Nitride semiconductor light-emitting element
The nitride semiconductor light emitting device achieves extended service life through a layered structure with a thin first electron blocking layer and silicon interface, enhancing electron injection and suppressing diffusion, thereby maintaining high optical output.
Patent Information
- Application Number
- JP2023045022
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
The configuration of existing nitride semiconductor light emitting devices, as described in Patent Document 1, does not adequately address the issue of extending their service life.
The device incorporates an n-type semiconductor layer with specific Al, Ga, and N composition, an active layer with varying Al composition well and barrier layers, and an electron blocking layer composed of multiple undoped semiconductor layers, particularly with a thin first electron blocking layer less than 2 nm, and includes silicon at the interface with the p-type semiconductor layer to suppress diffusion and dislocation propagation.
This configuration significantly extends the service life of the nitride semiconductor light emitting device by maintaining high optical output over extended periods.
Smart Images

Figure 2024134693000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nitride semiconductor light emitting device. [Background technology]
[0002] Patent Document 1 discloses a nitride semiconductor light-emitting element in which an n-side layer, an active layer, an electron block structure layer, and a p-side layer are stacked. The electron block structure layer includes, from the active layer side, a first electron block layer, an intermediate layer, and a second electron block layer. The first electron block layer has a band gap larger than that of the barrier layer. The second electron block layer has a band gap larger than that of the barrier layer and smaller than that of the first electron block layer. The intermediate layer has a band gap smaller than that of the second electron block layer. Patent Document 1 also describes that a longer life can be achieved by configuring the electron block structure layer as described above. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 057149 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the configuration of the nitride semiconductor light-emitting device described in Patent Document 1 leaves room for improvement in terms of extending the lifespan.
[0005] The present invention has been made in view of the above circumstances, and has an object to provide a nitride semiconductor light-emitting device that can achieve a long life. [Means for solving the problem]
[0006] In order to achieve the above-mentioned object, the present invention provides a nitride semiconductor light-emitting device comprising: an n-type semiconductor layer containing Al, Ga, and N; an active layer formed on one side of the n-type semiconductor layer, the active layer having a well layer containing Al, Ga, and N and a barrier layer containing Al, Ga, and N and having a higher Al composition ratio than the well layer; an electron block layer formed on the side of the active layer opposite to the n-type semiconductor layer and containing Al and N; and a p-type semiconductor layer formed on the electron block layer opposite to the active layer, the electron block layer being made of a plurality of undoped semiconductor layers, a first electron block layer located closest to the active layer among the plurality of semiconductor layers constituting the electron block layer has a higher Al composition ratio than the other semiconductor layers and the barrier layer constituting the electron block layer, and the first electron block layer has a film thickness of less than 2 nm. Effect of the Invention
[0007] According to the present invention, it is possible to provide a nitride semiconductor light emitting device that can achieve a longer life. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic diagram illustrating a configuration of a nitride semiconductor light emitting device according to an embodiment. [Diagram 2] 4 is a graph showing a silicon concentration distribution in the vicinity of the interface between an electron blocking layer and a p-type semiconductor layer of a nitride semiconductor light emitting device according to an embodiment. [Diagram 3] 1 is a graph showing the relationship between power-on time and light output maintenance rate in Experimental Example 1. [Figure 4] 13 is a graph showing the relationship between the film thickness of a first electron blocking layer and the light output maintenance ratio in Experimental Example 2. [Diagram 5] 13 is a graph showing the relationship between the film thickness of the first electron blocking layer and the initial light output in Experimental Example 2. [Figure 6] 13 is a graph showing the relationship between the film thickness of the p-type contact layer and the light output maintenance ratio in Experimental Example 3. [Figure 7]13 is a graph showing the relationship between the thickness of a p-type contact layer and the initial light output in Experimental Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Embodiment Mode] An embodiment of the present invention will be described with reference to Figures 1 and 2. Note that the embodiment described below is shown as a preferred specific example for carrying out the present invention, and while there are some parts that specifically exemplify various technical matters that are technically preferable, the technical scope of the present invention is not limited to this specific embodiment.
[0010] (Nitride semiconductor light emitting device 1) FIG. 1 is a schematic diagram showing the configuration of a nitride semiconductor light-emitting element 1. In FIG. 1, the dimensional ratio of each layer in the stacking direction of the nitride semiconductor light-emitting element 1 (hereinafter also simply referred to as "light-emitting element 1") does not necessarily match the actual one. Hereinafter, the stacking direction of each layer of the light-emitting element 1 is referred to as the up-down direction. Also, one side in the up-down direction, that is, the side on which each semiconductor layer of the substrate 2 is grown (e.g., the upper side in FIG. 1) is referred to as the upper side, and the opposite side (e.g., the lower side in FIG. 1) is referred to as the lower side. Note that the expressions up and down are for convenience and do not limit the attitude of the light-emitting element 1 with respect to the vertical direction, for example, when the light-emitting element 1 is used.
[0011] The light-emitting element 1 is, for example, a light-emitting diode (LED) or a semiconductor laser (LD). In this embodiment, the light-emitting element 1 is a light-emitting diode that emits light with a wavelength in the ultraviolet region. In particular, the light-emitting element 1 in this embodiment emits ultraviolet light with a central wavelength of 250 nm or more and 365 nm or less. The light-emitting element 1 can be used in the fields of, for example, sterilization (e.g., air purification, water purification, etc.), medicine (e.g., phototherapy, measurement and analysis, etc.), UV curing, etc.
[0012] The light-emitting element 1 includes a buffer layer 3, an n-type cladding layer 4, a compositionally graded layer 5, an active layer 6, an electron blocking layer 7, and a p-type semiconductor layer 8, which are arranged in this order on a substrate 2. The light-emitting element 1 also includes an n-side electrode 11 provided on the n-type cladding layer 4, and a p-side electrode 12 provided on the p-type semiconductor layer 8.
[0013] The semiconductor constituting the light emitting element 1 is, for example, Al. a Ga b In 1-a-b In this embodiment, the semiconductor constituting the light emitting element 1 can be Al. c Ga 1-c The semiconductor material uses a binary or ternary group III nitride semiconductor represented by N (0≦c≦1). Some of these group III elements may be replaced with boron (B), thallium (Tl), etc. Also, some of the nitrogen may be replaced with phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc.
[0014] The substrate 2 is made of a material that transmits the light emitted by the active layer 6. The substrate 2 is made of, for example, sapphire (Al 2 O 3 ) substrate. The upper surface of the substrate 2 (i.e., the surface on which the semiconductor layers of the light-emitting element 1 are laminated) is a c-plane. This c-plane may have an off-axis angle. Furthermore, the substrate 2 may be, for example, an aluminum nitride (AlN) substrate or an aluminum gallium nitride (AlGaN) substrate.
[0015] The buffer layer 3 is formed on the substrate 2. In this embodiment, the buffer layer 3 is made of aluminum nitride. When the substrate 2 is an aluminum nitride substrate or an aluminum gallium nitride substrate, the buffer layer 3 is not necessarily provided. The buffer layer 3 may be an undoped Al gallium nitride substrate formed on a semiconductor layer made of aluminum nitride. p Ga 1-p The semiconductor layer may include a semiconductor layer consisting of N (0≦p≦1).
[0016] The n-type cladding layer 4 is an n-type semiconductor layer formed on the buffer layer 3. The n-type cladding layer 4 is, for example, Al doped with n-type impurities. q Ga 1-q N (0≦q≦1). In this embodiment, silicon (Si) is used as the n-type impurity. Note that germanium (Ge), selenium (Se), tellurium (Te), or the like may also be used as the n-type impurity. The Al composition ratio q of the n-type cladding layer 4 is preferably, for example, 20% or more, and more preferably, 25% or more and 70% or less. Note that the Al composition ratio is also called AlN mole fraction. The film thickness of the n-type cladding layer 4 may be, for example, 1 μm or more and 4 μm or less. In this embodiment, the n-type cladding layer 4 has a single-layer structure, but may have a multi-layer structure.
[0017] The compositionally graded layer 5 is formed on the n-type cladding layer 4. The compositionally graded layer 5 is made of silicon-doped Al r Ga 1-r N (0≦r≦1). The Al composition ratio at each position in the vertical direction of the composition gradient layer 5 increases toward the active layer 6. Note that the composition gradient layer 5 may include a region in which the Al composition ratio does not increase toward the active layer 6, for example, in a very small region in the vertical direction (for example, a region of 5% or less of the entire vertical direction of the composition gradient layer 5).
[0018] The Al composition ratio of the composition gradient layer 5 at its end on the n-type cladding layer 4 side is preferably approximately the same (e.g., within a difference of 5%) as the Al composition ratio of the end on the composition gradient layer 5 side of the n-type cladding layer 4. Also, the Al composition ratio of the composition gradient layer 5 at its end on the active layer 6 side is preferably approximately the same (e.g., within a difference of 5%) as the Al composition ratio of the end on the composition gradient layer 5 side of the active layer 6. The film thickness of the composition gradient layer 5 can be, for example, 5 nm or more and 50 nm or less.
[0019] The active layer 6 is formed on the composition gradient layer 5. The active layer 6 has a multiple quantum well structure having a plurality of well layers 621 to 623. The band gap of the active layer 6 is adjusted so that it can emit ultraviolet light having a center wavelength of 250 nm or more and 365 nm or less.
[0020] In this embodiment, the active layer 6 has three barrier layers 61 and three well layers 621 to 623, and the barrier layers 61 and the well layers 621 to 623 are alternately laminated. In the active layer 6, the barrier layer 61 is located at the end on the side of the composition gradient layer 5, and the well layer 623 is located at the end on the side of the electron blocking layer 7. Note that the number of the barrier layers 61 and the number of the well layers 621 to 623 in the active layer 6 are not particularly limited.
[0021] Each barrier layer 61 is formed of Al s Ga 1-s N (0 < s < 1). The Al composition ratio s of each barrier layer 61 is, for example, 60% or more and 100% or less. Also, the film thickness of each barrier layer 61 is, for example, 2 nm or more and 50 nm or less.
[0022] The well layers 621 to 623 are formed of Al t Ga 1-t N (0 < t < 1). The Al composition ratio t of each of the well layers 621 to 623 is smaller than the Al composition ratio s of the barrier layer 61 (that is, t < s).
[0023] In this embodiment, the three well layers 621 to 623 are referred to as the first well layer 621, the second well layer 622, and the third well layer 623 in order from the side of the composition gradient layer 5. The film thickness of the first well layer 621 is 1 nm or more greater than the film thickness of each of the second well layer 622 and the third well layer 623. Thereby, each layer of the active layer 6 is planarized, and the monochromaticity of the output light is improved. The difference between the film thickness of the first well layer 621 and the film thickness of each of the second well layer 622 and the third well layer 623 is preferably 2 nm or more and 4 nm or less. Each of the second well layer 622 and the third well layer 623 has a film thickness of 2 nm or more and 4 nm or less, and the first well layer 621 has a film thickness of 4 nm or more and 6 nm or less.
[0024] Moreover, the Al composition ratio of the first well layer 621 is 2% or more higher than the Al composition ratios of the second well layer 622 and the third well layer 623. By making the Al composition ratio of the first well layer 621 higher than the Al composition ratios of the second well layer 622 and the third well layer 623, the crystallinity of the first well layer 621 is improved. This is because the difference in the Al composition ratio between the first well layer 621 and the n-type cladding layer 4 is reduced. By improving the crystallinity of the first well layer 621, the crystallinity of each semiconductor layer formed on the first well layer 621 in the active layer 6 is also improved. This improves the mobility of carriers in the active layer 6 and improves the optical output. This effect is more remarkable as the film thickness of the first well layer 621 increases, but from the viewpoint of suppressing an increase in the electrical resistance value of the entire light-emitting element 1, the film thickness of the first well layer 621 is designed to be equal to or less than a predetermined value.
[0025] In this embodiment, the second well layer 622 and the third well layer 623 each have an Al composition ratio of 25% or more and 45% or less, and the first well layer 621 has an Al composition ratio of 35% or more and 55% or less. The multiple well layers 621-623 may be configured such that the Al composition ratio increases toward the composition gradient layer 5 side, for example.
[0026] The electron blocking layer 7 is formed on the active layer 6. The electron blocking layer 7 has a role of improving the efficiency of electron injection into the active layer 6 by suppressing the occurrence of an overflow phenomenon in which electrons leak from the active layer 6 to the p-type semiconductor layer 8 side (hereinafter, also referred to as the electron blocking effect). In this embodiment, the electron blocking layer 7 is made of undoped Al u Ga 1-u N (0.7≦u≦1). That is, the electron blocking layer 7 is composed of a semiconductor layer with an Al composition ratio u of 70% or more. The electron blocking layer 7 has a layered structure in which a first electron blocking layer 71 and a second electron blocking layer 72 are layered in this order from the active layer 6 side. The electron blocking layer 7 may be formed of three or more layers.
[0027] The first electron blocking layer 71 is provided so as to be in contact with the active layer 6. Of the multiple semiconductor layers (the first electron blocking layer 71 and the second electron blocking layer 72 in this embodiment) constituting the electron blocking layer 7, the first electron blocking layer 71 has a higher Al composition ratio than the other semiconductor layers (i.e., the second electron blocking layer 72) constituting the electron blocking layer 7 and the barrier layer 61. The Al composition ratio of the first electron blocking layer 71 is, for example, 90% or more and may be 100% (i.e., the first electron blocking layer 71 may be made of AlN).
[0028] In this embodiment, the first electron blocking layer 71 is formed extremely thin, with a thickness of less than 2 nm. As shown in Experimental Example 2 described later, the electron blocking layer 7 is composed of a plurality of undoped semiconductor layers, and the thickness of the first electron blocking layer 71 is extremely thin, less than 2 nm, as described above, thereby extending the life of the light-emitting element 1. Furthermore, as shown in Experimental Example 2 described later, from the viewpoint of extending the life of the light-emitting element 1, the thickness of the first electron blocking layer 71 is preferably less than 1.4 nm, 1.0 nm or less, less than 1.0 nm, and 0.8 nm or less, in that order. Furthermore, the thickness of the first electron blocking layer 71 is preferably 0.5 nm or more, from the viewpoint of ensuring initial light output.
[0029] The Al composition ratio of the second electron blocking layer 72 is smaller than that of the first electron blocking layer 71, and is, for example, not less than 70% and not more than 90%. The film thickness of the second electron blocking layer 72 is larger than that of the first electron blocking layer 71. If the film thickness of the first electron blocking layer 71 is small, the probability that electrons will pass through the first electron blocking layer 71 from the active layer 6 side to the p-type semiconductor layer 8 side due to the tunnel effect may increase, but the provision of the second electron blocking layer 72 can reduce this probability.
[0030] The total thickness of the electron blocking layer 7 is preferably less than 70 nm. Since an increase in the thickness of a semiconductor layer having a relatively large Al composition ratio, such as the electron blocking layer 7, increases the electrical resistance of the light-emitting element 1, the thickness of the electron blocking layer 7 is preferably less than 70 nm.
[0031] Silicon is contained between the electron blocking layer 7 and the p-type semiconductor layer 8. Magnesium is easily attracted to silicon, and hydrogen is easily bonded to magnesium. The presence of silicon between the electron blocking layer 7 and the p-type semiconductor layer 8 suppresses the diffusion of magnesium and hydrogen from the p-type semiconductor layer 8 to the active layer 6, thereby extending the life of the light-emitting element 1. Furthermore, the presence of silicon between the electron blocking layer 7 and the p-type semiconductor layer 8 may form a layer having pits (for example, so-called V pits) between the electron blocking layer 7 and the p-type semiconductor layer 8. The pits are formed by supplying a silicon source to a location where dislocations exist, and therefore the formation of the pits suppresses the dislocations from progressing upward beyond the pits, thereby extending the life of the light-emitting element 1.
[0032] FIG. 2 is a diagram showing the silicon concentration distribution in the vertical direction of the light-emitting element 1 obtained by secondary ion mass spectrometry (SIMS). The depth on the horizontal axis in FIG. 2 represents the vertical distance from the surface of the p-type semiconductor layer 8 on the p-side electrode 12 side. When silicon is contained between the electron block layer 7 and the p-type semiconductor layer 8, when the silicon concentration distribution in the vertical direction of the light-emitting element 1 (hereinafter simply referred to as "silicon concentration distribution") is observed by secondary ion mass spectrometry, a silicon concentration peak P appears between the electron block layer 7 and the p-type semiconductor layer 8. Even if the electron block layer 7 is undoped, when the silicon concentration distribution is observed, the bottom part of the peak P appears at the end of the electron block layer 7 on the p-type semiconductor layer 8 side, making it appear as if silicon is contained, but this is a problem in SIMS measurement. Therefore, when silicon is contained in the interface between the electron block layer 7 and the semiconductor layer adjacent thereto, in the silicon concentration distribution obtained by SIMS measurement, in the region of the electron block layer 7 excluding the range in which the peak P appears near the aforementioned interface (for example, the range from the interface position between the p-type semiconductor layer and the second electron block layer to a position at a depth of about 50 nm), the silicon concentration is at the background level (for example, the silicon concentration is 5.0×10 17 atoms / cm 3hereinafter), the electron blocking layer 7 can be said to be undoped.
[0033] The p-type semiconductor layer 8 is formed on the electron blocking layer 7. The p-type semiconductor layer 8 is made of p-type Al v Ga 1-v N (0≦v<0.7). That is, the p-type semiconductor layer 8 is composed of a semiconductor layer with an Al composition ratio of less than 70%.
[0034] The p-type semiconductor layer 8 has a p-type contact layer. The p-type contact layer is a layer to which a p-side electrode 12 is connected, and is made of Al v Ga 1-v N (0≦v<0.7). The p-type contact layer is configured to have a low Al composition ratio in order to realize ohmic contact with the p-side electrode 12, and from this viewpoint, it is preferable to form it from p-type gallium nitride (GaN). Since a semiconductor layer made of p-type gallium nitride is prone to absorbing ultraviolet light, from the viewpoint of preventing absorption of ultraviolet light and improving the optical output of the light-emitting element 1, the thickness of the p-type contact layer is preferably 25 nm or less. Furthermore, as shown in Experimental Example 3 described later, from the viewpoint of extending the life of the light-emitting element 1, the thickness of the p-type contact layer is preferably 25 nm or less, and more preferably 18 nm or less. Furthermore, from the viewpoint of suppressing the occurrence of short circuits, the thickness of the p-type contact layer is preferably 5 nm or more.
[0035] The p-type semiconductor layer 8 may further include a p-type cladding layer on the electron block layer 7 side of the p-type contact layer. The p-type cladding layer is made of p-type AlGaN with an Al composition ratio of less than 70%. The p-type cladding layer may be, for example, a single layer or multiple layers. When the p-type cladding layer is made of multiple layers, for example, the p-type cladding layer may have a first p-type cladding layer formed on the second electron block layer 72 side and a second p-type cladding layer formed between the first p-type cladding layer and the p-type contact layer. The Al composition ratio at each position in the vertical direction of the second p-type cladding layer may be smaller toward the p-type contact layer side. Note that the second p-type cladding layer may include a region in which the Al composition ratio does not increase toward the p-type contact layer, for example, in a very small region in the vertical direction (for example, a region of 5% or less of the entire vertical direction of the second p-type cladding layer). The second p-type cladding layer preferably has an Al composition ratio at its end on the first p-type cladding layer side that is substantially the same (e.g., within a difference of 5%) as the Al composition ratio at the end of the first p-type cladding layer on the second p-type cladding layer side. Also, the second p-type cladding layer preferably has an Al composition ratio at its end on the p-type contact layer side that is substantially the same (e.g., within a difference of 5%) as the Al composition ratio at the end of the p-type contact layer on the second p-type cladding layer side.
[0036] In the light-emitting element 1, the total optical film thickness of the semiconductor layers (i.e., the electron blocking layer 7 and the p-type semiconductor layer 8) present above the active layer 6 is preferably designed to be an optical film thickness that enhances the light emitted upward from the active layer 6, reflected by the p-side electrode 12 and directed downward, and the light emitted directly downward from the active layer 6. When the central wavelength of the light emitted from the active layer 6 is wavelength λ [nm], for example, the total optical film thickness of the semiconductor layers present above the active layer 6 is preferably 0.5λ or more and 1.4λ or less, more preferably 0.5λ or more and 0.8λ or less, or 1.0λ or more and 1.3λ or less, and even more preferably 0.5λ or more and 0.8λ or less.
[0037] The n-side electrode 11 is formed on an exposed surface 41 that is formed on the upper side of the n-type cladding layer 4 and is exposed from the active layer 6. The n-side electrode 11 may be, for example, a multilayer film in which titanium (Ti), aluminum, titanium, and gold (Au) are laminated in this order on the n-type cladding layer 4. In addition, when the light-emitting element 1 is flip-chip mounted as described later, the n-side electrode 11 may be made of a material that can reflect ultraviolet light emitted by the active layer 6.
[0038] The p-side electrode 12 is formed on the upper surface of the p-type semiconductor layer 8. The p-side electrode 12 may be made of, for example, indium tin oxide (ITO) or the like. When the light-emitting element 1 is flip-chip mounted as described later, the p-side electrode 12 may be made of a material capable of reflecting ultraviolet light emitted by the active layer 6.
[0039] The light emitting element 1 can be used by being flip-chip mounted on a package substrate (not shown). That is, the side of the light emitting element 1 on which the n-side electrode 11 and the p-side electrode 12 are provided in the up-down direction faces the package substrate, and each of the n-side electrode 11 and the p-side electrode 12 is mounted on the package substrate via a gold bump or the like. In the flip-chip mounted light emitting element 1, light is extracted from the substrate 2 side. However, the light emitting element 1 may be mounted on the package substrate by wire bonding or the like. In this embodiment, the light emitting element 1 is a so-called horizontal type light emitting element 1 in which both the n-side electrode 11 and the p-side electrode 12 are provided on the upper side of the light emitting element 1, but the light emitting element 1 may be a vertical type light emitting element 1. The vertical type light emitting element 1 is a light emitting element 1 in which the active layer 6 is sandwiched between the n-side electrode 11 and the p-side electrode 12. When the light emitting element 1 is a vertical type light emitting element, it is preferable to remove the substrate 2 and the buffer layer 3 by laser lift-off or the like.
[0040] (Method of Manufacturing Light-Emitting Element 1) Next, an example of a method for manufacturing the light emitting device 1 of this embodiment will be described. In this embodiment, a buffer layer 3, an n-type cladding layer 4, a compositionally graded layer 5, an active layer 6, an electron blocking layer 7, and a p-type semiconductor layer 8 are epitaxially grown in sequence on a disk-shaped substrate 2 by metal organic chemical vapor deposition (MOCVD). That is, in this embodiment, the disk-shaped substrate 2 is placed in a pocket of a susceptor disposed in a chamber, and the source gases of each semiconductor layer formed on the substrate 2 are introduced into the chamber to form each semiconductor layer on the substrate 2. The MOCVD method is sometimes called metal organic vapor phase epitaxy (MOVPE).
[0041] The source gases for epitaxial growth of each layer were trimethylaluminum (TMA) as the aluminum source, trimethylgallium (TMG) as the gallium source, and ammonia (NH 3 ), tetramethylsilane (TMSi) as a silicon source, and biscyclopentadienylmagnesium (Cp 2 Regarding the manufacturing conditions such as growth temperature, growth pressure, and growth time for epitaxially growing each semiconductor layer of the wafer, conditions according to the configuration of each semiconductor layer can be appropriately adopted.
[0042] When epitaxially growing each semiconductor layer on the substrate 2, other epitaxial growth methods such as molecular beam epitaxy (MBE) and hydride vapor phase epitaxy (HVPE) can also be used.
[0043] After each semiconductor layer is formed on the disk-shaped substrate 2, a mask is formed on a portion of the p-type semiconductor layer 8, i.e., on a portion other than the portion that will become the exposed surface 41 of the n-type cladding layer 4. Then, the region where the mask is not formed is removed by etching from the top surface of the p-type semiconductor layer 8 to the middle of the n-type cladding layer 4 in the vertical direction. As a result, an exposed surface 41 that is exposed upward is formed in the n-type cladding layer 4. After the exposed surface 41 is formed, the mask is removed.
[0044] Next, an n-side electrode 11 is formed on the exposed surface 41 of the n-type cladding layer 4, and a p-side electrode 12 is formed on the p-type semiconductor layer 8. The n-side electrode 11 and the p-side electrode 12 may be formed by a well-known method such as an electron beam deposition method or a sputtering method. The above-completed product is cut into pieces of desired dimensions, and a plurality of light-emitting elements 1 as shown in FIG. 1 are manufactured from one wafer.
[0045] (Functions and Effects of the Embodiments) In the light-emitting device 1 of this embodiment, the electron blocking layer 7 is composed of a plurality of undoped semiconductor layers. Among the plurality of semiconductor layers constituting the electron blocking layer 7, the first electron blocking layer 71 located closest to the active layer has a higher Al composition ratio than the other semiconductor layers constituting the electron blocking layer 7 (i.e., the second electron blocking layer 72 in this embodiment) and the barrier layer 61. The film thickness of the first electron blocking layer is less than 2 nm. This can extend the life of the light-emitting device 1, as shown in Experimental Example 2 described later. Furthermore, as shown in Experimental Example 2 described later, by further satisfying the requirement that the film thickness of the first electron blocking layer 71 be less than 1.4 nm, the life of the light-emitting device 1 can be further extended.
[0046] Moreover, the p-type semiconductor layer 8 has a p-type contact layer made of p-type gallium nitride (GaN), and the thickness of the p-type contact layer is 25 nm or less. Therefore, as shown in Experimental Example 3 described later, it is possible to extend the life of the light-emitting element 1. Furthermore, as shown in Experimental Example 3 described later, by setting the thickness of the p-type contact layer to 18 nm or less, it is possible to further extend the life of the light-emitting element 1.
[0047] In addition, silicon is contained at the interface between the electron blocking layer 7 and the p-type semiconductor layer 8. Here, magnesium is easily attracted to silicon, and hydrogen is easily bonded to magnesium. The presence of silicon between the electron blocking layer 7 and the p-type semiconductor layer 8 suppresses the diffusion of magnesium and hydrogen from the p-type semiconductor layer 8 to the active layer 6, thereby extending the life of the light-emitting element 1. Furthermore, the presence of silicon between the electron blocking layer 7 and the p-type semiconductor layer 8 may form a layer having pits between the electron blocking layer 7 and the p-type semiconductor layer 8. The pits are formed by supplying a silicon source to a location where dislocations exist, and therefore the formation of the pits suppresses the dislocations from progressing upward beyond the pits, thereby extending the life of the light-emitting element 1.
[0048] As described above, according to this embodiment, it is possible to provide a nitride semiconductor light emitting device that can achieve a longer life.
[0049] [Experimental Example 1] This Experimental Example 1 is an example in which the change in light output maintenance rate over time was evaluated for two light emitting elements that have the same basic structure as the light emitting element described in the embodiment, but have different film thicknesses of the first electron blocking layer. The light output maintenance rate is the ratio of the light output of the light emitting element after a current is applied for an arbitrary time to the initial light output of the light emitting element. Among the terms used in this Experimental Example 1 and subsequent examples, those that are the same as those used in the above-mentioned embodiments have the same meanings as those in the above-mentioned embodiments, unless otherwise specified.
[0050] In this experimental example 1, Example A1, which is a light-emitting device in which the thickness of the first electron blocking layer is 0.8 nm, and Example A2, which is a light-emitting device in which the thickness of the first electron blocking layer is 1.6 nm, were prepared. That is, both Examples A1 and A2 satisfy the requirement that the thickness of the first electron blocking layer is less than 2 nm, similar to the embodiment. Each of Examples A1 and A2 is a packaged light-emitting device. The structure, thickness of each layer, Al composition ratio of each layer, and silicon concentration of each layer of Examples A1 and A2 are shown in Table 1 below.
[0051] [Table 1]
[0052] The thickness of each layer listed in Table 1 was measured by a transmission electron microscope (TEM), except for the thickness of the first electron block layer. The thickness of the first electron block layer listed in Table 1 will be described later. The Al composition ratio of each layer listed in Table 1 is a value estimated from the secondary ion intensity of Al measured by secondary ion mass spectrometry. The column of Al composition ratio of the composition gradient layer in Table 1 indicates that the Al composition ratio at each position in the vertical direction of the composition gradient layer varies from 55% to 85% from the n-type cladding layer side to the active layer side. Similarly, the column of Al composition ratio of the second p-type cladding layer in Table 1 indicates that the Al composition ratio at each position in the vertical direction of the second p-type cladding layer varies from 55% to 0% from the first p-type cladding layer side to the p-type contact layer side. The silicon concentration of each layer listed in Table 1 was obtained by using secondary ion mass spectrometry. In each of Table 1, the portion marked with "*" in the column of Si concentration indicates that the semiconductor layer is thin and it is difficult to accurately measure the silicon concentration. In addition, in the column of the Si concentration in Table 1, the notation "BG" means the background level. The background level silicon concentration is the silicon concentration detected when silicon is not doped, specifically, 5.0 × 10 17 atoms / cm 3 The silicon concentration is:
[0053] Then, for each of Examples A1 and A2, a current of 500 mA was continued to flow for a cumulative total of more than 1000 hours, and the light output maintenance rate was evaluated at multiple points in time. The results are shown in FIG.
[0054] As can be seen from Fig. 3, in both Examples A1 and A2, the light output maintenance rate after 1000 hours of current application exceeds 70%. Generally, a light-emitting element is required to have a light output maintenance rate of 70% or more after 1000 hours of current application, and it is found that Examples A1 and A2, in which the film thickness of the first electron blocking layer is less than 2 nm, satisfy this requirement.
[0055] Also, from FIG. 3, it can be seen that Example A1, in which the thickness of the first electron blocking layer is relatively small, has a longer life than Example A2, in which the thickness of the first electron blocking layer is relatively large.
[0056] In both Examples A1 and A2, the light output maintenance ratio drops significantly until the current application time reaches 100 hours, but the drop in the light output maintenance ratio thereafter becomes gradual. Even in Example A2, where the difference between the light output maintenance ratio at 100 hours of current application and the light output maintenance ratio at 1000 hours of current application is relatively large, the difference was about 10%. Therefore, in a light-emitting element in which the film thickness of the first electron blocking layer is less than 2 nm, if the light output maintenance ratio at 100 hours of current application exceeds 80%, the light output maintenance ratio at 1000 hours of current application is expected to exceed 70%. Based on this, in the next Experimental Example 2, the relationship between the film thickness of the first electron blocking layer and the maintenance ratio at 100 hours of current application of the light-emitting element was evaluated.
[0057] [Experimental Example 2] The present experimental example 2 is an example in which the relationship between the film thickness of the first electron blocking layer and the light output maintenance rate at the time of applying current for 100 hours was evaluated for a light emitting device having the same basic configuration as the embodiment.
[0058] In this experimental example 2, Examples B1 to B10, which are light-emitting devices having a first electron blocking layer with a thickness of 1.6 nm, Examples B11 and B12, which are light-emitting devices having a first electron blocking layer with a thickness of 1.2 nm, Examples B13 and B14, which are light-emitting devices having a first electron blocking layer with a thickness of 1.0 nm, and Examples B15 to B18, which are light-emitting devices having a first electron blocking layer with a thickness of 0.8 nm, were prepared. Examples B1 to B18 are packaged light-emitting devices. The structure, thickness of each layer, Al composition ratio of each layer, and silicon concentration of each layer of Examples B1 to B18 are the same as those shown in Table 1 of Example 1, except for the thickness of the first electron blocking layer.
[0059] For each example, first, a current of 350 mA was applied to measure the initial light output. Then, for each example, a current of 500 mA was applied continuously for 100 hours to cause light emission. After that, for each example, a current of 350 mA was applied to measure the light output after 100 hours of application, and the light output maintenance rate was calculated.
[0060] The film thickness, initial light output, and maintenance rate of the first electron blocking layer of each Example are shown in Table 2. The relationship between the film thickness of the first electron blocking layer and the light output maintenance rate of each Example is shown in FIG. 4, and the relationship between the film thickness of the first electron blocking layer and the initial light output is shown in FIG. 5. Here, the light output maintenance rate of each Example shown in Table 2 and FIG. 4 is the average value of the light output maintenance rate obtained using 10 packaged light-emitting elements created from one wafer. Similarly, the initial light output of each Example shown in Table 2 and FIG. 5 is the average value of the light output maintenance rate measured using 10 light-emitting elements.
[0061] [Table 2]
[0062] 4, in all of Examples B1 to B18 in which the thickness of the first electron blocking layer is less than 2 nm, the light output maintenance rate after 100 hours of current application is 85% or more, and a high light output maintenance rate is obtained. As described in Experimental Example 1, in light-emitting devices in which the thickness of the first electron blocking layer is less than 2 nm, it is preferable that the light output maintenance rate after 100 hours of current application exceeds 80%, and this is fully satisfied in Examples B1 to B18.
[0063] Furthermore, as can be seen from Table 2 and FIG. 4, in terms of obtaining a high light output maintenance ratio, the thickness of the first electron blocking layer is preferably less than 1.4 nm, 1.0 nm or less, less than 1.0 nm, and 0.8 nm or less, in that order.
[0064] Furthermore, as can be seen from Table 2 and FIG. 5, good initial light output was obtained in all of Examples B1 to B18 in which the film thickness of the first electron blocking layer was less than 2 nm.
[0065] [Experimental Example 3] The present experimental example 3 is an example in which a relationship between the thickness of the p-type contact layer and the light output maintenance rate after 100 hours of current application was evaluated for a light emitting device having the same basic configuration as the embodiment.
[0066] In this Experimental Example 3, five light-emitting elements, each having a different thickness of the p-type contact layer, were prepared as Examples C1 to C5. Examples C1 to C5 are packaged light-emitting elements. The structures, thicknesses of each layer, Al composition ratios of each layer, and silicon concentrations of each layer of Examples C1 to C5 are the same as those shown in Table 1 of Example 1, except for the thickness of the p-type contact layer. In each of Examples C1 to C5, the thickness of the first electron blocking layer was uniformly set to 1.6 nm.
[0067] For each example, the light output maintenance rate was calculated in the same manner as in Experimental Example 2. That is, for each example, first, a current of 350 mA was applied to measure the initial light output. Then, for each example, a current of 500 mA was applied continuously for 100 hours to cause light emission. After that, for each example, a current of 350 mA was applied to measure the light output after 100 hours of application, and the light output maintenance rate was calculated.
[0068] The thickness of the p-type contact layer, the initial light output, and the light output maintenance rate of each example are shown in Table 3. The relationship between the thickness of the p-type contact layer and the light output maintenance rate of each example is shown in FIG. 6. The relationship between the thickness of the p-type contact layer and the initial light output is shown in FIG. 7.
[0069] [Table 3]
[0070] 6, in all of Examples C1 to C5 in which the thickness of the p-type contact layer is 25 nm or less, the light output maintenance rate after 100 hours of power supply is 85% or more, and a high light output maintenance rate is obtained. As described in Experimental Example 1, in a light-emitting device in which the thickness of the first electron blocking layer is less than 2 nm, it is preferable that the light output maintenance rate after 100 hours of power supply exceeds 80%, and Examples C1 to C5 fully satisfy this.
[0071] Furthermore, as can be seen from Table 3 and FIG. 6, in order to obtain a high light output maintenance ratio, the thickness of the p-type contact layer is preferably 18 nm or less, and more preferably 15 nm or less.
[0072] Furthermore, as can be seen from Table 3 and FIG. 7, from the viewpoint of improving the initial light output, the thickness of the p-type contact layer is preferably 18 nm or less, and more preferably 5 nm or more and 15 nm or less.
[0073] (Summary of the embodiment) Next, the technical ideas grasped from the above-described embodiment will be described by using the reference numerals and the like in the embodiment. However, the reference numerals and the like in the following description do not limit the components in the claims to the members and the like specifically shown in the embodiment.
[0074] [1] A first embodiment of the present invention is a nitride semiconductor light-emitting element 1 comprising: an n-type semiconductor layer 4 containing Al, Ga, and N; an active layer 6 formed on one side of the n-type semiconductor layer 4, the active layer 6 having well layers 621-623 containing Al, Ga, and N and a barrier layer 61 containing Al, Ga, and N and having a higher Al composition ratio than the well layers 621-623; an electron block layer 7 formed on a side of the active layer 6 opposite to the n-type semiconductor layer 4 and containing Al and N; and a p-type semiconductor layer 8 formed on a side of the electron block layer 7 opposite to the active layer 6, the electron block layer 7 being made of a plurality of undoped semiconductor layers, a first electron block layer 71 located closest to the active layer 6 among the plurality of semiconductor layers constituting the electron block layer 7 has a higher Al composition ratio than the other semiconductor layers and the barrier layer 61 constituting the electron block layer 7, and the film thickness of the first electron block layer 71 is less than 2 nm. This makes it possible to extend the life of the light emitting element 1.
[0075] [2] A second embodiment of the present invention is the first embodiment, wherein the film thickness of the first electron blocking layer 71 is less than 1.4 nm. This makes it possible to extend the life of the light emitting element 1.
[0076] [3] A third embodiment of the present invention is the first or second embodiment, wherein the p-type semiconductor layer 8 has a p-type contact layer formed of p-type GaN, and the thickness of the p-type contact layer is 25 nm or less. This makes it possible to extend the life of the light emitting element 1.
[0077] [4] A fourth embodiment of the present invention is the third embodiment, in which the p-type contact layer has a thickness of 18 nm or less. This makes it possible to extend the life of the light emitting element 1.
[0078] [5] A fifth embodiment of the present invention is any one of the first to fourth embodiments, in which silicon is contained in the interface between the electron blocking layer 7 and the p-type semiconductor layer 8. This makes it possible to extend the life of the light emitting element 1.
[0079] (Additional Note) Although the embodiment of the present invention has been described above, the invention according to the claims is not limited to the above embodiment. It should be noted that not all of the combinations of features described in the embodiment are essential to the means for solving the problems of the invention. The present invention can be modified appropriately without departing from the spirit of the invention. [Explanation of symbols]
[0080] 1...Nitride semiconductor light emitting device 4...n-type cladding layer (n-type semiconductor layer) 6…Active layer 61...Barrier layer 621…First well layer 622…Second well layer 623…Third well layer 7...Electron blocking layer 71…First electron blocking layer 8...p-type semiconductor layer
Claims
1. an n-type semiconductor layer containing Al, Ga, and N; an active layer formed on one side of the n-type semiconductor layer, the active layer having a well layer containing Al, Ga, and N and a barrier layer containing Al, Ga, and N and having a higher Al composition ratio than the well layer; an electron blocking layer containing Al and N, the electron blocking layer being formed on a side of the active layer opposite to the n-type semiconductor layer; a p-type semiconductor layer formed on the side of the electron blocking layer opposite to the active layer side, the electron blocking layer is composed of a plurality of undoped semiconductor layers, a first electron block layer located closest to the active layer among the plurality of semiconductor layers constituting the electron block layer has a higher Al composition ratio than the other semiconductor layers constituting the electron block layer and the barrier layer; The first electron blocking layer has a thickness of less than 2 nm. Nitride semiconductor light emitting device.
2. The first electron blocking layer has a thickness of less than 1.4 nm. The nitride semiconductor light emitting device according to claim 1 .
3. the p-type semiconductor layer has a p-type contact layer formed of p-type GaN, The thickness of the p-type contact layer is 25 nm or less. The nitride semiconductor light emitting device according to claim 1 .
4. The thickness of the p-type contact layer is 18 nm or less. The nitride semiconductor light emitting device according to claim 3 .
5. Silicon is contained at the interface between the electron blocking layer and the p-type semiconductor layer. The nitride semiconductor light emitting device according to claim 1 .
Citation Information
Patent Citations
Group iii nitride semiconductor light emitting element and manufacturing method of the same
JP2016149544A
Group iii nitride semiconductor light-emitting device and manufacturing method thereof
JP2020077874A
Manufacturing method of nitride semiconductor light emitting element
JP2021193726A
Nitride semiconductor light-emitting element and manufacturing method for nitride semiconductor light-emitting element
JP2022003660A
Semiconductor light-emitting element
JP2022163904A