Tungsten electrode for rare-earth molten salt electrolysis and manufacturing method thereof
The tungsten electrode with a copper alloy and buffer layer addresses the high mass and resistance issues of conventional electrodes, achieving lower power consumption and improved conductivity through a lightweight, stable design.
Patent Information
- Application Number
- JP2023086391
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2023-05-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-05-25
AI Technical Summary
Conventional tungsten electrodes used in rare earth molten salt electrolysis are heavy, have high resistance, and result in high power consumption due to their high density and low conductivity.
A tungsten electrode design comprising an open tungsten housing with a copper alloy inside, a tungsten buffer layer between the copper alloy sidewall and housing, and a copper alloy bottom contacting the inner bottom of the housing, utilizing a copper-vanadium or copper-niobium alloy to reduce mass and enhance conductivity.
The design results in a lightweight electrode with improved conductivity, reducing power consumption and enhancing stability by mitigating damage from copper alloy expansion.
Smart Images

Figure 2024132775000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of rare earth metal electrolysis, and more particularly to a tungsten electrode for rare earth molten salt electrolysis and a method for producing the same. [Background technology]
[0002] Rare earth metals are mainly used in the production of high-performance rare earth permanent magnet materials, and are important basic raw materials in the fields of electronic information, new energy automobiles, new materials, etc. The production process of rare earth metals is mainly based on the molten salt electrolysis method. The molten salt electrolysis method is mainly divided into two types according to the electrolyte system, one is the rare earth chloride electrolyte system, i.e., the binary electrolyte system such as RECl3-KCl (RE is rare earth metal), and the other is the fluoride-oxide electrolyte system, i.e., the ternary system such as RE2O3-REF3-LiF. The rare earth chloride electrolyte system has high volatility of the chloride molten salt and high solubility of the rare earth metal in the chloride molten salt, so the power consumption is high, the current efficiency is low, and the yield is low. The fluoride-oxide electrolyte system has high current efficiency and stable raw materials, and is the main electrolyte system of the current molten salt electrolysis method.
[0003] In the fluoride-oxide electrolyte system, the raw material rare earth oxide dissociates during the electrolysis process, becoming rare earth cations and oxygen anions. Under the action of a direct current electric field, the rare earth cations migrate to the cathode, where they gain electrons and are reduced to rare earth metals, while the oxygen anions migrate to the anode, where they lose electrons to produce oxygen.
[0004] Cathode is usually made of expensive tungsten metal, which on the one hand has a high density, which leads to a high mass of conventional tungsten electrodes, and on the other hand, its high resistance and low conductivity lead to high power consumption. Summary of the Invention [Problem to be solved by the invention]
[0005] The object of the present invention is to provide a tungsten electrode for electrolysis of rare earth molten salt and a manufacturing method thereof. The tungsten electrode provided by the present invention is lightweight, has excellent electrical conductivity, and can reduce the power consumption of the tungsten electrode. [Means for solving the problem]
[0006] To achieve the above objectives, the present invention provides the following technical solutions:
[0007] The present invention provides a tungsten electrode for rare earth molten salt electrolysis, comprising an open tungsten housing and a copper alloy; the copper alloy is located within the open tungsten housing; a tungsten buffer layer is disposed between the copper alloy sidewall and the open tungsten housing; The bottom of the copper alloy contacts the inner bottom of the open tungsten housing.
[0008] Preferably, the copper alloy comprises a copper-vanadium alloy and / or a copper-niobium alloy.
[0009] Preferably, the mass percent content of vanadium in the copper-vanadium alloy is between 5 and 15%; The mass percent content of niobium in the copper-niobium alloy is 3-20%.
[0010] Preferably, the outer diameter of the open tungsten housing is 65-120 mm and the inner diameter is 40-70 mm; The thickness of the bottom of the open tungsten housing is 10-20 mm.
[0011] Preferably, the diameter of the copper alloy is 20 to 60 mm, The tungsten buffer layer has a thickness of 3 to 8 mm.
[0012] Preferably, the density of the open tungsten housing is 18 g / cm 3 That's all. The density of the tungsten buffer layer is 12 to 14 g / cm 3 It is.
[0013] The present invention further includes the steps of placing a copper alloy in the open tungsten housing, adding tungsten powder between the copper alloy and the open tungsten housing, and pressing to obtain an electrode blank, and the central axis of the copper alloy overlaps with the central axis of the open tungsten housing; and forging the electrode blank to obtain the tungsten electrode for rare earth molten salt electrolysis.
[0014] Preferably, the pressure of the press is 50 to 80 MPa and the time is 2 to 5 hours.
[0015] Preferably, the forging temperature is 1000 to 1500°C. Effect of the Invention
[0016] The present invention provides a tungsten electrode for rare earth molten salt electrolysis, comprising an open tungsten housing and a copper alloy, the copper alloy is located in the open tungsten housing, a tungsten buffer layer is provided between the side wall of the copper alloy and the open tungsten housing, and the bottom of the copper alloy contacts the inner bottom of the open tungsten housing.The present invention uses copper alloy as the core of tungsten electrode, replaces a part of tungsten metal, can reduce the mass of the whole tungsten electrode, can further improve the conductivity of tungsten electrode, can reduce the power consumption of tungsten electrode, and can be provided with a tungsten buffer layer between copper alloy and tungsten housing, can avoid the destruction of tungsten housing caused by the linear expansion of copper alloy in practical use, and can improve the stability of the whole tungsten electrode. [Brief description of the drawings]
[0017] [Figure 1]FIG. 1 is a schematic diagram of the cross-sectional structure of a tungsten electrode for rare earth molten salt electrolysis provided by the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention provides a tungsten electrode for rare earth molten salt electrolysis, comprising an open tungsten housing and a copper alloy; the copper alloy is located within the open tungsten housing; a tungsten buffer layer is disposed between the copper alloy sidewall and the open tungsten housing; The bottom of the copper alloy contacts the inner bottom of the open tungsten housing.
[0019] The cross-sectional structure schematic diagram of the tungsten electrode for rare earth molten salt electrolysis provided by the present invention is as shown in FIG. 1, where 1 is the copper alloy, 2 is the open tungsten housing, and 3 is the tungsten buffer layer.
[0020] In the present invention, the copper alloy preferably includes a copper-vanadium alloy and / or a copper-niobium alloy.
[0021] In the present invention, the purity of the copper alloy is preferably greater than 99.9%. In the present invention, the mass percent content of vanadium in the copper-vanadium alloy is preferably 5-15%, more preferably 8-13%, and more preferably 10-12%. In the present invention, the mass percent content of niobium in the copper-niobium alloy is preferably 3-20%, more preferably 5-18%, and more preferably 10-15%. In the present invention, the components of the copper alloy are uniform and free of segregation and inclusion phenomena.
[0022] In the present invention, the diameter of the copper alloy is preferably 20 to 60 mm, more preferably 25 to 55 mm, and even more preferably 30 to 50 mm.
[0023] In the present invention, the length of the copper alloy is preferably the same as the length of the cavity of the open tungsten housing.
[0024] In the present invention, the outer diameter of the open tungsten housing is preferably 65 to 120 mm, and the inner diameter is preferably 40 to 70 mm. In the present invention, the length of the open tungsten housing is preferably 700 to 1100 mm. In the present invention, the thickness of the bottom of the open tungsten housing is preferably 10 to 20 mm, more preferably 12 to 18 mm, and more preferably 13 to 15 mm.
[0025] In the present invention, the open tungsten housing is preferably obtained by manufacturing. In the present invention, the manufacturing method of the open tungsten housing is preferably: The method includes the steps of putting tungsten powder into a mold to form the mold, and then pressing, sintering and forging the resulting mold in sequence to obtain the open-ended tungsten housing.
[0026] In the present invention, the purity of the tungsten powder is preferably greater than 99%. In the present invention, the particle size D50 of the tungsten powder is preferably 6 μm. In the present invention, the molding process is not particularly limited, and may be performed using a process well known to those skilled in the art.
[0027] In the present invention, the pressure of the pressing is preferably 200 to 240 MPa, more preferably 210 to 230 MPa, and even more preferably 220 MPa, and the time is preferably 22 to 24 hours, and even more preferably 23 hours. In the present invention, the pressing is preferably performed by an isostatic press. In the present invention, the pressing process is not particularly limited, and may be performed using a process well known to those skilled in the art.
[0028] In the present invention, the sintering is preferably carried out in a hydrogen atmosphere. In the present invention, the sintering temperature is preferably 2200 to 2350°C, more preferably 2250 to 2300°C, the heating rate to the sintering temperature is preferably 10 to 12°C / min, and the warming time is preferably 18 to 22 hours, more preferably 19 to 21 hours, more preferably 20 hours. After the sintering is completed, the present invention also preferably includes cooling the obtained product. In the present invention, the cooling method is preferably natural cooling to room temperature in a hydrogen atmosphere. In the present invention, the sintering is preferably carried out in an atmospheric sintering furnace.
[0029] In the present invention, the forging temperature is preferably 1300 to 1500° C., more preferably 1350 to 1450° C., and even more preferably 1400° C. In the present invention, the forging process is not particularly limited, and may be performed using a process well known to those skilled in the art.
[0030] After the forging is completed, the present invention also preferably includes straightening and polishing the obtained product. In the present invention, the straightening process is not particularly limited, and may be performed using a process well known to those skilled in the art. In the present invention, the polishing process is not particularly limited, and may be performed using a process well known to those skilled in the art to control the thickness tolerance of the product to 0.1-0.5 mm.
[0031] In the present invention, the density of the open tungsten housing is preferably 18 g / cm 3 That's all.
[0032] In the present invention, the thickness of the tungsten buffer layer is preferably 3 to 8 mm, more preferably 4 to 7 mm, and even more preferably 5 to 6 mm. In the present invention, the density of the tungsten buffer layer is preferably 12 to 14 g / cm. 3 , and more preferably 13 g / cm 3In the present invention, the tungsten buffer layer can prevent the destruction of the tungsten housing caused by the linear expansion of the copper alloy in practical use, and improve the stability of the entire tungsten electrode.
[0033] The present invention also provides an electrode blank by the steps of: placing a copper alloy in the open tungsten housing, adding tungsten powder between the copper alloy and the open tungsten housing, and pressing the copper alloy to obtain an electrode blank; and a central axis of the copper alloy overlaps with a central axis of the open tungsten housing. and forging the electrode blank to obtain the tungsten electrode for rare earth molten salt electrolysis.
[0034] In the present invention, unless otherwise specified, all raw materials are commercially available products familiar to those skilled in the art.
[0035] The present invention places a copper alloy in the open tungsten housing, adds tungsten powder between the copper alloy and the open tungsten housing, and presses it to obtain an electrode blank, so that the central axis of the copper alloy overlaps with the central axis of the open tungsten housing.
[0036] In the present invention, the tungsten powder is the same as the tungsten powder described in the above technical solutions, so the description is omitted here.
[0037] In the present invention, the pressure of the press is preferably 50 to 80 MPa, more preferably 55 to 75 MPa, and even more preferably 60 to 70 MPa, and the time is preferably 2 to 5 hours, and even more preferably 3 to 4 hours. In the present invention, the press is preferably performed by an isostatic press. In the present invention, the pressing process is not particularly limited, and may be performed using a process well known to those skilled in the art.
[0038] In the present invention, after obtaining the electrode blank, the electrode blank is forged to obtain the tungsten electrode for rare earth molten salt electrolysis.
[0039] In the present invention, the forging temperature is preferably 1000 to 1500° C., more preferably 1100 to 1400° C., and even more preferably 1200 to 1300° C. In the present invention, the forging process is not particularly limited, and may be performed using a process well known to those skilled in the art.
[0040] After the forging is completed, the present invention also preferably includes straightening and polishing the obtained product. In the present invention, the straightening process is not particularly limited, and may be performed using a process well known to those skilled in the art. In the present invention, the polishing process is not particularly limited, and may be performed using a process well known to those skilled in the art to control the thickness tolerance of the product to 0.03-0.1 mm.
[0041] In order to further explain the present invention, the tungsten electrode for rare earth molten salt electrolysis and the manufacturing method thereof provided by the present invention will be described in detail below with reference to the drawings and examples, but they should not be understood as limiting the protection scope of the present invention.
[0042] Example 1
[0043] Tungsten powder (purity is greater than 99% and particle size D50 is 6μm) is put into a mold to form it, the obtained model is put into an isostatic press and pressed at 220MPa for 22h, the obtained blank is put into an atmospheric sintering furnace, heated to 2300℃ at a heating rate of 12℃ / min in a hydrogen atmosphere to sinter, and kept at the temperature for 22h, after sintering is completed, it is naturally cooled to room temperature in a hydrogen atmosphere, and then heated to 1500℃ and forged, after forging is completed, the obtained article is straightened and polished (thickness tolerance is controlled to 0.1~0.5mm) to form an open tungsten housing (density is 18.1g / cm 3 The outer diameter was 84 mm, the length was 800 mm, the wall thickness was 15 mm, and the bottom thickness was 20 mm.
[0044] A copper-vanadium alloy (with a purity of more than 99.9% and a vanadium mass percentage content of 8%) with a length of 780 mm and a diameter of 44 mm was placed in an open tungsten housing (with the central axis of the copper-vanadium alloy overlapping with the central axis of the open tungsten housing), and tungsten powder (with a purity of more than 99% and a grain size D50 of 6 μm) was added between the copper alloy and the tungsten housing to a thickness of 5 mm, and then placed in an isostatic press and pressed at 60 MPa for 3 h to obtain an electrode blank.
[0045] The electrode blank is forged at 1350°C, then straightened and polished (thickness tolerance is controlled to 0.03-0.1 mm), and the tungsten electrode (diameter 80 mm, length 800 mm, density of tungsten buffer layer is 13 g / cm) is made. 3 ) was obtained.
[0046] Example 2
[0047] Tungsten powder (purity is greater than 99% and particle size D50 is 6μm) is put into a mold to form it, the obtained model is put into an isostatic press and pressed at 230MPa for 20h, the obtained blank is put into an atmospheric sintering furnace, heated to 2300℃ at a heating rate of 12℃ / min in a hydrogen atmosphere to sinter, and kept at the temperature for 23h. After sintering is completed, it is naturally cooled to room temperature in a hydrogen atmosphere, and then heated to 1500℃ and forged. After forging is completed, the obtained article is straightened and polished (thickness tolerance is controlled to 0.1-0.5mm) to form an open tungsten housing (density is 18.0g / cm 3 The outer diameter was 105 mm, the length was 930 mm, the wall thickness was 18 mm, and the bottom thickness was 20 mm.
[0048] A copper-niobium alloy (with a purity of more than 99.9% and a mass percent content of niobium of 10%) with a length of 910 mm and a diameter of 57 mm was placed in an open tungsten housing (with the central axis of the copper-niobium alloy overlapping with the central axis of the open tungsten housing), and tungsten powder (with a purity of more than 99% and a grain size D50 of 6 μm) was added between the copper alloy and the tungsten housing to a thickness of 6 mm, and then placed in an isostatic press and pressed at 70 MPa for 5 h to obtain an electrode blank.
[0049] The electrode blank is forged at 1400 °C, then straightened and polished (thickness tolerance is controlled to 0.03-0.1 mm), and the tungsten electrode (diameter is 100 mm, length is 930 mm, density of tungsten buffer layer is 14 g / cm) is made. 3 ) was obtained.
[0050] Example 3
[0051] Tungsten powder (purity is greater than 99% and particle size D50 is 6μm) is put into a mold to form it, the obtained model is put into an isostatic press and pressed at 220MPa for 22h, the obtained blank is put into an atmospheric sintering furnace, heated to 2200℃ at a heating rate of 10℃ / min in a hydrogen atmosphere to sinter, and kept at room temperature for 22h. After sintering is completed, it is naturally cooled to room temperature in a hydrogen atmosphere, and then heated to 1500℃ and forged. After forging is completed, the article is straightened and polished (thickness tolerance is controlled to 0.1~0.5mm) to form an open tungsten housing (density is 18.2g / cm 3 The outer diameter was 78 mm, the length was 750 mm, the wall thickness was 14 mm, and the bottom thickness was 15 mm.
[0052] A copper-niobium alloy (with a purity of more than 99.9% and a mass percent content of niobium of 8%) with a length of 735 mm and a diameter of 42 mm was placed in an open tungsten housing (with the central axis of the copper alloy overlapping with the central axis of the open tungsten housing), and tungsten powder (with a purity of more than 99% and a grain size D50 of 6 μm) was added between the copper alloy and the tungsten housing with a thickness of 4 mm, and then placed in an isostatic press and pressed at 50 MPa for 2 h to obtain an electrode blank.
[0053] The electrode blank is forged at 1300°C, then straightened and polished (thickness tolerance is controlled to 0.03-0.1 mm), and the tungsten electrode (diameter 75 mm, length 750 mm, density of tungsten buffer layer is 12 g / cm) is made. 3 ) was obtained.
[0054] Performance Testing
[0055] Test Example 1
[0056] The masses of the tungsten electrodes obtained in Examples 1 to 3 are shown in Table 1.
[0057] Table 1. Mass of tungsten electrodes obtained in Examples 1 to 3 TIFF2024132775000002.tif26141
[0058] As can be seen from Table 1, the tungsten electrode provided by the present invention has a significantly reduced mass compared to a conventional pure tungsten electrode with the same dimensions.
[0059] Test Example 2
[0060] The resistance of the tungsten electrodes obtained in Examples 1 to 3 was tested, and the test results obtained are shown in Table 2.
[0061] Table 2 Resistance of tungsten electrodes obtained in Examples 1 to 3 TIFF2024132775000003.tif26118
[0062] As can be seen from Table 2, the tungsten electrode provided by the present invention has improved conductivity compared to the conventional pure tungsten electrode at the same size.
[0063] Test Example 3
[0064] The tungsten electrodes and pure tungsten electrodes obtained in Examples 1 to 3 were used as cathodes, graphite was used as anodes, and Pr(Nd)2O3-Pr(Nd)F3-LiF was used as electrolyte. A rare earth molten salt electrolysis test was performed at an electrolysis temperature of 1100°C and a current intensity of 6000 to 8000A, and the cathode voltage drop was tested. The test results are shown in Table 3.
[0065] Table 3. Cathode voltage drop of tungsten electrodes and pure tungsten electrodes obtained in Examples 1 to 3. TIFF2024132775000004.tif31143
[0066] As can be seen from Table 3, the tungsten electrode provided by the present invention has a lower voltage drop than the conventional pure tungsten electrode with the same dimensions.
[0067] Although the above embodiments have described the present invention in detail, they are only some of the embodiments of the present invention, not all of the embodiments, and other embodiments can be obtained based on the embodiments without inventive step, and all of these embodiments belong to the protection scope of the present invention. [Explanation of symbols]
[0068] 1 Copper alloy, 2 Open tungsten housing, 3 Tungsten buffer layer
Claims
1. A tungsten electrode for rare earth molten salt electrolysis, comprising an open tungsten housing and a copper alloy; the copper alloy is located within the open tungsten housing; a tungsten buffer layer is disposed between the copper alloy sidewall and the open tungsten housing; A tungsten electrode for rare earth molten salt electrolysis, characterized in that the bottom of the copper alloy is in contact with the inner bottom of the open tungsten housing.
2. The tungsten electrode of claim 1, wherein the copper alloy comprises a copper-vanadium alloy and / or a copper-niobium alloy.
3. The vanadium content in the copper-vanadium alloy is 5-15% by weight; 3. The tungsten electrode of claim 2, wherein the mass percent content of niobium in the copper-niobium alloy is 3-20%.
4. The open tungsten housing has an outer diameter of 65-120 mm and an inner diameter of 40-70 mm; The tungsten electrode of claim 1, wherein the thickness of the bottom of the open tungsten housing is 10 to 20 mm.
5. The diameter of the copper alloy is 20 to 60 mm; 2. The tungsten electrode according to claim 1, wherein the thickness of the tungsten buffer layer is 3 to 8 mm.
6. The density of the open tungsten housing is 18 g / cm 3 That's all. The density of the tungsten buffer layer is 12 to 14 g / cm 3 2. The tungsten electrode according to claim 1 .
7. A copper alloy is placed in the open tungsten housing, and tungsten powder is added between the copper alloy and the open tungsten housing, and pressed to obtain an electrode blank, and the central axis of the copper alloy overlaps with the central axis of the open tungsten housing; The method for producing a tungsten electrode for rare earth molten salt electrolysis according to any one of claims 1 to 6, further comprising the step of forging the electrode blank to obtain the tungsten electrode for rare earth molten salt electrolysis.
8. The method according to claim 7, characterized in that the pressure of the press is 50 to 80 MPa and the time is 2 to 5 hours.
9. The manufacturing method according to claim 7, characterized in that the forging temperature is 1000 to 1500°C.