Reflective mask blank, method of manufacturing reflective mask, reflective mask, and method of manufacturing semiconductor device

The reflective mask blank and mask design with a multilayer structure addresses the challenge of achieving both high phase shift effect and large exposure margin, enabling precise and integrated semiconductor device manufacturing using a single mask.

JP2024134733APending Publication Date: 2024-10-04HOYA CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023045077
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional phase shift type reflective masks face challenges in achieving both high phase shift effect and large exposure margin due to varying reflectance requirements for different pattern types, necessitating multiple masks for regions with high and low reflectance, which complicates the design and manufacturing process.

Method used

A reflective mask blank and mask design that incorporates a multilayer structure with specific reflectance and phase difference characteristics, utilizing materials like ruthenium, tantalum, and chromium, allowing for a single mask to achieve both high phase shift effect and large exposure margin by adjusting reflectance and phase shift properties.

Benefits of technology

Enables highly accurate fine pattern transfer with a single mask, ensuring high phase shift effect and exposure margin, facilitating high integration and precision in semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134733000001_ABST
    Figure 2024134733000001_ABST
Patent Text Reader

Abstract

To provide a reflective mask blank capable of producing a reflective mask which enables precise transferring of a fine pattern by achieving both a high phase shift effect and a large exposure margin.SOLUTION: A reflective mask blank comprises a substrate, a multilayer reflective film formed on the substrate, and a thin film formed on the multilayer reflective film. The thin film includes a first layer and a second layer. The first layer has a reflectance greater than 2.5% with respect to EUV light. The second layer has a reflectance greater than the reflectance of the first layer with respect to the EUV light.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask blank, a method for manufacturing a reflective mask, a reflective mask, and a method for manufacturing a semiconductor device. [Background technology]

[0002] In semiconductor devices, the finer the patterns such as wiring are and the higher the precision of the pattern dimensions and pattern positions are, the higher the electrical characteristics and performance will be, and the higher the integration density and the smaller the chip size will be. For this reason, EUV lithography using extreme ultraviolet (EUV: Extreme Ultra Violet) rays with a wavelength of about 13.5 nm has been developed, and there is a demand for this EUV lithography to have the ability to transfer fine-dimensional patterns with higher precision.

[0003] In EUV lithography, a reflective mask is used because there are few materials that are transparent to EUV light. Even with such a reflective mask, by using a phase-shift reflective mask that has a phase shift effect, it is expected that the contrast of the transferred pattern and therefore the resolution will be improved. Therefore, in order to transfer a fine dimension pattern with high accuracy, it is effective to use a phase-shift reflective mask, as described in the following Patent Documents 1 and 2. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-080659 A [Patent Document 2] JP 2004-207593 A Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, in exposure using a phase-shifting reflective mask, the reflectance required to obtain a good phase shift effect may differ depending on the type of pattern. Depending on the type (shape) and pitch of the pattern to be transferred, a high reflectance may be preferable, or a low reflectance may be preferable. However, in a portion having a high reflectance, a high phase shift effect can be obtained, but the exposure margin is reduced. This creates a risk that the resist on the transferee (semiconductor) substrate will be exposed in an area that should not be exposed. In contrast, a low reflectance increases the exposure margin, but reduces the phase shift effect.

[0006] For this reason, in order to form a pattern region where a relatively high reflectance is preferable and a pattern region where a relatively low reflectance is preferable on a transfer target substrate using a conventional phase shift mask, it is necessary to prepare two or more phase shift masks. Also, how to set the region having a relatively high reflectance and the region having a relatively low reflectance differs depending on the semiconductor device to be transferred. For this reason, it is preferable that the mask blank has a high degree of design freedom so that a region having a desired reflectance can be set according to the type of pattern to be formed on the transfer target.

[0007] Therefore, the present invention aims to provide a reflective mask capable of achieving high-precision fine pattern transfer by achieving both a high phase shift effect and a large exposure margin, to provide a reflective mask blank from which this reflective mask can be manufactured, to provide a method for manufacturing a reflective mask that can simultaneously achieve a high phase shift effect and a large exposure margin with a single mask, and to provide a method for manufacturing a semiconductor device that can achieve high performance and high integration by using this reflective mask. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration.

[0009] (Configuration 1) A substrate; a multilayer reflective film formed on the substrate; a thin film formed on the multilayer reflective film, the thin film includes a first layer and a second layer; the reflectance of the first layer to EUV light is greater than 2.5%; The reflectance of the second layer to the EUV light is higher than the reflectance of the first layer. A reflective mask blank comprising:

[0010] (Configuration 2) A phase difference between a first reflected light reflected from the first layer irradiated with EUV light and a second reflected light reflected from the second layer irradiated with EUV light is 30 degrees or less. 2. The reflective mask blank according to claim 1,

[0011] (Configuration 3) When the light reflected from the multilayer reflective film irradiated with EUV light is used as the reference reflected light, a phase difference between the reference reflected light and a first reflected light reflected from the first layer irradiated with the EUV light is 150 degrees or more; A phase difference between the reference reflected light and the second reflected light reflected from the second layer irradiated with the EUV light is 150 degrees or more. 2. The reflective mask blank according to claim 1,

[0012] (Configuration 4) The thin film has a bottom layer provided closest to the substrate. 2. The reflective mask blank according to claim 1,

[0013] (Configuration 5) The first layer or the second layer is made of a material containing at least one of ruthenium, tantalum, and chromium. 2. The reflective mask blank according to claim 1,

[0014] (Configuration 6) The first layer is formed on the second layer. 2. The reflective mask blank according to claim 1,

[0015] (Configuration 7) An etching mask film is provided on the thin film. 2. The reflective mask blank according to claim 1,

[0016] (Configuration 8) The etching mask film includes two or more layers. 8. The reflective mask blank according to claim 7.

[0017] (Configuration 9) A method for producing a reflective mask using the reflective mask blank according to configuration 7, comprising the steps of: When one of the first layer and the second layer that is formed closer to the substrate is defined as a lower layer and the other is defined as an upper layer, etching the etching mask film to form an etching mask pattern; etching the upper layer using the etching mask pattern as a mask to form a first upper layer pattern; a step of etching the lower layer using the first upper layer pattern as a mask to form a lower layer pattern; forming a transfer pattern by etching the first upper layer pattern and forming a second upper layer pattern; 2. A method for manufacturing a reflective mask comprising the steps of:

[0018] (Configuration 10) the thin film has a bottom layer disposed below the underlayer, In the step of forming the second upper layer pattern or after the step of forming the second upper layer pattern, the lowermost layer is removed in the region where the lower layer is etched. 10. The method for producing a reflective mask according to claim 9,

[0019] (Configuration 11) A substrate; a multilayer reflective film formed on the substrate; a thin film provided on the multilayer reflective film and having a transfer pattern formed thereon; the thin film includes a first layer and a second layer; the reflectance of the first layer to EUV light is greater than 2.5%; The reflectance of the second layer to the EUV light is higher than the reflectance of the first layer. A reflective mask characterized by:

[0020] (Configuration 12) A phase difference between a first reflected light reflected from the first layer irradiated with EUV light and a second reflected light reflected from the second layer irradiated with EUV light is 30 degrees or less. 12. The reflective mask according to claim 11,

[0021] (Configuration 13) When the light reflected from the multilayer reflective film irradiated with EUV light is used as the reference reflected light, a phase difference between the reference reflected light and the first reflected light reflected from the first layer irradiated with the EUV light is 150 degrees or more; A phase difference between the reference reflected light and the second reflected light reflected from the second layer irradiated with the EUV light is 150 degrees or more. 12. The reflective mask according to claim 11,

[0022] (Configuration 14) The thin film has a bottom layer provided closest to the substrate. 12. The reflective mask according to claim 11,

[0023] (Configuration 15) The first layer or the second layer is made of a material containing at least one of ruthenium, tantalum, and chromium. 12. The reflective mask according to claim 11,

[0024] (Configuration 16) The first layer is formed on the second layer. 12. The reflective mask according to claim 11,

[0025] (Configuration 17) The first layer and the second layer are each at least partially exposed in a plan view. 12. The reflective mask according to claim 11,

[0026] (Configuration 18) a laminated region in which at least a portion of the second layer is covered by the first layer; The second layer is exposed at an outer periphery of the laminated region in a plan view. 12. The reflective mask according to claim 11,

[0027] (Configuration 19) A reflective mask having a transfer pattern manufactured by using the reflective mask blank according to any one of configurations 1 to 8, a reflective mask manufactured by the manufacturing method according to configuration 9 or 10, or a reflective mask according to any one of configurations 11 to 18, is used to transfer the transfer pattern onto a semiconductor substrate. 4. A method for manufacturing a semiconductor device comprising the steps of: Effect of the Invention

[0028] The present invention makes it possible to provide a reflective mask capable of achieving both a high phase shift effect and a large exposure margin, thereby enabling high-precision fine pattern transfer, a reflective mask blank from which this reflective mask can be manufactured, a method for manufacturing a reflective mask that can simultaneously obtain a high phase shift effect and a large exposure margin with a single mask, and a method for manufacturing a semiconductor device that uses this reflective mask and enables high performance and high integration. [Brief description of the drawings]

[0029] [Figure 1]1 is a cross-sectional view showing a configuration of a reflective mask blank according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a configuration of a reflective mask according to an embodiment of the present invention. [Diagram 3] 1 is a plan view showing a configuration of a reflective mask according to an embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view showing another configuration of the reflective mask according to the embodiment of the present invention. [Diagram 5] 5A to 5C are cross-sectional process diagrams illustrating an example of a method for manufacturing a reflective mask according to an embodiment of the present invention. [Figure 6] FIG. 2 is a diagram showing the compositions and physical properties of thin films in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] In this specification, the reflectance (absolute reflectance and relative reflectance) refers to a value when the angle of incidence of EUV light on the thin film 40 (first layer 41 and second layer 42) or the multilayer reflective film 20 (including the protective film 30, the same applies below) is the same as the angle of incidence of EUV light on an irradiation target used in exposure when transferring a pattern using the reflective mask 1a, 1a' or the reflective mask 1a, 1a' manufactured from the reflective mask blank 1. When transferring a pattern, the light from the EUV light source is irradiated onto the reflective mask 1a, 1a' via an illumination optical system at an angle inclined, for example, from 6 degrees to 8 degrees with respect to a plane perpendicular to the main surface of the reflective mask 1a, 1a'. The angle of incidence of EUV light on the thin film 40 or the multilayer reflective film 20 is not particularly limited, but can be, for example, 6 degrees.

[0031] <Reflective mask blanks and reflective masks> FIG. 1 is a cross-sectional view showing the configuration of a reflective mask blank 1 according to an embodiment of the present invention. The reflective mask blank 1 shown in this figure is an original plate of a reflective mask for EUV lithography using extreme ultraviolet (EUV: Extreme Ultra Violet, hereinafter referred to as EUV light) as exposure light. EUV light is light (electromagnetic waves) including light with a wavelength of 13.5 nm, and can be light with a wavelength of 13 nm to 14 nm, more specifically, light with a wavelength of 13.5 nm. In this specification, light includes not only visible light but also electromagnetic waves. FIG. 2 is a cross-sectional view showing the configuration of a reflective mask 1a according to an embodiment of the present invention, which is manufactured by processing the reflective mask blank 1 shown in FIG. This reflective mask 1a is for EUV lithography and is a phase-shift type mask.

[0032] The reflective mask blank 1 shown in FIG. 1 has a substrate 10, and a multilayer reflective film 20, a protective film 30, and a thin film 40, which are laminated in this order from the substrate 10 side on one main surface (first main surface) of the substrate 10. The thin film 40 is a film on which a transfer pattern is formed by processing. The reflective mask blank 1 may also have a configuration in which an etching mask film 50 is provided on the thin film 40 as necessary. The reflective mask blank 1 may also include a resist film formed on the etching mask film 50 as necessary. The etching mask film 50 and the resist film are removed in the manufacturing process of the reflective mask 1a.

[0033] 2 is obtained by patterning the thin film 40 in the reflective mask blank 1 shown in Fig. 1 as a transfer pattern 40a. Hereinafter, the details of each part constituting the reflective mask blank 1 and the reflective mask 1a will be described with reference to Figs. 1 and 2.

[0034] <Substrate 10> The substrate 10 is preferably made of a material having a low thermal expansion coefficient within the range of 0±5 ppb / °C in order to prevent distortion of the transfer pattern 40a due to heat generation during exposure (EUV exposure) with EUV light [H1] using the reflective mask 1a. Examples of such materials include SiO2-TiO2 glass and multi-component glass ceramics. The transfer pattern 40a is a pattern formed by processing the thin film 40 as described above.

[0035] The back surface of the substrate 10, on which the thin film 40 is not provided, is the surface that is electrostatically chucked when the reflective mask 1a is set in the exposure tool, and is provided with a conductive film (not shown here). The back surface refers to the other main surface that faces the first main surface on which the thin film 40 is provided.

[0036] The first main surface of the substrate 10 on which the transfer pattern 40a is formed is surface-processed to have a high flatness in terms of obtaining at least pattern transfer accuracy and positional accuracy. In the case of EUV exposure, the flatness is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less in a 132 mm×132 mm region of the first main surface of the substrate 10. Also, the flatness is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less in a 132 mm×132 mm region of the back surface of the substrate 10. The flatness of the back surface of the reflective mask blank 1 is preferably 1 μm or less, more preferably 0.5 μm or less, and particularly preferably 0.3 μm or less in a 142 mm×142 mm region. In this specification, the flatness is a value representing the warpage (deformation amount) of the surface indicated by TIR (Total Indicated Reading). This value is the absolute value of the difference in height between the highest point on the surface of substrate 10 above the focal plane, which is determined by the least squares method using the surface of substrate 10 as a reference, and the lowest point on the surface of substrate 10 below the focal plane.

[0037] In addition, the substrate 10 preferably has a high surface smoothness. The surface roughness of the first main surface on which the transfer pattern 40a is formed is preferably 0.1 nm or less in root mean square roughness (RMS). The surface smoothness can be measured by an atomic force microscope.

[0038] Furthermore, the substrate 10 preferably has high rigidity to prevent deformation due to film stress of the films (such as the multilayer reflective film 20) formed thereon. In particular, the substrate 10 preferably has a high Young's modulus of 65 GPa or more.

[0039] <Multilayer reflective film 20> The multilayer reflective film 20 is formed on the first main surface of the substrate 10 and reflects the EUV light [H1], which is the exposure light, with a high reflectance. In the reflective mask 1a formed using the reflective mask blank 1, the multilayer reflective film 20 has a function of reflecting the EUV light [H1], and is a multilayer film in which layers mainly composed of materials with different refractive indices are periodically laminated. The multilayer reflective film 20 may further include a protective film 30 on a surface layer described later. In this case, the reflected light of the multilayer reflective film 20 refers to light that is incident on the multilayer reflective film 20 through the protective film 30 and is reflected through the protective film 30. That is, when the reflective mask blank 1 or the reflective mask 1a includes the protective film 30, the reflected light from the surface of the protective film 30 in a state in which the protective film 30 is formed on the multilayer reflective film 20 on the substrate 10 is measured as the reflected light of the multilayer reflective film 20.

[0040] Generally, a multilayer film in which thin films (high refractive index layers) of a light element or its compound, which is a high refractive index material, and thin films (low refractive index layers) of a heavy element or its compound, which is a low refractive index material, are alternately stacked in about 30 to 60 periods is used as the multilayer reflective film 20.

[0041] To form the multilayer reflective film 20, high refractive index layers and low refractive index layers may be laminated in this order on the substrate 10 in multiple periods. In this case, one laminate structure of (high refractive index layer / low refractive index layer) constitutes one period. To form the multilayer reflective film 20, low refractive index layers and high refractive index layers may be laminated in this order on the substrate 10 in multiple periods. In this case, one laminate structure of (low refractive index layer / high refractive index layer) constitutes one period.

[0042] In addition, the top layer of the multilayer reflective film 20, that is, the surface layer of the multilayer reflective film 20 opposite to the substrate 10, is preferably a high refractive index layer. When a high refractive index layer and a low refractive index layer are laminated in this order on the substrate 10, the top layer is a low refractive index layer. However, when the low refractive index layer is the surface of the multilayer reflective film 20, the reflectance of the surface of the multilayer reflective film 20 may decrease due to the low refractive index layer being easily oxidized. For this reason, it is preferable to form a high refractive index layer on the low refractive index layer. On the other hand, when a low refractive index layer and a high refractive index layer are laminated in this order on the substrate 10, the top layer is a high refractive index layer. In that case, the top high refractive index layer is the surface of the multilayer reflective film 20.

[0043] In this embodiment, a layer containing silicon (Si) is used as the high refractive index layer. In addition to simple Si, a Si compound containing at least one of boron (B), carbon (C), nitrogen (N), and oxygen (O) can be used as the material containing Si. By using a layer containing Si as the high refractive index layer for the multilayer reflective film 20, a reflective mask 1a for EUV lithography with excellent reflectance of EUV light [H1] can be obtained. In this embodiment, a glass substrate is preferably used as the substrate 10, and Si is also excellent in adhesion to the glass substrate, so it is preferable as a material for forming the high refractive index layer.

[0044] The low refractive index layer is made of a metal selected from molybdenum (Mo), ruthenium (Ru), rhodium (Rh), and platinum (Pt), or an alloy thereof. For example, the multilayer reflective film 20 for EUV light [H1] with a wavelength of 13 nm to 14 nm is preferably a Mo / Si periodic laminate film in which Mo films and Si films are alternately laminated for about 30 to 60 periods.

[0045] Other examples of the multilayer reflective film 20 that can be used in the EUV light [H1] region include Ru / Si periodic multilayer film, Mo / beryllium (Be) periodic multilayer film, Mo compound / Si compound periodic multilayer film, Si / niobium (Nb) periodic multilayer film, Si / Mo / Ru periodic multilayer film, Si / Mo / Ru / Mo periodic multilayer film, Si / Ru / Mo / Ru periodic multilayer film, etc. The material of the multilayer reflective film 20 can be selected taking into consideration the exposure wavelength.

[0046] The reflectance of such a multilayer reflective film 20 is preferably, for example, 65% or more. The upper limit of the reflectance of the multilayer reflective film 20 is preferably, for example, 73%. The thickness and period of the layers included in the multilayer reflective film 20 can be selected so as to satisfy Bragg's law. In this specification, the reflectance of the multilayer reflective film 20 means the reflectance from the surface of the multilayer reflective film 20 in a state in which the multilayer reflective film 20 is formed on the substrate 10. When the multilayer reflective film 20 includes a protective film 30, the reflectance of the multilayer reflective film 20 means the reflectance from the protective film 30 in a state in which the protective film 30 is formed on the multilayer reflective film 20 on the substrate 10.

[0047] The multilayer reflective film 20 can be formed by a known method, for example, an ion beam sputtering method.

[0048] For example, when the multilayer reflective film 20 is a Mo / Si multilayer film, a Si film having a thickness of about 4 nm is formed on the substrate 10 by ion beam sputtering using a Si target. Next, a Mo film having a thickness of about 3 nm is formed using a Mo target. By repeating such an operation, the multilayer reflective film 20 can be formed in which 30 to 60 periods of Mo / Si films are laminated. At this time, it is preferable that the surface layer of the multilayer reflective film 20 on the side opposite to the substrate 10 is a layer containing Si (Si film). The thickness of one period of the Mo / Si film is 7 nm.

[0049] <Protective film 30> The protective film 30 is a film provided to protect the surface layer of the multilayer reflective film 20 and layers below the surface layer from etching and cleaning when the reflective mask blank 1 is processed to manufacture a reflective mask 1a for EUV lithography. The protective film 30 is provided on the surface layer of the multilayer reflective film 20, in contact with the surface layer, or via another film. The protective film 30 can also serve to protect the multilayer reflective film 20 when a black defect in the transfer pattern 40a is repaired using an electron beam (EB) in the reflective mask 1a.

[0050] Here, although FIG. 1 and FIG. 2 show the case where the protective film 30 is one layer, the protective film 30 may have a laminated structure of two or more layers. The protective film 30 is formed of a material that is resistant to an etchant and a cleaning solution used when patterning the thin film 40. By forming the protective film 30 on the multilayer reflective film 20, damage to the surface of the multilayer reflective film 20 can be suppressed when manufacturing a reflective mask 1a using a substrate 10 having the multilayer reflective film 20 and the protective film 30. Therefore, the reflectance characteristic of the multilayer reflective film 20 with respect to EUV light [H1] becomes good. The following will explain the case where the protective film 30 is one layer as an example.

[0051] In the reflective mask blank 1 of this embodiment, a material that is resistant to an etching gas used in dry etching for patterning the thin film 40 formed on the protective film 30 can be selected as the material of the protective film 30. The thickness of the protective film 30 is not particularly limited as long as the protective film 30 can fulfill the function of protecting the layers below the surface layer of the multilayer reflective film 20, but the thickness of the protective film 30 is preferably 1 nm or more and 20 nm or less. From the viewpoint of the reflectance of EUV light, the thickness of the protective film 30 is preferably 1.0 nm to 8.0 nm, more preferably 1.5 nm to 6.0 nm.

[0052] When the thin film 40 is configured by stacking multiple layers, a material that is resistant to the etching gas used to pattern the bottom layer of the thin film 40 is used as the material for the protective film 30. When the protective film 30 is configured by stacking multiple layers, a material that is resistant to the etching gas used to pattern the bottom layer of the thin film 40 is used as the material for the top layer of the protective film 30.

[0053] The material of the protective film 30 is preferably a material that provides an etching selectivity of the bottom layer of the thin film 40 to the protective film 30 (etching rate of the bottom layer of the thin film 40 / etching rate of the protective film 30) of 1.5 or more, preferably 3 or more.

[0054] For example, when the bottom layer of the thin film 40 is made of a material (predetermined Ru-based material) containing metal including ruthenium (Ru) and at least one of chromium (Cr), nickel (Ni) and cobalt (Co), or a material (predetermined Ru-based material) containing metal including ruthenium (Ru) and at least one of vanadium (V), niobium (Nb), molybdenum (Mo), tungsten (W) and rhenium (Re), the bottom layer of the thin film 40 can be etched by a mixed gas of chlorine gas and oxygen gas, or a dry etching gas using oxygen gas. As a material of the protective film 30 that is resistant to this etching gas, a silicon-based material such as silicon (Si) alone or a material containing silicon (Si) and oxygen (O) and / or nitrogen (N) can be selected. Therefore, when the bottom layer of the thin film 40 in contact with the surface of the protective film 30 is made of a thin film made of a predetermined Ru-based material, the protective film 30 is preferably made of the above-mentioned silicon-based material. The silicon-based material is resistant to a mixed gas of a chlorine-based gas and an oxygen gas, or a dry etching gas using an oxygen gas, and the higher the oxygen content of the silicon-based material, the higher the resistance. Therefore, the material of the protective film 30 is preferably silicon oxide (SiOx, 1≦x≦2), more preferably a larger x, and particularly preferably SiO2.

[0055] Furthermore, when the bottom layer of the thin film 40 in contact with the surface of the protective film 30 is a thin film made of a material containing tantalum (Ta), the bottom layer of the thin film 40 can be etched by dry etching using a halogen-based gas that does not contain oxygen gas. A material containing ruthenium (Ru) as a main component can be used as a material for the protective film 30 that is resistant to this etching gas. "Containing substance A as a main component" means that substance A is contained at 50 atomic % or more.

[0056] Furthermore, when the bottom layer of the thin film 40 in contact with the surface of the protective film 30 is a thin film made of a material containing chromium (Cr), the bottom layer of the thin film 40 can be etched by dry etching using a dry etching gas that is a chlorine-based gas that does not contain oxygen gas, or a mixed gas of oxygen gas and a chlorine-based gas. A material containing ruthenium (Ru) as a main component can be used as a material of the protective film 30 that is resistant to this etching gas.

[0057] When the bottom layer of the thin film 40 is a material containing tantalum (Ta) or chromium (Cr), the material of the protective film 30 that can be used can be a material containing ruthenium as a main component, as described above. Specific examples of materials containing ruthenium as a main component include simple Ru metal, Ru alloys containing at least one metal selected from titanium (Ti), niobium (Nb), molybdenum (Mo), zirconium (Zr), yttrium (Y), boron (B), lanthanum (La), cobalt (Co), chromium (Cr), rhodium (Rh) and rhenium (Re), Ru metal, and materials containing nitrogen in Ru alloys can be mentioned.

[0058] The Ru content of the Ru alloy is 50 atomic % or more and less than 100 atomic %, preferably 80 atomic % or more and less than 100 atomic %, and more preferably 95 atomic % or more and less than 100 atomic %. In particular, when the Ru content of the Ru alloy is 95 atomic % or more and less than 100 atomic %, the element (silicon) constituting the multilayer reflective film 20 can be suppressed from diffusing into the protective film 30. In addition, the cleaning resistance of the mask can be improved while ensuring sufficient reflectance of EUV light. Furthermore, the protective film 30 functions as an etching stopper when the thin film 40 is etched. In addition, the protective film 30 can prevent the multilayer reflective film 20 from changing over time.

[0059] The material of the protective film 30 may be a compound containing Ru, for example, a material containing at least one selected from RuNb, RuN, and RuTi. Alternatively, the material of the protective film 30 may be a compound containing Y and O, for example, a material containing Y2O3. Alternatively, the material of the protective film 30 may be a compound containing Cr, for example, a material containing CrN.

[0060] In addition to the above materials, the material of the protective film 30 may further contain at least one selected from oxygen (O), nitrogen (N), carbon (C), and boron (B).

[0061] The method for forming the protective film 30 may be any known film forming method without any particular limitations. Specific examples include various sputtering methods, such as DC sputtering, RF sputtering, and ion beam sputtering, as well as atomic layer deposition (ALD).

[0062] <Thin film 40 and transfer pattern 40a> The thin film 40 is a film used as a phase shift film for EUV light [H1], and serves as a film for forming a transfer pattern 40a in a reflective mask 1a constructed using this reflective mask blank 1. The transfer pattern 40a is formed by patterning this thin film 40.

[0063] In this embodiment, the thin film 40 includes at least a first layer 41 and a second layer 42. The first layer 41 and the second layer 42 each function as a phase shift film for the EUV light [H1]. The first layer 41 and the second layer 42 absorb the EUV light [H1] and reflect a part of the EUV light [H1] at a level that does not adversely affect the pattern transfer. The thin film 40 may include a film other than the first layer 41 and the second layer 42, for example, a bottom layer 43 provided closer to the substrate 10 than the first layer 41 and the second layer 42, and may further include other layers not shown here. The configurations of the first layer 41 and the second layer 42 will be described below.

[0064] [Reflectance to EUV light [H1] (thin film 40 and transferred pattern 40a)] The first layer 41 and the second layer 42 can both be films that function as phase shift films for the EUV light [H1].

[0065] The absolute reflectance [R1] from the first layer 41 and the absolute reflectance [R2] from the second layer 42 to EUV light [H1] are higher than 2.5%, and more preferably 3.0% or more. The absolute reflectance [R1] from the first layer 41 and the absolute reflectance [R2] from the second layer 42 to EUV light are preferably 20% or less, and more preferably 15% or less. This allows each of the first layer 41 and the second layer 42 to function as a phase shift film.

[0066] However, the first layer 41 and the second layer 42 have different absolute reflectances for the EUV light [H1]. Regarding the absolute reflectance for the EUV light [H1], the absolute reflectance [R2] for the EUV light [H1] from the second layer 42 is higher than the absolute reflectance [R1] from the first layer 41, that is, the absolute reflectance [R2]>absolute reflectance [R1].

[0067] In this specification, the absolute reflectance (reflectance) [R1] of the first layer 41 means the absolute reflectance from the surface of the first layer 41 in a state in which the first layer 41 is formed on the multilayer reflective film 20 (and the bottom layer) formed on the substrate 10, when the first layer 41 is provided on the multilayer reflective film 20 (and the bottom layer) without the second layer 42. When the first layer 41 is provided on the multilayer reflective film 20 via the second layer 42, the absolute reflectance (reflectance) [R1] of the first layer 41 means the absolute reflectance from the surface of the first layer 41 in a state in which the first layer 41 is formed on the second layer 42 formed on the multilayer reflective film 20 (and the bottom layer) on the substrate 10. The same applies to the relative reflectance described later.

[0068] Moreover, the absolute reflectance (reflectance) [R2] of the second layer 42 means the absolute reflectance from the surface of the second layer 42 in a state in which the second layer 42 is formed on the multilayer reflective film 20 (and the bottom layer) formed on the substrate 10 when the second layer 42 is provided on the multilayer reflective film 20 (and the bottom layer) without the first layer 41 therebetween, and means the absolute reflectance from the surface of the second layer 42 in a state in which the second layer 42 is formed on the first layer 41 formed on the multilayer reflective film 20 (and the bottom layer) on the substrate 10 when the second layer 42 is provided on the multilayer reflective film 20 (and the bottom layer) via the first layer 41. The same applies to the relative reflectance described later.

[0069] Absolute reflectance refers to the reflected intensity from an object of irradiation relative to the incident intensity of light (electromagnetic waves) on the object of irradiation. That is, the absolute reflectance of a film or layer is a value calculated by (amount of light reflected from the surface of the film or layer of the object) / (amount of light incident on the surface of the film or layer of the object). When the unit of absolute reflectance is %, it is further multiplied by 100. In this specification, when simply referring to reflectance, it means absolute reflectance unless otherwise specified.

[0070] Furthermore, when the reflectance from the multilayer reflective film 20 to the EUV light [H1] is used as a reference, the relative reflectance from the first layer 41 to the EUV light is preferably greater than 3%, more preferably 4% or more, even more preferably 5% or more, and even more preferably 8% or more. This allows a high phase shift effect to be obtained. Furthermore, the relative reflectance from the first layer 41 to the EUV light is preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. This also applies to the second layer 42. This allows unnecessary exposure of the resist film during pattern transfer to be suppressed or reduced. The relative reflectance can be calculated by (absolute reflectance of the target film or layer surface) / (absolute reflectance from the multilayer reflective film 20). If the unit of the relative reflectance is %, it is further multiplied by 100.

[0071] The first layer 41 and the second layer 42 having the reflectances as described above are films stacked above one of the main surfaces of the substrate 10, but the order of stacking them is not limited. For example, even if the second layer 42 is stacked on the first layer 41, the effect of forming a fine pattern can be obtained. However, by stacking the first layer 41, which has a relatively low reflectance to EUV light [H1], on the second layer 42, which has a relatively high reflectance to EUV light [H1], the effect of forming a fine pattern can be further increased, as described below.

[0072] [Phase difference of reflected light (thin film 40 and transfer pattern 40a)] The phase difference between the first reflected light [Rf1] obtained by reflecting the EUV light [H1] on the first layer 41 and the second reflected light [Rf2] obtained by reflecting the EUV light [H1] on the second layer 42 is preferably 30 degrees or less, and more preferably 20 degrees or less. In this way, a better phase shift effect can be obtained.

[0073] In addition, when the reflected light reflected from the multilayer reflective film 20 irradiated with EUV light [H1] is defined as the reference reflected light [Rf0], the phase difference between the reference reflected light [Rf0] and the first reflected light [Rf1] and the second reflected light [Rf2] is 150 degrees or more. Here, when the protective film 30 is provided on the surface layer of the multilayer reflective film 20, the reflected light that is incident on the multilayer reflective film 20 irradiated with EUV light [H1] through the protective film 30 and reflected is defined as the reference reflected light [Rf0]. In addition, the phase difference of the first reflected light [Rf1] with respect to the reference reflected light [Rf0] is preferably 180 degrees or more, more preferably 200 degrees or more, and even more preferably 210 degrees or more. In addition, the phase difference is preferably 300 degrees or less, more preferably 280 degrees or less, even more preferably 250 degrees or less, and even more preferably 240 degrees or less. The phase difference of the second reflected light [Rf2] with respect to the reference reflected light [Rf0] is the same. By setting such a phase difference, a high phase shift effect can be obtained in the exposure using this reflective mask 1a. Here, the difference between the phase difference of the first reflected light [Rf1] relative to the reference reflected light [Rf0] and the phase difference of the second reflected light [Rf2] relative to the reference reflected light [Rf0] is preferably within 30 degrees, more preferably within 20 degrees.

[0074] [Materials (thin film 40 and transfer pattern 40a)] The material of the thin film 40 is not limited as long as the reflectance and phase difference of the first layer 41 and the second layer 42 with respect to the EUV light [H1] are as described above. Examples of materials constituting such a thin film 40 include materials containing one or more selected from ruthenium (Ru), tantalum (Ta), chromium (Cr), rhodium (Rh), molybdenum (Mo), niobium (Nb), titanium (Ti), zirconium (Zr), yttrium (Y), silicon (Si), palladium (Pd), silver (Ag), platinum (Pt), gold (Au), iridium (Ir), tungsten (W), cobalt (Co), manganese (Mn), tin (Sn), vanadium (V), nickel (Ni), iron (Fe), hafnium (Hf), copper (Cu), tellurium (Te), zinc (Zn), magnesium (Mg), germanium (Ge), and aluminum (Al). In addition to these, at least one or more selected from oxygen (O), nitrogen (N), carbon (C), and boron (B) may be further included.

[0075] Specific examples of materials constituting the thin film 40 include HfAl material, AlSi material, RuN material, RuCr material, RuPt material, RuTa material, TaNb material, IrTa material, Cr material, and materials containing at least one selected from oxygen (O), nitrogen (N), carbon (C), and boron (B) in addition to these materials. For example, one selected from these materials can be used as the first layer 41, and the other can be used as the second layer 42.

[0076] At least one of the first layer 41 and the second layer 42 is preferably made of a material containing at least one of ruthenium (Ru), tantalum (Ta), and chromium (Cr). Ru has a small refractive index n and extinction coefficient k for EUV light, so a film having a good phase shift effect and a relatively high reflectance can be formed with a thin film thickness. Therefore, the shadowing effect can also be reduced. Ta and Cr have a large absorption coefficient for EUV light, so a phase shift film having a relatively low reflectance can be formed. Therefore, unnecessary exposure of the resist film during pattern transfer can be reduced or suppressed. In addition, if the extinction coefficient k is large, the film thickness of the phase shift film can be reduced, and the shadowing effect can also be reduced. Furthermore, Ta and Cr have a high etching rate for chlorine-based gas and / or fluorine-based gas, and can be easily dry-etched. Therefore, Ta and Cr can form a phase shift film with excellent processability. Furthermore, by adding B, Si, Ge, etc. to Ta, an amorphous material can be easily obtained, and the smoothness of the thin film can be improved. Furthermore, by adding N or O to Ta, the resistance of the thin film to oxidation is improved, which has the effect of improving stability over time.

[0077] Moreover, either the first layer 41 or the second layer is preferably made of a material containing Al. Examples of materials containing Al include HfAl material and AlSi material. For example, when HfAl material is used for either the first layer 41 or the second layer, Hf / [Hf+Al], which is the ratio of the Hf content (atomic %) to the total content (atomic %) of Hf and Al in the HfAl material, is preferably 0.40 or more. This can improve the resistance of the HfAl material to chemical cleaning. Moreover, Hf / [Hf+Al] is preferably 0.86 or less.

[0078] Furthermore, when an AlSi material is used for either the first layer 41 or the second layer, from the viewpoint of resistance to chemical cleaning, it is preferable that Si / [Al+Si], which is the ratio of the Si content (atomic %) to the total content (atomic %) of Al and Si in the AlSi material, is 0.20 or more. This can improve the resistance of the AlSi material to chemical cleaning. It is also preferable that Si / [Al+Si] is 0.80 or less.

[0079] Both the HfAl material and the AlSi material preferably contain oxygen (O). The oxygen content of both the HfAl material and the AlSi material is preferably 60 atomic % or more. This improves the resistance to oxidation of the thin film made of the HfAl material or the AlSi material, thereby improving stability over time. The oxygen content of the HfAl material and the AlSi material is preferably 70 atomic % or less, and more preferably 66 atomic % or less.

[0080] In addition, the first layer 41 and the second layer 42 of the thin film 40 preferably have etching selectivity with respect to each other. That is, the first layer 41 preferably has resistance to an etchant for etching the second layer 42, and the second layer 42 preferably has resistance to an etchant for etching the first layer 41.

[0081] For example, if either the first layer 41 or the second layer 42 is a layer made of a material containing ruthenium (Ru) and at least one of chromium (Cr), oxygen (O), and nitrogen (N), this layer can be etched with a mixed gas of chlorine-based gas and oxygen gas, or a dry etching gas using oxygen gas. In this case, the other of the first layer 41 and the second layer 42 is made of a material that is resistant to this mixed gas or oxygen gas. Examples of such resistant materials include HfAl material, AlSi material, and materials that further contain at least one selected from oxygen (O), nitrogen (N), carbon (C), and boron (B).

[0082] In this case, the other of the first layer 41 and the second layer 42 can be etched by dry etching gas using a halogen-based gas (chlorine-based gas, fluorine-based gas, etc.) that does not contain oxygen gas. In this case, either the first layer 41 or the second layer 42 has resistance to this halogen-based gas.

[0083] Furthermore, the first layer 41 and the second layer 42 of the thin film 40 do not need to have etching selectivity with respect to each other. In this case, the thin film 40 preferably has an etching stopper layer between the first layer 41 and the second layer 42.

[0084] The material of the etching stopper layer only needs to have etching selectivity with respect to the first layer 41 and the second layer 42. The material of such an etching stopper layer is not particularly limited, and a material can be selected from the materials containing the elements exemplified above as the materials constituting the thin film 40, taking into consideration the etching selectivity.

[0085] <Etching mask film 50> The etching mask film 50 can be provided on the thin film 40 as necessary. The etching mask film 50 may be a single layer or a laminated film formed by laminating a plurality of films. When the etching mask film 50 is a laminated film, each layer preferably has etching selectivity with respect to each of the other layers provided above and below.

[0086] The material of the etching mask film 50 may be any material that has etching selectivity with respect to the layer (for example, the first layer 41 in the drawing) provided on the top of the thin film 40. The material of such an etching mask film is not particularly limited, and examples thereof include a material containing one or more selected from Cr, Ta, and Si, and a material further containing one or more selected from O, N, C, and B in addition to these materials. In particular, a material containing Cr (Cr-based material) is preferable because it has high adhesion to the resist film. A material containing Ta (Ta-based material) is similarly preferable.

[0087] When the etching mask film 50 is a laminated film including two or more layers, it is preferably a laminated structure of three layers, more preferably four layers. When the etching mask film 50 is a laminated film, it is preferable to combine a layer made of a material containing Cr with a layer made of a material containing Ta. In addition, when the etching mask film 50 is a laminated film, the layer formed closest to the thin film 40 is made of a material with a high etching rate (such as CrOCN), thereby further improving the accuracy of the pattern.

[0088] For example, when the etching mask film 50 has three layers, the etching mask film 50 may include an etching mask lower layer made of a Cr-based material formed on the thin film 40, an etching mask intermediate layer made of a Ta-based material on the etching mask lower layer, and an etching mask upper layer made of a Cr-based material on the etching mask intermediate layer.

[0089] Also, for example, when the etching mask film 50 has four layers, the etching mask film 50 may include a bottom layer (etching mask lower layer) of a Cr-based material formed on the thin film 40, an etching mask middle layer made of a Ta-based material on the etching mask lower layer, an etching mask upper layer made of a Cr-based material on the etching mask middle layer, and an etching mask top layer made of a Ta-based material on the etching mask upper layer.

[0090] In this way, when the etching mask film 50 has three or four layers, the lower etching mask layer is made of a material with a high etching rate (such as CrOCN) and has a small thickness. It is preferable that the upper etching mask layer is made of a material with a low etching rate (such as CrOC) and has a larger thickness than the lower etching mask layer. This allows the upper etching mask layer to remain when the lower etching mask layer is etched, and the thickness of the etching mask film required for the subsequent etching of the first layer 41 and the second layer 42 can be made sufficient.

[0091] <Structure of reflective mask 1a> The reflective mask 1a has a transfer pattern 40a formed by patterning a thin film 40. The reflective mask 1a may have a patterned region in which the transfer pattern 40a is formed, as well as a non-patterned region in which the transfer pattern 40a is not formed. The non-patterned region is provided as a peripheral region of the patterned region in which the transfer pattern 40a is formed. Such a non-patterned region may be, for example, a region covered with a film (binary film) having an absolute reflectance of 2.5% or less, not shown here. This binary film may be provided separately between the etching mask film 50 and the thin film 40. If the etching mask film 50 has an absolute reflectance of 2.5% or less, the etching mask film 50 may be used as a binary film.

[0092] <Configuration of transfer pattern 40a in reflective mask 1a> FIG. 3 is a plan view showing the configuration of a reflective mask 1a according to an embodiment of the present invention. The reflective mask 1a shown in FIG. 2 and FIG. 3 has an island-shaped transfer pattern 40a formed by patterning a thin film 40. The transfer pattern 40a is formed by patterning a thin film 40 in which a bottom layer 43, a second layer 42, and a first layer 41 are laminated in this order on a substrate 10. Such a transfer pattern 40a is composed of a first layer pattern (second upper layer pattern) 41a obtained by patterning the first layer 41, a second layer pattern (lower layer pattern) 42a obtained by patterning the second layer 42, and a bottom layer pattern 43a obtained by patterning the bottom layer 43. In FIG. 2 and FIG. 3, a configuration in which the first layer pattern 41a (first layer 41) is formed on the second layer pattern 42a (second layer 42) is illustrated, but the second layer pattern 42a may be provided on the first layer pattern 41a. In this case, the first layer pattern is the lower layer pattern, the second layer pattern is the second upper layer pattern, and so on.

[0093] In addition, the transfer pattern 40a is in a state where the surface of the outer edge part of the lower layer pattern 42a arranged below the second upper layer pattern 41a is exposed in a plan view over the entire circumference of the second upper layer pattern 41a. Therefore, the shape of the transfer pattern 40a in a plan view is a state where the entire circumference of the second upper layer pattern 41a is surrounded by the lower layer pattern 42a. The cross-sectional shape of the transfer pattern 40a is a step shape in which the lower layer pattern 42a protrudes from a position one step lower than the second upper layer pattern 41a. In addition, in the plan view of the transfer pattern 40a, the exposed width of the lower layer pattern 42a from the second upper layer pattern 41a can be 10 nm to 40 nm. In addition, the exposed width may be set to a different value depending on the position depending on the incident direction of the EUV light [H1] as the exposure light to the reflective mask 1a.

[0094] As a result, the reflective mask 1a has a configuration in which the first layer 41 and the second layer 42 are at least partially exposed in a plan view, the second layer 42 has a laminated region in which at least a part of the second layer 42 is covered with the first layer 41, and the second layer 42 is exposed on the periphery of the laminated region. Note that the bottom layer pattern 43a preferably has the same planar shape as the lower layer pattern 42a. In addition, when another layer is provided between the first layer 41 and the second layer 42, the other layer preferably has the same planar shape as the second upper layer pattern 41a located thereon.

[0095] In the reflective mask 1a having such a configuration, the lower layer pattern 42a having a high reflectance to the EUV light [H1] is exposed at the outer periphery of the island-shaped transfer pattern 40a in plan view, i.e., at the portion constituting the outline of the transfer pattern 40a. This allows pattern exposure with a high phase shift effect for the reflected light [Rf0] from the multilayer reflective film 20. Moreover, the second upper layer pattern 41a having a low reflectance to the EUV light [H1] is exposed at the center of the island-shaped transfer pattern 40a. This reduces the amount of reflected light in the entire transfer pattern 40a, allowing pattern exposure with a sufficient exposure margin. As a result, it is possible to perform pattern exposure with a large exposure margin and high resolution without impeding the phase shift effect in the phase-shifting reflective mask 1a.

[0096] When the transfer pattern 40a is a line-and-space pattern, the outer periphery of the lower layer pattern 42a may be exposed from the side periphery of the second upper layer pattern 41a along the longitudinal direction of the line pattern in a plan view. The transfer pattern 40a may also be a hole pattern. In this case, the lower layer pattern 42a may be formed so as to surround the hole region in which the multilayer reflective film 20 (including the protective film 30) is exposed in a plan view, and the second upper layer pattern 41a may be formed so as to cover the lower layer pattern 42a while exposing the surface of the periphery in contact with the hole region of the lower layer pattern 42a by a predetermined width.

[0097] 1 may have a thin film 40 having a configuration in which a first layer 41 is laminated on top of the above-mentioned second layer 42. In this way, by stepwise patterning of the thin film 40, it is possible to obtain the reflective mask 1a shown in Figures 2 and 3, that is, a reflective mask 1a having a transfer pattern 40a whose contour is constituted by the second layer 42 having a relatively high reflectance and whose central portion is constituted by the first layer 41 having a relatively low reflectance.

[0098] <Another example of the reflective mask 1a'> FIG. 4 is a cross-sectional view showing another configuration of a reflective mask 1a' according to an embodiment of the present invention. The reflective mask 1a' shown in FIG. 4 has a first transfer pattern 40a' and a second transfer pattern 40a" formed by patterning the thin film 40 of the reflective mask blank 1 shown in FIG.

[0099] In a plan view of the first transfer pattern 40a', the lower layer pattern 42a is covered by the second upper layer pattern 41a and is not exposed. That is, the first transfer pattern 40a' can be configured in such a way that the second upper layer pattern 41a, the lower layer pattern 42a, and the bottom layer pattern 43a are stacked in substantially the same planar shape. On the other hand, the second transfer pattern 40a" is configured in such a way that the lower layer pattern 42a and the bottom layer pattern 43a are stacked in substantially the same shape. This second transfer pattern 40a" does not include the first layer 41, and in a plan view, only the second layer 42 is exposed on the surface.

[0100] As a result, the reflective mask 1a' has a configuration in which the first layer 41 and the second layer 42 are each at least partially exposed in plan view.

[0101] In the reflective mask 1a' having such a configuration, the second transfer pattern 40a'' exposing the lower layer pattern 42a having a high reflectance to EUV light [H1] enables pattern exposure with a high phase shift effect for the reflected light [Rf0] from the multilayer reflective film 20 (including the protective film 30). Such a second transfer pattern 40a'' is particularly effective when the dimensions of the second transfer pattern 40a'' are very fine and it is preferable for the second transfer pattern 40a'' to have a relatively high reflectance (for example, more than 6%) in order to obtain a sufficient phase shift effect. In addition, the first transfer pattern 40a' exposing the second upper layer pattern 41a having a low reflectance to EUV light [H1] suppresses the amount of reflected light from the first transfer pattern 40a', and the exposure mark This enables pattern exposure utilizing the phase shift effect while ensuring a sufficient reflectance. Such a first transfer pattern 40a' is particularly effective when the dimensions of the first transfer pattern 40a' are large enough to obtain a sufficient phase shift effect with a relatively low reflectance (for example, about 6%). As a result, it becomes possible to obtain a high phase shift effect and a large exposure margin at the same time by using one reflective mask 1a in accordance with the dimensions of the pattern. And even if there are areas where a high reflectance is preferable and areas where a low reflectance is preferable depending on the type (shape) or pitch of the pattern to be transferred, it becomes possible to form a pattern by exposure using only one reflective mask 1a.

[0102] 1 has a thin film 40 including the first layer 41 and the second layer 42 described above, and therefore it is possible to manufacture the reflective mask 1a' shown in Fig. 4. By using this reflective mask blank 1, it is possible to manufacture a reflective mask 1a' capable of transferring a fine pattern with high accuracy and with a sufficient margin, without complicating the process for manufacturing a phase shift mask (mask manufacturing process).

[0103] The reflective mask 1a' shown in Figure 4 is formed using the reflective mask blank 1 described using Figure 1, but an equivalent reflective mask can also be formed using a mask in which the stacking order of the first layer 41 and the second layer 42 is reversed.

[0104] <Reflection mask manufacturing method> Fig. 5 is a manufacturing process diagram showing one example of the manufacturing method of the reflective mask of the present invention, and shows the procedure for manufacturing the reflective mask 1a shown in Fig. 2 and Fig. 3 using the reflective mask blank 1 shown in Fig. 1. Hereinafter, the manufacturing method of the reflective mask will be described with reference to Fig. 5.

[0105] First, a reflective mask blank 1 is prepared as shown in Fig. 5(1). This reflective mask blank 1 is the reflective mask blank 1 described with reference to Fig. 1, and has a thin film 40 including a first layer 41 and a second layer 42. This thin film 40 is a laminated film in which one of the first layer 41 and the second layer 42, which is formed closer to the substrate 10, is the lower layer and the other is the upper layer. Here, as an example, the second layer 42 is the lower layer and the first layer 41 is the upper layer.

[0106] The reflective mask blank 1 may also have an etching mask film 50 formed on the thin film 40. However, if the reflective mask blank 1 does not have the etching mask film 50, the etching mask film 50 is formed on the thin film 40 as necessary. Thereafter, a resist film 101 is formed on the etching mask film 50 by, for example, spin coating. Note that the reflective mask blank 1 may also have the resist film 101, in which case the step of forming the resist film 101 is not necessary.

[0107] 5(2), a lithography process is performed on the resist film 101 to form a resist pattern 101a by patterning the resist film 101. In this lithography process, for example, exposure by electron beam lithography, a development process, and a rinsing process are performed.

[0108] Thereafter, the etching mask film 50 is etched using the resist pattern 101a as a mask to form an etching mask pattern 50a. The gas used to etch the etching mask film 50 may be appropriately selected depending on the material of the etching mask film 50. For example, when the etching mask film 50 is made of a Cr-based material, chlorine gas (Cl2) and oxygen gas (O2) may be used as etching gas. Also, for example, when the etching mask film 50 is made of a TaO material as a Ta-based material, the etching mask film 50 may be etched using a fluorine-based gas. Although not shown, when the etching mask film 50 is a laminated film including a plurality of layers made of different materials, the etching mask film 50 may be etched by changing the etching gas depending on the material of each layer.

[0109] Next, as shown in FIG. 5(3), the first layer 41 of the thin film 40 is etched using the etching mask pattern 50a (and the resist pattern 101a) as a mask to form a first upper layer pattern 41aa.

[0110] In this case, the etching gas for the first layer 41 can be appropriately selected depending on the material of the first layer 41. For example, when the first layer 41 is made of a HfAl material or an AlSi material, a mixed gas of chlorine gas (Cl2) and boron trichloride (BCl3) can be used as the etching gas. In this etching, the resist pattern 101a is also removed. The HfAl material and the AlSi material may further contain at least one selected from oxygen (O), nitrogen (N), carbon (C), and boron (B).

[0111] 5(4), the second layer 42 of the thin film 40 is etched using the etching mask pattern 50a and the first upper layer pattern 41aa as a mask to form a lower layer pattern 42a. The lower layer pattern 42a is formed by patterning the second layer 42 as the lower layer of the thin film 40.

[0112] In this case, the etching gas for the second layer 42 can be appropriately selected depending on the material of the second layer 42. For example, when the second layer 42 is made of a RuN material or a RuCr material, a mixed gas of chlorine gas (Cl2) and oxygen gas (O2) can be used as the etching gas. When the second layer 42 is made of a RuPt material or a RuTa material, for example, a fluorine-based gas can be used as the etching gas. The RuCr material, the RuN material, the RuPt material, and the RuTa material may further contain at least one selected from oxygen (O), nitrogen (N), carbon (C), and boron (B).

[0113] Next, as shown in FIG. 5(5), a resist film 102 is formed by coating above the substrate 10 on which the first upper layer pattern 41aa has been formed.

[0114] Thereafter, as shown in FIG. 5(6), the resist film 102 is subjected to lithography processing to form a resist pattern 102a by patterning the resist film 102. Here, the resist pattern 102a is formed to have a shape that is slightly smaller than the lower layer pattern 42a in a planar view. In this lithography processing, for example, exposure by electron beam lithography, development processing, and rinsing processing are performed. In this lithography processing, depending on the material of the lowermost layer 43, the resist film 102 may be left on the lowermost layer 43 as shown in the figure, or electron beam lithography may be performed so that the resist film 102 on the lowermost layer 43 is removed.

[0115] Thereafter, the first upper layer pattern 41aa is further etched using the resist pattern 102a as a mask to form a second upper layer pattern 41a having a planar shape slightly smaller than the lower layer pattern 42a. The second upper layer pattern 41a has a planar shape slightly smaller than the lower layer pattern 42a.

[0116] In the etching of the first upper layer pattern 41aa, the same etching gas as that in the process of Fig. 5(3) can be used. In this etching, the resist pattern 102a is also reduced in thickness.

[0117] Subsequently, as shown in FIG. 5(7), the resist pattern 102a (and the resist film 102) remaining above the substrate 10 is removed. Thereafter, the lowermost layer 43 is etched using the lower layer pattern 42a as a mask, thereby patterning the lowermost layer 43 to have the same planar shape as the lower layer pattern 42a, thereby forming the lowermost layer pattern 43a. At this time, an etching gas can be appropriately selected depending on the material of the lowermost layer 43. For example, if the lowermost layer 43 is made of TaON, a fluorine-based gas can be used as the etching gas.

[0118] As a result of the above, a reflective mask 1a having the transfer pattern 40a described with reference to FIGS. 2 and 3 is obtained.

[0119] The reflective mask 1a' described with reference to FIG. 4 is also formed partway through the same procedure as that shown in FIGS. 5(1) to (5). In the process after FIG. 5(5), a resist pattern 102a is formed so that the first upper layer pattern 41aa in the region corresponding to the second transfer pattern 40a'' is exposed. Then, after etching the exposed first upper layer pattern 41aa, the resist pattern 102a is removed, and the lower layer pattern 42a is used as a mask to etch the bottom layer 43, thereby forming the first transfer pattern 40a' and the second transfer pattern 40a''. However, in this reflective mask 1a', the lamination order of the first layer 41 and the second layer 42 may be reversed. For this reason, the reflective mask blank prepared in FIG. 5(1) may have a thin film 40 configured with the first layer 41 as the lower layer and the second layer 42 as the upper layer. EXAMPLES

[0120] Next, examples to which the present invention is applied and comparative examples will be described. Fig. 6 is a diagram showing the composition and physical properties of the thin film of the examples. Each example and comparative example will be described below with reference to Figs. 1 and 6.

[0121] In Examples 1 to 3 and Comparative Example, each layer of the reflective mask blank 1 having the layer structure shown in FIG. 1 was formed from the material shown in FIG. 6. In each Example and Comparative Example, as an example, the first layer 41 was the upper layer and the second layer 42 was the lower layer, but the present invention is not limited thereto. The first layer 41 and the second layer 42 constituting the thin film 40 were adjusted in reflectance to EUV light [H1] and phase difference of the first reflected light [Rf1] and the second reflected light [Rf2] with respect to the reference reflected light [Rf0] from the multilayer reflective film 20 via the protective film 3 as follows, depending on the material, the composition ratio of the material, and the film thickness.

[0122] Example 1 An SiO2-TiO2-based glass substrate (6 inch square, 6.35 mm thick) was prepared. The edges of this substrate were chamfered and ground, and then coarsely polished with a polishing solution containing cerium oxide abrasive grains. After these processes, the substrate was set on the carrier of a double-sided polishing machine, and precision polishing was performed under specified polishing conditions using an alkaline aqueous solution containing colloidal silica abrasive grains as the polishing solution. After precision polishing was completed, the substrate was cleaned. The surface roughness of the main surface of the obtained glass substrate was 0.10 nm or less in root-mean-square roughness (Rq). The flatness of the main surface of the obtained substrate was 30 nm or less in a measurement area of ​​132 mm x 132 mm.

[0123] A back surface conductive film made of CrN was formed on the back surface of the above substrate by magnetron sputtering under the following conditions. (Conditions): Cr target, Ar+N2 gas atmosphere, film composition (Cr: 90 atomic %, N: 10 atomic %), film thickness 20 nm

[0124] A multilayer reflective film was formed by periodically laminating Mo films / Si films on the main surface of the substrate opposite to the side on which the back conductive film was formed. Specifically, Mo films and Si films were alternately laminated on the substrate in an Ar gas atmosphere by ion beam sputtering using a Mo target and a Si target. The thickness of the Mo film was 2.8 nm. The thickness of the Si film was 4.2 nm. The thickness of one period of the Mo / Si film was 7.0 nm. Such Mo / Si films were laminated 40 times, and finally a Si film was formed to a thickness of 4.0 nm to form a multilayer reflective film.

[0125] A protective film containing Ru was formed on the multilayer reflective film. Specifically, a Ru target was used and a protective film made of Ru film was formed on the multilayer reflective film by DC sputtering in an Ar gas atmosphere. The thickness of the protective film was 3.5 nm.

[0126] Next, a TaON film was formed as the bottom layer on the protective film by DC sputtering using a Ta target in an atmosphere of Ar gas, oxygen gas, and nitrogen gas.

[0127] A second layer (lower layer) made of RuCrON film was formed on the lowermost layer made of TaON film by DC sputtering. The RuCrON film was deposited using a RuCr target in an atmosphere of Ar gas, oxygen gas, and nitrogen gas.

[0128] A HfAlO film was formed as a first layer (upper layer) on the second layer made of a RuCrON film by RF sputtering. The HfAlO film was formed in an argon (Ar) gas atmosphere using an Al2O3 target and a HfO2 target. As a result, a reflective mask blank of Example 1 was obtained.

[0129] Example 2 Example 2 is different from Example 1 in the film thickness of the second layer (lower layer) made of a RuCrON film and in the first layer (upper layer).

[0130] A back conductive film, a multilayer reflective film, a protective film, and a RuCrON film were formed on the substrate in the same manner as in Example 1. However, the thickness of the RuCrON film was changed from that in Example 1.

[0131] An AlSiO film was formed as a first layer (upper layer) on the lower layer made of a RuCrON film by RF sputtering. The AlSiO film was formed in an argon (Ar) gas atmosphere using an Al2O3 target and a SiO2 target. As a result, a reflective mask blank of Example 2 was obtained.

[0132] Example 3 In Example 3, the composition ratio and film thickness of the second layer (lower layer) made of a RuCrON film and the film thickness of the first layer (upper layer) were changed from those in Example 1.

[0133] A back conductive film, a multilayer reflective film, and a protective film were formed on the substrate in the same manner as in Example 1. Furthermore, the flow rate ratio of the sputtering gas during the RuCrON film formation in Example 1 was adjusted, and the RuCrON film of Example 3 was formed as the lower layer. The film thickness of this RuCrON film was also changed from that of Example 1.

[0134] As in Example 1, a HfAlO film was formed as a first layer (upper layer) on a lower layer made of a RuCrON film. However, the thickness of this HfAlO film was changed from that in Example 1. In this way, a reflective mask blank of Example 3 was obtained.

[0135] Comparative Example The thin film of the comparative example is different from that of Example 1. A second layer (lower layer) made of a TaTiN film was formed on the protective film by DC magnetron sputtering. The TaTiN film was formed using a TaTi target in an atmosphere of Ar gas and N2 gas.

[0136] A first layer (upper layer) was formed on a lower layer made of a TaTiN film using a material containing Ru. Specifically, a Ru film was formed by DC sputtering in an Ar gas atmosphere using a Ru target. As a result, a reflective mask blank 1 of the comparative example was obtained.

[0137] Using the reflective mask blanks 1 of Examples 1 to 3 and Comparative Example, the reflective mask 1a having the island-shaped transfer pattern 40a described with reference to FIG. 2 and FIG. 3 was fabricated by the procedure described with reference to FIG. 5. The HfAlO film and the AlSiO film were etched with BCl3 gas and Cl2 gas. The Ru film and the RuCrON film were etched with Cl2 gas and O2 gas. The TaTiN film was etched with Cl2 gas. The TaON film was etched with fluorine gas. The transfer pattern 40a was a rectangular shape with one side measuring 200 nm×200 nm in the planar shape of the lower layer pattern 42a. In the planar view of the transfer pattern 40a, the exposed width of the lower layer pattern 42a was 20 nm.

[0138] In the reflective mask blanks 1 of Examples 1 to 3, the absolute reflectance [R1] of the first layer 41 constituting the thin film 40 to the EUV light [H1] was higher than 2.5%. Also, the absolute reflectance [R2] of the second layer 42 constituting the thin film 40 to the EUV light [H1] was higher than the absolute reflectance [R1] of the first layer 41.

[0139] In addition, the phase difference of the first reflected light [Rf1] from the first layer 41 and the phase difference of the second reflected light [Rf2] from the second layer 42 with respect to the reference reflected light [Rf0] from the multilayer reflective film 20 (including the protective film 30) irradiated with EUV light [H1] were 150 degrees or more. In addition, the phase differences of the reflected lights from the first layer 41 and the second layer 42 were 30 degrees or less.

[0140] In contrast, in the comparative reflective mask blank 1, the first layer 41 constituting the thin film 40 had an absolute reflectance [R1] for EUV light [H1] of 1.7%, which was lower than 2.5% and fell outside the range of the embodiment of the present invention.

[0141] Furthermore, in the comparative reflective mask blank 1, the phase difference between the first reflected light [Rf1] from the first layer 41 and the second reflected light [Rf2] from the second layer 42 was 37 degrees, which was outside the preferred range of the embodiment of the present invention.

[0142] In addition, a simulation of EUV exposure using each of the manufactured reflective masks 1a was performed. As a result, it was confirmed that a transferred optical image having a high contrast was obtained in the EUV exposure using each of the reflective masks 1a of Examples 1 to 3. In addition, the absolute reflectance was relatively low in the region where the first layer 41 and the second layer 42 were stacked. Therefore, it was found that when a pattern transfer was performed using the reflective masks 1a of Examples 1 to 3, the risk of the resist on the transferee (semiconductor) substrate being exposed in a region that should not be exposed to light can be sufficiently reduced. That is, it was found that the reflective masks 1a of Examples 1 to 3 can achieve both a high phase shift effect and a large exposure margin. As a result, it was found that by applying EUV exposure using the reflective mask 1a of the present invention to the manufacture of a semiconductor device, it is possible to form a fine circuit pattern with high precision, and it is possible to achieve high performance and high integration of the semiconductor device.

[0143] On the other hand, in the reflective mask 1a of the comparative example, the absolute reflectance in the region where the first layer 41 and the second layer 42 are stacked is low at 1.7%, and the phase shift effect was not sufficiently obtained. Therefore, in the EUV exposure using the reflective mask 1a of the comparative example, the contrast of the transferred optical image obtained was insufficient. As a result, it was found that even if EUV exposure using the reflective mask 1a outside the scope of the present invention is applied to the manufacture of a semiconductor device, it is difficult to form a fine circuit pattern with high accuracy. In addition, in the comparative example, the phase difference between the first reflected light [Rf1] from the first layer 41 and the second reflected light [Rf2] from the second layer 42 was larger than that in the example. Therefore, it was thought that the interference between the first reflected light [Rf1] and the second reflected light [Rf2] reduced the reflected light amount (intensity) near the edge of the transfer pattern 40a, and the phase shift effect was not sufficiently obtained. [Explanation of symbols]

[0144] 1...Reflective mask blank 1a, 1a'...Reflective mask 10...Substrate 20…Multilayer reflective film 40…Thin film 40a, 40a', 40a"...Transfer pattern 41...1st layer (upper layer) 41a…First layer pattern (second upper layer pattern) 41aa…First upper layer pattern 42...2nd layer (lower layer) 42a…Second layer pattern (lower layer pattern) 43…Lowest floor 50...Etching mask film 50a…Etching mask pattern [H1]…EUV light [R1]…Reflectance of the first layer [R2]…Reflectance of the second layer [Rf1]…First reflected light [Rf2]…Second reflected light [Rf0]…Reference reflected light

Claims

1. A substrate; a multilayer reflective film formed on the substrate; a thin film formed on the multilayer reflective film, the thin film includes a first layer and a second layer; the reflectance of the first layer to EUV light is greater than 2.5%; The reflectance of the second layer to the EUV light is higher than the reflectance of the first layer. A reflective mask blank comprising:

2. A phase difference between a first reflected light reflected from the first layer irradiated with EUV light and a second reflected light reflected from the second layer irradiated with EUV light is 30 degrees or less.

2. The reflective mask blank according to claim 1 .

3. When the light reflected from the multilayer reflective film irradiated with EUV light is used as a reference reflected light, a phase difference between the reference reflected light and a first reflected light reflected from the first layer irradiated with the EUV light is 150 degrees or more; A phase difference between the reference reflected light and the second reflected light reflected from the second layer irradiated with the EUV light is 150 degrees or more.

2. The reflective mask blank according to claim 1 .

4. The thin film has a bottom layer provided closest to the substrate.

2. The reflective mask blank according to claim 1 .

5. The first layer or the second layer is made of a material containing at least one of ruthenium, tantalum, and chromium.

2. The reflective mask blank according to claim 1 .

6. The first layer is formed on the second layer.

2. The reflective mask blank according to claim 1 .

7. An etching mask film is provided on the thin film.

2. The reflective mask blank according to claim 1 .

8. The etching mask film includes two or more layers. The reflective mask blank according to claim 7 .

9. A method for producing a reflective mask using the reflective mask blank according to claim 7, comprising the steps of: When one of the first layer and the second layer formed closer to the substrate is defined as a lower layer and the other is defined as an upper layer, etching the etching mask film to form an etching mask pattern; etching the upper layer using the etching mask pattern as a mask to form a first upper layer pattern; a step of etching the lower layer using the first upper layer pattern as a mask to form a lower layer pattern; forming a transfer pattern by etching the first upper layer pattern and forming a second upper layer pattern; 2. A method for manufacturing a reflective mask comprising the steps of:

10. the thin film has a bottom layer disposed below the underlayer, In the step of forming the second upper layer pattern or after the step of forming the second upper layer pattern, the lowermost layer is removed in the region where the lower layer is etched.

10. The method for producing a reflective mask according to claim 9.

11. A substrate; a multilayer reflective film formed on the substrate; a thin film provided on the multilayer reflective film and having a transfer pattern formed thereon; the thin film includes a first layer and a second layer; the reflectance of the first layer to EUV light is greater than 2.5%; The reflectance of the second layer to the EUV light is higher than the reflectance of the first layer. A reflective mask characterized by:

12. A phase difference between a first reflected light reflected from the first layer irradiated with EUV light and a second reflected light reflected from the second layer irradiated with EUV light is 30 degrees or less.

12. The reflective mask according to claim 11.

13. When the light reflected from the multilayer reflective film irradiated with EUV light is used as a reference reflected light, a phase difference between the reference reflected light and the first reflected light reflected from the first layer irradiated with the EUV light is 150 degrees or more; A phase difference between the reference reflected light and the second reflected light reflected from the second layer irradiated with the EUV light is 150 degrees or more.

12. The reflective mask according to claim 11.

14. The thin film has a bottom layer provided closest to the substrate.

12. The reflective mask according to claim 11.

15. The first layer or the second layer is made of a material containing at least one of ruthenium, tantalum, and chromium.

12. The reflective mask according to claim 11.

16. The first layer is formed on the second layer.

12. The reflective mask according to claim 11.

17. The first layer and the second layer are each at least partially exposed in a plan view.

12. The reflective mask according to claim 11.

18. a laminated region in which at least a portion of the second layer is covered by the first layer; The second layer is exposed at an outer periphery of the laminated region in a plan view.

12. The reflective mask according to claim 11.

19. A reflective mask having a transfer pattern, which is manufactured by using the reflective mask blank according to any one of claims 1 to 8, a reflective mask manufactured by the manufacturing method according to claim 9 or 10, or a reflective mask according to any one of claims 11 to 18, which transfers the transfer pattern onto a semiconductor substrate.

4. A method for manufacturing a semiconductor device comprising the steps of:

Citation Information

Patent Citations

  • Mask for extreme ultra-violet exposure, blank, and method for pattern transfer

    JP2004207593A

  • Reflective mask

    JP2009141223A

  • Reflective mask blank and reflective mask

    JP2017223905A

  • Reflective mask blank, reflective mask and manufacturing method of semiconductor device

    JP2021144075A

  • Phase shift blankmask and photomask for extreme ultraviolet lithography

    JP2022130293A