Silica particles and method for producing silica particles
By carbonizing core-shell particles before firing, the method produces hollow silica particles with low true density and excellent dispersibility, addressing the limitations of existing silica particle production methods and enhancing their applicability in electronic materials.
Patent Information
- Application Number
- JP2024117430
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-21
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-10-19
AI Technical Summary
Existing methods for producing silica particles using citric acid result in particles with high true density and poor dispersibility, limiting their application in articles requiring antireflection properties.
The production method involves carbonizing core-shell particles before firing to create hollow silica particles with a true density of 0.8g/cm³ to 1.4g/cm³ and a particle size distribution where particles larger than twice the average diameter are 15% or less, achieving excellent dispersibility.
The method produces silica particles with low true density and improved dispersibility, suitable for applications in multilayer printed circuit boards and semiconductor sealing materials.
Smart Images

Figure 2024133364000001
Abstract
Description
[Technical field]
[0001] The present invention relates to silica particles and a method for producing silica particles. [Background technology]
[0002] Patent Document 1 is a technology disclosed by the present applicant, which has the following features: (1) an average particle size of 50 to 150 nm, (2) an average shell thickness of 5 to 25 nm, and (3) solid-state NMR ( 29 In the Si / MAS measurement, the integrated intensity (I Q2 ) and the integrated intensity (I Q4 ) and the ratio (I Q2 / I Q4 ) is 0.20 or less, and (4) the ratio Psa / Psm of the peak intensity Psa of associated particles to the peak intensity Psm of main particles, which are non-associated hollow nanosilica particles, in a particle size distribution in the particle diameter range of 50 to 500 nm measured using a disk centrifugal particle size distribution measuring device is 0.4 or less. This technology is a technology in which dispersibility is improved by baking at 700°C in the presence of an organic acid such as citric acid. Since the formation of associated particles is suppressed and light reflection is suppressed in these hollow nanosilica particles, they can be suitably used in various articles that require anti-reflection properties. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-176037 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides a method for producing silica particles without using citric acid, and provides silica particles having excellent true density and dispersibility. [Means for solving the problem]
[0005] As a result of extensive research, the present inventors have developed new silica particles (preferably hollow silica particles) that have low true density and excellent dispersibility by subjecting core-shell particles to a carbonization treatment before firing when producing silica particles.
[0006] The present invention includes the following silica particles and a method for producing silica particles.
[0007] Section 1. (1) True density is 0.8 g / cm 3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less; (3) The water absorption amount is 1.0% by mass or less. Silica particles.
[0008] Section 2. Item 4. The silica particles according to item 1, wherein the silica particles are carbonized and calcined.
[0009] Section 3. 3. The silica particles according to item 1 or 2, wherein (5) the average particle size is 0.2 μm to 1.0 μm.
[0010] Section 4. 3. The silica particles according to item 1 or 2, wherein the silica particles are hollow silica particles.
[0011] Section 5. A method for producing silica particles, comprising the steps of: The method includes a step of first carbonizing the core-shell particles and then calcining the same, Silica particles are (1) True density is 0.8 g / cm 3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less; (3) The water absorption amount is 1.0% by mass or less. A method for producing silica particles.
[0012] The silica particles of the present invention are novel silica particles (preferably hollow silica particles) that have a low true density and excellent dispersibility. Effect of the Invention
[0013] The present invention provides a method for producing silica particles without using citric acid, and provides silica particles having excellent true density and dispersibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below.
[0015] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.
[0016] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."
[0017] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."
[0018] In this specification, the designations parts, % etc. are generally used.
[0019] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.
[0020] [1] Silica particles The present invention includes silica particles.
[0021] The silica particles of the present invention are (1) True density is 0.8 g / cm3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less; (3) The water absorption amount is 1.0 mass% or less.
[0022] The silica particles are preferably (4) carbonized and calcined.
[0023] The silica particles preferably have (5) an average particle size of 0.2 μm to 1.0 μm.
[0024] The silica particles are preferably hollow silica particles.
[0025] The silica particles of the present invention are novel silica particles having a low true density and excellent dispersibility.
[0026] The silica particles of the present invention are useful for multi-layer printed circuit boards, wire covering materials, semiconductor encapsulation materials, etc.
[0027] Silica-based compounds and metal oxides The silica-based compound forming the silica particles is not particularly limited as long as it contains silica, and the silica particles may be formed only from silica.
[0028] When the silica-based compound contains a compound other than silica, the silica particles preferably contain silica and a metal oxide.
[0029] The metal oxide is preferably an oxide of a metal capable of forming a metal alkoxide, specifically, an oxide of aluminum, titanium, zirconium, etc.
[0030] The metal oxide may be used alone or in combination of two or more kinds (blend).
[0031] When aluminum oxide is used as the metal oxide, the surface charge (zeta potential, etc.) of the shell of the silica particles can be adjusted.
[0032] When titanium or zirconium oxide is used as the metal oxide, the refractive index of the shell of the silica particle can be adjusted.
[0033] (1) True density of silica particles The silica particles of the present invention have a true density of 0.8 g / cm 3 ~1.4g / cm 3 It is.
[0034] The silica particles of the present invention have a true density that is lower than that of general silica (2.2 g / cm) due to the presence of a low-density air layer. 3 ) is lower than that.
[0035] The true density of the silica particles was measured using a nitrogen gas pycnometer (Ultrapyc 5000 Micro, manufactured by Anton Paar Japan Co., Ltd.) to determine the true density of the silica particles (0.2 g of powder).
[0036] The silica particles to be subjected to the measurement of true density are preferably dried under reduced pressure at a temperature of 120° C. for 2 hours, and then the true density of the dried silica particles is measured.
[0037] The true density of silica particles is 0.8 g / cm 3 ~1.4g / cm 3 and preferably 0.8 g / cm 3 ~1.3g / cm 3 and more preferably 0.9 g / cm 3 ~1.2g / cm 3 and more preferably 0.9 g / cm 3 ~1.1g / cm 3 By adjusting the true density to fall within the above range, the silica particles can be produced satisfactorily, and the shell is not broken, the silica particles have a low true density, and are excellent in dispersibility.
[0038] (2) Particle size distribution of silica particles The silica particles of the present invention have a particle size distribution in which the frequency of particles larger than twice the average particle size is 15% or less.
[0039] "Particles larger than twice the average particle size" refers to particles whose size exceeds twice the average particle size, but does not include particles whose size is twice the average particle size.
[0040] The frequency of particles larger than twice the average particle size in the particle size distribution of silica particles is a value obtained by measuring the particle size distribution of silica particle powder using a laser diffraction / scattering particle size distribution analyzer (LA-950, Horiba, Ltd.) and calculating the frequency (%) of particles larger than twice the average particle size in the silica particle powder.
[0041] The lower the frequency of particles larger than twice the average particle size in the particle size distribution of silica particles, the more preferable. The frequency of particles larger than twice the average particle size in the particle size distribution of silica particles is 15% or less, preferably 12% or less, more preferably 9% or less, and even more preferably 6% or less. The lower limit of the frequency of particles larger than twice the average particle size in the particle size distribution of silica particles is about 0%. Silica particles can be produced well by adjusting the frequency of particles with a particle size of 1 μm or more in the particle size distribution to the above range, and the silica particles have a low true density and excellent dispersibility.
[0042] (3) Water absorption of silica particles The silica particles of the present invention have a water absorption amount of 1.0% by mass or less.
[0043] Water absorption test for silica particles The water absorption amount of the silica particles was determined by storing the silica particles (1 g of powder) for 7 days in an environment with a temperature of 50°C and a humidity of 75%, then sampling 0.1 g of the powder and measuring the water content of the silica particles using a Karl Fischer moisture meter (MKA-610, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).
[0044] The lower the water absorption of the silica particles, the more preferable. The water absorption of the silica particles is 1.0% by mass or less, preferably 0.9% by mass or less, more preferably 0.8% by mass or less, and even more preferably 0.7% by mass or less. The lower limit of the water absorption of the silica particles is about 0.1% by mass. By adjusting the water absorption within the above range, the silica particles can be produced well, and the silica particles have a low true density and excellent dispersibility.
[0045] (4) Carbonization and calcination of silica particles The silica particles of the present invention are preferably carbonized and calcined. By being carbonized and calcined, the silica particles can be produced well, and the silica particles have a low true density and excellent dispersibility.
[0046] (5) Average particle size of silica particles The silica particles of the present invention preferably have an average particle size of 0.2 μm to 1.0 μm.
[0047] The average particle size of the silica particles was determined by taking photographs of the particles using a SEM (scanning electron microscope: JSM-7900F, manufactured by JEOL Ltd.) at an acceleration voltage of 8 kV, measuring the short diameters of 100 randomly selected particles, and calculating the average value.
[0048] For image analysis, the image analysis and measurement software WinROOF was used.
[0049] The average particle size of the silica particles is preferably 0.2 μm to 1.0 μm, more preferably 0.3 μm to 0.9 μm, even more preferably 0.4 μm to 0.8 μm, and particularly preferably 0.4 μm to 0.7 μm. By adjusting the average particle size within the above range, the silica particles can be produced more satisfactorily, and the silica particles have a low true density and excellent dispersibility.
[0050] (6) Hollow silica particles The silica particles of the present invention may have a particle structure of a dense type, a porous type, a hollow type, or the like.
[0051] The silica particles are preferably hollow silica particles. The hollow silica particles are preferably silica particles in which a hollow portion (cavity) is formed.
[0052] The silica particles can be produced more satisfactorily because they are hollow silica particles, and the silica particles have a low true density and excellent dispersibility.
[0053] (7) MEK filterability of silica particles The silica particles of the present invention preferably have a methyl ethyl ketone (MEK) filterability of 80 mass % or more.
[0054] The MEK filterability of the silica particles was measured by first mixing the silica particles (2 g of powder) with methyl ethyl ketone (MEK) (8 g) for 2 hours at 500 rpm and then filtering the mixture of the silica particles and MEK using a syringe filter with a pore size of 5 μm (filter paper that allows passage of substances with a size of 5 μm or less).
[0055] The MEK filterability (mass %) of the silica particles is a value calculated by weighing the amount of the mixture solution passed through and using the following formula. (MEK filtration (mass%, wt%)) = [Amount of liquid passed (g)] ÷ [Amount of MEK dispersion of silica particles (10 g)] × 100
[0056] The higher the MEK filterability of the silica particles, the more preferable. The MEK filterability of the silica particles is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more. The upper limit of the MEK filterability of the silica particles is about 100%. By adjusting the MEK filterability to the above range, the silica particles can be produced well, and the silica particles have a low true density and excellent dispersibility.
[0057] Average shell thickness of silica particles The average thickness of the shell (membrane) forming the silica particle of the present invention is preferably from 25 nm to 170 nm, more preferably from 30 nm to 150 nm, and even more preferably from 35 nm to 100 nm.
[0058] The average thickness of the shell forming the silica particles was determined by taking photographs of the particles using a TEM (transmission electron microscope: JEM-2010, manufactured by JEOL Ltd.) at an acceleration voltage of 200 kV, measuring the shell thicknesses of 100 randomly selected particles, and calculating the average value.
[0059] By adjusting the average shell thickness within the above range, the silica particles can be produced satisfactorily, and the shell is not broken, and the silica particles have a low true density and excellent dispersibility.
[0060] The silica particles of the present invention are silica particles having a low true density and excellent dispersibility. The silica particles of the present invention are silica particles that exhibit a low true density and high dispersibility by optimizing the firing conditions (pre-carbonization treatment).
[0061] [2] Core-shell particles The present invention encompasses core-shell particles.
[0062] The core-shell particles of the present invention are core-shell particles having an organic polymer particle as a core and a silica shell covering the organic polymer particle. The silica particles of the present invention can be produced satisfactorily by pyrolyzing the organic polymer particle of the core-shell particle.
[0063] Organic Polymer Particles The organic polymer particles are not particularly limited. The organic polymer particles are preferably organic polymer particles that are easily burned away by pyrolysis after forming a shell. Specifically, the organic polymer particles are polystyrene particles, polymethylmethacrylate (PMMA) (resin) particles, etc.
[0064] When polystyrene particles are used as the organic polymer particles, a positive zeta potential is imparted to the polystyrene particles, making it possible to suppress the generation of associated particles.
[0065] Dispersants The organic polymer particles preferably contain a dispersant. When the organic polymer particles contain a dispersant, the dispersant is present on the surface of the organic polymer particles, and aggregation of the organic polymer particles can be further suppressed.
[0066] The dispersant is not particularly limited as long as it can produce organic polymer particles. Specific examples of the dispersant include polyvinylpyrrolidone (PVP), hydroxypropyl cellulose (HPC), polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene glycol (PPG), polypropylene oxide (PPO), collagen, polysaccharides (gum arabic), etc.
[0067] When polyvinylpyrrolidone, hydroxypropyl cellulose or the like is used as a dispersant, it is possible to suppress the aggregation of the organic polymer particles and thereby the aggregation of the core-shell particles.
[0068] The dispersant may be used alone or in combination of two or more kinds (blend).
[0069] The content of the dispersant in the organic polymer particles is not particularly limited. The content of the dispersant in the organic polymer particles is preferably 0.01% by mass to 100% by mass, more preferably 0.05% by mass to 100% by mass, based on 100% by mass of the organic polymer particles. By adjusting the content of the dispersant to the above range, it is possible to suppress the aggregation of the organic polymer particles.
[0070] Silica coating for organic polymer particles The silica-based compound that forms the shell that covers the organic polymer particles is the same as the silica-based compound that forms the silica particles. The average thickness of the shell (film) of the core-shell particles is the same as the film thickness (average thickness) of the shell (film) that forms the silica particles.
[0071] Average particle size of core-shell particles The average particle size of the core-shell particles is preferably 0.2 μm to 1 μm, more preferably 0.3 μm to 0.9 μm, and even more preferably 0.4 μm to 0.8 μm.
[0072] The average particle diameter of the core-shell particles, like the average particle diameter of the silica particles, is a value obtained by taking photographs of the particles using an SEM (scanning electron microscope: JSM-7900F, manufactured by JEOL Ltd.) at an acceleration voltage of 8 kV, measuring the short diameters of 100 arbitrarily selected particles, and calculating the average value.
[0073] Image analysis was performed using the image analysis and measurement software WinROOF.
[0074] By using the core-shell particles, it is possible to produce silica particles satisfactorily, and the silica particles have a low true density and excellent dispersibility.
[0075] [3] Manufacturing method of silica particles The method for producing silica particles of the present invention preferably comprises the steps of: (1) Step 1 of preparing organic polymer particles by carrying out a polymerization reaction of an organic monomer in a solution containing an organic monomer, a dispersant, and a solvent; (2) adding the organic polymer particles obtained in step 1, an alkoxysilane or an alkoxysilane and a metal alkoxide, and a basic catalyst to a solvent and stirring to prepare a solution, and forming core-shell particles having the organic polymer particles as a core and a shell covering the organic polymer particles in the solution; (3) Step 3, in which the core-shell particles obtained in step 2 are first carbonized (pyrolyzed) and then calcined to remove the organic polymer particles that are the cores of the core-shell particles; and (4) After step 3, the hollow silica particles obtained in step 3 are subjected to a hydrophobic treatment (hydrophobic surface treatment) Includes.
[0076] In the method for producing silica particles of the present invention, the step 3 is The method includes a step of first carbonizing the core-shell particles and then calcining the same, The silica particles are (1) True density is 0.8 g / cm 3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less; (3) Silica particles having a water absorption of 1.0 mass % or less can be produced.
[0077] In the method for producing silica particles of the present invention, when producing silica particles, core-shell particles are subjected to a carbonization treatment before being fired, making it possible to produce new silica particles having a low true density and excellent dispersibility.
[0078] In the method for producing silica particles of the present invention, preferably, The carbonization treatment is carried out at 400°C to 1,200°C, The baking treatment is carried out for 3 hours or more.
[0079] The silica particles of the present invention can be preferably produced satisfactorily through the following steps.
[0080] (1) Step 1 (production of organic polymer particles) Step 1 is a step of preparing organic polymer particles by carrying out a polymerization reaction of an organic monomer in a solution containing an organic monomer, a dispersant, and a solvent.
[0081] Organic Monomers The organic monomer is not particularly limited as long as it can produce organic polymer particles.
[0082] The organic monomer is preferably an organic monomer capable of forming organic polymer particles that are easily burned off by pyrolysis after forming the shell, specifically styrene for producing polystyrene, methyl methacrylate for producing polymethyl methacrylate (PMMA) (resin), etc.
[0083] When styrene is used as the organic monomer, a positive zeta potential is imparted to the polystyrene particles, making it possible to suppress the generation of associated particles.
[0084] The polystyrene is not particularly limited. The polystyrene is preferably a polystyrene containing a structural unit derived from a hydrophobic monomer such as alkyl (meth)acrylate, and other copolymerizable monomer structural units. The polystyrene is preferably an alkyl (meth)acrylate styrene having an alkyl group having 3 to 22 carbon atoms, 2-methylstyrene, or the like.
[0085] In step 1, the concentration of the organic monomer in the solution is not particularly limited. The concentration of the organic monomer in the solution is preferably 0.1% by mass to 20% by mass, more preferably 0.2% by mass to 10% by mass, relative to 100% by mass of the solution. By adjusting the concentration of the organic monomer within the above range, the average particle size of the silica particles in the final product can be well controlled.
[0086] Dispersants The dispersant is not particularly limited as long as it can produce organic polymer particles. Specific examples of the dispersant include polyvinylpyrrolidone (PVP), hydroxypropyl cellulose (HPC), polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene glycol (PPG), polypropylene oxide (PPO), collagen, polysaccharides (gum arabic), etc.
[0087] If polyvinylpyrrolidone or hydroxypropyl cellulose is used as a dispersant, aggregation of the polystyrene particles can be suppressed, and aggregation of the core-shell particles formed in the next step 2 can also be suppressed.
[0088] The dispersant may be used alone or in combination of two or more kinds (blend).
[0089] In step 1, the concentration of the dispersant in the solution is not particularly limited. The concentration of the dispersant in the solution is preferably 0.01% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, relative to 100% by mass of the solution. By adjusting the concentration of the dispersant within the above range, it is possible to suppress the aggregation of the organic polymer particles, and it is possible to suppress the aggregation of the core-shell particles formed in the next step 2.
[0090] solvent The solvent used in step 1 is preferably water.
[0091] The solvent used is preferably a hydrophilic solvent.
[0092] The hydrophilic solvent is preferably an alcohol such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol, 1,4-butanediol, etc. The hydrophilic solvent is preferably a ketone such as acetone, methyl ethyl ketone, etc. The hydrophilic solvent is preferably an ester such as ethyl acetate, etc.
[0093] As the hydrophilic solvent, preferably, alcohols are used, and more preferably, methanol, ethanol, isopropanol, or the like is used.
[0094] The solvent may be one of these solvents alone or a mixture (blend) of two or more of them.
[0095] The solvent used in step 1 is preferably a mixed solvent of water and methanol. By using a mixed solvent of water and methanol, aggregation of the organic polymer particles can be suppressed, and aggregation of the core-shell particles formed in the next step 2 can be suppressed.
[0096] The mass ratio of water to methanol (water:methanol) in the mixed solvent is preferably 5:95 to 50:50, more preferably 8:92 to 40:60, and even more preferably 10:90 to 30:70. By adjusting the mass ratio of water to methanol within the above range, aggregation of the organic polymer particles can be suppressed, and aggregation of the core-shell particles formed in the next step 2 can be suppressed.
[0097] Cationic Polymerization Initiator In step 1, the solution preferably contains a cationic polymerization initiator. The cationic polymerization initiator is not particularly limited as long as organic polymer particles can be obtained. The cationic polymerization initiator is preferably an inorganic peroxide, an organic initiator, a redox agent, or the like. The cationic polymerization initiator is more preferably a radical polymerization initiator such as an organic oxide or an azo compound.
[0098] The organic oxide is represented by the general formula RO-OR.
[0099] Azo compounds are represented by the general formula A-CN=CN-A.
[0100] Specific examples of the cationic polymerization initiator include benzoyl peroxide, 2,2'-azobis(isobutylamidine) dihydrochloride (AIBA), 4,4'-azobis-4-cyanovaleric acid, azobisisobutyronitrile (AIBN), and 2,2'-azobis(2-methylpropioamide) dihydrochloride (AAPH).
[0101] The cationic polymerization initiator is preferably 2,2'-azobis(isobutylamidine) dihydrochloride (AIBA), 2,2'-azobis(2-methylpropioamide) dihydrochloride (AAPH), more preferably 2,2'-azobis(isobutylamidine) dihydrochloride (AIBA), 4,4'-azobis-4-cyanovaleric acid, etc., and further preferably 2,2'-azobis(isobutylamidine) dihydrochloride (AIBA).
[0102] The cationic polymerization initiator may be used alone or in combination of two or more kinds (blend).
[0103] In step 1, the concentration of the cationic polymerization initiator in the solution is not particularly limited. The concentration of the cationic polymerization initiator is preferably 0.01% by mass to 1% by mass, with the solution being 100% by mass. By adjusting the concentration of the cationic polymerization initiator to the above range, the average particle size of the silica particles in the final product can be well controlled.
[0104] Polymerization Reaction In step 1, a polymerization reaction of the organic monomer is carried out in a solution containing the organic monomer, a dispersant, and a solvent. The polymerization reaction is preferably carried out by mixing and stirring the solution.
[0105] There is no particular limitation on the temperature during the polymerization reaction of the solution in step 1. The reaction temperature of the polymerization reaction is preferably 40° C. or higher and not higher than the boiling point of the solvent used, more preferably 50° C. to 90° C. By adjusting the reaction temperature of the polymerization reaction within the above range, the solvent does not evaporate, and the polymerization reaction can proceed smoothly.
[0106] The reaction time of the polymerization reaction is not particularly limited. The reaction time of the polymerization reaction is preferably 1 minute to 12 hours, and more preferably 10 minutes to 10 hours. By adjusting the reaction time of the polymerization reaction within the above range, the polymerization reaction can be smoothly carried out.
[0107] Organic polymer particles are prepared by carrying out a polymerization reaction. The average particle size of the organic polymer particles is preferably 0.1 μm to 0.9 μm, more preferably 0.2 μm to 0.8 μm, and even more preferably 0.3 μm to 0.7 μm. By adjusting the average particle size of the organic polymer particles to the above range, the average particle size of the core-shell particles formed in the next step 2 and the average particle size of the hollow silica particles produced in step 3 can be adjusted to appropriate ranges.
[0108] According to step 1, organic polymer particles can be successfully produced.
[0109] Yield of organic polymer particles (polystyrene particles, etc.) 2 g of the organic polymer particle reaction liquid is weighed out into a petri dish and dried on a hot plate at 120° C. for 1 hour, and the yield of the organic polymer particles is calculated according to the following formula.
[0110] (Yield of organic polymer particles (%)) = {[(Sample weight after drying (g)) - (Weight of dispersant (PVP, etc.) in sample before drying (g))] ÷[Weight of organic monomer (styrene, etc.) in sample before drying (g)] × 100
[0111] (2) Step 2 (production of core-shell particles) Step 2 is a step in which the organic polymer particles prepared in step 1, an alkoxysilane or an alkoxysilane and a metal alkoxide, and a basic catalyst are added to a solvent, and stirred to prepare a solution, and core-shell particles having the organic polymer particles as a core and a shell covering the organic polymer particles are formed in the solution.
[0112] solvent Water is preferably used as the solvent used in step 2. When water is used, core-shell particles can be formed inexpensively and safely.
[0113] The solvent used is preferably a hydrophilic solvent.
[0114] The hydrophilic solvent is preferably an alcohol such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol, 1,4-butanediol, etc. The hydrophilic solvent is preferably a ketone such as acetone, methyl ethyl ketone, etc. The hydrophilic solvent is preferably an ester such as ethyl acetate, etc.
[0115] As the hydrophilic solvent, preferably, alcohols are used, and more preferably, methanol, ethanol, isopropanol, or the like is used.
[0116] The solvent is preferably the same type of alcohol as that produced by hydrolysis of the silicon compound. By using the same type of alcohol as that produced by hydrolysis of the silicon compound, the solvent can be easily recovered and reused.
[0117] The solvent may be one of these solvents alone or a mixture (blend) of two or more of them.
[0118] The solvent is preferably a mixed solvent of water and a hydrophilic solvent. In the mixed solvent, the mass ratio of the hydrophilic solvent (e.g., methanol) to water is not particularly limited. In the mixed solvent, the hydrophilic solvent:water (mass ratio) is preferably 50:50 to 90:10, and more preferably 60:40 to 80:20. By adjusting the mass ratio of the hydrophilic solvent to water in the mixed solvent to the above range, the average particle size of the silica particles can be set to an appropriate range.
[0119] The solvent is preferably a hydrophobic solvent. The hydrophobic solvent is preferably an organic hydrocarbon solvent having a water solubility of less than about 1 g per 100 g at 100° C. The hydrophobic solvent is preferably a linear, branched or cyclic alkane having 6 to 10 carbon atoms. Specific examples of the hydrophobic solvent include hexane, cyclohexane, heptane, octane and isooctane. More preferably, the hydrophobic solvent is octane.
[0120] Organic Polymer Particles As the organic polymer particles used in step 2, the organic polymer particles prepared in step 1 are used.
[0121] The concentration of the organic polymer particles in the solution is preferably 0.01% by mass to 50% by mass, and more preferably 0.01% by mass to 20% by mass.
[0122] Alkoxysilane The alkoxysilane used in step 2 is not particularly limited.
[0123] The alkoxysilane preferably has the general formula (1): Si(OR 1 )4(1) The compound is a tetraalkoxysilane represented by the following formula (I) or a derivative thereof.
[0124] In the general formula (1), R 1 are the same or different and are alkyl groups, preferably lower alkyl groups having 1 to 8 carbon atoms, more preferably lower alkyl groups having 1 to 4 carbon atoms, and even more preferably lower alkyl groups having 1 to 3 carbon atoms.
[0125] In the general formula (1), R 1 Specifically, it is a methyl group, an ethyl group, a propyl group, an isobutyl group, a butyl group, a pentyl group, or a hexyl group.
[0126] In the general formula (1), R 1 Tetramethoxysilane (TMOS), where R is a methyl group 2 When tetraethoxysilane (TEOS), in which the alkoxysilane group is an ethyl group, is used, silica is produced well and a dense shell can be obtained. The alkoxysilane used in step 2 is more preferably tetramethoxysilane (TMOS). A dense shell is a shell in which siloxane bonds are more (almost) formed and there are fewer remaining silanol groups.
[0127] The alkoxysilane preferably has the general formula (2): Si(OR 1 )3R 2 (2) or a derivative thereof.
[0128] In the general formula (2), R 1 is R in the general formula (1). 1 In the general formula (2), R 2is hydrogen, or 1 (R in general formula (1) 1 ) is the same alkyl group as
[0129] The derivative of an alkoxysilane is preferably a low condensate obtained by partially hydrolyzing an alkoxysilane.
[0130] The alkoxysilane may be used alone or in combination of two or more kinds (blend).
[0131] When trialkoxysilane or tetraalkoxysilane is used as the alkoxysilane, aggregation can be prevented at the core-shell particle stage, and surface modification with a silane coupling agent or the like can be easily performed.
[0132] The concentration of the alkoxysilane in the solution is preferably 0.1% by mass to 70% by mass, more preferably 1% by mass to 60% by mass, even more preferably 5% by mass to 50% by mass, and particularly preferably 10% by mass to 40% by mass.
[0133] Metal Alkoxide In step 2, the alkoxysilane and the metal alkoxide may be used in combination.
[0134] The metal alkoxide is not particularly limited, but the metal alkoxide preferably used is aluminum alkoxide, titanium alkoxide, zirconium alkoxide, or the like.
[0135] By using aluminum alkoxide, the surface charge (zeta potential, etc.) of the shell can be adjusted.
[0136] By using titanium alkoxide or zirconium alkoxide, the refractive index of the shell can be adjusted.
[0137] The metal alkoxide may be used alone or in combination of two or more kinds (blend).
[0138] The concentration of the metal alkoxide in the solution is preferably 0.01% by mass to 50% by mass, and more preferably 0.01% by mass to 20% by mass.
[0139] In step 2, the alkoxysilane and the metal alkoxide may be added separately to prepare the solution.
[0140] In step 2, an alkoxysilane and a metal alkoxide may be mixed, hydrolyzed, and then added to the solution. By mixing an alkoxysilane and a metal alkoxide, hydrolyzing the mixture, and then adding the mixture to the solution, the reaction proceeds according to the following formula (1): Si-OM (1) and capable of forming a shell in which the metal represented by M in formula (1) is uniformly contained.
[0141] In the formula (1), M represents a metal, and is a metal derived from a metal alkoxide, and preferably represents aluminum, titanium, or zirconium.
[0142] The above-mentioned alkoxysilane and metal alkoxide are mixed, hydrolyzed, and then added to the solution, for example, the method described in JP-A-2005-41722 is adopted.
[0143] Basic Catalyst The basic catalyst used in step 2 is not particularly limited.
[0144] When an organic base catalyst not containing a metal component or an inorganic catalyst not containing a metal component is used as the basic catalyst, it is possible to prevent the inclusion of metal impurities in the production process.
[0145] The organic base catalyst is preferably a nitrogen-containing organic base catalyst such as ethylenediamine, diethylenetriamine, triethylenetetraamine, urea, ethanolamine, tetramethylammonium hydroxide (TMAH), tetramethylguanidine, or a basic amino acid.
[0146] In step 2, if a low-volatility organic base catalyst is used, the reaction can proceed smoothly without volatilization in the temperature range in which step 2 is performed. When a volatile base is used, the pH of the solution can be maintained by continuously adding the base.
[0147] The inorganic base catalyst is preferably aqueous ammonia, which is inexpensive, economically advantageous, and allows the reaction to proceed smoothly.
[0148] The basic catalyst may be used alone or in combination of two or more kinds (blend).
[0149] The concentration of the basic catalyst in the solution is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass.
[0150] In step 2, the organic polymer particles (polystyrene particles, etc.) prepared in step 1, an alkoxysilane or an alkoxysilane and a metal alkoxide, and a basic catalyst are added to a solvent and stirred to prepare a solution, and core-shell particles having the organic polymer particles as a core and a shell covering the organic polymer particles can be formed in the solution.
[0151] Production of core-shell particles The temperature of the solution in step 2 is not particularly limited. The temperature of the solution in step 2 is preferably 5° C. to 200° C., and more preferably 5° C. to 150° C. By adjusting the temperature of the solution in step 2 within the above range, the solvent does not evaporate, and the reaction can proceed smoothly.
[0152] The stirring time in step 2 is not particularly limited. The stirring time in step 2 is preferably 1 minute to 1,200 minutes, and more preferably 1 minute to 600 minutes. By adjusting the stirring time in step 2 to within the above range, the polymerization reaction can be smoothly carried out.
[0153] By the step 2, it is possible to satisfactorily form core-shell particles having the organic polymer particles (polystyrene particles, etc.) prepared in the step 1 as a core and a silica-based shell covering the polystyrene particles.
[0154] (3) Step 3 (production of silica particles) The method for producing silica particles of the present invention includes a step (step 3) of first carbonizing (thermally decomposing) the core-shell particles (the core-shell particles obtained in step 2) and then baking the particles, thereby removing the organic polymer particles that are the cores of the core-shell particles.
[0155] The carbonization treatment is preferably carried out in the temperature range of 400°C to 1,200°C.
[0156] The calcination treatment is preferably carried out for a treatment time of 3 hours or more.
[0157] Step 3 is a step of removing the organic polymer particles, which are the cores of the core-shell particles, by carbonizing (thermal decomposition) the core-shell particles obtained in step 2. The inside of the core-shell particles is filled with organic polymer particles as the cores, and by carbonizing (thermal decomposing) these organic polymer particles, the organic polymer particles, which are the cores of the core-shell particles, are removed, making the inside of the shell hollow, and it is possible to produce silica particles that can be used satisfactorily as a highly functional material.
[0158] In the method for producing silica particles of the present invention, when producing silica particles, core-shell particles are subjected to a carbonization treatment before being fired, making it possible to produce new silica particles having a low true density and excellent dispersibility.
[0159] In step 3, the organic polymer particles are removed by pyrolysis. The pyrolysis is carried out by first carbonizing the silica particles and then baking them. The temperatures of the carbonizing and baking processes are adjusted so that the shells of the silica particles (hollow silica particles) are not destroyed, and the organic polymer particles and other organic components that may remain inside the silica particles are removed.
[0160] Carbonization Step 3 is carried out by first carbonizing the core-shell particles and then calcining them.
[0161] When the core-shell particles are heat-treated in air, the organic polymer in the core of the silica particles decomposes and gasifies (cracked gas). When the cracked gas is generated in this way, it may ignite in the electric furnace, or the cracked gas may pass through the shell of the silica particles and be ejected, causing holes in the shell, which may reduce the true density of the hollow silica.
[0162] From this point of view, the carbonization treatment is preferably a heat treatment performed in a low-oxygen state.
[0163] The carbonization treatment is preferably a heat treatment in a low-oxygen state, for example, by filling a heating furnace with an inert gas (Ar gas, CO2, etc.), N2 gas, or water vapor (H2O) to prevent the generation of decomposition gas. The carbonization treatment may be performed using a carbonization device that can be used appropriately under an atmosphere of an inert gas, N2 gas, or water vapor (H2O).
[0164] When the carbonization treatment is carried out under an inert gas or N2 gas atmosphere, for example, a batch furnace (a gas atmosphere device in which an inert gas such as N2, CO2, or Ar is introduced into the furnace to perform heat treatment in a low oxygen concentration, heat treatment temperature: about 550°C, for example, Thermal Corporation, hot air circulation type inert gas atmosphere device, medium temperature heat treatment machine RBA type) is preferably used.
[0165] When the carbonization treatment is carried out under an inert gas or N2 gas atmosphere, for example, a continuous furnace (heat treatment temperature: about 450°C to 800°C, a gas heating device that continuously carries out the carbonization treatment within a single tube, for example, Takasago Industrial Co., Ltd., gas heated rotary kiln) is preferably used.
[0166] When the carbonization treatment is carried out in a superheated steam atmosphere, for example, a batch furnace (for example, CYC Corporation, batch type carbonization apparatus, CYT series, CYT-200, etc.) is preferably used.
[0167] The carbonization treatment (pyrolysis) is carried out using a carbonization apparatus, preferably a batch-type carbonization apparatus.
[0168] When a batch-type carbonization device is used, 1. the thermal effect due to direct heating is excellent, 2. the temperature inside the carbonization chamber (pyrolysis chamber, dry distillation box) can be made uniform due to the convection effect, 3. the contact area with the material to be carbonized can be increased due to the convection effect, and 4. it is a sealed type (with a double structure) that blocks oxygen (under oxygen-free conditions) and heats the pyrolysis chamber, allowing carbonization to proceed smoothly.
[0169] By using a carbonizer to carbonize the core-shell particles (dry powder), the carbonization process can be carried out efficiently. In the carbonizer, the carbonization chamber is heated and superheated steam is used to evaporate the moisture from the organic polymer particles when the temperature reaches around 400°C.
[0170] In the carbonization process, the core-shell particles (dry powder) are placed in a carbonization chamber (carbonization box), and while supplying superheated steam into the carbonization chamber (carbonization box), the core-shell particles (dry powder) are heated from outside the carbonization chamber (carbonization box) by combustion gas. In the carbonization process, the core-shell particles (dry powder) are carbonized by supplying superheated steam into the carbonization chamber (carbonization box).
[0171] In the carbonization treatment, the core-shell particles (dry powder) are carbonized using superheated steam, preferably in a temperature range of 400° C. to 1,200° C. In the carbonization step, the core-shell particles (dry powder) are carbonized using superheated steam, more preferably in a temperature range of 450° C. to 800° C., and even more preferably in a temperature range of 500° C. to 700° C. (low temperature region).
[0172] The carbonization time is not particularly limited and is appropriately adjusted, preferably 1 hour to 12 hours, more preferably 2 hours to 10 hours, and further preferably 4 hours to 8 hours.
[0173] The carbonization process uses superheated steam, which reduces the temperature difference within the carbonization chamber (distillation box) through the convection effect, allowing the carbonization process to proceed smoothly.
[0174] The carbonization treatment can be preferably performed using a commercially available carbonization device, using superheated steam at a temperature range of about 450° C. to 550° C. for 4 to 8 hours. The carbonization device can be, for example, a batch-type carbonization device manufactured by CYC Corporation (CYT series, CYT-200, etc.).
[0175] In the method for producing silica particles of the present invention, when producing silica particles, core-shell particles are subjected to a carbonization treatment before being fired, making it possible to produce new silica particles having a low true density and excellent dispersibility.
[0176] Firing process Step 3 is carried out by first carrying out a carbonization treatment and then a calcination treatment.
[0177] The firing treatment is preferably carried out using an electric furnace.
[0178] The calcination treatment is performed by calcining the core-shell particles (dry powder) after the carbonization treatment in an electric furnace, preferably in a temperature range of 350°C to 1,500°C, more preferably in a temperature range of 400°C to 1,200°C, and even more preferably in a temperature range of 600°C to 1,100°C (high temperature range).
[0179] The calcination treatment is preferably performed for a treatment time of 3 hours or more. The calcination treatment time is more preferably 4 hours or more, even more preferably 5 hours or more, and particularly preferably 6 hours or more. The upper limit of the calcination treatment time is about 10 hours.
[0180] In order to remove the organic polymer particles, a baking treatment is carried out after the carbonization treatment, whereby destruction of the shell is suppressed and the organic polymer particles can be satisfactorily removed from the core-shell particles.
[0181] The firing treatment can be preferably performed using a commercially available electric furnace at a temperature range of about 1,000° C. to 1,100° C. for a treatment time of 3 hours or more.
[0182] The powder of hollow silica particles obtained by removing the organic polymer particles from the organic core-shell particles is called hollow silica particles. The obtained powder of hollow silica particles can be dispersed in a solvent using a dispersing machine, and subsequently subjected to a hydrophobizing treatment.
[0183] A dispersing machine, preferably an ultrasonic homogenizer, a bead mill or the like is used.
[0184] In step 3, the organic polymer particles, which are the cores of the core-shell particles, are thermally decomposed, and the organic polymer particles can be removed.
[0185] Through step 3 and the subsequent steps, (1) True density is 0.8 g / cm 3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less; (3) Silica particles (hollow silica particles) having a water absorption of 1.0 mass % or less can be produced.
[0186] (4) Shell coating process The method for producing silica particles of the present invention may further include, after step 3, a step of coating the surfaces of the silica particles (hollow silica particles) with a shell.
[0187] The average thickness of the shell of the silica particles can be adjusted by further coating the surface of the silica particles with a shell.
[0188] The method of coating the surface of the silica particles with a shell is not particularly limited. The method of coating the surface of the silica particles with a shell is preferably similar to the method of producing the core-shell particles in step 2, and the organic polymer particles in step 2 are changed to the hollow silica particles obtained in step 3, and the surface of the hollow silica particles can be further coated with a shell.
[0189] (5) Step 4 (Hydrophobic treatment of hollow silica particles) The method for producing silica particles of the present invention preferably includes, after step 3 or the shell-coating step, step 4 of subjecting the hollow silica particles obtained in step 3 to a hydrophobic treatment (hydrophobic surface treatment). Step 4 can effectively impart hydrophobicity to the surfaces of the hollow silica particles.
[0190] The method of hydrophobization is not particularly limited. The method of hydrophobization is preferably a method of adding trialkoxysilane and organosilazane to the hollow silica particles obtained in step 3 or the shell coating step in a solvent and heating the mixture after step 3 or the shell coating step.
[0191] A trialkoxysilane and an organosilazane may be used in combination.
[0192] solvent The solvent used in step 4 is preferably water.
[0193] The solvent used is preferably a hydrophilic solvent.
[0194] The hydrophilic solvent is preferably an alcohol such as methanol, ethanol, n-propanol, isopropanol (IPA), ethylene glycol, propylene glycol, 1,4-butanediol, etc. The hydrophilic solvent is preferably a ketone such as acetone, methyl ethyl ketone, etc. The hydrophilic solvent is preferably an ester such as ethyl acetate, etc.
[0195] As the hydrophilic solvent, preferably, alcohols are used, and more preferably, methanol, ethanol, isopropanol, or the like is used.
[0196] When an alcohol such as isopropanol is used as the solvent, the hollow silica particles can be effectively subjected to the hydrophobic treatment.
[0197] The solvent may be one of these solvents alone or a mixture (blend) of two or more of them.
[0198] The solvent is preferably a mixed solvent of water and a hydrophilic solvent. In the mixed solvent, the mass ratio of the hydrophilic solvent (e.g., methanol) to water is not particularly limited. In the mixed solvent, the hydrophilic solvent:water (mass ratio) is preferably 90:10 to 10:90, and more preferably 30:70 to 10:90. By adjusting the mass ratio of the hydrophilic solvent to water in the mixed solvent to within the above range, the hollow silica particles can be satisfactorily hydrophobized.
[0199] Trialkoxysilane The trialkoxysilane is not particularly limited. The trialkoxysilane is preferably 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, trifluoropropyltrimethoxysilane, etc. The trialkoxysilane is more preferably 3-methacryloxypropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, trifluoropropyltrimethoxysilane, etc.
[0200] The trialkoxysilane may be used alone or in combination of two or more kinds (blend).
[0201] The concentration of the trialkoxysilane in the solution is preferably 0.01% by mass to 30% by mass, and more preferably 0.05% by mass to 25% by mass.
[0202] The amount of trialkoxysilane used is not particularly limited. The amount of trialkoxysilane used is preferably 0.01% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, and even more preferably 0.1% by mass to 3% by mass, based on 100% by mass of silica. By adjusting the amount of trialkoxysilane used within the above range, the hollow silica particles can be satisfactorily hydrophobized.
[0203] The hydrophobization treatment using trialkoxysilane is carried out by heating, preferably at 30° C. or higher, more preferably at 40° C. or higher, and even more preferably at 50° C. or higher. The upper limit of the heating temperature is preferably 90° C. or lower, more preferably 80° C. or lower. By adjusting the heating temperature of the hydrophobization treatment using trialkoxysilane to within the above range, the reaction between the silica particles and the trialkoxysilane can be favorably carried out in the solvent without aggregation.
[0204] The heating time for the hydrophobization treatment using trialkoxysilane is not particularly limited, and is preferably 10 minutes to 48 hours, more preferably 30 minutes to 24 hours, and even more preferably 1 hour to 20 hours.
[0205] Organosilazanes The organosilazane is not particularly limited, but preferably, tetramethyldisilazane, hexamethyldisilazane, pentamethyldisilazane, or the like is used.
[0206] The organosilazanes may be used alone or in combination (blended) of two or more kinds.
[0207] The amount of organosilazane used is not particularly limited. The amount of organosilazane used is preferably 10% by mass to 100% by mass, more preferably 20% by mass to 90% by mass, and even more preferably 40% by mass to 80% by mass, based on 100% by mass of silica. By adjusting the amount of trialkoxysilane used within the above range, the hollow silica particles can be satisfactorily hydrophobized.
[0208] The hydrophobization treatment using organosilazane is carried out by heating, preferably at 30° C. or higher, more preferably at 40° C. or higher, and even more preferably at 50° C. or higher. The upper limit of the heating temperature is preferably 90° C. or lower, more preferably 80° C. or lower. By adjusting the heating temperature of the hydrophobization treatment using organosilazane to within the above range, the reaction between the silica particles and the organosilazane can be favorably carried out in the solvent without aggregation.
[0209] The heating time for the hydrophobization treatment using organosilazane is not particularly limited, and is preferably 10 minutes to 48 hours, more preferably 30 minutes to 24 hours, and even more preferably 1 hour to 20 hours.
[0210] A trialkoxysilane and an organosilazane may be used in combination.
[0211] The solvent of the solution containing the hydrophobized hollow silica particles may be replaced with another solvent (water, etc.). The solution containing the hydrophobized hollow silica particles may be filtered or dried (vacuum drying, etc.) to remove the solvent, and a solution powder containing the hydrophobized hollow silica particles may be prepared.
[0212] [4] Manufacturing method of core-shell particles The method for producing the core-shell particles of the present invention preferably comprises the steps of: (1) Step 1 of preparing organic polymer particles by carrying out a polymerization reaction of an organic monomer in a solution containing an organic monomer, a dispersant, and a mixed solvent; and (2) A step 2 includes adding the organic polymer particles obtained in the step 1, an alkoxysilane or an alkoxysilane and a metal alkoxide, and a basic catalyst to a solvent, and stirring the mixture to prepare a solution, thereby forming core-shell particles having the organic polymer particles as a core and a shell covering the organic polymer particles in the solution.
[0213] Steps 1 and 2 are the same as steps 1 and 2 described in the method for producing silica particles.
[0214] The core-shell particles produced by the core-shell particle manufacturing method of the present invention are suitable as the core-shell particles to be used in step 3 of the silica particle manufacturing method of the present invention, after the organic polymer particles, which are the cores of the core-shell particles, are removed by carbonization treatment (thermal decomposition). EXAMPLES
[0215] The present invention will now be described in detail with reference to examples.
[0216] However, the present invention is not limited to the examples.
[0217] Polystyrene particles and core-shell particles were prepared and hollow silica particles were produced according to the formulation and production conditions in Table 1. Specifically, the procedures are as follows.
[0218] (1) Examples and Comparative Examples Example 1 Step 1: Production of polystyrene particles First, 737 g of ultrapure water, 2949 g of methanol, and 369 g of styrene monomer (organic monomer) were poured into a four-neck flask, and the contents were heated to an internal temperature of 55°C to 70°C while stirring at 250 rpm in a nitrogen atmosphere.
[0219] Next, a 5 wt % aqueous solution of AIBA (2,2'-azobis(isobutylamidine)dihydrochloride) (AIBA 7 g, ultrapure water 140 g) previously dissolved in ultrapure water was added as a polymerization initiator, and a polymerization reaction was carried out at 55°C to 75°C for 3 hours.
[0220] Thereafter, a 5% aqueous methanol solution of polyvinylpyrrolidone (PVP) (37 g PVP, 560 g methanol, 140 g water) was added as a dispersant, and the mixture was further heated under reflux for 3 hours to prepare a polystyrene particle reaction liquid.
[0221] As PVP, "PVP K-90 manufactured by Ashaland" and "Pittscol K-60L manufactured by Daiichi Kogyo Co., Ltd." are available. In the examples, "PVP K-90 manufactured by Ashaland" was used as PVP.
[0222] The polystyrene particle reaction liquid was poured into another four-neck flask and heated with a mantle heater to replace the reaction liquid with methanol, and the reaction was completed when the internal temperature reached 70°C.
[0223] Polystyrene particles, which are organic polymer particles, were prepared in methanol.
[0224] <Polystyrene particle yield> 2 g of the polystyrene particle reaction liquid was weighed out into a petri dish and dried on a hot plate at 120° C. for 1 hour, and the yield of polystyrene particles was calculated according to the following formula.
[0225] (Polystyrene particle yield (%)) = {[(Weight of sample after drying (g))-(Weight of PVP charged in sample before drying (g))] ÷ [Weight of styrene charged in sample before drying (g)]} × 100
[0226] Step 2: Preparation of core-shell particles First, a reaction apparatus equipped with a four-neck flask, a stirring blade, and a water bath was prepared.
[0227] Liquid A was prepared by mixing 376 g of TMOS (tetramethoxysilane) (alkoxysilane) and 744 g of methanol.
[0228] In addition, 1,427 g of the polystyrene particle dispersion liquid (polystyrene concentration: 7.6 wt %) produced in step 1 was placed in a flask, 829 g of water and 823 g of methanol were added as solvents, and 268 g of 28% aqueous ammonia solution (basic catalyst) was added to prepare liquid B.
[0229] While maintaining the temperature of solution B at 30° C., solution A was added thereto over a period of 190 minutes under stirring at 250 rpm.
[0230] In the solution, polystyrene particles were used as the core, and core-shell particles having a silica-based shell covering the polystyrene particles were formed to prepare a core-shell particle dispersion. Next, water was added dropwise, and while maintaining the same volume or more, the water and ammonia in the concentrated solution were replaced with water by heating and normal pressure distillation, thereby preparing a core-shell particle aqueous dispersion.
[0231] Step 3: Production of hollow silica particles (carbonization treatment) The aqueous dispersion of core-shell particles obtained in step 2 was dried on a hot plate at a temperature of 130° C. to obtain a powder of core-shell particles.
[0232] First, the obtained core-shell particle powder was carbonized in a batch carbonizer (CYT-200, manufactured by CYC Corporation) using superheated steam at a temperature of 500° C. for 4 hours.
[0233] Next, the mixture was calcined (heat-treated) in an electric furnace at 1,050° C. for 3 hours to remove the polystyrene particles and produce a powder of hollow silica particles.
[0234] Pure water was added to the obtained hollow silica particle powder (silica concentration: 20 wt%), and the mixture was dispersed for 135 minutes using an ultrasonic homogenizer (UP-400S, manufactured by Hielscher).
[0235] The obtained dispersion was centrifuged at 3,200 rpm for 10 minutes using a high-speed microcentrifuge (Hitachi Koki Co., Ltd., himac CF-16N) to recover the supernatant, which was then filtered using a 7 μm quantitative filter paper to obtain a hollow silica particle dispersion (silica concentration 16 wt%).
[0236] The silica concentration was calculated from the remaining amount after drying the hollow silica particle dispersion and then heating it at 800°C.
[0237] Step 4: Preparation of surface-treated hollow silica particles First, a reaction apparatus equipped with a four-neck flask, a stirring blade, and a water bath was prepared. In the flask, 400 g of the hollow silica water dispersion obtained in step 3, 274 g of ultrapure water, 404 g of IPA (isopropanol), and 1.4 g of N-phenyl-3-aminopropyltrimethoxysilane (KBM-573, manufactured by Shin-Etsu Chemical Co., Ltd.) (trialkoxysilane) were mixed and stirred, and heated at 75° C. for 1 hour.
[0238] Next, 39 g of hexamethyldisilazane (SZ-31, manufactured by Shin-Etsu Chemical Co., Ltd.) (organosilazane) was added dropwise, and the mixture was heated for a further 2 hours.
[0239] Next, the reaction liquid was cooled to 50° C., and 559 g of ultrapure water and 31 g of 3M sulfuric acid were added in that order, and the solid content was recovered by filtration under reduced pressure.
[0240] The recovered solid was washed with ultrapure water and dried in vacuum at 120°C to prepare hollow silica particles.
[0241] Example 2 In step 4 of Example 1, N-phenyl-3-aminopropyltrimethoxysilane was not mixed, and only 394 g of hexamethyldisilazane was added dropwise.
[0242] Other than that, the experiment was carried out under the same conditions as in Example 1.
[0243] Example 3 In step 4 of Example 1, 400 g of the hollow silica particle aqueous dispersion, 274 g of ultrapure water, 404 g of IPA, and 1.1 g of N-phenyl-3-aminopropyltrimethoxysilane were mixed and stirred, and heated at 75° C. for 1 hour.
[0244] Other than that, the experiment was carried out under the same conditions as in Example 1.
[0245] Comparative Example 1 In step 3 of Example 1, the core-shell particles were not carbonized but were calcined (heat-treated) in an electric furnace at 1,050° C. for 3 hours.
[0246] Other than that, the experiment was carried out under the same conditions as in Example 1.
[0247] Comparative Example 2 In step 3 of Example 1, the core-shell particle powder was first carbonized using superheated steam in a batch carbonizer (CYT-200, CYC Corporation) at a temperature of 500°C for 4 hours, and then calcined (heat-treated) in an electric furnace at a temperature of 1,075°C for 2 hours.
[0248] Other than that, the experiment was carried out under the same conditions as in Example 1.
[0249] Comparative Example 3 In step 3 of Example 1, the core-shell particle powder was first carbonized using superheated steam in a batch carbonizer (CYT-200, CYC Corporation) at a temperature of 500°C for 4 hours, and then calcined (heat-treated) in an electric furnace at a temperature of 1,000°C for 1 hour.
[0250] Other than that, the experiment was carried out under the same conditions as in Example 1.
[0251] Comparative Example 4 In step 3 of Example 1, 7.7 g of citric acid (anhydrous citric acid, manufactured by Fuso Chemical Co., Ltd.) was added to the aqueous dispersion of core-shell particles, and the mixture was dried on a hot plate at a temperature of 130°C to obtain a powder of core-shell particles.
[0252] The obtained core-shell particle powder was not carbonized, but was heat treated in an electric furnace at 1,050° C. for 3 hours.
[0253] Other than that, the experiment was carried out under the same conditions as in Example 1.
[0254] The properties of the particles obtained in the examples and comparative examples were measured by the following methods.
[0255] (2) Evaluation test Particle size The powder of hollow silica particles obtained in step 4 was photographed using a SEM (scanning electron microscope: JSM-7900F, manufactured by JEOL Ltd.) at an acceleration voltage of 8 kV, and the short diameters of 100 randomly selected particles were measured and the average value was calculated.
[0256] Image analysis was performed using the image analysis and measurement software WinROOF.
[0257] true density The true density of 0.3 g of the hollow silica particle powder obtained in step 4 was measured using a nitrogen gas pycnometer (Ultrapyc 5000 Micro, manufactured by Anton Paar Japan Co., Ltd.).
[0258] Water Absorption Test 1 g of the hollow silica particle powder obtained in step 4 was stored for 7 days in an environment with a temperature of 50°C and a humidity of 75%, and 0.1 g of the powder was sampled and the moisture content (mass%) was measured using a Karl Fischer moisture meter (MKA-610, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).
[0259] MEK filterability 2 g of the hollow silica particle powder obtained in step 4 and 8 g of methyl ethyl ketone (MEK) were mixed and stirred for 2 hours, filtered using a 5 μm pore size syringe filter (filter paper that allows substances with a size of 5 μm or less to pass through), and the amount of liquid passing through was weighed.
[0260] (MEK filtration performance (mass%, wt%)) = [Amount of liquid passed (g)] ÷ [Amount of MEK dispersion of hollow silica particles (10 g)] × 100
[0261] Number of particles over 1μm (particle size distribution) The particle size distribution of the hollow silica particle powder obtained in step 4 was measured using a laser diffraction / scattering particle size distribution analyzer (LA-950, manufactured by Horiba, Ltd.), and the frequency (%) of particles with a particle diameter of 1 μm or more in the hollow silica particle powder was calculated.
[0262] The results are shown in Table 1.
[0263] [Table 1]
[0264] (3) Evaluation results The hollow silica particles in Comparative Example 1 were prepared by subjecting the core-shell particle powder to only a calcination treatment without a carbonization treatment. The hollow silica particles in Comparative Example 1 had a particle size distribution in which the frequency of particles larger than twice the average particle size exceeded 15%.
[0265] The hollow silica particles of Comparative Example 2 were prepared by carbonizing the core-shell particle powder and then calcining the carbonized core-shell particle powder for 2 hours. The hollow silica particles of Comparative Example 2 had a particle size distribution in which the frequency of particles larger than twice the average particle size exceeded 15%.
[0266] The hollow silica particles of Comparative Example 3 were prepared by carbonizing the core-shell particle powder and then calcining the carbonized core-shell particle powder for 1 hour. The hollow silica particles of Comparative Example 3 had a particle size distribution in which the frequency of particles larger than twice the average particle size exceeded 15%, and a water absorption amount exceeded 1.0% by mass.
[0267] The hollow silica particles of Comparative Example 4 were prepared by adding citric acid to an aqueous dispersion of core-shell particles, and then subjecting the core-shell particle powder to only a calcination treatment without a carbonization treatment. The hollow silica particles of Comparative Example 3 had a particle size distribution in which the frequency of particles larger than twice the average particle size exceeded 15%.
[0268] Examples 1 to 3 are embodiments of the present invention, and are hollow silica particles prepared by carbonizing a core-shell particle powder at a temperature range of 400° C. to 1,200° C. and then calcining the powder for a treatment time of 3 hours or more. The hollow silica particles of Examples 1 to 3 have the following characteristics: (1) a true density of 0.8 g / cm 3 ~1.4g / cm 3 (2) in the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less, and (3) the water absorption amount is 1.0 mass% or less.
[0269] (4) Industrial Applicability The hollow silica particles of the present invention are novel hollow silica particles having a low true density and excellent dispersibility.
[0270] According to the method for producing hollow silica particles of the present invention, when producing hollow silica particles, the core-shell particles are subjected to a carbonization treatment before being fired, whereby new hollow silica particles having a low true density and excellent dispersibility can be produced.
[0271] The hollow silica particles of the present invention are useful for multi-layer printed circuit boards, electric wire covering materials, semiconductor encapsulation materials, etc.
Claims
1. (1) True density is 0.8 g / cm 3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less, (3) The water absorption amount is 1.0% by mass or less. Silica particles.
2. The silica particles of claim 1, wherein the silica particles are (4) carbonized and calcined.
3. The silica particles according to claim 1 or 2, (5) having an average particle size of 0.2 μm to 1.0 μm.
4. The silica particles according to claim 1 or 2, wherein the silica particles are hollow silica particles.
5. A method for producing silica particles, comprising the steps of: The method includes a step of first carbonizing the core-shell particles and then calcining the same, The silica particles are (1) True density is 0.8 g / cm 3 ~1.4g / cm 3 and (2) In the particle size distribution, the frequency of particles larger than twice the average particle size is 15% or less; (3) The water absorption amount is 1.0% by mass or less. A method for producing silica particles.
Citation Information
Patent Citations
Hollow silica particles, compositions containing them, and methods for producing the same
JP2009504632A
Synthetic amorphous silica powder and method for producing same
JP2011157263A
Method for manufacturing spherical silica
JP2015113277A
Silica-based particle and use of the same
JP2015155373A
Hollow silica particles and method for producing the same
JP2020079165A