Materials, methods and techniques for generating doped cerium oxide

JP2024116296A5Active Publication Date: 2024-11-26LYNAS RARE EARTHS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024094190
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-24
Filing Date
2024-06-11
Publication Date
2024-11-26
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing cerium oxide materials lack optimal properties for efficient oxygen absorption and desorption in varying atmospheric conditions, limiting their effectiveness in applications such as vehicle exhaust gas purification and other catalytic processes.

Method used

Doped cerium oxide particles with specific compositions and production methods, including calcination and dopant addition, enhance oxygen storage capacity and mobility, resulting in improved catalytic performance across a range of temperatures.

Benefits of technology

The doped cerium oxide particles exhibit enhanced oxygen storage capacity and mobility, making them suitable for catalytic processes like hydrogen gas generation, carbon dioxide to methane conversion, and nitric acid production, with improved efficiency and performance in exhaust gas purification.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide doped cerium oxide having a large oxygen storage capacity, enabling not only its use as a co-catalyst in exhaust gas catalysts but also the removal of nitrous oxide and the conversion of carbon dioxide to nitrous oxide.SOLUTION: Doped cerium oxide particles may comprise about 90 weight percent (wt.%) to about 99.9 wt.% cerium oxide (CeO2) and up to about 10 wt.% dopant. Exemplary doped cerium oxide particles may have a BET specific surface area of more than 150 m2 / g after calcination at 500°C for 8 hours. Exemplary doped cerium oxide particles may have an oxygen storage capacity (OSC) of more than 900 μmol O2 / g after calcination at 500°C for 8 hours.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application was filed on November 24, 2020, and is incorporated herein in its entirety. Priority is claimed to U.S. Provisional Patent Application No. 63 / 117,558.

[0002] The materials, methods, and techniques disclosed herein relate to doped cerium oxide. In particular, the present disclosure relates to the production and properties of doped cerium oxide particles. [Background technology]

[0003] Cerium (Ce) is a trivalent metal also known as ceria or cerium. Cerium oxide is a rare earth element that can exist in either the tetravalent (cerium) or tetravalent (cerium) state. Rubber-containing materials have been used in a variety of applications, including catalysis, such as for cleaning vehicle exhaust gases. Cerium oxide materials typically absorb oxygen in an oxidizing atmosphere and desorb oxygen in a reducing atmosphere. This oxygen absorption / desorption ability allows cerium oxide materials to This will enable it to be used for a variety of purposes, such as purifying harmful substances contained in water. Summary of the Invention

[0004] In one aspect, doped cerium oxide particles are disclosed. Exemplary doped cerium oxide particles is about 90 weight percent (wt%) to about 99.9 wt% cerium oxide (CeO2) and and up to about 10 wt % of a dopant. An exemplary doped cerium oxide particle is After calcination at 00°C for 8 hours, 150 2 The BET specific surface area of ​​the doped polymer may be greater than 100 nm / g. The cerium oxide particles had more than 900 μmol O2 / g after calcination at 500°C for 8 hours. It may have oxygen storage capacity (OSC).

[0005] In another aspect, a method for producing doped cerium oxide particles is disclosed. An exemplary method is The rare earth oxide concentration was 10 grams to 50 grams of CeO2 per liter of solvent. adding at least one dopant to the Ce(NO3)4 solution; After adding at least one dopant, heat the Ce(NO3)4 solution containing the dopant. cooling the resulting mixture; and neutralizing the mixture to a pH of 8 to 9; and filtering the neutralized mixture to obtain a residue. ) and a permeate; calcining the residue; and drying. and

[0006] To obtain some benefit from the present disclosure, materials, techniques, and methods relating to doped cerium oxide are disclosed. There is no particular requirement that the method include all of the details characterized herein. The specific examples characterized herein are intended to be exemplary applications of the techniques described, and are not to be construed as limiting the scope of the invention. Substitutions are possible. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The materials, methods and techniques disclosed and contemplated herein are directed to the production of doped cerium oxide. Exemplary doped cerium oxides can be used in a variety of applications, particularly in combination with ceria. In comparison, improved oxygen mobility can be exhibited. Doped cerium oxide is used in hydrogen gas (H2) evolution processes, diacid The process of converting carbon dioxide (CO2) to methane (CH4), as well as nitric acid (HNO3) and and / or removal of nitrous oxide (N2O) from adipic acid (CH2)4(COOH)2 Certain of the compounds disclosed herein can be used as catalysts in processes such as those for the production of cyclohexane. The exemplary doped cerium oxide particles are characterized by high performance in the temperature range of about 300° C. to about 800° C. The exemplary doped cerium oxide is contemplated for other uses.

[0008] definition Unless otherwise defined, all technical and scientific terms used herein are understood to be within the skill of the art. In the event of any conflict, this document, including definitions, shall prevail. Exemplary methods and materials are described below, but may be used in a similar or alternative manner to those described herein. or equivalent methods and materials can be used in the practice or testing of the present disclosure. The materials, methods, and examples disclosed herein are illustrative only and are not intended to be limiting.

[0009] As used herein, "comprise," "include," "having" "has," "can," "contain" The terms and variations thereof are non-limiting and do not exclude the possibility of additional acts or structures. It is intended to be a transitional phrase, term, or word. Singular "one (a)" "an" and "the" refer to the plural unless the context clearly dictates otherwise. The present disclosure also includes references to the methods and apparatus provided herein, whether expressly stated or not. Other embodiments that "comprise," "consist," and "consist essentially of" the embodiments or elements shown are also contemplated. Embodiments are also contemplated.

[0010] Definitions of certain functional groups and chemical terms are described in more detail below. For purposes of this disclosure, For chemical elements, see the Periodic Table of Elements, CAS version, Handbook of Chemistry and Phys Identified according to ICS 75th Edition inside cover, specific functional groups are identified as described therein. Generally defined.

[0011] For any numerical ranges set forth herein, each intervening value is expressly included to the same degree of precision. For example, for the range 6-9, the numbers 7 and 8 in addition to 6 and 9 are For the range 6.0 to 7.0, 6.0, 6.1, 6.2, 6.3, 6.4, The numbers 6.5, 6.6, 6.7, 6.8, 6.9, and 7.0 are explicitly envisaged.

[0012] The modifier "about" used in connection with a quantity is inclusive of the stated value and is dictated by context. have meaning (e.g., include at least the degree of error associated with the measurement of a particular quantity). The word "about" should also be considered to disclose a range defined by the absolute values ​​of the two endpoints. For example, the expression "about 2 to about 4" also discloses the range "2 to 4." The term may refer to plus or minus 10% of the indicated number. For example, "about 1 "0%" could indicate a range of 9% to 11%, and "about 1" could indicate 0.9 to 1.1. Other meanings of "about" may be apparent from the context, such as rounded numbers. Thus, for example, "about 1" means 0. It can also mean .5 to 1.4.

[0013] I. Exemplary Doped Cerium Oxide Particles Exemplary doped cerium oxide particles can have a variety of chemical compositions and physical properties. Various aspects are discussed below.

[0014] Exemplary doped cerium oxide particles have a majority of cerium oxide (CeO2). Typically, exemplary doped cerium oxide particles have a doped cerium oxide content of about 90.0 weight percent (wt%) to about 90.0 wt%. It may comprise approximately 99.9 wt% cerium oxide (CeO2). In various implementations, an exemplary The doped cerium oxide particles are about 90.0 wt% to about 99.9 wt% cerium oxide (C Cerium oxide (CeO2); about 90 wt% to about 95 wt% 99.9wt% cerium oxide (CeO2); 90wt% to 92wt% cerium oxide Cerium oxide (CeO2); 92wt%~94wt% 6wt% cerium oxide (CeO2); 96wt%~98wt% cerium oxide (CeO 2);97wt%~99wt%;95wt%~96wt%;96wt%~97wt% acid cerium oxide (CeO2); 97wt%-98wt% cerium oxide (CeO2); or % cerium oxide (CeO2). Exemplary doped cerium oxide particles are composed of more than 90 wt% cerium oxide (CeO2); t% or more of cerium oxide (CeO2); 92wt% or more of cerium oxide (CeO2); 9 3wt% or more of cerium oxide (CeO2); 94wt% or more of cerium oxide (CeO2) ;95wt% or more cerium oxide (CeO2);96wt% or more cerium oxide (CeO 2); 97wt% or more cerium oxide (CeO2); 98wt% or more cerium oxide (C eO2); or 99 wt% or more of cerium oxide (CeO2). In one embodiment, the exemplary doped cerium oxide particles are less than 99.9 wt % cerium oxide (Ce O2); less than 98 wt% cerium oxide (CeO2); less than 97 wt% cerium oxide ( CeO2); less than 96 wt% cerium oxide (CeO2); less than 95 wt% cerium oxide Cerium oxide (CeO2); less than 94 wt% cerium oxide (CeO2); less than 93 wt% cerium oxide Cerium oxide (CeO2); less than 92 wt% Cerium oxide (CeO2); or less than 91 wt% It may contain cerium oxide (CeO2).

[0015] Exemplary doped cerium oxide particles have between about 0.1 wt % and about 10 wt % dopant. In various implementations, the doped cerium oxide particles may be present in an amount of 0.1 wt % to 10.0 wt %. % dopant;0wt%~5wt% dopant;0.1wt%~5wt% dopant 5wt%~10wt% dopant; 0.1wt%~3.0wt% dopant; 3 .0wt%~6.0wt% dopant; 6.0wt%~9.0wt% dopant; 7 .0wt%~10.0wt% dopant;0.1wt%~1wt% dopant;1w t%~2wt% dopant; 2wt%~3wt% dopant; 3wt%~4wt% Dopant;4wt%~5wt% dopant;5wt%~6wt% dopant;6w t%~7wt% dopant; 7wt%~8wt% dopant; 8wt%~9wt% or 9 wt% to 10 wt% dopant. Exemplary doped cerium oxide particles include 10 wt. % or less dopant; 9 wt. % or less dopant; -pant;8wt% or less of dopant;7wt% or less of dopant;6wt% or less of dopant 5wt% or less of dopant; 4wt% or less of dopant; 3wt% or less of dopant 2wt% or less of dopant; 1wt% or less of dopant; 0.5wt% or less of dopant or having 0.1 wt % or less of a dopant. The doped cerium oxide particles are those having greater than 0.1 wt. % dopant; greater than 0.5 wt. % dopant ;More than 1wt% dopant;More than 2wt% dopant;More than 3wt% dopant;4wt % dopant; 5wt% dopant; 6wt% dopant; 7wt% dopant % dopant; or greater than 8 wt. % dopant; or greater than 9 wt.

[0016] Exemplary doped cerium oxide particles may include one or more dopants. The material may be selected having regard to the end use or end uses of the doped cerium oxide particles. Exemplary components that can be doped into the exemplary cerium oxide particles include silicon dioxide. Silicon dioxide (SiO2) powder, silicon dioxide (SiO2) gel, tetraethyl orthosilicate (TE OS), white carbon black (precipitated silica), aluminum oxide (Al2O3) powder rare earth elements such as lanthanum oxide (La2O3) and neodymium(III) oxide (Nd2O3). The zeolites may be selected from the group consisting of zeolites, zeolites of ... Zeolite Socony Mobil-5 (H-ZSM-5), HY Zeola Examples of zeolite include zeolite, beta zeolite, and H-beta zeolite.

[0017] Exemplary doped cerium oxide particles have BET specific surface area, oxygen storage capacity, total pore volume, and It can be described in terms of physical properties such as crystal size, and TPR profile. BET surface area measurements are performed using a fluororesin manufactured by Micromeritics Company. Using N2 physisorption / desorption measurements performed on an automated ASAP2020 physisorption instrument The specific surface area of ​​the sample can be calculated by the BET method at P / P0 = 0.05 to 0.35. It can be calculated by the multipoint method of (Brunauer-Emmett-Teller) The total pore volume is calculated by using single-point adsorption at P / P0=0.99 and the pore volume distribution can be calculated using the BJH method of desorption isotherms.

[0018] X-ray diffraction (XRD) was performed using a D / max2550VB / manufactured by Rigaku Corporation. PC X-ray diffractometer, CuKα radiation source (40 kV, 40 mA), scanning range 2θ=10 The crystal size (nm) can be calculated by the following method: Feller's formula d = kλ / βcosθ [where d is the crystal size (nm) and λ is the wavelength of the X-rays] is the diffraction peak half-width (degrees), and θ is the diffraction angle ( where K is the Scherrer constant (0.89).

[0019] Hydrogen temperature-programmed reduction (H2-TPR) measurements is manufactured by AUTOChem Micromeritics Company A chemisorption instrument of type II 2920 was used containing 90% argon and 10% hydrogen. The temperature was measured from 100 to 800°C for 10 minutes at a gas flow rate of 50 ml / min using a carrier gas with A heating rate of °C / min can be performed using 0.1 g of sample.

[0020] The oxygen storage capacity (OSC) of a sample can be determined by a thermal conductivity detector (TCD). The hydrogen consumption of the sample can be converted by the reduction peak area of ​​a certain amount of copper oxide powder. In the H2-TPR curve, the baseline in the temperature range of 200 to 600°C is The area between the TPR curve and the baseline (S1) in the temperature range of 600 to 800 °C The ratio S1 / S2 was defined as the ratio of the area between the TPR curve (S2).

[0021] The doped cerium oxide particles can be characterized in terms of their BET specific surface area. In the case of the exemplary doped cerium oxide particles, after calcination at 300° C. for 10 hours, the 0m 2 / g, 210m 2 / g, 220m 2 / g over;230m 2 / g or more; or 240 m 2 In some cases, the exemplary doped cerium oxide may have a BET specific surface area of ​​greater than 100 nm / g. The particles were calcined at 300°C for 10 hours and then 2 / g or less; 240m 2 / g or less;2 30m 2 / g or less; 220m 2 / g or less; or 210m 2 / g or less BET specific surface area In various implementations, the exemplary doped cerium oxide particles can be heated to 300° C. for 10 hours. After calcination for about 200m 2 / g ~ approx. 250m 2 / g;200m 2 / g~225m 2 / g ;225m 2 / g~250m 2 / g;200m 2 / g~210m 2 / g;210m 2 / g ~220m 2 / g;220m 2 / g~230m 2 / g;230m 2 / g~240m 2 / g ; or 240m 2 / g~250m 2 / g.

[0022] In some cases, the exemplary doped cerium oxide particles, after calcination at 500° C. for 8 hours, 150m 2 / g over;160m 2 / g over;170m 2 / g over;180m 2 / g or more; or 1 90m 2 In some cases, the exemplary doped cerium oxide may have a BET specific surface area of ​​greater than 100 nm / g. The sintered particles were calcined at 500°C for 8 hours and then 2 / g or less; 190m 2 / g or less; 180m 2 / g or less; 170m 2 / g or less; or 160m 2 / g or less BET specific surface area In various implementations, the exemplary doped cerium oxide particles can have a melting point of 8 hours at 500° C. After calcination, about 150m 2 / g~about 200m 2 / g;150m 2 / g~175m 2 / g ;175m 2 / g~200m 2 / g;150m 2 / g~160m 2 / g;160m 2 / g ~170m 2 / g;170m 2 / g~180m 2 / g;180m 2 / g~190m 2 / g ; or 190m 2 / g~200m 2 / g.

[0023] In some cases, the exemplary doped cerium oxide particles, after calcination at 700° C. for 5 hours, 100m 2 / g over;110m 2 / g over;120m 2 / g over;130m 2 / g or more; or 1 40m 2 In some cases, the exemplary doped cerium oxide may have a BET specific surface area of ​​greater than 100 nm / g. The sintered particles were calcined at 700°C for 5 hours and then 2 / g or less; 140m 2 / g or less; 130m 2 / g or less; 120m 2 / g or less; or 110m 2 / g or less BET specific surface area In various implementations, the exemplary doped cerium oxide particles can be thermally bonded at 700° C. for 5 hours. After calcination for about 100m 2 / g~about 150m 2 / g;100m 2 / g~125m 2 / g ;125m 2 / g~150m 2 / g;100m 2 / g~110m 2 / g;110m 2 / g ~120m 2 / g;120m 2 / g~130m 2 / g;130m 2 / g~140m 2 / g ; or 140m 2 / g~150m 2 / g.

[0024] In some cases, the exemplary doped cerium oxide particles, after calcination at 900° C. for 5 hours, 55m 2 / g over;65m 2 / g over;75m 2 / g over;85m 2 / g or more than 90m 2 / In some cases, the exemplary doped cerium oxide particles may have a BET specific surface area of ​​greater than 100 nm. After calcination at 900°C for 5 hours, 2 / g or less;90m 2 / g or less; 80m 2 / g Below;70m 2 / g or less; or 60m 2 / g or less. In an implementation, the exemplary doped cerium oxide particles have a melting point of about 5° C. after calcination at 900° C. for 5 hours. 5m 2 / g~about 100m 2 / g;55m 2 / g~80m 2 / g;75m 2 / g~100m 2 / g;55m 2 / g~65m 2 / g;65m 2 / g~75m 2 / g;75m 2 / g~8 5m 2 / g;85m 2 / g~95m 2 / g; or 90m 2 / g~100m 2 / g BE T specific surface area.

[0025] The doped cerium oxide particles can be characterized in terms of their oxygen storage capacity (OSC). Exemplary doped cerium oxide particles have a mass of 900 μmol after calcination at 500° C. for 8 hours. More than 1000 μmol O2 / g; or more than 1100 μmol O2 / g Exemplary doped cerium oxide particles may have a .OSC after calcination at 500° C. for 8 hours. 1200μmol·O2 / g or less; 1100μmol·O2 / g or less; or 1000μ In various implementations, the exemplary doped oxide ceramics may have an OSC of 0.1 to 1.0 mol O2 / g or less. After calcination at 500°C for 8 hours, the lithium particles had a concentration of 900μmol·O2 / g~1200μm ol·O2 / g;900μmol·O2 / g~1050μmol·O2 / g;1050μ mol·O2 / g~1200μmol·O2 / g;900μmol·O2 / g~1000 μmol·O2 / g; 1000μmol·O2 / g~1100μmol·O2 / g; also can have an OSC of 1100 μmol·O2 / g to 1200 μmol·O2 / g.

[0026] Exemplary doped cerium oxide particles, after calcination at 700 °C for 5 h, contained 800 μmol· OS > 900 μmol O2 / g; > 1000 μmol O2 / g Exemplary doped cerium oxide particles may have a 11% yield after calcination at 700° C. for 5 hours. 00μmol·O2 / g or less; 1000μmol·O2 / g or less; or 900μmol In various implementations, the exemplary doped cerium oxide may have an OSC of 0.1 to 0.5 μm. After calcination at 700 °C for 5 h, the particles had a concentration of 800 μmol·O2 / g–1100 μmol· O2 / g;800μmol·O2 / g~950μmol·O2 / g;950μmol·O 2 / g~1100μmol·O2 / g;800μmol·O2 / g~900μmol·O 2 / g; 900μmol·O2 / g~1000μmol·O2 / g; or 1000μm ol·O2 / g to 1100 μmol·O2 / g.

[0027] Exemplary doped cerium oxide particles, after calcination at 900 °C for 5 h, contained 700 μmol· OSC > 800 μmol O2 / g; > 900 μmol O2 / g Exemplary doped cerium oxide particles may have a 100% yield after calcination at 900° C. for 5 hours. 0 μmol O2 / g or less; 900 μmol O2 / g or less; or 800 μmol O In various implementations, the exemplary doped cerium oxide particles may have an OSC of 2 / g or less. After calcination at 900℃ for 5 hours, the concentration of O2 / g was 700μmol·O2 / g~1000μmol·O2 / g;700μmol·O2 / g~850μmol·O2 / g;850μmol·O2 / g~1000μmol·O2 / g;700μmol·O2 / g~800μmol·O2 / g; 800 μmol O2 / g to 900 μmol O2 / g; or 900 μmol O It can have an OSC of 2 / g to 1000 μmol·O2 / g.

[0028] The doped cerium oxide particles can be characterized in terms of total pore volume. The doped cerium oxide particles had a mass fraction larger than 0.40 mL / g after calcination at 300°C for 10 h. greater than 0.50 mL / g; greater than 0.60 mL / g; or greater than 0.70 mL / g Exemplary doped cerium oxide particles may have a total pore volume of greater than 1 g at 300° C. After 0 hours of calcination, the or a total pore volume greater than 0.70 mL / g. The exemplary doped cerium oxide particles had a volume of 0.4 mL / cm2 after calcination at 300° C. for 10 hours. g~0.8mL / g;0.4mL / g~0.6mL / g;0.6mL / g~0.8mL / g;0.4mL / g~0.5mL / g;0.5mL / g~0.6mL / g;0.6mL / g to 0.7 mL / g; or a total pore volume of 0.7 mL / g to 0.8 mL / g.

[0029] The doped cerium oxide particles can be characterized in terms of total pore volume. The doped cerium oxide particles have a mass fraction larger than 0.40 mL / g after calcination at 500°C for 8 h. greater than 0.50 mL / g; greater than 0.60 mL / g; or 0.70 mL / g Exemplary doped cerium oxide particles can be heated to 500° C. for 8 hours. After calcination for 1 hour, 0.80 mL / g or less; 0.70 mL / g or less; 0.60 mL / g or more or a total pore volume greater than 0.70 mL / g. Exemplary doped cerium oxide particles have a melting point of 0.4 mL / g-0 after calcination at 500° C. for 8 hours. .8mL / g;0.4mL / g~0.6mL / g;0.6mL / g~0.8mL / g;0 .4mL / g~0.5mL / g;0.5mL / g~0.6mL / g;0.6mL / g~0 0.7 mL / g; or a total pore volume of 0.7 mL / g to 0.8 mL / g.

[0030] The doped cerium oxide particles can be characterized in terms of total pore volume. The doped cerium oxide particles have a mass fraction larger than 0.35 mL / g after calcination at 700°C for 5 h. greater than 0.45 mL / g; greater than 0.55 mL / g; or 0.65 mL / g Exemplary doped cerium oxide particles can be heated to 700° C. for 5 hours. After calcination for a period of time, 0.70 mL / g or less; 0.60 mL / g or less; greater than 0.50 mL / g or a total pore volume greater than 0.40 mL / g. Exemplary doped cerium oxide particles have a melting point of 0.35 mL / g-1 after calcination at 700° C. for 5 hours. 0.7mL / g;0.35mL / g~0.53mL / g;0.52mL / g~0.7mL / g;0.35mL / g~0.45mL / g;0.45mL / g~0.55mL / g;0 Total pore volume of 0.55mL / g to 0.65mL / g; or 0.6mL / g to 0.7mL / g It may have a product.

[0031] The doped cerium oxide particles can be characterized in terms of total pore volume. The doped cerium oxide particles have a mass fraction larger than 0.35 mL / g after calcination at 900°C for 5 h. greater than 0.45 mL / g; greater than 0.55 mL / g; or 0.65 mL / g Exemplary doped cerium oxide particles can be heated to 900° C. for 5 hours. After calcination for a period of time, 0.70 mL / g or less; 0.60 mL / g or less; greater than 0.50 mL / g or a total pore volume greater than 0.40 mL / g. Exemplary doped cerium oxide particles have a melting point of 0.35 mL / g-1 after calcination at 900° C. for 5 hours. 0.7mL / g;0.35mL / g~0.53mL / g;0.52mL / g~0.7mL / g;0.35mL / g~0.45mL / g;0.45mL / g~0.55mL / g;0 Total pore volume of 0.55mL / g to 0.65mL / g; or 0.6mL / g to 0.7mL / g It may have a product.

[0032] The doped cerium oxide particles are characterized in terms of pore volume (d>3 nm) divided by total pore volume. Exemplary doped cerium oxide particles were calcined at 300° C. for 10 hours. After the above process, the pore volume (d>3 nm) may be at least 98% of the total pore volume. The cerium oxide particles have at least 98% of the pore volume ( Exemplary doped cerium oxide particles may have a pore volume of 700° C. After 5 hours of calcination, it can have at least 98% of the pore volume (d>3 nm) / total pore volume. Exemplary doped cerium oxide particles have at least 98% solubility after calcination at 900° C. for 8 hours. pore volume (d>3 nm) / total pore volume.

[0033] The doped cerium oxide particles can be characterized in terms of crystallite size. The doped cerium oxide particles had a crystal size of less than about 10 nm after calcination at 500 °C for 8 h. In various implementations, the exemplary doped cerium oxide particles can have a melting point of 8 hours at 500° C. After calcination between 6nm~10nm; 6nm~8nm; 8nm~10nm; 6nm~7nm 7 nm to 8 nm; 8 nm to 9 nm; or 9 nm to 10 nm. In various implementations, the exemplary doped cerium oxide particles may be calcined at 500° C. for 8 hours. , 6 nm or more; 7 nm or more; 8 nm or more; or 9 nm or more. In various implementations, the exemplary doped cerium oxide particles, after calcination at 500° C. for 8 hours, It may have a crystal size of 10 nm or less; 9 nm or less; 8 nm or less; or 7 nm or less.

[0034] Doped cerium oxide particles were investigated from the viewpoint of hydrogen (H2)-temperature programmed reduction (TPR) profile. In one embodiment, the graph generated by the H2-TPR profile can be used to characterize the The rough outline is (A1) H2-TPR curve and baseline in the temperature range of 200℃ to 600℃. (A2) H2-TPR curve in the temperature range of 600℃ to 800℃ and the baseline, the ratio of the areas defined by the baseline, A1 / A2. Exemplary doped cerium oxide particles have a molecular weight of 1.0-1.0% after calcination at 500° C. for 8 hours. An exemplary doped cerium oxide particle may have an A1 / A2 ratio of 0.5 at 700° C. for 5 hours. After calcination for a period of time, the A1 / A2 ratio may be between 0.7 and 1.0. The aluminum particles may have an A1 / A2 ratio of 0.35 to 0.7 after calcination at 900°C for 5 hours. The doped cerium oxide particles had a solubility of 1.5 or less and 1.25 or less after calcination at 500°C for 8 hours. , or a ratio of A1 / A2 of 1.0 or less. After calcination at 40° C. for 8 hours, the ratio of A1 / A2 may be greater than 0.7, greater than 1.0, or greater than 1.3. .

[0035] II. Exemplary Methods for Producing Cerium(IV) Hydroxide Using the exemplary method, cerium (IV) hydroxide (Ce(OH)4) precipitate and nitrate were prepared. Now, during the synthesis of doped cerium oxide, Using the resulting cerium(IV) hydroxide precipitate and cerium(IV) nitrate solution, Embodiments other than those discussed below may include more or fewer operations. stomach.

[0036] An exemplary method can begin with a basic solution. An exemplary basic solution is 1.0 It can be prepared to have a base concentration of 20 to 4.0 mol / L. It may be at a temperature below 30° C., such as 30° C. An exemplary basic solution is NaOH. While preparing the basic solution, stirring can be performed at about 800 rpm to about 1200 rpm. can.

[0037] The raw materials are then added to the basic solution. In some cases, the raw materials are added as a batch operation. Typically, the temperature of the basic solution is 20-30° C. Exemplary raw materials include: It may be cerium chloride (CeCl3). In some cases, the raw material added to the basic solution contains 50-200 g CeO2 / L and has free [H + ] is 0.05~0.5mol / L In some cases, the exemplary ingredients can be diluted before being added to the NaOH solution. For example, dilution of 300-500 g of CeO2 / L of initial solution will result in a dilution of 50-200 A solution of 1000 g of CeO2 / L of CeCl3 can be prepared. Deionized water is used for dilution. It is possible.

[0038] The resulting mixture of the raw material and the basic solution is subjected to air bubbling and / or stirring. In some cases, the basic solution may be bubbled with air prior to adding the ingredients. For example, air bubbling can be performed at 150 to 300 L of air per hour. Air bubbling and / or stirring may be provided at a rate of 100-200 rpm or faster. The reaction can be carried out for a predetermined period of time, such as 1 hour to 5 hours. During this period, reverse precipitation precipitation) may occur.

[0039] After reverse precipitation, the resulting mixture is stirred for a period of time, such as 2 to 6 hours, typically at a temperature of 20°C to 30°C. The resulting mixture can be aged. Typically, the resulting mixture is kept at a pH of 12.0-13. During aging, the resulting mixture changes from a purple hue to a yellowish hue. May cause color shift to color hues.

[0040] Filtration can be performed to remove various ions. For example, NaOH is basic. When used as a solution, Na is removed during filtration. + and Cl - Ions can be removed To achieve filtration of the target ions, various filtration methods known in the art can be selected. To further remove the target ions, the ion exchange may be performed one or more times. The washing operation can be carried out.

[0041] After removal of the target ions, the concentration is 0.01 to 0.1 mol base per liter The precipitate can be re-pulped into a basic solution having In some cases, NaOH can be used in the basic solution. Repulping can be performed at, for example, 80 It can involve stirring at 0 rpm to 1200 rpm and can be performed at room temperature, such as 20°C to 30°C. It is possible.

[0042] Aging of the solution can be accompanied by air bubbling through a porous air distributor. - Bubbling can be provided at a flow rate of 150-300 liters of air per hour. Aging is Do this for a set period of time, such as at least 30 minutes or 1 to 6 hours, at a temperature between 20°C and 30°C. The resulting mixture is then subjected to a second filtration process.

[0043] After filtration, the mixture can be washed. The first wash is with hot deionized water (40°C). The first wash can be performed using a temperature of 100° C. to 80° C., or 50° C. to 65° C. may be performed multiple times, such as 2, 3, 4, 5, or up to 10 times.

[0044] The second wash is with hot deionized water (which can be 40°C to 80°C or 50°C to 65°C) This can be done using a mixture of nitric acid (HNO3) and a strong acid such as nitric acid (HNO3). The resulting mixture may have a pH of about 4 to about 5. The resulting residue may have a pH of 8 to 10. The resulting residue may have an electrical conductivity (EC) of less than 20 μS / cm. The second wash may be performed multiple times, such as 2, 3, 4, 5, or up to 10 times.

[0045] After washing, a wet cake of cerium(IV) hydroxide remains. The aluminium(IV) wet cake has a loss of ignition (LOI) of 55% to 65%. In some cases, the total cerium in the cerium(IV) hydroxide wet cake may be At least 95% or at least 97% of the cerium species are cerium(IV) (Ce 4+ In some cases, the CeO2 / total ratio in the cerium(IV) hydroxide wet cake may be The ratio of rare earth oxides (TREO) is at least 99% or at least 99.5%. In some cases, the percentage of cerium oxide in the cerium(IV) hydroxide wet cake is It could be 35% to 60%.

[0046] The cerium(IV) hydroxide wet cake may have one or more impurities. For example, an exemplary cerium(IV) hydroxide wet cake may be prepared by mixing aluminum oxide (AlO 3) Cl - , Na + , iron oxide (Fe2O3), zinc oxide (ZnO), and silicon oxide (SiO2) at less than 0.01 wt% of each impurity. can be done.

[0047] Cerium(IV) hydroxide wet cake can be dissolved in a strong acid solution such as HNO3. In some implementations, the weight percentage of the strong acid in the strong acid solution is about 65% to about 100%. The strong acid solution may be at a high temperature, such as from about 65° C. to about 100° C. The molar ratio of the strong acid to CeO2 may be 4.1 to 5.5. In this case, the weight percentage of wet cake is about 42%. The mixture can be stirred at 100°C for 5-30 minutes. In some cases, the slurry becomes clear red. Stirring can be terminated when the mixture has a bright color.

[0048] The resulting Ce(NO3)4 solution had a CeO2 concentration of 250-300 g per liter. and more than 97% of all cerium species are cerium(IV) (Ce 4+ ) The obtained Ce(NO3)4 solution was dissolved in 0.1-0.5 [H + ] / Total Cerium Chemistry The molar ratio of the species may be:

[0049] III. Exemplary Methods for Synthesizing Doped Cerium Oxide Particles Exemplary methods can be used to synthesize doped cerium oxide particles, as discussed below. Other embodiments than those discussed may include more or less operations. An exemplary method for producing sodium particles is to form the sodium ions by reacting the sodium ions with the sodium hydroxide solution, typically prior to hydrolysis, but following precipitation. In some cases, the dopant added prior to hydrolysis may be added. In addition to the pant, the dopant may be added after hydrolysis.

[0050] An exemplary method is to use 10 grams to 50 grams of rare earth CeO2 per liter of solvent. We can start by preparing a Ce(NO3)4 solution with similar oxide concentrations. In some implementations, the cerium nitrate (I nitrate) produced using the methods described above can be used. V) Dilute the (Ce(NO3)4) solution to, for example, 10 grams per liter of solvent. 50 grams CeO2; 10 grams to 30 grams CeO2 per liter of solvent; solvent 15 grams to 25 grams of CeO2 per liter; or 20 grams per liter of solvent Rare earth oxide concentrations ranging from 1 g to 40 g CeO2 can be achieved. For example, The prepared Ce(NO3)4 solution contained at least 10 grams of Ce per liter of solvent. O2; at least 20 grams CeO2 per liter of solvent; at least 20 grams CeO2 per liter of solvent At least 30 grams of CeO2 per liter of solvent; or at least 40 grams of C per liter of solvent eO2. Deionized water can be used as a diluent.

[0051] One or more dopants can then be added to the Ce(NO3)4 solution. Various dopants can be added at this stage. Exemplary dopants are those discussed above. The paper discusses in detail the properties of silicon dioxide (SiO2) powder, silicon dioxide (SiO2) gel, and , Tetraethyl orthosilicate (TEOS), White carbon black, Aluminum oxide Examples include aluminum (Al2O3) powder, lanthanum (La), and zeolite. The amount of dopant added is 0.1wt% to 10wt% of the Ce(NO3)4 solution. An exemplary silicon dioxide (SiO2) powder has a particle size of 200 to 250 μm. 2 BET surface area / g An exemplary aluminum dioxide (Al2O3) powder may have a particle size of 200-250 μm. 2 / g of BET surface area.

[0052] After the dopant is added, the mixture is heated to a predetermined temperature. Typically, the predetermined temperature is The predetermined temperature may be between 120° C. and 150° C. In various implementations, the predetermined temperature may be between 120° C. and 130° C. ℃; 130℃ to 140℃; or 140℃ to 150℃. Heating to a predetermined temperature is After the desired temperature is reached, the mixture is allowed to stand at the desired temperature for about 6 hours to 24 hours. It can be maintained for about 12 hours, during which time hydrolysis can occur.

[0053] After the hydrolysis operation, the resulting mixture can be cooled. The temperature of the mixture is reduced to below 50°C.

[0054] At this point, optionally, one or more dopants can be added. Suitable dopants are discussed in more detail above and include silicon dioxide (SiO2) powder, diacid Silicon dioxide (SiO2) gel, tetraethyl orthosilicate (TEOS), white carbon Black, aluminum oxide (Al2O3) powder, lanthanum (La), zeolite, and The amount of dopant added is typically Ce. The dopant is added at this stage. If so, the results are obtained for a given period of time, usually 30 to 90 minutes, such as 30, 60, or 90 minutes. The resulting mixture can be stirred.

[0055] The resulting mixture, usually a slurry, is then neutralized to a pH of 8-9. The precipitated slurry is neutralized and precipitates. In some cases, hydroxide hydrate is added to neutralize the pH. A weak base such as ammonium hydroxide (NH4OH) can be used. When used, the concentration may be greater than 25%. Neutralization of the resulting mixture may take 10 to 3 minutes. This may involve stirring for a predetermined period of time, such as 0 minutes.

[0056] After neutralization, optionally, one or more dopants can be added. Suitable dopants are discussed in more detail above and include silicon dioxide (SiO2) powder, Silicon (SiO2) gel, tetraethyl orthosilicate (TEOS), white carbon black Examples include lac, aluminum oxide (Al2O3) powder, lanthanum (La), and zeolite. Typically, the amount of dopant added is 0.1% of the Ce(NO3)4 solution. If a dopant is added at this stage, it is usually added for a certain period of time. The resulting mixture may be stirred for 30 to 90 minutes, such as 30, 60, or 90 minutes. can.

[0057] The resulting precipitate is then subjected to filtration. An exemplary filtration procedure removes the residue, typically To produce a wet cake as a residue, the Any type of filtration known in the art can be used.

[0058] The wet cake residue can be dried and calcined at a given temperature for a given time. The product is typically a doped cerium oxide powder. For example, the wet cake residue can be calcined at 500° C. for 8 hours. For example, the wet cake residue can be calcined at 700° C. for 5 hours. In one particular implementation, the wet cake residue is calcined at 300° C. for 10 hours, and then The eO2 powder is calcined at 900°C for 5 hours.

[0059] In some cases, one or more dopants are added to the calcined residue (typically a powder). For example, silicon dioxide (SiO2) gel or orthosilicic acid Tetraethylorthophosphate (TEOS) can be doped into the calcined residue. In this form, doping can be followed by drying and then calcination at a given temperature for a given time. For example, the impregnated powder can be calcined at 500° C. for 5 hours.

[0060] IV. Illustrative Uses Exemplary embodiments of the doped cerium oxide can be used in a variety of applications. In this case, doped cerium oxide can be particularly useful for using the particles as catalysts. For example, exemplary doped cerium oxide particles have , purification of exhaust gas, oxidation of carbon monoxide (CO), hydrogenation of carbon dioxide (CO2), aqueous gas Production of hydrogen gas (H2) by the water-gas shift reaction, and methane (CH4) or alcohol modification.

[0061] In some cases, an exemplary method for generating hydrogen gas (H2) can be described herein. In some cases, the method includes contacting the doped cerium oxide with a precursor material. Exemplary methods for converting carbon dioxide (CO2) to methane (CH4) are described herein. The exemplary method includes contacting the doped cerium oxide with carbon dioxide (CO2). In this case, an exemplary method for removing nitrous oxide (NO) from a feedstock is described herein. An exemplary doped cerium oxide is prepared by dissolving nitric acid (HNO3) and / or adipic acid (CH2 The method includes contacting a feedstock comprising:

[0062] V. Experimental Examples Without limiting the scope of the present disclosure, various examples of the embodiments discussed above have been prepared and The results are discussed below.

[0063] A. Preparation of Ce(OH)4 source and Ce(NO3)4 solution An experimental example of Ce(OH)4 raw material was prepared by the following procedure. First, 2.5 mol / L 0.5 L of NaOH solution having a concentration of 1.0 g was added to a 2 L beaker. The resulting mixture was The mixture was stirred at 25 to 30°C at a stirring speed of 800 to 1,000 rpm.

[0064] Next, 200-250 L of air / min is introduced into the NaOH solution through a porous air distributor. Air was then blown in at a flow rate of 100 g-CeO2 / L. The CeCl3 solution was immersed in the above air-blown NaOH solution at 25-30°C for 2 hours. The above 100g-CeO2 / L CeCl3 solution was added dropwise to approximately 300g-CeO 2 / L of initial CeCl3 solution (free [H + ]=0.1mol / L) in deionized water. It was prepared by dilution.

[0065] After 2 hours of reverse settling, the slurry was continuously aged at 25-30°C for 2 hours. The color changed from purple to yellow, and the final pH was 12.5-13.5. The mixture was filtered, washed with deionized water, and then dehydrated. + and Cl - Impurities were removed.

[0066] The first washed precipitate was placed in 1 L of 0.025 mol / L NaOH solution. Re-pulp the mixture and stir it vigorously at 25-30℃ with a stirring speed of 800-1,000 rpm. Then, air was blown into the repulped slurry at a flow rate of 200 to 250 L / hour. After aging at 25-30 °C for 1 h, the color of the slurry changed to a brighter yellow color.

[0067] The precipitate was subjected to a second filtration, five times with 1 L of deionized water (60-65 °C), and then 1 L of Wash once with HNO3 solution diluted with deionized water (pH = 4.5-5, 60-65 °C). The final residue had a pH of 8-9 and an electrical conductivity (EC) of less than 20 μS / cm. After the second washing and filtration, a Ce(OH)4 wet cake was obtained. 4. The composition has the following properties: 4+ / ΣCe=98.5%;CeO2 / TREO=99.8 %; TREO=42.0% (TREO is total rare earth oxides).

[0068] An exemplary Ce(NO3)4 solution was prepared as follows: The moist cake (TREO = 42.0%) was treated with 65-68% HNO3 / CeO2 molar ratio. = 4.5. The CeO2 solution had a concentration of about 300 g / L. The slurry was stirred and dissolved at 65-100°C for several minutes until a clear red solution was formed. Ta.

[0069] B. Preparation of Experimental Powders

[0070] [Example 1] A certain amount of Ce(NO3)4 initial solution (approximately 300 g-CeO2 / L) was dissolved in deionized water. Dilute with 0.5 L of Ce(NO3)4 solution with a concentration of 20 g-CeO2 / L. 5 wt% SiO2 powder (BET surface area = 200–250 m 2 / g) above dilution C e(NO3)4 solution.

[0071] The mixed solution was added to a 1 L autoclave, and then stirred and heated from room temperature to 125°C. The temperature was increased in 0.5 hours. The hydrolysis reaction was carried out at 125°C for 6 hours. After this time the slurry was cooled to below 50°C.

[0072] The slurry was neutralized with NH4OH solution (>25%) until a pH of 8.5 was achieved and precipitated. The mixture was then stirred for 10 minutes, and the precipitate was then filtered off.

[0073] The wet cake was dried and then heated at 300°C / 10 hours, 500°C / 8 hours, and 700°C / 10 hours. The CeO2 powder calcined at 300°C for 10 hours was then calcined at 900°C for 5 hours. It was calcined again for 5 hours.

[0074] [Example 2] The same preparation method as in Example 1 was followed, except that the amount of added SiO2 powder was changed to 10 wt%. I did.

[0075] [Example 3] After 6 hours of hydrolysis, 10 wt% SiO2 powder was added to the cooled slurry. The preparation method of Example 1 was followed except for the addition of

[0076] [Example 4] After the neutralization step with NH4OH solution, 10 wt% Si was added to the precipitated slurry. The preparation method of Example 1 was followed, except that O2 powder was added and then stirred for 30 minutes. .

[0077] [Example 5] Conventional Al2O3 powder with 10 wt% dopant (BET surface area = 200–250 m 2 The preparation method of Example 3 was followed, except that the cellulose acetate solution was changed to cellulose acetate / g.

[0078] C. Physical properties of experimental powders Various physical properties of the exemplary powders were measured and the results are shown in Table 1 below: BET surface area, The X-ray diffraction (XRD) and hydrogen temperature programmed reduction (H2-TPR) test procedures are described in more detail above. It is described in.

[0079] [Table 1]

[0080] Exemplary embodiments For reasons of completeness, various aspects of the technology are described below in numbered embodiments.

[0081] Embodiment 1. About 90 weight percent (wt%) to about 99.9 wt% cerium oxide (C eO2); and about 10 wt. % or less of a dopant. , After calcination at 500°C for 8 hours, 150m 2 / g; Oxygen storage capacity (OSC) of over 900 μmol O2 / g after calcination at 500°C for 8 hours having Doped cerium oxide particles.

[0082] Embodiment 2. The dopant is present at 0.1 wt% to 5 wt%; Dopants are silicon dioxide (SiO2) powder, silicon dioxide (SiO2) gel, ortho Tetraethyl silicate (TEOS), white carbon black, aluminum oxide (Al 2O3) powder, La2O3, Nd2O3, zeolite, or a combination thereof; 2. Doped cerium oxide particles as described in embodiment 1.

[0083] Embodiment 3. After calcination at 500° C. for 8 hours, the total particle size is 0.40 mL / g to 0.8 mL / g. 3. The doped cerium oxide particles of embodiment 1 or embodiment 2, having a pore volume.

[0084] Embodiment 4. After calcination at 500° C. for 8 hours, at least 98% of the pore volume (d>3 nm 4. The doped cerium oxide according to any one of the preceding claims, having a total pore volume of 1 / 1000 μm / (1 / 100 μm). particle.

[0085] Embodiment 5. After calcination at 700° C. for 5 hours, about 800 μmol O2 / g to about 1100 Any one of embodiments 1 to 4, having an oxygen storage capacity (OSC) of μmol·O2 / g. 3. The doped cerium oxide particles according to claim 1.

[0086] Embodiment 6. A method for producing a crystalline zeolite having a crystal size of less than 10 nm after calcination at 500° C. for 8 hours. 6. The doped cerium oxide particles of any one of the preceding claims.

[0087] Embodiment 7. After calcination at 900° C. for 5 hours, about 55 m 2 / g~about 100m 2 / g BE Doped cerium oxide particles according to any one of the preceding claims, having a specific surface area T .

[0088] Embodiment 8. The doped cerium oxide according to any one of embodiments 1 to 7 is used as a precursor. 2. A method for generating hydrogen gas (H2), comprising the step of contacting a fuel with a

[0089] Embodiment 9. The doped cerium oxide according to any one of embodiments 1 to 7 is mixed with carbon dioxide. The method includes the step of contacting carbon dioxide (CO2) with methane (CH4). How to convert.

[0090] Embodiment 10. A method for removing nitrous oxide (NO) from a feedstock comprising the steps of embodiment 1 7. The doped cerium oxide according to any one of claims 1 to 7 is mixed with nitric acid (HNO3) and / or A method comprising the step of contacting a feedstock comprising adipic acid (CH2)4(COOH)2.

[0091] Embodiment 11. A method for producing doped cerium oxide particles, comprising the steps of: The rare earth oxide concentration was 10 g to 50 g CeO2 per liter of solvent. adding at least one dopant to the Ce(NO3)4 solution; After the step of adding at least one dopant, the doped Ce(N O3) Heating the solution to cause hydrolysis; cooling the resulting mixture; neutralizing the resulting mixture to a pH of 8-9; filtering the neutralized mixture to produce a retentate and a permeate; calcining the residue; A drying step and The method includes:

[0092] Embodiment 12. The step of calcining the residue comprises calcining the residue in an environment at 300° C. for at least 10 hours. 12. The method of embodiment 11, wherein

[0093] Embodiment 13. The step of calcining the residue is carried out in an environment at 500° C. for at least 5 hours. 13. The method of claim 11 or 12, wherein

[0094] Embodiment 14. A CeO2 equivalent of 250 grams to 300 grams per liter of solvent. 14. Any of embodiments 11 to 13, further comprising diluting the Ce(NO3)4 solution. The method according to any one of the above.

[0095] Embodiment 15. The method of embodiment 14, wherein deionized water is used for dilution.

[0096] Embodiment 16. The Ce(NO3)4 solution is heated to about 120° C. to about 150° C. 16. The method according to any one of aspects 11 to 15.

[0097] Embodiment 17. The Ce(NO3)4 solution is heated for about 6 hours to about 12 hours. 6. The method according to claim 6.

[0098] Embodiment 18. The cooling step reduces the temperature of the resulting mixture to less than 50° C. 18. The method of any one of embodiments 11 to 17,

[0099] Embodiment 19. After the cooling step and before the neutralizing step, a second dopant 19. The method of any one of embodiments 11 to 18, further comprising adding

[0100] Embodiment 20. After the neutralizing step and before the filtering step, a third dopant 20. The method of any one of claims 11 to 19, further comprising adding How to.

[0101] Embodiment 21. Impregnating TEOS or SiO2 gel into the calcined residue 21. The method of any one of embodiments 11 to 20, further comprising:

[0102]

[0036] Embodiment 22. The process further comprises calcining the impregnated residue at 500°C for at least 5 hours. 22. The method according to embodiment 21, comprising:

[0103] Embodiment 23. Ammonium hydroxide (NH4OH) is used during neutralization. 23. The method according to any one of 1 to 22.

[0104] Embodiment 24. The neutralization comprises stirring; and the concentration of the NH4OH solution is at least 25%. 24. The method of embodiment 23.

[0105] Embodiment 25. The dopant is silicon dioxide (SiO2) powder, silicon dioxide (SiO2 ) gel, tetraethyl orthosilicate (TEOS), white carbon black, aluminum oxide Aluminum (Al2O3) powder, lanthanum (La), zeolite, or a combination of these 25. The method of any one of embodiments 11 to 24, comprising:

[0106] The foregoing detailed description and accompanying examples are merely illustrative and are not intended to limit the scope of the present disclosure. It should not be understood that various changes and modifications to the embodiments of the present disclosure will occur to those skilled in the art. It is clearly clear that, without limitation, chemical structures, substituents, derivatives, intermediates, Such changes and modifications, including those relating to the synthesis, composition, formulation, or method of use, , can be made without departing from the spirit and scope of the present disclosure.

Claims

1. About 90 weight percent (wt%) to about 99.9 wt% cerium oxide (CeO 2 ); and about 10 wt % or less of a dopant, The doped cerium oxide particles were calcined at 500° C. for 8 hours and then dried for 150 minutes. 2 / g; The doped cerium oxide particles had a dopant concentration of 900 μmol O after calcination at 500° C. for 8 hours. 2 / g or more of oxygen storage capacity (OSC); Doped cerium oxide particles.

2. the dopant is present at 0.1 wt % to 5 wt %; The dopant is silicon dioxide (SiO 2 ) powder, silicon dioxide (SiO 2 ) gel, tetraethyl orthosilicate (TEOS), white carbon black, aluminum oxide (Al 2 O 3 ) powder, La 2 O 3 , Nd 2 O 3 , zeolites, or combinations thereof; 2. The doped cerium oxide particles of claim 1.

3. 2. The doped cerium oxide particles of claim 1, wherein the doped cerium oxide particles have a total pore volume of 0.40 mL / g to 0.8 mL / g after calcination at 500° C. for 8 hours.

4. 2. The doped cerium oxide particles of claim 1, wherein the doped cerium oxide particles have at least 98% pore volume (d>3 nm) / total pore volume after calcination at 500° C. for 8 hours.

5. The doped cerium oxide particles had a dopant concentration of about 800 μmol O after calcination at 700° C. for 5 hours. 2 / g ~ approx. 1100 μmol・O 2 2. The doped cerium oxide particles of claim 1 having an oxygen storage capacity (OSC) of 1.0 / g.

6. 2. The doped cerium oxide particles of claim 1, wherein the doped cerium oxide particles have a crystal size of less than 10 nm after calcination at 500° C. for 8 hours.

7. The doped cerium oxide particles had a diameter of about 55 mm after calcination at 900° C. for 5 hours. 2 / g ~ approx. 100m 2 2. The doped cerium oxide particles of claim 1 having a BET specific surface area of ​​1.0 to 1.0 nm / g.

8. 2. A process for producing a cerium oxide doped cerium oxide particle according to claim 1, comprising contacting the doped cerium oxide particle with a precursor feedstock, comprising hydrogen gas (H 2 ) generation method.

9. The doped cerium oxide particles according to claim 1 are treated with carbon dioxide (CO 2 ) in contact with carbon dioxide (CO 2 ) to methane (CH 4 ) how to convert it.

10. Nitrous oxide (N 2 10. A method for removing cerium oxide from a doped cerium oxide particle according to claim 1, comprising the steps of: 3 ) and / or adipic acid (CH 2 ) 4 (COOH) 2 with a feedstock comprising: