Adhesive sheet for polishing process
The adhesive sheet with a maleimide compound, acrylonitrile-butadiene copolymer, and phenol resin addresses peel and shear strength imbalances, enhancing adhesion and reducing contamination in polishing processes.
Patent Information
- Application Number
- JP2023044206
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing adhesive sheets for polishing processes do not adequately balance peel strength and shear strength, leading to potential contamination and adhesion issues during polishing.
An adhesive sheet comprising an adhesive layer containing a compound with two or more maleimide groups, an acrylonitrile-butadiene copolymer, and a phenol resin, with specific ratios and properties to enhance peel and shear strength, and a thickness range of 5 to 80 μm.
The adhesive sheet achieves improved peel and shear strength, reducing contamination risks and ensuring effective adhesion in polishing processes.
Smart Images

Figure 2024134096000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive sheet for use in a polishing process. [Background technology]
[0002] The use of adhesive sheets in the polishing process is being considered. Patent Document 1 describes fixing a polishing pad to a stainless steel plate using an adhesive sheet that exhibits a 180-degree peel strength of 30 N / 20 mm or more. Patent Document 2 describes an adhesive for fixing abrasive members, which contains a synthetic rubber containing a styrene-isoprene block copolymer and a tackifier resin containing a terpene phenol resin. Patent Document 3 describes a method of fixing an abrasive to a platen of a polishing machine using a double-sided adhesive tape in which the gel fraction of the acrylic adhesive is 70 to 90%. Patent Document 4 describes the use of an adhesive sheet made of resin impregnated with sound absorbing and shock absorbing materials to bond components of a cutting saw machine or the like. Patent Document 5 describes an abrasive material in which an abrasive layer is laminated on a substrate via an adhesive layer formed by curing a photocurable adhesive composition whose main component is an ethylene-vinyl acetate copolymer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-78348 A [Patent Document 2] JP 2018-65982 A [Patent Document 3] JP 2000-309760 A [Patent Document 4] JP 2001-106997 A [Patent Document 5] Japanese Patent Application Publication No. 9-235384 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide an adhesive sheet for a polishing process that can be suitably used in a polishing process. [Means for solving the problem]
[0005] A first aspect of the present invention is an adhesive sheet for use in a polishing process, characterized by having an adhesive layer containing a compound containing two or more maleimide groups, an acrylonitrile-butadiene copolymer, and a phenol resin.
[0006] In the second aspect, in the first aspect, the adhesive layer is heated from 25° C. at a rate of 3° C. / min to reach 100° C., and the melt viscosity is 1.0×10 3 ~1.0×10 6 It is characterized by its Pa·s. A third aspect is characterized in that in the first or second aspect, the adhesive layer has a thickness of 5 to 80 μm. The fourth aspect is characterized in that, in any one of the first to third aspects, the adhesive layer contains at least one of the following compound (1) or the following compound (2) as the compound containing two or more maleimide groups.
[0007] [ka]
[0008] [ka]
[0009] A fifth aspect is characterized in that in any one of the first to fourth aspects, the content of the acrylonitrile-butadiene copolymer in the adhesive layer is 20 to 70 mass %. Effect of the Invention
[0010] According to the present invention, an adhesive sheet for a polishing process that can be suitably used in a polishing process can be provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a cross-sectional view showing an example of an adhesive sheet for a polishing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the present invention will be described based on preferred embodiments.
[0013] An example of an adhesive sheet for the polishing process is shown in Figure 1. In this adhesive sheet for the polishing process 10, separators 12 and 13 are laminated on both sides of an adhesive layer 11. The separators 12 and 13 may have the same peel strength with respect to the adhesive layer 11 or may have different peel strengths. When the separators 12 and 13 are peeled off, both sides of the adhesive layer 11 are exposed as adhesive surfaces and can be used in the polishing process.
[0014] The adhesive layer 11 contains a compound containing two or more maleimide groups, an acrylonitrile-butadiene copolymer, and a phenol resin.
[0015] A compound containing two or more maleimide groups (hereinafter sometimes referred to as a "maleimide compound") is used for the adhesive layer 11. The maleimide compound exhibits thermosetting properties due to having two or more maleimide groups in the molecule.
[0016] The maleimide group is a monovalent group that bonds to another atom at the position of the nitrogen atom of maleimide. For example, in the above-mentioned compound (1) and chemical formula (2), a cyclic group containing one nitrogen atom, two carbonyl groups, and one C=C double bond at both the left and right ends is a maleimide group. The linking group that links two or more maleimide groups can include one or more types selected from an aliphatic hydrocarbon group, an aromatic hydrocarbon group, an ether bond, a siloxane bond, etc.
[0017] Examples of the aliphatic hydrocarbon group that may be contained in the maleimide compound include alkylene groups such as a methylene group, an ethylene group, and a dialkyl-substituted methylene group. Examples of the aromatic hydrocarbon group that may be contained in the maleimide compound include a phenylene group and a dialkyl-substituted phenylene group.
[0018] The ether bond that may be contained in the maleimide compound is preferably an ether bond that links aliphatic hydrocarbon groups and / or aromatic hydrocarbon groups, and more preferably an ether bond that links aromatic hydrocarbon groups. The siloxane bond that may be contained in the maleimide compound includes a dimethyl-substituted siloxane group.
[0019] It is preferable that the adhesive layer 11 contains at least one of the compound (1) shown in the above formula (1) or the compound (2) shown in the above formula (2) as a maleimide compound. Compound (1) is bis(4-maleimidophenyl)ether of bisphenol A. Compound (2) is bis(3-ethyl-4-maleimido-5-methylphenyl)methane.
[0020] The proportion of the maleimide compound contained in the adhesive layer 11 (hereinafter sometimes referred to as "MI proportion") is not particularly limited, but is preferably 10 to 50 mass %, more preferably 15 to 45 mass %. When the MI proportion is within the above range, both the peel strength and the shear strength are achieved, and the adhesive layer 11 can be suitably used in the polishing process.
[0021] An acrylonitrile-butadiene copolymer is used for the adhesive layer 11. The acrylonitrile-butadiene copolymer is not particularly limited, but may be an acrylonitrile-butadiene copolymer having a carboxyl group, or an acrylonitrile-butadiene copolymer not having a carboxyl group.
[0022] The carboxyl group equivalent of the acrylonitrile-butadiene copolymer having a carboxyl group is preferably 1000 to 20000. When the carboxyl group equivalent is within the above range, the peel strength and the shear strength are improved, and the copolymer can be suitably used in a polishing process. Here, the carboxyl group equivalent is calculated from the number average molecular weight of the acrylonitrile-butadiene copolymer.
[0023] For example, acrylonitrile-butadiene copolymer has a Mooney viscosity of 50 to 110 M as specified in JIS K6300-1 (Unvulcanized rubber - Physical properties - Part 1: Determination of viscosity and scorch time using a Mooney viscometer). 1+4 (100° C.) When the Mooney viscosity is within the above range, both the peel strength and the shear strength are achieved, and the composition can be suitably used in a polishing process.
[0024] For measuring the Mooney viscosity, an L-type rotor is usually used, but an S-type rotor may be used for high viscosity. Heating may be performed, for example, after 1 minute of preheating and 4 minutes after the start of rotation.
[0025] The acrylonitrile content in the acrylonitrile-butadiene copolymer (hereinafter sometimes referred to as "AN content") is, for example, preferably 5 to 50 mass%, more preferably 10 to 40 mass%. When the AN content is within the above range, both the peel strength and the shear strength are achieved, and the copolymer can be suitably used in the polishing process.
[0026] The proportion of acrylonitrile-butadiene copolymer contained in the adhesive layer 11 (hereinafter sometimes referred to as "NB proportion") is not particularly limited, but the NB proportion is preferably 5 to 80 mass%, more preferably 20 to 70 mass%, and even more preferably 30 to 45 mass%. When the NB proportion is within the above range, both peel strength and shear strength are achieved, and the adhesive layer 11 can be suitably used in the polishing process.
[0027] The phenolic resin may be a compound obtained by condensing a compound having a phenolic hydroxyl group (hereinafter sometimes referred to as a "phenolic compound") with formaldehyde. The phenolic resin may be a novolac type phenolic resin or a resol type phenolic resin, or these may be used in combination.
[0028] The phenol compound used in the phenol resin is not particularly limited, but examples thereof include unsubstituted phenol (also known as hydroxybenzene), cresol, p-tert-butylphenol, bisphenol A, and the like.
[0029] The proportion of phenolic resin contained in the adhesive layer 11 (hereinafter sometimes referred to as "PF proportion") is not particularly limited, but is preferably 10 to 45 mass %, more preferably 15 to 40 mass %. When the PF proportion is within the above range, both peel strength and shear strength are achieved, and the adhesive layer 11 can be suitably used in a polishing process. The proportion of novolac-type phenolic resin and resol-type phenolic resin in the phenolic resin is also not particularly limited, and can be set appropriately.
[0030] The adhesive layer 11 may be composed of only the maleimide compound, the acrylonitrile-butadiene copolymer, and the phenol resin, or may contain other optional components. For example, the adhesive layer 11 may contain a diamine compound.
[0031] The melt viscosity of the adhesive layer 11 at the time when the temperature of the adhesive layer 11 reaches 100° C. by heating the adhesive layer 11 from 25° C. at a rate of 3° C. / min is 1.0×10 2 ~1.0×10 7 Pa s is preferred, and 1.0×10 3 ~1.0×10 6 It is more preferable that the melt viscosity is in the above range, since both the peel strength and the shear strength are satisfied, the composition can be suitably used in a polishing process.
[0032] The melt viscosity may be measured using a DMA (dynamic viscoelasticity device) in accordance with JIS K 7244-10 (Plastics - Test methods for dynamic mechanical properties - Part 10: Complex shear viscosity using a parallel plate oscillatory rheometer).
[0033] The thickness of the adhesive layer 11 is not particularly limited, but is preferably, for example, 5 to 80 μm. If the adhesive layer 11 is too thin, the peel strength and shear strength may decrease. If the adhesive layer 11 is too thick, the adhesive layer 11 may protrude outward during bonding, causing contamination of the polished object and the polishing device.
[0034] The separators 12 and 13 are not particularly limited, but are preferably release sheets whose base material is a polyester resin such as polyethylene terephthalate (PET), or an olefin resin such as polypropylene (PP) or polymethylpentene.
[0035] To use the adhesive sheet 10 for the polishing process in the polishing process, the separators 12, 13 are peeled off and the adhesive layer 11 is applied between the first and second adherends. For example, one of the separators 12, 13 may be peeled off and the adhesive layer 11 may be attached to the first adherend, and then the remaining separator 12, 13 may be peeled off and the adhesive layer 11 may be attached to the second adherend.
[0036] The first and second adherends are not particularly limited, but one adherend may be a grindstone and the other adherend may be a fixed base that supports the grindstone. One adherend may be a workpiece to be polished by the grindstone and the other adherend may be a fixed base that supports the workpiece.
[0037] The material of the grindstone is not particularly limited, but may be a composite material in which abrasive grains such as ceramics are mixed with a binder such as resin. The material of the fixing table is not particularly limited, but may be a metal such as stainless steel (SUS).
[0038] Although the present invention has been described above based on the preferred embodiment, the present invention is not limited to the above embodiment, and various modifications can be made without departing from the gist of the present invention. Modifications include addition, substitution, omission, and other changes to components in the embodiment.
[0039] In addition, it is possible to appropriately select the configurations considered to be preferred in the above-mentioned embodiments and combine any two or more configurations. However, the word "preferable" in this specification is not intended to limit the configurations to those considered to be preferred. EXAMPLES
[0040] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.
[0041] (Examples 1 to 14) Using the materials shown in "Composition of adhesive layer" in Table 1, adhesive layers containing a compound containing two or more maleimide groups, an acrylonitrile-butadiene copolymer, and a phenolic resin and having the thickness shown in Table 1 were produced. The materials used for the adhesive layer are as follows.
[0042] "NB1" has a Mooney viscosity of 70M 1+4 (100℃), AN content 27%, carboxyl group equivalent weight 1400, acrylonitrile-butadiene copolymer. "NB2" is Mooney viscosity 100M 1+4 (100℃), AN content 27%, carboxyl group equivalent weight 1400, acrylonitrile-butadiene copolymer.
[0043] "PF1" is a resol type phenolic resin (product name CKM-1282, manufactured by Aica Kogyo Co., Ltd.). "PF2" is a novolac type phenolic resin (product name CKM-2400, manufactured by Aica Kogyo Co., Ltd.).
[0044] "MI1" is compound (1) described above, i.e., bis(4-maleimidophenyl) ether of bisphenol A. "MI2" is the compound (2) above, i.e., bis(3-ethyl-4-maleimido-5-methylphenyl)methane.
[0045] The "NB ratio," "PF ratio," and "MI ratio" shown in Table 1 are the ratios of the acrylonitrile-butadiene copolymer, phenolic resin, and maleimide compound contained in the adhesive layer, respectively.
[0046] The acrylic adhesive used in Comparative Example 1 is an adhesive using 100 parts by mass of a polymer constituted by a monomer composition containing alkyl acrylate as a main component, and 0.1 parts by mass of an isocyanate curing agent. Comparative Example 1 "Polymer" is an acrylic polymer (product name Finetack (registered trademark) CT-6030, manufactured by DIC Corporation). The "curing agent" is an isocyanate curing agent (product name Burnock (registered trademark) DN, manufactured by DIC Corporation).
[0047] (Preparation of adhesive sheet) An adhesive solution was prepared by dissolving each material in tetrahydrofuran according to the "Adhesive Layer Composition" in Table 1. The obtained adhesive solution was applied to a separator (PET substrate) so that the adhesive layer after drying had a thickness shown in Table 1. After drying for 5 minutes at 160°C in a hot air circulation dryer, the separator was attached to the adhesive layer to obtain adhesive sheets of Examples 1 to 14 and Comparative Example 1.
[0048] (Method of measuring melt viscosity) The adhesive sheets of Examples 1 to 7, 12 to 14 and Comparative Example 1 obtained above (Production of Adhesive Sheet) were laminated to an adhesive layer thickness of 500 μm to obtain test pieces. Using the above test piece, the viscosity at the time when the temperature reached 100° C. by heating from 25° C. at a rate of 3° C. / min was taken as the “melt viscosity”. Measurement equipment: HAAKE MARS I type rheometer Thermo Fischer Scientific Frequency: 1Hz
[0049] The adhesive sheets of Examples 8 to 11 had the same adhesive layer composition as that of Example 1 (only the thickness was different), so the results of the adhesive sheet of Example 1 were used. q ” (p is a number between 1 and 10, and q is an exponent) is expressed as “pEq”.
[0050] (Method of measuring peel strength) The separator on one side of the adhesive sheet obtained above (preparation of adhesive sheet) was peeled off, and the sheet was heated and pressed to a plasma surface-treated polyimide film (75 μm thick) at 100 ° C, 0.2 MPa, and 10 seconds, and then cut into a width of 10 mm to obtain an adhesive tape. The separator of the obtained adhesive tape was peeled off, and the sheet was heated and pressed to an adherend under conditions of 100 ° C, 0.2 MPa, and 10 seconds, and then heated at 175 ° C for 60 minutes in a hot air circulation dryer to thermally cure the adhesive layer. Thereafter, the 90 ° tape peel strength was measured at a peel speed of 50 mm / min under conditions of 23 ° C, and the obtained value was taken as "peel strength".
[0051] (Method of measuring shear strength) The adhesive sheet obtained above (Preparation of adhesive sheet) was cut to 5 mm x 5 mm, the separators on both sides were peeled off, and the adhesive layer was sandwiched between two adherends of the same type, heated and pressed at 100°C, 0.2 MPa, and 10 seconds, and then heated at 175°C for 60 minutes in a hot air circulation dryer to thermally cure the adhesive layer. The value obtained at 23°C and a shear rate of 50 mm / min was taken as the "shear strength".
[0052] (Method of measuring overhang amount) The separator on one side of the adhesive sheet obtained above (preparation of adhesive sheet) was peeled off, and the sheet was heated and pressed to a plasma surface-treated polyimide film (75 μm thick) at 100° C., 0.2 MPa, and 10 seconds, and then cut to a width of 10 mm to obtain an adhesive tape. The separator of the obtained adhesive tape was peeled off, and the sheet was heated and pressed to an adherend at 100° C., 0.2 MPa, and 10 seconds, and then heated at 175° C. for 60 minutes in a hot air circulation dryer to thermally cure the adhesive layer. The maximum protruding width of the adhesive layer in the width direction was measured and recorded as the "protruding amount."
[0053] (adherent) Three types of grindstones were used as adherends. The numbers marked with # indicate roughness (grain size of abrasive grains). Wheel A is a #2400 grit wheel made of green silicon carbide grit and a vitrified bond. Wheel B is a #1200 grit wheel made of green silicon carbide abrasive grains and a vitrified bond. Wheel C is a #120 grit wheel made of green silicon carbide abrasive grains and a vitrified bond.
[0054] (Evaluation criteria for peel strength) The peel strength was measured for grinding wheels A, B, and C, and evaluated according to the following criteria. Excellent (3): Peel strength is 10N / 10mm or more. Good (2): Peel strength is 6N / 10mm or more and 9N / 10mm or less. Acceptable (-1): Peel strength is 3N / 10mm or more and less than 6N / 10mm. Unacceptable (-2): The peel strength is less than 3N / 10mm.
[0055] (Shear strength evaluation criteria) The shear strength was measured for Grinding Wheel B and Grinding Wheel C and evaluated according to the following criteria. Excellent (3): Shear strength is 12N / mm 2 That's all. Good (2): Shear strength is 6N / mm 2 More than 12N / mm 2 is less than. Acceptable (-1): Shear strength is 3N / mm 2 More than 6N / mm 2 is less than. Unacceptable (-2): Shear strength is 3N / mm 2 is less than.
[0056] (Evaluation criteria for overhang amount) The amount of overhang was measured for grinding wheel A and evaluated according to the following criteria. Good (2): The amount of overhang is 50 μm or less. Acceptable (-1): The amount of overhang is more than 50 μm and 150 μm or less. Unacceptable (-2): The amount of protrusion is more than 150 μm.
[0057] (Evaluation criteria for overall evaluation) The overall evaluation was based on the combined results of the six individual evaluations above, and was assessed according to the following criteria. Excellent: The combined value is 15 or more. Good: The combined value is 10 or more and less than 15. Passable: The combined value is 5 or more and less than 10. Failed: The combined value is less than 5.
[0058] The above results are summarized in Table 1.
[0059] [Table 1]
[0060] As shown in Table 1, Examples 1 to 14 were given the overall evaluation of excellent, good, or fair. Comparative Example 1 received an overall rating of "Fail." [Explanation of symbols]
[0061] 10...adhesive sheet for polishing process, 11...adhesive layer, 12, 13...separators.
Claims
1. An adhesive sheet for use in a polishing process, comprising an adhesive layer containing a compound having two or more maleimide groups, an acrylonitrile-butadiene copolymer, and a phenol resin.
2. The adhesive layer was heated from 25° C. at a temperature increase of 3° C. / min to reach 100° C., and the melt viscosity was 1.0×10 3 ~1.0 x 10 6 2. The adhesive sheet for use in a polishing process according to claim 1, characterized in that it has a viscosity of Pa·s.
3. 2. The adhesive sheet for use in a polishing process according to claim 1, wherein the adhesive layer has a thickness of 5 to 80 μm.
4. 2. The adhesive sheet for use in a polishing process according to claim 1, characterized in that the adhesive layer contains at least one of the following compound (1) or the following compound (2) as the compound containing two or more maleimide groups: 【Chemistry 1】 【Chemistry 2】
5. 2. The adhesive sheet for use in a polishing process according to claim 1, wherein the content of the acrylonitrile-butadiene copolymer in the adhesive layer is 20 to 70 mass %.
Citation Information
Patent Citations
Abrasive
JP1997235384A
Double-coated pressure-sensitive adhesive tape
JP2000309760A
Adhesive sheet for sound absorption and shock buffering, saw blade using the same and method for producing the same
JP2001106997A
Pressure-sensitive adhesive sheet for fastening polishing pad
JP2015078348A
Adhesive for fixing abrasive member, adhesive sheet for fixing abrasive member, and abrasive member laminate
JP2018065982A