light is irradiated continuously or in a pulsed form. One example is a Nd:YAG laser, with a wavelength of around 1070 nm.
[0055] The powder bed fusion method will be described with reference to Figure 1. The device used in this method includes a powder container 11, a modeling stage unit 12, a recoater unit 13, a scanner unit 14, and a laser light source 15. In operation, the powder container 11 and the modeling stage unit 12 move up and down as appropriate, while the recoater unit 13 manipulates the powder to spread it thinly and evenly over an area larger than the intended object. Furthermore, a cross-sectional shape of the object is directly drawn on the powder layer using a laser beam generated by the laser light source 15 and the scanner unit 14. The drawn area is sintered or melted and solidified, and this process is repeated to stack the cross-section of the object and form the final object.
[0056] The cladding method will be explained with reference to Fig. 2. This is a method in which powder is ejected from multiple powder supply holes 22 in a cladding nozzle 21, and a laser beam 23 is irradiated onto the area where the powder is focused, successively forming objects at desired locations, and is characterized by its ability to mold objects on curved surfaces.
[0057] According to the manufacturing process of the present invention as described above, it is possible to obtain a three-dimensional object with stable modeling and with assured modeling accuracy. EXAMPLES
[0058] [Example 1] This example relates to the improvement of molding accuracy by including the absorbent of the present invention. In order to clarify the difference in molding accuracy, a powder bed with a thickness of 1.5 mm was melted and solidified by irradiating it with a laser beam, and the state of the boundary between the irradiated and unirradiated areas of the laser beam was observed. 2 O 3 Powder, Gd 2 O 3 powder, Tb 4 O 7 Mixture of powder (composition ratio is Al 2 O 3 : 64.40vol%, Gd 2 O 3 : 32.73 vol%, Tb 4 O 7A powder bed of 1.5 mm thick was formed using a Nd:YAG laser (1070 nm) with a focal diameter of 100 μm and a laser power of 30 W. The laser light was irradiated at two different speeds, 100 mm / sec and 250 mm / sec, to irradiate 40 lines of 10 mm length with a 50 μm pitch.
[0059] In addition, Al was used as comparative sample 1. 2 O 3 Powder only, (GdTb)AlO 3 -Al 2 O 3 A single crushed powder consisting of a eutectic (the raw material composition ratio for forming the eutectic is Al 2 O 3 : 64.40vol%, Gd 2 O 3 : 32.73 vol%, Tb 4 O 7 %.: 2.87 vol%) was used, and laser light was irradiated in the same manner as in Sample 1.
[0060] An example of the absorber used here is Tb 4 O 7 is Tb 3+ Not only Tb 4+ The volume composition is calculated using the true density of Al. 2 O 3 :3.96[g / cm 3 ], Gd 2 O 3 :7.40[g / cm 3 ], Tb 4 O 7 :7.60[g / cm 3 Even if this true density is a slightly different value, the essence of the present invention is not affected.
[0061] Comparative sample 1 does not contain an absorber, and comparative sample 2 contains Tb in GdAlO 3 Gd 3+ It exists as a substitution at the Tb site. 4+There is almost no absorption effect, and the absorption effect has disappeared. In these two comparison samples without an absorber effect, the material remained almost in a powder state under the irradiation condition of 250 mm / sec laser light, and melted and then solidified structure was clearly obtained at 100 mm / sec. However, because there was no absorption effect, the heating state was largely non-uniform within the surface, and a two-dimensional surface was not obtained as a solidified object, and the solidified grains were melted locally and rolled around.
[0062] On the other hand, Sample 1 showed sufficient melting at 250 mm / sec, and it was confirmed that a two-dimensional object was formed in a planar shape. 4 O 7 GdAlO 3 Gd site on Tb 3+ Fluorescence observation with ultraviolet excitation confirmed that the tetravalent ions were incorporated into the powder, and the absorption effect reached a low state similar to that of comparative sample 2. In sample 1, the valence state of the absorber indicates that the powder was mixed with the powder at an absorption rate of 60% or more, and after irradiation with laser light, fluorescence observation showed that there was almost no tetravalent ions, resulting in an absorption rate of 30% or less. Furthermore, in comparative sample 2, fluorescence observation showed that the absorption rate was 30% or less from the powder state before molding, and there was no change after irradiation with laser light, remaining at 30% or less.
[0063] Figure 4 shows the results of calculating the deviation width of the outline of the boundary, cut out at a width of 3.83 mm from a micrograph of the boundary between the irradiated area 42 and the unirradiated area 41 of the laser light. The width was 391 μm for Comparative Sample 1, 273 μm for Comparative Sample 2, and 85 μm for Sample 1. In addition, since the post-printing area of Sample 1 and the powder of Comparative Sample 2 are in the same state in terms of the effect of the absorber, it was revealed that in Sample 1, the powder area where the absorber is functioning can be printed at 250 mm / sec, while the post-printing area has almost no effect at 250 mm / sec.
[0064] From the above results, it was found that the sample of the present invention had superior molding accuracy compared to the comparative sample, and a molded object could be obtained without disturbing the area where the process was completed.4 O 7 contains 4+ in its valence, but in the region after molding, the absorption characteristics changed due to a decrease in the valence to 3+. The conditions for irradiating the laser light are not limited to the values described in this example, since they are changed depending on the surrounding environment, material composition, powder layer thickness, etc.
[0065] [Example 2] In this example, Tb 4 O 7 The effect of adding Tb 4 O 7 has an absorption rate of 60% or more at around 1070 nm, and Tb 2 O 3 etc. 3+ In Example 1, sample 1 is made of Al 2 O 3 Powder, Gd 2 O 3 powder, Tb 4 O 7 Mixture of powder (composition ratio is Al 2 O 3 : 64.40vol%, Gd 2 O 3 : 32.73 vol%, Tb 4 O 7 In addition, samples 2, 3, 4, 5, and comparative sample 3 were prepared as shown in Table 1 below. 4 O 7 The particle size of the powder used was approximately 2 μm.
[0066] These powders are Al 2 O 3 After spreading the film evenly on the substrate to a thickness of about 20 μm, it was irradiated with a Nd:YAG laser under the following conditions: focal size 20 μm, 10 W, 50 mm / sec, 12 lines of 4.5 mm length with a 50 μm pitch.
[0067] [Table 1]
[0068] For each sample, the width of the boundary between the irradiated and unirradiated areas was observed within a range of 2 mm. The results are shown in Table 1. The table shows the blending amount (vol%) of each composition, the width of the boundary (μm), and the Tb 4 O 7 The effect of the addition is expressed as Excellent ◎, Good ○, or Poor ×. The width of the boundary (wave width) is an index that is essentially equivalent to the surface roughness of the side surface of the molded object, and the larger the width, the rougher the surface of the molded object produced. The standard surface roughness of objects manufactured using metal powder is said to be about 10-odd μm. Therefore, cases that are equivalent to this are rated as ◎. Other examples are also rated using the same criteria.
[0069] In the comparative sample 3, which does not contain an absorbent, many granular dissolved matter was generated at the boundary, and the width of the boundary was the widest. On the other hand, it was found that the width of the boundary was narrowed by adding an absorbent (samples 1 to 5). In other words, it is clear that the effect of including the absorbent of the present invention is obtained. In particular, it was confirmed that the width was narrower in samples 1 to 3. Therefore, it is possible to confirm that the width of the boundary was narrower in the comparative sample 3, which contains Tb, which is an example of an absorbent of the present invention. 4 O 7 When added, the evaluation results shown in Table 1 were obtained, and it was found that the effect of improving molding accuracy was obtained over a wide range of composition compared to the case where no additive was added.
[0070] [Example 3] In this example, Pr is one of the candidates for the absorber. 6 O 11 Regarding the effect of adding praseodymium oxide. 6 O 11 , and in a valence state close to that, the absorption rate is 80% or more at around 1070 nm, and Pr 2 O 3 Pr etc. 3+ When the state is high, the absorption rate is less than 50%. 2 O 3 Powder, Gd 2 O 3 Powder, Pr 6 O 11 Mixture of powder (composition ratio is Al2 O 3 : 63.85vol%, Gd 2 O 3 : 33.29 vol%, Pr 6 O 11 At this time, Pr 6 O 11 The particle size of the powder used was about 2 μm. The true density of Al was used for the volume composition calculation. 2 O 3 :3.96[g / cm 3 ], Gd 2 O 3 :7.40[g / cm 3 ], Pr 6 O 11 :7.20[g / cm 3 Even if this true density is a slightly different value, the essence of the present invention is not affected.
[0071] As in Example 2, these powders were 2 O 3 After spreading the film evenly on the substrate to a thickness of about 20 μm, it was irradiated with a Nd:YAG laser under the following conditions: focal size 20 μm, 10 W, 50 mm / sec, 12 lines of 4.5 mm length with a 50 μm pitch.
[0072] [Table 2]
[0073] The width of the boundary between the irradiated and unirradiated areas was observed over a range of 2 mm. The results are shown in Table 2. As shown in Table 2, the blending amounts (vol%) of each composition were as described above, and the width of the boundary was 42.7 μm, Pr 6 O 11 The effect of the addition was good.
[0074] It is shown that the width of the boundary portion is narrower than that of Comparative Sample 3 of Example 2, and Pr 6 O 11When added, the evaluation results shown in Table 2 were obtained, and it was found that the effect of improving the molding accuracy was obtained compared to the case where no additive was added.
[0075] [Example 4] This example concerns the effect of the absorbent on compositions other than the absorbent. The compositions examined are shown in Table 3. The volume composition was calculated using Al 2 O 3 :3.96[g / cm 3 ], ZrO 2 :5.68, Y 2 O 3 :5.01[g / cm 3 ], Tb 4 O 7 :7.60[g / cm 3 Even if this true density is a slightly different value, the essence of the present invention is not affected. Powders containing these compositions were 2 O 3 After spreading the material evenly on the substrate to a thickness of about 20 μm, the material was irradiated with laser light. The conditions were a focal size of 100 μm, 30 W, and scanning speeds of 50, 100, 200, and 500 mm / sec to draw two lines with a length of 4.5 mm and a pitch of 50 μm, and to compare the melting states.
[0076] [Table 3]
[0077] Comparative sample 4, pure Al 2 O 3 The pure ZrO in Comparative Sample 5 was melted and solidified in a line shape at a speed of up to 100 mm / sec, but the pure ZrO in Comparative Sample 5 was melted and solidified in a line shape at a speed of up to 500 mm / sec in Sample 7 to which an absorbent was added. 2 The sample 8, which had an absorber added, was capable of melting and solidifying in a line shape at speeds up to 100 mm / sec, but the speed was up to 500 mm / sec. 2 O 3 -ZrO 2Comparative sample 6, which is close to the eutectic composition of the system, was in a state where it could melt and solidify in a line shape up to 200 mm / sec, but sample 9, which had an absorber added, was capable of melting up to 500 mm / sec. Furthermore, the Al 2 O 3 -Y 2 O 3 Comparative sample 7, which had a eutectic composition close to the system, was in a state where it could melt and solidify in a line shape up to 200 mm / sec, but sample 10, which had an absorber added, was capable of melting up to 500 mm / sec.
[0078] From the above results, it is possible to determine whether Tb 4 O 7 As a result of adding the absorbent, it was confirmed that it was possible to melt and solidify the material at a faster scanning speed. Therefore, this absorbent can be used for any material, and contributes to improving the molding accuracy of the object.
[0079] [Example 5] This example relates to the 3D modeling property when an absorbent is contained. The particle sizes of the compositions constituting the powder used in this example are shown in Tables 4 and 5. The particles of these compositions are also Tb 4 O 7 ,Pr 6 O 11 All the other specimens were spherical.
[0080] [Table 4]
[0081] [Table 5]
[0082] Tables 6 and 7 show the volumetric compositions of the materials used. [Table 6]
[0083] [Table 7]
[0084] To calculate the volume composition, the true density is Al 2 O 3 :3.96[g / cm 3 ], ZrO 2 Y 2 O 3 :6.05[g / cm 3 ], Gd 2 O 3 :7.40[g / cm 3 ], Y 2 O 3 :5.01[g / cm 3 ], SiO 2 :2.20[g / cm 3 ], Tb 4 O 7 :7.60[g / cm 3 ], Pr 6 O 11 :7.20[g / cm 3 ], Al 2 O 3 ZrO 2 (85:15wt%):4.13[g / cm 3 ], Al 2 O 3 ZrO 2 (70:30wt%):4.46[g / cm 3 ], 2MgO 2Al 2 O 3 5SiO 2 :2.60[g / cm 3 Even if this true density is a slightly different value, the essence of the present invention is not affected.
[0085] In the study of this embodiment, a 3D systems ProX (trade name) series DMP100 was used as a modeling device. Comparative sample 8 not containing an absorbent, and samples 11 to 24 consisting of a plurality of compositions containing an absorbent were used to produce 6x6x6mm models under the modeling conditions shown in Table 8. The modeling properties were judged as follows: no shape: poor ×, roughness on the surface or side: slightly poor ◯, modeled objects according to the specified dimensions were obtained: good ◎. In addition, in all cases, the thickness of the powder layer was set to 20 μm, and an alumina plate was used as the base material. The thickness of the powder layer is the value at which the modeling stage part 12 in FIG. 1 is lowered, and the powder layer melts and shrinks in the thickness direction due to the irradiation of the laser light, so the apparent thickness of the powder layer gradually increases as the layers are repeatedly stacked, and converges to a range of 67 to 133 μm. Therefore, although the average particle size of the composition listed in Tables 4 and 5 is larger than the powder layer of 20 μm during modeling, this does not pose a problem in use. For the objects that could be molded, the surface roughness Ra was measured using Alpha-step (product name) manufactured by KLA Tencor Corporation to confirm the molding accuracy. Since the roughness was relatively larger on the side of the object than on the surface, the evaluation was performed on the side. The scan width during calculation was 1 mm.
[0086] [Table 8]
[0087] As shown in Table 8, in comparative sample 8, which does not contain the absorbent of the present invention, like comparative sample 1 in Example 1, although it partially dissolved, it was unable to maintain the shape of the object as a result of additive manufacturing. The other samples 11 to 24 were densely formed as additively molded objects, and the surface roughness of the side surfaces could be measured. The absorbent of the present invention improved the surface roughness, and in particular, it was possible to obtain molded objects with a roughness of around 10 μm, demonstrating that molding can be performed with high precision.
[0088] [Example 6] This example relates to the case where the composition other than the absorbent is a separate particle and the case where the composition is the same particle.2 O 3 and Gd 2 O 3 The eutectic powder (Al 2 O 3 and GdAlO 3 (mixture of Tb 4 O 7 and sample 15 and Al 2 O 3 and Y 2 O 3 The eutectic powder (Al 2 O 3 and Y 3 Al 5 O 12 (mixture of Tb 4 O 7 A comparison was made with a mixed sample.
[0089] As in Example 5, a ProX (product name) DMP100 from 3D Systems was used as the modeling device. A 6x6x6mm model was produced under the modeling conditions in Table 11. The modeling properties were judged as follows: no shape: poor ×, roughness on the surface or side: slightly poor ◯, model with the specified dimensions: good ◎. In all cases, the powder layer was 20 μm thick, and an alumina plate was used as the substrate.
[0090] [Table 9]
[0091] [Table 10]
[0092] [Table 11]
[0093] As shown in Table 11, both Samples 25 and 26 were rated as excellent moldability, with surface roughness of about 10 μm. As such, Sample 25 was compared to Sample 13, and Sample 26 was compared to Sample 15. It was confirmed that both cases, such as when a powder in which the composition constitutes individual particles was used, and when a powder in which a composition other than the absorbent is contained within the same particle as in this embodiment, had good moldability. This shows that the effect of the absorbent of the present invention does not depend on the composition of the powder other than the absorbent.
[0094] [Example 7] This example relates to an example of the tolerance to changes in the irradiation conditions of laser light when the absorber of the present invention is used. 2 O 3 Powder, Gd 2 O 3 powder, Tb 4 O 7 Mixture of powder (composition ratio is Al 2 O 3 : 64.40vol%, Gd 2 O 3 : 32.73 vol%, Tb 4 O 7 The material was a 3D systems' ProX (product name) DMP200 model.
[0095] The laser light irradiation speed was fixed at 500 mm / s, and the laser light irradiation line pitch was fixed at 130 μm, and the laser power was changed to increase or decrease the energy density during modeling. The powder layer was 25 μm thick, and an alumina plate was used as the base material. A 6 x 6 x 6 mm model was created using the laser power shown in Table 12, and the modeling properties were judged as follows: no shape: poor ×, roughness occurred on the surface and sides: slightly poor ◯, model obtained according to the specified dimensions: good ◎.
[0096] [Table 12]
[0097] At a laser power of 65W, there was almost no melting and the shape of the printed object was distorted, so it was poorly rated X. At 75W and 84W, the energy required for melting was insufficient, and the surface of the printed object became powdery, so it was rated as slightly poor ◯. In the range of 95W to 140W, the surface of the printed object was flat and was rated as good ◎. Furthermore, in the range of 146W to 154W, the amount of energy input was too high and the surface became wavy and tended to become uneven, so it was rated as slightly poor ◯. At 160W, the amount of energy input was too high and the shape of the printed object was distorted, so it was poorly rated X.
[0098] From the above, it was confirmed that stable modeling was possible while allowing an increase in energy density of about 2.0 times at least in the range of 75 W to 154 W. This reflects the fact that the powder of the present invention has absorption ability only when in powder form, and after being incorporated into a model, it has a low absorption rate and is not easily affected by the irradiation of laser light, so that even if the power of the laser light fluctuates, it is unlikely to affect modeling.
[0099] [Example 8] In this embodiment, SiO 2 This is an example of adding particles. The ceramic molding powder of this example was manufactured by the following procedure. 2 O 3 Powder (purity 99.99% or more, particle size 20 μm) and Gd 2 O 3 The powder (purity 99.99% or more, particle size 20 μm) was mixed in a mass ratio of 1:1. 4 O 7 Powder (purity 99.9% or more, particle size 4 μm) was used. SiO 2 The particles used had a purity of 99.9% or more and a particle size of 4 μm. Particles that make up the main component, particles that make up the absorber, and SiO 2 Each powder was weighed so that the particles had a mass ratio of 96.4:3.5:0.14. The weighed powders were mixed in a dry ball mill for 30 minutes to obtain a mixed powder (powder for ceramic molding) (Sample 27).
[0100] The above ceramic molding powder was dissolved by heating in dilute sulfuric acid, and the composition was analyzed by ICP emission spectrometry. 2 O 3 , Gd 2 O 3 , Tb 4 O 7 and SiO 2 The mass ratio of SiO : 3.5:0.14 was 48.2:48.2:3.5:0.14, which was the same as the charged composition ratio. The content of other components was less than 0.2 mass% relative to the powder for ceramics molding. From the composition ratio obtained by analysis, the ratio of SiO : 3.5:0.14 to the mass of particles consisting of the composition other than the absorbent (the main component constituting the ceramic structure) contained in the powder for ceramics molding of Sample 27 was 3.5:3.5:0.14. 2 Mass of particles α [%], i.e., α = SiO 2 / (Al 2 O 3 +Gd 2 O 3 +ZrO 2 The ratio of the SiO 2 Mass of particles β [%], i.e., β = SiO 2 / (Tb 4 O 7 +Pr 6 O 11 ) was calculated to be β = 4.03 [%]. The mass γ [%] of the particles that make up the main component and the particles that make up the absorber, that is, γ = (Tb 4 O 7 +Pr 6 O 11 ) / (Al 2 O 3 +Gd 2 O 3 +ZrO 2 ) was calculated to be γ = 3.61%. A part of the powder for ceramic molding was analyzed by SEM-EDX (scanning electron microscope-energy dispersive X-ray spectroscopy), and it was found that the powder contained SiO 2 It was possible to confirm that the particles were dispersed within the powder.
[0101] [Examples 9 to 25] Powders for ceramic molding of Samples 28 to 44 were produced as Examples 9 to 25 in the same manner as in Example 8, except that the raw material types and compounding ratios were changed according to Table 13. ZrO 2 The praseodymium oxide powder used was Pr 6 O 11 Powder (purity 99.9% or more, particle size 4 μm) was used. The composition of the powder for ceramic molding of samples 28 to 44 was analyzed in the same manner as in Example 8. 2 O 3 , Gd 2 O 3 , ZrO 2 , Tb 4 O 7 ,Pr 6 O 11 and SiO 2 The mass ratio of was the same as the charged composition ratio. The content of other components was less than 0.5 mass% with respect to the powder for ceramic molding. From the composition ratio obtained by analysis, α, β, and γ were calculated in the same manner as in Example 8, and the results are summarized in Table 14. When a part of the powder for ceramic molding produced was analyzed by SEM-EDX, SiO with a particle size of several μm was found. 2 It was possible to confirm that the particles were dispersed within the powder.
[0102] [Comparative Example] A comparative ceramic molding powder was produced in the same manner as in Example 8 according to the compounding ratio shown in Table 13. However, in this comparative example, SiO 2 No particles are used, Al 2 O 3 and Gd 2 O 3 , and the absorber particles Tb 4 O 7 The comparative ceramic molding powder was composed of only Al. 2 O 3 , Gd 2 O 3 , Tb 4 O 7 The mass ratio of SiO was the same as the composition ratio of the feed.2 was less than 50 ppm relative to the comparative ceramic molding powder. The content of other components was less than 0.2 mass % relative to the ceramic molding powder.
[0103] [Table 13]
[0104] [Table 14]
[0105] Ceramic shaped objects were formed using the powders for ceramic shaping of Examples 8 to 25 and the Comparative Example. To form the molded object, a 3D SYSTEMS ProX (trade name) series DMP100 equipped with a 50 W Nd:YAG laser (beam diameter 65 μm) was used. As shown in FIG. 5, first, ceramic molding powder was spread evenly on the laser irradiation area on an alumina base 130 to form a 20 μm-thick first powder layer 102. Next, a 30 W laser beam 180 was irradiated from a laser source 181 onto the powder layer to melt and solidify the powder in a rectangular area of 5 mm × 42 mm. The drawing speed was 100 mm / s to 140 mm / s, and the drawing pitch was 100 μm. In addition, as shown in FIG. 5(a), the drawing line was set to be obliquely 45 degrees to the sides of the rectangle. Next, a new 20 μm-thick powder layer was spread evenly to cover the melted and solidified area. As shown in FIG. 5(b), the powder layer directly above the rectangular region was irradiated with laser light in a manner perpendicular to the drawing line of the first layer, and a 5 mm×42 mm region was melted and solidified. This additive manufacturing process was repeated to form a prism-shaped object with a bottom surface of 5 mm×42 mm and a height of 6 mm for use in a three-point bending strength test. A similar process was also used to form a prism-shaped object with a bottom surface of 22 mm square and a height of 12 mm for a water absorption test. When the surfaces of the objects of Samples 27 to 44 and Comparative Sample 9 were observed with an optical microscope, the unevenness of the surfaces of the objects was 30 μm or less for the objects of Samples 27 to 39 and Samples 42 to 44, and 40 μm or less for the objects of Samples 40, Sample 41, and Comparative Sample 9. The molded object was separated from the alumina base and polished to obtain a ceramic molded object of W40mm×D4mm×H3mm (FIG. 6(a)) for a three-point bending strength test and a ceramic molded object of W20mm×D20mm×H10mm (FIG. 6(b)) for a water absorption test. An Instron compression testing machine was used for the three-point bending test. The three-point bending strength of the ceramic molded objects of each Example and Comparative Example 1 is shown in Table 15.
[0106] The water absorption rate is expressed as a percentage of the total amount of water contained in a ceramic object in a dry, water-saturated state relative to the amount of ceramic object in an absolutely dry state. If the mass of the ceramic object in an absolutely dry state is w1 and the mass of the ceramic object in a dry, water-saturated state is w2, the water absorption rate w [%] can be calculated as w = (w2 - w1) / w1 x 100.
[0107] First, the mass w1 [g] of the ceramics molded object in an absolutely dry state, which had been dried at 80°C for 4 hours, was measured. Next, the ceramics molded object was submerged under the water surface in a boiling tank and boiled for 30 minutes, after which water was added and cooled to room temperature to obtain a water-saturated sample. The water-saturated sample was removed from the water, and the surface was quickly wiped with wet gauze to remove water droplets, and the mass w2 [g] of the ceramics molded object in a surface-dried water-saturated state was measured. The water absorption rate w [%] was calculated using w = (w2 - w1) / w1 x 100, and is summarized in Table 15.
[0108] [Table 15]
[0109] The ceramic objects produced using the powders for ceramic molding of Examples 8 to 25 had high three-point bending strength of 20 MPa or more and low water absorption of 1.0% or less. In particular, the ceramic objects of Samples 27, 28, 30 to 36, 38, 39, and 42 to 44, which satisfied α≦1.0, 0.04≦β≦5, and γ≦20, had high three-point bending strength of 25 MPa or more. [Industrial Applicability]
[0110] The ceramic molding powder of the present invention can be used in the powder bed fusion method or cladding method to obtain ceramic objects with high molding accuracy by adding an absorber, and can be used in the field of ceramic parts that require complex shapes. [Explanation of symbols]
[0111] 11 Powder volume 12 Modeling stage section 13 Recoater Section 14 Scanner section 15, 181 Laser source 21 Cladding nozzle 22 Powder supply hole 23, 180 Laser light 41 Unirradiated area 42 Laser light irradiation area 102 Powder bed 130 Foundations
Claims
1. A method for manufacturing a ceramic object, comprising the steps of: heating a material by irradiating the material with light, the method comprising the steps of: The material includes a first composition containing a first compound and a second composition containing a second compound; The second composition absorbs the light and becomes hotter, thereby causing a temperature rise in the first composition, and changing the second compound into a third compound having a lower absorption ability for the light than the second compound.
2. The manufacturing method described in claim 1, wherein the second composition has a higher absorption ability for the light than the first composition.
3. A manufacturing method as described in claim 1 or 2, wherein the increase in temperature causes the first composition to melt.
4. A manufacturing method described in any one of claims 1 to 3, wherein the second compound is an oxide, the third compound is an oxide, and the second compound and the third compound have different oxidation states.
5. A manufacturing method described in any one of claims 1 to 4, wherein the first compound is a compound of a first element, the second compound is a compound of a second element, the third compound is a compound of the second element, and the second compound and the third compound have different valences of the second element.
6. A manufacturing method described in any one of claims 1 to 5, wherein the absorptivity of the second composition for the light is 10% or more.
7. A manufacturing method described in any one of claims 1 to 5, wherein the second composition has an absorptivity for the light of 40% or more.
8. A manufacturing method described in any one of claims 1 to 5, wherein the second composition has an absorptivity of 60% or more for the light.
9. A manufacturing method described in any one of claims 1 to 8, wherein the absorptance of the second compound for the light is 1.2 times or more greater than the absorptance of the third compound for the light.
10. A manufacturing method described in any one of claims 1 to 9, wherein the absorptivity of the second compound for the light is at least twice the absorptivity of the third compound for the light.
11. A manufacturing method described in any one of claims 1 to 10, wherein the absorptivity of the third compound for the light is 40% or less.
12. A manufacturing method described in any one of claims 1 to 10, wherein the absorptivity of the third compound for the light is 20% or less.
13. A manufacturing method described in any one of claims 1 to 12, wherein the material is a powder.
14. A manufacturing method described in any one of claims 1 to 13, wherein the material includes a first group of particles containing the first compound and a second group of particles containing the second compound.
15. A manufacturing method described in any one of claims 1 to 13, wherein the material includes a first group of particles consisting of the first composition and a second group of particles consisting of the second composition.
16. A manufacturing method described in claim 14 or 15, wherein the median particle size of the second particle group is 1 / 5 or less of the median particle size of the first particle group.
17. A manufacturing method described in any one of claims 14 to 16, wherein the median particle size of the first particle group is 5 μm or more.
18. A manufacturing method described in any one of claims 14 to 17, wherein the median particle size of the second particle group is 1 μm or more.
19. A manufacturing method described in any one of claims 14 to 18, wherein the median particle size of the second particle group is 10 μm or less.
20. A method for producing a material according to any one of claims 13 to 19, wherein the material comprises a third group of particles consisting of a third composition containing a fourth compound.
21. A manufacturing method described in any one of claims 13 to 20, wherein the material includes a fourth group of particles consisting of a fourth composition containing a fifth compound.
22. A method of manufacturing any one of claims 1 to 19, wherein the material includes a third composition containing a fourth compound.
23. A method for manufacturing a semiconductor device according to any one of claims 1 to 22, wherein the first composition contains a compound selected from aluminum oxide, zirconium oxide, silicon oxide, silicon nitride, yttrium oxide, and aluminum titanate.
24. A method for manufacturing a semiconductor device according to any one of claims 1 to 23, wherein the material comprises an oxide of a metal element selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Hf, Ta, W, In, Sn, Bi, Ce, Pr, Sm, Eu, Tb, and Yb.
25. A method for manufacturing a semiconductor device according to any one of claims 1 to 24, wherein the material comprises an oxide of a metal element selected from Sc, Y, La, Ce, Nd, Sm, Eu, Gd, Dy, Ho, Er, Tm, Yb, and Lu.
26. A manufacturing method described in any one of claims 1 to 25, wherein the material includes silicon oxide.
27. A method of manufacturing any one of claims 1 to 26, wherein in the material, the amount of the second composition is 0.5 volume % or more and 53 volume % or less.
28. A manufacturing method described in any one of claims 1 to 27, wherein the carbon content in the material is 1000 ppm or less relative to the metal elements in the material.
29. A manufacturing method described in any one of claims 1 to 28, wherein the ceramic object is formed by additive modeling technology.
30. A manufacturing method described in any one of claims 1 to 29, wherein the ceramic object is formed by powder bed fusion bonding.
31. The method of claim 30, further comprising: irradiating the material with the light based on modeling data; The method according to claim 1 , further comprising repeating the steps of:
32. The manufacturing method described in claim 31, wherein the three-dimensional object is heat-treated.
33. The manufacturing method described in claim 32, wherein glaze is impregnated or applied to the three-dimensional object during the heat treatment.
34. A manufacturing method described in any one of claims 1 to 33, wherein the light is laser light.
35. The manufacturing method described in claim 34, wherein the focal size of the laser light is 10 μm to 2 mm.
36. A method according to any one of claims 1 to 35, wherein the irradiation is performed with a Nd:YAG laser.
37. A method of manufacturing as described in any one of claims 1 to 36, wherein the increase in temperature causes the temperature of the first composition to exceed the melting point of the first composition.
38. A manufacturing method described in any one of claims 1 to 37, wherein the ceramic object includes crystals.
39. A manufacturing method described in any one of claims 1 to 38, wherein the ceramic object has a eutectic structure.
40. A manufacturing method described in any one of claims 1 to 39, wherein the ceramic object has an amorphous region.