Air filter medium, filter pack, air filter unit, and method for manufacturing air filter medium
The air filter medium uses core-sheath structural fibers in support materials to minimize pressure loss and maintain high collection efficiency by stabilizing the fluororesin porous membrane, addressing thermal fusion-induced issues in conventional filters.
Patent Information
- Application Number
- JP2023044461
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional air filters using heat-sealed fluororesin porous membranes and support materials experience increased pressure loss due to changes in fiber structure during thermal fusion, necessitating a solution to suppress this increase.
The air filter medium incorporates a fluororesin porous membrane supported by core-sheath structural fibers in the support materials, with specific fabric weight and fiber cross-sectional area ratios to minimize thermal fusion-induced pressure loss, and optionally includes a second support material for enhanced stability and protection.
The solution effectively suppresses pressure loss and maintains low pressure drop while ensuring high collection efficiency and protection against static electricity, allowing for easy deformation into pleated shapes.
Smart Images

Figure 2024134255000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to air filter media, filter packs, air filter units, and methods of manufacturing air filter media. [Background technology]
[0002] Conventionally, for example, a porous film made of polytetrafluoroethylene (hereinafter, sometimes referred to as PTFE) (hereinafter, sometimes referred to as PTFE porous film) has been used as an air filter. The PTFE porous film is thin and may have difficulty in maintaining its shape by itself, so it is used as a filter medium in a state where it is laminated with an air-permeable support material.
[0003] For example, Patent Document 1 (JP Patent Publication No. 2002-66226 A) proposes an air filter medium obtained by heat-sealing a relatively soft nonwoven fabric to a PTFE porous membrane. DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0004] Here, in the air filter medium obtained by heat fusing fluororesin porous membrane and supporting material, fiber structure may change during heat fusing.Therefore, the pressure loss of the air filter medium obtained by heat fusing may be greater than the pressure loss of the filter medium that is simply laminated before heat fusing fluororesin porous membrane and supporting material.Therefore, it is desired to suppress the increase in the pressure loss of the air filter medium caused by heat fusing. [Means for solving the problem]
[0005] The air filter medium according to a first aspect includes a fluororesin porous membrane and a first support material. The first support material supports the fluororesin porous membrane. The fluororesin porous membrane and the first support material are heat-sealed. The first support material has core-sheath structure fibers including a first core portion and a first sheath portion having a lower melting point than the first core portion. The first support material satisfies the following formula: Basis weight (g / m 2) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 )×thickness(cm)×1000000}≦380(m / cm 3 ).
[0006] In addition, if the air filter medium further includes a second support material and the fluororesin porous membrane is disposed between the first support material and the second support material, the above values of both the first support material and the second support material are 380 (m / cm 3 In this case, the first support material and the second support material may have the same physical properties or different physical properties.
[0007] The fluororesin porous membrane may be composed of one porous membrane, or may be composed of a plurality of porous membranes, such as two porous membranes.
[0008] This air filter medium is able to minimize an increase in pressure loss, compared to a filter medium in which the first support material is simply layered on the fluororesin porous membrane and is not thermally bonded to the two.
[0009] The air filter medium according to a second aspect is the air filter medium according to the first aspect, further comprising a second support material supporting the fluororesin porous membrane. The fluororesin porous membrane is located between the first support material and the second support material. The fluororesin porous membrane and the second support material are heat-sealed. The second support material has core-sheath structure fibers including a second core portion and a second sheath portion having a lower melting point than the second core portion. The second support material satisfies the following formula. Formula: basis weight (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 )×thickness(cm)×1000000}≦380(m / cm 3 ).
[0010] This air filter medium is able to minimize an increase in pressure loss, compared to a filter medium in which the second support material is simply layered on the fluororesin porous membrane and is not thermally bonded to the two.
[0011] An air filter medium according to a third aspect is the air filter medium according to the first or second aspect, and has a dielectric breakdown voltage of 0.8 kV or more.
[0012] This air filter medium can protect the fluororesin porous membrane from static electricity and minimize damage to the fluororesin porous membrane.
[0013] An air filter medium according to a fourth aspect is the air filter medium according to any one of the first aspect to the third aspect, and has a thickness of 350 μm or more and 1000 μm or less.
[0014] This air filter medium can physically protect the fluororesin porous membrane, and can be easily deformed, for example, into a pleated shape.
[0015] An air filter medium according to a fifth aspect is the air filter medium according to any one of the first to fourth aspects, and has a PF value of 20 or more. The PF value is determined by the formula: PF value={-log((100-collection efficiency (%)) / 100)} / (pressure loss (Pa) / 1000). The PF value is calculated using the pressure loss when air is passed through the air filter medium at a flow rate of 5.3 cm / sec, and the collection efficiency of the air filter medium ascertained using NaCl particles with a particle diameter of 0.1 μm.
[0016] When a relatively high-performance fluororesin porous membrane is used, the degree of increase in pressure loss due to heat fusion of the first support material tends to be particularly large. Even in this case, this air filter medium makes it possible to keep the degree of increase in pressure loss due to heat fusion of the first support material small.
[0017] An air filter medium according to a sixth aspect is the air filter medium according to any one of the first aspect to the fifth aspect, wherein the basis weight of the first support material is 25 g / m 2 More than 60g / m 2 The following is the result.
[0018] This air filter medium can easily provide a first support material that is likely to suppress an increase in pressure loss caused by heat fusion to the fluororesin porous membrane.
[0019] An air filter medium according to a seventh aspect is the air filter medium according to any one of the first aspect to the sixth aspect, in which the average fiber diameter of the first support material is 23 μm or more.
[0020] This air filter medium can easily provide a first support material that is likely to suppress an increase in pressure loss caused by heat fusion to the fluororesin porous membrane.
[0021] A filter pack according to an eighth aspect is an air filter medium according to any one of the first to seventh aspects, which is folded so as to produce mountain folds and valley folds. This filter pack makes it possible to keep pressure loss low.
[0022] An air filter unit according to a ninth aspect includes the air filter medium according to any one of the first to seventh aspects, or a pleated air filter medium according to any one of the first to seventh aspects that is folded so as to produce mountain folds and valley folds, and a frame. The frame holds the air filter medium or the pleated air filter medium.
[0023] This air filter unit makes it possible to keep pressure loss low.
[0024] A method for producing an air filter medium according to a tenth aspect includes the steps of preparing a fluororesin porous membrane, preparing a first support material, and heat fusing the fluororesin porous membrane and the first support material. The first support material to be prepared has a core-sheath structure fiber including a first core portion and a first sheath portion having a lower melting point than the first core portion. The first support material to be prepared satisfies the following formula. Formula: basis weight (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 )×thickness(cm)×1000000}≦380(m / cm 3)
[0025] According to this manufacturing method of the air filter medium, the first support material to be heat-sealed to the fluororesin porous membrane is made of the material having the above-mentioned specific physical properties. Therefore, it is possible to obtain an air filter medium that can suppress the increase in pressure loss to a small extent, compared to a filter medium in which the first support material is simply layered on the fluororesin porous membrane and is not heat-sealed to each other. [Brief description of the drawings]
[0026] [Figure 1] FIG. 2 is a schematic cross-sectional view showing the layer structure of the air filter medium (No. 1). [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the layer structure of the air filter medium (No. 2). [Diagram 3] FIG. 2 is a schematic cross-sectional view showing the layer structure of the air filter medium (No. 3). [Figure 4] FIG. 2 is a schematic configuration diagram of a side view of an apparatus for performing longitudinal stretching. [Diagram 5] FIG. 2 is a schematic configuration diagram of a side view of an apparatus for performing width direction stretching. [Figure 6] FIG. 2 is a schematic perspective view of an apparatus for performing widthwise stretching. [Figure 7] FIG. 2 is a schematic external perspective view of the filter pack. [Figure 8] FIG. 2 is a schematic external perspective view of the air filter unit. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, an air filter medium (hereinafter also simply referred to as a filter medium), a filter pack, an air filter unit, and a manufacturing method of an air filter medium will be described with reference to examples.
[0028] (1) Air filter media The air filter medium includes a fluororesin porous membrane and a support material. The support material is heat-sealed to the fluororesin porous membrane in a state where the support material is laminated in the thickness direction of the membrane.
[0029] The layer structure of the air filter medium is not particularly limited, and may be, for example, an air filter medium 30 shown in Fig. 1, in which a fluororesin porous membrane 31 and a first support material 32 are laminated in the air flow direction. The first support material 32 may be provided on the leeward side of the fluororesin porous membrane 31 as shown in Fig. 1, or may be provided on the windward side of the fluororesin porous membrane 31 as shown in Fig. 2. In addition, the air filter medium may be provided with a first support material 32 laminated on the fluororesin porous membrane 31 in the air flow direction, and a second support material 33 laminated on the opposite side of the first support material 32 side of the fluororesin porous membrane 31 as shown in Fig. 3, and the fluororesin porous membrane 31 may be supported from both the leeward side and the windward side.
[0030] The pressure loss of the air filter medium may be, for example, 250 Pa or less, preferably 200 Pa or less. The pressure loss of the air filter medium is not particularly limited, but may be 50 Pa or more. The pressure loss of the air filter medium can be measured as the pressure loss when air is passed through the air filter medium at a flow rate of 5.3 cm / sec.
[0031] The air filter medium may have a particle collection efficiency of 99.00% or more, and preferably 99.99% or more, when air containing NaCl particles having a particle size of 0.1 μm is passed through it at a flow rate of 5.3 cm / sec.
[0032] As the air filter medium, the PF value determined by the following formula: PF value = {-log ((100-collection efficiency (%)) / 100)} / (pressure loss (Pa) / 1000) using the pressure loss and collection efficiency grasped using NaCl particles with a particle diameter of 0.1 μm is preferably 20 or more, more preferably 21 or more. The PF value of the air filter medium is mainly determined by the performance of the fluororesin porous membrane, but when a relatively high-performance fluororesin porous membrane with a high PF value is used in the air filter medium, the increase in pressure loss due to the heat fusion of the first support material and / or the second support material to the fluororesin porous membrane tends to be large. Even in this case, by using the above-mentioned specified first support material and / or the second support material, it is possible to suppress the increase in pressure loss due to heat fusion.
[0033] The thickness of the air filter medium is, for example, preferably 350 μm or more, more preferably 380 μm or more. This makes it easy to ensure the sufficient thickness of the first support material and / or the second support material for protecting the fluororesin porous membrane, and makes it possible to physically protect the fluororesin porous membrane. When the air filter medium is used in a state where it has a folded part, the thickness is, for example, preferably 1000 μm or less, more preferably 750 μm or less, from the viewpoint of suppressing the thickness of the folded part from becoming too large. By preventing the thickness of the air filter medium from becoming too large, it becomes easy to deform when deforming into a pleated shape or the like. The thickness of the air filter medium is the thickness value when a load of 0.3 N is applied to the measurement target in a specific measurement device. For example, a thickness gauge (1D-110MH type, manufactured by Mitutoyo Corporation) is used to measure the total thickness by stacking five measurement targets, and the value is divided by 5 to obtain the thickness of one sheet.
[0034] The dielectric breakdown voltage of the air filter medium is preferably 0.8 kV or more, more preferably 0.85 kV or more. By ensuring sufficient dielectric breakdown voltage, the damage caused by static electricity to the fluororesin porous membrane is suppressed, and the occurrence of leakage is suppressed.
[0035] (2) Fluorine resin porous membrane The fluororesin porous membrane is preferably mainly composed of fluororesin and has a porous membrane structure having fibrils and nodes connected to the fibrils. Here, "mainly" means that when a plurality of kinds of components are contained, the fluororesin is contained in the largest amount. The fluororesin porous membrane may contain, for example, 50% by weight or more of fluororesin relative to the weight of the fluororesin porous membrane, preferably 80% by weight or more of fluororesin, more preferably 95% by weight or more of fluororesin, or may be composed of only fluororesin.
[0036] An example of a component different from the fluororesin contained in the fluororesin porous membrane is an inorganic filler which is a non-melt processable component that does not become fibrous.
[0037] The fluororesin used in the fluororesin porous membrane may be composed of one kind of component, or may be composed of two or more kinds of components. In addition, the fluororesin may be, for example, one containing fibrous PTFE. In addition, the fluororesin may be a mixture of three components: fibrous PTFE, non-fibrous non-thermal melt processable component, and non-fibrous non-thermal melt processable component with a melting point of less than 320°C.
[0038] The PTFE that can be made into a fiber is a high molecular weight PTFE obtained by emulsion polymerization or suspension polymerization of tetrafluoroethylene (TFE). The term "high molecular weight" as used herein means that the PTFE is easily made into a fiber during stretching in the production of a porous membrane, and that the fibrils having a long fiber length can be obtained. The molecular weight has a standard specific gravity (SSG) of 2.130 to 2.230 and a high melt viscosity so that the PTFE does not melt and flow substantially. Whether or not the PTFE can be made into a fiber can be determined by whether or not paste extrusion, which is a typical method for molding a high molecular weight PTFE powder made from a polymer of TFE, is possible. If the unsintered molded body obtained by paste extrusion has no substantial strength or elongation, for example, if the elongation is 0% and it breaks when pulled, it can be considered that the PTFE has no fiber-making property. The high molecular weight PTFE may be modified polytetrafluoroethylene, homopolytetrafluoroethylene, or a mixture of modified PTFE and homoPTFE.
[0039] Examples of non-thermal melt processable components that do not form fibers include components with thermoplastic properties such as low molecular weight PTFE, thermosetting resins, inorganic fillers, and mixtures of these. Low molecular weight PTFE has a number average molecular weight of 600,000 or less, a melting point of 320°C to 335°C, and a melt viscosity at 380°C of 100 Pa·s to 7.0×10 5 It is PTFE with a viscosity of Pa·s.
[0040] The non-fibrous heat melt processable component with a melting point of less than 320°C preferably has a melt viscosity of less than 10000 Pa·s at 380°C. The melting point of the non-fibrous heat melt processable component is the peak top of the heat of fusion curve obtained by heating the component to above the melting point at a heating rate of 10°C / min using a differential scanning calorimeter (DSC), melting it completely once, cooling it to below the melting point at a heating rate of 10°C / min, and then heating it again at a heating rate of 10°C / min.
[0041] These fibrous PTFE, non-fibrous non-thermal melt processable components, and non-fibrous non-thermal melt processable components having a melting point of less than 320 ° C. may be those described in detail in, for example, International Publication No. WO 2020 / 067182.
[0042] In addition, the manufacturing method of the fluororesin porous membrane is to use fine powder obtained by coagulation and co-coagulation from emulsion polymerization of TFE, and after dehydration and drying, mix with liquid lubricant (extrusion aid) and perform paste extrusion to obtain sheet-like extrudate. The sheet-like extrudate is rolled with a calendar roll or the like to obtain an unsintered film, from which the liquid lubricant is removed and stretched to obtain a fluororesin porous membrane.
[0043] The fluororesin porous membrane thus obtained has a pressure loss of 250 Pa or less, and preferably 200 Pa or less, when air is passed through it at a flow rate of 5.3 cm / sec. The pressure loss of the fluororesin porous membrane is not particularly limited, but may be 50 Pa or more, or may be 80 Pa or more.
[0044] The fluororesin porous membrane may have a particle collection efficiency of 99.00% or more, and preferably 99.99% or more, when air containing NaCl particles with a particle diameter of 0.1 μm is passed through it at a flow rate of 5.3 cm / sec.
[0045] The PF value of the fluororesin porous membrane is not less than 20, and more preferably not less than 21. The PF value is determined by the following formula, PF value={-log((100-collection efficiency(%)) / 100)} / (pressure loss(Pa) / 1000), using the pressure loss and collection efficiency determined using NaCl particles with a particle diameter of 0.1 μm.
[0046] The thickness of the fluororesin porous film can be, for example, 1.0 μm or more, and is preferably 3.0 μm or more. By increasing the film thickness of the fluororesin porous film, it is possible to increase the dust amount. The film thickness of the fluororesin porous film is, for example, 100 μm or less, and is preferably 50.0 μm or less. The thickness of the fluororesin porous film can be determined, for example, by using a film thickness meter (1D-110MH type, manufactured by Mitutoyo Corporation) to measure the total film thickness by stacking five measurement objects, and dividing the measured value by 5 to obtain the film thickness of one film.
[0047] The average fiber diameter of the fluororesin porous membrane may be, for example, 0.01 μm or more, preferably 0.05 μm or more, and more preferably 0.08 μm or more. The average fiber diameter of the fluororesin porous membrane may be, for example, 0.5 μm or less, preferably 0.25 μm or less, and more preferably 0.2 μm or less. The average fiber diameter may be calculated as the number average fiber diameter by randomly selecting 50 fibers from the image of the scanning electron microscope photograph.
[0048] (3) Support material The fluororesin porous membrane is supported by laminating the support material. Therefore, even if the fluororesin porous membrane is difficult to stand on its own due to its thin thickness, the support material makes it possible to make the fluororesin porous membrane stand upright. In addition, the strength of the air filter medium is ensured, and even if it is folded into a specific shape, the shape is easily maintained. The support material may be only a first support material laminated on one side of the fluororesin porous membrane in the air flow direction, or may further include a second support material laminated on the opposite side of the first support material side in the air flow direction to the fluororesin porous membrane. The material of the support material is not particularly limited, but examples thereof include nonwoven fabric, woven fabric, etc. Here, the nonwoven fabric is preferably, for example, a spunbond nonwoven fabric.
[0049] (3-1) First support material The air filter medium includes a first support material disposed on either the upstream side or the downstream side of the fluororesin porous membrane in the airflow direction. The first support material has a first core-sheath structure fiber including a first core and a first sheath having a lower melting point than the first core. When the first support material is heat-sealed to the fluororesin porous membrane, at least a portion of the first sheath having a lower melting point than the first core is melted to heat-seal the fluororesin porous membrane and the first support material.
[0050] Here, when comparing the pressure loss of a filter medium in which the fluororesin porous membrane and the first support material are simply laminated without being heat-sealed to each other, with the pressure loss of an air filter medium obtained by heat-sealing the first support material to the fluororesin porous membrane, it is known that the air filter medium obtained by heat-sealing the fluororesin porous membrane and the first support material has a larger pressure loss due to changes in the fiber structure caused by heat fusion. Then, the inventors have made intensive studies to suppress the increase in pressure loss during the heat fusion, and have newly found that the fewer the contact points between the fluororesin porous membrane and the first support material, the more the increase in pressure loss due to heat fusion can be suppressed. Through further studies, the inventors have found that it is preferable to use a first support material with a short average total fiber length per unit volume as the first support material used by heat-sealing the fluororesin porous membrane in the air filter medium. The average total fiber length per unit volume is determined by the basis weight (g / m 2 ) and the average fiber cross-sectional area (cm 2 ) and material specific gravity (g / cm 3 ) and thickness (cm), this can be expressed by the following Equation 1. Formula 1: Weight per unit area (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 )×thickness(cm)×1000000}
[0051] The inventors have also found that, from the viewpoint of suppressing an increase in pressure loss of the resulting air filter medium, it is preferable for the average total fiber length per unit volume in the first support material to satisfy the following formula 2. Formula 2: Weight per unit area (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 )×thickness(cm)×1000000}≦380(m / cm 3 )
[0052] The first support material has a value calculated by the above formula 2 of 350 (m / cm 3 ) or less, and 300 (m / cm 3 ) or less is more preferable.
[0053] This allows the number of contact points between the first support material and the fluororesin porous membrane to be reduced, and even when the first sheath portion of the first support material is melted and heat-fused to the fluororesin porous membrane, an increase in pressure loss of the resulting air filter medium is suppressed.
[0054] The melting point of the first core is preferably 30°C or more higher than the melting point of the first sheath, and more preferably 50°C or more higher. This can prevent the entire first support material from melting during heat fusion. Examples of the components of the first core include polyesters such as polyethylene terephthalate (PET) or composites thereof. Examples of the components of the first sheath include polyolefins such as polyethylene (PE) and polypropylene (PP), polyamide (PA), or composites thereof. The combination of the components of the first core and the first sheath is not particularly limited, and may be, for example, a polyester such as polyethylene terephthalate and a polyolefin such as polyethylene for the first core, or a high melting point polyester and a low melting point polyester having a melting point lower than that of the high melting point polyester.
[0055] The first support material preferably has a pressure loss of, for example, 10 Pa or less when air is passed through it at a flow rate of 5.3 cm / sec.
[0056] The first support material may have a particle collection efficiency of 10% or less, and preferably 5% or less, when air containing NaCl particles having a particle diameter of 0.1 μm is passed through it at a flow rate of 5.3 cm / sec.
[0057] The thickness of the first support material is, for example, preferably 500 μm or less, more preferably 300 μm or less. When the fluororesin porous membrane is folded and deformed into a non-flat shape such as a pleated shape, the thickness of the breathable support material is preferably 140 μm or more from the viewpoint of easily maintaining the shape. The thickness of the first support material is preferably 195 μm or more, more preferably 200 μm or more from the viewpoint of ensuring the dielectric breakdown voltage and easily protecting the fluororesin porous membrane from external static electricity.
[0058] The average fiber diameter of the first support material is preferably 23 μm or more, more preferably 25 μm or more, from the viewpoint of reducing the number of contact points with the fluororesin porous membrane. The average fiber diameter of the first support material can be, for example, 50 μm or less, and may be 40 μm or less. The average fiber diameter can be evaluated for fibers present within a predetermined range of an image observed using a microscope or the like, and may be, for example, the number average fiber diameter of 200 fibers.
[0059] The basis weight of the first support material is not particularly limited, and is, for example, 25 g / m 2 More than 60g / m 2 It may be the following:
[0060] The specific gravity of the first support material is not particularly limited and may be, for example, 0.8 or more and 1.4 or less.
[0061] (3-2)Second support material The air filter medium preferably further comprises a second support material arranged on either the upstream side or downstream side of the fluororesin porous membrane in the airflow direction, on the opposite side of the fluororesin to the side on which the first support material is provided. The second support material preferably has a second core-sheath structure fiber including a second core portion and a second sheath portion having a melting point lower than that of the second core portion.
[0062] The value calculated by the above formula for the first support material is 380 (m / cm 3) or less, the value calculated by the above formula for the second supporting material is not particularly limited, but it is preferable that the second supporting material also satisfies the following formula 3. Formula 3: Weight per unit area (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 )×thickness(cm)×1000000}≦380(m / cm 3 )
[0063] The second support material has a value calculated by the above formula 3 of 350 (m / cm 3 ) or less, and 300 (m / cm 3 ) or less is more preferable.
[0064] This reduces the number of contact points between the second support material and the fluororesin porous membrane, and even when the second sheath of the second support material is melted and heat-sealed to the fluororesin porous membrane, the increase in pressure loss of the resulting air filter medium is suppressed. Also, by supporting the fluororesin porous membrane from both sides with the support material, the handleability of the air filter medium is improved.
[0065] The second supporting material is the same as the first supporting material, and the melting point of the second core is preferably 30°C or more higher than the melting point of the second sheath, more preferably 50°C or more higher. This can prevent the entire second supporting material from melting during heat fusion. Examples of the components of the second core include polyesters such as polyethylene terephthalate, or composites thereof. Examples of the components of the second sheath include polyolefins such as polyethylene and polypropylene, polyamides, or composites thereof. The combination of the components of the second core and the second sheath is not particularly limited, and may be, for example, a polyester such as polyethylene terephthalate and a polyolefin such as polyethylene for the second core, or a high melting point polyester and a low melting point polyester having a melting point lower than that of the high melting point polyester.
[0066] The second support material preferably has a pressure loss of, for example, 10 Pa or less when air is passed through it at a flow rate of 5.3 cm / sec.
[0067] The second support material may have a particle collection efficiency of 10% or less, and preferably 5% or less, when air containing NaCl particles having a particle diameter of 0.1 μm is passed through it at a flow rate of 5.3 cm / sec.
[0068] The thickness of the second support material is, for example, preferably 500 μm or less, more preferably 300 μm or less. When the fluororesin porous membrane is folded and deformed into a non-flat shape such as a pleated shape, the thickness of the breathable support material is preferably 140 μm or more from the viewpoint of easily maintaining the shape. The thickness of the second support material is preferably 195 μm or more, more preferably 200 μm or more from the viewpoint of ensuring the dielectric breakdown voltage and easily protecting the fluororesin porous membrane from external static electricity.
[0069] The average fiber diameter of the second supporting material is preferably 23 μm or more, more preferably 25 μm or more, from the viewpoint of reducing the number of contact points with the fluororesin porous membrane. The average fiber diameter of the second supporting material can be, for example, 50 μm or less, and may be 40 μm or less. The average fiber diameter can be evaluated for fibers present within a predetermined range of an image observed using a microscope or the like, and may be, for example, the number average fiber diameter of 200 fibers.
[0070] The basis weight of the second support material is not particularly limited, and is, for example, 25 g / m 2 More than 60g / m 2 It may be the following:
[0071] The specific gravity of the second support material is not particularly limited and may be, for example, 0.8 or more and 1.4 or less.
[0072] (4) Bonding of fluororesin porous membrane and supporting material, etc. The procedure for the stretching step of the fluororesin porous membrane and the subsequent steps of bonding to a support material will be described below.
[0073] A fluororesin sheet that has been wound into a roll or the like can be stretched using, for example, the device shown in FIG. 4 and the devices shown in FIGS.
[0074] In the device shown in Fig. 4, a fluororesin sheet wound in a roll shape is set as roll 41, and the longitudinally stretched sheet stretched in the longitudinal direction (longitudinal direction) is wound up on take-up roll 42. Note that 43 to 45 are rolls, 46 and 47 are heat rolls, and 48 to 52 are rolls, respectively.
[0075] Next, the longitudinally stretched sheet is stretched in the width direction by the device shown in FIG. 5 and FIG. 6. Specifically, the wound longitudinally stretched sheet is set on a roll 61, and while being sequentially sent out, is stretched in the width direction by a tenter 65. In the tenter 65, both ends of the stretched sheet in the width direction are held by opposing continuous clips (not shown), and the opposing continuous clips move away from each other while the stretched sheet is sent out, thereby stretching the sheet in the width direction. The continuous clips are configured to be sent from the upstream side to the downstream side along a line that can be adjusted to a specific shape. The tenter 65 can preheat the stretched sheet in the preheating region 62 on the upstream side, stretch the stretched sheet in the width direction in the intermediate stretching region 63 while heating the sheet to a predetermined temperature, and heat-set the stretched sheet in the heat-setting region 64 on the downstream side. The fluororesin porous membrane 31 that has been heat-fixed is then layered on a first support material 32 and, if necessary, a second support material 33, and thermally laminated using a combination of a heated hot plate and an opposing plate of a hot press device or a pair of heating rolls 66, etc., to become an air filter medium 30, which is then wound up around a roll 67.
[0076] The first sheath of the first support material 32 and the second sheath of the second support material 33 are partially melted when heated by a combination or pair of plates facing the heated hot plate of the hot press device or by the heating roll 66, and adhere to the fluororesin porous membrane 31. In this manner, the first support material 32 and the second support material 33 are heat-fused to the fluororesin porous membrane 31, thereby obtaining the air filter medium 30.
[0077] (5) Filter pack Next, the filter pack of this embodiment will be described with reference to FIG.
[0078] FIG. 7 is an external perspective view of the filter pack 20 of the present embodiment.
[0079] The filter pack 20 includes the air filter medium (for example, the air filter medium 30) described above. The air filter medium of the filter pack 20 is a processed filter medium that has been processed (pleated) into a zigzag shape in which mountain folds and valley folds are alternately repeated. The pleating can be performed, for example, by a rotary folding machine. The folding width of the filter medium is not particularly limited, but is, for example, 25 mm or more and 280 mm or less. Since the filter pack 20 is pleated, the folding area of the filter medium can be increased when used in an air filter unit, and thus an air filter unit with high collection efficiency can be obtained.
[0080] In addition to the filter medium, the filter pack 20 may further include a spacer (not shown) for maintaining the pleat interval when used in an air filter unit. The material of the spacer is not particularly limited, but a hot melt resin can be preferably used. In addition, the air filter medium 30 may have a plurality of embossed protrusions, and the pleat interval may be maintained by the embossed protrusions.
[0081] (6) Air filter unit Next, the air filter unit 1 will be described with reference to FIG.
[0082] FIG. 8 is an external perspective view of the air filter unit 1 of the present embodiment.
[0083] The air filter unit 1 includes the air filter medium or filter pack described above, and a frame 25 that holds the air filter medium or filter pack. The air filter unit may be produced so that a filter medium that is not folded in peaks or valleys is held in the frame, or so that the filter pack 20 is held in the frame 25. The air filter unit 1 shown in FIG. 8 is produced using the filter pack 20 and the frame 25.
[0084] Frame 25 is made, for example, by combining plate materials or by molding resin, and the gap between filter pack 20 and frame 25 is preferably sealed with a sealant. The sealant is for preventing leakage between filter pack 20 and frame 25, and is made of, for example, epoxy, acrylic, urethane, or other resin.
[0085] The air filter unit 1, which is equipped with a filter pack 20 and a frame body 25, may be a mini-pleat type air filter unit in which one filter pack 20 extending in a flat plate shape is held inside the frame body 25, or may be a V-bank type air filter unit or a single-header type air filter unit in which a plurality of filter packs extending in a flat plate shape are arranged side by side and held in a frame body.
[0086] (7) Examples of uses The air filter medium, the filter pack, and the air filter unit according to the present embodiment are used, for example, in the following applications.
[0087] ULPA filters (Ultra low Penetration Air Filters) (for semiconductor manufacturing), HEPA filters (for hospitals and semiconductor manufacturing), cylindrical cartridge filters (for industrial use), bag filters (for industrial use), heat-resistant bag filters (for exhaust gas treatment), heat-resistant pleated filters (for exhaust gas treatment), SINBRAN (registered trademark) filters (for industrial use), catalytic filters (for exhaust gas treatment), adsorbent filters (for HDD installation), adsorbent vent filters (for HDD installation), vent filters (for HDD installation, etc.), vacuum cleaner filters (for vacuum cleaners), general-purpose multi-layer felt material, gas turbine cartridge filters (for compatible products for gas turbines), cooling filters (for electronic device housings), etc.
[0088] Freeze-drying materials such as freeze-drying containers, automotive ventilation materials for electronic circuits and lamps, container applications such as container caps, protective ventilation applications for electronic devices, ventilation / internal pressure adjustment applications such as medical ventilation.
[0089] Masks such as flat, pleated, and three-dimensional (to prevent dust, oily smoke, bacteria, viruses, etc. from entering the body through the mouth and nose). EXAMPLES
[0090] The contents of the present disclosure will be specifically described below with reference to examples and comparative examples.
[0091] Example 1 300 g of hydrocarbon oil (IP Solvent 2028, Idemitsu Kosan Co., Ltd.) was added as an extrusion liquid lubricant per 1 kg of PTFE fine powder (Polyflon Fine Powder F106, Daikin Industries, Ltd.) with an average molecular weight of 6.5 million and mixed at 20°C. The mixture was then extruded using a paste extrusion device to obtain a rod-shaped molded body. This rod-shaped molded body was formed into a sheet using a calendar roll heated to 70°C to obtain a fluororesin sheet. The fluororesin sheet was passed through a hot air drying oven at 250°C to evaporate and remove the hydrocarbon oil, and a strip-shaped unsintered fluororesin sheet with an average thickness of 200 μm and an average width of 150 mm was obtained.
[0092] Next, the unsintered fluororesin sheet was stretched in the longitudinal direction at a stretch ratio of 5. The stretching temperature in the longitudinal direction was 250° C. Here, the stretching rate (% / s) in the longitudinal direction was 150 (% / s).
[0093] Next, the stretched unsintered fluororesin sheet was stretched in the width direction at a stretch ratio of 36 times using a tenter capable of continuous clipping. The stretching temperature in the width direction was 290°C.
[0094] Here, the first supporting material is laminated on the windward side of the fluororesin porous membrane obtained by stretching the fluororesin sheet, and the second supporting material is laminated on the leeward side in the direction of air flow, and the first supporting material and the second supporting material are thermally fused to the fluororesin porous membrane using a hot press device, thereby obtaining the air filter medium of Example 1. Note that, the thermal lamination by the hot press device is performed by sandwiching between the hot plate heated to 160 ° C and the plate opposite to it, and applying a load of 0.4 MPa for 8 seconds.
[0095] The first supporting material on the windward side used in Example 1 was a spunbond nonwoven fabric (average fiber diameter 26 μm, basis weight 40 g / m) made of fibers with a core / sheath structure using PET as the core and PE as the sheath. 2 The second supporting material on the leeward side used in Example 1 was a spunbond nonwoven fabric (average fiber diameter 26 μm, basis weight 40 g / m2) made of fibers with a core / sheath structure using PET as the core and PE as the sheath. 2 , thickness 210 μm).
[0096] Example 2 290 g of hydrocarbon oil (IP Solvent 2028, Idemitsu Kosan Co., Ltd.) was added as an extrusion liquid lubricant per 1 kg of PTFE fine powder (Polyflon Fine Powder F106, Daikin Industries, Ltd.) with an average molecular weight of 6.5 million and mixed at 20°C. The mixture was then extruded using a paste extrusion device to obtain a rod-shaped molded body. This rod-shaped molded body was formed into a sheet using a calendar roll heated to 70°C to obtain a fluororesin sheet. The fluororesin sheet was passed through a hot air drying oven at 250°C to evaporate and remove the hydrocarbon oil, and a strip-shaped unsintered fluororesin sheet with an average thickness of 200 μm and an average width of 150 mm was obtained.
[0097] Next, the unsintered fluororesin sheet was stretched in the longitudinal direction at a stretch ratio of 5. The stretching temperature in the longitudinal direction was 250° C. Here, the stretching rate (% / s) in the longitudinal direction was 150 (% / s).
[0098] Next, the stretched unsintered fluororesin sheet was stretched in the width direction at a stretch ratio of 36 times using a tenter capable of continuous clipping. The stretching temperature in the width direction was 290°C.
[0099] Here, the fluororesin porous membrane obtained by stretching the fluororesin sheet is laminated with the first supporting material on the windward side in the direction of air flow, and the second supporting material is laminated on the leeward side, and the first supporting material and the second supporting material are thermally fused to the fluororesin porous membrane by using a hot press device, thereby obtaining the air filter medium of Example 2. Note that, the thermal lamination by the hot press device is performed by sandwiching between the hot plate heated to 160 ° C and the plate opposite to it, and applying the load of 0.4 MPa for 8 seconds.
[0100] The first supporting material on the windward side used in Example 2 was a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 40 g / m) made of fibers with a core / sheath structure using PET as the core and PE as the sheath. 2 The second supporting material on the leeward side used in Example 2 was a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 40 g / m2) made of fibers with a core / sheath structure using PET as the core and PE as the sheath.2 , thickness 210 μm).
[0101] Example 3 In Example 3, a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 30 g / m) made of fibers with a core / sheath structure using PET as the core and PP as the sheath was used as the first support material for the air filter medium. 2 As the second support material used in the air filter media, a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 30 g / m2) consisting of fibers with a core / sheath structure using PET as the core and PP as the sheath was used. 2 An air filter medium was produced in the same manner as in Example 1, except that a 350 μm thick PET filter sheet (350 μm thick) was used and thermal lamination was performed using a hot press device by applying a load of 0.4 MPa for 8 seconds using a hot plate heated to 195°C.
[0102] Example 4 In Example 4, a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 50 g / m) made of fibers with a core / sheath structure using PET as the core and PP as the sheath was used as the first support material for the air filter medium. 2 As the second support material used in air filter media, a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 50 g / m) consisting of fibers with a core / sheath structure using PET as the core and PP as the sheath was used. 2 An air filter medium was produced in the same manner as in Example 1, except that a 400 μm thick PET filter sheet (100 μm thick) was used and thermal lamination was performed using a hot press device by applying a load of 0.4 MPa for 8 seconds using a hot plate heated to 195°C.
[0103] Example 5 In Example 5, a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 30 g / m) made of fibers with a core / sheath structure using PET as the core and PE as the sheath was used as the first support material for the air filter medium. 2 As the second support material used in the air filter media, a spunbond nonwoven fabric (average fiber diameter 37 μm, basis weight 30 g / m2) consisting of fibers with a core / sheath structure using PET as the core and PE as the sheath was used. 2An air filter medium was produced in the same manner as in Example 1, except that a 100 mm thick filter medium (190 μm thick) was used.
[0104] Comparative Example 1 In Comparative Example 1, an air filter medium was obtained in the same manner as in Example 2, except that the first support material and the second support material used in the air filter medium were changed as described below.
[0105] The first supporting material on the windward side used in Comparative Example 1 was a spunbond nonwoven fabric (average fiber diameter 20 μm, basis weight 40 g / m) made of fibers with a core / sheath structure using PET as the core and PE as the sheath. 2 The second supporting material on the leeward side used in Comparative Example 1 was a spunbond nonwoven fabric (average fiber diameter 20 μm, basis weight 40 g / m2) made of fibers with a core / sheath structure using PET as the core and PE as the sheath. 2 , thickness 200 μm).
[0106] The physical properties measured in Examples 1 to 5 and Comparative Example 1 are as follows.
[0107] (Pressure loss in laminates) The measurement sample, which was made by simply laminating the first and second supporting materials to the fluororesin porous membrane but not heat-sealing it, was set in a filter holder with a diameter of 100 mm, the inlet side was pressurized with a compressor, and the air flow rate was adjusted to 5.3 cm / sec with a flow meter. The pressure loss at this time was measured with a manometer.
[0108] (Pressure loss of air filter media) The measurement sample of the air filter medium was set in a filter holder with a diameter of 100 mm, the inlet side was pressurized with a compressor, and the air flow rate was adjusted to 5.3 cm / sec with a flow meter. The pressure loss at this time was measured with a manometer.
[0109] (Increase in pressure loss due to heat fusion) The increase in pressure loss due to heat fusion was calculated by subtracting the value obtained by measuring the pressure loss in the laminate from the value obtained by measuring the pressure loss in the air filter medium.
[0110] (Thickness of fluororesin porous membrane) Using a thickness gauge (1D-110MH, manufactured by Mitutoyo Corporation), five measurement targets were stacked and the total thickness was measured, and the value was divided by 5 to obtain the thickness of one sheet.
[0111] (Thickness of the first support material, thickness of the second support material) An ABS Digimatic Indicator (Mitutoyo, ID-C112CX) was fixed to a gauge stand, and the thickness value was read when a load of 0.3 N was applied to the measurement object.
[0112] (Air filter media thickness) An ABS Digimatic Indicator (Mitutoyo, ID-C112CX) was fixed to a gauge stand, and the thickness value was read when a load of 0.3 N was applied to the measurement object.
[0113] (Weight of first support material, weight of second support material) The basis weight was calculated by dividing the mass (g) of a sample cut into a rectangle of 4.0 cm x 12.0 cm by the area (0.0048 m) measured on a precision balance. 2 ) was used as the value.
[0114] (Average fiber diameter of the first support material, average fiber diameter of the second support material) The surface of the test sample was photographed at 1000 to 5000 times magnification with a scanning electron microscope (SEM), two lines were drawn perpendicular to each other on one photographed image, and the thickness of the image of the fiber intersecting these lines was measured as the fiber diameter. The number of fibers measured was 200 or more. The fiber diameters thus obtained were plotted in a log-normal manner with the horizontal axis representing the fiber diameter and the vertical axis representing the cumulative frequency, and the value at which the cumulative frequency was 50% was taken as the average fiber diameter. The geometric standard deviation, which represents the distribution of fiber diameters, was calculated from the results of the log-normal plot described above by reading the fiber diameters at the cumulative frequency of 50% and the fiber diameters at the cumulative frequency of 84% and using the following formula. Geometric standard deviation [-] = cumulative frequency 84% fiber diameter / cumulative frequency 50% fiber diameter
[0115] (Total fiber length within unit volume of first support material, total fiber length within unit volume of second support material) Weight (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 The value obtained by calculating {length (cm) × thickness (cm) × 1,000,000} was regarded as the total fiber length within a unit volume.
[0116] (Average fiber cross-sectional area of the first support material, average fiber cross-sectional area of the second support material) The value was calculated from the average fiber diameter obtained in the above measurements (average fiber diameter of the first supporting material, average fiber diameter of the second supporting material) assuming that the cross-sectional shape was a circle.
[0117] (Total fiber length of support material) The total fiber length of the support materials was determined by adding the total fiber length of the first support material within a unit volume of the second support material to the total fiber length of the second support material within a unit volume of the first support material.
[0118] (Collection efficiency of NaCl particles with a particle diameter of 0.1 μm in laminated products) According to the method described in JIS B9928 Appendix 5 (Regulations) NaCl aerosol generation method (pressure spray method), NaCl particles generated by an atomizer were classified to a particle size of 0.1 μm using an electrostatic classifier (TSI), and the particle charge was neutralized using americium 241. The permeating flow rate was then adjusted to 5.3 cm / sec. A particle counter (TSI, CNC) was used to count the number of particles before and after the laminate in which the first and second support materials were simply laminated to the fluororesin porous membrane but not heat-fused, and the collection efficiency was calculated using the following formula. Collection efficiency (%) = (CO / CI) x 100
[0119] CO = Number of 0.1 μm NaCl particles collected by the measurement sample CI = Number of 0.1 μm particles of NaCl supplied to the measurement sample
[0120] (Transmittance of NaCl particles with a particle size of 0.1 μm in a laminate) The value obtained by subtracting {100(%)-collection efficiency (%) of NaCl particles having a particle diameter of 0.1 μm in the laminate} was taken as the transmittance (%) of NaCl particles having a particle diameter of 0.1 μm in the laminate.
[0121] (Collection efficiency of NaCl particles with a particle diameter of 0.1 μm in air filter media) According to the method described in JIS B9928 Appendix 5 (Regulations) NaCl aerosol generation method (pressure spray method), NaCl particles generated by an atomizer were classified to a particle size of 0.1 μm using an electrostatic classifier (TSI), and the particle charge was neutralized using americium-241. The permeating flow rate was then adjusted to 5.3 cm / sec. The number of particles before and after the air filter medium was determined using a particle counter (TSI, CNC), and the collection efficiency was calculated using the following formula. Collection efficiency (%) = (CO / CI) x 100
[0122] CO = Number of 0.1 μm NaCl particles collected by the measurement sample CI = Number of 0.1 μm particles of NaCl supplied to the measurement sample
[0123] (Permeability of NaCl particles with a particle size of 0.1 μm in air filter media) The value obtained by subtracting {100(%) from the collection efficiency (%) of NaCl particles having a particle diameter of 0.1 μm in the air filter medium} was taken as the transmittance (%) of NaCl particles having a particle diameter of 0.1 μm in the air filter medium.
[0124] (transmittance ratio) The value obtained by {permeability of NaCl particles having a particle size of 0.1 μm in the air filter medium / permeability of NaCl particles having a particle size of 0.1 μm in the laminate} was calculated as the permeability ratio.
[0125] (PF value of NaCl particles with a particle diameter of 0.1 μm in air filter media) Using NaCl particles with a particle diameter of 0.1 μm, the PF value was calculated from the pressure loss and collection efficiency (collection efficiency of NaCl particles with a particle diameter of 0.1 μm) of the air filter medium according to the following formula. PF value = {-log((100-collection efficiency (%)) / 100)} / (pressure loss (Pa) / 1000)
[0126] (Breakdown voltage of air filter media) In accordance with JIS C2110-1, Solid Electrical Insulating Materials - Test Method for Dielectric Breakdown Strength, the dielectric breakdown voltage of the target air filter media samples was measured using a short-time (rapid voltage increase) test.
[0127] The physical properties of the air filter media of Examples 1 to 5 and Comparative Example 1 are shown in the following table. [Table 1]
[0128] Although the embodiments of the present disclosure have been described above, it will be understood that various changes in form and details can be made without departing from the spirit and scope of the present disclosure described in the claims. [Explanation of symbols]
[0129] 1 Air filter unit 20 Filter pack (pleated filter material) 25 Frame 30 Air filter media 31 Fluororesin porous membrane 32 1st support material 33 Second support material [Prior art documents] [Patent documents]
[0130] [Patent Document 1] JP 2002-66226 A
Claims
1. A fluororesin porous membrane (31); A first support material (32) for supporting the fluororesin porous membrane; Equipped with The fluororesin porous membrane and the first support material are heat-sealed, The first support material has a core-sheath structure fiber including a first core portion and a first sheath portion having a melting point lower than that of the first core portion, The first support material satisfies the following formula: Formula: basis weight (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 ) × thickness (cm) × 1,000,000}≦380 (m / cm 3 ) Air filter media (30).
2. Further provided is a second support material (33) for supporting the fluororesin porous membrane, the fluororesin porous membrane is located between the first support material and the second support material, The fluororesin porous membrane and the second support material are heat-sealed, The second support material has a core-sheath structure fiber including a second core portion and a second sheath portion having a melting point lower than that of the second core portion, The second support material satisfies the following formula: Formula: basis weight (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 ) × thickness (cm) × 1,000,000}≦380 (m / cm 3 ) The air filter medium according to claim 1 .
3. The dielectric breakdown voltage is 0.8 kV or more. The air filter medium according to claim 1 or 2.
4. The thickness is 350 μm or more and 1000 μm or less. The air filter medium according to claim 1 or 2.
5. The PF value, which is determined by the pressure loss when air is passed through the air filter medium at a flow rate of 5.3 cm / sec and the collection efficiency of the air filter medium using NaCl particles having a particle diameter of 0.1 μm, is 20 or more, as determined by the following formula: PF value = {-log ((100 - collection efficiency (%)) / 100)} / (pressure loss (Pa) / 1000). The air filter medium according to claim 1 or 2.
6. The basis weight of the first support material is 25 g / m 2 60g / m or more 2 Below is the The air filter medium according to claim 1 or 2.
7. The first support material has an average fiber diameter of 23 μm or more. The air filter medium according to claim 1 or 2.
8. 3. The air filter medium according to claim 1, wherein the filter pack (20) is folded so as to have mountain folds and valley folds.
9. An air filter medium according to claim 1 or 2, or a pleated filter medium (20) according to claim 1 or 2, which is folded so that mountain folds and valley folds are generated; A frame (25) for holding the air filter medium or the pleated filter medium; An air filter unit (1) comprising:
10. A step of preparing a fluororesin porous membrane (31); A step of preparing a first supporting material (32) having a core-sheath structure fiber including a first core and a first sheath having a melting point lower than that of the first core, and satisfying the following formula: Formula: basis weight (g / m 2 ) / {average fiber cross-sectional area (cm 2 ) x material specific gravity (g / cm 3 ) × thickness (cm) × 1,000,000}≦380 (m / cm 3 ) a step of heat-sealing the fluororesin porous membrane and the first support material; A method for manufacturing an air filter medium (30) comprising the steps of:
Citation Information
Patent Citations
Air filter medium, air filter pack and air filter unit using the same, and manufacturing method for air filter medium
JP2002066226A
Ventilation member and ventilation case including the same
JP2011233580A
Air filter material, air filter material manufacturing method, filter material for mask and pleat-like filter material for mask
JP2022119497A
Air filter medium, pleat-like filter medium, air filter unit, filter medium for mask, and regeneration method for air filter medium
JP2022186658A
Composite filter media
US20050193696A1