Light emitting diode epitaxial wafer and preparation method thereof
By using periodic alternating growth and H2 processing technology of multiple quantum well layers in the light emitting diode epitaxial sheet, the In distribution of the InGaN layer is optimized, and the wavelength consistency and brightness uniformity in Mini-LED and Micro-LED chips are difficult to achieve. The problem is that luminous efficiency and uniformity are improved, and production costs and time are reduced.
Patent Information
- Application Number
- CN202411097868.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
In Mini-LED and Micro-LED chips, as the chip size decreases, point measurement and sorting becomes more difficult, especially the size of the Micro-LED chip is below 100μm, which makes it difficult to achieve wavelength consistency and brightness uniformity. Due to the unevenness of In distribution in the InGaN layer.
During the preparation of the light emitting diode epitaxial sheet, a periodic alternating growth method of multiple quantum well layers is adopted, including growing the InGaN layer and performing H2 treatment, followed by growing the InN layer, using H2 to optimize the InGaN layer's In distribution to reduce free states In atoms improve the consistency of the InGaN layer.
The luminous efficiency and wavelength consistency of the light emitting diode are improved, the luminous uniformity is improved, and the cost and time of chip production is reduced.
Smart Images

Figure CN119008790A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof. Background Art
[0002] Mini-LED and Micro-LED have become the development trend of the industry due to their outstanding advantages in the display field. However, with the reduction of chip size, the pressure of post-process testing and sorting has increased dramatically, especially for Micro-LED chips with a size below 100μm. Taking a 4-inch wafer as an example, the point testing and sorting operation takes more than 48 hours. In order to reduce costs and operation time, mass transfer of wafers has been introduced. However, the premise of mass transfer of wafers is that the front-end epitaxial wafer has good intra-wafer consistency. The main influencing factors of wavelength consistency and brightness uniformity are the In distribution in the quantum well layer. During the growth of InGaN, In as a doping element has lattice mismatch and growth stress, so it is difficult to obtain a good In distribution. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a light emitting diode epitaxial wafer and a preparation method thereof, which can improve the light emitting efficiency of the light emitting diode and enhance the wavelength consistency and light emitting uniformity.
[0004] In order to solve the above problems, the present invention discloses a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0005] (1) providing a substrate;
[0006] (2) growing a buffer layer on the substrate;
[0007] (3) growing a non-doped GaN layer on the buffer layer;
[0008] (4) growing an N-type GaN layer on the undoped GaN layer;
[0009] (5) growing a stress release layer on the N-type GaN layer;
[0010] (6) growing a multi-quantum well layer on the stress release layer, wherein the multi-quantum well layer includes a quantum well layer and a quantum barrier layer that are periodically and alternately grown, wherein the growth of the quantum well layer includes:
[0011] (6.1) Using N2 as carrier gas, introduce Ga source, In source and N source to grow InGaN layer;
[0012] (6.2) Turn off the Ga source, In source and N source, and introduce N2 and H2 to treat the InGaN layer;
[0013] (6.3) Using N2 as carrier gas, introduce In source to grow InN layer;
[0014] (7) growing an electron blocking layer on the multi-quantum well layer;
[0015] (8) Growing a P-type GaN layer on the electron blocking layer.
[0016] As an improvement of the above solution, the growth of the quantum well layer further comprises: periodically repeating steps (6.1), (6.2) and (6.3), with the number of repetition cycles being 2 to 6.
[0017] As an improvement of the above solution, in step (6.2), the flow rate of H2 accounts for 1% to 10% of the total flow rate.
[0018] As an improvement of the above solution, the growth temperature of the quantum well layer is 700° C. to 850° C., and the growth pressure is 100 Torr to 300 Torr;
[0019] The growth temperature of the quantum barrier layer is 850° C. to 920° C., and the growth pressure is 100 Torr to 300 Torr.
[0020] As an improvement of the above scheme, in step (6.2), the treatment time of introducing N2 and H2 is 1 min to 10 min.
[0021] As an improvement of the above solution, in step (6.3), the time for introducing the In source to grow the InN layer is 1 min to 10 min.
[0022] As an improvement of the above solution, the In component ratio of the InGaN layer is 0.1-0.3.
[0023] As an improvement of the above solution, the thickness of the InGaN layer is 2nm to 4nm.
[0024] As an improvement of the above solution, the number of periods of the multi-quantum well layer is 6-14.
[0025] Correspondingly, the present invention also discloses a light emitting diode epitaxial wafer, and the light emitting diode epitaxial wafer is prepared by the above-mentioned preparation method.
[0026] The implementation of the present invention has the following beneficial effects:
[0027] The growth of the quantum well layer of the present invention includes growing an InGaN layer, performing H2 treatment on the InGaN layer, and growing an InN layer. When the InGaN layer is treated with H2, the more active H2 will react first and take away defective In atoms, generating N vacancies, and then the InN layer is grown, and In atoms fill the N vacancies, reducing free or weakly bound In, improving the consistency of InGaN growth, and improving the In distribution in InGaN. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention provides a flow chart of the method for preparing a light emitting diode epitaxial wafer. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0030] like Figure 1 As shown, the present invention provides a method for preparing a light-emitting diode epitaxial wafer, comprising the following steps:
[0031] S100, providing a substrate;
[0032] The substrate can be selected from one of sapphire substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate and zinc oxide substrate. In one embodiment, the substrate is selected from sapphire substrate, which is widely used in current LED production and has the advantages of mature preparation process, low price, good chemical stability and thermal stability.
[0033] S200, growing a buffer layer on the substrate;
[0034] The buffer layer may be one or more of an AlN buffer layer, an AlGaN buffer layer, and a GaN buffer layer.
[0035] In one embodiment, the growth of the buffer layer comprises:
[0036] S201, growing an AlN buffer layer by PVD, wherein the thickness of the AlN buffer layer is 10 nm to 30 nm;
[0037] S202, growing a GaN buffer layer on the AlN buffer layer;
[0038] The GaN buffer layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 1000°C to 1200°C, the pressure is 100Torr to 600Torr, and N source and Ga source are introduced. The thickness of the GaN buffer layer is 15nm to 35nm.
[0039] S203, growing a three-dimensional GaN buffer layer on the GaN buffer layer;
[0040] The three-dimensional GaN buffer layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 1000°C to 1200°C, the pressure is 100Torr to 600Torr, and N source and Ga source are introduced. The thickness of the three-dimensional GaN buffer layer is 500nm to 2000nm.
[0041] S300, growing a non-doped GaN layer on the buffer layer;
[0042] The non-doped GaN layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 1000°C to 1200°C, the pressure is 100Torr to 600Torr, and N source and Ga source are introduced. The thickness of the non-doped GaN layer is 800nm to 1200nm.
[0043] S400, growing an N-type GaN layer on the undoped GaN layer;
[0044] The N-type GaN layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 1000℃~1200℃, the pressure is 100Torr~600Torr, and N source, Ga source and N-type doping source are introduced. The thickness of the N-type GaN layer is 1μm~3μm, and the N-type doping concentration is 1×10 19 cm -3 ~1×10 20 cm -3 .
[0045] S500, growing a stress release layer on the N-type GaN layer;
[0046] The InGaN / GaN periodic alternating stacking structure is grown by MOCVD, the temperature of the reaction chamber is controlled to be 800°C to 900°C, the pressure is 100Torr to 600Torr, N source, Ga source and In source are introduced to grow the InGaN layer, N source and Ga source are introduced to grow the GaN layer, and the InGaN layer and the GaN layer are repeatedly stacked to grow periodic InGaN layer and GaN layer. The number of cycles of the stress release layer is 5 to 8, and the thickness is 35nm to 120nm.
[0047] S600, growing a multi-quantum well layer on the stress release layer;
[0048] Using MOCVD growth, control the reaction chamber temperature to 700°C to 850°C, the pressure to 100Torr to 300Torr, and grow a quantum well layer; control the reaction chamber temperature to 850°C to 920°C, the growth pressure to 100Torr to 150Torr, and grow a quantum barrier layer; repeat the periodic growth of quantum well layers and quantum barrier layers. The number of periods of the multi-quantum well layer is 6 to 14, exemplarily 8, 9, 10, 12 or 13, but not limited thereto. In one embodiment, the quantum barrier layer is a GaN quantum barrier layer with a thickness of 8nm to 12nm, exemplarily 8.5nm, 9nm, 10nm, 10.5nm or 11nm, but not limited thereto.
[0049] The growth of the quantum well layer specifically includes:
[0050] S601, using N2 as carrier gas, introducing Ga source, In source and N source to grow an InGaN layer;
[0051] The In component ratio of the InGaN layer is 0.1-0.3, and is exemplarily 0.15, 0.18, 0.2, 0.25 or 0.28, but is not limited thereto. The thickness of the InGaN layer is 2nm-4nm. If the thickness of the InGaN layer is less than 2nm, it is not conducive to the subsequent H2 treatment to form N vacancies, and it is difficult to effectively improve the luminous efficiency; if the thickness of the InGaN layer is greater than 4nm, it will bring too many defects, and is exemplarily 2.5nm, 2.8nm, 3nm, 3.2nm or 3.5nm, but is not limited thereto.
[0052] S602, turning off the Ga source, In source and N source, and introducing N2 and H2 to process the InGaN layer;
[0053] N2 and H2 are continuously introduced for 1 min to 10 min, wherein the flow rate of H2 accounts for 1% to 10% of the total flow rate.
[0054] S603, using N2 as carrier gas, introducing an In source to grow an InN layer.
[0055] Continue to introduce In source for 1 min to 10 min.
[0056] After the InGaN layer is grown, the present invention performs H2 treatment on the InGaN layer. Since H2 is highly active, it will preferentially react with In atoms that are not strongly bound or in a free state and take away these defective In atoms. These defective In atoms only exist as defects and do not participate in luminescence, and will also affect subsequent In doping. Therefore, these defective In atoms are taken away by H2 treatment and N vacancies are generated. Then the InN layer is grown. Since only In source and N2 are introduced into the InN layer, N2 does not participate in the reaction, and the In source will decompose, which is equivalent to only providing In atoms, and In atoms will fill N vacancies, thereby reducing free or weakly bound In atoms, improving the consistency of subsequent InGaN growth, and improving the In distribution in the InGaN layer.
[0057] In one embodiment, the process further includes periodically repeating steps (6.1), (6.2) and (6.3), wherein the number of repetition periods is 2 to 6, and is exemplarily 3, 4 or 5. By arranging the quantum well layer to be a periodically alternately stacked structure, the quantum barrier layer defects are further reduced, thereby further improving the uniformity of the In component distribution.
[0058] S7, growing an electron blocking layer on the multi-quantum well layer;
[0059] MOCVD is used to grow an AlGaN / GaN periodic alternating stacked structure, the reaction chamber temperature is controlled to be 800°C to 900°C, the pressure is 100Torr to 600Torr, N source, Ga source and Al source are introduced to grow an AlGaN layer, N source and Ga source are introduced to grow a GaN layer, and AlGaN layers and GaN layers are repeatedly stacked to grow periodic layers. The number of cycles of the electron blocking layer is 5 to 8, and the thickness is 10nm to 60nm.
[0060] S8. Growing a P-type GaN layer on the electron blocking layer.
[0061] The P-type GaN layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 800℃~980℃, the pressure is 100Torr~600Torr, and N source, Ga source and P-type doping source are introduced. The thickness of the P-type GaN layer is 5nm~100nm, and the P-type doping concentration is 1×10 15 cm -3 ~1×10 18 cm -3 .
[0062] During the MOCVD growth process, the N source may be NH3, the Ga source may be TMGa and / or TEGa, the Al source may be TMAl, the In source may be TMIn, the N-type doping source may be SiH4, and the P-type doping source may be CP2Mg, but are not limited thereto.
[0063] Correspondingly, the present invention also discloses a light emitting diode epitaxial wafer, and the light emitting diode epitaxial wafer is prepared by the above-mentioned preparation method.
[0064] The present invention will be further described below with specific embodiments:
[0065] Example 1
[0066] This embodiment provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0067] S100, providing a substrate;
[0068] The substrate is a sapphire substrate.
[0069] S200, growing a buffer layer on a substrate, including:
[0070] S201, growing an AlN buffer layer by PVD, the thickness of the AlN buffer layer is 20 nm;
[0071] S202, growing a GaN buffer layer on the AlN buffer layer;
[0072] The GaN buffer layer was grown by MOCVD, the temperature of the reaction chamber was controlled to be 1000°C, the pressure was controlled to be 120 Torr, and N source and Ga source were introduced. The thickness of the GaN buffer layer was 20nm.
[0073] S203, growing a three-dimensional GaN buffer layer on the GaN buffer layer;
[0074] The three-dimensional GaN buffer layer was grown by MOCVD, the temperature of the reaction chamber was controlled to be 1050°C, the pressure was 150 Torr, and N source and Ga source were introduced. The thickness of the three-dimensional GaN buffer layer was 1500nm.
[0075] S300, growing a non-doped GaN layer on the buffer layer;
[0076] The non-doped GaN layer was grown by MOCVD, the reaction chamber temperature was controlled to be 1100°C, the pressure was 120 Torr, and N source and Ga source were introduced. The thickness of the non-doped GaN layer was 1000nm.
[0077] S400, growing an N-type GaN layer on the non-doped GaN layer;
[0078] The N-type GaN layer was grown by MOCVD, the reaction chamber temperature was controlled at 1100°C, the pressure was 120 Torr, and N source, Ga source and N-type doping source were introduced. The thickness of the N-type GaN layer was 1.5 μm, and the N-type doping concentration was 5×10 19 cm -3 cm -3 .
[0079] S500, growing a stress release layer on the N-type GaN layer;
[0080] MOCVD was used to grow the InGaN / GaN periodic alternating stacked structure. The temperature of the reaction chamber was controlled at 850°C and the pressure was 120Torr. N source, Ga source and In source were introduced to grow the InGaN layer. N source and Ga source were introduced to grow the GaN layer. The InGaN layer and GaN layer were repeatedly stacked to grow periodically. The number of cycles of the stress release layer was 6 and the thickness was 80nm.
[0081] S600, growing a multi-quantum well layer on the stress release layer;
[0082] MOCVD growth was adopted, and the reaction chamber temperature was controlled at 800°C and the pressure was 120Torr to grow the quantum well layer; the reaction chamber temperature was controlled at 900°C and the growth pressure was 120Torr to grow the quantum barrier layer; the quantum well layer and the quantum barrier layer were repeatedly stacked and grown periodically. The period number of the multi-quantum well layer was 14, and the quantum barrier layer was a GaN quantum barrier layer with a thickness of 10nm.
[0083] The growth of the quantum well layer specifically includes:
[0084] S601, using N2 as carrier gas, introducing Ga source, In source and N source to grow an InGaN layer;
[0085] The In component ratio of the InGaN layer is 0.3 and the thickness is 4nm.
[0086] S602, turning off the Ga source, In source and N source, and introducing N2 and H2 to process the InGaN layer;
[0087] N2 and H2 were continuously introduced for 5 min, wherein the flow rate of H2 accounted for 5% of the total flow rate.
[0088] S603, using N2 as carrier gas, introducing an In source to grow an InN layer.
[0089] The In source was continuously introduced for 8 min.
[0090] S7, growing an electron blocking layer on the multi-quantum well layer;
[0091] MOCVD is used to grow an AlGaN / GaN periodic alternating stacked structure, the reaction chamber temperature is controlled to be 850°C, the pressure is 120Torr, N source, Ga source and Al source are introduced to grow an AlGaN layer, N source and Ga source are introduced to grow a GaN layer, and AlGaN and GaN layers are repeatedly stacked to grow periodic layers. The number of cycles of the electron blocking layer is 6, and the thickness is 40nm.
[0092] S8. Growing a P-type GaN layer on the electron blocking layer.
[0093] The P-type GaN layer was grown by MOCVD, the reaction chamber temperature was controlled at 900°C, the pressure was 150 Torr, and N source, Ga source and P-type doping source were introduced. The thickness of the P-type GaN layer was 60nm, and the P-type doping concentration was 1×10 17 cm -3 .
[0094] Example 2
[0095] This embodiment provides a method for preparing a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the multi-quantum well layer includes six quantum well layers and quantum barrier layers that are periodically and alternately stacked.
[0096] The growth of the quantum well layer further includes periodically repeating steps S601, S602 and S603, with the number of cycles being 2. The In component ratio of the InGaN layer is 0.1, and the thickness is 2 nm.
[0097] The rest are the same as in Example 1.
[0098] Example 3
[0099] This embodiment provides a method for preparing a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the multi-quantum well layer includes 10 quantum well layers and quantum barrier layers that are periodically and alternately stacked.
[0100] The growth of the quantum well layer further includes periodically repeating steps S601, S602 and S603, with the number of cycles being 3. The In component ratio of the InGaN layer is 0.25, and the thickness is 3 nm.
[0101] The rest are the same as in Example 1.
[0102] Example 4
[0103] This embodiment provides a method for preparing a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the multi-quantum well layer includes 10 quantum well layers and quantum barrier layers that are periodically and alternately stacked.
[0104] The growth of the quantum well layer further includes periodically repeating steps S601, S602 and S603, with the number of cycles being 6. The In component ratio of the InGaN layer is 0.25, and the thickness is 3 nm.
[0105] The rest are the same as in Example 1.
[0106] Comparative Example 1
[0107] This comparative example provides a method for preparing a light-emitting diode epitaxial wafer, which is different from Example 1 in that the multi-quantum well layer includes 14 periodically alternately stacked InGaN quantum well layers and GaN quantum barrier layers. The In component ratio of the InGaN quantum well layer is 0.3, the thickness is 4nm, and the thickness of the GaN quantum barrier layer is 10nm.
[0108] The rest are the same as in Example 1.
[0109] The light-emitting diode epitaxial wafers obtained in Examples 1 to 4 and Comparative Example 1 were used to prepare chips with a size of 3 mil×6 mil. The emission wavelength (WD) and wavelength standard deviation (WD_STD), emission brightness (IV) and emission brightness standard deviation (IV_STD) were tested at a test current of 8 mA. The specific results are as follows:
[0110]
[0111] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A method for preparing a light emitting diode epitaxial wafer, It is characterized in that The following steps are involved: (1) providing a substrate; (2) growing a buffer layer on the substrate; (3) growing a non-doped GaN layer on the buffer layer; (4) growing an N-type GaN layer on the undoped GaN layer; (5) growing a stress release layer on the N-type GaN layer; (6) growing a multi-quantum well layer on the stress release layer, wherein the multi-quantum well layer includes a quantum well layer and a quantum barrier layer that are periodically and alternately grown, wherein the growth of the quantum well layer includes: (6.1) with N 2 As carrier gas, Ga source, In source and N source are introduced to grow InGaN layer; (6.2) Turn off the Ga source, In source and N source, and pass N 2 and H 2 Processing the InGaN layer; (6.3) with N 2 As carrier gas, an In source is introduced to grow an InN layer; (7) growing an electron blocking layer on the multi-quantum well layer; (8) Growing a P-type GaN layer on the electron blocking layer.
2. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that The growth of the quantum well layer further comprises: periodically repeating steps (6.1), (6.2) and (6.3), with the number of repetition cycles being 2 to 6.
3. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that In step (6.2), H 2 The proportion of traffic to the total traffic is 1% to 10%.
4. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that The growth temperature of the quantum well layer is 700° C. to 850° C., and the growth pressure is 100 Torr to 300 Torr; The growth temperature of the quantum barrier layer is 850° C. to 920° C., and the growth pressure is 100 Torr to 300 Torr.
5. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that In step (6.2), N 2 and H 2 The processing time is 1min to 10min.
6. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that In step (6.3), the time for introducing the In source to grow the InN layer is 1 min to 10 min.
7. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that The In component ratio of the InGaN layer is 0.1-0.
3.
8. The method for preparing a light emitting diode epitaxial wafer according to claim 1, It is characterized in that The thickness of the InGaN layer is 2nm-4nm.
9. The light emitting diode epitaxial wafer according to claim 1, It is characterized in that The period number of the multi-quantum well layer is 6-14.
10. A light emitting diode epitaxial wafer, It is characterized in that The light emitting diode epitaxial wafer is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Epitaxial structure and growing method for improving gallium nitride (GaN) based light-emitting diode (LED) lighting efficiency
CN103066174A
InGaN / GaN quantum well structure and preparation method thereof as well as LED epitaxial wafer and preparation method thereof
CN109888069A
LED preparation method and LED
CN110061105A
LED epitaxial structure based on III-V group compound application and preparation method thereof
CN116093224A
Nitride semiconductor light emitting element
JP2000223741A
Cited By
Epitaxial structure of LED quantum well and growth method thereof
CN119403313A
Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode
CN121078857A