Ceramic ball material and ceramic ball production method using the same as well as ceramic ball

The ceramic ball material with a band-like part and specific Rtb/Rts ratio addresses the chipping issue during polishing, enabling efficient and damage-free polishing by preferentially engaging the band-shaped portion, thus improving polishing speed and surface plate durability.

JP2024133684AActive Publication Date: 2024-10-02NITERRA MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024111261
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2024-07-10
Publication Date
2024-10-02
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Ceramic ball materials with a spherical and band-shaped part are prone to chipping during polishing due to their brittleness and require long polishing times, especially at corners or shoulders, which are more susceptible to impact.

Method used

The ceramic ball material is designed with a band-like part around the circumference of the spherical part, where the ratio of the maximum cross-sectional height of the band-shaped portion to the spherical portion (Rtb/Rts) is 1.0 or more, facilitating preferential polishing and reducing the density of the band-shaped portion, thus minimizing chipping and shortening polishing time.

Benefits of technology

This design allows for efficient polishing with reduced material damage and improved polishing speed by preferentially engaging the band-shaped portion, enhancing polishing efficiency and durability of the polishing surface plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133684000001_ABST
    Figure 2024133684000001_ABST
Patent Text Reader

Abstract

To provide ceramic ball production method capable of suppressing damage on ceramic material upon a polishing process to reduce polishing time.SOLUTION: Ceramic ball material in accordance with an embodiment is provided with a spherical surface part and a belt-like part formed along a circumference of a surface of the spherical surface part. A ratio of Rtb / Rts of a max sectional height Rtb on a roughness curve of an outer peripheral surface of the belt-like part and a max sectional height Rts on a roughness curve of an outer peripheral surface of the spherical surface part is 1.0 or more. Preferably, any diameter of the spherical surface part is 0.5 mm or more. And, the ceramic ball material, preferably, includes any one of alumina, silicon nitride, silicon carbide, boron nitride, and zirconia.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiments described below relate to a material for a ceramic ball, a method for manufacturing a ceramic ball, and a ceramic ball. [Background technology]

[0002] Various ceramic materials have properties such as high hardness, insulation, and wear resistance, and fine ceramics, which have particularly high purity and uniform particle size, exhibit properties that are used in various fields such as capacitors, actuator materials, and fireproof materials. Among the properties of ceramic materials, products for ball applications take advantage of wear resistance and insulation. Products for ball applications include bearings, jigs, tools, gauges, solenoid valves, check valves, and various valves. Among these, ceramic materials such as aluminum oxide, silicon nitride, and zirconium oxide are used for products for bearing ball applications. For example, bearing balls using silicon nitride materials are disclosed in JP-A-6-48813 (Patent Document 1) and JP-A-2764589 (Patent Document 2), and bearing balls using zirconium oxide materials are disclosed in JP-A-60-18620 (Patent Document 3).

[0003] In the process of manufacturing these materials for bearing balls, a method of sintering a molded body is used. In addition, press molding using a die is used as a molding method to obtain the molded body. Press molding is generally a method in which an upper punch 2, a lower punch 3, and a die 4 are provided, and powder is inserted between the upper punch 2 and the lower punch 3 and pressure is applied, as shown in FIG. 1. In order to protect the die during press molding, a gap must be provided between the tip 2a of the upper punch 2 and the tip 3a of the lower punch 3 when press molding. For this reason, a spherical portion and a band-shaped portion are formed in the molded body obtained by press molding. For example, Japanese Patent No. 4761613 (Patent Document 4) discloses a material for bearing balls having a spherical portion and a band-shaped portion, which is obtained by sintering a molded body having a spherical portion and a band-shaped portion. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-48813 [Patent Document 2] Patent No. 2764589 [Patent Document 3] Japanese Patent Application Publication No. 18620 / 1983 [Patent Document 4] Patent No. 4761613 Summary of the Invention [Problem to be solved by the invention]

[0005] After the sintering process, ceramic ball materials with a spherical surface and a strip-shaped surface are polished to produce ceramic balls. Ceramic ball materials with a spherical surface and a strip-shaped surface are sometimes called bare balls. For example, ceramic ball materials are polished to a mirror finish with a surface roughness Ra of 0.1 μm or less. A surface plate is used for the mirror finish.

[0006] Generally, ceramic materials have excellent wear resistance, but because they are brittle materials, they are prone to chipping when subjected to strong impact. Curved surfaces are good at dissipating impact, but corners are prone to chipping due to impact. For this reason, when performing surface processing on ceramic ball materials with band-shaped parts, the two shoulders, which are the corners of the band-shaped parts, are selectively brought into contact with the surface, and processing is performed to suppress the possibility of chipping, which causes the polishing time to be long.

[0007] The present invention is intended to solve these problems, and provides a material for ceramic balls that can suppress damage to the ceramic material during polishing and shorten the polishing time. [Means for solving the problem]

[0008] A ceramic ball material according to an embodiment includes a spherical portion and a band-shaped portion formed around the circumference of the spherical portion, and a ratio Rtb / Rts of a maximum profile height Rtb of a roughness curve of an outer peripheral surface of the band-shaped portion to a maximum profile height Rts of a roughness curve of an outer peripheral surface of the spherical portion is 1.0 or more. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a general die press molding apparatus. [Diagram 2] FIG. 2 is an external view showing an example of a ceramic ball material according to the embodiment. [Diagram 3] FIG. 2 is an external view showing an example of a die of the die press molding apparatus according to the embodiment. [Figure 4] FIG. 2 is a cross-sectional view showing an example of cold isostatic press rubber molding according to the embodiment. [Diagram 5] FIG. 2 is a cross-sectional view showing an example of a hole shape and a molded body provided in a cold isostatic press rubber mold according to an embodiment. [Figure 6] FIG. 2 is a cross-sectional view showing an example of a hole shape and a molded body provided in a cold isostatic press rubber mold according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of a ceramic ball material, a method for producing a ceramic ball using the same, and a ceramic ball will be described in detail with reference to the drawings.

[0011] A ceramic ball material according to an embodiment includes a spherical portion and a band-shaped portion formed around the circumference of the spherical portion, and a ratio Rtb / Rts of a maximum profile height Rtb of a roughness curve of an outer peripheral surface of the band-shaped portion to a maximum profile height Rts of a roughness curve of an outer peripheral surface of the spherical portion is 1.0 or more.

[0012] FIG. 2 shows a schematic diagram of a ceramic ball material according to an embodiment. In FIG. 2, 5 is a ceramic ball material according to an embodiment, 6 is a spherical portion, and 7 is a band-shaped portion. In addition, of the maximum cross-sectional height of the roughness curve Rt, the maximum cross-sectional height of the roughness curve relating to the outer peripheral surface (outermost surface) of the band-shaped portion 7 is Rtb, and the maximum cross-sectional height of the roughness curve relating to the outer peripheral surface (outermost surface) of the spherical portion 6 is Rts. In addition, W is the width of the band-shaped portion 7. The width W of the band-shaped portion 7 is sometimes simply referred to as "width W". In addition, in FIG. 3, the height and width of the band-shaped portion 7 relative to the spherical portion 6 are illustrated for convenience of explanation.

[0013] The ceramic ball material 5 has a spherical portion 6 and a band-shaped portion 7. The band-shaped portion 7 is formed around the circumference of the surface of the spherical portion 6. The circumference of the surface of the spherical portion 6 may be any one of a plurality of circumferences of the surface of the spherical portion 6. The surface of the spherical portion 6 may be a quadratic curved surface. Therefore, examples of the spherical portion 6 include a perfect sphere and an ellipsoid. The band-shaped portion 7 is provided on the circumference of the spherical portion 6. The width W of the band-shaped portion 7 is, for example, the widest width of the band-shaped portion 7, but may be the average value of a plurality of points.

[0014] When the maximum cross-sectional height of the roughness curve of the spherical portion 6 is Rts and the maximum cross-sectional height of the roughness curve of the band-shaped portion 7 is Rtb, the ratio of Rtb to Rts, Rtb / Rts, is in the range of 1.0 or more. When Rts / Rtb is within this range, the band-shaped portion 7 is preferentially in contact with the abrasive due to the roughness of the surface, and the polishing process (for example, platen processing) proceeds. In addition, since the density of the band-shaped portion 7 of the sintered body is smaller than that of the spherical portion 6, the polishing process of the band-shaped portion 7 becomes easier and the polishing time during the polishing process can be shortened. For this reason, Rtb / Rts is preferably 1.0 or more, more preferably 1.1 or more, and even more preferably 1.2 or more.

[0015] In addition, it is preferable that Rtb / Rts is in the range of 3.0 or less. If Rtb / Rts exceeds 3.0, even if the maximum cross-sectional height Rts of the roughness curve of the spherical portion 6 can be controlled, the maximum cross-sectional height Rtb of the roughness curve of the band-shaped portion 7 becomes large. This is because there is a possibility that the strength of the ceramic ball material 5 having the band-shaped portion 7 is reduced, resulting in chipping defects, or that the protrusions of the band-shaped portion 7 of the ceramic ball material 5 may damage the polishing table.

[0016] If Rtb / Rts is less than 1.0, the density of the band-shaped portion 7 of the material 5 for ceramic balls becomes larger than that of the spherical portion 6, making it difficult to polish the band-shaped portion 7 and lengthening the polishing time during polishing of the material 5 for ceramic balls. Furthermore, brittle fracture is likely to occur when the band-shaped portion comes into contact with a grindstone during polishing of the material 5 for ceramic balls. In particular, brittle fracture is likely to occur when the material 5 for ceramic balls comes into contact with a platen during platen processing.

[0017] Here, a method for measuring the maximum cross-sectional height Rtb of the roughness curve of the band-like portion 7 of the material 5 for ceramic balls and the maximum cross-sectional height Rts of the roughness curve of the spherical portion 6 will be described. Note that the maximum cross-sectional height Rt of the roughness curve is based on JIS B 0601 (2013) "Geometric characteristic specifications for products (GPS)-Surface quality: Profile curve method-Terminology, definitions and surface quality parameters."

[0018] The maximum cross-sectional height Rt of the roughness curve is measured using a surface roughness measuring instrument. The surface roughness measuring instrument is Tokyo Seimitsu's SURFCOM2000, and the measurement is performed using the evaluation and analysis software of the same instrument. Any measuring instrument with equivalent functions will do.

[0019] The measurement distance of the maximum cross-sectional height Rt of the roughness curve, i.e., the evaluation length U, is 10 to 25% of the diameter of the ceramic ball material 5, and the evaluation lengths U of the spherical portion 6 and the band-like portion 7 are the same. The measurement conditions are as follows: the measurement cutoff wavelength is 0.08 mm, the cutoff type is Gaussian, the slope correction is least squares linear correction, and the λs cutoff ratio is 300. The measurement is performed three times, and the measured value is the average value of the three measurements.

[0020] The measurement area of ​​the maximum profile height Rtb of the roughness curve relating to the outer peripheral surface of the band-like portion 7 has a length corresponding to the evaluation length U at any position on the curve 7C. On the other hand, the measurement area of ​​the maximum profile height Rts of the roughness curve relating to the outer peripheral surface of the spherical portion 6 has a length corresponding to the evaluation length U at a position on the curve 6C that is the furthest from the curve 7C (center position, position at 90° from the curve 7C) 6D as the center. This is because, even if the material 5 for ceramic balls is a perfect sphere or an ellipsoid, similar values ​​can be obtained regardless of the position or direction from which the measurement is performed. If the measurement cannot be performed at the center position 6D (or the center position 6D') of the spherical portion 6 due to the presence of defects or the like, it is also possible to perform the measurement on the outer surface of the spherical crown from a position (45° position) 6E that is half the distance from the curve 7C to the center position 6D to the center position 6D.

[0021] A cross-sectional curve is obtained in a cross section formed by a curve 7C extending in the circumferential direction of the outer peripheral surface formed by the band-shaped portion 7 and passing through the center of the outer peripheral surface, and a straight line in the depth direction of the band-shaped portion 7. The long wavelength shape (waviness curve) is removed from the cross-sectional curve, and the sum of the maximum peak height and the maximum valley depth of the profile curve in the evaluation length U is obtained, thereby obtaining a maximum cross-sectional height Rtb of the roughness curve related to the outer peripheral surface of the band-shaped portion 7. The cross-sectional curve is obtained in a cross section formed by a curve 6C passing through the center positions 6D, 6D' on the outer peripheral surface of the spherical portion 6, and a straight line in the depth direction of the spherical portion 6. The long wavelength shape (waviness curve) is removed from the cross-sectional curve, and the sum of the maximum peak height and the maximum valley depth of the profile curve in the evaluation length U is obtained, thereby obtaining a maximum cross-sectional height Rts of the roughness curve related to the outer peripheral surface of the spherical portion 6. It is preferable to exclude from the measurement 10% of one end and 10% of the other end in the width direction of the outer circumferential surface of the band-shaped portion 7 from the measurement points because defects such as chipping are likely to occur there and affect the measured values. Also, the evaluation length U of the maximum cross-sectional height Rt of the roughness curve does not need to be the entire curves 6C, 7C on the outer circumferential surface, and may be a part of the curves 6C, 7C (for example, about 1 mm to 20 mm).

[0022] In the ceramic ball material 5, the spherical portion 6 has a diameter of preferably 0.5 mm or more. If the diameter of the spherical portion 6 is less than 0.5 mm, it becomes difficult to control the powder press die for forming the strip portion 7. For this reason, the diameter of the spherical portion 6 is preferably 1 mm or more. More preferably, it is 2 mm or more.

[0023] The ceramic ball material 5 preferably contains 85 mass% or more of any one of aluminum oxide (Al2O3), silicon nitride (Si3N4), silicon carbide (SiC), boron nitride (BN), and zirconium oxide (ZrO2). The ceramic ball material 5 is made of a ceramic sintered body. The content of 85 mass% or more of any one of aluminum oxide, silicon nitride, silicon carbide, boron nitride, and zirconium oxide refers to the content in the ceramic sintered body, and by containing 85 mass% or more, the physical properties of ceramics can be satisfied and the physical properties required for a ceramic ball can be exhibited. In other words, the ceramic sintered body may contain 15 mass% or less of substances other than the above. It is preferable that the ceramic ball material 5 contains 85 mass% or more of silicon nitride.

[0024] For example, aluminum oxide sintered body, silicon nitride sintered body, silicon carbide sintered body, boron nitride sintered body, zirconium oxide sintered body, and aridil sintered body are used as bearing balls. Incidentally, aridil sintered body is a sintered body made by mixing aluminum oxide and zirconium oxide. Among these, bearing balls made of silicon nitride sintered body have the best wear resistance. For example, aluminum oxide, zirconium oxide, and aridil have a Vickers hardness of about 1200 to 1700, but a fracture toughness value of 3 to 6 MPa m 1 / 2 In contrast, silicon nitride sintered body has a Vickers hardness of 1400 to 1800 and a fracture toughness of 5 to 10 MPa m 1 / 2and high. Silicon nitride sintered bodies have both high toughness and Vickers hardness, which gives them excellent wear resistance. Silicon nitride sintered bodies have a structure mainly composed of β-type silicon nitride crystal grains. β-type silicon nitride crystal grains have a long and thin shape, and the long and thin crystal grains are intricately intertwined to achieve high toughness. Silicon nitride sintered bodies have a very poor polishing efficiency due to their high mechanical strength. However, as described above, by increasing the maximum cross-sectional height of the roughness curve of the band-shaped portion 7, it is possible to improve the polishing efficiency even for ceramic ball material 5 made of a ceramic sintered body with high strength, such as silicon nitride sintered bodies.

[0025] Next, a method for manufacturing the ceramic ball material 5 will be described. As long as the ceramic ball material 5 according to the embodiment satisfies the above-mentioned configuration, the manufacturing method is not particularly limited, but the following manufacturing method can be mentioned as a method for efficiently manufacturing the ceramic ball material 5. The manufacturing method for the ceramic ball material 5 will be described using a silicon nitride sintered body as an example.

[0026] First, appropriate amounts of sintering aid, additives, solvent, binder, etc. are added to silicon nitride as a raw material, mixed, crushed, and granulated using a spray dryer. This process prepares granulated powder of the raw powder. When the total of the silicon nitride powder and the sintering aid powder is 100 mass%, it is preferable that the silicon nitride powder is 85 mass% or more. The additive is a plasticizer. The solvent is water or an organic solvent. Examples of organic solvents include alcohol, ketone, and benzene. The binder is an organic substance. The amount of binder added is within the range of 3 to 20 mass parts when the total of the silicon nitride powder and the sintering aid powder is 100 mass parts.

[0027] Next, the average particle size of the obtained granulated powder is reduced. If the average particle size of the granulated powder is large, spaces are formed between the granulated powder when the granulated powder is filled into the press die, so the granulated powder is easily crushed. Conversely, if the average particle size is reduced, the spaces between the granulated powder are reduced, so the granulated powder is less likely to be crushed. Therefore, by reducing the average particle size of the granulated powder, it becomes less likely to be crushed in the center of the press where the pressure from the punch is smaller. However, if the average particle size of the granulated powder is simply reduced, the flowability of the granulated powder into the press die is reduced, which may affect productivity. For this reason, it is necessary to reduce the average particle size without impairing the flowability of the granulated powder.

[0028] The granulated powder usually obtained by a spray dryer is generally normally distributed and shows a distribution that accumulates near the average value. Therefore, by mixing two types of granulated powder with different particle sizes by classification, it is possible to obtain granulated powder with a smaller average particle size while reducing the decrease in flowability. For example, the average particle size of granulated powder used in mold press molding is 50 to 150 μm, but if the granulated powder has an average particle size of 120 μm, it is possible to reduce the average particle size by classification. The granulated powder is divided and classified using a 60 mesh (opening size: about 250 μm) sieve to obtain granulated powder smaller than 60 mesh. In addition, the remaining granulated powder is classified using a 100 mesh (opening size: about 150 μm) to obtain granulated powder smaller than 100 mesh. By mixing granulated powder smaller than 60 mesh and granulated powder classified smaller than 100 mesh in a certain ratio, it is possible to change the average particle size of the granulated powder from 120 μm to 90 μm. This makes it easier to increase the maximum cross-sectional height Rtb of the roughness curve of the belt-like portion 7 in the process described below.

[0029] Next, the adjusted granulated powder is used for press molding. The press molding may be performed using an upper punch 2, a lower punch 3, and a die 4 of a die press molding apparatus shown in FIG. 1. By filling the granulated powder and applying pressure vertically to the upper punch 2 and the lower punch 3, the spherical shape inside the punch becomes the spherical portion 6 of the ceramic ball material 5. In addition, the planar shape of the upper punch tip 2a, the lower punch tip 3a, and the inner side of the die 4 becomes the band-shaped portion 7 of the ceramic ball material 5. The inside of the cross section of the die 4 is a straight line, but it is preferable to make it slightly concave as shown in FIG. 3. If the depth of the concave portion is H, the size of H is preferably 0.01 mm or more and 0.10 mm or less. This concave portion prevents pressure from being applied to the band-shaped portion 7 of the molded body 13, and the sintering density of the band-shaped portion 7 of the ceramic ball material 5 after the sintering process can be reduced, and the maximum cross-sectional height Rtb of the roughness curve of the band-shaped portion becomes large. If the depth of H is less than 0.01 mm, the effect of preventing pressure is small. On the other hand, if it is deeper than 0.10 mm, the effect of preventing pressure is large, but the load on the die increases, which may shorten the life of the die.

[0030] By adjusting the shape of the tip 2a of the upper punch 2 and the tip 3a of the lower punch 3 and the amount of powder filled during press molding, it is possible to adjust the width W and height of the band-shaped portion 7 of the ceramic ball material 5 after the sintering process. Similarly, it is possible to adjust the diameter of the compact 13 in the direction of the spherical portion 14 and the diameter in the direction of the band-shaped portion 15. The compact 13 obtained by press molding has a spherical portion 14 and a band-shaped portion 15. The spherical portion 14 and the band-shaped portion 15 of the compact 13 (shown in Figs. 5 and 6) respectively correspond to the spherical portion 6 and the band-shaped portion 7 (shown in Fig. 2) of the above-mentioned ceramic ball material 5.

[0031] It is also preferable to perform isostatic pressing on the compact after press molding. By performing isostatic pressing, the granulated powder in the compact can be uniformly compressed. This makes it possible to reduce the amount of granulated powder that remains in the compact. By reducing the amount of granulated powder that remains in the compact, it is possible to control the shrinkage rate in the sintering process.

[0032] As an example of isotropic pressure molding, an isotropic pressure molding method using a rubber mold will be described. Figure 4 shows an example of a disk-shaped rubber mold 8. In Figure 4, 9 is an upper rubber mold, 10 is a lower rubber mold, 11 is a spherical space, 12 is a band-shaped space, 13 is a molded body, 14 is a spherical portion of the molded body, and 15 is a band-shaped portion of the molded body. Figure 5 is a cross-sectional view showing an example in which a molded body 13 is disposed in the spherical space 11 in the upper rubber mold 9 and the lower rubber mold 10.

[0033] The upper rubber mold 9 and the lower rubber mold 10 have hemispherical holes on both sides, each hole being 1% to 35% larger than the maximum diameter of the molded body 13. The molded body 13 is placed in the hole and the rubber mold is placed on top of it, sealing the molded body 13 in the spherical space 11 surrounded by the rubber mold. A hydrostatic pressure higher than the pressure during molding is applied to the rubber mold. In addition, it is preferable to use a rubber mold having a Shore hardness Hs of 30 to 50. By setting the hardness of the rubber mold within this range, it is possible to provide the molded body 13 with a deformability that allows the surface of the molded body 13 to be in uniform contact with the rubber mold. This allows the molded body 13 to be uniformly compressed. This process reduces the amount of crushed granulated powder remaining.

[0034] Further, as shown in Fig. 6, it is preferable to perform isostatic pressing by installing the strip portion 15 of the molded body 13 in the strip portion space 12 between the upper rubber mold 9 and the lower rubber mold 10 provided with the strip portion space 12. Let the distance between the upper rubber mold 9 and the molded body 13 in the spherical surface portion space 11 be L1, and the distance between the upper rubber mold 9 or the lower rubber mold 10 and the molded body 13 in the strip portion space 12 be L2. At this time, L1 is the sum (L11 + L12) of the distance L11 between the molded body 13 and the upper rubber mold 9 and the distance L12 between the lower rubber mold 10. Also, L2 is the sum (L21 + L22) of the distance L21 and the distance L22 between the molded body 13 and the side surface of the strip portion space 12 of the lower rubber mold 10. At this time, if L1 < L2, it is possible to prevent pressure from being applied to the strip portion 15 of the molded body 13, reduce the sintering density of the strip portion 15, and increase the maximum cross-sectional height Rtb of the roughness curve of the ceramic ball material 5 after the sintering process. Note that the strip portion space 12 may be formed in only one of the upper rubber mold 9 and the lower rubber mold 10 as long as the strip portion 15 can be accommodated.

[0035] Also, conventionally, the distance between the molded body 13 and the rubber mold was L1 ≥ L2. This is because the design of the spherical surface portion space 11 formed by overlapping the upper rubber mold 9 and the lower rubber mold 10 is a true spherical shape (L1 = L2). Furthermore, this was because powder or the like tended to adhere to the gap between the upper and lower rubber molds during use, causing L1 > L2. If the shape is provided with the strip portion space 12 as shown in Fig. 6, L1 < L2, and the load on the strip portion 15 with respect to the spherical surface portion 14 of the molded body 13 is relaxed. Therefore, the maximum cross-sectional height Rtb of the roughness curve of the strip portion 7 of the ceramic ball material 5 after the sintering process becomes larger than the maximum cross-sectional height Rts of the roughness curve of the spherical surface portion 6, and Rtb / Rts becomes 1.0 or more.

[0036] Next, a debinding process for debinding the molded body 13 is performed. The debinding process is a process of heating at a temperature equal to or higher than the decomposition temperature of organic components such as a binder and removing the organic components. The debinding process may be performed in a nitrogen atmosphere or an air atmosphere. A debound body can be obtained by the debinding process.

[0037] Next, a sintering process is performed to sinter the degreased body. The sintering process is preferably performed at a temperature of 1600°C or higher and 2000°C or lower. The sintering process is preferably performed in a nitrogen atmosphere. The sintering pressure is preferably in the range of atmospheric pressure or higher and 300 MPa or lower. The atmospheric pressure is 0.10133 MPa (=1 atm). The sintered body obtained by the sintering process may be subjected to a HIP (hot isostatic press) process. A ceramic ball material 5 can be obtained by this process. The ceramic ball material 5 is a ceramic sintered body having a theoretical density of 98% or higher.

[0038] Ceramic balls can be manufactured by polishing the ceramic ball material 5. A typical example of polishing a ball is plate processing. For example, the ceramic ball material 5 is inserted between two platens arranged in parallel above and below. The movement of the polishing platen can be used to plate-process the ceramic ball material 5 into a perfect sphere. The surface roughness of the bearing ball is specified in ASTM F2094. Depending on the application, a grade conforming to ASTM F2094 is adopted for the bearing ball. The bearing ball is polished to a surface roughness Ra conforming to that grade. For higher grades, some are mirror-finished to a surface roughness Ra of 0.01 μm or less. Note that ASTM is a standard issued by ASTM International. ASTM International was formerly known as the American Society for Testing and Materials (ASTM).

[0039] In the material 5 for ceramic balls according to the embodiment, the maximum cross-sectional height Rtb of the roughness curve of the belt-shaped portion 7 is larger than that of the spherical portion 6, so that polishing starts preferentially. In addition, the sintering density of the belt-shaped portion 7 is smaller than that of the spherical portion 6, so that the platen processing proceeds preferentially. Therefore, the platen processing can be performed without being aware of the contact of the belt-shaped portion 7 with a grindstone such as a polishing platen. This makes it possible to suppress damage to the material 5 for ceramic balls during the polishing process. In addition, the durability of the polishing platen can be improved. In addition, even when the polishing speed is increased to shorten the polishing time, the polishing processability (polishing process efficiency) can be improved while maintaining the damage suppression effect.

[0040] (Examples 1 to 9, Comparative Examples 1 to 6) Sintering aids, additives, solvents, binders, etc. were added to the ceramic powder as raw material, mixed, crushed, and granulated by a spray dryer. The ceramics of Examples 1 to 7 and Comparative Examples 1 to 4 were silicon nitride sintered bodies. The ceramics of Example 8 and Comparative Example 5 were aluminum oxide sintered bodies. The ceramics of Example 9 and Comparative Example 6 were silicon carbide sintered bodies. The silicon nitride sintered bodies contained 85 mass% or more of silicon nitride. The aluminum oxide sintered bodies contained 85 mass% or more of aluminum oxide. The silicon carbide sintered bodies contained 85 mass% or more of silicon carbide. When the total of the main component and sintering aid was 100 mass parts, the amount of binder added was within the range of 3 to 20 mass parts.

[0041] Next, the granulated powder was divided into two and classified using a 60 mesh sieve. The remaining divided granulated powder was classified using a 100 mesh sieve. The granulated powder classified using the 60 mesh sieve and the granulated powder classified using the 60 mesh and 100 mesh sieves were mixed to obtain a granulated powder.

[0042] Next, press molding was performed using the obtained granulated powder. The press molding was die molding using the upper and lower dies of the die press molding apparatus shown in FIG. 1. For the press dies, dies with the same clearance were used for the same ceramic ball diameter, and straight dies without a recess in the center of the die 4 and dies with a recess were used. After die molding, isostatic pressing was performed. The isostatic pressing used a disk-shaped rubber mold with a Shore hardness Hs of 30 or more and 50 or less. Further, for the rubber mold 8, a spherical rubber mold (L1 = L2) was prepared in which the distance L1 between the upper rubber mold 9 and the ceramic ball material 5 in the spherical surface portion space 11 and the distance L2 between the upper rubber mold 9 or the lower rubber mold 10 and the molded body 13 in the belt-shaped portion space 12 were made equal. Also, a rubber mold (L1 < L2) provided with a belt-shaped portion space 12 was prepared. At this time, L1 / L2, which is the ratio of the distance L1 and the distance L2 of the rubber mold provided with the belt-shaped portion space 12, was set to 1.05. Further, in addition to the press molding, the belt-shaped portion 15 of the molded body 13 was arranged perpendicular to the circumferential direction of the rubber mold. Also, in the rubber mold having the belt-shaped portion space 12, the belt-shaped portion 15 was arranged in the belt-shaped portion space. In this state, in the isostatic pressing process, a hydrostatic pressure higher than the pressure during molding was applied.

[0043] Next, after the debinding process, a sintering process was performed. The sintering process was carried out at 1600 to 2000 °C in a nitrogen atmosphere at atmospheric pressure. Thereafter, HIP treatment was performed at 1600 to 2000 °C in a nitrogen atmosphere at a pressure of 200 MPa.

[0044] Through this process, the ceramic ball material 5 according to the example was produced. In the comparative example, 100-mesh granulated powder was not mixed (mixing ratio 0%), and only 60-mesh mixed powder was used. Also, in the comparative example, the die 4 was not provided with the recess shown in FIG. 3. Further, in the comparative example, the rubber mold having the belt-shaped portion space 12 was not used. The manufacturing conditions of the examples and comparative examples are shown in Table 1.

[0045]

Table 1

[0046] Examples 1 to 4, 8 to 9 and Comparative Examples 1, 5, and 6 are ceramic ball materials 5 for ceramic balls that will be 3 / 8 inch (9.525 mm) after polishing. Example 5 and Comparative Example 2 are ceramic ball materials 5 for 7 / 8 inch (22.225 mm) ceramic balls. Example 6 and Comparative Example 3 are ceramic ball materials 5 for 1-3 / 16 inch (30.165 mm) ceramic balls. Example 7 and Comparative Example 4 are ceramic ball materials for 1-7 / 8 inch (47.625 mm) ceramic balls. All of the ceramic ball materials 5 of Examples 1 to 9 and the ceramic ball materials of Comparative Examples 1 to 6 can be used as bearing balls.

[0047] The maximum cross-sectional height Rt of the roughness curve of the material for ceramic ball 5 according to the embodiment and the maximum cross-sectional height Rt of the roughness curve of the material for ceramic ball according to the comparative example were each measured at the evaluation length U. The respective measurement methods were as described above. As described above, the maximum cross-sectional height Rt of the roughness curve is the sum of the maximum peak height and the maximum valley depth of the profile curve at the evaluation length U. In addition, Rtb / Rts was calculated for the material for ceramic ball 5 according to the embodiment and the material for ceramic ball according to the comparative example. The maximum cross-sectional heights Rtb, Rts of the roughness curve, the ratio Rtb / Rts, and the evaluation length U in the embodiment and the comparative example are as shown in Table 2.

[0048] In Comparative Examples 1 to 6, the ratio Rtb / Rts of the maximum profile height Rtb of the roughness curve of the band-like portion of the ceramic ball material to the maximum profile height Rts of the roughness curve of the spherical portion is less than 1.0, which is outside the range.

[0049] Using the ceramic ball material 5 of the embodiment and the ceramic ball material of the comparative example, the polishing accuracy (for example, the rate of acceptable stripping) and the damage suppression effect (for example, the rate of defective material chipping) were evaluated. The evaluation was performed by fixing the polishing conditions for polishing each ceramic ball material using a ball processing polisher and examining the processed state of the strip portion. The polishing conditions were that the upper surface plate was unpressurized (no pressure), the lower surface plate was rotated, and an abrasive using glycerin as a lubricant was supplied to diamond for 24 hours. Note that the same size ceramic balls were under the same conditions for the gap distance with the upper surface plate, the rotation speed of the lower surface rotation, the amount of ceramic ball material input, and the amount of abrasive supplied. After polishing, 100 pieces were sampled and the appearance of the strip portion was visually inspected, and those in which the strip shape could not be confirmed were regarded as acceptable products and shown as the rate of acceptable stripping (%).

[0050] In addition, after the above-mentioned polishing process, the rate of occurrence of defects in the state where the ceramic ball material 5 of the embodiment and the ceramic ball material of the comparative example were chipped was investigated. The rate of occurrence of defects was determined by visually inspecting the entire surface of the 100 pieces sampled above with an optical microscope, and the rate of occurrence of chipping was shown as the material chipping defect rate (%). The results are shown in Table 2.

[0051] [Table 2]

[0052] In the materials for ceramic balls according to Comparative Examples 1 to 6, the stripping process yield rate and the material chipping defect rate are improved to some extent at a relatively low polishing speed, but at a relatively high polishing speed, as shown in Table 2, the stripping process yield rate and the material chipping defect rate are not favorable. On the other hand, as can be seen from Table 2, in the materials for ceramic balls 5 according to Examples 1 to 9, the stripping process yield rate and the material chipping defect rate are improved compared to the materials for ceramic balls according to Comparative Examples 1 to 6, even at a relatively high polishing speed, and the polishing accuracy and damage suppression effect are improved. In other words, in the materials for ceramic balls 5 according to Examples 1 to 9, it can be said that the polishing processability of the strip portion 7 is also improved while improving the polishing process accuracy and the damage suppression effect. In other words, it can be seen that the materials for ceramic balls 5 according to Examples 1 to 9 can shorten the polishing process time.

[0053] In addition, the examples do not include examples in which the ceramic ball material 5 is a boron nitride sintered body or a zirconium oxide sintered body. However, if the ceramic ball material 5 satisfies at least the condition of the ratio Rtb / Rts, it is considered to be superior in polishing processability and damage suppression compared to the comparative examples, similarly to the cases of an aluminum oxide sintered body, a silicon nitride sintered body, and a silicon carbide sintered body.

[0054] As described above, according to the material 5 for a ceramic ball, the polishing processability of the ceramic material during polishing can be improved and damage can be suppressed.

[0055] Although some embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. Modifications of these embodiments are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other.

Claims

1. A method for producing a ceramic ball material, comprising: a granulation step for preparing a granulated powder; a molding step for molding a green body from the granulated powder; and a sintering step for sintering the green body to obtain a ceramic ball material, the ceramic ball material obtained in the sintering step has a spherical surface portion and a band-shaped portion formed around a circumference of the spherical surface portion, the ceramic ball material obtained in the sintering step has a ratio Rtb / Rts of a maximum cross-sectional height Rtb of a roughness curve on the outer peripheral surface of the band-shaped portion to a maximum cross-sectional height Rts of a roughness curve on the outer peripheral surface of the spherical portion, the ratio being greater than 1.0 and less than 3.

0.

2. 2. The method for manufacturing a material for a ceramic ball according to claim 1, wherein the arbitrary diameter of the spherical portion is 0.5 mm or more.

3. 2. The method for producing a material for a ceramic ball according to claim 1, wherein the material for a ceramic ball is one selected from the group consisting of an aluminum oxide sintered body, a silicon nitride sintered body, a silicon carbide sintered body, a boron nitride sintered body, and a zirconium oxide sintered body.

4. 2. The method for producing a material for a ceramic ball according to claim 1, wherein the material for a ceramic ball is a sintered ceramic body containing 85 mass % or more of silicon nitride.

5. The granulation step includes mixing two or more types of granulated powder having different particle size ranges by classification, 2. The method for producing a ceramic ball material according to claim 1, wherein the molding step comprises molding the green body from the granulated powder mixed after the classification.

6. 6. The method for producing a raw material for ceramic balls according to claim 5, wherein the molding step comprises press-molding the granulated powder mixed after the classification to form the green body.

7. 7. The method for manufacturing a material for ceramic balls according to claim 6, characterized in that the pressing step is performed using a die press molding device in which the inside of a cross section of a die is concave and the depth of the concave portion is 0.01 mm or more and 0.10 mm or less.

8. 8. A method for producing a ceramic ball, comprising the steps of: polishing a ceramic ball material produced by the method for producing a ceramic ball material according to claim 1, by using a surface plate.

Citation Information

Patent Citations

  • Silicon nitride ceramic ball and ceramic ball bearing using the same

    JP2001146479A

  • Raw material for ceramic ball and method of producing ceramic ball

    JP2001163673A

  • Rough ceramic ball and method for manufacturing the same

    JP2003137640A

  • Ceramic ball stock sphere, mold for forming ceramic ball stock sphere and method for manufacturing ceramic ball stock sphere

    JP2011093789A

  • Ceramic ball base sphere

    JP2013209283A