Sensor element, gas sensor, and method for manufacturing sensor element
The sensor element with controlled noble metal particle states in porous layers balances catalytic ability and response speed, improving detection accuracy and maintaining sensor efficiency.
Patent Information
- Application Number
- JP2023044010
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
The increase in noble metal particles on the catalyst layer improves combustion of unburned gas but decreases the response speed of the sensor due to oxygen adsorption and release, affecting detection accuracy.
A sensor element design with porous layers containing noble metal particles, where the absorption intensity of the noble metal particles is controlled between pure metal and oxide states through specific heat treatment, maintaining a balance between catalytic ability and response speed.
The sensor element effectively burns unburned gas, enhances detection accuracy, and suppresses a decrease in response speed by optimizing the electronic state of noble metal particles.
Smart Images

Figure 2024133966000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sensor element suitable for use in a gas sensor for detecting the concentration of a specific gas contained in combustion gas or exhaust gas from a combustor, an internal combustion engine, etc., a gas sensor, and a method for manufacturing the sensor element. [Background technology]
[0002] A known gas sensor capable of measuring the concentration of a specific gas component in a measurement gas such as the exhaust gas of an internal combustion engine of an automobile has a configuration including a cell having a pair of electrodes formed on the surface of an oxygen ion conductive solid electrolyte layer such as zirconia, etc. Here, each electrode is formed by screen printing a paste containing particles of a precious metal such as Pt, followed by firing. Also, in order to improve the degree of combustion of unburned gas in the measured gas, a technology is known in which a catalyst layer is provided to cover the detection electrode on the measured side (Patent Document 1). This catalyst layer is made by supporting precious metal particles on a porous layer of alumina, titania, etc., and burns unburned gas (H2, NOx, HC, etc.) in the measured gas before it reaches the detection electrode, preventing its influence on the measurement and improving the detection accuracy. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-186458 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the greater the amount of precious metal particles supported on the catalyst layer, the greater the degree of combustion of unburned gas (catalytic activity), but the combustion of gas in the catalyst layer tends to decrease the sensor's response speed. This is thought to be because the precious metal particles in the catalyst layer adsorb and release oxygen, slowing down the sensor's response speed to changes in the measured gas.
[0005] Therefore, an object of the present invention is to provide a sensor element, a gas sensor, and a method for manufacturing the sensor element that can burn unburned gas in a gas to be measured well to improve detection accuracy and suppress a decrease in the response speed of the sensor.
Means for Solving the Problems
[0006] To solve the above problems, a sensor element of the present invention includes a first electrode provided on a solid electrolyte layer, a second electrode that serves as a counter electrode to the first electrode and is provided on the solid electrolyte layer, and at least one or more porous layers interposed between the outside and one of the electrodes so that a gas to be measured introduced from the outside toward at least one of the first electrode and the second electrode passes through. The sensor element is for detecting a specific gas in the gas to be measured, and at least one of the porous layers is a catalyst layer supporting one or more noble metal particles selected from the group consisting of Pt, Pd, and Rh. When X-ray absorption fine structure analysis is performed, the absorption intensity Ip at the absorption edge of the noble metal particles supported on the catalyst layer is between the absorption intensity Im at the absorption edge of the pure metal of the noble metal particles and the absorption intensity Io at the absorption edge of the oxide of the noble metal particles.
[0007] According to this sensor element, Im < Ip < Io, and since the electronic state of the noble metal particles in the catalyst layer by X-ray absorption fine structure analysis (XAFS) is located between that of the pure metal and the oxide, both advantages can be achieved. The unburned gas in the gas to be measured can be burned well to improve detection accuracy, and a decrease in the response speed of the sensor can be suppressed.
[0008] In the sensor element of the present invention, when the noble metal particles contain Pt, the Im of Pt is set to 0%, the Io of Pt is set to 100%, and the Ip of Pt may be 2 to 20%. According to this sensor element, the electronic state of the noble metal particles in the catalyst layer can be surely maintained between that of the pure metal and the oxide.
[0009] The gas sensor of the present invention is a gas sensor including a sensor element and a metallic shell that holds the sensor element, wherein the sensor element is the sensor element according to claim 1 or 2.
[0010] The present invention provides a method for manufacturing a sensor element, which comprises a first electrode provided on a solid electrolyte layer, a second electrode that serves as a counter electrode of the first electrode and is provided on the solid electrolyte layer, and at least one porous layer interposed between an outside and at least one of the first electrode and the second electrode so that a measurement gas introduced from the outside toward at least one of the first electrode and the second electrode passes through the porous layer, and detects a specific gas in the measurement gas, comprising: At least one of the porous layers is a catalyst layer supporting one or more types of precious metal particles selected from the group consisting of Pt, Pd, and Rh, and the method is characterized by comprising a penetration step of penetrating the porous layer that becomes the catalyst layer with a precious metal salt solution containing ions or particles of the precious metal, and a heat treatment step of heat-treating the porous layer penetrated with the precious metal salt solution in an inert atmosphere or an inert atmosphere containing 2000 mass ppm or less of oxygen, at a temperature equal to or higher than the temperature at which a component of the precious metal salt solution thermally decomposes. Effect of the Invention
[0011] According to the present invention, a sensor element can be obtained which satisfactorily combusts unburned gas in a gas to be measured to improve detection accuracy and which prevents a decrease in the response speed of the sensor. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a cross-sectional view showing a gas sensor 200 according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an exploded perspective view of the sensor element 10. [Diagram 3] 1 is a cross-sectional view of a sensor element 10. FIG. [Figure 4] FIG. 2 is a schematic diagram showing the relationship between catalytic activity and the response speed of a sensor. [Diagram 5]FIG. 1 is a graph showing the relationship between the VR value in an H2-rich atmosphere and the absorption intensity of Pt particles in a catalyst layer. [Figure 6] FIG. 1 is a graph showing the relationship between the VR value in a CO-rich atmosphere and the absorption intensity of Pt particles in a catalyst layer. [Figure 7] FIG. 7 is a graph showing the VR value in the H2-rich atmosphere of FIG. 5 subtracted from the VR value in the CO-rich atmosphere of FIG. 6 at each absorption intensity Xμ. [Figure 8] FIG. 1 shows the XAFS spectrum of Pt particles between the metallic state (PtM) and the oxide state (PtO2). [Figure 9] FIG. 9 is an enlarged view of the vicinity of the peak in FIG. 8. [Figure 10] FIG. 1 is a graph showing the relationship between the oxygen concentration in the atmosphere in which a precious metal salt solution is heat-treated and the absorption intensity of Pt particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described. Fig. 1 is a cross-sectional view showing a gas sensor 200 according to an embodiment of the present invention. The gas sensor 200 is fixed to an exhaust pipe of an internal combustion engine (not shown) to measure the concentration of oxygen, which is a gas to be measured. Fig. 1 shows a cross section parallel to a longitudinal direction D1 of the gas sensor 200. Hereinafter, the downward direction (lower side) in Fig. 1 will be referred to as the front end side (FWD) of the gas sensor 200, and the upward direction (upper side) in Fig. 1 will be referred to as the rear end side (BWD) of the gas sensor 200.
[0014] The gas sensor 200 includes a cylindrical metal shell 138, a plate-like sensor element 10 extending in the longitudinal direction D1, a cylindrical ceramic sleeve 106 surrounding the sensor element 10, an insulating contact member 166, and six connection terminals 110 (four are shown in FIG. 1). A threaded portion 139 for fixing to an exhaust pipe is formed on the outer surface of the metal shell 138. The ceramic sleeve 106 holds the sensor element 10 within the ceramic sleeve 106 so that the front end of the sensor element 10 is positioned outside the front end side (FWD) of the ceramic sleeve 106 and the rear end side of the sensor element 10 is positioned outside the rear end side (BWD) of the ceramic sleeve 106. The insulating contact member 166 has a contact insertion hole 168 formed therethrough in the longitudinal direction D1. The insulating contact member 166 is disposed such that the inner wall surface of the contact insertion hole 168 surrounds the rear end portion of the sensor element 10. Each connection terminal 110 is disposed between the sensor element 10 and the insulating contact member 166.
[0015] The metal shell 138 has a through hole 154 penetrating in the axial direction, and is configured in a generally cylindrical shape having a shelf portion 152 protruding radially inward of the through hole 154. The metal shell 138 holds the sensor element 10 in the through hole 154 such that a leading end of the sensor element 10 is disposed outside the leading end side (FWD) of the through hole 154, and a rear end side of the sensor element 10 is disposed outside the rear end side (BWD) of the through hole 154. The shelf portion 152 includes a tapered surface inclined with respect to a plane perpendicular to the longitudinal direction D1. The tapered surface is formed such that the diameter of the leading edge (FWD) of the shelf 152 is smaller than the diameter of the trailing edge (BWD).
[0016] A ceramic holder 151, powder filled layers 153 and 156 (hereinafter also referred to as talc rings 153 and 156), and a ceramic sleeve 106 are layered in this order from the front end side (FWD) to the rear end side (BWD) inside the through hole 154 of the metallic shell 138. The ceramic holder 151, the talc rings 153 and 156, and the ceramic sleeve 106 are collectively referred to as a retaining portion 160. The holding portion 160 holds the sensor element 10 therein such that the front end of the sensor element 10 is disposed outside the front end side (FWD) of the holding portion 160 and the rear end side of the sensor element 10 is disposed outside the rear end side (BWD) of the holding portion 160. The sensor element 10 is held by the holding portion 160.
[0017] A crimping packing 157 is disposed between the ceramic sleeve 106 and the rear end portion 140 of the metal shell 138. A metal holder 158 is disposed between the ceramic holder 151 and the shelf portion 152 of the metal shell 138 to hold the talc ring 153 and the ceramic holder 151 and maintain airtightness. The rear end 140 of the metallic shell 138 is crimped so as to press the ceramic sleeve 106 against the front end side via a crimp packing 157 .
[0018] 1, an outer protector 142 and an inner protector 143 are attached by welding or the like to the outer periphery of the front end side (FWD) of the metallic shell 138. These double protectors 142, 143 are made of metal (e.g., stainless steel), each of which has a plurality of gas introduction holes and covers the protruding portion of the sensor element 10.
[0019] An outer cylinder 144 is fixed to the outer periphery on the rear end side of the metallic shell 138. A grommet 150 is disposed in an opening on the rear end side (BWD) of the outer cylinder 144. A lead wire insertion hole 161 is formed in the grommet 150. Six lead wires 146 are inserted into the lead wire insertion hole 161 (only five lead wires 146 are shown in FIG. 1). These lead wires 146 are each electrically connected to an electrode pad (not shown) provided on the outer surface on the rear end side of the sensor element 10.
[0020] An insulating contact member 166 is disposed on the rear end side (BWD) of the sensor element 10 protruding from the rear end portion 140 of the metallic shell 138. This insulating contact member 166 is disposed around an electrode pad (not shown) formed on the surface of the rear end side of the sensor element 10. The insulating contact member 166 is formed in a cylindrical shape having a contact insertion hole 168 penetrating in the longitudinal direction D1, and includes a flange portion 167 protruding radially outward from the outer surface on the rear end side. A holding member 169 is inserted between the insulating contact member 166 and the outer cylinder 144. The holding member 169 contacts the outer cylinder 144 and the flange portion 167, thereby positioning the insulating contact member 166 inside the outer cylinder 144.
[0021] Fig. 2 is an exploded perspective view of the sensor element 10. In Fig. 2, the left direction indicates the front end direction (front end side) FWD of the sensor element 10, and the right direction indicates the rear end direction (rear end side) BWD. The sensor element 10 includes an insulating layer 21, a solid electrolyte layer 30, an insulating layer 22, an insulating layer 23, and porous layers 80 and 81. The insulating layer 21, the solid electrolyte layer 30, the insulating layer 22, and the insulating layer 23 are stacked along a stacking direction D2 perpendicular to the longitudinal direction D1. Note that in Fig. 2, the porous layers 80 and 81 are omitted, and only the insulating layer 21, the solid electrolyte layer 30, the insulating layer 22, and the insulating layer 23 are shown.
[0022] In this embodiment, the solid electrolyte layer 30 is formed mainly from zirconia having oxygen ion conductivity, with yttria or calcia added as a stabilizer.
[0023] The insulating layers 21, 22, and 23 are formed using alumina as a main component. The solid electrolyte layer 30 and the insulating layers 21, 22, and 23 are each formed using a sheet of a raw material (for example, a sheet of ceramic such as zirconia or alumina).
[0024] A measured gas side electrode 41 is disposed between the solid electrolyte layer 30 and the insulating layer 21, and a reference gas electrode 42 is disposed between the solid electrolyte layer 30 and the insulating layer 22. A detection lead 41a extends from the measured gas side electrode 41 toward the rear end (rear end side) BWD, and a detection lead 42a also extends from the reference gas electrode 42 toward the rear end (rear end side) BWD. The measured gas side electrode 41 and the reference gas electrode 42 are formed using, for example, platinum, rhodium, lead, or the like.
[0025] The measurement gas side electrode 41 and the reference gas electrode 42 correspond to the "first electrode" and "second electrode" in the claims, respectively, and the first electrode corresponds to "one electrode" in the claims.
[0026] The oxygen concentration in the exhaust gas is detected by an oxygen concentration cell. The oxygen concentration cell is composed of a solid electrolyte layer 30, a measured gas side electrode 41, and a reference gas electrode 42. The measured gas side electrode 41 is electrically connected to an electrode terminal 61 from a detection lead 41a via a through hole 21a formed in the insulating layer 21. The reference gas electrode 42 is electrically connected to an electrode terminal 62 from a detection lead 42a via a through hole 30a formed in the solid electrolyte layer 30 and a through hole 21b formed in the insulating layer 21.
[0027] A porous protective layer 60 made of alumina or the like is provided on the tip side of the insulating layer 21. The porous protective layer 60 is a porous layer provided to diffuse gas (measurement gas) that enters the measurement gas side electrode 41.
[0028] A heater 50 extending along the longitudinal direction D1 is embedded between the insulating layer 22 and the insulating layer 23. The heater 50 is used to heat the sensor element 10 to a predetermined activation temperature and increase the conductivity of oxygen ions in the solid electrolyte layer to stabilize the operation of the gas sensor 200. The heater 50 is a heating resistor formed of a conductor such as tungsten, and generates heat when power is supplied to the heater 50. The heater 50 is sandwiched between the insulating layer 22 and the insulating layer 23.
[0029] The heater 50 includes a heat generating portion 50a and electrode terminals 50b, 50c. The heat generating portion 50a is located at the tip side. The heat generating portion 50a has a heating wire arranged in a serpentine shape, and generates heat when electricity is applied. The heater 50 is electrically connected from the electrode terminals 50b, 50c to electrode terminals 63, 64 via through holes 23a, 23b formed in the insulating layer 23, respectively. The electrode terminals 61 to 64 can be formed using, for example, platinum, rhodium, lead, or the like.
[0030] 2 also shows a control unit CU of the gas sensor 200 (sensor element 10). The control unit CU is connected to the heater 50 and each of the electrode terminals 61-64 via the connection terminal 110 and lead wire 146 shown in FIG. 1. The control unit CU supplies power to the heater 50. The control unit CU also controls the gas sensor 200 (sensor element 10) by transmitting and receiving signals to and from each of the electrode terminals 61-64. The control unit CU may be formed using a computer having a CPU and a memory.
[0031] 3 is a cross-sectional view of the sensor element 10. This cross-sectional view shows a cross section parallel to the stacking direction D2, and is a cross-sectional view taken along line II-II shown in FIG.
[0032] Fig. 3 shows porous layers 80 and 81, which are omitted in Fig. 2. In this embodiment, the range S from the tip of the sensor element 10 to the rear end of the porous protective layer 60 in Fig. 2 is covered with the porous layers 80 and 81. The porous layer 80 contacts and covers the sensor element 10, and the porous layer 81 covers the outer surface of the porous layer 80.
[0033] The porous layers 80 and 81 prevent cracks from occurring in the body of the sensor element 10 when water droplets adhere to the sensor element 10. The outer porous layer 81 is a catalyst layer supporting one or more types of precious metal particles 90 selected from the group consisting of Pt, Pd, and Rh. The porous layers 80 and 81 are formed mainly from ceramic particles (alumina and spinel), and the ceramic particles are bonded together via gaps by firing. The porous layer 81 corresponds to the "catalyst layer" in the claims. The catalyst may be supported not only in the outermost layer (porous layer 81) but also in the inner layer (porous layer 80).
[0034] The precious metal particles 90 supported on the porous layer 81 serve as a catalyst that improves the degree of combustion of unburned gas. In other words, the precious metal particles 90 burn unburned gas (H2, NOx, HC, etc.) in the measured gas (exhaust gas) before it reaches the measured gas side electrode 41, thereby preventing the unburned gas from affecting the measurement and improving the detection accuracy. Incidentally, the degree of combustion (catalytic activity) of unburned gas changes depending on the state (oxidation state and particle size) and amount of the precious metal particles 90 supported on the catalyst layer. For example, the greater the amount of the precious metal particles 90, the higher the degree of combustion (catalytic activity) of unburned gas, but the combustion of gas in the catalyst layer tends to decrease the response speed of the sensor.
[0035] Fig. 4 is a schematic diagram showing the relationship between catalytic activity and the response speed of a sensor. There is a trade-off between catalytic activity and the response speed of a sensor. The reason why the response speed of the sensor decreases as the amount of precious metal particles 90 supported on the catalyst layer increases is thought to be that the precious metal particles in the catalyst layer adsorb and release oxygen, decreasing the response speed to changes in the measured gas.
[0036] As a result of the inventor's investigation, it was found that, as described below, even when the same amount of precious metal particles 90 is used, when the catalytic activity is low, the precious metal particles 90 (Pt in FIG. 4) tend to become an oxide (PtO2 in FIG. 4). On the other hand, when the response speed of the sensor is slow, the precious metal particles 90 (Pt in FIG. 4) tend to become a metal state (PtM in FIG. 4). Therefore, if it is possible to identify the state of the precious metal particles 90 in region R in Figure 4, where both catalytic activity and sensor response speed are achieved, it is expected that the unburned gas in the measured gas can be burned effectively to improve detection accuracy while suppressing a decrease in the sensor response speed. For this reason, the present inventors experimentally determined an index for identifying the state of the precious metal particles 90 in the region R in FIG.
[0037] First, a precious metal salt solution containing Pt ions (specifically, dinitrodiammine Pt nitrate) was permeated into the porous layer 81 to prepare the precious metal particles 90 supported on the catalyst layer. Then, the entire sensor element 10 including the porous layer 81 was heat-treated in a predetermined atmosphere at a temperature equal to or higher than the temperature at which the components of the precious metal salt solution thermally decompose, thereby obtaining the precious metal particles 90. Here, by varying the amount of Pt in the precious metal salt solution and the heat treatment atmosphere, the electronic state of the resulting Pt particles was changed between the metallic state (PtM) and the oxide state (PtO2). The lower the oxygen content in the heat treatment atmosphere, the closer the alloy became to the metallic state, and the higher the oxygen content in the heat treatment atmosphere, the closer the alloy became to the metallic state. The latter behavior is the opposite of what was expected, and will be discussed later.
[0038] The electronic state of the Pt particles obtained by heat treatment was identified by the absorption intensity (X-ray absorption amount or absorbance) Xμ at the absorption edge in X-ray absorption fine structure analysis (XAFS). In addition, Xμ of Pt foil, which indicates a metallic state (PtM), was 1.237 (arbitrary unit: au), and Xμ of the oxide (PtO2) was 2.214.
[0039] The obtained sensor element 10 was assembled into a gas sensor 200, and the sensor output in a predetermined test gas atmosphere was measured. Figures 5 and 6 show the relationship between the VR value in an H2-rich atmosphere and a CO-rich atmosphere, respectively, and the absorption intensity of the Pt particles in the catalyst layer. As shown in Figure 5, the smaller the absorption intensity Xμ (left side of Figure 5), the closer the electronic state of the Pt particles is to a metallic state (PtM), and the larger the absorption intensity Xμ (right side of Figure 5), the closer it is to an oxide (PtO2).
[0040] FIG. 7 shows a graph (VR(H2-CO)) in which the VR value in the H2-rich atmosphere in FIG. 5 is subtracted from the VR value in the CO-rich atmosphere in FIG. 6 at each absorption intensity Xμ. The smaller the difference in the VR values (VR(H2-CO)) in FIG. 7, the more stable the detection can be (the more accurate the detection) regardless of the composition of the gas to be measured, which is preferable. Table 1 shows VR(H2), VR(CO), and differential VR(H2 - CO) for the metallic state (PtM: Pt foil) and the oxide (PtO2).
[0041] [Table 1]
[0042] According to Table 1, in the metallic state (PtM), the differential VR is extremely small, and while the detection accuracy is excellent, the response speed of the sensor is low as shown in FIG. 4. On the other hand, in the case of the oxide (PtO2), the differential VR is large, and while the response speed is excellent, the detection accuracy is poor. From these facts, it can be seen that a state where the value of the differential VR is between the metallic state (PtM) and the oxide (PtO2) is good. Note that the metallic state (PtM) was obtained by setting the heat treatment atmosphere of the noble metal salt solution to a reducing atmosphere (H2), and the oxide (PtO2) was obtained by setting the heat treatment atmosphere of the noble metal salt solution to an air atmosphere.
[0043] Then, FIGS. 8 and 9 show the XAFS spectra of Pt particles (the "Example Group of the Present Invention" in FIG. 9) in which the value of the differential VR is between the metallic state (PtM) and the oxide (PtO2) as described above, together with the XAFS spectra of the metallic state (PtM) and the oxide (PtO2). Note that FIG. 9 is an enlarged view of the vicinity of the peak in FIG. 8.
[0044] As shown in FIGS. 8 and 9, in XAFS, it can be seen that the absorption intensity Ip at the absorption edge of the Pt particles is between the absorption intensity Im at the absorption edge of the metallic state (PtM: pure metal) and the absorption intensity Io at the absorption edge of the oxide (PtO2). Based on this, as an index for specifying the state of the noble metal particles 90 in the R region of FIG. 4, Im < Ip < Io was defined as the present invention. If Im < Ip < Io, the noble metal particles 90 in the catalyst layer are in the R region of FIG. 4, that is, their electronic state is located between that of the pure metal and the oxide. Therefore, both advantages of the two can be achieved, and the unburned gas in the gas to be measured can be burned well to improve the detection accuracy, and at the same time, the decrease in the response speed of the sensor can be suppressed.
[0045] As described above, the actual Im of Pt was 1.237, and the Io of Pt was 2.214. Also, the Ip of the example group in FIG. Calculations based on this show that when the precious metal particles in the catalyst layer contain Pt, and the Im of Pt is taken as 0% and the Io of Pt is taken as 100%, the Ip of Pt is preferably 2 to 20%. When the precious metal particles in the catalyst layer contain Pt, for example, when the precious metal particles are a mixture of Pt and Rh, the Ip of Pt may be 2 to 20%.
[0046] Next, an example of the operation of the sensor element 10 will be described. First, the control unit CU controls the supply of power to the heater 50, and the heater 50 heats the measured gas side electrode 41 and the reference gas electrode 42 to their activation temperatures. Then, in response to the measured gas side electrode 41 and the reference gas electrode 42 being heated to their activation temperatures, the control unit CU controls the flow of current between the measured gas side electrode 41 and the reference gas electrode 42. This causes oxygen in an amount that corresponds to the reference concentration to be pumped from the measured gas side electrode 41 to the reference gas electrode 42.
[0047] The electromotive force between the measurement gas side electrode 41 and the reference gas electrode 42 changes rapidly near the theoretical air-fuel ratio (λ=1) according to the oxygen concentration in the measurement gas (exhaust gas) that has flowed into the measurement gas side electrode 41. This allows the control unit CU to detect whether the measurement gas (exhaust gas) is in a lean or rich state. Here, the "lean state" refers to an atmosphere in which the proportion of oxygen is high relative to λ=1. Also, the "rich state" refers to an atmosphere in which the proportion of oxygen is low relative to λ=1.
[0048] In this embodiment, the reference gas is stored in the reference gas electrode 42, but a space (air inlet) for introducing air may be provided between the reference gas electrode 42 and the insulating layer 22.
[0049] Next, a method for manufacturing the sensor element according to the embodiment of the present invention will be described. A method for manufacturing a sensor element according to an embodiment of the present invention includes a penetration step of penetrating a porous layer that will become a catalyst layer with a precious metal salt solution containing precious metal ions or particles, and a heat treatment step of heat treating the porous layer that has been penetrated with the precious metal salt solution in an inert atmosphere or an inert atmosphere containing 2000 mass ppm or less of oxygen at a temperature equal to or higher than the temperature at which the components of the precious metal salt solution thermally decompose.
[0050] Here, as shown in the experimental results already mentioned, depending on the heat treatment atmosphere of the porous layer permeated with the precious metal salt solution, the electronic state of the obtained precious metal (e.g., Pt) particles becomes somewhere between the metallic state (PtM) and the oxide (PtO2) (including PtM and PtO2). Therefore, the heat treatment atmosphere is important.
[0051] The reason for using an inert atmosphere or an inert atmosphere containing 2000 mass ppm or less of oxygen as the heat treatment atmosphere is as follows. First, as mentioned above, if the heat treatment atmosphere is a reducing atmosphere (H2), the oxide of the precious metal (e.g., Pt) is completely reduced to a metallic state (PtM), so an inert atmosphere other than a reducing atmosphere is used. Examples of the inert atmosphere include rare gases such as Ar, and N2 gas. Furthermore, as described above, if the heat treatment atmosphere was an air atmosphere (oxygen at approximately 200,000 mass ppm), the precious metal (for example, Pt) would be completely oxidized to an oxide, so an inert atmosphere was used.
[0052] However, it was surprisingly found that, as shown in FIG. 10, in an inert atmosphere containing oxygen at 2000 mass ppm or less, more preferably 1000 ppm or less, and even more preferably 100 ppm or less, the higher the oxygen concentration, the closer the material approaches the metallic state (PtM). Since Xμ=1.237 in the metallic state (PtM), the oxygen concentration at which the value is higher than Xμ=1.237 is estimated to be approximately 1000 mass ppm or more. Therefore, if the inert atmosphere contains oxygen at 1000 mass ppm or less, the electronic state of the precious metal particles can be adjusted between the metallic state (PtM) and the oxide state (PtO2). In addition, the minimum oxygen concentration in FIG. 10 was 20 mass ppm, and the maximum was 780 ppm.
[0053] Examples of the method for permeating the precious metal salt solution into the porous layer 81 include spray coating, impregnation, etc. The heat treatment temperature can be set to about 900 to 1100°C.
[0054] The present invention is not limited to the above-described embodiment, and various modifications and equivalents are included within the spirit and scope of the present invention. For example, the present invention can be applied to oxygen sensors such as a full range air-fuel ratio sensor in addition to a NOx sensor, but is not limited to these applications.
[0055] For example, in the above embodiment, the sensor element 10 is in the shape of a plate, but it is not limited to a plate-shaped sensor element, and may be a cylindrical sensor element. Note that a cylindrical sensor element refers to a sensor element having a heater in the center and a solid electrolyte layer that encases the heater. More specifically, a sensor element that includes a heater, a reference gas electrode, a solid electrolyte layer, a measured gas side electrode, and a porous layer from the center toward the outside in the radial direction is called a cylindrical sensor element.
[0056] In the above embodiment, the porous layer carrying the catalytic metal is two layers (porous layers 80, 81), but it may be one layer. By using one layer, the sensor element can be made smaller. Conversely, the porous layer carrying the catalytic metal may be three or more layers. By increasing the number of porous layers, it is possible to more reliably prevent water from entering the inside of the sensor element. [Explanation of symbols]
[0057] 10 Sensor element 30 Solid electrolyte layer 41 First electrode, one electrode (measurement gas side electrode) 42 Second electrode (reference gas electrode) 80 Porous Layer 81 Porous layer (catalyst layer) 90 Precious metal particles 138 Metal fitting 200 Gas Sensor
Claims
1. A sensor element for detecting a specific gas in a measurement gas, comprising: a first electrode provided on a solid electrolyte layer; a second electrode that serves as a counter electrode of the first electrode and is provided on the solid electrolyte layer; and at least one porous layer interposed between the outside and at least one of the first electrode and the second electrode so that a measurement gas introduced from the outside toward at least one of the first electrode and the second electrode passes through the first electrode, At least one of the porous layers is a catalyst layer supporting one or more kinds of precious metal particles selected from the group consisting of Pt, Pd, and Rh; A sensor element characterized in that, when subjected to X-ray absorption fine structure analysis, the absorption intensity Ip at the absorption edge of the precious metal particles supported on the catalyst layer is between the absorption intensity Im at the absorption edge of the pure metal of the precious metal particles and the absorption intensity Io at the absorption edge of the oxide of the precious metal particles.
2. 2. The sensor element according to claim 1, wherein the precious metal particles contain Pt, and when the Im of Pt is 0% and the Io of Pt is 100%, the Ip of Pt is 2 to 20%.
3. A gas sensor comprising a sensor element and a metal shell for holding the sensor element, 3. A gas sensor comprising the sensor element according to claim 1 or 2.
4. A method for manufacturing a sensor element for detecting a specific gas in a measurement gas, the sensor element comprising: a first electrode provided on a solid electrolyte layer; a second electrode that serves as a counter electrode of the first electrode and is provided on the solid electrolyte layer; and at least one porous layer interposed between the outside and at least one of the first electrode and the second electrode so that a measurement gas introduced from the outside toward at least one of the first electrode and the second electrode passes through the porous layer, the method comprising the steps of: At least one of the porous layers is a catalyst layer supporting one or more kinds of precious metal particles selected from the group consisting of Pt, Pd, and Rh; a permeation step of permeating the porous layer that becomes the catalyst layer with a precious metal salt solution containing ions or particles of the precious metal; and a heat treatment step of heat-treating the porous layer permeated with the precious metal salt solution in an inert atmosphere or an inert atmosphere containing 2000 mass ppm or less of oxygen at a temperature equal to or higher than a temperature at which a component of the precious metal salt solution thermally decomposes.
Citation Information
Patent Citations
Tubular sensing element with excellent performance and preparation method thereof
CN111505079A
Limiting current type oxygen sensor
JP1997203719A
Oxygen sensor element and production method thereof
JP2002181769A
Gas sensor and manufacturing method thereof
JP2014178179A
Sensor element and gas sensor
JP2019117135A