Film having excellent near-infrared ray shielding properties
A laminated film with specific polyester resin layers addresses the challenge of maintaining high visible light transmittance and near-infrared shielding on large surfaces by using naphthalene dicarboxylic acid and cyclohexanedimethanol units, ensuring uniformity and performance.
Patent Information
- Application Number
- JP2024035482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-01
AI Technical Summary
Existing films struggle to maintain high visible light transmittance and near-infrared shielding properties while avoiding issues like haze, crystallization, and streaks, especially when applied to large surfaces such as automobile windshields.
A laminated film structure with alternating layers of polyester resins, where layer A contains naphthalene dicarboxylic acid units and layer B contains cyclohexanedimethanol units, ensuring a refractive index difference and interference reflection, with specific optical properties to achieve high transmittance and shielding performance.
The film maintains excellent visible light transmittance, near-infrared shielding, and uniform appearance even under severe conditions, with minimal haze and streaks, suitable for large applications like vehicle windshields.
Smart Images

Figure 2024132948000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a film that blocks near-infrared radiation. [Background technology]
[0002] In buildings such as houses and offices, or in transportation such as vehicles and ships, the temperature inside the room or inside the vehicle rises due to the incidence of light from light sources such as sunlight, fluorescent lights, and lamps through light-transmitting bodies such as window glass. One method for keeping the temperature inside buildings and transportation constant is to operate air conditioning equipment, but air conditioning equipment consumes extra energy, and in transportation, the operation of air conditioning equipment also causes a problem of deterioration in fuel efficiency. Even if the temperature is controlled to a comfortable level by operating air conditioning equipment, it is difficult to suppress the unpleasant burning or stinging sensation caused by light rays from outside the building or transportation, especially near-infrared rays, hitting the human body. Therefore, the light-transmitting body is required to have the property of blocking near-infrared rays contained in the light from the sun or light source. Furthermore, the light-transmitting body used for the above-mentioned purposes is also required to transmit visible light contained in the light from the sun or light source from the viewpoint of ensuring brightness and visibility.
[0003] In order to solve the above problem, Patent Document 1 proposes the use of a sheet material in which near-infrared absorbing particles are dispersed. On the other hand, by dispersing particles in a sheet material, the visible light transmittance is reduced, so it is difficult to simultaneously satisfy near-infrared shielding and visible light transmittance. Patent Documents 2 and 3 propose a heat ray reflective film that utilizes the light interference phenomenon that occurs when two or more materials with different refractive indices are alternately laminated at a layer thickness of the wavelength level of the light reflection band. Since this technology does not substantially contain particles inside the film, it is possible to simultaneously satisfy near-infrared shielding and visible light transmittance. The heat ray reflective films of Patent Documents 2 and 3 use polyethylene terephthalate or polyethylene naphthalate as one resin and a copolymer polyester with a low refractive index as the other resin for reasons such as transparency, heat resistance, weather resistance, chemical resistance, strength, and dimensional stability, but when polyethylene naphthalate is used in particular, the refractive index difference between the materials becomes large, and a film with high reflectance can be obtained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-100880 A [Patent Document 2] JP 2017-177810 A [Patent Document 3] Patent Publication No. 2022-91206 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the method described in Patent Document 2 has a problem in that, when a reliability test is conducted when the near-infrared reflective film is applied to an actual product such as a window glass, the haze increases due to crystallization of the organic small molecules in the film. Also, the method described in Patent Document 3 has a problem in that, when the film is sized to be applied to a large product such as an automobile windshield, streaks extending in one direction are generated, resulting in portions that are inferior in appearance and heat ray reflection performance.
[0006] An object of the present invention is to overcome the drawbacks of the conventional techniques and to provide a film which is capable of maintaining excellent visible light transmittance, near-infrared shielding properties and appearance even under severe conditions. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention has the following configuration: A film having an average transmittance of 80% or more in the wavelength band of 400 nm or more and 800 nm or less, an average transmittance of less than 20% in the wavelength band of 900 nm or more and 1200 nm or less, a change in the half-maximum wavelength end λmin on the short wavelength side of less than 30 nm, a haze of less than 3.0%, and an increase in haze of less than 1.0% in a heating test at 100°C for 24 hours.
[0008] The film of the present invention can also be in the following form. (1) A film having an average transmittance of 80% or more in the wavelength band of 400 nm or more and 800 nm or less, and an average transmittance of less than 20% in the wavelength band of 900 nm or more and 1200 nm or less, over the entire surface of the film measuring 1 m x 1 m, a change in the half-maximum wavelength end λmin on the short wavelength side of less than 30 nm, a haze of less than 3.0%, and an increase in haze of less than 1.0% in a heating test at 100°C for 24 hours. (2) The film according to (1), in which a layer having a relatively high refractive index is designated as layer A and a layer having a relatively low refractive index is designated as layer B, and the layer A and the layer B are alternately laminated in 51 or more layers. (3) The film according to (2), wherein the layer A is mainly composed of a polyester resin. (4) The film according to (3), wherein the polyester resin which is the main component of the layer A is a copolymer containing naphthalenedicarboxylic acid units as dicarboxylic acid units. (5) The film according to (4), wherein in the polyester resin which is the main component of the layer A, the main dicarboxylic acid unit is a naphthalenedicarboxylic acid unit. (6) The film according to any one of (2) to (5), wherein in the polyester resin which is the main component of the layer A, the polyalkylene glycol unit accounts for 1 wt % or more and 15 wt % or less of the entire diol component. (7) The film according to any one of (2) to (6), wherein the layer B is mainly composed of a polyester resin. (8) The film according to (7), wherein the polyester resin that is the main component of the layer B is a polyester resin containing a cyclohexanedimethanol unit. (9) The film according to any one of (1) to (8), which shows a change in average transmittance in the wavelength range of 900 nm or more and 1200 nm or less of less than 8% in a heating test at 100° C. for 24 hours. (10) The film according to any one of (1) to (9), which is used as an element constituting a light-transmitting body used in a vehicle or building material. Effect of the Invention
[0009] According to the present invention, it is possible to provide a film that can maintain excellent visible light transmittance, near-infrared shielding properties, and appearance even under severe conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The film of the present invention is characterized in that, over the entire surface of a film measuring 1 m x 1 m, the average transmittance in the wavelength band of 400 nm to 800 nm is 80% or more, the average transmittance in the wavelength band of 900 nm to 1200 nm is less than 20%, the change in the half-maximum wavelength end λmin on the short wavelength side is less than 30 nm, the haze is less than 3.0%, and the increase in haze in a heating test at 100°C for 24 hours is less than 1.0%. The film of the present invention will be specifically described below.
[0011] It is important that the film of the present invention has an average transmittance of 80% or more in the wavelength band of 400 nm to 800 nm over the entire surface of the film having a size of 1 m x 1 m. Since the wavelength band of 400 nm to 800 nm corresponds to the wavelength band of visible light, if the average transmittance of the film in this band decreases, coloring may be observed or visibility may be impaired due to scattering of visible light. From the above viewpoint, the average transmittance in this band is preferably 85% or more. On the other hand, from the above viewpoint, the higher the average transmittance in this band, the more preferable it is, so the upper limit is not particularly limited, but it is 100% from the viewpoint of feasibility.
[0012] In the present invention, the average transmittance in the wavelength band of 400 nm to 800 nm can be calculated as the average value of all the measured values obtained by measuring the transmittance at an incident angle Φ=0° at wavelength intervals of 1 nm in the wavelength band of 400 nm to 800 nm. The transmittance can be measured using a known spectrophotometer, the details of which will be described later (the method of measuring the transmittance is the same for other wavelength bands described later, except that the target wavelength bands change).
[0013] In the present invention, "the average transmittance of 80% or more in the wavelength band of 400 nm to 800 nm over the entire surface of a 1 m x 1 m film" means that the average transmittance of 80% or more in the wavelength band of 400 nm to 800 nm over the entire surface of a 1 m x 1 m film is a 50 mm x 50 mm sample centered at the intersection of the diagonal lines and all four 50 mm x 50 mm samples including each apex (total number of samples is 5). The same applies to each indicator specified "over the entire surface of a 1 m x 1 m film" except for the change in the half-value wavelength end λmin on the short wavelength side. The reason for this interpretation is that each indicator specified "over the entire surface of a 1 m x 1 m film" is due to stretching unevenness or lamination unevenness in the longitudinal direction or width direction, so if the requirements of these indicators are met in all of the above five samples, it is considered that the other parts of the 1 m x 1 m film will also meet them.
[0014] The method of obtaining a film having an average transmittance of 80% or more in the wavelength band of 400 nm to 800 nm on the entire surface of the film having a size of 1 m x 1 m is not particularly limited, but for example, the composition of the film may be a composition that does not contain a pigment or dye that absorbs or reflects light in the wavelength band of 400 nm to 800 nm. In addition, for example, when the film is a laminated film utilizing the principle of interference reflection, a method of adjusting the reflection band by the refractive index and thickness of each layer to increase the transmittance in the wavelength band of 800 nm or less may be used. In the case of such a laminated film, the reflection wavelength is determined according to the following formula 1. That is, in such a laminated film, the reflection in the wavelength band of 400 nm to 800 nm can be suppressed by adjusting the refractive index and thickness of each layer. In obtaining a film having an average transmittance of 80% or more in the wavelength band of 400 nm to 800 nm on the entire surface of the film having a size of 1 m x 1 m, the preferable condition film configuration and manufacturing method will be described later. 2×(nA dA + nB dB)=mλ Equation 1 nA: Average in-plane refractive index of A layer nB: Average in-plane refractive index of B layer dA: Layer thickness of A layer (nm) dB: Layer thickness of layer B (nm) λ: Main reflection wavelength (reflection wavelength). m:1,2,3,...(m:1=1st-order reflection, m:2=2nd-order reflection, m:3=3rd-order reflection,...).
[0015] The film of the present invention is not particularly limited as long as it does not impair the effects of the present invention, but in a film of 1 m x 1 m, the color tone of the transmitted color in the film plane is preferably a saturation C* value of 10.0 or less. The film of the present invention is intended to be used in a portion where visibility is required, and if the C* value of the transmitted color is high, the film will be colored, impairing the appearance and visibility. From the above viewpoint, the C* value of the transmitted color is preferably 5.0 or less, more preferably 3.0 or less. In addition, since the coloring is preferably small, it is not necessary to set a lower limit for the C* value of the transmitted color, but from the viewpoint of feasibility, the lower limit is 0. The method of obtaining such a film is not particularly limited, but it can be obtained by the film configuration and manufacturing method described later. Note that C* can be calculated from the a* value and b* value of the transmitted light by the following formula 2, and the details of the method of measuring the a* value and b* value of the transmitted light will be described later. C*={(a*) 2 +(b*) 2} 1 / 2 formula 2 It is important that the film of the present invention has an average transmittance of less than 20% in the wavelength band of 900 nm to 1200 nm in a film of 1 m x 1 m. Sunlight has an intensity distribution mainly in the visible light region, and the intensity distribution tends to become smaller as the wavelength increases. However, in order to use it in applications where high visibility is required, it is possible to provide high heat shielding performance while maintaining high visibility by efficiently blocking light with a wavelength of 900 nm to 1200 nm (about 18% of the total sunlight intensity) that is slightly larger than the visible light region. From the above viewpoint, the average transmittance is preferably less than 15%, more preferably less than 13%, in the wavelength band of 900 nm to 1200 nm. Since it is possible to provide high heat shielding performance as the average reflectance in the wavelength range of 900 to 1200 nm increases, it is not necessary to set a lower limit for the average transmittance, but the lower limit is 0% from the viewpoint of feasibility. The method for obtaining such a film is not particularly limited, but it can be obtained by the film configuration and manufacturing method described below.
[0016] It is important that the film of the present invention has a change of less than 30 nm in the half-value wavelength end λmin on the short wavelength side in a film of 1 m x 1 m. When the film of the present invention is used, for example, as an automobile windshield or a large window glass, it is desirable that the appearance, visibility, and heat shielding properties are uniform in the size used. For this reason, in order to be able to respond to various applications in which a certain size is desired, it is desirable that the change of the half-value wavelength end λmin on the short wavelength side in a film of 1 m x 1 m is less than 30 nm. Here, the definition of λmin is the wavelength of the shortest wavelength part in the wavelength band Π where the transmittance is less than 50%, when the wavelength band Π is the wavelength band that shows a transmittance of less than 80% continuously for 100 nm or more located at a wavelength of 400 nm or more in the spectrum in the wavelength band of 240 nm to 2600 nm, with the horizontal axis being the wavelength (nm) and the vertical axis being the reflectance (%).
[0017] If the change in λmin is 30 nm or more, it will affect the appearance, visibility, and heat insulation. The factors that change λmin are not limited to this example, but may include, for example, longitudinal streak defects and thickness unevenness due to interference between the film and the die lip, and the influence of layer disorder in the laminated film. Here, the change in λmin can be specified by the following method. First, for example, light from a three-wavelength fluorescent lamp is applied to a film sample, followed by a polarizing plate and then the film, and the film is observed while wearing polarized sunglasses from the opposite side of the fluorescent lamp with the film in between, to check for color changes such as streaks. If there is no color change at this stage, it is considered that the change in the half-value wavelength end λmin on the short wavelength side is less than 30 nm. On the other hand, if there is a color change, the area without color change is designated as S1, the λmin of S1 is designated as λmin(S1), the color tone area is designated as S2, and the λmin of S2 is designated as λmin(S2) (details of the method of specifying the area will be described later). Thereafter, the reflection spectra of S1 and S2 are obtained using a spectrophotometer under the conditions described below, and λmin(S1) and λmin(S2) are determined.
[0018] When λmin(S1)≧λmin(S2)+30 nm or λmin(S1)≦λmin(S2)-30 nm, the near-infrared heat shielding property of S2 deteriorates and the thickness changes corresponding to the wavelength shift, resulting in a deterioration in the appearance of the film. From the above viewpoint, in a film having a size of 1 m×1 m, the change in λmin is preferably less than 20 nm, more preferably less than 15 nm, and even more preferably less than 10 nm. In a film having a size of 1 m×1 m, the smaller the change in λmin, the more uniform the final product obtained, so there is no need to set a lower limit for the change in λmin, but from the viewpoint of feasibility, the lower limit is 0 nm.
[0019] The method for obtaining such a film is not particularly limited, but for example, a method can be used in which the effect of die swelling, in which the resin expands when it is discharged from a T-die, is suppressed to reduce interference between the resin and the lip, thereby suppressing the occurrence of streaks. More specifically, adjustment of the die lip width and adjustment of the melting temperature of the thermoplastic resin (particularly, when a layer with a relatively high refractive index is layer A and a layer with a relatively low refractive index is layer B, layer A is used in the case where 51 or more layers of layers A and B are alternately laminated) are effective for adjusting the change in λmin. The method for obtaining such a film will be described in detail later in the film configuration and manufacturing method.
[0020] It is important that the film of the present invention has a haze of less than 3.0% in a film of 1 m x 1 m. If the haze is 3.0% or more, the visibility of the film is impaired. From the above viewpoint, the haze of the film of the present invention is preferably less than 2.0%, more preferably less than 1.5%, and particularly preferably less than 1.3. The lower the haze of the film, the better the visibility, so there is no need to set a lower limit for the haze, but from the viewpoint of feasibility, the lower limit is 0%. The method of obtaining such a film is not particularly limited, but for example, a method of producing a film using a resin that does not contain particles inside can be mentioned. The haze of the film can be measured according to the old JIS-K-7105 (1994), and the details will be described later.
[0021] It is important that the film of the present invention, with a size of 1 m x 1 m, has a haze increase of less than 1.0% in a heating test at 100°C for 24 hours. If the haze increase is 1.0% or more in a heating test at 100°C for 24 hours, the haze may increase and visibility may be impaired when the product using the film is used under harsh conditions such as outdoors or in direct sunlight, or when used for a long period of time. From the above perspective, the haze increase in a heating test at 100°C for 24 hours is preferably less than 0.5%, more preferably less than 0.3%. The method of obtaining such a film is not particularly limited, but for example, a method of producing a film using a resin that does not contain organic low molecules inside is mentioned below in detail.
[0022] In the film of the present invention, when a layer having a relatively high refractive index is designated as an A layer and a layer having a relatively low refractive index is designated as a B layer, it is preferable that the A layer and the B layer are alternately laminated in 51 or more layers. The layer having a relatively high refractive index here refers to a layer having a relatively high in-plane refractive index. Also, the term "alternately laminated" here refers to layers made of different resins being laminated in a regular arrangement in the thickness direction. For example, layers are laminated in a regular arrangement such as A(BA)n (n is a natural number representing the number of repeating units).
[0023] By alternately laminating resins with different optical properties in this way, it becomes possible to reflect light of a specific wavelength by the principle of interference reflection due to the relationship between the difference in refractive index of each layer and the layer thickness. In addition, the more layers are laminated, the higher the reflectance can be obtained over a wider band. From the above viewpoint, the number of layers A and B is more preferably 201 layers or more in total, and even more preferably 401 layers or more in total. A laminated film that applies the principle of interference reflection can achieve a higher reflectance for light of a wider wavelength band as the number of layers increases, so that a laminated film with high near-infrared shielding performance can be obtained. Therefore, although there is no upper limit to the number of layers, as the number of layers increases, the manufacturing cost increases due to the enlargement of the manufacturing equipment, and the handling property deteriorates due to the thickening of the film, so that in reality, the practical range is within a total of 1001 layers. The method of obtaining such a film is not particularly limited, but for example, a co-extrusion method using multiple extruders and a lamination method in which films are bonded together are known. Among them, the co-extrusion method can laminate a large number of layers in one process, and is very advantageous in terms of productivity and cost, so it can be suitably used as a manufacturing method for the film of the present invention. In the coextrusion method, for example, a multi-manifold die, a feed block, a static mixer, etc. can be used to laminate a large number of layers with high precision. A preferred production method for obtaining such a laminated film will be described later.
[0024] The thickness of the film of the present invention is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 10 μm or more and 200 μm or less. When the film of the present invention is used, for example, for automobile windshield applications, it may be required to conform to a 3D shape. Therefore, from the viewpoint of conformity to a 3D shape, the thickness is preferably 200 μm or less. In addition, if it is less than 10 μm, while maintaining transparency in the visible light region, the thickness of each layer of the laminate as the total thickness may be thin and the number of layers may be reduced, making it difficult to set the near-infrared shielding property within the range of the present invention.
[0025] The film of the present invention preferably contains a polyester resin as a main component. Here, the main component refers to a component contained in an amount of more than 50 wt% to 100 wt% or less when the entire layer is taken as 100 wt% (hereinafter, the main component can be interpreted in the same way). Polyester resins are generally cheaper than thermosetting resins and photocurable resins, and can be easily and continuously formed into a sheet by known melt extrusion. Therefore, by using a polyester resin in layer A, it is possible to obtain a laminated film at low cost and with good productivity.
[0026] The polyester resin as the main component of the A layer is preferably a polyester obtained by polymerization of a monomer mainly composed of an aromatic dicarboxylic acid or an aliphatic dicarboxylic acid and a diol, in other words, a polyester resin mainly composed of an aromatic dicarboxylic acid unit or an aliphatic dicarboxylic acid unit and a diol unit. Here, examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid (1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid), 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, etc. Examples of aliphatic dicarboxylic acids include adipic acid, suberic acid, sebacic acid, dimer acid, dodecanedioic acid, cyclohexanedicarboxylic acid, and their ester derivatives.
[0027] Among them, from the viewpoint of realizing a high refractive index, it is preferable that the polyester resin, which is the main component of the A layer, is a copolymer containing naphthalenedicarboxylic acid units as dicarboxylic acid units. More preferably, the polyester resin, which is the main component of the A layer, is a copolymer containing naphthalenedicarboxylic acid as the main dicarboxylic acid unit, and even more preferably, the main dicarboxylic acid unit in the polyester resin, which is the main component of the A layer, is naphthalenedicarboxylic acid units. The main dicarboxylic acid unit here refers to a dicarboxylic acid unit contained in the polyester at more than 50 wt% and 100 wt% or less of the dicarboxylic acid units constituting the polyester. In addition, in the polymerization of the polyester resin, only one of these dicarboxylic acid components may be used, or two or more may be used in combination, and further, oxyacids such as hydroxybenzoic acid may be partially copolymerized.
[0028] Examples of diol components for obtaining the polyester resin as the main component of the A layer include ethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, 2,2-bis(4-hydroxyethoxyphenyl)propane, isosorbate, and spiroglycol. Among these, ethylene glycol is preferably used in terms of high refractive index, crystallinity, melt viscosity, and film-forming properties. These diol components may be used alone or in combination of two or more. More preferably, ethylene glycol is used as the main diol component. The term "used as the main diol component" used herein refers to the use of ethylene glycol in a proportion of more than 50 wt% and not more than 100 wt% of the diol components constituting the polyester.
[0029] In the film of the present invention, the polyester resin which is the main component of Layer A preferably contains naphthalene dicarboxylic acid units as main dicarboxylic acid units from the viewpoint of glass transition temperature (hereinafter, such a polyester resin may be referred to as polyethylene naphthalate).
[0030] In addition, from the viewpoint of heat resistance and film-forming property, the film of the present invention is preferably such that the polyalkylene glycol unit is 1 wt% or more and 15 wt% or less of the total diol component in the polyester resin, which is the main component of the A layer. For example, when polyethylene naphthalate is used as the main component of the A layer, it is preferable that the polyethylene naphthalate contains a polyalkylene glycol unit. The amount of the polyalkylene glycol unit is preferably 1 wt% or more and 15 wt% or less of the total diol component in terms of crystal controllability, heat resistance, film-forming property, and reactivity in polyester resin production. When the amount of the polyalkylene glycol unit is 1 wt% or more, the heat resistance and film-forming property are improved. On the other hand, when the amount of the polyalkylene glycol unit is 15 wt% or less, the generation of decomposition gas caused by the decomposition product of the polyalkylene glycol is suppressed, air bubbles are less likely to be generated in the film, and the occurrence of optical defects is reduced.
[0031] As such polyalkylene glycol, polyethylene glycol, polytrimethylene glycol, polytetramethylene glycol, etc. can be preferably used, but polyethylene glycol is preferable from the viewpoint of designing the glass transition temperature related to crystallinity and film formability. The number average molecular weight of polyethylene glycol is preferably 200 or more and less than 1000 from the viewpoint of reactivity and heat resistance. By having a number average molecular weight of less than 1000, the decrease in reactivity accompanying an increase in molecular weight and the whitening of the polyester resin due to incompatibility are reduced.
[0032] In the film of the present invention, polyester resin, acrylic resin, polycarbonate resin, etc. can be used as the thermoplastic resin constituting the B layer. Among them, it is preferable that the B layer is mainly composed of a polyester resin. Polyester resin is generally cheaper than thermosetting resin or photocurable resin, and can be easily and continuously formed into a sheet by known melt extrusion. Therefore, it is possible to obtain a laminated film at low cost and with good productivity.
[0033] In the film of the present invention, it is preferable that Layer A and Layer B are made of polyester resins having different optical properties. Different optical properties here means that the refractive index differs by 0.01 or more in any one of two orthogonal directions arbitrarily selected within a plane and a direction perpendicular to the plane.
[0034] In the film of the present invention, the difference in the in-plane average refractive index between the A layer and the B layer is preferably 0.05 or more. More preferably, it is 0.12 or more, and even more preferably, it is 0.14 or more and 0.35 or less. If the difference in the in-plane average refractive index is less than 0.05, it may be difficult to have a band in which the average transmittance from 900 to 1200 nm is 20% or less. As an example of a method for achieving this, a method in which the main component of the A layer is a crystalline polyester resin (hereinafter referred to as crystalline polyester A) and the B layer contains an amorphous polyester resin (hereinafter referred to as amorphous polyester B) can be mentioned. The term "crystalline" as used herein means that the heat of fusion is 20 J / g or more in differential scanning calorimetry (DSC). On the other hand, the term "amorphous" means that the heat of fusion is 5 J / g or less. The crystalline polyester resin can be oriented and crystallized in the stretching and heat treatment process to have a higher in-plane average refractive index than that in the amorphous state before stretching. On the other hand, in the case of amorphous polyester resin, by performing heat treatment at a temperature far above the glass transition temperature in the heat treatment process, the slight orientation that occurs in the stretching process can be completely alleviated and the in-plane average refractive index can be maintained. In this way, since a refractive index difference can be easily created between the crystalline polyester resin and the amorphous polyester resin in the stretching and heat treatment processes in the production of the film, it is possible to improve the near-infrared reflection shielding performance. If the difference in the in-plane average refractive index is greater than 0.35, the lamination of the resin deteriorates, making the lamination itself difficult, and the film becomes inferior in heat resistance and handling. The in-plane average refractive index of each layer can be measured according to JIS K7142 (2014) Method A, the details of which will be described later.
[0035] In the film of the present invention, the polyester resin, which is the main component of the B layer, is preferably a polyester resin containing cyclohexanedimethanol units, and more preferably the resin is amorphous. The polyester resin containing cyclohexanedimethanol units refers to a copolyester copolymerized with cyclohexanedimethanol, a homopolyester, or a polyester blended with them. Such polyester resins are preferred because they have a small difference in glass transition temperature with polyethylene terephthalate, so they are unlikely to be overstretched during molding and are unlikely to peel off between layers.
[0036] Polyester resins containing cyclohexanedimethanol units are very strongly bonded to polyethylene terephthalate and polyethylene naphthalate. In addition, the cyclohexanedimethanol group has a geometric isomer such as a cis isomer or a trans isomer, and a conformational isomer such as a chair or boat isomer, so that even when co-stretched with polyethylene terephthalate or polyethylene naphthalate, it is difficult to be oriented and crystallized, and while having near-infrared shielding performance, it is also difficult to break during film formation. More preferably, polymers having different optical properties are preferably made of a combination having similar basic skeletons. The basic skeleton here refers to a repeating unit constituting a resin. For example, when polyethylene naphthalate is used as one of the thermoplastic resins, it is preferable that the basic skeleton contains an ethylene naphthalate skeleton, or that the basic skeleton contains an ethylene terephthalate skeleton, which is a basic skeleton similar to ethylene naphthalate, from the viewpoint of easily realizing a highly accurate laminate structure. When thermoplastic resins having different optical properties contain the same or similar basic skeletons, the lamination precision is increased, and further, delamination at the lamination interface is less likely to occur.
[0037] From the viewpoint of suppressing the variation in the reflection properties of the film, it is preferable that the difference in glass transition temperature between the main components of each layer is 20° C. or less. When the difference in glass transition temperature between the two is 20° C. or less, problems such as overstretching during film formation of the laminated film are alleviated, and the variation in the near-infrared shielding performance is suppressed.
[0038] When the film of the present invention is a laminated film in which layers A and B are alternately laminated, the reflection wavelength is determined according to the following formula 1, which is the principle of interference reflection. In other words, the reflection band can be adjusted by the refractive index and thickness of each layer. 2×(nA dA + nB dB)=mλ Equation 1 nA: Average in-plane refractive index of A layer nB: Average in-plane refractive index of B layer dA: Layer thickness of A layer (nm) dB: Layer thickness of layer B (nm) λ: Main reflection wavelength (reflection wavelength) m:1,2,3,...(m:1=1st-order reflection, m:2=2nd-order reflection, m:3=3rd-order reflection,...).
[0039] In order to make the film of the present invention a film with reduced coloring of the film itself, it is preferable to adjust the thickness of each layer to sufficiently reflect the wavelength band of 900 nm or more, while sufficiently transmitting the wavelength band of 800 nm or less. In addition, by reflecting the wavelength band of 1200 nm or more, the third reflection becomes 400 nm or more, so the reflection wavelength is preferably 1200 nm or less. In the film-making process, it is difficult to control slight thickness unevenness or slight reflectance difference in the film plane, but by reducing the difference in transmittance in the wavelength band, it is preferable to make a film with reduced color variation of the film itself even in a film with thickness unevenness or reflectance difference in the film plane.
[0040] The film of the present invention preferably has a change rate of the average transmittance in the wavelength band of 900 nm to 1200 nm in a heating test at 100°C for 24 hours of less than 8%. If the average transmittance in the wavelength band of 900 nm to 1200 nm in a heating test changes, the performance of the film may change during the film processing process or harsh usage conditions, and the heat-shielding performance may deteriorate, so it is preferable that the change in the average transmittance after the heating test is small. From the above viewpoint, the change rate of the average transmittance is more preferably 5% or less, and even more preferably 3% or less. The change rate of the average transmittance in the wavelength band of 900 nm to 1200 nm in a heating test at 100°C for 24 hours can be measured by a known spectrophotometer after heating in an oven in an atmosphere of 100°C and cooling to room temperature, and the details of the measurement method will be described later.
[0041] In order to make the change rate of the average transmittance of the film of the present invention in the wavelength band of 900 nm to 1200 nm in a heating test at 100°C for 24 hours less than 8% or within the above-mentioned preferred range, a method of adjusting the heat treatment conditions after stretching can be mentioned. More specifically, for example, by lowering the heat treatment temperature within the preferred range described later, the change rate of the average transmittance can be suppressed low.
[0042] Next, a preferred method for producing the film of the present invention will be described below using a laminated film as an example. Of course, the present invention is not limited to this example. The formation of the laminated structure of the laminated film can be realized by referring to the description in paragraphs
[0053] to
[0063] of JP-A-2007-307893.
[0043] The thermoplastic resin is prepared in the form of pellets or the like. The pellets are dried in hot air or under vacuum as necessary, and then fed to separate extruders. In the extruder, the resin is heated to above its melting point, and the extrusion amount of the resin is uniformized by a gear pump or the like, and foreign matter and denatured resin are removed through a filter or the like. These resins are molded into the desired shape by a T-die and then discharged. The film discharged from the T-die is extruded onto a cooling body such as a casting drum, and cooled and solidified to obtain a casting film. At this time, it is preferable to use a wire-shaped, tape-shaped, needle-shaped, or knife-shaped electrode to adhere to a cooling body such as a casting drum by electrostatic force and rapidly solidify. In addition, a method in which air is blown out from a slit-shaped, spot-shaped, or planar device to adhere to a cooling body such as a casting drum and rapidly solidify, or a method in which the film is adhered to a cooling body such as a nip roll and rapidly solidified is also preferable.
[0044] Here, when a copolymer containing naphthalene dicarboxylic acid units as dicarboxylic acid units is used in the outermost layer (A layer), longitudinally extending streaks accompanied by deformation frequently occur on the film surface, which may impair the visible light transmittance, near infrared shielding properties, and appearance of the film. The resin properties of polyethylene naphthalate include a large die swell and resin viscosity compared to polyethylene terephthalate, and the reason for the occurrence of streaks is thought to be that the die swell of polyethylene naphthalate is large, which causes interference between the die lip and the resin to increase, resulting in the occurrence of streaks. From the above perspective, the die swell of the thermoplastic resin of the A layer is preferably 1.19 or less, more preferably 1.17 or less, and even more preferably 1.15 or less. In addition, the lower limit of the die swell is 0 or more from the viewpoint of feasibility. The die swell of the thermoplastic resin of the A layer can be measured by ISO 11443 (2021), the details of which will be described later.
[0045] The die swell of the thermoplastic resin of the A layer occurs when the resin passes through the gap, due to the effect of the normal stress difference and the speed difference on the resin, and is released from the gap, due to the effect of the relaxation of the normal stress and the elimination of the speed difference. Therefore, one method of reducing the die swell is to adjust the die lip width to relax the normal stress during extrusion. On the other hand, when the die lip width is widened, the streaks extending in the longitudinal direction are relaxed, but the film thickness variation increases. In addition, when the die lip width is narrowed, the interference between the die lip and the resin becomes greater, and the streaks extending in the longitudinal direction become more visible, which is not preferable. From the above viewpoint, the die lip width is preferably 3 mm or more and 6 mm or less, more preferably 4 mm or more and 6 mm or less.
[0046] A method for alleviating normal stress is to reduce the viscosity of the thermoplastic resin of layer A. From the viewpoint of alleviating normal stress, the viscosity of the thermoplastic resin of layer A is preferably 200 Pa·s or more and less than 400 Pa·s, more preferably 200 Pa·s or more and less than 350 Pa·s. As a method for reducing the resin viscosity, for example, the addition of a good flow agent can be mentioned, but this method involves mixing low molecules into the resin, which causes issues such as an increase in haze of the original film and an increase in haze over time due to long-term use. Another solution is, for example, a method of reducing the intrinsic viscosity (IV), but there is also the issue that reducing the IV makes the film itself brittle and makes film formation difficult. Therefore, the present inventors have studied diligently and found that a method of reducing the resin viscosity by increasing the extrusion temperature is preferable. The method of increasing the extrusion temperature does not change the properties of the resin, so it is preferable because it does not change the properties when made into a film. The viscosity of the thermoplastic resin of layer A can be measured by ISO 11443 (2021), the details of which will be described later.
[0047] When the method of decreasing the die swell is to increase the extrusion temperature to decrease the melt viscosity, for example, when polyethylene naphthalate or its copolymer is used as the thermoplastic resin of the main component of the A layer, the extrusion temperature is preferably 290°C or higher, more preferably 295°C or higher. By increasing the extrusion temperature to 290°C or higher, the melt viscosity can be decreased to 350 Pa·s, and as a result, the shear stress is relaxed and the die swell can be relaxed. When the polyethylene naphthalate with reduced viscosity during extrusion is extruded into a film, the die swell is reduced, so that interference with the die is reduced, and the occurrence of streaks can be suppressed. The upper limit of the extrusion temperature is preferably 400°C from the viewpoint of reducing the deterioration of the appearance of the film due to the denaturation of the resin and the occurrence of defects due to the denatured resin.
[0048] In addition, when preparing a multi-layer laminated film made of a plurality of thermoplastic resins, it is preferable to use two or more extruders to send the plurality of thermoplastic resins from different flow paths and feed them into a multi-layer lamination device. As the multi-layer lamination device, a multi-manifold die, a feed block, a static mixer, etc. can be used, but in particular, in order to efficiently obtain the configuration of the present invention, it is preferable to use a feed block that includes at least two or more separate members having a large number of fine slits. When such a feed block is used, the device does not become extremely large, so that there is little foreign matter due to thermal deterioration, and even if the number of layers is extremely large, high-precision lamination is possible. In addition, the lamination accuracy in the width direction is significantly improved compared to the conventional technology. In addition, it is also easy to form an arbitrary layer thickness configuration. In this device, the thickness of each layer can be adjusted by the shape (length, width) of the slit, so that it is easy to achieve an arbitrary layer thickness. The molten multi-layer laminate formed in the desired layer configuration in this way is guided to a T-die, and a casting film is obtained in the same manner as described above.
[0049] The casting film thus obtained is preferably biaxially stretched as necessary. Here, biaxial stretching refers to stretching in the longitudinal direction and the width direction. Stretching may be performed in two directions successively or simultaneously. The longitudinal direction refers to the direction in which the film runs, and the width direction refers to the direction perpendicular to the longitudinal direction within the film plane.
[0050] Here, the case of sequential biaxial stretching will be described. Here, stretching in the longitudinal direction refers to stretching for giving the film molecular orientation in the longitudinal direction, and is usually performed by the difference in peripheral speed of rolls. This stretching may be performed in one stage, or may be performed in multiple stages using a pair of rolls. The stretching ratio varies depending on the type of thermoplastic resin, but is usually preferably 2 to 15 times, and particularly preferably 2 to 7 times. The stretching temperature is preferably the glass transition temperature of the thermoplastic resin having the highest glass transition temperature among the main components of each layer constituting the multilayer laminate film to the glass transition temperature + 100°C.
[0051] The uniaxially stretched film thus obtained may be subjected to a surface treatment such as corona treatment, frame treatment, or plasma treatment as necessary, and then may be imparted with properties such as easy slippage, easy adhesion, and antistatic properties by in-line coating.
[0052] Subsequently, the film is stretched in the width direction. The stretching in the width direction refers to stretching for giving the film a width direction orientation, and is usually performed by conveying the film while holding both ends of the film with clips or the like in a direction perpendicular to the running direction of the film using a tenter to widen the width. The stretching ratio varies depending on the type of thermoplastic resin, but is usually preferably 2.0 to 15 times, and particularly preferably 2.0 to 7.0 times. The stretching temperature is preferably the glass transition temperature of the thermoplastic resin having the higher glass transition temperature among the main components of each layer to the glass transition temperature + 120°C. In order to give a temperature equal to or higher than the glass transition temperature of the thermoplastic resin while holding it with clips or the like, when the laminated film is stretched in the width direction, it is preferable that both surfaces of the surface layer are made of layer A.
[0053] The biaxially stretched film is preferably subsequently heat-treated in a tenter at a temperature equal to or higher than the stretching temperature and equal to or lower than the melting point in order to impart flatness and dimensional stability. During this heat treatment, it is preferable to instantly relax the film in the longitudinal direction immediately before and / or after entering the heat treatment zone in order to suppress the distribution of the main orientation axis in the width direction. The heat treatment time is preferably 3 to 200 seconds, more preferably 5 to 100 seconds, and even more preferably 10 to 30 seconds. The preferred degree of relaxation treatment is a ratio of the relaxation treatment to the film width before the relaxation treatment of 0% to 5.0%. After being heat-treated in this way, the film is uniformly and gradually cooled, cooled to room temperature, and wound up.
[0054] The heat treatment temperature is preferably 180° C. or more and 245° C. or less from the viewpoint of improving the dimensional stability of the film and maintaining the flatness. From the viewpoint of improving the dimensional stability of the film and obtaining a sufficient reflectance, the heat treatment temperature is preferably 180° C. or more. On the other hand, from the viewpoint of suppressing deterioration of the flatness due to the film itself starting to melt, the heat treatment temperature is preferably 245° C. or less.
[0055] In addition, if the heat treatment temperature is increased, the minute oriented crystals that occur when the amorphous resin is stretched laterally can be destroyed, lowering the refractive index of the amorphous resin and increasing the difference in refractive index with the crystalline resin. As a result, the average transmittance of the film itself in the wavelength range of 900 nm to 1200 nm can be lowered (in other words, the reflectance can be increased). On the other hand, if the heat treatment temperature is increased, the movement of the free molecules in the amorphous resin becomes active due to heat, generating minute thermal crystals, resulting in a large decrease in the average reflectance in that range after the heat test.
[0056] On the other hand, if the heat treatment temperature is low, the minute oriented crystals that are generated when the amorphous resin is stretched laterally remain unbroken, suppressing the decrease in the refractive index of the amorphous resin. As a result, the difference in refractive index with the crystalline resin does not increase, and the average transmittance of the film itself in the wavelength range of 900 nm to 1200 nm is higher than when the heat treatment temperature is high. On the other hand, if the heat treatment temperature is kept low, when a heating test is performed at 100°C for 24 hours, the minute oriented crystals in the amorphous resin inhibit the movement of the molecules that make up the amorphous resin, making it difficult for microcrystals to be generated by heat, and suppressing the decrease in the average reflectance in the relevant range after the heating test.
[0057] Considering the above, there is a trade-off between the heat shielding performance of the film itself and the maintenance of near-infrared shielding properties under harsh conditions, and from the viewpoint of achieving a high level of both of these properties, the heat treatment temperature is more preferably 180°C or higher and 235°C or lower.
[0058] The film of the present invention contributes to suppressing the inflow and outflow of heat, and can maintain its excellent characteristics of visible light transmittance, near-infrared shielding properties, and appearance even under harsh usage conditions. In particular, since the film uniformly retains the above-mentioned excellent characteristics even in a size of 1 m x 1 m, it is suitable for use as a component of large, light-transmitting objects that require high visibility, such as window glass used in buildings such as homes and offices, or in mobile objects such as vehicles and ships. EXAMPLES
[0059] The present invention will be described below with reference to examples of the film. [Methods for measuring physical properties and evaluating effects] The methods for evaluating the characteristic values and the effects are as follows.
[0060] (1) Layer thickness, number of layers, layer structure, layer ratio The layer structure of the film was determined by observing a sample cut out from the center of the film width direction using a microtome with a transmission electron microscope (TEM). That is, a transmission electron microscope H-7100FA (manufactured by Hitachi, Ltd.) was used to observe the cross section of the film at 10,000 to 40,000 times magnification under conditions of an acceleration voltage of 75 kV, and a cross-sectional photograph was taken to measure the layer structure and thickness of each layer. In addition, the lamination ratio (total thickness of each A layer / total thickness of each B layer) was calculated from the total thickness of each A layer and the total thickness of each B layer. In some cases, in order to obtain high contrast, a known RuO 4 Or OsO 4 We used dyeing techniques such as the following.
[0061] (2) Film thickness In the width direction of the film, samples were cut out at 100 mm intervals from the center of the film width direction to both ends of the film width direction, with a size of 50 mm in the width direction x 50 mm in the length direction. The film thickness was measured at the center of the sample using a dial gauge thickness meter (JIS B7503 (1997), PEACOCK UPRIGHT DIAL GAUGE (0.001 x 2 mm), No. 25, 5 mm diameter flat gauge), and the average value was taken as the film thickness.
[0062] (3) Average in-plane refractive index The A layer was measured according to JIS K7142 (2014) A method for the films obtained in the examples and comparative examples described later. As for the B layer, since the resin constituting the B layer is an amorphous resin, an unstretched film was prepared from the resin constituting the B layer, and the refractive index of the B layer was determined. That is, the unstretched film was obtained by melting the resin composition at 280°C in a vented twin-screw extruder, and then shaping it into a sheet shape by introducing it into a T-die through a gear pump and a filter, and then rapidly solidifying it on a casting drum whose surface temperature was kept at 25°C by applying static electricity, thereby obtaining a film with a thickness of 100 μm. The refractive index of the obtained unstretched film was obtained by using an Abbe refractometer 4T (manufactured by Atago Co., Ltd.) to determine the refractive index in MD and TD according to JIS K7142 (2014) A method, and the average of these was determined as the in-plane refractive index. The light source used was a sodium D line wavelength of 589 nm. Note that methylene iodide was used as the immersion liquid, and the refractive index of the test piece was 1.74.
[0063] (4) Heat of fusion, glass transition temperature A sample mass of 5 g was collected, and measured and calculated according to JIS K7122 (1987) using a differential scanning calorimeter (DSC) robot DSC-RDC220 manufactured by Seiko Denshi Kogyo Co., Ltd. The temperature was raised from 25°C to 290°C at 5°C / min. The glass transition temperature here was determined by reading the specific heat change based on the transition from the glass state to the rubber state, and determining the midpoint between the line equidistant from the extended line of each baseline in the vertical axis (axis indicating heat flow) direction and the curve of the stepwise change part of the glass transition, and was taken as the glass transition temperature. The melting point here was taken as the point at which the difference from the DSC baseline was maximum. The heat of fusion was taken as the integrated value from the baseline in the range of the melting point ±20°C. Here, when measuring a single pellet, etc., a resin with a heat of fusion of 20 J / g or more was taken as a crystalline resin, and a resin with a heat of fusion of 5 J / g or less was taken as an amorphous resin.
[0064] (5) Measurement method for resin viscosity and die swell A mass of 5 g was taken from the sample that had been dried overnight, and the viscosity was measured and calculated according to ISO 11443 (2021) using a Capillograph 1D PMD-C manufactured by Toyo Seiki Seisakusho Co., Ltd. The capillary was L / D=20 / φ1, and the shear rate was 25, 50, 100, 300, and 1000 sec -1 The die swell was measured at a position 3 mm below the discharge port.
[0065] (6) Average transmittance in the wavelength range from 400 nm to 800 nm A film sample of 1m×1m was prepared, and one sample was cut out with a size of 50mm×50mm so that the center of the film was the intersection of the diagonal lines. In addition, four samples were cut out with a size of 50mm×50mm so as to include the apex of the film sample, for a total of five samples. Next, the transmittance at the center of the five samples was measured at an incidence angle Φ=0° using a spectrophotometer (Hitachi, Ltd., U-4100 Spectrophotometer, the inner wall of the attached integrating sphere was barium sulfate, and the standard plate was aluminum oxide). At this time, the measurement wavelength was 240 to 2600nm, the slit was 2nm (visible) / automatic control (infrared), the gain was 2, the scanning speed was 600nm / min, and the measurement interval was 1nm. From the obtained data, all the transmittance data from 400nm to 800nm for each sample was added up, and then divided by the number of data to calculate the average transmittance from 400nm to 800nm.
[0066] (7) Average transmittance in the wavelength range from 900 nm to 1200 nm The transmittance of the five samples cut out by the method described in (6) was measured by the method described in (6), and the data for 900 nm to 1200 nm for each sample was added together, and then the average transmittance for 900 nm to 1200 nm was calculated by dividing the total data by the number of data. S has the best average transmittance, and contributes to suppressing the flow of heat in and out. S: The average transmittance from 900 nm to 1200 nm was less than 13%. A: The average transmittance from 900 nm to 1,200 nm was 13% or more and less than 15%. B: The average transmittance from 900 nm to 1,200 nm was 15% or more and less than 20%. C: The average transmittance from 900 nm to 1,200 nm was 20% or more.
[0067] (8) Bandwidth difference at half-value wavelength end on the short wavelength side A film sample measuring 1m x 1m was exposed to light from a three-wavelength fluorescent lamp, which was then irradiated with a polarizing plate and then the film. The film was observed while wearing polarized sunglasses from the opposite side of the fluorescent lamp, and the presence or absence of color changes such as streaks was confirmed. The area where color changes occurred was designated as area S2, and the area adjacent to that area where color changes did not occur was designated as area S1. For films without streaky areas, the appearance was observed while wearing the modified sunglasses described above, and two points with large color tone differences were selected 50 mm apart, and designated as areas S1 and S2, respectively. Next, the transmittance at an incidence angle Φ = 0° was measured using a spectrophotometer (Hitachi, Ltd., U-4100 Spectrophotometer, the inner wall of the attached integrating sphere was barium sulfate, and the standard plate was aluminum oxide). At this time, the measurement wavelength was 240 to 2600 nm, the slit was 2 nm (visible) / automatic control (infrared), the gain was 2, the scanning speed was 600 nm / min, and the measurement interval was 1 nm. Next, the wavelength band located on the shortest wavelength side among the wavelength bands that show a transmittance of less than 80% continuously over 100 nm or more that exist in the wavelength range of 400 nm to 800 nm was defined as the wavelength band Π, and the wavelength of the shortest wavelength part in the wavelength band Π where the transmittance is less than 50% was defined as the half-value wavelength end λmin on the short wavelength side. Then, the λmin of region S1 was expressed as λmin(S1), and the λmin of region S2 was expressed as λmin(S2). The band difference of the half-value wavelength end on the short wavelength side was calculated as |λmin(S1)-λmin(S2)|. Note that S is the most excellent band difference of the half-value wavelength end |λmin(S1)-λmin(S2)|, and is an index of the appearance of the film. S: The band difference at the half-value wavelength end on the short wavelength side was less than 10 nm. A: The band difference at the half-value wavelength end on the short wavelength side was 10 nm or more and less than 20 nm. B: The band difference at the half-value wavelength end on the short wavelength side was 20 nm or more and less than 30 nm. C: The band difference at the half-value wavelength end on the short wavelength side was 30 nm or more.
[0068] (9) Hayes For the five samples cut out by the method described in (6), the haze was measured in accordance with the old JIS K7105 (1994) using a haze meter (HZ-V3) manufactured by Suga Test Instruments Co., Ltd., and the average value of the five data obtained was regarded as the haze of the film.
[0069] (10) Haze after 100℃ heating test for 24 hours Five samples cut out by the method described in (6) were heated in a gear oven (Espec Corp., GPHH-202) in an atmosphere of 100°C for 24 hours. The samples were then cooled to room temperature, and the haze was measured by the method described in (9). The average value of the five data obtained was taken as the haze after the 100°C heating test for 24 hours.
[0070] (11) Haze increase after 24-hour heating test at 100℃ The haze value obtained by the method described in (9) was subtracted from the haze value obtained by the method described in (10) to evaluate the increase in haze after a 24-hour heating test at 100°C according to the following criteria. The increase in haze after the heating test is an index of appearance under harsh usage conditions, with S being the most excellent. S: The difference in haze between the original sheet and the sheet after a 24-hour heating test at 100°C was less than 0.3%. A: The difference in haze between the original fabric and the sample after a 24-hour heating test at 100℃ was 0.3% or more and less than 0.5%. B: The difference between the haze after a 100℃ heating test for 24 hours and the haze of the original fabric was 0.5% or more and less than 1.0%. C: The difference between the haze after a 100℃ heating test for 24 hours and the haze of the original fabric was 1.0 or more.
[0071] (12) Measurement of intrinsic viscosity The solvent for each thermoplastic resin was orthochlorophenol, and the viscosity was calculated from the solution viscosity measured with an Ostwald viscometer in an environment at a temperature of 25°C.
[0072] (13) Measurement of the C* value of transmitted light The a* and b* values of the transmitted light at the center of the five samples cut out by the method described in (6) were measured using a spectrophotometer (CM-3600A, manufactured by Konica Minolta Japan, Inc.), and the chroma C* was calculated based on the following formula 2 (measurement mode: transmitted light, light source: C (angle: 10 degrees), measurement diameter: 25.4 mm). C*={(a*) 2 +(b*) 2} 1 / 2 formula 2 (14) Average transmittance from 900 to 1200 nm after 24-hour heating test at 100℃ Five samples cut out by the method described in (6) were heated by the method described in (10) and cooled to room temperature, after which the transmittance was measured by the method described in (6) and the average transmittance was calculated by the method described in (7).
[0073] (15) Change in average transmittance from 900 to 1200 nm after 24-hour heating test at 100℃ It was calculated by subtracting the average transmittance in the 900-1200 nm range measured by the method described in (7) from the average transmittance in the 900-1200 nm range after a 100℃ 24-hour heating test measured by the method described in (14). The change in average transmittance in the 900-1200 nm range after a 100℃ 24-hour heating test is an index of performance stability under harsh usage conditions, with S being the most excellent. S: After a 24-hour heating test at 100℃, the change in average transmittance from 900 to 1200 nm was less than 3%. A: After a 100℃ heating test for 24 hours, the change in average transmittance from 900 to 1200 nm was greater than 3% and less than 5%. B: The change in average transmittance from 900 to 1200 nm after a 100℃ heating test for 24 hours was greater than 5% and less than 8%. C: The change in average transmittance from 900 to 1200 nm after a 24-hour heating test at 100°C was 8% or more.
[0074] Example 1 The thermoplastic resin (thermoplastic resin A) constituting the A layer was crystalline polyethylene 2,6-naphthalate (intrinsic viscosity 0.62, glass transition temperature 96°C, melting point 249°C, refractive index (in-plane average refractive index) of the film after stretching and heat treatment was about 1.74) with 6 wt% of polyethylene glycol (average molecular weight 400) copolymerized with respect to the total diol constituents (hereinafter, this polyethylene 2,6-naphthalate is also referred to as PEN / PEG). The thermoplastic resin (thermoplastic resin B) constituting the B layer was polyethylene terephthalate (intrinsic viscosity 0.73, glass transition temperature 81°C, amorphous resin (no melting point), refractive index (in-plane average refractive index) of the film was about 1.58) with 50 wt% of cyclohexanedimethanol (CHDM) copolymerized with respect to the total diol constituents (hereinafter, this resin is also referred to as CHDM-copolymerized PET). The thermoplastic resins A and B thus prepared were melted at 290°C and 280°C, respectively, in separate vented twin-screw extruders, and fed to a 549-layer feed block through a gear pump and a filter to be laminated alternately. At this time, both surface layers were made of thermoplastic resin A, and the discharge rate of each extruder was adjusted so that the lamination ratio of thermoplastic resin A to thermoplastic resin B was 2:1. Next, the molten laminate obtained in the feed block was guided to a T-die with a lip width of 4 mm to be formed into a sheet, and then rapidly cooled and solidified on a casting drum whose surface temperature was kept at 25°C by electrostatic application to obtain a cast film. The obtained cast film was heated with a roll group set at 90°C, and then the cast film was stretched 3.2 times in the longitudinal direction while being rapidly heated from both sides by a radiation heater within a stretching section length of 100 mm, and then cooled once. At this time, the film temperature during stretching was 90°C. The obtained uniaxially stretched film was then introduced into a tenter, preheated with hot air at 110°C, and stretched 3.58 times in the transverse direction at a temperature of 125°C. The stretched film was then heat-treated with hot air at 225°C in the tenter, and then subjected to a 4.2% relaxation treatment in the transverse direction at the same temperature, and then gradually cooled to room temperature and wound up to a film width of 2400 mm. The thickness of the obtained film was 100 μm. The evaluation results of the obtained film are shown in Table 1.
[0075] (Examples 2 to 8, Comparative Examples 1 and 2) A film was obtained in the same manner as in Example 1, except that the melting temperature of thermoplastic resin A, the die lip width, the number of layers, and the heat treatment temperature were as shown in Table 1. The thickness of the obtained film was 100 μm. The evaluation results of the obtained film are shown in Table 1. The number of layers was adjusted by the number of layers (number of slits) of the feed block.
[0076] Example 9 The thermoplastic resin B in Example 1 was changed to a spiro glycol copolymer resin having an intrinsic viscosity of 0.72 (a spiro glycol copolymer resin obtained by copolymerizing 70% by mass of dimethyl terephthalate component based on the total dicarboxylic acid components, 30% by mass of cyclohexanedicarboxylic acid component based on the total dicarboxylic acid components, 40% by mass of ethylene glycol component based on the total diol components, and 60% by mass of spiro glycol component based on the total diol components, the refractive index (in-plane average refractive index) in the film is about 1.54, hereinafter also referred to as SPG copolymerized PET) and PET in a mass ratio of 85:15, and the melting temperature, number of layers, and heat treatment temperature of the thermoplastic resin A were as shown in Table 1. A film was obtained in the same manner as in Example 1. The thickness of the obtained film was 20 μm. The evaluation results of the obtained film are shown in Table 1.
[0077] Comparative Example 3 A film was obtained in the same manner as in Example 1, except that the thermoplastic resin A in Example 1 was changed to crystalline polyethylene 2,6-naphthalate (intrinsic viscosity 0.62, melting point 267°C, refractive index (in-plane average refractive index) of the film after stretching and heat treatment was approximately 1.74) to which polybutylene terephthalate (hereinafter also referred to as PBT) having a molecular weight of 2000 was added in an amount of 3 mass %, and the melting temperature of thermoplastic resin A was set as shown in Table 1. The thickness of the obtained film was 100 μm. The evaluation results of the obtained film are shown in Table 1.
[0078] Comparative Example 4 The thermoplastic resin A in Example 1 was changed to polyethylene terephthalate (intrinsic viscosity 0.65, glass transition temperature 77°C, melting point 255°C, refractive index (in-plane average refractive index) of the film after stretching and heat treatment is about 1.66) [Toray F20K] (hereinafter also referred to as PET), the thermoplastic resin B was changed to a spiro glycol copolymer resin with an intrinsic viscosity of 0.72 (spiroglycol copolymer resin in which dimethyl terephthalate component is 70 wt% relative to the total dicarboxylic acid component, cyclohexane dicarboxylic acid component is 30 wt% relative to the total dicarboxylic acid component, ethylene glycol component is 40 wt% relative to the total diol component, and spiro glycol component is 60 wt% relative to the total diol component, refractive index (in-plane average refractive index) of the film is about 1.54, hereinafter also referred to as SPG copolymerized PET) and PET in a mass ratio of 85:15, and the melting temperature of thermoplastic resin A was as shown in Table 1. A film was obtained in the same manner as in Example 1. The thickness of the obtained film was 100 μm. The evaluation results of the obtained film are shown in Table 1.
[0079] Comparative Example 5 A film was obtained in the same manner as in Example 1, except that the thermoplastic resin A in Example 1 was changed to PET and the melting temperature of the thermoplastic resin A was set as shown in Table 1. The thickness of the obtained film was 100 μm. The evaluation results of the obtained film are shown in Table 1.
[0080] [Table 1] [Industrial Applicability]
[0081] The film of the present invention can maintain excellent visible light transmittance, near infrared shielding properties, and appearance even under harsh conditions. More specifically, since it can be provided with a function of preventing heat inflow and outflow without impairing visibility even if it has a large area, it can be suitably used as a component of a light-transmitting body that requires high visibility, such as window glass used in buildings such as houses and offices, or moving bodies such as vehicles and ships.
Claims
1. A film having a size of 1 m x 1 m, characterized in that, over the entire surface of the film, the average transmittance in the wavelength band of 400 nm or more and 800 nm or less is 80% or more, the average transmittance in the wavelength band of 900 nm or more and 1200 nm or less is less than 20%, the change in the half-maximum wavelength end λmin on the short wavelength side is less than 30 nm, the haze is less than 3.0%, and the increase in haze in a heating test at 100°C for 24 hours is less than 1.0%.
2. 2. The film according to claim 1, wherein a layer having a relatively high refractive index is designated as an A layer and a layer having a relatively low refractive index is designated as a B layer, and the A layer and the B layer are alternately laminated in a total of 51 or more layers.
3. The film according to claim 2 , wherein the A layer is mainly composed of a polyester resin.
4. 4. The film according to claim 3, wherein the polyester resin which is the main component of the layer A is a copolymer containing naphthalenedicarboxylic acid units as dicarboxylic acid units.
5. 5. The film according to claim 4, wherein in the polyester resin which is the main component of the layer A, the main dicarboxylic acid unit is a naphthalenedicarboxylic acid unit.
6. 6. The film according to claim 2, wherein in the polyester resin which is the main component of said layer A, the polyalkylene glycol unit accounts for 1 wt % or more and 15 wt % or less of the total diol component.
7. The film according to any one of claims 2 to 5, wherein the layer B is mainly composed of a polyester resin.
8. The film according to claim 7 , wherein the polyester resin which is the main component of the layer B is a polyester resin containing cyclohexanedimethanol units.
9. The film according to any one of claims 1 to 8, wherein the change in average transmittance in the wavelength range of 900 nm or more and 1200 nm or less is less than 8% in a heating test at 100°C for 24 hours.
10. The film according to any one of claims 1 to 9, which is used as an element constituting a light-transmitting body used in a vehicle or building material.
Citation Information
Patent Citations
Laminate film
JP2017177810A
Polyester resin composition, and polyester film
JP2022091206A
Haet ray-shielding resin sheet material
JP2022100880A