Thin type film treatment processing

A helium-containing plasma treatment with controlled substrate heating and RF bias improves the mechanical and electrical properties of thin films deposited by ALD and CVD, addressing the issues of poor film quality and enhancing device performance.

JP2024133460AInactive Publication Date: 2024-10-02APPLIED MATERIALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024088973
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-10-04
Filing Date
2024-05-31
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing thin film deposition methods, such as ALD and CVD, result in films with poor mechanical and electrical properties, leading to issues like current leakage and reduced dielectric constant, which are not effectively addressed by current ALD strategies.

Method used

A method involving the use of a helium-containing process gas and controlled plasma treatment to modify deposited thin films, with substrate heating and RF bias application, to improve film quality by removing impurities and altering bonding structures.

Benefits of technology

The treatment process enhances the mechanical and electrical properties of thin films, reducing gate leakage and ensuring proper device functionality by densifying and uniforming the film structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133460000001_ABST
    Figure 2024133460000001_ABST
Patent Text Reader

Abstract

To provide a method for modifying a film with a low quality in a semiconductor device.SOLUTION: A method comprises: a film deposition process 410 for accumulating a film with a low quality onto a semiconductor substrate; a first treatment process 420 for exposing a front surface of the film with the low quality to a first process gas containing helium during heating a substrate to a first temperature; and a second treatment process 430 for exposing a front surface of the film with the low quality to a second process gas containing an oxygen gas during heating the substrate at a second temperature that is different from the first temperature, and thereby an electrical characteristic of the film is improved. The first treatment process 420 and the second treatment process 430 are continuously repeated at a plurality of times in order to continue the improvement of a characteristic of a thin film to be treated.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to methods and apparatus for processing thin films used in semiconductor devices. [Background technology]

[0002]

[0002] In integrated circuits, smaller transistors, such as metal oxide semiconductor field effect transistors (MOSFETs), are highly desirable. First, smaller transistors allow more transistors to be formed in a given chip area, thereby reducing chip size. Second, smaller transistors typically switch faster than larger transistors, thereby improving chip performance.

[0003]

[0003] One approach to reduce the size of MOSFETs is by device scaling, where key device dimensions such as transistor length, transistor width, and oxide (or dielectric) thickness are scaled down proportionally. In this approach, the resistance of the transistor channel does not change as the transistor size is scaled down, but the gate capacitance and RC delay of the transistor decrease proportionally with the size scale down. A common method in the art to grow these increasingly thin films is to use atomic layer deposition (ALD) processes, which allow good control of thickness at the atomic level and provide good conformality of the film. One of the disadvantages of ALD is that the mechanical and electrical properties of the deposited thin films can be poor, leading to, for example, current leakage and reduced dielectric constant.

[0004]

[0004] As mentioned above, what is needed in the art is a method to improve the film properties of films deposited by chemical vapor deposition (CVD) or atomic layer deposition (ALD) processes. In addition, post-CVD or post-ALD film modification would allow those skilled in the art to use current ALD recipes and subsequently perform treatments to improve the as-deposited film without having to modify current ALD methods that are already functional and optimized.

[0005]

[0005] Therefore, what is needed is an apparatus and method for treating a deposited thin film to improve its mechanical and / or electrical properties. Summary of the Invention

[0006]

[0006] Embodiments of the present disclosure include a method of modifying a layer in a semiconductor device, comprising depositing a film having a poor film quality on a semiconductor substrate and exposing a surface of the poor quality film to a process gas comprising helium while the substrate is heated to a first temperature. In some embodiments, the process gas consists essentially of helium.

[0007]

[0007] Embodiments of the present disclosure may further include a method of modifying a layer used in a semiconductor device by exposing a surface of the layer to a first process gas comprising helium while the substrate is heated to a first temperature, and exposing the surface of the layer to a second process gas comprising oxygen gas while the substrate is heated to a second temperature different from the first temperature.

[0008]

[0008] The embodiments of the present disclosure can further include modifying layers used to form semiconductor devices to improve the mechanical and electrical properties of the layers. The electrical properties of the films are improved by subjecting them to the aforementioned methods. In addition, for films formed by ALD processes, post-ALD treatment processes allow users to use currently developed and optimized ALD process recipes.

[0009]

[0009] An embodiment of the present disclosure may further include a method of modifying a film having poor film quality in a semiconductor device, comprising exposing a surface of the poor film on the substrate to a plasma comprising a process gas including helium (He) while the substrate is heated to a first temperature between about 150°C and about 500°C and a substrate RF bias is applied to cause ions formed in the plasma to bombard the surface of the poor film. The method may also include applying a bias power to the substrate to energize the ions, where the ions have an energy between about 2 eV and about 2,000 eV and the plasma bombards the surface of the poor film with an energy of about 1 cubic centimeter (cm) over the surface of the poor film during processing. -3 ) has an average ion density of between about 1E10 and 1E12 ions per 100 .mu.m.

[0010]

[0010] An embodiment of the present disclosure may further include a method of modifying a poor quality film in a semiconductor device, comprising exposing a surface of a film disposed on a surface of a substrate to a plasma comprising a process gas including helium (He). The substrate is heated to a first temperature between about 350°C and about 500°C. The plasma is generated by applying a source power. The plasma is applied to the entire surface of the film being treated, with a volume of about 1 cubic centimeter (cm -3 ) has an ion density of about 1E10 to 1E12 ions per 100 .mu.m. In some embodiments of the method, the self-bias created causes ions created in the plasma to bombard the surface of the membrane.

[0011]

[0011] In order that the above-mentioned features of the present disclosure may be understood in detail, a more particular description of the present disclosure briefly summarized above will now be made with reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only exemplary embodiments and therefore should not be considered as limiting the scope thereof, as other equally effective embodiments may be recognized. [Brief description of the drawings]

[0012] [Figure 1]1 is a cross-sectional side view of a processing system according to one embodiment. [Diagram 2]

[0013] 1 is a method for treating poor quality membranes according to one embodiment. [Diagram 3]

[0014] FIG. 1A is a side view of a substrate according to one embodiment.

[0015] FIG. 2B is a side view of a substrate during growth of a film according to one embodiment.

[0016] FIG. 2C is a side view of a substrate having a film undergoing a first process according to one embodiment. [Figure 4]

[0017] 1 is a method for treating a dielectric film according to one embodiment. [Diagram 5]

[0018] FIG. 1A is a side view of a substrate according to one embodiment.

[0019] FIG. 2B is a side view of a substrate during growth of a film according to one embodiment.

[0020] FIG. 2C is a side view of a substrate having a film undergoing a first process according to one embodiment.

[0021] FIG. 4D is a side view of a substrate having a film undergoing a second process according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013]

[0022] To facilitate understanding, the same reference numbers have been used, where possible, to designate identical elements that are common to multiple figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.

[0014]

[0023] The embodiments of the present disclosure provided herein include a process for treating a film to improve the electrical and / or mechanical properties of the film having poor quality. In some embodiments, the process includes improving the properties of a deposited chemical vapor deposition (CVD) or atomic layer deposition (ALD) layer by exposing the deposited film, maintained at a controlled temperature, to a plasma having a desired ion density while a controlled bias power bombards the surface of the deposited thin film with ions formed in the plasma. In some embodiments, the ions formed in the plasma include helium ions, which, due to the bias power and / or self-bias created by the plasma, can impart kinetic energy to the constituent atoms of the deposited film, densifying the deposited thin film, removing contaminants (e.g., hydrogen-containing impurities) found in the deposited thin film, and changing the bonding structure of atoms in the deposited thin film. The kinetic energy of the ions generated in the plasma can be controlled by controlling the plasma ion density and the applied bias power or the sheath voltage generated by the self-bias created by the plasma, which allows for adjustment of the kinetic energy and the amount and depth of the film that the ions can penetrate. The embodiments of the disclosure provided herein can be particularly useful, without limitation, for improving the properties of poor quality films deposited by ALD processes.

[0015]

[0024] FIG. 1 is a schematic cross-sectional view of a processing chamber assembly 100 according to one embodiment. As shown, the processing chamber assembly 100 includes a plasma processing chamber 101, a plasma source 160, a bias power system 161, and a controller 146. The plasma processing chamber 101 provides a chamber for processing a thin film formed on a surface of a substrate 128. Typically, the thin film is deposited on the surface of the substrate 128 in a separate thin film deposition chamber disposed within the processing chamber assembly 100, which in this case may include a cluster tool (not shown) including a separate thin film deposition chamber (not shown). In some embodiments, the plasma processing chamber 101 may additionally be configured to deposit a thin film layer on the surface of the substrate. The plasma source 160 converts the gaseous mixture 134 into a plasma 136, which impinges on the substrate 128 to change the properties of the film grown thereon. The bias power system 161 provides a voltage bias across the substrate 128 to facilitate the processing process. The controller 146 implements special process conditions for both film growth and film processing. The entire processing chamber assembly 100 is configured to grow or process a film formed on the substrate 128 using a specialized plasma treatment provided by use of commands provided by a controller 146. The thin film treatment process is assisted by a plasma source 160 and a bias power system 161.

[0016]

[0025] As shown, the plasma processing chamber 101 includes chamber walls 106, a chamber lid 108, a substrate support pedestal 104, an electrostatic chuck 105, an electrical ground 116, a gas panel 130, an inlet port 132, a throttle valve 138, a vacuum pump 140, and a gas source 142. The plasma processing chamber 101 may be any suitable plasma processing chamber, such as an inductively coupled plasma (ICP) processing chamber. In one embodiment, the ICP is a chamber downstream of a thin film deposition chamber (not shown). In one embodiment, the processing chamber 101 and the thin film deposition chamber (not shown) are part of the same cluster tool (not shown). Cluster tools (e.g., a Centura® system from Applied Materials, Inc.) are configured to allow substrates to be transferred between the thin film deposition chambers and the processing chambers 101 without exposure to the atmosphere. In one configuration, the cluster tool includes a central robotic device (not shown) positioned within a reduced pressure environment created in the transfer chamber and configured to transfer substrates between the processing chambers attached to the transfer chamber of the cluster tool. The central robotic device is configured to transfer substrates at least between the processing chambers 101 and the thin film deposition chambers.

[0017]

[0026] As shown in FIG. 1, the process chamber 101 may include chamber walls 106, a dielectric chamber lid 108, and a substrate support pedestal 104 disposed within the chamber walls 106. The chamber walls 106 and the dielectric chamber lid 108 serve to isolate the growth process from the outside environment. Typically, the chamber walls 106 are coupled to an electrical ground 116. The dielectric chamber lid 108 may be constructed of any suitable dielectric, such as quartz. In some implementations, the dielectric chamber lid 108 may be of a different shape (e.g., dome-shaped). In some implementations, the chamber lid 108 may be coated with a ceramic coating for protection from plasma species. In one implementation, the ceramic coating includes aluminum oxide. The ceramic coating may have a thickness ranging from about 100 microns to about 300 microns, for example, about 200 microns.

[0018]

[0027] In operation, a substrate 128, such as a semiconductor substrate, may be placed on the pedestal 104 and process gases may be supplied from a gas panel 130 through an inlet port 132 to form a gaseous mixture 134. The substrate 128 is a bare silicon wafer according to one embodiment. In another embodiment, the substrate 128 is a patterned silicon wafer, typically used in logic gates, I / O gates, field effect transistors, FINFETs, or memory applications. The device is a combination of a low quality film 320 (FIG. 3B) grown on the substrate 128. Exemplary process gases that may be used in one or more of the processes described herein are described below. The gaseous mixture 134 may be energized into a plasma 136 in the process chamber 101 by application of power from an RF power source 114. The pressure within the process chamber 101 may be controlled using a throttle valve 138 and a vacuum pump 140. In some embodiments, the temperature of the chamber walls 106 may be controlled using a liquid-containing conduit (not shown) that passes through the chamber walls 106 or a heating element embedded in the chamber walls 106 (e.g., a heating cartridge or coil) or is wrapped around the processing chamber 101 (e.g., a heater wrap or tape).

[0019]

[0028] The temperature of the substrate 128 can be controlled by controlling the temperature of the pedestal 104. In some embodiments, the pedestal 104 includes an electrostatic chuck 105, and the substrate 128 is disposed on the electrostatic chuck. In some embodiments, the temperature of the electrostatic chuck 105 can be controlled from a range of 20-500° C. through the use of heating and cooling elements. In some embodiments, the substrate 128 is “chucked” to the substrate support surface of the electrostatic chuck 105 during processing to actively control the temperature of the substrate. Temperature control of the electrostatic chuck 105 and the substrate via cooling elements embedded within the pedestal 104 helps to reduce undesirable temperature rise due to ion bombardment, as described below. In some embodiments, helium (He) gas from a gas source 142 can be supplied via a gas conduit 144 to channels (not shown) formed in the pedestal surface below the substrate 128. The helium gas can facilitate heat transfer between the pedestal 104 and the substrate 128. During processing, the pedestal 104 may be heated to a steady temperature and then the helium gas may facilitate uniform heating of the substrate 128. The pedestal 104 may be so heated by a heating element (not shown), such as a resistive heater embedded within the pedestal 104, or by lamps directed generally toward the pedestal 104 or substrate 128 when on it. Using such thermal control, the substrate 128 may be maintained at a first temperature between about 20-500° C. The components of the plasma source 160 provide the environment for film growth and densification.

[0020]

[0029] As shown, the plasma source 160 includes a coil element 110, a first impedance matching network 112, an RF power supply 114, an electrical ground 117, a shielding electrode 118, an electrical ground 119, a switch 120, and a detector 122. A radio frequency (RF) antenna including at least one inductive coil element 110 is disposed above the dielectric chamber lid 108. In one configuration, as shown in FIG. 1, two coaxial coil elements disposed about a central axis of the process chamber are driven at RF frequencies to generate a plasma 136 in a processing region of the processing chamber assembly 100. In some implementations, the inductive coil element 110 may be disposed about at least a portion of the chamber wall 106. As shown, one end of the inductive coil element 110 may be coupled to an RF power supply 114 through a first impedance matching network 112, and the other end may be connected to an electrical ground 117. The power supply 114 is typically capable of generating up to 4 kilowatts (kW) at a frequency of 13.56 MHz. The RF power supplied to the inductive coil element 110 may be pulsed (i.e., switched between on and off states) or power cycled (i.e., varying the power input from high to low levels) in the frequency range of 1 to 100 kHz. The average ion density of the plasma 136 is about 100 volts per cubic centimeter (cm -3 ) can vary from 1E10 to 1E12 ions per ion. The plasma density can be measured by using any conventional plasma diagnostic technique, such as using self-excited electron plasma resonance spectroscopy (SEER), a Langmuir probe, or other suitable technique. It is believed that the inductively coupled coaxial coil element 110 configuration shown in FIG. 1 offers significant advantages in the control and generation of high density plasma over conventional plasma source configurations, including capacitively coupled and plasma source configurations.

[0021]

[0030] A shielding electrode 118 may be interposed between the RF antenna inductive coil element 110 and the dielectric chamber lid 108. The shielding electrode 118 may be alternately electrically floating or coupled to an electrical ground 119 via any suitable means for making and breaking an electrical connection, such as a switch 120, as illustrated in FIG.

[0022]

[0031] In some implementations, a detector 122 can be attached to the chamber walls 106 to facilitate determining when the gas mixture in the chamber 101 is energized into a plasma. The detector 122 may, for example, detect radiation emitted by the excited gas or use optical emission spectroscopy (OES) to measure the intensity of one or more wavelengths of light associated with the generated plasma. The plasma source 160 overall generates a plasma 136 from the gaseous mixture 134 to process the deposited thin film.

[0023]

[0032] As shown, the bias power system 161 includes a second impedance matching network 124 and a bias power supply 126. The pedestal 104 may be coupled to the bias power supply 126 through the second impedance matching network 124. The bias power supply 126 may generally generate an RF signal having a drive frequency in the range of 1 to 160 MHz and a power between about 0 kW and about 3 kW, similar to the RF power supply 114. The bias power supply 126 may typically generate about 1 W to 1 kilowatt (kW) at a frequency in the range of 2 to 160 MHz, at a frequency of 13.56 MHz or a frequency of 2 MHz. Optionally, the bias power supply 126 may be a direct current (DC) or pulsed DC source. In some implementations, an electrode coupled to the bias power supply 126 is disposed within the electrostatic chuck 105. The bias power system 161 provides a substrate voltage bias across the substrate 128 to facilitate processing of the deposited thin film. In one embodiment, the RF bias provides energetic ions having an ion energy up to 2000 eV.

[0024]

[0033] As shown, the controller 146 includes a central processing unit (CPU) 148, a memory 150, and support circuits 152. The controller 146 can interact with the RF power supply 114, the switch 120, the detector 122, and the bias power supply 126. The controller 146 can be any suitable type of general-purpose computer processor that can be used in an industrial environment to control various chambers and sub-processors. The memory 150 for the CPU 148, or other computer readable medium, can be one or more of any readily available form of memory, such as a local or remote random access memory (RAM), a read-only memory (ROM), a floppy disk, a hard disk, or any other form of digital storage. The support circuits 152 can be coupled to the CPU 148 in an effort to support the processor in a conventional manner. These circuits can include cache, power supplies, clock circuits, input / output (I / O) circuits and subsystems, and the like. In some implementations, the techniques disclosed herein for energizing and sustaining a plasma can be software routines stored in the memory 150. The software routines may also be stored and / or executed by a second CPU (not shown) located remotely from the hardware controlled by CPU 148. A controller 146 provides instructions to the processing chamber assembly 100 and various subcomponents described above regarding temperature control, bias voltages, gas flow rates, etc.

[0025]

[0034] FIG. 2 is a flow diagram of method steps for densifying a dielectric film 200, according to one embodiment. The method steps are described in conjunction with FIG. 2, however, one skilled in the art will understand that any system configured to perform the method steps in any order falls within the scope of the embodiments described herein. As shown, the method includes a deposition process 210 and a treatment process 220. FIG. 3A shows a substrate 128 disposed on a substrate support pedestal 104 prior to the deposition process 210, according to one embodiment. In the following description, the deposition process 210 is described as a low quality film deposition process, however, this configuration is not intended to be limiting with respect to the scope of the disclosure herein, as other deposited thin films (e.g., metal or semiconductor material layers, high-k dielectrics, gate oxides) may benefit from the subsequent treatment process 220 described herein. However, it has been found that ALD and CVD films formed with low film quality may receive significant benefits by using one or more of the processes described herein.

[0026]

[0035] In one embodiment, as shown in FIG. 3B, the deposited poor film 320 is formed during the deposition process 210 on the substrate 128. According to one embodiment, in the deposition process 210, the poor film 320 is deposited by an ALD process. The poor film 320 can be hafnium oxide, silicon oxide, silicon nitride, or silicon oxynitride. According to one embodiment, the poor film 320 can be a gate oxide. A primary precursor 321 and a secondary precursor 322 are applied to the surface of the substrate 128. In one embodiment, the primary precursor is silane or another Si-containing precursor. In one embodiment, the secondary precursor 322 is water. The film can also be grown by chemical vapor deposition, pulsed laser deposition, chemical oxidation, and the like. In one exemplary embodiment, the poor film 320 is a silicon oxide film grown to a thickness between 25-100 Å, for example, between 25-35 Å. The poor quality film 320 deposited in this manner is often of poor quality, with undesirable interstitial hydrogen, dangling silicon bonds, and oxygen or nitrogen vacancies. The irregular crystal structure of the poor quality film 320 deposited can lead to problems such as trapped charge states, non-uniform growth, and reduced dielectric constant, all of which can result in gate leakage and cause problems in device function. The dangling silicon bonds can be sp or sp 2 Non-sp such as bonding 3 This can result in bonding, cause uneven and non-3D growth, and contribute to domain formation or island growth. In addition, the poor quality of the deposited low-quality film 320 can lead to poor wet and dry etch rates.

[0027]

[0036] FIG. 3C shows the substrate 128 with the deposited poor quality film 330 exposed to the treatment process 220. In the treatment process 220, according to one embodiment, the poor quality film 320 is bombarded with a process gas 331. The process gas 331 includes helium. Helium is selected as the non-reactive process gas 331 because it is the lightest of the inert elements and therefore will cause the least damage to the film treated at the same bias voltage. In addition, because helium is an inert element, it will not form undesirable chemical bonds with the atoms in the poor quality film 320. The poor quality film 330 is bombarded with the process gas 331, and the supply kinetic energy of the process gas can be used to break undesirable hydrogen bonds previously formed between hydrogen atoms and other atoms in the film. The hydrogen atoms that are free at this point combine with other free hydrogen atoms to form hydrogen gas, which then exits the poor quality film 320. Alternatively, the free hydrogen atoms combine with hydrogen impurities present in the inferior film 320 to form hydrogen gas, which then exits the inferior film. In one embodiment, the inferior film 320 includes oxygen, and the free hydrogen atoms combine with the oxygen to form water, which vaporizes or desorbs from the inferior film. In one embodiment, the inferior film 320 includes silicon, and the silicon atoms form new silicon-oxygen bonds in the case of silicon oxide-containing films, or new silicon-nitrogen bonds in the case of silicon nitride-containing films, after removing the hydrogen impurities as described above. In some embodiments, the electrical and / or mechanical properties of the inferior film, such as the dielectric properties, density, hardness, and tensile strength of the film, are improved.

[0028]

[0037] In one embodiment, the process gas 331 further comprises a secondary gas comprising oxygen gas, nitrogen gas, ammonia, trifluoride nitride gas, argon gas, or any combination of the above, wherein the process gas is Ar + , O + , O2 + , He + , N2 + , NH2 + , N.H. + , NF3 + , NF2 + , or NF +The low-quality film 320 may be energized into a plasma by application of a source power 114 that generates ions such as SiO 2 , SiO 3 , or radicals such as O , NH , N , or F 2 . In one embodiment, the low-quality film 320 includes silicon oxide, silicon nitride, or silicon oxynitride, and ions or radicals of oxygen or nitrogen may be embedded in the deposited low-quality film 330, which repairs oxygen or nitrogen vacancies and facilitates the formation of silicon-oxygen or silicon-nitrogen bonds from undesired dangling bonds. The percentage of oxygen or nitrogen in the process gas 331 may be varied to control the amount of oxygen or nitrogen vacancies repaired in the deposited low-quality film 330. A higher ion density allows more ions to affect the low-quality film 320, increasing the number of repaired vacancies and the number of impurities removed.

[0029]

[0038] In one embodiment, the process gas 331 essentially comprises a single type of gas, such as helium. In another embodiment, the process gas 331 is a mixture of helium and a secondary gas including oxygen (i.e., gaseous mixture 134), with the volume percentage of oxygen being about 5-90% and the remainder being helium. In one embodiment, the flow time of the process gas is about 1 second to 10 minutes. In one embodiment, the pressure can be controlled to about 5-200 mTorr. In one embodiment, the secondary gas can be provided without helium.

[0030]

[0039] In one embodiment, the substrate support pedestal 104 can be coupled to a bias power supply 126 that can apply a bias power to the substrate 128. In one embodiment, the substrate 128 is a patterned wafer, and the bias power increases the conformality of the poor quality film 320 on the sidewalls of the wafer pattern. In one embodiment, the bias power charges the substrate 128. As the substrate 128 is charged, it electrostatically attracts ions from the plasma 136, and the charged ions impinge on the poor quality film 320. In another embodiment, the bias power creates a plasma sheath on the surface of the substrate 128, which allows the ions to impinge on and interact with atoms in the substrate. A higher bias power increases the penetration depth of the ions, allowing for the processing of a thicker poor quality film 320. In another embodiment, no bias power is provided, and the charged ions are attracted to the surface of the substrate by a formed sheath voltage created by a self-bias. The self-bias is created by a voltage difference formed between the electrically charged plasma and the at least partially grounded substrate support. The self-bias can be adjusted by adjusting the process gas pressure in the chamber and by adjusting the power applied to the process gas by the RF power supply 114, both of which affect the density of the plasma and the voltage formed between the formed plasma and the grounded substrate.

[0031]

[0040] In one embodiment, the substrate 128 comprises silicon oxide or silicon oxynitride, the secondary gas comprises oxygen gas, and the bias power facilitates filling of oxygen vacancies in the deposited poor quality film 320 by creating a plasma sheath over the surface of the substrate, which causes oxygen ions to collide with and interact with oxygen vacancies at or beneath the exposed surface of the film on the substrate. The oxygen ions become embedded in the poor quality film 128 and form silicon-oxygen bonds, filling all oxygen vacancies in the poor quality film. In some cases, oxygen radicals (O * The formation of .alpha.-alkyloxygen (.alpha.) is useful because the thermal energy supplied to the radicals by the plasma allows them to diffuse to the surface of the film so that they can interact with oxygen vacancies at or beneath the exposed surface of the film on the substrate.

[0032]

[0041] In another embodiment, the substrate 128 comprises silicon nitride or silicon oxynitride, the secondary gas comprises nitrogen gas or ammonia, and the bias power facilitates filling of nitrogen vacancies in the deposited poor quality film 320 by attracting nitrogen ions or radicals. In some embodiments, the bias power is used to facilitate filling of nitrogen vacancies in the deposited poor quality film 320 by creating a plasma sheath on the surface of the substrate, which causes nitrogen ions to collide with and interact with nitrogen vacancies at or beneath the exposed surface of the film on the substrate. The nitrogen ions embed in the poor quality film 128 and form silicon-nitrogen bonds, filling all of the nitrogen vacancies in the poor quality film. In one embodiment of an ALD nitride film treatment process, the substrate temperature is held between about 150 and about 350° C., an RF power of between about 2000 W and about 2250 W is provided to the process gas to form a plasma, a substrate RF bias power of about 0-10 W (e.g., 1-10 W) is applied, the chamber is held at about 10 mTorr, and helium is flowed for a treatment period of about 10 minutes.

[0033]

[0042] Bombardment of the poor quality film with ionized process gas 331 tends to reduce trapped charge states and planarize the grown film, and can improve the mechanical and electrical properties (e.g., dielectric constant) of the film, all of which reduces gate leakage and ensures proper device function. The treatment process densifies the formed poor quality film by removing dangling silicon bonds, which are sp 3 This provides bonding and promotes uniform film mechanical and electrical properties. The wet and dry etch rates of the film are also improved. The overall process of process gas bombardment results in a better quality layer than the originally deposited layer. Better control of the quality of the poor quality film allows for lower gate leakage current density and better equivalent oxide thickness scaling required for the functionality of current semiconductor devices.

[0034]

[0043] In one embodiment, the substrate support pedestal 104 is heated by a heating element (not shown), such as a resistive heater embedded within the pedestal 104, or by lamps generally directed at the pedestal 104 or substrate 128 when on it. Using such thermal control, the substrate 128 can be maintained at a temperature between about 20-500° C. In one embodiment, the pedestal is maintained at a temperature greater than about 150° C., such as greater than about 250° C. In one embodiment, the low quality film 320 is silicon oxide, silicon nitride, or silicon oxynitride, and the thermal control increases the rate of departure of hydrogen impurities and therefore the rate of formation of silicon-oxygen and silicon-nitrogen bonds during the treatment process.

[0035]

[0044] During the treatment process 220, the substrate temperature is held and controlled at a temperature between about 20 and 500° C., an RF power between about 50 W and 4 kW is supplied to the process gas, a substrate RF bias power between about 1 W and 1000 W is applied, and a chamber process pressure between about 5 mTorr and about 200 mTorr is applied for a period between about 1 second and about 15 minutes. The combination of temperature control of the substrate, bias power, and source power 114 allows for the production of a better quality film 320. By using all three process parameters at once during the treatment process 220, the desired ion bombardment rate (ions / sec) and bombardment density (ions / cm 2 ) is achieved, the bombarding ions have a desired kinetic energy (eV), and the bombarded film has a desired amount of added thermal energy (watts / cm) that increases the process reaction rate, allows atoms to migrate to more preferential binding sites, removes impurities, and increases the densification of the film. 2 ), which results in a more uniform and conformal film with a reduced amount of vacancies or undesirable impurity atoms. In one embodiment of the process, the average plasma ion density on the substrate surface during processing is about 1 cubic centimeter (cm -3) and an RF bias is applied to the substrate to provide ions generated within the plasma with an average ion energy of between about 2 eV and about 2,000 eV, and the substrate is maintained at between about 20° C. and about 500° C., e.g., between 350° C. and 500° C. In another process embodiment, the average plasma ion density above the substrate surface during processing is between about 1E10 and 1E12 ions per cubic centimeter (cm -3 ), an RF bias is applied to the substrate to provide an average ion energy to ions generated within the plasma of between about 2 eV and about 30 eV, e.g., between about 2 eV and 10 eV, and the substrate is maintained at a temperature of between about 20° C. and about 500° C., e.g., between 150° C. and 500° C., or between 250° C. and 500° C., or between 350° C. and 500° C.

[0036]

[0045] As discussed above, control of plasma ion density during processing is dependent on the desired ion bombardment rate (ions / sec) and ion bombardment density (ions / cm 2 ) is achieved, which among other things affects the amount of damage created in the poor quality film 320 during processing. In one example, a 1E10 ion density is preferred for applications that require ions to be implanted to a desired depth in the film, since a higher plasma ion density, e.g., 1E12, would significantly increase the damage caused during processing when other process variables (e.g., substrate bias and temperature) are held constant. In some implementations, the implanted ions include oxygen or nitrogen. Control of the substrate bias allows the kinetic energy (eV) of the bombarding ions to be controlled to adjust the penetration depth and / or densification effect of the bombarding ions, which helps to remove undesired impurities from the poor quality film 320. Apart from other variables, the thermal energy (watts / cm) delivered to the film during processing can be adjusted. 2 ) can increase the reaction rates of any chemical reactions occurring in the film, move atoms to more preferential binding sites, reduce or alter damage caused by bombarding ions, remove impurities found in the formed poor quality film 320 layer, and increase densification of the poor quality film 320.

[0037]

[0046] In one exemplary implementation of treatment process 220, the substrate temperature is held at about 250° C., about 2000 W of RF power is supplied to the process gas, about 0-10 W (e.g., 1 to 10 W) of substrate RF bias power is applied, the chamber is held at about 20 mTorr, and helium is flowed for about 4 minutes without a secondary gas. In another exemplary implementation of treatment process 220, the substrate temperature is held at about 250° C., about 2250 W of RF power is supplied to the process gas, about 0-10 W (e.g., 1-10 W) of substrate RF bias power is applied, the chamber is held at about 5 mTorr, and helium is flowed for about 15 minutes without a secondary gas.

[0038]

[0047] FIG. 4 is a flow diagram of method steps for processing a dielectric film 400, according to one embodiment. Although the method steps are described with reference to FIG. 4, one skilled in the art will understand that any system configured to perform the method steps in any order falls within the scope of the embodiments described herein. As shown, the method includes a film deposition process 410, a first treatment process 420, and a second treatment process 430. FIG. 5 illustrates a substrate during the method of 400, according to one embodiment. FIG. 5A illustrates a substrate 128 disposed on a substrate support pedestal 104 prior to the film deposition process 410, according to one embodiment.

[0039]

[0048] FIG. 5B illustrates a substrate 128 having a deposited poor quality film 320 deposited by a film deposition process 410. The film deposition process 410 proceeds similarly to the deposition process 210. The film can be grown by atomic layer deposition, chemical vapor deposition, pulsed laser deposition, chemical oxidation, or other similar processes. In an exemplary embodiment, the poor quality film can be a silicon oxide, hafnium silicate, zirconium silicate, hafnium oxide, or zirconium oxide film grown to a thickness between 25-100 Å. In one example of an ALD process, the substrate surface is periodically contacted with at least one oxygen gas (e.g., O2, H2O), nitrogen-containing gas (e.g., N2, NH3), and / or silicon-containing precursor (e.g., silane-containing precursor) to deposit a film comprising silicon, and the substrate surface has a temperature of about 200° C. or higher.

[0040]

[0049] 5C shows the substrate 128 having the poor quality film 330 deposited thereon exposed to a first treatment process 420. The first treatment process 420 is performed similarly to the treatment process 320 described above.

[0041]

[0050] 5D shows the substrate 128 with the processed poor quality film 540 exposed to a second treatment process 430. In the second treatment process 430, the deposited poor quality film 330 is bombarded by ionized portions of a second process gas 331 according to one embodiment. The second process gas 331 includes oxygen and may further include a secondary gas including helium, nitrogen gas, ammonia, argon, nitrogen trifluoride gas, or any combination thereof. In one embodiment, the process gas 331 further includes a secondary gas including nitrogen gas, ammonia, fluorine gas, or any combination thereof, and the secondary gas may include Ar. + , He + , N2 + , NH2 + , N.H. + , NF3 + , NF2 + , or NF +The gas may be energized into a plasma by source power 114 to generate ions such as NH or F, or radicals such as NH or F.

[0042]

[0051] The first treatment process 420 and the second treatment process 430 can be repeated multiple times in succession to continue improving the properties of the processed thin film. It is believed that repeating the process steps at least twice can improve the properties of the poor quality film with each pass. The first and second treatment processes can be performed in any order or simultaneously. The overall process of impacting the deposited poor quality film will result in a poor quality film that is better than the as-deposited poor quality film.

[0043]

[0052] In an exemplary embodiment, the first temperature during the first treatment process 420 is held at 450° C., the second temperature during the second treatment process 430 is held at 450° C., the first source power 114 is 200 W, the bias power is between 0 and 100 W (e.g., 1-100 W), the pressure is held at 100 mTorr, the helium and oxygen are co-flowed at 50% oxygen and 50% helium by volume, and the process is performed for 1 minute or less. In another exemplary embodiment, the first temperature is held at 450° C., the second temperature is held at 450° C., the first source power 114 is 100 W, the bias power is 800 W, the pressure is held at 10 mTorr, the helium and oxygen are co-flowed at 10% oxygen and 90% helium by volume, and the process is performed for 4 minutes.

[0044]

[0053] Poor film quality of the deposited ALD layer can be improved by bombarding the deposited film with helium. Helium imparts kinetic energy to the constituent atoms of the film, which can be used in silicon-containing films to remove hydrogen impurities as hydrogen gas or hydrogen water, leading to the creation of silicon-silicon, silicon-nitrogen, or silicon-oxygen bonds. The kinetic energy of the helium is controlled by the source power, which allows for the adjustment of the depth of the film that the helium can penetrate and the adjustment of the kinetic energy. The addition of oxygen plasma generated by the source power also replenishes oxygen vacancies with oxygen, restoring the crystal structure closer to the original silicon oxide.

[0045]

[0054] The above shows one way to improve poor quality films deposited by ALD. By being subjected to the above-mentioned process, the electrical properties of the poor quality films are improved. In addition, the modification of the poor quality films after ALD allows those skilled in the art to use current ALD strategies and perform treatments to improve the poor quality films after deposition, instead of having to modify the current ALD methods that are already functional and optimized.

[0046]

[0055] While the forgoing is directed to embodiments of the present disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, the scope of the disclosure being determined by the appended claims.

Claims

1. 1. A method for modifying a poor quality film in a semiconductor device, comprising: The method includes heating the substrate to a first temperature between about 150° C. and about 500° C., and exposing a surface of a film disposed on a surface of the substrate to a plasma comprising a process gas including helium (He) while applying a substrate RF bias to cause ions formed in the plasma to bombard the surface of the film.

2. 10. The method of claim 1, wherein applying a substrate RF bias imparts an energy of between about 2 eV and about 2,000 eV to at least a portion of ions formed in the plasma.

3. The plasma reaches a depth of 1 cubic centimeter (cm -3 3. The method of claim 2, wherein the ion density is between about 1E10 and 1E12 ions per 100 s.p.m.

4. The method of claim 2 , wherein the plasma is generated by applying a source power and the first temperature is between about 350° C. and about 500° C.

5. The process gas is oxygen gas (O 2 ), nitrogen trifluoride gas (NF 3 ), nitrogen gas (N 2 ), and ammonia (NH 3 10. The method of claim 1 further comprising a secondary gas comprising:

6. The method of claim 1 , wherein the film is selected from the group consisting of silicon, silicon oxide, silicon nitride, and silicon oxynitride.

7. 8. The method of claim 7, wherein depositing the film further comprises exposing the surface to a primary precursor and a secondary precursor, the primary precursor being a silicon-based precursor and the secondary precursor being water.

8. Depositing the film further comprises exposing the surface to a primary precursor and a secondary precursor, the primary precursor being a silicon-based precursor and the secondary precursor being nitrogen gas (N 2) and ammonia (NH 3 8. The method of claim 7, wherein the compound is selected from the group consisting of:

9. A poor quality film is grown in a thin film deposition chamber; Exposing a surface of the film on the substrate is performed in a processing chamber; the thin film deposition chamber and the processing chamber are coupled to a cluster tool configured to enable transfer of the substrate between the thin film deposition chamber and the processing chamber without exposure to atmosphere; The method of claim 1.

10. 1. A method for modifying a poor quality film in a semiconductor device, comprising: depositing a film on a substrate in a first processing chamber; exposing a surface of the film to a first plasma comprising a first process gas comprising helium (He) in a second processing chamber while the semiconductor substrate is heated to a first temperature between about 150 and about 500° C. and a first RF bias is applied to bombard ions formed in the plasma with the substrate surface; and While the substrate is heated to a second temperature different from the first temperature, and while a second RF bias is applied to the substrate, the surface of the film is irradiated with a gas mixture of helium (He) and oxygen gas (O 2 exposing the second plasma to a second process gas comprising a second process gas comprising The method includes:

11. 12. The method of claim 11, wherein the first RF bias energizes ions created in the first plasma such that the ions impact the surface of the film, the ions having an average ion energy between about 2 eV and 2,000 eV.

12. The first and second plasmas were applied to the entire surface of the film with a volume of 1 cubic centimeter (cm -3 13. The method of claim 12, wherein the particle size distribution is between about 1E10 and 1E12 ions per particle.

13. The first process gas is nitrogen trifluoride gas (NF 3 ), nitrogen gas (N 2 ), and ammonia (NH 3 12. The method of claim 11 further comprising a gas selected from the group consisting of:

14. The second process gas is nitrogen fluoride gas (NF 3 ), nitrogen gas (N 2 ), and ammonia (NH 3 12. The method of claim 11 further comprising a secondary process gas selected from the group consisting of:

15. 1. A method for modifying a poor quality film in a semiconductor device, comprising: The method includes exposing a surface of a film disposed on a surface of a substrate to a plasma including a process gas including helium (He) while the substrate is heated to a first temperature between about 150° C. and about 500° C., the plasma being generated by applying a source power to the process gas, and the plasma being heated to a plasma concentration of about 1 cubic centimeter (cm ) across the surface of the film being treated. -3 ) having an average ion density of between about 1E10 and 1E12 ions per 100 s.

Citation Information

Patent Citations

  • Multilayer high quality gate dielectric for low temperature poly silicon tft

    JP2008521218A

  • Methods and apparatuses for uniform reduction of in-feature wet etch rate of silicon nitride film formed by ald

    JP2016066794A

  • Plasma processing method and plasma processing device

    JP2017092265A

  • Apparatus for generating plasma and method for controlling impedance thereof

    KR1020180046713A

  • Treatments for decreasing ETCH rates after flowable deposition of silicon-carbon-and-nitrogen-containing layers

    US20130217241A1