Copper-ceramic circuit board and manufacturing method thereof

The copper-ceramic circuit board manufacturing method addresses the challenges of dimensional accuracy and productivity by using a copper plate with low roughness and precise etching resist patterns, resulting in a cost-effective solution with reduced variation.

JP2024132437APending Publication Date: 2024-10-01DOWA METALTECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023043190
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Conventional methods for manufacturing metal-ceramic circuit boards struggle with higher dimensional accuracy and productivity issues, especially with the miniaturization of wiring patterns required for power modules using wide bandgap semiconductors, and are not cost-effective.

Method used

A copper-ceramic circuit board manufacturing method involving a copper plate with an arithmetic mean roughness Ra of 0.1 μm or less, bonded to a ceramic substrate via a brazing material, with precise etching resist patterns formed to achieve high dimensional accuracy.

Benefits of technology

The method produces a copper-ceramic circuit board with significantly lower dimensional variation and improved accuracy, enhancing productivity and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132437000001_ABST
    Figure 2024132437000001_ABST
Patent Text Reader

Abstract

To provide an inexpensive copper-ceramic circuit board capable of responding to dimension accuracy higher than the prior arts (lower dimension variation) and a manufacturing method thereof.SOLUTION: A copper plate for circuit patterns and a copper plate for radiator plate patterns of which arithmetic average roughness Ra of one-side faces is equal to or less than 0.1 μm are prepared and other-side faces of the copper plate for circuit patterns and the copper plate for radiator plate patterns are bonded through a brazing filler metal to one-side face and the other-side face of a ceramic board. Thereafter, etching resists of a circuit pattern shape and a radiator plate pattern shape are formed on the one-side faces of the copper plate for circuit patterns and the copper plate for radiator plate patterns and the copper plate for circuit patterns and the copper plate for radiator plate patterns are partially etched, thereby manufacturing a copper-ceramic circuit board in which a circuit pattern copper plate 114 in the circuit pattern shape and a radiator plate pattern copper plate 116 in the radiator plate pattern shape are bonded to a ceramic board 12 via a brazing filler metal 118.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper-ceramic circuit board and a manufacturing method thereof, and in particular to a copper-ceramic circuit board in which a circuit pattern copper plate is bonded to a ceramic substrate by a brazing material. [Background technology]

[0002] Conventionally, power modules are used to control large amounts of power in electric vehicles, trains, machine tools, and the like. As an insulating substrate for such power modules, a metal-ceramic circuit board is used in which a metal circuit plate made of Cu, Al, or the like having a predetermined circuit pattern is bonded to one side of a ceramic substrate. In such a metal-ceramic circuit board, a power semiconductor such as a Si semiconductor is mounted on the metal circuit plate, and a metal heat sink is usually bonded to the other side of the ceramic substrate.

[0003] In recent years, wide band gap semiconductors such as SiC semiconductors and GaN semiconductors have begun to be used as power semiconductors instead of conventional Si semiconductors. Such wide band gap semiconductors have a low on-resistance, so they can control the same amount of power as Si semiconductors even with smaller chips compared to conventional Si semiconductor chips. For this reason, there is a demand to make the space (line and space (L / S)) of the wiring pattern of metal-ceramic circuit boards for power modules finer than before.

[0004] Also, a method has been proposed for producing a metal-ceramic circuit board, in which a metal plate is joined to at least one surface of a ceramic substrate via a brazing material, the metal plate is etched into a predetermined shape, and then the brazing material and other materials exposed by the etching are removed with a chemical solution containing a chelating agent and hydrogen peroxide, or a chemical solution containing a chelating agent, hydrogen peroxide, and an alkali, to produce a ceramic circuit board (see, for example, Patent Document 1).

[0005] In addition, a method has been proposed for producing a circuit board by forming a metal layer on at least one surface of an insulator to obtain a metal-insulator composite member, and then milling at least a portion of the metal layer to form a pattern (see, for example, Patent Document 2).

[0006] Also, a method has been proposed in which an active metal-containing brazing material is applied to almost the entire surface of one side of a ceramic substrate, a metal plate is placed on this active metal-containing brazing material to bond the metal plate to the ceramic substrate, a resist is formed on almost the entire surface of the metal plate, a laser is applied to this resist to remove predetermined portions of the resist to form a resist for forming a circuit pattern, unnecessary portions of the metal plate are etched, and then the resist for forming the circuit pattern is removed to form a plurality of circuit patterns and the unnecessary portions of the active metal-containing brazing material are removed, and then a scribe line is formed between adjacent circuit patterns on one side of the ceramic substrate, and the ceramic substrate is divided along the scribe line, thereby producing a plurality of metal-ceramic bonded circuit substrates (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2003-60111 A (paragraph number 0006) [Patent Document 2] JP 2004-296619 A (paragraph number 0008) [Patent Document 3] JP 2019-67854 A (paragraph number 0012) Summary of the Invention [Problem to be solved by the invention]

[0008] However, the methods of Patent Documents 1 and 2 could not meet the higher dimensional accuracy (lower dimensional variation) required to meet the demand for finer wiring pattern spaces (line and space (L / S)) required for metal-ceramic circuit boards for recent power modules. Also, the methods of Patent Documents 2 and 3 required many manufacturing steps and were insufficient in terms of productivity and cost.

[0009] In view of the above-mentioned problems in the prior art, the present invention has an object to provide an inexpensive copper-ceramic circuit board that can meet higher dimensional accuracy (lower dimensional variation) than in the past, and a method for manufacturing the same. [Means for solving the problem]

[0010] As a result of intensive research to solve the above-mentioned problems, the inventors have discovered that an inexpensive copper-ceramic circuit board can be manufactured that can meet higher dimensional accuracy (lower dimensional variation) than conventional methods by preparing a copper plate for a circuit pattern having an arithmetic mean roughness Ra of 0.1 μm or less on one side, joining the other side of this copper plate for a circuit pattern to one side of a ceramic substrate via a brazing material, and then forming an etching resist in the shape of a circuit pattern on one side of the copper plate for a circuit pattern and etching a portion of the copper plate for a circuit pattern to form a copper plate for a circuit pattern in the shape of a circuit pattern, thereby completing the present invention.

[0011] That is, the manufacturing method of a copper-ceramic circuit board according to the present invention is characterized in that a copper plate for a circuit pattern having an arithmetic mean roughness Ra of 0.1 μm or less on one side is prepared, the other side of this copper plate for the circuit pattern is joined to one side of a ceramic substrate via a solder material, and then an etching resist having a circuit pattern shape is formed on one side of the copper plate for the circuit pattern, and a part of the copper plate for the circuit pattern is etched to form a copper plate for a circuit pattern having the circuit pattern shape.

[0012] In this method for producing a copper-ceramic circuit board, the thickness of the copper plate for circuit pattern is preferably 0.1 to 1.0 mm, and the copper plate for circuit pattern is preferably obtained by reducing the surface roughness of one side of the copper plate by skin pass rolling or chemical polishing. The arithmetic mean roughness Ra of one side of the copper plate for circuit pattern is preferably 0.07 μm or less, and the etching resist in the shape of a circuit pattern is preferably formed by printing an etching resist ink on one side of the copper plate for circuit pattern and then curing it. The ceramic substrate is preferably made of aluminum nitride, silicon nitride or alumina, and the brazing material preferably contains silver and copper, and Ti or Zr as an active metal. Furthermore, when joining the other surface of the copper plate for the circuit pattern to one surface of the ceramic substrate via a solder material, it is preferable to join the copper plate for the heat sink pattern to the other surface of the ceramic substrate via the solder material, form an etching resist in the shape of the heat sink pattern on the surface of this copper plate for the heat sink pattern, and etch a portion of the copper plate for the heat sink pattern to form a copper plate for the heat sink pattern in the shape of the heat sink pattern.

[0013] The copper-ceramic circuit board according to the present invention is characterized in that one surface of a circuit pattern copper plate having an arithmetic mean roughness Ra of 0.1 μm or less is joined to one surface of a ceramic substrate via a brazing material.

[0014] In this copper-ceramic circuit board, it is preferable that the other surface of the heat sink copper plate having an arithmetic mean roughness Ra of 0.1 μm or less is joined to the other surface of the ceramic substrate via a brazing material. It is also preferable that the thickness of the circuit pattern copper plate is 0.1 to 1.0 mm, and that the arithmetic mean roughness Ra of one surface of the circuit pattern copper plate is 0.07 μm or less. It is also preferable that the ceramic substrate is made of aluminum nitride, silicon nitride, or alumina, and that the brazing material contains silver and copper, and contains Ti or Zr as an active metal. Effect of the Invention

[0015] According to the present invention, it is possible to provide an inexpensive copper-ceramic circuit board that can meet higher dimensional accuracy (lower dimensional variation) than conventionally, and a method for manufacturing the same. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a plan view showing a state in which a copper plate is joined to a ceramic substrate via a brazing material (copper-ceramic joined substrate) in a manufacturing process of an embodiment of a copper-ceramic circuit substrate according to the present invention. [Diagram 2] 2 is a cross-sectional view of the copper-ceramic bonding substrate taken along line II-II of FIG. 1. [Diagram 3] FIG. 2 is a plan view showing a state in which an etching resist having a circuit pattern shape is formed on a copper plate for circuit pattern of a copper-ceramic bonding substrate in a manufacturing process of an embodiment of a copper-ceramic circuit substrate according to the present invention. [Figure 4] 1 is a plan view showing a state in which an etching resist having a shape of a heat sink pattern is formed on a copper plate for a heat sink pattern of a copper-ceramic bonding substrate in a manufacturing process of an embodiment of a copper-ceramic circuit board according to the present invention. FIG. [Diagram 5] FIG. 1 is a plan view of a copper-ceramic circuit board manufactured according to an embodiment of the copper-ceramic circuit board of the present invention. [Figure 6] 6 is a cross-sectional view of the copper-ceramic bonding substrate taken along line VI-VI of FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of a copper-ceramic circuit board and a method for manufacturing the same according to the present invention will be described in detail with reference to the accompanying drawings.

[0018] In an embodiment of the method for manufacturing a copper-ceramic circuit board according to the present invention, as shown in Figures 1 and 2, a copper plate 14 for a circuit pattern and a copper plate 16 for a heat sink pattern, each having an arithmetic mean roughness Ra of 0.1 μm or less on one side, are prepared, and the other side of each of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern are bonded to each side of a ceramic substrate 12 via a brazing material 18, thereby producing a copper-ceramic bonded substrate 10.

[0019] Next, as shown in FIG. 3, an etching resist 20 having a circuit pattern shape is formed on one side of the copper plate 14 for the circuit pattern, and as shown in FIG. 4, an etching resist 22 having a heat sink pattern shape is formed on one side of the copper plate 16 for the heat sink pattern.

[0020] Next, as shown in Figures 5 and 6, parts of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern are etched to form a circuit pattern copper plate 114 in the shape of a circuit pattern and a heat sink pattern copper plate 116 in the shape of a heat sink pattern, thereby producing a copper-ceramic circuit board 100 in which the circuit pattern copper plate 114 and the heat sink pattern copper plate 116 are bonded to the ceramic substrate 12 via a brazing material 118 as an embodiment of the copper-ceramic circuit board according to the present invention.

[0021] The ceramic substrate 12 is made of a material that maintains insulation between circuit patterns on the substrate and between the front and back of the substrate, and a non-oxide ceramic substrate such as a ceramic substrate mainly composed of aluminum nitride or a ceramic substrate mainly composed of silicon nitride, or an oxide ceramic substrate mainly composed of alumina, etc. The size of the ceramic substrate 12 is preferably 5 to 200 mm in length, 5 to 200 mm in width, and 0.2 to 3.0 mm in thickness, and more preferably 10 to 100 mm in length, 10 to 100 mm in width, and 0.25 to 2.0 mm in thickness.

[0022] The copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern are preferably rolled copper plates made of oxygen-free copper plate (C1020) or the like, and the arithmetic mean roughness Ra of one surface of each of them is preferably 0.1 μm or less, more preferably 0.07 μm or less. The arithmetic mean roughness Ra of the other surface of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern may be 0.1 μm or less, or may be 0.07 μm or less. The thickness of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern used in the copper-ceramic bonding substrate 10 for the power module is about 0.1 to 1.0 mm, but the arithmetic mean roughness Ra of the surface (plate surface) of such a rolled copper plate exceeds 0.1 μm, and is usually about 0.15 to 0.3 μm. In other words, since it is not possible to make the arithmetic mean roughness Ra of the surface (sheet surface) of such a rolled copper plate 0.1 μm using a normal rolling process, when such a rolled copper plate is used as a copper plate 14 for a circuit pattern and a copper plate 16 for a heat sink pattern, each of which has an arithmetic mean roughness Ra of 0.1 μm or less on one side, it is necessary to reduce the surface roughness of one side of each of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern by using a temper rolling process such as skin pass rolling or a chemical polishing process to make the surface smooth. In this manner, by using a copper plate 14 for a circuit pattern and a copper plate 16 for a heat sink pattern, each of which has an arithmetic mean roughness Ra of 0.1 μm or less on one surface, joining the other surface of each of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern to the respective surfaces of the ceramic substrate 12 via a solder material 18, forming an etching resist 20 in the shape of a circuit pattern on one surface of the copper plate 14 for the circuit pattern and forming an etching resist 22 in the shape of a heat sink pattern on one surface of the copper plate 16 for the heat sink pattern, and then etching a portion of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern to form a circuit pattern copper plate 114 in the shape of a circuit pattern and a heat sink pattern copper plate 116 in the shape of a heat sink pattern, it is possible to obtain a circuit pattern copper plate 114 and a heat sink pattern copper plate 116 with extremely high dimensional precision (significantly low dimensional variation). From the viewpoint of manufacturing costs, it is preferable that the arithmetic mean roughness Ra of one surface of each of the copper plate 14 for circuit pattern and the copper plate 16 for heat sink pattern is 0.01 μm or more.

[0023] The brazing material 18 as a bonding material for bonding the ceramic substrate 12 to the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern is preferably a so-called Ag-Cu-Ti or Ag-Cu-Zr active metal-containing brazing material containing Ag and Cu as main components and Ti or Zr as an active metal. When using an Ag-Cu-Ti or Ag-Cu-Zr active metal-containing brazing material, the content of Ag in the brazing material (the ratio of the mass of Ag to the total mass of the metal components contained in the brazing material) is not particularly limited, but is preferably 30 to 95 mass%, more preferably 50 to 90 mass%, and most preferably 65 to 90 mass%, from the viewpoint of improving reliability such as bonding strength. In addition, the content of the active metal component in the brazing material (the ratio of the mass of the active metal component to the total mass of the metal components contained in the brazing material) is preferably 1.0 to 7.0 mass%, and more preferably 1.5 to 6.5 mass%. By using such a brazing material, the bonding strength between the ceramic substrate 12 and the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern can be improved. When an Ag-Cu-based active metal-containing brazing material is used as the active metal-containing brazing material, the content of the metal components other than Ag and the active metal components (the remaining part) is the Cu content. Although a paste-like or foil-like brazing material can be used as the brazing material 18, it is preferable to use a paste-like brazing material from the viewpoint of manufacturing cost and workability. When a paste-like brazing material is used, for example, the brazing material 18 can be formed on the ceramic substrate 12 by applying it on the ceramic substrate 12 by a screen printing method or the like and then drying it at 200°C or less in the air or in an inert gas atmosphere. The thickness of the brazing material 18 is not particularly limited, but is preferably 3 to 50 μm, more preferably 5 to 20 μm, from the viewpoint of ensuring the thermal shock resistance and bonding strength of the copper-ceramic bonding substrate 10.

[0024] The etching resist 20 in the shape of a circuit pattern and the etching resist 22 in the shape of a heat sink pattern are preferably formed by printing and curing using a known method such as screen printing, lamination, or photomask, but from the viewpoint of productivity, it is preferable to form them by printing and curing an etching resist ink by screen printing. As the etching resist ink, it is preferable to use an ultraviolet-curing alkali-peeling type etching resist ink.

[0025] The etching of a part (unnecessary part) of the copper plate 14 for the circuit pattern and the copper plate 16 for the heat sink pattern (parts of the copper plate 114 for the circuit pattern and the copper plate 116 for the heat sink pattern on which no etching resist is formed) is carried out by removing a known etching solution, for example, an etching solution containing cupric chloride, ferric chloride or hydrogen peroxide, and then using hydrofluoric acid or a chelating agent, etc., to remove unnecessary brazing material (remaining on the surface of the ceramic substrate 12 around the copper plate 114 for the circuit pattern and the copper plate 116 for the heat sink pattern), thereby forming the desired copper plate 114 for the circuit pattern and the copper plate 116 for the heat sink pattern, thereby producing the copper-ceramic circuit substrate 100. The surfaces of the copper plate 114 for the circuit pattern and the copper plate 116 for the heat sink pattern of the copper-ceramic circuit substrate 100 thus produced may be plated by electroless Ni-P plating, electric Ni plating, etc.

[0026] In addition, when the etching resist 20 in the shape of a circuit pattern is formed, for example, by a screen printing method, if the surface of the copper plate 14 for the circuit pattern has large irregularities, the difference in the spread of the etching resist ink will become large depending on the location, and it is thought that the dimensional variation between the etching resist 20 and the circuit pattern copper plate 114 will increase.

[0027] In the embodiment of the copper-ceramic circuit board according to the present invention manufactured by the embodiment of the manufacturing method of the copper-ceramic circuit board according to the present invention described above, one surface of the circuit pattern copper plate having an arithmetic mean roughness Ra of 0.1 μm or less is joined to one surface of the ceramic substrate via a brazing material, and preferably, the other surface of the heat sink pattern copper plate having one surface of an arithmetic mean roughness Ra of 0.1 μm or less is joined to the other surface of the ceramic substrate via a brazing material.

[0028] In this embodiment of the copper-ceramic circuit board, the thickness of the circuit pattern copper plate 114 is preferably 0.1 to 1.0 mm, and the arithmetic mean roughness Ra of one surface of the circuit pattern copper plate 114 is preferably 0.07 μm or less. The ceramic substrate 12 is preferably made of aluminum nitride, silicon nitride, or alumina, and the brazing material 18 preferably contains silver and copper, and contains Ti or Zr as an active metal. EXAMPLES

[0029] Hereinafter, examples of the copper-ceramic circuit board and the manufacturing method thereof according to the present invention will be described in detail.

[0030] [Example 1] An aluminum nitride (AlN) substrate measuring 68 mm x 68 mm x 0.38 mm was prepared as a ceramic substrate. This AlN substrate had dividing lines (division grooves) so that it could be divided into four substrates measuring 34 mm x 34 mm x 0.38 mm.

[0031] In addition, oxygen-free copper plates (C1020-1 / 2H) measuring 70 mm x 70 mm x 0.15 mm were prepared as copper plates for circuit patterns and heat sink patterns, and the surface roughness of the copper plates was reduced by skin pass rolling (by adjusting the surface roughness of the rolling rolls and the load during rolling). The surface roughness of one side of this copper plate was measured according to JIS B0601 (2001) using a laser microscope (VK-X1000 manufactured by Keyence Corporation) with cutoff values ​​λs = 2.5 μm, λc = 0.8 mm, and (horizontal) measurement distance = 200 μm, and the arithmetic mean roughness Ra of one side of the copper plate was 0.028 μm. In addition, an Ag-Cu-Ti brazing material paste (mass ratio Ag:Cu:Ti=88:10:2) containing Ti as an active metal was prepared as a brazing material for joining the ceramic substrate and the copper plate.

[0032] Next, the brazing material was applied to substantially the entire surfaces of both sides of the ceramic substrate by screen printing, and the brazing material was dried in the air to form the brazing material on both sides of the ceramic substrate.

[0033] Next, the copper plate for the circuit pattern and the copper plate for the heat sink pattern were placed on the brazing material on both sides of the ceramic substrate so that the other side of each copper plate was in contact with the brazing material to form a laminate, and this laminate was heated in a vacuum furnace at 830°C and then cooled to produce a copper-ceramic bonded substrate in which the copper plate for the circuit pattern and the copper plate for the heat sink pattern were bonded to both sides of the ceramic substrate via the brazing material.

[0034] Next, an ultraviolet-curable alkaline peelable etching resist ink having the shape of the circuit pattern and the shape of the heat sink pattern was applied by screen printing to the surfaces of the copper plate for the circuit pattern and the copper plate for the heat sink pattern of the above-mentioned copper-ceramic bonding substrate, respectively, and cured by ultraviolet light to form an etching resist on the copper plate for the circuit pattern and the copper plate for the heat sink pattern.

[0035] Next, unnecessary portions (portions not covered with the etching resist) of the copper plate for the circuit pattern and the copper plate for the heat sink pattern were etched away using an etching solution containing copper chloride, and then the etching resist was peeled off and removed using an aqueous sodium hydroxide solution to form the copper plate for the circuit pattern and the copper plate for the heat sink pattern.

[0036] Next, unnecessary solder material remaining around the copper plate for the circuit pattern and the copper plate for the heat sink pattern on the ceramic substrate was etched away using an etching solution containing ethylenediaminetetraacetic acid (EDTA), and the ceramic substrate was then divided into four along the dividing lines to produce four copper-ceramic circuit substrates in which the copper plate for the circuit pattern and the copper plate for the heat sink pattern were bonded to both sides of the ceramic substrate.

[0037] In addition, after forming an etching resist on the copper plate for the circuit pattern and the copper plate for the heat sink pattern of the above-mentioned copper-ceramic bonding substrate, and before removing unnecessary portions of the copper plate for the circuit pattern and the copper plate for the heat sink pattern by etching, in order to evaluate the adhesion of the etching resist on the copper plate for the circuit pattern, 10 of the above-mentioned copper-ceramic bonding substrates were prepared, and 25 squares of 2 mm square were formed on the surface of the etching resist on the copper plate for the circuit pattern of each copper-ceramic bonding substrate with a cutter, and then adhesive tape (cellophane tape made by Nichiban) was attached, and a cross-cut tape peeling test was performed in accordance with JIS H8504 to visually evaluate whether the etching resist had peeled off. As a result, none of the 25 squares of the etching resist had peeled off in any of the 10 copper-ceramic bonding substrates, and the adhesion of the etching resist was very good.

[0038] In addition, after forming an etching resist on the copper plate for the circuit pattern and the copper plate for the heat sink pattern of the above-mentioned copper-ceramic bonding substrate, and before etching away unnecessary portions of the copper plate for the circuit pattern and the copper plate for the heat sink pattern, in order to evaluate the dimensional variation of the etching resist on the copper plate for the circuit pattern, 10 of the above-mentioned copper-ceramic bonding substrates were prepared and the dimensions between adjacent etching resists (between circuit patterns) were measured using a high-precision image dimension measuring device (High-Precision Image Dimension Measuring Device LM-1000 manufactured by Keyence Corporation).The average of the dimensions between adjacent etching resists (between circuit patterns) (target value: 0.5 mm) was 0.533 mm, the difference between the maximum and minimum values ​​(variation range) was 0.007 mm, and the standard deviation was 0.003 mm, indicating that the dimensional variation of the etching resist was very small.

[0039] In addition, in order to evaluate the dimensional variation of the circuit pattern on the copper plate of the circuit pattern of the fabricated copper-ceramic circuit board, 10 of the above copper-ceramic circuit boards were prepared, and the dimensions between adjacent circuit patterns were measured using a high-precision image dimension measuring device (High-Precision Image Dimension Measuring Device LM-1000 manufactured by Keyence Corporation).The average dimension between adjacent circuit patterns (target value 0.8 mm) was 0.828 mm, the difference between the maximum and minimum values ​​(variation range) was 0.026 mm, and the standard deviation was 0.009 mm, indicating that the dimensional variation of the circuit patterns was extremely small.

[0040] [Example 2] An aluminum nitride (AlN) substrate measuring 68 mm × 68 mm × 0.64 mm with dividing lines (dividing grooves) so that it could be divided into four substrates measuring 34 mm × 34 mm × 0.64 mm was used as the ceramic substrate, and an oxygen-free copper plate (C1020-1 / 2H) measuring 70 mm × 70 mm × 0.25 mm was used as the copper plate for the circuit pattern and the copper plate for the heat sink pattern. A copper-ceramic bonding substrate and a copper-ceramic circuit substrate were produced in the same manner as in Example 1, except that the surface roughness of the copper plate was reduced by skin pass rolling so that the arithmetic mean roughness Ra of one side of the copper plate was 0.038 μm.

[0041] The adhesion of the etching resist on the copper plate for the circuit pattern of the above copper-ceramic bonding substrate was evaluated in the same manner as in Example 1. As a result, none of the 25 squares of the etching resist had peeled off in any of the 10 copper-ceramic bonding substrates, and the adhesion of the etching resist was very good.

[0042] In addition, when the dimensional variation of the etching resist on the copper plate for the circuit pattern of the above-mentioned copper-ceramic bonding substrate was evaluated by the same method as in Example 1, the average dimension (target value: 0.5 mm) between adjacent etching resists (between circuit patterns) was 0.532 mm, the difference between the maximum and minimum values ​​(variation range) was 0.008 mm, and the standard deviation was 0.004 mm, indicating that the dimensional variation of the etching resist was very small.

[0043] In addition, when the dimensional variation of the circuit pattern on the circuit pattern copper plate of the above copper-ceramic circuit board was evaluated in the same manner as in Example 1, the average of the dimension between adjacent circuit patterns (target value 0.8 mm) was 0.829 mm, the difference between the maximum and minimum values ​​(variation range) was 0.036 mm, and the standard deviation was 0.011 mm, indicating that the dimensional variation of the circuit pattern was very small.

[0044] [Example 3] An aluminum nitride (AlN) substrate measuring 68 mm x 68 mm x 1.0 mm with dividing lines (dividing grooves) so that it could be divided into four substrates measuring 34 mm x 34 mm x 1.0 mm was used as the ceramic substrate, and an oxygen-free copper plate (C1020-1 / 2H) measuring 70 mm x 70 mm x 0.40 mm was used as the copper plate for the circuit pattern and the copper plate for the heat sink pattern. A copper-ceramic bonding substrate and a copper-ceramic circuit substrate were produced in the same manner as in Example 1, except that the surface roughness of the copper plate was reduced by skin pass rolling so that the arithmetic mean roughness Ra of one side of the copper plate was 0.047 μm.

[0045] The adhesion of the etching resist on the copper plate for the circuit pattern of the above copper-ceramic bonding substrate was evaluated in the same manner as in Example 1. As a result, none of the 25 squares of the etching resist had peeled off in any of the 10 copper-ceramic bonding substrates, and the adhesion of the etching resist was very good.

[0046] In addition, when the dimensional variation of the etching resist on the copper plate for the circuit pattern of the above-mentioned copper-ceramic bonding substrate was evaluated by the same method as in Example 1, the average dimension (target value: 0.5 mm) between adjacent etching resists (between circuit patterns) was 0.528 mm, the difference between the maximum and minimum values ​​(variation range) was 0.011 mm, and the standard deviation was 0.004 mm, indicating that the dimensional variation of the etching resist was very small.

[0047] In addition, when the dimensional variation of the circuit pattern on the circuit pattern copper plate of the above copper-ceramic circuit board was evaluated in the same manner as in Example 1, the average of the dimensions between adjacent circuit patterns (target value: 0.8 mm) was 0.830 mm, the difference between the maximum and minimum values ​​(variation range) was 0.042 mm, and the standard deviation was 0.013 mm, indicating that the dimensional variation of the circuit pattern was very small.

[0048] [Example 4] A silicon nitride substrate measuring 68 mm x 68 mm x 0.32 mm with dividing lines (dividing grooves) so that it could be divided into four substrates measuring 34 mm x 34 mm x 0.32 mm was used as the ceramic substrate, and an oxygen-free copper plate (C1020-1 / 2H) measuring 70 mm x 70 mm x 0.80 mm was used as the copper plate for the circuit pattern and the copper plate for the heat sink pattern. A copper-ceramic bonding substrate and a copper-ceramic circuit substrate were produced in the same manner as in Example 1, except that the surface roughness of the copper plate was reduced by skin pass rolling so that the arithmetic mean roughness Ra of one side of the copper plate was 0.092 μm.

[0049] The adhesion of the etching resist on the copper plate for the circuit pattern of the above copper-ceramic bonding substrate was evaluated in the same manner as in Example 1. As a result, none of the 25 squares of the etching resist had peeled off in any of the 10 copper-ceramic bonding substrates, and the adhesion of the etching resist was very good.

[0050] In addition, when the dimensional variation of the etching resist on the copper plate for the circuit pattern of the above-mentioned copper-ceramic bonding substrate was evaluated in the same manner as in Example 1, the average dimension (target value: 0.5 mm) between adjacent etching resists (between circuit patterns) was 0.535 mm, the difference between the maximum and minimum values ​​(variation range) was 0.013 mm, and the standard deviation was 0.005 mm, indicating that the dimensional variation of the etching resist was very small.

[0051] In addition, when the dimensional variation of the circuit pattern on the circuit pattern copper plate of the above copper-ceramic circuit board was evaluated in the same manner as in Example 1, the average of the dimension between adjacent circuit patterns (target value: 0.8 mm) was 0.836 mm, the difference between the maximum and minimum values ​​(variation range) was 0.052 mm, and the standard deviation was 0.014 mm, indicating that the dimensional variation of the circuit pattern was very small.

[0052] [Comparative Example 1] As the copper plate for the circuit pattern and the copper plate for the heat sink pattern, oxygen-free copper plates (C1020-1 / 2H) measuring 70 mm × 70 mm × 0.25 mm and having an arithmetic mean roughness Ra of 0.146 μm were used, and a copper-ceramic bonding substrate and a copper-ceramic circuit substrate were produced in the same manner as in Example 2, except that skin pass rolling was not performed on the surface of the copper plate.

[0053] The adhesion of the etching resist on the copper plate for the circuit pattern of the above copper-ceramic bonding substrate was evaluated in the same manner as in Example 1. As a result, none of the 25 squares of the etching resist had peeled off in any of the 10 copper-ceramic bonding substrates, and the adhesion of the etching resist was very good.

[0054] In addition, when the dimensional variation of the etching resist on the copper plate for the circuit pattern of the above-mentioned copper-ceramic bonding substrate was evaluated by the same method as in Example 1, the average dimension (target value: 0.5 mm) between adjacent etching resists (between circuit patterns) was 0.552 mm, the difference between the maximum and minimum values ​​(variation range) was 0.060 mm, and the standard deviation was 0.014 mm, indicating that the dimensional variation of the etching resist was large.

[0055] In addition, when the dimensional variation of the circuit pattern on the circuit pattern copper plate of the above copper-ceramic circuit board was evaluated in the same manner as in Example 1, the average of the dimensions between adjacent circuit patterns (target value: 0.8 mm) was 0.850 mm, the difference between the maximum and minimum values ​​(variation range) was 0.103 mm, and the standard deviation was 0.020 mm, indicating that the dimensional variation of the circuit pattern was very large.

[0056] [Comparative Example 2] As the copper plate for the circuit pattern and the copper plate for the heat sink pattern, oxygen-free copper plates (C1020-1 / 2H) measuring 70 mm × 70 mm × 0.25 mm and having an arithmetic mean roughness Ra of 0.246 μm were used, and a copper-ceramic bonding substrate and a copper-ceramic circuit substrate were produced in the same manner as in Example 2, except that skin pass rolling was not performed on the surface of the copper plate.

[0057] The adhesion of the etching resist on the copper plate for the circuit pattern of the above copper-ceramic bonding substrate was evaluated in the same manner as in Example 1. As a result, none of the 25 squares of the etching resist had peeled off in any of the 10 copper-ceramic bonding substrates, and the adhesion of the etching resist was very good.

[0058] In addition, when the dimensional variation of the etching resist on the copper plate for the circuit pattern of the above-mentioned copper-ceramic bonding substrate was evaluated by the same method as in Example 1, the average dimension (target value: 0.5 mm) between adjacent etching resists (between circuit patterns) was 0.550 mm, the difference between the maximum and minimum values ​​(variation range) was 0.092 mm, and the standard deviation was 0.021 mm, indicating that the dimensional variation of the etching resist was large.

[0059] In addition, when the dimensional variation of the circuit pattern on the circuit pattern copper plate of the above copper-ceramic circuit board was evaluated in the same manner as in Example 1, the average of the dimensions between adjacent circuit patterns (target value: 0.8 mm) was 0.855 mm, the difference between the maximum and minimum values ​​(variation range) was 0.180 mm, and the standard deviation was 0.030 mm, indicating that the dimensional variation of the circuit pattern was very large. [Explanation of symbols]

[0060] 10 Copper-ceramic bonded substrate 12 Ceramic substrate 14 Copper plate for circuit patterns 16 Copper plate for heat sink pattern 18 Brazing material 20 Circuit pattern etching resist 22 Etching resist for heat sink pattern 100 Copper-ceramic circuit board 114 Circuit Pattern Copper Plate 116 Heat sink pattern copper plate 118 Brazing material

Claims

1. A method for producing a copper-ceramic circuit board, comprising the steps of: preparing a copper plate for a circuit pattern having one surface with an arithmetic mean roughness Ra of 0.1 μm or less; joining the other surface of the copper plate for the circuit pattern to one surface of a ceramic substrate via a brazing material; forming an etching resist in the shape of a circuit pattern on one surface of the copper plate for the circuit pattern; and etching a portion of the copper plate for the circuit pattern to form a copper plate for a circuit pattern in the shape of a circuit pattern.

2. 2. The method for producing a copper-ceramic circuit board according to claim 1, wherein the copper plate for circuit pattern has a thickness of 0.1 to 1.0 mm.

3. 2. The method for producing a copper-ceramic circuit board according to claim 1, wherein the copper plate for circuit pattern is obtained by reducing the surface roughness of one surface of a copper plate by skin pass rolling or chemical polishing.

4. 2. The method for producing a copper-ceramic circuit board according to claim 1, wherein the arithmetic mean roughness Ra of one surface of the copper plate for circuit pattern is 0.07 μm or less.

5. 2. The method for producing a copper-ceramic circuit board according to claim 1, wherein the etching resist having the circuit pattern shape is formed by printing an etching resist ink on one surface of the copper plate for circuit pattern and then curing the ink.

6. 2. The method for producing a copper-ceramic circuit board according to claim 1, wherein the ceramic substrate is made of aluminum nitride, silicon nitride or alumina.

7. 2. The method for producing a copper-ceramic circuit board according to claim 1, wherein the brazing material contains silver and copper, and contains Ti or Zr as an active metal.

8. The method for manufacturing a copper-ceramic circuit board according to claim 1, characterized in that when the other surface of the copper plate for the circuit pattern is joined to one surface of the ceramic substrate via a brazing material, a copper plate for a heat sink pattern is joined to the other surface of the ceramic substrate via a brazing material, an etching resist having a shape of the heat sink pattern is formed on the surface of the copper plate for the heat sink pattern, and a part of the copper plate for the heat sink pattern is etched to form a copper plate for the heat sink pattern having the shape of the heat sink pattern.

9. A copper-ceramic circuit board, characterized in that one surface of a circuit pattern copper plate having an arithmetic mean roughness Ra of 0.1 μm or less is joined to one surface of a ceramic substrate via a brazing material.

10. The copper-ceramic circuit board according to claim 9, characterized in that the other surface of the heat sink pattern copper plate having an arithmetic mean roughness Ra of 0.1 μm or less on one surface is joined to the other surface of the ceramic substrate via a brazing material.

11. 10. The copper-ceramic circuit board according to claim 9, wherein the thickness of the circuit pattern copper plate is 0.1 to 1.0 mm.

12. 10. The copper-ceramic circuit board according to claim 9, wherein the arithmetic mean roughness Ra of one surface of the circuit pattern copper plate is 0.07 μm or less.

13. 10. The copper-ceramic circuit board according to claim 9, wherein the ceramic substrate is made of aluminum nitride, silicon nitride or alumina.

14. 10. The copper-ceramic circuit board according to claim 9, wherein the brazing material contains silver and copper, and contains Ti or Zr as an active metal.

Citation Information

Patent Citations

  • Manufacture of ceramic circuit substrate

    JP1989251690A

  • Method of manufacturing metal-ceramic joined circuit board

    JP2003110222A

  • Substrate for power module and manufacturing method therefor

    WO2013146881A1

  • Semiconductor circuit board, semiconductor device using same, and method for producing semiconductor circuit board

    WO2014054609A1