Packaging paper

A dual-layer resin coating system in packaging paper with specific melting point resins reduces plastic use and enhances water resistance, blocking resistance, and heat-sealability, addressing the limitations of conventional laminated papers.

JP2024134336APending Publication Date: 2024-10-03HOKUETSU CORP

Patent Information

Application Number
JP2023044579
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing packaging solutions using laminated paper still rely heavily on polyethylene and polypropylene, failing to adequately reduce plastic usage, and lack sufficient water resistance, blocking resistance, and heat-sealability.

Method used

A packaging paper design with at least two resin coating layers, where inner layers have a lower melting point for flexibility and outer layers have a higher melting point for adhesion, using resins like ionomer, ethylene copolymer, and polyvinylidene chloride, with a total coating amount controlled to minimize plastic use.

Benefits of technology

The solution reduces plastic usage by up to 67% while maintaining excellent processing suitability, including water resistance, blocking resistance, and heat-sealability, addressing environmental impact and practical usability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134336000001
    Figure 2024134336000001
Patent Text Reader

Abstract

To provide packaging paper with excellent processing suitability and heat sealability, such as water resistance and blocking resistance after folding, by reducing the amount of plastic used.SOLUTION: Packaging paper has at least two or more resin coating layers on at least one surface of a paper base material, and it is composed of a first resin coating layer which is a resin coating layer close to the paper base material, a second resin coating layer which is a resin coating layer on the opposite surface of the first resin coating layer, and so on, among the resin coating layers. The resin coating layer comprises one or more selected from the group consisting of ionomers, ethylene copolymers, thermoplastic polyurethanes, polyvinylidene chloride, polylactic acid, and polybutylene succinate, and one or more resins with a melting point lower than that of the resin contained in the outermost resin coating layer of the resin coating layers are contained in the layers other than the outermost resin coating layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging paper that uses a reduced amount of plastic and has excellent processability, such as water resistance after folding and blocking resistance, and excellent heat sealability. [Background technology]

[0002] In recent years, the problem of plastic waste has become more serious. It is said that the world's plastic production exceeds 400 million tons per year, of which a large amount is produced in the packaging container sector, which is the cause of plastic waste. Plastic does not decompose for a long time, and the waste breaks down into microplastics in the natural environment, causing serious adverse effects on the ecosystem. Marine pollution is particularly severe, and it is said that the plastic waste is impossible to recover. In the future, it will be necessary for the global environment to reduce the use of plastic.

[0003] On the other hand, the use of biodegradable plastics that can be completely decomposed by microorganisms has been proposed around the world as a measure against plastic waste. Biodegradable plastics decompose in nature within a certain period of time, but until they decompose they are still waste, and unless their usage and disposal amounts are reduced, this cannot be said to be an immediate solution (see Patent Documents 1 and 2).

[0004] The most commonly used plastics for packaging containers are polyethylene terephthalate (PET) for beverage bottles, polyethylene (PE) and polypropylene (PP) for laminating shopping bags and containers. Substituting paper for plastic has been proposed as a measure to reduce the amount of plastic used. However, even when replacing plastic with paper, polyethylene or polypropylene is laminated in large quantities as a heat sealant when processed into bags and containers. The amount of lamination of these plastics varies depending on the product concept, but is generally 30 to 50 g / m 2 Depending on the application, it may be up to 300g / m 2Therefore, even in laminated paper, which replaces plastic with paper, the amount of plastic used is still not sufficiently reduced, and there is an urgent need for a direct method of reducing plastic use. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-148444 A [Patent Document 2] JP 2013-141763 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention relates to a packaging paper that can reduce the amount of plastic used and has excellent processing suitability, such as water resistance after folding (hereinafter sometimes abbreviated as "folding resistance") and blocking resistance (hereinafter sometimes abbreviated to "processing suitability"), as well as excellent heat sealability.

[0007] Other objects and advantages of the present invention will become readily apparent to those skilled in the art by reading the following description. [Means for solving the problem]

[0008] In the present invention, in order to reduce the amount of polyethylene or polypropylene used in conventional plastic laminated paper (hereinafter sometimes abbreviated as polylaminated paper), a packaging paper having at least two resin coating layers is provided, characterized in that all layers of the resin coating layers contain at least one selected from the group consisting of ionomer, ethylene copolymer, thermoplastic urethane, polyvinylidene chloride, polylactic acid, and polybutylene succinate, and at least one resin having a melting point lower than that of the resin in the outermost layer is contained in layers other than the outermost layer. The resin contained in the resin coating layer is a resin with excellent film-forming properties, so that it can impart good folding resistance. In addition, these resins also have excellent heat sealing properties, so that it can also impart heat sealing suitability. With this configuration, folding resistance is imparted by any layer other than the outermost layer containing a resin with a low melting point and a softness, and blocking resistance is imparted by the outermost layer containing a resin with a high melting point and poor adhesion, so that a packaging paper with excellent processing suitability can be obtained.

[0009] In the present invention, the total coating amount of the resin coating layer on one side is 2 to 20 g / m 2 With such a configuration, the amount of plastic used is preferably within 30 g / m per side while maintaining excellent processability. 2 Compared to conventional polylaminated paper, which uses more than 100% plastic, the amount of plastic used in the resin coating layer can be reduced to approximately 7-67% of the conventional amount.

[0010] In the present invention, it is preferable that the melting point of the resin in the outermost layer of the resin coating layer is 90° C. or higher. By adopting such a configuration, it is possible to obtain a packaging paper with excellent blocking resistance, since a resin with a melting point of 90° C. or higher has poor adhesion.

[0011] In the present invention, it is preferable that a pigment is contained in at least one layer other than the outermost layer of the resin coating layer. By adopting such a configuration, the pigment plays a role of filling the gaps, resulting in a wrapping paper with better folding resistance.

[0012] In the present invention, it is preferable to further provide an underlayer containing a pigment and a binder between the paper base material and the resin coating layer. With such a configuration, the underlayer plays a role of sealing, resulting in a wrapping paper with better folding resistance.

[0013] In the present invention, it is preferable that the paper base material contains bleached softwood kraft pulp. By using such a constitution, the elongation of the paper base material is improved and the paper base material is less likely to crack, resulting in a wrapping paper with good folding resistance.

[0014] In the present invention, the paper base material preferably contains polyacrylamide as a paper strength agent. With this configuration, the polyacrylamide reinforces the entanglement between pulp fibers, thereby increasing the paper strength of the paper base material and providing a packaging paper that is less likely to deteriorate in folding resistance. Effect of the Invention

[0015] According to the present invention, it is possible to produce packaging paper that can reduce the amount of plastic used and has excellent processing suitability such as water resistance and blocking resistance after folding, and excellent heat sealing properties. Even if the packaging paper of the present invention is inappropriately released into the natural world as garbage, it is possible to reduce the adverse effects of plastic garbage on the natural environment, which helps to solve the plastic garbage problem. The packaging paper of the present invention can be processed into, for example, primary and secondary bags for food packaging, food cups for ice cream, etc., lids for cup containers, beverage cups for coffee, etc., food containers for hot snacks, etc., and trays, boxes, cases, containers, and other paper containers in general. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, the present invention will be described in detail by showing an example of an embodiment, but the present invention is not limited to the description. The embodiment may be modified in various ways as long as the effects of the present invention are achieved.

[0017] In this embodiment, the present invention is characterized in that the present invention has at least two resin coating layers, all of which contain at least one selected from the group consisting of ionomer, ethylene copolymer, thermoplastic urethane, polyvinylidene chloride, polylactic acid, and polybutylene succinate, and that at least one resin having a melting point lower than that of the resin of the outermost layer, which is the layer farthest from the paper substrate, is contained in layers other than the outermost layer. Since a resin with a low melting point has excellent film-forming properties, it produces a high sealing effect and is easy to impart water resistance and oil resistance. Furthermore, since a resin with a low melting point is soft, even when the packaging paper is folded, the resin coating layer easily expands and contracts as it is folded, and cracks are unlikely to occur, so that the water resistance after folding is unlikely to be impaired. The melting point of the resin used here is preferably 100°C or less. More preferably, it is 70 to 95°C. On the other hand, a disadvantage is that the soft resin is highly adhesive, and blocking is likely to occur. Therefore, in this embodiment, the resin of the outermost layer has a higher melting point than the resin with the lowest melting point other than the outermost layer. That is, a resin coating layer containing a resin with a lower melting point is arranged on the inside, and a resin coating layer containing a resin with a higher melting point is arranged as the outermost layer. When a plurality of resins are included in the layer, the melting point here refers to the melting point of the resin mixture. A resin with a higher melting point contained in the outermost layer is hard, has poor adhesion, and has excellent blocking resistance, so that blocking resistance is imparted to the outermost layer. The melting point of the resin of the outermost layer is preferably 85°C or higher. More preferably, it is 90°C or higher. By stacking two or more resin coating layers with different melting points in this order, a packaging paper with a good balance of both folding resistance and blocking resistance can be obtained. Furthermore, the difference in melting point between the resin with the lowest melting point and the resin of the outermost layer is preferably 5°C to 85°C, for example, 5°C to 80°C, 5°C to 70°C. This is because such a difference in melting point makes it possible to obtain a packaging paper that is excellent in water resistance, oil resistance, and processing characteristics while also having excellent blocking resistance.

[0018] In an embodiment of the present invention, the resin coating layer may be composed of three or more layers. Even in the case of three or more layers, one or more resins having a lower melting point than the resin contained in the outermost layer of the resin coating layer are contained in layers other than the outermost layer. By making the resin coating layer three or more layers, minute pinholes occurring in the resin coating layer can be filled more reliably, so that the air permeability of the packaging paper can be further improved, and water resistance, oil resistance, and moisture resistance are further improved. In this embodiment, it is preferable that the melting point of the resin contained in the innermost resin coating layer closest to the paper substrate is lower than the melting points of the resins in the other resin coating layers. For example, when the resin coating layer is composed of three layers, the melting point of the resin contained in the innermost resin coating layer is lower than the melting point of the resin in the outermost layer and the middle layer, and the folding resistance tends to be superior than the case where the melting point of the resin contained in the resin coating layer located in the middle is lower than the melting point of the resin in the outermost layer and the innermost layer.

[0019] In an embodiment of the present invention, the resin in the resin coating layer is characterized by including at least one selected from the group consisting of ionomer, ethylene copolymer, thermoplastic urethane, polyvinylidene chloride, polylactic acid, and polybutylene succinate. The resin coating layer is made of a resin, and may include any resin other than the above, as long as it does not affect the processability, and may further include a mixture of multiple resins. In each resin coating layer, it is preferable that a resin selected from the above is the main component, and furthermore, it is preferable that the resin selected from the above is included in the resin layer at 90 mass % or more, and the resin in the resin coating layer is preferably at least one selected from the group consisting of ionomer, ethylene copolymer, thermoplastic urethane, polyvinylidene chloride, polylactic acid, and polybutylene succinate. Here, ionomer refers to a synthetic resin in which a polymer is aggregated by utilizing the cohesive force of metal ions, and includes all aggregates formed by intermolecular bonding between a resin and a metal cation. For example, metal salts of ethylene-methacrylic acid copolymers, metal salts of ethylene-acrylic acid copolymers, metal salts of urethane-acrylic acid copolymers, metal salts of urethane-methacrylic acid copolymers, metal salts of styrene-acrylic acid copolymers, metal salts of styrene-methacrylic acid copolymers, metal salts of ethylene-fluorine polymer copolymers, etc. In the present invention, metal salts of ethylene-acrylic acid or ethylene-methacrylic acid copolymers are preferred among ionomers because they can impart excellent folding resistance and blocking resistance. In addition, as the ethylene copolymer, it is preferable to use any one of ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid ester copolymers, and ethylene-vinyl acetate copolymers because they have particularly excellent folding resistance. There is no particular restriction on the thermoplastic urethane, but it is preferable to use any one of thermoplastic urethanes of ester type, ester-ether type, carbonate type, and aromatic isocyanate type. As the polyvinylidene chloride, vinylidene chloride alone or copolymers with other polymers may be used.Although there is no particular limitation, the copolymer is preferably a copolymer with any of latex, vinyl chloride, methacrylic acid ester, acrylic acid ester, and unsaturated carboxylic acid. The polylactic acid may be polylactic acid alone or a copolymer with other polymers. Lactic acid includes L-lactic acid and D-lactic acid, which are polymerized to form polylactic acid, and the ratio of L-lactic acid to D-lactic acid may be any ratio as long as it does not affect the heat seal performance. In addition, the copolymer is preferably a copolymer with any of hydroxycarboxylic acid, aliphatic cyclic ester, dicarboxylic acid, and polyhydric alcohols. The polybutylene succinate resin may be polybutylene succinate alone or a copolymer with other polymers. Although there is no particular limitation, the copolymer may be, for example, a copolymer with adipic acid or polyethylene glycol. These resins have excellent heat sealability, so when they are included in the outermost resin coating layer, a packaging paper that is imparted with heat sealability in addition to processability can be obtained. In addition, it is more preferable that the resin is one or more of ionomer and ethylene copolymer. Ionomer resins, especially metal salts of ethylene-acrylic acid or ethylene-methacrylic acid copolymers, are particularly excellent in folding resistance and blocking resistance, making it possible to obtain packaging paper that combines high processability and heat sealability. Ethylene copolymer resins are particularly excellent in folding resistance and oil resistance, making it possible to obtain packaging paper with high barrier performance.In a specific embodiment, for example, the packaging paper has, as the outermost resin coating layer, a layer containing an ionomer having a melting point of 90 to 99°C, preferably a melting point of 95 to 99°C (e.g., a metal salt of an ethylene-acrylic acid or ethylene-methacrylic acid copolymer) or vinylidene chloride having a melting point of 140 to 160°C, and also has, as the resin coating layer having a melting point lower than the melting point of the resin of the outermost layer, a layer containing an ionomer having a melting point of 80°C or more and less than 90°C, preferably a metal salt of an ethylene-acrylic acid or ethylene-methacrylic acid copolymer) having a melting point of 85°C or more and less than 90°C, or an ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-acrylic acid ester copolymer, ethylene-methacrylic acid ester copolymer, or ethylene-vinyl acetate copolymer having a melting point of 80°C or more and less than 90°C, preferably 85°C or more and less than 90°C.

[0020] In an embodiment of the present invention, a resin coating layer can be provided by applying a resin-containing coating solution for a resin coating layer to at least one surface of a paper substrate and drying it. The resin used for the resin coating layer is preferably a water-based emulsion. By using these, the coating amount can be controlled to be relatively low, and further, VOC emissions are eliminated, thereby further reducing the burden on the natural environment.

[0021] In an embodiment of the present invention, in addition to the aqueous emulsion containing a resin, various auxiliaries may be added to the resin coating layer coating liquid within a range that does not impair the intended effect of the present invention. For example, viscosity modifiers, defoamers, leveling agents such as surfactants and alcohols, color pigments, color dyes, lubricants such as wax, and pigments such as clay and calcium carbonate. For example, in the resin coating liquid, it is preferable to add 25 to 75 parts or 40 to 60 parts of a pigment, such as kaolin clay, heavy calcium carbonate, or light calcium carbonate, per 100 parts of resin. This may result in a packaging paper with excellent folding resistance. In addition, it is also preferable to add 0.05 to 0.5 parts of a dispersant in addition to the pigment per 100 parts of resin in the resin coating liquid. Note that auxiliaries other than those mentioned above may be included within a range that does not impair the intended effect of the present invention.

[0022] In the present invention, the total coating amount of the resin coating layer is 2 to 20 g / m in terms of solid content. 2 More preferably, it is 3 to 15 g / m 2 By setting the total coating weight of the resin coating layer in this range, sufficient folding resistance can be obtained. 2 If it is less than 20 g / m, sufficient folding resistance may not be obtained. 2 If it exceeds this limit, sufficient folding resistance can be obtained, but the amount of plastic used will also increase, so there is a risk that the effect of reducing plastic will be poor. If a resin coating layer is provided on both sides of the paper base material, the total coating amount of the resin coating layers provided on both sides of the paper base material must be 4 to 30 g / m2 in terms of solid content. 2 It is preferable that the thickness is 5 to 25 g / m 2 It is more preferable that the resin coating layer is formed in a thickness of 100 mm or less. This provides sufficient folding resistance while being excellent in the effect of reducing plastics. In the packaging paper of the present invention, the resin coating layer is usually formed not only on a part of the surface of the base paper, but on the entire surface. In other words, it is preferable that the resin coating layer is formed so as to cover the entire surface of the paper base material, rather than being formed only on the part required for adhesion by heat sealing, such as in a net, island, or line shape.

[0023] In the present invention, it is preferable that the coating amount of the resin coating layer is greater for the innermost layer closest to the paper substrate than for the other layers. This configuration can fill gaps in the paper substrate and layers directly below the innermost layer, such as the underlayer, and suppress the occurrence of pinholes in the innermost layer, thereby imparting good folding resistance, water resistance, and oil resistance. The coating amount of the innermost layer is 1.5 to 10 g / m2 in terms of solid content per side of the paper substrate. 2 and more preferably 3 to 8 g / m 2 The other resin coating layers can cover the surface of the paper substrate with a relatively small amount of coating by overcoating them on the innermost layer, which has fewer pinholes. Increasing the amount of resin in the resin coating layer also leads to an increase in the amount of plastic used, so it is desirable to use the minimum amount necessary to cover the surface. The coating amount of each resin coating layer other than the innermost layer is 0.5 to 5 g / m2 in solids equivalent per side of the paper substrate. 2 and more preferably 1 to 3 g / m 2 It is.

[0024] The method for applying the resin coating layer coating liquid in the present invention is not particularly limited, and any commonly used coating device can be used. For example, various known coating devices such as an air knife coater, a blade coater, a gravure coater, a flexo coater, a rod blade coater, a roll coater, a reverse roll coater, a bar coater, a curtain coater, a die slot coater, a champlex coater, a metering blade type size press coater, a short dwell coater, a spray coater, a gate roll coater, and a lip coater can be used.

[0025] In the embodiment of the present invention, any layer may be provided other than the paper substrate and the resin coating layer, as long as the intended effect of the present invention is not impaired. For example, an underlayer containing a pigment and a binder may be provided between the paper substrate and the resin coating layer. By providing the underlayer between the paper substrate and the resin coating layer, a sealing effect is generated that prevents the resin coating layer coating liquid from penetrating into the paper substrate, so that even with a small amount of resin coating layer, a resin film with few defects is easily formed, and packaging paper with better folding resistance, water resistance, and oil resistance can be obtained without increasing the amount of plastic used. The underlayer is preferably configured to use a pigment and a binder in combination. For example, the binder may be contained in an amount of 5 to 100 parts by mass per 100 parts by mass of the pigment. The pigment and binder in the under layer may be any known pigment and binder used in the coating layer of a typical coated printing paper. In addition, the under layer may contain various auxiliary agents within a range that does not impair the intended effects of the present invention. For example, the under layer may contain a viscosity adjuster, a softener, a gloss imparting agent, a water resistance agent, a dispersant, a flow modifier, an ultraviolet absorber, a stabilizer, an antistatic agent, a crosslinking agent, a sizing agent, a fluorescent brightening agent, a colorant, a pH adjuster, an antifoaming agent, a plasticizer, and a preservative. Examples of pigments used in the under layer include inorganic pigments such as kaolin clay, calcium carbonate (heavy calcium carbonate, light calcium carbonate, etc.), calcined clay, talc, magnesium carbonate, barium sulfate, calcium sulfate, titanium dioxide, zinc oxide, zinc sulfate, zinc carbonate, calcium silicate, aluminum silicate, magnesium silicate, diatomaceous earth, aluminum hydroxide, and magnesium hydroxide; and organic pigments such as acrylic, styrene, vinyl chloride, and nylon themselves, and those obtained by copolymerizing them (so-called plastic pigments (hereinafter, may be abbreviated as "PP particles")).Examples of binders used in the underlayer include starches such as butadiene-based copolymer latex, crosslinker-modified starch, oxidized starch, enzyme-modified starch, esterified starch, cationic starch, and amphoteric starch, water-soluble polymers such as gelatin, casein, soybean protein, and polyvinyl alcohol, and synthetic resins such as vinyl acetate, ethylene vinyl acetate, polyurethane resin, acrylic resin, polyester resin, polyamide resin, polyvinylidene chloride resin, and polylactic acid resin. Specific examples of the underlayer include a pigment containing 5 to 35 parts by mass of kaolin clay and 65 to 95 parts by mass of heavy calcium carbonate, and a binder containing 1 to 5 parts by mass of phosphated starch and 15 to 45 parts by mass of styrene-butadiene copolymer latex. By having such a composition, a wrapping paper with better folding resistance may be obtained.

[0026] In an embodiment of the present invention, a printed layer may be provided on the surface of the paper base material that is not coated with the resin coating layer. When the packaging paper is processed into a bag or a paper cup, the outer surface of the container may be printed with information about the contents or to advertise the contents, and providing a printed layer can provide good printability. It is also possible to print on the printed layer and then provide a resin coating layer on top of the printed layer. The composition of the printed layer is not particularly limited, and it can contain a pigment, a binder, and various auxiliaries in the same way as the underlayer described above, and can have the same composition as the coating layer of a known printing coated paper.

[0027] In an embodiment of the present invention, the paper substrate may include a step of smoothing the paper substrate. The method of smoothing the paper substrate is not particularly limited, and a commonly used calendaring device may be used. For example, various known smoothing devices such as a machine calendar, a soft calendar, a super calendar, a gloss calendar, and a shoe nip calendar may be used. In addition, the method may include a step of smoothing the paper substrate by transferring the mirror surface of a Yankee dryer, as used for one-sided gloss kraft paper. By applying a resin coating layer to the smoothed surface, the resin coating layer coating liquid is easily applied uniformly to the paper substrate surface, resulting in a high sealing effect, and a packaging paper having good folding resistance, water resistance, and oil resistance can be obtained.

[0028] The paper base material used in the embodiment of the present invention is not particularly limited, and a known base paper containing pulp as a main component can be used. As the pulp that is the main component of the base paper, chemical pulp such as LBKP (hardwood bleached kraft pulp) and NBKP (softwood bleached kraft pulp), mechanical pulp such as GP (groundwood pulp), PGW (pressurized groundwood pulp), RMP (refiner mechanical pulp), TMP (thermo-mechanical pulp), CTMP (chemi-thermo-mechanical pulp), CMP (chemi-mechanical pulp), and CGP (chemi-ground pulp), wood pulp such as DIP (deinked pulp), and non-wood pulp such as kenaf, bagasse, bamboo, and cotton can be used. These can be used alone or mixed in any ratio. For example, 90 to 100 parts by mass of LBKP (hardwood bleached kraft pulp) can be used as the pulp. In addition, synthetic fibers can be further blended within a range that does not impair the intended effect of the present invention. From the viewpoint of environmental conservation, ECF (Elemental Chlorine Free) pulp, TCF (Total Chlorine Free) pulp, waste paper pulp, and pulp obtained from planted trees are preferred. In addition, for example, the appropriate beating degree of pulp is 200 to 700 mlCSF, preferably 250 to 650 mlCSF, or further 400 to 620 mlCSF, for example, 480 to 580 mlCSF in Canadian Standard Freeness (JIS P 8121:1995 "Testing Method for Pulp Freeness").

[0029] In this embodiment, it is preferable to use LBKP (bleached hardwood kraft pulp) as the main pulp component, and further, it is preferable to use 1 to 50 parts by mass of NBKP (bleached softwood kraft pulp) in addition to LBKP, based on 100 parts by mass of the total pulp. More preferably, 70 to 95 parts by mass of LBKP and 5 to 30 parts by mass of NBKP, for example, 85 to 95 parts by mass of LBKP and 5 to 15 parts by mass of NBKP, are used. By adding NBKP, the elongation of the paper base material is improved, the paper base material is less likely to crack when folded, and the folding resistance is improved. For example, specifically, pulp containing 100 parts of bleached hardwood kraft pulp with a Canadian Standard Freeness of 460 to 580 mlcsf can be used as the main component of the base paper. Alternatively, for example, pulp containing 85 to 95 parts of bleached hardwood kraft pulp having a Canadian Standard Freeness of 400 to 500 mlcsf and 5 to 15 parts of bleached softwood kraft pulp having a Canadian Standard Freeness of 460 to 580 mlcsf can be used.

[0030] In an embodiment of the present invention, it is preferable that the paper base material does not contain a filler. Examples of fillers include kaolin clay, calcium carbonate (heavy calcium carbonate, light calcium carbonate, etc.), calcined clay, talc, titanium dioxide, and aluminum hydroxide. When a filler is contained in the paper base material, the interfiber bonds of the pulp are inhibited, the paper strength of the paper base material is reduced, and the paper base material becomes more likely to crack when folded. Following the cracks in the paper base material, cracks are also more likely to occur in the resin coating layer, which may deteriorate the water resistance after folding. The above fillers may be contained within a range that does not impair the intended effect of the present invention.

[0031] In addition to the pulp and the filler, the paper base material may contain various known papermaking additives. Examples of papermaking additives include internal paper strength enhancers such as sizing agents, bulk enhancers, retention improvers, drainage improvers, coloring dyes, coloring pigments, fluorescent brighteners, fluorescent decolorizers, and pitch control agents. In addition, water-soluble polymers such as starch, polyvinyl alcohol, and polyacrylamide may be applied. If the paper base material contains a wet strength enhancer, the recyclability of the packaging paper is poor, so it is preferable that the paper base material does not contain a wet strength agent. The papermaking additive may be incorporated in the pulp slurry, or may be impregnated into the interior of the paper base material using a size press or gate roll after papermaking. In particular, it is preferable to contain polyacrylamide as a paper strength agent. In a paper base material containing polyacrylamide, the polyacrylamide reinforces the entanglement between pulp fibers, thereby increasing the paper strength of the paper base material and making the paper base material less likely to break when folded. By making the paper base material less likely to crack, the resin coating layer is also less likely to crack, and water resistance after folding is less likely to deteriorate. For example, the paper base material can contain 0.05 to 1.0 part by mass of a sizing agent and 0.05 to 1.0 part by mass of polyacrylamide per 100 parts by mass of pulp, and can further contain 0.1 to 0.4 part by mass of a rosin sizing agent per 100 parts by mass of pulp.

[0032] The method for making the paper base material is not particularly limited, and the paper base material can be produced by various paper machines such as a Fourdrinier paper machine, a multi-layer Fourdrinier paper machine, a cylinder paper machine, a multi-layer cylinder paper machine, a multi-layer Fourdrinier cylinder combination paper machine, a twin-wire paper machine, etc. In the present invention, the paper base material may be a single-layer or multi-layer paper machine.

[0033] In the embodiment of the present invention, the basis weight of the packaging paper is not particularly limited, but is, for example, 10 to 1000 g / m 2 The basis weight of wrapping paper that can be used for flexible packaging is 30 to 500 g / m 2 is preferable, and 30 to 350 g / m 2 If possible, this would be preferable. EXAMPLES

[0034] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" refer to "parts by mass" and "% by mass", respectively, unless otherwise specified. The number of parts added is a value calculated as a solid content.

[0035] Example 1 (Preparation of paper substrate) A paper stock was prepared by adding 100 parts of hardwood bleached kraft pulp with a Canadian Standard freeness of 520 mlcsf, 0.3 parts of cationic polyacrylamide (product name: Polystron 705, manufactured by Arakawa Chemical Industries Co., Ltd.), and 0.2 parts of neutral rosin size (product name: CC167, manufactured by Seiko PMC Co., Ltd.) with water, and the paper stock was made into a paper with a basis weight of 58 g / m using a fourdrinier multi-cylinder papermaking machine. 2 A base paper having the above composition was prepared, and oxidized starch (product name: MS3800, manufactured by Nippon Shokuhin Kako Co., Ltd.) was added as a paper strength agent by a pond-type size press at a dry impregnation amount of 2 g / m 2 The paper is then impregnated and dried, and smoothed with a calendar to a basis weight of 60 g / m 2 Thus, a paper substrate having the following composition was obtained.

[0036] (Making wrapping paper) A water-based ionomer emulsion (product name: Chemipearl S-500, manufactured by Mitsui Chemicals, composition: metal salt of ethylene-methacrylic acid copolymer) with a melting point of 89°C was applied to one side of the paper substrate obtained above in a dry coating amount of 4.0 g / m 2 The first resin coating layer was then coated with an air knife coater so that the coating amount was 2.0 g / m2, and the coating was dried to form a first resin coating layer. Then, on the first resin coating layer, a water-based ionomer emulsion with a melting point of 96°C (product name: Chemipearl S-300, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer) was applied until the dry coating amount was 2.0 g / m2. 2 The second resin coating layer was applied using an air knife coater so that the thickness of the first resin coating layer was 66 g / m2. 2 We produced wrapping paper for the following items.

[0037] Example 2 In Example 1, the resin of the second resin coating layer was changed to an aqueous ionomer emulsion with a melting point of 89°C (product name: Chemipearl S-500, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer), and then an aqueous ionomer emulsion with a melting point of 96°C (product name: Chemipearl S-300, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer) was applied on the second resin coating layer in a dry coating amount of 2.0 g / m. 2 A wrapping paper was produced in the same manner as in Example 1, except that the third resin coating layer was provided by coating using an air knife coater so that the coating layer had a thickness of 100 μm and then drying.

[0038] Example 3 In Example 1, a water-based ionomer emulsion (product name: Chemipearl S-300, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer) having a melting point of 96°C was applied on the second resin coating layer in a dry coating amount of 2.0 g / m 2 A wrapping paper was produced in the same manner as in Example 1, except that the third resin coating layer was provided by coating using an air knife coater so that the coating layer had a thickness of 100 μm and then drying.

[0039] Example 4 A packaging paper was prepared in the same manner as in Example 1, except that the resin of the first resin coating layer was changed to an aqueous ethylene-acrylic acid copolymer emulsion having a melting point of 85°C (product name: MICHEM FLEX P1883, manufactured by Michelman Co.).

[0040] Example 5 A packaging paper was prepared in the same manner as in Example 1, except that the resin of the first resin coating layer was changed to an aqueous ethylene-vinyl acetate emulsion with a melting point of 88°C (product name: Aquatex MC-3800, manufactured by Japan Coating Resins Co., Ltd.).

[0041] Example 6 A packaging paper was prepared in the same manner as in Example 1, except that the resin of the second resin coating layer was changed to an aqueous polyvinylidene chloride emulsion having a melting point of 153°C (product name: Saran Latex L411A, manufactured by Asahi Kasei Corporation).

[0042] Example 7 In Example 1, the coating liquid for the first resin coating layer was changed to a coating liquid prepared by adding 50 parts of kaolin clay (product name: Contour 1500, manufactured by Imerys) and 0.1 parts of a dispersant (product name: Aron T-50, manufactured by Toa Gosei) and dispersing the pigment slurry in water using a Coress disperser, to which 100 parts of a water-based ionomer emulsion having a melting point of 89°C (product name: Chemipearl S-500, manufactured by Mitsui Chemicals, composition: metal salt of ethylene-methacrylic acid copolymer) was added as a resin, and further adding water to disperse the pigment slurry. The packaging paper was prepared in the same manner as in Example 1.

[0043] Example 8 (Preparation of coating liquid for underlayer) 20 parts of kaolin clay (trade name: Contour 1500, manufactured by Imerys) and 80 parts of heavy calcium carbonate (trade name: Carbilux, manufactured by Imerys) were mixed with 0.2 parts of a dispersant (trade name: Aron T-50, manufactured by Toa Gosei Co., Ltd.), and water was added and dispersed in water using a Coles disperser to prepare a pigment slurry. 2 parts of phosphated starch (trade name: MS4600, manufactured by Nihon Shokuhin Kako Co., Ltd.) and 30 parts of styrene butadiene copolymer latex (trade name: L-1432X, manufactured by Asahi Kasei Chemicals Co., Ltd., particle size 182 nm) were added to this pigment slurry as a binder, and water was further added to disperse the mixture to prepare a coating liquid for underlayer with a solid concentration of 50%.

[0044] (Preparation of paper substrate with underlayer) On one side of the paper substrate obtained in Example 1, the underlayer coating liquid was applied in a dry amount of 20 g / m 2 The paper is then coated with a blade coater so that the surface is dried and smoothed with a calendar to give a basis weight of 80 g / m 2 A paper base material with an underlayer was prepared.

[0045] (Making wrapping paper) A water-based ionomer emulsion (product name: Chemipearl S-500, manufactured by Mitsui Chemicals, composition: metal salt of ethylene-methacrylic acid copolymer) with a melting point of 89°C was applied to the underlayer surface of the paper base material with an underlayer obtained above in a dry coating amount of 4.0 g / m 2 The first resin coating layer was then coated with an air knife coater so that the coating amount was 2.0 g / m2, and the coating was dried to form a first resin coating layer. Then, on the first resin coating layer, a water-based ionomer emulsion with a melting point of 96°C (product name: Chemipearl S-300, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer) was applied until the dry coating amount was 2.0 g / m2. 2 The coated paper was dried to provide a second resin coating layer, thereby preparing a wrapping paper.

[0046] Example 9 (Preparation of paper substrate) A paper stock was prepared by adding water to 90 parts of hardwood bleached kraft pulp with a Canadian Standard Freeness of 450 mlcsf, 10 parts of softwood bleached kraft pulp with a Canadian Standard Freeness of 520 mlcsf, 0.3 parts of cationic polyacrylamide (product name: Polystron 705, manufactured by Arakawa Chemical Industries Co., Ltd.), and 0.2 parts of a neutral rosin sizing agent (product name: CC167, manufactured by Seiko PMC Co., Ltd.). A base paper was produced using a fourdrinier multi-cylinder papermaking machine, and smoothed using a calendar to give a basis weight of 250 g / m. 2 Thus, a paper substrate having the following composition was obtained.

[0047] (Making wrapping paper) A water-based ionomer emulsion (product name: Chemipearl S-500, manufactured by Mitsui Chemicals, composition: metal salt of ethylene-methacrylic acid copolymer) with a melting point of 89°C was applied to one side of the paper substrate obtained above in a dry coating amount of 4.0 g / m 2 The first resin coating layer was then coated with an air knife coater so that the coating amount was 2.0 g / m2, and the coating was dried to form a first resin coating layer. Then, on the first resin coating layer, a water-based ionomer emulsion with a melting point of 96°C (product name: Chemipearl S-300, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer) was applied until the dry coating amount was 2.0 g / m2. 2The second resin coating layer was applied using an air knife coater so that the coating had a basis weight of 256 g / m. 2 We produced wrapping paper for the following items.

[0048] Comparative Example 1 A wrapping paper was produced in the same manner as in Example 1, except that no resin coating layer was provided.

[0049] Comparative Example 2 In Example 1, the resin of the first resin coating layer was changed to an aqueous ionomer emulsion with a melting point of 96°C (product name: Chemipearl S-300, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer), and packaging paper was prepared in the same manner as in Example 1, except that the second or subsequent resin coating layers were not provided.

[0050] Comparative Example 3 A packaging paper was produced in the same manner as in Example 1, except that the resin in the first resin coating layer was changed to an aqueous polyvinylidene chloride emulsion having a melting point of 153°C (product name: Saran Latex L411A, manufactured by Asahi Kasei Corporation).

[0051] Comparative Example 4 A wrapping paper was prepared in the same manner as in Example 1, except that the resin of the second resin coating layer was changed to an aqueous ionomer emulsion having a melting point of 89°C (product name: Chemipearl S-500, manufactured by Mitsui Chemicals, Inc., composition: metal salt of ethylene-methacrylic acid copolymer).

[0052] Comparative Example 5 A packaging paper was prepared in the same manner as in Example 1, except that the resin of the second resin coating layer was changed to a water-based styrene-acrylic emulsion with a melting point of 187°C (product name: Brightone FC-621, manufactured by Sakata Inx Corporation).

[0053] Comparative Example 6 A packaging paper was prepared in the same manner as in Example 1, except that the resin of the second resin coating layer was changed to a polyvinyl alcohol aqueous solution having a melting point of 180°C (product name: JMR-20H, manufactured by Nippon Vacuum Acetate & Poval Co., Ltd.).

[0054] The wrapping papers obtained in each of the Examples and Comparative Examples were evaluated by the methods described below. The results are shown in Table 1.

[0055] (1) Melting point The melting point of the resin used in the resin coating layer was measured in accordance with JIS K 7121:1987 "Method of measuring transition temperature of plastics."

[0056] (2) Heat seal strength The obtained wrapping paper was cut into two pieces with a width of 15 mm and a length of 15 cm, and the resin surfaces of the wrapping paper were placed together and heat-sealed under certain conditions (adhesion width: 15 mm, temperature: 180°C, pressure: 0.2 MPa, pressing time: 1.0 seconds) using a hot tack tester (manufactured by Labthink, model number: HTT-L1). The heat-sealed sample was then peeled under certain conditions (peeling speed: 300 mm / min) using a peel strength tester (manufactured by Shimadzu Corporation, model number: Autograph AGS-X) to measure the heat seal strength. The higher the value, the higher the heat seal strength. In the present invention, a heat seal strength of 3.00 N / 15 mm or more was determined to be good.

[0057] (3) Heat seal material breakage resistance (2) The peeled surface of the packaging paper after peeling was visually evaluated. ◯: The entire seal portion is broken away from the paper base material and is usable. △: Part of the seal portion is torn from the paper base material, and it is usable. ×: The seal portion is peeled off at the interface of the resin coating layer or is not adhered, and is not usable.

[0058] (4) Water resistance of folded parts The obtained wrapping paper was cut to a size of 8 cm wide and 10 cm long, folded in half with the resin coating layer side facing outward, and a 5 kg metal roll was pressed against the crease and passed back and forth once. The crease was made in the MD (machine direction; the direction in which the papermaking machine moves) of the paper. The folded part was opened, and a methylene blue solution (4 g / L methylene blue dye) was applied to the folded part on the resin coating layer side, wiped off after 30 minutes, and the dyeing condition of the folded part was visually confirmed and evaluated on the following three-level scale. ◯: The folded portion is not dyed and can be used. △: Part of the folded portion is stained, but it can be used. ×: Not usable because more than half of the folded portion was stained or the methylene blue solution had permeated to the opposite side of the resin coating layer.

[0059] (5) Blocking property The obtained wrapping paper was cut to a size of 5 cm wide and 7 cm long, and the resin-coated layer side was placed on top of a PPC paper cut to the same size. The paper was then placed in a thermostatic chamber adjusted to 60°C and 65% RH for 24 hours at 250 g / m 2 After the test, the adhesion between the sample and the PPC was visually evaluated. ◯: The sample does not stick to the PPC paper and can be used. △: There is some sticking between the sample and the PPC paper, but it is slight and usable. ×: The sample was severely stuck to the PPC paper and was not suitable for practical use.

[0060] [Table 1]

[0061] As is clear from Table 1, the packaging papers of the present invention according to Examples 1 to 9 were superior in heat seal strength, heat seal material tear resistance, water resistance at folded parts, and blocking resistance, compared to the packaging papers obtained in Comparative Examples 1 to 6. As these results show, according to the present invention, it is possible to provide packaging paper that reduces the amount of plastic used compared to the amount of conventional polyethylene laminate, and that is also superior in processability, such as water resistance and blocking resistance after folding.

Claims

1. A packaging paper having at least two resin coating layers on at least one side of a paper base material, wherein all of the resin coating layers contain at least one type selected from the group consisting of ionomer, ethylene copolymer, thermoplastic urethane, polyvinylidene chloride, polylactic acid, and polybutylene succinate, and the layers other than the outermost layer of the resin coating layers contain at least one type of resin having a melting point lower than the melting point of the resin in the outermost layer.

2. The total coating amount of the resin coating layer on one side is 2 to 20 g / m 2 The wrapping paper according to claim 1, characterized in that the thickness is in the range of

3. 3. The wrapping paper according to claim 1, wherein the melting point of the resin in the outermost layer of the resin coating layer is 90° C. or higher.

4. 3. The wrapping paper according to claim 1, wherein a pigment is contained in at least one layer other than the outermost layer of the resin coating layer.

5. 3. The wrapping paper according to claim 1, further comprising an underlayer containing a pigment and a binder between the paper base material and the resin coating layer.

6. 3. The packaging paper according to claim 1, wherein the paper base material contains bleached softwood kraft pulp.

7. 3. The packaging paper according to claim 1, wherein the paper base material contains polyacrylamide as a paper strength agent.

8. 3. The packaging paper according to claim 1 or 2, wherein the pulp used in the paper base material has a Canadian standard freeness of 250 to 650 ml CSF.

9. 3. The packaging paper according to claim 1, wherein the difference in melting point between the resin having a low melting point and the resin of the outermost layer is 5° C. to 85° C.

10. The ionomer is a metal salt of an ethylene-acrylic acid or ethylene-methacrylic acid copolymer, and / or 3. The wrapping paper according to claim 1, wherein the ethylene copolymer is an ethylene-acrylic acid copolymer, an ethylene-methacrylic acid copolymer, an ethylene-acrylic acid ester copolymer, an ethylene-methacrylic acid ester copolymer, and / or an ethylene-vinyl acetate copolymer.

Citation Information

Patent Citations

  • Oilproof paper for food

    JP2006028697A

  • Low density paper

    JP2006037291A

  • Multilayer coated paper

    JP2007063693A

  • Multilayer film and soft bag for medical treatment

    JP2007245490A

  • Coated paper for printing use

    JP2007277772A

Cited By

  • Oil-resistant agent composition and oil-resistant base material

    WO2026116222A1