Light-emitting device

By employing a method that reduces the number of masks and photolithography steps through advanced film formation techniques, the manufacturing process for semiconductor devices becomes more efficient, cost-effective, and productive, addressing the challenges of high costs and prolonged times in existing methods.

JP2024133515AActive Publication Date: 2024-10-02SEMICON ENERGY LAB CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024099806
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2013-04-04
Filing Date
2024-06-20
Publication Date
2024-10-02
Estimated Expiration
2034-03-18

AI Technical Summary

Technical Problem

The existing semiconductor device manufacturing processes require multiple masks and photolithography steps, leading to high costs, prolonged manufacturing time, and reduced productivity, particularly in the production of active matrix display devices and light-emitting devices.

Method used

A method is introduced to reduce the number of masks and photolithography steps by forming conductive and insulating films in a manner that allows for the simultaneous etching of multiple layers, using a multi-tone mask to create openings with varying thicknesses and shapes, thereby minimizing the need for multiple masks and reducing the overall process complexity.

Benefits of technology

This approach decreases the number of masks and photolithography steps, shortens manufacturing time, and lowers the production costs of semiconductor devices while maintaining reliability and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133515000001_ABST
    Figure 2024133515000001_ABST
Patent Text Reader

Abstract

To reduce the number of masks used in a manufacturing step for a semiconductor device, and reduce the number of photolithography steps.SOLUTION: A first step of forming a first conductive film over a substrate, forming a first insulating film over the first conductive film, forming a semiconductor film over the first insulating film, forming a semiconductor film including a channel region by etching at least a part of the semiconductor film, forming a second insulating film over the semiconductor film including the channel region, forming a mask over the second insulating film, and removing a first part of the second insulating film that overlaps with the semiconductor film including the channel region and does not overlap with the mask and at the same time removing a second part of the first insulating film and the second insulating film that does not overlap with the mask and the semiconductor film including the channel region is performed. After the first step, the mask is removed and a second conductive film electrically connected to the semiconductor film including the channel region is formed over at least a part of the second insulating film.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a method for manufacturing the semiconductor device. [Background technology]

[0002] In recent years, a thin film with a thickness of several nm to several hundred nm has been formed on a substrate having an insulating surface such as a glass substrate. Transistors made of thin semiconductor films of about I C (Integrated Circuit) and electronic devices including electro-optical devices Transistors are also widely used in liquid crystal displays and organic light-emitting diodes (ELDs). Active luminescence (ALU) elements are used in light-emitting devices. It is also used as a switching element in a matrix type display device and a light emitting device.

[0003] The applications of such active matrix display devices and light emitting devices are expanding. There is a growing demand for larger screen size, higher resolution, and higher aperture ratio. The equipment must be highly reliable, and the manufacturing method must be highly productive and reduce production costs. What is required is...

[0004] In the manufacture of transistors used in active matrix display devices and light-emitting devices, Therefore, reducing the number of photolithography steps is important for cost reduction. Photomasks for the 19th generation cost tens of millions of yen each, while 10th and 11th generation photomasks cost In fact, each sheet can cost hundreds of millions of yen. The number of processes, including related processes, increases significantly when one process is added. Many technologies are being developed to reduce the number of lithography steps.

[0005] A representative method for reducing the number of photolithography steps in the transistor manufacturing process As a means, a multi-tone mask (also called a half-tone mask or gray-tone mask) A technique using a multi-tone mask is widely known. Examples thereof include Patent Documents 1 to 3. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-178545 A [Patent Document 2] JP 2011-155303 A [Patent Document 3] JP 2009-124124 A Summary of the Invention [Problem to be solved by the invention]

[0007] One aspect of the present invention has an object to reduce the number of masks used in a manufacturing process of a semiconductor device. Another object of the present invention is to reduce the number of photolithography steps. Another object of the present invention is to reduce the manufacturing time of the semiconductor device. One of the objectives of the Society is to [Means for solving the problem]

[0008] In one aspect of the present invention, a first conductive film is formed above a substrate, and a first insulating film is formed above the first conductive film. An insulating film is formed, a semiconductor film is formed above the first insulating film, and at least a part of the semiconductor film is etched. A semiconductor film including a channel region is formed by etching the semiconductor film. A second insulating film is formed on the second insulating film, a mask is formed on the second insulating film, removing a first portion that overlaps the semiconductor film including the channel region and that does not overlap the mask; At the same time, the first insulating film and the second insulating film are masked and the semiconductor film including the channel region is A first step is performed to remove the second portion that does not overlap with the mask, and the mask is removed after the first step. A semiconductor film including a channel region is electrically connected to the second insulating film at least partially above the second insulating film. and forming a second conductive film on the first conductive layer. .

[0009] In the above, after the first step, before removing the mask, the mask is retracted and It is preferable to expose a part of the second insulating film and remove a part of the second insulating film.

[0010] In another embodiment of the present invention, a first conductive film is formed above a substrate, and A first insulating film is formed on the first insulating film, a semiconductor film is formed on the first insulating film, and at least a portion of the semiconductor film is A semiconductor film including a channel region is formed by etching a part of the semiconductor film including the channel region. A second insulating film is formed above the main film, and a first region and a second insulating film are formed above the second insulating film. a second region having a thickness smaller than the thickness in the first region; A first step is performed to remove the portions of the first insulating film and the second insulating film that do not overlap with the mask. After the step, a second step is performed in which the mask in the second region is removed by retracting the mask. After the second step, a third step is performed to remove a portion of the second insulating film that overlaps with the second region. After the third step, the mask is removed, and a chamfer is formed on at least a part of the second insulating film. forming a second conductive film electrically connected to the semiconductor film including the panel region. The present invention relates to a method for manufacturing a semiconductor device.

[0011] In another embodiment of the present invention, a first conductive film is formed above a substrate, and A first insulating film is formed on the semiconductor film, and a semiconductor film is formed on the first insulating film. A first region and a second region having a thickness smaller than the thickness in the first region. A mask is formed on the first insulating film and the semiconductor film, and the portions of the first insulating film and the semiconductor film that do not overlap with the mask are removed to form a first a first step of forming an opening in the insulating film; and after the first step, the mask is retracted. A second step of removing the mask in the second region is performed by A third step is performed to remove the portion overlapping with the second region to form a semiconductor film including a channel region. After the third step, the mask is removed and a second insulating film is formed above the semiconductor film including the channel region. A film is formed, and at least a portion of the second insulating film overlapping the opening is removed, and a small amount of the second insulating film is removed. A second conductive film is formed which is electrically connected to the semiconductor film including the channel region at least partially above the semiconductor film. The present invention relates to a method for manufacturing a semiconductor device, and

[0012] In another embodiment of the present invention, a first electrode is formed on a substrate, and a first An insulating film is formed, a second insulating film is formed above the first insulating film, and a third insulating film is formed above the second insulating film. a first conductive film is formed, and a first region and a second region are formed above the first conductive film, the second region being thicker than the first region; and forming a mask having a first insulating film, a second region having a thickness smaller than the first insulating film, and A first step is performed to remove the portions of the insulating film and the first conductive film that do not overlap with the mask; After the step, a second step is performed in which the mask in the second region is removed by retracting the mask. After the second step, a third step is performed to remove a portion of the first conductive film that overlaps with the second region. After the third step, the mask is removed, and a third insulating film is formed on at least a part of the second insulating film. An insulating film is formed, and a first electrode is electrically connected to at least a part of the third insulating film. and forming a second conductive film on the first conductive layer.

[0013] In the above, before forming the first electrode, a step of forming a semiconductor film above the substrate is performed. A step of forming a fourth insulating film above the semiconductor film is performed, and the first opening is formed in the fourth insulating film. The method may further include a step of forming a hole. The electrode may be electrically connected to the semiconductor film through a first opening formed in a fourth insulating film. In the above, the semiconductor film may include an oxide semiconductor. The second insulating film may have a tapered shape. The opening formed in the first step may have a tapered shape. The opening formed in the insulating film may have a tapered shape. The insulating film may have a tapered shape on the side surface.

[0014] In another embodiment of the present invention, a first electrode is formed on a substrate, and a first An insulating film is formed, a second insulating film is formed above the first insulating film, and a third insulating film is formed above the second insulating film. a first conductive film is formed, and a first region and a second region are formed above the first conductive film, the second region being thicker than the first region; and forming a mask having a first insulating film, a second region having a thickness smaller than the first insulating film, and A first step is performed to remove the portions of the insulating film and the first conductive film that do not overlap with the mask; After the step, a second step is performed in which the mask in the second region is removed by retracting the mask. After the second step, a third step is performed to remove a portion of the first conductive film that overlaps with the second region. After the third step, the mask is removed, and the upper surface of at least a part of the second insulating film and At least one of the side surfaces of the second insulating film in the opening formed in the second insulating film by the first step A third insulating film is formed above at least a portion of the first insulating film. forming a second conductive film electrically connected to the first electrode. A method for manufacturing a body device.

[0015] In another embodiment of the present invention, a first electrode is formed on a substrate, and a first An insulating film is formed, a second insulating film is formed above the first insulating film, and a third insulating film is formed above the second insulating film. a first conductive film is formed, and a first region and a second region are formed above the first conductive film, the second region being thicker than the first region; and forming a mask having a first insulating film, a second region having a thickness smaller than the first insulating film, and A first step is performed to remove the portions of the insulating film and the first conductive film that do not overlap with the mask; After the step, a second step is performed in which the mask in the second region is removed by retracting the mask. After the second step, a third step is performed to remove a portion of the first conductive film that overlaps with the second region. After the third step, the mask is removed, and the upper surface of at least a part of the second insulating film and above the side surface of the second insulating film in the opening formed in the second insulating film by the first process, A third insulating film is formed above at least a part of the first electrode, and a small part of the third insulating film is forming a second conductive film electrically connected to the first electrode above at least a portion of the first conductive film; The present invention relates to a method for manufacturing a semiconductor device. Effect of the Invention

[0016] According to one embodiment of the present invention, the number of masks used in a manufacturing process of a semiconductor device can be reduced. In addition, the number of photolithography steps can be reduced. In addition, the manufacturing cost of the semiconductor device can be reduced. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a top view illustrating a semiconductor device. [Diagram 2] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Diagram 3] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 4] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Diagram 5] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 6] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 7] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 8] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 9] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 10] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 11] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 12]1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. [Figure 13] 1A and 1B are diagrams illustrating a liquid crystal display device. [Figure 14] 1A to 1C are diagrams illustrating electronic devices. [Figure 15] 1A to 1C are cross-sectional views illustrating a manufacturing method of a semiconductor device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and it is understood by those skilled in the art that various modifications can be made to the form and details of the present invention. It will be easily understood. In addition, the present invention is not limited to the description of the embodiment shown below. In explaining the configuration of the invention using the drawings, the same symbols are used The numbers are used commonly across different drawings. When referring to similar objects, the hatch pattern is used instead. Similarly, there are cases where no particular reference numeral is given.

[0019] In this specification, the ordinal numbers such as 1st and 2nd are used for convenience. It does not indicate the order of processes or stacking. For example, "first" may be changed to "second" or " " can be appropriately replaced with "the third" etc. The ordinal numbers used to identify an aspect of the present invention may not match those used in the present invention. be.

[0020] In addition, in this specification, the term "above" means that the positional relationship of a component is "directly above." For example, the expression "gate electrode on an insulating layer" means that the insulating layer This does not exclude the inclusion of other components between the gate electrode and the gate electrode. In addition, cases where there is no planar overlap (which may also be called cases where there is no overlap) are not excluded.

[0021] In addition, the terms "electrode" and "wiring" used in this specification and the like refer to these components functionally. For example, an "electrode" may be used as a part of a "wiring". Furthermore, the terms "electrode" and "wiring" are used interchangeably to refer to the plural "electrodes". This also includes cases where "conductor" and "wiring" are formed as one unit.

[0022] In addition, the functions of the "source" and "drain" may differ depending on whether transistors of different polarities are used or not. However, they may be swapped when the direction of the current changes during circuit operation. In this specification, the terms "source" and "drain" are used interchangeably. It is assumed that this is possible.

[0023] In addition, "electrically connected" means connected via "something that has some kind of electrical effect." In this case, "something that has some kind of electrical effect" refers to the electrical connection between the objects to be connected. There are no particular restrictions as long as it is capable of transmitting and receiving electrical signals. "Items having an electrochemical effect" include electrodes and wiring.

[0024] Even if a material is described as a "semiconductor," if its electrical conductivity is sufficiently low, it may be considered an "insulator." In addition, the boundary between "semiconductor" and "insulator" is unclear, and Therefore, the term "semiconductor" in this specification is sometimes called "insulator". Similarly, the term "insulator" as used herein may be interchangeable with "semiconductor." Sometimes it can be rephrased.

[0025] In addition, even if a material is written as a "semiconductor," if the material has a sufficiently high electrical conductivity, it should be written as a "conductor." In addition, the boundary between "semiconductor" and "conductor" is unclear, and Therefore, the term "semiconductor" used in this specification is sometimes used to refer to "conductor". Similarly, the term "conductor" as used herein may be interchangeable with "semiconductor." Sometimes it can be rephrased.

[0026] In addition, in this specification, "parallel" means that two straight lines are at an angle of -10° or more and 10° or less. Therefore, it includes the case where the angle is between -5° and 5°. "Perpendicular" refers to two straight lines that form an angle between 80° and 100°. Therefore, cases between 85° and 95° are also included.

[0027] In this specification and the like, when the crystal is a trigonal or rhombohedral crystal, it is represented as a hexagonal crystal system. vinegar.

[0028] (Embodiment 1) A manufacturing method of a semiconductor device according to one embodiment of the present invention will be described with reference to FIGS. FIG. 1 is a top view of a semiconductor device. FIG. 1(A) shows a semiconductor device that functions as a pixel region of a liquid crystal display device. 1B and 1C are the parts where the drivers for the liquid crystal display device and the like are provided. For the sake of simplicity, only one of the components is shown. For example, insulating film 104 and insulating film 108, which will be described later, are not shown. The cross-sectional structure of the portion indicated by the dashed line X1-X2 in FIG. 1(A) is shown in the cross-sectional views of FIGS. The cross section X1-X2 is a cross-sectional view of a portion of the region in which a transistor is formed. The cross-sectional structure of the portion indicated by the dashed line Y1-Y2 in FIG. 1(B) is shown in FIG. 2 to FIG. 10. The cross section Y1-Y2 is a cross section of the conductive film and the semiconductor film provided under the semiconductor film. 1 is a cross-sectional structure of a portion of a region where a conductive film provided on a film is electrically connected.

[0029] ≪Manufacturing method 1≫ First, referring to FIG. 2 and FIG. 3, the transistor 150 and the connection portion 16 shown in FIG. Explain how to form 0.

[0030] <Substrate> First, a substrate 100 is prepared (FIG. 2(A)). There are no significant limitations on the material of the substrate 100. However, materials that have at least the heat resistance to withstand the subsequent heat treatment are used. For example, Glass substrate, ceramic substrate, quartz substrate, sapphire substrate, YSZ (yttria stabilized zirconia) A silicon substrate or the like may be used as the substrate 100. Also, silicon or silicon carbide may be used. Single crystal semiconductor substrates, polycrystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium It is also possible to use an SOI substrate or the like.

[0031] In addition, a semiconductor substrate or an SOI substrate on which a semiconductor element is provided may be used as the substrate 100. In that case, the transistor 150 is formed on the substrate 100 via an interlayer insulating layer. At this time, the conductive film of the transistor 150 is connected to the connection electrode embedded in the interlayer insulating layer. At least one of the conductive film 114b and the conductive film 114c is connected to the semiconductor element. The transistor 1 is electrically connected to the semiconductor element via an interlayer insulating layer. By providing the transistor 50, the increase in area due to the addition of the transistor 150 is suppressed. It is possible.

[0032] Alternatively, a flexible substrate such as plastic may be used as the substrate 100, and the substrate may be directly formed on the flexible substrate. Alternatively, the transistor 150 may be formed between the substrate 100 and the transistor 150. A peeling layer may be provided on the upper layer of the transistor. After that, it can be separated from the substrate 100 and used for transfer to another substrate. Therefore, the transistor 150 can be transferred to a substrate having low heat resistance or a flexible substrate.

[0033] <Conductive film formation> Next, a conductive film is formed above the substrate 100 by a sputtering method, a CVD method, a vapor deposition method, or the like. A resist mask is formed over the conductive film by a photolithography process. A part of the conductive film is etched using a mask to form the conductive film 102a and the conductive film 102b. The conductive film 102b is a gate electrode of the transistor 150. It can function as a pole.

[0034] The conductive film 102a and the conductive film 102b may be made of aluminum, chromium, copper, tantalum, titanium, or the like. , molybdenum, tungsten, or an alloy containing the above metals. The above-mentioned metals can be combined to form an alloy. Metals selected from any one or more of zirconium may be used.

[0035] The conductive film 102a and the conductive film 102b may have a single-layer structure or a laminated structure of two or more layers. For example, a layer of tungsten, titanium, or molybdenum may be formed on or under the aluminum film. A film that functions as a barrier film, such as a selected metal or an alloy containing the above-mentioned metals, is deposited. Alternatively, a two-layer structure may be used in which a layer of the aluminum film is formed on the top and bottom of the aluminum film, and the layer functions as the barrier film. Similarly, the above-mentioned barrier film may be laminated on or under the copper film to form a three-layer structure. Alternatively, the copper film may have a two-layer structure in which the above-mentioned barrier film is laminated on the top and bottom of the copper film. Alternatively, a three-layer structure may be formed by laminating films functioning as the above.

[0036] Since the aluminum film and the copper film have low resistance, they are used for the conductive film 102a and the conductive film 102b. This can reduce the power consumption of the semiconductor device. A film that functions as a barrier film, such as a silicon film or a molybdenum film, is bonded to an aluminum film or a copper film, etc. By stacking the layers in layers, it is possible to suppress these diffusions and improve the reliability of the semiconductor device. Cut.

[0037] In addition, an In-Ga-Zn-based oxynitride semiconductor is formed between the conductive film 102b and an insulating film 104 described later. Conductor film, In-Sn-based oxynitride semiconductor film, In-Ga-based oxynitride semiconductor film, In-Zn-based Oxynitride semiconductor film, Sn-based oxynitride semiconductor film, In-based oxynitride semiconductor film, metal nitride film (I These films may have a thermal conductivity of 5 eV or more, preferably 5.5 eV or more. Since the work function is larger than the electron affinity of the oxide semiconductor, When an oxide semiconductor is used for a conductor film, the threshold voltage of a transistor is shifted to the positive side. Therefore, a switching element having a so-called normally-off characteristic can be realized. When a Ga-Zn-based oxynitride semiconductor film is used, the nitrogen concentration is at least higher than that of the semiconductor film 106b. A semiconductor film of an In-Ga-Zn-based oxynitride with a concentration of 7 atomic % or more is used.

[0038] <Insulating film formation> Next, an insulating film 104 is formed above the substrate 100, the conductive film 102a, and the conductive film 102b. (FIG. 2C). The insulating film 104 serves as a gate insulating film in the transistor 150. It can be made to function.

[0039] The insulating film 104 is, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, or silicon nitride. Copper, aluminum oxide, hafnium oxide, gallium oxide or Ga-Zn-based metal oxide The above may be used, and the layer may be a laminate or a single layer.

[0040] The insulating film 104 is made of hafnium silicate (HfSiO x ), nitrogen added Hafnium Silicate (HfSi x O y N z ), nitrogen-doped hafnium aluminate HfAl x O y N z ), high-k materials such as hafnium oxide and yttrium oxide By using this, the gate leakage of the transistor can be reduced.

[0041] The insulating film 104 is formed by a sputtering method, a CVD method, a vapor deposition method, or the like.

[0042] When forming a silicon nitride film as the insulating film 104, it is preferable to use a two-stage formation method. First, a mixture of silane, nitrogen, and ammonia gases was used as the source gas. A first silicon nitride film with few defects is formed by the plasma CVD method. Next, the source gas The hydrogen concentration is low and hydrogen is blocked by switching to a mixture of silane and nitrogen. By this method, the insulating film is formed. As the substrate 104, a silicon nitride film having few defects and hydrogen blocking properties is formed. It is possible.

[0043] In addition, when a gallium oxide film is formed as the insulating film 104, MOCVD (Metal O Formed using the organic chemical vapor deposition (OCVD) method It is possible.

[0044] <Semiconductor film formation> Next, a semiconductor film is formed on the insulating film 104 by sputtering, CVD, deposition, or the like. Then, a resist mask is formed on the semiconductor film by a photolithography process. At least a part of the semiconductor film is etched using the resist mask to form a semiconductor film 10. 2D, the semiconductor film 106b is formed. The channel region in the sta 150 is also included.

[0045] Various semiconductor materials can be used for the semiconductor film 106a and the semiconductor film 106b. Specifically, amorphous silicon, microcrystalline silicon, polycrystalline silicon, and single crystal silicon can be used. These films can be provided as a single layer or a laminate. A part of these semiconductor films, or at least one layer in the case of stacked layers, contains impurities that impart a conductivity type. Materials may also be added.

[0046] In addition to the above semiconductor materials, oxide semiconductors can be used. Some of these transistors have the characteristic of having an extremely low off-state current. When the above-mentioned method is used, the capacity of the capacitance element of each pixel in the liquid crystal display device to hold a signal is increased. This makes it possible to reduce the frame frequency, for example, when displaying still images. By reducing the system frequency, the power consumption of the display device can be reduced.

[0047] An oxide semiconductor that can be used for the semiconductor film 106a and the semiconductor film 106b will be described below. Reveal.

[0048] The oxide semiconductor contains, for example, indium. The oxide semiconductor containing indium is In addition, the oxide semiconductor preferably contains an element M. The element M may be, for example, aluminum, gallium, yttrium, or tin. The element M is, for example, an element having a high bond energy with oxygen. The element M is, for example, an oxide. It is an element that has the function of widening the energy gap of semiconductors. The oxide semiconductor preferably contains zinc. When the oxide semiconductor contains zinc, it becomes a crystalline oxide semiconductor. In addition, the energy (Ev) of the top of the valence band of an oxide semiconductor is, for example, This can sometimes be controlled by the atomic ratio.

[0049] However, the oxide semiconductor does not necessarily contain indium. It may be n-Sn oxide or Ga-Sn oxide.

[0050] In addition, when the sum of In and M is 100 atomic %, the oxide semiconductor is The atomic ratio of In is less than 50 atomic %, M is 50 atomic % or more, or I In-M-Zn oxide with n less than 25 atomic % and M greater than or equal to 75 atomic % In addition, the oxide semiconductor may be formed such that the sum of In and M is 100 atomic %. When the atomic ratio of In and M is 25 atomic % or more, the atomic ratio of In is 75 atomic % or more. or In- with 34 atomic % or more and M less than 66 atomic % M-Zn oxide may also be used.

[0051] In addition, oxide semiconductors have a large energy gap. The electron pump is 2.7 eV or more and 4.9 eV or less, preferably 3 eV or more and 4.7 eV or less, and more preferably Preferably, the value is 3.2 eV or more and 4.4 eV or less.

[0052] In order to stabilize the electrical characteristics of a transistor, the impurity concentration in the oxide semiconductor is reduced, It is effective to make it highly intrinsic. Light elements, semi-metallic elements, metallic elements, etc. that are present in the alloy at less than omic percent are considered impurities. For example, hydrogen, Lithium, carbon, nitrogen, fluorine, sodium, silicon, chlorine, potassium, calcium, Titanium, iron, nickel, copper, germanium, strontium, zirconium and hafnium Therefore, the impurity concentration in the adjacent film is also It is preferable to reduce it.

[0053] For example, when silicon is contained in an oxide semiconductor, an impurity level is formed in some cases. In addition, the presence of silicon on the surface of the oxide semiconductor may form an impurity level. Therefore, the silicon concentration inside and on the surface of the oxide semiconductor was measured by secondary ion mass spectrometry (S In IMS (Secondary Ion Mass Spectrometry) , 1×10 19 atoms / cm 3 Less than 5 x 10 18 atoms / cm 3 Not yet More preferably, 2×10 18 atoms / cm 3 Less than.

[0054] In addition, hydrogen in an oxide semiconductor forms an impurity level and increases the carrier density. Therefore, the hydrogen concentration of the oxide semiconductor is 2×10 20 at oms / cm 3 Less than or equal to 5×10 19 atoms / cm 3 More preferably, 1×10 19 atoms / cm 3 Less than 5×10, more preferably 18 atoms / cm 3 In addition, nitrogen in an oxide semiconductor forms an impurity level and increases the carrier density. Therefore, the nitrogen concentration in the oxide semiconductor is , 5×10 19 atoms / cm 3 Less than 5 x 10 18 atoms / cm 3 Below or less, more preferably 1×10 18 atoms / cm 3 Less than 5×10, more preferably 1 7 atoms / cm 3 The following applies.

[0055] Oxide semiconductor films are roughly classified into non-single-crystal oxide semiconductor films and single-crystal oxide semiconductor films. The single-crystal oxide semiconductor film is called CAAC-OS (C Axis Aligned Crystal Talline Oxide Semiconductor film, polycrystalline oxide semiconductor film The oxide semiconductor film includes a microcrystalline oxide semiconductor film, an amorphous oxide semiconductor film, and the like.

[0056] The oxide semiconductor film may include a CAAC-OS film. We will explain about this.

[0057] The CAAC-OS film is one of the oxide semiconductor films that has multiple crystal parts. The crystal part is so large that it fits inside a cube with one side less than 100 nm. The crystals contained in the S film are in the form of cubes with sides of less than 10 nm, 5 nm, or 3 nm. This also includes cases where the size fits within .

[0058] The CAAC-OS film was observed under a transmission electron microscope (TEM). When observed under a ferromagnetic microscope, clear boundaries between the crystals, i.e., crystal boundaries, were observed. It is not possible to confirm the grain boundaries. It can be said that the C-OS film is less susceptible to the decrease in electron mobility caused by grain boundaries.

[0059] The CAAC-OS film was observed by TEM from a direction roughly parallel to the sample surface (cross-sectional TEM observation ) It can be confirmed that the metal atoms are arranged in layers in the crystal part. Each layer has a roughness on the surface on which the CAAC-OS film is to be formed (also called the surface on which the film is to be formed) or on the top surface. The shape is a reflection of the CAAC-OS film and is aligned parallel to the surface on which the CAAC-OS film is formed or the top surface.

[0060] On the other hand, the CAAC-OS film was observed by TEM from a direction roughly perpendicular to the sample surface (planar TEM). When the metal atoms were observed, they were found to be arranged in triangular or hexagonal shapes in the crystals. However, no regularity was observed in the arrangement of metal atoms between different crystal parts. stomach.

[0061] Cross-sectional and planar TEM observations revealed that the crystals in the CAAC-OS film had an orientation. It is clear that there are

[0062] X-ray diffraction (XRD) was performed on the CAAC-OS film. For example, InGaZnO 4 CAAC-OS film with crystals In the out-of-plane analysis, a peak was observed at a diffraction angle (2θ) of approximately 31°. This peak may appear in InGaZnO 4 It is assigned to the (009) plane of the crystal of This indicates that the crystals in the CAAC-OS film have a c-axis orientation, and the c-axis is generally aligned on the surface on which the film is formed or on the upper surface. It can be seen that it is oriented in a substantially vertical direction.

[0063] On the other hand, in-plane X-ray irradiation is performed on the CAAC-OS film in a direction perpendicular to the c-axis. In the analysis by the ane method, a peak may appear at 2θ around 56°. This peak is , InGaZnO 4 It is attributed to the (110) plane of the InGaZnO crystal. 4 Single crystal oxidation of In the case of a semiconductor film, 2θ is fixed at around 56°, and the normal vector of the sample surface is set as the axis (φ axis). When the sample is rotated and analyzed (φ scan), the crystal plane equivalent to the (110) plane is In contrast, in the case of the CAAC-OS film, the 2θ is set to 5 Even when the φ is fixed at around 6° and scanned, no clear peak appears.

[0064] From the above, it is considered that the a-axis and b-axis orientations are inconsistent between different crystal regions in the CAAC-OS film. The crystal is regular, but has a c-axis orientation, and the c-axis is parallel to the normal vector of the surface on which the crystal is formed or the upper surface. Therefore, the layered arrangement confirmed by the cross-sectional TEM observation mentioned above is consistent with the above. Each layer of aligned metal atoms is a plane parallel to the ab plane of the crystal.

[0065] The crystalline portion is formed when the CAAC-OS film is formed or when a crystallization process such as a heat treatment is performed. As described above, the c-axis of the crystal is aligned along the surface on which the CAAC-OS film is formed or along the surface on which the CAAC-OS film is formed. The orientation of the CAAC-OS film is parallel to the normal vector of the top surface. When the shape of the CAAC-OS film is changed by etching, the c-axis of the crystal is aligned with the surface on which the CAAC-OS film is formed. Or it may not be parallel to the normal vector of the upper surface.

[0066] In addition, the degree of crystallinity in the CAAC-OS film may not be uniform. When the crystal part of the CAAC-OS film is formed by crystal growth from the vicinity of the top surface, The adjacent regions may have a higher degree of crystallinity than the regions adjacent the surface to be formed. When impurities are added to a C-OS film, the crystallinity of the region to which the impurities are added changes, resulting in partial In some cases, regions of differing crystallinity may be formed.

[0067] In addition, InGaZnO 4 Out-of-plane synthesis of CAAC-OS films with crystallites In the analysis by , in addition to the peak at 2θ near 31°, a peak also appeared at 2θ near 36°. The peak at 2θ of around 36° may be due to the c-axis orientation in some parts of the CAAC-OS film. The CAAC-OS film contains crystals that do not have a 2θ of around 31°. It is preferred that the spectrum exhibits a peak and does not exhibit a peak at 2θ of around 36°.

[0068] The CAAC-OS film is an oxide semiconductor film with a low concentration of impurities. The impurities include hydrogen, carbon, and The elements are other than the main components of the oxide semiconductor film, such as silicon and transition metal elements. The elements that bond to oxygen more strongly than the metal elements that form the oxide semiconductor film, such as arsenic, are oxidized. By removing oxygen from the oxide semiconductor film, the atomic arrangement of the oxide semiconductor film is disrupted, reducing its crystallinity. In addition, heavy metals such as iron and nickel, argon, and carbon dioxide have an atomic radius of Since the molecular radius is large, when the cation is contained in the oxide semiconductor film, the The impurities in the oxide semiconductor film may cause the atomic arrangement to be disturbed, which may result in a decrease in crystallinity. Objects can act as carrier traps or carrier generation sources.

[0069] The CAAC-OS film is an oxide semiconductor film having a low density of defect states. Oxygen vacancies in the semiconductor film can become carrier traps or trap hydrogen, It can be a carrier source.

[0070] A material with a low impurity concentration and a low defect level density (few oxygen vacancies) is called a high-purity intrinsic or The term "substantially high-purity intrinsic" refers to a highly-purified intrinsic oxide semiconductor film. Since the carrier generation source is small, the carrier density can be reduced. A transistor using an oxide semiconductor film has electrical characteristics in which the threshold voltage is negative ( Also called marion.) It is rare for it to become high purity genuine or substantially high purity genuine. The oxide semiconductor film has few carrier traps. A transistor using such a material has small fluctuation in electrical characteristics and is highly reliable. Note that it takes a long time for charges trapped in the carrier traps in the oxide semiconductor film to be released. The charge is long and can behave like a fixed charge. In addition, a transistor using an oxide semiconductor film having a high density of defect states has unstable electrical characteristics. There are cases.

[0071] In addition, the electrical characteristics of transistors using CAAC-OS films were improved by irradiation with visible light or ultraviolet light. The fluctuation is small.

[0072] Next, a microcrystalline oxide semiconductor film will be described.

[0073] In the microcrystalline oxide semiconductor film, crystal parts can be clearly seen in the TEM image. The crystal parts contained in the microcrystalline oxide semiconductor film may have a size of 1 nm or more and 100 nm or less. In particular, the size of the particles is between 1 nm and 10 nm. Nanocrystals (nc) are microcrystals with a diameter of 1 nm or less and 3 nm or less. The oxide semiconductor film having Al was formed by The nc-OS film is called a TE semiconductor film. In the M image, the grain boundaries may not be clearly visible.

[0074] The nc-OS film is a microscopic region (e.g., a region of 1 nm to 10 nm, especially a region of 1 nm or more). The atomic arrangement has periodicity in the region of 3 nm or less. There is no regularity in the crystal orientation between the crystal parts. Therefore, no orientation is observed throughout the film. Therefore, depending on the analysis method, the nc-OS film may be indistinguishable from an amorphous oxide semiconductor film. For example, an XRD apparatus that uses X-rays with a diameter larger than that of the crystal part for an nc-OS film may be used. When the structure was analyzed using the out-of-plane method, the crystal plane was not shown. In addition, the nc-OS film has a larger diameter (e.g., 50 nm) than the crystalline part. When electron diffraction (also called selected area electron diffraction) is performed using an electron beam of 1000 nm or more, halo On the other hand, the nc-OS film shows a diffraction pattern similar to the size of the crystals. Electron beam diffraction ( When nanobeam electron diffraction (NCD) is performed, spots are observed. When nanobeam electron diffraction is performed on the film, a circular (ring-shaped) area of ​​high brightness is observed. In addition, nanobeam electron diffraction of the nc-OS film reveals ring-shaped Multiple spots may be observed within an area.

[0075] The nc-OS film is an oxide semiconductor film that has higher order than an amorphous oxide semiconductor film. Therefore, the nc-OS film has a lower density of defect states than the amorphous oxide semiconductor film. In the nc-OS film, there is no regularity in the crystal orientation between different crystal parts. The S film has a higher density of defect states than the CAAC-OS film.

[0076] The oxide semiconductor film may be, for example, an amorphous oxide semiconductor film, a microcrystalline oxide semiconductor film, or a CA The AC-OS film may be a laminate film having two or more kinds of films.

[0077] For example, an oxide semiconductor layer (S1) and an oxide semiconductor layer (S2) are formed in this order. It may be a multi-layer film.

[0078] At this time, for example, the energy (Ec) of the conduction band minimum of the oxide semiconductor layer (S2) is Specifically, the oxide semiconductor layer (S2) is made of an oxide The electron affinity of the semiconductor layer (S1) is 0.07 eV or more and 1.3 eV or less, preferably 0 0.1 eV or more and 0.7 eV or less, more preferably 0.15 eV or more and 0.4 eV or less An oxide semiconductor is used. Note that the electron affinity is the difference between the vacuum level and the energy at the bottom of the conduction band. It is.

[0079] Alternatively, for example, the energy gap of the oxide semiconductor layer (S The energy gap is larger than that of 1). For example, the energy gap can be derived by optical methods. Specifically, the oxide semiconductor layer (S1) can be used as the oxide semiconductor layer (S2). ) with an energy gap of 0.1 eV or more and 1.2 eV or less, preferably 0.2 eV or less. An oxide semiconductor with a larger peak voltage of 0.8 eV or less is used.

[0080] Alternatively, the oxide semiconductor may be, for example, an oxide semiconductor layer (S1) and an oxide semiconductor layer (S2). and the oxide semiconductor layer (S3) may be formed in this order.

[0081] Alternatively, for example, the energy (Ec) of the conduction band minimum of the oxide semiconductor layer (S2) is The temperature is set lower than that of the semiconductor layer (S1) and the oxide semiconductor layer (S3). The conductor layer (S2) has a higher electrical conductivity than the oxide semiconductor layer (S1) and the oxide semiconductor layer (S3). The electron affinity is 0.07 eV or more and 1.3 eV or less, preferably 0.1 eV or more and 0.7 eV or less More preferably, an oxide semiconductor having a larger polarization ratio by 0.15 eV or more and 0.4 eV or less is used.

[0082] Alternatively, for example, the energy gap of the oxide semiconductor layer (S Specifically, the oxide semiconductor layer (S 2) As the oxide semiconductor layer (S1) and the oxide semiconductor layer (S3), The gap is 0.1 eV or more and 1.2 eV or less, preferably 0.2 eV or more and 0.8 eV or less. A thin oxide semiconductor is used.

[0083] Alternatively, for example, in order to increase the on-state current of the transistor, the oxide semiconductor layer (S3) For example, the oxide semiconductor layer (S3) is preferably less than 10 nm. The thickness of the oxide semiconductor layer (S3) is preferably 5 nm or less, and more preferably 3 nm or less. The element (silicon) constituting the insulating film 104 is introduced into the oxide semiconductor layer (S2) having a high current density. It also has the function of blocking the intrusion of oxide semiconductor layers (S3 ) preferably has a certain degree of thickness. For example, the thickness of the oxide semiconductor layer (S3) is 0.3 nm or more, preferably 1 nm or more, and more preferably 2 nm or more.

[0084] In addition, the thickness of the oxide semiconductor layer (S1) is thicker than the thickness of the oxide semiconductor layer (S2). The thickness of the semiconductor layer (S2) is preferably set to be thicker than the thickness of the oxide semiconductor layer (S3). Specifically, the thickness of the oxide semiconductor layer (S1) is 20 nm or more, preferably 30 nm or more. The oxide semiconductor is preferably 1.0 nm or more, more preferably 40 nm or more, and even more preferably 60 nm or more. The thickness of the conductor layer (S1) is set to 20 nm or more, preferably 30 nm or more, and more preferably 4 0 nm or more, more preferably 60 nm or more, so that the insulating film and the oxide semiconductor layer (S ) to the oxide semiconductor layer (S2) having a high current density, preferably 20 nm or more. The distance is preferably 30 nm or more, more preferably 40 nm or more, and even more preferably 60 nm or more. However, the productivity of the semiconductor device may decrease, so The thickness of the layer is 200 nm or less, preferably 120 nm or less, and more preferably 80 nm or less. The thickness of the oxide semiconductor layer (S2) is preferably 3 nm or more and 100 nm or less. The thickness is preferably 3 nm or more and 80 nm or less, and more preferably 3 nm or more and 50 nm or less.

[0085] Next, a method for forming an oxide semiconductor film will be described. The method may be a CVD method, an MBE method, an ALD method or a PLD method.

[0086] As the oxide semiconductor film to be the semiconductor film 106, In-M-Zn oxide was deposited by sputtering. When forming a film, the atomic ratio of the target is In:M:Zn 3:1:1, 3:1:2, 3:1:4, 1:1:0.5, 1:1:1, 1:1:2, 1:3:1, 1:3:2, 1: 3:4, 1:3:6, 1:6:2, 1:6:4, 1:6:6, 1:6:8, 1:6:10 , 1:9:2, 1:9:4, 1:9:6, 1:9:8, 1:9:10, etc. The element M is, for example, aluminum, gallium, yttrium, or tin.

[0087] When the oxide semiconductor film is formed by a sputtering method, the film is formed in an atmosphere containing oxygen. For example, the ratio of oxygen in the entire atmosphere is set to 10 volume % or more, preferably 20 volume % or more. % or more, more preferably 50% or more, and even more preferably 80% or more. In particular, the ratio of oxygen in the entire atmosphere is set to 100 volume percent. If the ratio of oxygen in the entire atmosphere is 100 volume %, In order to reduce the concentration of impurities such as rare gases contained in the oxide semiconductor film that becomes the insulating film 106, can.

[0088] In the case where the oxide semiconductor film to be the semiconductor film 106 is formed by a sputtering method, In some cases, a film with a different atomic ratio may be formed. For example, zinc contains oxygen. When a film is formed in an atmosphere, the atomic ratio of the film tends to be smaller than that of the target. Specifically, the ratio of the number of zinc atoms contained in the target is 40 atomic % or more. In some cases, the concentration of indium may be about 0 atomic % or less. When a film is formed in an atmosphere, the atomic ratio of the film tends to be smaller than that of the target. There is.

[0089] It is preferable to perform first heat treatment after forming the oxide semiconductor film which is to be the semiconductor film 106. The first heat treatment is performed at a temperature of 70° C. or higher and 450° C. or lower, preferably 100° C. or higher and 300° C. or lower. More preferably, the first heat treatment is performed at a temperature of 150° C. or higher and 250° C. or lower. Inert gas atmosphere, or oxidizing gas of 10 ppm or more, 1 volume % or more The first heat treatment is carried out in an atmosphere containing 10 volume % or more of fluorine. The first heat treatment may be carried out under reduced pressure. Alternatively, the atmosphere of the first heat treatment is an inert gas atmosphere, and then the desorbed oxygen is removed. To supplement the base, oxidizing gas is added at 0.001 volume% or more, 1% or more, or 10% or more. The first heat treatment may be performed in an atmosphere containing the semiconductor film 106. Impurities such as hydrogen and water can be removed from the oxide semiconductor film. By this process, the oxide semiconductor film to be the semiconductor film 106 can be highly purified and made intrinsic.

[0090] <Insulating film formation> Next, an insulating film 108 is formed above the insulating film 104, the semiconductor film 106a, and the semiconductor film 106b. The insulating film 108 is formed on the semiconductor film 10 in the transistor 150 (FIG. 2(E)). It functions as a membrane to protect the channel region of 6b.

[0091] The insulating film 108 can be formed using the same material, structure and method as the insulating film 104 .

[0092] When the insulating film 104 is formed by laminating films made of different materials, the upper layer of the insulating film 104 and The same material can be applied to the insulating film 108. If the insulating films 104 and 108 are made of the same material, The upper layer of the insulating film 104 and the insulating film 108 can be etched at the same time. The lower layer of the insulating film 104 is then etched. The taper angle of the insulating film 108 is different from the taper angle of the lower layer of the insulating film 104 to form an opening. By forming the openings with different taper angles, the conductive film formed in the openings can be cut stepwise. This suppresses the

[0093] <Mask formation and insulating film etching> Next, a resist mask 110 is formed on the insulating film 108 by a photolithography process. (Figure 3(A)).

[0094] Next, the portions of the insulating film 104 and the insulating film 108 that do not overlap with the resist mask 110 are etched. The insulating layer is removed by etching to form openings 111a, 111b, 111c, and 111d (FIG. 3( B).

[0095] As shown in FIG. 3B, the openings 111a, 111c, and 111d are formed by removing the semiconductor The resist mask 110 is formed by applying a resist pattern to the semiconductor film 106a or the semiconductor film 106b. It is formed by removing a portion.

[0096] The opening 111b overlaps the conductive film 102a of the insulating film 104 and the insulating film 108. The semiconductor film 106a, the semiconductor film 106b, and the resist mask 110 do not overlap with each other. It is formed by removing

[0097] Next, the resist mask 110 is removed (FIG. 3(C)).

[0098] <Conductive film formation> Next, the insulating film 108, the semiconductor film 106a, the semiconductor film 106b, and the conductive film 102a are A conductive film is formed on the conductive film, and a resist mask is formed on the conductive film by a photolithography process. Next, the conductive film is partly etched using the resist mask to form the conductive film 114a. 114b and 114c are formed (FIG. 3(D)).

[0099] The conductive film 114a is electrically connected to the conductive film 102a and the semiconductor film 106a. The conductive film 114b and the conductive film 114c are electrically connected to the semiconductor film 106b.

[0100] The conductive film 114a functions as a wiring that electrically connects the conductive film 102a and the semiconductor film 106a. The conductive film 114b can function as a source electrode in the transistor 150. The conductive film 114c can function as a drain electrode in the transistor 150. It can function as a.

[0101] The conductive films 114a, 114b, and 114c are similar to the conductive films 102a and 102b. It can be formed by a material, a configuration and a method.

[0102] Through the above steps, the transistor 150 and the connection portion 160 can be formed.

[0103] In this way, in the manufacturing method 1, an opening is formed in the portion of the insulating film 108 that overlaps with the semiconductor film. At the same time, in the portion not overlapping the semiconductor film, an opening is formed not only in the insulating film 108 but also in the insulating film 104. By performing such a process, the openings in the insulating film 108 and the insulating film 104 are formed separately. This allows the number of masks and photolithography steps to be reduced compared to when a semiconductor device is formed by a conventional method. Therefore, the manufacturing time of the semiconductor device can be shortened and the manufacturing costs can be suppressed.

[0104] ≪Manufacturing method 2≫ Next, referring to FIG. 4 and FIG. 5, the transistor 150 and the connection portion 16 shown in FIG. 5(E) will be described. Explain how to form 0.

[0105] As shown in FIGS. 4(A) to 4(E), the substrate 100, the conductive film 102a and the conductive film 102b, the insulating film 102a, the insulating film 102b, and the insulating film 102b are Regarding the film 104, the semiconductor film 106a and the semiconductor film 106b, and the insulating film 108, The insulating film 10 can be formed using the same materials, configuration and method as in manufacturing method 1.

[0106] <Mask formation and insulating film etching> A resist mask 210 is formed above the insulating film 108 by a photolithography process. (FIG. 4(F)). As shown in FIG. 4(F), the resist mask 210 has different thicknesses depending on the region. 210a and 210b, which have a thickness smaller than that of the region 210a. The region 210b includes a portion overlapping the semiconductor film 106a and the semiconductor film 106b. has a share.

[0107] The resist mask 210 is a multi-tone mask (half-tone photomask or gray-tone It is formed by a photolithography process using a photomask.

[0108] Next, the insulating film 104 and the insulating film 108 are formed by etching the conductive film 102a and the resist mask. The portion that does not overlap with the gate 210 is removed by etching to form an opening 111b (FIG. 5( A)).

[0109] Next, the resist mask 210 is subjected to ashing. The area (volume when viewed three-dimensionally) shrinks and the thickness becomes smaller. Therefore, the area with a small thickness The resist mask 210 at 210b is removed, and a resist mask 212 is formed (FIG. 5). In other words, the resist mask 210 is recessed, so that the resist in the region 210b is removed. The resist mask 210 is removed, and a resist mask 212 is formed.

[0110] The ashing can be carried out, for example, by oxygen plasma.

[0111] Next, the portion of the insulating film 108 that does not overlap with the resist mask 212 is removed by etching. , openings 211a, 211b, 211c, and 211d are formed (FIG. 5(C)).

[0112] As shown in FIG. 5C, the openings 211a, 211c, and 211d are formed by removing the semiconductor The resist mask 212 is formed by applying a resist mask 213 to the semiconductor film 106a or the semiconductor film 106b. It is formed by removing a portion.

[0113] The opening 211b is formed between the semiconductor film 106a, the semiconductor film 106b and the resist of the insulating film 108. The portions that do not overlap with the mask 212 are removed. As shown in FIG. 1, the insulating film 108 around the opening 111b is removed, and the opening 211b becomes wider. This allows the conductive film to be formed in the opening 211b in a later step. Breaking of the step is suppressed.

[0114] Next, the resist mask 212 is removed (FIG. 5(D)).

[0115] <Conductive film formation> Next, the insulating film 108, the semiconductor film 106a, the semiconductor film 106b, and the conductive film 102a are A conductive film is formed on the conductive film, and a resist mask is formed on the conductive film by a photolithography process. Next, the conductive film is partly etched using the resist mask to form the conductive film 114a. 114b and 114c are formed (FIG. 5(E)).

[0116] The conductive films 114a, 114b, and 114c are formed using the same materials, configurations, and methods as those in the manufacturing method 1. It can be achieved.

[0117] Through the above steps, the transistor 150 and the connection portion 160 can be formed.

[0118] In this way, in the manufacturing method 2, the openings 211a and 211b are formed by using a multi-tone mask. , 211c, and 211d can be formed using a single mask. In this case, the opening in the insulating film 108 can be made wider than the opening in the insulating film 104. It is possible to suppress the step break of 4a.

[0119] By adopting such a process, the number of masks and photolithography processes can be reduced. This allows the manufacturing time of the semiconductor device to be shortened and the manufacturing costs to be reduced. In addition, the yield and reliability of the semiconductor device can be improved.

[0120] ≪Manufacturing method 3≫ Next, referring to FIG. 6 and FIG. 7, the transistor 150 and the connection part 16 shown in FIG. Explain how to form 0.

[0121] As shown in FIG. 6(A) to (C), the substrate 100, the conductive film 102a, and the conductive film 102b are The insulating film 104 is formed using the same material, structure and method as in manufacturing method 1. can be done.

[0122] <Semiconductor film formation> A semiconductor film 106 is formed above the insulating film 104. The semiconductor film 106 is manufactured by It can be formed using the same materials, configuration and method as in Method 1.

[0123] <Mask formation and etching of insulating and semiconductor films> Next, a resist mask 307 is formed above the semiconductor film 106 by a photolithography process. As shown in FIG. 6D, the resist mask 307 is formed in some areas. The thickness is different, and the thickness of the region 307a is different from that of the region 307a. The region 307b has a portion overlapping with the semiconductor film 106.

[0124] The resist mask 307 is a multi-tone mask (half-tone photomask or gray-tone It is formed by a photolithography process using a photomask.

[0125] Next, the insulating film 104 and the semiconductor film 106 are formed by etching the conductive film 102a and the resist film 104. The portion that does not overlap with the mask 307 is removed by etching to form an opening 308b (FIG. 6 (E)).

[0126] Next, the resist mask 307 is subjected to ashing. The area (volume when viewed three-dimensionally) shrinks and the thickness becomes smaller. Therefore, the area with a small thickness The resist mask 307 of 307b is removed, and a resist mask 309 is formed (FIG. 7). In other words, the resist mask 307 is recessed to form a recess in the region 307b. The resist mask 307 is removed, and a resist mask 309 is formed.

[0127] The ashing can be carried out, for example, by oxygen plasma.

[0128] Next, the portion of the semiconductor film 106 that does not overlap with the resist mask 309 is removed by etching. The semiconductor film 106a and the semiconductor film 106b are formed (FIG. 7(B)). 6b functions as a semiconductor film including a channel region in the transistor 150. can be done.

[0129] Next, the resist mask 309 is removed (FIG. 7(C)).

[0130] <Insulating film formation> Next, an insulating film is formed above the insulating film 104, the semiconductor film 106a, and the semiconductor film 106b. Then, a resist mask is formed on the insulating film by a photolithography process. A resist mask is used to etch a portion of the insulating film to form openings 311a, 311b, and 311c. c, and an insulating film 108 having 311d is formed (FIG. 7(D)).

[0131] As shown in FIG. 7D, the openings 311a, 311c, and 311d are formed in the semiconductor film 106a or is formed in a portion overlapping with the semiconductor film 106b.

[0132] In addition, the opening 311b is formed by removing the portion that does not overlap with the semiconductor film 106a and the semiconductor film 106b. As shown in FIG. 7D, the opening 311b is formed by The opening 311b is formed in a portion overlapping with the opening of the insulating film 104. The opening of the insulating film 108 can be made wider. This allows the opening to be formed more easily in a later process. This suppresses step discontinuity in the conductive film formed on 311b.

[0133] The insulating film 108 protects the channel region of the semiconductor film 106b in the transistor 150. The film functions as a protective film, and can be formed using the same materials, configuration and method as in Production Method 1.

[0134] <Conductive film formation> Next, the insulating film 108, the semiconductor film 106a, the semiconductor film 106b, and the conductive film 102a are A conductive film is formed on the conductive film, and a resist mask is formed on the conductive film by a photolithography process. Next, the conductive film is partly etched using the resist mask to form the conductive film 114a. 114b and 114c are formed (FIG. 7(E)).

[0135] The conductive films 114a, 114b, and 114c are formed using the same materials, configurations, and methods as those in the manufacturing method 1. It can be achieved.

[0136] Through the above steps, the transistor 150 and the connection portion 160 can be formed.

[0137] In this manner, in the manufacturing method 3, the insulating film 10 is formed by using a half-tone photomask. The opening of No. 4 and the formation of the semiconductor film 106a and the semiconductor film 106b are formed using one mask. In addition, the opening 311b is larger in the insulating film 108 than in the insulating film 104. The opening can be made wider, and step disconnection of the conductive film 114a can be suppressed.

[0138] By adopting such a process, the number of masks and photolithography processes can be reduced. This allows the manufacturing time of the semiconductor device to be shortened and the manufacturing costs to be reduced. In addition, the yield and reliability of the semiconductor device can be improved.

[0139] <Opening Variations> By changing the shape of the resist mask 307, the connection portion 160 shown in FIG. A connecting portion 160 shown in FIG. 8(D) can be formed, which has a different shape.

[0140] For this, first, a resist mask 307 is formed in a shape as shown in FIG. 8(A)) and an opening 308b is formed (see FIG. 8(A)). )).

[0141] Next, the semiconductor film 106a and the semiconductor film 106b are formed by the same steps as those shown in FIGS. (Figure 8(B)).

[0142] Next, an insulating film is formed above the insulating film 104, the semiconductor film 106a, and the semiconductor film 106b. Then, a resist mask is formed on the insulating film by a photolithography process. A resist mask is used to etch a portion of the insulating film to form openings 311a, 312b, and 311c. At this time, the insulating film 108 having the openings 311c and 311d is formed. The opening 12b is formed so as to be smaller than the opening 308b in the insulating film 104.

[0143] Through the above steps, the connection portion 160 shown in FIG. 8(D) can be formed.

[0144] As such a process, the opening of the insulating film 104 and the semiconductor film 106a and the semiconductor film 10 6b can be formed using one mask, and step discontinuity of the conductive film 114a can be suppressed. This reduces the number of masks and photolithography processes, and shortens the manufacturing time of the semiconductor device. In addition, the yield and reliability of the semiconductor device can be improved. It can be improved.

[0145] ≪Manufacturing method 4≫ Next, referring to FIG. 9 and FIG. 10, the transistor 150 and the connection part shown in FIG. 10(E) will be described. A method for forming 160 is described.

[0146] The substrate 100, the conductive film 102a and the conductive layer 102b shown in FIG. 9(A) to FIG. The conductive film 102b, the insulating film 104, the semiconductor film 106a and the semiconductor film 106b, and the insulating film 108 The openings 111a, 111b, 111c, and 111d are made of the same material as in the manufacturing method 1. It can be formed by the structure and method.

[0147] <Mask Ashing> As shown in FIG. 10A, openings 111a, 111b, and 111c are formed by using a resist mask 110. After forming the resist mask 110, the resist mask 110 is ashed. For example, ashing using oxygen plasma can be performed.

[0148] As a result, the area (volume when viewed three-dimensionally) of the resist mask 110 is reduced, and the thickness is reduced. As a result, the insulating film 10 is thinned, and a resist mask 412 is formed (FIG. 10(B)). 8, there are portions that are not covered by the resist mask 412. By retracting the mask 110, a part of the insulating film 108 is exposed.

[0149] Next, the portion of the insulating film 108 that does not overlap the resist mask 412 is removed by etching. , openings 411a, 411b, 411c, and 411d are formed (FIG. 10(C)).

[0150] As shown in FIG. 10C, the openings 411a, 411c, and 411d are formed in the semiconductor film 106a. Alternatively, it is formed in a portion overlapping with the semiconductor film 106b.

[0151] The opening 411b overlaps the conductive film 102a and the semiconductor film 106a and the semiconductor film 106b. It is formed by removing the part that does not overlap with 06b. As shown in FIG. 1, the insulating film 108 around the opening 111b is removed to widen the opening 411b. This prevents the step of the conductive film to be formed in the opening 411b in a later process from being cut off. This suppresses the

[0152] In addition, the resist mask 110 is ashed to form a resist mask 412. Therefore, the difference in size between the resist mask 110 and the resist mask 412, i.e., the The width of the insulating film 108 exposed from the resist mask 412 is approximately the same.

[0153] Therefore, the width of the step formed by the insulating film 104 and the insulating film 108 in the opening 411b, that is, That is, L in FIG. 10(C) is approximately equal around the opening 411b.

[0154] Next, the resist mask 412 is removed (FIG. 10(D)).

[0155] <Conductive film formation> Next, the insulating film 108, the semiconductor film 106a, the semiconductor film 106b, and the conductive film 102a are A conductive film is formed on the conductive film, and a resist mask is formed on the conductive film by a photolithography process. Next, the conductive film is partly etched using the resist mask to form the conductive film 114a. 114b and 114c are formed (FIG. 10(E)).

[0156] The conductive films 114a, 114b, and 114c are formed using the same materials, configurations, and methods as those in the manufacturing method 1. It can be achieved.

[0157] Through the above steps, the transistor 150 and the connection portion 160 can be formed.

[0158] In this manner, in the manufacturing method 4, an opening is formed in the portion of the insulating film 108 that overlaps with the semiconductor film. At the same time, in the portion not overlapping the semiconductor film, an opening is formed not only in the insulating film 108 but also in the insulating film 104. By performing such a process, the openings in the insulating film 108 and the insulating film 104 are formed separately. This allows the number of masks and photolithography steps to be reduced compared to when a semiconductor device is formed by a conventional method. The resist mask 110 is removed by ashing, so that the insulating film 1 is The opening in the insulating film 108 can be made wider than the opening in 04, and the step discontinuity of the conductive film 114a can be prevented. It can be suppressed.

[0159] By adopting such a process, the number of masks and photolithography processes can be reduced. This allows the manufacturing time of the semiconductor device to be shortened and the manufacturing costs to be reduced. In addition, the yield and reliability of the semiconductor device can be improved.

[0160] (Embodiment 2) A method for manufacturing a semiconductor device according to one embodiment of the present invention will now be described with reference to FIGS. As described above, FIG. 1 is a top view of a semiconductor device. The cross-sectional structure of the portion indicated by 1-X2 is shown in cross section X1-X2 of FIG. 11 and FIG. X1-X2 is a region where a transistor is electrically connected to a conductive film provided above the transistor. 1B is a cross-sectional view of a portion of the region shown in FIG. The surface structure is shown in cross section Y1-Y2 of FIG. 11 and FIG. 12. Cross section Y1-Y2 is a cross section of the semiconductor film. A region where a conductive film provided below and a conductive film provided above the semiconductor film are electrically connected The cross-sectional structure of the portion indicated by the dashed line Z1-Z2 in FIG. 1(C) is shown in FIG. 1 and cross section Z1-Z2 in FIG. 12. Cross section Z1-Z2 is a cross section of a source electrode of a transistor. and a conductive film formed simultaneously with the conductive film that can function as a drain electrode; A cross-sectional structure of a part of the region where two conductive films formed on the top of a transistor are electrically connected. It is made of.

[0161] The method for manufacturing a semiconductor device shown in this embodiment mode is to form a plurality of conductive films on the upper part of a transistor. For example, it can be applied to the case where a common electrode and a pixel electrode are formed on the same substrate. IPS (In Plane Switching) (or FFS (fringe This is suitable for liquid crystal display devices in a field switching mode.

[0162] ≪Manufacturing method 5≫ 11 and 12, the connection portion 550 and the connection portion 560 shown in FIG. 12(E) are formed. This article explains how to achieve this.

[0163] <Lower structure> First, a substrate provided with a conductive film is prepared. The substrate may be a substrate on which the conductive film 150 and the connection portion 160 are formed, or a conductive film formed by other methods and configurations. For example, the bottom gate transistor shown in the first embodiment may be formed on a substrate. The substrate is not limited to the transistor 150, but may be a substrate on which a transistor having a top gate structure is formed. .

[0164] In this embodiment, similarly to the manufacturing method 2 of the first embodiment, a transistor is formed on the cross section X1-X2. 150, a connection portion 160 is formed on the cross section Y1-Y2, and then the same process as in manufacturing method 2 is carried out. A substrate on which the insulating film 104, the insulating film 108 and the conductive film 114d are formed on the cross section Z1-Z2. The conductive film 114d is prepared by forming the conductive film 114a and the conductive film 114b. The conductive film 11 of the substrate can be formed with the same material, structure and method as those of the conductive film 114c. The connection parts 550 and 560 are formed on the conductive film 114a and the conductive film 114d by the following steps. do.

[0165] <Insulating film formation> An insulating film 500 is formed above the conductive films 114a, 114b, 114c, and 114d (FIG. 11(B)). The insulating film 500 is made of the same material, has the same structure, and is similar to the insulating film 104 of the first embodiment. It can be formed by the method.

[0166] <Insulating film formation> Next, an insulating film 502 is formed on the insulating film 500 (FIG. 11(C)). The film can function as a planarizing film in a semiconductor device.

[0167] The insulating film 502 is made of, for example, acrylic, acrylamide, ester, or other known materials. The insulating layer may be formed as a laminate or a single layer.

[0168] <Conductive film formation> Next, a conductive film 504 is formed above the insulating film 502 (FIG. 11(D)). It is preferable to use a light-transmitting material as the light-transmitting layer.

[0169] The conductive film 504 may be formed of indium oxide containing tungsten oxide or tungsten oxide. Indium zinc oxide, indium oxide with titanium oxide, indium Indium tin oxide, indium tin oxide (hereinafter referred to as ITO), indium zinc oxide, It is possible to use a conductive material having light transmission properties, such as indium tin oxide doped with silicon dioxide. can.

[0170] The conductive film 504 is made of a conductive composition containing a conductive polymer. The light-transmitting conductive film formed using the conductive composition can be formed by a sheet. Resistance is 10000Ω / □ or less, and light transmittance at a wavelength of 550nm is 70% or more. It is also preferable that the resistivity of the conductive polymer contained in the conductive composition is 0.1 Ω cm or less. It is preferable that:

[0171] As the conductive polymer, a so-called π-electron conjugated conductive polymer can be used. For example, polyaniline or its derivatives, polypyrrole or its derivatives, polythiophene or or its derivatives, copolymers of two or more of aniline, pyrrole and thiophene, or their derivatives.

[0172] The conductive film 504 can be provided as a single layer or a stack of the above-mentioned materials.

[0173] <Mask formation and etching of conductive and insulating films> Next, a resist mask 506 is formed above the conductive film 504 by a photolithography process. As shown in FIG. 11E, the resist mask 506 is The thickness of the thin film is different in the region 506a and the thickness of the thin film is smaller than the thickness of the thin film in the region 506a. The region 506b overlaps with the conductive film 504.

[0174] The resist mask 506 is a multi-tone mask (half-tone photomask or gray-tone It is formed by a photolithography process using a photomask.

[0175] Next, the insulating film 500, the insulating film 502, and the conductive film 504 are removed so as not to overlap with the resist mask 506. The non-contact portions are removed by etching to form openings 507a and 507c (FIG. 1 2(A)).

[0176] Next, the resist mask 506 is subjected to ashing. The area (volume when viewed three-dimensionally) shrinks and the thickness becomes smaller. Therefore, the area with a small thickness The resist mask 506 of 506b is removed, and a resist mask 508 is formed (FIG. 1 2(B)). That is, the resist mask 506 is recessed to expose the region 506b. The resist mask 506 is removed, and a resist mask 508 is formed.

[0177] The ashing can be carried out, for example, by oxygen plasma.

[0178] Next, the portion of the conductive film 504 that does not overlap with the resist mask 508 is removed by etching. Then, the resist mask 508 is removed to form a conductive film 504a (FIG. 12(C)). The conductive film 504a can function as a common electrode in a liquid crystal display device.

[0179] <Insulating film formation> Next, the conductive film 504a, the insulating film 502, the insulating film 500, the conductive film 114d and the conductive film 11 An insulating film is formed above 4c, and a resist mask is formed on the insulating film by a photolithography process. Next, a part of the insulating film is etched using the resist mask to form an insulating film. As shown in FIG. 12(D), an opening is formed in the insulating film 510. An opening 511a is formed in a portion overlapping with the conductive film 507a, and an opening 511b is formed in a portion overlapping with the conductive film 504a. An opening 511c is formed in a portion overlapping with the opening 507c.

[0180] The insulating film 510 is formed of the same material, with the same structure and by the same method as the insulating film 104 of the first embodiment. It is possible.

[0181] <Conductive film formation> Next, the insulating film 510, the conductive film 504a, the insulating film 502, the insulating film 500, the conductive film 114d, and A conductive film is formed above the conductive film 114c, and a photolithography process is performed on the conductive film. Then, a resist mask is formed by etching a part of the conductive film using the resist mask. Then, a conductive film 512a and a conductive film 512b are formed (FIG. 12(E)).

[0182] The conductive film 512a is electrically connected to the conductive film 114d and the conductive film 504a. The conductive film 512b is electrically connected to the conductive film 114c. In addition, although not shown, the conductive film 504a can function as a pixel electrode in the device. The portion where the conductive film 512b overlaps with the insulating film 512 can function as a capacitor. However, the capacitor may be formed in any portion other than the portion where the conductive film 504a and the conductive film 512b overlap. For example, a portion where the conductive film 504a and a separately formed conductive film overlap each other may be used as a capacitor element. It may also function as

[0183] The conductive film 512a and the conductive film 512b are formed using the same material, structure, and method as the conductive film 504a. It can be formed with.

[0184] Through the above steps, the connection portion 550 and the connection portion 560 can be formed.

[0185] In this manner, in the manufacturing method 5, by using a half-tone photomask, the opening 507 The opening 507a, the opening 507c, and the conductive film 504a can be formed using one mask.

[0186] By adopting such a process, the number of masks and photolithography processes can be reduced. This makes it possible to reduce the manufacturing time and costs of the semiconductor device.

[0187] (Embodiment 3) Regarding another aspect of the manufacturing method of the semiconductor device according to the second embodiment of the present invention, This will be described with reference to Fig. 1 and Fig. 15. As mentioned above, Fig. 1 is a top view of a semiconductor device. The cross-sectional structure of the portion indicated by the dashed line X1-X2 in FIG. 1(A) is shown in FIG. The cross section X1-X2 is a cross section of a transistor and a conductive film provided above the transistor. FIG. 1(B) shows a cross-sectional structure of a portion of the electrically connected region. The cross-sectional structure of the portion is shown in cross section Y1-Y2 of FIG. A region where a conductive film provided below and a conductive film provided above the semiconductor film are electrically connected The cross-sectional structure of the portion indicated by the dashed line Z1-Z2 in FIG. 1(C) is shown in FIG. The cross section Z1-Z2 of FIG. 5 shows the source and drain electrodes of the transistor. A conductive film that can function as a gate electrode and a transistor 1 is a cross-sectional structure of a portion of a region where two conductive films formed on the upper portion are electrically connected.

[0188] The method for manufacturing a semiconductor device shown in this embodiment mode is to form a plurality of conductive films on the upper part of a transistor. For example, it can be applied to the case where a common electrode and a pixel electrode are formed on the same substrate. IPS (In Plane Switching) (or FFS (fringe This is suitable for liquid crystal display devices in a field switching mode.

[0189] ≪Manufacturing method 6≫ A method for forming the connection portion 650 and the connection portion 660 shown in FIG. 15(C) will be described with reference to FIG. In the method for manufacturing a semiconductor device according to one embodiment of the present invention, a conductive film 5 The steps up to the formation of 04a are the same as those in manufacturing method 5 of embodiment 2, so the description thereof will be omitted. FIG. 15A shows a cross-sectional structure in a state where the conductive film 504a has been formed. The conductive film 504a, the opening 507a, and the opening 507c are one multi-tone mask (half-tone mask). Since the mask and the This reduces the number of photolithography steps and shortens the manufacturing time of the semiconductor device. This reduces the number of parts required and reduces manufacturing costs.

[0190] <Insulating film formation> Next, the conductive film 504a, the insulating film 502, the insulating film 500, the conductive film 114d and the conductive film 11 An insulating film is formed above 4c, and a resist mask is formed on the insulating film by a photolithography process. Next, a part of the insulating film is etched using the resist mask to form an insulating film. As shown in FIG. 15B, an opening is formed in the insulating film 610. An opening 611a is formed inside 507a, and an opening 511b is formed in the portion overlapping with the conductive film 504a. Furthermore, an opening 611c is formed inside the opening 507c.

[0191] Unlike the manufacturing method 5 of the second embodiment, the insulating film 610 has an opening 507a and an opening 507c. Therefore, the side surface of the insulating film 502 is formed in the opening 507a and the opening 507 At c, the insulating film 610 covers the insulating film 5. The impurities inside the insulating film 502 and the side surfaces of the insulating film 502 at the openings 507a and 507c are Impurities and the like that adhered during the ashing process of the multi-tone mask are directed toward the outside of the insulating film 502. For example, in the liquid crystal display device shown in the fourth embodiment described later, When the impurities are mixed into the liquid crystal, the liquid crystal deteriorates. By suppressing the diffusion of objects, deterioration of the liquid crystal display device can be suppressed.

[0192] <Conductive film formation> Next, the insulating film 610, the conductive film 504a, the insulating film 502, the insulating film 500, the conductive film 114d, and A conductive film is formed above the conductive film 114c, and a photolithography process is performed on the conductive film. Then, a resist mask is formed by etching a part of the conductive film using the resist mask. Then, a conductive film 612a and a conductive film 612b are formed (FIG. 15C).

[0193] The conductive film 612a is electrically connected to the conductive film 114d and the conductive film 504a. The conductive film 612b is electrically connected to the conductive film 114c. In addition, although not shown, the conductive film 504a can function as a pixel electrode in the device. The portion where the conductive film 612b overlaps with the capacitor can function as a capacitor. The capacitor is not limited to this, and the capacitor may include a portion other than the portion where the conductive film 504a and the conductive film 612b overlap. For example, the conductive film 504a may be formed outside the conductive film 504. may function as a capacitive element.

[0194] The conductive film 612a and the conductive film 612b are formed using the same material, structure and method as the conductive film 504a. It can be formed with.

[0195] Through the above steps, the connection parts 650 and 660 can be formed.

[0196] In addition, in the connection portion 650 and the connection portion 660, as can be understood from the cross-sectional view shown in FIG. As shown in FIG. 1, the insulating film 500, the insulating film 502, and the insulating film 610 have a tapered shape on the side surface. The insulating film 500, the insulating film 502, and the insulating film 610 may have tapered side surfaces. In this case, the conductive film 612a and the conductive film 612b are formed at the connection portion 650 and the connection portion 660. The insulating film b also has a tapered shape. When the side surfaces of the insulating film 500, the insulating film 502, and the insulating film 610 are vertical, the conductive film 612a In addition, the formation of the conductive film 612b may be insufficient, resulting in a step discontinuity. When the side surfaces of the insulating film 502 and the insulating film 610 are tapered, the conductive film 612a and In addition, it is possible to prevent the conductive film 612b from being broken, thereby improving the reliability of the semiconductor device. do.

[0197] In this manner, in the manufacturing method 6, the opening 507 is formed by using a half-tone photomask. The opening 507a and the conductive film 504a can be formed using one mask. In addition, diffusion of impurities from the side surfaces of the insulating film 502 can be suppressed.

[0198] By adopting such a process, the number of masks and photolithography processes can be reduced. This allows the manufacturing time of the semiconductor device to be shortened and the manufacturing costs to be reduced. In addition, the semiconductor device can be used without impairing its reliability.

[0199] (Embodiment 4) In this embodiment, the manufacturing method of the semiconductor device shown in the first to third embodiments is applied. A semiconductor device including a display device that can achieve the above-described object will be described below.

[0200] The manufacturing method shown in the first embodiment is for manufacturing a switching element of an active matrix type liquid crystal display device. It can be suitably used as a manufacturing method for a TN (Twisted Neutral c) mode, VA (Vertical Alignment) mode, IPS mode, etc. The present invention is applicable to liquid crystal display devices of each mode.

[0201] In addition, the manufacturing method shown in the first embodiment uses an active matrix type organic EL element. The present invention can also be suitably used as a method for manufacturing a switching element of a light emitting device.

[0202] The manufacturing methods shown in the second and third embodiments are particularly suitable for IPS mode liquid crystal displays. The method can be suitably used as a method for manufacturing a switching element for a device. The electrode is formed in a slit shape. The order of lamination of the common electrode and the common electrode may be interchanged to form the common electrode in a slit shape.

[0203] The manufacturing methods described in the first to third embodiments are not limited to display devices and light-emitting devices. Manufacturing methods for semiconductor devices such as memory devices, arithmetic units, CPUs, and microcomputers It can also be applied as

[0204] As an example of a semiconductor device, an IPS (F A liquid crystal display device 1000 in the FS mode will be described with reference to FIG.

[0205] FIG. 13A is a top view of the liquid crystal display device 1000. The cross-sectional structure of the indicated portion is shown in cross section M1-M2 of FIG. 1 is a cross-sectional view including a region in which a transistor 150 shown in the first embodiment is formed; This is a portion that can function as a pixel region of a display device. The cross-sectional structure of the portion indicated by N2 is shown in cross section N1-N2 of FIG. The LCD panel can function as a peripheral section and a connection section in which drivers and the like of a liquid crystal display device are provided. This is a possible part.

[0206] As shown in FIG. 13A, the liquid crystal display device 1000 includes a substrate 1111 and a substrate 1121. Between them, a pixel section 1201, a driver 1200 and a driver 1202 are provided.

[0207] As shown in FIGS. 13B and 13C, the liquid crystal display device 1000 has a substrate 1111 on which The liquid crystal display device 1000 includes a polarizing plate 1161, a liquid crystal layer 1115, a substrate 1121, a touch panel unit 1100, an adhesive layer 1163, a polarizing plate 1162, and The touch panel unit 1100 includes an electrode 1122, an electrode 1123, and a substrate 1131. In addition, an alignment film 1155 and an alignment film 1156 are provided above and below the liquid crystal layer. A spacer 1165 is provided to maintain the cell gap of the liquid crystal layer. In addition, a color filter 1114 is provided in a portion that does not overlap with the transistor 150. A conductive film 1113 and a conductive film 1235 are provided overlapping with the filter 1114 .

[0208] At the terminal portion, the substrate 1121 and the substrate 1111 are bonded with a sealing member 1421. The electrode 1122 and the FPC 1433 are electrically connected via the conductive films 1431 and 1432. The conductive film 1422 and the FPC 1424 are electrically connected via the conductive film 1423. are electrically connected.

[0209] FIG. 13 shows a structure having an insulating film 502 that can function as a planarizing film. However, one embodiment of the present invention is not limited thereto. This is also fine.

[0210] (Embodiment 5) In this embodiment, an example of an electronic device using a liquid crystal display device to which one embodiment of the present invention is applied will be described. This will be explained with reference to FIG.

[0211] An electronic device of this embodiment includes a liquid crystal display device according to one embodiment of the present invention in a display portion.

[0212] As an example of an electronic device to which a liquid crystal display device is applied, a television set (television or television vision receivers), computer monitors, digital cameras, digital video digital cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices) , portable game machines, personal digital assistants, audio playback devices, pachinko machines and other large game machines. Specific examples of these electronic devices are shown in Figure 14.

[0213] FIG. 14A shows an example of a television device. The television device 7100 includes: A display unit 7102 is built into a housing 7101. The display unit 7102 displays images. The liquid crystal display device to which one embodiment of the present invention is applied is used for the display portion 7102. In this embodiment, the housing 7101 is supported by a stand 7103. This shows that.

[0214] The television device 7100 can be operated using an operation switch provided on the housing 7101 or a separate remote control. This can be done by the remote control operation device 7111. This allows you to control the channel and volume, and the image displayed on the display unit 7102 In addition, the remote control operation device 7111 can be operated. A display unit for displaying information output from the

[0215] The television device 7100 includes a receiver and a modem. It is possible to receive more general television broadcasts, and furthermore, to receive them by wire or wirelessly via a modem. By connecting to a communication network, It is also possible to communicate information between followers and recipients, or between recipients themselves.

[0216] FIG. 14B shows an example of a computer. The computer 7200 includes a main body 72 01, housing 7202, display unit 7203, keyboard 7204, external connection port 7205, The computer includes a liquid crystal display (LCD) 7206 and the like. The display portion 7203 of the LCD panel is made of a liquid crystal display device.

[0217] FIG. 14C shows an example of a portable game machine. The portable game machine 7300 has a housing. It is composed of two housings, housing 7301a and housing 7301b, and the connecting part 7302 The display unit 7303a is incorporated in the housing 7301a, and the housing 7301b is connected to the display unit 7303b so as to be openable and closable. A display unit 7303b is built into the portable game console 301b. The console includes a speaker section 7304, a recording medium insertion section 7305, operation keys 7306, and a connection terminal. 7307, Sensor 7308 (force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light , liquid, magnetic, temperature, chemical, sound, time, hardness, electric field, current, voltage, power, radiation, flow (including functions to measure quantity, humidity, gradient, vibration, odor or infrared rays), LED lamp, Of course, the configuration of the portable game machine is not limited to the above. At least one of the display portion 7303a and the display portion 7303b may include a display according to the present invention. It is sufficient to use a liquid crystal display device such as the above, and other auxiliary equipment may be provided as appropriate. The portable game machine shown in FIG. 14(C) can be used to play a program recorded on a recording medium. Or it can read data and display it on the display, or communicate wirelessly with other portable game consoles. The portable game machine shown in FIG. 14(C) has the following functions: is not limited thereto and can have various functions.

[0218] FIG. 14D shows an example of a mobile phone. A mobile phone 7400 includes a housing 7401. In addition to the display unit 7402, operation buttons 7403, an external connection port 7404, The mobile phone 7400 includes a speaker 7405 and a microphone 7406. The liquid crystal display device of the above embodiment is used for the display portion 7402 .

[0219] In a mobile phone 7400 shown in FIG. 14D, information is displayed by touching a display portion 7402 with a finger or the like. You can also make calls, write emails, and perform other operations. This can be done by touching the display portion 7402 with a finger or the like.

[0220] The screen of the display unit 7402 has three main modes. The first is a display mode that is mainly used for displaying images. The first mode is a display mode, the second is an input mode for inputting information such as characters, and the third mode is a display mode. This is a display + input mode that combines the display mode and the input mode.

[0221] For example, when making a call or composing an e-mail, the display unit 7402 is used to input characters. This is the main character input mode, and the input operation of characters displayed on the screen can be performed.

[0222] In addition, the mobile phone 7400 includes a sensor for detecting tilt, such as a gyro sensor and an acceleration sensor. By providing a detection device having a sensor, the orientation of the mobile phone 7400 (portrait or landscape) can be determined. In this way, the screen display on the display portion 7402 can be automatically switched.

[0223] The screen mode can be changed by touching the display portion 7402 or by operating the housing 7401. This is done by operating the button 7403. Also, depending on the type of image displayed on the display unit 7402, For example, the image signal to be displayed on the display unit is a moving image. If it is data, the mode is switched to display mode, and if it is text data, the mode is switched to input mode.

[0224] In the input mode, the optical sensor of the display unit 7402 detects a signal and displays If there is no input by touch operation of the part 7402 for a certain period of time, the screen mode is changed to the input mode. Alternatively, the display mode may be switched from the normal mode to the display mode.

[0225] The display portion 7402 can also function as an image sensor. By touching the palm or fingers of the user on the sensor 02 and capturing an image of the palm print or fingerprint, the user can be authenticated. In addition, a backlight that emits near-infrared light to the display unit or a sensing light source that emits near-infrared light By using this, it is possible to image finger veins, palm veins, etc.

[0226] FIG. 14(E) shows an example of a foldable tablet terminal (in an open state). The tablet terminal 7500 includes a housing 7501a, a housing 7501b, a display unit 7502a, and a display The housing 7501a and the housing 7501b are connected by a shaft portion 7503. The housing 750 can be opened and closed around the shaft 7503. 1a includes a power supply 7504, operation keys 7505, a speaker 7506, etc. The tablet terminal 7500 includes a liquid crystal display device according to one embodiment of the present invention, a display unit 7502a, a display unit 7502b or both.

[0227] At least a part of the display portion 7502a or the display portion 7502b is a touch panel area. By touching the displayed operation keys, data can be input. For example, The display unit 7502a is configured to display keyboard buttons on the entire surface thereof to function as a touch panel. 02b can be used as a display screen.

[0228] This embodiment mode can be combined with other embodiment modes as appropriate. [Explanation of symbols]

[0229] 100 Substrates 102a Conductive film 102b Conductive film 104 Insulating film 106 Semiconductor Film 106a Semiconductor film 106b Semiconductor film 108 Insulating film 110 Resist mask 111a aperture 111b Aperture 111c aperture 111d aperture 114a Conductive film 114b Conductive film 114c conductive film 114d Conductive film 150 Transistors 160 Connection 210 Resist mask 210a area 210b area 211a aperture 211b aperture 211c aperture 211d aperture 212 Resist mask 307 Resist Mask 307a area 307b area 308b aperture 309 Resist Mask 311a aperture 311b aperture 311c aperture 311d aperture 312b aperture 411a aperture 411b aperture 411c aperture 411d aperture 412 Resist mask 500 Insulating film 502 Insulating film 504 Conductive film 504a Conductive film 506 Resist Mask 506a area 506b area 507a aperture 507c aperture 508 Resist Mask 510 Insulating film 511a aperture 511b aperture 511c aperture 512a Conductive film 512b Conductive film 550 Connection 560 Connection 610 Insulating film 612a Conductive film 612b Conductive film 650 Connection 660 Connection 1000 lcd display device 1100 Touch panel unit 1111 Board 1113 Conductive film 1114 Color Filter 1115 Liquid crystal layer 1121 Board 1122 Electrode 1123 Electrode 1131 Circuit Board 1155 Orientation film 1156 Orientation film 1161 Polarizing plate 1162 Polarizing plate 1163 Adhesive layer 1165 Spacer 1200 Driver 1201 Pixel section 1202 Driver 1235 Conductive film 1421 Sealing material 1422 Conductive film 1423 Conductive film 1424 FPC 1431 Conductive film 1432 Conductive film 1433 FPC 7100 Television equipment 7101 Case 7102 Display section 7103 Stand 7111 Remote control device 7200 Computer 7201 Main unit 7202 Case 7203 Display section 7204 Keyboard 7205 External connection port 7206 Pointing Device 7300 Portable Game Console 7301a Case 7301b Case 7302 Connection section 7303a Display section 7303b Display section 7304 Speaker section 7305 Recording medium insertion section 7306 Operation key 7307 Connection terminal 7308 Sensor 7400 Mobile Phone 7401 Case 7402 Display section 7403 Operation button 7404 External connection port 7405 Speaker 7406 Mike 7500 Tablet PC 7501a Housing 7501b Case 7502a Display section 7502b Display section 7503 Shaft 7504 Power supply 7505 Operation key 7506 Speaker

Claims

1. A first conductive film; a first insulating film having a region on the first conductive film; a first oxide semiconductor film having a region on the first insulating film; a second oxide semiconductor film having a region on the first insulating film; a second insulating film having a region over the first oxide semiconductor film and a region over the second oxide semiconductor film; a second conductive film having a region on the second insulating film; a third conductive film having a region on the second insulating film; a third insulating film having a region on the second conductive film and a region on the third conductive film; a fourth insulating film having a region on the third insulating film; a fourth conductive film having a region on the fourth insulating film; a fifth insulating film having a region on the fourth conductive film; the first oxide semiconductor film contains In, Ga, and Zn; the second oxide semiconductor film contains In, Ga, and Zn; the first oxide semiconductor film is provided in a first pixel, the second oxide semiconductor film is provided in a region different from the first pixel; the first pixel has an organic electroluminescence element; the second insulating film has a region in contact with an upper surface of the first oxide semiconductor film, a region in contact with a side surface of the first oxide semiconductor film, a region in contact with an upper surface of the second oxide semiconductor film, and a region in contact with a side surface of the second oxide semiconductor film; the second conductive film has a region in contact with an upper surface of the second oxide semiconductor film in a first opening provided in the second insulating film, and a region in contact with an upper surface of the first conductive film in a second opening provided in the first insulating film and the second insulating film; the third conductive film has a region in contact with an upper surface of the first oxide semiconductor film in a third opening provided in the second insulating film; the fourth conductive film has a region overlapping with the first oxide semiconductor film and a region overlapping with the second oxide semiconductor film, the fourth conductive film has a region in contact with the fourth insulating film, the fifth insulating film has a fourth opening; the fifth insulating film has a region in contact with the fourth insulating film.

2. A first conductive film; a first insulating film having a region on the first conductive film; a first oxide semiconductor film having a region on the first insulating film; a second oxide semiconductor film having a region on the first insulating film; a second insulating film having a region over the first oxide semiconductor film and a region over the second oxide semiconductor film; a second conductive film having a region on the second insulating film; a third conductive film having a region on the second insulating film; a third insulating film having a region on the second conductive film and a region on the third conductive film; a fourth insulating film having a region on the third insulating film; a fourth conductive film having a region on the fourth insulating film; a fifth insulating film having a region on the fourth conductive film; the first oxide semiconductor film contains In, Ga, and Zn; the second oxide semiconductor film contains In, Ga, and Zn; the first oxide semiconductor film is provided in a first pixel, the second oxide semiconductor film is provided in a region different from the first pixel; the first pixel has an organic electroluminescence element; the second insulating film has a region in contact with an upper surface of the first oxide semiconductor film, a region in contact with a side surface of the first oxide semiconductor film, a region in contact with an upper surface of the second oxide semiconductor film, and a region in contact with a side surface of the second oxide semiconductor film; the second conductive film has a region in contact with an upper surface of the second oxide semiconductor film in a first opening provided in the second insulating film, and a region in contact with an upper surface of the first conductive film in a second opening provided in the first insulating film and the second insulating film; the third conductive film has a region in contact with an upper surface of the first oxide semiconductor film in a third opening provided in the second insulating film; the fourth conductive film has a region overlapping with the first oxide semiconductor film and a region overlapping with the second oxide semiconductor film, the fourth conductive film has a region in contact with the fourth insulating film, the fifth insulating film has a fourth opening; the fifth insulating film has a region in contact with the fourth insulating film, The fourth conductive film includes a light-transmitting material.

3. A first conductive film; a first insulating film having a region on the first conductive film; a first oxide semiconductor film having a region on the first insulating film; a second oxide semiconductor film having a region on the first insulating film; a second insulating film having a region over the first oxide semiconductor film and a region over the second oxide semiconductor film; a second conductive film having a region on the second insulating film; a third conductive film having a region on the second insulating film; a third insulating film having a region on the second conductive film and a region on the third conductive film; a fourth insulating film having a region on the third insulating film; a fourth conductive film having a region on the fourth insulating film; a fifth insulating film having a region on the fourth conductive film; the first oxide semiconductor film contains In, the second oxide semiconductor film contains In, the first oxide semiconductor film is provided in a first pixel, the second oxide semiconductor film is provided in a region different from the first pixel; the first pixel has an organic electroluminescence element; the second insulating film has a region in contact with an upper surface of the first oxide semiconductor film, a region in contact with a side surface of the first oxide semiconductor film, a region in contact with an upper surface of the second oxide semiconductor film, and a region in contact with a side surface of the second oxide semiconductor film; the second conductive film has a region in contact with an upper surface of the second oxide semiconductor film in a first opening provided in the second insulating film, and a region in contact with an upper surface of the first conductive film in a second opening provided in the first insulating film and the second insulating film; the third conductive film has a region in contact with an upper surface of the first oxide semiconductor film in a third opening provided in the second insulating film; the fourth conductive film has a region overlapping with the first oxide semiconductor film and a region overlapping with the second oxide semiconductor film, the fourth conductive film has a region in contact with the fourth insulating film, the fifth insulating film has a fourth opening; the fifth insulating film has a region in contact with the fourth insulating film.

4. A first conductive film; a first insulating film having a region on the first conductive film; a first oxide semiconductor film having a region on the first insulating film; a second oxide semiconductor film having a region on the first insulating film; a second insulating film having a region over the first oxide semiconductor film and a region over the second oxide semiconductor film; a second conductive film having a region on the second insulating film; a third conductive film having a region on the second insulating film; a third insulating film having a region on the second conductive film and a region on the third conductive film; a fourth insulating film having a region on the third insulating film; a fourth conductive film having a region on the fourth insulating film; a fifth insulating film having a region on the fourth conductive film; the first oxide semiconductor film contains In, the second oxide semiconductor film contains In, the first oxide semiconductor film is provided in a first pixel, the second oxide semiconductor film is provided in a region different from the first pixel; the first pixel has an organic electroluminescence element; the second insulating film has a region in contact with an upper surface of the first oxide semiconductor film, a region in contact with a side surface of the first oxide semiconductor film, a region in contact with an upper surface of the second oxide semiconductor film, and a region in contact with a side surface of the second oxide semiconductor film; the second conductive film has a region in contact with an upper surface of the second oxide semiconductor film in a first opening provided in the second insulating film, and a region in contact with an upper surface of the first conductive film in a second opening provided in the first insulating film and the second insulating film; the third conductive film has a region in contact with an upper surface of the first oxide semiconductor film in a third opening provided in the second insulating film; the fourth conductive film has a region overlapping with the first oxide semiconductor film and a region overlapping with the second oxide semiconductor film, the fourth conductive film has a region in contact with the fourth insulating film, the fifth insulating film has a fourth opening; the fifth insulating film has a region in contact with the fourth insulating film, The fourth conductive film includes a light-transmitting material.

Citation Information

Patent Citations

  • Image display device and manufacturing method thereof

    JP2008129314A

  • Semiconductor device and manufacturing method thereof

    JP2010056540A

  • Semiconductor device and method for manufacturing the same

    JP2011049548A

  • Light-emitting device and manufacturing method thereof

    JP2011085923A

  • Information processing device, information processing method, and information processing program

    JP2023068981A