Liquid crystal aligning agent, liquid crystal alignment film and production method of the same, and liquid crystal element
The liquid crystal aligning agent with a specific polymer and leaving group-containing compound improves voltage holding and film strength, effectively reducing DC afterimages in liquid crystal elements.
Patent Information
- Application Number
- JP2024008163
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2024-01-23
- Publication Date
- 2024-10-03
AI Technical Summary
Existing liquid crystal elements face issues with insufficient voltage holding rate, film strength, and susceptibility to DC afterimages due to the use of crosslinking agents, which also affect mechanical properties and charge accumulation.
A liquid crystal aligning agent containing a polymer with a specific nitrogen-containing structure and a compound with leaving groups that are eliminated by heat or light, ensuring a predetermined content ratio of structural units derived from a diamine compound, forming a liquid crystal alignment film with improved liquid crystal orientation, voltage holding characteristics, and film strength.
The solution effectively suppresses DC afterimages, enhances voltage holding characteristics, and increases film strength while maintaining good liquid crystal alignment, addressing the limitations of traditional crosslinking agents.
Smart Images

Figure 2024134519000001 
Figure 2024134519000002 
Figure 2024134519000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film and a manufacturing method thereof, and a liquid crystal element. [Background technology]
[0002] A liquid crystal element is provided with a liquid crystal alignment film having a function of controlling the alignment of liquid crystal molecules in a liquid crystal layer. A liquid crystal alignment film is generally formed on a substrate by applying a liquid crystal alignment agent, which is a polymer component dissolved in an organic solvent, to the substrate surface and preferably by heating.
[0003] In recent years, large-screen, high-definition LCD televisions have become mainstream, and small display terminals such as smartphones and tablet PCs have become more widespread, further increasing the demand for high-quality liquid crystal elements. In view of this, various liquid crystal alignment agents have been proposed to improve the performance of liquid crystal alignment films and to improve various properties of liquid crystal elements (see, for example, Patent Document 1). Patent Document 1 discloses that a crosslinking agent such as a multifunctional epoxy compound is contained in the liquid crystal alignment agent together with a polymer component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-299318 A Summary of the Invention [Problem to be solved by the invention]
[0005] The use of a crosslinking agent is an effective means of improving the performance of a liquid crystal alignment film. On the other hand, the use of a crosslinking agent can lead to problems such as the inability to sufficiently increase the voltage retention rate of a liquid crystal element due to the increased density of the film. In recent years, mechanical properties have become important in liquid crystal elements, and there is a demand for sufficiently high film strength in addition to the basic property of liquid crystal alignment.
[0006] When a DC voltage is applied to a liquid crystal element, electric charge accumulates in the liquid crystal cell, which is perceived by the viewer as an afterimage (DC afterimage), and the display quality of the liquid crystal element may be reduced. Therefore, one of the properties required for liquid crystal alignment films is low electric charge accumulation, and with the demand for even higher quality liquid crystal elements, there is a demand to develop liquid crystal elements that are even less susceptible to afterimages.
[0007] Furthermore, in order to satisfy the demand for even higher quality liquid crystal elements, there is a demand for the decrease in voltage holding ratio due to illumination with a backlight to be small and for the reliability to be high.
[0008] The present invention has been made in consideration of the above problems, and has as its main object to provide a liquid crystal alignment agent that can obtain a liquid crystal alignment film excellent in liquid crystal alignment properties, voltage retention characteristics, reliability with respect to voltage retention rate, and film strength, and can obtain a liquid crystal element in which afterimages caused by charge accumulation are sufficiently suppressed. [Means for solving the problem]
[0009] According to the present invention, the following means are provided. [1] A polymer (A) comprising the following: (A) Polymer: A polymer having a structural unit derived from a diamine compound containing a diamine having a partial structure represented by the following formula (1): and a polymer component comprising the following (B) compound: (B) Compound: A compound (excluding polymers) having three or more partial structures (T) in one molecule in which one or more hydrogen atoms bonded to heteroatoms in a nucleophilic functional group or an acidic functional group are replaced with leaving groups that are eliminated by at least one of heat and light. and wherein the content ratio of the structural unit derived from a diamine having a partial structure represented by the following formula (1) in the polymer component is 0.13 mol or more per mol of the total amount of the structural units derived from the diamine compound in the polymer component. [ka] (In formula (1), Ar1 is a divalent aromatic ring group. 2 and R 1 Ar 2 is a divalent aromatic ring group, R 1 is a hydrogen atom or a monovalent organic group, or Ar 2 and R 1 are combined together, Ar 2 and R 1 represents a nitrogen-containing aromatic condensed ring structure formed together with the nitrogen atom to which it is bonded. "*" represents a bond.) [2] A liquid crystal alignment film formed using the liquid crystal alignment agent of [1] above. [3] A method for producing a liquid crystal alignment film, comprising applying the liquid crystal aligning agent according to [1] above onto a substrate, and then subjecting the applied liquid crystal aligning agent to a rubbing treatment or a light irradiation treatment to impart liquid crystal aligning ability. [4] A liquid crystal element having the liquid crystal alignment film described above in [2]. Effect of the Invention
[0010] According to the liquid crystal alignment agent of the present invention, by containing the polymer component containing the above-mentioned (A) polymer and the (B) compound, and containing a predetermined amount or more of the structural unit derived from the diamine having the partial structure represented by the above formula (1) relative to the total amount of the structural unit derived from the diamine compound contained in the polymer component, a liquid crystal alignment film excellent in liquid crystal alignment property, voltage holding property, reliability for voltage holding ratio, and film strength can be obtained. In addition, a liquid crystal element in which the afterimage caused by the accumulation of electric charge is sufficiently suppressed can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Liquid crystal alignment agent The liquid crystal aligning agent of the present disclosure contains a polymer having a specific nitrogen-containing structure (hereinafter also referred to as "polymer (A)") and a compound having a leaving group that is removed by at least one of heat and light (hereinafter also referred to as "compound (B)"). Each component contained in the liquid crystal aligning agent and components that are optionally blended as necessary (hereinafter also referred to as "other components") will be described below.
[0012] Here, in this specification, the term "hydrocarbon group" includes chain-shaped hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. The term "chain-shaped hydrocarbon group" means a straight-chain hydrocarbon group and a branched hydrocarbon group that do not include a cyclic structure in the main chain and are composed only of a chain structure. However, the chain-shaped hydrocarbon group may be saturated or unsaturated. The term "alicyclic hydrocarbon group" means a hydrocarbon group that includes only an alicyclic hydrocarbon structure as a ring structure and does not include an aromatic ring structure. However, the alicyclic hydrocarbon group does not necessarily have to be composed only of an alicyclic hydrocarbon structure, and also includes those that have a chain structure as a part of it. The term "aromatic hydrocarbon group" means a hydrocarbon group that includes an aromatic ring structure as a ring structure. However, the aromatic hydrocarbon group does not necessarily have to be composed only of an aromatic ring structure, and may include a chain structure or an alicyclic hydrocarbon structure as a part of it. The term "aromatic ring" includes aromatic hydrocarbon rings and aromatic heterocycles. The term "organic group" means an atomic group obtained by removing any hydrogen atom from a compound containing carbon (i.e., an organic compound).
[0013] The "main chain" of a polymer refers to the "trunk" portion of the polymer that is the longest chain of atoms. It is permissible for this "trunk" portion to contain a ring structure. For example, "having a specific structure in the main chain" means that the specific structure constitutes a part of the main chain. The "side chain" refers to a portion that branches off from the "trunk" of the polymer. The term "tetracarboxylic acid derivative" includes tetracarboxylic acid dianhydrides, tetracarboxylic acid diesters, and tetracarboxylic acid diester dihalides.
[0014] <(A) Polymer> The polymer (A) is a polymer having a structural unit derived from a diamine derived from a partial structure represented by the following formula (1) (hereinafter also referred to as "partial structure (AN)"). [ka] (In formula (1), Ar 1 is a divalent aromatic ring group. 2 and R 1 Ar 2 is a divalent aromatic ring group, R 1is a hydrogen atom or a monovalent organic group, or Ar 2 and R 1 are combined together, Ar 2 and R 1 represents a nitrogen-containing aromatic condensed ring structure formed together with the nitrogen atom to which it is bonded. "*" represents a bond.)
[0015] In the above formula (1), Ar 1 Or Ar 2 The divalent aromatic ring group represented by is a group obtained by removing two hydrogen atoms from the ring portion of a substituted or unsubstituted aromatic ring. The aromatic ring contained in the divalent aromatic ring group may be either an aromatic hydrocarbon ring or an aromatic heterocycle. In addition, the aromatic ring may be a monocycle or a condensed ring. Specific examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, an anthracene ring, and a phenanthrene ring. Specific examples of the aromatic heterocycle include a pyrrole ring, a pyrazole ring, an imidazole ring, a 1,2,4-triazole ring, a 1,2,3-triazole ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a 1,2,4-triazine ring, a 1,3,5-triazine ring, a 1,2,4-triazine ring, a carbazole ring, a benzimidazole ring, a quinoline ring, an isoquinoline ring, an indole ring, a purine ring, an acridine ring, an oxazole ring, a thiazole ring, an oxadiazole ring, a benzothiazole ring, and a ring represented by the following formula: [ka] and nitrogen-containing heterocycles such as the ring represented by the following formula: oxygen-containing heterocycles such as a furan ring, a benzofuran ring, a dibenzofuran ring, an oxazole ring, and an oxadiazole ring; and sulfur-containing heterocycles such as a thiophene ring, a dibenzothiophene ring, a thiazole ring, and a benzothiazole ring.
[0016] Ar 1 Or Ar 2Among the above, the divalent aromatic ring group represented by the formula (I) is preferably an aromatic hydrocarbon ring or a nitrogen-containing heterocycle, more preferably a benzene ring, a naphthalene ring, a pyrrole ring, a pyrazole ring, an imidazole ring, a pyridine ring, a pyrimidine ring, a carbazole ring, a benzimidazole ring, or a quinoline ring, and more preferably a benzene ring, a pyridine ring, or a carbazole ring.
[0017] Ar 1 Or Ar 2 The divalent aromatic ring group represented by the formula (1) may have a substituent on the ring portion. Examples of the substituent include an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a halogen atom, a hydroxy group, a carboxy group, a thermally detachable group (e.g., a tert-butoxycarbonyl group, etc.).
[0018] Ar 2 When R is a divalent aromatic ring group, 1 R is a hydrogen atom or a monovalent organic group. 1 The monovalent organic group represented by the formula (I) is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms or a monovalent thermally eliminable group. Examples of the monovalent hydrocarbon group having 1 to 10 carbon atoms include a monovalent chain hydrocarbon group having 1 to 10 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. Among these, an alkyl group having 1 to 6 carbon atoms, a cyclohexyl group, or a phenyl group is preferred, and an alkyl group having 1 to 3 carbon atoms is more preferred.
[0019] Examples of the monovalent thermally detachable group include a tert-butoxycarbonyl group (Boc group), a benzyloxycarbonyl group, a 1,1-dimethyl-2-haloethyloxycarbonyl group, an allyloxycarbonyl group, a 2-(trimethylsilyl)ethoxycarbonyl group, a 9-fluorenylmethyloxycarbonyl group (F-moc group), etc. Among these, the Boc group is preferred because it has excellent thermal detachability and can reduce the amount of the detached structure remaining in the film.
[0020] Ar 2 and R 1 are combined together, Ar 2 and R1 represents a nitrogen-containing aromatic fused ring structure formed together with the nitrogen atom to which it is bonded, examples of the nitrogen-containing aromatic fused ring structure include a benzimidazole ring structure and a carbazole ring structure.
[0021] Specific examples of the partial structure represented by formula (1) above include structures represented by the following formulas (1-1) to (1-16) and structures having a substituent on the ring portion of the structures represented by the following formulas. [ka] (In formulas (1-1) to (1-16), "*" represents a bond.)
[0022] In addition, when the structure represented by the above formula (1) has a nitrogen-containing aromatic condensed ring, a polymer having a structural unit derived from a diamine having a structure represented by the above formula (1) and a nitrogen-containing aromatic condensed ring corresponds to the polymer having the structure represented by the above formula (1). For example, a polymer having a structural unit derived from a diamine having a partial structure represented by each of the above formulas (1-2), (1-3), (1-5), (1-6), (1-8), (1-9), (1-11), and (1-13) to (1-16) corresponds to a polymer having a structural unit derived from a diamine having a structure represented by the above formula (1).
[0023] The polymer (A) preferably has the partial structure represented by the above formula (1) in that a liquid crystal element can be obtained which exhibits good voltage retention characteristics while exhibiting a higher effect of reducing residual images due to accumulated charges. In addition, the polymer (A) preferably has the partial structure (AN) in the main chain in that it exhibits good liquid crystal alignment characteristics while improving film strength, and the polymer (A) preferably has the partial structure (AN) in the side chain in that it can improve voltage retention characteristics.
[0024] The main skeleton of the (A) polymer is not particularly limited as long as it has a structural unit derived from a diamine compound. Examples of the (A) polymer include polymers having a polyamic acid, a polyamic acid ester, a polyimide, a polyamine, a polyenamine, a polyamide, a polyamideimide, and a polyurea as the main skeleton. The polyenamine is a polymer having a carbon-carbon double bond adjacent to the amino group of the polyamine, and examples thereof include polyenaminoketone, polyenaminoester, polyenaminonitrile, and polyenaminosulfonyl.
[0025] Of the above, the polymer (A) is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyurea, and polyamideimide, in that a liquid crystal element excellent in liquid crystal alignment property and voltage retention property can be obtained. Among these, the polymer (A) is more preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide, and particularly preferably at least one selected from the group consisting of polyamic acid and polyimide.
[0026] The (A) polymer preferably contains a structural unit derived from a diamine having a partial structure (AN) in that a liquid crystal element having good liquid crystal alignment, high voltage holding ratio, and sufficient suppression of generation of afterimages due to accumulation of residual charges can be obtained, and that a monomer having a partial structure (AN) is easy to synthesize or obtain and the partial structure (AN) is easy to introduce into the polymer. In the (A) polymer, the ratio of the structural unit derived from a diamine having a partial structure (AN) is preferably 1 mol % or more, more preferably 5 mol % or more, and even more preferably 10 mol % or more, based on the total amount of the structural units (i.e., monomer units) constituting the (A) polymer. In addition, the ratio of the structural unit derived from a diamine having a partial structure (AN) is, for example, 50 mol % or less, and preferably 40 mol % or less, based on the total amount of the structural units constituting the (A) polymer.
[0027] Next, a preferred example of the polymer contained in the liquid crystal aligning agent of the present disclosure will be described. When the polymer (A) is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide, the polymer (A) can be obtained, for example, by a method including a step of polycondensing a tetracarboxylic acid derivative and a diamine compound.
[0028] (Polyamic acid) When the polymer (A) is a polyamic acid, the polyamic acid having the partial structure (AN) (hereinafter, also referred to as "polyamic acid (A)") can be obtained by reacting a tetracarboxylic dianhydride with a diamine compound. A specific method is the following [Method 1]. [Method 1] A tetracarboxylic dianhydride and a diamine compound containing a diamine having a partial structure (AN) (hereinafter also referred to as a "specific diamine") are polycondensed. It is preferable to use [Method 1], since it allows for a wide range of monomer options and is easy to synthesize monomers and polymers.
[0029] Tetracarboxylic acid dianhydride Examples of the tetracarboxylic acid dianhydride used in the synthesis of the polyamic acid include aliphatic tetracarboxylic acid dianhydrides, aromatic tetracarboxylic acid dianhydrides, etc. The aliphatic tetracarboxylic acid dianhydrides include linear tetracarboxylic acid dianhydrides and alicyclic tetracarboxylic acid dianhydrides.
[0030] Specific examples of these include 1,2,3,4-butanetetracarboxylic dianhydride as a chain tetracarboxylic dianhydride; Alicyclic tetracarboxylic dianhydrides include 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentane tetracarboxylic dianhydride, cyclohexane tetracarboxylic dianhydride, and the like; Examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol bisanhydrotrimate, 4,4'-carbonyldiphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 3,3',4,4'-diphenylethertetracarboxylic dianhydride. As the tetracarboxylic dianhydride, the tetracarboxylic dianhydride described in JP-A-2010-97188 can be used. As the tetracarboxylic dianhydride, one type can be used alone or two or more types can be used in combination.
[0031] The tetracarboxylic dianhydride used in the synthesis of the polyamic acid preferably contains an aliphatic tetracarboxylic dianhydride, and more preferably contains an alicyclic tetracarboxylic dianhydride, in terms of increasing the solubility of the polymer and enabling the production of a liquid crystal alignment film exhibiting good electrical properties. The amount of the aliphatic tetracarboxylic dianhydride used is preferably 20 mol % or more, more preferably 40 mol % or more, and even more preferably 50 mol % or more, based on the total amount of the tetracarboxylic dianhydride used in the synthesis of the polyamic acid.
[0032] Diamine compounds The specific diamine may have the partial structure (AN) in the main chain, in the side chain, or in both. The number of partial structures (AN) that the specific diamine has is not particularly limited. Specific examples of the specific diamine include compounds represented by the following formulas (a1-1) to (a1-16), which are diamines having the partial structure represented by the above formula (1). [ka]
[0033] A compound having a partial structure represented by the above formula (1) can be preferably used as the specific diamine, in that a liquid crystal element can be obtained which exhibits good voltage retention characteristics while exhibiting a higher effect of reducing residual images due to accumulated charges. In addition, in that the specific diamine can exhibit good liquid crystal alignment characteristics while improving film strength, it is preferable that the specific diamine has a structure which allows the partial structure (AN) to be introduced into the main chain of the polymer, and in that the voltage retention characteristics can be improved, it is preferable that the specific diamine has a structure which allows the partial structure (AN) to be introduced into the side chain of the polymer.
[0034] In synthesizing the (A) polymer, only the specific diamine may be used as the diamine compound. In addition, a diamine not having a partial structure (AN) (hereinafter also referred to as "other diamine") may be used together with the specific diamine. As the other diamine, a known compound may be used. As the other diamine, for example, an aliphatic diamine, an aromatic diamine, or a diaminoorganosiloxane may be mentioned. The aliphatic diamine includes a chain diamine and an alicyclic diamine.
[0035] Specific examples of other diamines include chain diamines such as metaxylylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, and hexamethylenediamine; alicyclic diamines such as 1,4-diaminocyclohexane and 4,4'-methylenebis(cyclohexylamine); Aromatic diamines include p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylether, 4-aminophenyl-4-aminobenzoate, 4,4'-diaminoazobenzene, 3,5-diaminobenzoic acid, 1,5-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,6-bis(4-aminophenoxy)hexane, bis[2-(4-aminophenyl)ethyl]hexanedioic acid, 1,4-bis-(4-aminophenyl)-piperazine, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane ... bis(4-aminophenyl)hexafluoropropane, 4,4'-(phenylenediisopropylidene)bisaniline, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-[4,4'-propane-1,3-diylbis(piperidine-1,4-diyl)]dianiline, 4,4'-diaminobenzanilide, 4,4'-diaminostilbene, 1,4 - Main chain diamines such as bis(4-aminophenyl)-piperazine, bis[2-(4-aminophenyl)ethyl]hexanedioic acid, 4,4'-diaminodiphenethyl urea, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 1,4-bis(4-aminophenoxy)benzene, and 4,4'-bis(4-aminophenoxy)biphenyl; Dodecanoxy-2,4-diaminobenzene, pentadecanoxy-2,4-diaminobenzene, hexadecanoxy-2,4-diaminobenzene, octadecanoxy-2,4-diaminobenzene, pentadecanoxy-2,5-diaminobenzene, octadecanoxy-2,5-diaminobenzene, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-2,4-diaminobenzene, cholestanyloxy-2,4-diaminobenzene, 3,5-diamino Cholestanyl aminobenzoate, cholestenyl 3,5-diaminobenzoate, lanostannyl 3,5-diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestane, 3,6-bis(4-aminophenoxy)cholestane, 4-(4'-trifluoromethoxybenzoyloxy)cyclohexyl-3,5-diaminobenzoate, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-butylcyclohexane, 3,5-diaminobenzoic acid = 5ξ-cholestan-3-yl, the following formula (E-1) [ka] (In formula (E-1), X I and X II are each independently a single bond, -O-, *-COO-, or *-OCO- (wherein "*" indicates a bond to the diaminophenyl group). I R is an alkanediyl group having 1 to 3 carbon atoms. II R is a single bond or an alkanediyl group having 1 to 3 carbon atoms. III is an alkyl group, an alkoxy group, a fluoroalkyl group, or a fluoroalkoxy group having 1 to 20 carbon atoms. a is 0 or 1. b is an integer of 0 to 3. c is an integer of 0 to 2. d is 0 or 1, provided that 1≦a+b+c≦3. Side chain type diamines such as compounds represented by the following formula: As the diaminoorganosiloxane, for example, 1,3-bis(3-aminopropyl)-tetramethylsiloxane tetramethyldisiloxane, etc., and the diamines described in JP 2010-97188 A can be used. When synthesizing the polyamic acid, the diamine compounds can be used alone or in combination of two or more.
[0036] Examples of the compound represented by formula (E-1) include compounds represented by the following formulas (E-1-1) to (E-1-4). [ka]
[0037] Specific examples of other diamines include 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, 3,6-diaminoacridine, N-ethyl-3,6-diaminocarbazole, N-phenyl-3,6-diaminocarbazole, and compounds represented by the following formulas (a2-1) to (a2-24). [ka] [ka] (In formula (a2-15), t is an integer of 1 to 10.)
[0038] [ka]
[0039] From the viewpoint of obtaining a liquid crystal element having good liquid crystal alignment, high voltage holding ratio, and sufficient suppression of generation of afterimages due to accumulation of residual charges, the polyamic acid (A) preferably has structural units derived from a specific diamine in an amount of 2 mol % or more relative to the structural units derived from a diamine compound contained in the polyamic acid (A). The structural units derived from a specific diamine in the polyamic acid (A) are more preferably 5 mol % or more, even more preferably 10 mol % or more, even more preferably 15 mol % or more, and particularly preferably 20 mol % or more relative to the structural units derived from a diamine compound contained in the polyamic acid (A). In addition, the structural units derived from a specific diamine in the polyamic acid (A) are preferably 95 mol % or less, more preferably 90 mol % or less, and even more preferably 80 mol % or less relative to the structural units derived from a diamine compound contained in the polyamic acid (A).
[0040] Synthesis of polyamic acid (A) The polyamic acid can be obtained by reacting the above-mentioned tetracarboxylic dianhydride with a diamine compound, if necessary, together with a molecular weight modifier. The ratio of the tetracarboxylic dianhydride and the diamine compound used in the synthesis reaction of the polyamic acid (A) is preferably such that the acid anhydride group of the tetracarboxylic dianhydride is 0.2 to 2 equivalents per equivalent of the amino group of the diamine compound. Examples of the molecular weight modifier include acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride, monoamine compounds such as aniline, cyclohexylamine, and n-butylamine, and monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate. The ratio of the molecular weight modifier used is preferably 20 parts by mass or less per 100 parts by mass of the total of the tetracarboxylic dianhydride and the diamine compound used.
[0041] The synthesis reaction of the polyamic acid (A) is preferably carried out in an organic solvent, preferably at a reaction temperature of −20° C. to 150° C., and for a reaction time of 0.1 to 24 hours. Examples of the organic solvent used in the reaction include aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons. Particularly preferred organic solvents are one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphortriamide, m-cresol, xylenol, and halogenated phenols, or a mixture of one or more of these with other organic solvents (e.g., butyl cellosolve, diethylene glycol diethyl ether, etc.). The amount (a) of the organic solvent used is preferably an amount such that the total amount (b) of the tetracarboxylic dianhydride and the diamine is 0.1 to 50% by mass relative to the total amount (a+b) of the reaction solution.
[0042] In this manner, a reaction solution in which the polyamic acid (A) is dissolved is obtained. This reaction solution may be used as it is for the preparation of a liquid crystal aligning agent, or the polyamic acid (A) contained in the reaction solution may be isolated and then used for the preparation of a liquid crystal aligning agent.
[0043] (Polyimide) When the polymer (A) is a polyimide, the polyimide (hereinafter also referred to as "polyimide (A)") can be obtained, for example, by dehydrating and ring-closing polyamic acid (A) to form an imidized polyimide. The imidization rate of the polyimide (A) is preferably 20 to 90%, and more preferably 30 to 85%. The imidization rate is the ratio, expressed as a percentage, of the number of imide ring structures to the total number of amic acid structures and imide ring structures of the polyimide.
[0044] The dehydration ring-closing of the polyamic acid (A) is preferably carried out by dissolving the polyamic acid (A) in an organic solvent, adding a dehydrating agent and a dehydration ring-closing catalyst to the solution, and heating as necessary. In this method, the dehydrating agent may be, for example, an acid anhydride such as acetic anhydride, propionic anhydride, or trifluoroacetic anhydride. The amount of the dehydrating agent used is preferably 0.01 to 20 moles per mole of the amic acid structure of the polyamic acid (A). The dehydration ring-closing catalyst may be, for example, a tertiary amine such as pyridine, collidine, lutidine, or triethylamine. The amount of the dehydration ring-closing catalyst used is preferably 0.01 to 10 moles per mole of the dehydrating agent used.
[0045] Examples of the organic solvent used in the dehydration ring-closing reaction include the organic solvents exemplified as those used in the synthesis of polyamic acid (A). The reaction temperature in the dehydration ring-closing reaction is preferably 0 to 180°C. The reaction time is preferably 1.0 to 120 hours. The reaction solution containing polyimide (A) may be used as it is for the preparation of a liquid crystal alignment agent. Also, polyimide (A) may be isolated from the reaction solution, and the isolated polyimide (A) may be used for the preparation of a liquid crystal alignment agent. Polyimide (A) can also be obtained by dehydration ring-closing of a polyamic acid ester.
[0046] In addition, the polyamic acid ester and polyamideimide as the polymer (A) can be obtained by using a specific diamine as a monomer in polymerization, similarly to the polyamic acid (A) and polyimide (A). Specifically, the polyamic acid ester can be obtained by a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound containing a specific diamine, etc. The polyamideimide can be obtained by a method of reacting a tricarboxylic acid derivative with a diamine compound containing a specific diamine, etc. The polyurea can be obtained by a method of reacting a diisocyanate compound with a diamine compound containing a specific diamine, etc.
[0047] The solution viscosity of the polymer (A) is preferably 10 to 800 mPa·s, and more preferably 15 to 500 mPa·s, when the polymer (A) is prepared as a 10% by mass solution. The solution viscosity (mPa·s) is a value measured at 25°C using an E-type rotational viscometer for a 10% by mass polymer solution prepared using a good solvent for the polymer (A) (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).
[0048] The weight average molecular weight (Mw) of the polymer (A) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, and more preferably 2,000 to 300,000. The molecular weight distribution (Mw / Mn), which is expressed as the ratio of Mw to the number average molecular weight (Mn) measured by GPC in terms of polystyrene, is preferably 7 or less, and more preferably 5 or less.
[0049] The content of the (A) polymer in the liquid crystal alignment agent is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more, based on the total amount of solids contained in the liquid crystal alignment agent (i.e., the total mass of components other than the solvent of the liquid crystal alignment agent).
[0050] <(B) Compound> The (B) compound is a compound having three or more partial structures (T) in one molecule, in which one or more hydrogen atoms bonded to heteroatoms in a nucleophilic functional group or an acidic functional group are replaced with a leaving group (hereinafter, also simply referred to as a "leaving group") that is released by at least one of heat and light. However, the (B) compound is a compound different from the polymer. Therefore, the (B) compound is blended in the liquid crystal alignment agent as a component different from the (A) polymer. From the viewpoint of increasing the film strength, the molecular weight of the (B) compound is preferably 3,000 or less, more preferably 2,000 or less, even more preferably 1,000 or less, and even more preferably 800 or less.
[0051] Examples of the (B) compound include a compound having, as the partial structure (T), three or more partial structures in one molecule in which one or more hydrogen atoms bonded to heteroatoms in a nucleophilic functional group are replaced with leaving groups (hereinafter also referred to as "compound (B1)"), and a compound having, as the partial structure (T), three or more partial structures in one molecule in which one or more hydrogen atoms bonded to heteroatoms in an acidic functional group are replaced with leaving groups (hereinafter also referred to as "compound (B2)").
[0052] ·Compound (B1) In the compound (B1), examples of the nucleophilic functional group include a primary amino group, a secondary amino group, a thiol group, and a hydroxyl group. The hydroxyl group contained in the hydroxyalkylamide group does not fall under the category of a nucleophilic functional group. In the compound (B1), some of the multiple nucleophilic functional groups may be protected by a leaving group, or all of the multiple nucleophilic functional groups may be protected by a leaving group. From the viewpoint of improving the storage stability of the liquid crystal aligning agent, it is preferable that all of the nucleophilic functional groups are protected by a leaving group.
[0053] In addition, in the compound (B1), when the primary amino group as the nucleophilic functional group is protected by a leaving group, only one of the two hydrogen atoms bonded to the primary amino group may be replaced by a leaving group, or both hydrogen atoms may be replaced by leaving groups. In both cases where only one of the two hydrogen atoms bonded to the primary amino group is replaced by a leaving group and where both hydrogen atoms are replaced by leaving groups, the number of partial structures (T) is counted as one. That is, the number of partial structures (T) in the compound (B) represents the number of nucleophilic functional groups or acidic functional groups protected by leaving groups.
[0054] The compound (B1) may have a partial structure in which one or more hydrogen atoms bonded to heteroatoms in the nucleophilic functional group are replaced with leaving groups, and a partial structure in which one or more hydrogen atoms bonded to heteroatoms in the acidic functional group are replaced with leaving groups. However, from the viewpoint of improving the storage stability of the liquid crystal alignment agent, it is preferable that the compound (B1) does not have an acidic functional group (i.e., an unprotected acidic functional group).
[0055] The leaving group of the compound (B1) is preferably a group that is released by heat. Examples of the leaving group that replaces the hydrogen atom bonded to the nitrogen atom include a carbamate-based leaving group, an amide-based leaving group, an imide-based leaving group, and a sulfonamide-based leaving group. Among these, a carbamate-based leaving group is preferred because of its high thermal release property, and specific examples thereof include a tert-butoxycarbonyl group (Boc group), a benzyloxycarbonyl group, a 1,1-dimethyl-2-haloethyloxycarbonyl group, a 1,1-dimethyl-2-cyanoethyloxycarbonyl group, a 9-fluorenylmethyloxycarbonyl group (Fmoc group), an allyloxycarbonyl group, and a 2-(trimethylsilyl)ethoxycarbonyl group. Among these, a tert-butoxycarbonyl group (Boc group) is particularly preferred since it is easily removable by heat and can reduce the amount of the compound derived from the deprotected structure remaining in the film.
[0056] Examples of the leaving group that replaces the hydrogen atom bonded to an oxygen atom or a sulfur atom include ether-based leaving groups such as methyl, ethyl, tert-butyl, benzyl, p-methoxybenzyl, and trityl groups; acetal-based leaving groups such as methoxymethyl, ethoxyethyl, and 2-tetrahydropyranyl groups; acyl-based leaving groups such as acetyl, pivaloyl, benzoyl, and trichloroacetyl groups; allyl-based leaving groups such as allyl and methallyl groups; carbamate-based leaving groups such as tert-butoxycarbonyl groups; and silyl ether-based leaving groups such as trimethylsilyl, triethylsilyl, and tert-butyldimethylsilyl groups. From the viewpoint of achieving both ease of removal by heat and storage stability, the leaving group that replaces the hydrogen atom bonded to an oxygen atom or a sulfur atom is preferably an alkyl group having 1 to 7 carbon atoms, a 2-tetrahydropyranyl group, a methoxymethyl group, a 1-ethoxyethyl group, or an acetyl group.
[0057] The number of partial structures (T) contained in the compound (B1) may be 3 or more. From the viewpoint of obtaining a liquid crystal element exhibiting good liquid crystal alignment property, the number of partial structures (T) contained in the compound (B1) is preferably 12 or less, more preferably 10 or less, and further preferably 8 or less.
[0058] A preferred specific example of the compound (B1) is a compound represented by the following formula (2). [ka] (In formula (2), X 1 and X 5 are each independently a nitrogen atom, a sulfur atom, an oxygen atom, or a group represented by the following formula (x-1): 1 is a leaving group. R 2a and R 2b are each independently a hydrogen atom or a monovalent organic group. 3 is an organic group with a valence of (k1+k2). k1 is X 1 is an integer of 3 or more when it is a sulfur atom or an oxygen atom, 1is an integer of 2 or more when k1 is a nitrogen atom or a group represented by the following formula (x-1). However, when k1=2, R 3 has one or more leaving groups bonded to the nitrogen atom. 1 is a sulfur atom or an oxygen atom, m=1 and n1=0, and X 1 is a nitrogen atom or a group represented by the following formula (x-1), m is 1 or 2 and satisfies (m+n1)=2. k2 is an integer of 0 to 2. n2 is X 5 is a sulfur atom or an oxygen atom, then 1; 5 is a nitrogen atom or a group represented by the following formula (x-1), the value is 2. 1 are the same or different. 1 If there are multiple Ys, 1 are the same or different, and R 2a If there are multiple R 2a are the same or different. X in the formula 5 If there are multiple Xs, 5 are the same or different. 2b If there are multiple R 2b are the same or different.) [ka] (In formula (x-1), R 4 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. "*" represents a bond. However, when the carbonyl group in formula (x-1) is R 3 )
[0059] In the above formula (2), X 1 Or X 5 is a group represented by the above formula (x-1), R in formula (x-1) 4 Examples of the monovalent hydrocarbon group in R include an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 6 to 10 carbon atoms. 4 is preferably a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group, and more preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. X 1 Among the above, a nitrogen atom, a sulfur atom, or a group represented by the above formula (x-1) is preferred, and a nitrogen atom or a group represented by the above formula (x-1) is more preferred, in that the group generated by elimination of the leaving group has high crosslinking reactivity. X 5 Among the above, a nitrogen atom, a sulfur atom, or a group represented by the above formula (x-1) is preferred, and a nitrogen atom or a group represented by the above formula (x-1) is more preferred, in terms of high crosslinking reactivity.
[0060] Y 1 is preferably a group which is eliminated by heat. 1 is a nitrogen atom or a group represented by the above formula (x-1), 1 , X 1 is an oxygen atom or a sulfur atom, 1 Examples of the leaving group include the same specific and preferred examples as those given in the description of the leaving group contained in compound (B1).
[0061] R 2a or R 2b The monovalent organic group represented by the formula (I) is preferably a monovalent hydrocarbon group having 1 to 12 carbon atoms. 2 is preferably a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0062] R 3 The (k1+k2)-valent organic group represented by X 1 A structure that does not inhibit the nucleophilicity of R is preferred. 3 From the viewpoint of sufficiently increasing the film strength, the (k1+k2)-valent organic group represented by the formula (1) preferably has 1 to 40 carbon atoms. Specific examples of the (k1+k2)-valent organic group include (k1+k2)-valent hydrocarbon groups having 1 to 40 carbon atoms, and the hydrocarbon groups each having -O-, -S-, -CO-, -COO-, -NR 5 -, -CO-NR 5 -, -NR 5 -CO-O-, -NR 5 -CO-NR 6 -, -CO-NR 5-NR 6 -, a (k1+k2)-valent group containing a tertiary nitrogen atom or a heterocycle (wherein R 5 and R 6 are each independently a hydrogen atom or a monovalent organic group.) and the like. Here, examples of the hydrocarbon group having 1 to 40 carbon atoms include a chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Among these, a chain hydrocarbon group is preferred in that it can increase the crosslinking reactivity and can form a film having good liquid crystal alignment properties and voltage retention properties. R 5 or R 6 The monovalent organic group represented by the formula (I) is preferably a monovalent hydrocarbon group or a thermally eliminable group having 1 to 10 carbon atoms, more preferably a monovalent hydrocarbon group or a thermally eliminable group having 1 to 6 carbon atoms, and even more preferably an alkyl group or a tert-butoxycarbonyl group having 1 to 6 carbon atoms.
[0063] R is advantageous in that it has higher crosslinking reactivity and can produce a liquid crystal alignment film that exhibits good liquid crystal alignment properties. 3 is preferably a (k1+k2)-valent group that does not have an aromatic ring. 3 is a (k1+k2)-valent chain hydrocarbon group, or the chain hydrocarbon group has -O-, -S-, -CO-, -COO-, -NR 5 -, -CO-NR 5 -, -NR 5 -CO-O-, -NR 5 -CO-NR 6 -, -CO-NR 5 -NR 6 R is preferably a (k1+k2)-valent group containing a -, tertiary nitrogen atom, or a non-aromatic heterocycle. Here, the (k1+k2)-valent chain hydrocarbon group preferably has 2 to 30 carbon atoms, more preferably 3 to 20 carbon atoms. The non-aromatic heterocycle is preferably a nitrogen-containing ring, and examples of such rings include a piperidine ring, a pyrrolidine ring, a hexamethyleneimine ring, a morpholine ring, and an isocyanurate ring. 3 Preferred specific examples include structures represented by the following formulae (r-1) to (r-4). [ka] (In formulas (r-1) to (r-4), t is an integer of 0 to 18. 2 and X 3 are each independently -O-, -S-, -CO-, -COO-, -NR 5 -, -CO-NR 5 -, -NR 5 -CO-O-, -NR 5 -CO-NR 6 -or-CO-NR 5 -NR 6 t1, t2 and t3 are each independently an integer of 1 to 10. u is an integer of 0 to 3. R 20 is a divalent group represented by the above formula (r-1) or (r-2). 20 are the same or different. "*" represents a bond.)
[0064] X 1 When is a nitrogen atom or a group represented by the above formula (x-1), m is preferably 1 or 2 in that the liquid crystal alignment properties and voltage retention characteristics can be well maintained.
[0065] From the viewpoint of improving the liquid crystal alignment property, the voltage retention property, and the film strength in a well-balanced manner, k1 is preferably an integer of 2 to 10, more preferably an integer of 2 to 6, and further preferably an integer of 2 to 4. When k1 is 2, R 3 has one or more leaving groups bonded to a nitrogen atom, and has -NR 5a -(However, R 5a is a leaving group.) is preferred. Among them, k1 is 2 and R 3 Compounds having one or more leaving groups bonded to a nitrogen atom are particularly preferred in that they can maintain good liquid crystal alignment while improving voltage retention characteristics, film strength, and DC image retention characteristics in a well-balanced manner. 3 However, -NR is formed between the carbon-carbon bonds of the chain hydrocarbon group. 5a -, R 3 -NR 5a The number of - is preferably 1 to 5, and more preferably 1 to 3, from the viewpoint of maintaining good liquid crystal alignment. From the viewpoint of improving the storage stability of the liquid crystal aligning agent, k2 is preferably 0 or 1, and more preferably 0.
[0066] Specific examples of the compound (B1) include compounds represented by the following formulas (b1-1) to (b1-8). [ka]
[0067] ·Compound (B2) In the compound (B2), examples of the acidic functional group include a carboxylic acid group, a phosphoric acid group, a phosphorous acid group, and a sulfonic acid group. In the compound (B2), a part or all of the multiple acidic functional groups are protected by a leaving group. From the viewpoint of improving the storage stability of the liquid crystal aligning agent, it is preferable that all of the acidic functional groups present in the molecule are protected by a leaving group.
[0068] The leaving group of the compound (B2) is preferably a group that is released by heat. The leaving group is preferably a group that substitutes a hydrogen atom of an OH group contained in a carboxylic acid group, a phosphoric acid group, a phosphorous acid group, or a sulfonic acid group, and specifically, "*-OL 1 " (However, L 1 is a leaving group, and "*" represents a bond. 1 is preferably a group which is eliminated by heat and is replaced with a hydrogen atom. 1 Specific examples of the group represented by the formula (L1-1) include groups represented by the following formulas (L1-1) to (L1-8). [ka] (In formulas (L1-1) to (L1-8), "*" represents a bond.)
[0069] The compound (B2) may have a partial structure in which one or more hydrogen atoms bonded to heteroatoms in the acidic functional group are replaced with a leaving group, and a partial structure in which one or more hydrogen atoms bonded to heteroatoms in the nucleophilic functional group are replaced with a leaving group. However, from the viewpoint of increasing the storage stability of the liquid crystal alignment agent, it is preferable that the compound (B2) does not have a nucleophilic functional group (i.e., an unprotected nucleophilic functional group).
[0070] The number of partial structures (T) contained in the compound (B2) may be 3 or more. From the viewpoint of obtaining a liquid crystal element exhibiting good liquid crystal alignment property, the number of partial structures (T) contained in the compound (B1) is preferably 12 or less, more preferably 10 or less, and further preferably 8 or less.
[0071] A preferred specific example of the compound (B2) is a compound represented by the following formula (3). [ka] (In formula (3), X 4 is a carboxylate group, a phosphate group, a phosphite group or a sulfonate group. 5 R is a protected carboxylic acid group, a protected phosphate group, a protected phosphite group, or a protected sulfonate group. 7 is an organic group having a valence of (i+j). i is an integer of 0 or more. j is an integer of 3 or more. When i is 2, multiple X 4 are the same or different. 5 are the same or different.)
[0072] In the above formula (3), X 5 is a group in which a hydrogen atom of an OH group contained in a carboxylic acid group, a phosphoric acid group, a phosphorous acid group, or a sulfonic acid group is replaced with a leaving group, and "*-OL 1 " has a group represented by "*-OL 1 Specific examples of the group represented by the formula (L1-1) include the groups represented by the formulas (L1-1) to (L1-8) above.
[0073] R 7The (i+j)-valent organic group represented by X 4 and X 5 It is preferable that the (i+j)-valent organic group has a carbon number of 1 to 40 from the viewpoint of sufficiently increasing the film strength. Specific examples of the (i+j)-valent organic group include (i+j)-valent hydrocarbon groups having 1 to 40 carbon atoms, -O-, -S-, -CO-, -COO-, -NR-, -O ... 8 -, -CO-NR 8 -, -NR 8 -CO-O-, -NR 8 -CO-NR 9 -, -CO-NR 8 -NR 9 -, a (i+j)-valent group containing a tertiary nitrogen atom or a heterocycle. 8 or R 9 The monovalent organic group represented by the formula (I) is preferably a monovalent hydrocarbon group or a thermally eliminable group having 1 to 10 carbon atoms, more preferably a monovalent hydrocarbon group or a thermally eliminable group having 1 to 6 carbon atoms, and even more preferably an alkyl group or a tert-butoxycarbonyl group having 1 to 6 carbon atoms.
[0074] R is advantageous in that it has higher crosslinking reactivity and can produce a liquid crystal alignment film with excellent liquid crystal alignment and voltage retention properties. 7 is preferably a (i+j)-valent group that does not have an aromatic ring. 7 is a (i+j)-valent chain hydrocarbon group, or the chain hydrocarbon group has -O-, -S-, -CO-, -COO-, -NR 8 -, -CO-NR 8 -, -NR 8 -CO-O-, -NR 8 -CO-NR 9 -, -CO-NR 8 -NR 9It is preferably an (i+j)-valent group containing a -, tertiary nitrogen atom or a non-aromatic heterocycle, or an (i+j)-valent alicyclic hydrocarbon group. Here, the (i+j)-valent chain hydrocarbon group preferably has 2 to 30 carbon atoms, more preferably 3 to 20 carbon atoms. The non-aromatic heterocycle is preferably a nitrogen-containing ring, such as a piperidine ring, a pyrrolidine ring, a hexamethyleneimine ring, a morpholine ring, or an isocyanurate ring.
[0075] From the viewpoint of adhesion of the liquid crystal alignment film, R 7 is a (i+j)-valent chain hydrocarbon group, or -O-, -S-, -CO-, -COO-, -NR 8 -, -CO-NR 8 -, -NR 8 -CO-O-, -NR 8 -CO-NR 9 -, -CO-NR 8 -NR 9 It is preferably a (i+j)-valent group containing a -, a tertiary nitrogen atom or a non-aromatic heterocycle.
[0076] Specific examples of the compound (B2) include polyfunctional carboxylic acids having three or more carboxy groups, polyfunctional phosphoric acids having three or more phosphoric acid groups, polyfunctional phosphorous acids having three or more phosphorous acid groups, and polyfunctional sulfonic acids having three or more sulfonic acid groups, in which at least three of the acidic groups of each compound are protected. Among these, from the viewpoint of increasing the reactivity with the functional groups of the (A) polymer, compounds in which at least three of the carboxy groups of a polyvalent carboxylic acid having three or more carboxy groups are protected can be preferably used.
[0077] Further specific examples of the compound (B2) include compounds in which three carboxy groups of tricarboxylic acids, such as 1,2,4-butanetricarboxylic acid, 1,2,3-cyclohexanetricarboxylic acid, trimellitic acid, and 1,2,4-naphthalenetricarboxylic acid, are protected; compounds in which three or more of four carboxy groups of tetracarboxylic acids, such as 1,2,3,4-cyclobutanetetracarboxylic acid, 2,3,5-tricarboxycyclopentylacetic acid, cyclopentanetetracarboxylic acid, cyclohexanetetracarboxylic acid, and pyromellitic acid, are protected; and compounds represented by the following formulae (b2-1) to (b2-3), respectively. [ka] (In the formulas (b2-1) to (b2-3), a plurality of L 2 are each independently a thermally labile group.
[0078] Among the above, compound (B1) is preferable as compound (B), since it is possible to obtain a liquid crystal alignment film having higher film strength while improving liquid crystal alignment properties and voltage retention characteristics, and a compound having three or more protected nitrogen atoms in one molecule is more preferable.
[0079] The content of the (B) compound in the liquid crystal alignment agent of the present disclosure is preferably 0.2 parts by mass or more relative to 100 parts by mass of the (A) polymer contained in the liquid crystal alignment agent from the viewpoint of obtaining a liquid crystal element having excellent voltage retention characteristics and from the viewpoint of sufficiently increasing the film strength of the liquid crystal alignment film. The content of the (B) compound is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the (A) polymer. In addition, from the viewpoint of suppressing the deterioration of the liquid crystal alignment property, the content of the (B) compound is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the (A) polymer.
[0080] The content of the (B) compound relative to a total of 100 parts by mass of the polymer components contained in the liquid crystal alignment agent is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more. The content of the (B) compound relative to a total of 100 parts by mass of the polymer components contained in the liquid crystal alignment agent is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less. As the (B) compound, one type may be used alone, or two or more types may be used in combination.
[0081] <Other ingredients> The liquid crystal aligning agent may further contain, in addition to the polymer (A) and the compound (B), a component (other component) different from the polymer (A) and the compound (B), if necessary.
[0082] ·(C) Polymer The liquid crystal alignment agent of the present disclosure may further contain a polymer different from the (A) polymer (hereinafter, also referred to as "(C) polymer") as a polymer component. The (C) polymer may be a polymer that does not have a partial structure (AN), and its main skeleton is not particularly limited. Examples of the (C) polymer include polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, polyester, polyenamine, polyurea, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivative, polyacetal, and addition polymer. From the viewpoint of obtaining a liquid crystal element having excellent properties such as liquid crystal alignment when used together with the (A) polymer, the (C) polymer is preferably a polymer having a structural unit derived from a diamine compound and not having a partial structure represented by the above formula (1). Specific examples of the (C) polymer when the (C) polymer has a structural unit derived from a diamine compound include polyamic acid, polyamic acid ester, polyimide, polyamine, polyenamine, polyamide, polyamideimide, and polyurea.
[0083] From the viewpoint of obtaining a highly reliable liquid crystal element, the polymer (C) is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyurea, polyamideimide, polyorganosiloxane, and addition polymer, and more preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymer. Of these, the polymer (C) is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, and addition polymer, and more preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
[0084] When the (C) polymer is contained in the liquid crystal alignment agent, the content of the (C) polymer is, for example, 1% by mass or more, and may be 2% by mass or more, based on the total amount of the (A) polymer and the (C) polymer. From the viewpoint of obtaining a liquid crystal element with better liquid crystal alignment, the content of the (C) polymer is preferably 5% by mass or more, and more preferably 10% by mass or more, based on the total amount of the (A) polymer and the (C) polymer. The content of the (C) polymer is preferably 95% by mass or less, and more preferably 90% by mass or less, based on the total amount of the (A) polymer and the (C) polymer. As the (C) polymer, one type may be used alone, or two or more types may be used in combination.
[0085] ·solvent The liquid crystal aligning agent of the present disclosure is prepared as a liquid composition in which the polymer (A), the compound (B), and other components used as necessary are preferably dispersed or dissolved in a suitable solvent.
[0086] As the solvent, an organic solvent is preferably used.Specific examples thereof include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,2-dimethyl-2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone, phenol, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, diacetone alcohol, 1-hexanol, 2-hexanol, propane-1,2-diol, 3-methoxy-1-butanol, ethylene glycol monomethyl ether, methyl lactate, ethyl lactate, butyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, ethyl acetoacetate, ethyl propionate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, and ethylene glycol-i-propyl ether. Examples of the solvent include ethylene glycol-n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, propylene carbonate, propylene glycol monomethyl ether (PGME), diethylene glycol diethyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol diacetate, cyclopentanone, cyclohexanone, etc. As the solvent, one type can be used alone or two or more types can be mixed and used.
[0087] Other components contained in the liquid crystal alignment agent include, in addition to the above, for example, antioxidants, metal chelate compounds, curing accelerators, surfactants, fillers, dispersants, photosensitizers, etc. The blending ratio of other components can be appropriately selected according to each compound within a range that does not impair the effects of the present disclosure.
[0088] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of the components other than the solvent of the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is appropriately selected in consideration of viscosity, volatility, etc. The solid content concentration of the liquid crystal alignment agent is preferably in the range of 1 to 10 mass %. If the solid content concentration is 1 mass % or more, it is preferable in that the thickness of the coating film can be sufficiently ensured and a liquid crystal alignment film showing better liquid crystal alignment properties can be obtained. On the other hand, if the solid content concentration is 10 mass % or less, the coating film can be made to have an appropriate thickness, and a liquid crystal alignment film showing good liquid crystal alignment properties can be easily obtained, and the viscosity of the liquid crystal alignment agent becomes appropriate, tending to improve the coatability.
[0089] In the liquid crystal alignment agent of the present disclosure, the content ratio of the structural unit derived from the diamine having the partial structure (AN) in the polymer component contained in the liquid crystal alignment agent (hereinafter also referred to as "specific N-containing structure ratio") is 0.13 mol or more per mol of the total amount of the structural units derived from the diamine compound in the polymer component. If the specific N-containing structure ratio is less than 0.13 mol per mol of the total amount of the structural units derived from the diamine compound in the polymer component, the reliability of the voltage holding ratio (VHR reliability) is insufficient and the DC afterimage characteristics are deteriorated.
[0090] From the viewpoint of obtaining a liquid crystal element having a well-balanced improvement in liquid crystal alignment property, voltage retention property, VHR reliability, and DC afterimage property, and obtaining a liquid crystal alignment film having sufficiently high film strength, the specific N-containing structure ratio is preferably 0.14 mol or more per mol of the total amount of structural units derived from diamine compounds in the polymer component. Also, the specific N-containing structure ratio is preferably 0.90 mol or less, more preferably 0.80 mol or less, per mol of the total amount of structural units derived from monomers in the polymer component. Note that the partial structure (AN) is considered to have a high degree of contribution to the effect of reducing the occurrence of afterimages caused by charge accumulation, and therefore, it is considered that the effect against afterimages caused by charge accumulation can be more accurately reflected by expressing the amount of the structural units derived from diamines having the partial structure (AN) as a ratio based on the total amount of structural units derived from diamine compounds in the polymer component.
[0091] Specifically, when the liquid crystal alignment agent contains only the (A) polymer as a polymer component (i.e., when it contains the (A) polymer and does not contain the (C) polymer), the specific N-containing structure ratio is calculated by the ratio of the structural units derived from the specific diamine contained in the (A) polymer to the total amount of the structural units derived from the diamine compound constituting the (A) polymer. For example, in the case of a liquid crystal alignment agent in which the content ratio of the structural units derived from the specific diamine in the (A) polymer is 20 mol% relative to the total amount of the structural units derived from the diamine compound constituting the (A) polymer, the specific N-containing structure ratio is 0.20 mol.
[0092] In addition, when the liquid crystal alignment agent contains the (A) polymer and the (C) polymer as the polymer components, the specific N-containing structure ratio is calculated by the ratio of the structural unit derived from the specific diamine contained in the (A) polymer to the total amount of the structural units derived from the diamine compound constituting the (A) polymer and the total amount of the structural units derived from the diamine compound constituting the (C) polymer (i.e., the total amount of the structural units derived from the diamine compound in the polymer components). For example, in the case of a liquid crystal alignment agent containing a first polymer having a structural unit derived from the specific diamine and a second polymer having no structural unit derived from the specific diamine as the polymer components, the content ratio of the first polymer is 80 parts by mass relative to 100 parts by mass of the total amount of the polymer components, the content ratio of the second polymer is 20 parts by mass relative to 100 parts by mass of the total amount of the polymer components, and the content ratio of the structural unit derived from the specific diamine in the first polymer is 20 mol% relative to the total amount of the structural units derived from the diamine compound constituting the first polymer, the specific N-containing structure ratio is 20 [mol%] × 0.8 / 100 = 0.16 mol.
[0093] <Liquid crystal alignment film and its manufacturing method> The liquid crystal alignment film of the present disclosure is formed by the liquid crystal alignment agent prepared as described above. The liquid crystal alignment film can be produced by a method including the following coating film formation process. The liquid crystal alignment film of the present disclosure may be provided with liquid crystal alignment ability by performing liquid crystal alignment treatment on the organic film obtained by the coating film formation process by the following alignment treatment process.
[0094] ·Coating film formation process In producing a liquid crystal alignment film, first, a liquid crystal alignment agent is applied onto a substrate, and then the applied surface is preferably heated to form a coating film on the substrate. As the substrate, for example, a transparent substrate made of glass such as float glass or soda glass, or plastic such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, or poly(alicyclic olefin) can be used.
[0095] The method of applying the liquid crystal alignment agent to the substrate is not particularly limited. The liquid crystal alignment agent can be applied to the substrate by, for example, a spin coat method, a printing method (for example, an offset printing method, a flexographic printing method, etc.), an inkjet method, a slit coat method, a bar coater method, an extrusion die method, a direct gravure coater method, a chamber doctor coater method, an offset gravure coater method, an impregnation coater method, an MB coater method, etc.
[0096] After the liquid crystal alignment agent is applied, preheating (prebaking) is preferably performed for the purpose of preventing dripping of the applied liquid crystal alignment agent. The prebaking temperature is preferably 30 to 200° C., and the prebaking time is preferably 0.25 to 10 minutes. Thereafter, the solvent is completely removed, and a baking (postbaking) step is performed, if necessary, for the purpose of thermally imidizing the amic acid structure present in the polymer. The baking temperature (postbaking temperature) at this time is preferably 80 to 280° C., more preferably 80 to 250° C. The postbaking time is preferably 5 to 200 minutes. The thickness of the film formed is preferably 0.001 to 1 μm.
[0097] ·Orientation process In the alignment treatment step, the liquid crystal alignment agent is applied onto the substrate, and after the application, a heat treatment is preferably performed, and then a rubbing treatment or a light irradiation treatment is preferably performed to impart liquid crystal alignment ability. In the rubbing treatment, the coating film formed on the substrate is rubbed in a certain direction with a roll wrapped with a cloth made of fibers such as nylon, rayon, or cotton, to impart liquid crystal alignment ability to the coating film. In the light alignment treatment, the coating film formed on the substrate is irradiated with light to impart liquid crystal alignment ability to the coating film.
[0098] In the photo-alignment treatment, the light irradiation can be performed by a method of irradiating the coating film after the post-bake step, a method of irradiating the coating film after the pre-bake step but before the post-bake step, or a method of irradiating the coating film during heating in at least one of the pre-bake step and the post-bake step. For example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm can be used as the radiation to be irradiated to the coating film. Preferably, ultraviolet light containing light with a wavelength of 200 to 400 nm is used. When the radiation is polarized, it may be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the irradiation may be performed from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When the radiation is non-polarized, the irradiation direction is an oblique direction.
[0099] Examples of the light source used include a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. The radiation dose is preferably 400 to 50,000 J / m 2 and more preferably 1,000 to 20,000 J / m 2 After the light irradiation for imparting the alignment ability, the surface of the substrate may be washed with, for example, water, an organic solvent (e.g., methanol, isopropyl alcohol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.
[0100] Liquid crystal element The liquid crystal element of the present disclosure includes a liquid crystal alignment film formed using the liquid crystal alignment agent described above. The driving method of the liquid crystal in the liquid crystal element is not particularly limited, and can be applied to various modes such as TN type, STN type, VA type (including VA-MVA type, VA-PVA type, etc.), IPS (In Plane Switching) type, FFS (Fringe Field Switching) type, OCB (Optically Compensated Bend) type, PSA (Polymer Sustained Alignment) type, etc. The liquid crystal element can be manufactured, for example, by a method including the above-mentioned coating film formation step and alignment treatment step, and the following cell construction step.
[0101] The substrates used in the coating film formation process vary depending on the desired operation mode. For example, when manufacturing a TN-type, STN-type, or VA-type liquid crystal element, two substrates with patterned transparent conductive films are used. When manufacturing an IPS-type or FFS-type liquid crystal element, a substrate with electrodes patterned into a comb-tooth shape and an opposing substrate with no electrodes are used. Tin oxide (SnO 2 NESA membrane (registered trademark of PPG, USA) made of indium oxide-tin oxide (In 2 O 3 -SnO 2 ) can be used.
[0102] When manufacturing a TN-type, STN-type, IPS-type or FFS-type liquid crystal element, a treatment (alignment treatment) is carried out to impart liquid crystal alignment ability to the coating film obtained by the coating film formation process. This imparts the alignment ability of liquid crystal molecules to the coating film, forming a liquid crystal alignment film. On the other hand, when manufacturing a vertical alignment (VA) type liquid crystal element, the coating film obtained by the coating film formation process can be used as a liquid crystal alignment film as it is. In addition, in order to further enhance the liquid crystal alignment ability, the coating film may be subjected to an alignment treatment. A liquid crystal alignment film suitable for a vertical alignment type liquid crystal element is also suitable for a PSA type liquid crystal element.
[0103] Cell construction process Two substrates on which the liquid crystal alignment film is formed as described above are prepared, and a liquid crystal cell is manufactured so that the liquid crystal is disposed adjacent to the liquid crystal alignment film between the two substrates. For example, the liquid crystal cell can be manufactured by disposing two substrates facing each other with a gap therebetween so that the liquid crystal alignment film faces each other, bonding the peripheries of the two substrates with a sealant, injecting liquid crystal into the cell gap surrounded by the substrate surfaces and the sealant, and sealing the injection hole, or by a method using the ODF method. For example, an epoxy resin containing a hardener and aluminum oxide spheres as a spacer can be used as the sealant. For the liquid crystal, nematic liquid crystal and smectic liquid crystal can be mentioned, and among them, nematic liquid crystal is preferred. In the PSA mode, after the liquid crystal cell is constructed, a process is performed in which the liquid crystal cell is irradiated with light while a voltage is applied between the conductive films of a pair of substrates.
[0104] The PSA type liquid crystal element can be produced by a method including the following steps. A process of applying the liquid crystal aligning agent of the present disclosure onto each conductive film of a pair of substrates having a conductive film to form a coating film. The process of constructing a liquid crystal cell by placing a pair of substrates coated with a liquid crystal alignment agent so that the coating films face each other, sandwiching the liquid crystal layer between them. A process in which light is irradiated onto the liquid crystal cell while a voltage is applied between the conductive films.
[0105] Specifically, a liquid crystal cell is constructed in the same manner as in steps 1 to 3 above, except that a photopolymerizable monomer is injected or dropped together with liquid crystal between a pair of substrates having a conductive film. As the photopolymerizable monomer to be injected or dropped together with liquid crystal, a conventionally known compound can be used. A polyfunctional (meth)acrylic monomer is preferable. (Meth)acrylic means acrylic and methacrylic.
[0106] In the manufacture of a PSA type liquid crystal element, after the liquid crystal cell is constructed, the liquid crystal cell is irradiated with light while a voltage is applied between the conductive films of a pair of substrates. The voltage to be applied can be, for example, 5 to 50 V DC or AC. As the light to be irradiated, for example, ultraviolet light containing light with a wavelength of 150 to 800 nm and visible light can be used. Of these, ultraviolet light containing light with a wavelength of 300 to 400 nm is preferred. As the light source for the irradiation light, for example, a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. can be used. The light irradiation dose is preferably 1,000 to 200,000 J / m 2 and more preferably 1,000 to 100,000 J / m 2 It is.
[0107] For each mode of liquid crystal cell, a polarizing plate is then attached to the outer surface of the liquid crystal cell as necessary to form a liquid crystal element. Examples of the polarizing plate include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, and a polarizing plate made of the H film itself.
[0108] Either positive or negative type liquid crystal may be used. When negative type liquid crystal is used in IPS type and FFS type liquid crystal elements, it is preferable because the transmission loss at the upper part of the electrode can be reduced and the contrast can be improved. Examples of liquid crystal include nematic liquid crystal and smectic liquid crystal, and among them, nematic liquid crystal is preferable.
[0109] The liquid crystal element of the present disclosure can be effectively applied to various applications, specifically, for example, it can be used as various display devices such as clocks, portable game machines, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays, as well as light control devices, retardation films, and the like.
[0110] According to the present disclosure described above, the following means are provided. [Means 1] A liquid crystal aligning agent containing a polymer component, comprising the following (A) polymer: (A) Polymer: A polymer having a structural unit derived from a diamine compound containing a diamine having a partial structure represented by the above formula (1). and a compound (B) as follows: (B) Compound: A compound (excluding polymers) having three or more partial structures (T) in one molecule in which one or more hydrogen atoms bonded to heteroatoms in a nucleophilic functional group or an acidic functional group are replaced with leaving groups that are eliminated by at least one of heat and light. and wherein the content ratio of the structural unit derived from the monomer having the partial structure represented by the above formula (1) in the polymer component is 0.065 mol or more per mol of the total amount of the structural units derived from the monomer in the polymer component. [2] The liquid crystal aligning agent according to [means 1], wherein the nucleophilic functional group has a structure in which a hydrogen atom is bonded to a nitrogen atom, a sulfur atom or an oxygen atom, and the (B) compound has, as the partial structure (T), three or more partial structures in one molecule in which one or more hydrogen atoms bonded to a nitrogen atom, a sulfur atom or an oxygen atom in the nucleophilic functional group are replaced with the leaving group. [Means 3] The liquid crystal aligning agent according to [Means 1] or [Means 2], wherein the compound (B) is a compound represented by the above formula (2). [Means 4] The R 3 is a (k1+k2)-valent group having no aromatic ring. [Means 5] The R 3 is a (k1+k2)-valent chain hydrocarbon group, or -O-, -S-, -CO-, -COO-, -NR 5 -, -CO-NR 5 -, -NR 5 -CO-O-, -NR 5 -CO-NR 6 -, -CO-NR 5 -NR 6 -, a (k1+k2)-valent group containing a nitrogen atom or a non-aromatic heterocycle (where R 5and R 6 are each independently a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms. [Means 6] The liquid crystal aligning agent according to any one of [Means 1] to [Means 5], wherein the acidic functional group is a carboxylic acid group, a phosphoric acid group, a phosphorous acid group or a sulfonic acid group, and the (B) compound has, as the partial structure (T), three or more partial structures in one molecule in which one or more hydrogen atoms bonded to heteroatoms in the acidic functional group are replaced with the leaving group. [Measure 7] The liquid crystal aligning agent according to any one of [Measure 1] to [Measure 6], wherein the compound (B) includes a compound represented by the above formula (3). [Means 8] The liquid crystal aligning agent according to any one of [Means 1] to [Means 7], wherein the (A) polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyurea, polyamideimide, polyorganosiloxane, and addition polymer. [Measure 9] The liquid crystal aligning agent according to any one of [Measure 1] to [Measure 8], further comprising, as the polymer component, a polymer not having the partial structure represented by the above formula (1). [Measure 10] A liquid crystal alignment film formed by using the liquid crystal aligning agent according to any one of [Measure 1] to [Measure 9]. [Means 11] A method for producing a liquid crystal alignment film, comprising applying the liquid crystal aligning agent according to any one of [Means 1] to [Means 9] onto a substrate, and then carrying out a rubbing treatment or a light irradiation treatment to impart liquid crystal aligning ability. [Means 12] A liquid crystal element comprising the liquid crystal alignment film according to [Means 10]. EXAMPLES
[0111] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0112] In the following examples, the solution viscosity and imidization rate of the polymer were measured by the following methods. <Polymer solution viscosity> The solution viscosity of the polymer was measured at 25° C. using an E-type viscometer. <Imidization rate of polyimide> The polyimide solution was poured into pure water, and the resulting precipitate was thoroughly dried under reduced pressure at room temperature. It was then dissolved in deuterated dimethyl sulfoxide and measured at room temperature using tetramethylsilane as a standard substance. 1 H-NMR measurement was performed. 1 The imidization rate [%] was calculated from the H-NMR spectrum using the following formula (1). Imidization rate [%] = (1-(β 1 / (β 2 ×α)))×100 …(1) (In formula (1), β 1 is the peak area due to the proton of the NH group that appears at a chemical shift of around 10 ppm, and β 2 is the peak area due to other protons, and α is the ratio of the number of other protons to one proton of the NH group in the polymer precursor (polyamic acid).
[0113] The abbreviations of the compounds used in the following examples are shown below. For convenience, hereinafter, a "compound represented by formula (X)" may be simply referred to as "compound (X)".
[0114] (Tetracarboxylic dianhydride) TA-1 to TA-6 [ka]
[0115] (Diamine compounds) DA-1 to DA-5, Da-6, Da-7, DB-1 to DB-12 [ka] [ka] [ka]
[0116] (Additives) AD-1 to AD-10 [ka] [ka]
[0117] 1. Synthesis of polyamic acid [Synthesis Example 1] A solution containing 20% by mass of polyamic acid (referred to as polymer (PA-1)) was obtained by dissolving 80 molar parts of compound (TA-2) and 20 molar parts of compound (TA-6) as tetracarboxylic dianhydrides, and 20 molar parts of compound (DA-1) and 80 molar parts of compound (DB-2) as diamine compounds in N-methyl-2-pyrrolidone (NMP) and reacting at 40°C for 24 hours. A small amount of this solution was taken and NMP was added to make a solution with a concentration of 15% by mass. The solution viscosity was measured and was 243 mPa s.
[0118] [Synthesis Examples 2-13] Polymerization was performed in the same manner as in Synthesis Example 1, except that the types and amounts of the tetracarboxylic dianhydride and diamine compound used in the polymerization were changed as shown in Table 1, to obtain solutions containing the polyamic acid polymers (PA-2) to (PA-13). The polymerization was performed with the molar ratio of the diamine compound to the tetracarboxylic dianhydride (diamine compound / tetracarboxylic dianhydride) adjusted to 0.900 to 0.995 so that the viscosity of the NMP solution with a polymer concentration of 15% by mass was 200 to 250 mPa·s. In Table 1, the numerical values of the acid dianhydride represent the ratio (molar parts) of each compound relative to 100 mole parts of the total amount of the tetracarboxylic dianhydride used in the synthesis. The numerical values of the diamine represent the ratio (molar parts) of each compound relative to 100 mole parts of the total amount of the diamine compound used in the synthesis.
[0119] [Table 1]
[0120] 2. Synthesis of Polyimide [Synthesis Example 14] 100 mol parts of compound (TA-1) as a tetracarboxylic dianhydride, and 30 mol parts of compound (DA-6), 40 mol parts of compound (DB-4), and 30 mol parts of compound (DB-3) as diamine compounds were dissolved in N-methyl-2-pyrrolidone (NMP) and reacted at 40°C for 24 hours to obtain a solution containing 20% by mass of polyamic acid. Next, NMP was added to the obtained polyamic acid solution, and pyridine and acetic anhydride were added in amounts of 1.8 molar equivalents each relative to the carboxyl group of the polyamic acid, and a dehydration ring-closing reaction was carried out at 60°C for 4 hours. After the dehydration ring-closing reaction, the solvent in the system was replaced with fresh NMP, and the mixture was further concentrated to obtain a solution containing 20% by mass of polyimide with an imidization rate of 55% (this is referred to as polymer (PI-1)). A small amount of this solution was taken, and NMP was added to make a solution with a concentration of 15% by mass. The solution viscosity was measured and was 395 mPa·s.
[0121] [Synthesis Example 15] Polymerization was carried out in the same manner as in Synthesis Example 14, except that the types and amounts of the tetracarboxylic dianhydride and diamine compound used in the polymerization were changed as shown in Table 2, and the amounts of pyridine and acetic anhydride were changed according to the target imidization rate, to obtain a solution containing a polymer (PI-2) that is a polyimide.
[0122] [Table 2]
[0123] 3. Preparation and evaluation of liquid crystal alignment agent [Example 1: Rubbed FFS type liquid crystal display element] 1. Preparation of Liquid Crystal Alignment Agent A solution containing 70 parts by mass of the polymer (PA-1) obtained in Synthesis Example 1 and a solution containing 30 parts by mass of the polymer (PA-10) obtained in Synthesis Example 10 were mixed, and 10 parts by mass of the compound (AD-4), NMP and butyl cellosolve (BC) were further added to obtain a solution with a solvent composition of NMP / BC=80 / 20 (mass ratio) and a solid concentration of 4.0 mass%. The solution was filtered through a filter with a pore size of 0.2 μm to prepare a liquid crystal alignment agent (AL-1).
[0124] Based on the blending amount of the polymer component, the ratio (specific N-containing structure ratio) of the structural unit derived from the diamine having the partial structure (AN) (specific diamine) to 1 mole of the structural unit derived from the diamine compound contained in the polymer component contained in the liquid crystal alignment agent (AL-1) was calculated to be 0.14 moles. The calculation formula is as follows: Specific N content structure ratio=20×0.7 / 100=0.14
[0125] 2. Fabrication of FFS-type LCD elements using the rubbing method A glass substrate (first substrate) having a flat electrode (bottom electrode), an insulating layer, and a comb-shaped electrode (top electrode) laminated in this order on one side thereof, and a glass substrate (second substrate) having no electrode were prepared. Next, a liquid crystal alignment agent (AL-1) was applied to the electrode-formed surface of the first substrate and one side of the second substrate, respectively, using a spinner, and heated (pre-baked) on a hot plate at 110°C for 3 minutes. Then, the substrate was dried (post-baked) for 30 minutes in an oven at 230°C, the inside of which was replaced with nitrogen, to form a coating film with an average thickness of 0.08 μm. Next, the coating film surface was subjected to rubbing treatment using a rubbing machine having a roll wrapped with rayon cloth, with a roll rotation speed of 1,000 rpm, a stage movement speed of 3 cm / sec, and a pile indentation length of 0.3 mm. Then, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then drying was performed in a clean oven at 100°C for 10 minutes to obtain a pair of substrates having a liquid crystal alignment film. Next, a pair of substrates having a liquid crystal alignment film was screen-printed with an epoxy resin adhesive containing aluminum oxide spheres having a diameter of 3.5 μm, leaving a liquid crystal injection port at the edge of the surface on which the liquid crystal alignment film was formed. The substrates were then superimposed and pressed together, and the adhesive was thermally cured at 150°C for 1 hour. Next, a negative liquid crystal (MLC-6608, manufactured by Merck) was filled into the gap between the pair of substrates through the liquid crystal injection port, and the liquid crystal injection port was then sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, the substrate was heated at 120°C and then slowly cooled to room temperature to produce a liquid crystal cell. Note that when the pair of substrates were superimposed, the rubbing methods of the respective substrates were set to be antiparallel. Next, polarizing plates were attached to both outer surfaces of the substrates in the liquid crystal cell to obtain an FFS-type liquid crystal display element.
[0126] 3. Evaluation (1) Evaluation of liquid crystal alignment (evaluation by retardation change rate) The FFS type liquid crystal display element manufactured by the rubbing method in 2. above was subjected to a 27,000 cd / m 2 The FFS-type liquid crystal display element was left standing for 500 hours on a high-brightness backlight, and the liquid crystal alignment was evaluated by the retardation change rate before and after backlight irradiation. First, the retardation of the FFS-type liquid crystal display element manufactured in 2 above was measured using Axoscan manufactured by Optoscience, and the retardation change rate α before and after backlight irradiation was calculated using the following formula (F1). The smaller the change rate α, the less likely the liquid crystal alignment to deteriorate due to backlight irradiation, and the better the liquid crystal alignment. A change rate α of less than 0.5% was judged as "excellent (◎)", 0.5% to less than 1% was judged as "good (○)", 1% to 2% was judged as "fair (△)", and more than 2% was judged as "poor (×)". α=Δθ / θ1 …(F1) (In formula (F1), Δθ represents the retardation difference before and after irradiation, and θ1 represents the retardation value before irradiation.) As a result, the liquid crystal alignment property of this example was evaluated as "excellent (A)".
[0127] (2) Evaluation of electrical characteristics by voltage holding ratio (VHR) For the FFS type liquid crystal display element manufactured by the rubbing method in 2 above, a voltage of 5V was applied for 60 microseconds over a span of 167 milliseconds, and then the voltage holding ratio (hereinafter also referred to as "initial VHR") 167 milliseconds after the application was removed was measured. A VHR-1 manufactured by Toyo Corporation was used as the measuring device. At this time, a voltage holding ratio of more than 85% was judged as "excellent (◎)", more than 75% and less than 85% was judged as "good (○)", 60% or more and less than 75% was judged as "fair (△)", and less than 60% was judged as "poor (×)". As a result, in this example, the initial VHR was rated as "good (○)".
[0128] (3) Evaluation of VHR reliability The FFS type liquid crystal display element manufactured by the rubbing method in 2. above was irradiated with CCFL (backlight) at 60°C for one week after the initial VHR was measured in (2) above, and then left to cool naturally to room temperature. After cooling, a voltage of 5V was applied to the liquid crystal cell for 60 microseconds with a span of 167 milliseconds, and the voltage retention rate (hereinafter also referred to as "post-irradiation VHR") 167 milliseconds after the application was removed was measured. The change rate of VHR at this time (ΔVHR) was calculated from the difference between the initial VHR and the post-irradiation VHR (ΔVHR = initial VHR - post-irradiation VHR), and the VHR reliability was evaluated based on ΔVHR. When ΔVHR was less than 5%, it was judged as "excellent (◎)", when it was 5% or more and less than 10%, it was judged as "good (○)", when it was 10% or more and less than 15%, it was judged as "fair (△)", and when it was 15% or more, it was judged as "poor (×)". As a result, the VHR reliability in this example was "fair (Δ)."
[0129] (4) Evaluation of membrane strength The liquid crystal alignment agent (AL-1) prepared in 1 above was filtered through a 1.0 μm filter, and then applied to the second substrate by spin coating. Then, it was heated (pre-baked) for 1 minute on a hot plate at 80° C. Then, it was dried (post-baked) for 30 minutes in an oven at 230° C. with the inside of the oven replaced with nitrogen, forming a coating film with an average thickness of 0.1 μm, and the haze value of the coating film was measured using a haze meter. Next, this coating film was subjected to rubbing treatment five times using a rubbing machine having a roll wrapped with cotton cloth at a roll rotation speed of 1000 rpm, a stage moving speed of 3 cm / sec, and a pile pressing length of 0.3 mm. Then, the haze value of the liquid crystal alignment film was measured using a haze meter, and the difference from the haze value before the rubbing treatment (haze change value) was calculated. When the haze value of the film before the rubbing treatment is Hz1 (%) and the haze value of the film after the rubbing treatment is Hz2 (%), the haze change value is expressed by the following formula (F2). Haze change value (%) = Hz2 - Hz1 ... (F2) A haze change value in the liquid crystal alignment film of less than 0.5% was evaluated as "excellent (◎)", a value between 0.5% and 0.8% was evaluated as "good (○)", a value between 0.8% and 1.0% was evaluated as "fair (△)", and a value of 1.0% or more was evaluated as "poor (×)". If the haze change value is less than 1.0%, the film strength is sufficiently high and the rubbing resistance is high, that is, the mechanical properties of the film are good. As a result, in this example, the film strength was evaluated as "good (○)".
[0130] (5) Evaluation of DC image retention characteristics The FFS type liquid crystal display element manufactured by the rubbing method in 2. above was driven at AC2.5V to set the luminance difference between any two pixels to 0, and then DC1V was applied to only one of the pixels for 20 minutes while driving at AC2.5V to accumulate electric charge. When the application of DC1V was stopped and the driving was returned to AC2.5V only, a luminance difference occurred between the two pixels due to the accumulated electric charge. By observing the change in this luminance difference over time, the relaxation time during the process of the residual DC value attenuation was calculated. When the relaxation time was less than 10 seconds, it was judged as "excellent (◎)", when the relaxation time was 10 seconds or more but less than 20 seconds, it was judged as "good (○)", when the relaxation time was 20 seconds or more but less than 30 seconds, it was judged as "fair (△)", and when the relaxation time was 30 seconds or more, it was judged as "poor (×)". As a result, in this example, it was rated as "excellent (◎)".
[0131] [Examples 2 to 9 and Comparative Examples 1, 2, 4 to 6] A liquid crystal alignment agent was prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, using the obtained liquid crystal alignment agent, an FFS-type liquid crystal display element was manufactured by a rubbing method in the same manner as in Example 1, and the liquid crystal alignment property, initial VHR, VHR reliability, film strength and DC image retention characteristics were evaluated. The results are shown in Table 3. In Table 3, the numerical values in the columns of polymer components (polymer 1 and polymer 2) and additives represent the blending ratio (parts by mass) of each compound in terms of solid content relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal alignment agent. In addition, the specific N-containing structure ratio is also shown in Table 4. [Comparative Example 3] A liquid crystal alignment agent (AR-3) was prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. However, the obtained liquid crystal alignment agent (AR-3) gelled, so no further evaluation was performed.
[0132] [Table 3]
[0133] [Example 10: Optical FFS type liquid crystal display element] 1. Preparation of Liquid Crystal Alignment Agent A solution containing 60 parts by mass of the polymer (PA-5) obtained in Synthesis Example 5 and a solution containing 40 parts by mass of the polymer (PA-13) obtained in Synthesis Example 13 were mixed, and 8 parts by mass of the compound (AD-4), NMP and BC were further added to obtain a solution with a solvent composition of NMP / BC=80 / 20 (mass ratio) and a solid content concentration of 3.5% by mass. The liquid crystal alignment agent (AL-10) was prepared by filtering this solution through a filter with a pore size of 0.2 μm. The specific N-containing structure ratio of the liquid crystal alignment agent (AL-10) was calculated to be 0.48.
[0134] 2. Fabrication of FFS-type LCD elements using the photoalignment method A first substrate and a second substrate were prepared similarly to those in Example 1. Next, a liquid crystal alignment agent (AL-10) was applied to the electrode-forming surface of the first substrate and one of the substrate surfaces of the second substrate using a spinner, and heated (pre-baked) on a hot plate at 80°C for 1 minute. Thereafter, the substrate was dried (post-baked) for 30 minutes in an oven at 230°C with the interior replaced with nitrogen, forming a coating film with an average thickness of 0.1 μm. The obtained coating film was irradiated with 1,000 J / m2 of linearly polarized ultraviolet light including a 254 nm emission line using an Hg-Xe lamp. 2 The coating film was irradiated with light from the normal direction of the substrate to perform a photo-alignment treatment. The amount of irradiation was measured using an actinometer that measures at a wavelength of 254 nm. Next, the coating film that had been subjected to the photo-alignment treatment was heated in a clean oven at 230°C for 30 minutes to perform a heat treatment, thereby forming a liquid crystal alignment film. Next, for one of the pair of substrates on which the liquid crystal alignment film was formed, an epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was applied by screen printing to the outer edge of the surface having the liquid crystal alignment film. Then, the substrates were overlapped and pressed together so that the projection direction of the polarization axis on the substrate surface during light irradiation was antiparallel, and the adhesive was thermally cured at 150°C for 1 hour. Next, negative liquid crystal (MLC-6608, manufactured by Merck) was filled between the pair of substrates through the liquid crystal injection port, and the liquid crystal injection port was sealed with an epoxy adhesive to obtain a liquid crystal cell. Furthermore, in order to remove the flow alignment during liquid crystal injection, the liquid crystal cell was heated at 120°C and then slowly cooled to room temperature. Then, polarizing plates were attached to both outer surfaces of the substrate in the liquid crystal cell to obtain a liquid crystal display element. In addition, the above series of operations was performed with a UV irradiation dose of 100 to 10,000 J / m after post-baking. 2 Three or more liquid crystal display elements with different amounts of ultraviolet light irradiation were manufactured by changing the exposure amount within the range of 1, and the liquid crystal display element with the exposure amount (optimum exposure amount) that showed the best alignment characteristics was used for the following evaluation.
[0135] 3. Evaluation The liquid crystal display element manufactured in the above 2 was evaluated for liquid crystal alignment, initial VHR, VHR reliability, and DC image retention characteristics in the same manner as in Example 1. In addition, the liquid crystal alignment agent (AL-10) prepared in the above 1 was used to evaluate the film strength in the same manner as in Example 1. The results are shown in Table 4.
[0136] [Examples 11 to 13 and Comparative Example 7] A liquid crystal alignment agent was prepared in the same manner as in Example 10, except that the composition of the liquid crystal alignment agent was changed as shown in Table 4. Using the obtained liquid crystal alignment agent, an FFS-type liquid crystal display element was manufactured by a photoalignment method in the same manner as in Example 10, and the liquid crystal alignment property, initial VHR, VHR reliability, film strength and DC image retention characteristics were evaluated. The results are shown in Table 4. In Table 4, the numerical values in the columns for polymer components (polymer 1 and polymer 2) and additives represent the blending ratio (parts by mass) of each compound in terms of solid content relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal alignment agent. Table 4 also shows the specific N-containing structure ratio.
[0137] [Table 4]
[0138] As shown in Tables 3 and 4, in Examples 1 to 13, which used a liquid crystal alignment agent containing a polymer having a partial structure (AN) and an additive having 3 or more partial structures (T) in one molecule and a specific N-containing structure ratio of 0.13 or more, the evaluation results of liquid crystal alignment, initial VHR, VHR reliability, film strength and DC image retention were excellent (◎), good (○) or fair (△), and various characteristics were improved in a well-balanced manner. In contrast, among Comparative Example 1, which used a liquid crystal alignment agent that did not contain a polymer having a partial structure (AN), and Comparative Examples 2 to 6, which used a liquid crystal alignment agent that did not contain an additive having 3 or more partial structures (T) in one molecule, Comparative Examples 2, 4, 5, and 7 had one or more poor (×) in the evaluation results of initial VHR, film strength and DC image retention, and Comparative Example 3 had gelled the liquid crystal alignment agent. In addition, Comparative Example 6, which had a specific N-containing structure ratio of 0.12, had poor (×) VHR reliability and DC image retention.
[0139] From the above results, it has become clear that a liquid crystal alignment agent containing a polymer having a partial structure (AN) and an additive having three or more partial structures (T) in one molecule, and containing a predetermined amount or more of structural units derived from a diamine having the partial structure (AN) relative to the structural units derived from a diamine compound in the polymer component, can provide a liquid crystal alignment film excellent in liquid crystal alignment properties, voltage retention characteristics, VHR reliability and film strength, and can provide a liquid crystal element in which the afterimage caused by accumulated charge is sufficiently reduced.
Claims
1. The following polymer (A): (A) Polymer: A polymer having a structural unit derived from a diamine compound containing a diamine having a partial structure represented by the following formula (1): and a polymer component comprising the following (B) compound: (B) Compound: A compound (excluding polymers) having three or more partial structures (T) in one molecule in which one or more hydrogen atoms bonded to a heteroatom in a nucleophilic functional group or an acidic functional group are replaced with a leaving group that is eliminated by at least one of heat and light. and A liquid crystal aligning agent, wherein the content ratio of a structural unit derived from a diamine having a partial structure represented by the following formula (1) in the polymer component is 0.13 mol or more per 1 mol of the total amount of structural units derived from diamine compounds in the polymer component: [Formula 1] (In formula (1), Ar 1 is a divalent aromatic ring group. 2 and R 1 is Ar 2 is a divalent aromatic ring group, R 1 is a hydrogen atom or a monovalent organic group, or Ar 2 and R 1 are combined together to form Ar 2 and R 1 represents a nitrogen-containing aromatic condensed ring structure formed together with the nitrogen atom to which it is bonded. "*" represents a bond.)
2. the nucleophilic functional group has a structure in which a hydrogen atom is bonded to a nitrogen atom, a sulfur atom, or an oxygen atom, The (B) compound has, as the partial structure (T), three or more partial structures in one molecule in which one or more hydrogen atoms bonded to a nitrogen atom, a sulfur atom, or an oxygen atom in the nucleophilic functional group are replaced with the leaving group. The liquid crystal aligning agent according to claim 1.
3. The liquid crystal aligning agent according to claim 1 , wherein the compound (B) is a compound represented by the following formula (2): [Case 2] (In formula (2), X 1 and X 5 are each independently a nitrogen atom, a sulfur atom, an oxygen atom, or a group represented by the following formula (x-1): 1 is the leaving group. 2a and R 2b are each independently a hydrogen atom or a monovalent organic group. 3 is an organic group having a valence of (k1+k2). k1 is X 1 is an integer of 3 or more when it is a sulfur atom or an oxygen atom, 1 is an integer of 2 or more when k1 is a nitrogen atom or a group represented by the following formula (x-1). However, when k1=2, R 3 has one or more of the above-mentioned leaving groups bonded to a nitrogen atom. 1 is a sulfur atom or an oxygen atom, m=1 and n1=0, 1 is a nitrogen atom or a group represented by the following formula (x-1), m is 1 or 2 and (m+n1)=2 is satisfied. k2 is an integer of 0 to 2. n2 is X 5 is a sulfur atom or an oxygen atom, then it is 1; 5 is a nitrogen atom or a group represented by the following formula (x-1), the value is 2. 1 are the same or different. 1 If there are multiple Y 1 are the same or different, and in the formula, R 2a When there are multiple R 2a are the same or different. 5 If there are multiple Xs, 5 are the same or different. 2b When there are multiple R 2b are the same or different.) [C3] (In formula (x-1), R 4 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. "*" represents a bond. However, when the carbonyl group in formula (x-1) is R 3 is bonded to.)
4. The R 3 The liquid crystal aligning agent according to claim 3 , wherein is a (k1+k2)-valent group having no aromatic ring.
5. The R 3 is a (k1+k2)-valent chain hydrocarbon group, or —O—, —S—, —CO—, —COO—, —NR— is present between the carbon-carbon bonds of the chain hydrocarbon group. 5 --CO-NR 5 --, --NR 5 -CO-O-, -NR 5 -CO-NR 6 --CO-NR 5 -NR 6 -, a (k1+k2)-valent group containing a nitrogen atom or a non-aromatic heterocycle (wherein R 5 and R 6 are each independently a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms.
6. the acidic functional group is a carboxylic acid group, a phosphoric acid group, a phosphorous acid group, or a sulfonic acid group; The (B) compound has, as the partial structure (T), three or more partial structures in which one or more hydrogen atoms bonded to a heteroatom in the acidic functional group are replaced with the leaving group in one molecule. The liquid crystal aligning agent according to claim 1.
7. The liquid crystal aligning agent according to claim 1 , wherein the compound (B) comprises a compound represented by the following formula (3): [C4] (In formula (3), X 4 is a carboxylic acid group, a phosphoric acid group, a phosphorous acid group, or a sulfonic acid group. 5 is a protected carboxylic acid group, a protected phosphate group, a protected phosphite group, or a protected sulfonic acid group. 7 is an organic group having a valence of (i+j). i is an integer of 0 to 2. j is an integer of 3 or more. When i is 2, a plurality of X 4 are the same or different. 5 are the same or different.)
8. The liquid crystal aligning agent according to claim 1, wherein the polymer (A) is at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyurea, and polyamideimide.
9. The liquid crystal aligning agent according to claim 1 , further comprising, as the polymer component, a polymer not having the partial structure represented by the formula (1).
10. A liquid crystal alignment film formed by using the liquid crystal aligning agent according to any one of claims 1 to 9.
11. A method for producing a liquid crystal alignment film, comprising applying the liquid crystal aligning agent according to any one of claims 1 to 9 onto a substrate, and then subjecting the applied liquid crystal aligning agent to a rubbing treatment or a light irradiation treatment to impart liquid crystal aligning ability.
12. A liquid crystal element comprising the liquid crystal alignment film according to claim 10.
Citation Information
Patent Citations
Vertical alignment type liquid crystal aligning agent and liquid crystal display element
JP2008299318A
Cited By
Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element
WO2026211586A1