Manufacturing method for semiconductor device
The method of laser-induced substrate separation in semiconductor manufacturing addresses the challenge of thermal damage by using films with high thermal conductivity and expansion coefficients, improving yield and reusability.
Patent Information
- Application Number
- JP2023044617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The challenge in manufacturing semiconductor devices lies in appropriately separating bonded substrates without causing thermal damage to the substrate, which affects the manufacturing yield and reusability of the substrates.
A method involving laser irradiation is used to separate substrates by focusing on specific films with materials that have higher thermal conductivity and expansion coefficients, allowing for controlled heat distribution and stress generation at the interface to facilitate separation while minimizing thermal damage.
This approach enhances the manufacturing yield of semiconductor devices by enabling efficient separation of substrates while preserving their integrity, allowing for easy reuse of the separated substrates.
Smart Images

Figure 2024134358000001_ABST
Abstract
Description
[Technical field]
[0001] The present embodiment relates to a method for manufacturing a semiconductor device. [Background technology]
[0002] When manufacturing a semiconductor device, two substrates are bonded together and then one of the substrates is separated. It is desirable to perform this separation appropriately. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-103725 [Patent Document 2] JP 2021-106197 A [Patent Document 3] International Publication No. 2020 / 213478 [Patent Document 4] International Publication No. 2021 / 010284 [Patent Document 5] International Publication No. 2021 / 131710 [Patent Document 6] International Publication No. 2021 / 131711 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of one embodiment is to provide a method for manufacturing a semiconductor device that can properly perform separation after substrate bonding. [Means for solving the problem]
[0005] According to one embodiment, a method for manufacturing a semiconductor device is provided. The method for manufacturing a semiconductor device includes stacking a first film on a first substrate, and stacking a second film, a third film, and a fourth film on a second substrate. The method for manufacturing a semiconductor device includes bonding a main surface of the first film opposite to the first substrate and a main surface of the fourth film opposite to the second substrate. The method for manufacturing a semiconductor device includes irradiating a laser beam from the side of the second substrate so that a focal point is located near the second film. The method for manufacturing a semiconductor device includes separating the second substrate. The second film and the fourth film each include a first material. The third film includes a second material. The second material is different from the first material. [Brief description of the drawings]
[0006] [Figure 1] 3 is a flowchart showing a method for manufacturing a semiconductor device according to the embodiment. [Diagram 2] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Diagram 3] 1A to 1C are enlarged cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Figure 4] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Diagram 5] 1A to 1C are enlarged cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Figure 6] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Figure 7] 5A and 5B are diagrams showing temperature distributions on a substrate when irradiated with laser light in an embodiment. [Figure 8] FIG. 4 is a cross-sectional view showing a heat flow in a substrate during laser light irradiation in an embodiment. [Figure 9] 5A and 5B are diagrams showing thermal conductivity and thermal diffusivity in the embodiment. [Figure 10] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Figure 11] FIG. 4 is a cross-sectional view showing the generation of stress in the embodiment. [Figure 12] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Figure 13]1A to 1C are enlarged cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment. [Figure 14] FIG. 11 is a diagram showing a temperature distribution of a substrate when irradiated with laser light in a first modified example of the embodiment. [Figure 15] FIG. 11 is a diagram showing a temperature distribution of a substrate when irradiated with laser light in a second modified example of the embodiment. [Figure 16] FIG. 13 is a diagram showing a temperature distribution of a substrate when irradiated with laser light in a fourth modified example of the embodiment. [Figure 17] FIG. 13 is a diagram showing a temperature distribution on a substrate when irradiated with laser light in a fifth modified example of the embodiment. [Figure 18] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to a sixth modified example of the embodiment. [Figure 19] FIG. 13 is a plan view showing a method for manufacturing a semiconductor device according to a sixth modified example of the embodiment. [Figure 20] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to a seventh modified example of the embodiment. [Figure 21] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to an eighth modified example of the embodiment. [Figure 22] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to an eighth modified example of the embodiment. [Figure 23] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to an eighth modified example of the embodiment. [Figure 24] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to an eighth modified example of the embodiment. [Diagram 25] 13A to 13C are cross-sectional views showing a method for manufacturing a semiconductor device according to a ninth modification of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, a method for manufacturing a semiconductor device according to an embodiment will be described in detail with reference to the accompanying drawings. Note that the present invention is not limited to the embodiment.
[0008] (Embodiment) In the following, the other of the two substrates to be joined that remains unpeeled is taken as the reference, the direction perpendicular to the main surface of the other substrate is taken as the Z direction, and the two directions perpendicular to each other in a plane perpendicular to the Z direction are taken as the X direction and the Y direction.
[0009] For example, the manufacturing method of the semiconductor device 1 can be performed as shown in FIG. 1 to FIG. 13. FIG. 1 is a flow chart showing the manufacturing method of the semiconductor device 1. FIG. 2(a) to FIG. 2(f), FIG. 3(a), FIG. 3(b), FIG. 4(a) to FIG. 4(b), FIG. 5, FIG. 6(a) to FIG. 6(c), FIG. 10(a) to FIG. 10(c), FIG. 11, FIG. 12(a) to FIG. 12(e), and FIG. 13 are YZ cross-sectional views showing the manufacturing method of the semiconductor device 1. FIG. 3(a) is an enlarged cross-sectional view of FIG. 2(b). FIG. 3(b) is an enlarged cross-sectional view of FIG. 2(e). FIG. 5 is an enlarged cross-sectional view of FIG. 4(a). FIG. 13 is an enlarged cross-sectional view corresponding to FIG. 12(c). FIG. 11 is a YZ cross-sectional view showing the generation of stress. FIG. 7 is a view showing the temperature distribution of the substrate when irradiated with laser light. FIG. 8 is a cross-sectional view showing the heat flow of the substrate when irradiated with laser light. FIG. 9 is a view explaining the thermal conductivity and the thermal diffusivity.
[0010] In the manufacturing method of the semiconductor device 1, as shown in Fig. 1, the processing of the lower substrate (S1-S2) and the processing of the upper substrate (S3-S4) are performed, for example, in parallel. The lower substrate is the substrate that is disposed on the -Z side of the two substrates to be joined when they are joined. The upper substrate is the substrate that is disposed on the +Z side of the two substrates to be joined when they are joined.
[0011] In preparation of the lower substrate (S1), as shown in Fig. 2(a), a substrate (lower substrate) 2 is prepared. The substrate 2 may be formed of a material mainly composed of a semiconductor (e.g., silicon) that does not substantially contain impurities.
[0012] In the film formation (S2), a predetermined device structure is formed on the main surface 2a side (+Z side) of the substrate 2, as shown in FIG. 2(b).
[0013] For example, a peripheral circuit structure PHC as shown in Fig. 3(a) may be formed. Impurities are introduced near the main surface 2a on the +Z side of the substrate 2 to form a semiconductor region SR. A conductive pattern GT is formed on the main surface 2a of the substrate 2. This forms a plurality of transistors TR, each of which includes a semiconductor region SR and a conductive pattern GT. The peripheral circuit structure PHC including the plurality of transistors TR functions as a peripheral circuit for the memory cell array structure MAR described later.
[0014] After a predetermined device structure is formed, a film 3 covering the main surface 2a of the substrate 2 is formed by a CVD method or the like. For example, an interlayer insulating film 40 is deposited on the main surface 2a of the substrate 2. The interlayer insulating film 40 may be formed of a material mainly composed of an insulating material, or may be formed of a material mainly composed of a semiconductor oxide (e.g., silicon oxide). In addition, holes are processed in the interlayer insulating film 40 while the interlayer insulating film 40 is being deposited, and a conductive material is filled in the holes, or a conductive pattern is formed, thereby forming a wiring structure WR electrically connected to the transistor TR. An electrode PD1 electrically connected to the wiring structure WR is formed on the main surface 40a of the +Z side of the interlayer insulating film 40 by plating or the like. For simplification, in FIG. 2(b) and subsequent figures, a film including the conductive pattern GT, the wiring structure WR, the electrode PD1, and the interlayer insulating film 40 is illustrated and described as a film 3. In addition, since the interlayer insulating film 40 occupies the majority of the film 3 in terms of volume, the film 3 is treated as being formed of a material mainly composed of a semiconductor oxide (e.g., silicon oxide). The device structure shown in FIG. 3(a) is just an example and is not particularly limited.
[0015] In preparation of the upper substrate (S3), a substrate (upper substrate) 100 is prepared as shown in Fig. 2(c). The substrate 100 may be formed of a material mainly composed of a semiconductor (e.g., silicon) that does not substantially contain impurities.
[0016] In the film formation (S4), as shown in FIG. 2(d), the film 6 is deposited on the main surface 100b side of the substrate 100 by a CVD method or the like. The film 6 may be formed of any material having a higher absorptance of infrared light than the substrate 100. The film 6 may be formed of, for example, a material having a higher absorptance of a laser wavelength (e.g., 9.2 μm or more and 10.8 μm or less) suitable for the film 4 to function as a laser absorption layer than the substrate 100. The film 6 may be formed of a material that can be removed by wet etching. The film 6 may be formed of a material mainly composed of a semiconductor oxide (e.g., silicon oxide). The film 6 may have any thickness suitable for functioning as a laser absorption layer, and may be, for example, 0.1 μm or more and 1 μm or less.
[0017] As shown in FIG. 2(e), the film 5 is deposited on the −Z side of the film 6 by a CVD method or the like. The film 5 may be formed of any material having a thermal expansion coefficient larger than that of the film 6. The film 5 may be formed of any material having a thermal conductivity larger than that of the film 6. The film 5 may be formed of any material having a thermal diffusivity larger than that of the film 6. The film 5 may be formed of a material mainly composed of a polycrystalline material (e.g., polycrystalline silicon) of a semiconductor, or a material mainly composed of an amorphous material (e.g., amorphous silicon) of a semiconductor. The film 5 may be formed of a material mainly composed of a porous material (e.g., porous silicon) of a semiconductor. When the film 5 is formed of a material mainly composed of porous silicon, the porosity may be 40% or more and 90% or less, and preferably 50% or more and 90% or less. The porosity may be a value measured by spectroscopic ellipsometry or a gas adsorption method. The thickness of film 5 may be any thickness suitable for the interface with film 6 to become a peel interface, and may be, for example, 0.05 μm or more and 1 μm or less, preferably 0.05 μm or more and 0.2 μm or less.
[0018] On the −Z side of the film 5, the film 4 is deposited by a CVD method or the like, as shown in FIG. 2(f).
[0019] For example, a film 4 including a memory cell array structure MAR as shown in FIG. 3(b) may be formed. After depositing an insulating film 60 on the −Z side of the film 5, a conductive film is deposited and the conductive film is patterned to form a conductive layer SL. The insulating film 60 may be formed of an insulator such as silicon oxide. The conductive layer SL may be formed of a semiconductor provided with conductivity such as polysilicon containing impurities. Then, an insulating layer and a sacrificial layer (not shown) are alternately deposited multiple times on the +Z side of the conductive layer SL to form a stacked body LM. The insulating layer may be formed of an insulator such as silicon oxide. The sacrificial layer may be formed of an insulator capable of ensuring an etching selectivity between the insulating layer and the insulating layer such as silicon nitride. Each insulating layer and each sacrificial layer may be deposited with approximately the same film thickness.
[0020] A resist pattern with linear openings extending in the Y direction is formed on the -Z side of the laminate LM. Using the resist pattern as a mask, anisotropic etching such as RIE (Reactive Ion Etching) is performed to form a groove penetrating the laminate LM in the YZ direction. Then, a dividing film (not shown) is embedded in the groove. The dividing film may be formed of a material mainly composed of an insulator (e.g., silicon oxide). The dividing film extends in the YZ direction on the -X side of the laminate LM. The dividing film divides the laminate LM from the other laminates LM on the -X side. In each laminate LM, insulating layers and sacrificial layers are alternately stacked multiple times. Each laminate LM has a substantially rectangular shape with the Y direction as the longitudinal direction in the XY plane view.
[0021] A resist pattern with an opening corresponding to the position where the memory hole is to be formed is formed on the -Z side of each laminate LM. Anisotropic etching such as RIE is performed using the resist pattern as a mask to form a memory hole that penetrates the laminate LM and reaches the conductive layer SL.
[0022] A block insulating film, a charge storage film, and a tunnel insulating film are deposited in this order on the side and bottom of the memory hole. The block insulating film may be made of an insulating material such as silicon oxide. A portion of the tunnel insulating film on the bottom of the memory hole is selectively removed.
[0023] A semiconductor film is deposited on the side and bottom surfaces of the memory hole. The semiconductor film may be made of a material mainly composed of a semiconductor (e.g., polysilicon). Then, a core member is embedded in the memory hole. The core member may be made of an insulator such as silicon oxide. This forms a plurality of pillars PL each penetrating the stack LM in the Z direction. The plurality of pillars PL are formed so as to be arranged in the XY directions.
[0024] The sacrificial layer of the laminate LM is removed. A block insulating film is formed on the exposed surface of the void formed by the removal. The block insulating film may be made of an insulator such as aluminum oxide. A conductive layer WL is further embedded in the void. The conductive layer WL may be made of a material mainly composed of a conductor (e.g., a metal such as tungsten). This forms a laminate LM in which the conductive layers WL and insulating layers are alternately and repeatedly stacked. A memory cell is formed at the position where the conductive layer WL intersects with the semiconductor film of the pillar PL. That is, a memory cell array structure MAR is formed in which a plurality of memory cells are arranged three-dimensionally.
[0025] An interlayer insulating film 50 is further formed to cover the laminate LM. By repeatedly forming a resist pattern and slimming and etching, a staircase structure is formed in which the conductive layers WL are drawn out in a staircase shape on both sides of the laminate LM in the Y direction. A conductive plug CC electrically connected to each conductive layer WL is formed by forming holes in the interlayer insulating film 50 and filling a conductive material therein. In addition, as the interlayer insulating film 50 is deposited, holes are processed in the interlayer insulating film 50, a conductive material is filled in the interlayer insulating film 50, and a conductive pattern is formed, thereby forming a wiring structure WR2 electrically connected to the conductive plug CC. An electrode PD2 electrically connected to the wiring structure WR2 is formed on the main surface 50a on the -Z side of the interlayer insulating film 50 by plating or the like. In FIG. 2(f) and subsequent figures, for simplification, a film including the memory cell array structure MAR, the conductive plug CC, the wiring structure WR2, the electrode PD2, and the interlayer insulating films 50 and 60 is illustrated and described as a film 4. In addition, since the interlayer insulating film 60 is the part of interest in this embodiment, the material of the film 4 is mainly treated as the material of the interlayer insulating film 60. Note that the device structure shown in Fig. 3(b) is an example and is not particularly limited. Also, although one memory cell array structure MAR is shown in Fig. 3(b), there may be a plurality of memory cell array structures.
[0026] The film 4 may be formed of approximately the same material as the film 6. The film 4 may be formed of any material having a higher absorptance of infrared light than the substrate 100. The film 4 may be formed of, for example, a material having a higher absorptance than the substrate 100 at a laser wavelength (e.g., 9.2 μm or more and 10.8 μm or less) suitable for the film 4 to function as a laser absorbing layer. The film 6 may be formed of a material containing a semiconductor oxide (e.g., silicon oxide) as a main component. The film 4 may have any thickness suitable for functioning as a laser absorbing layer, and may be, for example, 0.1 μm or more and 1 μm or less.
[0027] As shown in FIG. 1, when the processing of the lower substrate (S1-S2) and the processing of the upper substrate (S3-S4) are both completed, the upper substrate and the lower substrate are bonded (S5). The main surface 3a (see FIG. 2(b)) on the +Z side of the film 3 and the main surface 4b (see FIG. 2(f)) on the -Z side of the film 4 are activated by plasma irradiation or the like, and the substrate 2 and the substrate 100 are disposed opposite to each other in the Z direction so that the main surfaces 3a and 4b face each other, as shown in FIG. 2(g). As shown in FIG. 2(g), FIG. 4(a) and FIG. 5, the XY position of the substrate 2 and the XY position of the substrate 100 are aligned so that the XY position of the electrode PD1 on the main surface 3a corresponds to the XY position of the electrode PD2 on the main surface 4b. As shown in FIG. 4(a) and FIG. 5, the substrate 2 and the substrate 100 are brought close to each other in the Z direction, and the main surface 3a on the substrate 2 side and the main surface 4b on the substrate 100 side are bonded. At this time, atoms of the main surface 3a and atoms of the main surface 4b are bonded by hydrogen bonds or the like, and the substrate 2 and the substrate 100 are temporarily bonded to each other.
[0028] Therefore, as shown in FIG. 1, a heat treatment (annealing) is performed at a relatively low temperature (S6). In the heat treatment (annealing), the substrate 2 and the substrate 100 are heated as a whole, as shown by the dotted arrow in FIG. 4(b). In the heat treatment, for example, the substrate 2 and the substrate 100 are each heated to a relatively low temperature (i.e., an allowable temperature of the device structure, for example, about 200° C.) for a predetermined time. At this time, the atoms of the main surface 3a and the atoms of the main surface 4b are bonded by covalent bonds or the like due to water molecules being removed from the interface, and the substrate 2 and the substrate 100 are in a fully bonded state. As a result, a bonded body CB of the substrate 2 and the substrate 100 is formed. At this time, the electrode PD1 and the electrode PD2 are bonded by direct bonding, and the peripheral circuit structure PHC and the memory cell array structure MAR can be electrically connected.
[0029] When S6 shown in FIG. 1 is completed, laser light 200 is irradiated from the substrate 100 side (S7).
[0030] The laser light is irradiated with laser light 200 having a wavelength range (for example, a wavelength range of 9.2 μm or more and 10.8 μm or less) in which the light absorption rate of the film 6 and film 4, which are the laser absorbing layers, is higher than that of the substrate 100. A pulsed laser is used as the laser light 200. An infrared laser may be used as the laser light 200. A carbon dioxide laser (CO2 laser) may be used as the laser light 200. Absorption of the laser light 200 occurs depending on the absorption coefficient and thickness of the substrate or film, and in this structure, laser absorption occurs mainly in the film 6 and film 4, which are the laser absorbing layers.
[0031] In addition, in a laser irradiation device having a stage and a light source, the light source may gradually move from the center position of the substrate to the outer periphery position while the stage is rotated. In this case, it is possible to realize an irradiation pattern of a spot area from the center position to the outer periphery position along a spiral orbit OB (not shown). The light source may move from the outer periphery position to the center position.
[0032] For example, as shown in FIG. 6(a), the XY plane position to be irradiated with the first laser beam 200 is determined, and the focus of the laser beam 200 is adjusted to be located within the film 6. The XY plane position to be irradiated may be the starting position of the spiral trajectory OB. The absorptance of the laser beam 200 in the film 6 is greater than that of the substrate 100, and the absorptance of the laser beam 200 in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200 irradiated to the film 6 through the substrate 100 is absorbed mainly in the vicinity of the irradiation point in the film 6 and the film 4, and the film 6 and the film 4 are locally heated at the XY plane position.
[0033] For example, as shown in Figures 7(a) and 7(b), localized heat generation in film 6 and film 4 causes the temperatures of film 6 and film 4 to become high at the XY position. At this time, the thermal conductivity of film 5 is greater than that of film 6, and the thermal conductivity of film 5 is greater than that of film 4. As a result, as shown in Figure 8(b), the heat in film 6 is transferred to substrate 100 in the +Z direction and to film 5 in the -Z direction.
[0034] As shown in Figure 9, if a material has a high thermal conductivity (W / (m K)), the heat flow (W) is large and a lot of heat (J) is transferred per unit time and temperature gradient. On the other hand, even if heat (J) is transferred, if the heat capacity (J / K) is large, the temperature (K) does not increase easily. If the thermal conductivity is relatively large compared to the heat capacity (J / K), the temperature (K) increases easily. In other words, the thermal diffusivity (m 2 / s) = Thermal conductivity (W / (m K) / (specific heat (J / (kg K) × density (kg / m 3 If the linear expansion coefficient (1 / K) is higher than that of film 6 or film 4, the difference in linear expansion coefficient can cause large stress at the interface between the two.
[0035] The thermal diffusivity of film 5 shown in Fig. 7(a) is greater than that of film 6, which in turn is greater than that of film 4. Therefore, as shown in Fig. 8(b), the heat transferred to film 5 is further transferred in the XY directions within film 5. This forms a heat flow that pulls the heat within film 6 toward film 5, and as shown in Figs. 7(b) and 7(c), the temperature of substrate 100 can be suppressed to a target temperature Tth or lower, and the temperature of film 5 can be increased to near maximum temperature T1.
[0036] At this time, the thermal expansion coefficient of film 5 is larger than that of film 6, which is larger than that of film 4. As the temperature of film 5 rises, film 5 expands more than films 6 and 4. As a result, stress due to the difference in expansion at that XY plane position is generated at the interface between films 5 and 6. As a result, as shown in FIG. 6(b), peeling occurs at the interface between films 5 and 6 at that XY plane position. Alternatively, peeling may occur at the interface between films 5 and 4.
[0037] As shown in FIG. 6(c), the XY plane position to which the second laser beam 200 is to be irradiated is determined to be a position shifted in the XY plane direction from the XY plane position in FIG. 6(a), and the focus of the laser beam 200 is adjusted to be located within the film 6. The position shifted in the XY plane direction from the XY plane position in FIG. 6(a) may be a position shifted from the start position along the spiral trajectory OB. The absorptance of the laser beam 200 in the film 6 is greater than that of the substrate 100, and the absorptance of the laser beam 200 in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200 irradiated to the film 6 through the substrate 100 is mainly absorbed at the irradiated portion within the film 6, and the film 6 and film 4 are locally heated at the XY plane position.
[0038] For example, as shown in Figures 7(a) and 7(b), localized heat generation in film 6 and film 4 causes the temperatures of film 6 and film 4 to become high at the XY position. At this time, the thermal conductivity of film 5 is greater than that of film 6, and the thermal conductivity of film 5 is greater than that of film 4. As a result, as shown in Figure 8(b), the heat in film 6 is transferred to substrate 100 in the +Z direction and to film 5 in the -Z direction.
[0039] The thermal diffusivity of film 5 is greater than that of film 6, which in turn is greater than that of film 4. Therefore, as shown in Fig. 8(b), the heat transferred to film 5 is further transferred in the XY directions within film 5. This forms a heat flow that pulls the heat within film 6 toward film 5, and as shown in Figs. 7(b) and 7(c), the temperature of substrate 100 can be suppressed to a target temperature Tth (e.g., 600°C) or lower, and the temperature of film 5 can be increased to near maximum temperature T1.
[0040] At this time, the thermal expansion coefficient of film 5 is larger than that of film 6, which is larger than that of film 4. As the temperature of film 5 rises, film 5 expands more than films 6 and 4. As a result, stress due to the difference in expansion at that XY plane position occurs at the interface between films 5 and 6. As a result, as shown in FIG. 10(a), peeling occurs at the interface between films 5 and 6 at that XY plane position. Alternatively, peeling may occur at the interface between films 5 and 4.
[0041] As shown in FIG. 10(b), the final XY plane position to which the final Nth irradiation of the laser beam 200 should be irradiated is determined, and the focal point of the laser beam 200 is adjusted to be located within the film 4. N is any integer equal to or greater than 3. The final XY plane position may be the final position along the spiral trajectory OB. The absorptance of the laser beam 200 in the film 6 is greater than that of the substrate 100, and the absorptance of the laser beam 200 in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200 irradiated to the film 6 through the substrate 100 is absorbed mainly at the irradiated portion within the film 6, and the film 6 and film 4 are locally heated at the XY plane position.
[0042] For example, as shown in Figures 7(a) and 7(b), localized heat generation in film 6 and film 4 causes the temperatures of film 6 and film 4 to become high at the XY position. At this time, the thermal conductivity of film 5 is greater than that of film 6, and the thermal conductivity of film 5 is greater than that of film 4. As a result, as shown in Figure 8(b), the heat in film 6 is transferred to substrate 100 in the +Z direction and to film 5 in the -Z direction.
[0043] The thermal diffusivity of film 5 is greater than that of film 6, which in turn is greater than that of film 4. Therefore, as shown in Fig. 8(b), the heat transferred to film 5 is further transferred in the XY directions within film 5. This forms a heat flow that pulls the heat within film 6 toward film 5, and as shown in Figs. 7(b) and 7(c), the temperature of substrate 100 can be suppressed to a target temperature Tth or lower, and the temperature of film 5 can be increased to near maximum temperature T1.
[0044] At this time, the thermal expansion coefficient of film 5 is larger than that of film 6, which is larger than that of film 4. As the temperature of film 5 rises, film 5 expands more than films 6 and 4. As a result, stress due to the difference in expansion at that XY plane position is generated at the interface between films 5 and 6. As a result, as shown in FIG. 10(c), films 5 and 6 peel off at the interface at that XY plane position. Alternatively, films 5 and 4 may peel off at the interface.
[0045] By irradiating the film 6 with the laser light 200 so that a plurality of spot regions are distributed two-dimensionally, the main surface 5a on the +Z side of the film 5 has two-dimensionally distributed convex portions 5a2, as shown in Fig. 11. On the main surface 5a, the plurality of convex portions 5a2 are arranged spaced apart from each other in the XY directions. This can generate local stresses in which each of the plurality of convex portions 5a2 on the main surface 5a pushes the film 6 outward in the XY directions near the main surface 6b, as shown by the dotted arrows in Fig. 11.
[0046] Note that local stress occurs at multiple locations spaced apart from each other in the XY directions at the interface between films 5 and 6 and at the interface between films 5 and 4. If the temperature at the interface between films 5 and 6 is higher than the temperature at the interface between films 5 and 4, the stress at the interface between films 5 and 6 may be larger than the stress at the interface between films 5 and 4. For simplification, Fig. 11 selectively shows the local stress occurring at the interface between films 5 and 6, which is relatively large.
[0047] As a result, peeling occurs at the interface between the film 5 and the film 6 (S8). In the peeling, the laminate 8 is peeled off from the laminate 7, as shown in Fig. 12(a). In the laminate 7, the film 3, the film 4, and the film 5 are laminated on the substrate 2. In the laminate 8, the film 6 is laminated on the substrate 100. For example, since local stress is generated at the multiple protrusions 5a2 distributed two-dimensionally, the laminate 8 is easily peeled off from the laminate 7 starting from the multiple protrusions 5a2.
[0048] In consideration of subsequent processing, the laminate 7 has a peeled surface treated (S9) as shown in Fig. 1. In the laminate 7, as shown in Fig. 12(b), a plurality of convex portions 5a2 are distributed in the XY direction on the main surface 5a on the +Z side of the film 5, and a plurality of convex portions 5b2 are distributed in the XY direction on the main surface 5b on the -Z side of the film 5. The film 5 is removed by dry etching or wet etching.
[0049] 12(c), in the laminate 7a from which the film 5 has been removed, a plurality of recesses 4a2 each corresponding to a protrusion 5b2 are distributed in the XY direction on the main surface 4a on the +Z side of the film 4. The main surface 4a of the film 4 is polished and flattened by a CMP method or the like.
[0050] As a result, as shown in FIG. 12(d), a semiconductor device 1 is obtained in which the film 3 and the film 4 are laminated on the substrate 2 and the main surface 4a of the film 4 is flattened.
[0051] 13, after planarization, holes are formed in the main surface 60a on the +Z side of the interlayer insulating film 60 and a conductive material is filled in to form a conductive plug PG electrically connected to the conductive layer SL. An electrode pattern EL electrically connected to the conductive plug PG is formed on the main surface 60a of the interlayer insulating film 60 by plating or the like. Although not shown, an electrode pattern EL connected to the peripheral circuit structure PHC, bypassing the memory cell array structure MAR, is also formed on the main surface 60a of the interlayer insulating film 60. This makes it possible to supply power, signals, etc. from the outside to the memory cell array structure MAR and the peripheral circuit structure PHC.
[0052] The film 4 including the memory cell array structure MAR can be regarded as a chip region for the memory cell array, and the film 3 including the peripheral circuit structure PHC and the substrate 2 can be regarded as a chip region for the peripheral circuit. The semiconductor device 1 has a structure obtained by directly bonding the chip region for the memory cell array and the chip region for the peripheral circuit. This structure is also called CBA (CMOS directly bonded to array). In the CBA, the number of chip regions for the memory cell array bonded to the +Z side of the chip region for the peripheral circuit is not limited to one, and may be two or more.
[0053] On the other hand, the peeled substrate 100 is reused (S10) as shown in Fig. 1. The substrate 100 may be reused as an upper substrate 100 as shown by the solid arrow in Fig. 2.
[0054] 12(d), in the laminate 8 immediately after peeling, the main surface 100b on the -Z side of the substrate 100 is covered with the film 6. The film 6 is removed by wet etching.
[0055] For example, when film 6 is formed of a material mainly composed of a semiconductor oxide (e.g., silicon oxide), it can be easily removed by wet etching while maintaining an etching selectivity with the material of substrate 100 (e.g., a semiconductor such as silicon).
[0056] As a result, the substrate 100 is obtained as shown in Fig. 12(e). The substrate 100 shown in Fig. 12(e) can be easily reused, for example, as the upper substrate 100. In addition, since polishing by a CMP method or the like is not required, the substrate 100 can be reused in almost its original state.
[0057] Instead of being reused as the upper substrate 100, the peeled substrate 100 may be reused as the lower substrate 2 as indicated by the dotted arrow in FIG.
[0058] As described above, in the embodiment, after the substrate 2 on which the film 3 is laminated and the substrate 100 on which the film 6, the film 5, and the film 4 are laminated are joined, the laser light 200 is irradiated from the side of the substrate 100 so that the focal point is located near the film 6. For example, the film 6 and the film 4 are formed of substantially the same material, and the material of the film 5 is different from the material of the film 6 and the film 4. The material of the film 5 may have a higher thermal expansion coefficient than the material of the film 6 and the film 4. Furthermore, the material of the film 5 may have a higher thermal conductivity and a higher thermal diffusivity than the material of the film 6 and the film 4. This allows the film 6 and the film 4 to absorb the laser light, draw the heat in the film 6, etc., to the film 5 side, and easily diffuse it in the film 5, and local stress can be generated at the interface between the film 5 and the film 6 separated from the substrate 100 in the Z direction. As a result, the substrate 100 can be easily separated from the substrate 2 while suppressing thermal damage to the substrate 100 (for example, lattice distortion due to thermal stress, etc.). Therefore, it is possible to improve the manufacturing yield of the semiconductor device 1 including the substrate 2, and to easily reuse the substrate 100. That is, the separation of the substrate 100 during the manufacture of the semiconductor device 1 can be appropriately performed.
[0059] In addition, in the embodiment, when the upper substrate 100 is separated, the film 6 is interposed between the peeling interface and the upper substrate 100. That is, peeling is performed at the interface between the film 5 and the film 6 spaced from the substrate 100 in the Z direction, and the laminate 8 can be peeled off from the laminate 7. Then, the film 6 is removed from the laminate 8 by wet etching. This makes it possible to suppress damage to the substrate 100 during peeling, and to suppress damage to the substrate 100 during the subsequent removal of the film 6. As a result, peeling can be performed well, and the substrate 100 can be reused in almost its original state.
[0060] For example, as shown in Fig. 8(a), when the film 6 and the film 4 absorb the laser light, if most of the heat is directed toward the substrate 100, the substrate 100 will suffer thermal damage (e.g., lattice distortion due to thermal stress, etc.). If the thermal damage is large, there is a possibility that the damage cannot be completely repaired even if a heat treatment is subsequently performed to repair the damage. This may make it difficult to reuse the substrate 100.
[0061] In contrast, in this embodiment, the laser is absorbed by the films 6 and 4, and the heat in the film 6 etc. is drawn to the film 5 side and can be easily diffused in the film 5, so that local stress can be generated at the interface between the films 5 and 6 separated from the substrate 100 in the Z direction. As a result, the substrate 100 can be easily separated from the substrate 2 while suppressing thermal damage to the substrate 100 (for example, lattice distortion due to thermal stress etc.). Therefore, the manufacturing yield of the semiconductor device 1 including the substrate 2 can be improved, and the substrate 100 can be easily reused.
[0062] The separation of the substrate 100 may be performed by peeling at the interface between the film 5 and the film 4 instead of peeling at the interface between the film 5 and the film 6 (see FIG. 12(a)).
[0063] Moreover, the material of film 5 can be any material that efficiently absorbs heat from the materials of films 6 and 4, that easily increases its own temperature, and that has large thermal expansion.
[0064] (Variation 1) As a first modification of the embodiment, the material of the film 5i may be a material mainly composed of a semiconductor nitride (e.g., silicon nitride) as shown in Fig. 14. Fig. 14 is a diagram showing the temperature distribution of the substrate during laser light irradiation in the first modification of the embodiment. The film 5i may have any thickness suitable for the interface with the film 6 to become a peeling interface, and may be, for example, 0.05 µm to 1 µm, and preferably 0.05 µm to 0.2 µm.
[0065] For example, when laser light 200 is irradiated from the side of substrate 100 as shown in FIG. 6(a), localized heating of films 6 and 4 causes the temperatures of films 6 and 4 to become high at the XY position as shown in FIG. 14(a) and FIG. 14(b).
[0066] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5i is a material mainly composed of a semiconductor nitride (e.g., silicon nitride) and has a higher thermal conductivity than the material of films 6 and 4.
[0067] As a result, as shown in FIG. 8(b), the heat in the film 6 is transferred to the substrate 100 in the +Z direction, and is also transferred to the film 5i in the -Z direction.
[0068] When the material of the films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of the film 5i shown in FIG. 14(a) is a material mainly composed of a semiconductor nitride (e.g., silicon nitride) and has a higher thermal diffusivity than the material of the films 6 and 4.
[0069] Therefore, as shown in Fig. 8(b), the heat transferred to the film 5i is further transferred in the XY directions within the film 5i. This forms a heat flow that pulls the heat within the film 6 toward the film 5i, and as shown in Fig. 14(b) and Fig. 14(c), the temperature of the substrate 100 can be suppressed to a target temperature Tth or lower, and the temperature of the film 5i can be increased to near the maximum temperature T11.
[0070] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5i is a material mainly composed of a semiconductor nitride (e.g., silicon nitride) and has a larger thermal expansion coefficient than the material of films 6 and 4.
[0071] Therefore, as the temperature of film 5i rises, stress due to the difference in thermal expansion coefficient at the XY plane position occurs at the interface between film 5i and film 6 and the interface between film 5 and film 4. As a result, as shown in Fig. 6(b), film 5i expands toward film 6 at the XY plane position, and film 5i expands toward film 4.
[0072] In this way, by using a material containing a semiconductor nitride (e.g., silicon nitride) as the main component as the material for film 5i, the laser light is absorbed by films 6 and 4, the heat from within film 6 etc. is drawn toward film 5i and can be easily diffused within film 5i, and local stress can be generated at the interface between films 5 and 6 spaced apart from substrate 100 in the Z direction.
[0073] (Variation 2) As a second modified example of the embodiment, the material of the film 5j may be a material mainly composed of a metal oxide (e.g., aluminum oxide) as shown in Fig. 15. Fig. 15 is a diagram showing the temperature distribution of the substrate during laser light irradiation in the second modified example of the embodiment. The film 5j may have any thickness suitable for the interface with the film 6 to become a peeling interface, and may be, for example, 0.05 µm or more and 1 µm or less, and preferably 0.05 µm or more and 0.2 µm or less.
[0074] For example, when laser light 200 is irradiated from the side of substrate 100 as shown in FIG. 6(a), localized heating of films 6 and 4 causes the temperatures of films 6 and 4 to become high at the XY position as shown in FIG. 15(a) and FIG. 15(b).
[0075] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5j is a material mainly composed of a metal oxide (e.g., aluminum oxide) and has a higher thermal conductivity than the material of films 6 and 4.
[0076] As a result, as shown in FIG. 8(b), the heat in the film 6 is transferred to the substrate 100 in the +Z direction, and is also transferred to the film 5j in the -Z direction.
[0077] When the material of the films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of the film 5j shown in FIG. 15(a) is a material mainly composed of a metal oxide (e.g., aluminum oxide) and has a higher thermal diffusivity than the material of the films 6 and 4.
[0078] Therefore, as shown in Fig. 8(b), the heat transferred to the film 5j is further transferred in the XY direction within the film 5j. This forms a heat flow that pulls the heat within the film 6 toward the film 5j, and as shown in Fig. 15(b) and Fig. 15(c), the temperature of the substrate 100 can be suppressed to the target temperature Tth or lower, and the temperature of the film 5j can be increased to near the maximum temperature T21.
[0079] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5j is a material mainly composed of a metal oxide (e.g., aluminum oxide) and has a larger thermal expansion coefficient than the material of films 6 and 4.
[0080] Therefore, as the temperature of film 5j rises, thermal stress due to the difference in thermal expansion coefficient occurs at the interface between film 5j and film 6 and the interface between film 5 and film 4 in the XY plane. As a result, as shown in FIG. 6(b), film 5j expands toward film 6 and film 4 in the XY plane.
[0081] In this way, by using a material mainly composed of a metal oxide (e.g., aluminum oxide) as the material for film 5j, the laser light is absorbed by films 6 and 4, the heat from within film 6 etc. is drawn toward film 5j and can be easily diffused within film 5j, and local stress can be generated at the interface between films 5j and 6 spaced apart from substrate 100 in the Z direction.
[0082] (Variation 3) As a third modified example of the embodiment, the material of the film 5m may be a material mainly composed of a metal nitride (e.g., aluminum nitride, tungsten nitride, titanium nitride, etc.) though not shown in the figure. The thickness of the film 5m may be any thickness suitable for the interface with the film 6 to become a peeling interface, and may be, for example, 0.05 μm or more and 1 μm or less, and preferably 0.05 μm or more and 0.2 μm or less.
[0083] For example, as shown in FIG. 6(a), when laser light 200 is irradiated from the substrate 100 side, the films 6 and 4 are locally heated, causing the temperatures of the films 6 and 4 to become high at the XY position.
[0084] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5m is a material mainly composed of a metal nitride (e.g., aluminum nitride) and has a higher thermal conductivity than the material of films 6 and 4.
[0085] As a result, as shown in FIG. 8(b), the heat in the film 6 is transferred to the substrate 100 in the +Z direction, and is also transferred to the film 5m in the -Z direction.
[0086] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5m is a material mainly composed of a metal nitride (e.g., aluminum nitride, tungsten nitride, titanium nitride, etc.) and has a higher thermal diffusivity than the material of films 6 and 4.
[0087] 8(b), the heat transferred to the film 5m is further transferred in the XY directions within the film 5m. This forms a heat flow that pulls the heat within the film 6 toward the film 5m, making it possible to suppress the temperature of the substrate 100 to a target temperature Tth or lower and to raise the temperature of the film 5m to near the maximum temperature.
[0088] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5m is a material mainly composed of a metal nitride (e.g., aluminum nitride) and has a larger thermal expansion coefficient than the material of films 6 and 4.
[0089] Therefore, as the temperature of film 5m rises, stress due to the difference in thermal expansion coefficient at the XY plane position occurs at the interface between film 5m and film 6 and at the interface between film 5m and film 4. As a result, as shown in Figure 6(b), film 5m expands toward film 6 at the XY plane position, and film 5m expands toward film 4.
[0090] In this way, by using a material whose main component is a metal nitride (e.g., aluminum nitride) as the material for film 5m, the laser light is absorbed by films 6 and 4, the heat from within film 6 etc. is drawn toward film 5m and can be easily diffused within film 5m, and local stress can be generated at the interface between film 5m and film 6 spaced apart from substrate 100 in the Z direction.
[0091] (Variation 4) As a fourth modified example of the embodiment, the material of the film 5k may be a material mainly composed of a metal (e.g., tungsten, molybdenum, titanium, etc.) as shown in Fig. 16. Fig. 16 is a diagram showing the temperature distribution of the substrate during laser light irradiation in the fourth modified example of the embodiment. The film 5k may have any thickness suitable for the interface with the film 6 to become a peeling interface, and may be, for example, 0.05 µm to 1 µm, and preferably 0.05 µm to 0.2 µm.
[0092] For example, when laser light 200 is irradiated from the side of substrate 100 as shown in FIG. 6(a), localized heating of films 6 and 4 causes the temperatures of films 6 and 4 to become high at the XY position as shown in FIG. 16(a) and FIG. 16(b).
[0093] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5k is a material mainly composed of a metal (e.g., tungsten, molybdenum, titanium, etc.) and has a higher thermal conductivity than the material of films 6 and 4.
[0094] As a result, as shown in FIG. 8(b), the heat in the film 6 is transferred to the substrate 100 in the +Z direction, and is also transferred to the film 5k in the -Z direction.
[0095] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5k shown in FIG. 16(a) is a material mainly composed of a metal (e.g., tungsten, molybdenum, titanium, etc.) and has a higher thermal diffusivity than the material of films 6 and 4.
[0096] Therefore, as shown in Fig. 8(b), the heat transferred to the film 5k is further transferred in the XY direction within the film 5k. This forms a heat flow that pulls the heat within the film 6 toward the film 5k, and as shown in Fig. 16(b) and Fig. 16(c), the temperature of the substrate 100 can be suppressed to the target temperature Tth or lower, and the temperature of the film 5k can be increased to near the maximum temperature T31.
[0097] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5k is a material mainly composed of a metal (e.g., tungsten, molybdenum, titanium, etc.) and has a larger thermal expansion coefficient than the material of films 6 and 4.
[0098] Therefore, as the temperature of film 5k rises, stress due to the difference in thermal expansion coefficient at the XY plane position occurs at the interface between film 5k and film 6 and at the interface between film 5k and film 4. As a result, as shown in FIG. 6(b), film 5k expands toward film 6 at the XY plane position, and film 5k expands toward film 4.
[0099] In this way, by using a material mainly composed of metal (e.g., tungsten, molybdenum, titanium, etc.) as the material for film 5k, light absorption of the laser can be performed by films 6 and 4, heat from within film 6 etc. can be drawn toward film 5k and easily diffused within film 5k, and local stress can be generated at the interface between film 5k and film 6 spaced apart from substrate 100 in the Z direction.
[0100] (Variation 5) As a fifth modified example of the embodiment, the material of the film 5p may be a material mainly composed of a metal (e.g., copper) having a relatively high thermal conductivity, as shown in Fig. 17. Fig. 17 is a diagram showing the temperature distribution of the substrate during laser light irradiation in the fifth modified example of the embodiment. The film 5p may have any thickness suitable for the interface with the film 6 to become a peeling interface, and may be, for example, 0.05 µm or more and 1 µm or less, and preferably 0.05 µm or more and 0.5 µm or less.
[0101] For example, when laser light 200 is irradiated from the side of substrate 100 as shown in FIG. 6(a), localized heating of films 6 and 4 causes the temperatures of films 6 and 4 to become high at the XY position as shown in FIG. 17(a) and FIG. 17(b).
[0102] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5p is a material mainly composed of a metal (e.g., copper) and has a higher thermal conductivity than the material of films 6 and 4.
[0103] As a result, as shown in FIG. 8(b), the heat in the film 6 is transferred to the substrate 100 in the +Z direction, and is also transferred to the film 5p in the -Z direction.
[0104] When the material of films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of film 5p shown in Figure 17(a) is a material mainly composed of a metal (e.g., copper) and has a higher thermal diffusivity than the material of films 6 and 4.
[0105] Therefore, as shown in Fig. 8(b), the heat transferred to the film 5p is further transferred in the XY direction within the film 5p. This forms a heat flow that pulls the heat within the film 6 toward the film 5p, and as shown in Fig. 17(b) and Fig. 17(c), the temperature of the substrate 100 can be suppressed to the target temperature Tth or lower, and the temperature of the film 5p can be increased to near the maximum temperature T41.
[0106] When the material of the films 6 and 4 is a material mainly composed of a semiconductor oxide (e.g., silicon oxide), the material of the film 5p is a material mainly composed of a metal (e.g., copper) and has a larger thermal expansion coefficient than the material of the films 6 and 4.
[0107] Therefore, as the temperature of film 5p rises, stress due to the difference in thermal expansion coefficient at the XY plane position occurs at the interface between film 5p and film 6 and at the interface between film 5p and film 4. As a result, as shown in FIG. 6(b), film 5p expands toward film 6 at the XY plane position, and film 5p expands toward film 4.
[0108] In this way, by using a material mainly composed of metal (e.g., copper) as the material for film 5p, the laser light can be absorbed by films 6 and 4, the heat from within film 6 etc. can be drawn toward film 5p and easily diffused within film 5p, and local stress can be generated at the interface between film 5p and film 6 spaced apart from substrate 100 in the Z direction.
[0109] (Variation 6) As a sixth modified example of the embodiment, the film 5q formed on the -Z side of the film 6 in the film formation (S4) of Fig. 1 may be a film having a plurality of patterns PT_1 to PT_n arranged two-dimensionally, where n is any integer of 2 or more.
[0110] In the film formation (S4) shown in FIG. 1, as in the embodiment, a film 6 is deposited on the main surface 100b side of the substrate 100, and a film 5 is deposited on the -Z side of the film 6. For example, the film 5 may be the same as the films 5, 5i, 5m, 5k, and 5p in the above embodiment. Then, a resist pattern corresponding to a plurality of patterns is formed on the -Z side of the film 5, and dry or wet etching is performed using the resist pattern as a mask to form a film 5q having a plurality of patterns PT_1 to PT_n. Then, a film 4 is deposited so as to cover the plurality of patterns PT_1 to PT_n of the film 5q. The process thereafter is the same as in the embodiment. Alternatively, after the various films 5 are formed, a film 5 patterned by a so-called damascene process using lithography, etching, CMP, or the like may be formed.
[0111] For example, a stacked body CB including a film 5q (see FIG. 4(b)) may be irradiated with a laser 200 from the substrate 100 side as shown in FIG. 18. FIG. 18 is a cross-sectional view showing a method for manufacturing a semiconductor device according to a sixth modified example of the embodiment, and shows a step corresponding to FIG. 6(a).
[0112] The arrangement direction of the multiple patterns PT_1 to PT_n is arbitrary, but may be a direction along the X direction and / or the Y direction, or may be a direction intersecting the X direction and / or the Y direction. The arrangement pitch of the multiple patterns PT_1 to PT_n may be uniform along the arrangement direction. The arrangement pitch may be 1 / 5 of the wavelength of the laser 200, for example, 2 μm or less.
[0113] Each pattern PT may be a line shape in the XY plane view, as shown in Fig. 19(a). Fig. 19 is a plan view showing a manufacturing method of a semiconductor device. Each pattern PT shown in Fig. 19(a) extends in the X direction. The multiple patterns PT_1 to PT_n are arranged at a substantially uniform pitch P in the Y direction. Y The elements are arranged as follows:
[0114] Each pattern PT may be in the form of dots in the XY plane view, as shown in Figs. 19(b) and 19(c). Each pattern PT may be in the form of approximately rectangular dots or approximately circular dots. In Figs. 19(b) and 19(c), a pattern PT in the form of approximately rectangular dots is exemplified. The arrangement of each pattern PT may be in a staggered arrangement as shown in Fig. 19(b), or in a lattice arrangement as shown in Fig. 19(c). The pitch P is approximately uniform in the X direction. X are arranged at a substantially uniform pitch P in the Y direction. Y The elements may be arranged as follows:
[0115] Each pattern PT may be cross-shaped in the XY plane view as shown in FIG. 19(d). Each pattern PT may be a cross-shaped pattern in which a line extending in the X direction intersects a line extending in the Y direction. The multiple patterns PT_1 to PT_n are arranged at a substantially uniform pitch P in the X direction. X are arranged at a substantially uniform pitch P in the Y direction. Y The 3D patterns may be arranged as follows:
[0116] Alternatively, each pattern PT may be T-shaped.
[0117] Each pattern PT may be an asymmetric pattern such as an L-shape in the XY plane view as shown in FIG. 19(d). Each pattern PT may be an L-shape pattern in which a line extending in the X direction and a line extending in the Y direction are connected at their ends. The multiple patterns PT_1 to PT_n are arranged at an arrangement pitch P X is offset in the X direction, and the array pitch P in the Y direction Y may be constant.
[0118] In this way, by including a plurality of two-dimensionally arranged PT_1 to PT_n in the film 5q, when local stress occurs at the interface between the film 5q and the film 6, the stress distribution at the interface can be controlled.
[0119] (Variation 7) As a seventh modification of the embodiment, separation of the upper substrate 100 may be performed by mechanical peeling, as shown in Fig. 20. Fig. 20 is a cross-sectional view showing a manufacturing method of the semiconductor device 1 according to the seventh modification of the embodiment.
[0120] When mechanical peeling is performed, the laser irradiation (S7) shown in Fig. 1 is omitted. The processing of the lower substrate (S1 to S2) and the processing of the upper substrate (S3 to S4) are performed, for example, in parallel, as in the embodiment, but the step of S4 differs from the embodiment in the following respect.
[0121] 1, a film 6 is deposited on the main surface 100b side of the substrate 100. The film 6 may be formed of a material that can be removed by wet etching. The film 6 may be formed of a material mainly composed of a semiconductor oxide (e.g., silicon oxide) or a material mainly composed of a semiconductor nitride (e.g., silicon nitride).
[0122] The film 5 is deposited on the -Z side of the film 6. At this time, the film 5 may be formed of a material having a relatively weak mechanical strength. The film 5 may be formed of a material mainly composed of a semiconductor polycrystalline material (e.g., polycrystalline silicon), or may be formed of a material mainly composed of a semiconductor amorphous material (e.g., amorphous silicon). It may be formed of a material mainly composed of a semiconductor porous material (e.g., porous silicon). When the film 5 is formed of a material mainly composed of porous silicon, the porosity may be 40% or more and 90% or less, and preferably 50% or more and 90% or less. The porosity may be a value measured by spectroscopic ellipsometry or gas adsorption method. The following is the same as S4 of the embodiment.
[0123] Once the processing of the lower substrate (S1 to S2) and the processing of the upper substrate (S3 to S4) shown in FIG. 1 are both completed, the upper substrate and the lower substrate are bonded (S5) and a heat treatment (S6) is performed, similarly to the embodiment.
[0124] Thereafter, peeling is performed as shown in Fig. 1 (S8). In the peeling, mechanical peeling is performed using film 5 as a peeling layer, and stack 208 is peeled off from stack 207 as shown in Fig. 20(a). In stack 207, film 3, film 4, and film 51 are stacked on substrate 2. Film 51 is a part of film 5. In stack 208, film 6 and film 52 are stacked on substrate 100. Film 52 is another part of film 5.
[0125] For example, the tip of the blade member BL is inserted near the center in the Z direction of the film 5. The tip of the blade member BL has a sharp shape forming an acute angle. Since the film 5 is made of a material with relatively low mechanical strength, the film 5 is divided into films 51 and 52 in the Z direction by the stress caused by the insertion of the tip of the blade member BL.
[0126] In consideration of subsequent processing, the peeled surface of the laminate 207 is treated (S9) as shown in Fig. 1. In the laminate 207 shown in Fig. 20(b), the main surface 51a on the +Z side of the film 51 is roughened due to the influence of mechanical peeling. The film 51 is removed by dry etching or wet etching.
[0127] As a result, as shown in FIG. 20(c), a semiconductor device 1 is obtained in which the film 3 and the film 4 are laminated on the substrate 2 and the main surface 4a of the film 4 is flat.
[0128] On the other hand, the peeled substrate 100 is reused (S10) as shown in Fig. 1. The substrate 100 may be reused as an upper substrate 100 as shown by the solid arrow in Fig. 2.
[0129] 20(d), in the laminate 208 immediately after peeling, the main surface 100b on the -Z side of the substrate 100 is covered with the film 6 and the film 52. The film 6 is removed by wet etching, and the film 52 is also removed accordingly.
[0130] For example, when the film 6 is made of a material mainly composed of a semiconductor oxide (e.g., silicon oxide), it can be easily removed by wet etching while ensuring an etching selectivity with respect to the material of the substrate 100 (e.g., a semiconductor such as silicon). Alternatively, when the film 6 is made of a material mainly composed of a semiconductor nitride (e.g., silicon nitride), it can be easily removed by wet etching while ensuring an etching selectivity with respect to the material of the substrate 100 (e.g., a semiconductor such as silicon).
[0131] As a result, the substrate 100 is obtained as shown in Fig. 20(e). The substrate 100 shown in Fig. 20(e) can be easily reused, for example, as the upper substrate 100. In addition, since polishing by a CMP method or the like is not required, the substrate 100 can be reused in almost its original state.
[0132] Even in such a process, when the upper substrate 100 is separated, the film 6 is interposed between the peeling interface and the upper substrate 100. That is, the film 5 separated from the substrate 100 in the Z direction is used as a peeling layer to peel the laminate 208 from the laminate 207. Thereafter, the film 6 is removed from the laminate 208 by wet etching. This makes it possible to suppress damage to the substrate 100 during peeling, and to suppress damage to the substrate 100 during the subsequent removal of the film 6. As a result, peeling can be performed satisfactorily, and the substrate 100 can be reused in almost its original state.
[0133] (Variation 8) 21 to 24, as an eighth modified example of the embodiment, a process may be performed in which a sacrificial substrate 300 is interposed between the peeling interface and the upper substrate 100. Figures 21(a) to 21(f), 22(a) to 22(e), 23(a) to 23(d), and 24(a) to 24(e) are YZ cross-sectional views showing a manufacturing method of the semiconductor device 1.
[0134] In preparation of the lower substrate (S1), a laminate 308 including a substrate (lower substrate) 2 is prepared. In S1, the steps shown in Figures 21(a) to 21(b) and the steps shown in Figures 21(c) to 21(d) are performed, for example, in parallel.
[0135] The preparation of the lower substrate (S1) is performed in the same manner as in the embodiment (see FIG. 2(a)), as shown in FIG. 21(a).
[0136] The film formation (S2) is performed in the same manner as in the embodiment (see FIG. 2(b)), as shown in FIG. 21(b).
[0137] In preparation of the upper substrate (S3), as shown in Fig. 21(c), a laminate 308 including a substrate (upper substrate) 100 is prepared. The laminate 308 is formed as shown in Fig. 22(a) to Fig. 22(e). In S3, the steps shown in Fig. 22(a) to Fig. 22(b) and the steps shown in Fig. 22(c) to Fig. 22(d) may be performed in parallel.
[0138] 22(a), a sacrificial substrate 300 is prepared. The sacrificial substrate 300 may be formed of a material that is mainly composed of a semiconductor (e.g., silicon) that does not substantially contain impurities. The sacrificial substrate 300 is a substrate that is not reused and is thinner than the substrate 100.
[0139] 22(b), a film 9 is deposited by CVD or the like on the main surface 300a on the +Z side of the sacrificial substrate 300. The film 9 is a dummy film and can be made of any material.
[0140] 22(c), a substrate (upper substrate) 100 is prepared. The substrate 100 may be made of a material mainly composed of a semiconductor (for example, silicon) that does not substantially contain impurities.
[0141] 22(d), a film 6 is deposited by CVD or the like on the main surface 100b side of the substrate 100. The film 6 may be the same as the film 6 in the embodiment.
[0142] When both the process shown in FIG. 22(b) and the process shown in FIG. 22(d) are completed, the sacrifice substrate 300 and the substrate 100 are bonded. The main surface 9a (see FIG. 22(b)) on the +Z side of the film 9 and the main surface 6b (see FIG. 22(d)) on the -Z side of the film 6 are activated by plasma irradiation or the like, and the sacrifice substrate 300 and the substrate 100 are arranged to face each other in the Z direction so that the main surfaces 9a and 6b face each other, as shown in FIG. 22(e). As shown in FIG. 21(c), the sacrifice substrate 300 and the substrate 100 are brought close to each other in the Z direction, and the main surface 9a on the sacrifice substrate 300 side and the main surface 6b on the substrate 100 side are bonded. At this time, the atoms of the main surface 9a and the atoms of the main surface 9b are bonded by hydrogen bonds or the like, and the sacrifice substrate 300 and the substrate 100 are temporarily bonded. As a result, a laminate 308 in which the film 9, the film 6, and the sacrifice substrate 300 are laminated on the substrate 100 is formed.
[0143] In the film formation (S4), as shown in Fig. 21(d), a film 5 is deposited by a CVD method or the like on the main surface 300b on the -Z side of the laminate 308. The film 5 may be similar to the films 5, 5i, 5j, 5m, 5k, 5p, and 5q of the embodiment.
[0144] 21(e), the film 4 is deposited by a CVD method or the like on the -Z side of the film 5. The film 4 may be the same as the film 4 of the embodiment.
[0145] As shown in FIG. 1, when the processing of the lower substrate (S1-S2) and the processing of the upper substrate (S3-S4) are both completed, the upper substrate and the lower substrate are bonded (S5). The main surface 3a (see FIG. 21(b)) on the +Z side of the film 3 and the main surface 4b (see FIG. 21(e)) on the -Z side of the film 4 are activated by plasma irradiation or the like, and the substrate 2 and the substrate 100 are disposed facing each other in the Z direction so that the main surfaces 3a and 4b face each other, as shown in FIG. 21(f). The substrate 2 and the substrate 100 are brought close to each other in the Z direction, and the main surface 3a on the substrate 2 side and the main surface 4b on the substrate 100 side are bonded. At this time, the atoms of the main surface 3a and the atoms of the main surface 4b are bonded by hydrogen bonds or the like, and the substrate 2 and the substrate 100 are temporarily bonded.
[0146] Thereafter, a heat treatment (annealing) is performed at a relatively low temperature (S6), and as a result of water molecules being removed from the interface, the atoms of the main surface 3a and the atoms of the main surface 4b are bonded by covalent bonds or the like, and the substrate 2 and the substrate 100 are finally bonded together. As a result, a bonded body CB1 of the substrate 2 and the substrate 100 is formed, as shown in FIG. 23(a).
[0147] When S6 shown in FIG. 1 is completed, laser light 200 is irradiated from the substrate 100 side (S7).
[0148] 23(a), the position in the XY plane to which the first laser beam 200 is to be irradiated is determined, and the focus of the laser beam 200 is adjusted to be located within the film 4. The laser beam 200 irradiated onto the film 4 through the substrate 100, the film 6, the film 9, and the sacrificial substrate 300 is efficiently absorbed in the film 4 near the irradiated location, and locally generates heat (localized heating) in the film 4 at that XY plane position.
[0149] As a result, as shown in FIG. 23(b), the film 5 expands toward the sacrificial substrate 300 at that position in the XY plane, and the film 5 expands toward the film 4.
[0150] 23(c), the XY plane position to be irradiated with the second laser beam 200 is determined to be a position shifted in the XY plane direction from the XY plane position in FIG. 23(a), and the focus of the laser beam 200 is adjusted to be located within the film 4. The laser beam 200 irradiated to the film 4 through the substrate 100, the film 6, the film 9, and the sacrificial substrate 300 is efficiently absorbed at the irradiated point within the film 4, and locally generates heat (localized heating) in the film 4 at that XY plane position.
[0151] As a result, as shown in FIG. 23(d), film 5 expands toward the sacrificial substrate 300 side at that XY plane position, and film 5 expands toward film 4 side.
[0152] Similarly, when the final N-th irradiation of the laser beam 200 is performed, the main surface 5a on the +Z side of the film 5 has two-dimensionally distributed convex portions 5a2, as shown in Fig. 24(a). This can generate local stress in which each of the multiple convex portions 5a2 on the main surface 5a pushes the sacrificial substrate 300 outward in the XY directions near the main surface 300b.
[0153] As a result, peeling occurs at the interface between the film 5 and the sacrificial substrate 300 (S8). In the peeling, as shown in Fig. 24(a), the laminate 308 is peeled off from the laminate 307. In the laminate 307, the film 3, the film 4, and the film 5 are laminated on the substrate 2. In the laminate 308, the film 6, the film 9, and the sacrificial substrate 300 are laminated on the substrate 100. For example, since local stress is generated at the multiple protrusions 5a2 distributed two-dimensionally, the laminate 308 is easily peeled off from the laminate 307 starting from the multiple protrusions 5a2.
[0154] In consideration of subsequent processing, the laminate 307 has a peeled surface treated (S9) as shown in Fig. 1. In the laminate 307, as shown in Fig. 24(b), a plurality of convex portions 5a2 are distributed in the XY direction on the main surface 5a on the +Z side of the film 5, and a plurality of convex portions 5b2 are distributed in the XY direction on the main surface 5b on the -Z side of the film 5. The film 5 is removed by dry etching or wet etching.
[0155] In the laminate 307a from which the film 5 has been removed, a plurality of recesses each corresponding to the protrusion 5b2 are distributed in the XY directions on the main surface 4a on the +Z side of the film 4. The main surface 4a of the film 4 is polished and flattened by a CMP method or the like.
[0156] As a result, as shown in FIG. 24(c), a semiconductor device 1 is obtained in which the film 3 and the film 4 are laminated on the substrate 2 and the main surface 4a of the film 4 is flattened.
[0157] On the other hand, the peeled substrate 100 is reused (S10) as shown in Fig. 1. The substrate 100 may be reused as an upper substrate 100 as shown by the solid arrow in Fig. 2.
[0158] 24(d), in the laminate 308 immediately after peeling, the main surface 100b on the -Z side of the substrate 100 is covered with the film 6, the film 9, and the sacrificial substrate 300. The film 6 is removed by wet etching, and accordingly, the film 9 and the sacrificial substrate 300 are also removed.
[0159] For example, when the film 6 is made of a material mainly composed of a semiconductor oxide (e.g., silicon oxide), it can be easily removed by wet etching while ensuring an etching selectivity with respect to the material of the substrate 100 (e.g., a semiconductor such as silicon). Accordingly, the film 9 and the sacrificial substrate 300 are also removed.
[0160] As a result, the substrate 100 is obtained as shown in Fig. 24(e). The substrate 100 shown in Fig. 24(e) can be easily reused, for example, as the upper substrate 100. In addition, since polishing by a CMP method or the like is not required, the substrate 100 can be reused in almost its original state.
[0161] Even with such a process, when the upper substrate 100 is separated, the film 6, the film 9, and the sacrificial substrate 300 are interposed between the peeling interface and the upper substrate 100. That is, peeling is performed at the interface between the film 5 and the sacrificial substrate 300, which are spaced apart from the substrate 100 in the Z direction, and the laminate 308 can be peeled off from the laminate 307. Thereafter, the film 6 is removed from the laminate 308 by wet etching, and the film 9 and the sacrificial substrate 300 are also removed accordingly. This makes it possible to suppress damage to the substrate 100 during peeling, and to suppress damage to the substrate 100 during the subsequent removal of the film 6, the film 9, and the sacrificial substrate 300. As a result, peeling can be performed well, and the substrate 100 can be reused in almost its original state.
[0162] (Variation 9) As a ninth modification of the embodiment, the separation of the upper substrate 100 in the eighth modification of the embodiment may be performed by mechanical peeling, as shown in Fig. 25. Fig. 25 is a cross-sectional view showing a manufacturing method of the semiconductor device 1 according to the ninth modification of the embodiment.
[0163] When mechanical peeling is performed, the laser irradiation (S7) shown in Fig. 1 is omitted. The processing of the lower substrate (S1-S2) and the processing of the upper substrate (S3-S4) are performed, for example, in parallel, as in the seventh modified embodiment. However, the step of S4 differs from that of the seventh modified embodiment in the following respect.
[0164] 1, in the step shown in FIG. 22(d), a film 6 is deposited on the main surface 100b side of the substrate 100. The film 6 may be formed of a material that can be removed by wet etching. The film 6 may be formed of a material mainly composed of a semiconductor oxide (e.g., silicon oxide) or a material mainly composed of a semiconductor nitride (e.g., silicon nitride).
[0165] In the step shown in FIG. 21(d), the film 5 is deposited on the -Z side of the sacrificial substrate 300. At this time, the film 5 may be formed of a material having a relatively weak mechanical strength. The film 5 may be formed of a material mainly composed of a semiconductor polycrystalline material (e.g., polycrystalline silicon), may be formed of a material mainly composed of a semiconductor amorphous material (e.g., amorphous silicon), or may be formed of a material mainly composed of a semiconductor porous material (e.g., porous silicon). When the film 5 is formed of a material mainly composed of porous silicon, the porosity may be 40% or more and 90% or less, and preferably 50% or more and 90% or less. The porosity may be a value measured by spectroscopic ellipsometry or a gas adsorption method. The following steps are the same as S4 of the seventh modified example of the embodiment.
[0166] Once the processing of the lower substrate (S1-S2) and the processing of the upper substrate (S3-S4) shown in FIG. 1 are both completed, the upper and lower substrates are bonded (S5) and a heat treatment (S6) is performed, which is similar to the seventh modified example of the embodiment.
[0167] Thereafter, peeling is performed as shown in Fig. 1 (S8). In the peeling, mechanical peeling is performed using film 5 as a peeling layer, and stack 408 is peeled off from stack 407 as shown in Fig. 25(a). In stack 407, film 3, film 4, and film 51 are stacked on substrate 2. Film 51 is a part of film 5. In stack 408, film 6, film 9, sacrificial substrate 300, and film 52 are stacked on substrate 100. Film 52 is another part of film 5.
[0168] For example, the tip of the blade member BL is inserted near the center in the Z direction of the film 5. The tip of the blade member BL has a sharp shape forming an acute angle. Since the film 5 is made of a material with relatively low mechanical strength, the film 5 is divided into films 51 and 52 in the Z direction by the stress caused by the insertion of the tip of the blade member BL.
[0169] In consideration of subsequent processing, the peeled surface of the laminate 407 is treated (S9) as shown in Fig. 1. In the laminate 407 shown in Fig. 25(b), the main surface 51a on the +Z side of the film 51 is roughened due to the influence of mechanical peeling. The film 51 is removed by dry etching or wet etching.
[0170] As a result, as shown in FIG. 25(c), a semiconductor device 1 is obtained in which the film 3 and the film 4 are laminated on the substrate 2 and the main surface 4a of the film 4 is flat.
[0171] On the other hand, the peeled substrate 100 is reused (S10) as shown in Fig. 1. The substrate 100 may be reused as an upper substrate 100 as shown by the solid arrow in Fig. 2.
[0172] 25(d), in the laminate 208 immediately after peeling, the main surface 100b on the -Z side of the substrate 100 is covered with the film 6 and the film 52. The film 6 is removed by wet etching, and accordingly, the film 9, the sacrificial substrate 300, and the film 52 are also removed.
[0173] For example, when the film 6 is made of a material mainly composed of a semiconductor oxide (e.g., silicon oxide), it can be easily removed by wet etching while ensuring an etching selectivity with respect to the material of the substrate 100 (e.g., a semiconductor such as silicon). Alternatively, when the film 6 is made of a material mainly composed of a semiconductor nitride (e.g., silicon nitride), it can be easily removed by wet etching while ensuring an etching selectivity with respect to the material of the substrate 100 (e.g., a semiconductor such as silicon). Accordingly, the film 9, the sacrificial substrate 300, and the film 52 are also removed.
[0174] As a result, the substrate 100 is obtained as shown in Fig. 25(e). The substrate 100 shown in Fig. 25(e) can be easily reused, for example, as the upper substrate 100. In addition, since polishing by a CMP method or the like is not required, the substrate 100 can be reused in almost its original state.
[0175] Even in such a process, when the upper substrate 100 is separated, the film 6, the film 9, and the sacrificial substrate 300 are interposed between the peeling interface and the upper substrate 100. That is, the film 5 separated from the substrate 100 in the Z direction is used as a peeling layer to peel the laminate 408 from the laminate 407. Thereafter, the film 6 is removed from the laminate 408 by wet etching, and the film 9 and the sacrificial substrate 300 are also removed accordingly. This makes it possible to suppress damage to the substrate 100 during peeling, and to suppress damage to the substrate 100 during the subsequent removal of the film 6, the film 9, and the sacrificial substrate 300. As a result, peeling can be performed well, and the substrate 100 can be reused in almost its original state.
[0176] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0177] 1 semiconductor device, 2, 100 substrate, 3-6, 9, 51, 52 film, 300 sacrificial substrate.
Claims
1. laminating a first film on a first substrate, and laminating a second film, a third film, and a fourth film on a second substrate; bonding a main surface of the first film opposite to the first substrate and a main surface of the fourth film opposite to the second substrate; Irradiating the second substrate with laser light; Separating the second substrate; and Equipped with the second film and the fourth film each include a first material; The third film includes a second material different from the first material. A method for manufacturing a semiconductor device.
2. The second material has a greater coefficient of thermal expansion than the first material. The method for manufacturing a semiconductor device according to claim 1 .
3. The thermal conductivity of the second material is higher than the thermal conductivity of the first material. The method for manufacturing a semiconductor device according to claim 1 .
4. The thermal diffusivity of the second material is greater than the thermal diffusivity of the first material. The method for manufacturing a semiconductor device according to claim 1 .
5. the first material comprises a semiconductor oxide; The second material includes a material mainly composed of at least one of a semiconductor, a semiconductor nitride, a metal, a metal oxide, and a metal nitride. The method for manufacturing a semiconductor device according to claim 1 .
6. The second material includes at least one of a semiconductor polycrystalline material and a semiconductor amorphous material. The method for manufacturing a semiconductor device according to claim 5 .
7. The second material includes at least one of polysilicon and amorphous silicon. The method for manufacturing a semiconductor device according to claim 6 .
8. The third film has a plurality of patterns. The method for manufacturing a semiconductor device according to claim 1 .
9. The pattern is a line shape, a dot shape, a cross shape, an L shape, or a T shape in a plan view. The method for manufacturing a semiconductor device according to claim 8 .
10. laminating a first film on a first substrate, and laminating a second film, a third film, and a fourth film on a second substrate; bonding a main surface of the first film opposite to the first substrate and a main surface of the fourth film opposite to the second substrate; Separating a stack in which the second film is stacked on the second substrate; and removing the second film from the stack; and A method for manufacturing a semiconductor device comprising the steps of:
11. The removal may include wet etching the second film. The method for manufacturing a semiconductor device according to claim 10.
12. The separation may include and separating the laminate by irradiating the laminate with laser light from the side of the second substrate. The method for manufacturing a semiconductor device according to claim 10.
13. The separation may include mechanically removing the third film and separating the stack. The method for manufacturing a semiconductor device according to claim 10.
14. The stack is and laminating the second film, a sacrificial substrate, the third film, and the fourth film on the second substrate. The method for manufacturing a semiconductor device according to claim 10.
15. A substrate; A first film disposed on a main surface side of the substrate; a second film disposed on the opposite side of the substrate with the first film therebetween; a third membrane disposed on the opposite side of the first membrane with the second membrane therebetween; and Equipped with the first membrane and the third membrane contact the second membrane on opposite sides; the first film and the third film each include a first material; the second film includes a second material different from the first material; The second material has a greater coefficient of thermal expansion than the first material. Semiconductor device.
16. The thermal conductivity of the second material is higher than the thermal conductivity of the first material. The method for manufacturing a semiconductor device according to claim 15.
17. The thermal diffusivity of the second material is greater than the thermal diffusivity of the first material. The method for manufacturing a semiconductor device according to claim 15.
Citation Information
Patent Citations
Substrate processing method and substrate processing system
JP2021103725A
Substrate processing device and substrate processing method
JP2021106197A
Processing device and processing method
WO2020213478A1
Processing device and processing method
WO2021010284A1
Substrate processing apparatus, and substrate processing method
WO2021131710A1