Separator and electrochemical device including that separator
The innovative separator design with an inorganic particle layer and adhesive layer of organic particles with protrusions and valleys addresses adhesion and air permeability issues in ceramic coated separators, improving battery stability and performance.
Patent Information
- Application Number
- JP2024044005
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional ceramic coated separators (CCS) lack sufficient adhesion to electrodes, leading to misalignment and potential short circuits, fire hazards, and reduced battery performance due to poor air permeability and thickness deviations during cell assembly.
A separator design featuring a porous substrate with an inorganic particle layer and an adhesive layer composed of organic particles with protrusions and valleys, ensuring strong electrode adhesion, anti-blocking properties, and maintained air permeability, even at a small thickness.
The separator achieves excellent electrode adhesion, prevents blocking, and maintains air permeability, enhancing battery stability and performance by ensuring secure electrode alignment and reducing the risk of short circuits.
Smart Images

Figure 2024134548000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a separator and an electrochemical device including the separator. Specifically, the present disclosure relates to a separator having excellent electrode adhesion, anti-blocking properties, and air permeability, and an electrochemical device including the separator. [Background technology]
[0002] To solve the high-temperature stability problem of the separator, a ceramic coated separator (CCS) has been used, in which a porous inorganic particle layer is formed on one or both sides of a porous substrate. The ceramic coated separator has low thermal shrinkage rate at high temperatures and excellent heat resistance, so it is applied to large battery systems for EVs.
[0003] However, conventional ceramic-coated separators have poor adhesion to electrodes, and the separator and electrode often separate during the cell assembly process, causing warping and deformation of the electrode assembly. In other words, when the adhesion between the ceramic coating layer of the separator and the electrode is poor as described above, misalignment between the electrodes and the separator occurs within the jelly roll during cell stacking. When a stack cell battery with misalignment as described above is operated, local resistance occurs due to the misalignment, and short circuits occur between the electrodes due to physical damage caused by continuous use, resulting in safety issues such as fire.
[0004] Therefore, improving the adhesion between the ceramic-coated separator and the electrodes is an issue that must be improved for the stability of the battery.
[0005] One method for improving the adhesion between the separator and the electrode is to form an adhesive organic layer on the inorganic particle layer of the ceramic-coated separator, but the organic layer reduces air permeability, making it difficult to form a thin film, and still results in poor electrode adhesion. In addition, a blocking phenomenon occurs in which the adhesive organic layer is detached when the separator is wound up. Therefore, there are still problems to be solved, such as a decrease in the ion conductivity of the separator and / or a thickness deviation occurs during alignment of the electrode assembly, which inhibits battery performance. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Registration No. 4414165 (Publication date: 2005.03.03) Summary of the Invention [Problem to be solved by the invention]
[0007] In order to solve the above problems, one aspect of the present disclosure aims to provide a separator that has excellent electrode adhesion, anti-blocking properties, and air permeability even when it is thin, and an electrochemical device including the separator.
[0008] In one embodiment, a separator can be provided in which the thickness of the adhesive layer is 2 μm or less and the overall thickness of the separator is 20 μm or less, or 15 μm or less, and the object is to provide a separator that has excellent electrode adhesion, anti-blocking properties, and air permeability even within the above range, and an electrochemical element including the separator. [Means for solving the problem]
[0009] As one means for achieving the above-mentioned object, the present disclosure provides a separator including a porous substrate, an inorganic particle layer disposed on at least one surface of the porous substrate, in which inorganic particles are connected to each other to form pores between the inorganic particles, and an adhesive layer disposed on the inorganic particle layer, in which organic particles having a plurality of protrusion parts and a plurality of valley parts are connected to each other to form pores.
[0010] In one embodiment, the ratio of the average particle size (D50) of the organic particles to the average particle size (D50) of the inorganic particles may be 0.5 to 3.
[0011] In one embodiment, the organic particles may have a D50 of 0.1 μm to 2 μm.
[0012] In one embodiment, the organic particles may have a particle size distribution in which the D10 / D90 value is 0.3 to 0.9.
[0013] In one embodiment, the organic particles may have a glass transition temperature (Tg) of 50 to 90°C.
[0014] In one embodiment, the adhesive layer may have a thickness of more than 0 μm and not more than 2 μm.
[0015] In one embodiment, the organic particles may be secondary particles in which primary particles are aggregated together through surface melting to form a plurality of protrusion parts and a plurality of valley parts, or may be primary particles having a plurality of protrusion parts and a plurality of valley parts on the surface.
[0016] In one embodiment, the adhesive layer may contain 70% by weight or more of organic particles based on the weight of the entire adhesive layer.
[0017] In one embodiment, the adhesive layer contains the organic particles in an amount of 0.2 to 2.0 g / m 2 It may be included in.
[0018] In one embodiment, the separator may be laminated on a 200 μm thick carbon sheet (TOYO Tanso Korea, PF-20HP) with the adhesive layer of the separator facing each other, and then pressed and bonded in a heat press at 80° C. and 20 MPa for 30 seconds, and the electrode adhesive strength measured by peeling at 180° using an INSTRON UTM device based on ASTM D903 may be 1.5 gf / 15 mm to 4.0 gf / 15 mm.
[0019] In one embodiment, the separator may have an air permeability change ΔG of 50 seconds / 100 cc or less, as measured by the following formula:
[0020] ΔG=G1-G2
[0021] In the above formula, G1 is the gully permeability of the separator in which an inorganic particle layer and an adhesive layer are laminated in sequence on both sides of the porous substrate, and G2 is the gully permeability of the porous substrate itself. The gully permeability was measured according to the ASTM D726 standard using a Densometer manufactured by Toyoseiki Co., Ltd., and the unit is seconds / 100cc.
[0022] In one embodiment, when two separators are arranged with the adhesive layers facing each other, and then pressed together at a temperature of 60° C. and a pressure of 7.5 MPa for 1 hour, and then peeled at 180 degrees in accordance with ASTM D903, the adhesive layers do not adhere to each other and are partially or entirely peeled off, but rather the adhesive layers are separated as they are and blocking does not occur.
[0023] As another means for achieving the above object, according to one aspect of the present disclosure, there is provided an electrochemical element including the separator of the above embodiment. Effect of the Invention
[0024] The separator of the present disclosure can have excellent electrode adhesion, anti-blocking properties, and breathability even at a small thickness.
[0025] In one embodiment, the separator is laminated on a carbon sheet having a thickness of 200 μm so that the adhesive layer of the separator faces each other, and then pressed and bonded by a hot press at 80° C. and 20 MPa for 30 seconds, and then peeled at 180° using a UTM device according to ASTM D903. The electrode adhesive strength measured may be 1.5 gf / 15 mm or more, 2.0 gf / 15 mm or more, 2.3 gf / 15 mm or more, 2.5 gf / 15 mm or more, or 3.0 gf / 15 mm or more. For example, it may be 1.5 gf / 15 mm to 4.0 gf / 15 mm. According to the embodiment, sufficient electrode adhesiveness can be ensured even when a relatively small amount of organic particles having a secondary particle shape in which the surface of a primary particle of a polymer having a high glass transition temperature is melted and aggregated are included.
[0026] The separator of one embodiment can ensure excellent electrode adhesion even with a thin thickness and can also have excellent anti-blocking properties. For example, two separators each having a porous substrate, an inorganic particle layer, and an adhesive layer are laminated so that the adhesive layers face each other, and then pressed together at a temperature of 60°C and a pressure of 7.5 MPa for 1 hour. When the bonded portions are then peeled off and it is confirmed by SEM whether the adhesive layer has peeled off partially or entirely to cause blocking between the separator surfaces, the adhesive layer can have excellent blocking prevention properties without blocking, which is a phenomenon in which the adhesive layer is partially peeled off from each other separator.
[0027] In one embodiment, the separator can have excellent breathability even when it has a multi-layer structure, for example, by disposing an adhesive layer on an inorganic particle layer, and the change in air permeability (ΔG) expressed by the following formula may be 50 sec / 100 cc or less, 40 sec / 100 cc or less, 35 sec / 100 cc or less, or 30 sec / 100 cc or less.
[0028] ΔG=G1-G2
[0029] In the above formula, G1 is the gully permeability of a separator in which an inorganic particle layer and an adhesive layer are laminated in sequence on both sides of a porous substrate, and G2 is the gully permeability of the porous substrate itself. The gully permeability is measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D726 standard, and the unit is seconds / 100cc. In addition, the above-mentioned change in air permeability can be satisfied even in the case of a separator in which an inorganic particle layer and an adhesive layer are laminated in sequence on one side of the porous substrate.
[0030] The separator of the one embodiment may be excellent in two or more of electrode adhesion, anti-blocking property, and air permeability, and more preferably, may be excellent in all of electrode adhesion, anti-blocking property, and air permeability. [Brief description of the drawings]
[0031] [Figure 1] 1 is a photograph showing the morphology of organic particles according to one embodiment of the present invention, observed by SEM. [Diagram 2] FIG. 2 illustrates the morphology of organic particles according to one embodiment of the present invention. [Diagram 3] 1 is a photograph of an adhesive layer of a separator in Example 1 observed by SEM. [Figure 4] 1 is a photograph of an adhesive layer of a separator in Comparative Example 1 observed by SEM. [Diagram 5] 1 is a photograph of an adhesive layer of a separator in Comparative Example 2 observed by SEM. [Figure 6] 1 is a photograph of an adhesive layer of a separator in Comparative Example 3 observed by SEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The present disclosure will be described in more detail below through aspects and examples. However, the following aspects of the present invention are merely a reference for explaining the present disclosure, and the present disclosure is not limited thereto, and may be implemented in a variety of forms.
[0033] Additionally, as used in the specification and the appended claims, the singular forms "a," "an," and "the" can be intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0034] Also, when a part is said to "comprise" a certain component, this does not mean to exclude other components, but rather that it can further include other components, unless specifically stated to the contrary.
[0035] In the present disclosure, the organic particles (100) may be polymer particles, and may have a plurality of protrusion parts (10) and a plurality of valley parts (20) formed thereon, as shown in FIG. 1 and FIG. 2. As an example, the organic particles may be aggregates, i.e., secondary particles, in which a plurality of polymerized primary particles are aggregated together by surface melting. The plurality of protrusion parts (10) and the plurality of valley parts (20) may be formed by aggregation of the primary particles. The binder particles in the form of secondary particles may refer to a particle form having a plurality of protrusion parts corresponding to a portion of the primary particles, and having valleys or shrink cavities formed between the protruding protrusion parts. For example, the secondary particles may refer to a form including a plurality of protruding protrusion parts in the form of primary particles having 3 or more, 4 or more, 5 or more, 5 or more, 6 or more, or 8 or more protruding protrusion parts in the form of primary particles on the surface of the organic particles, and a plurality of valley parts or sink parts formed between the protrusion parts.
[0036] Or, it may be a primary particle with multiple peaks and multiple valleys on its surface.
[0037] The protrusions and valleys of the organic particles may be irregular in size and shape. The term "irregular" means not substantially linear, not substantially uniform, or not substantially symmetrical. The term "protrusion" refers to a protruding portion on the surface of a particle, and is shown at 10 in Figures 1 and 2. The term "valley or depression" refers to a concavity on the surface of a particle, and is formed by the height difference between the multiple protrusions formed radially from the center of the organic particle, or a concavity formed between the protrusions, and is shown at 20 in Figures 1 and 2.
[0038] In the present disclosure, "Dn" (n is a real number) refers to the diameter of a particle corresponding to n% of the volume-based cumulative fraction. For example, "D50" refers to the diameter of a particle corresponding to 50% of the volume-based cumulative fraction. "D90" refers to the diameter of a particle corresponding to 90% of the volume-based cumulative fraction. "D10" refers to the diameter of a particle corresponding to 10% of the volume-based cumulative fraction. The Dn can be derived from the particle size distribution results obtained by collecting a sample of the particles to be measured according to the ISO 13320-1 standard and analyzing it using a particle size analyzer, Microtrac's S3500.
[0039] In one embodiment, the separator of the present disclosure can be a separator including: a porous substrate; an inorganic particle layer disposed on at least one surface of the porous substrate, in which inorganic particles are connected to each other to form pores between the inorganic particles; and an adhesive layer disposed on the inorganic particle layer, in which organic particles having a plurality of protrusion parts and a plurality of valley parts are connected to each other to form pores.
[0040] Each component of the separator will be described in detail below.
[0041] In one embodiment, the porous substrate may be a polyolefin-based porous substrate such as polyethylene or polypropylene, but is not particularly limited thereto, and any porous substrate known as a porous substrate for a separator of an electrochemical element may be used. In one embodiment, the porous substrate may be manufactured as a film or sheet, but is not particularly limited thereto. As an example, the porous substrate may include a polyolefin such as polyethylene or polypropylene, and a multilayer film of two or more layers may be used.
[0042] In one embodiment, the thickness of the porous substrate may be, for example, 1 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, or 6 μm or more. The upper limit is not limited, but may be, for example, 100 μm or less, 50 μm or less, 30 μm or less, 20 μm or less, 15 μm or less, 12 μm or less, or a value between the above numerical values, and may be, for example, 1 to 100 μm, or 3 to 50 μm, 5 to 20 μm, or 5 to 15 μm for realizing a high-capacity battery.
[0043] In one embodiment, the inorganic particle layer may include inorganic particles and an organic binder that connects the inorganic particles to each other, and may be a porous inorganic particle layer in which the inorganic particles are connected and fixed by the organic binder to form pores between the inorganic particles. In one embodiment, the inorganic particle layer may be disposed on one or both sides of the porous substrate, and may be applied with an area fraction of 60% or more, 70% or more, 80% or more, or 90% or more, preferably 100%, based on the entire surface of the porous substrate, except for some defects.
[0044] In one embodiment, the inorganic particle layer can be disposed on one or both sides of the porous substrate. When the inorganic particle layer is disposed on both sides of the porous substrate, the thicknesses of the inorganic particle layers disposed on one side and the other side may be the same or different from each other.
[0045] In one embodiment, the thickness of the inorganic particle layer disposed on one surface of the porous substrate may be more than 0 μm, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, 0.4 μm or more, or 0.5 μm or more, and may be 5 μm or less, 4 μm or less, 3 μm or less, 2 μm or less, or a value between the above values. Specifically, the thickness may be more than 0 μm and 5 μm or less, 0.1 to 5 μm, 0.2 to 3 μm, or 0.5 to 2 μm, but is not limited thereto.
[0046] In one embodiment, the inorganic particles are added to improve the heat resistance of the separator, and the type is not particularly limited. According to a non-limiting example, the inorganic particles may include one or more of metal hydroxides, metal oxides, metal nitrides, and metal carbides. Specific examples include, but are not limited to, any one or more selected from the group consisting of SiO2, SiC, MgO, Y2O3, Al2O3, CeO2, CaO, ZnO, SrTiO3, ZrO2, TiO2, and AlO(OH). In order to improve the stability of the battery, the inorganic particles are more preferably metal hydroxide particles such as boehmite, pseudo-boehmite, aluminum hydroxide, and magnesium hydroxide, but are not limited thereto.
[0047] In one embodiment, when boehmite is used as the inorganic particles, the specific surface area (BET) of the boehmite is 10 m 2 / g or more or 15m 2 / g or more, but is not particularly limited thereto.
[0048] In one embodiment, the D50 of the inorganic particles may be greater than 0 μm, greater than 0.05 μm, greater than 0.1 μm, less than 5 μm, less than 3 μm, less than 2 μm, less than 1 μm, less than 0.5 μm, or a value between the above values. For example, it may be greater than 0 μm and less than 5 μm, or greater than 0 μm and less than 3 μm, greater than 0.05 μm and less than 2 μm, greater than 0.1 μm and less than 1 μm, or greater than 0.1 μm and less than 0.5 μm.
[0049] In one embodiment, the organic binder of the inorganic particle layer is not limited in type as long as it can connect and fix inorganic particles to form a porous inorganic particle layer in which inorganic particles are connected to each other and spaces are formed between the inorganic particles. As an example, the organic binder may be in a particulate form or a non-particulate form, and if in a particulate form, it may be a particle form that is different from the organic particles having a plurality of protrusion parts and a plurality of valley parts. In addition, the organic binder may be a water-based latex.
[0050] Examples of the organic binder include, but are not limited to, acrylic polymers such as polymethylmethacrylate, polybutylacrylate, and polyacrylonitrile; (3-aminopropyl)triethoxysilane, (3-aminopropyl)trimethoxysilane, (3-glycidyloxypropyl)trimethoxysilane, and oligomers thereof or silane compounds produced therefrom; styrene butadiene rubber; carboxylmethylcellulose (CMC); and polyvinylidene fluoride. The polyvinyl fluoride (PVdF), polyvinylpyrolidone (PVP), and polyvinylaccetate (PVAc), and the like may be included, but are not limited to these.
[0051] The content of the organic binder may be, but is not limited to, 0.1 to 30 parts by weight, 0.2 to 10 parts by weight, or 0.2 to 5 parts by weight relative to 100 parts by weight of the inorganic particles.
[0052] The inorganic particle layer may be prepared by a conventional method for disposing an inorganic particle layer on a porous substrate, and is not particularly limited. As a non-limiting example, a slurry of water or an organic solution containing the inorganic particles and an organic binder may be prepared, and then the slurry may be applied to one or both sides of the porous substrate by any one or a combination of slot die coating, roll coating, spin coating, dip coating, bar coating, die coating, slit coating, and inkjet printing to form an inorganic particle layer on the porous substrate.
[0053] Next, the adhesive layer of this embodiment and the organic particles that form the adhesive layer will be described in detail.
[0054] The adhesive layer in the present disclosure is a porous layer formed by applying a composition containing organic particles of the embodiment shown in Figures 1 and 2, and by containing organic particles of the specific form, the adhesive layer has excellent adhesion to the electrode while being a thin film, specifically a thickness of 20 μm or less, and the increase in permeability after the adhesive layer is formed is small compared to the permeability of the porous substrate itself, blocking does not occur, and problems that occur during battery assembly can be solved. In addition, a separator with better adhesion to the electrode can be provided compared to using general spherical organic particles.
[0055] The organic particles may be secondary particles formed by agglomeration of primary particles due to surface melting, or may be single particles having a plurality of protruding protrusions and a plurality of depressions or valleys between the protrusions.
[0056] The organic particles are not particularly limited, and may be, for example, "organic particles in the form of secondary particles" having a D50 particle size of 0.1 to 1.5 μm, 0.2 to 1.5 μm, or 0.3 to 1 μm. A typical form of the binder particles in the form of secondary particles may refer to a particle form in which a plurality of polymerized primary particles are fused to each other, for example, fused at the surface, and aggregated, as shown in FIG. 1, so that the surface of the aggregate is protruded by the primary particles, and valleys are formed between the primary particles. As another example, it may refer to a particle in which three or more protruding parts and a plurality of valleys or a plurality of shrunken cavity parts are formed between the protruding parts, even if not aggregated. For example, it may refer to a particle in which three or more, four or more, five or more, six or more protruding parts are formed on the surface of the organic particles, and a plurality of valleys or a plurality of shrunken cavity parts are formed between the protruding parts.
[0057] The organic particles of the present invention having the above size and shape can sufficiently improve adhesion to an electrode and remarkably improve breathability and anti-blocking properties even when contained in a relatively small amount, compared to organic particles having a spherical shape as shown in FIG.
[0058] Furthermore, the average particle size (D50) of the organic particles is not particularly limited as long as they have the above-mentioned morphology, and can be, for example, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 0.5 μm or less, 0.1 μm or more, 0.3 μm or more, or 0.5 μm or more, and may be preferably 0.1 to 10 μm, more preferably 0.1 to 2 μm, even more preferably 0.1 to 1.5 μm, and extremely preferably 0.2 to 1.0 μm.
[0059] Within this range of average particle size, the binding effect with the inorganic particles is better achieved, and at the same time, the adhesive strength with the electrode is significantly improved. In particular, when the size is 0.1 to 1.5 μm, the blocking phenomenon in which adhesive layers block each other during transportation or lamination, or the adhesive adheres to other parts in contact with the adhesive layer, causing the adhesive layer on the upper part of the inorganic particle layer to detach, is significantly reduced, and the adhesive strength with the electrode is dramatically increased, and furthermore, it is possible to make the film thinner, which is even better.
[0060] In one embodiment, the particle size distribution of the organic particles may have a D10 / D90 value of 0.3 or more, 0.4 or more, 0.9 or less, 0.8 or less, or a value between the above values. Alternatively, it may be 0.3 to 0.9 or 0.4 to 0.8. When the particle size distribution range of the organic particles is satisfied, the content of the organic particles for ensuring electrode adhesive strength can be further reduced, which is more advantageous in ensuring breathability and anti-blocking properties, and is therefore preferable, but not necessarily limited thereto.
[0061] In one embodiment, when the ratio of the average particle diameter of the organic particles to the average particle diameter of the inorganic particles (D50) is 0.5 or more, 0.6 or more, 0.7 or more, 3 or less, 1.7 or less, 1.5 or less, 1.3 or less, 1.0 or less, or a value between the above numerical values, the content of the organic particles flowing into the surface irregularities or voids of the inorganic particle layer can be further reduced, which is more preferable for ensuring breathability and anti-blocking properties, but is not limited thereto. Preferably, the ratio of the average diameter of the organic particles to the average diameter of the inorganic particles may be 0.5 to 3, 0.5 to 2.0, 0.5 to 1.7, 0.5 to 1.5, 0.6 to 1.3, or 0.7 to 1.0.
[0062] In one embodiment, the adhesive layer may contain 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, 99% by weight or more, or 100% by weight of the organic particles based on the total weight of the adhesive layer in order to provide a separator having excellent electrode adhesion, anti-blocking properties, and breathability even with a thin thickness. The more the organic particles in the form of secondary particles are contained, the more advantageous it is for achieving the object of the present disclosure, so there is no particular upper limit on the content.
[0063] According to one embodiment, the separator has organic particles constituting an adhesive layer formed on an inorganic particle layer, which has a specific shape as defined above as shown in Figure 1, and thus has excellent physical properties such as electrode adhesion, air permeability, and anti-blocking properties, which are the same polymer as the organic particles, but are spherical or circular without valleys as shown in Figure 5. Therefore, the composition of the organic particles of the present invention is not particularly limited, and any composition of organic particles commonly used in the art to improve electrode adhesion may be used.
[0064] As a non-limiting example, the organic particles may be made of a particulate acrylic polymer or fluoropolymer, which may be crosslinked or not crosslinked, or may have a core-shell structure. The particulate acrylic polymer of the core-shell structure may be, for example, a polymer containing an acrylic monomer and, if necessary, other comonomers and a crosslinking agent on the surface of a core rubber or crosslinked particle, but is not particularly limited thereto.
[0065] The organic particles of the specific form according to the embodiment can remarkably improve electrode adhesion even in a small amount due to their structural characteristics, and when they have a high glass transition temperature, can further improve anti-blocking properties, which is preferable. In this case, the glass transition temperature (Tg) of the organic particles can be 50°C or more, 60°C or more, 90°C or less, 80°C or less, 70°C or less, or a value between the above values, for example, 50 to 90°C, 55 to 75°C, or 60 to 70°C, but is not limited thereto.
[0066] In one embodiment, the adhesive layer may further include, in addition to the organic particles, other components such as an activator, a surfactant, etc., which are known in the art to be added to an electrode adhesive organic layer of a separator, but are not particularly limited thereto.
[0067] In one embodiment, the adhesive layer is a porous particle layer in which the organic particles are connected and fixed to each other, and may have an area ratio of 60% or more, 70% or more, 80% or more, or 100% based on the entire surface of the inorganic particle layer, and may be laminated 100% except for defects that occur specifically. In one embodiment, after forming a porous inorganic particle layer on a porous substrate, a porous adhesive layer having the above-mentioned shape and size may be laminated on the porous inorganic particle layer to further improve the air permeability and ion conductivity of the separator, but is not particularly limited.
[0068] In one embodiment, the thickness of the adhesive layer may be greater than 0 μm, greater than 0.1 μm, greater than 0.2 μm, greater than 0.3 μm, less than 2 μm, less than 1.5 μm, less than 1 μm, less than 0.9 μm, less than 0.7 μm, or a value between the above values. The thickness of the adhesive layer may be greater than 0 μm and less than 2 μm, or 0.1 to 1 μm to achieve a high capacity battery.
[0069] In one embodiment, the total thickness of the separator in which the inorganic particle layer and the adhesive layer are disposed on one or both sides of the porous substrate may be 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, 30 μm or more, 50 μm or less, 30 μm or less, 20 μm or less, 15 μm or less, or a value between the above numerical values. The total thickness of the separator may be 5 to 50 μm, or 5 to 25 μm or 7 to 20 μm to realize a high-capacity battery, but is not particularly limited.
[0070] In one embodiment, the content of the organic particles in the adhesive layer is 0.2 g / m 2 More than 0.5g / m 2 More than 1g / m 2 More than 2.0g / m 2 Below, 1g / m 2 Below 0.5g / m 2 It may be less than or equal to the above-mentioned values, and preferably is 0.2 to 1.0 g / m 2 may be also possible.
[0071] The method for producing the organic particles having the specific shape is not particularly limited. In one embodiment, a polymerization solution of primary particles is produced by a polymerization method such as emulsion polymerization or suspension polymerization of various radical polymerizable monomers such as acrylic or fluorine-based monomers, and the solution is spray-dried at a high temperature of 200°C to 300°C for several seconds and classified by size to produce secondary particle aggregates, or the protrusions and valleys can be formed by removing non-reacted monomers from the polymer particles by vacuum distillation after suspension polymerization, but is not limited thereto.
[0072] The adhesive layer may be disposed on the inorganic particle layer using any method known in the art, and the method is not particularly limited. As a non-limiting example, the organic particles may be added with water and stirred to prepare a slurry for the adhesive layer, and the slurry may be applied onto the inorganic particle layer by any one or a combination of slot die coating, roll coating, spin coating, dip coating, bar coating, die coating, slit coating, and inkjet printing, to form an adhesive layer on the inorganic particle layer.
[0073] In one embodiment, the separator may be laminated on a carbon sheet having a thickness of 200 μm so that the adhesive layers of the separator face each other, and then pressed and bonded in a hot press at 80° C. and 20 MPa for 30 seconds, and the electrode adhesive strength measured by peeling at 180° using a UTM device according to ASTM D903 may be 1.5 gf / 15 mm or more, 2.0 gf / 15 mm or more, 2.5 gf / 15 mm or more, or 3 gf / 15 mm or more, or 1.5 gf / 15 mm to 4.0 gf / 15 mm, or 2.0 to 4.0 gf / 15 mm.
[0074] According to the above embodiment, the organic particles having the above morphology and a high glass transition temperature are more preferable because they can ensure sufficient electrode adhesion and improve anti-blocking properties even when used in a small amount to be thinly coated or when coated on the inorganic particle layer in a well-distributed manner even if the coating area is not sufficient.
[0075] For example, two separators each having a porous substrate, an inorganic particle layer, and an adhesive layer laminated in that order are arranged so that the adhesive layers face each other, and then they are pressed together at a temperature of 60°C and a pressure of 7.5 MPa for one hour. When they are separated, it is checked with an SEM to see whether the adhesive layer has peeled off in part or in whole, causing blocking between the separator surfaces. This ensures excellent anti-blocking properties, with no blocking being observed.
[0076] The separator of one embodiment may have an air permeability change (ΔG) represented by the following formula of 50 sec / 100 cc or less, 45 sec / 100 cc or less, 40 sec / 100 cc or less, 35 sec / 100 cc or less, or 30 sec / 100 cc or less.
[0077] ΔG=G1-G2
[0078] In the above formula, G1 is the gully permeability of the separator in which an inorganic particle layer and an adhesive layer are laminated in sequence on both sides of the porous substrate, and G2 is the gully permeability of the porous substrate itself. The gully permeability was measured according to the ASTM D726 standard using a Densometer manufactured by Toyoseiki Co., Ltd., and the unit is seconds / 100cc.
[0079] According to one embodiment, the separator may have excellent two or more of electrode adhesion, anti-blocking property, and air permeability, and more preferably, may have excellent electrode adhesion, anti-blocking property, and air permeability.
[0080] Another aspect is to provide an electrochemical device including the separator. The electrochemical device may be an energy storage device, and is not particularly limited thereto, but a non-limiting example thereof may be a lithium secondary battery. The lithium secondary battery is well known, and its configuration is also well known, so it will not be described in detail in the present disclosure.
[0081] The lithium secondary battery according to one embodiment may include the separator between the positive electrode and the negative electrode. In this case, the positive electrode and the negative electrode may be any electrode that is generally used in lithium secondary batteries, without any limitation.
[0082] The present disclosure will be described in more detail below based on examples and comparative examples. However, the following examples and comparative examples are merely examples for describing the present disclosure in more detail, and the present disclosure is not limited to the following examples and comparative examples.
[0083] The separator properties were measured as follows.
[0084] 1.Adhesion strength of electrodes The separator adhesive layer is layered on a 200μm thick carbon sheet (TOYO Tanso Korea, PF-20HP) with the adhesive layer facing each other, then pressed and bonded in a heat press at 80℃ and 20MPa for 30 seconds, and the electrode adhesive strength is measured by peeling at 180° using INSTRON's UTM device according to ASTM D903. If the adhesive strength of the separator adhesive layer is too low to even be peeled using the UTM device, it is evaluated as "unmeasurable."
[0085] 2.Change in air permeability The change in air permeability ΔG is calculated as follows:
[0086] ΔG=G1-G2
[0087] In the above formula, G1 is the gully permeability of a separator in which an inorganic particle layer and an adhesive layer are laminated in sequence on both sides of a porous substrate, and G2 is the gully permeability of the porous substrate itself. Gully permeability is measured using a Toyoseiki Densometer in accordance with the ASTM D726 standard, and the time it takes for 100cc of air to pass through an area of 1 square inch of the separator is recorded in seconds. The unit is seconds / 100cc.
[0088] 3. Anti-blocking properties Two separators each having a porous substrate, an inorganic particle layer, and an adhesive layer laminated thereon were arranged so that the adhesive layers faced each other, and then pressed together at a temperature of 60°C and a pressure of 7.5 MPa for 1 hour. Next, when peeled at 180° according to ASTM D903, it was evaluated whether the adhesive layers adhered to each other and peeled off partially or entirely. If even a portion peeled off, blocking was deemed to have occurred, and if no peeling occurred and the adhesive layers separated as they were, blocking was deemed not to have occurred. The occurrence of blocking was confirmed by SEM. If blocking was confirmed through SEM, it was evaluated as "NG", and if blocking was not confirmed, it was evaluated as "OK".
[0089] 4.Measuring method for average particle size The average particle size (D50), D10 and D90 were measured using a particle size analyzer, Microtrac S3500, based on the ISO 13320-1 standard.
[0090] 5. Glass transition temperature The glass transition temperature was measured using a TA DSC (model: Q200) by heating from -50°C to 300°C at a heating rate of 20°C / min in a nitrogen atmosphere. The temperature was raised twice (first run, second run, and cooling) to measure.
[0091] [Example 1] 1) Preparation of adhesive layer slurry Acrylic latex (acrylic latex made by polymerizing methyl methacrylate and butyl methacrylate) with an average particle size (D50) of 550nm and a glass transition temperature (Tg) of 65℃, as shown in Figure 1, was added to water to a solid content of 5% by weight and stirred to prepare a uniformly mixed adhesive layer slurry. At this time, the D10 / D90 of the organic particles was 0.57.
[0092] 2) Manufacturing of slurry for inorganic particle layer 100 parts by weight of boehmite particles (Nabaltec, Apyral AOH60) having a D50 of 600 nm as inorganic particles were mixed with 3 parts by weight of a water-soluble acrylic binder (Ashland, PVP K120) and water to prepare a slurry with an inorganic particle content of 40% by weight.
[0093] 3) Separator manufacturing The slurry for the inorganic particle layer was applied to both sides of a polyolefin-based porous substrate (SKinnovation, ENPASS) with a thickness of 8.5 μm and a gallium permeability of 125 sec / 100 cc using two slot coating dies, and the substrate was thoroughly dried at 40° C. to form an inorganic particle layer. The slurry for the adhesive layer was then applied to the upper surface of the inorganic particle layer, and the substrate was thoroughly dried at 40° C. to form an adhesive layer. The inorganic particle layer of the separator had a thickness of 1.5 μm, the adhesive layer had a thickness of 0.5 μm, and the total thickness of the separator was 12.5 μm. The content of organic particles in the coated adhesive layer was 0.4 g / m 2 A photograph of the surface of the adhesive layer is shown in Figure 3, and its physical properties are listed in Table 1.
[0094] [Example 2] A separator was manufactured in the same manner as in Example 1, except that the D50 of the slurry for the adhesive layer was 400 nm. The results are shown in Table 1.
[0095] [Example 3] A separator was manufactured under the same conditions as in Example 1, except that the organic particles in Example 1 were coated with an acrylic latex having a D50 of 1.8 μm and a glass transition temperature (Tg) of 65° C. in the amounts shown in Table 1. The results are shown in Table 1.
[0096] [Example 4] A separator was produced under the same conditions as in Example 1, except that when producing the slurry for the adhesive layer, an acrylic latex having the same composition as the organic particles in Example 1, a D50 of 1.0 μm, and a glass transition temperature (Tg) of 62° C. was coated in the amount shown in Table 1. The results are shown in Table 1.
[0097] [Comparative Example 1] The same procedure was carried out as in Example 1, except that the acrylic latex in Example 1 was dissolved in an organic solution and applied to the inorganic particle layer. The results are shown in FIG.
[0098] [Comparative Example 2] A separator was manufactured under the same conditions as in Example 1, except that instead of the organic particles in Example 1, perfectly spherical organic particles as shown in Figure 5, which were produced by suspension polymerization using the same monomers as in Example 1, were coated with an acrylic latex having a D50 of 540 nm and a glass transition temperature (Tg) of 65°C in the amount shown in Table 1. The results are shown in Figure 5 and Table 1.
[0099] [Comparative Example 3] A separator was manufactured under the same conditions as in Example 1, except that, instead of the organic particles in Example 1, perfectly spherical organic particles were coated with acrylic latex having a D50 of 200 nm and a glass transition temperature (Tg) of 65° C. in the amounts shown in Table 1. The results are shown in FIG. 6 and Table 1.
[0100] The physical property evaluation results of the separators manufactured in the above examples and comparative examples of the present invention are summarized in Table 1 below.
[0101] [Table 1]
[0102] Referring to the results in Table 1 and the drawings, as shown in FIG. 3, an adhesive layer was formed of organic particles having a secondary convex shape including convex protrusions on the surface and valley parts between the protrusions. In Examples 1 and 2, in which the average particle size ratio of organic particles to inorganic particles is between 0.5 and 1.5 and the average particle size of the organic particles is 1.5 μm or less, it was confirmed that the adhesive layer having the best electrode adhesion and anti-blocking properties was well formed on the inorganic particle layer.
[0103] In addition, Example 4, in which the average size of the organic particles is 1 μm and the organic particle / inorganic particle ratio is 1.67, is inferior to Examples 1 and 2, but has significantly better electrode adhesion and anti-blocking properties than the comparative examples. Example 3, in which the average size is 1.8 μm and the organic particle / inorganic particle ratio is 3, is inferior to Examples 1, 2, and 4 in anti-blocking properties, but has better adhesion than the comparative examples.
[0104] On the other hand, Comparative Example 1 used a soluble acrylic polymer, which blocked the voids on the surface, resulting in poor breathability and very low electrode adhesion, as shown in Figure 4. In addition, in Comparative Examples 2 and 3, which have spherical adhesive layers, as shown in Figures 5 and 6, the adhesive layers were spherical, resulting in poor electrode adhesion and very poor anti-blocking properties.
[0105] As described above, the present disclosure has been described using specific details and limited examples, but these are provided to facilitate a more complete understanding of the present disclosure. The present disclosure is not limited to the above examples, and various modifications and variations can be made from these descriptions by those having ordinary knowledge in the field to which the present disclosure pertains.
[0106] Therefore, the present disclosure is not limited to the embodiments described above, and it can be said that not only the scope of the claims described below, but also all modifications that are equivalent or equivalent to the scope of the claims fall within the scope of the present disclosure. [Explanation of symbols]
[0107] 100: Organic particles 10:Protrusion 20: Valley
Claims
1. A porous substrate; an inorganic particle layer disposed on at least one surface of the porous substrate, in which inorganic particles are connected to each other to form pores between the inorganic particles; an adhesive layer disposed on the inorganic particle layer, the adhesive layer including organic particles having a plurality of protrusion parts and a plurality of valley parts connected to each other to form pores.
2. 2. The separator according to claim 1, wherein a ratio of an average particle size (D50) of said organic particles to an average particle size (D50) of said inorganic particles is 0.5 to 1.
5.
3. The separator according to claim 1, wherein the organic particles have a D50 of 0.1 to 1.5 μm.
4. The separator according to claim 1, wherein the particle size distribution D10 / D90 of the organic particles is 0.3 to 0.
9.
5. The separator according to claim 1, wherein the organic particles have a glass transition temperature (Tg) of 50 to 90°C.
6. The separator according to claim 1 , wherein the adhesive layer has a thickness of more than 0 μm and not more than 2 μm.
7. 2. The separator according to claim 1, wherein the organic particles are secondary particles in which primary particles are aggregated together due to surface melting to form a plurality of protrusion parts and a plurality of valley parts, or primary particles having a plurality of protrusion parts and a plurality of valley parts on a surface.
8. The separator according to claim 1 , wherein the adhesive layer contains 70% by weight or more of the organic particles based on the weight of the entire adhesive layer.
9. The adhesive layer contains the organic particles at a concentration of 0.2 to 2.0 g / m 2 The separator of claim 1 comprising:
10. The separator according to claim 1, wherein the separator is laminated on a 200 μm thick carbon sheet (TOYO Tanso Korea, PF-20HP) with the adhesive layer of the separator facing each other, and then pressed at 80° C. and 20 MPa for 30 seconds using a hot press machine, and peeled at 180° using an INSTRON UTM device according to ASTM D903, and the electrode adhesive strength measured is 1.5 gf / 15 mm to 4.0 gf / 15 mm.
11. The separator according to claim 10, wherein the separator has an air permeability change ΔG of 50 seconds / 100 cc or less, as measured by the following formula: ΔG = G 1 -G 2 In the above formula, G 1 is the gully permeability of a separator in which an inorganic particle layer and an adhesive layer are laminated in this order on both sides of a porous substrate, and G 2 is the gully permeability of the porous substrate itself. The gully permeability was measured using a Densometer from Toyo Seiki Co., Ltd. in accordance with the ASTM D726 standard, and is expressed in units of seconds / 100 cc.
12. The separator according to claim 11, wherein when two separators are arranged with the adhesive layers facing each other, and then pressed together at a temperature of 60° C. and a pressure of 7.5 MPa for one hour, and then peeled off at 180° in accordance with ASTM D903, the adhesive layers do not adhere to each other and are partially or entirely peeled off, but rather the adhesive layers are separated as they are and blocking does not occur.
13. An electrochemical element comprising the separator according to any one of claims 1 to 12.
Citation Information
Patent Citations
Separators for electronic components and electronic components
JP4414165B2