Toner, developer, toner storage unit, image forming apparatus, and image forming method
The toner formulation with controlled particle size and defined coarse particle content addresses the issue of abnormal images and cleaning performance, ensuring high-quality image output by managing coarse particles and improving toner transfer efficiency.
Patent Information
- Application Number
- JP2024036803
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-16
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-01
AI Technical Summary
Existing toner production methods, particularly those using polymerization, struggle with the removal of coarse particles that cause abnormal images such as black spots, and the cleaning performance of small, spherical toner particles is compromised due to their ability to slip through the gaps between the cleaning blade and the image carrier.
A toner formulation with a volume average particle size of 4.0 μm or more and less than 6.0 μm, defined by the presence of 10 to 250 coarse particles that do not pass through a 20 μm sieve, utilizing a specific combination of binder resin, colorant, wax, and external additives to enhance cleaning performance and image quality.
The solution achieves both high cleaning performance and high image quality by effectively managing coarse particles, preventing slip-through and reducing abnormal images, while maintaining toner transfer efficiency.
Smart Images

Figure 2024132969000002 
Figure 2024132969000003 
Figure 2024132969000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner, a developer, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]
[0002] Toner is required to produce high quality output images. Conventionally, toners produced by a kneading and pulverizing method have been used, but the toners produced by the kneading and pulverizing method have problems such as difficulty in reducing the particle size, indefinite shape, and broad particle size distribution, resulting in insufficient quality of output images and high fixing energy.
[0003] In order to overcome the problems with the kneading and pulverizing method, a method for producing toner using a polymerization method has been proposed (see Patent Documents 1 to 4). Toner produced by the polymerization method can be easily made small in particle size, and the particle size distribution has a smaller volume average particle size than toner produced by the kneading and pulverizing method, making it possible to produce toner that is sharp and nearly spherical. These toners are of higher quality and less prone to abnormal images than toner produced by the kneading and pulverizing method, resulting in improved quality.
[0004] In recent years, there has been a demand for a method of manufacturing a toner with a smaller particle size that is less likely to cause abnormal images (see Patent Document 5). Among these, black spots are a problem as an abnormal image. The cause is coarse particles that are extremely different from the volume average particle size. The coarse particles are not transferred well, and the surrounding area becomes dark, causing black spots. Even in the polymerization manufacturing method, coarse particles that are different from the volume average particle size exist, and a process of removing them is required. If the conditions of the above process are made stricter, the quality improves, but the loss increases accordingly. Many documents specify that coarse particles are 25 μm or more, but in order to further improve image quality, it is necessary to focus on finer coarse particles. Also, from the viewpoint of image quality and resolution, a smaller volume average particle size Dv of the toner is advantageous, and it is preferable that it is 6.0 μm or less. Therefore, if the volume average particle size is large, abnormal images such as black spots are more likely to occur.
[0005] On the other hand, an image forming apparatus goes through a charging process for uniformly charging the image forming area on the surface of the electrostatic latent image carrier, an exposure process for writing to the electrostatic latent image carrier, a developing process for forming an image on the electrostatic latent image carrier with frictionally charged toner, and a transfer process for transferring the image on the electrostatic latent image carrier directly to printing paper or indirectly via an intermediate transfer body, and then fixes the image on the printing paper. In addition, residual toner that could not be transferred to the electrostatic latent image carrier and remains there is scraped off from the electrostatic latent image carrier in a cleaning process, and the apparatus enters the next image forming process.
[0006] As the cleaning member of the cleaning means, a cleaning blade in a rectangular shape is well known, which can simplify the device configuration and has excellent cleaning performance. Specifically, the base end of the cleaning blade is supported by a support member, and the contact portion (tip ridge portion) is pressed against the peripheral surface of the image carrier, blocking and scraping off the toner remaining on the image carrier.
[0007] In the toner manufacturing method using the polymerization method, the toner has a small particle size and a spherical shape, so it has become difficult to remove the toner with a cleaning blade compared to the toner manufactured by the conventional kneading and pulverizing method. This is because the toner, which has a small particle size and a high degree of sphericity, slips through the small gap formed between the cleaning blade and the image carrier. In order to prevent such toner from slipping through, there is a method of increasing the contact pressure between the image carrier and the cleaning blade, but increasing the contact pressure causes the blade to turn over. In addition, if the blade is used in a turned over state, local wear occurs, which ultimately shortens the life of the cleaning blade, causing cleaning failures and making it easier to produce abnormal images. Various other studies have been conducted on the cleaning performance. However, at present, no universal solution has been clearly stated. As a solution, if coarse particles with a large particle size are present, slipping through is less likely to occur, but abnormal images are more likely to occur. In addition, the smaller the volume average particle size, the more the slipping through particles increase, making cleaning failures more likely to occur. Summary of the Invention [Problem to be solved by the invention]
[0008] Patent Document 1 describes that an image in which the occurrence of white streaks is suppressed can be formed by reducing the content of coarse particles with a relatively high degree of circularity, but does not fully disclose the definition of coarse particles that can ensure abnormal images (black spots) and cleanability.
[0009] An object of the present invention is to provide a toner that can achieve both high cleaning performance and high image quality at a high level. [Means for solving the problem]
[0010] The above problems can be solved by the present invention having the following configuration. A toner containing at least a binder resin, a colorant, a wax and an external additive, the toner particles having a volume average particle size of 4.0 μm or more and less than 6.0 μm, and the number of coarse particles, as defined below, in 10 mg of the toner is 10 or more and 250 or less. Definition of coarse particles: Toner particles that do not pass through a sieve with 20 μm openings when passed through the wet method Effect of the Invention
[0011] According to the present invention, it is possible to provide a toner that can achieve both high cleaning performance and high image quality at a high level. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram illustrating another example of an image forming apparatus according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating another example of an image forming apparatus according to the present invention. [Diagram 3] FIG. 3 is a partially enlarged view of FIG. [Figure 4] FIG. 2 is a schematic diagram illustrating an example of a process cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The toner, developer, toner storage unit, image forming apparatus, and image forming method according to the present invention will be described below with reference to the drawings as appropriate. Note that the present invention is not limited to the following embodiments, and may be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, and deletions, and any aspect is within the scope of the present invention as long as it achieves the functions and effects of the present invention.
[0014] The toner of the present invention comprises toner base particles including a binder resin, a colorant, a wax, etc., and an external additive.
[0015] (coarse particles) The toner of the present invention has a number of coarse particles per 10 mg of toner of 10 to 250. Here, the term "coarse particles" refers to toner particles that do not pass through a sieve having an opening of 20 μm when the toner is passed through the sieve by a dry method. The number of coarse particles is preferably 15 or more and 150 or less, and more preferably 15 or more and 60 or less.
[0016] In the toner of the present invention, the number of coarse particles having a size of 25 μm or more per 2 g of toner is preferably 48 or less, and more preferably 25 or less.
[0017] (Toner base particles) The toner base particles contain at least a binder resin and a colorant, and may further contain other components as required. The toner base particles are preferably obtained by dissolving or dispersing at least a binder resin and a colorant in an organic solvent, adding the obtained solution or dispersion to an aqueous phase, and removing the organic solvent from the obtained dispersion.More preferably, the toner base particles are obtained by dissolving or dispersing at least a binder resin precursor and a colorant in an organic solvent, adding the obtained solution or dispersion to an aqueous phase to crosslink or elongate the binder resin precursor, and removing the organic solvent.
[0018] The toner base particles usually contain a polyester resin as a binder resin, preferably a non-linear amorphous polyester, and more preferably a crystalline polyester. The THF-insoluble component usually preferably contains a non-linear amorphous polyester or a crystalline polyester.
[0019] The amorphous polyester resin is obtained by using a polyhydric alcohol component and a polycarboxylic acid component such as a polycarboxylic acid, a polycarboxylic acid anhydride, or a polycarboxylic acid ester. In the present invention, the amorphous polyester resin refers to a resin obtained by using a polyhydric alcohol component and a polycarboxylic acid component such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic acid ester, as described above. Modified polyester resins, such as the prepolymers described below, and resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, do not belong to the amorphous polyester resins.
[0020] Examples of the polyhydric alcohol component include alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of bisphenol A such as polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol, propylene glycol, neopentyl glycol, glycerin, pentaerythritol, trimethylolpropane, hydrogenated bisphenol A, sorbitol, or alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts thereof. These may be used alone or in combination of two or more.
[0021] Examples of the polyvalent carboxylic acid component include dicarboxylic acids such as adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, and maleic acid; succinic acids substituted with an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms such as dodecenylsuccinic acid and octylsuccinic acid; trimellitic acid, pyromellitic acid; anhydrides of these acids, and alkyl (carbon number 1 to 8) esters of these acids. These may be used alone or in combination of two or more.
[0022] It is preferable that the amorphous polyester resin, the prepolymer described below, and the resin obtained by crosslinking and / or elongation reaction of this prepolymer are at least partially compatible with each other. By being compatible with each other, low-temperature fixability and high-temperature offset resistance can be improved. For this reason, it is preferable that the polyhydric alcohol component and polyvalent carboxylic acid component constituting the amorphous polyester resin and the polyhydric alcohol component and polyvalent carboxylic acid component constituting the prepolymer described below have similar compositions.
[0023] The molecular weight of the amorphous polyester resin is not particularly limited and can be appropriately selected depending on the purpose. However, if the molecular weight is too low, the toner may be inferior in heat-resistant storage stability and durability against stress such as stirring in a developing device, whereas if the molecular weight is too high, the toner may have high viscoelasticity when melted and may have inferior low-temperature fixing properties. Therefore, it is preferable that the weight average molecular weight (Mw) is 2,500 to 10,000, the number average molecular weight (Mn) is 1,000 to 4,000, and the Mw / Mn is 1.0 to 4.0, as measured by GPC.
[0024] The glass transition temperature (Tg) of the amorphous polyester resin is not particularly limited and can be appropriately selected depending on the purpose. However, if the Tg is too low, the toner may have poor heat-resistant storage stability and poor durability against stress such as stirring in a developing device, whereas if the Tg is too high, the toner may have high viscoelasticity when melted and poor low-temperature fixability. Therefore, the glass transition temperature is preferably 40°C to 70°C, and more preferably 45°C to 60°C.
[0025] The content of the amorphous polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 50 parts by mass to 95 parts by mass, more preferably 60 parts by mass to 90 parts by mass, relative to 100 parts by mass of the toner. If the content is less than 50 parts by mass, the dispersibility of the pigment and release agent in the toner may deteriorate, and image fogging and disturbance may easily occur, and if it exceeds 95 parts by mass, the content of the crystalline polyester may be reduced, resulting in poor low-temperature fixability. If the content is within the above more preferred range, it is advantageous in that high image quality, high stability, and low-temperature fixability are all excellent.
[0026] The molecular structure of the amorphous polyester resin can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 and 990±10cm -1 One method is to detect amorphous polyester resins that do not have absorption due to olefin δCH (out-of-plane bending vibration).
[0027] The substance (aqueous medium) used in the aqueous dispersion is not particularly limited as long as it dissolves in water, and can be appropriately selected depending on the purpose, and examples thereof include a surfactant (D), a buffering agent, a protective colloid, etc. These may be used alone or in combination of two or more.
[0028] <Crystalline polyester resin> The crystalline polyester resin has structural units derived from a saturated aliphatic diol. As the saturated aliphatic diol, it is preferable to use an alcohol component containing a straight-chain aliphatic diol having 2 to 8 carbon atoms. This enables the crystalline polyester resin to be uniformly and finely dispersed within the toner, prevents filming of the crystalline polyester resin, improves stress resistance, and achieves low-temperature fixability of the toner.
[0029] The crystalline polyester resin has high crystallinity and exhibits a thermal melting characteristic in which the viscosity drops sharply near the fixing start temperature. By using the crystalline polyester resin having such characteristics in the toner, the toner has good heat-resistant storage stability due to the crystallinity until just before the melting start temperature, and at the melting start temperature, the toner has a good heat-resistant storage stability and low-temperature fixing property because the toner has a sharp viscosity drop (sharp melt property) and is fixed. In addition, the toner also shows good results in terms of the release width (the difference between the minimum fixing temperature and the hot offset occurrence temperature).
[0030] The crystalline polyester resin is obtained by using a polyhydric alcohol component and a polycarboxylic acid component such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester. In the present invention, the crystalline polyester resin refers to a resin obtained by using a polyhydric alcohol component and a polycarboxylic acid component such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic acid ester, as described above. Modified crystalline polyester resins, such as the prepolymers described below, and resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resins.
[0031] -Polyhydric alcohol component- The polyhydric alcohol component is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyhydric alcohol component include diols and trihydric or higher alcohols. Examples of the diol include saturated aliphatic diols. Examples of the saturated aliphatic diols include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 8 carbon atoms are more preferred. If the saturated aliphatic diol is branched, the crystallinity of the crystalline polyester resin may decrease, and the melting point may decrease. If the carbon number of the main chain is less than 2, the melting temperature may increase when polycondensing with an aromatic dicarboxylic acid, making low-temperature fixing difficult. On the other hand, if the carbon number exceeds 8, it is difficult to obtain a practical material. It is more preferred that the carbon number is 8 or less.
[0032] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanedecanediol, etc. Among these, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol are preferred in terms of the high crystallinity of the crystalline polyester resin and excellent sharp melt properties. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. These may be used alone or in combination of two or more.
[0033] -Polycarboxylic acid component- As the polyvalent carboxylic acid component, sebacic acid is used, but other divalent carboxylic acids and trivalent or higher carboxylic acids can be used in combination depending on the purpose. Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and further, anhydrides and lower alkyl esters of these.
[0034] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, as well as anhydrides and lower alkyl esters of these. The polycarboxylic acid component may contain a dicarboxylic acid component having a sulfonic acid group in addition to the saturated aliphatic dicarboxylic acid and aromatic dicarboxylic acid, and may contain a dicarboxylic acid component having a double bond in addition to the saturated aliphatic dicarboxylic acid and aromatic dicarboxylic acid. These may be used alone or in combination of two or more.
[0035] The melting point of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 60° C. or more and less than 80° C. If the melting point is less than 60° C., the crystalline polyester resin is likely to melt at low temperatures, and the heat-resistant storage stability of the toner may decrease, whereas if the melting point is 80° C. or more, the polyester resin A may not melt sufficiently due to heating during fixing, and the low-temperature fixability may decrease. The melting point can be measured from the endothermic peak value on a differential scanning calorimeter (DSC) chart in DSC measurement.
[0036] The molecular weight of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. However, from the viewpoint that a resin having a sharp molecular weight distribution and a low molecular weight has excellent low-temperature fixability, and a large amount of low-molecular-weight components deteriorates heat-resistant storage stability, it is preferable that the ortho-dichlorobenzene-soluble portion of the crystalline polyester resin has a weight average molecular weight (Mw) of 3,000 to 30,000, a number average molecular weight (Mn) of 1,000 to 10,000, and an Mw / Mn ratio of 1.0 to 10, as measured by GPC.
[0037] The acid value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of affinity between paper and resin, in order to achieve the desired low-temperature fixability, it is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, while in order to improve high-temperature offset resistance, it is preferably 45 mgKOH / g or less.
[0038] The hydroxyl value of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose. In order to achieve the desired temperature fixing property and good charging characteristics, the hydroxyl value is preferably 0 mgKOH / g to 50 mgKOH / g, and more preferably 5 mgKOH / g to 50 mgKOH / g.
[0039] The molecular structure of the crystalline polyester resin can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 One method is to detect a crystalline polyester resin that has absorption based on the δCH (out-of-plane bending vibration) of olefin.
[0040] The content of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 to 20 parts by mass, more preferably 5 to 15 parts by mass, relative to 100 parts by mass of the toner. If the content is less than 2 parts by mass, the sharp melting by the crystalline polyester resin is insufficient, so that the low-temperature fixing property may be poor, and if it exceeds 20 parts by mass, the heat-resistant storage stability may be deteriorated and the image may be easily fogged. If the content is within the above more preferred range, it is advantageous in that high image quality, high stability, and low-temperature fixing property are all excellent.
[0041] <Inorganic filler> The toner base particles in the toner of the present invention are produced by adding an inorganic filler to the above-mentioned toner base particles. The inorganic filler is not particularly limited, but one or more types selected from calcium carbonate, kaolin clay, talc, barium sulfate, etc. can be added alone or in combination. These inorganic fillers may be surface-treated with a silane coupling agent, a surfactant, a metal soap, or the like, and may be adjusted to a desired particle size distribution by classification or the like.
[0042] In addition to the above, the inorganic filler contained in the toner of the present invention is preferably a layered inorganic mineral, and more preferably a layered inorganic mineral modified with an organic ion. Layered inorganic minerals are inorganic minerals that are made up of layers several nanometers thick stacked on top of each other, and modifying them with organic ions means introducing organic ions into the ions that exist between the layers.
[0043] Known layered inorganic minerals include the smectite group (montmorillonite, saponite, etc.), the kaolin group (kaolinite, etc.), magadiite, and kanemite. The modified layered inorganic minerals are highly hydrophilic due to their modified layered structure. Therefore, if the layered inorganic mineral is used in a toner that is dispersed in an aqueous medium and granulated without being modified, the layered inorganic mineral migrates into the aqueous medium, and the toner cannot be deformed, but the modification increases hydrophilicity, and the modified layered inorganic mineral is finely divided and deformed during the production of the toner, and is present in particularly large amounts on the surface of the toner particles, and can be uniformly dispersed and arranged throughout the toner base particles, fulfilling a charge adjustment function and contributing to low-temperature fixation. In this case, the content of the modified layered inorganic mineral in the toner material is preferably 0.2 to 1.5% by mass.
[0044] The modified layered inorganic mineral used in the present invention is preferably one that has a basic smectite crystal structure and is modified with an organic cation. In addition, metal anions can be introduced by replacing a part of the divalent metal of the layered inorganic mineral with a trivalent metal. However, since the introduction of metal anions results in high hydrophilicity, it is preferable to use a layered inorganic compound in which at least a part of the metal anion is modified with an organic anion.
[0045] Examples of organic ion modifiers for the layered inorganic mineral in which at least a portion of the ions of the layered inorganic mineral are modified with organic ions include quaternary alkyl ammonium salts, phosphonium salts, and imidazolium salts, with quaternary alkyl ammonium salts being preferred. Examples of the quaternary alkyl ammonium include trimethylstearyl ammonium, dimethylstearylbenzyl ammonium, dimethyloctadecyl ammonium, and oleylbis(2-hydroxyethyl)methyl ammonium.
[0046] The organic ion modifier further includes sulfates, sulfonates, carboxylates, or phosphates having branched, unbranched, or cyclic alkyl (C1-C44), alkenyl (C1-C22), alkoxy (C8-C32), hydroxyalkyl (C2-C22), ethylene oxide, propylene oxide, etc. Carboxylic acids having an ethylene oxide skeleton are preferred.
[0047] By modifying at least a portion of the layered inorganic mineral with an organic ion, the layered inorganic mineral has a suitable hydrophobicity, the oil phase containing the toner composition and / or the toner composition precursor has a non-Newtonian viscosity, and the toner can be deformed. In this case, the content of the layered inorganic mineral partially modified with an organic ion in the toner material is preferably 0.2% by mass to 1.5% by mass.
[0048] The layered inorganic mineral partially modified with organic ions can be appropriately selected, and examples thereof include montmorillonite, bentonite, hectorite, attapulgite, sepiolite, and mixtures thereof. Among these, montmorillonite or bentonite containing Al element is preferred because Al element is effective in improving charging ability.
[0049] Commercially available layered inorganic minerals partially modified with organic cations include quaternium-18 bentonites such as Bentone 3, Bentone 38, Bentone 38V (all manufactured by Rheox Corporation), Thixogel VP (manufactured by United Catalyst Corporation), Kraton 34, Kraton 40, Kraton XL (all manufactured by Southern Clay Corporation); stearalkonium bentonites such as Bentone 27 (manufactured by Rheox Corporation), Thixogel LG (manufactured by United Catalyst Corporation), Kraton AF, Kraton APA (all manufactured by Southern Clay Corporation); and quaternium-18 / benzalkonium bentonites such as Kraton HT, Kraton PS (all manufactured by Southern Clay Corporation).
[0050] Particularly preferred are Clayton AF and Clayton APA. As the layered inorganic mineral partially modified with an organic anion, DHT-4A (manufactured by Kyowa Chemical Industry Co., Ltd.) modified with an organic anion represented by the following general formula (3) is particularly preferred. An example of the compound represented by the following general formula (3) is Hitenol 330T (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.). R 1 (OR 2 ) n OSO3M...General formula (3) [In the above formula, R1 is an alkyl group having 13 carbon atoms, R 2 represents an alkylene group having 2 to 6 carbon atoms, n represents an integer of 2 to 10, and M represents a monovalent metal element.
[0051] <Other ingredients> The other components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other components include a separator, a colorant, a polymer having a site capable of reacting with an active hydrogen group-containing compound, an active hydrogen group-containing compound, a charge control agent, an external additive, a flowability improver, a cleaning property improver, and a magnetic material.
[0052] <Release agent> The release agent is not particularly limited and can be appropriately selected from known agents. Examples of waxes and wax release agents include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusine; and petroleum waxes such as paraffin, microcrystalline, and petrolatum.
[0053] In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; synthetic waxes such as esters, ketones, and ethers; and the like can also be used. Further, fatty acid amide compounds such as 12-hydroxystearic acid amide, stearic acid amide, phthalimide anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups in their side chains may be used. Among these, hydrocarbon waxes such as paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyethylene wax, and polypropylene wax are preferred.
[0054] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 60° C. or higher and lower than 95° C.
[0055] The release agent is more preferably a hydrocarbon wax having a melting point of 60° C. or more and less than 95° C. Such a release agent can effectively act as a release agent between the fixing roller and the toner interface, and therefore can improve high-temperature offset resistance without applying a release agent such as oil to the fixing roller. In particular, hydrocarbon waxes are preferred because they have almost no compatibility with the polyester resin A and can function independently of each other, and therefore do not impair the softening effect of the crystalline polyester resin as a binder resin or the offset property of the release agent. If the melting point of the release agent is less than 60° C., the release agent is likely to melt at low temperatures, and the heat-resistant storage stability of the toner may be poor.If the melting point of the release agent is more than 95° C., the release agent may not melt sufficiently due to heating during fixing, and sufficient offset properties may not be obtained.
[0056] The content of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 to 10 parts by mass, more preferably 3 to 8 parts by mass, relative to 100 parts by mass of the toner. If the content is less than 2 parts by mass, the high-temperature offset resistance and low-temperature fixability during fixing may be poor, and if it exceeds 10 parts by mass, the heat-resistant storage stability may be deteriorated and image fogging may be easily caused. If the content is within the above more preferred range, it is advantageous in terms of improving image quality and fixing stability.
[0057] <Coloring agent> The colorant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, and anthrazan yellow BG. L, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Riant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue - Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone. The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass to 15 parts by mass, and more preferably 3 parts by mass to 10 parts by mass, relative to 100 parts by mass of the toner.
[0058] The colorant can also be used as a masterbatch composited with a resin. Examples of resins to be used in the preparation of a masterbatch or to be kneaded with a masterbatch include, in addition to the hybrid resin, styrene or its substituted polymers such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, and styrene-α-chloromethyl methacrylate copolymer. styrene-based copolymers such as styrene-acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resins, epoxy polyol resins, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic or alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffin, and paraffin wax. These may be used alone or in combination of two or more.
[0059] The master batch can be obtained by mixing and kneading the resin and colorant for the master batch under high shear force. In this case, an organic solvent can be used to enhance the interaction between the colorant and the resin. In addition, a method called the flushing method, in which an aqueous paste containing water of the colorant is mixed and kneaded with the resin and organic solvent to transfer the colorant to the resin side and remove the water and organic solvent components, is also preferably used because it does not require drying since the wet cake of the colorant can be used as it is. A high shear dispersing device such as a three-roll mill is preferably used for mixing and kneading.
[0060] -Polymer (prepolymer) having a site capable of reacting with an active hydrogen group-containing compound- The polymer having a site capable of reacting with the active hydrogen group-containing compound (sometimes referred to as a "prepolymer") is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polyol resins, polyacrylic resins, polyester resins, epoxy resins, and derivatives thereof. These may be used alone or in combination of two or more. Among these, polyester resins are preferred in terms of high fluidity and transparency when melted.
[0061] Examples of the site of the prepolymer that can react with the active hydrogen group-containing compound include an isocyanate group, an epoxy group, a carboxyl group, a functional group represented by -COCl, etc. These may be used alone or in combination of two or more. Of these, an isocyanate group is preferred.
[0062] The prepolymer is not particularly limited and can be appropriately selected depending on the purpose, but a polyester resin having an isocyanate group or the like capable of generating a urea bond is preferred, in that it is easy to adjust the molecular weight of the polymer component, and it has oil-less low-temperature fixing properties in a dry toner, and in particular, it can ensure good releasability and fixability even when there is no mechanism for applying release oil to the heating medium for fixing.
[0063] -Active hydrogen group-containing compounds- The active hydrogen group-containing compound acts as an elongation agent, a crosslinking agent, or the like when a polymer having a site capable of reacting with the active hydrogen group-containing compound undergoes an elongation reaction, a crosslinking reaction, or the like in an aqueous medium.
[0064] The active hydrogen group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, a mercapto group, etc. These may be used alone or in combination of two or more kinds.
[0065] The active hydrogen group-containing compound is not particularly limited and can be appropriately selected according to the purpose, but when the polymer having a site capable of reacting with the active hydrogen group-containing compound is a polyester resin containing an isocyanate group, amines are preferred because they can be made high molecular weight by elongation reaction, crosslinking reaction, etc. with the polyester resin. The amines are not particularly limited and can be appropriately selected according to the purpose, and examples thereof include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, and those in which the amino groups are blocked. These may be used alone or in combination of two or more. Among these, diamines and mixtures of diamines with small amounts of trivalent or higher amines are preferred.
[0066] The diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aromatic diamines, alicyclic diamines, and aliphatic diamines. The aromatic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane. The alicyclic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, and isophoronediamine. The aliphatic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ethylenediamine, tetramethylenediamine, and hexamethylenediamine.
[0067] The trivalent or higher amine is not particularly limited and can be appropriately selected depending on the purpose. Examples of the trivalent or higher amine include diethylenetriamine and triethylenetetramine.
[0068] The amino alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino alcohol include ethanolamine and hydroxyethylaniline. The amino mercaptan is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino mercaptan include aminoethyl mercaptan and aminopropyl mercaptan.
[0069] The amino acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino acid include aminopropionic acid and aminocaproic acid. The blocked amino group is not particularly limited and can be appropriately selected depending on the purpose. Examples of the blocked amino group include ketimine compounds obtained by blocking the amino group with ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, and oxazoline compounds.
[0070] -Polyester resin containing isocyanate groups- The polyester resin containing an isocyanate group (hereinafter, sometimes referred to as a "polyester prepolymer having an isocyanate group") is not particularly limited and can be appropriately selected depending on the purpose. For example, a reaction product of a polyester resin having an active hydrogen group obtained by polycondensation of a polyol and a polycarboxylic acid and a polyisocyanate can be mentioned.
[0071] -Polyol- The polyol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diols, trihydric or higher alcohols, mixtures of diols and trihydric or higher alcohols, etc. These may be used alone or in combination of two or more kinds. Among these, diols and mixtures of diols with small amounts of trihydric or higher alcohols are preferred.
[0072] The diol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alkylene glycols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol; diols having an oxyalkylene group such as diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; and alkylene oxide adducts of bisphenols such as those to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added to bisphenols. The number of carbon atoms of the alkylene glycol is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 to 12. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols and mixtures of alkylene oxide adducts of bisphenols and alkylene glycols having 2 to 12 carbon atoms are more preferred.
[0073] The trihydric or higher alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the trihydric or higher alcohol include aliphatic trihydric or higher alcohols, trihydric or higher polyphenols, and alkylene oxide adducts of trihydric or higher polyphenols. The trihydric or higher aliphatic alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol. The trivalent or higher polyphenols are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include trisphenol PA, phenol novolac, and cresol novolac. Examples of the alkylene oxide adducts of trivalent or higher polyphenols include those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trivalent or higher polyphenols. When the diol and the trihydric or higher alcohol are used in combination, the mass ratio of the trihydric or higher alcohol to the diol is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01 mass % to 10 mass %, more preferably 0.01 mass % to 1 mass %.
[0074] -Polycarboxylic acid- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include dicarboxylic acids, trivalent or higher carboxylic acids, mixtures of dicarboxylic acids and trivalent or higher carboxylic acids, etc. These may be used alone or in combination of two or more. Among these, dicarboxylic acids and mixtures of dicarboxylic acids with a small amount of trivalent or higher polycarboxylic acids are preferred.
[0075] The dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dicarboxylic acid include divalent alkanoic acids, divalent alkenoic acids, and aromatic dicarboxylic acids. The divalent alkanoic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the divalent alkanoic acid include succinic acid, adipic acid, and sebacic acid. The divalent alkenoic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a divalent alkenoic acid having 4 to 20 carbon atoms. The divalent alkenoic acid having 4 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include maleic acid and fumaric acid. The aromatic dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms. The aromatic dicarboxylic acid having 8 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.
[0076] The tri- or higher carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the tri- or higher carboxylic acid include aromatic tri- or higher carboxylic acids. The trivalent or higher aromatic carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms. The trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include trimellitic acid and pyromellitic acid.
[0077] As the polycarboxylic acid, anhydrides or lower alkyl esters of any of dicarboxylic acids, tri- or higher carboxylic acids, and mixtures of dicarboxylic acids and tri- or higher carboxylic acids can also be used. The lower alkyl ester is not particularly limited and can be appropriately selected depending on the purpose. Examples of the lower alkyl ester include methyl ester, ethyl ester, and isopropyl ester. When the dicarboxylic acid and the tri- or higher carboxylic acid are used in combination, the mass ratio of the tri- or higher carboxylic acid to the dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 10% by mass, and more preferably 0.01% by mass to 1% by mass.
[0078] When the polyol and the polycarboxylic acid are polycondensed, the equivalent ratio of the hydroxyl groups of the polyol to the carboxyl groups of the polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 2, more preferably 1 to 1.5, and particularly preferably 1.02 to 1.3.
[0079] The content of the polyol-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the high-temperature offset resistance decreases, and it may be difficult to achieve both the heat-resistant storage stability and low-temperature fixability of the toner. If the content exceeds 40% by mass, the low-temperature fixability may decrease.
[0080] -Polyisocyanate- The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate include aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates, and those blocked with phenol derivatives, oximes, caprolactam, etc.
[0081] The aliphatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aliphatic diisocyanate include tetramethylene diisocyanate, hexamethylene diisocyanate, methyl 2,6-diisocyanatocaproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, and tetramethylhexane diisocyanate.
[0082] The alicyclic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the alicyclic diisocyanate include isophorone diisocyanate and cyclohexylmethane diisocyanate.
[0083] The aromatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aromatic diisocyanate include tolylene diisocyanate, diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatodiphenyl, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 4,4'-diisocyanato-3-methyldiphenylmethane, and 4,4'-diisocyanato-diphenyl ether.
[0084] The aromatic aliphatic diisocyanate is not particularly limited and may be appropriately selected depending on the purpose. Examples of the aromatic aliphatic diisocyanate include α,α,α',α'-tetramethylxylylene diisocyanate. The isocyanurates are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include tris(isocyanatoalkyl)isocyanurate, tris(isocyanatocycloalkyl)isocyanurate, etc. These may be used alone or in combination of two or more kinds.
[0085] When the polyisocyanate is reacted with a polyester resin having a hydroxyl group, the equivalent ratio of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 5, more preferably 1.2 to 4, and particularly preferably 1.5 to 3. If the equivalent ratio is less than 1, the offset resistance may decrease, and if it exceeds 5, the low-temperature fixability may decrease.
[0086] The content of the polyisocyanate-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, high-temperature offset resistance may decrease, and if it exceeds 40% by mass, low-temperature fixability may decrease.
[0087] The average number of isocyanate groups in the polyester prepolymer having an isocyanate group per molecule is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 1 or more, more preferably 1.2 to 5, and particularly preferably 1.5 to 4. If the average number is less than 1, the molecular weight of the urea-modified polyester resin becomes low, and high-temperature offset resistance may decrease.
[0088] The mass ratio of the polyester prepolymer having an isocyanate group to the polyester resin containing 50 mol % or more of a propylene oxide adduct of bisphenols in the polyhydric alcohol component and having a specific hydroxyl value and acid value is not particularly limited and can be appropriately selected depending on the purpose, but is preferably less than 5 / 95 to more than 25 / 75, and more preferably 10 / 90 to 25 / 75. If the mass ratio is less than 5 / 95, high-temperature offset resistance may decrease, and if it exceeds 25 / 75, low-temperature fixability and image gloss may decrease.
[0089] -Charge control agent- The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives. Specific examples include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (both manufactured by Hodogaya Chemical Co., Ltd.), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit Co., Ltd.), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.
[0090] The content of the charge control agent is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, relative to 100 parts by mass of the toner. If the content exceeds 10 parts by mass, the chargeability of the toner is too high, the effect of the main charge control agent is reduced, and the electrostatic attraction force with the developing roller increases, which may lead to a decrease in the fluidity of the developer and a decrease in image density. These charge control agents can be melt-kneaded together with the master batch and resin and then dissolved and dispersed, or of course they can be added when directly dissolved and dispersed in an organic solvent, or they can be fixed on the toner surface after the toner particles are produced.
[0091] The acid value of the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 mgKOH / g to 40 mgKOH / g in terms of controlling low-temperature fixability (lower limit temperature of fixation) and hot offset occurrence temperature. If the acid value is less than 0.5 mgKOH / g, the effect of improving dispersion stability by a base during production cannot be obtained, or when the prepolymer is used, the elongation reaction and / or crosslinking reaction may easily proceed, resulting in a decrease in production stability. If the acid value is more than 40 mgKOH / g, when the prepolymer is used, the elongation reaction and / or crosslinking reaction may be insufficient, resulting in a decrease in high-temperature offset resistance.
[0092] The glass transition temperature (Tg) of the toner is not particularly limited and can be appropriately selected depending on the purpose, but the glass transition temperature (Tg1st) calculated at the first temperature rise in DSC measurement is preferably 45° C. or more and less than 65° C., and more preferably 50° C. or more and 60° C. or less. This allows low-temperature fixability, heat-resistant storage stability, and high durability to be obtained. If the Tg1st is less than 45° C., blocking in the developing machine or filming on the photoreceptor may occur, and if it is 65° C. or more, the low-temperature fixability may decrease. The glass transition temperature (Tg2nd) calculated at the second temperature rise in the DSC measurement of the toner is preferably 20° C. or more and less than 40° C. If the Tg2nd is less than 20° C., blocking in a developing machine or filming on a photoreceptor may occur, and if it exceeds 40° C., low-temperature fixability may decrease.
[0093] (Volume average particle size of toner) The toner of the present invention has a volume average particle diameter of 4.0 μm or more and less than 6.0 μm, and preferably 5.0 μm or more and 5.5 μm or less.
[0094] <<Method of measuring particle size distribution>> The volume average particle diameter (D4) and number average particle diameter (Dn) of the toner, and the ratio thereof (D4 / Dn) can be measured using, for example, a Coulter Counter TA-II or a Coulter Multisizer II (both manufactured by Coulter, Inc.). In the present invention, a Coulter Multisizer II was used. The measurement method is described below. First, 0.1 mL to 5 mL of a surfactant (preferably polyoxyethylene alkyl ether (nonionic surfactant)) is added as a dispersant to 100 mL to 150 mL of the electrolyte solution. Here, the electrolyte solution is a 1 mass % NaCl aqueous solution prepared using first-class sodium chloride, and for example, ISOTON-II (manufactured by Coulter) can be used. Then, 2 mg to 20 mg of a measurement sample is further added. The electrolyte solution in which the sample is suspended is subjected to a dispersion process for about 1 minute to 3 minutes using an ultrasonic disperser, and the volume and number of toner particles or toner are measured using a 100 μm aperture as an aperture with the above-mentioned measuring device, and the volume distribution and number distribution are calculated. From the obtained distribution, the volume average particle size (D4) and number average particle size (Dn) of the toner can be obtained. Thirteen channels are used: 2.00 μm or more but less than 2.52 μm; 2.52 μm or more but less than 3.17 μm; 3.17 μm or more but less than 4.00 μm; 4.00 μm or more but less than 5.04 μm; 5.04 μm or more but less than 6.35 μm; 6.35 μm or more but less than 8.00 μm; 8.00 μm or more but less than 10.08 μm; 10.08 μm or more but less than 12.70 μm; 12.70 μm or more but less than 16.00 μm; 16.00 μm or more but less than 20.20 μm; 20.20 μm or more but less than 25.40 μm; 25.40 μm or more but less than 32.00 μm; and 32.00 μm or more but less than 40.30 μm, and the target particles are 2.00 μm or more but less than 40.30 μm in diameter.
[0095] (External additives) -Inorganic fine particles- The inorganic fine particles used as the external additive can be used in combination with hydrophobized inorganic fine particles, the volume average particle diameter of which is preferably 1 nm to 200 nm, more preferably 10 nm to 150 nm. It is also preferable that the hydrophobized primary particles contain at least one type of inorganic fine particles having a volume average particle diameter of 30 nm or less, and at least one type of inorganic fine particles having a volume average particle diameter of 50 nm or more. When the volume average particle diameter of the inorganic fine particles is 50 nm or more, they are easily blocked by the blade, improving filming and cleaning. The specific surface area according to the BET method is 20 m 2 / g~500m 2 It is preferred that the molecular weight is / g.
[0096] The inorganic fine particles are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include silica fine particles, hydrophobic silica, metal oxides (such as titania, alumina, tin oxide, and antimony oxide), and fluoropolymers.
[0097] The content of the inorganic fine particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 parts by mass to 6.0 parts by mass, and more preferably 1.0 parts by mass to 4.0 parts by mass, relative to 100 parts by mass of the toner base particles.
[0098] -Fatty acid metal salts- The most common industrial methods for producing fatty acid metal salts used as external additives are a wet method in which fatty acids are saponified with caustic soda or caustic potash to form an alkali soap, which is then reacted with a metal salt to obtain the metal soap, and a dry method in which fatty acids are reacted with a metal oxide or hydroxide to obtain the metal soap. Known methods for microparticulating fatty acid metal salts include dry pulverization using compressed air of the dried metal soap obtained by a wet method or a dry method, or dispersing the metal soap in silicone oil or the like and wet pulverizing the resulting mixture in a bead mill.
[0099] The fatty acid metal salt is not particularly limited, and examples thereof include zinc stearate and aluminum stearate.
[0100] The content of the fatty acid metal salt is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.05 parts by mass to 0.20 parts by mass, and more preferably 0.08 parts by mass to 0.16 parts by mass, relative to 100 parts by mass of the toner base particles.
[0101] -Other external additives- Other additives include titania, titanium oxide, and alumina fine particles. Examples of titania fine particles include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, STT-65C-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-140 (manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-150W, MT-500B, MT-600B, and MT-150A (all manufactured by Teika Co., Ltd.).
[0102] Examples of hydrophobically treated titanium oxide microparticles include T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-500T, TAF-1500T (all manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-100S, MT-100T (all manufactured by Teika Corporation), and IT-S (manufactured by Ishihara Sangyo Co., Ltd.).
[0103] Hydrophobized oxide particles, hydrophobized silica particles, hydrophobized titania particles, and hydrophobized alumina particles can be obtained by treating hydrophilic particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, octyltrimethoxysilane, etc. Silicone oil-treated oxide particles and inorganic particles, which are treated with silicone oil by heating if necessary, are also suitable.
[0104] Examples of the silicone oil include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methylhydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, acrylic, methacrylic-modified silicone oil, and α-methylstyrene-modified silicone oil. Examples of inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengalla, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride. Among these, silica and titanium dioxide are particularly preferred.
[0105] The content of the external additive is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1% by mass to 5% by mass, and more preferably 0.3% by mass to 3% by mass, based on the toner. The volume average particle diameter of the primary particles of the inorganic fine particles is not particularly limited and can be appropriately selected according to the purpose, but is preferably 200 nm or less, more preferably 10 nm to 100 nm. If it is smaller than this range, the inorganic fine particles are buried in the toner, and it is difficult to effectively exert their function. On the other hand, if it is larger than this range, it is not preferable because it will damage the photoreceptor surface unevenly.
[0106] <<Other ingredients>> The other components are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other components include magnetic materials, cleaning improvers, flow improvers, and charge control agents.
[0107] -Flow improver- The flowability improver is not particularly limited as long as it is capable of performing a surface treatment to increase hydrophobicity and prevent deterioration of flowability and charging properties even under high humidity, and can be appropriately selected according to the purpose, and examples thereof include silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, modified silicone oils, etc. It is particularly preferable that the silica and titanium oxide are surface-treated with such a flowability improver and used as hydrophobic silica and hydrophobic titanium oxide.
[0108] -Cleaning improver- The cleaning property improver is not particularly limited as long as it is added to the toner to remove the developer remaining on the photoconductor or primary transfer medium after transfer, and can be appropriately selected depending on the purpose, and examples thereof include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymer fine particles produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particles and polystyrene fine particles, etc. The polymer fine particles preferably have a relatively narrow particle size distribution, and are preferably ones having a volume average particle size of 0.01 μm to 1 μm.
[0109] -Magnetic materials- The magnetic material is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include iron powder, magnetite, ferrite, etc. Among these, those that are white in color are preferred.
[0110] <Toner manufacturing method> The method for producing the toner is not particularly limited and can be appropriately selected depending on the purpose. However, it is preferable that the toner is granulated by dispersing an oil phase containing at least the amorphous polyester resin, the crystalline polyester resin, the release agent, and the colorant in an aqueous medium. An example of the method for producing such a toner is a known dissolution suspension method. As another example of the toner manufacturing method, a method of forming toner base particles while producing a product (hereinafter, sometimes referred to as "adhesive substrate") by elongation reaction and / or crosslinking reaction between the active hydrogen group-containing compound and a polymer having a site capable of reacting with the active hydrogen group-containing compound is described below. In such a method, preparation of an aqueous medium, preparation of an oil phase containing toner materials, emulsification or dispersion of the toner materials, removal of organic solvent, etc. are performed.
[0111] - Preparation of aqueous medium (aqueous phase) - The aqueous medium can be prepared, for example, by dispersing resin particles in the aqueous medium. The amount of the resin particles added to the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 10% by mass. The resin particles are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, and polymer-based protective colloids. These may be used alone or in combination of two or more types. Among these, surfactants are preferred.
[0112] The aqueous medium is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include water, a solvent miscible with water, a mixture thereof, etc. These may be used alone or in combination of two or more. Of these, water is preferred. The water-miscible solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, lower ketones, etc. The alcohol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include methanol, isopropanol, ethylene glycol, etc. The lower ketone is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include acetone, methyl ethyl ketone, etc.
[0113] - Preparation of oil phase - The oil phase containing the toner materials can be prepared by dissolving or dispersing the toner materials, including the active hydrogen group-containing compound, the polymer having a site capable of reacting with the active hydrogen group-containing compound, the crystalline polyester resin, the amorphous polyester resin, the release agent, the hybrid resin, and the colorant, in an organic solvent.
[0114] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, but an organic solvent having a boiling point of less than 150° C. is preferred in terms of ease of removal. The organic solvent having a boiling point of less than 150° C. is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, etc. These may be used alone or in combination of two or more. Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, carbon tetrachloride, etc. are preferable, and ethyl acetate is more preferable.
[0115] -Emulsification or dispersion- The toner materials can be emulsified or dispersed by dispersing an oil phase containing the toner materials in the aqueous medium. When the toner materials are emulsified or dispersed, an active hydrogen group-containing compound and a polymer having a site capable of reacting with the active hydrogen group-containing compound undergo an elongation reaction and / or a crosslinking reaction to produce an adhesive substrate.
[0116] The adhesive substrate may be produced, for example, by emulsifying or dispersing an oil phase containing a polymer having reactivity with active hydrogen groups, such as a polyester prepolymer having an isocyanate group, together with a compound containing active hydrogen groups, such as amines, in an aqueous medium, and then carrying out an elongation reaction and / or crosslinking reaction between the two in the aqueous medium, or by emulsifying or dispersing an oil phase containing toner materials in an aqueous medium to which a compound having an active hydrogen group has been added in advance, and carrying out an elongation reaction and / or crosslinking reaction between the two in the aqueous medium, or by emulsifying or dispersing an oil phase containing toner materials in an aqueous medium, adding a compound having an active hydrogen group, and carrying out an elongation reaction and / or crosslinking reaction between the two from the particle interface in the aqueous medium. When carrying out an elongation reaction and / or crosslinking reaction between the two from the particle interface, the urea-modified polyester resin is preferentially formed on the surface of the toner produced, and a concentration gradient of the urea-modified polyester resin can also be provided in the toner.
[0117] The reaction conditions (reaction time, reaction temperature) for producing the adhesive base material are not particularly limited, and can be appropriately selected depending on the combination of the active hydrogen group-containing compound and the polymer having a site capable of reacting with the active hydrogen group-containing compound. The reaction time is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 minutes to 40 hours, and more preferably 2 hours to 24 hours. The reaction temperature is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0°C to 150°C, and more preferably 40°C to 98°C.
[0118] The method for stably forming a dispersion liquid containing a polymer having a site capable of reacting with an active hydrogen group-containing compound, such as a polyester prepolymer having an isocyanate group, in the aqueous medium is not particularly limited and may be appropriately selected depending on the purpose. For example, there is a method in which an oil phase prepared by dissolving or dispersing a toner material in a solvent is added to an aqueous medium phase, and the mixture is dispersed by shear force.
[0119] The dispersing machine for the dispersion is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dispersing machine include a low-speed shear dispersing machine, a high-speed shear dispersing machine, a friction dispersing machine, a high-pressure jet dispersing machine, and an ultrasonic dispersing machine. Among these, a high-speed shear type disperser is preferred because it is possible to control the particle size of the dispersion (oil droplets) to 2 μm to 20 μm. When the high-speed shear type dispersing machine is used, the conditions such as the rotation speed, dispersing time, and dispersing temperature can be appropriately selected depending on the purpose. The rotation speed is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1,000 rpm to 30,000 rpm, and more preferably 5,000 rpm to 20,000 rpm. The dispersion time is not particularly limited and can be appropriately selected depending on the purpose, but in the case of a batch method, it is preferably 0.1 to 5 minutes. The dispersion temperature is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0° C. to 150° C. under pressure, and more preferably 40° C. to 98° C. In general, the higher the dispersion temperature, the easier the dispersion.
[0120] The amount of the aqueous medium used when emulsifying or dispersing the toner materials is not particularly limited and can be appropriately selected depending on the purpose. However, the amount is preferably 50 parts by mass to 2,000 parts by mass, and more preferably 100 parts by mass to 1,000 parts by mass, relative to 100 parts by mass of the toner materials. If the amount of the aqueous medium used is less than 50 parts by mass, the dispersion state of the toner materials may become poor, and toner base particles having the specified particle size may not be obtained. If the amount of the aqueous medium used is more than 2,000 parts by mass, the production cost may become high.
[0121] When the oil phase containing the toner materials is emulsified or dispersed, it is preferable to use a dispersant from the viewpoints of stabilizing the dispersion such as oil droplets, forming a desired shape, and sharpening the particle size distribution. The dispersant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, polymer-based protective colloids, etc. These may be used alone or in combination of two or more. Among these, surfactants are preferred.
[0122] The surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. can be used. The anionic surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the anionic surfactant include alkylbenzene sulfonate, α-olefin sulfonate, and phosphoric acid ester. Among these, those having a fluoroalkyl group are preferred.
[0123] A catalyst may be used in the elongation reaction and / or crosslinking reaction in producing the adhesive substrate. The catalyst is not particularly limited and can be appropriately selected depending on the purpose. Examples of the catalyst include dibutyltin laurate and dioctyltin laurate.
[0124] -Removal of organic solvents- The method for removing the organic solvent from the dispersion liquid such as the emulsified slurry is not particularly limited and can be appropriately selected depending on the purpose. For example, the method includes a method of gradually increasing the temperature of the entire reaction system to evaporate the organic solvent in the oil droplets, a method of spraying the dispersion liquid in a dry atmosphere to remove the organic solvent in the oil droplets, and the like.
[0125] When the organic solvent is removed, toner base particles are formed, which may then be washed, dried, and so on.
[0126] The obtained toner base particles may be mixed with particles of the external additive, the charge control agent, etc. At this time, by applying a mechanical impact force, it is possible to suppress the particles of the external additive, etc. from being detached from the surface of the toner base particles. The method of applying the mechanical impact force is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method of applying an impact force to the mixture using a blade rotating at high speed, and a method of introducing the mixture into a high-speed air stream and accelerating it to cause particles to collide with each other or against an appropriate collision plate. The apparatus used in the above method is not particularly limited and can be appropriately selected depending on the purpose. Examples of the apparatus include Angmill (manufactured by Hosokawa Micron Corporation), an apparatus obtained by modifying an I-type mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.) to reduce the grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works, Ltd.), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), an automatic mortar, and the like.
[0127] -Classification process- In the production of the toner of the present invention, classification with a sieve is preferred. Classification by sieve makes it possible to control coarse particles larger than the mesh size. The toner base particles after the drying process have no fluidity, and the sieve has poor processing capacity, which causes clogging easily.
[0128] Therefore, it is desirable to sieve the slurry after the formation of the toner base particles or the toner after the addition of external additives with a sieve having an opening of 20 μm. The material of the sieve can be changed according to the sieve, but nylon, SUS, and polyester are generally available and therefore preferable.
[0129] <Developer> The developer of the present invention contains at least the toner, and optionally contains other components such as a carrier that are appropriately selected. By using the developer of the present invention, it is possible to stably form high-quality images with excellent transferability, charging property, etc. The developer may be a one-component developer or a two-component developer, but when used in a high-speed printer corresponding to the recent improvement in information processing speed, a two-component developer is preferable because of its improved life. When the developer is used as a one-component developer, even if the toner is balanced, there is little variation in the particle size of the toner, there is little filming of the toner on the developing roller, and there is little melting of the toner to components such as blades that thin the toner layer, and good and stable developability and images can be obtained even with long-term stirring in the developing device. When the developer is used as a two-component developer, the particle size of the toner changes little even when the toner is balanced over a long period of time, and good and stable developability and images can be obtained even when the toner is stirred for a long period of time in a developing device. When the toner is used in a two-component developer, it may be mixed with the carrier. The content of the carrier in the two-component developer is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 90% by mass to 98% by mass, more preferably 93% by mass to 97% by mass.
[0130] <Career> The carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably one having a core material and a resin layer covering the core material.
[0131] -Core material- The material of the core material is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include manganese-strontium-based materials and manganese-magnesium-based materials of 50 emu / g to 90 emu / g. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more and magnetite of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 emu / g to 80 emu / g, since it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for improving image quality. These may be used alone or in combination of two or more.
[0132] The volume average particle size of the core material is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 μm to 150 μm, and more preferably 40 μm to 100 μm. If the volume average particle diameter is less than 10 μm, the amount of fine powder in the carrier increases, the magnetization per particle decreases, and the carrier may scatter. If the volume average particle diameter exceeds 150 μm, the specific surface area decreases, and the toner may scatter. In particular, in full color toners that have many solid areas, the reproduction of the solid areas may become poor.
[0133] -Resin layer- The material for the resin layer is not particularly limited and can be appropriately selected from known resins depending on the purpose. Examples of the material include amino-based resins, polyvinyl-based resins, polystyrene-based resins, polyhalogenated olefins, polyester-based resins, polycarbonate-based resins, polyethylene, polyvinyl fluoride, polyvinylidene fluoride, polytrifluoroethylene, polyhexafluoropropylene, fluoro terpolymers such as copolymers of vinylidene fluoride and an acrylic monomer, copolymers of vinylidene fluoride and vinyl fluoride, copolymers of tetrafluoroethylene, vinylidene fluoride and a monomer not having a fluoro group, and silicone resins. These may be used alone or in combination of two or more.
[0134] The amino resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino resin include urea-formaldehyde resin, melamine resin, benzoguanamine resin, urea resin, polyamide resin, and epoxy resin. The polyvinyl resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyvinyl resin include acrylic resin, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyvinyl alcohol, and polyvinyl butyral. The polystyrene-based resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polystyrene-based resin include polystyrene and styrene-acrylic copolymers. The polyhalogenated olefin is not particularly limited and can be appropriately selected depending on the purpose. For example, polyvinyl chloride is included. The polyester resin is not particularly limited and may be appropriately selected depending on the purpose. Examples of the polyester resin include polyethylene terephthalate and polybutylene terephthalate.
[0135] The resin layer may contain conductive powder, etc., if necessary. The conductive powder is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include metal powder, carbon black, titanium oxide, tin oxide, zinc oxide, etc. The average particle diameter of the conductive powder is preferably 1 μm or less. If the average particle diameter exceeds 1 μm, it may be difficult to control the electrical resistance.
[0136] The resin layer can be formed by preparing a coating solution by dissolving a silicone resin or the like in a solvent, coating the coating solution on the surface of the core material using a known coating method, drying, and then baking. The coating method is not particularly limited and may be appropriately selected depending on the purpose. For example, a dip coating method, a spray method, a brush coating method, etc. may be used. The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, and butyl cellosolve acetate. The baking may be performed by an external heating method or an internal heating method, and examples of the method include a method using a fixed electric furnace, a flow type electric furnace, a rotary type electric furnace, a burner furnace, etc., and a method using microwaves.
[0137] The content of the resin layer in the carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 5.0% by mass. If the content is less than 0.01% by mass, a uniform resin layer may not be formed on the surface of the core material, and if it exceeds 5.0% by mass, the resin layer is too thick and fusion between carrier particles may occur, resulting in a decrease in uniformity of the carrier.
[0138] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge. The toner storage container refers to a container that stores toner. The developing device has a means for containing toner and developing the toner.
[0139] <Process cartridge> The process cartridge according to the present invention is formed so as to be detachably mountable to various image forming apparatuses, and has at least a photoconductor for carrying an electrostatic latent image, and a developing means for developing the electrostatic latent image carried on the photoconductor with the developer of the present invention to form a toner image. The process cartridge of the present invention may further have other means as necessary. The developing means includes at least a developer container for containing the developer of the present invention, and a developer carrier for carrying and transporting the developer contained in the developer container. The developing means may further include a regulating member for regulating the thickness of the developer carried.
[0140] By mounting the toner storage unit on an image forming apparatus and forming an image, it is possible to take advantage of the characteristics of the toner, which has excellent offset resistance, charge stability, stress resistance, and background scumming properties, and can provide high-definition, high-quality images over a long period of time, thereby forming high-quality, high-definition images with long-term image stability.
[0141] (Image forming apparatus and image forming method) The image forming apparatus of the present invention comprises at least an electrostatic latent image carrier, an electrostatic latent image forming means, and a developing means, and further comprises other means as necessary. The image forming method according to the present invention includes at least an electrostatic latent image forming step and a development step, and further includes other steps as necessary. The image forming method can be suitably performed by the image forming apparatus, the electrostatic latent image forming process can be suitably performed by the electrostatic latent image forming means, the developing process can be suitably performed by the developing means, and the other processes can be suitably performed by the other means.
[0142] More preferably, the image forming apparatus of the present invention includes an electrostatic latent image carrier, an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier, a developing means provided with toner for developing the electrostatic latent image formed on the electrostatic latent image carrier with toner to form a toner image, a transfer means for transferring the toner image formed on the electrostatic latent image carrier to a surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. Furthermore, the image forming method of the present invention more preferably includes an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with toner to form a toner image, a transfer step of transferring the toner image formed on the electrostatic latent image carrier to a surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0143] The toner is used in the developing means. Preferably, the toner image is formed by using a developer containing the toner and, if necessary, other components such as a carrier.
[0144] <Electrostatic latent image carrier> The material, structure, and size of the above-described electrostatic latent image carrier (hereinafter also referred to as "photoconductor") are not particularly limited and can be appropriately selected from known ones. Examples of the material include inorganic photoconductors such as amorphous silicon and selenium, and organic photoconductors such as polysilane and phthalopolymethine.
[0145] <Electrostatic latent image forming means> The electrostatic latent image forming means is not particularly limited as long as it is a means for forming an electrostatic latent image on the electrostatic latent image carrier, and can be appropriately selected according to the purpose. For example, it includes means having at least a charging member for charging the surface of the electrostatic latent image carrier and an exposure member for imagewise exposing the surface of the electrostatic latent image carrier.
[0146] <Developing means> The developing means is not particularly limited as long as it is a developing means provided with toner for developing the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, and can be appropriately selected according to the purpose.
[0147] <Cleaning means> In the image forming apparatus of the present invention, it is preferable to have a cleaning means. As described above, the toner of the present invention is excellent in cleanability. Therefore, by applying the toner to the image forming apparatus having a cleaning means, the cleanability is improved in the following points. · By improving the spacer effect of the toner, the fluidity of the toner is maintained even under stress, and the cleanability is improved. · By satisfying 0.3 < B < 2.0 for the free amount B (mass%) of the external additive (silica), the external additive sufficiently dissociates from the toner on the photoconductor, and a high cleanability can be achieved by forming a deposition layer (dam layer) of the external additive at the cleaning blade nip portion.
[0148] The cleaning means is not particularly limited as long as it is capable of removing the toner remaining on the photoreceptor, and can be appropriately selected depending on the purpose. Examples of the cleaning means include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, and a web cleaner.
[0149] <Other methods> Examples of the other means include a transfer means, a fixing means, a discharging means, a recycling means, and a control means.
[0150] Next, one embodiment of the method for forming an image by the image forming apparatus of the present invention will be described with reference to FIG.
[0151] An example of an image forming apparatus of the present invention is shown in Fig. 1. The color image forming apparatus 100A shown in Fig. 1 includes a photoconductor drum 10 (hereinafter sometimes referred to as "photoconductor 10") as the electrostatic latent image carrier, a charging roller 20 as the charging means, an exposure device 30 as the exposure means, a developing device 40 as the developing means, an intermediate transfer body 50, a cleaning device 60 as the cleaning means having a cleaning blade, and a static elimination lamp 70 as the static elimination means.
[0152] The intermediate transfer body 50 is an endless belt, and is designed to be movable in the direction of the arrow by three rollers 51 arranged inside and stretching it. Some of the three rollers 51 also function as transfer bias rollers capable of applying a predetermined transfer bias (primary transfer bias) to the intermediate transfer body 50. A cleaning device 90 having a cleaning blade is arranged near the intermediate transfer body 50. Also, a transfer roller 80 as the transfer means capable of applying a transfer bias for transferring (secondary transfer) a developed image (toner image) to a transfer paper P as a recording medium is arranged near the intermediate transfer body 50 so as to face the intermediate transfer body 50. Around the intermediate transfer body 50, a corona charger 52 for applying a charge to the toner image on the intermediate transfer body 50 is arranged between the contact portion between the photoconductor 10 and the intermediate transfer body 50 and the contact portion between the intermediate transfer body 50 and the transfer paper P in the rotation direction of the intermediate transfer body 50.
[0153] Around the photosensitive drum 10, a black developing unit 45K, a yellow developing unit 45Y, a magenta developing unit 45M, and a cyan developing unit 45C are disposed directly facing each other. The black developing unit 45K includes a developer container 42K, a developer supply roller 43K, and a developing roller 44K. The yellow developing unit 45Y includes a developer container 42Y, a developer supply roller 43Y, and a developing roller 44Y. The magenta developing unit 45M includes a developer container 42M, a developer supply roller 43M, and a developing roller 44M. The cyan developing unit 45C includes a developer container 42C, a developer supply roller 43C, and a developing roller 44C. The developing belt 41 is an endless belt that is rotatably stretched around a plurality of belt rollers, and a part of the belt 41 contacts the electrostatic latent image carrier 10.
[0154] In a color image forming apparatus 100A shown in FIG. 1, for example, a charging roller 20 uniformly charges a photoconductor drum 10. An exposure device 30 exposes the photoconductor drum 10 imagewise to light to form an electrostatic latent image. The electrostatic latent image formed on the photoconductor drum 10 is developed by supplying toner from a developing device 40 to form a toner image. The toner image is transferred (primary transfer) onto an intermediate transfer body 50 by a voltage applied from a roller 51, and is further transferred (secondary transfer) onto a transfer paper P. As a result, a transfer image is formed on the transfer paper P. Note that residual toner on the photoconductor 10 is removed by a cleaning device 60, and the charge on the photoconductor 10 is temporarily removed by a discharging lamp 70.
[0155] Another example of the image forming apparatus of the present invention is shown in Fig. 2. The image forming apparatus 100B shown in Fig. 2 includes a copying machine main body 150, a paper feed table 200, a scanner 300, and an automatic document feeder (ADF) 400. An endless belt-like intermediate transfer body 50 is provided in the center of the copying machine main body 150. The intermediate transfer body 50 is stretched around support rollers 14, 15, and 16, and can rotate clockwise in FIG. 2. An intermediate transfer body cleaning device 17 for removing residual toner on the intermediate transfer body 50 is provided near the support roller 15. A tandem type developing device 120 is provided on the intermediate transfer body 50 stretched around the support rollers 14 and 15 along the conveying direction of the intermediate transfer body 50, in which four image forming means 120 for yellow, cyan, magenta, and black are arranged in a row facing each other. An exposure device 21, which is the exposure member, is provided near the tandem type developing device 120. A secondary transfer device 22 is provided on the side of the intermediate transfer body 50 opposite the side on which the tandem type developing device 120 is provided. In the secondary transfer device 22, a secondary transfer belt 24, which is an endless belt, is stretched around a pair of rollers 23, and the transfer paper transported on the secondary transfer belt 24 and the intermediate transfer body 50 can come into contact with each other. A fixing device 25, which is the fixing means, is disposed near the secondary transfer device 22. The fixing device 25 includes a fixing belt 26, which is an endless belt, and a pressure roller 27 disposed so as to be pressed against the fixing belt 26. In the tandem image forming apparatus, a sheet inverting device 28 is disposed near the secondary transfer device 22 and the fixing device 25 for inverting the transfer paper so that images can be formed on both sides of the transfer paper.
[0156] Next, a description will be given of the formation of a full-color image (color copy) using the tandem type developing device 120. That is, first, an original is set on the original table 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and an original is set on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed.
[0157] When a start switch (not shown) is pressed, the scanner 300 is driven after the original is transported and moved onto the contact glass 32 when an original is set on the automatic original transport device 400, or immediately when an original is set on the contact glass 32. Then, the first traveling body 33 and the second traveling body 34 travel. At this time, light from a light source is irradiated by the first traveling body 33, and the reflected light from the original surface is reflected by a mirror in the second traveling body 34, and is received by the reading sensor 36 through the imaging lens 35 to read the color original (color image), which is converted into image information of black, yellow, magenta, and cyan.
[0158] Then, the image information for black, yellow, magenta, and cyan is transmitted to the image forming means 120 (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the tandem developing device 120. Then, in each image forming means, a toner image for black, yellow, magenta, and cyan is formed. That is, as shown in FIG. 3, each image forming means 120 (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the tandem developing device 120 includes an electrostatic latent image carrier 10 (electrostatic latent image carrier for black 10K, electrostatic latent image carrier for yellow 10Y, electrostatic latent image carrier for magenta 10M, and electrostatic latent image carrier for cyan 10C), a charging device 20 which is the charging means for uniformly charging the electrostatic latent image carrier 10, and a charging device 20 which charges the electrostatic latent image carrier 10 based on each color image information. The image forming apparatus includes an exposure device that exposes the electrostatic latent image carrier to light (L in FIG. 3) in the form of an image corresponding to each color image to form an electrostatic latent image corresponding to each color image on the electrostatic latent image carrier, a developing device 61 that is the developing means that develops the electrostatic latent image with each color toner (black toner, yellow toner, magenta toner, and cyan toner) to form a toner image with each color toner, a transfer charger 62 for transferring the toner image onto the intermediate transfer body 50, a cleaning device 63, and a charge remover 64. Each image forming means 120 is capable of forming a single color image (black image, yellow image, magenta image, and cyan image) based on image information of the respective color. The black image formed on the black electrostatic latent image carrier 10K, the yellow image formed on the yellow electrostatic latent image carrier 10Y, the magenta image formed on the magenta electrostatic latent image carrier 10M, and the cyan image formed on the cyan electrostatic latent image carrier 10C are sequentially transferred (primary transfer) onto the intermediate transfer body 50 which is rotated by the support rollers 14, 15, and 16. Then, the black image, the yellow image, the magenta image, and the cyan image formed on the cyan electrostatic latent image carrier 10C are superimposed on the intermediate transfer body 50 to form a composite color image (color transfer image).
[0159] On the other hand, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed a sheet (recording paper) from one of the paper feed cassettes 144 provided in multiple stages in the paper bank 143. The sheets are separated one by one by the separation roller 145 and sent to the paper feed path 146, then conveyed by the conveyance roller 147 and guided to the paper feed path 148 in the copying machine main body 150, where they are stopped by striking against the registration roller 49. Alternatively, the paper feed roller 142 is rotated to feed the sheets (recording paper) on the manual feed tray 54, and the sheets are separated one by one by the separation roller 52 and placed in the manual feed path 53, where they are also stopped by striking against the registration roller 49. The registration roller 49 is generally used while being grounded, but may be used with a bias applied to remove paper dust from the sheets. Then, the registration roller 49 is rotated in synchronization with the composite color image (color transfer image) composited on the intermediate transfer body 50, a sheet (recording paper) is sent between the intermediate transfer body 50 and the secondary transfer device 22, and the composite color image (color transfer image) is transferred (secondary transfer) onto the sheet (recording paper) by the secondary transfer device 22. In this way, a color image is transferred and formed on the sheet (recording paper). Note that residual toner on the intermediate transfer body 50 after the image transfer is cleaned by the intermediate transfer body cleaning device 17.
[0160] The sheet (recording paper) on which the color image has been transferred and formed is transported by the secondary transfer device 22 and sent to the fixing device 25, where the composite color image (color transfer image) is fixed onto the sheet (recording paper) by heat and pressure. Thereafter, the sheet (recording paper) is switched by a switching claw 55, discharged by discharge rollers 56, and stacked on a paper output tray 57. Alternatively, the sheet is switched by a switching claw 55, inverted by a sheet inverting device 28, and guided to the transfer position again, an image is also recorded on the back side, and then the sheet is discharged by discharge rollers 56 and stacked on a paper output tray 57.
[0161] An example of a process cartridge according to the present invention is shown in Fig. 4. The process cartridge 110 has the photosensitive drum 10, a corona charger 52, a developing device 40, a transfer roller 80 and a cleaning device 90. EXAMPLES
[0162] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0163] Example 1 <Synthesis of prepolymer A (amorphous polyester resin A)> Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.5, the diol component was 100 mol% 3-methyl-1,5-pentanediol, the dicarboxylic acid component was 40 mol% isophthalic acid and 60 mol% adipic acid, and the amount of trimellitic anhydride in all monomers was 1 mol%. Thereafter, the temperature was raised to 200°C over about 4 hours, and then to 230°C over 2 hours, and the reaction was continued until no water was discharged. Thereafter, the mixture was further reacted for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester A-1]. Next, [Intermediate polyester A-1] and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate group of IPDI / hydroxyl group of intermediate polyester) of 2.0, and after diluting with ethyl acetate to make a 50% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain [Prepolymer A-1]. In addition, [Prepolymer A] is used to generate [Polyester Resin A], which corresponds to the polyester resin component, during the process of producing the toner in the examples and comparative examples described below.
[0164] <Synthesis of prepolymer B (amorphous polyester resin B)> In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, ethylene oxide 2 moles of bisphenol A, propylene oxide 2 moles of bisphenol A, terephthalic acid and adipic acid were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the molar ratio of hydroxyl group to carboxyl group, OH / COOH, was 1.1, the composition of the diol component was 80 mol% of ethylene oxide 2 moles of bisphenol A, 20 mol% of propylene oxide 2 moles of bisphenol A, and the composition of the dicarboxylic acid component was 60 mol% of terephthalic acid and 40 mol% of adipic acid. After that, the temperature was raised to 200°C in about 4 hours, and then raised to 230°C in 2 hours, and the reaction was carried out until no water was discharged. After that, the reaction was further carried out for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester B]. Next, the obtained [intermediate polyester B] and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate group of IPDI / hydroxyl group of intermediate polyester) of 2.0, and after diluting with ethyl acetate to make a 50% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain [prepolymer B]. In addition, from [Prepolymer B], [Polyester Resin B] corresponding to the polyester resin component is generated during the process of producing the toner in the examples and comparative examples described below.
[0165] <Synthesis of amorphous polyester resin C> In a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, bisphenol A ethylene oxide side 2 mole adduct, bisphenol A propylene oxide 3 mole adduct, terephthalic acid, adipic acid, and trimethylolpropane were added, and the molar ratio of bisphenol A ethylene oxide side 2 mole adduct and bisphenol A propylene oxide 3 mole adduct was 85 / 15 (bisphenol A ethylene oxide side 2 mole adduct / bisphenol A propylene oxide 3 mole adduct), and the molar ratio of terephthalic acid and adipic acid was 85 / 15 (bisphenol A ethylene oxide side 2 mole adduct / bisphenol A propylene oxide 3 mole adduct). The monomers were charged so that the molar ratio (terephthalic acid / adipic acid) was 75 / 25, the amount of trimethylolpropane in the total monomers was 1 mol%, and the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.2, and reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at normal pressure and 230°C for 8 hours, and then reacted for a further 4 hours at a reduced pressure of 10 mmHg to 15 mmHg. After that, trimellitic anhydride was added to the reaction vessel so that the amount was 1 mol% relative to the total resin components, and reacted at 180°C and normal pressure for 3 hours to obtain [Amorphous Polyester Resin C].
[0166] <Synthesis of crystalline polyester resin D> Dodecanedioic acid and 1,6-hexanediol were charged into a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 0.9, and reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at 180°C for 10 hours, then the temperature was raised to 200°C and reacted for 3 hours, and further reacted at a pressure of 8.3 kPa for 2 hours to obtain [Crystalline Polyester Resin D].
[0167] <Preparation of Crystalline Polyester Resin Dispersion> A container equipped with a stirrer and a thermometer was charged with 50 parts of [Crystalline Polyester Resin D] and 450 parts of ethyl acetate. The temperature was raised to 80 °C with stirring and held at 80 °C for 5 hours. Then, it was cooled to 30 °C over 1 hour, and dispersion was carried out using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.) under the conditions of a liquid feeding rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume filling of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain [Crystalline Polyester Resin Dispersion 1].
[0168] <Preparation of Masterbatch (MB)> 1,200 parts of water, 500 parts of carbon black (Printex 35 dexer manufactured) [DBP oil absorption = 42 mL / 100 mg, pH = 9.5], and 500 parts of [Amorphous Polyester Resin C-1] were added and mixed using a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). The mixture was kneaded at 150 °C for 30 minutes using two rolls, then rolled and cooled and pulverized with a pelletizer to obtain [Masterbatch 1].
[0169] <Preparation of WAX Dispersion> A container equipped with a stirrer and a thermometer was charged with 50 parts of paraffin wax (manufactured by Nippon Seiro Co., Ltd., HNP-9, hydrocarbon wax, melting point 75 °C, SP value 8.8) as a release agent and 450 parts of ethyl acetate. The temperature was raised to 80 °C with stirring and held at 80 °C for 5 hours. Then, it was cooled to 30 °C over 1 hour, and dispersion was carried out using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.) under the conditions of a liquid feeding rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume filling of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain [WAX Dispersion 1].
[0170] <Synthesis of Ketimine Compound> A reaction vessel equipped with a stirrer and a thermometer was charged with 170 parts of isophoronediamine and 75 parts of methyl ethyl ketone, and the reaction was carried out at 50 °C for 5 hours to obtain [Ketimine Compound 1]. The amine value of [Ketimine Compound 1] was 418.
[0171] <Preparation of Oil Phase> 500 parts of [WAX dispersion 1], 956 parts of [Crystalline polyester dispersion 1], 76 parts of [Prepolymer A], 152 parts of [Prepolymer B], 836 parts of [Amorphous polyester resin C-1], 100 parts of [Master batch 1], and 2 parts of [Ketimine compound 1] as a curing agent were placed in a container and mixed at 5,000 rpm for 60 minutes with a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.) to obtain [Oil phase 1].
[0172] <Synthesis of organic fine particle emulsion (fine particle dispersion)> In a reaction vessel equipped with a stirring rod and a thermometer, 683 parts of water, 11 parts of sodium salt of methacrylic acid ethylene oxide adduct sulfate (Eleminol RS-30: manufactured by Sanyo Chemical Industries, Ltd.), 138 parts of styrene, 138 parts of methacrylic acid, and 1 part of ammonium persulfate were charged and stirred at 400 rpm for 15 minutes, resulting in a white emulsion. The mixture was heated to an internal temperature of 75°C and reacted for 5 hours. Furthermore, 30 parts of a 1% aqueous ammonium persulfate solution was added, and the mixture was aged at 75°C for 5 hours to obtain an aqueous dispersion of a vinyl resin (a copolymer of styrene-methacrylic acid-sodium salt of methacrylic acid ethylene oxide adduct sulfate) [fine particle dispersion 1]. The volume average particle diameter of [Fine Particle Dispersion 1] was measured with an LA-920 (manufactured by HORIBA Corp.) and was found to be 0.14 μm. A part of [Fine Particle Dispersion 1] was dried to isolate the resin content.
[0173] <Preparation of aqueous phase> 990 parts of water, 83 parts of [fine particle dispersion 1], 37 parts of a 48.5% aqueous solution of sodium dodecyldiphenyletherdisulfonate (Eleminol MON-7: manufactured by Sanyo Chemical Industries, Ltd.), and 90 parts of ethyl acetate were mixed and stirred to obtain a milky white liquid, which was designated as [aqueous phase 1].
[0174] <Emulsification / solvent removal> 1,200 parts of [water phase 1] was added to the container containing [oil phase 1], and mixed with a TK homomixer at 13,000 rpm for 20 minutes to obtain [emulsified slurry 1]. Next, [emulsified slurry 1] was placed in a container equipped with a stirrer and thermometer, and the solvent was removed at 30°C for 8 hours, and then aged at 45°C for 4 hours to obtain [dispersed slurry 1].
[0175] <Classification process> The obtained slurry was sieved using a SUS test sieve with 20 μm openings to obtain [sieved slurry 1].
[0176] <Washing and drying> 100 parts of [Sieved Slurry 1] was filtered under reduced pressure, and the following operations were then carried out. (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 100 parts of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), mixed with a TK homomixer (at 12,000 rpm for 30 minutes), and then filtered under reduced pressure. (3): 100 parts of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at 12,000 rpm for 10 minutes) and then filtered. (4): 300 parts of ion-exchanged water was added to the filter cake of (3), and the mixture was mixed with a TK homomixer (at 12,000 rpm for 10 minutes) and then filtered. The above steps (1) to (4) were repeated twice to obtain a filter cake. The filtered cake was dried in a circulating air dryer at 45° C. for 48 hours, and sieved through a 75 μm mesh to obtain toner base particles 1.
[0177] <External Addition Treatment> 100 parts by mass of [toner base particles 1] were mixed in a Henschel mixer with 2.2 parts by mass of hydrophobic silica A with a volume average particle size of 160 nm, 1.0 part by mass of titanium oxide with a volume average particle size of 20 nm, and 0.8 parts of hydrophobic silica fine powder with a volume average particle size of 15 nm. The mixture was sieved through a sieve with 38 μm openings to remove excess material, and [toner 1] was obtained.
[0178] <Preparation of carrier> 100 parts by mass of silicone resin (organo straight silicone), 5 parts by mass of γ-(2-aminoethyl)aminopropyltrimethoxysilane, and 10 parts by mass of carbon black were added to 100 parts by mass of toluene, and dispersed for 20 minutes with a homomixer to prepare a resin layer coating liquid. Using a fluidized bed type coating device, the resin layer coating liquid was applied to the surface of 1,000 parts by mass of spherical magnetite having a volume average particle size of 50 μm to prepare a [carrier].
[0179] <Preparation of developer> Five parts by weight of [Toner 1] and 95 parts by weight of [Carrier] were mixed in a ball mill to prepare [Developer 1].
[0180] Example 2 [Toner 2] and [Developer 2] were prepared in the same manner as in Example 1, except that the mesh size of the sieve in the classification step was changed to 21 μm.
[0181] Example 3 [Toner 3] and [Developer 3] were prepared in the same manner as in Example 1, except that the mesh size of the sieve in the classification step was changed to 23 μm.
[0182] Example 4 [Toner 4] and [Developer 4] were prepared in the same manner as in Example 1, except that the mesh size of the sieve in the classification process was changed to 25 μm and the mesh size of the sieve after the external additive treatment was changed to 20 μm.
[0183] Comparative Example 1 [Toner 5] and [Developer 5] were prepared in the same manner as in Example 1, except that in Example 1, the mesh size of the sieve in the classification process was changed to 20 μm, and the mesh size of the sieve after the external additive treatment was changed to 20 μm.
[0184] Comparative Example 2 [Toner 6] and [Developer 6] were prepared in the same manner as in Example 1, except that the mesh size of the sieve in the classification step was changed to 26 μm.
[0185] Comparative Example 3 [Toner 7] and [Developer 7] were prepared in the same manner as in Example 1, except that in Example 1, the mesh size of the sieve in the classification process was changed to 25 μm, and the mesh size of the sieve after the external additive treatment was changed to 25 μm.
[0186] Comparative Example 4 [Toner 8] and [Developer 8] were prepared in the same manner as in Example 1, except that wet sieving was not performed as the classification step in Example 1, and coarse particles were removed from [toner base particles 1] by air classification.
[0187] Comparative Example 5 [Toner 9] and [Developer 9] were prepared in the same manner as in Example 1, except that the aging time was extended.
[0188] Comparative Example 6 [Toner 10] and [Developer 10] were prepared in the same manner as in Example 1, except that the amount of [Microparticle Dispersion 1] was increased, wet screening was performed as the classification process, and coarse particles were removed from [Toner Base Particles 1] by air classification.
[0189] (measurement) <Black spots> Using a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), print a black solid image in a laboratory environment of 27°C and 80% humidity. While appropriately changing the primary transfer current, find the condition that produces the highest number of black spots, and record this number as the number of black spots. [Evaluation Criteria] .circle.: Black spots are barely visible in the image. ○: Black spots are slightly visible in the image. △: More than 50 black spots are visible in the image. ×: Many black spots are clearly visible (100 or more).
[0190] <Cleaning ability> Using a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), 50,000 sheets (A4 size landscape) of a 5% image area ratio chart were output at 3 prints / job in a laboratory environment of 21°C and 65% RH, and the 50,000 sheets were passed through as follows. Thereafter, in a laboratory environment of 32°C and 54% RH, 100 sheets of A4 size landscape printouts of a vertical band pattern (relative to the paper travel direction) of 43 mm wide and three charts were printed as evaluation images, and the resulting images were visually observed to evaluate the cleaning performance based on the presence or absence of image abnormalities due to poor cleaning. [Evaluation Criteria] ⊚: Toner that has slipped through due to poor cleaning cannot be visually confirmed on the printed paper or on the photoconductor, and no streaks of toner can be confirmed even when observing the photoconductor in the longitudinal direction with a microscope. ◯: The toner that has slipped through due to poor cleaning cannot be visually confirmed on the printed paper or on the photoconductor. Δ: Toner that has slipped through due to poor cleaning can be visually confirmed slightly on the photoconductor, but cannot be confirmed on the printed paper. ×: Toner that has slipped through due to poor cleaning can be visually confirmed on the printed paper and on the photoconductor.
[0191] <Measurement method for coarse particles (1)> At room temperature of about 20°C, a rag and a sieve with 20μm mesh size are placed on the hose (φ38mm) of a blower (vacuum cleaner). The center of the sieve is placed on the center of the hose. Next, the sieve is sucked from the bottom at a wind speed of 8-12m / s, 10mg of toner is placed on the sieve, and the sieve is sucked back and forth five times in the X-axis direction and five times in the Y-axis direction. After that, the sieve is removed and lightly tapped on a desk or similar five times. Thereafter, the surface of the sieve is photographed under a microscope, and the number of all toner particles (coarse toner particles having a particle size of 20 μm or more) remaining on the sieve in the photographed image is counted.
[0192] <Measurement method for coarse particles (2)> At room temperature of about 20°C, a rag and a sieve with 25μm mesh size are placed on the hose (φ38mm) of a blower (vacuum cleaner). The center of the sieve is placed on the center of the hose. Next, the sieve is sucked from the bottom at a wind speed of 8-12m / s, 2g of toner is placed on the sieve, and the sieve is sucked back and forth five times in the X-axis direction and five times in the Y-axis direction. After that, the sieve is removed and lightly tapped on a desk or similar five times. Thereafter, the surface of the sieve is photographed under a microscope, and the number of all toner particles (coarse toner particles having a particle size of 25 μm or more) remaining on the sieve in the photographed image is counted.
[0193] Table 1 shows the evaluation results of the toners of the examples and comparative examples.
[0194] [Table 1]
[0195] As described above, in Examples 1 to 4, excellent results were obtained in terms of the prevention of black spots and the cleaning properties. In contrast to this, in Comparative Example 1, when the number of coarse particles of 20 μm was 10 or less, poor cleaning occurred. In Comparative Example 2, the number of coarse particles of 20 μm was 250 or more, so the number of black spots increased. In Comparative Example 3, there were no coarse particles of 25 μm or more, but there were more than 250 coarse particles of 20 μm or more, so the number of black spots increased. In Comparative Example 4, air classification is used, but this is disadvantageous because air classification cannot selectively remove coarse particles. In Comparative Example 5, the number of coarse particles of 20 μm or more was 250 or less, but the volume average particle size exceeded 6.0 μm, so the number of black spots increased. In Comparative Example 6, the number of coarse particles of 20 μm or more was 250 or less, but the volume average particle size was too small, so the cleaning performance was deteriorated.
[0196] For example, aspects of the present invention are as follows. (1) A toner containing at least a binder resin, a colorant, a wax, and an external additive, The volume average particle size of the toner particles is 4.0 μm or more and less than 6.0 μm, The toner, wherein the number of coarse particles, defined as below, per 10 mg of the toner is 10 to 250. Definition of coarse particles: Toner particles that do not pass through a sieve with 20 μm openings when passed through the dry method (2) The toner according to (1) above, wherein the number of the coarse particles having a size of 25 μm or more per 2 g of the toner is 25 or less. (3) A developer comprising the toner according to (1) or (2) above. (4) A toner storage unit containing the toner according to (1) or (2) above. (5) an electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit which develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image, and which is provided with a toner; 2. An image forming apparatus, comprising the toner according to claim 1, wherein the toner is a toner according to claim 1. (6) forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image, The toner is the toner according to (1) or (2). [Explanation of symbols]
[0197] 10 Electrostatic latent image carrier (photoconductor drum) 10K Black Electrostatic Latent Image Carrier 10Y Yellow electrostatic latent image carrier 10M Magenta electrostatic latent image carrier 10C Cyan electrostatic latent image carrier 14 Support roller 15 Support roller 16 Support roller 17 Cleaning equipment 18 Image forming means 20 Charging roller 21 Exposure equipment 22 Secondary transfer device 23 Laura 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 32 Contact Glass 33 First Running Body 34 Second Running Body 35 Imaging Lens 36 Reading sensor 40 Developer 41 Developing belt 42K Developer compartment 42Y Developer storage unit 42M Developer compartment 42C Developer container 43K Developer supply roller 43Y Developer supply roller 43M Developer supply roller 43C Developer supply roller 44K developing roller 44Y Developing roller 44M Developing roller 44C Developing roller 45K Black Development Unit 45Y Yellow Development Unit 45M Magenta Development Unit 45C Cyan Development Unit 49 Registration roller 50 Intermediate transfer body 51 Lola 52 Separation roller 53 Manual feed path 54 Manual feed tray 55 Switching claw 56 Discharge roller 57 Output Tray 58 Corona charging device 60 Cleaning Equipment 61 Developing device 62 Transfer charger 63 Cleaning Equipment 64 Static electricity removal lamp 70 Static electricity removal lamp 80 Transfer roller 90 Cleaning Equipment 95 Transfer paper 100A, 100B, 100C image forming device 110 Process cartridge 120 Tandem type developer 130 Manuscript stand 142 Paper feed roller 143 Paper Bank 144 Paper feed cassette 145 Separation roller 146 Paper feed path 147 Transport roller 148 Paper feed path 150 Copying device body 160 Charging device 200 Paper feed table 300 Scanner 400 Automatic Document Feeder (ADF) L exposure light [Prior art documents] [Patent documents]
[0198] [Patent Document 1] JP 2022-103861 A [Patent Document 2] JP 2016-139064 A [Patent Document 3] JP 2014-164186 A [Patent Document 4] JP 2013-190493 A [Patent Document 5] JP 2006-126360 A
Claims
1. A toner containing at least a binder resin, a colorant, a wax, and an external additive, The volume average particle size of the toner particles is 4.0 μm or more and less than 6.0 μm, The toner, wherein the number of coarse particles, as defined below, per 10 mg of the toner is 10 to 250. Definition of coarse particles: Toner particles that do not pass through a sieve with 20 μm openings when the toner is passed through the sieve by a dry method.
2. 2. The toner according to claim 1, wherein the number of said coarse particles having a diameter of 25 μm or more per 2 g of said toner is 25 or less.
3. A developer comprising the toner according to claim 1 or 2.
4. A toner storage unit containing the toner according to claim 1 or 2.
5. An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit which develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image, and which is provided with a toner; 3. An image forming apparatus, comprising the toner according to claim 1 or 2.
6. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image, 3. An image forming method, comprising the toner according to claim 1 or 2.
Citation Information
Patent Citations
Image forming apparatus
JP2006126360A
Electrostatic charge image developer, process cartridge, image forming apparatus, and image forming method
JP2013190493A
Electrostatic charge image developer, developer cartridge, process cartridge, image forming apparatus, and image forming method
JP2014164186A
Toner
JP2016139064A
Toner for electrostatic charge image development and method for manufacturing the same
JP2022103861A