Manufacturing method of rare earth magnet powder

By applying high-temperature heating after the recombination step in the HDDR process, the method enhances the magnetic properties of rare earth magnet powders containing Ce, overcoming structural non-uniformity issues and improving squareness.

JP2024134583APending Publication Date: 2024-10-04AICHI STEEL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044847
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing rare earth magnet powders containing Ce do not exhibit sufficient magnetic properties, particularly in terms of squareness (Hk), despite efforts to stabilize the supply of rare earth elements through the use of Ce in place of Nd and Pr, which are unevenly distributed.

Method used

A manufacturing method involving high-temperature heating after the recombination step in the HDDR process to suppress structural unevenness in magnet raw materials containing Nd and Ce, enhancing magnetic properties.

Benefits of technology

The method results in rare earth magnet powder with improved magnetic properties, including higher squareness (Hk), by addressing structural non-uniformity through controlled high-temperature heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134583000001_ABST
    Figure 2024134583000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a rare earth magnet powder containing Nd and Ce.SOLUTION: A manufacturing method of a rare earth magnet powder includes: a disproportionation step (HD) of causing a disproportionation reaction to occur by absorbing hydrogen in a magnet raw material containing a rare earth element, which contains at least Nd and Ce, a transition element and B; and a recombination step (DR) of causing a recombination reaction to occur by performing dehydrogenation from the magnet raw material after the disproportionation step. The manufacturing method includes a tissue control step of heating the magnet raw material at 850 to 900°C. The tissue control step may also be included in at least a part of a forced exhaustion step of bringing a processing atmosphere into a vacuum atmosphere after a controlled exhaustion step of controlling the processing atmosphere of the magnet raw material into a predetermined hydrogen pressure, for example. Tissue nonuniformity is decreased by the tissue control step, so that it may be considered that magnetic characteristics of the rare earth magnet powder are improved.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing rare earth magnet powder used in bonded magnets and the like. [Background technology]

[0002] Bonded magnets, which are made by binding rare earth magnet powder with a binder resin, have excellent shape flexibility and exhibit high magnetic properties, and are therefore used in a variety of electromagnetic devices such as electrical appliances and automobiles, where energy savings and weight reduction are desired. In order to expand the use of bonded magnets, in addition to improving the magnetic properties of the rare earth magnet powder, a stable supply of rare earth elements (sources), which are the main raw materials of rare earth magnet powder, is required. Proposals related to these issues are made, for example, in the following patent documents. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2016-115774 Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Document 1 describes a rare earth magnet powder obtained by subjecting a raw alloy in which part of Nd has been replaced (substituted) with Ce to HDDR, and then subjecting the powder to a diffusion infiltration treatment using an NdCu alloy. By effectively utilizing Ce, which generally has a high abundance ratio in rare earth deposits, the supply instability of light rare earth elements (Nd, Pr, etc.) and heavy rare earth elements (Dy, etc.) that accompanies uneven distribution of rare earth deposits can be reduced.

[0005] The rare earth magnet powder in Patent Document 1 contains rare elements (Co, Ga) that are generally effective in improving magnetic properties, but the magnetic properties are not necessarily sufficient. Bonded magnets using magnet powder containing Ce are required to have further improved magnetic properties (for example, squareness: Hk, which is an index of reverse magnetic field resistance, etc.).

[0006] Incidentally, HDDR (reaction / treatment / step) mainly consists of a disproportionation reaction caused by hydrogen absorption (Hydrogenation-Disproportionation / HD) and a recombination reaction caused by desorption (Desorption-Recombination / DR). In this specification, unless otherwise specified, the term "HDDR" also refers to its improved version, d-HDDR (dynamic-Hydrogenation-Disproportionation-Desorption-Recombination), etc.

[0007] The present invention has been made under these circumstances, and has an object to provide a production method and the like that can obtain rare earth magnet powder that exhibits high magnetic properties while still containing Ce. [Means for solving the problem]

[0008] The inventors of the present invention have conducted extensive research to solve this problem, and have succeeded in further improving the magnetic properties of rare earth magnet powder containing Nd and Ce by performing high temperature heating after the DR process, contrary to conventional technical wisdom. Based on this result, the inventors have completed the present invention, which will be described below.

[0009] <Production method of rare earth magnet powder> (1) The present invention is a method for producing rare earth magnet powder, comprising a disproportionation step in which a magnet raw material containing rare earth elements including at least Nd and Ce, a transition element, and B is caused to absorb hydrogen to cause a disproportionation reaction, and a recombination step in which hydrogen is removed from the magnet raw material after the disproportionation step to cause a recombination reaction, and further comprising a structure control step after the recombination step in which the magnet raw material is heated at 850 to 900°C.

[0010] (2) According to the manufacturing method of the present invention, rare earth magnet powder with high magnetic properties can be obtained using magnet raw materials that contain at least Nd and Ce. The reason for this is not entirely clear, but at present it is thought to be as follows.

[0011] If the rare earth elements (R) contained in the magnet raw materials are different, the three-phase decomposition structure (αFe phase, RH2 phase, Fe2B phase, etc.) generated by the disproportionation reaction (HD) will be transformed into R2Fe by the recombination reaction (DR). 14 The conditions under which B etc. are produced (hydrogen pressure and temperature in the treatment atmosphere) may also vary. 14 Even if the conditions are set such that B (including hydrides) are generated, R2Fe 14 The timing of generation of B, etc. may differ for each rare earth element. For convenience, Fe, which is a typical transition element (TM), is used as an example for explanation (the same applies below).

[0012] For this reason, when a magnet raw material contains a significant amount of rare earth elements, the metal structure (magnet structure) obtained after DR may have non-uniformity (sometimes referred to as "structural unevenness") according to the number of rare earth elements. It was speculated that such structural unevenness was one of the factors that deteriorated the magnetic properties of rare earth magnet powder that contains Ce in addition to Nd.

[0013] It is believed that by subjecting the magnet raw material after HD processing to high-temperature heat treatment as in the present invention, the occurrence of the above-mentioned structural irregularities is suppressed, or irregularities that have already occurred are reduced or eliminated. As a result, it is presumed that a rare earth magnet powder that exhibits better magnetic properties than conventional rare earth magnet powders can be obtained, despite the inclusion of Ce.

[0014] In addition, it was previously generally believed that heating magnet particles to high temperatures (e.g., 850°C or higher) would cause the crystal grains that make them to coarsen or grow abnormally, resulting in a decline in magnetic properties. For this reason, even magnet raw materials that contain Ce in addition to Nd were actually subjected to hydrogen treatment at temperatures below 850°C (e.g., 840°C).

[0015] 《Rare earth magnet powder, compounds, bonded magnets》 The present invention can be understood as a rare earth magnet powder, a bonded magnet in which the rare earth magnet powder is bound with a resin, and a compound used in the manufacture of the bonded magnet. The compound is made by attaching a resin as a binder to the surface of the powder particles in advance. The powder used for the bonded magnet or compound may be a composite powder in which powders other than the rare earth magnet powder of the present invention (one or more of NdFeB powder, SmFeN powder, ferrite powder, etc.) are mixed.

[0016] "others" (1) Rare earth magnet powder may be either isotropic or anisotropic. Anisotropic magnet powder consists of magnet particles whose magnetic flux density (Br) in one direction (easy axis of magnetization, c-axis direction) is greater than the magnetic flux density in other directions. Isotropy and anisotropy can be distinguished by the degree of anisotropy (DOT: Degree of Texture) = [Br( / / )-Br(⊥)] / Br( / / ) obtained when a magnetic field is applied parallel ( / / ) and perpendicular (⊥) to the c-axis direction; if the DOT value is 0, the material is isotropic, and if it is greater than 0, the material is anisotropic.

[0017] (2) The rare earth elements (R) may include La, Pr, Y, Sm, Tb, Dy, etc. The transition (metal) elements (TM) include 3d transition elements (Sc-Cu) and 4d transition elements (Y-Ag). Representative examples of R are Nd, Ce, La, or Pr, and representative examples of TM are Fe, Co, and Ni. In this specification, Fe is used as an example of a transition element as appropriate. Note that a part of B may be substituted with C.

[0018] The magnet raw material or rare earth magnet powder may contain modifier elements or (unavoidable) impurities that are effective in improving the properties. Modifier elements include, for example, Cu, Al, Ti, V, Cr, Ni, Zn, Ga, Zr, Nb, Mo, Sn, Hf, Ta, W, Dy, Tb, Co, etc., which are effective in improving the coercive force.

[0019] (3) Unless otherwise specified, "x to y" in this specification includes a lower limit of x and an upper limit of y. Any numerical value included in the various numerical values ​​or numerical ranges described in this specification may be used as a new lower limit or upper limit to create a range such as "a to b." In addition, "x to y kPa" means x kPa to y kPa, and the same applies to other units. [Brief description of the drawings]

[0020] [Figure 1A] 3 shows a manufacturing process for the rare earth magnet powder according to the first embodiment. [Figure 1B] The d-HDDR process is shown below. [Figure 1C] The structure control process is shown below. [Figure 1D] The magnetic properties of the rare earth magnet powder are shown below. [Figure 2A] 1 shows a manufacturing process for rare earth magnet powder and a d-HDDR process according to a second embodiment. [Figure 2B] The magnetic properties of the rare earth magnet powder are shown below. [Figure 3A] 1 shows a d-HDDR process according to a third embodiment. [Figure 3B] The magnetic properties of the rare earth magnet powder are shown below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] One or more components selected from this specification may be added to the above-mentioned components of the present invention. The contents described in this specification apply not only to the manufacturing method of the present invention, but also to rare earth magnet powder, compounds, bonded magnets, etc., as appropriate, and even method-related components can become product-related components. Which embodiment is best depends on the target, required performance, etc.

[0022] 《Magnet raw materials》 The magnet raw material is made of a magnet alloy containing at least a rare earth element (R), a transition element (TM), and B. R contains at least Nd and Ce. The magnet raw material may be in any form or state, such as a lump, particle, or powder. The magnet raw material is obtained, for example, by subjecting a cast alloy to homogenization treatment, dispersion treatment, hydrogen crushing, classification, etc. The details of these are as follows.

[0023] (1) Casting alloy The casting alloy may be an ingot alloy obtained by pouring a molten R-TM-B alloy into a mold and solidifying it, or a rapidly solidified alloy obtained by rapidly solidifying the molten alloy. The rapidly solidified alloy may be obtained, for example, by the strip casting method (SC).

[0024] When the diffusion process is performed, the component composition of the cast alloy may be adjusted taking into consideration the amount of the diffusion raw material mixed in. For example, when the entire cast alloy is taken as 100 at%, the cast alloy contains 11 to 15 at%, or 12 to 13 at%, of R, and 5 to 9 at%, or 6 to 7 at%, of B. The remainder is a transition element (e.g., Fe) or a modifier element (e.g., Nb, Ga, etc.).

[0025] (2) Homogenization The cast alloy may be subjected to homogenization treatment (solution treatment) before hydrogen cracking. The homogenization treatment makes it easier to obtain a homogenous structure consisting of fine crystal grains (e.g., grain size: 50 to 250 μm). In particular, when the ingot alloy is subjected to homogenization treatment, it is possible to eliminate the soft magnetic αFe phase and eliminate segregation.

[0026] The homogenization treatment is performed, for example, by heating the cast alloy at 1000 to 1200° C., or 1050 to 1150° C. The treatment time is, for example, 3 to 70 hours, 15 to 60 hours, or 30 to 50 hours. The heating atmosphere is, for example, an inert atmosphere (an inert gas atmosphere such as Ar, or a vacuum atmosphere).

[0027] (3) Distributed processing The cast alloy may be subjected to a dispersion treatment after the homogenization treatment or before the hydrogen cracking described below. The dispersion treatment uniformly forms an R-rich (e.g., Nd-rich) grain boundary phase at the grain boundaries of the cast alloy. As a result, when the hydrogen cracking treatment is performed on the cast alloy after the dispersion treatment, fracture (separation) occurs preferentially at the grain boundaries, and the occurrence of intragranular cracks is suppressed.

[0028] The dispersion treatment is performed by heating to a temperature higher than the hydrocracking temperature or lower than the homogenization treatment temperature. The temperature is, for example, 650 to 1000°C, 650 to 900°C, or 680 to 750°C. The treatment time is, for example, 10 minutes to 5 hours, or 0.5 to 3 hours. The heating atmosphere is, for example, an inert atmosphere.

[0029] (4) Hydrocrackling Hydrogen cracking is performed by exposing the cast alloy to a hydrogen atmosphere at, for example, 350 to 585°C, 400 to 575°C, or 425 to 550°C. The hydrogen partial pressure is, for example, 1 kPa to 250 kPa, or 5 kPa to 150 kPa. The treatment time (the time elapsed after the atmospheric temperature reaches the target temperature) is, for example, 0.1 to 10 hours, or 0.5 to 5 hours. Hydrogen may be introduced into the treatment furnace after the atmospheric temperature (or the temperature of the cast alloy) reaches the set temperature.

[0030] When exposed to a hydrogen atmosphere, the cast alloy absorbs hydrogen and either collapses or is lightly crushed into grains or lumps with a maximum length of about several centimeters to several mm. Such grains or lumps may be used as the magnet raw material as is, or may be further crushed or pulverized to adjust the particle size (for example, to a maximum particle length of about 100 μm to 1 mm) and then used as the magnet raw material. The hydrogen-crushed magnet raw material may still have absorbed hydrogen, or may be dehydrogenated.

[0031] As used in this specification, "hydrogen crushing (process / treatment)" is not for the purpose of macroscopically crushing or pulverizing a cast alloy, but is carried out to minimize the generation of cracks in the crystal grains (single crystal grains) that make up the cast alloy. During hydrogen crushing, hydrogen hardly penetrates into the crystal grains, but mainly penetrates into the grain boundary phase (R-rich phase / Nd-rich phase), and cracks preferentially occur between the crystal grains due to the volume expansion of the grain boundary phase. As a result, the cast alloy is separated between the crystal grains, and a crushed raw material (magnet raw material) composed of crystal grains with few cracks or cracks is obtained. The effects and mechanisms of such hydrogen crushing are described in detail in WO2020 / 017529, and the content (full text) thereof shall be incorporated into this application as appropriate.

[0032] (5) Particle size adjustment (classification) The magnet raw material may be subjected to particle size adjustment. For example, a material obtained by partially removing fine particles (particles belonging to the smaller particle size side) contained in the crushed raw material may be used as the magnet raw material. Such particle size adjustment (classification) is performed, for example, by sieving.

[0033] The particle size is indicated by, for example, the particle size (d). For example, particles with a particle size less than α (μm) (d < α) are particles that pass through a sieve with a nominal mesh opening (mesh size) of α. Also, particles with a particle size greater than β (μm) (β < d) are particles that do not pass through a sieve with a mesh size of β. Although the particle size of the magnet raw material is not limited, for example, it may be d < 500 μm, d < 250 μm or d < 212 μm, or 53 μm < d, 106 μm < d or 150 μm < d.

[0034] 《HDDR》 By HDDR (hydrogen treatment), a magnet powder composed of polycrystals (magnet particles) in which fine R2TM 14 B1-type crystals (average crystal grain size: 0.05 to 2 μm) are aggregated is obtained. HDDR (including d-HDDR) is roughly composed of a disproportionation step (HD) and a recombination step (DR). The details are as follows.

[0035] (1) Disproportionation step (HD) In the disproportionation process, the magnet raw material is placed in a treatment furnace and exposed to a specified hydrogen atmosphere to cause a disproportionation reaction in the hydrogen-absorbed magnet raw material. Through this process, the magnet raw material undergoes a disproportionation reaction (forward transformation reaction) and becomes a three-phase decomposed structure (αFe phase, RH2 phase, and Fe2B phase).

[0036] The disproportionation step is carried out, for example, at a hydrogen partial pressure of 10 to 300 kPa or 15 to 60 kPa, a treatment temperature of 600° C. or higher and lower than 850° C. or 750 to 845° C., and a treatment time of 1 to 6 hours or 2 to 5 hours (high-temperature hydrogenation step).

[0037] Prior to this step, the magnet raw material may be kept in a hydrogen atmosphere (hydrogen partial pressure, for example, 20 to 100 kPa) at a temperature lower than the temperature at which the disproportionation reaction occurs (for example, room temperature to 300°C or room temperature to 100°C) (low-temperature hydrogenation step). Note that the hydrogen atmosphere referred to in this specification may be a mixed gas atmosphere of hydrogen and an inert gas.

[0038] During the disproportionation step, the hydrogen partial pressure or the treatment temperature (ambient temperature) does not have to be constant from start to finish. For example, at the end of the step when the reaction rate is decreasing, at least one of the hydrogen partial pressure or the temperature may be increased to adjust the reaction rate and promote three-phase decomposition (structure stabilization step). For example, during or at the end of the disproportionation step, the treatment temperature may be increased by 10 to 60°C or 30 to 50°C.

[0039] (2) Recombination process (DR) In the recombination process, hydrogen is removed from the magnet raw material after the disproportionation process, causing a recombination reaction in the magnet raw material. This process causes a recombination reaction (reverse transformation reaction) associated with dehydrogenation in the magnet raw material after the high-temperature hydrogenation process. In other words, the three-phase decomposed structure is formed by removing hydrogen from the RH2 phase and forming fine R2TM phases with the crystal orientation of the Fe2B phase transferred thereto. 14 B1 type crystal hydride (RFeBH X )

[0040] The recombination step is performed, for example, at a hydrogen partial pressure of 0.5 to 10 kPa, 1 to 6 kPa, or 1.5 to 4 kPa, a treatment temperature of 600 to 900° C. or 750 to 890° C., and a treatment time of 1 to 12 hours or 3 to 10 hours.

[0041] By exposing the magnet raw material after the disproportionation process to a hydrogen atmosphere with a specified hydrogen partial pressure, the recombination reaction can be allowed to proceed slowly (controlled evacuation process). If the disproportionation process (structure stabilization process) and the recombination reaction (controlled evacuation process) are carried out at approximately the same temperature, it is possible to transition between processes simply by changing the hydrogen partial pressure.

[0042] In the latter stage of the recombination process (after the controlled evacuation process), residual hydrogen is removed from the magnet raw material exposed to a vacuum atmosphere (for example, 1 Pa or less), and dehydrogenation is completed (forced evacuation process). The treatment temperature is, for example, 600 to 900°C or 750 to 890°C.

[0043] The controlled evacuation process and the forced evacuation process may have the same processing temperature or different temperatures. The processing temperature may change during each process. For example, in the recombination process, the processing atmosphere for the magnet raw materials may transition from a low temperature range to a high temperature range in at least two stages. The timing of the transition, the temperature range of the high temperature range, etc. may be set taking into consideration the structure control process described below.

[0044] The controlled evacuation process and the forced evacuation process do not have to be performed consecutively. After the controlled evacuation process, the magnet raw material may be cooled, and then the forced evacuation process may be performed as a batch process. Such a forced evacuation process may also serve as a structure control process. The cooling process in each process may be rapid cooling with an inert gas or the like to suppress the growth of crystal grains.

[0045] <<Structure Control Process>> In the structure control step, at least after the recombination step, the magnet raw material is heated at a specific temperature (850-900°C, 855-890°C, or 860-880°C). The structure control step reduces or eliminates non-uniformity (structure irregularities) that occurs in the metal structure (magnetic structure) that constitutes the magnet particles, and can improve the magnetic properties of the rare earth magnet powder.

[0046] If the heating temperature is too low, the unevenness of the structure cannot be sufficiently eliminated, whereas if the heating temperature is too high, the crystal grains constituting the magnet structure may become coarse or grow abnormally, which may result in a deterioration of the magnetic properties.

[0047] The structure control step may be performed in a hydrogen atmosphere or an inert atmosphere (vacuum atmosphere, inert gas atmosphere, etc.) as long as the start time, duration, or temperature range is appropriate. Therefore, the structure control step may be performed subordinately to (combined with, incorporated into, or combined with) the recombination step (controlled evacuation step, forced evacuation step) after the start of the recombination step, or may be performed independently after the recombination step. Performing the structure control step subordinately to the recombination step allows for more efficient production of rare earth magnet powder.

[0048] For example, when at least a part of the recombination process doubles as the texture control process, the processing temperature of the entire recombination process may be set to the above-mentioned specific temperature range, or the processing temperature may be set to the specific temperature range from the middle of the recombination process. For example, when the recombination process includes a controlled evacuation process for controlling the processing atmosphere of the magnet raw materials to a predetermined hydrogen pressure, and a forced evacuation process for changing the processing atmosphere to a vacuum atmosphere after the controlled evacuation process, the start timing of the texture control process may be set to after the middle of the controlled evacuation process. The start timing may be, for example, the middle of the controlled evacuation process, or the beginning or middle of the forced evacuation process.

[0049] If the processing temperature of the recombination step is changed from a low temperature range to a high temperature range, the high temperature range may be matched to a specific temperature range of the texture control step. The timing of the change to the high temperature range may be during the controlled evacuation step or at the beginning or middle of the forced evacuation step.

[0050] The structure control process is R2TM 14 It is efficient to carry out the structure control step after the generation of B (including hydrides) is substantially completed. Therefore, the structure control step may be carried out, for example, after a controlled evacuation step in which the processing atmosphere of the magnet raw material is controlled to a predetermined hydrogen pressure. For example, at least a part of a forced evacuation step in which the processing atmosphere is made into a vacuum atmosphere may also serve as the structure control step.

[0051] The processing time of the texture control step may be long, for example, 0.25 to 8 hours, 0.4 to 6 hours, or 1.5 to 4 hours. Note that, although the texture control step is meaningful after the recombination step, the processing temperature may be set to the above-mentioned specific temperature range before the recombination step (for example, during the disproportionation step).

[0052] Diffusion treatment process The magnet raw material after the texture control process may be subjected to a diffusion process. The diffusion process is performed, for example, by heating a mixed raw material obtained by adding a diffusion raw material to the magnet raw material after the HDDR and texture control processes. The diffusion process is performed, for example, in an inert atmosphere. The diffusion process can be used to obtain the R2TM 14 The diffusion raw material penetrates into the surface or grain boundaries of the B1 type crystals to form a non-magnetic phase, which can improve the coercive force of the magnet particles (rare earth magnet powder).

[0053] The diffusion raw materials include, for example, alloys and compounds of light rare earth elements, heavy rare earth elements (Dy, Tb, etc.) or their alloys and compounds (e.g., fluorides), etc. If a light rare earth element (Nd, etc.)-Cu-(Al) alloy or compound is used, the use of rare heavy rare earth elements can be avoided.

[0054] Rare earth magnet powder (1) Rare earth magnet powder (simply referred to as "magnet powder") is made of magnet particles, which are fine R2TM particles that are tetragonal compounds. 14 It consists of B1 type crystals (main phase) and a grain boundary phase surrounding the crystal grains. The stoichiometric composition of the tetragonal compound constituting the main phase is R: 11.8 at%, B: 5.9 at%, and the remainder is TM. Considering the grain boundary phase, the total amount of rare earth elements (Rt) of the magnet particles relative to the whole (100 at%) is, for example, 12 to 18 at%, 12.5 to 16.5 at%, or even 13 to 15 at%. B is contained, for example, 5.5 to 8 at%, or even 6 to 7 at% relative to the whole magnet particles. The remainder other than R and B is transition metal elements (Fe, Cu, etc.), typical metal elements (Al, etc.), typical nonmetal elements (C, O, etc.), impurities, etc.

[0055] (2) The magnetic particles contain at least Nd and Ce. The magnetic particles may contain La. In terms of the atomic ratio to the total amount (Rt) of rare earth elements, Ce / Rt or R1 / Rt (R1 = Ce + La) is, for example, 0.2 to 0.6, 0.25 to 0.55 or 0.3 to 0.5. With respect to the entire magnetic particles (100 at%), for example, Ce may be contained in an amount of 1 to 8 at%, 2 to 7 at% and further 3 to 6 at%, and La may be contained in an amount of 0.05 to 2 at%, 0.1 to 1.5 at% and further 0.15 to 1 at%. Even if the amount of Ce or La is too small, magnetic powder with high magnetic properties can be obtained, but the reduction amount of Nd or the like decreases. If the amount of Ce or La becomes excessive, the magnetic properties of the magnetic powder may deteriorate.

[0056] When both Ce and La are contained, the atomic ratio of La to R1 (= Ce + La) (La / R1) is, for example, 0.01 to 0.35, 0.02 to 0.2 or 0.03 to 0.1. La is not an essential element, but when 0 < La / R1, the La contained together with Ce in the rare earth mineral can be effectively utilized. If La / R1 becomes excessive, the magnetic properties of the magnetic powder may deteriorate.

[0057] (3) As R other than Nd, Ce and La, there are, for example, Pr, Dy, Tb, etc. The magnetic particles may contain at least one kind of modifying elements such as Cu, Al, Si, Ti, V, Cr, Ni, Zn, Ga, Zr, Nb, Mo, Mn, Sn, Hf, Ta, W, Dy, Tb, Co. With respect to the entire magnetic particles, for example, if it is Cu, it may be contained in an amount of 0.1 to 3 at%, 0.3 to 2.5 at% and further 0.5 to 2.0 at%; if it is Al, it may be contained in an amount of 0.2 to 3 at%, 0.5 to 2.5 at% and further 0.8 to 2 at%; if it is Nb, it may be contained in an amount of 0.05 to 0.7 at%, 0.07 to 0.5 at% and further 0.1 to 0.3 at%; if it is Ga, it may be contained in an amount of 0.35 at% or less (0 to 0.35 at%), 0.3 at% or less, 0.2 at% or less and further 0.15 at% or less.

[0058] 《Use》 Rare earth magnet powder can be used for various purposes. A typical example is a bonded magnet. A bonded magnet is mainly composed of rare earth magnet powder and a binder resin. The binder resin may be a thermosetting resin or a thermoplastic resin. The bonded magnet may be compression molded or injection molded. A bonded magnet using rare earth anisotropic magnet powder is preferably molded in an aligning magnetic field. EXAMPLES

[0059] A rare earth magnet powder containing Nd and Ce was produced and its magnetic properties were evaluated. The present invention will be described in detail based on such examples.

[0060] [First Example] In order to clarify the direct effect of the texture control process itself on the magnetic properties of the magnet powder, samples 10 to 13 shown in Fig. 1D were produced and evaluated according to the process shown in Fig. 1A to Fig. 1C. Specifically, the process is as follows.

[0061] <Sample Preparation> (1) Casting An ingot (raw material / base material) having the alloy composition shown in FIG. 1A (R: 12.5 at%, B: 6.5 at%, Nb: 0.2 at%, Fe: balance) was obtained by strip casting (SC).

[0062] The atomic composition of rare earth elements (R) is Nd 0.6 (La 0.05 Ce 0.95 ) 0.4 , that is, Nd 0.6 La 0.02 Ce 0.38 In terms of the entire cast alloy, the Nd content is 7.5 at%, Ce content is 4.75 at%, and La content is 0.25 at%. The atomic ratio (R1 / Rt) of the total amount of Ce and La (R1) to the total amount (Rt) is 0.4.

[0063] (2) Homogenization The ingot was heated in an Ar gas flow at 1100°C for 40 hours.

[0064] (3) Distributed processing The ingot after the homogenization treatment (hereinafter referred to as the "cast alloy") was placed in a vacuum atmosphere (Vac: 10 -2 The test piece was kept at 700°C for 1 hour in a treatment furnace (temperature 100°C or less).

[0065] (4) Hydrocrackling Following the dispersion treatment, the cast alloy in the treatment furnace was heated to 500°C while still in a vacuum state, and hydrogen was then introduced into the treatment furnace. The cast alloy was held at 500°C for 1 hour in a treatment furnace with a hydrogen partial pressure of 100 kPa. The treatment temperature (ambient temperature in the treatment furnace) was measured using a thermocouple in contact with the cast alloy (the treatment temperatures in other processes were the same). The hydrogen partial pressure was measured using a pressure gauge installed in the treatment furnace. For the hydrogen crushing, the contents of WO2020 / 017529 (Patent Document 1) were appropriately referred to.

[0066] (5) Crushing and classification The introduction of hydrogen into the treatment furnace was stopped, and the cast alloy was cooled to room temperature. After the hydrogen in the treatment furnace was replaced with an inert gas (Ar at atmospheric pressure), the cast alloy was removed from the treatment furnace and lightly crushed to obtain a powdered crushed raw material.

[0067] The crushed raw material was sieved to classify the powder (d<212μm) as the magnet raw material to be subjected to d-HDDR. Classification was performed using a test sieve specified in JIS Z 8801. Crushing (pulverization) and classification were performed in an inert gas atmosphere.

[0068] (6)d-HDDR After evacuating the treatment furnace containing the classified magnet raw material samples (12.5 g), the hydrogen partial pressure and temperature in the treatment furnace were controlled according to the chart shown in Figure 1B. Specifically, the procedure was as follows:

[0069] First, a (high-temperature) hydrogenation process (20 kPa x 800°C x 2 hours) was carried out, followed by a structure stabilization process (20 kPa x 840°C x 2 hours). These processes caused a disproportionation reaction (forward transformation reaction) in the magnet raw material (HD: disproportionation process).

[0070] Next, a controlled evacuation process (2.5 kPa × 840°C × 6 hours) was performed to continuously evacuate hydrogen from the treatment furnace, followed by a forced evacuation process (10 -2 Pa x 840℃ x 0.5 hours). In this way, a recombination reaction (reverse transformation reaction) was caused in the magnet raw materials (DR: Recombination process). The furnace was cooled in this vacuum state, and the hydrogen-treated material in the treatment furnace was lightly crushed in Ar gas.

[0071] (7) Structure Control The treatment furnace containing the crushed hydrogen-treated material was again evacuated to a vacuum, and the hydrogen-treated material was heat-treated (10 -2 The treatment time was changed for each sample (sample 11: 1 hour, sample 12: 2 hours, sample 13: 3 hours). Sample 10 was not subjected to the texture control process.

[0072] (8) Diffusion treatment The mixture of the hydrogen-treated sample and the diffusion material was placed in a vacuum atmosphere (10 -1 The diffusion source was heated at 875°C for 3 hours in a vacuum of 10 Pa. 51 Cu 15 Al 34 The alloy powder (average particle size: about 6 μm (D50)) was used. The ratio of the diffusion raw material to the entire mixed raw material was 3.5 mass% (wt%).

[0073] The obtained diffusion-treated product was cooled to near room temperature in a furnace maintained in a vacuum state and then taken out, thus obtaining magnet powder for each sample.

[0074] 《Component composition》 The component composition of the magnet powder of sample 10 was analyzed by an ICP (Inductively Coupled Plasma) emission spectrometer. The components of the magnet powder (100 at%) were Nd: 8.5 at%, Ce: 4.6 at%, La: 0.3 at%, B: 6.3 at%, Nb: 0.2 at%, Cu: 0.4 at%, Al: 0.8 at%, and Fe: the balance. The atomic ratio (R1 / Rt) of the total amount of Ce and La (R1) to the total amount of rare earth elements Rt (Nd+Ce+La): 13.4 at% was 0.37.

[0075] Magnetic properties The magnetic properties of each magnet powder were measured at room temperature using a pulse BH tracer (manufactured by OP Electronics Co., Ltd.). The results are summarized in Figure 1D. The squareness (Hk) shown in Figure 1D is an index of the resistance of magnet particles to reverse magnetic fields, and is the magnitude of the reverse magnetic field that reduces the residual magnetic flux density (Br), an index of magnetization potential, by 10%.

[0076] "evaluation" As is clear from Fig. 1D, when the texture control step was performed, the magnetic properties (especially Hk) of the magnet powder were significantly improved depending on the treatment time. The results of this example made it clear that the texture control step contributes to improving the magnetic properties.

[0077] [Second Example] (1) Based on the results of the first embodiment, Samples 21 and 22 were also prepared by performing the texture control process as part of the recombination process (forced evacuation process). The chart of each process and d-HDDR is shown in Figure 2A, and the magnetic properties of each sample are shown in Figure 2B. For comparison, the magnetic properties of Sample 10 described above are also shown in Figure 2B.

[0078] (2) As is clear from FIG. 2B, Sample 22, in which the structure control process was superimposed on the forced evacuation process (875°C × 3 hours), exhibited even higher magnetic properties than Sample 13, in which the structure control process (875°C × 3 hours) was carried out independently after the forced evacuation process.

[0079] From the results of this example, it became clear that magnet powder with high magnetic properties can be obtained more efficiently by using part of the recombination process (the forced evacuation process) as a structure control process as well.

[0080] [Third Example] (1) Based on the results of the second embodiment, Samples 31 and 32 were also fabricated in which the texture control process was superimposed on the entire recombination process, part of the controlled evacuation process (last 3 hours), and the forced evacuation process. Except for the d-HDDR, each process was the same as in the second embodiment (see FIG. 2A). The chart of the d-HDDR according to this embodiment is shown in FIG. 3A, and the magnetic properties of each sample are summarized in FIG. 3B. For comparison, the magnetic properties of Sample 10 described above are also shown in FIG. 3B.

[0081] (2) As is clear from Fig. 3B, all of the samples exhibited higher magnetic properties than Sample 13, which did not undergo the structure control step. A comparison of Samples 31, 32, and the aforementioned Sample 22 also reveals that magnet powder with higher magnetic properties can be obtained by incorporating the structure control step midway through the controlled evacuation step or after completion of the controlled evacuation step.

[0082] [supplement] (1) Structure control process Sample 41 was also produced by changing the atmosphere in the texture control process from a vacuum atmosphere to a hydrogen atmosphere (2.5 kPa x 875°C x 2.5 hours) for sample 13. After the treatment, the treatment furnace was evacuated (10 -2 Pa x 875℃ x 0.5 hours).

[0083] The magnetic properties of sample 41 were (BH)max: 33.0 MGOe, Br: 12.2 kG, iHc: 14.7 kOe, and Hk: 7.3 kOe. Compared with sample 10, which was not subjected to the structure control process, it was confirmed that the magnetic properties of sample 41, which was subjected to the structure control process in a hydrogen atmosphere, were also sufficiently improved.

[0084] (2) Diffusion treatment process Sample 42 was also produced by performing the diffusion treatment process at a lower temperature and for a shorter time (800℃ x 1 hour) in the same vacuum atmosphere as sample 31. The magnetic properties of sample 42 were (BH)max: 34.0MGOe, Br: 12.4kG, iHc: 13.6kOe, and Hk: 6.7kOe.

[0085] Compared to Sample 10, the magnetic properties were improved by carrying out the structure control step, even when the diffusion treatment step was carried out at a low temperature and for a short time. Also, a comparison between Sample 31 and Sample 42 revealed that the magnetic properties were improved more when the diffusion treatment step was carried out at, for example, 840 to 900°C or 850 to 890°C for 1 to 5 hours or 2 to 4 hours.

[0086] From the above, it was confirmed that according to the present invention, the magnetic properties can be further improved even with rare earth magnet powder containing Ce in addition to Nd.

Claims

1. a disproportionation step of causing a magnet raw material containing rare earth elements including at least Nd and Ce, transition elements, and B to absorb hydrogen to cause a disproportionation reaction; a recombination step of dehydrogenating the magnet raw material after the disproportionation step to cause a recombination reaction, The method for producing rare earth magnet powder further includes, after the recombination step, a structure control step of heating the magnet raw material at 850 to 900°C.

2. 2. The method for producing rare earth magnet powder according to claim 1, wherein at least a part of the recombination step also serves as the structure control step.

3. The recombination step includes transitioning the treatment atmosphere of the magnet raw materials from a low temperature range to a high temperature range in at least two stages, 3. The method for producing rare earth magnet powder according to claim 2, wherein at least a part of the high temperature region also serves as the structure controlling step.

4. the recombination step includes a controlled evacuation step of controlling a processing atmosphere of the magnet raw material to a predetermined hydrogen pressure, and a forced evacuation step of making the processing atmosphere a vacuum atmosphere after the controlled evacuation step, 4. The method for producing rare earth magnet powder according to claim 2, wherein the start time of the structure control step is set to be midway through or after the controlled evacuation step.

5. 2. The method for producing rare earth magnet powder according to claim 1, wherein the structure control step is carried out for 0.25 to 8 hours.

6. 2. The method for producing rare earth magnet powder according to claim 1, further comprising a diffusion treatment step of heating the mixed raw material of the magnet raw material and the diffusion raw material after the recombination step and the structure control step.

7. 7. The method for producing rare earth magnet powder according to claim 1, wherein the atomic ratio of Ce to the total amount of the rare earth elements (Rt) (Ce / Rt) is 0.2 to 0.

6.

8. The rare earth element further includes La, 7. The method for producing rare earth magnet powder according to claim 1, wherein the atomic ratio (R1 / Rt) of the total amount of Ce and La (R1) to the total amount of the rare earth elements (Rt) is 0.2 to 0.6.

Citation Information

Patent Citations

  • Rare-earth magnet powder and method of producing the same

    JP2016115774A