Curable resin composition, dry film, cured product, and printed wiring board

A curable resin composition with controlled particle size and surface area, along with specific additives, addresses film thickness variations and copper visibility in printed wiring boards, enhancing manufacturing efficiency and appearance.

JP2024133135AInactive Publication Date: 2024-10-01TAIYO HOLDINGS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024110515
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-06-04
Filing Date
2024-07-09
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing curable resin compositions for printed wiring boards suffer from variations in film thickness and copper appearance issues, particularly when forming thin films, due to imbalances in component mixing, leading to poor appearance and increased manufacturing complexity.

Method used

A curable resin composition with controlled average particle diameter and specific surface area, combined with specific extender pigments and carboxyl group-containing resins, to stabilize film thickness and reduce gloss variations, preventing copper visibility.

Benefits of technology

The composition achieves consistent film thickness and reduced gloss, minimizing copper appearance issues and simplifying manufacturing processes by maintaining uniformity even in thin films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133135000001_ABST
    Figure 2024133135000001_ABST
Patent Text Reader

Abstract

To provide a curable resin composition which has small variations in film thickness of a coating film before drying and a coating film after drying even when a film is thin, and prevents an exposed-copper phenomenon.SOLUTION: A curable resin composition according to the invention contains a curable resin and an extender pigment, wherein 60° glossiness in a cured coating film having a film thickness after curing of 12 μm of the curable resin composition is within a range of 0.5 or more and 40.0 or less, when 0.3 g of the curable resin composition and 30 g of propylene glycol monomethyl ether acetate are mixed, and the mixture is measured using microtrac, an average particle diameter D50 is 0.1 μm or more and 1.0 μm or less, and a specific surface CS is 10.0 m2 / ml or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition. The present invention further relates to a dry film, a cured product, and a printed wiring board using the curable resin composition. [Background technology]

[0002] At present, from the viewpoint of achieving high precision and high density, liquid alkali-developable solder resist ink is used for most solder resists on printed wiring boards. Specifically, the ink is printed, the coating film after drying is exposed to light, developed to form an image, and then cured by heating to obtain the desired solder resist.

[0003] It is known that the solder resist layer is roughened to improve the solder adhesion resistance and wiring concealment during solder flow. In addition, the roughened solder resist layer has a moderately suppressed glossiness, so that a good design can be obtained. For example, Patent Document 1 proposes that the solder resist layer is roughened to reduce glossiness by adding a matting agent to a photosensitive resin composition.

[0004] Moreover, in recent years, from the viewpoint of improving yields during component mounting, the thickness of coating films after drying or hardening has become thinner (for example, Patent Document 2). In recent years, there has been a demand for stricter film thickness control for thinner films. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-157574 [Patent Document 2] JP 2004-264560 A Summary of the Invention [Problem to be solved by the invention]

[0006] Generally, extender pigments and resins are included in the curable resin composition for the purpose of reducing warping during component mounting and improving heat resistance. However, since a curable resin composition contains multiple components other than extender pigments and resins to meet various required properties, if the mixing state of each component is insufficient, concentration imbalance may occur in the curable resin composition. Therefore, the thickness of the coating film before drying (hereinafter also referred to as the coating film before drying) applied to a substrate or the like using the curable resin composition varies, and when it is thin, for example, there is a problem of poor appearance due to "copper visibility" in which the metal (copper) wiring of the substrate underneath is unevenly visible through the coating film. Furthermore, when the coating film after curing (hereinafter also referred to as the cured coating film) has low gloss, the problem of the above-mentioned poor appearance is more prominent in the coating film after curing. It is presumed that the lower the gloss of the coating film, the more contrast there is, and the gloss of the underlying metal (copper) wiring becomes more uneven and is more likely to be visible through the coating film.

[0007] If the film thickness of the coating film before drying is highly variable, there is a risk that the film thickness of the coating film after drying (hereinafter also referred to as the dried coating film) and the coating film after hardening will also be highly variable, so when using expensive substrates in particular, judging a product as NG based on the degree of variation in the film thickness of the coating film before drying and repairing the parts with variations could complicate the manufacturing process and reduce productivity. In this way, in addition to the small variation in the film thickness of the coating film after drying, there were cases where the small variation in the film thickness of the coating film before drying was also important.

[0008] Therefore, an object of the present invention is to provide a curable resin composition which has small variation in thickness of the pre-dry coating film or the dried coating film even when it is thin, and does not cause the copper appearance phenomenon. Another object of the present invention is to provide a dry film having a resin layer consisting of a dried coating film of the resin composition, a cured product of the resin composition or the resin layer of the dry film, and a printed wiring board having the cured product. [Means for solving the problem]

[0009] As a result of intensive research, the present inventors have found that in a curable resin composition containing a powder, particularly a body pigment, the value measured using a Microtrack is adjusted, specifically the average particle diameter D50 The inventors have found that by adjusting not only the value but also the specific surface area CS, the effect of the powder on the coating film surface before and after drying can be reduced, and as a result, a curable resin composition can be obtained in which the variation in thickness of the coating film before and after drying is small even in the case of a thin film, and no copper appearance phenomenon occurs, and have completed the present invention.

[0010] That is, according to the present invention, the following inventions are provided: [1] A curable resin composition containing a curable resin and an extender pigment, The 60° gloss of a cured coating film having a thickness of 12 μm after curing of the curable resin composition is in the range of 0.5 to 40.0, 0.3 g of the curable resin composition was mixed with 30 g of propylene glycol monomethyl ether acetate, and the average particle diameter D 50 is 0.1 μm or more and 1.0 μm or less, and the specific surface area CS is 10.0 m 2 / ml or more. [2] The curable resin composition according to [1], wherein the average spacing Sm of irregularities in the coating thickness of the curable resin composition after drying is in the range of more than 0 μm and not more than 12.0 μm. [3] The curable resin composition according to [1] or [2], wherein the maximum height Ry of the coating thickness after drying of the curable resin composition is in the range of more than 0 μm and not more than 8.0 μm. [4] The curable resin composition according to any one of [1] to [3], wherein the extender pigment is at least one of silica and barium sulfate. [5] The curable resin composition according to [4], wherein the body pigment further contains amorphous silica having an oil absorption of 180 to 350 ml / 100 g. [6] The curable resin composition according to any one of [1] to [5], wherein the curable resin contains a carboxyl group-containing resin. [7] The curable resin composition according to any one of [1] to [6], wherein the curable resin contains two or more types of carboxyl group-containing resins. [8] The curable resin composition according to [7], wherein at least one of the two or more types of carboxyl group-containing resins is a carboxyl group-containing copolymer resin. [9] A dry film comprising a support film and a resin layer formed on the support film and comprising a dried coating film of the curable resin composition according to any one of [1] to [8].

[10] A cured product obtained by curing the curable resin composition according to any one of [1] to [8] or the resin layer of the dry film according to [9].

[11] A printed wiring board comprising the cured product according to

[10] . Effect of the Invention

[0011] According to the present invention, there is provided a curable resin composition which has a small variation in thickness of the pre-dry coating film or the dried coating film even when it is thin, and does not cause the phenomenon of copper being visible. Also, according to the present invention, there can be provided a dry film having a resin layer made of a dried coating film of the resin composition, a cured product of the resin composition or the resin layer of the dry film, and a printed wiring board having the cured product. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is an explanatory diagram showing the measurement of the variation in the dried coating film by step analysis using a surface roughness measuring device in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Curable resin composition] The curable resin composition according to the present invention contains a curable resin and an extender pigment. The curable resin composition according to the present invention may further contain a photopolymerization initiator, a sensitizer, a heat curing catalyst, a colorant, etc., as long as it satisfies the following physical properties. The curable resin may contain any one of a thermosetting resin, a carboxyl group-containing resin, and a photopolymerizable monomer, or a combination of a plurality of types. By satisfying the following physical properties, the curable resin composition according to the present invention can obtain a coating film before and after drying that is less uneven and sagging during application and has small film thickness variations even when it is a thin film, and can obtain a cured coating film that does not cause a copper appearance phenomenon after curing. In the present invention, a thin film refers to a coating film that is usually 20 μm or less before drying and 12 μm or less after drying or curing.

[0014] [Physical Properties] The curable resin composition of the present invention has a 60° gloss of a 12 μm thick cured coating film after curing in the range of 0.5 to 40.0, preferably 0.8 to 35.0, more preferably 1.0 to 20.0, even more preferably 1.0 to 10.0, and particularly preferably 2.0 to 6.0. The glossiness can be measured in accordance with JIS Z 8741. A specific method for measuring the glossiness will be described. As a premise, on a surface with a refractive index of 1.067, the light intensity at a reflectance of 10% in the case of an incident angle of 60° is set to a glossiness of 100, and the light intensity at a reflectance of 0% is assumed to be 0. Thus, a value that is 1 / 100 of the light intensity at a reflectance of 10% corresponds to a glossiness of 1. Using a reflectometer with a geometric condition of an incident angle of 60°, the light intensity of the surface of the cured coating film provided on the substrate is measured. Then, the glossiness is calculated by dividing the obtained light intensity by the value that is 1 / 100 of the light intensity at the reflectance of 10%. Simply, a digital variable-angle glossmeter (Micro-Tri-Gloss, manufactured by BYK Gardener) can be used to measure the glossiness of the surface of the cured coating film provided on the substrate at each angle. It should be noted that "60° gloss (Gs(60°))" is the gloss value when the measurement conditions are an incident angle of 60° and a receiving angle of 60°.

[0015] The cured coating film in the present invention refers to a coating film obtained by curing a curable resin composition by at least one of photocuring and thermal curing. On the other hand, the dried coating film in the present invention refers to a coating film obtained by drying a curable resin composition by thermal drying. As a thermal drying method, the coating film is printed by screen printing on a 300 mm×150 mm copper foil substrate having a thickness of 35 μm, the surface of which has been buff-rolled, so that the film thickness after drying is 12 μm, and then thermally dried using a hot air circulation drying oven. As a printing plate for screen printing, it is preferable to use a 100-200 mesh polyester plate (with bias), and it is more preferable to use a 150-180 mesh polyester plate (with bias), from the viewpoint of film thickness adjustment. As drying conditions, for example, a temperature of 60 to 100° C. is used for 15 to 90 minutes. In addition, as an apparatus, DF610 manufactured by Yamato Scientific Co., Ltd. is exemplified.

[0016] On the other hand, in the photocuring method, the dried coating film formed as described above is irradiated with active energy rays, specifically, photocured by a UV conveyor using a high-pressure mercury lamp. The irradiation dose is, for example, 1,000 to 2,000 mJ / cm. 2 Examples of the apparatus include QRM-2082 manufactured by Oak Manufacturing Co., Ltd.

[0017] As a thermal curing method, the composition is screen printed on a 300 mm x 150 mm copper foil substrate with a thickness of 35 μm, the surface of which has been buff-roll polished, so that the film thickness after curing is 12 μm, and then thermally cured using a hot air circulation drying oven. As a printing plate for screen printing, it is preferable to use a 100-200 mesh polyester plate (with bias), and it is more preferable to use a 150-180 mesh polyester plate (with bias), from the viewpoint of film thickness adjustment. As a thermal curing condition, for example, a temperature of 100 to 220°C is used for 30 to 90 minutes.

[0018] An example of a drying device used for drying and heat curing is DF610 manufactured by Yamato Scientific Co., Ltd. In the present invention, when measuring the gloss level, the measurement is performed using a cured coating film formed without carrying out a development step.

[0019] In addition, the method of confirming whether or not a cured coating film has been formed in the present invention can be as follows. That is, in an environment of 25°C and 50% RH, a cloth soaked in isopropyl alcohol (IPA) is placed on the surface of the cured coating film, and a weight of 500 g is placed on the cloth and left to stand for 1 minute, and then the cloth is peeled off. The state in which all or part of the resin layer does not adhere to the surface of the cloth that was in contact with the cured coating film is judged to be a "cured state", that is, a cured coating film has been formed. On the other hand, the method of confirming whether or not a dry coating film has been formed in the present invention is judged to be a "dry state", that is, a dry coating film has been formed, when the applied surface of the curable resin composition is touched with a finger and the curable resin composition does not adhere to the finger.

[0020] The curable resin composition of the present invention has an average particle diameter D 50 In order to further suppress the copper appearance phenomenon, the value of is preferably 0.1 μm or more and 0.8 μm or less, and more preferably 0.1 μm or more and 0.5 μm or less. The curable resin composition of the present invention has a specific surface area CS of 10.0 m 2 / ml or more, and while having a lower gloss, it is preferable to use a coating having a thickness of 11.5 ml or more in order to reduce the variation in thickness of the coating film before and after drying even when it is thin, and to suppress the copper appearance phenomenon. 2 / ml or more 30.0m 2 / ml or less, more preferably 13.0m 2 / ml or more 25.0m 2 / ml or less.

[0021] Average particle diameter D of the curable resin composition 50 The value of is 0.1 μm or more and 1.0 μm or less, and the specific surface area CS is 10.0 m 2 / ml or more, the variation in the thickness of the coating film before and after drying can be reduced even in the case of a thin film, and the copper appearance phenomenon can be suppressed. Although this is not entirely clear, it is speculated as follows. That is, by having a specific surface area CS within the above range, the powder contained in the composition maintains a high dispersion state, and as a result, even when forming a thin film using the composition, no sagging occurs, and the effect of the powder contained therein on the surface of the coating film before and after drying is small, and as a result, it is thought that the copper appearance phenomenon can be suppressed even in a low-gloss thin film. However, this is merely speculation and is not necessarily limited to this.

[0022] In the present invention, the average particle diameter D of the curable resin composition 50 In the above, the powder such as the extender pigment contained in the composition is assumed to be a single powder mass, and its particle size distribution is sought. In other words, when a cumulative curve is obtained with the total volume of the assumed single powder mass taken as 100%, the particle size at the point where the cumulative curve is 50% is taken as the 50% diameter (μm), and the average particle diameter D 50 On the other hand, the specific surface area CS is the surface area per unit volume when the particle shape in the composition is assumed to be spherical. 50 and specific surface area CS are calculated by the following measurements. 2 / ml) is the specific surface area (m2) measured by the BET method or other surface area measuring device. 2 / g) has a different meaning. First, prepare the following equipment and supplies. Particle size distribution meter: Nikkiso Microtrac MT3300EX Circulation device: ASVR manufactured by Nikkiso Co., Ltd. Next, enter the measurement conditions using the following procedure. Start the software that comes with the Microtrac ("Particle Size Distribution Measurement"), proceed from the SET UP screen, and set the time from the measurement condition setting options. Set the Set Zero time to 30 sec., the measurement to 30 sec., and the number of measurements to 2. Next, enter the analysis conditions. In the analysis information, set the particle refractive index to 1.81 (fixed value: average value of the refractive index of all inorganic substances), the particle characteristics to transparent, and the shape to non-spherical. In the solvent information, select PMA (propylene glycol monomethyl ether acetate) and set the solvent refractive index to 1.4. Next, enter the scale settings. In the particle size range, set the minimum particle size to 0.021 μm and the maximum particle size to 704 μm. Next, enter the sampling system. Set the number of ASVR cleanings to 4, the flow rate to 50%, the ultrasonic output to 40 W, and the ultrasonic time to 300 sec. After entering all the measurement conditions, click Save in the measurement condition settings to close. Next, the sample is adjusted according to the following procedure. 0.3 g of the sample (curable resin composition) is weighed out and placed in a screw bottle, 30 g of propylene glycol monomethyl ether acetate is gradually added using a dropper, and the screw bottle is shaken to dissolve the sample to prepare an adjusted sample. The adjusted sample is not subjected to external dispersion or pre-dispersion. Next, the adjusted sample is measured. Click on particle size distribution measurement in the software attached to the Microtrack to open the sample loading screen. Using a dropper, drip a few drops of the adjusted sample into the sample inlet of the main unit. When a red indication bar is displayed on the sample loading screen, drip the adjusted sample into the sample inlet until it is within the range from red to green. When it is within the green range, press the measurement button to start measurement. The process from sample adjustment to measurement of the adjusted sample is performed within 5 minutes. The cumulative average diameter 50% value and the area average diameter MA value displayed as the measurement results are read. The cumulative average diameter 50% value is used to measure the average particle diameter D measured with the Microtrack. 50 The value is taken as the specific surface area measured by the Microtrac. Also, calculate CS = 6 / MA. The calculated CS value is taken as the specific surface area measured by the Microtrac. The MA is calculated using the following formula. MA = Σ(ai d i ) / Σ(a i )=Σ(v i ) / Σ(v i / d i ) (a i : surface area per particle, d i : Particle diameter per particle, v i : volume per particle)

[0023] Average particle diameter D of the curable resin composition 50 The value of is 0.1 μm or more and 1.0 μm or less, and the specific surface area CS is 10.0 m 2 To achieve a concentration of 1 / ml or more, known and commonly used techniques can be applied, for example, by optimizing the selection of components in the composition and their amounts, and the method for dispersing powders, resins, etc. in the composition.

[0024] The curable resin composition of the present invention has an average spacing Sm of irregularities in the coating thickness after drying that is preferably in the range of more than 0 μm and not more than 12.0 μm, more preferably in the range of 1.0 μm or more and 11.0 μm or less, and even more preferably in the range of 2.0 μm or more and 8.0 μm or less. The curable resin composition of the present invention has a maximum coating thickness Ry after drying that is preferably in the range of more than 0 μm and not more than 8.0 μm, more preferably in the range of 0.1 μm or more and 6.5 μm or less, and even more preferably in the range of 0.2 μm or more and 2.5 μm or less. If the average interval Sm and maximum height Ry of the unevenness of the coating film thickness after drying of the curable resin composition are within the above numerical range, the variation in the film thickness will be smaller. This is not necessarily clear, but is thought to be as follows. That is, the surface state of the dried coating film is stable because the average interval and maximum height of the unevenness of the coating film thickness are constant, and as a result, the cured coating film has low gloss, but the variation is small even when it is thin, and the copper appearance phenomenon is suppressed. Note that the measurement of the average interval Sm and maximum height Ry of the unevenness of the coating film thickness in the present invention is performed after drying and leaving it at room temperature for 30 minutes.

[0025] In the present invention, the above-mentioned "average spacing Sm of irregularities" and "maximum height Ry" respectively refer to values ​​measured by a measuring device conforming to JIS B0601-1994. A specific measurement method will be described below. The average spacing Sm of irregularities and the maximum height Ry can be measured using a shape measuring laser microscope (for example, VK-X100 manufactured by Keyence Corporation). After starting the shape measuring laser microscope (VK-X100) main body (control unit) and the VK observation application (VK-H1VX manufactured by Keyence Corporation), the sample to be measured (dried coating film formed on a substrate or the like) is placed on the xy stage. Rotate the lens revolver of the microscope unit (VK-X110 manufactured by Keyence Corporation) to select an objective lens with a magnification of 10 times, and roughly adjust the focus and brightness in the image observation mode of the VK observation application (VK-H1VX manufactured by Keyence Corporation). Operate the xy stage to adjust so that the part of the sample surface to be measured is at the center of the screen. Change the 10x objective lens to a 50x magnification, and use the autofocus function in the image observation mode of the VK observation application (VK-H1VX) to focus on the surface of the sample. Select the easy mode in the shape measurement tab of the VK observation application (VK-H1VX), press the measurement start button, measure the surface shape of the sample, and obtain a surface image file. Start the VK analysis application (VK-H1XA, Keyence Corporation), display the obtained surface image file, and then perform tilt correction. The observation measurement range (horizontal) in measuring the surface shape of the sample is 270 μm. After displaying the line roughness window and selecting JIS B0601-1994 in the parameter setting area, select horizontal line from the measurement line button, display the horizontal line anywhere in the surface image, and press the OK button to obtain the average spacing Sm (μm) and maximum height Ry (μm) of the uneven surface. Furthermore, horizontal lines are displayed at four different locations in the surface image, and the average spacing Sm (μm) and maximum height Ry (μm) of each of the uneven surfaces are obtained. The average of the five values ​​obtained is calculated to obtain the average spacing Sm value and maximum height Ry value of the uneven surface of the sample surface. In addition, the Sm and Ry values ​​of the dried coating film are not affected by the type of substrate because the substrate surface is generally sufficiently smooth compared to the surface of the cured coating film. The substrate may be any known or commonly used one, but it is preferable to use a glass substrate.

[0026] In order to set the coating thickness of the curable resin composition after drying within the above-mentioned specific range of the average spacing Sm of the irregularities and the maximum height Ry, known and commonly used methods can be applied, such as optimizing the selection of the organic solvent and other components in the composition, the blending amount thereof, the dispersion method, or a combination of the above-mentioned methods. In addition, in order to set the 60° gloss of the curable resin composition in a 12 μm-thick cured coating film within a specific range, known and commonly used methods can be applied, such as adding an extender pigment with a coarse average particle size, or mixing multiple resins with poor compatibility.

[0027] Hereinafter, each component constituting the curable resin composition according to the present invention will be described.

[0028] [Curable resin] Examples of the curable resin include a thermosetting resin that contributes to a thermosetting reaction when heated, a photocurable resin that contributes to a photocuring reaction when irradiated with light, and a photocurable thermosetting resin that contributes to both of these reactions. Here, the curable resin preferably contains a thermosetting resin and a photocurable resin, and when both curable resins are contained, the thermosetting resin more preferably contains a carboxyl group-containing resin and a compound having a plurality of cyclic ether groups or cyclic thioether groups in the molecule.

[0029] The amount of the curable resin is preferably 20 to 80 mass %, more preferably 25 to 75 mass %, and further preferably 50 to 70 mass %, calculated as the solid content based on the total amount of the curable resin composition. By setting the amount of the curable resin within the above range, a better cured product can be obtained. Each curable resin will be described below.

[0030] [Thermosetting resin] Any known thermosetting resin can be used as the thermosetting resin. The curable resin composition contains a thermosetting resin, thereby improving the heat resistance of the cured coating film. As the thermosetting resin, for example, known thermosetting resins such as amino resins such as melamine resins, benzoguanamine resins, melamine derivatives, and benzoguanamine derivatives, isocyanate compounds, blocked isocyanate compounds, cyclocarbonate compounds, epoxy compounds, oxetane compounds, episulfide resins, bismaleimide, and carbodiimide resins can be used. Particularly preferred is a thermosetting resin having a plurality of cyclic ether groups or cyclic thioether groups (hereinafter abbreviated as cyclic (thio)ether groups) in the molecule. The thermosetting resin can be used alone or in combination of two or more types.

[0031] The thermosetting resin having a plurality of cyclic (thio)ether groups in the molecule is a compound having a plurality of 3-, 4-, or 5-membered cyclic (thio)ether groups in the molecule, and examples thereof include a compound having a plurality of epoxy groups in the molecule, i.e., a polyfunctional epoxy compound, a compound having a plurality of oxetanyl groups in the molecule, i.e., a polyfunctional oxetane compound, and a compound having a plurality of thioether groups in the molecule, i.e., an episulfide resin.

[0032] Examples of such epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, and the like.

[0033] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation; YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd.; EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation; and RE-306 manufactured by Nippon Kayaku Co., Ltd.

[0034] Examples of the polyfunctional oxetane compound include bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, and (3-ethyl-3-oxetanyl)methyl acrylate. Examples of the oxetanes include polyfunctional oxetanes such as acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and their oligomers or copolymers, as well as ethers of oxetane alcohols and novolac resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or resins having hydroxyl groups such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates.

[0035] Examples of compounds having multiple cyclic thioether groups in the molecule include bisphenol A episulfide resins, etc. Using a similar synthesis method, episulfide resins in which the oxygen atoms of the epoxy groups of novolac epoxy resins are replaced with sulfur atoms can also be used.

[0036] Examples of amino resins such as melamine derivatives and benzoguanamine derivatives include methylolmelamine compounds, methylolbenzoguanamine compounds, methylolglycoluril compounds, and methylolurea compounds.

[0037] The isocyanate compound may be a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate, o-xylylene diisocyanate, m-xylylene diisocyanate and 2,4-tolylene dimer; aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate) and isophorone diisocyanate; alicyclic polyisocyanates such as bicycloheptane triisocyanate; and adducts, biuret and isocyanurates of the above-mentioned isocyanate compounds.

[0038] The blocked isocyanate compound may be an addition reaction product of an isocyanate compound and an isocyanate blocking agent. Examples of isocyanate compounds that can react with an isocyanate blocking agent include the polyisocyanate compounds described above. Examples of isocyanate blocking agents include phenol-based blocking agents, lactam-based blocking agents, active methylene-based blocking agents, alcohol-based blocking agents, oxime-based blocking agents, mercaptan-based blocking agents, acid amide-based blocking agents, imide-based blocking agents, amine-based blocking agents, imidazole-based blocking agents, and imine-based blocking agents.

[0039] When the composition contains a carboxyl group-containing resin described later, the amount of the thermosetting resin to be added is preferably such that the number of functional groups in the thermosetting component to react with 1 mol of carboxyl groups contained in the carboxyl group-containing resin is 0.5 to 2.5 mol, and more preferably 0.8 to 2.0 mol.

[0040] The thermosetting component preferably contains an alkali-soluble resin having an alkali-soluble group, in that it can impart alkali developability to the composition. Examples of the alkali-soluble resin include a compound having two or more phenolic hydroxyl groups, a carboxyl group-containing resin, a compound having a phenolic hydroxyl group and a carboxyl group, and a compound having two or more thiol groups. Among them, a carboxyl group-containing resin or a phenolic resin is preferable because it improves adhesion to the base, and a carboxyl group-containing resin is more preferable because it is particularly excellent in developability. The carboxyl group-containing resin will be described below.

[0041] [Carboxyl group-containing resin] As the carboxyl group-containing resin, various conventionally known resins having a carboxyl group in the molecule can be used. The carboxyl group-containing resin may or may not have an ethylenically unsaturated double bond in the molecule, but in particular, a carboxyl group-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is preferable from the viewpoint of photocurability and development resistance. In such a case, it corresponds to a photocurable thermosetting resin. In addition, when the curable composition of the present invention contains a carboxyl group-containing resin, it may be used not only for applications in which alkaline development is performed, but also for applications in which alkaline development is not performed. The ethylenically unsaturated double bond is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. When only a carboxyl group-containing resin without an ethylenically unsaturated double bond is used, in order to make the composition photocurable, it is necessary to use a compound having a plurality of ethylenically unsaturated groups in the molecule, i.e., a photopolymerizable monomer, which will be described later. Specific examples of the carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers).

[0042] (1) Carboxyl group-containing resins obtained by copolymerizing unsaturated carboxylic acids such as (meth)acrylic acid with unsaturated group-containing compounds such as styrene, α-methylstyrene, lower alkyl (meth)acrylates, and isobutylene (lower alkyl (meth)acrylates include methyl (meth)acrylate, etc.).

[0043] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0044] (3) Carboxylic acid-containing photosensitive urethane resins obtained by the polyaddition reaction of diisocyanates with (meth)acrylates of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins, and biphenol type epoxy resins, or their partial acid anhydride modified products, carboxyl group-containing dialcohol compounds, and diol compounds.

[0045] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).

[0046] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).

[0047] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.

[0048] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0049] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0050] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.

[0051] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0052] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0053] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).

[0054] Among these, it is preferable that the curable resin contains two or more kinds of carboxyl group-containing resins. Furthermore, it is preferable that at least one of the two or more kinds of carboxyl group-containing resins is a carboxyl group-containing copolymer resin, in terms of being more uniformly dispersed while lowering the gloss. This is presumed as follows. That is, since the carboxyl group-containing copolymer resin has poor compatibility, it forms a sea-island structure dispersed in other carboxyl group-containing resins in the coating film formed from the curable resin composition, and it is considered that the difference in refractive index between them causes diffuse reflection of incident light, resulting in an excellent effect of low gloss. On the other hand, in the case of adding a carboxyl group-containing copolymer resin, even if the amount of the extender pigment is small, it is possible to disperse the resin uniformly while lowering the gloss, and therefore the copper appearance phenomenon is more suppressed.

[0055] Examples of the carboxyl group-containing copolymer resin include the resin of (1) and the copolymer resin of (12). The resin of (12) is preferably a carboxyl group-containing photosensitive resin obtained by further adding a (meth)acrylate having an alicyclic epoxy group, such as glycidyl methacrylate or 3,4-epoxycyclohexylmethyl (meth)acrylate, to a carboxyl group-containing resin obtained by copolymerizing (meth)acrylic acid and methyl (meth)acrylate. In addition, the resin to be combined with the carboxyl group-containing copolymer resin is preferable in that it is uniformly dispersed while lowering the gloss. A combination with a resin other than the carboxyl group-containing copolymer resin is preferable. Specifically, the resins (2) to (11) and the resin (12) other than the copolymer resin are mentioned, and among them, the resins (6), (10), and (11) and the resin (12) other than the copolymer resin are more preferable.

[0056] In this specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.

[0057] The carboxyl group-containing resins that can be used in the present invention are not limited to those listed above. The carboxyl group-containing resins listed above may be used alone or in combination.

[0058] In the present invention, in consideration of the developability and drawing ability of the resist pattern when using a weak alkaline developer such as an aqueous sodium carbonate solution, the acid value of the carboxyl group-containing resin is preferably in the range of 30 to 150 mgKOH / g, more preferably in the range of 50 to 120 mgKOH / g. The higher the acid value of the carboxyl group-containing resin, the better the developability, but the exposed area is more likely to be dissolved by the developer, and the exposed area may be dissolved and peeled off by the developer without distinction between the exposed area and the unexposed area.

[0059] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally in the range of 2,000 to 150,000, preferably in the range of 5,000 to 100,000. By using a carboxyl group-containing resin having a weight average molecular weight of 2,000 or more, it is possible to improve resolution and tack-free performance. In addition, by using a carboxyl group-containing resin having a weight average molecular weight of 150,000 or less, it is possible to improve developability and storage stability. The weight average molecular weight can be measured by gel permeation chromatography (GPC).

[0060] The amount of the carboxyl group-containing resin is preferably 20 to 80 mass %, more preferably 20 to 75 mass %, and even more preferably 20 to 50 mass %, calculated as solid content based on the total amount of the curable resin composition. By making it 20 mass % or more, the strength of the cured coating film can be improved. Also, by making it 80 mass % or less, the viscosity of the curable resin composition becomes appropriate, and the processability is improved.

[0061] Furthermore, when the carboxyl group-containing resin contains a carboxyl group-containing copolymer resin, the blending amount of the carboxyl group-containing copolymer resin, calculated as the solid content, relative to 100 parts by mass of the carboxyl group-containing resin, is preferably 5 to 90% by mass, more preferably 10 to 70% by mass, and still more preferably 15 to 50% by mass, in terms of suppressing copper appearance while further reducing gloss.

[0062] [Photocurable resin] The photocurable resin is a compound having an ethylenically unsaturated group, and may be a polymer, an oligomer, a monomer, or a mixture thereof. By including the photocurable resin, the strength of the cured film can be improved. The photocurable resin can be used alone or in combination of two or more kinds.

[0063] As the compound having an ethylenically unsaturated group, a known and commonly used photopolymerizable oligomer, photopolymerizable monomer, etc. can be used. Among these, it is preferable to use a photopolymerizable monomer, since it can impart more crosslinking property and curing property to the cured coating film.

[0064] The photopolymerizable oligomer is an oligomer having an ethylenically unsaturated double bond. Examples of the photopolymerizable oligomer include unsaturated polyester oligomers and (meth)acrylate oligomers. Examples of the (meth)acrylate oligomer include epoxy (meth)acrylates such as phenol novolac epoxy (meth)acrylate, cresol novolac epoxy (meth)acrylate, and bisphenol type epoxy (meth)acrylate, urethane (meth)acrylate, epoxy urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, and polybutadiene modified (meth)acrylate.

[0065] The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include alkyl (meth)acrylates such as 2-ethylhexyl (meth)acrylate and cyclohexyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; mono- or di(meth)acrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and the like. Examples of the photopolymerizable monomer include polyhydric alcohols such as tris(hydroxyethyl)isocyanurate and the like, polyhydric (meth)acrylates of their ethylene oxide or propylene oxide adducts, (meth)acrylates of ethylene oxide or propylene oxide adducts of phenols such as phenoxyethyl (meth)acrylate and polyethoxy di(meth)acrylate of bisphenol A, (meth)acrylates of glycidyl ethers such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether and triglycidyl isocyanurate, and melamine (meth)acrylate. One type of photopolymerizable monomer may be used alone, or two or more types may be used in combination.

[0066] The amount of the photocurable resin is preferably 3 to 20 mass %, more preferably 5 to 15 mass %, calculated as solid content based on the total amount of the curable resin composition. When the amount of the photopolymerizable monomer is 3 mass % or more, the photocurability is good and pattern formation is easy in alkaline development after irradiation with active energy rays. On the other hand, when the amount is 20 mass % or less, halation is unlikely to occur and good resolution is easily obtained.

[0067] [Extender pigment] The extender pigment of the present invention refers to a pigment having a refractive index of 1.40 or more, and examples thereof include silica such as amorphous silica, crystalline silica, fused silica, and spherical silica, talc, boehmite, hydrotalcite, slaked lime, calcium hydroxide, calcium carbonate, calcium sulfate, potassium carbonate, magnesium carbonate, clay, mica powder, aluminum oxide, aluminum hydroxide, barium sulfate, copper sulfide, alumina, zinc oxide, iron, zinc sulfide, zirconium oxide, chromium oxide, cadmium oxide, cadmium sulfide, titanium oxide, and copper oxide. Among these, silica and barium sulfate are preferred from the viewpoint of dispersibility. The extender pigment may be used alone or in combination of two or more kinds. By including the extender pigment, it is possible to improve heat resistance and reduce unevenness during application. In addition, from the viewpoint of further reducing gloss, aluminum silicate mainly composed of SiO2 and Al2O3 may be used.

[0068] The surface treatment of the extender pigment is not particularly limited, but the extender pigment may be surface-treated to enhance dispersibility. By using a surface-treated extender pigment, aggregation can be suppressed. The surface treatment method of the extender pigment is not particularly limited, and a publicly known and commonly used method may be used, but it is preferable to treat the surface of the inorganic extender pigment with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.

[0069] The average particle size of the extender pigment is preferably 10 μm or less, but from the viewpoint of dispersibility, it is more preferably 0.1 to 2.0 μm, even more preferably 0.15 to 1.0 μm, and particularly preferably 0.2 to 0.9 μm, except for amorphous silica, which will be described later. The average particle size of the extender pigment refers to the average particle size (D 50 ) and D measured by laser diffraction method 50 The value is 0.01 mm. The measurement device using the laser diffraction method is Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd. 100 ) and particle size (D 10) can also be measured in the same manner using the above-mentioned device. The particle size values ​​of the above-mentioned body pigments refer to values ​​measured as described above for the body pigments before the curable resin composition is prepared (preliminary mixing, kneading).

[0070] The amount of the extender pigment is preferably 20 to 80 mass %, more preferably 25 to 75 mass %, and even more preferably 30 to 50 mass %, calculated as solid content based on the total amount of the curable resin composition. By keeping the amount of the extender pigment within the above range, the cured product can have high strength.

[0071] In the curable resin composition of the present invention, the silica preferably contains amorphous silica having an oil absorption of 180 to 350 ml / 100 g, in order to provide a cured coating film with a lower gloss. The reason why the use of the amorphous silica provides a cured coating film with a lower gloss is presumed to be as follows. That is, it is presumed that amorphous silica having an oil absorption within a predetermined range is porous, and the amorphous silica and other extender pigments become denser due to the absorption of oil from organic solvents and the like during curing and drying, resulting in a lower gloss of the cured coating film. It is more preferable that the oil absorption is 200 to 300 ml / 100 g. In the present invention, the oil absorption refers to the value measured in accordance with "JIS K5101-13-1:2004 Pigment Testing Methods - Part 13: Oil Absorption - Section 1: Refined Linseed Oil Method".

[0072] The amorphous silica may be a known, commonly used one, and may be synthetic or natural. It may be surface-treated or not. The type of surface treatment is the same as that of the extender pigment. Examples of the product include ACEMATT 82, ACEMATT 790, ACEMATT OK 412, and ACEMATT OK 500 (all manufactured by EVONIK DEGUSSA).

[0073] The average particle size of the amorphous silica is preferably 3 to 10 μm, more preferably 4 to 8 μm, since the cured coating film has a lower gloss. The average particle size in this paragraph is measured before kneading into the curable resin composition. The method for measuring the average particle size is the same as that for the extender pigment.

[0074] When the extender pigment contains the amorphous silica, the amount of amorphous silica blended is preferably 5 to 90 parts by mass, more preferably 10 to 70 parts by mass, and even more preferably 12 to 50 parts by mass, per 100 parts by mass of the extender pigment, calculated as solid content, in order to provide a cured coating film with a lower gloss and uniform dispersion. When the extender pigment contains the amorphous silica and another extender pigment, barium sulfate is preferred in order to provide a cured coating film with a lower gloss and uniform dispersion.

[0075] The curable resin composition of the present invention may contain the following optional components.

[0076] [Photopolymerization initiator] The photopolymerization initiator is for reacting the carboxyl group-containing resin or the photopolymerizable monomer by exposure to light. Any known photopolymerization initiator can be used. The photopolymerization initiator may be used alone or in combination of two or more.

[0077] Specific examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentane. Bisacylphosphine oxides such as 2,6-dimethoxybenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloyl monoacylphosphine oxides such as phenylphosphinic acid isopropyl ester and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, and other benzoins; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, and other benzophenones;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone acetophenones such as acetophenone, N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, Anthraquinones such as 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetylacetone) oxime esters such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium, and other titanocenes; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, tetramethylthiuram disulfide, and the like.

[0078] Commercially available α-aminoacetophenone photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins. Commercially available acylphosphine oxide photopolymerization initiators include Omnirad TPO and 819 manufactured by IGM Resins. Commercially available oxime ester photopolymerization initiators include Irgacure OXE01 and OXE02 manufactured by BASF Japan Ltd., N-1919 manufactured by ADEKA Corporation, ADEKA Arcles NCI-831 and NCI-831E, and TR-PBG-304 manufactured by Changzhou Strong Electronic New Materials Co., Ltd.

[0079] Other examples include carbazole oxime ester compounds described in JP-A-2004-359639, JP-A-2005-097141, JP-A-2005-220097, JP-A-2006-160634, JP-A-2008-094770, JP-T-2008-509967, JP-T-2009-040762, and JP-T-2011-80036.

[0080] The amount of the photopolymerization initiator is preferably 0.1 to 10 mass %, more preferably 1 to 5 mass %, calculated as solid content based on the total amount of the curable resin composition. When the amount of the photopolymerization initiator is 0.1 mass % or more, the photocurability of the curable resin composition is good, and the coating film properties such as chemical resistance are also good. On the other hand, when the amount is 10 mass % or less, the light absorption at the surface of the resist film (cured coating film) is good, and the deep curability is less likely to decrease.

[0081] A photoinitiator assistant or a sensitizer may be used in combination with the above-mentioned photopolymerization initiator. Examples of the photoinitiator assistant or sensitizer include benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. In particular, it is preferable to use thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 4-isopropylthioxanthone. By including a thioxanthone compound, it is possible to improve the deep curing property. Although these compounds may be used as photopolymerization initiators, it is preferable to use them in combination with a photopolymerization initiator. In addition, the photoinitiator assistant or sensitizer may be used alone or in combination of two or more kinds.

[0082] In addition, since these photopolymerization initiators, photoinitiator assistants, and sensitizers absorb specific wavelengths, in some cases the sensitivity is reduced and they may function as ultraviolet absorbers. However, they are not used only for the purpose of improving the sensitivity of the resin composition. If necessary, they can absorb light of a specific wavelength to increase the photoreactivity of the surface, change the line shape and opening of the resist pattern to a vertical, tapered, or reverse tapered shape, and improve the accuracy of the line width and opening diameter.

[0083] [Thermosetting catalyst] The curable resin composition of the present invention may contain a heat curing catalyst. Examples of the heat curing catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. In addition, examples of commercially available products include 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (a trade name of a dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and their salts) manufactured by San-Apro Co., Ltd. In particular, the present invention is not limited to these, and any material that promotes the reaction of at least one of an epoxy resin or oxetane compound with a carboxyl group and at least one of an epoxy group and an oxetanyl group with a carboxyl group may be used alone or in combination of two or more types.

[0084] Furthermore, S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct can also be used, and preferably these compounds that also function as adhesion promoters are used in combination with the heat curing catalyst. The heat curing catalyst may be used alone or in combination of two or more types.

[0085] The amount of the thermosetting catalyst is preferably 0.1 to 5 parts by mass, and more preferably 1 to 3 parts by mass, calculated as the solid content based on the total amount of the curable resin composition.

[0086] [Coloring agent] A colorant can be blended in the curable resin composition of the present invention. The colorant is not particularly limited, and known colorants such as red, blue, green, and yellow can be used. Any of pigments, dyes, and coloring matters can be used, but from the viewpoint of reducing the environmental load and having little effect on the human body, it is preferable that the colorant does not contain halogen.

[0087] Red colorants include monoazos, disazos, azo lakes, benzimidazolone, perylene, diketopyrrolopyrrole, condensed azos, anthraquinones, and quinacridones. Specific examples of red colorants include those having the following Color Index (CI; published by The Society of Dyers and Colourists) numbers:

[0088] Examples of monoazo red colorants include Pigment Red 1, 2, 3, 4, 5, 6, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 112, 114, 146, 147, 151, 170, 184, 187, 188, 193, 210, 245, 253, 258, 266, 267, 268, and 269. Examples of disazo red colorants include Pigment Red 37, 38, and 41. Examples of monoazo lake-based red colorants include Pigment Red 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 52:2, 53:1, 53:2, 57:1, 58:4, 63:1, 63:2, 64:1, and 68. Examples of benzimidazolone-based red colorants include Pigment Red 171, 175, 176, 185, and 208. Examples of perylene-based red colorants include Solvent Red 135, 179, Pigment Red 123, 149, 166, 178, 179, 190, 194, and 224. Examples of diketopyrrolopyrrole red colorants include Pigment Red 254, 255, 264, 270, and 272. Examples of condensed azo red colorants include Pigment Red 220, 144, 166, 214, 220, 221, and 242. Examples of anthraquinone red colorants include Pigment Red 168, 177, and 216, Solvent Red 149, 150, 52, and 207. Examples of quinacridone red colorants include Pigment Red 122, 202, 206, 207, and 209.

[0089] Blue colorants include phthalocyanine and anthraquinone types, and pigment types include compounds classified as pigments, such as Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, and 60. Dye types include Solvent Blue 35, 63, 68, 70, 83, 87, 94, 97, 122, 136, 67, and 70. In addition to the above, metal-substituted or unsubstituted phthalocyanine compounds can also be used.

[0090] Examples of yellow colorants include monoazo, disazo, condensed azo, benzimidazolone, isoindolinone, and anthraquinone. For example, anthraquinone yellow colorants include Solvent Yellow 163, Pigment Yellow 24, 108, 193, 147, 199, and 202. Examples of isoindolinone yellow colorants include Pigment Yellow 110, 109, 139, 179, and 185. Examples of condensed azo yellow colorants include Pigment Yellow 93, 94, 95, 128, 155, 166, and 180. Examples of benzimidazolone yellow colorants include Pigment Yellow 120, 151, 154, 156, 175, and 181. Examples of monoazo yellow colorants include Pigment Yellow 1, 2, 3, 4, 5, 6, 9, 10, 12, 61, 62, 62:1, 65, 73, 74, 75, 97, 100, 104, 105, 111, 116, 167, 168, 169, 182, and 183. Examples of disazo yellow colorants include Pigment Yellow 12, 13, 14, 16, 17, 55, 63, 81, 83, 87, 126, 127, 152, 170, 172, 174, 176, 188, and 198.

[0091] In addition, colorants such as purple, orange, brown, and black may be added. Specific examples include Pigment Black 1, 6, 7, 8, 9, 10, 11, 12, 13, 18, 20, 25, 26, 28, 29, 30, 31, and 32, Pigment Violet 19, 23, 29, 32, 36, 38, and 42, Solvent Violet 13 and 36, CI Pigment Orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, and 73, Pigment Brown 23 and 25, and carbon black.

[0092] The blending amount of the colorant is preferably 0.1 to 2.0 mass %, more preferably 0.3 to 1.5 mass %, calculated as solid content based on the total amount of the curable resin composition.

[0093] [Organic solvents] The curable resin composition of the present invention may contain an organic solvent for the purpose of adjusting the viscosity when preparing the composition or when applying it to a substrate or film. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, diethylene glycol monoethyl ether acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. Among these, when the curable resin composition of the present invention uses a porous material such as amorphous silica, the silica surface is likely to absorb oil during curing and drying, resulting in a lower gloss of the cured coating film formed. Therefore, esters are preferred, and diethylene glycol monoethyl ether acetate is more preferred. These organic solvents may be used alone or in combination of two or more.

[0094] The amount of the organic solvent to be added is not particularly limited, and can be appropriately set according to the target viscosity so as to facilitate the preparation of the curable resin composition.

[0095] [Other added ingredients] The curable resin composition of the present invention may further contain, as necessary, components such as a photoinitiator assistant, a cyanate compound, an elastomer, a mercapto compound, a urethanization catalyst, a thixotropic agent, an adhesion promoter, a block copolymer, a chain transfer agent, a polymerization inhibitor, a copper inhibitor, an antioxidant, a rust inhibitor, a thickener such as fine silica, organic bentonite, or montmorillonite, at least one of silicone-based, fluorine-based, or polymer-based defoamers and leveling agents, imidazole-based, thiazole-based, or triazole-based silane coupling agents, phosphinates, phosphate ester derivatives, phosphorus compounds such as phosphazene compounds, or the like. These may be known in the field of electronic materials.

[0096] The curable resin composition of the present invention may be used in the form of a dry film.

[0097] [Preparation method] In preparing the curable resin composition of the present invention, each component is weighed, mixed, and then pre-mixed with a mixer. Subsequently, each component is dispersed and kneaded with a kneader, whereby the curable resin composition of the present invention can be prepared.

[0098] Examples of the kneading machine include a bead mill, a ball mill, a sand mill, a three-roll mill, and a two-roll mill. Among these, a bead mill is preferably used in terms of reducing the variation in the thickness of the coating film before and after drying while maintaining a lower gloss and suppressing the copper appearance phenomenon. The dispersion conditions of the bead mill, such as the type and particle size of the beads, can be appropriately set according to the target viscosity, and examples of the type of beads include zirconia beads and alumina beads. The particle size of the beads is, for example, in the range of φ0.015 to 2.0 mm. Among these, the range of φ0.3 to 1.5 mm is more preferable. The bead filling rate is preferably 50 to 95%, and the rotor rotation speed is preferably 800 to 1300 rpm. In addition, as the target viscosity, the viscosity of the composition when introduced into the bead mill is preferably 200 dPa·s or less in terms of improving dispersibility and making the cured coating film lower in gloss. On the other hand, the lower limit is preferably 50 dPa·s or more. The viscosity in the present invention is a value measured in accordance with the viscosity measurement method using a cone-plate type rotational viscometer of JIS Z 8803:2011, 10, at 50°C, 100 rpm, and 30 seconds using a cone-plate type viscometer (TVE-33H, manufactured by Toki Sangyo Co., Ltd.) using a 3°×R9.7 cone rotor.

[0099] On the other hand, the dispersion conditions such as the rotation ratio of each roll of the three-roll mill can also be appropriately set according to the target viscosity.

[0100] In order to further improve the dispersibility, the raw materials may be first slurried using a kneader such as a bead mill or a three-roll mill, weighed, mixed, and then pre-mixed with a stirrer. When slurried, it is preferable to weigh and mix a wetting dispersant such as a silane coupling agent, and then knead using a bead mill or the like. Then, each component including the one slurried using the kneader as exemplified above may be dispersed, and kneaded using a bead mill or the like to prepare the composition.

[0101] [Application] The curable resin composition according to the present invention is useful for forming a pattern layer as a permanent coating of a printed wiring board, such as a solder resist, a coverlay, or an interlayer insulating layer, and is particularly useful for forming a solder resist. In addition, since the curable resin composition according to the present invention can form a cured product having excellent film strength even in a thin film, it can be suitably used for forming a pattern layer in a printed wiring board that requires a thin film, such as a package substrate (a printed wiring board used in a semiconductor package). Furthermore, since the cured product obtained from the curable resin composition according to the present invention has excellent flexibility, it can be suitably used for a flexible printed wiring board.

[0102] Furthermore, the curable resin composition of the present invention can be used not only for forming a pattern layer of a cured coating film, but also for applications in which a pattern layer is not formed, such as molding applications (sealing applications).

[0103] [Dry film] The curable resin composition of the present invention can also be in the form of a dry film comprising a support (carrier) film and a resin layer consisting of a dried coating film of the curable resin composition formed on the support film. In forming the dry film, the curable resin composition of the present invention is diluted with the organic solvent to adjust the viscosity to an appropriate level, and is applied to a uniform thickness on a carrier film using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and is usually dried at a temperature of 50 to 130°C for 1 to 30 minutes to obtain a film. There is no particular restriction on the coating film thickness, but the thickness after drying is generally appropriately selected within the range of 1 to 150 μm, preferably 5 to 60 μm. By using the curable resin composition of the present invention, the variation of the coating film before drying can be reduced, so that the variation can be reduced even if the resin layer consisting of the dried coating film is thin. For example, the dry film can also be in the form of a dry film comprising a thin resin layer of 12 μm or less.

[0104] As the support film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the support film.

[0105] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.

[0106] The thickness of the support film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0107] After forming a resin layer consisting of a dried coating film of the curable resin composition of the present invention on a support film, it is preferable to further laminate a peelable protective (cover) film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer, etc. As the peelable protective film, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc. can be used, and it is sufficient that the adhesive strength between the resin layer and the protective film is smaller than the adhesive strength between the resin layer and the support film when the protective film is peeled off.

[0108] The thickness of the protective film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0109] To prepare a cured coating film on a printed wiring board using a dry film, the protective film is peeled off from the dry film, and the exposed resin layer of the dry film is placed on a substrate on which a circuit is formed, and the layers are laminated using a laminator or the like to form a resin layer on the substrate on which a circuit is formed. The formed resin layer is then exposed to light, developed, and cured by heating to form a cured coating film. The protective film may be peeled off either before or after exposure.

[0110] [Cured product] The cured product of the present invention is obtained by curing the curable resin composition of the present invention or the resin layer of the dry film of the present invention. The cured product of the present invention can be suitably used for printed wiring boards, electronic components, etc. The cured product of the present invention has excellent flexibility, and therefore can be suitably used for flexible printed wiring boards in particular. The cured product of the present invention also has excellent infrared shielding properties and stability over time.

[0111] [Printed wiring board] The printed wiring board of the present invention has a cured product obtained from the resin layer of the curable resin composition or dry film of the present invention. As a method for producing the printed wiring board of the present invention, for example, the curable resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and coated on a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100°C for 15 to 90 minutes to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the carrier film is peeled off to form a resin layer on the substrate.

[0112] The above-mentioned substrates include printed wiring boards and flexible printed wiring boards on which circuits have already been formed using copper or the like, as well as materials such as copper-clad laminates for high-frequency circuits made from paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.

[0113] The dry film is preferably laminated onto the substrate under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, even if the surface of the substrate is uneven, the dry film adheres closely to the substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.

[0114] The volatilization drying carried out after the curable resin composition of the present invention is applied to a substrate can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of bringing hot air in a dryer into countercurrent contact using a heat source of an air heating method using steam, and a method of blowing the hot air onto a substrate from a nozzle). As an apparatus, a hot air circulation drying oven such as DF610 manufactured by Yamato Scientific Co., Ltd. can be mentioned.

[0115] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed areas are developed with a dilute alkaline aqueous solution (e.g., a 0.3 to 3.0 mass % aqueous solution of sodium carbonate) to form a pattern of the cured product. In the case of a dry film, after exposure, the support film is peeled off from the dry film and development is performed to form a patterned cured product on the substrate. Note that, as long as the properties are not impaired, the support film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed.

[0116] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm, and further, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1,000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 As an example of the exposure device, HMW-680-GW20 manufactured by Oak Manufacturing Co., Ltd., etc., may be used as an exposure device equipped with a metal halide lamp.

[0117] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.

[0118] Furthermore, the cured product is irradiated with active energy rays and then heat-cured (for example, at a temperature of 100 to 220°C for 30 to 90 minutes), or irradiated with active energy rays after heat-curing (for example, at 1,000 to 2,000 mJ / cm 2), or by heat curing only for final finish curing (main curing), a cured coating film with excellent properties such as adhesion and hardness is formed. As an example of the equipment, QRM-2082 manufactured by Oak Seisakusho Co., Ltd. is a UV conveyor using a high-pressure mercury lamp.

[0119] The above is a method for forming a cured coating film using a photocurable or thermosetting resin composition, but in the case of only photocuring or only thermosetting, the coating film can be produced as follows. In the case of photocuring only, the curable resin composition of the present invention is applied to a substrate by pattern printing or the like, and then exposed to active energy rays (for example, 1,000 to 2,000 mJ / cm 2 ) to cure the coating, thereby forming a cured coating film. On the other hand, in the case of only thermal curing, the curable resin composition of the present invention is applied to a substrate by pattern printing or the like, and then heat cured (for example, at a temperature of 100 to 220°C for 30 to 90 minutes) to form a cured coating film. EXAMPLES

[0120] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.

[0121] (Synthesis of resin varnish 1 of carboxyl group-containing resin) In an autoclave equipped with a thermometer, a nitrogen introduction device / alkylene oxide introduction device, and a stirrer, 119.4 g of novolac cresol resin (manufactured by AICA Corporation, product name "Shonol CRG951", OH equivalent: 119.4), 1.19 g of potassium hydroxide, and 119.4 g of toluene were charged, and the system was replaced with nitrogen while stirring, and heated to increase the temperature. Next, 63.8 g of propylene oxide was gradually added dropwise, and the temperature was increased to 125-132°C and 0-4.8 kg / cm. 2The mixture was reacted at 100°C for 16 hours. After that, the mixture was cooled to room temperature, and 1.56 g of 89% phosphoric acid was added to the reaction solution to neutralize the potassium hydroxide, and a propylene oxide reaction solution of novolac cresol resin with a solid content of 62.1% and a hydroxyl value of 182.2 g / eq. was obtained. This was a mixture in which an average of 1.08 moles of alkylene oxide was added per equivalent of phenolic hydroxyl group. Next, 293.0 g of the alkylene oxide reaction solution of novolac cresol resin obtained, 43.2 g of acrylic acid, 11.53 g of methanesulfonic acid, 0.18 g of methylhydroquinone, and 252.9 g of toluene were charged into a reactor equipped with a stirrer, thermometer, and air blowing tube, and the mixture was reacted at 110°C for 12 hours while being stirred by blowing air at a rate of 10 ml / min. As for the water produced by the reaction, 12.6 g of water was distilled off as an azeotrope with toluene. After that, the reaction solution was cooled to room temperature, neutralized with 35.35g of 15% aqueous sodium hydroxide solution, and then washed with water. After that, toluene was distilled off while replacing it with 118.1g of diethylene glycol monoethyl ether acetate in an evaporator, and a novolac-type acrylate resin solution was obtained. Next, 332.5g of the obtained novolac-type acrylate resin solution and 1.22g of triphenylphosphine were charged into a reactor equipped with a stirrer, a thermometer, and an air blowing tube, and 60.8g of tetrahydrophthalic anhydride was gradually added while blowing air at a rate of 10ml / min and stirring, and reacted at 95 to 101°C for 6 hours. In this way, a resin varnish 1 of a carboxyl group-containing resin with a solid acid value of 88mgKOH / g, solid content of 71%, and weight average molecular weight of 2,000 was obtained.

[0122] (Synthesis of resin varnish 2 of carboxyl group-containing resin) 220 g of orthocresol novolac epoxy resin (DIC Corporation, EPICLON N-695, epoxy equivalent: 214, average functionality 7.6) was placed in a four-neck flask equipped with a stirrer and a reflux condenser, 214 g of diethylene glycol monoethyl ether acetate was added, and the mixture was heated and dissolved. Next, 0.1 g of hydroquinone as a polymerization inhibitor and 2.0 g of dimethylbenzylamine as a reaction catalyst were added. This mixture was heated to 95-105°C, 72 g of acrylic acid was gradually added dropwise, and the mixture was reacted for 16 hours. The reaction product was cooled to 80-90°C, 106 g of tetrahydrophthalic anhydride was added, the mixture was reacted for 8 hours, and the mixture was taken out after cooling. The resin varnish 2 of the carboxyl group-containing resin thus obtained had a solid content of 65%, an acid value of the solid matter of 100 mgKOH / g, and a weight average molecular weight Mw of about 3,500.

[0123] (Synthesis of resin varnish 3 of carboxyl group-containing resin) 650 parts by mass of diethylene glycol monoethyl ether acetate was charged with 1070g of orthocresol novolac epoxy resin (DIC Corporation, EPICLON N-695, softening point 95°C, epoxy equivalent 214, average functional group number 7.6), 360g of acrylic acid, and 1.5g of hydroquinone, and heated to 100°C with stirring to dissolve uniformly. Next, 4.3 parts by mass of triphenylphosphine was charged, heated to 110°C and reacted for 2 hours, and then 1.6 parts by mass of triphenylphosphine was added, heated to 120°C, and reacted for another 12 hours. 525g of aromatic hydrocarbon (Standard Oil Corporation, Osaka Sales Office, T-Sol 150) and 608g (4.0 moles) of tetrahydrophthalic anhydride were charged into the resulting reaction liquid, and reacted at 110°C for 4 hours. Further, 142.0 g of glycidyl methacrylate was added to the obtained reaction liquid, and the reaction was carried out for 4 hours at 115° C. In this manner, a resin varnish 3 of a carboxyl group-containing resin having a solid content acid value of 77 mgKOH / g and a solid content of 65% was obtained.

[0124] (Synthesis of resin varnish 4 of carboxyl group-containing resin) In a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, 325.0 parts by mass of dipropylene glycol monomethyl ether as a solvent was heated to 110°C, and a mixture of 174.0 parts by mass of methacrylic acid, 174.0 parts by mass of ε-caprolactone-modified methacrylic acid (average molecular weight 314), 77.0 parts by mass of methyl methacrylate, 222.0 parts by mass of dipropylene glycol monomethyl ether, and 12.0 parts by mass of t-butylperoxy 2-ethylhexanoate (Perbutyl O, manufactured by NOF Corporation) as a polymerization catalyst was added dropwise over 3 hours, and the mixture was further stirred at 110°C for 3 hours to inactivate the polymerization catalyst, thereby obtaining a resin solution. After cooling this resin solution, 289.0 parts by mass of Cyclomer M100 (3,4-epoxycyclohexylmethyl methacrylate) manufactured by Daicel Corporation, 3.0 parts by mass of triphenylphosphine, and 1.3 parts by mass of hydroquinone monomethyl ether were added, and the mixture was heated to 100°C and stirred to carry out a ring-opening addition reaction of the epoxy groups, thereby obtaining a carboxyl group-containing resin varnish 4. The carboxyl group-containing resin varnish 4 thus obtained had a nonvolatile content of 45.5% by mass and an acid value of the solid matter of 79.8 mgKOH / g.

[0125] (Examples 1 to 4, Comparative Examples 1 to 3) (Preparation of Curable Resin Composition) For each composition, the components were mixed according to the composition shown in Table 1 below, and an organic solvent (diethylene glycol monoethyl ether acetate) was mixed as necessary, and premixed with a stirrer. Then, the compositions of Formulation Examples 1 to 4 were all dispersed at 70°C or less using a bead mill, kneaded, and adjusted. On the other hand, the compositions of Formulation Examples 5 to 7 were all dispersed at 70°C or less using a roll mill, kneaded, and adjusted. Note that the components of the compositions of Formulation Examples 1 and 5 are the same, but the dispersion methods are different, the components of the compositions of Formulation Examples 2 and 6 are the same, but the dispersion methods are different, and the components of the compositions of Formulation Examples 3, 4, and 7 are the same, but the dispersion methods are different. The dispersion by the bead mill was carried out under the following conditions. The compositions of Formulation Examples 1 to 3 and 5 to 7, each of which had a viscosity adjusted to 100 dPa·s with an organic solvent (diethylene glycol monoethyl ether acetate), were milled in a horizontal wet mill (manufactured by Buhler) using zirconia beads with a particle size of φ1.0 mm, and the composition of Formulation Example 4 was milled in a horizontal wet mill using zirconia beads with a particle size of φ0.65 mm, to obtain the average particle size D 50 The dispersion treatment was carried out so that the viscosity of the mixture was 1000 rpm. The filling rate of the zirconia beads was 85%, and the rotor speed was 1000 rpm. The viscosity was measured at 50°C, 100 rpm, and 30 seconds using a cone-plate type viscometer (TVEE-33H, manufactured by Toki Sangyo Co., Ltd.) with a cone rotor of 3°×R9.7, in accordance with the viscosity measurement method using a cone-plate type rotational viscometer of JIS Z 8803:2011. In addition, for the dispersion by the roll mill, each composition was dispersed in a three-roll mill manufactured by Inoue Seisakusho Co., Ltd. to obtain an average particle diameter D 50 Dispersion processing was carried out so that

[0126] [Table 1]

[0127] The blend amounts in Table 1 are shown in parts by weight. Details of each component in Table 1 are as follows. *1: The amount of the carboxyl group-containing resin varnish 1 synthesized above is calculated as the solid content. *2: The amount of the carboxyl group-containing resin varnish 2 synthesized above is calculated as the solid content. *3: The amount of the carboxyl group-containing resin varnish 3 synthesized above is calculated as the solid content. *4: The amount of the carboxyl group-containing resin varnish 4 synthesized above is calculated as the solid content. *5: Photopolymerizable monomer (dipentaerythritol hexaacrylate (DPHA), manufactured by Nippon Kayaku Co., Ltd.) *6: 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane (IGM Resins, Omnirad 907) *7: Ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (BASF Japan Ltd., Irgacure OXE02) *8: Bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins, Omnirad 819) *9: 2,4-Diethylthioxanthone (KAYACURE DETX-S, manufactured by Nippon Kayaku Co., Ltd.) *10: Blue colorant (CI Pigment Blue 15:3) *11: Yellow colorant (CI Pigment Yellow 147) *12: Red colorant (Paliogen Red K3580, manufactured by BASF Japan Ltd.) *13: Bisphenol A epoxy resin (EPICLON 840-S, manufactured by DIC Corporation) *14: Phenol novolac epoxy resin (EPICLON N-770, manufactured by DIC Corporation) *15: Biphenyl type epoxy resin (Mitsubishi Chemical Corporation, YX-4000) *16: 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (high melting point type, Nissan Chemical Co., Ltd., TEPIC-HP) *17: Melamine *18: Barium sulfate (average particle diameter 0.3 μm (measured before kneading into a curable resin composition)) (Sakai Chemical Industry Co., Ltd., B-34) *19: Amorphous silica (average particle size 6.3 μm (measured before mixing into a curable resin composition), oil absorption: 260 ml / 100 g) (manufactured by Evonik Degussa Japan Co., Ltd., ACE MATT OK 500)

[0128] (Average particle diameter D 50 and specific surface area CS) The average particle diameter D50 (μm) and specific surface area CS (m 2 / ml) was measured. First, prepare the following equipment and supplies: Particle size distribution meter: Nikkiso Microtrac MT3300EX Circulation device: ASVR manufactured by Nikkiso Co., Ltd. Next, enter the measurement conditions using the following procedure. Start the software that comes with the Microtrac ("Particle Size Distribution Measurement"), proceed from the SET UP screen, and set the time from the measurement condition setting options. Set the Set Zero time to 30 sec., the measurement to 30 sec., and the number of measurements to 2. Next, enter the analysis conditions. In the analysis information, set the particle refractive index to 1.81 (fixed value: average value of the refractive index of all inorganic substances), the particle characteristics to transparent, and the shape to non-spherical. In the solvent information, select PMA (propylene glycol monomethyl ether acetate) and set the solvent refractive index to 1.4. Next, enter the scale settings. In the particle size range, set the minimum particle size to 0.021 μm and the maximum particle size to 704 μm. Next, enter the sampling system. Set the number of ASVR cleanings to 4, the flow rate to 50%, the ultrasonic output to 40 W, and the ultrasonic time to 300 sec. After entering all the measurement conditions, click Save in the measurement condition settings to close. Next, the sample is adjusted according to the following procedure. 0.3 g of the sample (curable resin composition) is weighed out and placed in a screw bottle, 30 g of propylene glycol monomethyl ether acetate is gradually added using a dropper, and the screw bottle is shaken to dissolve the sample to prepare an adjusted sample. The adjusted sample is not subjected to external dispersion or pre-dispersion. Next, the adjusted sample is measured. Click on particle size distribution measurement in the software attached to the Microtrack to open the sample loading screen. Using a dropper, drip a few drops of the adjusted sample into the sample inlet of the main unit. When a red indication bar is displayed on the sample loading screen, drip the adjusted sample into the sample inlet until it is within the range from red to green. When it is within the green range, press the measurement button to start measurement. The process from sample adjustment to measurement of the adjusted sample is performed within 5 minutes. The cumulative average diameter 50% value and the area average diameter MA value displayed as the measurement results are read. The cumulative average diameter 50% value is used to measure the average particle diameter D measured with the Microtrack. 50 The value is taken as the specific surface area measured by the Microtrac. Also, calculate CS = 6 / MA. The calculated CS value is taken as the specific surface area measured by the Microtrac.

[0129] (Measurement of the average spacing Sm (μm) and maximum height Ry (μm) of irregularities) Each curable resin composition of each Example and Comparative Example was solid-printed by screen printing using a 180 mesh polyester plate (with bias) on a clean glass substrate (76 mm x 26 mm x 1.1 mmt) so that the thickness after drying would be 12 μm, and then dried at 90 ° C for 15 minutes to form a dried coating film. The obtained "coating film after drying" (hereinafter, sample) was measured for the average spacing Sm (μm) of the irregularities and the maximum height Ry (μm) according to JIS B0601-1994 using a shape measuring laser microscope (VK-X100 manufactured by Keyence Corporation) as follows. The measurement was performed after drying at 90 ° C for 15 minutes and then leaving it at room temperature for 30 minutes. After starting the main body (control unit) of the shape measurement laser microscope (VK-X100) and the VK observation application (VK-H1VX, manufactured by Keyence Corporation), the above sample to be measured was placed on the xy stage. The lens revolver of the microscope unit (VK-X110, manufactured by Keyence Corporation) was turned to select a 10x objective lens, and the focus and brightness were roughly adjusted in the image observation mode of the VK observation application (VK-H1VX, manufactured by Keyence Corporation). The xy stage was operated to adjust so that the part of the sample surface to be measured was at the center of the screen. The 10x objective lens was replaced with a 50x magnification, and the focus was adjusted to the surface of the sample using the autofocus function of the image observation mode of the VK observation application (VK-H1VX, manufactured by Keyence Corporation). The easy mode was selected in the shape measurement tab of the VK observation application (VK-H1VX), the measurement start button was pressed, the surface shape of the sample was measured, and a surface image file was obtained. The VK analysis application (VK-H1XA manufactured by Keyence Corporation) was started and the obtained surface image file was displayed, after which tilt correction was performed. The observation measurement range (horizontal) in the measurement of the surface shape of the sample was 270 μm. After displaying the line roughness window and selecting JIS B0601-1994 in the parameter setting area, the horizontal line was selected from the measurement line button, and the horizontal line was displayed at any location in the surface image. The OK button was then pressed to obtain the average spacing Sm (μm) and maximum height Ry (μm) of the uneven surface. Furthermore, horizontal lines were displayed at four different locations in the surface image, and the average spacing Sm (μm) and maximum height Ry (μm) of each of the uneven surfaces were obtained. The average values ​​of the five values ​​obtained were calculated to obtain the average spacing Sm value and maximum height Ry value of the uneven surface of the sample surface. The measurement results are shown in Table 2.

[0130] (Gloss measurement) The coating was solid printed by screen printing on a 300 mm x 150 mm copper foil substrate with a thickness of 35 μm, the surface of which had been buff-roll polished, so that the film thickness after curing would be 12 μm. It was then cured for 60 minutes at 150°C using a hot air circulating drying oven (DF610, manufactured by Yamato Scientific Co., Ltd.) to form a cured coating film on the copper foil substrate. The coating was then allowed to cool at room temperature for 30 minutes under a yellow lamp, and left to stand to prepare an evaluation substrate. For each of the cured coating films formed on the copper foil substrate, a cloth soaked in isopropyl alcohol (IPA) was placed on the surface of the cured coating film in an environment of 25°C and 50% RH, and then a 500g weight was placed on top of the cloth and left to stand for 1 minute, after which the cloth was peeled off and it was confirmed that all or part of the resin layer was not attached to the surface of the cloth that had been in contact with the cured coating film. Note that the gloss level was measured using the cured coating film formed by thermal curing without performing a development process after exposure. Thereafter, the Gs (60°) of each cured coating surface was measured using a digital variable-angle gloss meter (Micro-Tri-Gloss, manufactured by BYK Gardener). The measurement results are shown in Table 2 below.

[0131] (Variation of coating film before drying when thin film is used) As a simple method for checking the variation in the coating film before drying when it is a thin film, a method for checking the variation in powder in the curable resin composition was adopted, and the degree of dispersion of the curable resin composition was measured. Specifically, the degree of dispersion of the curable resin compositions of each Example and Comparative Example was measured using a particle size gauge (manufactured by Daiichi Sokhan Seisakusho Co., Ltd.) with a width of 90 mm, a length of 240 mm, and a maximum depth of 25 μm in accordance with JIS K5101-5-2:2004 and JIS K5600-2-5:1999, and was evaluated based on the following evaluation criteria. The degree of dispersion was measured by observing the point where noticeable spots began to appear on the gauge. In particular, a point containing 5 to 10 particles in a width of 3 mm along the groove of the gauge was observed, and this point was regarded as the degree of dispersion. Spots that appeared sparsely before the point where noticeable spots began to appear were ignored. The average value of three measurements was calculated. The evaluation results are shown in Table 2. ◯: The degree of dispersion (average value of three measurements) was 20 μm or less. ×: The degree of dispersion (average value of three measurements) was more than 20 μm.

[0132] (Variation of dry coating film when thin) A printability test was conducted as a simple method for checking the variation of the dried coating film when it is a thin film. Specifically, a solid film was printed on a solid glass substrate by screen printing using a 180 mesh polyester plate (with bias) so that the film thickness after drying would be 12 μm, and the film was dried at 90 ° C. for 15 minutes using a hot air circulation drying oven (DF610 manufactured by Yamato Scientific Co., Ltd.), cooled at room temperature for 30 minutes under a yellow lamp, and then left to stand. After leaving it, it was confirmed that the curable resin composition did not adhere to the finger when the coated surface was touched with a finger. After leaving it, the step (P) between the dried coating film and the uncoated part was measured at four random points using a surface roughness measuring instrument (Surfcorder SE600: Kosaka Laboratory Co., Ltd.), and a step analysis was performed using a three-point designation type. Details will be described with reference to the cross section of the dried coating film shown in FIG. 1. In the three-point step analysis, two reference points 3 on the surface of the dried coating film 2 on the substrate 1 are input, and one evaluation point 5 on the uncoated portion 4 of the substrate 1 is input to obtain a reference line 6. Next, the step (P) between the reference line 6 and the evaluation point 5 is measured. The film thickness and the standard deviation of the film thickness were calculated from each measured step (P), and evaluated based on the following evaluation criteria. The measurement conditions were a measurement magnification of 2,000 times, a feed speed of 0.5 mm / s, and a trace length of 6.0 mm. The evaluation results are shown in Table 2. A: The standard deviation was within 1.0 μm. ×: The standard deviation was more than 1.0 μm.

[0133] (Confirmation of copper appearance phenomenon) A 300mm x 150mm copper foil substrate with a thickness of 35μm, the surface of which had been buff roll polished, was solid-printed by screen printing using a 180 mesh polyester plate (with bias) so that the film thickness after curing would be 12μm, and cured at 150°C for 60 minutes using a hot air circulation drying oven (DF610 manufactured by Yamato Scientific Co., Ltd.), and left to cool and stand at room temperature for 30 minutes under a yellow lamp to prepare an evaluation board. In each of the evaluation boards prepared, a cloth soaked in isopropyl alcohol (IPA) was placed on the surface of the cured coating in an environment of 25°C 50% RH, and a 500g weight was placed on top of it and left to stand for 1 minute, after which the cloth was peeled off and it was confirmed that all or part of the resin layer was not attached to the surface of the cloth that had been in contact with the cured coating. Thereafter, the areas within an area of ​​70 mm × 70 mm where the underlying copper was visible were confirmed using an optical microscope (50x magnification). The evaluation results are shown in Table 2. ◎: No copper was visible at all. ○: A few areas where copper was visible were confirmed, but the level was not problematic. ×: Many areas where copper was visible were confirmed.

[0134] [Table 2]

[0135] As is clear from Table 2, the curable resin compositions of the Examples have small variations in the pre-drying coating film and the dried coating film when formed into thin films, and do not cause the copper appearance phenomenon. [Explanation of symbols]

[0136] 1: Substrate 2: Dry coating film 3: Reference point 4: Uncoated area 5: Evaluation score 6: Reference line P: step X: Measurement direction of the surface roughness measuring instrument

Claims

[Claim 1] A curable resin composition containing a curable resin and an extender pigment, The 60° gloss of a cured coating film having a thickness of 12 μm after curing of the curable resin composition is in the range of 0.5 to 40.0, 0.3 g of the curable resin composition was mixed with 30 g of propylene glycol monomethyl ether acetate, and the average particle diameter D 50 is 0.1 μm or more and 1.0 μm or less, and the specific surface area CS is 10.0 m 2 / ml or more.

Citation Information

Patent Citations

  • Curable composition, dry film, cured material and print circuit board

    JP2018172632A

  • Photocurable resin composition, dry film, cured product, and printed wiring board

    WO2018143220A1

  • Photosensitive film and method for forming permanent mask resist

    WO2019221012A1

  • Photocuring, thermosetting delustering resist ink composition

    JP1997157574A

  • Photosensitive thermosetting resin composition and method for forming solder resist pattern