Multilayer ceramic capacitor

By designing the external electrode with a recessed shape formed by three ridges at different positions, the multilayer ceramic capacitor addresses issues of poor formation and thinning, improving reliability and moisture resistance.

JP2024132655APending Publication Date: 2024-10-01TAIYO YUDEN KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023043509
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The reduction in thickness of external electrodes in multilayer ceramic capacitors leads to poor electrode formation and increased vulnerability to deterioration factors, such as moisture intrusion, reducing reliability.

Method used

The external electrode is designed with a specific shape that covers the top portion of the multilayer chip, formed by arranging the end points of three ridges at different positions, creating a planar shape that is recessed inside the chip, thereby preventing poor formation and excessive thinning.

Benefits of technology

This design effectively suppresses defective electrode formation and excessive thinning, enhancing the capacitor's reliability by preventing moisture intrusion and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132655000001_ABST
    Figure 2024132655000001_ABST
Patent Text Reader

Abstract

To provide a multilayer ceramic capacitor in which a formation failure and an extreme thin layer are suppressed in an external electrode in a top part of a lamination chip.SOLUTION: A multilayer ceramic capacitor includes: a leading part in which a dielectric layer formed by a dielectric porcelain and an internal electrode containing a metal as a main component are alternately laminated, and in which the internal electrode is led out onto a surface that is parallel to a lamination direction; a rectangular shaped lamination chip 30 that includes a protection part containing a dielectric porcelain on a front surface other than the leading part; and an external electrode in which both of the internal electrodes led to the leading part are connected to the front surface of the layer chip, and that is provided by overlapping at least one rectangular top part formed by the lamination chip is overlapped. The top part overlapped by the external electrode of the lamination chip is formed by arranging both of end points e1, e2, and e3 of three ridge lines at a different position each other, and has a flat surface P passing through each end point of the three ridge lines or a shape concaved to an inner side of the lamination chip from the flat surface a flat surface P.SELECTED DRAWING: Figure 3c
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer ceramic capacitor. [Background technology]

[0002] In recent years, with the miniaturization of electronic devices, there is a demand for further miniaturization of the multilayer ceramic capacitors used therein. Means for miniaturizing a multilayer ceramic capacitor while maintaining its capacitance include reducing the thickness of the dielectric layers and internal electrodes, combining the thinning with an increase in the number of laminated dielectric layers and internal electrodes, and reducing the thickness of the external electrodes.

[0003] A known multilayer ceramic capacitor includes a rectangular parallelepiped laminated chip in which dielectric layers and internal electrodes are alternately stacked, the internal electrodes being drawn out every other layer to a pair of opposing pull-out surfaces parallel to the stacking direction, and the chip having a protective section containing dielectric ceramic on surfaces other than the pull-out surfaces, and an external electrode formed on a surface of the laminated chip that electrically connects the internal electrodes drawn out to the pull-out surfaces and wraps around from the pull-out surfaces to the surface of the protective section.

[0004] In a multilayer ceramic capacitor having the above-described structure, when the thickness of the external electrodes is reduced, the function of the external electrodes in preventing the intrusion of degradation factors such as moisture is reduced, resulting in a problem of reduced reliability.

[0005] The above-mentioned problems include the intrusion of a plating solution when plating is performed on a base layer to form an external electrode composed of multiple metal layers. As a means for solving such problems, Patent Document 1 discloses that the thickness of the external electrode satisfies 0.8≦|T1 / Tc|≦1.0, where Tc is the thickness of the central region in the thickness direction of the ceramic body, and T1 is the thickness at a point 25% of the length S in the thickness direction of the ceramic body away from the central region of the capacitance forming part where the internal electrodes are laminated and contribute to capacitance formation.

[0006] Furthermore, Patent Document 2 discloses that, as a means for suppressing the occurrence of cracks due to thermal stress caused by differences in thermal expansion coefficients between the ceramic dielectric layers and protective portion, and the metal external electrodes in a multilayer ceramic capacitor having the above-mentioned structure, the multilayer ceramic capacitor is structured such that the end faces (extraction faces) are connected to each other at a ridge portion having a recess, and the base film of the external electrode formed within the recess is separated from at least one of the base films formed on the peripheral surface (protective portion). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-149939 A [Patent Document 2] JP 2020-102479 A Summary of the Invention [Problem to be solved by the invention]

[0008] In a multilayer ceramic capacitor having the structure described above, when the thickness of the external electrodes is reduced, the external electrodes may be poorly formed or extremely thin at the apex where the pull-out surface of the multilayer chip and two protective parts that are perpendicular to and perpendicular to each other intersect, causing the problem of degradation factors entering through these points.

[0009] SUMMARY OF THE PRESENT DISCLOSURE An object of the present invention is to provide a multilayer ceramic capacitor in which poor formation of external electrodes on the top of a multilayer chip and excessive thinning are suppressed. [Means for solving the problem]

[0010] The inventors conducted various studies to solve the above-mentioned problems and discovered that by specifying the shape of the tops of the laminated chips that make up a multilayer ceramic capacitor, which are covered by the external electrodes, poor formation of the external electrodes and excessive thinning can be suppressed, which led to the completion of the present invention.

[0011] That is, a first aspect of the present invention for solving the above problem is a laminated ceramic capacitor comprising: a rectangular parallelepiped-shaped laminated chip in which dielectric layers formed of dielectric ceramic and internal electrodes mainly composed of metal are alternately stacked, the laminated chip having an extension portion from which the internal electrodes are extended on a surface parallel to the stacking direction, and a protective portion containing dielectric ceramic on a surface other than the extension portion; and an external electrode on a surface of the laminated chip, the external electrode electrically connecting the internal electrodes extended to the extension portion and covering at least one apex of the rectangular parallelepiped formed by the laminated chip, the apex of the laminated chip covered by the external electrode being formed by arranging the end points of three ridges at mutually different positions, and having a planar shape passing through each of the end points, or a shape recessed inward of the laminated chip from the plane.

[0012] A second aspect of the present invention for solving the above-mentioned problem comprises preparing a powder of a dielectric ceramic composition, mixing the powder of the dielectric ceramic composition with a binder and forming the mixture into a sheet to obtain a green sheet, forming an internal electrode pattern containing a metal on the green sheet, forming a dielectric pattern at a location on the green sheet where the internal electrode pattern is not formed, with a gap therebetween from a point that will become a ridge extending in a stacking direction in a pre-fired laminated chip to be described later, stacking a predetermined number of green sheets on which the internal pattern and the dielectric pattern are formed, and providing a protective green sheet on both ends in the stacking direction. and then pressing the laminated body using a flexible jig to obtain a raw laminate; singulating the raw laminate to obtain a pre-fired laminated chip having a rectangular parallelepiped shape, the pre-fired laminated chip having an internal electrode pattern drawn out on a plane parallel to the lamination direction, each apex being formed by arranging end points of three ridges at different positions from one another and having a shape recessed inwardly of the laminated chip with respect to a plane passing through each end point; removing the binder from the pre-fired laminated chip; and performing either one of the following (a) or (b). (a) After the binder is removed, a paste for external electrodes is applied to the surface of the pre-fired laminated chip, covering the lead-out portion and the top of the rectangular parallelepiped, and then the pre-fired laminated chip with the external electrodes attached is fired to obtain a sintered body. (b) After the binder has been removed, the pre-fired laminated chip is fired to obtain a laminated chip, and then a paste for external electrodes is applied to the surface of the laminated chip, covering the lead-out portions and the top of the rectangular parallelepiped, and baked. Effect of the Invention

[0013] According to the present invention, it is possible to provide a multilayer ceramic capacitor in which poor formation of external electrodes on the top of a laminated chip and excessive thinning are suppressed. [Brief description of the drawings]

[0014] [Figure 1] 1 is a schematic view (overall perspective view) showing a structure of a multilayer ceramic capacitor according to a first embodiment of the present invention. [Figure 2a] 1 is a schematic diagram showing a structure of a multilayer ceramic capacitor according to a first embodiment of the present invention (a cross-sectional view taken along the line AA in FIG. 1). [Figure 2b] 1 is a schematic diagram showing a structure of a multilayer ceramic capacitor according to a first embodiment of the present invention (a cross-sectional view taken along the line BB in FIG. 1). [Figure 2c] 1 is a schematic diagram showing a structure of a multilayer ceramic capacitor according to a first embodiment of the present invention (a cross-sectional view taken along line CC in FIG. 1). [Figure 2d] 1 is a schematic diagram (a cross-sectional view taken along the line DD in FIG. 1) showing a structure of a multilayer ceramic capacitor according to a first embodiment of the present invention. [Figure 3a] 1 is a perspective view showing an example of the shape of a top portion covered with an external electrode of a multilayer chip included in the multilayer ceramic capacitor according to the first embodiment of the present invention. FIG. [Figure 3b] 5 is a perspective view showing another example of the shape of the top portion covered with external electrodes of the multilayer chip included in the multilayer ceramic capacitor according to the first embodiment of the present invention. FIG. [Figure 3c]10 is a perspective view showing still another example of the shape of the top portion covered with an external electrode of the multilayer chip included in the multilayer ceramic capacitor according to the first embodiment of the present invention. FIG. [Figure 4a] 1 is an overall perspective view showing a maximum dimension tmax and a minimum dimension tmin in the lamination direction on a plane parallel to the lamination direction, of a laminated chip included in a multilayer ceramic capacitor according to a first aspect of the present invention. FIG. [Figure 4b] FIG. 2 is an overall perspective view showing a maximum dimension wmax and a minimum dimension wmin in the width direction in a plane parallel to the width direction, and a maximum dimension lmax and a minimum dimension lmin in the length direction in a plane parallel to the length direction, for a laminated chip provided in a multilayer ceramic capacitor according to a first aspect of the present invention. [Diagram 5] 2B is a schematic diagram showing a structure of a first modified example of the multilayer ceramic capacitor according to the first aspect of the present invention (a cross-sectional view taken at a position corresponding to FIG. 2C). [Figure 6] 1 is a schematic view (overall perspective view) showing a structure of a second modified example of the multilayer ceramic capacitor according to the first aspect of the present invention. [Figure 7] 5 is a plan view showing an example of the arrangement of internal electrode patterns and dielectric patterns on a green sheet in a manufacturing method for a multilayer ceramic capacitor according to a second aspect of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The configuration and effects of the present invention will be described below with reference to the drawings, together with the technical concept. However, the mechanism of action includes assumptions, and the correctness of such assumptions does not limit the present invention.

[0016] [Multilayer ceramic capacitors] <First embodiment> FIG. 1 shows an embodiment of a multilayer ceramic capacitor according to a first aspect of the present invention as a first embodiment. The multilayer ceramic capacitor 100 according to the first embodiment has a rectangular parallelepiped shape and includes a pair of faces perpendicular to three mutually perpendicular axes, i.e., an L axis in the length direction, a W axis in the width direction, and a T axis in the height direction. The rectangular parallelepiped is not limited to a mathematically defined rectangular parallelepiped, and may have any shape that is recognized as a rectangular parallelepiped when the overall shape is observed. For this reason, a rectangular parallelepiped having rounded edges or corners, a curved edge, or a curved surface with a small curvature also falls under the category of a rectangular parallelepiped in the present disclosure. The length (L) dimension, width (W) dimension, and height (T) dimension of the ceramic capacitor 100 may each independently take any value, and the magnitude relationship between them is not limited. For example, the relationship may be (L direction dimension)>(W direction dimension)≧(T direction dimension), or the relationship may be (W direction dimension)>(L direction dimension), or the relationship may be (T direction dimension)>(W direction dimension).

[0017] As shown in cross-sectional views of FIG. 2a (LT cross section) and FIG. 2b (WT cross section), the multilayer ceramic capacitor 100 according to the first embodiment includes a multilayer chip 30 in which dielectric layers 10 made of dielectric ceramic and internal electrodes 20 mainly made of metal are alternately laminated in the T direction. The multilayer chip 30 has a pair of lead-out portions 40a and 40b on a surface parallel to the lamination direction (T direction) from which the internal electrodes are drawn out every other layer. That is, the multilayer chip 30 has a lead-out surface 40a from which the internal electrodes 20a are drawn out in the L direction, and a lead-out surface 40b from which the internal electrodes 20b are drawn out in the L direction. In the multilayer ceramic capacitor 100 shown in FIG. 1, the pair of lead-out portions 40a and 40b are formed on substantially the entire areas of the mutually facing surfaces perpendicular to the L direction, but the arrangement of the lead-out portions in the multilayer ceramic capacitor according to the first aspect of the present invention is not limited thereto. The lead-out portion may be formed only in a part of a plane parallel to the lamination direction, may be formed only in one plane, or may be formed in a plurality of pairs. The multilayer ceramic capacitor 100 has a protective portion 50 including a dielectric ceramic on a surface other than the lead-out portion. The protective portion 50 includes a cover portion 51 arranged on a surface perpendicular to the T direction and a side margin portion 52 arranged on a surface perpendicular to the W direction. The multilayer ceramic capacitor 100 according to the first embodiment includes external electrodes 60a and 60b that are provided on the surface of the laminated chip 30 so as to cover at least one apex of the rectangular parallelepiped and electrically connect the internal electrodes led out to the lead-out portions 40a and 40b.

[0018] Hereinafter, each component constituting the multilayer ceramic capacitor 100 according to the first embodiment will be described in detail.

[0019] (Dielectric layer) The dielectric layer 10 is made of a dielectric ceramic. The composition of the dielectric ceramic is not particularly limited and may be appropriately selected according to the characteristics required for the multilayer ceramic capacitor. A preferable composition of the dielectric ceramic is, for example, one containing barium titanate (BaTiO3) as a main component. The dielectric layer 10 may contain the following additive elements. Examples of the additive elements include at least one selected from Mo, Nb, Ta, W, Mg, Mn, V, Cr, rare earth elements (Y, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, and Yb), and Co, Ni, Li, B, Na, K, and Si. The additive elements may be contained as simple elements or in the form of compounds such as oxides, nitrides, and carbides. The additive elements may be present in a state of solid solution in the main component barium titanate, or may form a different phase with the elements constituting the main component or other additive elements.

[0020] (Internal electrode) The internal electrode 20 is mainly composed of a metal. The type of metal is not particularly limited, but it is preferable to use a metal having nickel (Ni) as the main component element because it can be fired simultaneously with the dielectric layer 10 and is inexpensive. Here, the term "main component element" in this specification means the element having the largest content expressed in atomic percentage (atomic %).

[0021] The internal electrodes 20 may contain, in addition to metal, a dielectric powder having a composition similar to that of the dielectric ceramic constituting the dielectric layers 10, or a glass component.

[0022] (Protection Department) The protective portion 50 includes a cover portion 51 arranged on a plane perpendicular to the T direction of the laminated chip 30, and a side margin portion 52 arranged on a plane perpendicular to the W direction, and has the function of protecting the dielectric layer 10 and the internal electrode 20.

[0023] The material of the protective part 50 is not limited as long as it has high electrical insulation and low permeability to deterioration factors such as moisture. From the viewpoints of making the shrinkage during firing in manufacturing the multilayer ceramic capacitor 100 uniform and mitigating the internal stress within the multilayer ceramic capacitor 100, it is preferable that the main component of the protective part 50 is the same as that of the dielectric ceramic forming the dielectric layer 10.

[0024] (external electrode) The external electrodes 60a and 60b are provided on the surface of the laminated chip 30, electrically connecting the internal electrodes 20a and 20b drawn out to the lead-out portions 40a and 40b, respectively, and covering at least one apex of the rectangular parallelepiped formed by the laminated chip 30. That is, the external electrodes 60a and 60b are each formed from the surface on which the lead-out portions 40a and 40b of the laminated chip 30 are formed, straddling at least one apex of the rectangular parallelepiped formed by the laminated chip 30 and three ridges leading to the apex, and wrapping around to a protective portion located on a surface perpendicular to the apex.

[0025] The material of the external electrodes 60a and 60b is not particularly limited as long as it is conductive. Examples of the material include metals such as nickel (Ni), copper (Cu), tin (Sn), palladium (Pd), platinum (Pt), silver (Ag), and gold (Au), alloys containing any of these as main components, and conductive resins. However, when the external electrodes 60a and 60b are formed by simultaneous firing with the laminated chip 30, in addition to conductivity, thermal stability and chemical stability that do not melt or oxidize during firing are also required, so Ni, Pd, Pt, etc. are preferably used.

[0026] The external electrodes 60a and 60b may be formed by laminating a plurality of conductive materials. In the multilayer ceramic capacitor 100 according to the first embodiment shown in Fig. 1, the entire external electrodes 60a and 60b have a laminated structure in which a Cu layer 62, a Ni layer 63, and a Sn layer 64 are formed in this order on the surface of a base layer 61 containing nickel as a main component element.

[0027] (Stacked chip) The laminated chip 30 formed of the dielectric layers 10, the internal electrodes 20, and the protective portion 50 has a rectangular parallelepiped shape. Fig. 2c shows a cross-sectional view (CC cross-sectional view in Fig. 1) of the laminated ceramic capacitor 100 cut at a side margin portion 52 of the laminated chip 30. Fig. 2d shows a cross-sectional view (DD cross-sectional view in Fig. 1) of the laminated ceramic capacitor 100 cut at an end margin portion, which is a region in the laminated chip 30 where the internal electrodes 20a exposed on the same end face face each other without interposing an internal electrode 20b exposed on a different end face. The top portion covered by the external electrodes 60a and 60b of the laminated chip 30 is formed by arranging the end points of the three ridges at different positions from one another, as shown in Fig. 3a, and has a shape that coincides with a plane P that passes through the end points e1, e2, and e3, or is formed by arranging the end points of the three ridges at different positions from one another, and has a shape that is recessed inward of the laminated chip 30 from the plane P, as shown in Fig. 3b and Fig. 3c, respectively. External Electrodes When the top portion covered by the external electrodes 60a and 60b has such a shape, poor formation of the external electrodes and excessive thinning are suppressed.

[0028] As shown in Figures 3b and 3c, the top portion of the laminated chip 30 covered with the external electrodes 60a and 60b preferably has a shape recessed toward the inside of the laminated chip 30 from the plane P. A top portion of such a shape can more effectively prevent poor formation of the external electrodes or excessive thinning of the external electrodes by allowing the external electrode paste to accumulate in the recessed portion when the external electrodes 60a and 60b are formed by applying the external electrode paste to the surface of the laminated chip 30.

[0029] 3c, it is more preferable that the top portion of the laminated chip 30 covered by the external electrodes 60a and 60b has a curved shape recessed inward of the laminated chip 30 from the plane P. A top portion having such a shape is less susceptible to stress concentration than one having a corner, and therefore cracks and chips in the laminated ceramic capacitor 100 can be suppressed.

[0030] Here, whether the top part of the laminated chip 30 covered by the external electrodes 60a and 60b is formed by arranging the end points of three ridges at different positions from each other, and has a planar shape passing through the end points, or a shape recessed inward of the laminated chip from the plane is determined by the following procedure. First, the external electrodes 60a and 60b are dissolved and removed from the laminated ceramic capacitor 100 using a solution to obtain the laminated chip 30. The type of solution used may be appropriately selected depending on the material of the external electrodes 60a and 60b. When the external electrodes have a laminated structure of the above-mentioned underlayer 61, Cu layer 62, Ni layer 63, and Sn layer 64, which are mainly composed of nickel, nitric acid is preferably used. When the external electrodes 60a and 60b contain a conductive resin, an organic solvent that dissolves it can be used. Next, the apex covered by the external electrodes 60a and 60b of the obtained laminated chip 30 is observed from each of the three faces that intersect at the apex using an optical microscope or a scanning electron microscope (SEM). Next, in the microscopic images of each face obtained, a line segment connecting the end points of the ridges is drawn, and if the contour of the apex of all faces overlaps the line segment or is located inside the line segment, i.e., on the opposite side to the intersection of the extensions of the ridges, it is determined that the observed apex is formed by arranging the end points of the three ridges at different positions from one another and has a planar shape that passes through the end points, or a shape that is recessed inward of the laminated chip from the plane.

[0031] Since the shape of the laminated chip 30 has a recess only at the top and no recess at the ridges, the shape is closer to a mathematical rectangular parallelepiped, and the planar area can be maximized. This makes it easier to maintain the correct posture on the carrier tape when the laminated ceramic capacitor is attached to the carrier tape and handled during transportation or mounting on a circuit board. In addition, since there are no recesses at the ridges, the thickness of the side margins and cover, which are protective parts, is ensured, preventing the intrusion of deterioration factors such as moisture, and improving reliability.

[0032] As shown in FIG. 4A, the stacked chip 30 has a maximum dimension in the stacking direction of t max The minimum dimension in the stacking direction is t min Then, t max for t min The ratio of t min / t max However, 0.95≦(t min / t max It is preferable that the t min / t max By setting the value of t within the above range, it is possible to more effectively prevent the external electrodes from being poorly formed or from being extremely thin. min / t max The value of is 0.95≦(t min / t max )≦0.98, and more preferably 0.95≦(t min / t max )≦0.97 is even more preferable.

[0033] As shown in FIG. 4b, the laminated chip 30 has a maximum width dimension of w max The minimum dimension in the width direction is w min When we say, w max W for min The ratio of min / w max However, 0.95≦(w min / w max It is preferable that the w min / w max By setting the value of w within the above range, it is possible to more effectively prevent the external electrodes from being poorly formed or becoming extremely thin. min / w max The value of is 0.95≦(w min / w max )≦0.98, and more preferably 0.95≦(w min / w max )≦0.97 is even more preferable.

[0034] Furthermore, in each plane parallel to the length direction of the laminated chip 30, as shown in FIG. 4b, the maximum dimension in the length direction is lmax The minimum dimension in the length direction is l min When l max for l min The ratio of min / l max However, 0.95≦(l min / l max It is preferable that the above l ≦ 0.99 is satisfied. min / l max By keeping the value of l within the above range, it is possible to more effectively prevent the external electrodes from being poorly formed or from becoming extremely thin. min / l max The value of is 0.95≦(l min / l max )≦0.98, and more preferably 0.95≦(l min / l max )≦0.97 is even more preferable.

[0035] <Variation (1)> A first modified example of the multilayer ceramic capacitor according to the first aspect is a multilayer ceramic capacitor 200 in which external electrodes 60a and 60b are arranged on the surface of the multilayer chip 30 in an L-shape in cross section, as shown in Fig. 5. The multilayer ceramic capacitor 200 having such a structure has the advantage that it can be made low-profile because the external electrodes 60a and 60b do not wrap around the upper protective part (cover part). Note that Fig. 5 is a cross-sectional view of the multilayer ceramic capacitor 200 cut at the side margin part 52 of the multilayer chip 30, so the dielectric layer 10 and the internal electrode 20 are not shown in the figure, but it goes without saying that the multilayer ceramic capacitor 200 is provided with these.

[0036] <Variation (2)> A second modified example of the multilayer ceramic capacitor according to the first aspect is a multilayer ceramic capacitor 300 in which external electrodes 60 are arranged at four positions, as shown in Fig. 6. A multilayer ceramic capacitor having such a structure can also achieve the effect of the present invention, that is, a multilayer ceramic capacitor in which poor formation of the external electrodes at the top and excessive thinning are suppressed.

[0037] [Manufacturing method of multilayer ceramic capacitors] <Second embodiment> A method for manufacturing a multilayer ceramic capacitor according to the second aspect of the present invention will be described below as a second embodiment.

[0038] A method for producing a multilayer ceramic capacitor according to a second embodiment includes preparing a powder of a dielectric ceramic composition, mixing the powder of the dielectric ceramic composition with a binder and forming the powder into a sheet to obtain a green sheet, forming an internal electrode pattern containing a metal on the green sheet, forming a dielectric pattern at a location on the green sheet where the internal electrode pattern is not formed, with a gap from a point that will become a ridge portion extending in the stacking direction in a pre-fired laminated chip described later, stacking a predetermined number of green sheets on which the internal pattern and the dielectric pattern are formed, arranging protective green sheets at both ends in the stacking direction, and then crimping the green sheets using a flexible jig to obtain a green laminated body, dividing the green laminated body into individual pieces to obtain a pre-fired laminated chip having a rectangular parallelepiped shape, which has an extraction portion from which the internal electrode pattern is extracted on a plane parallel to the stacking direction, and each apex is formed by arranging the end points of three ridges at different positions from each other, and has a shape recessed inward of the laminated chip from a plane passing through each end point, removing the binder from the pre-fired laminated chip, and performing either one of the following (a) or (b). (a) After the binder is removed, a paste for external electrodes is applied to the surface of the pre-fired laminated chip, covering the lead-out portion and the top of the rectangular parallelepiped, and then the pre-fired laminated chip with the external electrodes attached is fired to obtain a sintered body. (b) After the binder has been removed, the pre-fired laminated chip is fired to obtain a laminated chip, and then a paste for external electrodes is applied to the surface of the laminated chip, covering the lead-out portions and the top of the rectangular parallelepiped, and baked. Each operation will be described in detail below.

[0039] (Preparation of dielectric ceramic composition powder) The powder of the dielectric ceramic composition is obtained by mixing various raw material powders containing the constituent elements in a predetermined ratio and pre-firing (calcining). When mixing the various raw material powders in a predetermined ratio, various additives such as the above-mentioned additive elements and sintering aids may be further added, and these various additives may be further added to the powder after calcination.

[0040] The method for mixing the raw material powders is not particularly limited as long as each powder can be mixed uniformly while suppressing the inclusion of impurities, and either dry mixing or wet mixing may be adopted. When wet mixing using a ball mill is adopted as the mixing method, for example, partially stabilized zirconia (PSZ) balls are used, and the mixture is stirred for about 8 to 60 hours in a ball mill using an organic solvent such as ethanol or water as a dispersion medium, and then the dispersion medium is evaporated and dried.

[0041] The conditions for calcining the raw material mixed powder are not particularly limited as long as the above-mentioned various raw material powders react to obtain a predetermined dielectric ceramic composition. One example is calcining in air at a temperature of 800°C to 1100°C for 1 hour to 10 hours. The powder after calcination may be processed into a green sheet as it is, but it is preferable to crush it using a ball mill or a stamp mill, etc., in that a smooth green sheet is obtained through a uniform slurry and sinterability is improved.

[0042] When a commercially available powder of the dielectric ceramic composition is available, the above-mentioned mixing and calcination of the raw material powders may not be carried out, and the subsequent operations may be carried out on this powder.

[0043] (Preparation of raw sheets) The green sheet is obtained by mixing the powder of the above-mentioned dielectric ceramic composition with a binder and a dispersion medium to prepare a slurry, and forming the slurry into a sheet.

[0044] The binder used should be one that can maintain the shape of the green sheet and volatilizes without leaving any carbon or other residues during the binder removal process prior to firing. Examples of binders that can be used include polyvinyl alcohol, polyvinyl butyral, cellulose, urethane, and vinyl acetate. There are no particular limitations on the amount of binder used, but since it will be removed in a later process, it is preferable to use as little as possible within the range that achieves the desired moldability and shape retention in order to reduce raw material costs.

[0045] The dispersion medium to be used is one that does not cause aggregation of the calcined powder and the binder and can be easily removed by volatilization, etc., after forming into a green sheet, which will be described later. Examples of the dispersion medium that can be used include water and alcohol-based solvents.

[0046] To the slurry, components for adjusting the properties of the slurry, such as a dispersant, a plasticizer, and a thickener, may be added.

[0047] The method for mixing the mixed powder with the binder and the dispersion medium is not particularly limited as long as the components are mixed uniformly while preventing the inclusion of impurities. One example is ball mill mixing.

[0048] The prepared slurry can be formed into a sheet to obtain a green sheet by a commonly used method such as a doctor blade method or a die coating method.

[0049] (Formation of internal electrode pattern) The formation of the internal electrode pattern containing metal on the green sheet described above can be carried out by a method of printing or applying an internal electrode paste onto the green sheet in a predetermined pattern, or by a method of forming a metal film on the green sheet in a predetermined pattern by vapor deposition or sputtering.

[0050] When forming an internal electrode pattern using an internal electrode paste, the internal electrode paste used is obtained by mixing metal particles forming the internal electrodes and a vehicle in a three-roll mill. The internal electrode paste may contain glass frit and dielectric ceramic composition powder in addition to the above-mentioned components.

[0051] The type and amount of the binder and solvent contained in the vehicle used are not limited, and may be appropriately selected in consideration of the viscosity of the internal electrode paste, ease of handling, compatibility with the green sheet, and the like.

[0052] The printing of the internal electrode paste onto the green sheet can be carried out, for example, by using a screen mask on which a predetermined internal electrode pattern is formed.

[0053] (Formation of dielectric pattern) A dielectric pattern is formed on the green sheet on which the internal electrode pattern is formed. As shown in FIG. 7, the dielectric pattern 3 is formed at a location on the green sheets s1 and s2 where the internal electrode pattern 2 is not formed, with a gap from a point r located on a ridge extending in the lamination direction when the green sheets are made into a pre-fired laminated chip described later. In the figure, the point r corresponds to the intersection of dotted lines indicating the cutting position when making the pre-fired laminated chip described later. The green sheets s1 and s2 are alternately laminated when making the green laminated body described later, and the positions of the internal electrode pattern and the dielectric pattern in the L direction (left and right direction in the figure) are different from each other.

[0054] The dielectric pattern can be formed by printing or applying a dielectric pattern paste onto a green sheet. The dielectric pattern paste is obtained by mixing dielectric particles and a vehicle in a triple roll mill. The dielectric particles used may have a different composition from the dielectric contained in the green sheet. In order to obtain a multilayer ceramic capacitor with high dimensional accuracy and interlayer bonding strength, it is preferable that the dielectric particles used have the same or similar composition as the dielectric contained in the green sheet.

[0055] (Preparation of green laminate) The green laminate is obtained by stacking a predetermined number of green sheets on which the internal electrode patterns and the dielectric patterns are formed, arranging protective green sheets at both ends in the stacking direction, and then pressing the green sheets together using a flexible jig. The green sheets may be pressed together while the jig and the green sheets are heated.

[0056] When the green sheets having the above-mentioned internal electrode pattern and dielectric pattern are laminated, the portions of each green sheet where neither the internal electrode pattern nor the dielectric pattern is formed form voids that overlap in the lamination direction. When the green sheets in this state are compressed using a flexible jig, the deformation that reduces the volume of the voids occurs prior to the deformation that reduces the volume of the entire green laminate. As a result, depressions are formed on the surface of the green laminate where the voids overlap. When this green laminate is singulated as described below, a pre-fired laminated chip having a rectangular parallelepiped shape is obtained in which each top has three ridges that do not intersect with each other and are recessed inward of the laminated chip from the plane passing through the end points of each ridge. Note that when the laminated green sheets are pressed and compressed using a material that does not have flexibility, such as a mold, the deformation that reduces the volume of the entire green laminate occurs preferentially, and it is difficult to obtain a pre-fired laminated chip having a top of the above-mentioned shape only by singulating the green laminate.

[0057] The protective green sheets added to both ends in the lamination direction during lamination and compression bonding will become protective parts (cover parts) when the laminated ceramic capacitor is made. The protective green sheets may have the same composition as the green sheets on which the internal electrode pattern and the dielectric pattern are formed, or a different composition. From the viewpoint of making the shrinkage rate during firing uniform, it is preferable that the composition of the added protective green sheets is the same as or similar to the green sheets on which the internal electrode pattern and the dielectric pattern are formed.

[0058] The material of the flexible jig used for pressure bonding is preferably rubber, and among these, silicone rubber is more preferable.

[0059] The green sheets may be pressed at room temperature, but it is preferable to heat the green sheets to a temperature of 50° C. or higher in order to increase the adhesive strength between the green sheets. The heating temperature is more preferably 60° C. or higher, and even more preferably 70° C. or higher. There is no particular upper limit to the heating temperature, but in order to prevent deformation of the green laminate due to softening of the binder and oxidation of the internal electrode pattern, it is preferably 200° C. or lower, more preferably 180° C. or lower, and particularly preferably 160° C. or lower.

[0060] The pressure when pressing the green sheet may be appropriately determined taking into consideration the composition and thickness of the green sheet, the material of the flexible jig, the capacity of the pressing device, the pressing temperature, etc. The pressure may be, for example, 80 MPa or more, preferably 100 MPa or more, and more preferably 120 MPa or more. The upper limit of the pressure is not particularly limited, and may be, for example, 240 MPa or less, preferably 220 MPa or less, and more preferably 200 MPa or less.

[0061] (Preparation of pre-fired laminated chips) The pre-fired laminated chip is obtained by dividing the raw laminate into individual laminated chip shapes through singulation. Through singulation, a pre-fired laminated chip is obtained that has a rectangular parallelepiped shape, with an internal electrode pattern extending from an extension portion on a surface parallel to the lamination direction, and each top portion is formed by arranging the end points of three ridges at different positions, and has a shape recessed inward from the plane passing through each end point. For singulation, a commonly used means such as a dicing saw or a laser cutting machine can be used.

[0062] (Removing the binder) The obtained pre-fired laminated chip is heated to remove the binder by volatilization. The heating conditions may be appropriately set in consideration of the volatilization temperature and content of the binder. One example is holding the chip in a nitrogen (N2) atmosphere at a temperature of 200°C to 500°C for 5 to 20 hours.

[0063] (Formation of external electrodes) The external electrodes are formed by applying an external electrode paste to the surface of the pre-fired laminated chip from which the binder has been removed, covering the lead-out portions and the top of the rectangular prism, and then firing the chip, or by applying an external electrode paste to the surface of the laminated chip obtained after firing as described below, covering the lead-out portions and the top of the rectangular prism, and then baking the chip.

[0064] The paste for the external electrodes used is obtained by mixing the metal particles forming the external electrodes and a vehicle in a triple roll mill. The paste for the internal electrodes may contain glass frit and / or a dielectric ceramic composition powder in addition to the above-mentioned components.

[0065] There are no limitations on the type and amount of binder and solvent contained in the vehicle used, and these may be appropriately selected taking into consideration the viscosity of the external electrode paste, ease of handling, and the like.

[0066] The external electrode paste can be applied, for example, by immersing (dipping) a part of the pre-fired laminated chip or the laminated chip obtained through firing, which will be described later, in a bath of the external electrode paste.

[0067] The external electrodes may be formed by using a metal layer formed by baking an external electrode paste onto the surface of the laminated chip as a base layer, and laminating a conductive layer on the base layer by means of plating, vapor deposition, or the like.

[0068] (Firing pre-fired stacked chips) The pre-fired laminated chip is fired by heating the pre-fired laminated chip to a predetermined temperature. When setting the firing conditions, it is preferable to consider the sinterability of the dielectric ceramic composition and the heat resistance and oxidation resistance of the metal contained in the internal electrode paste. In addition, when the external electrode paste is attached to the surface of the pre-fired laminated chip prior to firing, it is preferable to also consider the heat resistance and oxidation resistance of the metal contained therein. Examples of firing conditions include holding the chip at about 900°C, which is lower than the normal firing temperature, for about 3 hours in a reducing atmosphere containing a mixture of nitrogen (N2), hydrogen (H2), and water vapor (H2O), and then raising the temperature to 1000°C to 1350°C for 5 minutes to 2 hours. After firing, a reoxidation treatment may be performed in which the chip is held at 600°C to 1000°C in a nitrogen (N2) gas atmosphere or a low-oxygen atmosphere. By firing, the powder of the dielectric ceramic composition is sintered to become a dielectric layer, and the internal electrode pattern is sintered to become an internal electrode. When a paste for external electrodes is applied to the surface of the laminated chip before firing, this is sintered to form the external electrodes. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0070] [Example 1] As the powder of the dielectric ceramic composition, a pre-fired barium titanate (BaTiO3) powder was prepared as the main raw material, and powders of oxides of Mn, Ho, and Si were prepared as trace additive components. A polyvinyl butyral-based binder and an alcohol-based solvent were added to these powders and mixed with a wet ball mill. The obtained mixed slurry was molded on a carrier film using a die coater to obtain a green sheet with a thickness of 2.7 μm. After forming an internal electrode pattern on this green sheet by screen printing a nickel paste as an internal electrode paste, as shown in FIG. 7, a dielectric paste containing the above-mentioned dielectric ceramic composition powder was printed at a predetermined interval from a point r that becomes a ridge extending in the lamination direction when the pre-fired laminated chip is formed, in the area where the internal electrode pattern 2 is not printed, to form a dielectric pattern 3. The green sheets were stacked in 500 layers, and 20 green sheets for the cover were stacked on each of the top and bottom surfaces. Each green sheet was heated to 90°C, and while maintaining the heating temperature, the green sheets were pressed from both sides in the stacking direction at a pressure of 80 MPa using a pressure tool with a rubber surface to obtain a green laminate. This green laminate was divided into individual pieces to obtain a rectangular pre-fired laminated chip having a pair of opposing pull-out surfaces parallel to the stacking direction, from which the internal electrode patterns were pulled out every other layer. The obtained pre-fired laminated chip was heated to 300°C in a nitrogen atmosphere to perform a binder removal treatment. Each pull-out surface of this pre-fired laminated chip was immersed in nickel paste as an external electrode paste, and the nickel paste was attached to the surface of the pre-fired laminated chip. The pre-fired laminated chip with the nickel paste attached was heated to 1300°C in a so-called reducing-steam atmosphere in which reducing gas containing hydrogen and water vapor were introduced into nitrogen, and fired for 10 minutes, then cooled to around room temperature to obtain a laminated chip having a nickel layer on its surface. A Cu layer, a Ni layer, and a Sn layer were formed in this order by plating on the nickel layer formed on the surface of the obtained laminated chip, thereby obtaining a laminated ceramic capacitor according to Example 1. The obtained laminated ceramic capacitor had a rectangular shape with a surface perpendicular to the stacking direction of the laminated chip measuring 1.6 mm x 0.8 mm, and a dimension in the stacking direction was 0.8 mm.

[0071] [Examples 2 to 4] The multilayer ceramic capacitors according to Examples 2 to 4 were each produced in the same manner as in Example 1, except that the pressure used for pressing the green sheets was 100 MPa in Example 2, 135 MPa in Example 3, and 170 MPa in Example 4.

[0072] [Comparative Examples 1 and 2] The multilayer ceramic capacitors according to Comparative Examples 1 and 2 were produced in the same manner as in Example 1, except that the pressure used for compressing the green sheets was 25 MPa in Comparative Example 1 and 60 MPa in Comparative Example 2.

[0073] [Evaluation of multilayer ceramic capacitors] (Check the top shape of the stacked chip) For each of the obtained multilayer ceramic capacitors, it was judged by the above-mentioned method whether the top of the laminated chip covered with the external electrode has a planar shape in which the three ridges leading to the top do not intersect with each other and pass through the end points of the ridges, or a shape recessed inward from the plane of the laminated chip. As a result, in each of the multilayer ceramic capacitors according to Examples 1 to 3, it was judged that the top of the laminated chip has the shape shown in FIG. 3c, in which the three ridges leading to the top do not intersect with each other and have a shape recessed inward from the plane passing through the end points of the ridges. On the other hand, in the multilayer ceramic capacitors according to Comparative Examples 1 and 2, it was judged that the top of the laminated chip has a shape in which the three ridges leading to the top intersect with each other.

[0074] (t in a plane parallel to the stacking direction of the stacked chip min / t max (Calculation of For each multilayer ceramic capacitor obtained, the maximum dimension in the lamination direction on a plane parallel to the lamination direction of the laminated chip, t max and minimum dimension t min , the maximum width dimension w of the laminated chip on a plane parallel to the width direction max and minimum dimension w min , and the maximum lengthwise dimension l in a plane parallel to the lengthwise direction of the laminated chip max and minimum dimension l minwas measured and calculated from the optical microscope images of each surface, and the ratio of these values, t min / t max , w min / w max and l min / l max The values ​​of were calculated, and the results are shown in Table 1.

[0075] (Moisture resistance load test) A voltage of 35V was applied to each of the obtained multilayer ceramic capacitors (n=400 pieces) for 200 hours in an environment of relative humidity of 85%, and then the capacitors were left at room temperature for 24 hours, and their insulation resistance was measured. Samples with an insulation resistance value of less than 10MΩ were determined to have failed, and the percentage of failed samples out of the total number of samples tested was calculated as the failure rate. The results are shown in Table 1.

[0076] [Table 1]

[0077] From Table 1, it can be seen that a multilayer ceramic capacitor in which the top part covered with the external electrodes of the laminated chip is formed by arranging the end points of three ridges at different positions from each other and has a shape recessed inward of the laminated chip from the plane passing through each of the end points has a reduced failure rate in a high humidity environment. This is presumably because poor formation of the external electrodes at the top part of the laminated chip and excessive thinning are suppressed, thereby suppressing the intrusion of moisture into the laminated chip.

[0078] This specification also discloses the following techniques.

[0079] (Appendix 1) Dielectric layers made of dielectric ceramic and internal electrodes mainly made of metal are laminated alternately. a lead portion from which the internal electrode is led out is provided on a surface parallel to the lamination direction; A protective portion including a dielectric ceramic is provided on the surface other than the drawn-out portion. A stacked chip having a rectangular parallelepiped shape, and an external electrode provided on a surface of the laminated chip, the external electrode connecting the internal electrodes drawn out to the drawing portion and covering at least one apex of the rectangular parallelepiped formed by the laminated chip; Equipped with The top portion of the laminated chip covered with the external electrode is The three edges are formed by arranging the endpoints of the three edges at different positions from each other, and A planar shape passing through each of the end points or a shape recessed inward from the planar shape to the inside of the laminated chip Multilayer ceramic capacitor.

[0080] (Appendix 2) The multilayer ceramic capacitor according to (Supplementary Note 1), wherein the top portion covered with the external electrodes has a shape recessed inward of the laminated chip with respect to a plane passing through each of the end points.

[0081] (Appendix 3) The multilayer ceramic capacitor according to (Supplementary Note 2), wherein the top portion covered with the external electrode has a curved shape.

[0082] (Appendix 4) The laminated chip is The maximum dimension in the lamination direction on a plane parallel to the lamination direction is t max The minimum dimension in the stacking direction is t min Then, t max for t min The ratio of t min / t max However, 0.95≦(t min / t max )≦0.99, The maximum dimension in the width direction on the surface parallel to the width direction is w max The minimum dimension in the width direction is w min When we say, w max W for min The ratio of min / w max However, 0.95≦(w min / w max )≦0.99, and The maximum dimension in the lamination direction on the plane parallel to the length direction is l maxThe minimum dimension in the length direction is l min When l max for l min The ratio of min / l max However, 0.95≦(l min / l max )≦0.99 A multilayer ceramic capacitor according to any one of (Appendix 1) to (Appendix 3).

[0083] (Appendix 5) Providing a powder of a dielectric ceramic composition; mixing the powder of the dielectric ceramic composition with a binder and forming the mixture into a sheet to obtain a green sheet; forming an internal electrode pattern comprising a metal on the green sheet; forming a dielectric pattern at a location on the green sheet where the internal electrode pattern is not formed, with a space from a point that will become a ridge extending in the lamination direction in a pre-fired laminated chip described below; a predetermined number of green sheets on which the internal pattern and the dielectric pattern are formed are stacked, protective green sheets are disposed on both ends in the stacking direction, and then the green sheets are pressure-bonded via a flexible jig to obtain a green laminate; The raw laminate is singulated to obtain a rectangular parallelepiped pre-fired laminated chip having an extraction portion from which the internal electrode pattern is extracted on a surface parallel to the lamination direction, each apex being formed by arranging end points of three ridges at mutually different positions, and having a shape recessed inward of the laminated chip with respect to a plane passing through each end point. removing binder from the pre-fired laminated chips; and Do either (a) or (b) below: The method for producing a multilayer ceramic capacitor includes: (a) After the binder is removed, a paste for external electrodes is applied to the surface of the pre-fired laminated chip, covering the lead-out portion and the top of the rectangular parallelepiped, and then the pre-fired laminated chip with the external electrodes attached is fired to obtain a sintered body. (b) After the binder has been removed, the pre-fired laminated chip is fired to obtain a laminated chip, and then a paste for external electrodes is applied to the surface of the laminated chip, covering the lead-out portions and the top of the rectangular parallelepiped, and baked.

[0084] (Appendix 6) The method for producing a multilayer ceramic capacitor according to (Appendix 5), wherein the compression bonding is carried out at a temperature of 50° C. or higher and a pressure of 80 MPa or higher. [Industrial Applicability]

[0085] According to the present invention, it is possible to provide a multilayer ceramic capacitor in which poor formation of external electrodes at the top of the laminated chip and excessive thinning are suppressed. Such a multilayer ceramic capacitor is useful in that it has high reliability because the intrusion of degradation factors from the external electrodes is suppressed. [Explanation of symbols]

[0086] 100, 200, 300 Multilayer ceramic capacitors 10 Dielectric layer 20, 20a, 20b internal electrode 30 Stacked Chips 40a, 40b drawer surface 50 Protection Department 51 Cover part 52 Side margin 60, 60a, 60b external electrode 61 Base layer 62 Cu layer 63 Ni layer 64 Sn layer e1, e2, e3 (end points of the edge of the rectangular solid formed by the stacked chips) P A plane passing through e1, e2, and e3 t max The maximum dimension in the stacking direction of the stacked chip on a plane parallel to the stacking direction t min The minimum dimension in the stacking direction of the stacked chip on a plane parallel to the stacking direction w max The maximum width of the laminated chip on a surface parallel to the width direction w min The minimum dimension in the width direction of the laminated chip on a surface parallel to the width direction l max The maximum lengthwise dimension of the laminated chip on a plane parallel to the lengthwise direction l min The minimum lengthwise dimension of the stacked chip on a plane parallel to the lengthwise direction s1, s2 Raw sheets 2 Internal electrode pattern 3 Dielectric Pattern r A point located on the edge extending in the stacking direction when the chip is stacked before firing

Claims

1. Dielectric layers made of dielectric ceramic and internal electrodes mainly made of metal are laminated alternately. a lead portion from which the internal electrode is led out is provided on a surface parallel to the lamination direction; A protective portion including a dielectric ceramic is provided on the surface other than the drawn-out portion. A stacked chip having a rectangular parallelepiped shape, and an external electrode provided on a surface of the laminated chip, the external electrode connecting the internal electrodes drawn out to the drawing portion and covering at least one apex of the rectangular parallelepiped formed by the laminated chip; Equipped with The top portion of the laminated chip covered with the external electrode is The three edges are formed by arranging the end points of the three edges at different positions from each other, and A planar shape passing through each of the end points or a shape recessed inward from the planar shape to the inside of the laminated chip Multilayer ceramic capacitor.

2. 2. The multilayer ceramic capacitor according to claim 1, wherein the top portion covered with the external electrodes has a shape recessed inward of the laminated chip from a plane passing through each of the end points.

3. 3. The multilayer ceramic capacitor according to claim 2, wherein the top portion covered with the external electrode has a curved shape.

4. The laminated chip is The maximum dimension in the lamination direction on a plane parallel to the lamination direction is t max The minimum dimension in the stacking direction is t min Then, t max for t min The ratio of t min / t max However, 0.95≦(t min / t max )≦0.99, The maximum dimension in the width direction on the plane parallel to the width direction is w max The minimum dimension in the width direction is w min When we say, w max Replying to @ min The ratio w min / w max However, 0.95≦(w min / w max )≦0.99, and The maximum dimension in the lamination direction on a plane parallel to the length direction is l max The minimum dimension in the length direction is l min When we set max For min The ratio of min / l max However, 0.95≦(l min / l max )≦0.99 The multilayer ceramic capacitor according to claim 1 .

5. Providing a powder of a dielectric ceramic composition; mixing the powder of the dielectric ceramic composition with a binder and forming the mixture into a sheet to obtain a green sheet; forming an internal electrode pattern comprising a metal on the green sheet; forming a dielectric pattern at a location on the green sheet where the internal electrode pattern is not formed, with a space from a point that will become a ridge extending in the lamination direction in a pre-fired laminated chip described below; a predetermined number of green sheets on which the internal pattern and the dielectric pattern are formed are stacked, protective green sheets are disposed on both ends in the stacking direction, and then the green sheets are pressure-bonded via a flexible jig to obtain a green laminate; The raw laminate is singulated to obtain a rectangular parallelepiped pre-fired laminated chip having an extraction portion from which the internal electrode pattern is extracted on a surface parallel to the lamination direction, each apex being formed by arranging end points of three ridges at mutually different positions, and having a shape recessed inward of the laminated chip with respect to a plane passing through each end point. removing binder from the pre-fired laminated chips; and Do either (a) or (b) below. The method for producing a multilayer ceramic capacitor includes: (a) After the binder is removed, a paste for external electrodes is applied to the surface of the pre-fired laminated chip, covering the lead-out portion and the top of the rectangular parallelepiped, and then the pre-fired laminated chip with the external electrodes attached is fired to obtain a sintered body. (b) After the binder has been removed, the pre-fired laminated chip is fired to obtain a laminated chip, and then a paste for external electrodes is applied to the surface of the laminated chip, covering the lead-out portions and the top of the rectangular parallelepiped, and baked.

6. The method for producing a multilayer ceramic capacitor according to claim 5, wherein the compression bonding is carried out at a temperature of 50° C. or higher and a pressure of 80 MPa or higher.

Citation Information

Patent Citations

  • Multilayer ceramic electronic component and fabrication method thereof

    JP2013149939A

  • Multilayer ceramic electronic component and manufacturing method thereof

    JP2020102479A