Method for manufacturing semiconductor module, circuit board and method for manufacturing the same
The oxalic acid treatment effectively enhances solder wettability on Ni plating layers in semiconductor modules by reducing Ni hydroxide and P oxide, addressing hydrogen embrittlement and thermal stress issues in metal-ceramic composite circuit boards.
Patent Information
- Application Number
- JP2023163160
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2023-09-26
- Publication Date
- 2024-10-01
AI Technical Summary
Existing methods for improving solder wettability in semiconductor modules by incorporating hydrogen into the Ni plating layer face issues such as hydrogen embrittlement, and the thermal stress-induced warpage and deterioration of insulating layers in metal-ceramic composite circuit boards.
A method involving the use of an oxalic acid treatment to reduce Ni hydroxide and P oxide on the surface of the Ni plating layer, achieved by contacting the Ni plating layer with an oxalate ion-containing aqueous solution, thereby maintaining solder wettability without hydrogen addition or preheating processes.
Improves solder wettability on the Ni plating layer, reduces thermal stress-induced warpage, and maintains the integrity of the circuit board without hydrogen embrittlement, while eliminating the need for additional heating steps.
Smart Images

Figure 2024132810000001 
Figure 2024132810000002 
Figure 2024132810000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a semiconductor module, a circuit board, and a method for manufacturing the same. [Background technology]
[0002] Semiconductor modules such as power modules are used to control large amounts of power in electric vehicles, trains, machine tools, etc., and as circuit boards for these power modules, metal-ceramic bonded substrates using ceramics as an insulating layer (e.g., Patent Document 1) and resin insulating substrates using resin as an insulating layer (e.g., Patent Document 2) are used. A circuit pattern metal plate is formed on one side of the insulating layer of the circuit boards for these power modules, and a heat dissipation pattern metal plate is formed on the other side.
[0003] In general, in mounting a power module, a power semiconductor element is soldered to the circuit pattern metal plate, and a base plate (heat sink) or the like is attached to the heat dissipation metal plate by soldering, etc. Therefore, a Ni plating layer is applied to the surfaces of the circuit pattern metal plate and the heat dissipation metal plate to improve soldering and corrosion resistance.
[0004] As a method for improving the solder wettability of a Ni plating layer, Patent Document 3 proposes a Ni plating layer containing 10 ppm or more of hydrogen, and Patent Document 4 proposes a manufacturing method in which a member having a Ni plating layer is heated at 300°C to 400°C in an inert gas atmosphere before the soldering process. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-51778 A [Patent Document 2] JP 2007-288054 A [Patent Document 3] Japanese Patent Application Publication No. 9-36299 [Patent Document 4] JP 2015-8209 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the method of incorporating hydrogen into the Ni plating layer in Patent Document 3 has a problem in that the characteristics of the Ni plating layer deteriorate due to hydrogen embrittlement.
[0007] In addition, since the circuit board for the power module is a composite of metal and ceramics or insulating resin as described above, thermal stress and warping occur when heated due to the difference in thermal expansion coefficient between the metal and ceramics or insulating resin. Therefore, in order to prevent deterioration of the insulating layer and warping of the circuit board due to thermal stress, it is desirable to omit unnecessary heating steps such as those in Patent Document 4 in the mounting process of the power module.
[0008] Therefore, an object of the present invention is to provide a technology for improving the solder wettability of a Ni plating layer in the manufacture of a semiconductor module without incorporating hydrogen into the Ni plating layer or adding a preheating process before the soldering process. [Means for solving the problem]
[0009] As a result of intensive research to solve the above problems, the inventors found that hydroxides of Ni and composite oxides of P are generated on the surface of the Ni plating layer, inhibiting solder wettability. They also found that good solder wettability can be obtained by setting the peak area ratio of Ni(OH)2 to 10% or more and 60% or less of the total chemical bond state of Ni on the surface of the Ni plating layer. Furthermore, they found that the above chemical bond state can be obtained by treating the Ni plating layer with an aqueous solution containing oxalate ions.
[0010] The first aspect of the present invention is a preparation step of preparing a bonding substrate having a circuit pattern metal plate provided on one main surface of an insulating layer; a plating layer forming step of forming a Ni plating layer on the surface of the circuit pattern metal plate; a surface treatment step of contacting a surface of the Ni plating layer with an aqueous solution containing oxalate ions; and a soldering step of soldering an electronic component to the surface of the Ni plating layer after the surface treatment. A method for manufacturing a semiconductor module.
[0011] The second aspect of the present invention is the method according to the first aspect, In the surface treatment process, the surface treatment is performed so that when the chemical bond state of Ni in the Ni plating layer after surface treatment is measured by X-ray photoelectron spectroscopy, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less.
[0012] The third aspect of the present invention is the method according to the first or second aspect, In the plating layer forming step, the Ni plating layer is formed by electroless Ni-P plating, The Ni plating layer contains at least Ni and P.
[0013] A fourth aspect of the present invention relates to a method for producing a composition according to the third aspect, In the surface treatment step, the surface treatment is performed so that when the chemical bond state of P in the Ni plating layer after the surface treatment is measured by X-ray photoelectron spectroscopy, the peak area ratio of P-O bonds to the total chemical bond states of P is 10% or more and 40% or less.
[0014] A fifth aspect of the present invention is any one of the first to fourth aspects, In the surface treatment process, the surface treatment is carried out so that, when the Ni plating layer after the surface treatment is measured in the depth direction by X-ray photoelectron spectroscopy, the depth at which the oxygen concentration becomes 10 at% or less is 0.2 nm or more and 1.6 nm or less.
[0015] A sixth aspect of the present invention is any one of the first to fifth aspects, In the surface treatment step, the oxalic acid concentration of the oxalate ion-containing aqueous solution is set to 0.01 mass% to 8 mass% in terms of mass percent concentration of oxalic acid when oxalate ions are converted into oxalic acid, the temperature of the oxalic acid aqueous solution is set to 1°C to 40°C, and the treatment time is set to 1 second to 1000 seconds.
[0016] A seventh aspect of the present invention is any one of the first to sixth aspects, The insulating layer is a ceramic substrate.
[0017] An eighth aspect of the present invention is a method for producing a composition comprising the steps of: An insulating layer; a circuit pattern metal plate provided on at least one main surface of the insulating layer; A Ni plating layer is provided on the surface of the circuit pattern metal plate, The Ni plating layer is configured such that, when the chemical bond state of Ni is measured by X-ray photoelectron spectroscopy, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less. Circuit board.
[0018] A ninth aspect of the present invention relates to the eighth aspect, The Ni plating layer is a Ni-P alloy plating layer, and contains at least Ni and P.
[0019] A tenth aspect of the present invention relates to the ninth aspect, When the chemical bond state of P in the Ni plating layer is measured by X-ray photoelectron spectroscopy, the peak area ratio of PO bonds to all chemical bond states of P is 10% or more and 40% or less.
[0020] An eleventh aspect of the present invention is any one of the eighth to tenth aspects, When the Ni plating layer is measured in the depth direction by X-ray photoelectron spectroscopy, the depth at which the oxygen concentration becomes 10 at % or less is 0.2 nm or more and 1.6 nm or less.
[0021] A twelfth aspect of the present invention is any one of the eighth to eleventh aspects, The insulating layer is a ceramic substrate.
[0022] A thirteenth aspect of the present invention is a method for producing a composition comprising the steps of: a preparation step of preparing a bonding substrate having a circuit pattern metal plate provided on one main surface of an insulating layer; a plating layer forming step of forming a Ni plating layer on the surface of the circuit pattern metal plate; A surface treatment step of contacting a surface of the Ni plating layer with an aqueous solution containing oxalate ions. A method for manufacturing a circuit board.
[0023] A fourteenth aspect of the present invention relates to the thirteenth aspect, In the surface treatment process, the surface treatment is performed so that when the chemical bond state of Ni in the Ni plating layer after surface treatment is measured by X-ray photoelectron spectroscopy, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less.
[0024] A fifteenth aspect of the present invention relates to the thirteenth or fourteenth aspect, In the plating layer forming step, the Ni plating layer is formed by electroless Ni-P plating, The Ni plating layer contains at least Ni and P.
[0025] A sixteenth aspect of the present invention relates to the fifteenth aspect, In the surface treatment step, the surface treatment is performed so that when the chemical bond state of P in the Ni plating layer after the surface treatment is measured by X-ray photoelectron spectroscopy, the peak area ratio of P-O bonds to the total chemical bond states of P is 10% or more and 40% or less.
[0026] A seventeenth aspect of the present invention is any one of the thirteenth to sixteenth aspects, In the surface treatment process, the surface treatment is carried out so that, when the Ni plating layer after the surface treatment is measured in the depth direction by X-ray photoelectron spectroscopy, the depth at which the oxygen concentration becomes 10 at% or less is 0.2 nm or more and 1.6 nm or less.
[0027] The eighteenth aspect of the present invention is any one of the thirteenth to seventeenth aspects, In the surface treatment step, the oxalic acid concentration of the oxalate ion-containing aqueous solution is set to 0.01 mass% to 8 mass% in terms of mass percent concentration of oxalic acid when oxalate ions are converted into oxalic acid, the temperature of the oxalic acid aqueous solution is set to 1°C to 40°C, and the treatment time is set to 1 second to 1000 seconds.
[0028] A 19th aspect of the present invention is any one of the 13th to 18th aspects, The insulating layer is a ceramic substrate. Effect of the Invention
[0029] According to the present invention, it is possible to provide a manufacturing method for a semiconductor module and a circuit board that improve the solder wettability of a Ni plating layer formed on a circuit pattern metal plate without introducing hydrogen into the Ni plating layer or adding a preheating step before the soldering step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] <One embodiment of the present invention> A method for manufacturing a semiconductor module according to an embodiment of the present invention will be described below. The method for manufacturing a semiconductor module includes a method for manufacturing a circuit board. In this specification, a numerical range expressed using "to" means a range including the numerical values before and after "to" as the lower and upper limits.
[0031] (preparation process) First, a bonded substrate is prepared in which a circuit pattern metal plate is disposed on one main surface of an insulating layer and a heat dissipation pattern metal plate is disposed on the other main surface of the insulating layer. The bonded substrate can be produced, for example, as follows.
[0032] Specifically, first, an insulating layer, a metal plate for forming a circuit pattern for forming a metal plate with a predetermined circuit pattern, and a metal plate for forming a metal plate with a predetermined heat dissipation pattern are prepared.
[0033] The insulating layer is intended to support and fix the metal plate and to provide insulation between circuits and between the front and back of the circuit board. For example, an oxide-based insulating layer (insulating ceramic substrate) mainly composed of alumina or the like, or a non-oxide-based insulating layer (insulating ceramic substrate) mainly composed of aluminum nitride, silicon nitride, silicon carbide, boron nitride, or the like can be used as the insulating layer. For example, an insulating resin material in which insulating ceramic filler particles such as alumina, aluminum nitride, silicon nitride, silicon carbide, and boron nitride are dispersed in a polymer resin material can be used as the insulating layer. The size of the insulating layer is preferably 5 mm to 200 mm in length, 5 mm to 200 mm in width, and 0.05 mm to 3.0 mm in thickness, and more preferably 10 mm to 100 mm in length, 10 mm to 100 mm in width, and 0.1 mm to 2.0 mm in thickness, and is approximately rectangular.
[0034] The metal plate for forming a circuit pattern and the metal plate for forming a heat dissipation pattern are plate-like members made of pure metal or alloy. The metal plate includes a metal plate for forming a circuit pattern that is bonded to one side of an insulating layer and a metal plate for forming a heat dissipation pattern that is bonded to the other side of an insulating layer and a metal plate for forming a heat dissipation pattern. From the viewpoint of improving thermal conductivity and heat dissipation, the metal plate is preferably made of copper or a copper alloy, or aluminum or an aluminum alloy.
[0035] Next, a metal plate for forming a circuit pattern is placed on one surface (plate surface, main surface) of the insulating layer, and a metal plate for forming a heat dissipation pattern is placed on the other surface (plate surface, main surface) of the insulating layer, and then bonded to obtain a bonded body. As a bonding method, a known method such as brazing, direct bonding, adhesive bonding, etc. can be used. For example, when brazing is used, a paste-like brazing material is applied to both main surfaces of the insulating layer (ceramic substrate), a metal plate is placed on it, and the laminate is heated until the brazing material melts (a liquid phase is generated) and then cooled.
[0036] The two metal plates bonded to both main surfaces of the insulating layer may have the same composition or different compositions, but from the viewpoint of production efficiency, it is preferable that they have the same composition.
[0037] Next, a predetermined pattern is formed on each surface of the metal plates of the bonded body. Specifically, in the case of pattern formation by an etching method, for example, a resist film for etching having a predetermined circuit pattern is formed on the surface of the metal plate for forming a circuit pattern bonded to one surface of the insulating layer of the bonded body. Also, a resist film for etching having a predetermined heat dissipation pattern is formed on the surface of the metal plate for forming a heat dissipation pattern bonded to the other surface (other surface) of the insulating layer of the bonded body. These resist films may be formed on the surface of each metal plate by forming a resist by a known method such as a screen printing method, a lamination method, or a photomask method, and then curing it.
[0038] Next, the area of the metal plate that is not covered with the resist film is removed using a known etching solution such as cupric chloride, ferric chloride, hydrofluoric acid, a chelating agent, etc., and then the resist film is removed. Furthermore, when the bonded body is produced by a brazing method, unnecessary brazing material is removed to form the circuit pattern metal plate and the heat dissipation pattern metal plate.
[0039] This results in a bonded substrate having the circuit pattern metal plate and the heat dissipation pattern metal plate provided on both main surfaces of the insulating layer.
[0040] (Plating layer formation process) Next, the bonded substrate is subjected to Ni plating treatment to form a Ni plating layer on at least the surface of the circuit pattern metal plate or the heat dissipation pattern metal plate, thereby obtaining a plated bonded substrate. Note that Ni plating layers may be formed on the surfaces of both the circuit pattern metal plate and the heat dissipation pattern metal plate. As the Ni plating treatment, a known method such as electroless Ni-P plating, electroless Ni-B plating, or electric Ni plating may be adopted.
[0041] The thickness of the Ni plating layer is not particularly limited, but may be, for example, 1 μm or more and 20 μm or less. The Ni plating layer is preferably formed by electroless Ni-P plating, and is preferably a Ni-P alloy plating layer containing at least Ni and P. Note that electroplating requires electrodes and increases the handling required for arranging the electrodes, so the manufacturing cost is higher than that of electroless Ni-P plating. Also, electroless Ni-P has a faster film formation speed and can be manufactured at a lower cost than electroless Ni-B plating, so it is preferable to form the Ni plating layer by electroless Ni-P plating.
[0042] (Surface treatment process) Next, the plated bonded substrate is subjected to a surface treatment (hereinafter also referred to as oxalic acid treatment) using an oxalic acid aqueous solution (oxalic acid ion-containing aqueous solution). Specifically, the Ni plating layer of the plated bonded substrate is brought into contact with the oxalic acid ion-containing aqueous solution. After the contact is performed for a predetermined time, the substrate is washed with water to obtain a circuit substrate. Note that the oxalic acid treatment can also serve as pickling of the circuit substrate, so that pickling with dilute sulfuric acid after washing with water can be omitted.
[0043] As described above, Ni hydroxides and P composite oxides are likely to occur on the surface of the Ni plating layer during its formation. In particular, when the Ni plating layer is formed by Ni-P plating, Ni hydroxides (e.g., Ni(OH)2, etc.) and P composite oxides are more likely to occur. When the proportion of Ni hydroxides and P oxides increases, the solder wettability of the Ni plating layer tends to decrease. In this regard, by performing an oxalic acid treatment, the Ni hydroxides and P oxides contained in the Ni plating layer, mainly in the surface layer of the Ni plating layer, can be removed and their proportions can be reduced.
[0044] The contact method with the oxalate ion-containing aqueous solution may be a method of immersing the plated bonded substrate in the oxalate ion-containing aqueous solution (immersion method), or a method of spraying the oxalate ion-containing aqueous solution onto the plated bonded substrate (shower method, spray method, mist spray method, etc.). If plating is performed by the immersion method in the plating layer formation step, it is preferable to also use the immersion method in the surface treatment step from the viewpoint of handling.
[0045] The treatment time for the oxalic acid treatment (the time during which the oxalate ion-containing aqueous solution is in contact with the Ni plating layer) is preferably 1 to 1000 seconds. By setting the treatment time to 1 second or more, excellent solderability can be ensured. On the other hand, the upper limit of the treatment time is not particularly limited, but it is preferable to set it to 1000 seconds or less from the viewpoint of sufficiently reducing hydroxides and complex oxides on the surface of the Ni plating layer while shortening the treatment time from a cost perspective.
[0046] The solution temperature during the surface treatment of the oxalate ion-containing aqueous solution is not particularly limited, but is, for example, in the range of 1° C. to 40° C., and preferably room temperature of 5 to 35° C. From the viewpoint of promoting the reduction reaction by oxalate ions, the solution temperature is preferably 1° C. or higher. On the other hand, if the solution temperature is high, hydroxides and oxides are likely to be generated on the surface layer of the Ni plating layer by the oxalic acid treatment, so from the viewpoint of efficiently reducing hydroxides and oxides, the solution temperature is preferably 40° C. or lower.
[0047] An aqueous solution containing oxalate ions can be obtained not only by dissolving oxalic acid in water, but also by dissolving an oxalate salt (such as ammonium oxalate or sodium oxalate) that produces oxalate ions upon ionization in water.
[0048] The oxalic acid concentration of the oxalate ion-containing aqueous solution is preferably in the range of 0.01 mass% to 8 mass% in terms of the mass percent concentration of oxalic acid, calculated by converting oxalate ions into oxalic acid. If it is less than 0.01 mass%, it is not economical because the treatment time becomes long. In addition, when the oxalic acid treatment process is performed continuously from the plating layer formation process, the oxalic acid concentration of the oxalate ion-containing aqueous solution is likely to decrease due to the introduction of the washing water from the previous process, and from this viewpoint as well, a concentration less than 0.01 mass% is inferior in mass productivity. On the other hand, the upper limit of the oxalic acid concentration is not particularly limited, but from an economic viewpoint, it is preferable that it is 8 mass% or less.
[0049] In addition, "the mass percent concentration of oxalic acid converted from oxalate ions to oxalic acid" refers to the mass percent concentration calculated by converting the oxalate ions contained in the oxalate salt to the same amount (mol) of oxalic acid. For example, ammonium oxalate has 1 oxalate ion C2O4 per molecule of ammonium oxalate (NH4)2C2O4. 2- Since the ammonium oxalate solution contains one oxalic acid ion, the "mass percent concentration of oxalic acid, calculated as oxalic acid, C2H2O4" is expressed by the following formula (1).
[0050]
number
[0051] The circuit board obtained by the oxalic acid treatment is composed of an insulating layer, a circuit pattern metal plate provided on one main surface (one side) of the insulating layer, a heat dissipation pattern metal plate provided on the other main surface (the other side) of the insulating layer, and Ni plating layers provided on the surfaces of the circuit pattern metal plate and the heat dissipation pattern metal plate. It is preferable that the Ni plating layer is configured so that its surface is in the following chemical bond state by the oxalic acid treatment.
[0052] Specifically, when the chemical bond state of Ni is measured by X-ray photoelectron spectroscopy (hereinafter, also simply referred to as XPS), the Ni plating layer preferably has a peak area ratio of Ni hydroxide in the total chemical bond state of Ni of 10% to 60%. Here, the total chemical bond state of Ni refers to all chemical bond states that Ni can take in the Ni plating layer, such as Ni-Ni bond, Ni-P bond, Ni(OH)2 bond, etc. These chemical bond states are detected in the XPS spectrum as, for example, a peak derived from Ni-P alloy (Ni-Ni bond or Ni-P bond) and a peak derived from Ni(OH)2. The peak area ratio of Ni hydroxide refers to the ratio of the peak area derived from Ni hydroxide to the sum of the peak areas of all chemical bond states of Ni, that is, the sum of the peak areas derived from the chemical bond states that Ni can take. This peak area ratio is an index of the amount of Ni hydroxide. By making the peak area ratio of hydroxide 60% or less, the solder wettability of the Ni plating layer can be maintained high. On the other hand, even if the amount of hydroxide of Ni is reduced, a certain amount of hydroxide still exists, so the peak area ratio is at least 10% or more. The peak area ratio is preferably 15% or more and 50% or less. The peak area ratio of the hydroxide of Ni in the total chemical bond state of Ni may be, for example, 20% or more, or 25% or more. An example of the hydroxide of Ni is Ni(OH)2. The peak area ratio may be calculated by determining each peak area based on a composite function obtained by fitting the XPS spectrum with, for example, a Gaussian function. Details will be described in the following examples.
[0053] The chemical bond state of Ni can be obtained by analyzing the XPS spectrum of the chemical bond state of Ni2p orbital obtained by XPS, as described later in the Examples. For example, when the Ni plating layer is formed by Ni-P plating and contains at least Ni and P, the peak area ratio is the ratio of the peak area originating from Ni(OH)2 to the sum of the areas of the peaks originating from Ni-P alloy (Ni-Ni bonds and Ni-P bonds) and the peaks originating from Ni(OH)2 as the hydroxide of Ni.
[0054] In addition, when the Ni plating layer is formed by electroless Ni-P plating and contains at least Ni and P, it is preferable that when the chemical bond state of P is measured for the Ni plating layer by X-ray photoelectron spectroscopy, the peak area ratio of PO bonds to the total chemical bond state of P is 10% or more and 40% or less. In electroless Ni-P plating, when the temperature of the plating bath is 50°C to 95°C and the Ni plating layer contains P, oxides of P are likely to be generated on the surface layer. In this regard, the oxalic acid treatment can reduce the oxides of P together with the hydroxides of Ni, and reduce the proportion of PO bonds. The peak area ratio of PO bonds may be, for example, 15% or more, 20% or more.
[0055] The total chemical bond state of P indicates all the chemical bond states that P can take in the Ni plating layer. The peak area ratio of the PO bond indicates the ratio of the peak area derived from the oxide of P to the total peak area derived from the chemical bond state that P can take in the Ni plating layer, and is an index of the amount of the oxide of P. As described later in the examples, the chemical bond state of P indicates the chemical bond state of the P2p orbital obtained by XPS, and can be obtained by analyzing the XPS spectrum. For example, when the Ni plating layer is formed by Ni-P plating and contains at least Ni and P, the peak area ratio of the PO bond is the ratio of the peak area derived from the PO bond to the total area of the peak derived from the P-Ni bond and the peak derived from the PO bond.
[0056] In addition, when the Ni plating layer is measured in the depth direction by X-ray photoelectron spectroscopy, the depth at which the oxygen concentration is 10 at% or less is preferably 0.2 nm to 1.6 nm. That is, in the Ni plating layer, the thickness of the region where the oxygen concentration is 10 at% or less by oxalic acid treatment is preferably 0.2 nm to 1.6 nm. By removing hydroxides and oxides in the surface layer of the Ni plating layer by oxalic acid treatment, the oxygen concentration in the surface layer can be reduced. By making the region where the oxygen concentration is 10 at% or less at a depth of at least 0.2 nm or more, the high solder wettability of the Ni plating layer can be more reliably achieved. The thickness of the surface-treated surface layer is calculated from the sputtering rate in terms of SiO2, as described later in the examples. The depth at which the oxygen concentration is 10 at% or less is preferably 1.4 nm or less.
[0057] The conditions for the oxalic acid treatment may be appropriately adjusted so that the surface of the Ni plating layer is in the above-mentioned chemically bonded state, such as the time for contacting the aqueous solution containing oxalic acid, the temperature, and the oxalic acid concentration.
[0058] (Module formation process) Next, electronic components such as semiconductor elements are mounted by soldering on the circuit pattern metal plate of the circuit board.
[0059] In this embodiment, the surface of the Ni plating layer formed on the metal plate for circuits is configured to have less Ni hydroxide and oxide, so that when solder is applied, the solder spreads easily, and electronic components can be fixed to the metal plate for circuits more stably.
[0060] As described above, the method for manufacturing a semiconductor module according to an embodiment of the present invention has been shown, and the circuit board of the present invention can be obtained.
[0061] (4) Effects of this embodiment According to this embodiment, one or more of the following advantages are achieved.
[0062] (a) In this embodiment, after a Ni plating layer is formed on the surface of the circuit pattern metal plate in the bonded substrate, the Ni plating layer is brought into contact with an oxalic acid ion-containing solution to perform an oxalic acid treatment. The oxalic acid treatment can remove, for example, Ni hydroxides that are generated in the Ni plating layer during the formation process of the Ni plating layer. This reduces hydroxides that inhibit the solder wettability of the surface of the circuit pattern metal plate, and achieves high solder wettability.
[0063] (b) In the surface treatment step, it is preferable to perform the oxalic acid treatment so that when the chemical bond state of Ni is measured by XPS on the surface of the Ni plating layer after the surface treatment, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less. By performing the oxalic acid treatment in this manner, the amount of hydroxide in the Ni plating layer can be further reduced, and the above-mentioned effect of (a) can be more reliably obtained. It is preferable to perform the oxalic acid treatment so that the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 15% or more and 50% or less. The oxalic acid treatment may be performed so that the peak area ratio of Ni hydroxide is, for example, 20% or more, 25% or more.
[0064] (c) In the plating layer forming step, a Ni plating layer is formed by electroless Ni-P plating, and in the surface treatment step, it is preferable to perform an oxalic acid treatment on the Ni plating layer containing at least Ni and P so that the peak area ratio of PO bonds to the total chemical bond state of P in the Ni plating layer is 10% to 40%. This makes it possible to more reliably obtain the effect of (a) described above. The oxalic acid treatment may be performed so that the peak area ratio of PO bonds is, for example, 15% or more, 20% or more.
[0065] (d) In the surface treatment step, it is preferable to perform the surface treatment so that the depth at which the oxygen concentration is 10 at% or less in the depth direction of the Ni plating layer is 0.2 nm to 1.6 nm. In other words, it is preferable to perform the surface treatment so that the oxygen concentration in the region of the Ni plating layer from the surface to a depth of 0.2 nm to 1.6 nm is 10 at% or less. This makes it possible to reduce hydroxides and oxides contained in the surface layer portion of the Ni plating layer that comes into contact with the solder, and to more reliably obtain the effect of (a) described above. It is preferable to perform the surface treatment so that the depth at which the oxygen concentration is 10 at% or less is 1.4 nm or less.
[0066] (e) Furthermore, according to the surface treatment process, the sulfuric acid washing can be omitted. Generally, the plated bonded substrate obtained in the plating layer formation process requires water washing or sulfuric acid washing using dilute sulfuric acid. However, if the water washing is insufficient, the dilute sulfuric acid may remain on the plated bonded substrate. If sulfur components derived from dilute sulfuric acid exist as sulfur residues, it may cause corrosion or migration of the Ni plating layer. In this regard, according to the oxalic acid treatment, the sulfuric acid washing can be omitted, and the corrosion or migration of the Ni plating layer can be suppressed. In addition, oxalic acid only produces carbon dioxide by reduction reaction, and the remaining components derived from oxalic acid can be suppressed. Even if oxalic acid remains in the Ni plating layer, oxalic acid has excellent thermal decomposition properties, so it can be easily decomposed by heating during soldering.
[0067] (f) In addition, as a method for improving the solder wettability, there is a method of making the Ni plating layer have a predetermined hydrogen content, but in this case, the Ni plating layer may be embrittled by hydrogen and its characteristics may deteriorate. In this regard, the oxalic acid treatment of the present embodiment can maintain the inherent characteristics of the Ni plating layer without causing hydrogen embrittlement.
[0068] (g) As a method for improving the solder wettability, there is a method in which after forming a Ni plating layer, the Ni plating layer is heated in an inert gas atmosphere at 300°C to 400°C before soldering, but in this case, further heating at a high temperature may cause residual thermal stress or warping in the circuit board due to the difference in thermal expansion coefficient between the insulating layer and the metal plate for the circuit. In this regard, the oxalic acid treatment of this embodiment can improve the solder wettability without further heating.
[0069] <Other embodiments of the present invention> Although the embodiment of the present invention has been specifically described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the gist of the present invention.
[0070] For example, in the above embodiment, a case has been described in which metal plates are bonded to both main surfaces of an insulating layer, but in a circuit board, it is sufficient that a metal plate is bonded to at least one main surface of an insulating layer.
[0071] In the above embodiment, the case where the surface treatment (oxalic acid treatment) step is performed continuously after the plating step has been described, but the surface treatment (oxalic acid treatment) step can be performed at any timing after the plating step. For example, the plating step may be performed, and other steps, such as a step of printing an individual identification number by laser marking, may be provided before the surface treatment (oxalic acid treatment) step. Alternatively, Ni plating may be applied to the raw metal plate of the circuit board in advance, the raw metal plate may be treated with oxalic acid, and a circuit pattern metal plate or a heat dissipation pattern metal plate may be formed by punching, and then the plated bonded substrate may be adhesively bonded to an insulating layer. Furthermore, the plated bonded substrate obtained in the plating layer formation step may be stored for a long period of time, such as six months or more, and then subjected to an oxalic acid treatment step in order to ensure solder wettability.
[0072] In the above embodiment, the case where the circuit pattern and the heat dissipation pattern are formed by the etching method has been described as an example, but the present invention is not limited to this. For example, after forming the circuit pattern metal plate and the heat dissipation pattern metal plate in advance by punching a metal plate, they may be bonded to the insulating layer (ceramic substrate or insulating resin material) by a known method (soldering, direct bonding, etc.). EXAMPLES
[0073] Next, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.
[0074] (1) Preparation of the circuit board Example 1 First, an aluminum nitride (AlN) substrate measuring 54 mm × 42 mm × 0.64 mm was prepared as an insulating layer, a copper plate for forming a circuit pattern and a copper plate for forming a heat dissipation pattern measuring 54 mm × 42 mm × 0.3 mm were prepared as metal plates, and Ag-Cu-Ti brazing material paste (the mass ratio of metal powder in the brazing material was Ag:Cu:Ti = 88:10:2) was prepared as an active metal-containing brazing material.
[0075] Next, copper plates were bonded to both sides of the AlN substrate using active metal brazing. Specifically, a paste-like brazing material was screen-printed on both sides of the AlN substrate. After that, a copper plate for forming a circuit pattern and a copper plate for forming a heat dissipation pattern were placed on both sides of the AlN substrate via the brazing material, and the laminate was heated in a vacuum furnace. In this way, the AlN substrate and the copper plate were bonded to produce a bonded body.
[0076] Next, etching resists of the circuit pattern shape and the heat dissipation pattern shape were formed by screen printing on the copper plate for forming the circuit pattern and the copper plate for forming the heat dissipation pattern on both sides of the bonded body. Next, unnecessary copper plates were etched and removed using a known etching solution containing copper chloride to form the circuit pattern metal plate and the heat dissipation pattern metal plate, and then the resist film was removed. Next, unnecessary brazing material remaining on the ceramic substrate around the circuit pattern metal plate and the heat dissipation pattern metal plate was removed using a known chemical solution containing a chelating agent to obtain a bonded substrate. Next, a Ni-P (alloy) plating layer having a thickness of 4 μm was formed on the surface of the copper circuit pattern metal plate and the heat dissipation pattern metal plate by electroless Ni-P plating method to obtain a plated bonded substrate. In this example, six plated bonded substrates (batch A) with the same treatment batch of electroless Ni-P plating were prepared. These were randomly divided into two equal parts.
[0077] Next, the plated bonded substrate obtained by dividing into two halves was subjected to an oxalic acid treatment under the following conditions. Specifically, first, oxalic acid (anhydrous) was dissolved in pure water to prepare an oxalic acid ion-containing aqueous solution with an oxalic acid concentration of 1 mass%. Next, the three plated bonded substrates obtained by dividing into two halves were immersed in the oxalic acid ion-containing aqueous solution (1 mass%) at a liquid temperature of 25°C for 640 seconds, removed, washed with pure water, and further dried by air blowing to obtain a circuit board as an evaluation sample of Example 1. The conditions for the oxalic acid treatment are summarized in Table 1 below.
[0078] [Table 1]
[0079] Comparative Example 1 In Comparative Example 1, as shown in Table 1, a plated bonded substrate of batch A, which was the same processing batch of electroless Ni-P plating as in Example 1, was pickled with dilute sulfuric acid, and a circuit board was obtained as an evaluation sample for Comparative Example 1 without performing oxalic acid treatment.
[0080] (Examples 2 and 3) In Examples 2 and 3, Ni plating was formed using a treatment batch (batch B) of electroless Ni-P plating different from that in Example 1, and nine plated bonded substrates were prepared. These were randomly divided into three equal parts, and the three plated bonded substrates were each subjected to an oxalic acid treatment under the conditions shown in Table 1. In Examples 2 and 3, the oxalic acid treatment was performed in the same manner as in Example 1, except that the oxalic acid concentration of the oxalic acid ion-containing aqueous solution and the treatment time were changed as shown in Table 1. Specifically, in Example 2, the oxalic acid concentration of the oxalic acid ion-containing aqueous solution was 0.5 mass%, and the treatment time (immersion time) was 5 seconds. In Example 3, the oxalic acid concentration of the oxalic acid ion-containing aqueous solution was 5 mass%, and the treatment time (immersion time) was 150 seconds. As a result, circuit boards were obtained as evaluation samples for Examples 2 and 3.
[0081] Comparative Example 2 In Comparative Example 2, as shown in Table 1, three plated bonded substrates of batch B obtained in Example 2 or Example 3 were subjected to pickling with dilute sulfuric acid, and no oxalic acid treatment was performed to obtain circuit boards as evaluation samples for Comparative Example 2.
[0082] (2) Evaluation method Each of the evaluation samples obtained above was evaluated by XPS and solder wettability. Each evaluation method is explained below.
[0083] (Evaluation by XPS) In the evaluation by XPS, XPS measurement was performed on each evaluation sample to measure the chemical bonding state of Ni in the Ni plating layer, the chemical bonding state of P, and the O atom concentration in the depth direction.
[0084] Specifically, first, each evaluation sample was introduced into a scanning X-ray photoelectron spectrometer (ULVAC-PHI Inc.'s "PHI 5000 VersaProbe III"), and XPS measurements were performed to obtain spectrum data. The measurement conditions were a monochromated AlKα X-ray source with an output of 25 W and an acceleration voltage of 15 kV. The X-ray incidence angle was 90 degrees and the photoelectron take-off angle was 45 degrees. The photoelectron measurement conditions were a pass energy of 69 eV, an integration time of 80 ms, a measurement energy interval of 0.125 eV / step, and 25 times of accumulation for the chemical bond state analysis, and a pass energy of 140 eV, an integration time of 40 ms, a measurement energy interval of 0.25 eV / step, and 5 times of accumulation for the depth direction analysis.
[0085] Next, the chemical bond state of Ni was analyzed from the acquired spectrum data. The chemical bond state of Ni was analyzed from the Ni2p orbital (measurement position 844.0 eV to 894.0 eV). Here, the background was removed by the interated Shirley method, and the peaks derived from the Ni-P alloy (Ni-Ni bond and Ni-P bond) were fitted with 10 bands (Band 1 to Band 10), and the peaks derived from Ni(OH)2 were fitted with 8 bands (Band 11 to Band 18). The Gaussian function was selected as the fitting waveform function. The fitting parameters, the area ratio to the reference band, the energy difference, and the half-width difference, were fixed as shown in Tables 2 and 3, and fitting was performed.
[0086] [Table 2]
[0087] [Table 3]
[0088] The ratio of the peak area of the composite function of the Ni(OH)2 peak to the peak area of the composite function of the entire Ni2p orbital obtained by the above fitting was obtained, and used as an index of the amount of Ni hydroxide in the surface layer of the Ni plating layer. In this embodiment, peaks derived from Ni-Ni bonds, Ni-P bonds, and Ni(OH)2 were detected as peaks in the composite spectrum of the entire Ni2p orbital, and the composite function of the entire Ni2p orbital was obtained by fitting these spectral peaks by the above method. That is, the peak area of the entire chemical bond state of Ni in this embodiment is the sum of the area of the composite function fitted with the peaks derived from the Ni-P alloy (Ni-Ni bonds and Ni-P bonds) and the area of the composite function fitted with the peaks derived from Ni(OH)2.
[0089] In addition, the chemical bond state of P was analyzed from the acquired spectrum data. The chemical bond state of P was analyzed in the P2p orbital (measurement position 123.0 eV to 143.0 eV). Here, the background was removed by the Shirley method, and fitting was performed as two components: the P-Ni bond peak (Band 1 to Band 2 in fitting) and the PO bond peak (Band 3 to Band 4 in fitting). The Gauss-Lorentz function was selected as the waveform function for fitting. Fitting was performed by fixing the area ratio, energy difference, and half-width difference relative to the reference band as fitting parameters, as shown in Tables 4 and 5.
[0090] [Table 4]
[0091] [Table 5]
[0092] The ratio of the peak area of the PO bond peak to the peak area of the composite function of the entire P2p orbital obtained by the above fitting was obtained, and used as an index of the amount of P oxide in the Ni-P plating layer. In this embodiment, peaks derived from P-Ni bonds and PO bonds were detected as peaks in the composite spectrum of the entire P2p orbital, and the composite function of the entire P2p orbital was obtained by fitting these spectral peaks by the above method. That is, the peak area of the entire chemical bond state of P in this embodiment is the sum of the area of the composite function fitted with the peak derived from the P-Ni bond and the area of the composite function fitted with the peak derived from the PO bond.
[0093] Furthermore, a depth profile analysis (depth profiling measurement) was performed on the O atom concentration in the depth direction. In this example, the depth at which the oxygen concentration was 10 at% or less was determined. The Ar ion sputtering conditions were an acceleration voltage of 2 kV, an emission current of 7 mA, and a sputtering rate of 2 nm / min in terms of SiO2.
[0094] (solder wettability) The solder wettability of each evaluation sample was evaluated as follows. Specifically, first, Sn-Pb eutectic cream solder was applied to the Ni plating layer of the circuit board using a metal mask under the conditions of 20 mm square x 0.6 mm thickness. Next, the board with the cream solder applied was placed on a hot plate and held at 210°C for 2 minutes in an air atmosphere to melt the solder, and then the board was brought into contact with a cooling plate to cool and solidify the solder. The area where the solder had wetted and spread was obtained by image analysis, and the wetted area (%) of the solder relative to the applied area was calculated. This evaluation was performed on two boards, and the average value was used as the evaluation result.
[0095] (3) Evaluation results The results of the evaluation methods described above are summarized in Table 1 above.
[0096] As shown in Table 1, in Examples 1 to 3 in which oxalic acid treatment was performed, the peak area ratio of Ni(OH)2 in the total chemical bond state of Ni in the Ni plating layer was 36.9% (Example 1), 45.4% (Example 2), and 27.6% (Example 3), respectively, and it was confirmed that it was 10% or more and 60% or less. In addition, in each Example, the peak area ratio of PO bond in the total chemical bond state of P in the Ni plating layer was 34.7% (Example 1), 32.8% (Example 2), and 24.7% (Example 3), respectively, and it was confirmed that it was 10% or more and 40% or less. In addition, when the depth at which the oxygen concentration becomes 10 at% or less in the Ni plating layer was obtained, it was 0.8 nm (Example 1), 1.2 nm (Example 2), and 0.6 nm (Example 3), respectively, and it was confirmed that it was 0.2 nm or more and 1.6 nm or less in each Example. From these results, it was found that there were few hydroxides of Ni and oxides of P in the surface layer of the Ni plating layer in Examples 1 to 3. In these examples, when soldering was performed on the Ni plating layer, the ratio of the area where the solder was wetted and spread to the area where the solder was applied was 100%, indicating high solder wettability.
[0097] In contrast, in Comparative Examples 1 and 2, the peak area ratios of Ni(OH)2 were 66.0% (Comparative Example 1) and 74.6% (Comparative Example 2), respectively, exceeding 60%, and the peak area ratios of PO bonds were 42.1% (Comparative Example 1) and 44.3% (Comparative Example 2), respectively, exceeding 40%. Moreover, it was confirmed that the depths at which the oxygen concentration was 10 at% or less were 1.8 nm (Comparative Example 1) and 1.8 nm (Comparative Example 2), respectively, exceeding 1.6 nm. In other words, it was found that in Comparative Examples 1 and 2, hydroxides and oxides of Ni and P generated in the process of forming the Ni plating layer existed from the surface to deep regions, and the ratios of hydroxides and oxides were high. Therefore, it was found that when solder was applied onto the Ni plating layer, the solder was difficult to wet and spread, and the solder wettability was lower than 100%.
[0098] As described above, by subjecting the Ni plating layer of a circuit board to surface treatment by contacting it with an aqueous solution containing oxalic acid, it is possible to reduce the amount of Ni hydroxides and oxides contained in the surface layer of the Ni plating layer and improve solder wettability.
Claims
1. a preparation step of preparing a bonding substrate having a circuit pattern metal plate provided on one main surface of an insulating layer; a plating layer forming step of forming a Ni plating layer on the surface of the circuit pattern metal plate; a surface treatment step of contacting a surface of the Ni plating layer with an aqueous solution containing oxalate ions; A soldering process of soldering an electronic component to the surface of the Ni plating layer after the surface treatment. A method for manufacturing a semiconductor module.
2. In the surface treatment step, the surface treatment is performed so that when the chemical bond state of Ni is measured by X-ray photoelectron spectroscopy for the Ni plating layer after the surface treatment, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less. The method for manufacturing the semiconductor module according to claim 1 .
3. In the plating layer forming step, the Ni plating layer is formed by electroless Ni-P plating, The Ni plating layer contains at least Ni and P. The method for manufacturing the semiconductor module according to claim 1 or 2.
4. In the surface treatment step, the surface treatment is performed so that when the chemical bond state of P in the Ni plating layer after the surface treatment is measured by X-ray photoelectron spectroscopy, the peak area ratio of P-O bonds to the total chemical bond state of P is 10% or more and 40% or less. The method for manufacturing the semiconductor module according to claim 3 .
5. In the surface treatment step, the surface treatment is performed so that the depth at which the oxygen concentration becomes 10 at% or less is 0.2 nm or more and 1.6 nm or less when the Ni plating layer after the surface treatment is measured in the depth direction by X-ray photoelectron spectroscopy. The method for manufacturing the semiconductor module according to claim 1 or 2.
6. In the surface treatment step, the oxalic acid concentration of the oxalate ion-containing aqueous solution is 0.01 mass% to 8 mass% in terms of mass percent concentration of oxalic acid content calculated by converting oxalate ions into oxalic acid, the temperature of the oxalic acid aqueous solution is 1°C to 40°C, and the treatment time is 1 second to 1000 seconds. The method for manufacturing the semiconductor module according to claim 1 or 2.
7. The insulating layer is a ceramic substrate. The method for manufacturing the semiconductor module according to claim 1 or 2.
8. An insulating layer; a circuit pattern metal plate provided on at least one main surface of the insulating layer; A Ni plating layer is provided on the surface of the circuit pattern metal plate, The Ni plating layer is configured such that, when the chemical bond state of Ni is measured by X-ray photoelectron spectroscopy, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less. Circuit board.
9. The Ni plating layer is a Ni-P alloy plating layer, and the Ni plating layer contains at least Ni and P. The circuit board according to claim 8.
10. When the chemical bond state of P in the Ni plating layer is measured by X-ray photoelectron spectroscopy, the peak area ratio of P-O bonds to the total chemical bond state of P is 10% or more and 40% or less. The circuit board according to claim 9.
11. When the Ni plating layer is measured in the depth direction by X-ray photoelectron spectroscopy, the depth at which the oxygen concentration is 10 at% or less is 0.2 nm or more and 1.6 nm or less. The circuit board according to claim 8 or 9.
12. The insulating layer is a ceramic substrate. The circuit board according to claim 8 or 9.
13. a preparation step of preparing a bonding substrate having a circuit pattern metal plate provided on one main surface of an insulating layer; a plating layer forming step of forming a Ni plating layer on the surface of the circuit pattern metal plate; A surface treatment step of contacting a surface of the Ni plating layer with an aqueous solution containing oxalate ions. A method for manufacturing a circuit board.
14. In the surface treatment step, the surface treatment is performed so that when the chemical bond state of Ni is measured by X-ray photoelectron spectroscopy for the Ni plating layer after the surface treatment, the peak area ratio of Ni hydroxide to the total chemical bond state of Ni is 10% or more and 60% or less. The method for manufacturing a circuit board according to claim 13 .
15. In the plating layer forming step, the Ni plating layer is formed by electroless Ni-P plating, The Ni plating layer contains at least Ni and P. The method for manufacturing a circuit board according to claim 13 or 14.
16. In the surface treatment step, the surface treatment is performed so that when the chemical bond state of P in the Ni plating layer after the surface treatment is measured by X-ray photoelectron spectroscopy, the peak area ratio of P-O bonds to the total chemical bond state of P is 10% or more and 40% or less. The method for manufacturing a circuit board according to claim 15 .
17. In the surface treatment step, the surface treatment is performed so that the depth at which the oxygen concentration becomes 10 at% or less is 0.2 nm or more and 1.6 nm or less when the Ni plating layer after the surface treatment is measured in the depth direction by X-ray photoelectron spectroscopy. The method for manufacturing a circuit board according to claim 13 or 14.
18. In the surface treatment step, the oxalic acid concentration of the oxalate ion-containing aqueous solution is 0.01 mass% to 8 mass% in terms of mass percent concentration of oxalic acid content calculated by converting oxalate ions into oxalic acid, the temperature of the oxalic acid aqueous solution is 1°C to 40°C, and the treatment time is 1 second to 1000 seconds. The method for manufacturing a circuit board according to claim 13 or 14.
19. The insulating layer is a ceramic substrate. The method for manufacturing a circuit board according to claim 13 or 14.
Citation Information
Patent Citations
Lead frame for semiconductor device
JP1997036299A
Power module
JP2007288054A
Soldering method and method of manufacturing semiconductor device
JP2015008209A
Metal-ceramic bonded substrate
JP2016051778A