Optical polymer material, optical film, and display device
The use of a styrene-maleimide alternating copolymer in optical polymer materials simplifies composition and design, achieving low birefringence and improved performance in display devices by controlling photoelastic coefficient and intrinsic birefringence, enhancing flexibility and heat resistance.
Patent Information
- Application Number
- JP2024109849
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-01
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-12-26
AI Technical Summary
Quinary optical polymer materials have a complex composition and are difficult to design for achieving desired low birefringence characteristics, which is necessary for display devices to maintain image quality under varying environmental conditions.
An optical polymer material comprising an alternating copolymer of a styrene derivative monomer and a maleimide derivative monomer, with specific composition ratios to achieve a photoelastic coefficient and intrinsic birefringence within predetermined absolute values, allowing for a simple binary or ternary system with easy design and low birefringence properties.
The solution results in optical polymer materials and films with extremely low birefringence, high flexibility, and improved heat resistance, maintaining optimal performance across a wide range of temperatures and environmental conditions.
Smart Images

Figure 2024133101000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical polymer material, an optical film, a display device, a method for producing an optical polymer material, and a method for producing an optical film. [Background technology]
[0002] In recent years, display devices such as liquid crystal displays (LCD) and organic light-emitting diode (OLED) displays have been used as display devices for various devices. For example, these display devices are used in computer display devices and television receivers, instrument panels and navigation devices installed in automobiles, airplanes, ships, etc., mobile information terminal devices such as smartphones, and digital signage (electronic billboards) used for advertisements and guidance displays.
[0003] Several kinds of optical polymer films are used in these displays, contributing to the realization of excellent image quality. For example, polarizing plate protective films are desired to have very low birefringence. Also, low birefringence is required for polymers used in pickup lenses and LCD backlights. In order to keep the birefringence low, it is preferable that the intrinsic birefringence and photoelastic birefringence are small. In addition, considering use in a wide range of environmental temperatures, it is preferable that the temperature dependence of the intrinsic birefringence is low (for example, Non-Patent Document 1). In order to realize such optical polymer materials with low temperature dependence and low birefringence, quaternary or quinary optical polymer materials have been required in the past. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] MD Shikanai, A. Tagaya and Y. Koike, Appl. Phys. Lett., 108 pp.131902(2016). Summary of the Invention [Problem to be solved by the invention]
[0005] However, five-component optical polymer materials have complex compositions and require complicated design to obtain the desired properties, which poses problems in their practical use.
[0006] The present invention has been made in view of the above, and aims to provide a low birefringence optical polymer material that has a simple composition and is easy to design to obtain desired characteristics, an optical film and a manufacturing method thereof, and a display device using the same. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems and achieve the object, an optical polymer material according to one embodiment of the present invention comprises an alternating copolymer consisting of a monomer of a styrene derivative and a monomer of a maleimide derivative, and has a nonlinear characteristic in which the photoelastic coefficient decreases to a first value as the composition ratio of the styrene derivative increases and increases above the first value as the composition ratio of the styrene derivative further increases, and is characterized in that the styrene derivative is within a predetermined composition ratio range, and within the composition ratio range, the absolute value of the photoelastic coefficient is a first absolute value or less, and the absolute value of the intrinsic birefringence is a second absolute value or less.
[0008] An optical polymer material according to one embodiment of the present invention comprises a polymer consisting of a monomer of a styrene derivative, a monomer of a maleimide derivative, and a monomer of a modified organic compound having physical properties related to mechanical strength different from those of the monomer of the styrene derivative and the monomer of the maleimide derivative, and has a nonlinear characteristic in which, in a relationship between the monomer of the styrene derivative and the monomer of the maleimide derivative, the photoelastic coefficient decreases to a second value as the composition ratio of the styrene derivative increases, and increases above the second value as the composition ratio of the styrene derivative further increases, and is characterized in that the styrene derivative is within a predetermined composition ratio range, and within the composition ratio range, the absolute value of the photoelastic coefficient is a third absolute value or less, and the absolute value of the intrinsic birefringence is a fourth absolute value or less.
[0009] An optical film according to one aspect of the present invention is characterized by including the optical polymer material.
[0010] A display device according to one aspect of the present invention includes the optical film.
[0011] A method for producing an optical polymer material according to one embodiment of the present invention includes a step of forming an optical polymer material containing an alternating copolymer consisting of a monomer of a styrene derivative and a monomer of a maleimide derivative, and is characterized in that the styrene derivative is within a predetermined composition ratio range, and an optical polymer material is formed in which, within the composition ratio range, the absolute value of the photoelastic coefficient is a first absolute value or less and the absolute value of the intrinsic birefringence is a second absolute value or less.
[0012] A method for producing an optical polymer material according to one embodiment of the present invention includes a step of forming an optical polymer material containing a polymer consisting of a monomer of a styrene derivative, a monomer of a maleimide derivative, and a monomer of a modified organic compound having physical properties related to mechanical strength different from those of the monomer of the styrene derivative and the monomer of the maleimide derivative, and is characterized in that the styrene derivative is within a predetermined composition ratio range, and an optical polymer material is formed in which, within the composition ratio range, the absolute value of the photoelastic coefficient is a third absolute value or less and the absolute value of the intrinsic birefringence is a fourth absolute value or less.
[0013] A method for producing an optical film according to one aspect of the present invention is characterized in that the optical polymer material produced by the above-mentioned production method is thinly molded to produce an optical film. Effect of the Invention
[0014] The present invention has the effect of realizing an optical polymer material and an optical film that have a simple composition of about a binary or ternary system, are easy to design, and have extremely favorable low birefringence characteristics. [Brief description of the drawings]
[0015] [Figure 1]FIG. 1 is a schematic exploded perspective view of a main part of a liquid crystal display device using an optical film made of an optical polymer material according to an embodiment. [Diagram 2] FIG. 2 is a graph showing intrinsic birefringence versus the mass ratio of styrene in optical polymer films containing P(St / EMI). [Diagram 3] FIG. 3 is a graph showing the photoelastic coefficient versus the mass ratio of styrene in an optical polymer containing P(St / EMI). [Figure 4] FIG. 4 is a graph showing the temperature coefficient of intrinsic birefringence versus the mass ratio of styrene in an optical polymer film containing P(St / EMI). [Diagram 5] FIG. 5 is a graph showing the ratio of monomer M1 in the alternating polymer versus the ratio of monomer M1 in the blended monomers. [Figure 6] FIG. 6 is a graph showing the molar ratio of monomer M1 versus the polymerization rate. [Figure 7] FIG. 7 is a histogram showing the composition distribution when the conversion rate is set to 80%. [Figure 8] FIG. 8 is a graph showing the photoelastic coefficient versus the mass ratio of styrene in optical polymer materials having different maleimide derivatives. [Figure 9] FIG. 9 is a graph showing intrinsic birefringence versus the mass ratio of styrene in optical polymer films containing P(St / MMA). [Figure 10] FIG. 10 is a graph showing the photoelastic coefficient versus the mass ratio of styrene in an optical polymer containing P(St / MMA). [Figure 11] FIG. 11 is a graph showing a two-dimensional birefringence map of P(St / EMI / MMA). [Figure 12] FIG. 12 is a graph showing a two-dimensional birefringence map of P(St / CHMI / MMA). [Figure 13] FIG. 13 is a graph showing a two-dimensional birefringence map of P(St / EMI / TCEMA). [Figure 14]FIG. 14 is a graph showing a two-dimensional birefringence map of P(St / EMI / tBuMI). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to this embodiment. In addition, in each drawing, the same or corresponding elements are appropriately assigned the same reference numerals. It should be noted that the drawings are schematic, and the dimensional relationship of each element may differ from the actual one. There may also be parts in which the dimensional relationship and ratio differ between the drawings.
[0017] The optical polymer material according to the embodiment of the present invention is used, for example, as a material for an optical film in a liquid crystal display device. Fig. 1 is a schematic exploded perspective view of a main part of a liquid crystal display device using an optical film made of the optical polymer material according to the embodiment. The liquid crystal display device 10 has a known configuration in which a backlight 1, a polarizing plate 2, a retardation film 3, a glass substrate 4 with a transparent electrode, a liquid crystal layer 5, a glass substrate 6 with a transparent electrode, an RGB color filter 7, a retardation film 8, and a polarizing plate 9 are laminated in this order.
[0018] In this liquid crystal display device 10, the optical film made of the optical polymer material according to the embodiment can be suitably used as the retardation films 3, 8 or protective films attached to both sides of the polarizing plates 2, 9.
[0019] The optical polymer material according to the embodiment of the present invention includes an alternating copolymer consisting of a monomer of a styrene derivative and a monomer of a maleimide derivative. According to the inventors' intensive research, the birefringence characteristics of the optical polymer material including the alternating copolymer consisting of a monomer of a styrene derivative and a monomer of a maleimide derivative change nonlinearly according to the composition ratio of the styrene derivative contained therein. Such a nonlinear change in the birefringence characteristics is a nonlinear characteristic in which the photoelastic coefficient decreases to a certain value as the composition ratio of the styrene derivative increases, and then increases above the certain value as the composition ratio of the styrene derivative further increases.
[0020] Therefore, the present inventors have found an optical polymer material that utilizes this nonlinearity, has a simple binary composition and is easy to design, and has a very favorable low birefringence characteristic. Specifically, the present inventors have found that a styrene derivative is within a predetermined composition ratio range, and within the composition ratio range, it is possible to achieve a characteristic in which the absolute value of the photoelastic coefficient is equal to or less than a relatively small first value, and the absolute value of the intrinsic birefringence is equal to or less than a relatively small second value.
[0021] Optical films used in display devices such as liquid crystal display devices and optical devices are generally subjected to stress during use, which causes photoelastic birefringence (also called stress birefringence). Since photoelastic birefringence is proportional to the photoelastic coefficient and stress, the smaller the photoelastic coefficient, the smaller the photoelastic birefringence. Therefore, if the absolute values of the photoelastic coefficient and intrinsic birefringence are small, extremely desirable low birefringence characteristics can be achieved. Note that the photoelastic coefficient and intrinsic birefringence are quantities that are specific to a material.
[0022] The first absolute value, which is the upper limit of the absolute value of the photoelastic coefficient, is, for example, 50×10 -12 Pa -1 If it is small enough, but preferably 10×10 -12 Pa -1 and more preferably 2×10 -12 Pa -1 The second absolute value, which is the upper limit of the absolute value of the intrinsic birefringence, is, for example, 20×10 -3If so, it should be small enough, but preferably 5×10 -3 and more preferably 1×10 -3 It is.
[0023] In addition, the absolute value of the temperature coefficient of intrinsic birefringence is 2×10 -5 ℃ -1 Less than or equal to 1×10 -5 ℃ -1 If the temperature dependence of the birefringence is small within this range, suitable birefringence characteristics can be maintained over a wide range of environmental temperatures.
[0024] In addition, in optical polymer materials containing random polymers, the intrinsic birefringence, photoelastic coefficient, and temperature coefficient of intrinsic birefringence generally change linearly with respect to the composition ratio of the monomers. However, in the optical polymer material according to the embodiment of the present invention, the birefringence characteristics change nonlinearly depending on the composition ratio of the styrene derivative, so it is believed that suitable birefringence characteristics can be achieved with a simple composition of a binary system and with easy design.
[0025] Furthermore, the present inventors have also found that the optical polymer material according to the embodiment of the present invention is far superior in flexibility and heat resistance to existing low birefringence optical polymer materials.
[0026] Here, maleimide has a basic structure of a five-membered ring formed by imidizing maleic acid, and various maleimide derivatives are formed by substituting the hydrogen atom bonded to the nitrogen atom with various substituents. Also, styrene has a basic structure in which one hydrogen atom of benzene is substituted with a vinyl group, and various styrene derivatives are formed by substituting the hydrogen atom with various substituents.
[0027] The structural formula of N-ethylmaleimide is shown below: The molecular weight of N-ethylmaleimide is 125.13. [ka]
[0028] The structural formula of styrene is shown below: The molecular weight of styrene is 104.15. [ka]
[0029] Furthermore, an example of the structural formula of an alternating copolymer of N-ethylmaleimide and styrene is shown below. [ka]
[0030] The maleimide derivative is represented by, for example, the following general formula: [ka] (R is hydrogen, methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, 1-methylpropyl, 2-methylpropyl, pentyl, cyclopentyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 2,2-dimethylpropyl, 1-ethylpropyl, 2-ethylpropyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, hexyl, cyclohexyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1-ethylbutyl, 2-ethylbutyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 1,1,2-trimethylpropyl, 1,2,2-trimethylpropyl, It is selected from the group consisting of a propyl group, a 1-methyl-1-ethylpropyl group, a 1-ethyl-2-methylpropyl group, a 1,1-diethylethyl group, a 2-ethylhexyl group, a dodecyl group, a lauryl group, a hydroxymethyl group, a 2-hydroxyethyl group, a chloromethyl group, a dichloromethyl group, a trichloromethyl group, a fluoromethyl group, a difluoromethyl group, a trifluoromethyl group, a chlorofluoromethyl group, a dichlorofluoromethyl group, a bromomethyl group, an iodomethyl group, a 1-chloroethyl group, a 2-chloroethyl group, a 2,2,2-trichloroethyl group, a 1,1,2,2,2-pentachloroethyl group, a 1-fluoroethyl group, a 2-fluoroethyl group, a 2,2,2-trifluoromethyl group, a 1,1,2,2,2-pentafluoroethyl group, a 2-bromoethyl group, and a 2,2,2-tribromoethyl group. 1 ,X 2 may be the same or different and are selected from hydrogen, fluorine, chlorine, bromine, iodine, a hydroxyl group, a methyl group, etc., provided that R, X 1 ,X 2 is not limited to these. For example, R may be a phenyl group or a benzyl group.
[0031] The styrene derivative is represented by the following general formula, for example. [ka] (X1 ~X 3 may be the same or different and are selected from hydrogen, fluorine, chlorine, bromine, iodine, a hydroxyl group, a methyl group, and the like. Y 1 ~Y 5 may be the same or different and are selected from hydrogen, fluorine, chlorine, bromine, iodine, hydroxyl group, methyl group, hydroxymethyl group, ethyl group, propyl group, isopropyl group, butyl group, tert-butyl group, pentyl group, hexyl group, etc., provided that X 1 ~X 3 ,Y 1 ~Y 5 are not limited to these.)
[0032] The maleimide derivatives and styrene derivatives shown in these general formulas have structures corresponding to monomers when viewed as monomer units that ultimately form the polymer in the optical polymer material according to the embodiment of the present invention.
[0033] In the polymerization reaction between maleimide derivatives and styrene derivatives, the monomer reactivity ratio r 1 , r 2 It has the characteristic that the molecular weight is extremely small and alternating copolymers are easily formed.
[0034] Hereinafter, an alternating copolymer consisting of a styrene derivative monomer and a maleimide derivative monomer may be referred to as a St / XMI polymer, or P(St / XMI). For example, XMI is written as EMI when the maleimide derivative is N-ethylmaleimide, MeMI when it is N-methylmaleimide, CHMI when it is N-cyclohexylmaleimide, and tBuMI when it is N-tert-butylmaleimide. In addition, hereinafter, St is represented by the chemical formula C unless otherwise specified. 6 H 5 CH=CH 2 It is styrene represented by the formula:
[0035] (Sample Preparation) A sample was prepared to confirm the properties of the optical polymer material according to the embodiment of the present invention. As a method for synthesizing an alternating copolymer consisting of a styrene derivative and a maleimide derivative, for example, a material that becomes a maleimide derivative and a material that becomes a styrene derivative are alternately copolymerized, and then the side chains are reacted to synthesize an alternating copolymer consisting of a maleimide derivative and a styrene derivative. A material that becomes a maleimide derivative is a material that can be made into a maleimide derivative as a monomer unit by a side chain reaction or the like after being incorporated into an alternating copolymer. Similarly, a material that becomes a styrene derivative is a material that can be made into a styrene derivative as a monomer unit by a side chain reaction or the like after being incorporated into an alternating copolymer. Examples of materials that become maleimide derivatives include maleic anhydride derivatives and maleic acid derivatives. In addition, a polymer having a desired structure may be prepared by reacting any side chain with the alternating copolymer synthesized in this way.
[0036] Here, we prepared an alternating copolymer using XMI and St. First, we prepared St, EMI, MeMI, tBuMI, and CHMI manufactured by Tokyo Chemical Industry Co., Ltd. as reagents. St was purified by vacuum distillation. In addition, we prepared methanol and methylene chloride manufactured by Wako Pure Chemical Industries, Ltd. as solvents. Then, polymerization was carried out by the following steps. 1. XMI (EMI, MeMI, tBuMI or CHMI) and St monomers, polymerization initiator, and chain transfer agent were added to a test tube and mixed. The mixing ratio of XMI to St was varied. For example, the monomers added were 100% XMI or 100% St. 2. After sealing the test tube, the contents were mixed by shaking thoroughly and then degassed and dispersed by ultrasonication. 3. The test tube was placed in a 70°C water bath for 24 hours to allow polymerization to occur.
[0037] Both ends of the cylindrical bulk of the optical polymer material produced by the above steps were cut off to obtain a bulk, which was then further purified by the following steps. 1. The bulk was crushed into pieces of about 1 cm square and added to methylene chloride to prepare a homogeneous polymer solution. 2. The polymer solution was added dropwise to methanol to precipitate the polymer. 3. The mixture was filtered through filter paper, and the polymer remaining on the filter paper was collected and dried under reduced pressure in a desiccator for about 2 to 3 hours, and then further dried under reduced pressure in a vacuum dryer at 105°C for more than 24 hours.
[0038] The glass transition temperature of the purified polymer obtained by the above steps was measured using a Shimadzu Corporation differential scanning calorimeter, DSC-60 (DSC).
[0039] Furthermore, the purified polymer was molded into a thin film by the following process. 1. 8 to 20 g of methylene chloride was added to 1 to 2 g of the purified polymer to prepare a homogeneous polymer solution. 2. In a draft chamber, the polymer solution was spread onto a peelable PET film using an applicator. 3. The developed polymer solution was covered with a lid and the solvent was allowed to evaporate slowly. 4. The polymer film formed on the peeled PET film was peeled off and dried under reduced pressure for 24 hours or more in a vacuum dryer. Polymer films with a glass transition temperature of 125°C or less were dried under reduced pressure at 90°C, and other polymer films were dried under reduced pressure at 105°C.
[0040] The photoelastic coefficient of the prepared polymer film was measured using an automatic birefringence control device ABR-EX manufactured by Uniopto Co., Ltd. The photoelastic coefficient was measured as follows. First, a stress of 0 to 2N was applied at intervals of about 0.1N to a sample film with a measurement portion of the film having a width of 4 to 5 mm and a thickness of about 35 to 55 μm to measure the retardation. Then, the photoelastic coefficient was calculated from the retardation in the range of about 0.3 to 2N and the width of the measurement portion. Therefore, the applied stress when measuring the photoelastic coefficient was about 2N at maximum.
[0041] Next, the prepared polymer film was uniaxially hot-stretched using IMC-C513, a film biaxial stretching device manufactured by Imoto Manufacturing Co., Ltd. Then, the film was left to stand for 24 hours or more to relax the internal stress, and the orientation degree of this stretched film was evaluated by the infrared dichroism method from the absorbance in the infrared region using a Fourier transform infrared spectrophotometer, Varian 7000e manufactured by Varian Corporation. In addition, the retardation of the stretched film was measured using an automatic birefringence control device ABR-10A manufactured by Uniopto Corporation. Then, the intrinsic birefringence was calculated from the retardation, the orientation degree, and the thickness of the film. In addition, the refractive index of some of the polymer films was measured, and the copolymerization composition ratio was estimated.
[0042] The film thickness is d, the retardation is Re, and the orientation birefringence is Δn or , the intrinsic birefringence is Δn 0 , and the degree of orientation is f, the following relationship holds: Re = Δn or d=Δn 0 f d Therefore, the intrinsic birefringence can be calculated from the retardation, the degree of orientation, and the thickness of the film.
[0043] An example of the measurement results is shown in Table 1. The intrinsic birefringence calculated from the measurement results can be defined as the intrinsic birefringence of each component polymer weighted by the weight fraction of each component polymer and calculated as the average of the entire polymer. [Table 1]
[0044] (Birefringence characteristics) The birefringence characteristics of the optical polymer film prepared as above will be described. First, the birefringence characteristics of the optical polymer film containing P(St / EMI) prepared by blending more EMI monomers than St monomers will be described. Figure 2 is a graph showing the intrinsic birefringence versus the mass ratio of styrene in the optical polymer film at 25°C. The vertical axis represents the intrinsic birefringence Δn 0The horizontal axis shows the composition ratio of St in the optical polymer film as a percentage (wt.%) as a mass ratio. It is considered that St exists in the optical polymer film in the state of an alternating copolymer or a homopolymer. The mass ratio means the ratio of the total mass of St constituting the alternating copolymer and St constituting the homopolymer to the mass of the optical polymer film. That is, the data point with a mass ratio of 0% is the data of the optical polymer film produced using only EMI without using St. Also, the data point with a mass ratio of 100% is the data of the optical polymer film produced using only St without using XMI. The mass ratio of St was calculated from the refractive index measured at a wavelength of 594 nm, assuming that the refractive index changes linearly with respect to the mass ratio. As shown in Figure 2, it was confirmed that the intrinsic refractive index changes linearly with respect to the mass ratio of St.
[0045] Figure 3 is a graph showing the photoelastic coefficient versus the mass ratio of styrene in the optical polymer. The horizontal axis shows the composition ratio of St in the optical polymer film as a percentage (wt.%) as a mass ratio. The vertical axis shows the photoelastic coefficient C. The mass ratio of St was calculated from the refractive index measured at a wavelength of 594 nm, assuming that the refractive index changes linearly with respect to the mass ratio.
[0046] As shown in Fig. 3, it was confirmed that the change in the photoelastic coefficient with respect to the mass ratio of St was significantly deviated from the linear relationship. Specifically, the change in the photoelastic coefficient with respect to the mass ratio of St was −2×10 -12 Pa -1 As the composition ratio increases further, it increases to -2×10 -12 Pa -1 It was confirmed that the shape of the saturation voltage changes from -2×10 to -10 in a nonlinear manner, i.e., a downward convex or V-shaped change. -12 Pa -1 does not necessarily coincide exactly with the minimum value of the V-shape.
[0047] FIG. 4 is a graph showing the temperature coefficient of intrinsic birefringence versus the mass ratio of styrene in an optical polymer film. The horizontal axis shows the composition ratio of St in the optical polymer film as a mass ratio expressed as a percentage (wt.%). The vertical axis shows the temperature coefficient of intrinsic birefringence (dΔn 0 / dT). The mass ratio of St was calculated from the refractive index measured at a wavelength of 594 nm, assuming that the refractive index changes linearly with respect to the mass ratio.
[0048] As shown in Fig. 4, it was confirmed that the temperature coefficient of intrinsic birefringence changes significantly from a linear relationship with respect to the mass ratio of St. Specifically, it was confirmed that the change is upwardly convex or inverted V-shaped. Furthermore, the temperature coefficient is 1.2 × 10 over the range of mass ratios from 0% to 100%. -5 ℃ -1 is less than or equal to 2 x 10 -5 ℃ -1 It was confirmed that the value was extremely small and satisfied the following criteria. As in Figure 3, the confirmed value of 1.2 × 10 -5 ℃ -1 does not necessarily coincide exactly with the maximum value of the V-shape, but it is 2×10 -5 ℃ -1 It is certain that the value is significantly smaller.
[0049] An example of the properties of the prepared optical polymer material and optical film is shown in Table 2. Tg is the glass transition temperature. St (wt.%) and EMI (wt.%) are the mass ratios at the time of blending, i.e., when the material is charged (in feed). As shown in Table 2, when St was 23.3 wt.% and EMI was 76.7 wt.%, an extremely high glass transition temperature of 193.9°C was obtained, and it was confirmed that the heat resistance was extremely high. In addition, the intrinsic birefringence Δn 0 is 0.07 x 10 at 25°C. -3 and the temperature coefficient dΔn 0 / dT is 0.72 × 10 -5 ℃ -1 and the photoelastic coefficient C is 0.91×10 -12 Pa -1 Both values were extremely low, close to zero, confirming favorable low birefringence characteristics.
[0050] [Table 2]
[0051] Next, the samples in Table 2 were analyzed by proton nuclear magnetic resonance ( 1 The composition ratio (In copolymer) was measured by H-NMR. The Δn 0 The composition ratio at which Δn 0 = 0) and the composition ratio ((in feed)) are shown in Table 3. As shown in Table 3, it was confirmed that good low birefringence characteristics can be achieved with P(St / EMI = 31 / 69 (wt.%)). It was also confirmed that such optical polymer materials and optical films can be realized with a feed composition of St of 23.3 wt.% and EMI of 76.7 wt.%. In addition, P(St / EMI = 31 / 69 (wt.%)) is expressed as P(St / EMI = 35 / 65 (mol%)). The difference between the calculated composition ratio and the actual composition ratio was within 1%. This suggests that in polymer systems containing P(St / EMI) (P(St / EMI) systems), an extremely high linearity is established between the intrinsic birefringence and the composition ratio. The optimal composition for reducing birefringence differs depending on the structure of each monomer. For example, the present inventors have predicted by calculation that in the P(St / CHMI) system, birefringence is particularly small at a composition in the vicinity of (St / CHMI=16 / 84(wt.%)). That is, in a certain range including (St / CHMI=16 / 84(wt.%)), the absolute value of the photoelastic coefficient is 50×10 -12 Pa -1 and the absolute value of the intrinsic birefringence is 20×10 -3 The following favorable properties are expected to be achieved:
[0052] [Table 3]
[0053] (Copolymer composition analysis based on the Mayo-Lewis equation) Next, the copolymer composition of the P(St / EMI) system was analyzed based on the Mayo-Lewis equation (see, for example, I. Skeist, J. Am. Chem. Soc., 68, p. 1781 (1946); M. Fineman, S. D. Ross, J. Polym. Sci., 5, 2, p. 259-265 (1949); R. Kitamura, kobunshi, 14, 160, p. 564-573(1965), etc.).
[0054] Monomer M 1 , monomer M 2 When St and EMI are respectively, the monomer reactivity ratio r 1 , r 2 is 0.05, 0.01. Also, the monomer M 1 , monomer M 2 When St and CHMI are respectively, the monomer reactivity ratio r 1 , r 2 are extremely small, 0.13 and 0.0053 (see, for example, H. Aida, I. Takase, M. Kobayashi, Fukui University Faculty of Engineering Research Report, 31, 1, p.43-50 (1985); T. Oishi, M. Fujimoto, and Y. Haruta, Kobunshi Ronbunshu, 48(3), p. 123-128 (1991)). 1 and monomer M 2 The copolymer composition was analyzed using St and EMI, respectively.
[0055] [Table 4]
[0056] Figure 5 shows the M 1 (St) ratio in polymer 1 The graph shows the ratio of the monomers in the horizontal axis. For example, 0 indicates that all the monomers in the 2(EMI), and 1 is where all the monomers are M 1 The vertical axis indicates the M of the polymer that is instantaneously formed when the ratio on the horizontal axis is used. 1 The ratio of is shown.
[0057] As shown in Figure 5, M 1 The ratio of M in a polymer increases only slightly from 0. 1 The ratio of M 1 The value of 0.5 is maintained until the ratio of 1 and M. 2 This shows that alternating copolymers with r 1 , r 2 It was confirmed that there was no significant change even when the value was changed within the range of about 0.01 to 0.1.
[0058] Figure 6 shows the M 1 , M 2 M for the polymerization rate when St and EMI are respectively 1 1 is a graph showing the molar ratio of the monomers in the polymer material. The polymerization rate is the ratio of the monomers that have become polymers to the total monomers that have been mixed to prepare the polymer material.
[0059] In Figure 6, Monomer composition is M 1 The molar ratio of monomers in M1 is approximately 23% when the polymerization rate P is 0%, but becomes 0% when the polymerization rate P is approximately 50%. This means that all of the monomers in M1 have become polymerized. The instantaneous copolymer composition is the molar ratio of polymers that are instantaneously produced at that polymerization rate P, and is 50% even when the polymerization rate P is 0%. This means that an alternating copolymer is produced from the early stage of the polymerization initiation. The molar ratio also drops rapidly to 0% when the polymerization rate P is close to 50%. This means that the amount of M1 required to produce an alternating copolymer 1 This is because the monomer content of M becomes 0%. 1This is the cumulative value of the polymer including the polymer. When the polymerization rate P is between 0% and 50%, the rate is about 50% because alternating copolymers are formed, but when it is 50% or more, the M 2 Since the homopolymer of M is produced, 1 The relative proportion of polymers containing r (almost alternating copolymers) decreases. Note that since Figure 6 is a calculated value, the polymerization rate P is shown up to 100%, but in reality, as the polymerization reaction proceeds, the monomer becomes less mobile within the polymer, so the polymerization reaction decreases once a certain polymerization rate is reached. This tendency also continues to increase with increasing r 1 , r 2 It was confirmed that there was no significant change even when the value was changed within the range of about 0.01 to 0.1.
[0060] Here, since the P(St / EMI=35 / 65 (mol%)) was found in the prepared optical polymer material and optical film, it is suggested that the conversion rate to polymer was about 80%.
[0061] FIG. 7 is a histogram showing the composition distribution when the conversion rate is set to 80%. FIG. 7 shows the following: 1 Polymers containing 40-50% (St) account for approximately 55% of the total, and M 1 Contains 5% or less, almost M 2 About 35% of the polymers are homopolymers of (EMI), and the remaining 10% are polymers with intermediate compositions. 1 A polymer containing 40-50% of r 1 , r 2 << 1, so M 1 and M. 2 This suggests that the copolymer is an alternating copolymer of St-alt-EMI and St-alt-EMI, i.e., P(St-alt-EMI).
[0062] (Photoelastic coefficient of various P(St / XMI)) Next, the measurement results of the photoelastic coefficient of P(St / XMI) with different maleimide derivatives will be described. FIG. 8 is a graph showing the photoelastic coefficient of P(St / XMI) when XMI is EMI, CHMI, MeMI, or tBuMI. In each case, the mass ratio of St was calculated from the refractive index measured at a wavelength of 594 nm, assuming that the refractive index changes linearly with respect to the mass ratio. In each case, it was confirmed that the photoelastic coefficient has a nonlinear characteristic in which it decreases as the mass ratio of St increases and increases as the mass ratio of St increases further. The cause of such nonlinearity is not necessarily clear, but it is expected to be an interaction between the skeleton of the maleimide derivative and the benzene ring of the St derivative.
[0063] (Haze value of blend polymer of P(St / EMI) and PEMI) Next, equal amounts of P (St / EMI=30 / 70 (wt.%)) and EMI homopolymer (PEMI) were mixed, dissolved in methylene chloride, and spread on a peelable PET film in the same manner as described above to produce a blended polymer film. The glass transition temperature and haze value of this blended polymer were then measured. As a result, the haze value was 1.26%, despite being a blended polymer, and was equivalent to the haze value of polymethyl methacrylate (PMMA), which is 1.25%.
[0064] The glass transition temperature of the blend polymer was 220°C. This was equivalent to 221°C, which is the average value of the glass transition temperature of P (St / EMI=30 / 70 (wt.%)) (185°C) and the glass transition temperature of PEMI (257°C). The blend polymer had one endothermic peak for the glass transition. This suggests that the blend polymers have high compatibility. The low haze value also suggests high compatibility.
[0065] On the other hand, it was confirmed that when preparing a P(St / EMI)-based polymer, if the amount of St charged is large, the polymer may become cloudy. For this reason, in order to reduce the haze value, it is preferable to mix a larger amount of maleimide derivative monomers (or materials that become maleimide derivatives) than styrene derivative monomers (or materials that become styrene derivatives) when producing an optical polymer material. Alternatively, the polymer may be prepared using a polymer blending method.
[0066] (Other embodiments) In order to modify the optical polymer material according to the above embodiment, the present inventors have considered including a monomer of a methacrylic acid derivative as a modifying organic compound in the constituent materials of the polymer in addition to the styrene derivative and the maleimide derivative. The styrene derivative and the maleimide derivative have, for example, a positive photoelastic coefficient, but the methacrylic acid derivative has a different physical property value related to mechanical strength, such as a glass transition temperature, from the monomer of the styrene derivative and the monomer of the maleimide derivative, and has, for example, a negative photoelastic coefficient.
[0067] As a result, the present inventors have found an optical polymer material that contains a polymer composed of a monomer of a styrene derivative, a monomer of a maleimide derivative, and a monomer of a methacrylic acid derivative, and has a nonlinear characteristic in which the photoelastic coefficient decreases to a second value as the composition ratio of the styrene derivative increases in relation to the monomer of the styrene derivative and the monomer of the maleimide derivative, and increases above the second value as the composition ratio of the styrene derivative increases further, the styrene derivative is within a predetermined composition ratio range, the absolute value of the photoelastic coefficient is a third absolute value or less within the composition ratio range, and the absolute value of the intrinsic birefringence is a fourth absolute value or less. The third absolute value is, for example, 50×10 -12 Pa -1 and the fourth absolute value is, for example, 20×10 -3Furthermore, the present inventors have conceived that, in this optical polymer material, by setting the composition ratio of the styrene derivative and the composition ratio of the maleimide derivative so that the coordinate point indicated by the first photoelastic coefficient and the first intrinsic birefringence determined by the composition ratio of the styrene derivative and the composition ratio of the maleimide derivative, and the coordinate point indicated by the second photoelastic coefficient and the second intrinsic birefringence of the methacrylic acid derivative are located on either side of the origin in a two-dimensional birefringence map defined by the photoelastic coefficient and the intrinsic birefringence, and by setting the composition ratio of the methacrylic acid derivative so as to offset the first photoelastic coefficient and the first intrinsic birefringence, an optical polymer material having a simple composition and ease of design as a ternary system, and having extremely preferable low birefringence characteristics and improved characteristics in terms of mechanical strength can be realized.
[0068] Furthermore, the present inventors have conceived of an optical polymer material containing a polymer consisting of a monomer of a styrene derivative, a monomer of a maleimide derivative, and a monomer of a methacrylic acid derivative, by setting the composition ratios of any two of the styrene derivative, the maleimide derivative, and the methacrylic acid derivative so that a coordinate point indicated by a first photoelastic coefficient and a first intrinsic birefringence determined by the composition ratios of any two of the styrene derivative, the maleimide derivative, and the methacrylic acid derivative and a coordinate point indicated by the second photoelastic coefficient and the second intrinsic birefringence of another one of the styrene derivative, the maleimide derivative, and the methacrylic acid derivative are located on either side of the origin in a two-dimensional birefringence map defined by the photoelastic coefficient and the intrinsic birefringence, and by setting the composition ratio of the other one so that the first photoelastic coefficient and the first intrinsic birefringence are offset, thereby realizing an optical polymer material having a simple composition and ease of design as a ternary system, and having extremely preferable low birefringence characteristics and improved characteristics in terms of mechanical strength.
[0069] In the above study, the present inventors first prepared a copolymer using St and a methacrylic acid derivative as a preliminary study. MMA (methyl methacrylate) was used as the methacrylic acid derivative. First, MMA manufactured by Wako Pure Chemical Industries, Ltd. was prepared as a reagent. MMA was purified by vacuum distillation. In addition, methanol and methylene chloride manufactured by Wako Pure Chemical Industries, Ltd. were prepared as solvents.
[0070] Then, polymerization was carried out in the same manner as in the case of the above-mentioned alternating copolymer, but under appropriately optimized conditions. The cylindrical bulk of the optical polymer material produced by this process was cut at both ends to obtain a bulk, which was then purified in the same manner as in the case of the above-mentioned alternating copolymer, but under appropriately optimized conditions.
[0071] The glass transition temperature of the purified polymer obtained by the above steps was measured using a DSC-60 (DSC).
[0072] The purified polymer was then molded into a thin film by a process similar to that for the above-mentioned alternating copolymer, but with appropriately optimized conditions.
[0073] The photoelastic coefficient of the prepared polymer film was measured using an ABR-EX.
[0074] Next, the prepared polymer film was uniaxially hot-stretched using an IMC-11A9 film biaxial stretching device manufactured by Imoto Manufacturing Co., Ltd. After that, the film was left to stand for more than 24 hours to relax the internal stress, and the orientation degree of this stretched film was evaluated using an infrared dichroic method based on the absorbance in the infrared region using a Varian 7000e. In addition, the retardation of the stretched film was measured using an ABR-10A. The intrinsic birefringence was calculated from the retardation, orientation degree, and film thickness. In addition, the refractive index of some of the polymer films was measured, and the copolymerization composition ratio was estimated.
[0075] 9 is a graph showing the intrinsic birefringence versus the mass ratio of styrene in an optical polymer film containing P(St / MMA) at 25° C. The vertical axis is the intrinsic birefringence Δn 0 The horizontal axis indicates the composition ratio of St in the optical polymer film as a percentage (wt.%) as a mass ratio. The mass ratio of St was calculated from the refractive index measured at a wavelength of 594 nm, assuming that the refractive index changes linearly with respect to the mass ratio. As shown in Figure 9, it was confirmed that the intrinsic refractive index changes linearly with respect to the mass ratio of St.
[0076] Figure 10 is a graph showing the photoelastic coefficient versus the mass ratio of styrene in an optical polymer containing P(St / MMA). The horizontal axis indicates the composition ratio of St in the optical polymer film as a percentage (wt.%) as a mass ratio. The vertical axis indicates the photoelastic coefficient C. The mass ratio of St was calculated from the refractive index measured at a wavelength of 594 nm, assuming that the refractive index changes linearly with respect to the mass ratio.
[0077] As shown in Fig. 10, it was confirmed that the change in the photoelastic coefficient with respect to the mass ratio of St deviates significantly from linearity and changes downward in a convex shape. It was also confirmed that when the mass ratio of St is 0%, that is, when MMA is 100%, the photoelastic coefficient of the optical polymer is a negative value.
[0078] Using the above results of P(St / MMA) and P(St / EMI), a two-dimensional birefringence map of a ternary optical polymer including P(St / EMI / MMA) was created. The two-dimensional birefringence map is a map obtained by connecting any two points of the intrinsic birefringence and photoelastic coefficient of each homopolymer St, EMI, and MMA with a line on the two-dimensional coordinate axis defined by the intrinsic birefringence and photoelastic coefficient.
[0079] Figure 11 is a graph showing the two-dimensional birefringence map of P(St / EMI / MMA). Note that the unmeasured parts are shown with a dashed line. As mentioned above, in a binary optical polymer containing St, the change in the photoelastic coefficient with respect to the composition ratio is nonlinear, so the line also has a nonlinear shape. Note that, for example, PSt indicates a point that represents the characteristics of a homopolymer of St. The same is true for PEMI and PMMA.
[0080] Using this two-dimensional birefringence map, an optical polymer with a composition ratio with small intrinsic birefringence and photoelastic coefficient can be designed, for example, as in the following example. That is, first, the composition ratio of P(St / EMMI) is set so that the coordinate point indicated by the photoelastic coefficient and intrinsic birefringence (first photoelastic coefficient and first intrinsic birefringence) determined by the composition ratio of St and the composition ratio of EMI and the coordinate point indicated by the photoelastic coefficient and intrinsic birefringence (second photoelastic coefficient and second intrinsic birefringence) of MMA are located on either side of the origin. Next, the composition ratio of the methacrylic acid derivative is set so that the second photoelastic coefficient and second intrinsic birefringence cancel out the first photoelastic coefficient and first intrinsic birefringence.
[0081] Here, the coordinate point represented by the first photoelastic coefficient and the first intrinsic birefringence and the coordinate point represented by the second photoelastic coefficient and the second intrinsic birefringence are located on either side of the origin, including the case where the three points are aligned in a straight line, but they do not necessarily have to be aligned in a straight line, and also including the case where a line connecting two coordinate points passes near the origin. In addition, the second photoelastic coefficient and the second intrinsic birefringence cancel out the first photoelastic coefficient and the first intrinsic birefringence, including the case where the sum of the second photoelastic coefficient and the first photoelastic coefficient is zero and the sum of the second intrinsic birefringence and the first photoelastic coefficient is zero, and also including the case where they are not completely canceled out, such that at least one of the sums is close to zero. As a result, the absolute value of the photoelastic coefficient is 50×10 -12 Pa -1 The absolute value of the intrinsic birefringence is 20×10 -3 It is possible to realize optical polymeric materials that are:
[0082] (Preparation of ternary optical polymers) Using the two-dimensional birefringence map of P(St / EMI / MMA) in FIG. 11, the monomer amounts and composition ratios shown in Table 5 were set, and a ternary optical polymer film was produced. [Table 5]
[0083] Specifically, the monomers shown in Table 5 were prepared and polymerization was carried out in the same manner as in the case of the alternating copolymer described above, but under appropriately optimized conditions. Both ends of the cylindrical bulk of the optical polymer material produced by this process were cut off to obtain a bulk, which was then purified in the same manner as in the case of the alternating copolymer described above, but under appropriately optimized conditions. For example, vacuum drying in a vacuum dryer was carried out at 90°C for 24 hours.
[0084] The glass transition temperature of the purified polymer obtained by the above steps was measured using a DSC-60 (DSC).
[0085] The purified polymer was then molded into a thin film by a process similar to that for the above-mentioned alternating copolymer, but with appropriately optimized conditions.
[0086] The photoelastic coefficient of the prepared polymer film was measured using an ABR-EX.
[0087] Next, the prepared polymer film was uniaxially hot-stretched using an IMC-11A9 film biaxial stretching device manufactured by Imoto Manufacturing Co., Ltd. After that, the film was left to stand for more than 24 hours to relax the internal stress, and the orientation degree of this stretched film was evaluated using an infrared dichroic method based on the absorbance in the infrared region using a Varian 7000e. In addition, the retardation of the stretched film was measured using an ABR-10A. The intrinsic birefringence was calculated from the retardation, orientation degree, and film thickness. In addition, the refractive index of some of the polymer films was measured, and the copolymerization composition ratio was estimated.
[0088] Table 6 shows an example of the properties of the optical polymer material and optical film produced. St (wt.%), EMI (wt.%), and MMA (wt.%) are the mass ratios at the time of charging. As shown in Table 6, a high glass transition temperature of 156°C was obtained when St was 17 wt.%, EMI was 63 wt.%, and MMA was 20 wt.%, confirming high heat resistance. Note that this optical polymer material and optical film were modified so that their glass transition temperatures were lower than 193.9°C in the case of a binary system not containing MMA shown in Table 2. The temperature of 156°C is higher than the glass transition temperature of acrylic resin and is equivalent to 150°C, which is the glass transition temperature of polycarbonate. Therefore, it can be said that this optical polymer material and optical film have high heat resistance and are easy to injection mold. In addition, the intrinsic birefringence Δn 0 is 0.10 x 10 at 25°C. -3 and the temperature coefficient dΔn 0 / dT is 1.21 × 10 -5 ℃ -1 and the photoelastic coefficient C is -0.24×10 -12 Pa -1 Both values were extremely low, close to zero, confirming favorable low birefringence characteristics.
[0089] [Table 6]
[0090] Furthermore, we created a two-dimensional birefringence map of a ternary optical polymer, P(St / CHMI / MMA), which uses N-cyclohexylmaleimide (CHMI) as a maleimide derivative.
[0091] Figure 12 is a graph showing the two-dimensional birefringence map of P(St / CHMI / MMA). Note that the unmeasured parts are shown with dashed lines. As in Figure 11, in a binary optical polymer containing St, the change in the photoelastic coefficient with respect to the composition ratio is nonlinear, so the line also has a nonlinear shape.
[0092] Using this two-dimensional birefringence map, an optical polymer with a composition ratio that provides small intrinsic birefringence and photoelastic coefficient can be designed, for example, as in the following example. That is, first, the composition ratio of P(St / CHMI) is set so that the coordinate point indicated by the photoelastic coefficient and intrinsic birefringence (first photoelastic coefficient and first intrinsic birefringence) determined by the composition ratio of St and the composition ratio of CHMI, and the coordinate point indicated by the photoelastic coefficient and intrinsic birefringence (second photoelastic coefficient and second intrinsic birefringence) of MMA are located on either side of the origin. Next, the composition ratio of the methacrylic acid derivative is set so that the second photoelastic coefficient and second intrinsic birefringence cancel out the first photoelastic coefficient and first intrinsic birefringence. As a result, the absolute value of the photoelastic coefficient is 50×10 -12 Pa -1 The absolute value of the intrinsic birefringence is 20×10 -3 It is possible to realize optical polymeric materials that are:
[0093] Using the two-dimensional birefringence map of P(St / CHMI / MMA) in FIG. 12, the monomer amounts and composition ratios shown in Table 7 were set, and a ternary optical polymer film was produced. [Table 7]
[0094] Specifically, the monomers shown in Table 7 were prepared and polymerized in the same manner as in the case of P(St / EMI / MMA) described above, but under appropriately optimized conditions. The bulk obtained by cutting both ends of the cylindrical bulk of the optical polymer material produced by this process was further purified in the same manner as in the case of P(St / EMI / MMA) described above, but under appropriately optimized conditions.
[0095] The glass transition temperature of the purified polymer obtained by the above steps was measured using a DSC-60 (DSC).
[0096] Furthermore, the purified polymer was molded into a thin film using a process similar to that for P(St / EMI / MMA) described above, but with appropriately optimized conditions.
[0097] The photoelastic coefficient of the prepared polymer film was measured using an ABR-EX.
[0098] Next, the prepared polymer film was uniaxially hot-stretched using IMC-11A9. After that, it was left to stand for more than 24 hours to relax the internal stress, and the orientation degree of this stretched film was evaluated by infrared dichroism method from the absorbance in the infrared region using Varian 7000e. In addition, the retardation of the stretched film was measured using ABR-10A. Then, the intrinsic birefringence was calculated from the retardation, orientation degree, and film thickness. In addition, the refractive index of some of the polymer films was measured, and the copolymerization composition ratio was estimated.
[0099] An example of the properties of the prepared optical polymer material and optical film is shown in Table 8. St (wt.%), CHMI (wt.%), and MMA (wt.%) are the mass ratios at the time of charging. As shown in Table 8, a high glass transition temperature of 161°C was obtained with St at 6 wt.%, CHMI at 40 wt.%, and MMA at 54 wt.%, and it was confirmed that the material had high heat resistance and was easy to injection mold. In addition, the intrinsic birefringence Δn 0 is -5.23 x 10 at 25°C -3 and the photoelastic coefficient C is -0.12×10 -12 Pa -1 Both values were extremely low, close to zero, confirming favorable low birefringence characteristics.
[0100] [Table 8]
[0101] Furthermore, we created a two-dimensional birefringence map of a ternary optical polymer, P(St / EMI / TCEMA), which uses a methacrylic acid derivative, TCEMA (2,2,2-trichloroethyl methacrylate), as a modifying organic compound.
[0102] FIG. 13 is a graph showing a two-dimensional birefringence map of P(St / EMI / TCEMA). Note that unmeasured parts are shown with dashed lines. Using this two-dimensional birefringence map, the absolute value of the photoelastic coefficient was calculated to be 50×10 -12 Pa -1 The absolute value of the intrinsic birefringence is 20×10 -3 It is possible to realize optical polymeric materials that are:
[0103] Using the two-dimensional birefringence map of P(St / EMI / TCEMA) in FIG. 13, the monomer amounts and composition ratios shown in Table 9 were set, and a ternary optical polymer film was produced. [Table 9]
[0104] An example of the properties of the prepared optical polymer material and optical film is shown in Table 10. St (wt.%), EMI (wt.%), and TCEMA (wt.%) are the mass ratios at the time of charging. As shown in Table 10, a high glass transition temperature of 188°C was obtained when St was 23 wt.%, EMI was 69 wt.%, and TCEMA was 8 wt.%, confirming high heat resistance. In addition, the intrinsic birefringence Δn 0 is -0.65 x 10 at 25°C -3 and the photoelastic coefficient C is 0.08×10 -12 Pa -1 Both values were extremely low, close to zero, confirming favorable low birefringence characteristics.
[0105] [Table 10]
[0106] Furthermore, we prepared two-dimensional birefringence maps of a ternary optical polymer, P(St / EMI / tBuMI), in which tBuMI, a maleimide derivative, was used as the modifying organic compound.
[0107] FIG. 14 is a graph showing a two-dimensional birefringence map of P(St / EMI / tBuMI). Note that unmeasured parts are shown with dashed lines. tBuMI has a positive photoelastic coefficient, but by using this two-dimensional birefringence map, the absolute value of the photoelastic coefficient is 50×10 -12 Pa -1 The absolute value of the intrinsic birefringence is 20×10 -3 It is possible to realize optical polymeric materials that are:
[0108] Using the two-dimensional birefringence map of P(St / EMI / tBuMI) in FIG. 14, the monomer amounts and composition ratios shown in Table 11 were set, and a ternary optical polymer film was produced. [Table 11]
[0109] An example of the properties of the prepared optical polymer material and optical film is shown in Table 12. St (wt.%), EMI (wt.%), and tBuMI (wt.%) are the mass ratios at the time of charging. As shown in Table 12, when St was 25.0 wt.%, EMI was 62.5 wt.%, and tBuMI was 12.5 wt.%, a glass transition temperature of 197°C, which is higher than that of P(St / EMI), was obtained, confirming high heat resistance. In addition, the intrinsic birefringence Δn 0 is 3.68 × 10 at 25°C. -3 and the photoelastic coefficient C is 0.27×10 -12 Pa -1 Both values were extremely low, close to zero, confirming favorable low birefringence characteristics.
[0110] [Table 12]
[0111] As the example of P(St / EMI / tBuMI) shows, the modified organic compound is not limited to methacrylic acid derivatives, and the sign of the photoelastic coefficient may be either positive or negative. In addition, in the modified organic compound, the physical property value different from that of the styrene derivative monomer and the maleimide derivative monomer is not limited to the glass transition temperature, and may be other physical property values related to mechanical strength. This makes it possible to obtain an optical polymer material with more preferable physical property values related to mechanical strength. In addition, the modified organic compound may contain two or more different monomers.
[0112] Furthermore, the present invention is not limited to the above-mentioned embodiment. The present invention also includes a configuration in which the above-mentioned components are appropriately combined. Further effects and modifications can be easily derived by those skilled in the art. Therefore, the broader aspects of the present invention are not limited to the above-mentioned embodiment, and various modifications are possible. [Explanation of symbols]
[0113] 10 LCD display device 1 Backlight 2, 9 Polarizing plate 3, 8 Phase difference film 4, 6 Glass substrate with transparent electrodes 5 Liquid crystal layer 7 RGB Color Filters
Claims
1. The copolymer includes an alternating copolymer of a styrene derivative monomer and a maleimide derivative monomer, a photoelastic coefficient has a nonlinear characteristic that decreases to a first value as the composition ratio of the styrene derivative increases and increases above the first value as the composition ratio of the styrene derivative further increases; The styrene derivative is within a predetermined composition ratio range, and within the composition ratio range, the absolute value of the photoelastic coefficient is a first absolute value or less, and the absolute value of the intrinsic birefringence is a second absolute value or less.
2. The first absolute value is 50×10 -12 P -1 and the second absolute value is 20×10 -3 2. The optical polymer material according to claim 1,
3. The absolute value of the temperature coefficient of intrinsic birefringence is 2×10 -5 ℃ -1 3. The optical polymer material according to claim 1, wherein:
4. 4. The optical polymer material according to claim 1, wherein the styrene derivative is styrene and the maleimide derivative is ethylmaleimide.
5. 5. The optical polymer material according to claim 4, wherein the range of the composition ratio of the styrene derivative is a range including 31% in the case of a mass ratio and a range including 35% in the case of a molar ratio.
6. a polymer including a monomer of a styrene derivative, a monomer of a maleimide derivative, and a monomer of a modified organic compound having a different physical property value relating to mechanical strength from the monomer of the styrene derivative and the monomer of the maleimide derivative; a photoelastic coefficient has a nonlinear characteristic in which, in relation to the monomer of the styrene derivative and the monomer of the maleimide derivative, the photoelastic coefficient decreases to a second value as the composition ratio of the styrene derivative increases, and increases above the second value as the composition ratio of the styrene derivative further increases; The styrene derivative is within a predetermined composition ratio range, and within the composition ratio range, the absolute value of the photoelastic coefficient is a third absolute value or less, and the absolute value of the intrinsic birefringence is a fourth absolute value or less.
7. In a two-dimensional birefringence map defined by the intrinsic birefringence and the photoelastic coefficient, The optical polymer material described in claim 6, characterized in that the composition ratio of the styrene derivative and the composition ratio of the maleimide derivative are set so that a coordinate point indicated by a first photoelastic coefficient and a first intrinsic birefringence determined by the composition ratio of the styrene derivative and the composition ratio of the maleimide derivative and a coordinate point indicated by a second photoelastic coefficient and a second intrinsic birefringence of the modified organic compound are located on either side of the origin, and the composition ratio of the modified organic compound is set so that the second photoelastic coefficient and the second intrinsic birefringence cancel out the first photoelastic coefficient and the first intrinsic birefringence.
8. The third absolute value is 50×10 -12 P -1 and the fourth absolute value is 20×10 -3 8. The optical polymer material according to claim 7,
9. 9. The optical polymer material according to claim 7 or 8, characterized in that the glass transition temperature is higher than that of an acrylic resin and lower than that when the modifying organic compound is not contained, or higher than that when the modifying organic compound is not contained.
10. 10. The optical polymer material according to any one of claims 6 to 9, wherein the styrene derivative is styrene, the maleimide derivative is ethylmaleimide or cyclohexylmaleimide, and the modifying organic compound is a methacrylic acid derivative or t-butylmaleimide.
11. The optical polymer material according to claim 10, characterized in that the range of the composition ratio of the styrene derivative is a range including 6%, 17%, 23% or 25% in the case of mass ratio, and a range including 7%, 18.8%, 27.3% or 29% in the case of molar ratio.
12. 12. The optical polymer material according to claim 1, wherein the maleimide derivative is contained in a larger amount than the styrene derivative.
13. The optical polymer material according to any one of claims 1 to 12, characterized in that it contains a homopolymer of the maleimide derivative.
14. An optical film comprising the optical polymer material according to any one of claims 1 to 13.
15. A display device comprising the optical film according to claim 14.
16. Forming an optical polymeric material comprising an alternating copolymer of styrene derivative monomers and maleimide derivative monomers. Including, The styrene derivative is within a predetermined composition ratio range, Within the composition ratio range, an optical polymer material is formed having a photoelastic coefficient whose absolute value is a first absolute value or less and an intrinsic birefringence whose absolute value is a second absolute value or less.
2. A method for producing an optical polymer material comprising the steps of:
17. 17. The method for producing an optical polymer material according to claim 16, wherein the alternating copolymer is formed by blending a material that becomes a maleimide derivative in a larger amount than a material that becomes a styrene derivative.
18. The first value is 50×10 -12 P -1 and the second value is 20×10 -3 18. The method for producing an optical polymer material according to claim 16, wherein
19. A step of forming an optical polymer material including a polymer made of a styrene derivative monomer, a maleimide derivative monomer, and a modified organic compound monomer having mechanical strength properties different from those of the styrene derivative monomer and the maleimide derivative monomer. Including, The styrene derivative is within a predetermined composition ratio range, Within the composition ratio range, an optical polymer material is formed having an absolute value of a photoelastic coefficient that is a third absolute value or less and an absolute value of an intrinsic birefringence that is a fourth absolute value or less.
2. A method for producing an optical polymer material comprising the steps of:
20. 20. The method for producing an optical polymer material according to claim 19, characterized in that the copolymer is formed by mixing a material that becomes a maleimide derivative in a larger amount than a material that becomes a styrene derivative.
21. The third absolute value is 50×10 -12 P -1 and the fourth absolute value is 20×10 -3 21. The method for producing an optical polymer material according to claim 19, wherein
22. In a two-dimensional birefringence map defined by the intrinsic birefringence and the photoelastic coefficient, a composition ratio of the styrene derivative and a composition ratio of the maleimide derivative are set so that a coordinate point indicated by a first photoelastic coefficient and a first intrinsic birefringence determined by the composition ratio of the styrene derivative and the composition ratio of the maleimide derivative, and a coordinate point indicated by a second photoelastic coefficient and a second intrinsic birefringence of the modified organic compound are located on either side of the origin; A composition ratio of the modified organic compound is set so as to offset the first photoelastic coefficient and the first intrinsic birefringence. The method for producing the optical polymer material according to any one of claims 18 to 21.
23. A method for producing an optical film, comprising forming an optical polymer material produced by the method according to any one of claims 16 to 22 into a thin film to produce an optical film.
Citation Information
Patent Citations
Polarizing plate with optical compensation layer, liquid crystal panel using polarizing plate with optical compensation layer, and image display unit
EP1930750A1
Polymer composition and manufacture
JP1986028540A
Alternating copolymer hydroxystyrene and maleimide and production thereof
JP1986218607A
Preparation of aromatic vinyl resin molding
JP1989079208A
Optical element
JP1994242301A